Co-overlay, shaped body
A tetrafluoroethylene/perfluoro(alkyl vinyl ether) copolymer with controlled composition and properties addresses the issue of poor surface smoothness in molded articles by reducing high-melting-point materials and functional groups, achieving superior surface smoothness in molded articles.
Patent Information
- Application Number
- JP2025078914
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Molded articles made from tetrafluoroethylene/perfluoro(alkyl vinyl ether) copolymers (PFA) often suffer from poor surface smoothness due to high-melting-point materials, which are typically high molecular weight components with a high proportion of tetrafluoroethylene units.
A copolymer comprising tetrafluoroethylene (unit A) and a monomer represented by formula CF2=CF-O-Rf (unit B), with specific ratios and functional group limitations, including a melt flow rate of 10-19 g/10 min and a heat of fusion ratio of 0.035 or less, to reduce high-melting-point materials and functional groups, enhancing surface smoothness.
The copolymer produces molded articles with excellent surface smoothness by minimizing high-melting-point components and functional groups, resulting in improved surface quality.
Smart Images

Figure 2026182577000001_ABST
Abstract
Description
[Technical Field]
[0001] The present invention relates to copolymers and molded articles. [Background technology]
[0002] Tetrafluoroethylene / perfluoro(alkyl vinyl ether) copolymer (hereinafter also referred to as "PFA") is known as a fluororesin that has excellent mechanical, chemical, and electrical properties, and is also melt-processable. For example, Patent Document 1 discloses an injection-molded article containing a copolymer containing tetrafluoroethylene units and fluoro(alkyl vinyl ether) units. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Patent No. 7137112 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] Recently, when PFA is used as a component material in molded products, the resulting products are required to have excellent surface smoothness. When the present inventors evaluated a molded article formed using the copolymer manufactured according to Patent Document 1, they found that further improvements were needed in terms of surface smoothness.
[0005] The present invention has been made in view of the above problems, and aims to provide a copolymer that can produce a molded article with excellent surface smoothness. Furthermore, the present invention also aims to provide molded articles. [Means for solving the problem]
[0006] The inventors have found that the above problems can be solved by the following configuration.
[0007] (1) A copolymer comprising a unit A based on tetrafluoroethylene and a unit B based on a monomer represented by formula (1), According to ASTM D1238 for copolymers, the melt flow rate measured under conditions of 297°C and 5 kg load is 10-19 g / 10 min. -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2, and -CH2OH - The total number of functional groups in the copolymer's main chain of 10 carbon atoms 6 Each unit contains less than 150 units. A copolymer characterized in that, when measured using a differential scanning calorimeter at a heating rate of 20°C / min, the ratio of the heat of fusion T2 in the temperature range of 310-320°C to the heat of fusion T1 in the temperature range of 270-310°C in the differential heat curve obtained is 0.035 or less. Formula (1) CF2=CF-O-Rf Rf represents a perfluoroalkyl group having 1 to 10 carbon atoms, and the perfluoroalkyl group may have an etheric oxygen atom between carbon atoms. (2) The copolymer according to (1), wherein the content of unit A is 95.00 to 99.50 mol% of the total units of the copolymer. (3) The copolymer according to (1), wherein the content of unit B is less than 2.0 mol% of the total units of the copolymer. (4) The copolymer according to (1), wherein unit B includes a unit based on perfluoro(propyl vinyl ether). (5) A molded article characterized by being obtained by molding a copolymer described in any of (1) to (4). [Effects of the Invention]
[0008] According to the present invention, a copolymer can be provided that can produce a molded article with excellent surface smoothness. Furthermore, according to the present invention, a molded article can be provided. [Brief explanation of the drawing]
[0009] [Figure 1] This is an example of a differential thermal curve measured using the copolymer of the present invention. [Modes for Carrying Out the Invention]
[0010] The meanings of the terms used in the present specification are as follows. A numerical range expressed using "~" means a range that includes the numerical values stated before and after "~" as the lower limit value and the upper limit value.
[0011] "Unit" is a general term for an atomic group derived from one molecule of the above monomer, which is directly formed by polymerization of the monomer, and an atomic group obtained by chemically converting a part of the above atomic group. In the following description, units derived from individual monomers are sometimes described by adding "unit" to the name of the monomer. "Unit A" is a unit based on tetrafluoroethylene contained in the copolymer. "Unit B" is a unit based on the compound represented by the following formula (1), which is contained in the copolymer. Formula (1) CF2=CF-O-Rf Rf represents a perfluoroalkyl group having 1 to 10 carbon atoms, and the perfluoroalkyl group may have an etheric oxygen atom between carbon atoms.
[0012] "Specific functional group" means a functional group included in the group consisting of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH. In addition, "number of functional groups" means the total number of specific functional groups possessed by the copolymer, unless otherwise specified.
[0013] The copolymer of the present invention (hereinafter also referred to as "this copolymer") is a copolymer comprising unit A based on tetrafluoroethylene and unit B based on a monomer represented by formula (1) described later, wherein the copolymer has a melt flow rate of 10-19 g / 10 min measured under conditions of a temperature of 297°C and a load of 5 kg in accordance with ASTM D1238, and the total number of functional groups -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2 and -CH2OH is such that the copolymer has 10 carbon atoms in its main chain. 6 The number of molecules per unit is less than 150. Measurements were taken using a copolymer with a differential scanning calorimeter at a heating rate of 20°C / min, and the ratio of the heat of fusion T2 in the temperature range of 310-320°C to the heat of fusion T1 in the temperature range of 270-310°C in the differential heat curve obtained was 0.035 or less.
