Method for producing fluorescent powder
By adding a solid compound to hydrofluoric acid with potassium ions and using inert particles to crush the product, the method produces phosphor powder with suppressed aggregation, improving dispersibility and color uniformity in liquids.
Patent Information
- Application Number
- JP2025078871
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Phosphorescent powder containing fluoride phosphors aggregates in liquids, leading to larger particle sizes that settle quickly, affecting color uniformity and dispersibility.
A method involving the addition of a solid compound containing element M and a solid manganese compound to hydrofluoric acid with potassium ions, followed by stirring and crushing with inert particles to produce phosphor powder with suppressed aggregation.
The method enhances the dispersibility and uniformity of the phosphor powder in liquids, reducing sedimentation and maintaining color consistency, with improved moisture resistance and productivity.
Smart Images

Figure 2026182553000003 
Figure 2026182553000001 
Figure 2026182553000002
Abstract
Description
[Technical Field]
[0001] This disclosure relates to a method for producing phosphor powder. [Background technology]
[0002] Phosphorescent particles with reduced particle size are used as color conversion materials in micro-LED displays and other applications that achieve high brightness and high definition light emission. Patent Document 1 describes CASN and SCASN phosphorescent particles obtained by grinding and decanting phosphorescent powder under appropriate conditions to reduce particle size while suppressing particle aggregation. Patent Document 2 describes red-emitting phosphorescent particles with reduced particle size obtained by liquid-liquid synthesis in the presence of inert particles. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] International Publication No. 2022 / 118600 [Patent Document 2] Special Publication No. 2019-501990 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] Phosphorescent powder containing fluoride phosphors may aggregate in a liquid such as a resin used as a encapsulant, forming clumps of phosphor particles. These aggregated phosphor particle clumps have a larger particle size, which, according to Stokes' law, increases their sedimentation velocity and makes them more likely to settle in the liquid. When these phosphorescent powder clumps settle in a liquid, there is a concern that the uniformity of the color of the phosphorescent powder in the liquid will decrease. On the other hand, if the aggregation of phosphorescent particles can be suppressed, the dispersibility of the phosphorescent powder can be improved, thereby enhancing the uniformity of its color. This disclosure provides a method for producing phosphorescent powder in which the aggregation of phosphorescent particles is suppressed. [Means for solving the problem]
[0005] One aspect of the present disclosure provides the following method for producing a phosphor powder of [1].
[0006] [1] General formula (1): A₂M (1-n) F₆:Mn 4+ n A method for producing a phosphor powder containing phosphor particles represented by: A method for producing a phosphor powder, comprising a step of adding a solid compound containing at least element M as a constituent element and a solid manganese compound to hydrofluoric acid containing potassium ions, and stirring and crushing the obtained product together with inert particles to obtain the phosphor powder. (In general formula (1), element A is one or more alkali metal elements containing K, element M is one or more elements selected from the group consisting of Si, Ge, Sn, Ti, Zr, and Hf, and 0 < n ≤ 0.1.)
[0007] The method for producing a phosphor powder according to the above [1] includes a step of stirring and crushing the above product together with inert particles. As a result, the aggregation of the phosphor particles forming the product is moderately broken up, so that a phosphor powder with suppressed aggregation can be obtained. Since the phosphor powder obtained in this way is less likely to precipitate in liquids such as resins that serve as LED sealing materials, the dispersibility of the phosphor powder is improved, and the uniformity of color tone can be enhanced. The term "inert particles" in the present disclosure means particles composed of a material that is stable in hydrofluoric acid.
[0008] The method for producing a phosphor powder according to the above [1] may be the following [2] to [6].
[0009] [2] The method for producing a phosphor powder according to [1], wherein in the step, the solid compound containing element M and the solid manganese compound are added while stirring the hydrofluoric acid containing the inert particles, to generate the product and crush the product at the same time.
[0010] The method for producing the phosphor powder described in [2] above allows for the generation of the product in hydrofluoric acid while simultaneously crushing the product. This improves the productivity of producing highly dispersible phosphor powder.
[0011] [3] The method for producing phosphor powder according to [1], wherein in the step described above, the product is removed from the hydrofluoric acid after the product has been formed, and the product is added to a mixture containing the inert particles and stirred to crush the product. [4] The method for producing fluorescent powder according to [3], wherein the mixture comprises an alcohol solution containing calcium chloride.
[0012] The method for producing the phosphor powder described in [3] above involves removing the product generated in hydrofluoric acid, transferring the removed product to a mixture containing inert particles, and stirring the mixture to break down the product. This allows the product to be broken down as a post-processing step after generation, making it possible to stably obtain a phosphor powder with high dispersibility.
[0013] The mixture in the method for producing the phosphor powder described in [4] above includes an alcohol solution containing calcium chloride. The alcohol solution containing calcium chloride is used as a surface treatment solution. Therefore, by the method described in [4] above, the phosphor powder can be crushed while surface treatment is performed, and a phosphor powder with excellent dispersibility and moisture resistance can be obtained.
[0014] [5] In the volume-based cumulative particle size distribution α measured by laser diffraction-scattering after ultrasonic homogenization of the dispersion of the phosphor powder, the particle size at which the cumulative value from the smallest particle size reaches 50% of the total is defined as Dy50. In the cumulative distribution β of volume-based particle size measured by laser diffraction / scattering without the aforementioned ultrasonic homogenization process, when the particle size at which the cumulative value from small particle size reaches 50% of the total is defined as Dx50, A method for producing phosphor powder according to any one of [1] to [4], wherein Dx50 / Dy50 is 1.2 to 1.6.
[0015] The phosphor powder obtained by the phosphor powder manufacturing method described in [5] above has a Dx50 / Dy50 of 1.2 to 1.6. Dy represents the particle size determined from the cumulative distribution α of particle size after ultrasonic homogenization treatment under predetermined conditions, and Dx represents the particle size determined from the cumulative distribution β of particle size before ultrasonic homogenization treatment. By performing ultrasonic homogenization treatment, it is possible to measure the particle size in a state where the aggregation due to the physical bonding of aggregated particles has been released. Therefore, the closer the value of Dx50 / Dy50 is to 1, the smaller the difference in particle size between aggregated phosphor particles and released phosphor particles, and it can be said that the aggregation of phosphor particles has been suppressed in the phosphor powder. Thus, the phosphor powder described in [5] above has further suppressed aggregation of phosphor particles. Since such phosphor powder is less likely to precipitate in liquids such as resins used as encapsulating materials, the dispersibility of the phosphor powder can be further improved.
[0016] [6] Let Q1 be the external quantum efficiency when the phosphor powder is irradiated with light of a wavelength of 455 nm. When the phosphor powder is stored for 25 hours in an environment of 60°C and 90% relative humidity, and then irradiated with light of a wavelength of 455 nm, the external quantum efficiency Q2 is defined as follows: A method for producing a phosphor powder according to any one of [1] to [5], wherein the moisture retention rate calculated by Q2 / Q1 × 100 is 89% or more.
