Case-hardened steel and machine structural components formed from case-hardened steel with excellent low-cycle fatigue and pitting fatigue properties.
A case-hardening steel with controlled composition and quenching temperature addresses the limitations of conventional steels by enhancing low-cycle and pitting fatigue properties, achieving superior performance in machine structural components.
Patent Information
- Application Number
- JP2025078855
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional case-hardening steels fail to meet the demands for smaller, lighter machine structural components with both excellent low-cycle fatigue and pitting fatigue properties due to issues such as grain boundary carbide precipitation, grain coarsening, and reduced surface hardness, which are exacerbated by the need for improved fuel efficiency in automobiles.
A case-hardening steel composition comprising specific elements (C, Si, Mn, Cr, Mo, Al, V) and controlled quenching temperatures to solidify grain boundary carbides and suppress grain coarsening, ensuring a carbon concentration range and quenching temperature that enhances low-cycle and pitting fatigue characteristics without adding boron.
The proposed steel achieves 100-cycle bending fatigue strength of 17 kN or more and a pitting life ratio over twice that of equivalent steels, demonstrating superior low-cycle and pitting fatigue performance.
Smart Images

Figure 2026182541000001_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to carburized components such as machine structural components that require excellent low-cycle fatigue properties and pitting fatigue properties, for example, drive train components of automobiles and the like, and case-hardening steel suitable for obtaining machine structural components having these properties.
Background Art
[0002] Gear components such as automobile differential gears and transmission gears are often subjected to impact loads when the vehicle suddenly starts, suddenly stops, or rides over a step on a road surface, and low-cycle fatigue fracture may occur under such repeated loads of large stress and strain.
[0003] Conventionally, for components for such applications, case-hardening steels with a C content of around 0.2% such as JIS (Japanese Industrial Standards) SCr420 steel and SCM420 steel are generally used to ensure the toughness of the core part, and by performing carburizing quenching treatment and low-temperature tempering at around 150°C, the component surface is made to have a tempered martensite structure with a C content of around 0.8%, so that those with improved high-cycle bending fatigue strength and wear resistance have been used.
[0004] However, with the growing interest in environmental issues in recent years, the demand for improved fuel efficiency of automobiles is increasing. Therefore, the demand for smaller and lighter machine structural components is further increasing. Accordingly, conventional JIS steels cannot obtain sufficient strength to meet these demands.
[0005] When high surface pressure and slippage occur due to differences in peripheral speed between parts, this slippage between parts is likely to cause pitting in parts such as gears. Therefore, the applicant has previously aimed to improve pitting life in case-hardened steel used in machine structural parts, that is, in particular case-hardened steel for power transmission parts such as automobiles that have excellent pitting life, by achieving both the generation of a soft carburized abnormal layer and the suppression of softening of the steel surface after the transition to sliding on the newly formed surface of the steel, In mass%, the material contains C: 0.15-0.30%, Si: 0.40-0.70%, Mn: 0.20-0.45%, P: 0.025% or less, S: 0.025% or less, Ni: 0.20% or less, Cr: 1.40-2.00%, Al: 0.025-0.050%, and N: 0.0100-0.0250%, with the remainder being Fe and unavoidable impurities. When formula A is given by 1.4 × [Mn%] + [Cr%] + 2 × [Si%], the value calculated using formula A is 3.25 ≤ 1.4 × [Mn%] + [Cr%] + 2 × [Si%]. A carburized mechanical structural component made of steel satisfies the condition [%] ≤ 3.85, and when formula B: 2.1 × [Si%] + [Cr%] + 3.3 × [Mo%], the value calculated by formula B satisfies 2.80 ≤ 2.1 × [Si%] + [Cr%] + 3.3 × [Mo%] (where [element%] in formulas A and B above is replaced with the mass% value of the element). The hardness of the component measured at 1 mm intervals at 1 mm intervals using nanoindentation at a depth of 5 μm from the outermost surface is 9000 H. IT There were at least 8 points that met the following criteria, and when 10 points were measured at 1 mm intervals using the nanoindentation method at a depth of 20 μm from the outermost surface, the hardness was 10,000 H. IT The invention proposes a carburized mechanical structural component that meets eight or more of the above criteria, has a carbon concentration of 0.6% to 0.9% at a depth of 20 μm, and has a retained austenite (γ) content of 40 vol.% or less at a depth of 20 μm (see Patent Document 1).
