Spunlace nonwoven fabric
The spunlace nonwoven fabric with a synthetic and water-retaining fiber structure addresses clogging issues in absorbent sheets by enhancing permeability and retention of both liquid and viscous fluids, particularly viscous bodily fluids with solid components, through a coarser weave and entanglement design.
Patent Information
- Application Number
- JP2025079008
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Existing bodily fluid absorbent sheets, such as those described in Patent Document 1, face issues with clogging when absorbing viscous fluids like stool or menstrual blood due to the presence of solid components, leading to poor absorption and retention performance.
A spunlace nonwoven fabric is designed with a skin-facing layer of synthetic fibers and a non-skin-facing layer of water-retaining fibers that are not heat-fused, allowing for a coarser weave and entanglement structure, enhancing permeability and retention of both liquid and viscous fluids.
The nonwoven fabric exhibits excellent liquid absorption and viscous fluid retention properties, reducing the likelihood of clogging and improving the retention of viscous fluids containing solid components, such as loose stools and menstrual blood, while minimizing adherence to the wearer's skin.
Smart Images

Figure 2026182628000001_ABST
Abstract
Description
[Technical Field]
[0001] This disclosure relates to spunlace nonwoven fabrics. [Background technology]
[0002] Research is being conducted on liquid-permeable sheets for absorbent materials. For example, Patent Document 1 discloses a body fluid absorbing sheet that takes a short time to absorb body fluids discharged onto the surface, allows body fluids to drain quickly from the surface, and makes it difficult for body fluids to return to the surface, that is, a body fluid absorbing sheet with high absorption performance (sweat absorption, absorption rate), high drainage, and resistance to rewetting. The body fluid absorbing sheet according to Patent Document 1 is a body fluid absorbing sheet having a first surface and a second surface, comprising: a nonwoven fabric layer containing a plurality of heat-fusible fibers heat-fused to each other, with one surface constituting the first surface; and a hydrophilic fiber layer containing a plurality of hydrophilic fibers, with one surface adjacent to the other surface of the nonwoven fabric layer and the other surface constituting the second surface, wherein a portion of the plurality of hydrophilic fibers in the hydrophilic fiber layer penetrates the nonwoven fabric layer and is exposed on the first surface (Claim 1). [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2022-46325 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] The bodily fluid absorbent sheet described in Patent Document 1 contains multiple heat-fusible fibers that are heat-fused together, thereby allowing bodily fluids to be quickly removed from the surface. However, stool, for example, soft stool, contains solid components such as undigested dietary fiber, undigested protein, and shed intestinal mucosa, while menstrual blood contains solid components such as the endometrium. The bodily fluid absorbent sheet disclosed in Patent Document 1 may become clogged when absorbing stool, menstrual blood, etc., posing a problem in absorbing stool, menstrual blood, etc. Therefore, the present disclosure aims to provide a spunlace nonwoven fabric that exhibits excellent liquid absorption and viscous fluid retention properties when used as a top sheet for absorbent articles. [Means for solving the problem]
[0005] The Disclosers have found a spunlace nonwoven fabric for use as a top sheet for absorbent articles, wherein the spunlace nonwoven fabric comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer containing water-retaining fibers, wherein the synthetic fibers and water-retaining fibers are not heat-fused, the spunlace nonwoven fabric has a maximum elongation of 10-70% in the transport direction during manufacturing in a tensile test, and the spunlace nonwoven fabric has a surface flow distance of 110 mm or less in a 45° inclined artificial urine absorption test. [Effects of the Invention]
[0006] The spunlace nonwoven fabric relating to this disclosure exhibits excellent liquid absorption and viscous fluid retention properties when used as a top sheet in absorbent articles. [Brief explanation of the drawing]
[0007] [Figure 1] Figure 1 is a cross-sectional photograph of nonwoven fabric No. 1 in the example. [Modes for carrying out the invention]
[0008] Specifically, this disclosure relates to the following aspects: [Aspect 1A] A spunlace nonwoven fabric for use as a top sheet in absorbent articles, The above spunlace nonwoven fabric comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer that contains water-retaining fibers. The above synthetic fibers and the above water-retaining fibers are not heat-fused. The above spunlace nonwoven fabric exhibits a maximum elongation of 10-70% in the transport direction during manufacturing in tensile tests. The above spunlace nonwoven fabric has a surface flow distance of 110 mm or less in a 45° incline artificial urine absorption test. The spunlace nonwoven fabric characterized by the above features.
[0009] In the spunlace nonwoven fabric described above, the synthetic fibers and water-retaining fibers are not heat-fused. Therefore, although the spunlace nonwoven fabric has entanglement points where the synthetic fibers and water-retaining fibers are intertwined by water flow, it can be said that the synthetic fibers and water-retaining fibers do not have heat-fused points. Consequently, the spunlace nonwoven fabric has a coarser weave (larger openings formed between fibers) compared to the nonwoven fabric having heat-fused points. As a result, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, it is more permeable to bodily fluids with liquid properties (hereinafter referred to as "liquid bodily fluids," e.g., urine) compared to the nonwoven fabric having heat-fused points. Furthermore, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, it is more permeable to some bodily fluids with viscous properties (hereinafter referred to as "viscous bodily fluids," e.g., loose stools, menstrual blood, vaginal discharge, etc.) compared to the nonwoven fabric having heat-fused points.
[0010] The above spunlace nonwoven fabric has a predetermined maximum elongation. Accordingly, the above spunlace nonwoven fabric can be said to have a predetermined degree of entanglement, and to include a skin-side layer in which water-retentive fibers in the non-skin-side layer penetrate into the skin-side layer to a certain extent, and a non-skin-side layer in which synthetic fibers in the skin-side layer penetrate into the non-skin-side layer to a certain extent. As a result, when the above spunlace nonwoven fabric is used as a topsheet of an absorbent article, for example, when the absorbent article absorbs body fluid, fiber shedding of synthetic fibers, water-retentive fibers and the like from the above spunlace nonwoven fabric is less likely to occur. Note that "the skin-side layer in which water-retentive fibers in the non-skin-side layer penetrate into the skin-side layer to a certain extent" may be referred to as "the skin-side layer having a predetermined entangled structure", and "the non-skin-side layer in which synthetic fibers in the skin-side layer penetrate into the non-skin-side layer to a certain extent" may be referred to as "the non-skin-side layer having a predetermined entangled structure".
[0011] The above spunlace nonwoven fabric has a predetermined surface flow distance in a 45° inclined artificial urine absorption test. Accordingly, when the body fluid is a liquid body fluid (for example, urine), when the above spunlace nonwoven fabric is used as a topsheet of an absorbent article, the skin-side layer having the predetermined entangled structure can draw in the liquid body fluid that has reached the skin contact surface, the non-skin-side layer having the predetermined entangled structure can draw the liquid body fluid drawn into the skin-side layer into the non-skin-side layer, and can transfer it to a layer adjacent to the non-skin-side layer (for example, an absorbent core). As a result, the above spunlace nonwoven fabric has excellent liquid body fluid absorbency when used in an absorbent article. Since 110 mm corresponds to the distance from the male infant's urethral opening to the ventral end of the product in a baby tape-type disposable diaper of size S, the fact that the above spunlace nonwoven fabric has the above predetermined surface flow distance makes it possible to say that liquid body fluid (for example, urine) is less likely to leak in all types of disposable diapers including baby disposable diapers.
[0012] Furthermore, when the body fluid is a viscous body fluid (e.g., loose stool, menstrual blood, vaginal discharge, etc.), when the above spunlace nonwoven fabric is used as a topsheet of an absorbent article, the skin-side layer having a predetermined entangled structure can draw in moisture in the viscous body fluid that has reached the skin contact surface, the non-skin-side layer having a predetermined entangled structure can draw the moisture in the body fluid drawn into the skin-side layer into the non-skin-side layer, and can transfer it to the layer adjacent to the non-skin-side layer (e.g., an absorbent core). As a result, the above spunlace nonwoven fabric can increase the solid content concentration of the viscous body fluid, make the viscous body fluid less likely to adhere to the wearer's skin, and exhibit viscous body fluid retention performance that retains the viscous body fluid in the spunlace nonwoven fabric.
[0013] Furthermore, when the above body fluid is a viscous body fluid containing solid components (e.g., loose stool containing undigested dietary fiber, undigested protein, shed intestinal mucosa, etc., menstrual blood containing endometrium, etc.), when the above spunlace nonwoven fabric is used as a topsheet of an absorbent article, as the topsheet is less prone to clogging when the skin-side layer having a predetermined entangled structure draws in moisture in the viscous body fluid that has reached the skin contact surface, the non-skin-side layer having a predetermined entangled structure can continue to draw the moisture in the body fluid drawn into the skin-side layer into the non-skin-side layer, and can continue to transfer it to the layer adjacent to the non-skin-side layer (e.g., an absorbent core). As a result, the above spunlace nonwoven fabric can increase the solid content concentration of the viscous body fluid containing solid components, make the viscous body fluid containing solid components less likely to adhere to the wearer's skin, and exhibit viscous body fluid retention performance that retains the viscous body fluid in the spunlace nonwoven fabric.