[0017] The phosphor powder described in [6] above can suppress the decrease in external quantum efficiency after being stored for 25 hours in an environment of 60°C and 90% relative humidity. Such phosphor powders have excellent storage stability because they have sufficiently high moisture resistance. [Effects of the Invention]
[0018] According to this disclosure, it is possible to provide a method for producing phosphor powder in which aggregation of phosphor particles is suppressed. [Brief explanation of the drawing]
[0019] [Figure 1] This figure shows an example of a light-emitting device. [Description of Embodiments]
[0020] Hereinafter, embodiments of the present disclosure will be described. However, the following embodiments are examples for explaining the present disclosure, and are not intended to limit the present disclosure to the following contents. In the following description, the expression "X to Y" (X and Y are any numerical values satisfying X<Y) means "X or more and Y or less" unless otherwise specified. The upper limit or lower limit of the numerical range explicitly stated in the present disclosure may be replaced with any of the values shown in the Examples. Further, the individually stated upper limit values and lower limit values may be arbitrarily combined. Unless otherwise specified, the materials or components exemplified in the present disclosure may be used alone or in combination of two or more thereof.
[0021] <Method for Producing Phosphor Powder> The method for producing a phosphor powder according to the first embodiment is a method for producing a phosphor powder containing phosphor particles represented by the general formula (1): A₂M (1-n) F₆:Mn 4+ n and the method includes a step of crushing a product obtained by adding a solid compound containing at least element M as a constituent element and a solid manganese compound to hydrofluoric acid containing potassium ions. In the phosphor powder thus obtained, which is represented by the general formula (1): A₂M (1-n) F₆:Mn 4+ n the aggregation between the phosphor particles in the product is moderately broken by crushing. Therefore, precipitation of the phosphor particles can be suppressed, the dispersibility of the phosphor powder in a liquid such as a resin serving as an LED sealing material is improved, and the uniformity of color tone can be enhanced. In the present disclosure, the term "phosphor particles" may include both phosphor particles in an aggregated state (for example, secondary particles) and phosphor particles in a deaggregated state (for example, primary particles).
[0022] The phosphor particles represented by the general formula (1): A₂M (1-n) F₆:Mn 4+ n contain elemental fluorine (F) and tetravalent manganese ions (Mn 4+) and is sometimes referred to as a manganese-activated complex fluoride phosphor. Therefore, in the present disclosure, the phosphor particles represented by the general formula (1) may also be referred to as a manganese-activated complex fluoride phosphor.
[0023] The phosphor particles represented by the general formula (1) can absorb blue light and emit red light due to the presence of tetravalent manganese ions in part of the fluoride. Therefore, the phosphor particles represented by the general formula (1) are used as a phosphor that converts light with a short wavelength such as blue light into light with a long wavelength such as red light. The phosphor powder in the present disclosure means an aggregate including a plurality of such phosphor particles.
[0024] In general formula (1), element A is one or more alkali metal elements containing K. Examples of the alkali metal element include K, Na, Li, and Rb. From the viewpoint of improving light emission characteristics and production ease, element A may be K alone.
[0025] In general formula (1), element M is one or more elements selected from the group consisting of Si, Ge, Sn, Ti, Zr, and Hf. From the viewpoint of improving light emission characteristics and production ease, element M may be Si alone or Ge alone.
[0026] General formula (1): A₂M (1-n) F₆:Mn 4+ n From the viewpoint of improving light emission characteristics and production ease, the phosphor particles represented by the formula may be, for example, those represented by the general formula: K₂Si (1-n) F₆:Mn 4+ n It may be the KSF phosphor represented by the formula.
[0027] In general formula (1), n satisfies 0 < n ≦ 0.1. From the viewpoint of further improving light emission characteristics, n may be, for example, 0.01 to 0.1, 0.01 to 0.07, or 0.015 to 0.04.
[0028] General formula (1): A₂M (1-n) F₆:Mn 4+n In the composition of the constituent elements of the manganese-attached active fluoride phosphor represented by , elements A, M, and Mn 4+ This can be quantitatively analyzed by ICP-MS. Furthermore, in the composition represented by general formula (1), F can be analyzed by ion chromatography. Through the above measurements, the above-mentioned polyfluoride phosphor can be identified, and its composition is determined by general formula (1): A2M (1-n) F6:Mn 4+ n This can be confirmed by the formula shown. A simple measurement method involves performing an X-ray diffraction measurement on the object to be measured and checking whether a diffraction pattern can be observed at the same position as the standard sample. This allows confirmation of whether the object to be measured is a phosphor represented by the composition formula of general formula (1).
[0029] General formula (1): A2M (1-n) F6:Mn 4+ n In a method for producing a phosphorescent powder containing phosphorescent particles represented by , the concentration of hydrogen fluoride in hydrofluoric acid may be 40 to 70% by mass. When the concentration of hydrogen fluoride is within the above range, the MnF6 produced when a solid manganese compound is dissolved in hydrofluoric acid is reduced. 2- This can further stabilize the complex ion.
[0030] Hydrofluoric acid containing potassium ions may be prepared, for example, by adding a compound containing element A (one or more alkali metal elements containing potassium) as a constituent element to hydrofluoric acid. Examples of compounds containing element A as a constituent element include potassium hydrofluoric acid compounds (e.g., KHF2) and potassium fluorides (e.g., KF). These can act as both a potassium source and a fluorine source.
[0031] The lower limit of the amount of compound containing element A as a constituent element added may exceed the minimum amount of potassium added that allows the manganese-attached double fluoride phosphor to reach a saturation concentration or higher, so that the product (manganese-attached double fluoride phosphor) produced by the reaction precipitates in the aqueous solution. The upper limit of the amount of compound containing element A added may be the saturation solubility of element A in the compound in the solvent. These upper and lower limits vary depending on the solvent and the temperature of the aqueous solution used, and therefore cannot be uniquely defined.
[0032] The solid compound containing element M as a constituent element may be at least one selected from the group consisting of, for example, silica (SiO2), germanium dioxide (GeO2), tin oxide (SnO2), titanium oxide (TiO2), zirconium oxide (ZrO2), and hafnium oxide (HfO2). From the viewpoint of ease of manufacture, the solid compound containing element M as a constituent element may be, for example, elemental silica or elemental germanium dioxide.
[0033] The solid manganese compound may be capable of supplying manganese with a valence of +4 or less, and in particular may be capable of supplying manganese with a valence of +4. A manganese compound capable of supplying manganese with a valence of +4 is, for example, readily soluble in hydrofluoric acid and MnF6 in aqueous solution. 2- It may be potassium manganese hexafluoride (K2MnF6) which forms a complex ion.
[0034] When adding a solid compound containing element M and a solid manganese compound to hydrofluoric acid containing potassium ions, the reaction may be carried out at room temperature or below (for example, 30°C or below, 25°C or below, or 15°C or below). From the viewpoint of suppressing the degradation of the phosphor powder and controlling the reaction rate slowly, the hydrofluoric acid may be cooled to 0°C or below 0°C before the reaction. The temperature of the hydrofluoric acid at the start of the reaction may be, for example, -30 to 30°C, -30 to 25°C, -30 to 15°C, -30 to 0°C, -20 to 0°C, -10 to 0°C, or -10°C or above but below 0°C. Furthermore, from the viewpoint of ease of production, the temperature of the hydrofluoric acid at the start of the reaction may be 0°C or above, or 10°C or above, or 0 to 30°C, or 10 to 25°C.
[0035] The order in which a solid compound containing element M and a solid manganese compound are added to hydrofluoric acid containing potassium ions is not particularly limited. The solid compound containing element M may be added first, followed by the solid manganese compound, or the solid compound containing element M may be added after the solid manganese compound, or they may be added simultaneously. In this way, as the solid compound containing element M dissolves, the concentration of the general formula (1): A2M reaches saturation. (1-n) F6:Mn 4+ n Phosphorescent particles represented by can be precipitated as a product. The resulting phosphorescent particles may be aggregated into secondary particles, or they may contain primary particles.
