tire

The tire design with a hollowed-out insulation and specific rubber components addresses the trade-off between insulation removal and adhesion, enhancing durability and fuel efficiency by maintaining adhesion and reducing heat generation.

JP2026182548APending Publication Date: 2026-11-19SUMITOMO RUBBER INDUSTRIES LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2025078865
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

The insulation in tires tends to lower low fuel consumption performance, and removing it compromises the adhesion between the inner liner and the carcass ply, particularly after thermal degradation.

Method used

A tire design with a hollowed-out insulation structure that is not continuous in the tire width direction, composed of a rubber composition containing butyl-based rubber, and an inner liner thickness of 1.0 mm or less, along with specific rubber components like isoprene-based rubber and styrene-butadiene rubber, enhances adhesion and reduces heat generation.

Benefits of technology

Improves durability and fuel efficiency by maintaining adhesion and reducing heat generation, resulting in improved overall performance post-thermal degradation.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182548000001_ABST
    Figure 2026182548000001_ABST
Patent Text Reader

Abstract

We provide tires that improve overall performance, including durability after thermal degradation and fuel efficiency. [Solution] A tire comprising a tread, an inner liner, a carcass ply, and an insulation between the inner liner and the carcass ply, wherein the insulation has a hollow structure that is not continuous in the tire width direction and is not located on the tire equatorial plane, the insulation is made of a rubber composition containing a rubber component including butyl rubber, and the thickness t of the inner liner is 1.0 mm or less.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a tire.

Background Art

[0002] The insulation is a member disposed between an inner liner containing butyl rubber and a carcass ply containing a diene rubber to secure the adhesion therebetween.

[0003] For example, Patent Document 1 describes a pneumatic tire that has excellent interfacial adhesion between an inner liner and an insulation by respectively formulating the rubber compositions for the inner liner and the insulation to have predetermined formulations.

Prior Art Documents

Patent Documents

[0004]

Patent Document 1

Summary of the Invention

Problems to be Solved by the Invention

[0005] On the other hand, since the insulation tends to lower the low fuel consumption performance of the tire, it is an unfavorable member from the viewpoint of low fuel consumption performance. Therefore, it is conceivable to remove the insulation in order to improve the low fuel consumption performance. However, when the insulation is completely removed, the adhesion between the inner liner and the carcass ply decreases. In particular, the adhesion between the inner liner and the carcass ply after thermal degradation of the tire decreases.

[0006] An object of the present invention is to provide a tire that improves the overall performance of durability performance after thermal degradation and low fuel consumption performance.

Means for Solving the Problems

[0007] The present invention relates to the following tire. A tire comprising a tread, an inner liner, a carcass ply, and an insulation between the inner liner and the carcass ply, wherein the insulation has a hollowed-out structure that is not continuous in the tire width direction and is not disposed on the tire equatorial plane, the insulation is composed of a rubber composition containing a rubber component including a butyl-based rubber, and the thickness t of the inner liner is 1.0 mm or less. Effects of the Invention

[0008] According to the present invention, a tire that improves the overall performance of durability performance after thermal degradation and low fuel consumption performance is provided. Brief Description of the Drawings

[0009] [Figure 1] This is a cross-sectional view of a tire according to one embodiment of the present invention, taken along a plane passing through the tire rotation axis. Modes for Carrying Out the Invention

[0010] Hereinafter, a tire which is one embodiment of the present invention will be described. The tire according to one embodiment of the present invention is a tire comprising a tread, an inner liner, a carcass ply, and an insulation between the inner liner and the carcass ply, wherein the insulation has a hollowed-out structure that is not continuous in the tire width direction and is not disposed on the tire equatorial plane, the insulation is composed of a rubber composition containing a rubber component including a butyl-based rubber, and the thickness t of the inner liner is 1.0 mm or less.

[0011] While not intending to be bound by theory, the reason why the overall performance of durability performance after thermal degradation and low fuel consumption performance is improved in the present invention is considered as follows.

[0012] First, in the tire according to the present invention, (1) since the insulation is not continuous in the tire width direction, the tire can be made lighter and its fuel efficiency can be improved. (2) Since the insulation contains butyl rubber, the adhesion to the inner liner is improved, so the adhesion between the carcass ply and the inner liner is improved and the durability after thermal degradation is improved. (3) Since the thickness t of the inner liner is 1.0 mm or less, the tire can be made lighter, and (4) since the amount of rubber composition for the inner liner, which has high heat generation properties, is reduced, the heat generation of the inner liner during driving can be suppressed. It is believed that the above (1) to (4) work together to provide a tire that improves the overall performance of durability after thermal degradation and fuel efficiency, which is a remarkable effect.

[0013] Preferably, the rubber component constituting the insulation further contains 50% by mass or more of isoprene-based rubber.

[0014] By incorporating 50% or more by mass of isoprene-based rubber, which has good adhesion to the inner liner and excellent fracture strength, into the insulation, the durability of the tire is expected to be further improved.

[0015] Preferably, the rubber component constituting the insulation further contains 15% by mass or more of styrene-butadiene rubber.

[0016] By incorporating 15% by mass or more of styrene-butadiene rubber into the insulation, the heat resistance of the rubber composition constituting the insulation is improved, and the durability performance after thermal degradation is expected to be further enhanced.

[0017] The maximum load capacity of the aforementioned tire is W L (kg), if the tire weight is G (kg), then G / W L It is preferable that the value is 0.0140 or less.

[0018] Golden Week LBy keeping the weight below a certain level and reducing the weight of the tires, it is believed that fuel efficiency can be further improved.

[0019] The rubber composition constituting the insulation preferably contains recycled carbon black.

[0020] By incorporating recycled carbon black with a wide particle size distribution into the insulation, the insulation can move more flexibly in response to various inputs during driving, which is expected to further improve the tire's durability.

[0021] Preferably, the end of the insulation closest to the tire equator is located outside a width of half the tread contact width, centered on the tire equator, and inside the tread contact edge.

[0022] By positioning the end of the insulation closest to the tire's equator at the above location, the insulation is placed in the area where the greatest distortion occurs during driving, thus enabling a higher level of balance between durability and fuel efficiency.

[0023] When the tanδ of the rubber composition constituting the insulation at 70°C is defined as 70°Ctanδ, it is preferable that the product of 70°Ctanδ and t (mm) (70°Ctanδ × t) is less than 0.15.

[0024] If the tanδ of the insulation at 70°C is large, it is thought that low fuel consumption performance can be ensured by reducing the thickness t of the inner liner.

[0025] When M is the 100% modulus of the rubber composition constituting the insulation at a 23°C atmosphere, 70°C E* is the complex modulus of the rubber composition constituting the insulation at 70°C, and 70°C tanδ is the tanδ of the rubber composition constituting the insulation at 70°C, it is preferable that the product of M and 70°C E* / 70°C tanδ (M × 70°C E* / 70°C tanδ) is greater than 70.

[0026] By setting M×70℃E* / 70℃tanδ within the above range, it is possible to suppress tire heat generation and further improve fuel efficiency.

[0027] The tread has one or more circumferential grooves, and when the groove depth of the deepest part of the circumferential groove is H, it is preferable that the product of H and the 70°C tanδ (H × 70°C tanδ) is less than 1.2.

[0028] By setting H × 70°C tanδ within the above range, it is possible to suppress tire heat generation and further improve fuel efficiency.

[0029] The rubber component constituting the insulation preferably contains more than 1.0% by mass and less than 20% by mass of butyl rubber.

[0030] It is believed that this can improve the air permeability of the insulation and also improve the adhesion between the insulation and the inner liner.

[0031] [Definition] "Normal condition" refers to a state of no load where the wheel is mounted on a normal rim and filled with air at the normal internal pressure.

[0032] A "standard rim" refers to the rim specified for each tire within the standards system that the tire is based on. For example, for JATMA (Japan Automobile Tire Manufacturers Association), it refers to the standard rim for the applicable size listed in the "JATMA YEAR BOOK," for ETRTO (The European Tyre and Rim Technical Organisation), it refers to the "Measuring Rim" listed in the "STANDARDS MANUAL," and for TRA (The Tire and Rim Association, Inc.), it refers to the "Design Rim" listed in the "YEAR BOOK." Refer to JATMA, ETRTO, and TRA in that order, and if an applicable size is available at the time of reference, follow that standard. In the case of a tire not specified in the above standards, it refers to the narrowest rim width among the smallest diameter rims that can be mounted on that tire and that can maintain internal pressure (i.e., do not cause air leakage between the rim and tire).

[0033] "Regular internal pressure" refers to the air pressure specified for each tire in the standards system, including the standard on which the tire is based. For example, for JATMA it refers to "maximum air pressure," for ETRTO it refers to "INFLATION PRESSURE," and for TRA it refers to the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES." As with regular rims, refer to JATMA, ETRTO, and TRA in that order, and if there is an applicable size at the time of reference, follow that standard. In the case of tires not specified in the above standards, it refers to the regular internal pressure (but at least 250kPa) of another tire size (but specified in the standard) that is listed with the aforementioned regular rim as the standard rim. If multiple regular internal pressures of 250kPa or higher are listed, refer to the lowest value among them.

[0034] "Regular load (kg)" refers to the load specified for each tire in the standard system that the tire is based on. For example, for JATMA it is "Maximum Load Capacity," for ETRTO it is "LOAD CAPACITY," and for TRA it is the maximum value listed in the table "TIRE LOAD LIMITS AT VARIOUS COLD INFLATION PRESSURES." As with regular rims and regular in-tire pressure, refer to JATMA, ETRTO, and TRA in that order, and if an applicable size is available at the time of reference, follow that standard. For tires not specified in the above standards, the maximum load capacity (kg) is calculated separately. L This is considered the normal load.

[0035] "Maximum load capacity W L The weight (kg) is calculated using the following formula: "V" is the virtual volume of the tire (mm²). 3 ), "Dt" is the outer diameter of the tire in the normal state (mm), "Ht" is the height of the tire's cross-section in the radial direction in a plane containing the tire's axis of rotation (mm), and "Wt" is the width of the tire's cross-section in the normal state (mm). Ht can be calculated by (Dt-R) / 2, where R is the rim diameter of the tire. Wt is the value obtained by removing any patterns or letters on the tire's sidewall. Note that the maximum load capacity is synonymous with the normal load mentioned above.

