Cooling member and method for manufacturing a cooling member
The cooling member uses thermal diffusion bonding of copper and aluminum with optimized joint ratios and R-shaped joints to simplify manufacturing, enhance cooling performance, and reduce deformation, addressing the limitations of traditional methods.
Patent Information
- Application Number
- JP2025079025
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Existing cooling member manufacturing methods, such as brazing, welding, and adhesion, are complex and limit shape freedom, while thermal diffusion bonding risks shape distortion and requires multiple joining points.
A cooling member design using thermal diffusion bonding to join copper and aluminum materials, with specific area ratios and R-shaped joints, simplifying the manufacturing process and improving shape freedom.
The design allows for easy manufacturing, enhanced cooling performance, reduced deformation, and improved bonding strength, while enabling dissimilar metal bonding without excessive force application.
Smart Images

Figure 2026182638000001_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a technology of a cooling member that cools a heating element such as an electronic component, and a method for manufacturing the cooling member.
BACKGROUND ART
[0002] Conventionally, technologies for cooling members that cool heating elements such as electronic components and methods for manufacturing the cooling members are publicly known. For example, as described in Patent Document 1.
[0003] Patent Document 1 discloses a water jacket type heat sink that includes a water jacket (cooler) which forms a fluid flow path by a bottom portion and side walls erected on the bottom portion, and a heat sink (cooling fin base) which is joined to the side walls and has a plurality of fins formed on the flow path side, wherein a heating element (power semiconductor device) is mounted on the surface of the heat sink opposite to the fins. Such a water jacket type heat sink can cool the heating element (power semiconductor device).
[0004] Here, as a joining method for metal materials, brazing, welding, and adhesion are generally employed. In addition, a heat spreader may be provided between the heat sink and the heating element to improve heat dissipation performance. The heat spreader is joined to the heat sink. When the number of parts to be joined (the number of joining points) is relatively large in this way, joining methods such as brazing, welding, and adhesion have a problem that the joining work process becomes complicated.
[0005] Further, in a water jacket type heat sink, the side wall of the water jacket and the heat sink may be joined by bolts. However, in the case of bolt joining, it is necessary to widen the width of the side wall to secure a space for fastening the bolts, which poses a problem that the degree of freedom in shape is limited.
[0006] Furthermore, thermal diffusion bonding, which involves heating and pressurizing the metal materials, is known as a method for joining metal materials. However, because thermal diffusion bonding involves heating and pressurizing the metal materials, the shape of the joined materials is more easily distorted during manufacturing compared to other methods. [Prior art documents] [Patent Documents]
[0007] [Patent Document 1] Japanese Patent Publication No. 2017-5181 [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] However, thermal diffusion bonding has the advantage of being able to join dissimilar metals. Furthermore, the inventors have found that if the fins of the heat sink are in contact with the bottom of the water jacket, the overall shape of the water jacket type heat sink is less likely to collapse even when heated and pressurized during thermal diffusion bonding.
[0009] This invention was made in view of the above circumstances, and the problem it aims to solve is to provide a cooling member and a method for manufacturing a cooling member that can be easily manufactured and have improved freedom of shape. [Means for solving the problem]
[0010] The problems that this invention aims to solve are as described above, and the means for solving these problems will now be explained.
[0011] In other words, claim 1 comprises a flow path forming member that forms a fluid flow path by a bottom and a side wall erected on the bottom; a heat sink joined to the side wall and separating the flow path from the outside of the flow path forming member; and a heat conductive member joined to an exposed portion of the heat sink that is exposed on the outside side of the flow path forming member and into contact with a heating element, wherein the heat sink has a plurality of fins that are in contact with the bottom on the flow path side, and the flow path forming member, the heat sink and the heat conductive member are made of at least two or more metal materials and are joined together using thermal diffusion bonding.
[0012] In claim 2, the at least two types of metallic materials include copper and aluminum.
[0013] In claim 3, the joint formed by thermal diffusion bonding includes a portion where copper and aluminum are joined, and a portion where aluminum and aluminum are joined.
[0014] In claim 4, the total area C of the joint surface between the fin and the bottom, and the total area B of the joint surface between the heat sink and the side wall are (C / 2) <B<(C×2)であるものである。
[0015] In claim 5, the joint between the fin and the bottom is formed to have an R shape.