[0036] From the viewpoint of improving the efficiency of solid solution of manganese with respect to precipitated phosphor particles, the mixing ratio of the amount of solid manganese compound to the amount of solid compound containing element M may be 0.02 or higher, 0.03 or higher, or 0.04 or higher. From the viewpoint of suppressing excessive solid solution of manganese, the mixing ratio of the amount of solid manganese compound to the amount of solid compound containing element M may be 0.10 or lower, 0.08 or lower, or 0.07 or lower. The range of the above mixing ratios may be, for example, 0.02 to 0.10, 0.03 to 0.08, or 0.04 to 0.07.
[0037] The addition of the solid compound containing element M and the solid manganese compound to hydrofluoric acid may be done in a single step or in multiple steps. For example, the method of adding the solid compound containing element M and the solid manganese compound to hydrofluoric acid may involve adding the entire amount of the solid compound containing element M and a portion of the solid manganese compound first, and then gradually adding the solid manganese compound multiple times as the phosphor particles precipitate. This allows for sufficient growth of the phosphor particle nuclei while obtaining a phosphor powder with high compositional uniformity. The number of times the solid manganese compound is added may be, for example, 1 to 6 times, 2 to 5 times, or 2 to 4 times.
[0038] Another method for adding a solid compound containing element M and a solid manganese compound to hydrofluoric acid may involve adding a portion of the solid compound containing element M and a portion of the solid manganese compound to hydrofluoric acid to grow seed crystals of precipitated phosphor particles. In this method, both the solid manganese compound and the solid compound containing element M may be added to the hydrofluoric acid containing the precipitated seed crystals multiple times to grow seed crystals. Since the seed crystals have small particle size variations, this method can be used to obtain phosphor powder with even smaller particle size variations. The number of times the solid compound containing element M and the solid manganese compound are added may be, for example, 2 to 7 times or 2 to 6 times, respectively. The number of times the solid compound containing element M and the solid manganese compound are added may be the same or different.
[0039] The present disclosure's method for producing phosphor powder includes a step of stirring and crushing the product obtained by the above method together with inert particles to obtain phosphor powder. The phosphor powder obtained by crushing the product has suppressed aggregation of phosphor particles because the aggregation of phosphor particles is moderately dissolved. Therefore, precipitation of phosphor particles can be suppressed, the dispersibility of the phosphor powder in liquids such as resins used as LED encapsulants can be improved, and the uniformity of the color can be enhanced.
[0040] The inert particles may be any number of particles made of a material stable in hydrofluoric acid, and may be spherical, rectangular, lenticular, flake-shaped, and any other shape. The inert particles may be, for example, spherical beads made of fluororesin, or polytetrafluoroethylene (Teflon®) beads.
[0041] If the inert particles are spherical, the average particle size of the inert particles may be, for example, 1.0 to 10.0 mm or 3.0 to 8.0 mm. The volume of liquid during crushing may be, for example, 100 to 1000 mL or 100 to 700 mL. The number of inert particles used may be 100 to 500 or 200 to 400. The stirring speed during crushing may be 100 to 500 rpm or 150 to 400 rpm. The above stirring conditions in the method of stirring the product together with the inert particles can be adjusted as appropriate.
[0042] In the step of stirring and crushing the product with inert particles, a solid compound containing element M and a solid manganese compound may be added to hydrofluoric acid containing inert particles while stirring to generate the product and crush it. In this case, the inert particles may be added to the hydrofluoric acid beforehand, and the solid compound containing element M and the solid manganese compound may be added while stirring. This allows for both precipitation and crushing of the product, improving the productivity of highly dispersible phosphor powder.
[0043] In the step of disintegrating the product by stirring with inert particles, the product may be removed from the hydrofluoric acid after its formation, added to a mixture containing inert particles, and stirred to disintegrate the product. Alternatively, the product precipitated in the hydrofluoric acid may be transferred to the mixture containing inert particles and stirred to disintegrate it. Alternatively, the product may be precipitated in the hydrofluoric acid, the supernatant liquid removed, and the remaining product may be mixed with the mixture containing inert particles and stirred to disintegrate the product. This allows for the disintegration of the product as a post-processing step after the synthesis of the phosphor, thereby enabling the stable acquisition of highly dispersible phosphor powder. The term "mixture" here refers to the liquid containing inert particles used when disintegrating the product. The mixture containing inert particles may also contain methanol and alcohols such as ethanol.
[0044] In the above process, surface treatment may be performed after crushing the product. Surface treatment of the product can be carried out by stirring the product (phosphor powder) precipitated in hydrofluoric acid in a surface treatment solution. The surface treatment solution may contain, for example, a surface treatment agent containing calcium and a solvent. The solvent of the surface treatment solution may be an alcohol, specifically methanol and ethanol. Through this surface treatment, the surface treatment agent containing calcium (e.g., calcium chloride, calcium nitrate) reacts with the hydrofluoric acid attached to the product to produce calcium fluoride microparticles. At this time, the surface treatment solution is suspended by the produced calcium fluoride microparticles to form a suspension. The produced calcium fluoride microparticles cover the product, thereby surface treating the product and improving its moisture resistance. The concentration of the surface treatment agent in the surface treatment solution may be, for example, 1 to 10% by mass or 2 to 5% by mass.
[0045] In the above process, the product may be crushed and its surface treated simultaneously. For example, the product may be crushed in a mixed solution containing inert particles while its surface is being treated. In this case, the crushing and surface treatment can be performed using a mixed solution containing both inert particles and a surface treatment agent. When crushing and surface treatment are performed simultaneously, a mixed solution prepared by adding inert particles to the surface treatment solution described above may be used.
[0046] Such a mixture also functions as a surface treatment solution and may be prepared by combining an alcohol solution containing calcium chloride with inert particles. The concentration of the surface treatment agent in the mixture may be, for example, 1 to 10% by mass, or 2 to 5% by mass.
[0047] In the above process, surface treatment may be performed before crushing the product. That is, the product that has been surface-treated using a surface treatment solution containing the above-mentioned surface treatment agent and solvent may be added to the mixture and crushed. In the above process, the product that has been surface-treated once may be added to the mixture containing the surface treatment agent and crushed while being surface-treated again. When crushing a product that has already been surface-treated, crushing it in a mixture containing the surface treatment solution suppresses the peeling of the surface treatment agent and allows the moisture resistance of the product to be maintained at a sufficiently high level. As a result, a phosphor powder with even better moisture resistance can be obtained.
[0048] Furthermore, the method for producing the phosphor powder in this disclosure may include other steps in addition to the above steps. Other steps include washing the phosphor powder, drying it, and classifying it. For washing the phosphor powder, for example, alcohols such as methanol and ethanol, acetone, and hydrofluoric acid can be used.
[0049] In the drying process, drying may be carried out to completely evaporate alcohols and other substances adhering to the phosphor powder. The classification process may be carried out to obtain phosphor powder having a desired average particle size. Examples of classification methods include sieving, liquid cyclone, and wind classification.
