Catalyst for fuel cells and method for manufacturing the same
By adjusting the pH of the carbon material surface and suspension to less than 7.0, the catalyst design facilitates proton entry into the pores, addressing proton diffusion challenges and enhancing fuel cell performance.
Patent Information
- Application Number
- JP2025079033
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2025-05-09
- Publication Date
- 2026-11-19
AI Technical Summary
Existing catalyst supports in fuel cells face challenges in promoting proton entry into pores due to the complex interplay of water and various functional groups on the carbon material surface, which affects the charge environment and proton diffusion.
The catalyst design focuses on achieving a pH of less than 7.0 for the carbon material surface and its aqueous suspension, ensuring a negative surface charge state that facilitates proton entry into the pores, using a carbon material with specific functional group concentrations and an ionomer coating.
This approach enhances proton mobility into the pores, reducing catalyst poisoning and improving fuel cell performance by stabilizing the electrostatic potential for proton entry.
Smart Images

Figure 2026182644000001_ABST
Abstract
Description
Technical Field
[0001] The present specification relates to a catalyst for fuel cells, a method for producing the same, and the like.
Background Art
[0002] A catalyst material used in a fuel cell generally includes a porous catalyst carrier, a catalyst supported inside the pores, and a proton-conductive ionomer covering the catalyst carrier. By supporting the catalyst inside the pores, it is possible to suppress the phenomenon (poisoning) in which the activity of the catalyst decreases when the catalyst is coated with the ionomer. Here, in order to promote the supply of protons to the catalyst supported inside the pores, it has been disclosed that the amount of acidic functional groups modifying the catalyst carrier is set within a certain range (Patent Document 1).
[0003] Patent Document 1 describes that the amount of phenolic hydroxyl groups, which are acidic functional groups, is adjusted by hydrophilizing a carbon material with nitric acid, that the amount of acidic functional groups is calculated based on the water vapor adsorption amount in the pores, and that protons can be supplied to the catalyst inside the pores via moisture in the vicinity of the inside of the pores (Paragraphs 0035, 0052, 0072, Figure 3 and the like of Patent Document 1).
Prior Art Documents
Patent Documents
[0004]
Patent Document 1
Summary of Invention
Problems to be Solved by the Invention
[0005] Since protons are charged ions, water is necessary as a diffusion pathway. However, the mere presence of water does not automatically promote proton entry into pores. Furthermore, catalyst supports possess various functional groups in addition to acidic functional groups. Therefore, the overall composition of these factors determines the charge environment of the carbon material and pores. For these reasons, it may be difficult to promote proton entry into pores based solely on the amount of acidic functional groups or water content.
[0006] This specification provides a technology that contributes to improving the performance of fuel cells by focusing on the movement of protons into the pores of carbon materials. [Means for solving the problem]
[0007] According to the present inventors, they focused on the ionization equilibrium state of various functional groups present in carbon materials. They found that in this ionization equilibrium state, when the carbon material surface as a whole has a negative charge, the electrostatic potential of protons is stabilized as more protons enter the pores. Based on this finding, the following means are provided. In the following, hydrogen ions derived from the functional groups present in the carbon material of the fuel cell catalyst are referred to as hydronium ions.