[0006] Furthermore, regarding carburized parts, a carburized part with excellent low-cycle fatigue characteristics has been proposed, characterized by containing, by mass%, C: less than 0.10-0.30%, Si: 0.10% or less, Mn: 0.20-0.60%, P: 0.015% or less, S: 0.035% or less, Cr: 0.50-1.00%, Mo: 0.50-1.00%, B: 0.0005-0.0030%, Ti: 0.010-0.100%, and Nb: 0.010-0.100%, with the remainder being Fe and unavoidable impurities; a surface layer C concentration of 0.40-0.60% after gas carburizing treatment; an effective hardened layer depth of 0.6-1.2 mm with a critical hardness of 513 HV; and a surface layer hardness of 700 HV or more after shot peening treatment (see Patent Document 2). [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Patent No. 7408331 [Patent Document 2] Japanese Patent Publication No. 2008-255470 [Overview of the project] [Problems that the invention aims to solve]
[0008] The proposal in Patent Document 1 describes a steel with excellent pitting fatigue strength, characterized by a structure where the outermost surface is soft and easily abraded, while the inner layer has excellent resistance to softening. However, at the quenching temperature of 830°C described in the examples of Patent Document 1, grain boundary carbides precipitate when the surface carbon concentration increases, reducing the low-cycle fatigue strength. For example, in the steel types No. 1-3 and 5-17 of Patent Document 1, the solid solution temperature of grain boundary carbides is higher than 830°C, and grain boundary carbides are formed in all cases, so the low-cycle fatigue strength is not sufficient. Although the invention steel No. 4 in Reference Document 1 may have solid solution of grain boundary carbides, grain coarsening occurs, resulting in a reduction in low-cycle fatigue strength. Thus, the low-cycle fatigue strength was not sufficient.
[0009] Patent Document 2 attempts to ensure low-cycle fatigue strength by controlling the surface carbon concentration to 0.4-0.6%, and to compensate for the reduced surface fatigue strength caused by suppressing the surface carbon concentration by performing shot peening and defining the effective hardened layer depth. However, Patent Document 2 adds carbon (B) to obtain the effective hardened layer depth, which leads to the manifestation of heat treatment strain.
[0010] Therefore, the present invention aims to provide a mechanical structural component that achieves both excellent low-cycle fatigue characteristics and pitting fatigue characteristics, and a case-hardening steel that can suitably produce mechanical structural components with such characteristics. [Means for solving the problem]
[0011] The inventors have discovered a method to obtain mechanical structural components that exhibit both excellent low-cycle fatigue characteristics and pitting fatigue characteristics without adding B, which is widely used to improve low-cycle fatigue strength. This is achieved by increasing the quenching temperature after gas carburizing, thereby solidifying the grain boundary carbides generated during carburizing, and by suppressing the grain coarsening that tends to occur with increasing quenching temperatures through the pinning effect of VC carbides.
[0012] Therefore, the first means for solving the problems of the present invention is a case-hardening steel that, in mass%, consists of C: 0.15~0.35%, Si: 0.05~1.20%, Mn: 0.10~0.90%, P: 0.030% or less, S: 0.030% or less, Cr: 1.00~3.00%, Mo: 0.30% or less, Al: 0.015~0.300%, V: 0.10~0.40%, with the remainder being Fe and impurity elements, satisfying formula A: 17.8 ≤ 31.2[C]-8.7[Cr]+216.8[V]. However, in the formula, substitute the mass percentage values of the elemental composition of the element in brackets [ ] into the brackets [ ].
[0013] The second method is a mechanical structural component formed from the case-hardened steel described in the first method.
[0014] The third method is a mechanical structural component described in the second method, which is in a carburized state, with a carbon concentration (Cs) of 0.55-0.85% at a depth of 20 μm from the outermost surface after carburizing, and a quenching temperature T that satisfies formula B: 594.2 + 188 [Cs] + 70.5 [Cr] ≤ T ≤ 711.4 + 310.3 [C] + 38.9 [Si] + 415.4 [V]. However, in the formula, substitute the mass percentage value of the elemental composition within the brackets [ ] for [ ], and the carbon concentration (%) at a depth of 20 μm from the outermost surface after carburization for [Cs].