[0036]

number

[0037] "Tire weight G" refers to the weight of the tire alone, excluding the weight of the rim. However, if the tire's internal cavity contains components such as sponge or sealant, or sensor components, the weight includes these components.

[0038] Unless otherwise specified, the "dimensions of each part of the tire" refer to values ​​determined in the normal state for those visible on the outer surface of the tire, and values ​​determined for those located inside the tire or on the cut surface of the tire by cutting the tire in a plane containing the tire's axis of rotation and holding the cut tire piece within the rim width of the normal rim.

[0039] "Inner liner thickness t" refers to the thickness of the inner liner in the tire radial direction on the tire equatorial plane in a cross-section of the tire containing the tire rotation axis. If the component is not located on the tire equatorial plane, it refers to the thickness of one layer of the component in the tire radial direction at the center of the component in the tire width direction.

[0040] "Tread" refers to the component that forms the contact surface of the tire with the ground.

[0041] "Circumferential grooves" refer to grooves that extend continuously in the circumferential direction of the tire. Circumferential grooves may extend in a straight line along the circumferential direction, or they may extend in a wavy, sinusoidal, or zigzag pattern along the circumferential direction.

[0042] A "carcass ply" is a component that forms the skeleton of a pneumatic tire, and the carcass ply comprises carcass cords and carcass stopping rubber that covers the carcass cords.

[0043] The "contact area" is the tread area obtained from the contour when the tire is pressed against the ground. It is obtained by mounting the tire on a standard rim, filling it with standard internal pressure, letting it stand at 25°C for 24 hours, then applying ink to the surface of the tire tread, applying a standard load (a load equal to the maximum load capacity) to the tire, pressing it perpendicularly to cardboard (camber angle of 0°), and transferring the ink.

[0044] "Tread contact edge Te" refers to the outermost edge in the tire width direction within the contact area.

[0045] "Tread contact width" refers to the distance in the axial direction of the tire's rotation from one tread contact edge to the other.

[0046] The "loss tangent and complex modulus of the rubber composition" are the loss tangent (tanδ) and complex modulus E* (MPa) measured in extension mode under various conditions using a dynamic viscoelasticity measuring device (e.g., the Iplexer series from GABO). The sample used for dynamic viscoelasticity measurement is a vulcanized rubber composition with dimensions of 20 mm in length, 4 mm in width, and 1 mm in thickness. When creating a sample by cutting it from a tire, if the material used to create the sample is insulation, the length direction of the sample should be aligned with the tire's circumferential direction, the thickness direction of the sample should be aligned with the tire's radial direction, and the sample should be created as close as possible to the specified dimensions.

[0047] "70℃tanδ" and "70℃E*" are the loss tangent (tanδ) and complex modulus E* (MPa), respectively, measured under conditions of 70℃ temperature, 10Hz frequency, 5% initial strain, ±1% dynamic strain, and extension mode.

[0048] The "100% modulus of the rubber composition" is the 100% tensile stress (MPa) obtained when a 1 mm thick, No. 7 dumbbell-shaped test specimen is prepared and subjected to a tensile test at a 23°C atmosphere and a tensile speed of 3.3 mm / second, in accordance with JIS K 6251:2017. When preparing the measurement sample from a test tire, the longitudinal and thickness directions are the same as those for measuring tanδ and E* of the rubber composition. If it is difficult to take a sample with a thickness of 1 mm, the sample should be taken as close to 1 mm as possible. This is because the 100% modulus is measured as a standardized value and is therefore not affected by thickness.

[0049] "Rubber components of a rubber composition" refer to components that contribute to crosslinking within a rubber composition, and generally have a weight-average molecular weight (Mw) of 10,000 or more.

[0050] "Styrene content" can be determined by pyrolysis gas chromatography or NMR measurement. 1 H-NMR and 13C-NMR). Unlike physical property values such as complex modulus of elasticity (E*), component amounts such as "styrene content" have a true value that does not depend on the measurement method, so it is preferable to use a measurement method with as high accuracy as possible. As used in the present specification, "pyrolysis gas chromatography" refers to a method in which a sample is heated by a pyrolyzer, individual components contained in the gas phase components generated by this heating are separated by a separation column, and each isolated component is analyzed.

[0051] "Vinyl content (amount of 1,2-bonded butadiene units)" is calculated by pyrolysis gas chromatography or NMR measurement ( 1 H-NMR or 13 C-NMR). Like the "styrene content", the "vinyl content" also has a true value that does not depend on the measurement method, so it is preferable to use a measurement method with as high accuracy as possible.

[0052] "Cis content (amount of cis-1,4-bonded butadiene units)" is a value measured by an infrared absorption spectrum analysis method or NMR measurement ( 1 H-NMR or 13 C-NMR) in accordance with JIS K 6239-2:2017, and is applied, for example, to rubber components having repeating units derived from butadiene such as BR. Like the "styrene content", the "cis content" also has a true value that does not depend on the measurement method, so it is preferable to use a measurement method with as high accuracy as possible.

[0053] "Weight average molecular weight (Mw)" can be determined in terms of standard polystyrene based on the measurement value obtained by gel permeation chromatography (GPC) (for example, GPC-8000 series manufactured by Tosoh Corporation, detector: differential refractometer, column: TSKgel (registered trademark) SuperMultipore HZ-M manufactured by Tosoh Corporation). It is applied, for example, to SBR, BR, plasticizers and the like.

[0054] "Nitrogen adsorption specific surface area (N2SA) of carbon black" is measured in accordance with JIS K 6217-2:2017.

[0055] The "average primary particle diameter" is a value obtained by photographing particles with a transmission or scanning electron microscope and taking the arithmetic mean of the particle diameters of 400 particles. If the particle is spherical, the diameter of the sphere is used as the particle diameter; if it is not spherical, the equivalent diameter of a circle (the positive square root of {4 × (particle area) / π}) is calculated from the microscope image and used as the particle diameter.

[0056] A "plasticizer" is a material that imparts plasticity to rubber components and is extracted from rubber compositions using acetone. This definition includes both liquid plasticizers at 25°C and solid plasticizers at 25°C. However, it excludes waxes and stearic acid commonly used in the tire industry.

[0057] "Plasticizer content" includes the amount of plasticizer in the rubber component that has been stretched by the plasticizer.

[0058] The "softening point of resin" is the temperature at which the sphere descends when the softening point specified in JIS K 6220-1:2015 7.7 is measured using a ring-type softening point measuring device.

[0059] [tire] The embodiments will be described in more detail below. However, the following description is illustrative for explaining the present invention, and the present invention is not limited to these. Drawings will be used as appropriate, but the drawings are for illustrative purposes only.

[0060] (Tire weight G) From the viewpoint of the effects of the present invention, the tire weight G of the tire according to this embodiment is preferably 10.0 kg or less, more preferably 9.0 kg or less, even more preferably 8.0 kg or less, even more preferably 7.8 kg or less, and particularly preferably 7.5 kg or less. Furthermore, the tire weight G is preferably 6.0 kg or more, and more preferably 6.5 kg or more.

[0061] (Maximum load capacity of the tire W L ) The maximum load capacity W of the tire according to this embodiment LThe weight is preferably 400 kg or more, more preferably 450 kg or more, and even more preferably 500 kg or more. L The weight is preferably 800 kg or less, more preferably 750 kg or less, and even more preferably 700 kg or less. L Such W is obtained by the above calculation formula. L For example, a suitable tire size would be 205 / 55R16.

[0062] (G / W L ) G / W of the tire according to this embodiment L From the viewpoint of the effects of the present invention, a value of 0.0150 or less is preferred, a value of 0.0145 or less is more preferred, and a value of 0.0140 or less is even more preferred. Also, G / W L Preferably, the value is 0.0110 or higher, more preferably 0.0120 or higher, and even more preferably 0.0125 or higher.

[0063] A tire according to one embodiment of the present invention will be described below with reference to the drawings. Note that the embodiments shown below are merely examples, and the tire of the present invention is not limited to the embodiments described below.

[0064] Figure 1 shows a portion of a cross-section of a tire according to one embodiment of the present invention, when cut by a plane including the tire's rotation axis. In Figure 1, the direction perpendicular to the plane of the paper is the circumferential direction of the tire. In Figure 1, the dashed line CL represents the tire equator.

[0065] The tire according to this embodiment comprises a tread 1, an inner liner 2, a carcass ply 3, and an insulation 4, the insulation 4 being located between the inner liner 2 and the carcass ply 3. The insulation 4 according to this embodiment is not continuous in the tire width direction.

[0066] In Figure 1, the tire has a band layer 6 and a belt layer 5 on the radially inward side of the tread 1. The belt layer 5 is laminated in two layers, with the band layer 6 positioned between the tread 1 and the belt layer 5. The band layer 6 consists of an edge band 6b that covers only the edge portion of the belt layer 5 and a full band 6a that covers the entire area of ​​the belt layer 5. Below the belt layer 5, a carcass ply 3 and an inner liner 2 are laminated. The tire according to this embodiment is not limited to this configuration, but it is preferable to have a belt layer 5 and a band layer 6, and it is more preferable to have a belt layer consisting of two or more belt plies and a band layer consisting of one or more band plies.

[0067] In Figure 1, the insulation 4 is located on the radially inner side of the carcass ply 3 and on the radially outer side of the inner liner 2. The insulation 4 is not continuous in the tire width direction and is not located on the tire equatorial plane where the tire equator CL exists.

[0068] The thickness t of the inner liner according to this embodiment is 1.0 mm or less, preferably 0.9 mm or less. The thickness t of the inner liner is a value measured by the measurement method described above.

[0069] The insulation 4 according to this embodiment is not continuous in the tire width direction and has two or more insulation ends in the tire width direction. The insulation ends may be located at any position on the tire, but it is preferable that each of the two or more insulation ends closest to the tire equator is located outside a width of half the tread contact width centered on the tire equator, and inside the tread contact edge.

[0070] From the viewpoint of fuel efficiency, the ratio of the width of the insulation rubber in the tire width direction to the tread contact width TW is preferably 60% or less, more preferably 45% or less, and even more preferably 30% or less. From the viewpoint of durability, this ratio is preferably 10% or more, and more preferably 15% or more.

[0071] The tanδ (70°C tanδ) of the rubber composition constituting the insulation at 70°C is preferably 0.11 or higher, more preferably 0.115 or higher, and even more preferably 0.12 or higher. Furthermore, the 70°C tanδ is preferably 0.15 or lower, more preferably 0.145 or lower, and even more preferably 0.14 or lower.