[0016] In claim 6, a method for manufacturing a cooling member comprising: a flow path forming member that forms a fluid flow path by a bottom portion and a side wall erected on the bottom portion; a heat sink joined to the side wall, partitioning the flow path from the outside of the flow path forming member, and having a plurality of fins on the flow path side; and a heat conductive member joined to an exposed portion of the heat sink exposed to the outside of the flow path forming member and brought into contact with a heating element, wherein the flow path forming member, the heat sink, and the heat conductive member are each composed of at least two or more metallic materials, the method comprising a joining step of bringing the plurality of fins into contact with the bottom portion on the flow path side, and joining the flow path forming member, the heat sink, and the heat conductive member to one another using thermal diffusion bonding. [Effects of the Invention]
[0017] The present invention achieves the following effects as described below.
[0018] In claim 1, manufacturing can be performed easily, and the degree of freedom in shape can be improved.
[0019] In claim 2, cooling performance can be improved.
[0020] In claim 3, cooling performance can be improved.
[0021] In claim 4, shape deformation can be made less likely to occur.
[0022] In claim 5, the bonding strength between the fins and the bottom portion can be improved.
[0023] In claim 6, manufacturing can be performed easily, and the degree of freedom in shape can be improved. [Brief Description of the Drawings]
[0024] [Figure 1] A front cross-sectional view showing a cooling member according to an embodiment of the present invention. [Figure 2] A flowchart showing each step of a method for manufacturing a cooling member according to an embodiment of the present invention. [Figure 3] (a) A front cross-sectional view showing the water jacket and the heat sink after the first contact step is performed. (b) A front cross-sectional view showing the water jacket, the heat sink and the copper spreader after the second contact step is performed. [Figure 4] (a) A front cross-sectional view showing a state where the copper spreader and the heat sink, and the side wall of the water jacket and the heat sink are joined in the joining step. (b) A front cross-sectional view showing a state where the bottom of the water jacket and the fins of the heat sink are further joined in the joining step.
[0025] In the following description, the directions indicated by arrow U, arrow D, arrow L and arrow R in the drawings are defined as the upward direction, downward direction, left direction and right direction respectively for explanation.
[0026] In the following, the outline of the configuration of the cooling member 1 according to the first embodiment of the present invention will be described with reference to Figure 1. The cooling member 1 is a water jacket type heat sink that cools a heating element by circulating a fluid. The heating element is, for example, an electronic component. In the present embodiment, the cooling member 1 is formed so as to cool the electronic component E by circulating cooling water.
[0027] Figure 1 is a cross-sectional view showing the cooling member 1, showing a cross section perpendicular to the flow direction of the cooling water. In the illustrated example, the cooling member 1 is shown such that the flow direction of the cooling water is the depth direction of the drawing sheet. In addition, in the illustrated example, the left direction (left direction on the drawing sheet) when viewed in the flow direction of the cooling water is shown as the left direction, and the right direction (right direction on the drawing sheet) when viewed in the flow direction of the cooling water is shown as the right direction.
[0028] The cooling member 1 mainly includes a water jacket 10, a heat sink 20 and a copper spreader 30.
[0029] The water jacket 10 forms a flow path P for the cooling water. The water jacket 10 is formed to extend along the direction of flow of the cooling water. The water jacket 10 is made of aluminum. The water jacket 10 has a bottom 11 and side walls 12.
[0030] The bottom portion 11 constitutes the lower part of the water jacket 10. The bottom portion 11 is formed in a plate shape with its plate surface oriented vertically.
[0031] The side walls 12 are formed to be erected at the left and right ends of the bottom portion 11. The side walls 12 are formed in a rectangular shape in a front cross-sectional view. The left-right width d of each side wall 12 (width of the side wall 12 in the left-right direction when viewed in the direction of extension of the flow path P (direction of cooling water flow)) is preferably set to 1 to 20 [mm].
[0032] The water jacket 10, configured in this way, forms a fluid flow path P with its bottom portion 11 and side walls 12.
[0033] The heat sink 20 dissipates heat from the electronic component E. The heat sink 20, like the water jacket 10, is formed to extend along the direction of the cooling water flow. The heat sink 20 is made of aluminum. In this specification, the term "aluminum" includes aluminum and aluminum alloys. The heat sink 20 comprises a body 21 and fins 22.