[0014] From the above, when the above spunlace nonwoven fabric is used in a topsheet of an absorbent article, it is excellent in liquid body fluid absorbency and viscous body fluid retention performance. In this specification, the case where the above spunlace nonwoven fabric is used as a topsheet of an absorbent article may be simply referred to as "when used in an absorbent article".
[0015] [Aspect 1B] A spunlace nonwoven fabric for a topsheet of an absorbent article, The above spunlace nonwoven fabric comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer that contains water-retaining fibers. The above synthetic fibers and the above water-retaining fibers are not heat-fused. The spunlace nonwoven fabric characterized by the above features.
[0016] In the spunlace nonwoven fabric described above, the synthetic fibers and water-retaining fibers are not heat-fused. Therefore, although the spunlace nonwoven fabric has entanglement points where the synthetic fibers and water-retaining fibers are intertwined by water flow, it can be said that the synthetic fibers and water-retaining fibers do not have heat-fused points. Consequently, the spunlace nonwoven fabric has a coarser weave (larger openings formed between fibers) compared to the nonwoven fabric having heat-fused points. As a result, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, the top sheet is more permeable to liquid fluids and a portion of viscous fluids compared to the nonwoven fabric having heat-fused points.
[0017] The above spunlace nonwoven fabric, during the water flow entanglement treatment, has a skin-side layer having a predetermined entanglement structure and a non-skin-side layer having a predetermined entanglement structure, as the water-retaining fibers in the non-skin-side layer penetrate to a certain extent into the skin-side layer and the synthetic fibers in the skin-side layer penetrate to a certain extent into the non-skin-side layer.
[0018] When the bodily fluid is a liquid bodily fluid, such as urine, and the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid that reaches the skin-contact surface, and the non-skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid drawn into the skin-side layer to the non-skin-side layer, and then transfer it to the layer adjacent to the non-skin-side layer (for example, the absorbent core). As a result, the spunlace nonwoven fabric exhibits excellent liquid bodily fluid absorption when used in an absorbent article.
[0019] Furthermore, when the bodily fluid is a viscous fluid (e.g., loose stool, menstrual blood, vaginal discharge, etc.), when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the skin-side layer having a predetermined entanglement structure can draw in moisture from the viscous fluid that reaches the skin-contact surface, the non-skin-side layer having a predetermined entanglement structure can draw in the moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and then transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent core). As a result, the spunlace nonwoven fabric can increase the solid content concentration of the viscous fluid, making it less likely to adhere to the wearer's skin, and can also exhibit viscous fluid retention properties that hold the viscous fluid in the spunlace nonwoven fabric.
[0020] Furthermore, when the bodily fluid is a viscous bodily fluid containing solid components (for example, soft stool containing undigested dietary fiber, undigested protein, shed intestinal mucosa, etc., menstrual blood containing endometrium, etc.), when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the top sheet is less likely to clog when the skin-side layer having a predetermined entanglement structure draws in moisture from the viscous bodily fluid that has reached the skin-contact surface. As a result, the non-skin-side layer having a predetermined entanglement structure can continue to draw in moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the layer adjacent to the non-skin-side layer (for example, the absorbent core). Consequently, the spunlace nonwoven fabric can increase the solid content concentration of the viscous bodily fluid containing solid components, making it less likely for the viscous bodily fluid containing solid components to adhere to the wearer's skin, while also exhibiting viscous bodily fluid retention properties that allow the viscous bodily fluid to be retained in the spunlace nonwoven fabric.
[0021] Based on the above, the spunlace nonwoven fabric exhibits excellent liquid absorption and viscous fluid retention properties when used as a top sheet for absorbent articles.
[0022] [Aspect 2A] The spunlace nonwoven fabric described above has a Klem water absorption of 30 to 170 mm, as described in embodiment 1A or 1B.
[0023] The spunlace nonwoven fabric described above has a predetermined Klem water absorption rate. Therefore, when used in absorbent articles, the spunlace nonwoven fabric facilitates the diffusion of bodily fluids in both the planar and thickness directions. As a result, when used as a top sheet in absorbent articles, the spunlace nonwoven fabric exhibits excellent liquid bodily fluid absorption and viscous bodily fluid retention properties.
[0024] [Aspect 2B] The spunlace nonwoven fabric described above has a maximum elongation of 10-70% in the transport direction during manufacturing, as shown in the tensile test, as described in Embodiment 1B.
[0025] The spunlace nonwoven fabric described above has a predetermined maximum elongation in tensile tests. Therefore, it can be said that the spunlace nonwoven fabric has a predetermined degree of entanglement and comprises a skin-side layer having a predetermined entanglement structure and a non-skin-side layer having a predetermined entanglement structure. Based on the above, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, for example, when the absorbent article absorbs bodily fluids, it becomes less likely for synthetic fibers, water-retaining fibers, etc., to come loose from the spunlace nonwoven fabric. Furthermore, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, it exhibits excellent liquid bodily fluid absorption and viscous bodily fluid retention properties.
[0026] [Aspect 2C] The spunlace nonwoven fabric described above has a surface flow distance of 110 mm or less in a 45° inclined artificial urine absorption test, as described in Embodiment 1B.
[0027] The spunlace nonwoven fabric described above has a predetermined surface flow distance in a 45° inclined artificial urine absorption test. Therefore, when the bodily fluid is a liquid bodily fluid (e.g., urine), when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, the skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid that reaches the skin-contact surface, the non-skin-side layer having a predetermined entanglement structure can draw in the liquid bodily fluid drawn into the skin-side layer to the non-skin-side layer, and then transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent core). As a result, the spunlace nonwoven fabric exhibits excellent liquid bodily fluid absorption when used in absorbent articles. Note that 110 mm corresponds to the distance from the urinary opening of a male baby to the ventral end of the product in a size S tape-type disposable diaper for babies. Therefore, because the spunlace nonwoven fabric has the predetermined surface flow distance described above, it can be said that liquid bodily fluids (e.g., urine) are less likely to leak in disposable diapers in general, including baby disposable diapers.
[0028] [Aspect 3] The spunlace nonwoven fabric described above is a spunlace nonwoven fabric according to any one of embodiments 1A, 1B, 2A, 2B, and 2C, having a rewetting rate of 20% by mass or less in a rewetting test.
[0029] The spunlace nonwoven fabric described above has a predetermined rewetting rate. Therefore, it can be said that the spunlace nonwoven fabric has a predetermined entanglement structure in its skin-facing layer and contains a predetermined ratio of synthetic fibers and water-retaining fibers. Consequently, when used in absorbent articles, the spunlace nonwoven fabric exhibits excellent rewetting properties.
[0030] [Aspect 4] The spunlace nonwoven fabric described above is a spunlace nonwoven fabric according to any one of embodiments 1A, 1B, 2A, 2B, 2C, and 3, having a tensile strength of 1.10 to 4.25 N / 25 mm in the transport direction during manufacturing when tested in the above tensile test.
[0031] The spunlace nonwoven fabric described above has a predetermined strength at 5% elongation. Therefore, when the spunlace nonwoven fabric is used in absorbent articles, for example, when the absorbent article absorbs bodily fluids, it becomes less likely for synthetic fibers, water-retaining fibers, etc., to detach from the spunlace nonwoven fabric.
[0032] [Aspect 5] The spunlace nonwoven fabric described above contains the synthetic fiber and the water-retaining fiber in a mass ratio of 40-80:60-20 in a total of 100 parts by mass of the synthetic fiber and the water-retaining fiber, as described in any one of embodiments 1A, 1B, 2A, 2B, 2C, 3, and 4.
[0033] The above-mentioned spunlace nonwoven fabric contains synthetic fibers and water-retaining fibers in a predetermined mass ratio. Therefore, the skin-side layer and the non-skin-side layer are able to perform their respective functions more easily, and when the above-mentioned spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid fluid absorption and viscous fluid retention properties.
[0034] [Aspect 6] The above spunlace nonwoven fabric has a density of 25-70 g / m². 2 A spunlace nonwoven fabric according to embodiment 5, having the basis weight.
[0035] The above-mentioned spunlace nonwoven fabric contains synthetic fibers and water-retaining fibers in a predetermined mass ratio and has a predetermined basis weight. Therefore, the skin-side layer and the non-skin-side layer are able to perform their respective functions more easily, and when the above-mentioned spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid absorption and viscous liquid retention properties.
[0036] [Aspect 7] The spunlace nonwoven fabric according to any one of embodiments 1A, 1B, 2A, 2B, 2C and 3-6, wherein the synthetic fibers have an average fiber length of 30-60 mm, and the water-retaining fibers have an average fiber length of 30-60 mm.
[0037] In the spunlace nonwoven fabric described above, each of the synthetic fibers and the water-retaining fibers has a predetermined average fiber length. Therefore, the spunlace nonwoven fabric tends to have a predetermined degree of entanglement, and in the skin-side layer having the predetermined degree of entanglement, a certain amount of water-retaining fibers tends to be present within the skin-side layer, but they tend not to be excessively present on the skin-contact surface of the skin-side layer. As a result, after the skin-side layer draws in moisture from bodily fluids that have reached the skin-contact surface (moisture in urine, moisture in loose stool, etc.), it is easier for the moisture to be transferred to the non-skin-side layer without being retained in the skin-side layer, and the non-skin-side layer then easily transfers the moisture from the bodily fluids that has been transferred to it to the layer adjacent to the non-skin-side layer (for example, the absorbent core). Based on the above, when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, it exhibits excellent adhesion to liquid bodily fluids and retention of viscous bodily fluids.