[0072] The complex modulus of elasticity (70°CE*) of the rubber composition constituting the insulation at 70°C is preferably 2.5 MPa or higher, more preferably 3.0 MPa or higher, and even more preferably 4.0 MPa or higher. Furthermore, the 70°CE* is preferably 5.5 MPa or lower, more preferably 5.2 MPa or lower, and even more preferably 5.0 MPa or lower.

[0073] The 100% modulus M of the rubber composition constituting the insulation at a 23°C atmosphere is preferably 1.2 MPa or higher, more preferably 1.4 MPa or higher, even more preferably 1.5 MPa or higher, even more preferably 1.7 MPa or higher, and particularly preferably 1.8 MPa or higher. Furthermore, the 100% modulus M is preferably 2.5 MPa or lower, and more preferably 2.3 MPa or lower.

[0074] Furthermore, the physical properties of the rubber composition, such as tanδ, E*, and 100% modulus, can be appropriately adjusted depending on the type and amount of rubber components, fillers, plasticizers, etc., as described below. For example, 70°C E* can be increased by increasing the amount of isoprene-based rubber in the rubber components.

[0075] The value of 70°C tanδ × t is preferably less than 0.17, more preferably less than 0.15, and even more preferably less than 0.14. Furthermore, there is no particular lower limit for 70°C tanδ × t, but it can be, for example, greater than 0.98, greater than 0.10, greater than 0.11, etc.

[0076] M×70℃E* / 70℃tanδ is preferably greater than 45, more preferably greater than 60, and even more preferably greater than 70. Furthermore, there is no particular upper limit to M×70℃E* / 70℃tanδ, but it can be, for example, less than 100, less than 90, or less than 80.

[0077] The tread 1 according to this embodiment may be a tread consisting of a single rubber layer, or it may be a tread having an outer layer that constitutes the tread surface (cap rubber layer) and one or more rubber layers (inner rubber layers) that exist between the cap rubber layer and the band layer 6. The tread 1 according to this embodiment preferably has one or more circumferential grooves 11.

[0078] The groove depth H at the deepest part of the circumferential grooves of the tread is preferably 5.0 mm or more, more preferably 5.5 mm or more, even more preferably 6.0 mm or more, and particularly preferably 6.5 mm or more. Furthermore, the groove depth H at the deepest part of the circumferential grooves is preferably 12.0 mm or less, more preferably 10.0 mm or less, and even more preferably 9.0 mm or less.

[0079] When the groove depth of the deepest part of the circumferential groove 11 of the tread according to this embodiment is H, the product of H and 70°C tanδ (H × 70°C tanδ) is preferably less than 2.0, more preferably less than 1.5, even more preferably less than 1.2, and even more preferably less than 1.1. Furthermore, H × 70°C tanδ is preferably greater than 0.5, more preferably greater than 0.6, and even more preferably greater than 0.7.

[0080] [Rubber composition constituting the insulation] The rubber composition constituting the insulation contains rubber components including butyl rubber, and all of these can be manufactured using the raw materials described below. The rubber composition constituting the insulation will be described below.

[0081] <Rubber components> The rubber component contains butyl rubber, preferably contains butyl rubber and diene rubber, and more preferably consists only of butyl rubber and diene rubber.

[0082] ≪Butyl rubber≫ As butyl rubbers, polymers and derivatives containing isobutylene units and isoprene units as repeating units are preferred. Examples of such butyl rubbers include butyl rubber (IIR), brominated butyl rubber (Br-IIR), chlorinated butyl rubber (Cl-IIR), and other halogenated butyl rubbers. Among these, halogenated butyl rubber is preferred because it can improve sheet processability and air barrier properties in a balanced way, and brominated butyl rubber and chlorinated butyl rubber are more preferred. Butyl rubbers may be used alone or in combination of two or more types.

[0083] In addition to regular butyl rubber (butyl rubber other than recycled butyl rubber), recycled butyl rubber can also be used in combination. Since recycled butyl rubber usually has a high content of unhalogenated butyl rubber (regular butyl rubber), using it in combination with halogenated butyl rubber ensures good air barrier properties and vulcanization speed. Recycled butyl rubber may be used alone or in combination of two or more types.

[0084] Examples of butyl-based rubbers that can be used include products from ExxonMobil, ENEOS Material Corporation, Arlanxeo, JSR Corporation, and Nippon Butyl Co., Ltd.

[0085] From the viewpoint of durability, the butyl rubber content in 100% by mass of the rubber component is preferably more than 1.0% by mass, more preferably more than 3% by mass, preferably 5% by mass or more, more preferably 8% by mass or more, and even more preferably 10% by mass or more. On the other hand, since other rubber components such as diene rubber are blended, the content of these components is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and particularly preferably less than 20% by mass.

[0086] Diene-based rubber Any diene rubber commonly used in the tire industry can be suitably used as the diene rubber. Specifically, examples include isoprene rubber, butadiene rubber (BR), styrene-butadiene rubber (SBR), styrene-isoprene rubber (SIR), styrene-isoprene-butadiene rubber (SIBR), chloroprene rubber (CR), acrylonitrile-butadiene rubber (NBR), etc., and it is preferable that isoprene rubber is included. The diene rubber may be used alone or in combination of two or more types.

[0087] (Isoprene rubber) As isoprene-based rubbers, for example, isoprene rubber (IR) and natural rubber, which are common in the tire industry, can be used. Natural rubber includes not only unmodified natural rubber (NR), but also modified natural rubbers such as epoxidized natural rubber (ENR), hydrogenated natural rubber (HNR), deproteinized natural rubber (DPNR), high-purity natural rubber, and grafted natural rubber. These isoprene-based rubbers may be used individually or in combination of two or more types.

[0088] NR is not particularly limited and can be any that is common in the tire industry, such as SIR20, RSS#3, TSR20, etc.

[0089] From the viewpoint of durability, the isoprene-based rubber content in the rubber component is preferably 30% by mass or more, more preferably 40% by mass or more, even more preferably 50% by mass or more, and particularly preferably 55% by mass or more. Furthermore, the content is preferably 90% by mass or less, more preferably 85% by mass or less, and even more preferably 70% by mass or less.

[0090] (SBR) There are no particular limitations on SBR, and examples include solution-polymerized SBR (S-SBR), emulsion-polymerized SBR (E-SBR), and modified SBRs thereof (modified S-SBR, modified E-SBR). Modified SBRs include SBRs in which the terminals and / or main chain are modified, and modified SBRs coupled with tin, silicon compounds, etc. (condensates, those with branched structures, etc.). Furthermore, hydrogenated versions of these SBRs (hydrogenated SBRs) can also be used. These SBRs may be used individually or in combination of two or more types.

[0091] As the SBR, either oil-expanded SBR or non-oil-expanded SBR can be used. In this specification, as the SBR, commercially available products from JSR Corporation, Sumitomo Chemical Co., Ltd., UBE Corporation, Asahi Kasei Corporation, ZS Elastomer Corporation, ARLANXEO, etc. can be used.

[0092] From the viewpoint of heat resistance, the styrene content of SBR is preferably more than 10% by mass, more preferably more than 15% by mass, and even more preferably more than 20% by mass. On the other hand, the styrene content of SBR is preferably less than 55% by mass, more preferably less than 50% by mass, and even more preferably less than 45% by mass. If the styrene content of SBR exceeds 55% by mass, the styrene groups will be adjacent to each other, the polymer will become too hard, the crosslinking will tend to be uneven, and the heat resistance may deteriorate. In this specification, the styrene content of SBR is measured by the measurement method described above.

[0093] The vinyl content of SBR is preferably more than 10 mol%, more preferably more than 15 mol%, and even more preferably more than 17 mol%. Furthermore, the vinyl content of SBR is preferably less than 70 mol%, more preferably less than 65 mol%, and even more preferably less than 60 mol%. In this specification, the vinyl content of SBR is measured by the measurement method described above.

[0094] The weight-average molecular weight (Mw) of SBR is preferably greater than 200,000, more preferably greater than 300,000, even more preferably greater than 400,000, and particularly preferably greater than 500,000. Furthermore, from the viewpoint of crosslinking uniformity, the Mw is preferably less than 2,000,000, more preferably less than 1,500,000, and even more preferably less than 1,000,000. The Mw of SBR is measured by the measurement method described above.

[0095] The content of SBR in the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, and even more preferably 15% by mass or more. Furthermore, the content of SBR in the rubber component is preferably 50% by mass or less, more preferably 40% by mass or less, even more preferably 30% by mass or less, and even more preferably 20% by mass or less.

[0096] (BR) BR is not particularly limited, and for example, BR with a cis content of less than 50 mol% (low-cis BR), BR with a cis content of 90 mol% or more (high-cis BR), rare-earth butadiene rubber synthesized using a rare-earth element catalyst (rare-earth BR), BR containing syndiotactic polybutadiene crystals (SPB-containing BR), modified BR (high-cis modified BR, low-cis modified BR), etc., which are common in the tire industry, can be used. These BRs may be used individually or in combination of two or more types.

[0097] High-cis BR can be commercially available from companies such as Nippon Zeon Co., Ltd., UBE Corporation, and JSR Corporation. Including high-cis BR can improve low-temperature properties and wear resistance. The cis content of high-cis BR is preferably more than 95 mol%, more preferably more than 96 mol%, and even more preferably more than 97 mol%. The cis content of BR is measured by the measurement method described above.

[0098] Rare earth-based BR is synthesized using a rare earth element catalyst, and has a vinyl content of preferably less than 1.8 mol%, more preferably less than 1.6 mol%, and even more preferably 1.5 mol% or less, and a cis content of preferably more than 95 mol%, more preferably more than 96 mol%, and even more preferably 97 mol% or more. As rare earth-based BR, commercially available products from companies such as Lanxess can be used.

[0099] SPB-containing BR refers to a type in which 1,2-syndiotactic polybutadiene crystals are not simply dispersed in BR, but are chemically bonded to and dispersed in BR. Such SPB-containing BR can be commercially available from companies such as UBE Corporation.

[0100] Examples of modified BR include BR modified with functional groups similar to those described for SBR above, as well as modified butadiene rubber (modified BR) in which the terminal and / or main chain is modified with functional groups containing at least one element selected from the group consisting of silicon, nitrogen, and oxygen.

