Method for manufacturing cooling components

Thermal diffusion bonding of cooling members for heating elements simplifies manufacturing and enhances cooling performance by reducing thermal resistance and manufacturing costs, addressing the challenges of complex processes and reduced performance in existing methods.

JP2026182637APending Publication Date: 2026-11-19TAIHO KOGYO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2025079024
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2025-05-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing methods for manufacturing cooling members for heating elements, such as electronic components, are costly due to complex work processes and reduced cooling performance due to the use of joining materials that act as thermal resistance.

Method used

A method involving thermal diffusion bonding is used to join a flow path forming member, a heat sink, and a heat conductive member, with specific ratios and shapes of joint surfaces and thicknesses to simplify the manufacturing process and improve cooling performance.

Benefits of technology

The method allows for inexpensive manufacturing with improved cooling performance by reducing thermal resistance and simplifying the joining process, while enabling the use of dissimilar metals and maintaining the structural integrity of the cooling component.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182637000001_ABST
    Figure 2026182637000001_ABST
Patent Text Reader

Abstract

To provide a method for manufacturing a cooling component that can be produced inexpensively and has improved cooling performance. [Solution] A method for manufacturing a cooling member 1 comprising: a water jacket 10 that forms a fluid flow path P with a bottom 11 and side walls 12 erected on the bottom 11; a heat sink 20 joined to the side walls 12, separating the flow path P from the outside of the water jacket 10, and having a plurality of fins 22 on the flow path P side; and a copper spreader 30 joined to an exposed surface 21a of the heat sink 20 that is exposed on the outside side of the water jacket 10, and in contact with an electronic component E (heating element), wherein the method comprises a joining step (step S3 in Figure 2) in which the water jacket 10, the heat sink 20, and the copper spreader 30 are joined using thermal diffusion bonding.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to a technique for a method of manufacturing a cooling member that cools a heating element such as an electronic component.

Background Art

[0002] Conventionally, techniques for methods of manufacturing cooling members that cool heating elements such as electronic components are publicly known. For example, such a technique is described in Patent Document 1.

[0003] Patent Document 1 discloses a water jacket (cooler) that forms a fluid flow path with a bottom portion and side walls erected on the bottom portion, and a heat sink (cooling fin base) that is joined to the side walls and has a plurality of fins formed on the flow path side, and discloses a water jacket type heat sink (cooling member) on which a heating element (power semiconductor device) is mounted on the surface of the heat sink opposite to the fins. Such a water jacket type heat sink can cool the heating element (power semiconductor device). Further, in such a water jacket type heat sink, a technique of providing a heat spreader between the heat sink and the heating element is known to improve heat dissipation performance.

[0004] Here, in the configuration described in Patent Document 1, the water jacket (cooler) and the heat sink (cooling fin base) are metal-joined by a joining material, and a brazing material such as solder or a sintered material containing metal particles is used as the joining material.

[0005] In this way, when separate metal materials (for example, the water jacket and the heat sink as described above, or the heat spreader and the heat sink) are joined by a joining material, the work process becomes complicated, which may increase the manufacturing cost of the cooling member. In addition, since the joining material acts as resistance to heat transfer, the cooling performance of the cooling member may be reduced.

Prior Art Documents

Patent Documents

[0006] [Patent Document 1] Japanese Patent Publication No. 2017-5181 [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] This invention was made in view of the above circumstances, and the problem it aims to solve is to provide a method for manufacturing a cooling component that can be manufactured inexpensively and has improved cooling performance. [Means for solving the problem]

[0008] The problems that this invention aims to solve are as described above, and the means for solving these problems will now be explained.

[0009] That is, claim 1 is a method for manufacturing a cooling member comprising: a flow path forming member that forms a fluid flow path by a bottom and a side wall erected on the bottom; a heat sink joined to the side wall, separating the flow path from the outside of the flow path forming member, and having a plurality of fins on the flow path side; and a heat conductive member joined to an exposed portion of the heat sink that is exposed on the outside side of the flow path forming member, and in contact with a heating element, wherein the method comprises a joining step of joining the flow path forming member, the heat sink, and the heat conductive member using thermal diffusion bonding.

[0010] In claim 2, the ratio of the total area A of the joint surfaces between the heat conductive member and the heat sink, the total area B of the joint surfaces between the heat sink and the side wall, and the total area C of the joint surfaces between the fin and the bottom is A:B:C = 1:0.5 to 5:0.5 to 5.