[0014] By using this copolymer, it is possible to form molded articles with excellent surface smoothness. The detailed reasons for this are not yet clear, but it is presumed to be due to the following reasons. The inventors of the present invention investigated the cause of poor surface smoothness in molded articles in the prior art and found that high-melting-point materials are a contributing factor. In other words, they found that a high content of high-melting-point materials results in poor surface smoothness of the molded article. It is presumed that high-melting-point materials consist of high molecular weight components of the copolymer and components in the copolymer that have a high proportion of units formed from tetrafluoroethylene. In the present invention, by adjusting the ratio of the heat of fusion T2 to the heat of fusion T1 defined above to a predetermined value or less, the content of high-melting-point materials in the copolymer can be reduced, and as a result, the deterioration of surface smoothness is suppressed. Furthermore, the inventors have found that the total number of specific functional groups in the copolymer is also related to the surface smoothness of the molded article. In the present invention, the total number of specific functional groups in the copolymer is related to the number of carbon atoms in the main chain of the copolymer. 6 It is presumed that having fewer than 150 particles per unit suppressed the generation of decomposition products, and as a result, prevented the deterioration of surface smoothness. Thus, it is presumed that a molded article with excellent surface smoothness was obtained by satisfying each requirement.
[0015] This copolymer contains at least unit A and unit B. The content of unit A is preferably 95.00 to 99.50 mol%, more preferably 97.00 to 99.50 mol%, and even more preferably 98.00 to 99.50 mol%, relative to the total units of the copolymer, in terms of superior heat resistance.
[0016] Unit B is a unit based on monomers represented by the following formula (1). CF2 = CF - O - Rf (1) In formula (1), Rf represents a perfluoroalkyl group having 1 to 10 carbon atoms, and the perfluoroalkyl group may have an etheric oxygen atom between carbon atoms. The number of carbon atoms in the perfluoroalkyl group represented by Rf is preferably 1 to 8, more preferably 1 to 6, even more preferably 1 to 5, and particularly preferably 1 to 3, from the standpoint of superior polymerization reactivity. Perfluoroalkyl groups may be linear or branched. When a perfluoroalkyl group has an etheric oxygen atom between carbon atoms, the number of etheric oxygen atoms is preferably 1 to 3, and more preferably 1 or 2. It is preferable that the perfluoroalkyl group does not have an etheric oxygen atom.
[0017] Specific examples of monomers represented by formula (1) include perfluoro(methyl vinyl ether) (PMVE), perfluoro(ethyl vinyl ether) (PEVE), and perfluoro(propyl vinyl ether) (PPVE), with PMVE or PPVE being preferred, and PPVE being more preferred.
[0018] Incidentally, the content of Unit B is preferably less than 2.00 mol%, more preferably 0.50 to 1.80 mol%, and even more preferably 0.80 to 1.50 mol%, based on all units of the present copolymer. In such a case, the ratio of the heat of fusion T2 to the heat of fusion T1 of the present copolymer tends to be small, and the molded article formed from the present copolymer tends to have excellent surface smoothness. The present copolymer may contain two or more types of Unit B. When the present copolymer contains two or more types of Unit B, it means that the total content of the two or more types of Unit B is within the above range.
[0019] In the present copolymer, the total content of Unit A and Unit B is preferably 95.50 to 100.00 mol%, more preferably 97.50 to 100.00 mol%, even more preferably 99.00 to 100.00 mol%, and particularly preferably 99.50 to 100.00 mol%, based on all units of the present copolymer, from the viewpoint that the obtained molded article is less likely to be easily deformed by compression or tension.
[0020] The present copolymer may contain, in addition to Unit A and Unit B, units based on other monomers copolymerizable with TFE and PAVE. Examples of other monomers include ethylene, vinylidene fluoride (VdF), hexafluoropropylene (HFP), CX 1 X 2 =CX 3 (CF2) n X 4 (wherein, X 1 , X 2 and X 3 each independently represent a hydrogen atom or a fluorine atom, X 4 represents a hydrogen atom, a fluorine atom or a chlorine atom, and n represents an integer of 1 to 10.), and the monomer represented by CF2=CF-OCH2-Rf 2 (wherein, Rf 2 represents a perfluoroalkyl group having 1 to 5 carbon atoms.) can be mentioned. If the copolymer contains units based on other monomers, the content of units based on other monomers is preferably less than 4.50 mol%, more preferably less than 2.50 mol%, more preferably less than 1.00 mol%, and particularly preferably less than 0.50 mol%, relative to the total units of the copolymer.
[0021] This copolymer preferably contains only units A and B, and does not contain units based on the other monomers mentioned above, in order to form molded articles with superior surface smoothness. In this case, the total content of units A and B is 100.00 mol% of the total units of the copolymer.
[0022] The respective content of unit A, unit B, and other monomer-based units in this copolymer is: 19 It can be measured by known methods such as F-NMR (nuclear magnetic resonance analysis).