[0101] Other modified BRs include those obtained by polymerizing 1,3-butadiene with a lithium initiator and then adding a tin compound, and in which the ends of the modified BR molecule are linked by a tin-carbon bond (tin-modified BR). Furthermore, the modified BR may be either unhydrogenated or hydrogenated.

[0102] From the viewpoint of wear resistance, the weight-average molecular weight (Mw) of BR is preferably over 300,000, more preferably over 350,000, and even more preferably over 400,000. From the viewpoint of crosslinking uniformity, it is preferably less than 2,000,000, more preferably less than 1,000,000, and even more preferably less than 500,000. Mw can be determined by the method described above.

[0103] When BR is included, its content in the rubber component is preferably 5% by mass or more, more preferably 10% by mass or more, even more preferably 20% by mass or more, and even more preferably 30% by mass or more. Furthermore, the content of BR in the rubber component is preferably 50% by mass or less, more preferably 40% by mass or less, and even more preferably 35% by mass or less.

[0104] The content of diene rubber in the rubber component is preferably more than 50% by mass, more preferably more than 55% by mass, even more preferably more than 60% by mass, and particularly preferably more than 70% by mass. Furthermore, the content of diene rubber in the rubber component is preferably less than 95% by mass, and more preferably less than 90% by mass.

[0105] (Other rubber components) The rubber component may contain rubber components other than the butyl rubber and diene rubber described above, to the extent that it does not affect the effects of the invention. Other rubber components that can be used include those commonly used in the tire industry, such as ethylene propylene rubber, polynorbornene rubber, silicone rubber, polyethylene chloride rubber, fluororubber (FKM), acrylic rubber (ACM), and hydrin rubber. Other rubber components may be used individually or in combination of two or more.

[0106] Furthermore, the rubber composition may or may not contain known thermoplastic elastomers in addition to the rubber components mentioned above.

[0107] ≪Rubber components synthesized from recycled and biomass-derived raw materials≫ Monomers, which are the constituent units of synthetic rubbers such as IR, SBR, and BR, may be derived from underground resources such as petroleum and natural gas, or they may be recycled from rubber products such as tires or non-rubber products such as polystyrene. The monomers obtained by recycling (recycled monomers) are not particularly limited, but include recycled polyisoprene, recycled butadiene, and recycled aromatic vinyl compounds. Examples of butadiene include 1,2-butadiene and 1,3-butadiene. Examples of aromatic vinyl compounds are not particularly limited, but include styrene. In particular, it is preferable to use recycled polyisoprene (recycled isoprene), recycled butadiene (recycled butadiene), and / or recycled styrene (recycled styrene) as raw materials.

[0108] The method for producing recycled monomer is not particularly limited, and for example, it can be synthesized from recycled naphtha obtained by decomposing rubber products such as tires. Furthermore, the method for producing recycled naphtha is not particularly limited, and for example, rubber products such as tires may be decomposed under high temperature and pressure, decomposed by microwaves, or extracted after mechanical grinding.

[0109] Furthermore, the monomers that make up polymers such as IR, SBR, and BR may be derived from biomass. In this specification, biomass refers to substances derived from natural resources such as plants. Biomass is not particularly limited, but examples include agricultural, forestry, and fishery products, sugars, wood chips, plant residues after obtaining useful components, plant-derived ethanol, and biomass naphtha.

[0110] The biomass-derived monomer (biomass monomer) is not particularly limited and includes biomass-derived butadiene and biomass-derived aromatic vinyl compounds. Examples of the butadiene include 1,2-butadiene and 1,3-butadiene. Examples of the aromatic vinyl compound are not particularly limited but include styrene. Furthermore, the method for producing the biomass monomer is not particularly limited and includes, for example, biological and / or chemical and / or physical transformations of plants and animals. Typical biological transformations include fermentation by microorganisms, while chemical and / or physical transformations include those by catalysts, high heat, high pressure, electromagnetic waves, critical liquids, and combinations thereof.

[0111] The polymer synthesized from biomass monomer components (biomass polymer) is not particularly limited, and examples include polybutadiene rubber synthesized from biomass-derived butadiene, and aromatic vinyl / butadiene copolymers synthesized from biomass-derived butadiene and / or biomass-derived aromatic vinyl compounds. Examples of the aromatic vinyl / butadiene copolymer include styrene-butadiene rubber synthesized from biomass-derived butadiene and / or biomass-derived styrene.

[0112] Whether the raw materials for a polymer are biomass-derived can be determined by measuring pMC (percent Modern Carbon) according to ASTM D6866-10. pMC refers to the percentage of modern standard reference carbon. 14 Sample relative to C concentration 14 This is a ratio of C concentrations and is used as an indicator of the biomass ratio of a compound. The significance of this value is described below.

[0113] 1 mole of carbon atoms (6.02 × 10⁻¹⁰) 23 (Each) contains approximately 6.02 × 10¹⁶ atoms, which is about one trillionth of the amount of carbon atoms in a normal atom. 11 individual 14 C exists. 14The half-life of C is 5730 years. 14 C is decreasing regularly. Therefore, in fossil fuels such as coal, oil, and natural gas, which are thought to have been fixed after more than 226,000 years have passed since atmospheric carbon dioxide was taken in and fixed by plants, etc., C was initially included in these as well. 14 All elements of C have decayed. Therefore, in the 21st century, fossil fuels such as coal, oil, and natural gas are no longer viable. 14 It contains absolutely no element C. Therefore, chemical substances produced using these fossil fuels as raw materials also contain C. 14 It contains absolutely no element C.

[0114] on the other hand, 14 C is continuously produced when cosmic rays undergo nuclear reactions in the atmosphere. Therefore, 14 In the Earth's atmospheric environment, carbon (C) is produced in a state where its decrease due to radioactive decay and its production through nuclear reactions are in equilibrium. 14 The amount of C is constant. Therefore, the amount of biomass resource-derived substances currently circulating in the environment 14 As mentioned above, the carbon concentration is approximately 1 × 10¹⁶ of the total carbon atoms. -12 These values ​​are approximately in mole percent. Therefore, the difference between these values ​​can be used to calculate the biomass ratio in a given compound.

[0115] this 14 C is typically measured as follows: Using accelerator mass spectrometry based on a tandem accelerator, 13 C concentration ( 13 C / 12 C), 14 C concentration ( 14 C / 12 Perform measurement C). In the measurement, 14 As a modern standard reference for the concentration of C, the amount of cyclic carbon in nature as of 1950 14The C concentration will be used. The specific standard material will be the oxalic acid standard provided by NIST (National Institute of Standards and Technology). The specific radioactivity of carbon in this oxalic acid (per gram of carbon) will be used. 14 The radioactivity intensity of C is separated by carbon isotope, 13 The standard value is obtained by correcting C to a constant value and applying decay correction from 1950 AD to the measurement date. 14 This value is used as the C concentration value (100%). The ratio of this value to the value of the sample actually measured is the pMC value.

[0116] Therefore, if rubber is made from 100% biomass-derived materials, although there are regional differences, under normal conditions it will often not reach 100, and will show a value of approximately 110 pMC. On the other hand, regarding chemical substances derived from fossil fuels such as petroleum, 14 When the C concentration is measured, it will show a value of approximately 0 pMC (for example, 0.3 pMC). This value corresponds to the aforementioned biomass ratio of 0%.

[0117] For the reasons stated above, using materials such as rubber with a high pMC value, that is, materials such as rubber with a high biomass ratio, in rubber compositions is preferable from an environmental protection standpoint.

[0118] (Filler) The rubber composition preferably contains a filler, and preferably the filler contains carbon black. The carbon black may also contain recycled carbon black (rCB). The filler may also contain other fillers besides carbon black, such as silica, aluminum hydroxide, calcium carbonate, alumina, clay, talc, and other fillers that have been commonly used in the tire industry. The filler may consist only of carbon black, or it may contain carbon black and silica.

[0119] Carbon Black The carbon black used is not particularly limited and includes N134, N110, N220, N234, N219, N339, N330, N326, N351, N550, N762, etc. The raw materials for carbon black may be biomass materials such as lignin and vegetable oil, from the perspective of life cycle assessment. The manufacturing method of carbon black may be by combustion such as the furnace process, by hydrothermal carbonization (HTC), or by thermal decomposition of methane such as the thermal black process. Commercially available products include those from Asahi Carbon Co., Ltd., Cabot Japan Co., Ltd., Tokai Carbon Co., Ltd., Mitsubishi Chemical Corporation, Lion Corporation, Nippon Steel Carbon Co., Ltd., and Columbia Chemical Corporation. Carbon black may be used alone or in combination of two or more types.

[0120] The nitrogen adsorption specific surface area (N2SA) of carbon black is 55 m², considering air permeability resistance and durability. 2 It is preferable that the amount be less than / g, and more preferably 50m 2 Less than / g, more preferably 45m 2 It is less than / g. Carbon black with a low N2SA is generally called large-particle carbon black. There is no particular lower limit to the N2SA of carbon black, but for example, 20m 2 The value is greater than / g. The N2SA of carbon black is measured by the method described above.

[0121] The carbon rack content is preferably more than 20 parts by mass, more preferably more than 30 parts by mass, even more preferably more than 50 parts by mass, and even more preferably more than 60 parts by mass, per 100 parts by mass of rubber component, from the viewpoint of reinforcing properties. Furthermore, the content is preferably less than 110 parts by mass, more preferably less than 100 parts by mass, even more preferably less than 90 parts by mass, and even more preferably less than 80 parts by mass.

[0122] Recycled carbon black In this specification, "recycled carbon black" refers to carbon black obtained by crushing used tires and other products containing carbon black, and calcining the crushed material, wherein, according to the thermogravimetric method compliant with JIS K 6226-2:2003, when oxidative combustion occurs by heating in air, the proportion of the mass of ash (ash content), which is the component that does not burn, is 13% by mass or more. In other words, the proportion of the mass (carbon content) lost due to the aforementioned oxidative combustion of recycled carbon black is 87% by mass or less. Recycled carbon black may also be represented as rCB.

[0123] Recycled carbon black can be obtained from the pyrolysis process of used pneumatic tires. For example, European Patent Application Publication No. 3427975, referring to "Rubber Chemistry and Technology," Vol. 85, No. 3, pp. 408-449 (2012), particularly pp. 438, 440, and 442, states that it can be obtained by the pyrolysis of organic materials at 550-800°C in the absence of oxygen, or by vacuum pyrolysis at relatively low temperatures (

[0027] ). Carbon black obtained from such pyrolysis processes usually lacks functional groups on its surface, as referred to in

[0004] of Japanese Patent Publication No. 6856781 (Comparison of Surface Morphology and Chemistry of Pyrolysis Carbon Black and Commercial Carbon Black, Powder Technology 160 (2005) 190-193). Therefore, recycled carbon black is considered to have low surface reactivity and thus reduced physical bonding strength in rubber compositions.