[0038] [Aspect 8] The non-skin-facing layer is a spunlace nonwoven fabric according to any one of embodiments 1A, 1B, 2A, 2B, 2C and 3 to 7, having a higher fiber density than the skin-facing layer.
[0039] In the above-described spunlace nonwoven fabric, the non-skin-facing layer has a higher fiber density than the skin-facing layer. Therefore, after the skin-facing layer, which has a predetermined entanglement structure, draws in moisture from bodily fluids that have reached the skin-contacting surface (e.g., moisture from liquid bodily fluids, viscous bodily fluids, etc.), the water-retaining fibers with a high fiber density present in the non-skin-facing layer can further draw in the moisture from the bodily fluids that have been drawn into the skin-facing layer. As a result, when the above-described spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid bodily fluid absorption and viscous bodily fluid retention.
[0040] [Aspect 9] The above synthetic fiber is a spunlace nonwoven fabric according to any one of embodiments 1A, 1B, 2A, 2B, 2C and 3 to 8, comprising a durable hydrophilic oil agent.
[0041] In the spunlace nonwoven fabric described above, the synthetic fibers contain a durable hydrophilic oil agent. Therefore, during the spunlace treatment, the spunlace nonwoven fabric becomes more prone to entanglement between synthetic fibers, between water-retaining fibers, and between synthetic fibers and water-retaining fibers. Furthermore, the spunlace nonwoven fabric is more likely to have a skin-side layer having a predetermined entanglement structure and a non-skin-side layer having a predetermined entanglement structure. As a result, when used as a top sheet for absorbent articles, the spunlace nonwoven fabric exhibits excellent liquid absorption and viscous fluid retention properties.
[0042] [Aspect 10] The spunlace nonwoven fabric according to any one of embodiments 1A, 1B, 2A, 2B, 2C and 3 to 9, wherein the synthetic fiber is polyethylene terephthalate fiber and the water-retaining fiber is rayon fiber.
[0043] In the above-mentioned spunlace nonwoven fabric, the synthetic fiber is polyethylene terephthalate fiber, and the water-retaining fiber is rayon fiber. The use of polyethylene terephthalate fiber as the synthetic fiber makes the spunlace nonwoven fabric easy to manufacture. Furthermore, when used in absorbent articles, the spunlace nonwoven fabric excels in top sheet durability, water retention, versatility, and homogeneity.
[0044] [Aspect 11] A spunlace nonwoven fabric according to any one of embodiments 1A, 1B, 2A, 2B, 2C and 3 to 10, wherein at least one of the above-mentioned synthetic fibers and the above-mentioned water-retaining fibers is not bonded.
[0045] In the spunlace nonwoven fabric described above, at least one of the synthetic fibers and the water-retaining fibers is not bonded. Therefore, when the spunlace nonwoven fabric is used in an absorbent article, the top sheet is more permeable to liquid bodily fluids and a portion of viscous bodily fluids compared to a nonwoven fabric in which at least one of the synthetic fibers and the water-retaining fibers is bonded with an adhesive. Furthermore, when the bodily fluid is a viscous bodily fluid containing solid components, when the spunlace nonwoven fabric is used in an absorbent article, the top sheet (especially the skin-side layer) is less likely to clog when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous bodily fluid that has reached the skin-contact surface. As a result, the non-skin-side layer, which also has a predetermined entanglement structure, can continue to draw in moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the adjacent layer (e.g., the absorbent material). Consequently, the viscous bodily fluid containing solid components has a higher solid content concentration, making it less likely to adhere to the wearer's skin.
[0046] [Aspect 12] The spunlace nonwoven fabric described above is a spunlace nonwoven fabric according to any one of embodiments 1A, 1B, 2A, 2B, 2C and 3 to 11, which is not heat-sealed or bonded.
[0047] The spunlace nonwoven fabric described above is not heat-sealed. Therefore, when used in absorbent articles, the spunlace nonwoven fabric allows the top sheet to permeate liquid fluids and a portion of viscous fluids more easily than nonwoven fabrics with heat sealing and / or adhesion. Furthermore, when the fluid is a viscous fluid containing solid components, when the spunlace nonwoven fabric is used in absorbent articles, the top sheet (especially the skin-side layer) is less likely to clog when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous fluid that has reached the skin-contact surface. As a result, the non-skin-side layer, which also has a predetermined entanglement structure, can continue to draw in moisture from the fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the adjacent layer (e.g., the absorbent material). Consequently, the viscous fluid containing solid components has a higher solid content concentration, making it less likely to adhere to the wearer's skin.
[0048] [Aspect 13] The absorbent article described above is a spunlace nonwoven fabric as described in any one of embodiments 1A, 1B, 2A, 2B, 2C and 3 to 12, which is an absorbent article for absorbing loose stool or menstrual blood.
[0049] The spunlace nonwoven fabric described above is for use as a top sheet in absorbent articles for absorbing loose stools or menstrual blood. In other words, the spunlace nonwoven fabric described above is for use as a top sheet in absorbent articles for absorbing viscous bodily fluids containing solid components. Generally, loose stools contain solid components such as undigested dietary fiber, undigested proteins, and shed intestinal mucosa, while menstrual blood contains solid components such as the uterine lining, making the top sheet prone to clogging. In contrast, the spunlace nonwoven fabric described above, having the configuration of Embodiment 1, is less prone to clogging when used in absorbent articles, even when it absorbs a viscous liquid containing solid components. As a result, the spunlace nonwoven fabric can increase the solid content concentration of the viscous liquid containing solid components, making it less likely for the viscous liquid containing solid components to adhere to the wearer's skin, while also exhibiting viscous liquid retention properties that allow the viscous liquid to be retained by the spunlace nonwoven fabric.
[0050] The spunlace nonwoven fabric for the top sheet of the absorbent article described herein (hereinafter sometimes simply referred to as "spunlace nonwoven fabric") will be described in detail below. The spunlace nonwoven fabric relating to this disclosure is intended for use as a top sheet in absorbent articles. The spunlace nonwoven fabric mentioned above refers to a nonwoven fabric manufactured by the spunlace method.
[0051] The absorbent articles mentioned above are not particularly limited, as long as they absorb bodily fluids and have a liquid-permeable top sheet. The above-mentioned bodily fluids are not particularly limited and include urine, feces (e.g., loose stools), menstrual blood, vaginal discharge, breast milk, blood, exudate, etc. From the viewpoint of the effects of this disclosure, the above-mentioned bodily fluids are preferably viscous, and more preferably viscous, containing solid components. Examples of the above-mentioned viscous bodily fluids include loose stools, menstrual blood, vaginal discharge, and exudate, while examples of viscous bodily fluids containing the above-mentioned solid components include loose stools containing undigested dietary fiber, undigested protein, and shed intestinal mucosa, and menstrual blood containing endometrium, etc.
[0052] Examples of the absorbent items mentioned above include diapers (e.g., disposable diapers, adult disposable diapers, baby disposable diapers), urine pads, incontinence pads, sanitary napkins, panty liners, shorts-type sanitary napkins, absorbent shorts, breast pads, pet sheets, and pressure ulcer pads. Absorbent items for absorbing the above-mentioned viscous bodily fluids include diapers (e.g., disposable diapers, e.g., adult disposable diapers, baby disposable diapers), sanitary napkins, panty liners, shorts-type sanitary napkins, and pressure ulcer pads. Absorbent articles for absorbing viscous bodily fluids containing the above-mentioned solid components include diapers (e.g., disposable diapers, e.g., disposable adult diapers, disposable baby diapers), sanitary napkins, panty-type sanitary napkins, and pressure ulcer pads.
[0053] The absorbent article described above generally comprises a liquid-permeable top sheet, a liquid-impermeable back sheet, and an absorbent core positioned between the top sheet and the back sheet. Furthermore, the absorbent core may be provided in the absorbent article as an absorbent body comprising the absorbent core and a core wrap covering the absorbent core.
[0054] The absorbent article described above may further include, as constituent materials of the absorbent article, a diffusion sheet (second sheet) disposed between the top sheet and the absorbent core (absorbent body), a diffusion sheet (third sheet) disposed between the absorbent core (absorbent body) and the back sheet, and so on. The top sheet described above comprises a skin-contact surface that comes into contact with the user's skin and a non-skin-contact surface opposite to the skin-contact surface.