[0034] The main body portion 21 constitutes the main structure of the heat sink 20. The main body portion 21 is formed in a plate shape with its plate surface oriented vertically. The length of the main body portion 21 in the left-right direction is formed to be approximately the same as the length of the water jacket 10 in the left-right direction. The main body portion 21 is provided so that its lower surface is in contact with the upper surface of the side wall 12 of the water jacket 10, and is joined to the side wall 12 of the water jacket 10 using thermal diffusion bonding. By being joined to the side wall 12 of the water jacket 10, the main body portion 21 separates the flow path P from the outside of the water jacket 10.
[0035] An exposed surface 21a is formed on the main body portion 21. The exposed surface 21a is the upper surface of the main body portion 21 and is formed to be exposed to the outside side of the water jacket 10.
[0036] The fins 22 are formed to extend from the lower surface of the main body 21 toward the flow path P side (downward). Multiple fins 22 are provided at intervals in the left-right direction. The tips of the fins 22 are joined to the bottom 11 of the water jacket 10 using thermal diffusion bonding. The fins 22 configured in this way increase the surface area of the heat sink 20, thereby improving the heat dissipation effect.
[0037] The copper spreader 30 is a heat dissipation spreader that dissipates heat from the electronic component E. The copper spreader 30 is formed in a plate shape with its plate surface oriented vertically. The copper spreader 30 is made of copper. In this specification, the term "copper" includes copper and copper alloys. The copper spreader 30 is provided so that its lower surface is in contact with the exposed surface 21a of the heat sink 20, and is joined to the exposed surface 21a using thermal diffusion bonding. The copper spreader 30 is positioned in the left-right center of the main body 21 of the heat sink 20.
[0038] As described above, the water jacket 10, heat sink 20, and copper spreader 30 are not all made of the same metal material, but are made of two different metal materials: aluminum and copper. Furthermore, the water jacket 10, heat sink 20, and copper spreader 30 are joined together using thermal diffusion bonding.
[0039] Next, a method for manufacturing the cooling member 1 according to one embodiment of the present invention will be described using Figures 2 to 4. Note that the joints of each member (the first joint 40, the second joint 50, and the third joint 60, which will be described later) do not actually have thickness, but are shown as having thickness in order to clearly indicate the position of each joint.
[0040] First, the first contact step S1 shown in Figure 2 is performed. The first contact step is the process of bringing the heat sink 20 into contact with the side wall 12 of the water jacket 10 with the multiple fins 22 spaced apart from the bottom 11 of the water jacket 10. As shown in Figure 3(a), in the first contact step, the heat sink 20 is placed on the side wall 12 of the water jacket 10 with the surface on which the fins 22 are provided facing downwards. The component dimensions (mm) of the water jacket 10 and heat sink 20 before joining are set to satisfy the following equation 1.
[0041] ab>X1...(Formula 1)
[0042] In Equation 1, "a" represents the height (length in the vertical direction) [mm] of the side wall 12 of the water jacket 10 before joining from the bottom 11. "b" represents the height (length of the fin 22 in the vertical direction of the side wall 12) [mm] of the fin 22 of the heat sink 20 before joining from the main body 21. "X1" is a predetermined positive value, preferably greater than 0 [mm] and set to any value less than or equal to 0.1 [mm].
[0043] In this way, before joining, the height a of the side wall 12 is set to be greater than the height b of the fin 22 (satisfying equation 1), so that, as shown in Figure 3(a), when the heat sink 20 is in contact with the side wall 12, the fin 22 and the bottom 11 do not come into contact, and there is a gap between the fin 22 and the bottom 11. The value of "ab" is set to a value that satisfies the conditions of equation 1 and allows the fin 22 and the bottom 11 to be joined in the joining process described later.
[0044] Next, the second contact step of step S2 is performed. The second contact step is the step of bringing the copper spreader 30 into contact with the exposed surface 21a of the heat sink 20. As shown in Figure 3(b), in the second contact step, the copper spreader 30 is placed in the center of the exposed surface 21a of the heat sink 20. Note that the second contact step (step S2) may be performed before the first contact step (step S1), or it may be performed simultaneously with the first contact step (step S1).
[0045] Here, the thicknesses t1, t2, and t3 of the copper spreader 30, the main body 21 of the heat sink 20, and the bottom 11 of the water jacket 10 (thickness in the vertical direction of the side wall 12) are set to satisfy the following equation 2.