[0015] The fourth method is to use a composition in mass percent consisting of C: 0.15-0.35%, Si: 0.05-1.20%, Mn: 0.10-0.90%, P: 0.030% or less, S: 0.030% or less, Cr: 1.00-3.00%, Mo: 0.30% or less, Al: 0.015-0.300%, V: 0.10-0.40%, with the remainder being Fe and impurity elements, given the formula A: 17.8 ≤ 31.2[C]-8.7[Cr]+216.8 This method for manufacturing machine structural parts includes the steps of: forming the shape of a machine structural part from case-hardened steel satisfying [V]; carburizing the steel so that the C concentration (Cs) at a depth of 20 μm from the outermost surface is 0.55 to 0.85%; and quenching the steel so that the quenching temperature T satisfies the formula B: 594.2 + 188 [Cs] + 70.5 [Cr] ≤ T ≤ 711.4 + 310.3 [C] + 38.9 [Si] + 415.4 [V]. [Effects of the Invention]
[0016] The mechanical structural components of the present invention can be made to achieve both excellent low-cycle fatigue characteristics and pitting fatigue characteristics. Specifically, the mechanical structural components of the present invention have excellent low-cycle fatigue characteristics, with a 100-cycle bending fatigue strength of 17kN or more in a four-point bending fatigue test, and are L compared to steel equivalent to SCM420. 50 The pitting life ratio to the total life is more than 2. Furthermore, according to the means of the present invention, by quenching the surface at a specified C concentration and a specified quenching temperature T, it is possible to provide a case-hardened steel that can suitably produce machine structural parts with excellent low-cycle fatigue characteristics and pitting fatigue characteristics. [Brief explanation of the drawing]
[0017] [Figure 1] It is a side view showing the shape of a four-point bending fatigue test piece. [Figure 2] It is a schematic diagram showing a four-point bending fatigue test method. [Figure 3] In FIG. 3, (a) is a shape diagram of a roller pitting test piece, and (b) is a conceptual diagram of a roller pitting test. [Figure 4] FIG. 4 is a diagram showing the carburizing, quenching and tempering patterns of the present invention. [Mode for Carrying Out the Invention]
[0018] Prior to describing the embodiments of the case-hardened steel according to the present invention, the reasons for specifying the component composition of the steel and the reasons for specifying Formula A and Formula B will be explained first. The "%" in the following component compositions means mass%. In addition, the value of the mass% of the component composition of the element inside [ ] is substituted into [ ] in the formulas.
[0019] C: 0.15 to 0.35%, C is a component that increases the hardness of the base material and increases the core hardness after carburizing. If the C content is too low, the core hardness after carburizing will be insufficient, and the low-cycle fatigue strength will decrease. Therefore, the C content is set to 0.15% or more. If the C content is too high, the hardness of the base material will increase excessively, and the workability will decrease. In addition, the toughness of the core portion decreases, and the low-cycle fatigue strength decreases. Therefore, the C content is set to 0.35% or less. If the C content is too high, the hardness of the base material will increase excessively, and the workability will decrease. Therefore, the C content is set to 0.35% or less.
[0020] Si: 0.05 to 1.20%, Si is a component useful for deoxidation during steel production, and improves hardenability. Insufficient Si content leads to inadequate deoxidation during manufacturing. Furthermore, insufficient hardenability reduces core hardness after carburizing and quenching, resulting in decreased low-cycle fatigue strength. Additionally, reduced tempering softening resistance of the carburized layer leads to decreased pitting fatigue strength. Therefore, Si content should be 0.05% or more, preferably 0.20% or more. If there is an excess of Si, the hardness of the material increases too much, reducing its machinability. Therefore, the Si content should be 1.20% or less, and preferably 0.80% or less.