[0050] The phosphor powder can be manufactured by the above process. However, the above manufacturing method is just one example and is not limited thereto. For example, in the step of stirring and crushing the product together with inert particles, a solid compound containing element M and a solid manganese compound may be added to hydrofluoric acid containing inert particles while stirring to generate a product and crush the product. After that, the product may be removed from the hydrofluoric acid and added to a mixture containing inert particles, and stirred to further crush the product. The phosphor powder obtained by the manufacturing method of this embodiment has sufficient suppression of phosphor particle aggregation. Such phosphor powder can be suitably used in light-emitting devices equipped with mini-LEDs and micro-LEDs.
[0051] The phosphor powder obtained by the manufacturing method of this disclosure is of general formula (1):A2M (1-n) F6:Mn 4+ n A phosphor powder containing phosphor particles represented by [formula], wherein in the cumulative distribution of volume-based particle size α measured by laser diffraction / scattering after ultrasonic homogenization of the phosphor powder dispersion, Dy50 is defined as the particle size when the cumulative value from small particles reaches 50% of the total, and in the cumulative distribution of volume-based particle size β measured by laser diffraction / scattering without ultrasonic homogenization, Dx50 is defined as the particle size when the cumulative value from small particles reaches 50% of the total, then Dx50 / Dy50 may be 1.2 to 1.6. In such a phosphor, the difference in particle size before and after ultrasonic homogenization is small, so aggregation of phosphor particles is further suppressed. Therefore, precipitation of phosphor particles can be further suppressed, and the dispersibility of the phosphor powder in liquids such as resins used as encapsulants for LEDs can be further improved.
[0052] From the viewpoint of further suppressing the aggregation of phosphor particles, the Dx50 / Dy50 ratio may be 1.5 or less. From the viewpoint of ease of manufacturing phosphor particles, the Dx50 / Dy50 ratio of the phosphor powder may be 1.3 or higher, or 1.4 or higher. The range of the Dx50 / Dy50 ratio of the phosphor powder may be, for example, 1.3 to 1.6, 1.4 to 1.6, or 1.4 to 1.5.
[0053] Ultrasonic homogenization of a phosphor powder dispersion is a process used to break down aggregation between phosphor particles in a phosphor powder. By performing ultrasonic homogenization, the physical bonds between phosphor particles can be broken. Therefore, by comparing the particle size at a predetermined cumulative value in the volume-based cumulative distribution of the phosphor powder, which can be measured by laser diffraction and scattering, before and after ultrasonic homogenization, the degree of aggregation of phosphor particles in the phosphor powder can be evaluated. For example, the less aggregation of phosphor particles in the phosphor powder, the closer Dx50 / Dy50 will be to 1.
[0054] Ultrasonic homogenization is performed as follows: 30 mL of ethanol is placed in a 50 mL beaker, and 0.03 g of phosphor powder is added to obtain a dispersion. The dispersion is then subjected to ultrasonic treatment for 3 minutes using an ultrasonic homogenizer. The phosphor powder is homogenized using the method described above. The ultrasonic homogenizer used is the Ultrasonic Homogenizer US-150E (product name) manufactured by Nippon Seiki Seisakusho Co., Ltd., or a device with equivalent performance. When using the above-mentioned device as the ultrasonic homogenizer, the homogenization conditions are as follows. Altitude: 100% Amplitude: 100% Oscillation frequency: 19.5kHz Tip size: φ20mm Amplitude: 32±2μm If homogenization is performed using equipment other than those described above, the homogenization process should be carried out under conditions equivalent to those described above.
[0055] The laser diffraction and scattering method can be used for measurement in accordance with the method described in JIS Z 8825:2013 "Particle size analysis - Laser diffraction and scattering method". A laser diffraction and scattering particle size distribution analyzer (Microtrac MT3300EX II, manufactured by Microtrac-Bell Co., Ltd.) can be used for measurement. In this disclosure, the cumulative distribution of volume-based particle size measured by the laser diffraction and scattering method after ultrasonic homogenization of the phosphor powder dispersion is defined as the cumulative distribution α. The cumulative distribution of volume-based particle size measured by the laser diffraction and scattering method before ultrasonic homogenization of the phosphor powder dispersion is defined as the cumulative distribution β.
[0056] In the cumulative distribution α, Dy50 is defined as the particle size at which the cumulative value from small particle sizes reaches 50% of the total, and Dy50 may be 30.0 μm or less, 29.0 μm or less, or 27.0 μm or less. By having Dy50 within the above range, the phosphor particles in the phosphor powder after ultrasonic homogenization are sufficiently small, so the dispersibility of the phosphor powder in liquid can be further improved even when it contains small phosphor particles that tend to aggregate. Dy50 may be 15.0 μm or more, or 20.0 μm or more. The range of Dy50 may be, for example, 15.0 to 30.0 μm, 20.0 to 30.0 μm, 20.0 to 29.0 μm, or 20.0 to 27.0 μm.
[0057] In the cumulative distribution β, when the particle size Dx50 is defined as the particle size at which the cumulative value from small particle size reaches 50% of the total, Dx50 may be 45.0 μm or less, or 40.0 μm or less. By having Dx50 within the above range, aggregation of phosphor particles is further suppressed, and the dispersibility of the phosphor powder in liquid can be further improved. Dx50 may also be 30.0 μm or more. The range of Dx50 may be, for example, 30.0 to 45.0 μm or 30.0 to 40.0 μm.
[0058] In the cumulative distribution α, if Dy10 is the particle size when the cumulative value from small particle size reaches 10% of the total, and Dy90 is the particle size when the cumulative value from small particle size reaches 90% of the total, then (Dy90-Dy10) / Dy50 may be 0.90 or less, 0.86 or less, or 0.80 or less. The value calculated by (Dy90-Dy10) / Dy50 is also called the span value. When (Dy90-Dy10) / Dy50 is within the above range, the variation in particle size of the phosphor powder is reduced, which further suppresses the aggregation of phosphor particles and further suppresses the dispersion of the phosphor powder in liquid. (Dy90-Dy10) / Dy50 may be 0.60 or more, or 0.70 or more. The range of (Dy90-Dy10) / Dy50 may be, for example, 0.60~0.90, 0.70~0.90, 0.70~0.86, or 0.70~0.80.
[0059] Dy90 may be 30.0 to 50.0 μm, or 30.0 to 40.0 μm. Having Dy90 within the above range can further reduce the variation in particle size of the phosphor powder. Dy10 may be 10.0 to 25.0 μm, or 15.0 to 20.0 μm. Having Dy10 within the above range can further reduce the variation in particle size of the phosphor powder.
[0060] Let Q1 be the external quantum efficiency when a phosphor powder is irradiated with light of a wavelength of 455 nm, and let Q2 be the external quantum efficiency when the phosphor powder is stored for 25 hours in an environment of 60°C and 90% relative humidity and then irradiated with light of a wavelength of 455 nm. The humidity retention rate calculated as Q2 / Q1 × 100 may be 89% or higher, or 93% or higher. Having a humidity retention rate within the above range suppresses the reduction of the external quantum efficiency and maintains performance even when stored in a harsh environment. Therefore, such a phosphor powder has high reliability. The humidity retention rate may be 97% or lower. Phosphor powders with a humidity retention rate within the above range have sufficiently high humidity resistance and are even more reliable. The range of the humidity retention rate may be, for example, 89-97% or 93-97%.