[0124] Recycled carbon black may lack functional groups on its surface, or it may be treated to contain functional groups on its surface. Treatment to contain functional groups on the surface of recycled carbon black can be carried out by conventional methods. For example, in European Patent Application Publication No. 3173251, carbon black obtained from a thermal decomposition process is treated with potassium permanganate under acidic conditions to obtain carbon black containing hydroxyl and / or carboxyl groups on its surface. In addition, in Japanese Patent Publication No. 6856781, carbon black obtained from a thermal decomposition process is treated with an amino acid compound containing at least one thiol group or disulfide group to obtain carbon black with an activated surface. The recycled carbon black according to this embodiment also includes carbon black treated to contain functional groups on its surface. Recycled carbon black may be used alone or in combination of two or more types.

[0125] Recycled carbon black can be purchased from companies such as Strable Green Carbon and LD Carbon.

[0126] Silica The silica used is not particularly limited, and common silica used in the tire industry can be used, such as silica prepared by the dry method (anhydrous silica) or silica prepared by the wet method (hydrated silica). The raw material for silica is not particularly limited, and may be a mineral-derived raw material such as quartz, or a biological-derived raw material such as rice husks (for example, silica made from biomass materials such as rice husks), or silica recycled from products containing silica may be used. Silica may be used alone or in combination of two or more types.

[0127] The silica recycled from silica-containing products can be, for example, silica recovered from products containing silica such as semiconductors and other electronic components, tires, desiccants, and diatomaceous earth and other filter materials. The recovery method is not particularly limited and can include thermal decomposition and decomposition by electromagnetic waves. Among these, silica recovered from semiconductors and other electronic components or tires is preferred.

[0128] When silica crystallizes, it becomes insoluble in water, and its component, silicic acid, cannot be utilized. By controlling the combustion temperature and combustion time, the crystallization of silica in rice husk ash can be suppressed (see Japanese Patent Publication No. 2009-2594, Akita Prefectural University Web Journal B / 2019, vol.6, pp.216-222, etc.).

[0129] Amorphous silica extracted from rice husks can be commercially available from companies such as Wilmar.

[0130] Silica derived from biomass materials can be obtained, for example, by extracting silicates from rice husk ash obtained by burning rice husks using a sodium hydroxide solution, and then using these silicates to react with sulfuric acid in the same way as conventional wet silica, the precipitate of silicon dioxide is filtered, washed with water, dried, and pulverized.

[0131] The silica recycled from silica-containing products can be, for example, silica recovered from products containing silica such as semiconductors and other electronic components, tires, desiccants, and diatomaceous earth and other filter materials. The recovery method is not particularly limited and can include thermal decomposition and decomposition by electromagnetic waves. Among these, silica recovered from semiconductors and other electronic components or tires is preferred.

[0132] ≪Silane coupling agents≫ When silica is used, it is preferable to further include a silane coupling agent. The silane coupling agent is not particularly limited and includes, for example, bis(3-triethoxysilylpropyl)tetrasulfide, bis(2-triethoxysilylethyl)tetrasulfide, bis(4-triethoxysilylbutyl)tetrasulfide, bis(3-trimethoxysilylpropyl)tetrasulfide, bis(2-trimethoxysilylethyl)tetrasulfide, bis(2-triethoxysilylethyl) trisulfide, bis(4-trimethoxysilylbutyl) trisulfide, bis(3-triethoxysilylpropyl) disulfide, bis(2-triethoxysilylethyl) disulfide, bis Examples of silane coupling agents include sulfide compounds such as (4-triethoxysilylbutyl) disulfide, bis(3-trimethoxysilylpropyl) disulfide, bis(2-trimethoxysilylethyl) disulfide, bis(4-trimethoxysilylbutyl) disulfide, 3-trimethoxysilylpropyl-N,N-dimethylthiocarbamoyl tetrasulfide, 2-triethoxysilylethyl-N,N-dimethylthiocarbamoyl tetrasulfide, and 3-triethoxysilylpropyl methacrylate monosulfide, as well as 3-mercaptopropyltrimethoxysilane and 2-mercaptoethyltriethoxysilane. Silane coupling agents may be used alone or in combination of two or more.

[0133] (Other combination drugs) In addition to rubber components and fillers, the rubber composition may appropriately contain compounding agents commonly used in the tire industry, such as plasticizers, processing aids, vulcanized rubber particles, waxes, stearic acid, antioxidants, zinc oxide, vulcanizing agents, and vulcanization accelerators.

[0134] Plasticizers A plasticizer is a material that imparts plasticity to rubber components, and the concept includes both liquid and solid plasticizers at 25°C. Examples of plasticizers include resins, oils, liquid polymers, and ester-based plasticizers. These plasticizers may be derived from petroleum, biomass, or naphtha recycled from rubber or non-rubber products. Low molecular weight hydrocarbon components obtained by thermal decomposition and extraction of used tires or products containing various components may also be used as plasticizers. Plasticizers may be used individually or in combination of two or more types.

[0135] ·resin The rubber composition preferably contains a resin among the other compounding agents mentioned above. The resin is not particularly limited, but resins commonly used in the tire industry can be used, such as C9 resins, C5 resins, C5C9 resins, dicyclopentadiene resins, aromatic vinyl resins, coumarone resins, indene resins, terpene resins, rosin resins, and phenolic resins. These resins may be used individually or in combination of two or more. Each resin may also be used individually or in combination of two or more.

[0136] ≪C9 series resin≫ A "C9 resin" refers to a resin obtained by polymerizing a C9 fraction, and may be a polymer obtained by polymerizing the C9 fraction alone, or a copolymer obtained by copolymerizing the C9 fraction with other components. For example, a resin obtained by copolymerizing dicyclopentadiene (DCPD) and a C9 fraction is called a DCPD / C9 resin. Furthermore, the C9 resin may be a hydrogenated or modified version of these resins. Examples of C9 fractions include petroleum fractions with 8 to 10 carbon atoms, such as vinyltoluene, alkylstyrene, coumarone, indene, methylindene, and dicyclopentadiene. As for C9 resins, commercially available products from companies such as BASF, Zeon Corporation, and ENEOS Corporation can be used.

[0137] ≪C5 series resin≫ "C5 resins" refer to resins obtained by polymerizing C5 fractions, and may be hydrogenated or modified versions of these resins. Examples of C5 fractions other than dicyclopentadiene include petroleum fractions with 4 to 5 carbon atoms, such as cyclopentadiene, isoprene, piperylene, 2-methyl-1-butene, 2-methyl-2-butene, and 1-pentene. As C5 resins, commercially available products from companies such as Structol, Nippon Zeon Co., Ltd., and ENEOS Corporation can be used.

[0138] ≪C5C9 resin≫ "C5C9 resin" refers to a resin obtained by copolymerizing the C5 fraction and the C9 fraction, and may be hydrogenated or modified. As C5C9 petroleum resin, commercially available products from companies such as Tosoh Corporation and LUHUA can be used.

[0139] <Dicyclopentadiene resins> A "dicyclopentadiene-based resin" refers to a resin in which cyclopentadiene (CPD) and / or dicyclopentadiene (DCPD) are the most abundant monomer components, and these may be hydrogenated or modified resins. Preferred dicyclopentadiene-based resins include polymers obtained by polymerizing only dicyclopentadiene as a monomer, and copolymers (DCPD / C9 resins) obtained by copolymerizing dicyclopentadiene with the C9 fraction. Commercially available dicyclopentadiene-based resins from companies such as ExxonMobil, ENEOS Corporation, Nippon Zeon Corporation, and Maruzen Petrochemical Co., Ltd. can be used.

[0140] Aromatic vinyl resin "Aromatic vinyl resin" refers to a resin in which aromatic vinyl compounds such as styrene, α-methylstyrene, vinyltoluene, and p-chlorostyrene are the most abundant monomer components, and these may be hydrogenated or modified. As aromatic vinyl resins, α-methylstyrene or a homopolymer of styrene or a copolymer of α-methylstyrene and styrene is preferred, and a copolymer of α-methylstyrene and styrene is more preferred, for reasons of being economical, easy to process, and having excellent heat generation properties. As aromatic vinyl resins, commercially available products from companies such as Kraton, Eastman Chemical Company, and Mitsui Chemicals, Inc. can be used.

[0141] Coumaron-based resin "Coumarone-based resin" refers to a resin containing coumarone as a monomer component, and may be hydrogenated or modified. Preferred coumarone-based resins include, for example, coumarone resin, which is a polymer with coumarone as the monomer component; coumarone-indene resin, which is a copolymer with coumarone and indene as monomer components; and coumarone-indene-styrene resin, which is a copolymer with coumarone, indene, and styrene as monomer components. As coumarone-based resins, commercially available products from companies such as Rutgers, Nippon Paint Chemical Co., Ltd., and Mitsui Chemicals, Inc. can be used.

[0142] Indene resin "Indene-based resin" refers to a resin containing indene as a monomer component, and may be hydrogenated or modified resins. Preferred indene-based resins include, for example, coumarone-indene resin, which is a copolymer of coumarone and indene as monomer components, and coumarone-indene-styrene resin, which is a copolymer of coumarone, indene, and styrene as monomer components. Commercially available indene-based resins from companies such as Rutgers, Nippon Paint Chemical Co., Ltd., and Mitsui Chemicals, Inc. can be used.

[0143] Terpene resins "Terpene resin" refers to a resin containing terpene compounds such as α-pinene, β-pinene, limonene, and dipentene as monomer components, and may be hydrogenated or modified. Preferred terpene resins include, for example, polyterpene resins, which are polymers in which one or more of the aforementioned terpene compounds are used as monomer components; aromatically modified terpene resins, which are copolymers in which the aforementioned terpene compounds and aromatic compounds are used as monomer components; and terpene phenol resins, which are copolymers in which the aforementioned terpene compounds and phenol compounds are used as monomer components. Examples of aromatic compounds that serve as monomer components in aromatically modified terpene resins include styrene, α-methylstyrene, vinyltoluene, and divinyltoluene. Examples of phenol compounds that serve as monomer components in terpene phenol resins include phenol, bisphenol A, cresol, and xylenol. As terpene resins, commercially available products from companies such as Yasuhara Chemical Co., Ltd., Arakawa Chemical Industries, Ltd., and Nippon Terpene Chemical Co., Ltd. can be used.