[0055] The spunlace nonwoven fabric described above comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer that contains water-retaining fibers. In the spunlace nonwoven fabric described above, the synthetic fibers and water-retaining fibers are not heat-fused (hereinafter, the heat-fusion of fibers will be simply referred to as "heat fusion"). That is, although the spunlace nonwoven fabric has entanglement points where the synthetic fibers and water-retaining fibers are intertwined by water flow, the synthetic fibers and water-retaining fibers do not have heat-fused points. As a result, the spunlace nonwoven fabric has a coarser weave compared to a nonwoven fabric with heat-fused points. Consequently, when the spunlace nonwoven fabric is used in absorbent articles, the top sheet is more permeable to liquid fluids and a portion of viscous fluids compared to a nonwoven fabric with heat-fused points. Furthermore, when the bodily fluid is a viscous fluid containing solid components, the spunlace nonwoven fabric, when used in absorbent articles, is less likely to clog the top sheet (especially the skin-side layer) when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous fluid that has reached the skin-contact surface. As a result, the non-skin-side layer, which also has a predetermined entanglement structure, can continue to draw in moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the layer adjacent to the non-skin-side layer (for example, the absorbent core). Consequently, the viscous fluid containing solid components has a higher solid content concentration, making it less likely to adhere to the wearer's skin. The above heat fusion refers to the heat fusion that occurs when forming the spunlace nonwoven fabric, and does not include the heat fusion between the spunlace nonwoven fabric and other materials constituting the absorbent article when used in such an article.
[0056] The spunlace nonwoven fabric described above has a maximum elongation of 10-70% in the transport direction during manufacturing, as measured by tensile testing. The maximum elongation is preferably 15% or more, and more preferably 20% or more. Furthermore, the maximum elongation is preferably 60% or less, and more preferably 55% or less. Thus, the spunlace nonwoven fabric has a predetermined degree of entanglement and comprises a skin-side layer having a predetermined entanglement structure and a non-skin-side layer having a predetermined entanglement structure. Therefore, when the spunlace nonwoven fabric is used as a top sheet for an absorbent article, for example, when the absorbent article absorbs bodily fluids, it becomes less likely for fibers such as synthetic fibers and water-retaining fibers to detach from the spunlace nonwoven fabric. In this specification, the conveying direction during manufacturing may be referred to as the MD direction, and the direction perpendicular to the MD direction during manufacturing may be referred to as the CD direction.
[0057] In this specification, the above tensile test is carried out as follows: [Tensile test] (1) Prepare a sample of spunlace nonwoven fabric (length 230 mm x width 25 mm). When measuring the maximum elongation (%) and strength at 5% elongation (N / 25 mm) in the MD direction, prepare the sample so that the MD direction is the length direction. When measuring the maximum elongation (%) and strength at 5% elongation (N / 25 mm) in the CD direction, prepare the sample so that the CD direction is the length direction. (2) The above sample is mounted on a tensile testing machine (Shimadzu Autograph AGS-1kNG) with a gripping distance of 100 mm, and a load is applied at a tensile speed of 100 mm / min until the sample breaks. The strength at 5% elongation (N / 25 mm) and the maximum elongation (%) are measured. The measurement is performed at 25°C ± 2°C.
[0058] (3) For the strength at 5% elongation (N / 25mm) and maximum elongation (%), measurements were taken on 10 different samples, and the average value was adopted. For the tensile tests described above, conditions not specified above shall be in accordance with JIS L 1913:2010, "6.3 Tensile strength and elongation (ISO method)". Note that the strength at n% elongation (N / 25mm) refers to the tensile strength (N) per 25mm width when the sample is elongated by n%. Also, the maximum elongation (%) refers to the elongation (%) at which the tensile strength reaches its maximum value.
[0059] The spunlace nonwoven fabric described above has a surface flow distance of 110 mm or less, preferably 107 mm or less, more preferably 96 mm or less, even more preferably 80 mm or less, and even more preferably 75 mm or less in a 45° inclined artificial urine absorption test. Furthermore, the spunlace nonwoven fabric has a surface flow distance of preferably 34 mm or more, and more preferably 46 mm or more, in a 45° inclined artificial urine absorption test. As a result, when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, it exhibits excellent liquid fluid absorption and viscous fluid retention. In addition, because the surface flow distance is within the preferred range, liquid fluid leakage is less likely to occur in tape-type disposable diapers for babies from size S to younger months. Note that 110 mm corresponds to the distance from the urinary opening of a male baby to the ventral end of the product in a size S tape-type disposable diaper for babies, and 96 mm corresponds to the distance from the urinary opening of a male baby to the ventral end of the product in a size NB disposable diaper for babies.
[0060] In this specification, the above 45° inclined artificial urine absorption test is performed as follows. [45° Inclined Artificial Urine Absorption Test] (1) In a constant temperature and humidity chamber with a temperature of 23°C ± 2°C and a relative humidity of 50 ± 5% RH, a rigid PVC sheet (length: 450 mm × width: 230 mm × thickness: 5 mm) is placed on the table surface of a table having a horizontal table surface, such that the angle formed by the length of the rigid PVC sheet and the table surface is 45°. (2) Prepare a sample of spunlace nonwoven fabric (length: 250 mm x width: 67 mm). The sample should be prepared so that the MD direction is the length direction and the CD direction is the width direction.
[0061] (3) Place the sample on the rigid PVC board in the following manner: (i) the longitudinal direction of the sample coincides with the longitudinal direction of the rigid PVC board, (ii) the center of the sample coincides with the center of the rigid PVC board, (iii) the non-skin side of the sample faces the rigid PVC board, and (iv) the longitudinal length of the sample is 254-256 mm (extended by approximately 2% from the original length). While maintaining the stretched state of the sample, secure the edges with cellophane tape or the like. (4) Mark the starting point of the X shape using a marker (Zebra, Hi-Mackie (blue)) 50 mm from the top edge in the longitudinal direction of the sample and at the center in the width direction.
[0062] (5) Aspirate 1 mL of artificial urine into a pipette (Gilson Microman E M1000E) equipped with a corresponding tip (capillary & piston CP-1000), and dispense 1 mL of artificial urine over 0.5 seconds from a height of 20 ± 3 mm above the starting mark. The above artificial urine is prepared by dissolving 200 g of urea, 80 g of sodium chloride, 8 g of magnesium sulfate, 3 g of calcium chloride, and approximately 1 g of the dye Blue No. 1 in 10 L of deionized water. (6) 2.0 seconds after the start of dripping, mark the endpoint with an X at the lowest point of the artificial urine. (7) Measure the longitudinal distance from the starting mark to the ending mark. (8) Using different samples, the longitudinal distance is measured a total of 10 times, and the average value is adopted as the surface flow distance.
[0063] The synthetic fibers mentioned above can be any synthetic fibers used in the field of absorbent articles without any particular limitations. Examples of such synthetic fibers include those containing a single component, such as single fibers. Examples of such components include polyolefin polymers, such as polyethylene and polypropylene; polyester polymers, such as terephthalate polymers, such as polyethylene terephthalate (PET), polybutylene terephthalate, and polypentylene terephthalate; polyamide polymers, such as nylon 6 and nylon 6,6; acrylic polymers; polyacrylonitrile polymers; and modified versions thereof. The synthetic fiber mentioned above is preferably polyethylene terephthalate (PET) fiber. This is due to its high heat resistance, which simplifies the manufacturing of spunlace nonwoven fabrics, and its high durability when used in absorbent articles.
[0064] Preferably, the synthetic fiber contains a durable hydrophilic oil agent, which is a hydrophilic oil agent that has sufficient durability to prevent it from flowing off during spunlace treatment. By containing the durable hydrophilic oil agent, the surface of the synthetic fiber becomes hydrophilic and the surface of the synthetic fiber becomes more likely to maintain its hydrophilic state. As a result, during spunlace treatment, the synthetic fibers become more likely to entangle with each other, with each other, and with each other, and the spunlace nonwoven fabric is more likely to have a skin-side layer with a predetermined entanglement structure and a non-skin-side layer with a predetermined entanglement structure. As a result, when the spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid absorption and viscous fluid retention.
[0065] The above-mentioned durable hydrophilic oil agents are not particularly limited, but examples include polyether esters, ether nonions, polyether-modified silicones, sulfosuccinates, polyoxyethylene amide ethers, alkylimidazoline type cations, polyglycerin polyesters, mixtures of alkyl phosphate ester salts having 10 to 30 carbon atoms with betaine compounds having 10 to 30 carbon atoms, sulfate ester salts, sulfonate salts, etc., or mixed oil agents such as mixtures of alkyl phosphate ester salts and polyether-modified silicones.
[0066] Some of the above synthetic fibers may include an initial hydrophilic oil agent, which is a hydrophilic oil agent that has sufficient durability to flow off during spunlace treatment. Examples of the above initial hydrophilic oil agent include alkyl phosphate ester salts and alkyl phosphate metal salts.
[0067] The above-mentioned synthetic fiber may contain the durable hydrophilic oil by treating the surface of the synthetic fiber with the durable hydrophilic oil, or by kneading the durable hydrophilic oil into the components constituting the synthetic fiber, thereby making the surface of the synthetic fiber hydrophilic. Similarly, the above-mentioned synthetic fiber may contain the initial hydrophilic oil by treating the surface of the synthetic fiber with the initial hydrophilic oil, or by kneading the initial hydrophilic oil into the components constituting the synthetic fiber.