[0061] The external quantum efficiency Q1 of the phosphor powder when irradiated with light of a wavelength of 455 nm may be, for example, 50-80% or 60-70%. The internal quantum efficiency of the phosphor powder when irradiated with light of a wavelength of 455 nm may be, for example, 70-90% or 80-90%. The absorption rate of light of a wavelength of 455 nm may be, for example, 70-85%. The external quantum efficiency, internal quantum efficiency, and absorption rate when irradiated with light of a wavelength of 455 nm can be measured using, for example, a spectrophotometer manufactured by Otsuka Electronics Co., Ltd. (e.g., product name: QE-2000) by the method described in the examples.
[0062] The chromaticity pass rate of 1000 or more white LEDs produced using the phosphor powder obtained by the manufacturing method of this disclosure may be 88% or higher, or 90% or higher. White LEDs with a chromaticity pass rate within the above range have reduced color variation and excellent color rendering. The chromaticity pass rate may be 98% or lower, or 95% or lower. The range of the chromaticity pass rate may be, for example, 88-98% or 90-98%. The chromaticity pass rate can be measured, for example, by the method described in the examples.
[0063] Figure 1 shows an example of a light-emitting device. The light-emitting device 10 comprises a light-emitting element 20 that emits primary light, and a wavelength converter 30 that absorbs a portion of the primary light and emits secondary light having a wavelength longer than the wavelength of the primary light. The wavelength converter 30 contains the phosphor powder described above. The wavelength converter 30 is provided in contact with the upper part of the light-emitting element 20.
[0064] The light-emitting element 20 emits excitation light and may be a blue LED. A terminal 40 is located at the bottom of the light-emitting element 20. When the terminal 40 is connected to a power supply, the light-emitting element 20 can emit light.
[0065] The excitation light emitted from the light-emitting element 20 may be wavelength-converted by the wavelength converter 30. When the excitation light is blue light, the blue light is converted by the general formula (1): A2M (1-n) F6:Mn 4+ n The wavelength is converted to red light by a wavelength converter 30 containing phosphor particles represented by [the given symbol].
[0066] The wavelength converter 30 may be composed of the above-mentioned phosphor particles and a sealing material that encapsulates the phosphor particles. Various curable resins can be used as the sealing material. Any curable resin can be used as long as it is sufficiently transparent and can obtain the optical properties necessary for the display. Silicone resin can be used as an example of a sealing material. Silicone resin is preferably used from the viewpoint of transparency and heat resistance.
[0067] The light-emitting element 20 includes at least one selected from the group consisting of mini-LEDs and micro-LEDs. The size of the mini-LED may be 100-2000 μm, 200-1000 μm, or 300-800 μm. On the other hand, the size of the micro-LED may be 1 μm or more and less than 100 μm, 10-80 μm, or 30-60 μm. By having the sizes of the mini-LEDs and micro-LEDs within this range, high-brightness and high-precision light emission can be achieved in displays and the like equipped with the light-emitting device 10.
[0068] Although several embodiments of this disclosure have been described above, this disclosure is not limited in any way to the embodiments described above. [Examples]
[0069] The contents of this disclosure will be explained in more detail below with reference to examples and comparative examples. However, this disclosure is not limited to the examples described below.
[0070] (Example 1) The following method allows for the general formula (1): A2M (1-n) F6:Mn 4+ n A phosphor powder containing phosphor particles represented by [the formula shown] was manufactured.
[0071] [Measurement of volume-based median diameter (D50) of silica (SiO2) powder] Two types of amorphous SiO2 powder (product names: FB-50R and FB-5D, both manufactured by Denka Co., Ltd.) were prepared. The D50 of the SiO2 powder was measured in advance according to the following procedure. 100 mL of filtered water containing 0.001% by mass of sodium hexametaphosphate was weighed into a 200 mL beaker, and 0.03 g of SiO2 powder (FB-50R or FB-5D) was added to it. The sample was then dispersed for 3 to 4 minutes using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho Co., Ltd., product name: Ultrasonic Homogenizer US-150E) to prepare the measurement sample. The ultrasonic homogenizer settings were: Altitude: 100%, Amplitude: 100%, Oscillation frequency: 19.5 kHz, Tip size: φ20 mm, and Amplitude: 32 ± 2 μm. Subsequently, a volume-based particle size distribution curve was obtained for the measurement sample using a laser diffraction scattering particle size distribution analyzer (Microtrac MT3300EX II, manufactured by Microtrac-Bell Co., Ltd.). The D50 (cumulative 50th percentile) of the SiO2 powder was determined from the obtained particle size distribution curve and used as the volume-based D50. As a result of the measurement, the D50 of FB-50R was 55.1 μm, and the D50 of FB-5D was 7.7 μm.
[0072] [Preparation of fluorescent powder] At room temperature, 2100 mL of 55% by mass hydrofluoric acid (HF) was measured and added to a 3000 mL fluororesin beaker. The fluororesin beaker was then cooled by immersion in antifreeze in a cooling bath, and 320 g of potassium hydrogen fluoride (KHF2, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) powder was added to the hydrofluoric acid in the beaker. The hydrofluoric acid was then thoroughly stirred using a magnetic stirrer to prepare a solution in which the KHF2 powder was dissolved in the hydrofluoric acid. When the prepared solution cooled to -7°C, 72.0 g of SiO2 powder (product name: FB-50R) and 4.0 g of K2MnF6 (KMF, manufactured by Stella Chemifa Co., Ltd.) powder were added to the solution. Using the initial addition of KMF powder as a reference point, an additional 4.0 g of KMF powder was added at 45 seconds, 90 seconds, and 135 seconds, respectively. The solution was stirred and cooled continuously until 25 minutes had elapsed from the baseline, at which point stirring and cooling were terminated. This resulted in the precipitation of a yellow solid (product) in the solution.
[0073] The beaker was removed from the cooling tank and allowed to stand to allow the product to precipitate sufficiently. The supernatant was then removed, and the product was washed in the beaker with hydrofluoric acid (HF concentration: approximately 24% by mass). After washing, the product was precipitated again in hydrofluoric acid, and the supernatant was removed by decantation to obtain the product wetted with hydrofluoric acid in the beaker. Next, a methanol solution containing calcium chloride at a concentration of 3.7% by mass was prepared as a surface treatment solution. 2000 mL of the prepared surface treatment solution was added to the beaker and stirred to treat the surface of the product. This surface treatment caused the hydrofluoric acid adhering to the product to react with the calcium chloride in the surface treatment solution, generating calcium fluoride microparticles, and a suspension of calcium fluoride microparticles was obtained.
[0074] The beaker containing the suspension was allowed to stand to allow the surface-treated product to precipitate, and the supernatant was removed. Approximately 30-40 g of the wet product was collected, and the remaining product was transferred to another 1000 mL fluororesin beaker. The collected product was used in Comparative Example 1, which will be described later. Then, 250 beads made of polytetrafluoroethylene (Teflon®, diameter: 6.4 mm), which are inert particles (hereinafter referred to as "Teflon beads"), and 500 mL of the above-mentioned surface treatment solution were added to this 1000 mL fluororesin beaker to obtain a mixture.