[0144] ≪Rosin-based resin≫ "Rosin-based resin" refers to a resin containing rosin acid compounds such as abietic acid, neoabietic acid, palastic acid, and isopimal acid, and may be hydrogenated or modified. Rosin-based resins are not particularly limited, but examples include natural resin rosin and rosin-modified resins obtained by hydrogenating, disproportionating, dimerizing, esterifying, etc. As rosin-based resins, commercially available products from companies such as Harima Chemical Industries, Ltd., Arakawa Chemical Industries, Ltd., and IREC Co., Ltd. can be used.

[0145] Phenolic resins "Phenol-based resins" refer to resins containing phenol compounds such as phenol and cresol as monomer components, and may also be hydrogenated or modified resins. Phenolic resins are not particularly limited, but examples include phenol-formaldehyde resins, alkylphenol-formaldehyde resins, alkylphenol-acetylene resins, oil-modified phenol-formaldehyde resins, and terpene-phenol resins. Phenolic resins that are commercially available from companies such as Sumitomo Bakelite Co., Ltd., DIC Corporation, and Asahi Organic Materials Co., Ltd. can be used.

[0146] ·oil Examples of oils include mineral oil, vegetable oil, and animal oil. Furthermore, from a life cycle assessment perspective, waste oil from rubber mixers and engines, or refined waste cooking oil from restaurants, may also be used. Oils may be used individually or in combination of two or more types.

[0147] In this specification, mineral oil refers to oil derived from mineral resources such as petroleum and natural gas. Examples of mineral oil include paraffinic oils (mineral oil), naphthenic oils, and aromatic oils. Specific examples of mineral oil include MES (Mild Extracted Solvate), DAE (Distillate Aromatic Extract), TDAE (Treated Distillate Aromatic Extract), TRAE (Treated Residual Aromatic Extract), and RAE (Residual Aromatic Extract). Furthermore, for environmental reasons, oils with a low content of polycyclic aromatic compounds (PCA) can be used. Examples of low-PCA oils include MES, TDAE, and heavy naphthenic oils. Mineral oil may be used alone or in combination of two or more types.

[0148] In this specification, vegetable oils include, for example, linseed oil, rapeseed oil, safflower oil, soybean oil, corn oil, cottonseed oil, rice oil, tall oil, sesame oil, perilla oil, castor oil, tung oil, pine oil, pine tar oil, sunflower oil, coconut oil, palm oil, palm kernel oil, olive oil, camellia oil, jojoba oil, macadamia nut oil, peanut oil, grapeseed oil, and wood wax. Furthermore, vegetable oils may also include refined oils (such as salad oil) obtained by refining the above oils, transesterified oils obtained by transesterifying the above oils, hydrogenated oils obtained by hydrogenating the above oils, thermally polymerized oils obtained by thermally polymerizing the above oils, oxidized polymerized oils obtained by oxidizing the above oils, and waste cooking oils recovered from use as edible oils. Note that vegetable oils may be liquid or solid at 25°C. Vegetable oils may be used individually or in combination of two or more types.

[0149] The vegetable oil according to this embodiment preferably contains acylglycerol, and more preferably contains triacylglycerol. In this specification, acylglycerol refers to a compound in which a hydroxyl group of glycerin and a fatty acid are ester-bonded. The acylglycerol is not particularly limited and may be 1-monoacylglycerol, 2-monoacylglycerol, 1,2-diacylglycerol, 1,3-diacylglycerol, or triacylglycerol. Furthermore, the acylglycerol may be a monomer, a dimer, or a polymer of three or more. Note that acylglycerols of two or more forms can be obtained by thermal polymerization, oxidative polymerization, etc. Also, the acylglycerol may be a liquid or a solid at 25°C.

[0150] The method for confirming whether the rubber composition contains the acylglycerol is not particularly limited, 1 This can be confirmed by 1H-NMR measurement. For example, a rubber composition containing triacylglycerol is immersed in deuterated chloroform at 25°C for 24 hours, and after removing the rubber composition, it is measured at room temperature. 1When 1H-NMR was measured and the tetramethylsilane (TMS) signal was set to 0.00 ppm, signals were observed around 5.26 ppm, 4.28 ppm, and 4.15 ppm. These signals are presumed to originate from hydrogen atoms bonded to carbon atoms adjacent to the oxygen atom of the ester group. In this paragraph, "around" refers to a range of ±0.10 ppm.

[0151] The aforementioned fatty acids are not particularly limited and may be unsaturated or saturated fatty acids. Examples of unsaturated fatty acids include monounsaturated fatty acids such as oleic acid, and polyunsaturated fatty acids such as linoleic acid and linolenic acid. Examples of saturated fatty acids include butyric acid and lauric acid.

[0152] In particular, it is desirable that the fatty acid contains fatty acids with few double bonds, i.e., saturated fatty acids or monounsaturated fatty acids, and oleic acid is preferred. As a vegetable oil containing such fatty acids, for example, a vegetable oil containing saturated fatty acids or monounsaturated fatty acids may be used, or a vegetable oil that has been modified by transesterification or other means may be used. Furthermore, in order to produce a vegetable oil containing such fatty acids, plants may be improved by breeding, genetic modification, genome editing, etc.

[0153] As for vegetable oils, commercially available products from companies such as Idemitsu Kosan Co., Ltd., Sankyo Yuka Kogyo Co., Ltd., ENEOS Corporation, Orisoy Co., Ltd., H&R Co., Ltd., Toyokuni Oil Co., Ltd., Fuji Kosan Co., Ltd., and Nisshin Oillio Group Ltd. can be used.

[0154] Examples of animal oils include fish oil, beef tallow, or oleyl alcohol which can be derived from them.

[0155] The oil content per 100 parts by mass of rubber component is preferably more than 5 parts by mass, more preferably more than 3 parts by mass, and even more preferably 8 parts by mass or more. Furthermore, the content is preferably less than 20 parts by mass, more preferably less than 15 parts by mass, and even more preferably 10 parts by mass or less. Note that the oil content includes the amount of oil contained in the rubber component as an oil spreading oil, as well as the amount of oil contained in other components such as sulfur.

[0156] • Liquid polymer A liquid polymer is a polymer that is liquid at 25°C, and examples include liquid diene polymers. Examples of liquid diene polymers include liquid styrene-butadiene copolymer (liquid SBR), liquid butadiene polymer (liquid BR), liquid isoprene polymer (liquid IR), and liquid styrene-isoprene copolymer (liquid SIR). The number average molecular weight (Mn) of the liquid diene polymer, measured in polystyrene terms by gel permeation chromatography (GPC), is preferably greater than 1000, more preferably greater than 3000, while the Mn is preferably less than 100,000, and more preferably less than 15,000. The Mn of the liquid polymer is the polystyrene equivalent value measured by gel permeation chromatography (GPC). Examples of liquid diene polymers that can be used include products from Sartomer Co., Ltd., Kuraray Co., Ltd., etc. Liquid polymers may be used alone or in combination of two or more types.

[0157] • Ester-based plasticizers Examples of ester-based plasticizers include dibutyl adipate (DBA), diisobutyl adipate (DIBA), dioctyl adipate (DOA), di-2-ethylhexyl azelaate (DOZ), dibutyl sebacate (DBS), diisononyl adipate (DINA), diethyl phthalate (DEP), dioctyl phthalate (DOP), diundecyl phthalate (DUP), dibutyl phthalate (DBP), dioctyl sebacate (DOS), tributyl phosphate (TBP), trioctyl phosphate (TOP), triethyl phosphate (TEP), trimethyl phosphate (TMP), thymidine triphosphate (TTP), tricresyl phosphate (TCP), and trixylenyl phosphate (TXP). Ester-based plasticizers may be used individually or in combination of two or more.

[0158] Processing aids Examples of processing aids include fatty acid metal salts, fatty acid amides, amide esters, silica surfactants, mixtures of fatty acid metal salts and amide esters, and mixtures of fatty acid metal salts and fatty acid amides. For example, commercially available processing aids from companies such as Schill+Seilacher and Performance Additives can be used. Processing aids may be used individually or in combination of two or more.

[0159] When processing aids are included, the content per 100 parts by mass of rubber components is preferably more than 0.5 parts by mass, more preferably more than 1 part by mass, and even more preferably more than 1.5 parts by mass, from the viewpoint of exhibiting an effect of improving processability. Furthermore, from the viewpoint of abrasion resistance and fracture strength, it is preferably less than 10 parts by mass, more preferably less than 8.0 parts by mass, and even more preferably less than 5.0 parts by mass.

[0160] Vulcanized rubber particles Vulcanized rubber particles are particles made of vulcanized rubber, and specifically, rubber powder as specified in JIS K 6316:2017 can be used. From the viewpoint of environmental considerations and cost, recycled rubber powder produced from crushed waste tires is preferred. The vulcanized rubber particles are not particularly limited and may be unmodified or modified. Commercially available vulcanized rubber products include those from Lehigh, Muraoka Rubber Industries, and others. One type of vulcanized rubber particle may be used alone, or two or more types may be used in combination.

[0161] ≪Wax≫ The wax is not particularly limited, and any wax commonly used in the tire industry can be suitably used, such as mineral waxes and plant-derived waxes. Mineral waxes refer to waxes derived from mineral resources such as oil and natural gas. Plant-derived waxes refer to waxes derived from natural resources such as plants. Among these, mineral waxes are preferred. Examples of plant-derived waxes include rice wax, carnauba wax, and candelilla wax. Examples of mineral waxes include paraffin wax, microcrystalline wax, and selected special waxes thereof, with paraffin wax being preferred. The wax according to this embodiment does not contain stearic acid. The wax can be commercially available from companies such as Ouchi Shinko Chemical Industry Co., Ltd., Nippon Seiro Co., Ltd., and Paramelt Co., Ltd. The wax may be used alone or in combination of two or more types.

[0162] When wax is included, the content per 100 parts by mass of rubber component is preferably more than 0.3 parts by mass, more preferably more than 0.7 parts by mass, and still more preferably more than 1.0 part by mass. On the other hand, the content is preferably less than 4.0 parts by mass, more preferably less than 3.0 parts by mass, and still more preferably less than 2.5 parts by mass.