[0011] In claim 3, the ratio of the total area A to the total area C is A:C = 1:0.5 to 1.

[0012] In claim 4, the ratio of the thicknesses t1, t2, and t3 in the vertical direction of the side wall of the heat conductive member, the portion of the heat sink excluding the fins, and the bottom portion is t1:t2:t3 = 1:1 to 3:1 to 10.

[0013] In claim 5, the left-right width d of the side wall is set to 1 to 20 [mm].

[0014] In claim 6, the joint between the fin and the bottom is formed to have an R shape. [Effects of the Invention]

[0015] The present invention provides the following effects:

[0016] Claim 1 allows for inexpensive manufacturing and improved cooling performance.

[0017] In claim 2, the flow path forming member, the heat sink, and the heat conducting member can be easily joined together.

[0018] Claim 3 makes it easier to join the flow path forming member, the heat sink, and the heat conducting member.

[0019] Claim 4 allows for further improvement of the cooling performance of the cooling element.

[0020] Claim 5 allows for greater freedom in the shape of the cooling member.

[0021] Claim 6 allows for improved strength of the joint between the fin and the bottom. [Brief explanation of the drawing]

[0022] [Figure 1] A front cross-sectional view showing a cooling member manufactured by a method for manufacturing a cooling member according to one embodiment of the present invention. [Figure 2]A flowchart showing each step of the method for manufacturing a cooling member according to an embodiment of the present invention. [Figure 3] (a) A front cross-sectional view showing the water jacket and the heat sink after the first contact step is performed. (b) A front cross-sectional view showing the water jacket, the heat sink and the copper spread after the second contact step is performed. [Figure 4] (a) A front cross-sectional view showing a state where the copper spread and the heat sink, and the side wall of the water jacket and the heat sink are joined in the joining step. (b) A front cross-sectional view showing a state where the bottom of the water jacket and the fins of the heat sink are further joined in the joining step.

[0023] In the following description, the directions indicated by arrow U, arrow D, arrow L and arrow R in the drawings are defined as the upward direction, downward direction, left direction and right direction, respectively.

[0024] In the following, the outline of the configuration of the cooling member 1 according to the first embodiment of the present invention will be described with reference to FIG. 1. The cooling member 1 is a water jacket type heat sink that cools a heating element by circulating a fluid. The heating element is, for example, an electronic component. In the present embodiment, the cooling member 1 is formed so as to cool the electronic component E by circulating cooling water.

[0025] FIG. 1 is a cross-sectional view showing the cooling member 1, showing a cross section perpendicular to the circulation direction of the cooling water. In the illustrated example, the cooling member 1 is shown such that the circulation direction of the cooling water is the depth direction of the drawing sheet. Further, in the illustrated example, the left direction (left direction of the drawing sheet) when viewed in the circulation direction of the cooling water is shown as the left direction, and the right direction (right direction of the drawing sheet) when viewed in the circulation direction of the cooling water is shown as the right direction.

[0026] The cooling member 1 mainly includes a water jacket 10, a heat sink 20, and a copper spreader 30.

[0027] The water jacket 10 forms a flow path P for the cooling water. The water jacket 10 is formed to extend along the direction of flow of the cooling water. The water jacket 10 is made of aluminum. The water jacket 10 has a bottom 11 and side walls 12.

[0028] The bottom portion 11 constitutes the lower part of the water jacket 10. The bottom portion 11 is formed in a plate shape with its plate surface oriented vertically.

[0029] The side walls 12 are formed to be erected at the left and right ends of the bottom portion 11. The side walls 12 are formed in a rectangular shape in a front cross-sectional view. The left-right width d of each side wall 12 (width of the side wall 12 in the left-right direction when viewed in the direction of extension of the flow path P (direction of cooling water flow)) is preferably set to 1 to 20 [mm].

[0030] The water jacket 10, configured in this way, forms a fluid flow path P with its bottom portion 11 and side walls 12.

[0031] The heat sink 20 dissipates heat from the electronic component E. The heat sink 20, like the water jacket 10, is formed to extend along the direction of the cooling water flow. The heat sink 20 is made of aluminum. In this specification, the term "aluminum" includes aluminum and aluminum alloys. The heat sink 20 comprises a body 21 and fins 22.