[0075] Using a stirrer, the mixture containing Teflon beads and the product was stirred at 200 rpm for 10 minutes, and the product was crushed while surface-treated again to obtain a suspension. After stirring, the beaker was allowed to stand to allow the crushed product to precipitate. The supernatant and Teflon beads were removed, and the suspension was filtered to separate and recover the solid. The recovered solid was dried to evaporate and remove any remaining methanol. After drying, a nylon sieve with a mesh size of 75 μm was used to collect the yellow powder that passed through the sieve, yielding 206 g of phosphor powder. X-ray diffraction measurements of the obtained yellow powder revealed that the powder was of general formula (1): A2M (1-n) F6:Mn 4+ n It was confirmed that the resulting material is a manganese-attached composite fluoride phosphor, where element A is potassium (K) and element M is silicon (Si). In this way, the phosphor powder of Example 1 was obtained.
[0076] [Measurement of the value of n in general formula (1)] The amount of manganese solid solution in the obtained phosphor powder was quantified by ICP-MS, and the general formula (1): A2M (1-n) F6:Mn 4+ n The value of n was determined for the manganese-containing activated composite fluoride phosphor represented by [formula]. The results are shown in Table 1.
[0077] [Particle size distribution measurement (with homogenization)] A dispersion was prepared by measuring 30 mL of ethanol into a 50 mL beaker and then adding 0.03 g of phosphor powder. The dispersion was then subjected to a 3-minute dispersion treatment using an ultrasonic homogenizer (manufactured by Nippon Seiki Seisakusho Co., Ltd., product name: Ultrasonic Homogenizer US-150E) to prepare the measurement sample. The ultrasonic homogenizer settings were Altitude: 100%, Amplitude: 100%, Oscillation frequency: 19.5 kHz, Tip size: φ20 mm, Amplitude: 32 ± 2 μm. A volume-based particle size distribution curve of the measurement sample was obtained using a laser diffraction scattering particle size distribution analyzer (manufactured by Microtrac-Bell Co., Ltd., product name: Microtrac MT3300EX II). In the obtained particle size distribution curve, the particle size Dy10 when the cumulative value from the smallest particle size reached 10% of the total, the particle size Dy50 when the cumulative value reached 50%, and the particle size Dy90 when the cumulative value reached 90% were determined. Furthermore, the span value was calculated by (Dy90-Dy10) / Dy50. The results are shown in Table 1.
[0078] [Particle size distribution measurement (without homogenization)] Similar to the case with homogenization, 30 mL of ethanol was measured into a 50 mL beaker, and 0.03 g of fluorescent powder was added to prepare the dispersion. The particle size distribution of the dispersion was measured in the same manner as in the case with homogenization, except that the dispersion treatment using the ultrasonic homogenizer described above was not performed, and a volume-based particle size distribution curve was obtained. In the obtained particle size distribution curve, the particle size Dx50 was determined when the cumulative value from the smallest particle size reached 50% of the total. From the values of Dy50 and Dx50, Dx50 / Dy50 was calculated. The results are shown in Table 1.
[0079] [Measurement of absorption rate, internal quantum efficiency, and external quantum efficiency for light with a wavelength of 455 nm] A standard reflector with a reflectivity of 99% (Labsphere, product name: Spectralon) was placed in the side opening (φ10 mm) of an integrating sphere (φ60 mm). Monochromatic light, spectrally separated to a wavelength of 455 nm from a light source (Xe lamp), was introduced into this integrating sphere via an optical fiber. The spectrum of the reflected light was then measured using a spectrophotometer (Otsuka Electronics Co., Ltd., product name: QE-2000). The number of excitation photons (Qex) was calculated from the spectrum in the wavelength range of 450 to 465 nm.
[0080] Next, a concave cell filled with phosphor powder to create a smooth surface was placed in the opening of an integrating sphere. The phosphor powder was then irradiated with monochromatic light at a wavelength of 455 nm. The excitation reflected light and fluorescence spectra were then measured using a spectrophotometer. From the obtained spectral data, the number of excitation reflected photons (Qref) and the number of fluorescence photons (Qem) were calculated. The number of excitation reflected photons was calculated in the same wavelength range as the number of excitation photons, and the number of fluorescence photons was calculated in the wavelength range of 465 to 800 nm.
[0081] The absorption rate, internal quantum efficiency, and external quantum efficiency of the phosphor powder at 455 nm were determined using the following formulas. The results are shown in Table 2. Absorption rate (%) = {(Qex - Qref) / Qex} × 100 Internal quantum efficiency (%) = {Qem / (Qex-Qref)} × 100 External quantum efficiency (%) = (Qem / Qex) × 100
[0082] [Measurement of moisture retention rate] The external quantum efficiency Q2 for 455 nm light was determined after storing phosphor powder in a constant temperature and humidity dryer at 60°C and 90% relative humidity for 25 hours. The external quantum efficiency for 455 nm light before storage was defined as Q1, and the humidity retention rate (%) was calculated by Q2 / Q1 × 100. The results are shown in Table 2.
[0083] [Calculation of chromaticity pass rate] A phosphor powder was added to silicone resin (Toray Dow Corning Ltd., product name: JCR6175) together with powder of green phosphor β-type sialon phosphor (Denka Co., Ltd., product name: GR-MW540K8SD), and mixed in a rotary-orbit mixer (Thinky Co., Ltd., product name: Awatori Rentaro, model: ARV-310) to obtain a slurry. This slurry was potted into a surface-mount type package to which a blue LED element with a peak wavelength of 450 nm was bonded, and then the package was heat-cured to produce a white LED. The ratio of β-type sialon phosphor to fluoride phosphor particles was adjusted so that the chromaticity coordinate (x,y) of the white LED was centered at (0.289, 0.280) when power was applied and light was emitted.
[0084] Over 1000 white LEDs were fabricated, and their chromaticity was measured using a total luminous flux measuring device (manufactured by Otsuka Electronics Co., Ltd., a device combining a 300mm diameter integrating hemisphere and a spectrophotometer / MCPD-9800). LEDs whose chromaticity (x,y) fell within the range of a parallelogram formed by connecting the four points (0.280,0.270), (0.288,0.270), (0.290,0.290), and (0.298,0.290) were deemed acceptable, while those outside this range were deemed unacceptable. The pass rate was calculated and is shown in Table 2.
[0085] (Example 2) Except for the fact that the initial amount of KHF2 powder added to the beaker containing hydrofluoric acid was 330 g, the amount of KMF powder added when the solution of KHF2 powder dissolved in hydrofluoric acid reached -7°C was 8.5 g, and the amounts of KMF powder added at 45 seconds, 90 seconds, and 135 seconds after the initial addition of KMF powder were 4.3 g, 2.1 g, and 1.1 g, respectively, the same procedure as in Example 1 was used to obtain 216 g of phosphor powder. The value of n, particle size distribution (with and without homogenization), absorptivity, internal quantum efficiency, external quantum efficiency, moisture retention rate, and chromaticity pass rate were determined using the same procedure as in Example 1. The results are shown in Tables 1 and 2.
[0086] (Example 3) 185 g of phosphor powder was obtained using the same procedure as in Example 1, except that the surface treatment solution, a calcium chloride-containing methanol solution added to a 1000 mL fluororesin beaker, was replaced with methanol. The value of n, particle size distribution (with and without homogenization), absorption rate, internal quantum efficiency, external quantum efficiency, moisture retention rate, and chromaticity pass rate were determined using the same procedure as in Example 1. The results are shown in Tables 1 and 2.