[0008] [1] A catalyst for fuel cells, A carbon material having pores, The catalyst supported inside the pores, An ionomer covering at least a portion of the carbon material, Equipped with, The carbon material is as follows (a) and (b): (a) The pH is less than 7.0 based on the difference in molar concentration between the molar concentration of hydronium ions based on acidic functional groups among the functional groups of the carbon material and the molar concentration of hydroxide ions based on basic functional groups among the functional groups. (b) The pH of the aqueous suspension of the carbon material is less than 7.0. A fuel cell catalyst that satisfies at least one of the following conditions. [2] The carbon material is the fuel cell catalyst according to [1], satisfying (b) above. [3] A method for manufacturing a catalyst for a fuel cell, As carbon materials having pores, the following (a) and (b): (a) The pH is less than 7.0 based on the difference in molar concentration between the molar concentration of hydronium ions based on acidic functional groups among the functional groups of the carbon material and the molar concentration of hydroxide ions based on basic functional groups among the functional groups. (b) The pH of the aqueous suspension of the carbon material is less than 7.0. A step of preparing a carbon material that satisfies at least one of the following conditions, A step of preparing a catalyst-supported carbon material by supporting a catalyst on the aforementioned carbon material, The process of preparing a catalyst-supported material involves coating at least a portion of the surface of the catalyst-supported carbon material with an ionomer, A manufacturing method that includes the following features. [4] A carbon material having pores used as a catalyst for fuel cells, The carbon material is as follows (a) and (b): (a) The pH is less than 7.0 based on the difference in molar concentration between the molar concentration of hydronium ions based on acidic functional groups among the functional groups of the carbon material and the molar concentration of hydroxide ions based on basic functional groups among the functional groups. (b) The pH of the aqueous suspension of the carbon material is less than 7.0. A carbon material that satisfies at least one of the following conditions.
[0009] The fact that the carbon material has a pH of less than 7.0 based on the predetermined differential molar concentration described above and / or the pH of the aqueous suspension is less than 7.0 indicates that the carbon material surface and the surfaces inside the pores have a negative charge in the ionization equilibrium state of the functional groups on the carbon material surface. By using such a carbon material, it becomes easier for positively charged protons to enter the pores of the carbon material. [Brief explanation of the drawing]
[0010] [Figure 1] This is a diagram schematically showing the relationship between the surface charge state of a carbon material (less than pH 7.0, pH 7.0, greater than pH 7.0) and proton mobility. [Figure 2] This is a diagram showing an overview of the simulation. [Figure 3] This is a diagram showing the simulation results. [Figure 4] This is a diagram showing the performance evaluation results of the fuel cell. [Mode for Carrying Out the Invention]
[0011] Hereinafter, the fuel cell catalyst disclosed in the present specification, the method for producing the same, and the like will be described with appropriate reference to the drawings. The fuel cell catalyst disclosed in the present specification is used, for example, in the cathode electrode of a polymer electrolyte fuel cell (PEFC). According to the present specification, a polymer electrolyte fuel cell including a cathode electrode containing the fuel cell catalyst is also disclosed.
[0012] (Fuel Cell Catalyst) The fuel cell catalyst includes a carbon material having pores, a catalyst supported inside the pores, and an ionomer that covers at least a part of the carbon material.
[0013] The carbon material is a porous carbon material having pores. The carbon material is not particularly limited, and known materials can be appropriately used. Examples thereof include carbon black, carbon nanotubes, carbon nanohorns, activated carbon, natural graphite, mesocarbon microbeads, and glassy carbon powder. The carbon material may be doped with nitrogen, boron, tungsten, aluminum, titanium, or the like.
[0014] Carbon materials have pores. Pores are recessed areas that extend from the surface of the carbon material into the interior. The pores only need to be large enough to support a catalyst inside. For example, the pores are mesopores with a diameter of 2.0 nm to 50 nm. The diameter of mesopores is also, for example, 5.0 nm to 20 nm. The diameter of pores such as mesopores can be measured using the BJH method with isothermal adsorption curves of an inert gas.
[0015] Carbon materials are particles with arbitrary shapes. The average particle size of carbon materials is not particularly limited, but for example, it is approximately between 200 nm and 1000 nm.
[0016] Carbon materials may have the following characteristics (a) and / or (b) based on the functional groups they have on their surface.
[0017] <Features (a)> The carbon material may have the following characteristics: (a) The pH, based on the difference in molar concentration between the molar concentration of hydronium ions based on acidic functional groups among the functional groups possessed by the carbon material and the molar concentration of hydroxide ions based on basic functional groups among the functional groups, is less than 7.0.