[0032] The main body portion 21 constitutes the main structure of the heat sink 20. The main body portion 21 is formed in a plate shape with its plate surface oriented vertically. The length of the main body portion 21 in the left-right direction is formed to be approximately the same as the length of the water jacket 10 in the left-right direction. The main body portion 21 is provided so that its lower surface is in contact with the upper surface of the side wall 12 of the water jacket 10, and is joined to the side wall 12 of the water jacket 10 using thermal diffusion bonding. By being joined to the side wall 12 of the water jacket 10, the main body portion 21 separates the flow path P from the outside of the water jacket 10.

[0033] An exposed surface 21a is formed on the main body portion 21. The exposed surface 21a is the upper surface of the main body portion 21 and is formed to be exposed to the outside side of the water jacket 10.

[0034] The fins 22 are formed to extend from the lower surface of the main body 21 toward the flow path P side (downward). Multiple fins 22 are provided at intervals in the left-right direction. The tips of the fins 22 are joined to the bottom 11 of the water jacket 10 using thermal diffusion bonding. The fins 22 configured in this way increase the surface area of ​​the heat sink 20, thereby improving the heat dissipation effect.

[0035] The copper spreader 30 is a heat dissipation spreader that dissipates heat from the electronic component E. The copper spreader 30 is formed in a plate shape with its plate surface oriented vertically. The copper spreader 30 is made of copper. In this specification, the term "copper" includes copper and copper alloys. The copper spreader 30 is provided so that its lower surface is in contact with the exposed surface 21a of the heat sink 20, and is joined to the exposed surface 21a using thermal diffusion bonding. The copper spreader 30 is positioned in the left-right center of the main body 21 of the heat sink 20.

[0036] As described above, the water jacket 10, heat sink 20, and copper spreader 30 are not all made of the same metal material, but are made of two different metal materials: aluminum and copper. Furthermore, the water jacket 10, heat sink 20, and copper spreader 30 are joined together using thermal diffusion bonding.

[0037] Next, a method for manufacturing the cooling member 1 according to one embodiment of the present invention will be described using Figures 2 to 4. Note that the joints of each member (the first joint 40, the second joint 50, and the third joint 60, which will be described later) do not actually have thickness, but are shown as having thickness in order to clearly indicate the position of each joint.

[0038] First, the first contact step S1 shown in Figure 2 is performed. The first contact step is the process of bringing the heat sink 20 into contact with the side wall 12 of the water jacket 10 with the multiple fins 22 spaced apart from the bottom 11 of the water jacket 10. As shown in Figure 3(a), in the first contact step, the heat sink 20 is placed on the side wall 12 of the water jacket 10 with the surface on which the fins 22 are provided facing downwards. The component dimensions (mm) of the water jacket 10 and heat sink 20 before joining are set to satisfy the following equation 1.

[0039] ab>X1...(Formula 1)

[0040] In Equation 1, "a" represents the height (length in the vertical direction) [mm] of the side wall 12 of the water jacket 10 before joining from the bottom 11. "b" represents the height (length of the fin 22 in the vertical direction of the side wall 12) [mm] of the fin 22 of the heat sink 20 before joining from the main body 21. "X1" is a predetermined positive value, preferably greater than 0 [mm] and set to any value less than or equal to 0.1 [mm].

[0041] In this way, before joining, the height a of the side wall 12 is set to be greater than the height b of the fin 22 (satisfying equation 1), so that, as shown in Figure 3(a), when the heat sink 20 is in contact with the side wall 12, the fin 22 and the bottom 11 do not come into contact, and there is a gap between the fin 22 and the bottom 11. The value of "ab" is set to a value that satisfies the conditions of equation 1 and allows the fin 22 and the bottom 11 to be joined in the joining process described later.

[0042] Next, the second contact step of step S2 is performed. The second contact step is the step of bringing the copper spreader 30 into contact with the exposed surface 21a of the heat sink 20. As shown in Figure 3(b), in the second contact step, the copper spreader 30 is placed in the center of the exposed surface 21a of the heat sink 20. Note that the second contact step (step S2) may be performed before the first contact step (step S1), or it may be performed simultaneously with the first contact step (step S1).

[0043] Here, the thicknesses t1, t2, and t3 of the copper spreader 30, the main body 21 of the heat sink 20, and the bottom 11 of the water jacket 10 (thickness in the vertical direction of the side wall 12) are set to satisfy the following equation 2.