[0068] The above synthetic fibers preferably have an average fiber length of 30 mm or more, more preferably 35 mm or more, and even more preferably 40 mm or more. Alternatively, the above synthetic fibers may have an average fiber length of 60 mm or less, more preferably 57 mm or less, and even more preferably 55 mm or less. This makes it easier for the spunlace nonwoven fabric to have a predetermined degree of entanglement, and while a certain amount of water-retaining fibers in the non-skin-side layer are likely to be present in the skin-side layer, they are less likely to be present in excess on the skin-contacting surface of the skin-side layer.
[0069] The synthetic fibers described above preferably have a fineness of 0.6 dtex or more, more preferably 1.0 dtex or more, and even more preferably 1.4 dtex or more. Alternatively, the synthetic fibers may have a fineness of 3.3 dtex or less, more preferably 2.5 dtex or less, and even more preferably 2.0 dtex or less. This makes it easier for the spunlace nonwoven fabric to have a predetermined degree of entanglement, and while a certain amount of water-retaining fibers in the non-skin-side layer are likely to be present in the skin-side layer, they are less likely to be present in excess on the skin-contacting surface of the skin-side layer.
[0070] In this disclosure, the average fiber length of the fibers is measured according to "A7.1 Measurement of fiber length" in Annex A of JIS L 1015:2010, "A7.1 Measurement of fiber length" and "A7.1.1 Method A (standard method) Method for measuring the length of individual fibers on a graduated glass plate." The above method is a test method equivalent to ISO 6989, which was published in 1981.
[0071] The above-mentioned water-retaining fibers are not particularly limited as long as the fibers themselves are capable of retaining moisture; for example, cellulose fibers can be mentioned. Examples of the cellulose fibers mentioned above include natural cellulose fibers, regenerated cellulose fibers, refined cellulose fibers, and semi-synthetic cellulose fibers. Examples of the above-mentioned natural cellulose fibers include plant fibers, such as seed hair fibers (e.g., cotton fibers), pulp fibers (e.g., hemp), leaf vein fibers (e.g., Manila hemp), and fruit fibers (e.g., coconut).
[0072] Examples of the cotton fibers mentioned above include cotton fibers from the cotton species *Hirstum* (e.g., Upland cotton), cotton fibers from the cotton species *Barbadense*, cotton fibers from the cotton species *Arboreum*, and cotton fibers from the cotton species *Herbacheum*. Furthermore, the cotton fibers mentioned above may be organic cotton fibers or pre-organic cotton (trademark) fibers. Organic cotton fibers refer to cotton that has been certified by GOTS (Global Organic Textile Standard).
[0073] Examples of the regenerated cellulose fibers mentioned above include rayon, such as viscose rayon obtained from viscose, polynosic and modal, and copper ammonia rayon (also called "cupro") obtained from a copper ammonia salt solution of cellulose.
[0074] The above-mentioned purified cellulose fibers include lyocell, specifically, pulp which is dissolved in an aqueous solution of N-methylmorpholine N-oxide to form a dope, and then extruded into a dilute solution of N-methylmorpholine N-oxide to produce fibers. The above-mentioned purified cellulose is commercially available, for example, as Tencel (trademark). Examples of the above-mentioned semi-synthetic fibers include semi-synthetic cellulose, such as acetate fibers, such as triacetate and diacetate.
[0075] The above-mentioned water-retaining fibers are preferably regenerated cellulose fibers, more preferably rayon fibers, and even more preferably rayon fibers that have not been modified with hydroxyl groups. This is because they have high water retention, high versatility, and high homogeneity.
[0076] The above-mentioned water-retaining fibers preferably have an average fiber length of 30 mm or more, more preferably 33 mm or more, and even more preferably 35 mm or more. Furthermore, the above-mentioned water-retaining fibers preferably have an average fiber length of 60 mm or less, more preferably 55 mm or less, and even more preferably 50 mm or less. As a result, the spunlace nonwoven fabric is more likely to have a predetermined degree of entanglement, and the water-retaining fibers in the non-skin-side layer are more likely to be present in a certain amount in the skin-side layer, but are less likely to be present in excess on the skin-contacting surface of the skin-side layer.
[0077] The above water-retaining fibers preferably have a fineness of 0.6 dtex or more, more preferably 1.0 dtex or more, and even more preferably 1.4 dtex or more. Furthermore, the above water-retaining fibers preferably have a fineness of 3.3 dtex or less, more preferably 2.5 dtex or less, and even more preferably 2.0 dtex or less. As a result, the spunlace nonwoven fabric is more likely to have a predetermined degree of entanglement, and the water-retaining fibers in the non-skin-side layer are more likely to be present in a certain amount in the skin-side layer, but are less likely to be present in excess on the skin-contacting surface of the skin-side layer.
[0078] The above spunlace nonwoven fabric contains the above synthetic fibers and the above water-retaining fibers in a mass ratio of preferably 40-80:60-20, more preferably 45-75:55-25, and even more preferably 50-70:50-30, in a total of 100 parts by mass of the above synthetic fibers and the above water-retaining fibers. As a result, the above skin-side layer and the above non-skin-side layer are able to perform their respective functions more easily, and when the above spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid fluid absorption and viscous fluid retention.
[0079] In the spunlace nonwoven fabric described above, the skin-facing layer and the non-skin-facing layer can have any fiber density. For example, the non-skin-facing layer can have a higher or lower fiber density than the skin-facing layer. Preferably, the non-skin-facing layer has a higher fiber density than the skin-facing layer. This makes it easier for the water-retaining fibers with a high fiber density in the non-skin-facing layer to further draw in the moisture from the bodily fluids (e.g., liquid bodily fluids, viscous bodily fluids, etc.) that have reached the skin-contacting surface of the skin-facing layer after the skin-facing layer has drawn in moisture from the bodily fluids.
[0080] The density relationship described above can be achieved, for example, by adjusting the fiber density of the skin-side web forming the skin-side layer and the fiber density of the non-skin-side web forming the non-skin-side layer before manufacturing the spunlace nonwoven fabric, by compressing the webs. The above-mentioned fiber density means the density of fibers constituting each layer (the above-mentioned skin-side layer, the above-mentioned non-skin-side layer, etc.), and the fiber density in each of the above-mentioned layers can be compared visually after magnifying each layer with a microscope or the like as necessary.
[0081] The above-mentioned spunlace nonwoven fabric preferably has a basis weight of 25 g / m 2 or more, more preferably 30 g / m 2 or more, and even more preferably 35 g / m 2 or more. Further, the above-mentioned spunlace nonwoven fabric preferably has a basis weight of 70 g / m 2 or less, more preferably 65 g / m 2 or less, and even more preferably 60 g / m 2 or less. Thereby, the above-mentioned skin-side layer and the above-mentioned non-skin-side layer can easily exhibit their respective functions, and when the above-mentioned spunlace nonwoven fabric is used as a topsheet of an absorbent article, it is excellent in liquid body fluid absorbency and viscous body fluid retention properties.
[0082] In the present specification, the basis weight is determined by taking 10 samples each having a size of 100 mm × 100 mm, measuring the mass of each sample, then for each sample, the value of mass (g) / area (m 2 ) is calculated as each basis weight (g / m 2 ), and the average value of the respective basis weights of the total 10 samples is taken as the basis weight. In addition, when it is difficult to collect samples of the above size, samples can be collected within a possible range.
[0083] In the spunlace nonwoven fabric described above, it is preferable that at least one of the synthetic fibers and the water-retaining fibers, and more preferably both, are not bonded with an adhesive (hereinafter, when the fibers are bonded with an adhesive, this is simply referred to as "bonding"). As a result, when the spunlace nonwoven fabric is used in an absorbent article, the top sheet is more permeable to liquid fluids and a portion of viscous fluids compared to a nonwoven fabric in which at least one of the synthetic fibers and the water-retaining fibers are bonded with an adhesive. Furthermore, when the bodily fluid is a viscous fluid containing solid components, the spunlace nonwoven fabric, when used in absorbent articles, is less likely to clog the top sheet (especially the skin-side layer) when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous fluid that has reached the skin-contact surface. As a result, the non-skin-side layer, which also has a predetermined entanglement structure, can continue to draw in moisture from the bodily fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the adjacent layer (e.g., the absorbent layer). Consequently, the viscous fluid containing solid components has a higher solid content concentration, making it less likely to adhere to the wearer's skin. From a similar viewpoint, in the spunlace nonwoven fabric described above, it is preferable that the fibers constituting the spunlace (including the synthetic fibers and the water-retentive fibers) do not have any bonding points other than entanglement points where they are intertwined with other fibers (for example, heat-sealed points where they are heat-sealed with other fibers, adhesive points where they are bonded with other fibers by an adhesive, etc.). Furthermore, the above-mentioned bonding refers to bonding at least one of the synthetic fibers and the water-retaining fibers to each other when forming the spunlace nonwoven fabric, and does not include bonding the spunlace nonwoven fabric to other materials constituting the absorbent article when used in such an article.