[0018] Generally, carbon materials have various functional groups on their surface depending on their raw materials, manufacturing process, surface treatment, heat treatment, etc. The functional groups that carbon materials possess are not particularly limited. Examples include acidic functional groups such as carboxyl groups, hydroxyl groups, carbonyl groups, lactone groups, ether groups, quinone groups, and carboxylic acid anhydrides, and various basic functional groups such as amino groups, amine-type nitrogen-containing groups, pyrrole-type nitrogen-containing groups, pyridine-type nitrogen-containing groups, pyridone-type nitrogen-containing groups, and quaternary-type nitrogen-containing groups.
[0019] When the pH, based on the difference in molar concentration between the molar concentration of hydronium ions due to acidic functional groups and the molar concentration of hydroxide ions due to basic functional groups of a carbon material, is less than 7.0, the surface charge state of the carbon material is negatively charged. Such pH values are, for example, less than 7.0, 6.5 or less, 6.0 or less, 5.5 or less, 5.0 or less, 4.5 or less, 4.0 or less, 3.5 or less, 3.0 or less, 2.5 or less, 2.0 or less, 1.5 or less, and 1.0 or less. In some cases, a more acidic pH is preferable.
[0020] As shown in Figure 1, when the surface charge state of the carbon material is negative (when the pH is less than 7.0), positively charged protons can easily enter the pores. This facilitates the proton-mediated reaction in the catalyst supported within the pores, thus avoiding poisoning by ions. When the surface charge state is zero (when the pH is 7.0), protons have difficulty entering the pores. Furthermore, when the surface charge state is positive (when the pH is greater than 7.0), protons have even more difficulty entering the pores.
[0021] Here, the molar concentrations of hydronium ions and hydroxide ions can be determined by dispersing the carbon material in a predetermined amount of water (pure water) at 25°C and 1 atm, and obtaining the concentrations in an aqueous suspension where a stable ionization equilibrium state with a stable pH is achieved. The pH can be measured based on the pH measurement method described in JIS K1474 Activated Carbon Test Method 7.11 pH.
[0022] The molar concentration of hydronium ions can be obtained from the molar concentration of acidic functional groups (moles / l) × degree of ionization. Similarly, the molar concentration of hydroxide ions can be obtained from the number of moles of basic functional groups (moles / l) × their degree of ionization. The differential molar concentration can be obtained, for example, by calculating the difference between the molar concentrations of hydronium ions and hydroxide ions, such that the difference value is a positive number. When the differential molar concentration is the molar concentration of hydronium ions, the pH can be determined based on the hydronium ion molar concentration. Alternatively, when the differential molar concentration is the molar concentration of hydroxide ions, the hydronium ion concentration can be calculated using the formula for the ion product of water, and then the pH can be determined based on the hydronium ion concentration.
[0023] By calculating the hydronium ion molar concentration and hydroxide ion molar concentration for all acidic and basic functional groups present in the carbon material, and obtaining the difference molar concentration from the sum of the hydronium ion molar concentration and the sum of the hydroxide ion molar concentration, respectively, it is possible to obtain a pH that reflects the surface charge state of the carbon material.
[0024] <Features (b)> If it is difficult to determine the type, amount, degree of ionization, etc., of the acidic and / or basic functional groups, satisfying characteristic (b) that the pH of the aqueous suspension of the carbon material (hereinafter also referred to as the immersion pH) is less than 7.0 will satisfy characteristic (a). In other words, with respect to the same aqueous suspension of the same carbon material, characteristic (a) and characteristic (b) are synonymous.
[0025] When the immersion pH is less than 7, the surface charge state of the carbon material is negatively charged; when the immersion pH is 7.0, the surface charge state of the carbon material is zero; and when the immersion pH is greater than 7.0, the surface charge state of the carbon material is positively charged. Therefore, similar to feature (a), feature (b) also adopts the same mode of proton entry into the pores as shown in Figure 1.
[0026] The pH of the water immersion can be measured in accordance with the pH measurement method described in JIS K1474 Activated Carbon Test Method 7.11 pH. Here, the suspension of the carbon material is an aqueous suspension obtained by suspending the carbon material in a predetermined amount of water (pure water) at 25°C and 1 atmosphere, until a stable ionization equilibrium state with a stable pH is achieved. The aqueous suspension can be the same concentration as that used for pH measurement (1 mass%). If necessary, the carbon material can be thoroughly suspended in water by dispersion treatment such as ultrasound or stirring. Furthermore, to obtain a stable ionization equilibrium state with a stable pH, stirring or standing can be performed for several hours to tens of hours, for example. The pH can be measured with a pH meter equipped with a glass electrode.