[0021] Mn: 0.10~0.90%, Mn is a useful component for deoxidation during manufacturing and improves hardenability. Insufficient Mn content leads to inadequate deoxidation during manufacturing. Furthermore, insufficient hardenability reduces core hardness after carburizing and quenching, resulting in decreased low-cycle fatigue strength. Therefore, Mn content should be 0.10% or higher. If the amount of Mn is excessive, the hardness of the material increases too much, reducing its machinability. Therefore, the amount of Mn should be 0.90% or less, and preferably 0.50% or less.
[0022] Cr: 1.00~3.00%, Cr is an ingredient that improves hardenability, and enhances softening resistance and pitting fatigue strength. If the chromium content is too low, the hardenability will be insufficient, the core hardness after carburizing and quenching will decrease, and the low-cycle fatigue strength will decline. In addition, the tempering softening resistance of the carburized layer will decrease, and the pitting fatigue strength will decline. Therefore, the chromium content should be 1.00% or more, and preferably 1.50% or more. If the chromium content is excessive, the material hardness increases too much, reducing workability. Furthermore, solid solution of grain boundary carbides generated during carburizing becomes difficult, leading to a decrease in low-cycle fatigue strength. Therefore, the chromium content should be 3.00% or less, preferably 2.50% or less.
[0023] Mo: 0.30% or less Mo is a component that improves hardenability and tempering softening resistance, but excessive addition leads to a decrease in workability due to increased material hardness. It also increases costs. Therefore, the amount of Mo should be kept below 0.30%.
[0024] Al: 0.015~0.300%, Al is a useful component for deoxidation during steel production. Too little Al leads to insufficient deoxidation during production, so the Al content should be 0.015% or higher. On the other hand, too much Al results in the formation of coarse nitrides (AlN), reducing workability. Therefore, the Al content should be 0.300% or less.
[0025] V: 0.10~0.40%, V is a component that improves low-cycle fatigue strength by suppressing grain coarsening during carburizing and quenching through the pinning effect obtained by the precipitation of VC. If V is too low, the amount of VC precipitated as pinning particles decreases, causing grain coarsening during carburizing and quenching, and reducing low-cycle fatigue strength. Therefore, V should be 0.10% or higher. If V is excessive, coarse VC precipitates, reducing low-cycle fatigue strength. It also leads to increased costs. Therefore, V should be kept below 0.40%.
[0026] The remaining steel components consist of Fe and unavoidable impurities. Of the unavoidable impurities, P and S shall each be limited to 0.030% or less.
[0027] P:0.030% or less Although phosphorus (P) is an unavoidable impurity, excessive P leads to reduced toughness due to grain boundary segregation and decreased low-cycle fatigue strength. Therefore, the P content should be kept below 0.030%.
[0028] S: 0.030% or less Although sulfur (S) is an unavoidable impurity, excessive S increases the amount of MnS, which is the crack propagation pathway, thus reducing the low-cycle fatigue strength. Therefore, the S content should be kept below 0.030%.
[0029] Formula A: 17.8≦31.2C-8.7Cr+216.8V Formula A relates to the precipitation amount of VC that functions as pinning particles. When the value of Formula A is below 17.8, the precipitation amount of VC as pinning particles decreases, crystal grains coarsen during carburizing and quenching, and the low-cycle fatigue strength will decrease.
[0030] C concentration (Cs) at a depth of 20 μm from the outermost surface after carburizing: 0.55 to 0.85% If the C concentration after carburizing is low, the surface hardness of the carburized layer will be insufficient, and the pitting fatigue strength and low-cycle fatigue strength will decrease. Therefore, Cs is set to 0.55% or higher. If the C concentration after carburizing is excessive, the toughness of the carburized layer will decrease, so the crack initiation life is reduced, and the low-cycle fatigue strength is lowered. In addition, retained austenite increases excessively, and the pitting fatigue strength decreases. Therefore, Cs is set to 0.85% or lower.