[0023] The MFR of this copolymer is 10 to 19 g / 10 min, and is preferably 10 to 16 g / 10 min, and more preferably 11 to 13 g / 10 min, in order to form a molded article with superior surface smoothness. A specific example of a method to bring the MFR of this copolymer within the above range is to adjust the molecular weight of the copolymer. The larger the molecular weight of this copolymer, the smaller the MFR. The MFR of a copolymer is defined as the mass (g) of copolymer flowing out of a 2mm diameter, 8mm length orifice in 10 minutes, measured under ASTM D1238 conditions of 297°C and a 5kg load.
[0024] In this copolymer, the total number of specific functional groups belonging to the group consisting of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2, and -CH2OH is equal to the number of carbon atoms in this copolymer. 6 The number is less than 150 per unit. From the standpoint of forming a molded article with superior surface smoothness, the total number of specific functional groups is preferably 50 or less, more preferably 20 or less, and even more preferably less than 10. The total number of specific functional groups may also be 0.
[0025] Specific functional groups are functional groups located at the ends of the main chain or side chains of the copolymer, and functional groups located within the main chain or side chains. The number of functional groups is the sum of the number of specific functional groups. Specific functional groups are introduced into the copolymer, for example, by chain transfer agents or polymerization initiators used in the production of the copolymer. More specifically, when an alcohol is used as a chain transfer agent, or when a peroxide having the structure -CH2OH is used as a polymerization initiator, -CH2OH is introduced to the main chain ends of the copolymer. Alternatively, the functional groups can be introduced to the side chain ends of the copolymer by polymerizing monomers having the functional groups. Furthermore, if the number of functional groups in a copolymer having a specific functional group exceeds a predetermined range, the number of functional groups can be reduced by fluorinating the copolymer and converting the specific functional group to a -CF3 terminal group. The number of functional groups in the copolymer can be adjusted by changing the conditions of the fluorination treatment (e.g., treatment time, etc.) described later.
[0026] Infrared spectroscopy can be used to identify the types of functional groups and measure the number of functional groups in copolymers. Specifically, the number of functional groups is measured using the following method. First, the copolymer is molded by hot pressing at 330°C to produce a film with a thickness of 0.30 to 0.35 mm. This film is analyzed by Fourier transform infrared spectroscopy to obtain the infrared absorption spectrum of the copolymer. Separately, an infrared absorption spectrum (base spectrum) is obtained from a completely fluorinated copolymer that does not contain specific functional groups, and the difference spectrum between the infrared absorption spectrum and the base spectrum of the copolymer is obtained. From the absorption peak of the specific functional group appearing in this difference spectrum, the number of carbon atoms in the copolymer is determined according to the following formula (A). 6 Calculate the number of functional units N per individual.
[0027] N = I × K / t (A) I: Absorbance K: Correction coefficient t: Film thickness (mm)
[0028] Table 1 shows the absorption frequency, molar extinction coefficient, and correction factor for specific functional groups. The molar extinction coefficient of specific functional groups is determined from FT-IR (Fourier transform infrared spectroscopy) measurement data of low-molecular-weight model compounds.
[0029] [Table 1]
[0030] In copolymers, the absorption frequencies of -CH2CF2H, -CH2COF, -CH2COOH, -CH2COOCH3, and -CH2CONH2 are calculated by subtracting several tens of Kaiser (cm) from the respective absorption frequencies of -CF2H, -COF, -COOH (free and bonded), -COOCH3, and -CONH2 shown in the table. -1 ) It will become lower. For example, the number of -COFs is such that the absorption frequency due to -CF2COF is 1883 cm⁻¹. -1 The number of functional groups determined from the absorption peak and the absorption frequency of 1840 cm² due to -CH2COF -1 This is the sum of the number of functional groups determined from the absorption peaks.
[0031] Using this copolymer, measurements were taken using a differential scanning calorimeter at a heating rate of 20°C / min. In the resulting differential heat curve, the ratio of the heat of fusion T2 in the temperature range of 310-320°C to the heat of fusion T1 in the temperature range of 270-310°C was 0.035 or less. From the viewpoint of forming molded articles with excellent surface smoothness, the above ratio is preferably 0.030 or less, more preferably 0.020 or less, and even more preferably 0.010 or less. There is no particular lower limit to the above ratio, but it is often 0 or greater, and more often 0.003 or greater.
[0032] The differential scanning calorimeter used is the DSC 8500 (manufactured by Perkin Elmer), or a similar device. The heat of fusion is determined using analysis software (Pyris Software, manufactured by Perkin Elmer). The measurement procedure involves holding the copolymer (10 mg) at 200°C for 1 minute, then increasing the temperature to 380°C at a heating rate of 20°C / min to obtain a differential thermal curve with temperature on the x-axis and heat capacity per unit time on the y-axis. Next, the heat of fusion T1 in the temperature range of 270-310°C and the heat of fusion T2 in the temperature range of 310-320°C are determined from the obtained differential heat curve, and the ratio of the heat of fusion T2 to the heat of fusion T1 (heat of fusion T2 / heat of fusion T1) is calculated (see Figure 1). When determining the heat of fusion, a baseline is created by connecting the 270°C point and the 320°C point on the obtained differential heat curve (the dashed line connecting the 270°C point and the 320°C point in Figure 1 corresponds to the baseline).