[0084] Preferably, the spunlace nonwoven fabric described above does not have heat fusion with synthetic fibers or heat fusion with heat-fusible fibers. Furthermore, preferably, the spunlace nonwoven fabric does not have adhesive properties. As a result, when the spunlace nonwoven fabric is used in an absorbent article, the top sheet is more permeable to liquid fluids and a portion of viscous fluids compared to nonwoven fabrics having heat fusion and / or adhesive properties. Also, when the fluid is a viscous fluid containing solid components, when the spunlace nonwoven fabric is used in an absorbent article, the top sheet (especially the skin-side layer) is less likely to clog when the skin-side layer, which has a predetermined entanglement structure, draws in moisture from the viscous fluid that has reached the skin-contact surface. Therefore, the non-skin-side layer, which has a predetermined entanglement structure, can continue to draw in moisture from the fluid drawn into the skin-side layer to the non-skin-side layer, and can also continue to transfer it to the layer adjacent to the non-skin-side layer (e.g., the absorbent). As a result, viscous fluids containing solid components have a higher concentration of solids, making them less likely to adhere to the wearer's skin. From a similar viewpoint, it is preferable that the spunlace nonwoven fabric does not have any bonding points other than entanglement points where a certain fiber constituting the spunlace nonwoven fabric is entangled with other fibers (for example, heat-sealed points where it is heat-sealed with other fibers, adhesive points where it is bonded with other fibers by an adhesive, etc.).
[0085] The spunlace nonwoven fabric described above has a tensile strength at 5% elongation in the MD direction of preferably 1.10 N / 25 mm or more, more preferably 2.00 N / 25 mm or more, and even more preferably 2.50 N / 25 mm or more in the tensile test described above. Furthermore, the spunlace nonwoven fabric has a tensile strength at 5% elongation in the MD direction of preferably 4.25 N / 25 mm or less, more preferably 4.00 N / 25 mm or less, and even more preferably 3.50 N / 25 mm or less in the tensile test described above. As a result, when the spunlace nonwoven fabric is used in an absorbent article, for example, when the absorbent article absorbs bodily fluids, it becomes less likely for fibers such as synthetic fibers and water-retaining fibers to come out of the spunlace nonwoven fabric. The strength at 5% elongation has already been explained in the "Tensile Test" section above.
[0086] The spunlace nonwoven fabric described above preferably has a Klem water absorption of 30 mm or more, more preferably 80 mm or more, and even more preferably 110 mm or more. Furthermore, the spunlace nonwoven fabric preferably has a Klem water absorption of 170 mm or less, and more preferably 150 mm or less. As a result, when the spunlace nonwoven fabric is used in an absorbent article, it facilitates the diffusion of bodily fluids in the planar and thickness directions. Therefore, when the spunlace nonwoven fabric is used as a top sheet in an absorbent article, it exhibits excellent liquid bodily fluid absorption and viscous bodily fluid retention.
[0087] In this specification, the above-mentioned Klem water absorption is measured in accordance with JIS P8141:2004 "Paper and cardboard - Water absorption test method - Klem method," and the differences from JIS P8141:2004 are as follows. - The dimensions of the test specimen will be changed from "length 200 mm or more" to "length 230 mm ± 1 mm," and the width will be changed from "width 15 ± 1 mm" to "width 25 ± 1 mm." - The specimen should have the MD direction as its longitudinal direction. - The time taken to read the water level rise will be changed from "10 minutes ± 10 seconds" to "5 minutes ± 10 seconds".
[0088] The above spunlace nonwoven fabric has a rewetting rate of preferably 20.0% by mass or less, more preferably 15.0% by mass or less, even more preferably 10.0% by mass or less, even more preferably 8.0% by mass or less, and even more preferably 6.0% by mass or less in a rewetting test. This means that the skin-side layer of the spunlace nonwoven fabric has a predetermined entanglement structure and contains a predetermined ratio of synthetic fibers and water-retaining fibers. As a result, the spunlace nonwoven fabric exhibits excellent rewetting properties when used in absorbent articles. The lower limit of the above rewetting rate is not particularly limited, but for example, 1.0% by mass is one example.
[0089] In this specification, the above rewet test is measured as follows: [Rewet Test] (1) Prepare a nonwoven fabric sample (length: 200 mm x width: 110 mm), a cylinder (inner diameter: 60 mm, height: 50 mm), filter paper (ADVANTEC, Item 2, Quality 1000, size: 100 x 100 mm), a burette (capable of dispensing 80 mL / 10 seconds), and a weight (3.5 kg, base (square) size: 100 mm x 100 mm) in a constant temperature and humidity chamber with a temperature of 23 °C ± 2 °C and a relative humidity of 50 ± 5% RH. The sample should be prepared so that the MD direction is the length direction. (2) Place 10 sheets of the above-mentioned filter paper, which mimics an absorbent material, on a plastic tray, and place the above-mentioned sample on top of the 10 sheets of filter paper so that the non-skin side layer is in contact with the filter paper, thereby forming a simulated absorbent article with the above-mentioned sample as the top sheet.
[0090] (3) Place the cylinder on top of the sample of the simulated absorbent material so that the center of the sample and the center of the cylinder coincide, and drop 10 mL of artificial urine onto the center of the cylinder using a burette at a rate of 80 mL / 10 seconds. The composition of the artificial urine is the same as that used in the "45° Inclined Artificial Urine Absorption Test". (4) After the artificial urine has been dispensed, remove the cylinder once the artificial urine has been dispensed, and 60 seconds after the artificial urine has been dispensed, place the filter paper weighing approximately 50 g, whose initial mass m0 (g) has been measured in advance, in the place where the artificial urine was dispensed, so that the center of the sample and the center of the filter paper coincide, and then place the weight on top of the filter paper so that the center of the sample and the center of the weight coincide.
[0091] (5) 120 seconds after placing the weight, remove the weight and approximately 50g of the filter paper, measure the post-test mass of the approximately 50g of filter paper: m1 (g), and calculate the rewetting rate: R (mass %) using the following formula: R (mass%)=100×(m1-m0) / 10 It is calculated by [method]. (6) The rewetting rate: R (mass%) is measured a total of five times using different samples and new filter paper, and the average value is adopted.
[0092] The spunlace nonwoven fabric described above may consist of two layers, including the skin-side layer and the non-skin-side layer, and may further include an additional layer positioned on the non-skin side of the non-skin-side layer. Examples of the additional layer include those containing cellulose acetate fibers and the water-retaining fibers described above.
[0093] The spunlace nonwoven fabric relating to this disclosure can be manufactured by a spunlace method known in the art. The spunlace nonwoven fabric relating to this disclosure can be manufactured, for example, by a spunlace process including the following steps. - A skin-side layer web preparation step (hereinafter referred to as the "skin-side layer web preparation step") which prepares a skin-side layer web that constitutes the skin-side layer, including synthetic fibers. - A non-skin layer web preparation step (hereinafter referred to as the "non-skin layer web preparation step") which prepares a non-skin layer web that constitutes the non-skin layer and contains water-retaining fibers. - A laminated web formation step (hereinafter referred to as the "laminated web formation step") involves stacking the above-mentioned skin-side layer web and the above-mentioned non-skin-side layer web to form a laminated web. - A water-entanglement treatment step (hereinafter referred to as the "water-entanglement treatment step") in which the laminated web is subjected to water-entanglement treatment to form a water-entangled spunlace nonwoven fabric. - A drying step (hereinafter referred to as the "drying step") to dry the spunlace nonwoven fabric that has been entangled with water flow as described above.
[0094] In the above skin-side layer web preparation step, a skin-side layer web constituting the skin-side layer, including synthetic fibers, is prepared. In the above skin-side layer web preparation step, for example, the synthetic fibers constituting the skin-side layer can be mechanically opened using a carding machine to prepare the skin-side layer web. In the above skin-side layer web preparation step, it is preferable that the synthetic fibers included in the skin-side layer web include a durable hydrophilic oil agent. The reason for this will be explained later. Since the above-mentioned card machine is publicly known in this technical field, its description will be omitted. Furthermore, the skin-side web may contain not only the synthetic fibers but also the water-retaining fibers in advance. In that case, from the viewpoint of obtaining the effects according to Embodiment 1, the skin-side web preferably contains 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 98% by mass or more of the synthetic fibers.
[0095] In the above non-skin layer web preparation step, a non-skin layer web constituting the non-skin layer, which includes water-retaining fibers, is prepared. In the above non-skin layer web preparation step, for example, a carding machine can be used to mechanically open the water-retaining fibers constituting the non-skin layer and prepare the non-skin layer web. Since the above-mentioned card machine is publicly known in this technical field, its description will be omitted. Furthermore, the skin-side web may contain not only the water-retaining fibers but also the synthetic fibers. In that case, the non-skin-side web contains, from the viewpoint of obtaining the effects of Embodiment 1, preferably 85% by mass or more, more preferably 90% by mass or more, even more preferably 95% by mass or more, even more preferably 97% by mass or more, and even more preferably 98% by mass or more of the water-retaining fibers.
[0096] In the above-described laminated web formation step, the skin-side layer web and the non-skin-side layer web are laminated to form a laminated web.