[0046] t1:t2:t3=1:1~3:1~10...(Formula 2)
[0047] Next, the joining process of step S3 is performed. The joining process is a process in which the water jacket 10, heat sink 20, and copper spreader 30 are joined using thermal diffusion bonding after the first contact process (step S1) and the second contact process (step S2) have been performed. In the joining process, the water jacket 10, heat sink 20, and copper spreader 30, which were positioned in the first contact process (step S1) and the second contact process (step S2), are heated and pressurized to perform thermal diffusion bonding simultaneously. More specifically, in thermal diffusion bonding, a load is applied to the joining surface while heating it, so that the joining surfaces are in close contact. The heat and load applied are set to appropriate values depending on the material and size of each component.
[0048] As a result, as shown in Figure 4(a), the lower surface of the copper spreader 30 and the exposed surface 21a of the heat sink 20 are thermally diffusively bonded. Hereinafter, the joint between the lower surface of the copper spreader 30 and the exposed surface 21a of the heat sink 20 will be referred to as the first joint 40.
[0049] Furthermore, as shown in Figure 4(a), the lower surface of the heat sink 20 and the upper surface of the side wall 12 of the water jacket 10 are thermally diffusively bonded. Hereinafter, the joint between the lower surface of the heat sink 20 and the upper surface of each side wall 12 of the water jacket 10 will be referred to as the second joint 50.
[0050] As described above, before the formation of the second joint 50, the height a of the side wall 12 is set to be greater than the height b of the fin 22, and the fin 22 and the bottom 11 are separated. On the other hand, as the second joint 50 is formed, the lower surface of the heat sink 20 and the upper surface of the side wall 12 of the water jacket 10 deform. As a result, the lower surface of the fin 22 of the heat sink 20 and the upper surface of the bottom 11 of the water jacket 10 come into contact.
[0051] Therefore, as the fins 22 of the heat sink 20 and the bottom 11 of the water jacket 10 are heated and pressurized, the lower surface of the fins 22 and the upper surface of the bottom 11 are thermally diffusively bonded, as shown in Figure 4(b). Hereinafter, the joint between the lower surface of each fin 22 of the heat sink 20 and the upper surface of the bottom 11 of the water jacket 10 will be referred to as the third joint 60.
[0052] In the cooling member 1 configured in this way, the ratio of the area of the joints of each member is set to satisfy the following equation 3.
[0053] A:B:C=1:0.5~5:0.5~5...(Formula 3)
[0054] In Equation 3, "A" represents the area of the first joint 40 (the joint surface between the copper spreader 30 and the main body 21 of the heat sink 20). If multiple first joints 40 are formed, "A" represents the sum of the areas of each first joint 40 (total area). "B" represents the sum of the areas of each second joint 50 (the joint surface between the main body 21 of the heat sink 20 and each side wall 12 of the water jacket 10). "C" represents the sum of the areas of each third joint 60 (the joint surface between each fin 22 of the heat sink 20 and the bottom 11 of the water jacket 10).
[0055] More preferably, the ratio between the total area A of the first joint portion 40 and the total area C of the third joint portion 60 is set so as to satisfy the following Formula 4.
[0056] A:C=1:0.5~1···(Formula 4)
[0057] Further, more preferably, the total area C of the third joint portion 60 and the total area B of the second joint portion 50 are set so as to satisfy the following Formula 5.
[0058] (C / 2)<B<(C×2)···(Formula 5)
[0059] In this manner, the copper spreader 30 and the main body portion 21 of the heat sink 20, the main body portion 21 of the heat sink 20 and the side wall 12 of the water jacket 10, and the fin 22 of the heat sink 20 and the bottom portion 11 of the water jacket 10 are joined using thermal diffusion bonding, whereby the cooling member 1 shown in Figure 1 can be manufactured.
[0060] In the cooling member 1 manufactured in this manner, the joint portion (orthogonal portion) between the fin 22 and the bottom portion 11 is formed to have an R shape (see the partially enlarged view of Figure 1). Thereby, the bonding strength between the fin 22 and the bottom portion 11 can be improved.
[0061] As described above, in the method for manufacturing the cooling member 1 according to the present embodiment, even when the number of components to be joined (joint locations) is relatively large, each joint location can be joined at one time by thermal diffusion bonding, so that the joining work process can be simplified. In addition, the cooling member 1 can be manufactured at lower cost than in the case of employing brazing, welding, or adhesion as the joining method. Further, compared with brazing, welding, and adhesion, resistance to heat transfer can be reduced, and cooling performance can be improved.