[0033] The method for producing this copolymer can employ known methods. For example, one method involves producing a copolymer and then fluorinating the produced copolymer. The process for producing the copolymer includes using the above monomers (TFE and the compound represented by formula (1)) by known methods such as bulk polymerization, solution polymerization, suspension polymerization, and emulsion polymerization, with the process of producing by solution polymerization being preferred. In the production of copolymers, in addition to the monomers mentioned above, polymerization initiators, polymerization media, and chain transfer agents can be used.
[0034] As described above, if the content of high-melting-point substances in this copolymer can be reduced, the ratio of the heat of fusion T2 to the heat of fusion T1 can be reduced. To obtain a copolymer exhibiting such properties, it is preferable to reduce the amount of the compound represented by formula (1) used in polymerization. If the amount of the compound represented by formula (1) used in polymerization is large, the polymer produced during polymerization does not swell easily in the solvent, and high-melting-point substances tend to be generated in the latter half of polymerization. The amount of the compound represented by formula (1) used relative to the total amount of monomers used in polymerization is preferably less than 2.00 mol%, more preferably 0.50 to 1.80 mol%, and even more preferably 0.80 to 1.50 mol%.
[0035] The polymerization initiator is preferably a radical polymerization initiator with a half-life of 10 hours and a temperature range of 0 to 100°C, and more preferably a radical polymerization initiator with a temperature range of 20 to 90°C. Specific examples of polymerization initiators include the various polymerization initiators exemplified in International Publication No. 2013 / 015202. Polymerization initiators may be used individually or in combination of two or more. The amount of polymerization initiator used is preferably 0.01 to 0.9 parts by mass, and more preferably 0.05 to 0.5 parts by mass, per 100 parts by mass of monomer used.
[0036] Polymerization media include water, organic solvents, and mixed solvents of water and organic solvents. As organic solvents, fluorine-based solvents such as perfluorocarbons, hydrofluorocarbons, and hydrofluoroethers can be used. Specific examples of organic solvents include the polymerization media exemplified in International Publication No. 2013 / 015202.
[0037] The polymerization medium may be used alone or in combination of two or more types. A mixed solvent of water and a fluorine-based solvent is preferred as the polymerization medium. To obtain a copolymer with a low ratio of heat of fusion T2 to heat of fusion T1, it is preferable to use a mixed solvent of water and a fluorinated solvent as the polymerization medium. The presence of a predetermined amount of the fluorinated solvent further suppresses the formation of high-melting-point substances with high molecular weight during polymerization, resulting in the acquisition of the copolymer. In producing this copolymer, the content of the fluorinated solvent relative to the total volume of water and the fluorinated solvent is preferably 40% by volume or more, more preferably 45% by volume or more, and even more preferably 50% by volume or more. There is no particular upper limit, but it is preferably 80% by volume or less, more preferably 75% by volume or less, and even more preferably 70% by volume or less. As the fluorine-based solvent mentioned above, hydrofluoroethers or hydrofluorocarbons are preferred. The amount of polymerization medium used is preferably 3 times or more by mass ratio of the amount of monomer used, more preferably 5 times or more. Furthermore, it is preferably 20 times or less, and more preferably 17 times or less.
[0038] Preferred chain transfer agents include alcohols such as methanol, ethanol, 2,2,2-trifluoroethanol, 2,2,3,3-tetrafluoropropanol, 1,1,1,3,3,3-hexafluoroisopropanol, and 2,2,3,3,3-pentafluoropropanol, due to their large chain transfer constants and the small amount of additive required; hydrocarbons such as n-pentane, n-hexane, and cyclohexane; hydrofluorocarbons such as CF2H2; ketones such as acetone; mercaptans such as methyl mercaptan; esters such as methyl acetate and ethyl acetate; and ethers such as diethyl ether and methyl ethyl ether. In particular, at least one selected from the group consisting of alcohols, hydrocarbons, and hydrofluorocarbons is preferred, more preferably at least one selected from the group consisting of alcohols and hydrocarbons, and even more preferably alcohols, due to their higher chain transfer constant and greater stability of the end groups of the copolymer. Among the alcohols, methanol or ethanol is preferred, with methanol being more preferred from the viewpoint of reactivity and availability. Two or more chain transfer agents may be used. The amount of chain transfer agent used is preferably 0.001 times or more by mass ratio of the amount of monomer used, more preferably 0.005 times or more. Furthermore, it is preferably 5 times or less, and more preferably 4 times or less.
[0039] The polymerization temperature is preferably 15 to 60°C, more preferably 20 to 58°C, and even more preferably 25 to 55°C. If the polymerization temperature is 25°C or higher, the polymerizability may be excellent. If the polymerization temperature is 60°C or lower, the reactivity of the monomer represented by formula (1) (especially PPVE) is excellent. The polymerization pressure is preferably 0.5 to 3.0 MPa, and more preferably 0.9 to 2.5 MPa. The polymerization time is preferably 1 to 12 hours.
[0040] If polymerization yields a dispersion containing the copolymer, the copolymer can be recovered by coagulating, washing, and drying the copolymer contained in the dispersion. Alternatively, if polymerization yields a slurry, the copolymer can be recovered by removing the slurry from the reaction vessel, washing, and drying it.
[0041] The copolymer obtained by polymerization may be in the form of a powdered solid. Alternatively, the recovered copolymer may be molded into pellet-shaped solids by known methods.