[0044] t1:t2:t3=1:1~3:1~10...(Formula 2)

[0045] Next, the joining process of step S3 is performed. The joining process is a process in which the water jacket 10, heat sink 20, and copper spreader 30 are joined using thermal diffusion bonding after the first contact process (step S1) and the second contact process (step S2) have been performed. In the joining process, the water jacket 10, heat sink 20, and copper spreader 30, which were positioned in the first contact process (step S1) and the second contact process (step S2), are heated and pressurized to perform thermal diffusion bonding simultaneously. More specifically, in thermal diffusion bonding, a load is applied to the joining surface while heating it, so that the joining surfaces are in close contact. The heat and load applied are set to appropriate values ​​depending on the material and size of each component.

[0046] As a result, as shown in Figure 4(a), the lower surface of the copper spreader 30 and the exposed surface 21a of the heat sink 20 are thermally diffusively bonded. Hereinafter, the joint between the lower surface of the copper spreader 30 and the exposed surface 21a of the heat sink 20 will be referred to as the first joint 40.

[0047] Furthermore, as shown in Figure 4(a), the lower surface of the heat sink 20 and the upper surface of the side wall 12 of the water jacket 10 are thermally diffusively bonded. Hereinafter, the joint between the lower surface of the heat sink 20 and the upper surface of each side wall 12 of the water jacket 10 will be referred to as the second joint 50.

[0048] As described above, before the formation of the second joint 50, the height a of the side wall 12 is set to be greater than the height b of the fin 22, and the fin 22 and the bottom 11 are separated. On the other hand, as the second joint 50 is formed, the lower surface of the heat sink 20 and the upper surface of the side wall 12 of the water jacket 10 deform. As a result, the lower surface of the fin 22 of the heat sink 20 and the upper surface of the bottom 11 of the water jacket 10 come into contact.

[0049] Therefore, as the fins 22 of the heat sink 20 and the bottom 11 of the water jacket 10 are heated and pressurized, the lower surface of the fins 22 and the upper surface of the bottom 11 are thermally diffusively bonded, as shown in Figure 4(b). Hereinafter, the joint between the lower surface of each fin 22 of the heat sink 20 and the upper surface of the bottom 11 of the water jacket 10 will be referred to as the third joint 60.

[0050] In the cooling member 1 configured in this way, the ratio of the area of ​​the joints of each member is set to satisfy the following equation 3.

[0051] A:B:C=1:0.5~5:0.5~5...(Formula 3)

[0052] In Equation 3, "A" represents the area of ​​the first joint 40 (the joint surface between the copper spreader 30 and the main body 21 of the heat sink 20). If multiple first joints 40 are formed, "A" represents the sum of the areas of each first joint 40 (total area). "B" represents the sum of the areas of each second joint 50 (the joint surface between the main body 21 of the heat sink 20 and each side wall 12 of the water jacket 10). "C" represents the sum of the areas of each third joint 60 (the joint surface between each fin 22 of the heat sink 20 and the bottom 11 of the water jacket 10).

[0053] More preferably, the ratio between the total area A of the first joint portion 40 and the total area C of the third joint portion 60 is set so as to satisfy the following Formula 4.

[0054] A:C=1:0.5~1···(Formula 4)

[0055] Further, more preferably, the total area C of the third joint portion 60 and the total area B of the second joint portion 50 are set so as to satisfy the following Formula 5.

[0056] (C / 2)<B<(C×2)···(Formula 5)

[0057] In this manner, the copper spreader 30 and the main body portion 21 of the heat sink 20, the main body portion 21 of the heat sink 20 and the side wall 12 of the water jacket 10, and the fins 22 of the heat sink 20 and the bottom portion 11 of the water jacket 10 are joined using thermal diffusion bonding, whereby the cooling member 1 shown in Figure 1 can be manufactured.

[0058] In the cooling member 1 manufactured in this manner, the joint portion (orthogonal portion) between the fin 22 and the bottom portion 11 is formed to have an R shape (see the partially enlarged view of Figure 1). Thereby, the joining strength between the fins 22 and the bottom portion 11 can be improved.