[0163] ≪Stearic Acid≫ When stearic acid is included, its content per 100 parts by mass of the rubber component is preferably more than 0.5 parts by mass, more preferably more than 0.7 parts by mass, and even more preferably 1.0 part by mass or more, from the viewpoint of processability. On the other hand, from the viewpoint of vulcanization rate, the content is preferably less than 10 parts by mass, more preferably less than 7 parts by mass, and even more preferably less than 5 parts by mass.

[0164] Anti-aging agent While not particularly limited, the following are examples of anti-aging agents: naphthylamine-based anti-aging agents such as phenyl-α-naphthylamine; diphenylamine-based anti-aging agents such as octylated diphenylamine and 4,4'-bis(α,α'-dimethylbenzyl)diphenylamine; N-isopropyl-N'-phenyl-p-phenylenediamine, N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine (6PPD), N,N'-bis(1,4-dimethylpentyl)-p-phenylenediamine (77PD), N,N'-diphenyl-p-phenylenediamine (DPPD), and N,N'-ditril-p-phenyl Examples include p-phenylenediamine-based antioxidants such as diamine (DTPD), N-isopropyl-N'-phenyl-p-phenylenediamine (IPPD), and N,N'-di-2-naphthyl-p-phenylenediamine (DNPD); quinoline-based antioxidants such as polymers of 2,2,4-trimethyl-1,2-dihydroquinoline; monophenol-based antioxidants such as 2,6-di-t-butyl-4-methylphenol and styrenated phenol; and bis-, tris-, and polyphenol-based antioxidants such as tetrakis-[methylene-3-(3',5'-di-t-butyl-4'-hydroxyphenyl)propionate]methane. Among these, p-phenylenediamine-based antioxidants and quinoline-based antioxidants are preferred, and polymers of N-(1,3-dimethylbutyl)-N'-phenyl-p-phenylenediamine and 2,2,4-trimethyl-1,2-dihydroquinoline are more preferred. Commercially available products include those from Seiko Chemical Co., Ltd., Sumitomo Chemical Co., Ltd., Ouchi Shinko Chemical Co., Ltd., Flexis, and others. The antioxidant may be used alone or in combination of two or more.

[0165] When an anti-aging agent is included, its content per 100 parts by mass of rubber component is preferably more than 0.5 parts by mass, more preferably more than 0.8 parts by mass, and even more preferably 1.0 part by mass or more. On the other hand, the content is preferably less than 7.0 parts by mass, more preferably less than 5.0 parts by mass, and even more preferably less than 3.0 parts by mass.

[0166] ≪Zinc Oxide≫ When zinc oxide is included, its content per 100 parts by mass of rubber component is preferably more than 0.5 parts by mass, more preferably more than 0.7 parts by mass, and even more preferably 1 part by mass or more, from the viewpoint of processability. On the other hand, from the viewpoint of wear resistance, the content is preferably less than 10 parts by mass, more preferably less than 7 parts by mass, and even more preferably less than 5 parts by mass.

[0167] ≪Sulfurizing agent≫ The vulcanizing agent is not particularly limited, and known vulcanizing agents can be used, such as organic peroxides, sulfur-based vulcanizing agents, resin vulcanizing agents, and metal oxides such as magnesium oxide. Among these, sulfur-based vulcanizing agents are preferred. As sulfur-based vulcanizing agents, for example, sulfur, sulfur donors such as morpholine disulfide can be used. Among these, the use of sulfur is preferred. The vulcanizing agent can be used one or in combination of two or more types.

[0168] Examples of sulfur include powdered sulfur, precipitated sulfur, colloidal sulfur, surface-treated sulfur (oil-treated sulfur, special sulfur treated with dispersants, masterbatch-type sulfur, etc.), and insoluble sulfur (oil-treated insoluble sulfur, etc.), all of which can be suitably used. Among these, powdered sulfur is preferred. Sulfur can be used from, for example, those manufactured and sold by Tsurumi Chemical Industries, Ltd., Karuizawa Sulfur Co., Ltd., Shikoku Chemicals, Ltd., Flexis Co., Ltd., Nippon Dry Distillation Industry Co., Ltd., Hosoi Chemical Industry Co., Ltd., etc.

[0169] Known organic crosslinking agents can also be used as vulcanizing agents. The organic crosslinking agents are not particularly limited as long as they can form crosslinking chains other than polysulfide bonds, but examples include alkylphenol-sulfur chloride condensates, 1,6-hexamethylene-dithiosulfate sodium dihydrate, 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane, and dicumyl peroxide, with 1,6-bis(N,N'-dibenzylthiocarbamoyldithio)hexane being preferred. These organic crosslinking agents can be commercially available from companies such as Taoka Chemical Industries, Ltd., Lanxess Corporation, and Flexis.

[0170] When a vulcanizing agent is included, its content per 100 parts by mass of rubber component is preferably more than 0.5 parts by mass, more preferably more than 1.0 part by mass, and still more preferably more than 1.5 parts by mass. On the other hand, the content is preferably less than 6.0 parts by mass, more preferably less than 4.0 parts by mass, and still more preferably less than 3.0 parts by mass. When the vulcanizing agent content is within the above range, an appropriate reinforcing effect tends to be obtained. Note that if the vulcanizing agent contains components other than sulfur, such as oil-treated sulfur, the vulcanizing agent content refers to the content of the sulfur component itself.

[0171] <<Vulcanization accelerator>> The vulcanization accelerator is not particularly limited, and known vulcanization accelerators can be used, such as sulfenamide, thiazole, guanidine, thiram, thiourea, dithiocarbamate, aldehyde-amine or aldehyde-ammonia, imidazoline, or xanthate vulcanization accelerators. Among these, sulfenamide, thiazole, guanidine, and thiram are preferred, sulfenamide and thiazole are more preferred, and thiazole is even more preferred. For example, vulcanization accelerators manufactured and sold by Ouchi Shinko Chemical Industry Co., Ltd., Sanshin Chemical Industry Co., Ltd., etc., can be used. One or more vulcanization accelerators can be used in combination.

[0172] Examples of sulfenamide-based vulcanization accelerators include N-tert-butyl-2-benzothiazolyl sulfenamide (TBBS), N-cyclohexyl-2-benzothiazolyl sulfenamide (CBS), and N,N-dicyclohexyl-2-benzothiazolyl sulfenamide (DZ). Examples of thiazole-based vulcanization accelerators include 2-mercaptobenzothiazole (MBT) or its salts, di-2-benzothiazolyl disulfide (MBTS), 2-(2,4-dinitrophenyl)mercaptobenzothiazole, and 2-(2,6-diethyl-4-morpholinothio)benzothiazole. Examples of guanidine-based vulcanization accelerators include 1,3-diphenylguanidine (DPG), diortotolylguanidine, and orthotolylbiguanidine. Examples of thiram-based vulcanization accelerators include tetramethylthiram monosulfide, tetramethylthiram disulfide, and tetrabenzylthiram disulfide (TBzTD).

[0173] The content of the vulcanization accelerator per 100 parts by mass of the rubber component is preferably more than 0.3 parts by mass, more preferably more than 0.5 parts by mass, and even more preferably more than 1.0 part by mass. On the other hand, the content is preferably less than 4.0 parts by mass, more preferably less than 3.0 parts by mass, and even more preferably less than 2.0 parts by mass. When the content of the vulcanization accelerator is within the above range, fracture strength and elongation tend to be ensured.

[0174] In this specification, various materials containing carbon atoms (e.g., rubber, oil, resin, vulcanization accelerator, antioxidant, surfactant, etc.) may be derived from atmospheric carbon dioxide. As a method for obtaining the formulations according to this embodiment from carbon dioxide, carbon dioxide may be directly converted, or methane obtained through a methanation process in which methane is synthesized from carbon dioxide may be converted.

[0175] <Manufacturing> The rubber composition according to this embodiment can be manufactured by known methods. For example, it can be manufactured by kneading each of the above components using a rubber kneading device such as an open roll or a closed kneader (Banbury mixer, kneader, etc.).

[0176] The mixing process includes, for example, a base mixing process in which compounding agents and additives other than the vulcanizing agent and vulcanization accelerator are mixed, and a final mixing (F mixing) process in which the vulcanizing agent and vulcanization accelerator are added to the mixture obtained in the base mixing process and mixed. Furthermore, the base mixing process can be divided into multiple processes as desired. When dividing the base mixing process, the method may be (1) a method in which some of the compounding agents and additives are mixed in advance to form a masterbatch, and then the remaining compounding agents and additives are added to the resulting masterbatch and mixed, or (2) a method in which all the compounding agents and additives to be mixed in the base mixing process are mixed at once, and then the mixture is remilled one or more times. In the method of (1) above, the number of masterbatches is not limited and may be two or more. Also, when the number of masterbatches is two or more, all the compounding agents and additives used in the base mixing process may be allocated to one of the masterbatches.

[0177] While there are no particular limitations on the mixing conditions, one example is to mix the base mixture at a discharge temperature of 150-170°C for 3-10 minutes, and then mix the final mixture at 70-110°C for 1-5 minutes.

[0178] The tire according to this embodiment can be manufactured by a conventional method using the unvulcanized rubber composition obtained above. That is, first, the unvulcanized rubber composition is extruded to match the shape of the insulation to obtain unvulcanized insulation. The unvulcanized insulation thus obtained is bonded together with other tire components on a tire molding machine by a conventional method to form an unvulcanized tire. At this time, the structure of the insulation is made to be predetermined. The tire according to this embodiment can be manufactured by heating and pressurizing the unvulcanized tire thus obtained in a vulcanizing machine. The vulcanization conditions are not particularly limited, and for example, a method of vulcanizing at 150 to 200°C for 10 to 40 minutes can be cited.

[0179] <Application> The tire according to this embodiment can be used for any application, including passenger car tires, large passenger car tires, large SUV tires, racing tires, motorcycle tires, heavy-duty tires, and run-flat tires. A passenger car tire refers to a tire intended for use on a four-wheeled vehicle with a maximum load capacity of less than 1400 kg. A heavy-duty tire refers to a tire with a maximum load capacity of 1400 kg or more. Furthermore, in this specification, the tire can be used as an all-season tire, a summer tire, or a winter tire such as a studless tire. [Examples]

[0180] The following examples (case studies) are shown as preferred for implementation, but the scope of the present invention is not limited to these examples. In accordance with each table, we examined the insulation and tire structure obtained using the various chemicals shown below, and the results calculated based on the evaluation method below are shown at the bottom of Tables 1, 2-1, and 2-2.