[0042] Next, it is preferable to perform a fluorination treatment on the copolymer obtained by polymerization. Fluorination treatment can reduce the number of the aforementioned specific functional groups, allowing the number of functional groups in the copolymer to be adjusted within a predetermined range. One method of fluorination treatment involves contacting a powder containing a copolymer obtained by polymerization with a fluorinating agent.
[0043] Examples of fluorinating agents include fluorine radical sources that generate fluorine radicals under fluorination treatment conditions. Examples of such fluorine radical sources include F2 gas, N2F2, and halogenated fluorides (e.g., IF5 and ClF3). The concentration of the fluorine radical source, such as F2 gas, may be 100% by volume. From a safety standpoint, it is preferable to use a mixed gas obtained by diluting F2 gas with an inert gas so that the concentration is 5-50% by volume (more preferably 15-30% by volume). Examples of the inert gas include nitrogen gas, helium gas, and argon gas, and from an economic standpoint, nitrogen gas is preferred.
[0044] The temperature during the fluorination treatment is preferably below the melting point of the copolymer, more preferably 20 to 240°C, and even more preferably 100 to 235°C. The fluorination treatment time is appropriately adjusted depending on the number of functional groups in the copolymer before fluorination and the desired number of functional groups, but is typically 0.5 to 30 hours, with 1 to 24 hours being preferred.
[0045] Specific methods for fluorination treatment include, for example, placing a tray containing powdered solid material inside an oven, filling the oven with F2 gas or the above-mentioned mixed gas, and heating for a certain period of time. Another method involves heating a flow-through column filled with powdered solid material while flowing F2 gas or the above-mentioned mixed gas through the column for a certain period of time. From the viewpoint of reaction efficiency, the method of placing a tray containing powdered solid material inside an oven, filling the oven with F2 gas or the above-mentioned mixed gas, and heating for a certain period of time is preferred for fluorination treatment.
[0046] [Molded body] The molded article of the present invention is obtained by molding this copolymer. Specific examples of molded articles of the present invention include injection-molded articles obtained by injection molding of the copolymer, extruded articles obtained by extrusion molding, blow-molded articles obtained by blow molding, transfer-molded articles obtained by transfer molding, press-molded articles obtained by press molding, rotationally molded articles obtained by rotational molding, and coatings obtained by electrostatic coating. Press-molded articles obtained by press molding are preferred for the molded articles of the present invention. Injection-molded articles are also preferred because they can be obtained with a beautiful appearance without corroding the mold used for molding.
[0047] Specific examples of molded articles of the present invention include nuts, bolts, fittings, films, bottles, gaskets, wire insulation materials, tubes, hoses, pipes, valves, seats, seals, packings, tanks, rollers, containers, cocks, connectors, filter housings, filter cages, flow meters, pumps, wafer carriers, and wafer boxes.
[0048] The molded articles of the present invention can also be used for the following applications. Fluid transfer components for food manufacturing equipment, such as food packaging films, lining materials, packings, seals, and sheets for fluid transfer lines used in food manufacturing processes; chemical stoppers, packaging films, lining materials, packings, seals, and sheets for fluid transfer lines used in pharmaceutical manufacturing processes; internal lining materials for chemical tanks and piping in chemical plants or semiconductor factories; O-rings, tubes, packings, valve cores, hoses, and seals used in automobile fuel systems and peripheral equipment, as well as fuel transfer components such as hoses and seals used in automobile automatic transmission systems; carburetor flange gaskets, shaft seals, valve stem seals, seals, and hoses used in automobile engines and peripheral equipment, as well as other automobile components such as brake hoses, air conditioning hoses, radiator hoses, and wire insulation materials; semiconductor components such as O-rings, tubes, packings, valve cores, hoses, seals, rolls, gaskets, diaphragms, and fittings for semiconductor manufacturing equipment. Examples include: chemical liquid transfer components for body equipment; paint and ink components such as paint rolls, hoses, tubes, and ink containers for painting equipment; food and beverage transfer components such as tubes or hoses for food and beverages, hoses, belts, gaskets, and fittings, as well as food packaging materials and glass cooking equipment; waste liquid transport components such as tubes and hoses for waste liquid transport; high-temperature liquid transport components such as tubes and hoses for high-temperature liquid transport; steam piping components such as tubes and hoses for steam piping; corrosion-resistant tapes for piping such as tapes wrapped around piping on ship decks, etc.; various coating materials such as wire coating materials, optical fiber coating materials, transparent surface coating materials and backing materials provided on the light incident side surface of photovoltaic elements of solar cells; sliding components such as diaphragms and various gaskets for diaphragm pumps; agricultural films, fuel cell carrier films, and weather-resistant covers for various roofing materials and side walls, etc.; interior materials used in the building sector, and coating materials for glass such as non-combustible fire-resistant safety glass; lining materials such as laminated steel sheets used in the home appliance sector, etc.
[0049] In particular, the molded articles of the present invention can be suitably used as piping components (e.g., pipes, fittings, gaskets and packings), tubes or films for transferring fluids. Furthermore, the molded body of the present invention can also be suitably used as a wire coating material. A specific example of its use is a coated wire comprising a core wire and a coating layer made of the molded body of the present invention, provided around the core wire. A coated wire equipped with a coating layer made of the molded body of the present invention has excellent electrical properties because the core wire is resistant to corrosion and its outer diameter hardly changes, and is therefore suitably used as a high-frequency transmission cable, flat cable, heat-resistant cable, etc. Such a coated wire can be manufactured, for example, by melt-extruding the copolymer onto a core wire to form the coating layer.