[0031] Quenching temperature T: Satisfy Formula B Formula B: 594.2+188[Cs]+70.5[Cr]<T<711.4+310.3[C]+38.9[Si]+415.4[V], That is, T1: 594.2+188[Cs]+70.5[Cr], When T2 is defined as 711.4+310.3[C]+38.9[Si]+415.4[V], T1<T<T2 T is the quenching temperature for machine structural parts, and it is desirable to perform quenching at a temperature higher than T1 and lower than T2. If the quenching temperature T is equal to or lower than T1, the grain boundary carbides precipitated in the carburized layer will not form a solid solution, and the low-cycle fatigue strength will decrease. If the quenching temperature T is equal to or higher than T2, the amount of VC required for pinning cannot be secured, crystal grains coarsen, and the low-cycle fatigue strength will decrease. Therefore, the quenching temperature T shall satisfy T1<T<T2. Note that the value of the mass% of the component composition of the element inside [ ] in the formula is substituted into [ ]. In addition, the value of the C concentration (%) at a depth of 20 μm from the outermost surface after carburizing is substituted into [Cs].
[0032] [Manufacturing Process of Test Material] Steels with the components of the inventive steels 1-17 and comparative steels 1-15 shown in Table 1 were melted in a 100 kg vacuum melting furnace, and these steels were hot forged at 1150°C to produce 40 mm diameter round steel bars. The remainder of the chemical components in Table 1 consists of Fe and unavoidable impurities.
[0033] [Table 1]
[0034] The obtained round steel bars were held at 1000°C for 15 minutes, then gas-cooled to 600°C, followed by air-cooling in a normalizing treatment. In this heat treatment, most of the V was dissolved in the matrix, while some precipitated as V-containing fine carbides. Subsequently, test specimens were prepared for four-point bending fatigue tests and roller pitting tests.
[0035] [Regarding evaluation criteria] The carbon concentration (Cs) after carburizing, the 100-cycle bending fatigue strength in the four-point bending fatigue test, and the life ratio in the roller pitting test are described in detail below. Furthermore, the evaluation results for the test specimens of the inventive steels 1-17 and comparative steels 1-15 are shown in Table 2.
[0036] I) Four-point bending fatigue test First, as shown in Figure 1, a 100 mm long square bar with a cross-section of 13 mm × 17 mm (17 mm for the notched surface) was formed from the middle circumference of a 40 mm diameter round steel bar. Next, these test pieces (1) were subjected to a carburizing treatment in a process described later, and the sides of the test pieces were machined by 2 mm on one side to finish them to 13 mm × 13 mm. That is, the hardened layer due to carburizing remained on the notched surface and the opposite surface. Next, as shown in Figure 1, a V-notch (2), which is a notch with a radius of 1.5 mm and a depth of 3 mm, was formed on one side of the central part of these carburized test pieces (1), 50 mm from the end in the longitudinal direction.
[0037] As shown in Figure 2, the test specimen (1) was placed on left and right support points (3) spaced 90 mm apart. In this case, the side of the test specimen (1) with the V-notch (2) was facing downwards, and the V-notch 2 of the test specimen (1) was positioned in the center of the left and right support points (3, 3) which were 13 mm apart. Furthermore, on the test specimen (1), left and right support points (4, 4) were placed 13 mm apart, evenly spaced 10 mm apart to the left and right from a position directly above the V-notch (2), with a distance of 20 mm between them. A backing plate (5) was then placed on the left and right support points (4, 4) which were 13 mm apart, and a load (6) was applied downwards from a position directly above the V-notch (2) on the backing plate (5) toward the test specimen (1). A four-point bending fatigue test was performed by repeating the bending test for 100 cycles until the test specimen fractured.
[0038] A bending fatigue strength is considered good if the bending fatigue strength after 100 cycles in a four-point bending fatigue test is 17 kN or higher.
[0039] II) Roller pitting test First, rough machining was performed on the middle circumference of a 40 mm diameter round steel bar, as shown in Figure 3(a) for the small roller (7) of the roller pitting test specimen. During the rough machining, the test section (8) was finished, and a 0.2 mm excess material was added to the gripping section (9) for finishing after carburizing. Next, these test specimens (7) were subjected to carburizing treatment in a process described later, and the small roller (7) of the roller pitting test specimen was produced by subsequent finishing.
[0040] To evaluate the pitting life using the small roller (7) of the roller pitting test specimen prepared as described above, the large roller (10) of the roller pitting test specimen shown in Figure 3(b), which is the mating material, was prepared from SCM420 equivalent steel, under the conditions shown in Table 2. A carburized abrasive of this SCM420 equivalent steel was used with a slip ratio of -40%, a surface pressure of 3.3 GPa, and a lubricating oil temperature of 80°C, and the roller pitting test shown in Figure 3(b) was performed.