[0087] (Example 4) Except for adding 150 mL of surface treatment solution to a 1000 mL fluororesin beaker and stirring the mixture at 350 rpm during product crushing, 187 g of phosphor powder was obtained using the same procedure as in Example 1. The value of n, particle size distribution (with and without homogenization), absorption rate, internal quantum efficiency, external quantum efficiency, moisture retention rate, and chromaticity pass rate were determined using the same procedure as in Example 1. The results are shown in Tables 1 and 2.
[0088] (Example 5) Except for adding 150 mL of surface treatment solution to a 1000 mL fluororesin beaker and stirring the mixture at 350 rpm during product crushing, 187 g of phosphor powder was obtained using the same procedure as in Example 2. The value of n, particle size distribution (with and without homogenization), absorption rate, internal quantum efficiency, external quantum efficiency, moisture retention rate, and chromaticity pass rate were determined using the same procedure as in Example 1. The results are shown in Tables 1 and 2.
[0089] (Example 6) At room temperature, 2100 mL of 55% by mass hydrofluoric acid (HF) was measured and added to a 3000 mL fluororesin beaker. Next, 260 g of potassium hydrogen fluoride (KHF2, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) powder was added at room temperature (20°C), and the mixture was thoroughly stirred using a magnetic stirrer to prepare a solution in which the KHF2 powder was dissolved in hydrofluoric acid. To this solution, 7.0 g of K2MnF6 (KMF, manufactured by Stella Chemifa Co., Ltd.) powder and 25.0 g of SiO2 powder (product name: FB-5D) were added simultaneously and stirred to precipitate seed crystals. Using the time when SiO2 powder (FB-5D) was added as a reference, 14.0g of SiO2 powder (product name: FB-50R) and 3.0g of KMF powder were added simultaneously 60 seconds later, another 3.0g of KMF powder was added 120 seconds later, another 14.0g of SiO2 powder (FB-50R) and 3.0g of KMF powder were added simultaneously 180 seconds later, another 14.0g of SiO2 powder (FB-50R) was added 300 seconds later, another 14.0g of SiO2 powder (FB-50R) was added 420 seconds later, and another 14.0g of SiO2 powder (FB-50R) was added 540 seconds later. The solution was stirred at room temperature, and stirring was stopped 20 minutes after the reference time to grow seed crystals and obtain a yellow solid (product).
[0090] The beaker was allowed to stand to allow the product to precipitate completely. The supernatant was then removed, and the product was washed in the beaker with hydrofluoric acid (HF concentration: approximately 24% by mass). After washing, the product was precipitated again in hydrofluoric acid, and the supernatant was removed by decantation, yielding the product wetted with hydrofluoric acid in the beaker. Next, a methanol solution containing calcium chloride at a concentration of 3.7% by mass was prepared as a surface treatment solution. 2000 mL of the prepared surface treatment solution was added to the beaker and stirred to treat the surface of the product. This surface treatment caused the hydrofluoric acid adhering to the product to react with the calcium chloride in the surface treatment solution, generating calcium fluoride microparticles, and a suspension of calcium fluoride microparticles was obtained.
[0091] The beaker containing the suspension was allowed to stand to allow the surface-treated product to precipitate, and the supernatant was removed. Approximately 30-40 g of the wet product was collected, and the remaining product was transferred to another 1000 mL fluororesin beaker. The collected product was used in Comparative Example 3, which will be described later. Then, 250 beads made of polytetrafluoroethylene (Teflon®, diameter: 6.4 mm), which are inert particles (hereinafter referred to as "Teflon beads"), and 500 mL of the above-mentioned surface treatment solution were added to this 1000 mL fluororesin beaker to obtain a mixture.
[0092] Using a stirrer, the mixture containing Teflon beads and the product was stirred at 200 rpm for 10 minutes, and the product was crushed while surface-treated again to obtain a suspension. After stirring, the beaker was allowed to stand to allow the crushed product to precipitate. The supernatant and Teflon beads were removed, and the suspension was filtered to separate and recover the solid. The recovered solid was dried to evaporate and remove any remaining methanol. After drying, a nylon sieve with a mesh size of 75 μm was used to collect the yellow powder that passed through the sieve, obtaining 200 g of phosphor powder. X-ray diffraction measurements of the obtained yellow powder revealed that the powder was of general formula (1): A2M (1-n) F6:Mn 4+ n It was confirmed that the material was a manganese-attached composite fluoride phosphor, represented as such, with element A being potassium (K) and element M being silicon (Si). In this way, the phosphor powder of Example 6 was obtained. The value of n, particle size distribution (with and without homogenization), absorptivity, internal quantum efficiency, external quantum efficiency, moisture retention rate, and chromaticity pass rate were determined using the same procedure as in Example 1. The results are shown in Tables 1 and 2.
[0093] (Example 7) At room temperature, 1050 mL of 55% by mass hydrofluoric acid (HF) was measured and placed into a 2000 mL fluororesin beaker. Furthermore, 250 beads made of polytetrafluoroethylene (Teflon®, diameter: 6.4 mm), which are inert particles (hereinafter referred to as "Teflon beads"), were added. Next, the fluororesin beaker was cooled by immersing it in antifreeze in a cooling bath. 130 g of potassium hydrogen fluoride (KHF2, manufactured by Fujifilm Wako Pure Chemical Industries, Ltd., special grade reagent) powder was added to the hydrofluoric acid in the beaker, and the hydrofluoric acid was thoroughly stirred using a magnetic stirrer to prepare a solution in which the KHF2 powder was dissolved in the hydrofluoric acid. When the prepared solution reached 0°C, 4.0 g of K2MnF6 (KMF, manufactured by Stella Chemifa Co., Ltd.) powder and 15.0 g of SiO2 powder (product name: FB-5D) were added simultaneously and stirred to precipitate seed crystals. Using the time when the SiO2 powder (FB-5D) was added as a reference, 7.0 g of SiO2 powder (product name: FB-50R) and 1.75 g of KMF powder were added simultaneously 60 seconds later, another 1.75 g of KMF powder was added 120 seconds later, another 7.0 g of SiO2 powder (FB-50R) and 1.75 g of KMF powder were added simultaneously 180 seconds later, another 7.0 g of SiO2 powder (FB-50R) was added 300 seconds later, another 7.0 g of SiO2 powder (FB-50R) was added 420 seconds later, and another 7.0 g of SiO2 powder (FB-50R) was added 540 seconds later. The solution was stirred and cooled continuously, and stirring was stopped 20 minutes after the baseline. Seed crystals were grown in the solution containing Teflon beads to obtain a yellow solid (product). In other words, the obtained product was formed and crushed in parallel by adding SiO2 powder and KMF powder while stirring hydrofluoric acid containing inert particles.
[0094] The beaker was removed from the cooling tank and allowed to stand to allow the product to precipitate sufficiently. The supernatant was then removed, and the product was washed in the beaker with hydrofluoric acid (HF concentration: approximately 24% by mass). After washing, the product was precipitated again in hydrofluoric acid, and the supernatant was removed by decantation to obtain the product wetted with hydrofluoric acid in the beaker. Next, a calcium chloride-containing methanol solution was prepared as a surface treatment solution, with methanol as the solvent and a concentration of 3.7% by mass. 2000 mL of the prepared surface treatment solution was added to the beaker and stirred to treat the surface of the product. This surface treatment caused a reaction between the hydrofluoric acid and the calcium chloride in the surface treatment solution, generating calcium fluoride microparticles, and a suspension of calcium fluoride microparticles was obtained.