[0027] Such pH can take the same form as characteristic (a). That is, such pH is, for example, less than 7.0, 6.5 or less, 6.0 or less, 5.5 or less, 5.0 or less, 4.5 or less, 4.0 or less, 3.5 or less, 3.0 or less, 2.5 or less, 2.0 or less, 1.5 or less, and 1.0 or less. Such pH may be preferable as it is more acidic.
[0028] Whether or not the carbon material satisfies characteristic (b) allows for a simple determination of whether the surface charge state of the carbon material is negative.
[0029] (catalyst) The catalyst is supported inside the pores of the carbon material. While at least a portion of the catalyst is supported inside the pores, a portion may be supported on the surface of the carbon material. The catalyst, although not particularly limited, is selected from platinum and other metals. Examples of other metals include cobalt, nickel, manganese, titanium, aluminum, chromium, iron, molybdenum, tungsten, ruthenium, palladium, rhodium, iridium, osmium, and copper. Alloys of platinum and other metals such as cobalt may be preferred.
[0030] (Ionoma) Any known ionomer can be used as appropriate. Typically, the ionomer is a random copolymer having sulfonic acid groups. The ionomer coats the surface of the carbon material.
[0031] (A carbon material with pores used as a catalyst for fuel cells) This specification provides a carbon material for use as a catalyst for a fuel cell, having feature (a) and / or feature (b).
[0032] (Method for manufacturing fuel cell catalysts) A method for manufacturing a fuel cell catalyst disclosed herein comprises the steps of: preparing a carbon material having pores that satisfies the above characteristics (a) and / or (b); preparing a catalyst-supported carbon material by supporting at least a portion of the catalyst inside the pores of the carbon material; and preparing a catalyst-supported material by coating at least a portion of the surface of the catalyst-supported carbon material with an ionomer. It can be equipped with.
[0033] By using a specific carbon material as a catalyst support material, surface charge situation Because the polarity is negative, protons can easily enter the interior of the pores. This suppresses catalyst poisoning by ions.
[0034] The steps of preparing the catalyst-supported carbon and coating the catalyst-supported carbon with an ionomer can be carried out as appropriate by known methods. [Examples]
[0035] The following examples illustrate the disclosures of this specification in more detail. The following examples are for illustrative purposes only and are not intended to limit the scope of the disclosures of this specification. [Examples]
[0036] Figure 2 shows an overview of a simulation that replaces the example. The following simulation is based on classical molecular dynamics and was performed using the supercomputer "Fugaku," owned by RIKEN and located at the RIKEN Center for Computational Science.
[0037] It should be noted that this embodiment is a simulation, not an experiment. This simulation explains, from the perspective of classical molecular dynamics, the technical ideas disclosed herein, which are clear in themselves and can be implemented by those skilled in the art. It is common technical knowledge to those skilled in the art that the surface charge state of a carbon material is determined by the balance of the ionization equilibrium states of the functional groups present on the carbon material surface (including the inner surface of the pores). On the other hand, the technical idea that the inventors first focused on—making the surface charge state of carbon negative to facilitate proton access to the pores—is also clear in itself and clear and sufficient to be implemented by those skilled in the art.
[0038] This simulation concerns the movement of protons in response to pH (water immersion pH in this specification, which corresponds to the surface charge state of the carbon material) when a carbon material is dispersed in water and in an ionization equilibrium state. The simulation shows the movement of protons (H3O) from the surface of the carbon material into the pores in response to the water immersion pH. + This method calculates the electrostatic potential when a particle moves. The more negative the electrostatic potential, the more energetically stable the system is.