[0041] [Table 2]
[0042] Then, SCM420 equivalent steel L 50 The lifespan value was set as the baseline value (1.0), and the lifespan ratio, which is how many times this value is compared to 1.0, was calculated. If the pitting lifespan ratio was 2 times or more, the pitting life was evaluated as good. Here, since comparative steel 9 is equivalent to SCM420 steel, the L of comparative steel 9 50 The evaluation was performed using the lifespan ratio, with the lifespan value set to 1.0. Note that the pitching life ratio value for this roller pitching test was obtained by conducting a test with n=5. 50 Based on the lifespan value.
[0043] [Carburizing process] For the inventive steels 1-17 and comparative steels 1-15, test specimens prepared according to the procedure described above were subjected to carburizing treatment (Cp: 0.55-0.85) in the pattern shown in Figure 4, and then oil quenched (OQ) at the quenching temperature T listed in Table 1.
[0044] III) Cs: C concentration at a depth of 20 μm from the outermost surface after carburizing. For a depth of 20 μm from the outermost surface after carburization, the specimen is first cut along a T-plane perpendicular to its length, and the carbon concentration at an arbitrary location on the T-plane corresponding to a depth of 20 μm from the outermost surface of the carburized specimen is measured using EPMA (electron beam microanalyzer).
[0045] Table 3 shows the evaluation results for the test specimens of the inventive steels 1-17 and comparative steels 1-15.
[0046] [Table 3]
[0047] Since the invention steels 1 to 17 of this invention satisfy the specified composition and formula A of case-hardened steel, it has been shown that when carburized so that Cs is within the specified range and hardened at a temperature between T1 and T2, they become parts with excellent low-cycle fatigue strength and pitting fatigue characteristics. That is, as shown in Table 3, all of the test pieces described in invention steels 1 to 17 have a 100-cycle bending fatigue strength of 17 kN or more, and exhibit excellent low-cycle fatigue strength. 50 The lifespan was more than twice that of steel equivalent to SCM420, and the pitting life ratio showed excellent pitting fatigue characteristics. Thus, by quenching the case-hardened steel specified in the means of the present invention with a predetermined carburizing concentration and appropriate temperature, machine structural components with excellent low-cycle fatigue characteristics and pitting fatigue characteristics can be obtained.
[0048] Comparative steel 1 had insufficient carbon content, resulting in insufficient core hardness after carburizing and inferior low-cycle fatigue strength. Comparative steel 2 had an excessive amount of carbon, resulting in reduced core toughness and inferior low-cycle fatigue strength. Comparative steel 3 had insufficient Si content, resulting in poor hardenability, reduced core hardness after carburizing and quenching, and inferior low-cycle fatigue strength. Furthermore, the carburized layer's resistance to tempering softening was reduced, leading to inferior pitting fatigue strength. Comparative steel 4 had insufficient manganese content, resulting in poor hardenability, a decrease in core hardness after carburizing and quenching, and inferior low-cycle fatigue strength. Comparative steel 5 had an excessive amount of the unavoidable impurity P, resulting in reduced toughness due to grain boundary segregation and inferior low-cycle fatigue strength. It also exhibited inferior pitting fatigue strength. Comparative steel 6 had an excessive amount of the unavoidable impurity sulfur (S), which increased MnS, a crack propagation pathway, resulting in inferior low-cycle fatigue strength. It also exhibited inferior pitting fatigue strength. Comparative steel 7 had insufficient Cr content, resulting in poor hardenability, reduced core hardness after carburizing and quenching, and inferior low-cycle fatigue strength. Furthermore, the carburized layer exhibited reduced tempering softening resistance, leading to inferior pitting fatigue strength. Comparative steel 8 had an excessive amount of Cr, which made solid solution of grain boundary carbides generated during carburizing difficult, resulting in inferior low-cycle fatigue strength. Comparative steel 9 is equivalent to SCM420, and its V value is too low, resulting in a low and incorrect value for equation