[0059] As described above, in the method for manufacturing the cooling member 1 according to the present embodiment, even when the number of components to be joined (number of joint locations) is relatively large, each joint location can be joined at once by thermal diffusion bonding, so that the joining work process can be simplified. In addition, the cooling member 1 can be manufactured at lower cost than when brazing, welding, or adhesion is employed as the joining method. Further, compared with brazing, welding, and adhesion, the resistance to heat transfer can be reduced, and the cooling performance can be improved.

[0060] Furthermore, since the main body portion 21 of the heat sink 20 and the side wall 12 of the water jacket 10 are bonded using thermal diffusion bonding, the left-right width d of the side wall 12 can be made smaller (for example, 1 to 20 [mm]) compared to the case where the main body portion 21 and the side wall 12 are bolted together. Therefore, the degree of freedom in the shape of the cooling member 1 can be improved. In addition, a large width of the flow path P can be secured, which in turn can improve the cooling performance.

[0061] Furthermore, in the method for manufacturing the cooling member 1 according to the present embodiment, the contact step (the first contact step and the second contact step) is completed in a state where the heat sink 20 is in contact with the side wall 12 of the water jacket 10, and the fins 22 are separated from the bottom portion 11 of the water jacket 10. After that, the water jacket 10, the heat sink 20, and the copper spreader 30 arranged in the contact step are heated and pressurized to start thermal diffusion bonding. The side wall 12 of the water jacket 10 shrinks appropriately under pressure, and the previously separated fins 22 come into contact with the bottom portion 11 of the water jacket 10. For this reason, application of excessive force to the fins 22 during bonding is suppressed, and the fins can be brought into contact and subjected to thermal diffusion bonding, which in turn can suppress deformation or damage of the fins 22.

[0062] Furthermore, in the method for manufacturing the cooling member 1 according to the present embodiment, since thermal diffusion bonding is used for bonding the respective members, even dissimilar metals can be easily bonded. In addition, during the bonding process, the water jacket 10 and the heat sink 20 come into contact not only at the side wall 12 and the main body portion 21 but also at the bottom portion 11 and the fins 22. For this reason, the occurrence of shape collapse of the entire cooling member 1 due to heating and pressurization can be suppressed. Furthermore, by adjusting the total area C of the third bonding portion 60 and the total area B of the second bonding portion 50 so as to satisfy "(C / 2) < B < (C×2)", the occurrence of shape collapse of the entire cooling member 1 due to heating and pressurization can be further suppressed.

[0063] Furthermore, the thicknesses t1, t2, and t3 of the copper spreader 30, the main body 21 of the heatsink 20, and the bottom 11 of the water jacket 10 are set to t1:t2:t3 = 1:1 to 3:1 to 10. By setting the ratio of each thickness t1, t2, and t3 in this way, the cooling performance can be improved.

[0064] Furthermore, the ratio of the total area A of the first joint 40, the total area B of the second joint 50, and the total area C of the third joint 60 is set to A:B:C = 1:0.5~5:0.5~5, preferably A:C = 1:0.5~1. By setting the ratio of the total areas A, B, and C in this way, it is possible to make it easier to join the water jacket 10, the heat sink 20, and the copper spreader 30. In addition, it is possible to further suppress the occurrence of deformation of the entire cooling member 1 due to heating and pressurization.

[0065] As described above, the method for manufacturing the cooling member 1 according to this embodiment is A water jacket 10 (flow channel forming member) that forms a fluid flow channel P with a bottom portion 11 and side walls 12 erected on the bottom portion 11, A heat sink 20 is joined to the side wall 12, demarcating the flow path P from the outside of the water jacket 10, and having a plurality of fins 22 on the flow path P side, A copper spreader 30 (heat conductive member) is bonded to the exposed surface 21a (exposed portion) of the heat sink 20 that is exposed to the outside of the water jacket 10, and the electronic component E (heating element) is in contact with it. A method for manufacturing a cooling member 1 comprising the following: The system includes a bonding step (step S3 in Figure 2) in which the water jacket 10, the heat sink 20, and the copper spreader 30 are bonded together using thermal diffusion bonding.

[0066] By configuring the components in this way, the water jacket 10, heat sink 20, and copper spreader 30 are joined to each other by thermal diffusion bonding. This simplifies the manufacturing process compared to joining components using solder or other brazing materials, or sintered materials containing metal particles, thus reducing manufacturing costs. Furthermore, because the components are joined by thermal diffusion bonding, the resistance to heat transfer is reduced compared to joining components using the aforementioned materials. In other words, the cooling component 1 can be manufactured at a low cost, and its cooling performance can be improved.