[0039] As a premise for the simulation, the following carbon material was set. Specifically, carboxyl groups and amino groups were set as functional groups on the surface of the carbon material (including the inner surface of the pores). The amount of ions based on the dissociation of carboxyl groups and amino groups was set so that the pH (surface charge state) of the carbon material immersed in water was the pH of Example and Comparative Examples 1-3. For example, at pH 6.00 (Example), the charge amount of each functional group was set so that the negative charge based on the carboxyl group was excessive, and at pH 7.00 (Comparative Example 2), it was set so that the negative charge based on the carboxyl group and the positive charge based on the amino group were equal in amount.
[0040] Furthermore, when the surface charge state of the carbon material is pH 6.00 (example), there is an excess of hydronium ions generated by the dissociation of carboxyl groups, and COO acts as a counterion. - Since it modifies the carbon material surface (including the inner surface of the pores), it can be said that the surface charge state of the carbon material is negative. On the other hand, when the pH is 7.00, 7.75, and 8.00 (Comparative Examples 1-3), there is an excess of hydroxide ions generated by the dissociation of amino groups, and NH3 acts as a counterion. + Since this modifies the carbon material surface (including the inner surface of the pores), it can be said that the surface charge state of the carbon material is positive.
[0041] Furthermore, it is assumed that water and Nafion (trade name) are present around each carbon material. Protons (H3O) are present at the interface between the carbon material and Nafion. + Select one proton and use it as a probe, while fixing the other protons. Scan the proton probe from the surface of the carbon material towards the interior of the pores in the carbon material (maximum 20 nm). Determine the electrostatic potential V (potential energy U / electric charge q) corresponding to this scan distance. The relationship between scan distance and electrostatic potential is shown in Figure 3 and Table 1.
[0042] [Table 1]
[0043] Figure 3 shows the distance from the carbon material surface (angstroms) on the horizontal axis and the electrostatic potential (V) on the vertical axis. As shown in Figure 3, in the carbon material of the example (surface charge state pH 6.00), the electrostatic potential decreased (increased negatively) as protons penetrated from the carbon material surface into the carbon material, i.e., into the pores. This indicates that the material becomes more stable as more protons penetrate into the pores.
[0044] In contrast, in the carbon materials of Comparative Examples 1-3 (with surface charge states of pH 7.00, 7.75, and 8.00, respectively), the electrostatic potential increased as protons penetrated from the carbon material surface into the pores. This indicates that the material becomes more unstable as more protons penetrate the pores.
[0045] From the above, it was found that making the charge state of the carbon material surface negative (or having a water immersion pH of less than 7.0) can promote the entry of protons into the pores.
[0046] This simulation was performed based on the amount of carboxyl and amino groups on the surface of the carbon material. However, it is believed that similar results can be obtained if the pH (water immersion pH) when carbon materials with various other functional groups are dispersed in water and brought to ionization equilibrium is less than 7.0. [Examples]
[0047] In this example, carbon materials with a water immersion pH of less than 7.0 were prepared, and a MEA was fabricated to evaluate the performance of the fuel cell. The results are shown in Figure 4.
[0048] (Preparing materials) Several commercially available carbon materials were obtained, and their pH (water suspension pH) (water immersion pH) was measured according to JIS K1474 7.11 pH. The water suspension pH of carbon materials 1-4 was 3.2, 3.3, 3.4, and 3.6, respectively. For these carbon materials, platinum-supported carbon materials, obtained by supporting the same amount of platinum-supported carbon material inside the pores of platinum-carbon material, were used as electrode catalysts.
[0049] For the catalyst layer ionomer, an ionomer solution (DE1020, manufactured by DuPont, polymer concentration: 10% by mass, aqueous dispersion) was used. Furthermore, a mixed solvent of water, diacetone alcohol, and ethanol (65:25:10, volume ratio) was used as the solvent.