[0062] Furthermore, since the main body portion 21 of the heat sink 20 and the side wall 12 of the water jacket 10 are bonded using thermal diffusion bonding, the left-right width d of the side wall 12 can be made smaller (for example, 1 to 20 [mm]) compared to the case where the main body portion 21 and the side wall 12 are bolted together. Accordingly, the degree of freedom in the shape of the cooling member 1 can be improved. In addition, a large width of the flow path P can be secured, which in turn makes it possible to improve cooling performance.
[0063] Furthermore, in the method for manufacturing the cooling member 1 according to the present embodiment, the contact step (the first contact step and the second contact step) ends in a state where the heat sink 20 is in contact with the side wall 12 of the water jacket 10, and the fins 22 are separated from the bottom portion 11 of the water jacket 10. After that, the water jacket 10, the heat sink 20 and the copper spreader 30 arranged in the contact step are heated and pressurized to start thermal diffusion bonding. The side wall 12 of the water jacket 10 contracts moderately under pressure, so that the previously separated fins 22 come into contact with the bottom portion 11 of the water jacket 10. For this reason, it is possible to suppress excessive force from being applied to the fins 22 during bonding, while enabling the fins 22 to come into contact and undergo thermal diffusion bonding, which in turn can suppress deformation or damage of the fins 22.
[0064] Furthermore, in the method for manufacturing the cooling member 1 according to the present embodiment, since thermal diffusion bonding is used for bonding the respective members, even dissimilar metals can be easily bonded. In addition, during the bonding process, the water jacket 10 and the heat sink 20 come into contact not only at the side wall 12 and the main body portion 21, but also at the bottom portion 11 and the fins 22. For this reason, it is possible to suppress the occurrence of shape collapse of the entire cooling member 1 due to heating and pressurization. Furthermore, by adjusting the total area C of the third bonding portion 60 and the total area B of the second bonding portion 50 so as to satisfy "(C / 2)<B<(C×2)", the occurrence of shape collapse of the entire cooling member 1 due to heating and pressurization can be further suppressed.
[0065] Furthermore, the thicknesses t1, t2, and t3 of the copper spreader 30, the main body 21 of the heatsink 20, and the bottom 11 of the water jacket 10 are set to t1:t2:t3 = 1:1 to 3:1 to 10. By setting the ratio of each thickness t1, t2, and t3 in this way, the cooling performance can be improved.
[0066] Furthermore, the ratio of the total area A of the first joint 40, the total area B of the second joint 50, and the total area C of the third joint 60 is set to A:B:C = 1:0.5~5:0.5~5, preferably A:C = 1:0.5~1. By setting the ratio of the total areas A, B, and C in this way, it is possible to make it easier to join the water jacket 10, the heat sink 20, and the copper spreader 30. In addition, it is possible to further suppress the occurrence of deformation of the entire cooling member 1 due to heating and pressurization.
[0067] As described above, the cooling member 1 according to this embodiment is A water jacket 10 (flow channel forming member) that forms a fluid flow channel P with a bottom portion 11 and side walls 12 erected on the bottom portion 11, A heat sink 20 is joined to the side wall 12 and separates the flow path P from the outside of the water jacket 10, A copper spreader 30 (heat conductive member) is bonded to the exposed surface 21a (exposed portion) of the heat sink 20 that is exposed to the outside of the water jacket 10, and the electronic component E (heating element) is in contact with it. It is equipped with, The heat sink 20 has a plurality of fins 22 that are in contact with the bottom portion 11 on the flow path P side, The water jacket 10, the heat sink 20, and the copper spreader 30 are composed of at least two or more metallic materials and are joined together using thermal diffusion bonding.
[0068] This configuration allows for easy manufacturing and improves the degree of freedom in shape.
[0069] Furthermore, the above-mentioned at least two types of metallic materials are It contains copper and aluminum.
[0070] By configuring it in this way, cooling performance can be improved.
[0071] Furthermore, the joint formed by thermal diffusion bonding is It includes a portion where copper and aluminum are joined (first joint 40) and portions where aluminum is joined to aluminum (second joint 50 and third joint 60).
[0072] By configuring it in this way, cooling performance can be improved.
[0073] Furthermore, the total area C of the joint surface between the fin 22 and the bottom portion 11, and the total area B of the joint surface between the heat sink 20 and the side wall 12 are (C / 2) <B<(C×2)であるものである。
[0074] By configuring it in this way, it becomes less likely for the shape to collapse.