[0050] Furthermore, the molded article of the present invention can also be suitably used as a compressible member. A compressible member is a member used in a compressed and deformed state, and the size and shape of the compressible member are appropriately set according to the application. The shape of the compressible member may be, for example, annular. Alternatively, the compressible member may have a circular, oval, or rounded-corner quadrilateral shape in plan view, and may have a through hole in its center. The compressible member can be used as a piping component for transferring fluids. Furthermore, the compressible member can be used as a component for constructing a non-aqueous electrolyte battery, and is particularly suitable as a component used in contact with the non-aqueous electrolyte in a non-aqueous electrolyte battery. The compressible member can also be suitably used as a sealing member, such as a sealing gasket and sealing packing, and as an insulating member, such as an insulating gasket and insulating packing. A sealing member is a member used to prevent leakage of liquid or gas, or intrusion of liquid or gas from the outside. An insulating member is a member used to insulate electricity. The compressible member may also be a member used for both sealing and insulating purposes. [Examples]
[0051] The present invention will be described in detail below with reference to examples. Examples 1 and 2 are examples, and Examples 3, 4, 5, and 6 are comparative examples. However, the present invention is not limited to these examples. The various measurement and evaluation methods are as follows.
[0052] [measurement] <Composition of copolymer> The content (mol%) of units A and B in each copolymer is: 19 The molar ratio was calculated by converting the results obtained from 1F-NMR analysis.
[0053] <mfr> For each example, a melt indexer (manufactured by Technoseven Co., Ltd.) was used to measure the mass (g) of the solid that flowed out of a 2mm diameter, 8mm length orifice in 10 minutes under ASTM D1238 conditions of a temperature of 297°C and a load of 5kg, and this was defined as MFR (g / 10 min).
[0054] <Ratio of heat of fusion T2 to heat of fusion T1> The results were obtained using a DSC 8500 (manufactured by Perkin Elmer). Specifically, the copolymer (10 mg) was held at 200°C for 1 minute in an air atmosphere, and then heated to 380°C at a heating rate of 20°C / min to obtain a differential thermal curve with temperature on the x-axis and heat capacity per unit time on the y-axis. Next, the heat of fusion T1 in the temperature range of 270-310°C and the heat of fusion T2 in the temperature range of 310-320°C were determined from the obtained differential heat curve, and the ratio of the heat of fusion T2 to the heat of fusion T1 (heat of fusion T2 / heat of fusion T1) was calculated. Furthermore, when determining the heat of fusion, a baseline was created by connecting the 210°C point and the 320°C point on the obtained differential heat curve.
[0055] <Surface smoothness> The solid material obtained in each example was press-molded at 340°C to obtain a 1 mm thick film. The press molding was performed using a heated press machine (SA-301, manufactured by Tester Industries Co., Ltd.). The smoothness of the surface of the obtained film was confirmed by touch when a finger was placed on the film surface and evaluated according to the following criteria. (Surface smoothness evaluation criteria) ○: The surface is smooth. △: The surface is slightly rough. ×: The surface is rough.
[0056] [Example 1] (Polymerization treatment) The polymerization tank with a stirrer was degassed, and then 45.3 kg of CF3CH2OCF2CF2H (AE-3000: product name, manufactured by AGC), 30.7 kg of water, 4.48 kg of CF2=CFO(CF2)3F(PPVE), and 2.49 kg of methanol were charged into the polymerization tank. Next, the temperature inside the polymerization tank was raised to 50°C (polymerization temperature), and 8.15 kg of tetrafluoroethylene (TFE) was further charged to raise the pressure inside the polymerization tank to 1.31 MPa (gauge pressure). 80 mL of a 0.2 mass% AE-3000 solution of heptafluorobutyroyl peroxide was charged as a polymerization initiator solution to start polymerization, and thereafter the polymerization initiator solution was continuously added. In addition, TFE was continuously charged so that the pressure during polymerization was maintained at the same level as the pressure at the start of polymerization. After adding 736 mL of polymerization initiator solution and 13.0 kg of TFE, the polymerization vessel was cooled, purged, and the unreacted TFE was recovered. The obtained copolymer slurry was filtered to separate the polymerization medium, and then dried at 150°C for 15 hours to obtain copolymer 1A. Based on the results of melt NMR analysis and infrared absorption spectroscopy analysis, the composition of copolymer 1A was determined to be TFE units / PPVE units = 98.59 / 1.41 (mol%). Note that "PPVE units" are units based on CF2 = CFO(CF2)3F for each copolymer.