[0050] (Preparation of catalyst ink) The catalyst ink was prepared according to the following procedure. The I / C ratio (ratio of the mass of the catalyst layer ionomer to the mass of the carbon support contained in the catalyst ink) of the catalyst ink was set to 0.75, and the solid content concentration was set to 10% by mass. (1) Electrode catalyst: A predetermined amount of water was added to 1 g and stirred with a spatula. (2) A predetermined amount of ionomer solution was added to the obtained mixture and dispersed using an ultrasonic homogenizer for 5 minutes. (3) A predetermined amount of ethanol was added to the obtained mixture and the mixture was dispersed using an ultrasonic homogenizer for 5 minutes. (4) A predetermined amount of diacetone alcohol was added to the obtained mixture and dispersed using an ultrasonic homogenizer for 5 minutes to obtain a catalyst ink. (5) The obtained catalyst ink was subjected to centrifugal degassing for 3 minutes.
[0051] (Fabrication of the catalyst layer) The obtained catalyst ink was coated onto a polytetrafluoroethylene (PTFE) sheet using an applicator. The coating resulted in a film thickness of 100 μm and a platinum mass of 0.5 mg / cm² per unit area. 2 The following procedure was followed: The coated sheet was placed on a hot plate at 80°C in an air atmosphere and left for 10 minutes. Furthermore, it was left overnight in a vacuum dryer at 100°C.
[0052] (MEA preparation) Nafion® 211 (20 μm thick, manufactured by Chemours) was used as the electrolyte membrane. Catalyst layers were thermally transferred to both sides of the electrolyte membrane to obtain a MEA. The thermal transfer conditions were: temperature: 140°C, pressure: 50 kg / cm². 2 The pressure was set to 4.9 MPa, and the pressurization time was 10 minutes.
[0053] (Fuel cell performance evaluation) Using the fabricated MEA, the electrode area was 1 cm². 2 The fuel cell was assembled and connected to an evaluation bench. Oxygen (flow rate: 1 L / min) was supplied to the cathode and hydrogen (flow rate: 1 L / min) to the anode, with a current density of 0.2 A / cm².2 The voltage was measured at that time.
[0054] As shown in Figure 4, it was observed that the voltage of samples 1-4 increased as the pH decreased. In other words, it was thought that the lower and more acidic the pH of the water immersion pH of the carbon material (the greater the negative surface charge), the more the protons moved into the pores, reaching the platinum catalyst supported inside the pores, promoting the electrode reaction, and consequently improving the fuel cell performance.
Claims
1. A catalyst for fuel cells, A carbon material having pores, The catalyst supported inside the pores, An ionomer covering at least a portion of the carbon material, Equipped with, The carbon material is as follows (a) and (b): (a) The pH is less than 7.0, based on the difference in molar concentration between the molar concentration of hydronium ions based on acidic functional groups among the functional groups of the carbon material and the molar concentration of hydroxide ions based on basic functional groups among the functional groups. (b) The pH of the aqueous suspension of the carbon material is less than 7.
0. A fuel cell catalyst that satisfies at least one of the following conditions.
2. The carbon material is the fuel cell catalyst according to claim 1, satisfying (b).
3. A method for manufacturing a catalyst for fuel cells, As carbon materials having pores, the following (a) and (b): (a) The pH is less than 7.0, based on the difference in molar concentration between the molar concentration of hydronium ions based on acidic functional groups among the functional groups of the carbon material and the molar concentration of hydroxide ions based on basic functional groups among the functional groups. (b) The pH of the aqueous suspension of the carbon material is less than 7.
0. A step of preparing a carbon material that satisfies at least one of the following conditions, A step of preparing a catalyst-supported carbon material by supporting at least a portion of the catalyst in the pores of the carbon material, The process of preparing a catalyst-supported material involves coating at least a portion of the surface of the catalyst-supported carbon material with an ionomer, A manufacturing method that includes the following features.
4. A carbon material having pores, used as a catalyst for fuel cells, The carbon material is as follows (a) and (b): (a) The pH is less than 7.0, based on the difference in molar concentration between the molar concentration of hydronium ions based on acidic functional groups among the functional groups of the carbon material and the molar concentration of hydroxide ions based on basic functional groups among the functional groups. (b) The pH of the aqueous suspension of the carbon material is less than 7.
0. A carbon material that satisfies at least one of the following conditions.
Citation Information
Patent Citations
Catalyst layer for fuel cell and electrolyte membrane-electrode assembly