A. This reduces the amount of VC precipitated as pinning particles, leading to grain coarsening during carburizing and quenching, and consequently, inferior low-cycle fatigue strength. It also exhibited inferior pitting fatigue strength. Comparative steel 10 had an excessive amount of V, resulting in the precipitation of coarse VC and inferior low-cycle fatigue strength. Comparative steel 11 had a low value for equation A, resulting in a reduced amount of VC precipitation as pinning particles, grain coarsening during carburizing and quenching, and inferior low-cycle fatigue strength. The C concentration on the carburized surface of the comparative steel 12 component was too low, falling outside the Cs range. As a result, the surface hardness after carburizing was insufficient, leading to poor low-cycle fatigue characteristics and poor pitting fatigue characteristics. In the comparative steel 13 component, the carbon concentration on the carburized surface was too high, exceeding the Cs range and deviating from the normal range. This resulted in a reduced crack initiation life in the carburized layer and poor low-cycle fatigue characteristics. Furthermore, the pitting fatigue strength was also inferior. In the comparative steel 14 component, the quenching temperature T was too low, below T1, resulting in poor low-cycle fatigue characteristics because the grain boundary carbides precipitated in the carburized layer did not solid dissolve. In the comparative steel 15 component, the quenching temperature T was too high, exceeding T2. As a result, the amount of VC required for pinning could not be secured, leading to grain coarsening and poor low-cycle fatigue characteristics. [Industrial applicability]
[0049] When mechanical structural parts are formed using the case-hardened steel of the present invention, they can be applied to applications that require low-cycle fatigue characteristics and pitting fatigue characteristics, such as carburized parts for drivetrain components in automobiles and the like. [Explanation of Symbols]
[0050] 1 Test specimen 2 V-notch 3 fulcrum 4 fulcrum 5 Toban 6 Load 7. Small rollers of the roller pitting test specimen 8. Testing Department 9. Grip part 10. Large roller (counter material) for roller pitting test specimens
Claims
1. A case-hardening steel having the following composition in mass%, C: 0.15-0.35%, Si: 0.05-1.20%, Mn: 0.10-0.90%, P: 0.030% or less, S: 0.030% or less, Cr: 1.00-3.00%, Mo: 0.30% or less, Al: 0.015-0.300%, V: 0.10-0.40%, with the remainder being Fe and impurity elements, satisfying formula A: 17.8 ≤ 31.2 [C] - 8.7 [Cr] + 216.8 [V]. However, in the formula, substitute the mass percentage value of the elemental composition within the brackets [ ].
2. A mechanical structural component formed from case-hardened steel as described in claim 1.
3. A mechanical structural component according to the second method, wherein the component is carburized, the carbon concentration (Cs) at a depth of 20 μm from the outermost surface after carburization is 0.55 to 0.85%, and the quenching temperature T satisfies formula B: 594.2 + 188 [Cs] + 70.5 [Cr] ≤ T ≤ 711.4 + 310.3 [C] + 38.9 [Si] + 415.4 [V]. However, in the formula, substitute the mass percentage value of the elemental composition within the brackets [ ] for [ ] and the carbon concentration (%) at a depth of 20 μm from the outermost surface after carburization for [Cs].
4. A process of forming machine structural parts from case-hardened steel that, in mass%, consists of C: 0.15-0.35%, Si: 0.05-1.20%, Mn: 0.10-0.90%, P: 0.030% or less, S: 0.030% or less, Cr: 1.00-3.00%, Mo: 0.30% or less, Al: 0.015-0.300%, V: 0.10-0.40%, with the remainder being Fe and impurity elements, satisfying formula A: 17.8 ≤ 31.2 [C] - 8.7 [Cr] + 216.8 [V]. A carburizing process in which the carbon concentration (Cs) at a depth of 20 μm from the outermost surface is 0.55 to 0.85%, A method for manufacturing a mechanical structural part, comprising the step of quenching the part to a quenching temperature T that satisfies the formula B: 594.2 + 188 [Cs] + 70.5 [Cr] ≤ T ≤ 711.4 + 310.3 [C] + 38.9 [Si] + 415.4 [V].
Citation Information
Patent Citations
Carburized component superior in low cycle fatigue characteristic
JP2008255470A
Case-hardened steel for machine structures having excellent tooth surface fatigue strength on carburized surface and machine structure parts using said case-hardened steel