[0067] Furthermore, the ratio of the total surface area A of the joint between the copper spreader 30 and the heat sink 20, the total surface area B of the joint between the heat sink 20 and the side wall 12, and the total surface area C of the joint between the fin 22 and the bottom 11 is A:B:C = 1:0.5~5:0.5~5.

[0068] This configuration makes it easier to join the water jacket 10, heat sink 20, and copper spreader 30. This simplifies the manufacturing process and, consequently, allows for the production of the cooling component 1 at a lower cost.

[0069] Furthermore, the ratio of the total area A to the total area C is A:C = 1:0.5 to 1.

[0070] This configuration makes it easier to join the water jacket 10, heat sink 20, and copper spreader 30. This simplifies the manufacturing process and, consequently, allows for the production of the cooling component 1 at a lower cost.

[0071] Furthermore, the ratio of the thicknesses t1, t2, and t3 of the side walls 12 in the vertical direction for the copper spreader 30, the main body 21 (the portion of the heat sink 20 excluding the fins 22), and the bottom 11 is t1:t2:t3 = 1:1 to 3:1 to 10.

[0072] By configuring it in this way, the cooling performance of the cooling component 1 can be further improved.

[0073] Furthermore, the width d of the side walls in the left-right direction when viewed in the direction of extension of the flow path P is 1 to 20 mm.

[0074] This configuration allows for greater flexibility in the shape of the cooling element 1.

[0075] Furthermore, the joint between the fin 22 and the bottom portion 11 (third joint portion 60) is formed to have an R shape.

[0076] This configuration improves the strength of the joint between the fin 22 and the bottom 11.

[0077] Although embodiments of the present invention have been described above, the present invention is not limited to the above configuration, and various modifications are possible within the scope of the invention as described in the claims.

[0078] For example, in this embodiment, the side wall 12 is provided on the water jacket 10, but it may also be provided on the heat sink 20.

[0079] Furthermore, in this embodiment, all fins 22 are in contact with and joined to the bottom 11, but it is also possible that only a portion of the fins 22 are in contact with and joined to the bottom 11.

[0080] Furthermore, the metal materials constituting the water jacket 10, heat sink 20, and copper spreader 30 are not limited to those of this embodiment and may be other metal materials. Also, the metal materials constituting the water jacket 10, heat sink 20, and copper spreader 30 may be three different types (i.e., each may be made of a different metal material). [Explanation of Symbols]

[0081] 1 Cooling component 10 Water Jackets 11 Bottom 12 Side wall 20 Heatsinks 21a Exposed surface 22 fins 30 Copper Spreaders

Claims

1. A flow path forming member that forms a fluid flow path with a bottom and side walls erected on the bottom, A heat sink is joined to the side wall, demarcating the flow path from the outside of the flow path forming member, and having a plurality of fins on the flow path side, A heat conductive member is joined to the exposed portion of the heat sink that is exposed on the outside side of the flow path forming member, and the heat generating element is in contact with it. A method for manufacturing a cooling member comprising: The invention comprises a joining process in which the flow channel forming member, the heat sink, and the heat conducting member are joined using thermal diffusion bonding. A method for manufacturing a cooling component.

2. The ratio of the total surface area A of the joint between the heat conductive member and the heat sink, the total surface area B of the joint between the heat sink and the side wall, and the total surface area C of the joint between the fin and the bottom is A:B:C = 1:0.5 to 5:0.5 to 5. A method for manufacturing a cooling member according to claim 1.

3. The ratio of the total area A to the total area C is A:C = 1:0.5 to 1. A method for manufacturing a cooling member according to claim 2.

4. The ratio of the thicknesses t1, t2, and t3 in the vertical direction of the side walls of the heat conductive member, the portion of the heat sink excluding the fins, and the bottom portion is t1:t2:t3 = 1:1 to 3:1 to 10. A method for manufacturing a cooling member according to claim 1.

5. The left-right width d of the aforementioned side wall is set to 1 to 20 [mm]. A method for manufacturing a cooling member according to any one of claims 1 to 4.

6. The joint between the fin and the bottom is formed to have an R shape. A method for manufacturing a cooling member according to any one of claims 1 to 4.

Citation Information

Patent Citations

  • Cooling device for power semiconductor device and method for manufacturing the same

    JP2017005181A