[0181] <Various chemicals> The various chemicals used in the examples and comparative examples are summarized below. IR-type rubber: TSR20 (natural rubber) BR: UBEPOL BR150B manufactured by UBE Corporation (unmodified BR, cis content: 96 mol%, Mw: 440,000) SBR: SBR1502 manufactured by JSR Corporation (unmodified E-SBR, styrene content: 23.5% by mass, vinyl content: 18 mol%, Mw: 420,000) Butyl rubber: Exxon Mobil's EXXON BROMOBUTYL 2222 (brominated butyl rubber: Br-IIR) Carbon Black 1: Dia Black (registered trademark) E (FEF, N550, N2SA) manufactured by Mitsubishi Chemical Corporation: 40m 2 / g, average primary particle diameter: 81nm) Carbon Black 2: Recycled carbon black obtained by crushing and calcining waste tires (ash content: 17% by mass) Oil: VivaTec500 (TDAE oil) manufactured by H&R Co., Ltd. Stearic acid: Beads of stearic acid manufactured by NOF Corporation Zinc oxide: Zinc oxide manufactured by Mitsui Mining & Smelting Co., Ltd. Sulfur: HK-200-5 (powdered sulfur, oil content: 5% by mass) manufactured by Hosoi Chemical Industry Co., Ltd. Vulcanization accelerator: Noxellar CZ (N-cyclohexyl-2-benzothiazolyl sulfenamide (CBS)) manufactured by Ouchi Shinko Chemical Industry Co., Ltd.

[0182] <Examples and Comparative Examples> According to the formulations shown in Tables 1, 2-1, and 2-2, the chemicals other than sulfur and vulcanization accelerator are mixed in a 1.7 L Banbury mixer for 5 minutes until the discharge temperature reaches 160°C to obtain a mixture. Next, sulfur and vulcanization accelerator are added to the mixture and mixed in a twin-screw open roll mixer for 4 minutes until the temperature reaches 105°C to obtain an unvulcanized rubber composition for insulation.

[0183] Using the obtained unvulcanized rubber composition, it is extruded to match the shape of the insulation using an extruder equipped with a die of a predetermined shape, and bonded together with other tire components while adjusting to achieve the predetermined tire structure shown in Tables 1, 2-1, and 2-2 to produce an unvulcanized tire. Each test tire (tire size: 205 / 55R16, 91V) is then manufactured by press vulcanization at 150°C for 35 minutes.

[0184] The tire structure of each test tire is described below. In Table 1, a "+" in the "Insulation Hollow Structure" column indicates that the insulation is not continuous in the tire width direction and is not located on the tire equatorial plane. On the other hand, a "-" in the same column indicates that the insulation is continuous in the tire width direction. Furthermore, a "+" in the "Position of Insulation Ends Satisfies Claim 6" column indicates that the end of the insulation closest to the tire equatorial plane is located outside the width of half the tread contact width, centered on the tire equator, and inside the tread contact edge. On the other hand, a "-" in the same column indicates that none of the insulation ends are located in the aforementioned positions.

[0185] <Measurement of 70°C E* and 70°C tanδ> Each vulcanized rubber test piece, cut from the insulation rubber of each test tire to a length of 20 mm, width of 4 mm, and thickness of 1 mm, with the tire circumference being the longer side and the tire radius being the thickness direction, will have its loss tangent tanδ and complex modulus E* measured using a dynamic viscoelasticity measuring device (GABO's Iplexer series) under the conditions of a temperature of 70°C, a frequency of 10 Hz, an initial strain of 5%, a dynamic strain of ±1%, and the extension mode.

[0186] <Tensile Test> For each test tire, a dumbbell-shaped No. 7 test specimen, cut to a thickness of 1 mm from the insulation rubber so that the tire circumference is the tensile direction and the tire radius is the thickness direction, is subjected to a tensile test in accordance with JIS K 6251:2017 at a 23°C atmosphere and a tensile speed of 3.3 mm / second, and the modulus (MPa) at 100% elongation is measured.

[0187] <Fuel efficiency> For each test tire, the rolling resistance coefficient (RRC) was measured in accordance with JIS D 4234:2009 (ISO 28580), and the reciprocal value of the rolling resistance coefficient was expressed as an index with the control tire (Comparative Example 10) set to 100. A larger index indicates lower rolling resistance and superior fuel efficiency. (Fuel efficiency index) = (Rolling resistance coefficient of Example 1) / (Rolling resistance coefficient of each test tire) × 100

[0188] <Durability after thermal degradation> Each test tire is left to degrade by heat in a controlled chamber at 70°C for 336 hours. After thermal degradation, each test tire is mounted on a standard rim and inflated to an internal pressure of 250 kPa. This tire is mounted on a drum-type running test machine, and a load greater than the standard load is applied. Under conditions of a slip angle of 1.5° and a speed of 100 km / h, the tire is run without replenishing air pressure, and the distance traveled until failure occurs at the edge of the belt layer is measured. This distance is expressed as an index, with the control tire (Comparative Example 3) set to 100. A higher value indicates higher durability.

[0189] The overall performance index is expressed as the sum of the fuel efficiency performance index and the durability performance index after thermal degradation.

[0190] [Table 1]

[0191] [Table 2-1]

[0192] [Table 2-2]

[0193] <Embodiment> Examples of embodiments of the present invention are shown below. [1] A tire comprising a tread, an inner liner, a carcass ply, and insulation between the inner liner and the carcass ply, The insulation is a hollow structure that is not continuous in the tire width direction and is not located on the tire equatorial plane. The insulation is composed of a rubber composition containing a rubber component including butyl rubber, A tire in which the thickness t of the inner liner is 1.0 mm or less, preferably 0.9 mm or less. [2] The tire according to [1] above, wherein the rubber component constituting the insulation further contains 50% by mass or more, preferably 55% by mass or more, of isoprene-based rubber. [3] The tire according to [1] or [2] above, wherein the rubber component constituting the insulation further contains 15% by mass or more, preferably 15% by mass or more and 20% by mass or less, of styrene-butadiene rubber. [4] The maximum load capacity of the tire is W L (kg), if the tire weight is G (kg), Golden Week L A tire according to any of the above [1] to [3], wherein the ratio is 0.0140 or less, preferably 0.0120 or more and 0.0140 or less. [5] The tire according to any one of [1] to [4] above, wherein the rubber composition constituting the insulation contains recycled carbon black. [6] The tire according to any of [1] to [5] above, wherein the end of the insulation closest to the tire equator is located outside a width of half the tread contact width centered on the tire equator, and inside the tread contact edge. [7] When the tanδ at 70°C of the rubber composition constituting the insulation is defined as 70°C tanδ, A tire according to any of the above [1] to [6], wherein the product of 70°C tanδ and t (mm) (70°C tanδ × t) is less than 0.15, preferably less than 0.14. [8] When M is the 100% modulus of the rubber composition constituting the insulation at a 23°C atmosphere, 70°CE* is the complex modulus of the rubber composition constituting the insulation at 70°C, and 70°Ctanδ is the tanδ of the rubber composition constituting the insulation at 70°C, A tire according to any of the above [1] to [7], wherein the product of M and the above 70°CE* / 70°Ctanδ (M × 70°CE* / 70°Ctanδ) is greater than 70. [9] The tread has one or more circumferential grooves, The tire according to [8] above, wherein, when the groove depth of the deepest part of the circumferential groove is H, the product of H and 70°C tanδ (H × 70°C tanδ) is less than 1.2, preferably greater than 0.6 and less than 1.1.

[10] The tire according to any one of [1] to [9] above, wherein the rubber component constituting the insulation contains butyl rubber in an amount greater than 1.0% by mass and less than 20% by mass, preferably 5% by mass or more and less than 20% by mass, and more preferably 8% by mass or more and less than 20% by mass. [Explanation of Symbols]

[0194] 1 tread 2 Inner Liner 3 Carcass ply 4 Insulation 5 Belt Layer 6-band layer 6a Full Band 6b Edge Band 7 Sidewall 10 Tread surface 11 Circumferential groove CL Tire Equator TW Tread contact width Te tread contact point t Thickness of the inner liner

Claims

1. A tire comprising a tread, an inner liner, a carcass ply, and insulation between the inner liner and the carcass ply, The insulation is a hollow structure that is not continuous in the tire width direction and is not located on the tire equatorial plane. The insulation is composed of a rubber composition containing a rubber component including butyl rubber, A tire in which the thickness t of the inner liner is 1.0 mm or less.

2. The tire according to claim 1, wherein the rubber component constituting the insulation further contains 50% by mass or more of isoprene-based rubber.

3. The tire according to claim 1 or 2, wherein the rubber component constituting the insulation further contains 15% by mass or more of styrene-butadiene rubber.

4. The maximum load capacity of the aforementioned tire is W L (kg), if the tire weight is G (kg), Golden Week L The tire according to claim 1 or 2, wherein the coefficient is 0.0140 or less.

5. The tire according to claim 1 or 2, wherein the rubber composition constituting the insulation contains recycled carbon black.

6. The tire according to claim 1 or 2, wherein the end of the insulation closest to the tire equator is located outside the width of half the tread contact width, centered on the tire equator, and inside the tread contact edge.

7. When the tanδ at 70°C of the rubber composition constituting the insulation is defined as 70°C tanδ, The tire according to claim 1 or 2, wherein the product of 70°C tanδ and t (mm) (70°C tanδ × t) is less than 0.

15.

8. When M is the 100% modulus of the rubber composition constituting the insulation at a 23°C atmosphere, E* is the complex modulus of the rubber composition constituting the insulation at 70°C, and tanδ of the rubber composition constituting the insulation at 70°C is tanδ, The tire according to claim 1 or 2, wherein the product of M and the 70°C E* / 70°C tanδ (M × 70°C E* / 70°C tanδ) is greater than 70.

9. The tread has one or more circumferential grooves, The tire according to claim 8, wherein, when the groove depth of the deepest part of the circumferential groove is H, the product of H and the 70°C tanδ (H × 70°C tanδ) is less than 1.

2.

10. The tire according to claim 1 or 2, wherein the rubber component constituting the insulation contains more than 1.0% by mass and less than 20% by mass of butyl rubber.

Citation Information

Patent Citations

  • Pneumatic tire

    JP2018165304A