[0097] In the above water flow entanglement treatment step, the laminated web is subjected to water flow entanglement treatment to form a water flow entangled spunlace nonwoven fabric. The above-described water flow entanglement treatment can be carried out according to methods known in the art. The above water flow entanglement treatment is performed, for example, with a transport speed of 5-20 m / min and a water flow rate of 0.05-0.2 m per unit time. 3 This can be performed under conditions such as: flow rate / minute, water flow pressure: 5-20 MPa (skin-side web and non-skin-side web), nozzle diameter: 80-120 μm, nozzle pitch: 0.5-2 mm, nozzle rows: 2-4 rows, etc.
[0098] The above-described water flow entanglement treatment can be performed, for example, by placing the laminated web on a support and, while conveying the laminated web, spraying a water flow from a nozzle onto the laminated web to entangle it. The water flow can be sprayed onto one side (single side) or both sides (double side) of the skin-side layer web and the non-skin-side layer web. That is, in the spunlace nonwoven fabric according to this disclosure, one or both sides of the skin-contacting surface of the skin-side layer and the non-skin-side surface of the non-skin-side layer may be water flow entangled surfaces.
[0099] When a stream of water is sprayed from the nozzle onto only one side of the non-skin layer web of the laminated web, a portion of the water stream passes from the non-skin layer web through the skin layer web to the support side, while the remaining portion of the water stream bounces back towards the nozzle. At this time, a portion of the water stream pushes the water-retaining fibers in the non-skin layer web into the skin layer web, forming a skin layer with a predetermined entanglement structure. Also, when the remaining portion of the water stream bounces back towards the nozzle, it pushes the synthetic fibers in the skin layer web back to the non-skin layer web, forming a non-skin layer with a predetermined entanglement structure. Furthermore, if the synthetic fibers in the skin layer web contain a durable hydrophilic oil, the water stream easily adheres to the skin layer web, and the water stream that reaches the skin layer web easily escapes to the support side, making it easier for synthetic fibers to entangle with each other, water-retaining fibers to entangle with each other, and synthetic fibers and water-retaining fibers to entangle with each other. As a result, when the above-mentioned spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid absorption and viscous fluid retention properties.
[0100] When a stream of water is sprayed from a nozzle onto only one side of the skin-side layer web of the laminated web, a portion of the water stream passes from the skin-side layer web (skin-side layer) through the non-skin-side layer web (non-skin-side layer) to the support side, while the remaining portion of the water stream bounces back towards the nozzle. At this time, a portion of the water stream can push the synthetic fibers in the skin-side layer web into the non-skin-side layer web, forming a non-skin-side layer with a predetermined entanglement structure. Also, when the remaining portion of the water stream bounces back towards the nozzle, it can push the water-retaining fibers in the non-skin-side layer web back to the skin-side layer web, forming a skin-side layer with a predetermined entanglement structure. Furthermore, if the synthetic fibers in the skin-side layer web contain a durable hydrophilic oil, the water stream will easily adhere to the skin-side layer web, and the water stream that reaches the skin-side layer web will easily pass through the non-skin-side layer web to the support side, making it easier for synthetic fibers to entangle with each other, water-retaining fibers to entangle with each other, and synthetic fibers and water-retaining fibers to entangle with each other. As a result, when the above-mentioned spunlace nonwoven fabric is used as a top sheet for absorbent articles, it exhibits excellent liquid absorption and viscous fluid retention properties.
[0101] The same applies when a stream of water is sprayed from the nozzle onto both the skin-side layer web and the non-skin-side layer web of the laminated web. In this specification, in the water entanglement treatment step, it is preferable to spray a water stream from the nozzle onto only one side of the non-skin side layer web of the laminated web. This makes it easier to form a spunlace nonwoven fabric in which the water-retaining fibers in the non-skin side layer are appropriately interwoven with the synthetic fibers in the skin side layer, and when the spunlace nonwoven fabric is used as the top sheet of an absorbent article, it exhibits excellent liquid absorption and viscous liquid retention.
[0102] In the drying step described above, the spunlace nonwoven fabric that has been entangled with water is dried. The drying step can be carried out at a predetermined temperature for a predetermined time. The predetermined temperature is preferably a temperature that allows the moisture to evaporate but does not cause the synthetic fibers to heat-fuse together, for example, 100 to 150°C. The predetermined time is, for example, 3 to 8 seconds.
[0103] Furthermore, the above-mentioned spunlace nonwoven fabric can also be manufactured by combining a web-like fiber sheet that constitutes the skin-facing layer and a web-like fiber sheet that constitutes the non-skin-facing layer to create a two-layer structure. [Examples]
[0104] The following examples illustrate this disclosure, but this disclosure is not limited to these examples. [Manufacturing Example 1] Laminated web No. 1 with the following composition was prepared. In laminated web No. 1, the skin-side layer web No. 1 and the non-skin-side layer web No. 1 were laminated in that order. [Skin-side web] Using a carding machine, a skin-side web No. 1 (basis weight: 15 g / m²) containing 100% by mass of polyethylene terephthalate (PET) fiber as a synthetic fiber (single fiber, synthetic fiber surface coated with a durable hydrophilic oil agent, average fiber length: 51 mm, fineness: 1.6 dtex, hereinafter referred to as "durable hydrophilic PET fiber") is created. 2 I prepared ).
[0105] [Non-skin layer web] Using a carding machine, a non-skin side layer web No. 1 (basis weight: 15g / m²) containing 100% by mass of rayon fibers (average fiber length: 40mm, fineness: 1.7dtex, hereinafter referred to as "rayon fibers") as a water-retaining fiber was created. 2 I prepared ).
[0106] Nonwoven fabric No. 1 (spunlace nonwoven fabric, SL) was formed by performing a water jet entanglement treatment step and a drying step on laminated web No. 1. In the water jet entanglement step, while conveying laminated web No. 1, water jet treatment was performed from the non-skin side of laminated web No. 1, and then from the skin side of laminated web No. 1. Figure 1 shows a cross-sectional photograph (magnification: 40x) of a cross-section of nonwoven fabric No. 1 in which rayon fibers were colored with Congo Red. In Figure 1, the upper part is the skin-facing layer, and the lower part is the non-skin-facing layer. From Figure 1, it can be seen that the skin-facing layer has a predetermined entanglement structure.
[0107] [Manufacturing Example 2] Using a carding machine, a skin-side web No. 2 (basis weight: 15 g / m²) containing 60% by mass of the above-mentioned durable hydrophilic PET fiber and 40% by mass of polyethylene terephthalate (PET) fiber as a synthetic fiber (single fiber, synthetic fiber surface coated with an initial hydrophilic oil agent, average fiber length: 51 mm, hereinafter referred to as "initial hydrophilic PET fiber") is created. 2 I prepared ). Laminated web No. 2 and nonwoven fabric No. 2 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that skin-side layer web No. 1 was changed to skin-side layer web No. 2.
[0108] [Manufacturing Example 3] Using a card machine, the skin-side layer web No. 3 (basis weight: 15g / m²) containing 100% by mass of the initial hydrophilic PET was processed. 2 I prepared ). Laminated web No. 3 and nonwoven fabric No. 3 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that skin-side layer web No. 1 was changed to skin-side layer web No. 3.
[0109] [Manufacturing Example 4] Using a carding machine, a non-skin side layer web No. 4 (basis weight: 30g / m²) containing 100% by mass of the above rayon fibers was produced. 2 I prepared ). Laminated web No. 4 and nonwoven fabric No. 4 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that skin-side web No. 1 was not used and non-skin-side web No. 1 was changed to non-skin-side web No. 4.
[0110] [Manufacturing Example 5] Using a card machine, the skin-side layer web No. 5 (basis weight: 9g / m²) containing 100% by mass of the above-mentioned initial hydrophilic PET was processed. 2 I prepared ). Using a carding machine, a non-skin side layer web No. 5 (basis weight: 21 g / m²) containing 100% by mass of the above rayon fibers was produced. 2 I prepared ). Laminated web No. 5 and nonwoven fabric No. 5 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that skin-side web No. 1 was changed to skin-side web No. 5 and non-skin-side web No. 1 was changed to non-skin-side web No. 5.
[0111] [Manufacturing Example 6] Using a card machine, the skin-side layer web No. 6 (basis weight: 21 g / m²) containing 100% by mass of the initial hydrophilic PET was processed. 2 I prepared ). Using a carding machine, a non-skin side layer web No. 6 (basis weight: 9g / m²) containing 100% by mass of the above rayon fibers was produced. 2 I prepared ). Laminated web No. 6 and nonwoven fabric No. 6 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that skin-side web No. 1 was changed to skin-side web No. 6 and non-skin-side web No. 1 was changed to non-skin-side web No. 6.
[0112] [Manufacturing Example 7] Using a card machine, the skin-side layer web No. 7 (basis weight: 30g / m²) containing 100% by mass of the initial hydrophilic PET was processed. 2 I prepared ). Laminated web No. 7 and nonwoven fabric No. 7 (spunlace nonwoven fabric, SL) were formed in the same manner as in Manufacturing Example 1, except that skin-side web No. 1 was changed to skin-side web No. 7 and non-skin-side web No. 1 was not used.
[0113] [Manufacturing Example 8] Air-through nonwoven fabric (AT) (Basis weight: 30g / m²) 2 A core-sheath fiber coated with a durable hydrophilic oil agent (core: polyester, sheath: polyethylene) was prepared and designated as nonwoven fabric No. 8.