[0057] (Fluorination treatment) Copolymer 1A, placed in a special tray, was placed in a box-type reaction oven, and the oven was sealed. After evacuating the oven, an F2 / N2 mixed gas, prepared by diluting F2 gas with N2 gas to a concentration of 20% by volume, was introduced into the oven. The pressure inside the oven was set to atmospheric pressure (1 atm), and the temperature was set to 230°C. One hour after the introduction of the F2 / N2 mixed gas, the oven was evacuated, the F2 / N2 mixed gas was introduced again, and the reaction was carried out at 230°C for one hour. After the reaction was complete, heating was stopped, and N2 gas was introduced into the oven to completely replace the F2 / N2 mixed gas inside the oven with N2 gas, thereby obtaining copolymer 1B. The number of functional groups was determined by infrared absorption spectroscopy analysis performed on copolymer 1B, which was removed from the oven, using the method described above. The number of functional groups was determined to be 10 carbon atoms in the main chain. 6 There were fewer than 10 per unit. In each example, the composition (content of each unit) of the unfluorinated copolymer was identical to that of the fluorinated copolymer.
[0058] [Example 2] The polymerization tank with a stirrer was degassed, and then 63.5 kg of CF3CH2OCF2CF2H (AE-3000: product name, manufactured by AGC), 18.4 kg of water, 6.28 kg of CF2=CFO(CF2)3F(PPVE), and 1.49 kg of methanol were charged into the polymerization tank. Next, the temperature inside the polymerization tank was raised to 50°C (polymerization temperature), and 9.96 kg of tetrafluoroethylene (TFE) was further charged to raise the pressure inside the polymerization tank to 1.31 MPa (gauge pressure). 80 mL of a 0.2 mass% AE-3000 solution of heptafluorobutyroyl peroxide was charged as a polymerization initiator solution to start polymerization, and thereafter the polymerization initiator solution was continuously added. In addition, TFE was continuously charged so that the pressure during polymerization was maintained at the same level as the pressure at the start of polymerization. After adding 887 mL of polymerization initiator solution and 13.0 kg of TFE, the polymerization vessel was cooled, purged, and the unreacted TFE was recovered. The obtained copolymer slurry was filtered to separate the polymerization medium, and then dried at 150°C for 15 hours to obtain copolymer 2A. Based on the results of melt NMR analysis and infrared absorption spectroscopy analysis, the composition of copolymer 2A was determined to be TFE units / PPVE units = 98.60 / 1.40 (mol%).
[0059] Copolymer 2B was obtained by performing the fluorination treatment in the same procedure as in Example 1, except that copolymer 2A was used instead of copolymer 1A.
[0060] [Example 3] The polymerization tank with a stirrer was degassed, and then 64.3 kg of CF3CH2OCF2CF2H (AE-3000: product name, manufactured by AGC), 19.3 kg of water, 5.37 kg of CF2=CFO(CF2)3F(PPVE), and 0.762 kg of methanol were charged into the polymerization tank. Next, the temperature inside the polymerization tank was raised to 50°C (polymerization temperature), and 9.20 kg of tetrafluoroethylene (TFE) was further charged to raise the pressure inside the polymerization tank to 1.31 MPa (gauge pressure). 80 mL of a 0.2 mass% AE-3000 solution of heptafluorobutyroyl peroxide was charged as a polymerization initiator solution to start polymerization, and thereafter the polymerization initiator solution was continuously added. In addition, TFE was continuously charged so that the pressure during polymerization was maintained at the same level as the pressure at the start of polymerization. After adding 604 mL of polymerization initiator solution and 13.0 kg of TFE, the polymerization vessel was cooled, purged, and the unreacted TFE was recovered. The obtained copolymer slurry was filtered to separate the polymerization medium, and then dried at 150°C for 15 hours to obtain copolymer 3A. Based on the results of melt NMR analysis and infrared absorption spectroscopy analysis, the composition of copolymer 3A was determined to be TFE units / PPVE units = 98.60 / 1.40 (mol%).
[0061] Copolymer 3B was obtained by performing the fluorination treatment in the same procedure as in Example 1, except that copolymer 3A was used instead of copolymer 1A.
[0062] [Example 4] The polymerization tank with a stirrer was degassed, and then 27.2 kg of CF3CH2OCF2CF2H (AE-3000: product name, manufactured by AGC), 43.0 kg of water, 2.69 kg of CF2=CFO(CF2)3F(PPVE), and 3.484 kg of methanol were charged into the polymerization tank. Next, the temperature inside the polymerization tank was raised to 50°C (polymerization temperature), and 9.20 kg of tetrafluoroethylene (TFE) was further charged to raise the pressure inside the polymerization tank to 1.31 MPa (gauge pressure). 80 mL of a 0.2 mass% AE-3000 solution of heptafluorobutyroyl peroxide was charged as a polymerization initiator solution to start polymerization, and thereafter the polymerization initiator solution was continuously added. In addition, TFE was continuously charged so that the pressure during polymerization was maintained at the same level as the pressure at the start of polymerization. After adding 650 mL of polymerization initiator solution and 13.0 kg of TFE, the polymerization vessel was cooled, and the inside of the polymerization vessel was purged to recover the unreacted TFE. The obtained copolymer slurry was filtered to separate the polymerization medium, and then dried at 150°C for 15 hours to obtain copolymer 4A. Based on the results of melt NMR analysis and infrared absorption spectroscopy analysis, the composition of copolymer 4A was determined to be TFE units / PPVE units = 98.55 / 1.45 (mol%).
[0063] Copolymer 4B was obtained by performing the fluorination treatment in the same procedure as in Example 1, except that copolymer 4A was used instead of copolymer 1A.