[0095] The beaker containing the suspension was allowed to stand to allow the surface-treated product to precipitate, and the supernatant was removed. After taking approximately 30-40 g of the wet product, the remaining solids and all the Teflon beads were transferred to a 1000 mL fluoropolymer beaker. 500 mL of the aforementioned surface treatment solution was added to the 1000 mL fluoropolymer beaker to obtain a mixture. Then, using a stirrer, the mixture containing the Teflon beads and product was stirred at 200 rpm for 10 minutes, crushing the product while re-surface-treating it, and a suspension was obtained. After stirring, the beaker was allowed to stand to allow the crushed product to precipitate. The supernatant and Teflon beads were removed, and the suspension was further filtered to separate and recover the solids. The recovered solids were dried to evaporate and remove any remaining methanol. After drying, a nylon sieve with a mesh size of 75 μm was used to collect the yellow powder that passed through the sieve, yielding 131 g of phosphor powder. X-ray diffraction measurements of the obtained yellow powder revealed that the powder is of the general formula (1): A2M (1-n) F6:Mn 4+ nIt was confirmed that the material was a manganese-attached composite fluoride phosphor, represented as such, with element A being potassium (K) and element M being silicon (Si). In this way, the phosphor powder of Example 7 was obtained. The value of n, particle size distribution (with and without homogenization), absorptivity, internal quantum efficiency, external quantum efficiency, moisture retention rate, and chromaticity pass rate were determined using the same procedure as in Example 1. The results are shown in Tables 1 and 2.
[0096] (Comparative Example 1) Approximately 30-40 g of the yellow solid (product) removed in Example 1 was placed in a 500 mL fluororesin beaker, and 100 mL of the same surface treatment solution as in Example 1 was added without adding Teflon beads. The product and surface treatment solution were stirred using a stirrer at 200 rpm for 5 minutes to perform surface treatment. After stirring, the beaker was allowed to stand to allow the surface-treated product to precipitate. The supernatant was removed, and the suspension was filtered to separate and recover the solid. The recovered solid was dried to remove any remaining methanol from the solid. After drying, a nylon sieve with a mesh size of 75 μm was used to collect the yellow powder that passed through the sieve, yielding 39 g of phosphor powder. The value of n, particle size distribution (with and without homogenization), absorption rate, internal quantum efficiency, external quantum efficiency, moisture retention rate, and chromaticity pass rate were determined using the same procedure as in Example 1. The results are shown in Tables 1 and 2.
[0097] (Comparative Example 2) Approximately 30-40 g of the yellow solid (product) removed in Example 2 was placed in a 500 mL fluororesin beaker, and 100 mL of the same surface treatment solution as in Example 1 was added without adding Teflon beads. The product and surface treatment solution were stirred using a stirrer at 200 rpm for 5 minutes to perform surface treatment. After stirring, the beaker was allowed to stand to allow the surface-treated product to precipitate. The supernatant was removed, and the suspension was filtered to separate and recover the solid. The recovered solid was dried to remove any remaining methanol from the solid. After drying, a nylon sieve with a mesh size of 75 μm was used to collect the yellow powder that passed through the sieve, yielding 30 g of phosphor powder. The value of n, particle size distribution (with and without homogenization), absorption rate, internal quantum efficiency, external quantum efficiency, moisture retention rate, and chromaticity pass rate were determined using the same procedure as in Example 1. The results are shown in Tables 1 and 2.
[0098] (Comparative Example 3) Approximately 30-40 g of the yellow solid (product) removed in Example 6 was placed in a 500 mL fluororesin beaker, and 100 mL of the same surface treatment solution as in Example 1 was added without adding Teflon beads. The product and surface treatment solution were stirred using a stirrer at 200 rpm for 5 minutes to perform surface treatment. After stirring, the beaker was allowed to stand to allow the surface-treated product to precipitate. The supernatant was removed, and the suspension was filtered to separate and recover the solid. The recovered solid was dried to remove any remaining methanol from the solid. After drying, a nylon sieve with a mesh size of 75 μm was used to collect the yellow powder that passed through the sieve, yielding 39 g of phosphor powder. The value of n, particle size distribution (with and without homogenization), absorption rate, internal quantum efficiency, external quantum efficiency, moisture retention rate, and chromaticity pass rate were determined using the same procedure as in Example 1. The results are shown in Tables 1 and 2.
[0099] [Table 1]
[0100] [Table 2]
[0101] As shown in Tables 1 and 2, the phosphor powders of Examples 1 to 7, obtained by disintegrating the product by stirring it with inert particles, had a higher chromaticity pass rate when mounted on LEDs than the phosphor powders of Comparative Examples 1 to 3, which did not use inert particles. Therefore, it was confirmed that the phosphor powders of Examples 1 to 7 have improved dispersibility and high color uniformity because the aggregation of phosphor particles in liquid is suppressed. [Industrial applicability]
[0102] According to this disclosure, it is possible to provide a method for producing phosphor powder in which aggregation of phosphor particles is suppressed. [Explanation of symbols]
[0103] 10...Light-emitting device, 20...Light-emitting element, 30...Wavelength converter, 40...Terminal.
Claims
1. General formula (1): A 2 M (1-n) F 6 : Mn 4+ n A method for producing a phosphor powder containing phosphor particles represented by, A method for producing fluorescent powder, comprising the step of adding a solid compound containing at least element M and a solid manganese compound to hydrofluoric acid containing potassium ions, and stirring and crushing the resulting product together with inert particles to obtain the fluorescent powder. (In general formula (1), element A is one or more alkali metal elements containing K, and element M is one or more elements selected from the group consisting of Si, Ge, Sn, Ti, Zr, and Hf, where 0 < n ≤ 0.1.)
2. The method for producing phosphor powder according to claim 1, wherein in the step described above, a solid compound containing element M and a solid manganese compound are added to the hydrofluoric acid containing the inert particles while stirring to produce the product and the product is crushed.
3. The method for producing phosphor powder according to claim 1, wherein in the above step, the product is removed from the hydrofluoric acid after the product has been generated, and the product is added to a mixture containing the inert particles and stirred to crush the product.
4. The method for producing fluorescent powder according to claim 3, wherein the mixed solution includes an alcohol solution containing calcium chloride.
5. In the volume-based cumulative particle size distribution α measured by laser diffraction / scattering after ultrasonic homogenization of the dispersion of the aforementioned phosphor powder, the particle size at which the cumulative value from the smallest particle size reaches 50% of the total is defined as Dy50. In the cumulative distribution β of volume-based particle size measured by laser diffraction / scattering without the aforementioned ultrasonic homogenization process, when the particle size at which the cumulative value from small particle size reaches 50% of the total is defined as Dx50, A method for producing a phosphor powder according to any one of claims 1 to 4, wherein Dx50 / Dy50 is 1.2 to 1.
6.
6. Let Q1 be the external quantum efficiency when the phosphor powder is irradiated with light of a wavelength of 455 nm. When the phosphor powder is stored for 25 hours in an environment of 60°C and 90% relative humidity, and then irradiated with light of a wavelength of 455 nm, the external quantum efficiency Q2 is defined as follows: A method for producing a phosphor powder according to any one of claims 1 to 4, wherein the moisture retention rate calculated by Q2 / Q1 × 100 is 89% or more.
Citation Information
Patent Citations
Red-emitting phosphors and related processes for the synthesis of red-emitting phosphors
JP2019501990A
Fluorescent body particles and light-emitting device
WO2022118600A1