[0114] [Example 1] The artificial soft stool adhesion test specified below was performed on nonwoven fabrics No. 1 to No. 8. The results are shown in Table 1. In Table 1, "Durability / Initial" represents the mass ratio of durable hydrophilic PET fibers to initial hydrophilic PET fibers. [Artificial soft stool adhesion test] (1) Prepare a constant temperature and humidity chamber with a temperature of 23℃±2℃ and a relative humidity of 50±5%RH, along with artificial leather (Ideatex Japan Co., Ltd., PBZ13001, size: 100mm x 100mm), an acrylic plate (size: 100mm x 100mm), and a weight (mass: 2kg, base (square) size: 100mm x 100mm) to use as a counterweight. Measure the mass of the artificial leather before testing: m²(g).
[0115] (2) Mix 80.0 parts by mass of deionized water, 0.7 parts by mass of sodium chloride, 10.7 parts by mass of glycerin, 1.4 parts by mass of CMC sodium, 0.04 parts by mass of Triton X-100, 0.01 parts by mass of Red No. 102, and 7.1 parts by mass of powdered cellulose to prepare a simulated soft stool. Dilute the prepared simulated soft stool with deionized water to adjust its viscosity to 400 mPa·s. The viscosity is measured using a TVB10 viscometer (manufactured by Toki Sangyo Co., Ltd.). (3) Peel off the top sheet of a commercially available Moony Natural newborn diaper, place the nonwoven fabric on top to create a simple absorbent item, and attach the simple absorbent item in an unfolded state to a hook tape board (a 500mm x 300mm cardboard box with hook-and-loop fasteners attached to the entire surface to secure the nonwoven fabric).
[0116] (4) Using a Terumo syringe 50 mL (needleless, side opening) manufactured by Terumo Corporation, draw up 5.0 mL of simulated soft stool and drop it onto the top sheet at a drop point located 20 cm behind the longitudinal center and width center of the simple absorbent material. Three seconds after dropping, place the artificial skin, acrylic plate, and weight on top of the drop point in that order. The artificial skin, acrylic plate, and weight should be placed so that their centers coincide with the drop point. (5) One minute after placing the weight, remove the weight, acrylic plate, and artificial skin from the absorbent material, measure the post-test mass of the artificial skin: m3 (g), and calculate the amount of soft stool adhering to the artificial skin: A (g) using the following formula: A(g) = m3 - m2 It is calculated from this. (6) The amount of loose stool attached: A(g) was measured a total of 10 times using different absorbent materials and new artificial skin, and the average value was adopted.
[0117] [Table 1]
[0118] Table 1 shows that nonwoven fabrics No. 1 to No. 4, which are spunlace nonwoven fabrics, exhibit less loose stool adhesion and superior resistance to loose stool adhesion compared to nonwoven fabric No. 8, which is an air-through nonwoven fabric. Furthermore, a comparison of nonwoven fabrics No. 1 to No. 3 shows that superior resistance to loose stool adhesion is maintained even when the ratio of durable water-resistant PET and initial hydrophilic PET changes. Additionally, a comparison of nonwoven fabrics No. 1 and No. 4 to No. 7 shows that resistance to loose stool adhesion deteriorates as the proportion of the non-skin side layer decreases.
[0119] [Manufacturing Example 9] Laminated web No. 9 with the following composition was prepared. In laminated web No. 9, the skin-side layer web No. 9 and the non-skin-side layer web No. 9 were laminated in that order. [Skin-side web] Using a carding machine, a skin-side layer web No. 9 (basis weight: 15 g / m²) containing 80% by mass of the durable hydrophilic PET fiber and 20% by mass of the initial hydrophilic PET fiber was created. 2 I prepared ).
[0120] [Non-skin layer web] Using a carding machine, a non-skin side layer web No. 9 (basis weight: 15 g / m²) containing 100% by mass of the above rayon fibers was produced. 2 I prepared ).
[0121] Laminated web No. 9 and nonwoven fabric No. 9 (SL) were formed by performing a water entanglement treatment step and a drying step on laminated web No. 9 under the same conditions as in Manufacturing Example 1.
[0122] [Manufacturing Example 10] Using a carding machine, a skin-side layer web No. 10 (basis weight: 15 g / m²) containing 60% by mass of the durable hydrophilic PET fiber and 40% by mass of the initial hydrophilic PET fiber was created. 2 I prepared ). Laminated web No. 10 and nonwoven fabric No. 10 (SL) were formed in the same manner as in manufacturing example 9, except that skin-side layer web No. 9 was changed to skin-side layer web No. 10.
[0123] [Example 2] Nonwoven fabrics No. 1, No. 3-7, No. 9, and No. 10 were subjected to a 45° incline artificial urine absorption test. The results are shown in Table 2. In Table 2, "Durability / Initial" represents the mass ratio of durable hydrophilic PET fibers to initial hydrophilic PET fibers. For nonwoven fabrics No. 1, No. 9, and No. 10, the maximum elongation (%) in the MD direction and the maximum elongation (%) in the CD direction were measured. The results are shown in Table 2. For nonwoven fabrics No. 3 to No. 5, the strength at 5% elongation in the MD direction and the Klem water absorption were measured. The results are shown in Table 2.
[0124] [Table 2]
[0125] Table 2 shows that nonwoven fabric No. 1 containing 100% by mass of durable hydrophilic PET fibers as synthetic fibers, and nonwoven fabric No. 9 containing 80% by mass of durable hydrophilic PET fibers as synthetic fibers, have shorter surface flow distances compared to nonwoven fabric No. 10 containing 60% by mass of durable hydrophilic PET fibers as synthetic fibers, and also compared to nonwoven fabrics No. 3, No. 4, No. 6, and No. 7 containing 100% of initial hydrophilic PET fibers as synthetic fibers. A comparison of nonwoven fabrics No. 1 to No. 3 reveals that as the proportion of durable hydrophilic PET fibers as synthetic fibers increases, the maximum elongation of the nonwoven fabric increases, and thus the strength of the nonwoven fabric also increases.
[0126] [Example 3] Rewet tests were performed on nonwoven fabrics No. 1, No. 4 to No. 8. The results are shown in Table 3.
[0127] [Table 3]
[0128] Table 3 shows that the rewetting properties are excellent when the mass ratio of PET fibers as synthetic fibers to rayon fibers as water-retaining fibers is within a predetermined range. Regarding the rewetting test, it is believed that there is no difference in the results between durable hydrophilic PET fibers and initially hydrophilic PET fibers.
Claims
1. A spunlace nonwoven fabric for use as a top sheet in absorbent articles, The spunlace nonwoven fabric comprises a skin-facing layer containing synthetic fibers that constitutes the skin-contacting surface, and a non-skin-facing layer adjacent to the skin-facing layer that contains water-retaining fibers. The aforementioned synthetic fibers and water-retaining fibers are not heat-fused together. The spunlace nonwoven fabric exhibits a maximum elongation of 10-70% in the transport direction during manufacturing in tensile tests. The spunlace nonwoven fabric has a surface flow distance of 110 mm or less in a 45° inclined artificial urine absorption test. The spunlace nonwoven fabric characterized by the above.
2. The spunlace nonwoven fabric according to claim 1, wherein the spunlace nonwoven fabric has a Klem water absorption of 30 to 170 mm.
3. The spunlace nonwoven fabric described above has a rewetting rate of 20% by mass or less in a rewetting test, as described in claim 1.
4. The spunlace nonwoven fabric according to claim 1, wherein the spunlace nonwoven fabric has a tensile strength of 1.10 to 4.25 N / 25 mm in the transport direction during manufacturing, as determined in the tensile test.
5. The spunlace nonwoven fabric according to claim 1, wherein the spunlace nonwoven fabric contains the synthetic fiber and the water-retaining fiber in a mass ratio of 40 to 80:60 to 20 in a total of 100 parts by mass of the synthetic fiber and the water-retaining fiber.
6. The aforementioned spunlace nonwoven fabric has a density of 25 to 70 g / m². 2 A spunlace nonwoven fabric according to claim 5, having the basis weight.
7. The spunlace nonwoven fabric according to claim 1, wherein the synthetic fibers have an average fiber length of 30 to 60 mm, and the water-retaining fibers have an average fiber length of 30 to 60 mm.
8. The spunlace nonwoven fabric according to claim 1, wherein the non-skin-facing layer has a higher fiber density than the skin-facing layer.
9. The spunlace nonwoven fabric according to claim 1, wherein the synthetic fiber contains a durable hydrophilic oil agent.
10. The spunlace nonwoven fabric according to claim 1, wherein the synthetic fiber is polyethylene terephthalate fiber and the water-retaining fiber is rayon fiber.
11. The spunlace nonwoven fabric according to claim 1, wherein at least one of the synthetic fibers and the water-retaining fibers is not bonded.
12. The spunlace nonwoven fabric according to claim 1, wherein the spunlace nonwoven fabric is not heat-sealed or bonded.
13. The spunlace nonwoven fabric according to claim 1, wherein the absorbent article is an absorbent article for absorbing loose stool or menstrual blood.
Citation Information