[0064] [Example 5] The polymerization tank with a stirrer was degassed, and then 62.0 kg of CF3CH2OCF2CF2H (AE-3000: product name, manufactured by AGC), 18.2 kg of water, 7.90 kg of CF2=CFO(CF2)3F(PPVE), and 1.688 kg of methanol were charged into the polymerization tank. Next, the temperature inside the polymerization tank was raised to 50°C (polymerization temperature), and 9.90 kg of tetrafluoroethylene (TFE) was further charged to raise the pressure inside the polymerization tank to 1.24 MPa (gauge pressure). 80 mL of a 0.2 mass% AE-3000 solution of heptafluorobutyroyl peroxide was charged as a polymerization initiator solution to start polymerization, and thereafter the polymerization initiator solution was continuously added. In addition, TFE was continuously charged so that the pressure during polymerization was maintained at the same level as the pressure at the start of polymerization. After adding 881 mL of polymerization initiator solution and 13.0 kg of TFE, the polymerization vessel was cooled, and the inside of the polymerization vessel was purged to recover the unreacted TFE. The obtained copolymer slurry was filtered to separate the polymerization medium, and then dried at 150°C for 15 hours to obtain copolymer 5A. Based on the results of melt NMR analysis and infrared absorption spectroscopy analysis, the composition of copolymer 5A was determined to be TFE units / PPVE units = 97.83 / 2.17 (mol%).
[0065] [Example 6] The polymerization tank with a stirrer was degassed, and then 51.8 L of pure water, 40.9 kg of perfluorocyclobutane, 1.57 kg of CF2=CFO(CF2)3F(PPVE), and 1.03 kg of methanol were charged into the polymerization tank. Next, the temperature was raised to 35°C, and tetrafluoroethylene (TFE) was charged to raise the pressure inside the polymerization tank to 0.64 MPa (gauge pressure). 0.103 kg of a 50% methanol solution of di-n-propyl peroxydicarbonate was added as a polymerization initiator solution to start the polymerization. TFE was continuously charged to maintain the pressure during polymerization at the same level as the pressure at the start of polymerization. When 13.0 kg of TFE had been charged, the polymerization tank was cooled, and the inside of the polymerization tank was purged to recover the unreacted TFE. The obtained copolymer slurry was filtered to separate the polymerization medium, and then dried at 150°C for 15 hours to obtain copolymer 6A.
[0066] Copolymer 6B was obtained by performing the fluorination treatment in the same procedure as in Example 1, except that copolymer 6A was used instead of copolymer 1A.
[0067] The table below shows the composition, various physical properties, and evaluation results of the copolymers in each example. The "water / fluorocarbon ratio" indicates the volume ratio of water, the solvent used during polymerization, to the fluorinated solvent. In the table, the "Unit A (mol%)" column shows the content of unit A relative to the total units of the copolymer (unit: mol%). The "Unit B (mol%)" column shows the content of unit B relative to the total units of the copolymer (unit: mol%). "Number of terminal groups (pcs / 10 6 The column "Number of carbon atoms in the main chain of the copolymer" indicates the number of carbon atoms in the main chain. 6 This represents the total number of -CF=CF2, -CF2H, -COF, -COOH, -COOCH3, -CONH2, and -CH2OH functional groups per unit. "10>" means there are fewer than 10 groups. "400<" means there are more than 400 groups. The "T2 / T1" column represents the ratio (T2 / T1) of the heat of fusion T2 in the temperature range of 310-320°C to the heat of fusion T1 in the temperature range of 270-310°C.
[0068] [Table 2]
[0069] As shown in Table 1, the copolymer was confirmed to exhibit the desired effect. A comparison of Examples 1 and 2 confirmed that the effect is superior when T2 / T1 is 0.020 or less.< / mfr>
Claims
1. A copolymer comprising unit A based on tetrafluoroethylene and unit B based on a monomer represented by formula (1), According to ASTM D1238, the melt flow rate of the copolymer measured under conditions of a temperature of 297°C and a load of 5 kg is 10 to 19 g / 10 min. -CF = CF 2 , -CF 2 H, -COF, -COOH, -COOCH 3 , -CONH 2 and -CH 2 The total number of OH functional groups is equal to the number of carbon atoms in the main chain of the copolymer. 6 Each unit contains less than 150 units. A copolymer characterized in that, when the copolymer is used and measured by differential scanning calorimeter at a heating rate of 20°C / min, the ratio of the heat of fusion T2 in the temperature range of 310 to 320°C to the heat of fusion T1 in the temperature range of 270 to 310°C in the differential heat curve obtained is 0.035 or less. Formula (1) CF 2 =CF-O-Rf Rf represents a perfluoroalkyl group having 1 to 10 carbon atoms, and the perfluoroalkyl group may have an etheric oxygen atom between carbon atoms.
2. The copolymer according to claim 1, wherein the content of unit A is 95.00 to 99.50 mol% relative to the total units of the copolymer.
3. The copolymer according to claim 1, wherein the content of unit B is less than 2.0 mol% of the total units of the copolymer.
4. The copolymer according to claim 1, wherein the unit B includes a unit based on perfluoro(propyl vinyl ether).
5. A molded article characterized by being obtained by molding a copolymer according to any one of claims 1 to 4.
Citation Information
Patent Citations
Injection molded article and manufacturing method thereof
JP7137112B2