[0075] Furthermore, the joint between the fin 22 and the bottom portion 11 (third joint portion 60) is formed to have an R shape.
[0076] This configuration improves the strength of the joint between the fin 22 and the bottom 11.
[0077] Furthermore, the method for manufacturing the cooling member 1 according to this embodiment is as follows: A water jacket 10 (flow channel forming member) that forms a fluid flow channel P with a bottom portion 11 and side walls 12 erected on the bottom portion 11, A heat sink 20 is joined to the side wall 12, demarcating the flow path P from the outside of the water jacket 10, and having a plurality of fins 22 on the flow path P side, A copper spreader 30 (heat conductive member) is bonded to the exposed surface 21a (exposed portion) of the heat sink 20 that is exposed to the outside of the water jacket 10, and the electronic component E (heating element) is in contact with it. A method for manufacturing a cooling member 1 comprising the following: The water jacket 10, the heat sink 20, and the copper spreader 30 are composed of at least two types of metallic materials. The invention comprises a bonding step in which the plurality of fins 22 are brought into contact with the bottom portion 11 on the flow path P side, and the water jacket 10, the heat sink 20, and the copper spreader 30 are bonded together using thermal diffusion bonding.
[0078] This configuration allows for easy manufacturing and improves the degree of freedom in shape.
[0079] Although embodiments of the present invention have been described above, the present invention is not limited to the above configuration, and various modifications are possible within the scope of the invention as described in the claims.
[0080] For example, in this embodiment, the side wall 12 is provided on the water jacket 10, but it may also be provided on the heat sink 20.
[0081] Furthermore, in this embodiment, all fins 22 are in contact with and joined to the bottom 11, but it is also possible that only a portion of the fins 22 are in contact with and joined to the bottom 11.
[0082] Furthermore, the metal materials constituting the water jacket 10, heat sink 20, and copper spreader 30 are not limited to those of this embodiment and may be other metal materials. Also, the metal materials constituting the water jacket 10, heat sink 20, and copper spreader 30 may be three different types (i.e., each may be made of a different metal material). [Explanation of symbols]
[0083] 1 Cooling component 10 Water Jackets 11 Bottom 12 Side wall 20 Heatsinks 21a Exposed surface 22 fins 30 Copper Spreaders
Claims
1. A flow path forming member that forms a fluid flow path with a bottom and side walls erected on the bottom, A heat sink is joined to the side wall and separates the flow path from the outside of the flow path forming member, A heat conductive member is joined to the exposed portion of the heat sink that is exposed on the outside side of the flow path forming member, and the heat generating element is in contact with it. It is equipped with, The heat sink has a plurality of fins that are in contact with the bottom on the flow path side, The channel forming member, the heat sink, and the heat conducting member are composed of at least two or more metal materials and are joined together using thermal diffusion bonding. Cooling component.
2. The aforementioned at least two types of metallic materials are Including copper and aluminum, The cooling member according to claim 1.
3. The joint formed by thermal diffusion bonding is Including a portion where copper and aluminum are joined, and a portion where aluminum and aluminum are joined, The cooling member according to claim 2.
4. The total area C of the joint surface between the fin and the bottom, and the total area B of the joint surface between the heat sink and the side wall, satisfy the condition (C / 2) < B < (C × 2). The cooling member according to claim 1.
5. The joint between the fin and the bottom is formed to have an R shape. A cooling member according to any one of claims 1 to 4.
6. A flow path forming member that forms a fluid flow path with a bottom and side walls erected on the bottom, A heat sink is joined to the side wall, demarcating the flow path from the outside of the flow path forming member, and having a plurality of fins on the flow path side, A heat conductive member is joined to the exposed portion of the heat sink that is exposed on the outside side of the flow path forming member, and the heat generating element is in contact with it. A method for manufacturing a cooling member comprising: The flow channel forming member, the heat sink, and the heat conducting member are composed of at least two types of metallic materials. The invention comprises a bonding step in which the plurality of fins are brought into contact with the bottom on the flow path side, and the flow path forming member, the heat sink, and the heat conducting member are bonded together using thermal diffusion bonding. A method for manufacturing a cooling component.
Citation Information
Patent Citations
Cooling device for power semiconductor device and method for manufacturing the same
JP2017005181A