hybrid memory element

The hybrid memory device addresses high voltage and slow speed issues in flash memory and read delay in FeFET memory by using a ferroelectric material, enhancing electric field and speed, enabling multi-bit storage and neuromorphic computing capabilities.

JP2026182689APending Publication Date: 2026-11-19MATERIAL ANALYSIS TECH INC +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2025122268
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-07-18
Filing Date
2025-07-22
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Flash memory has high operating voltage and slow operating speed, while ferroelectric field-effect transistor (FeFET) memory faces challenges in reducing post-write read delay.

Method used

A hybrid memory device incorporating a semiconductor substrate, tunnel layer, ferroelectric storage layer, and gate structure with a ferroelectric material, such as metal-doped hafnium oxide, to enhance electric field and reduce operating voltage and improve speed.

Benefits of technology

The hybrid memory device achieves lower operating voltage, faster read speed, multi-bit storage, and improved reliability, with potential applications in computation-in-memory (CIM) and neuromorphic computing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182689000001_ABST
    Figure 2026182689000001_ABST
Patent Text Reader

Abstract

This invention provides a hybrid memory element that reduces operating voltage, improves operating speed, and simultaneously achieves excellent results in read speed and reliability. [Solution] The hybrid memory element 10 includes a semiconductor substrate 100, a tunnel layer 102, a ferroelectric storage layer 104, a gate 106, and a plurality of doped regions 108. The tunnel layer is placed on the semiconductor substrate. The ferroelectric storage layer is placed on the tunnel layer and enhances the electric field of the tunnel layer, and includes a ferroelectric material having electron conservation properties and ferroelectric properties. The gate is placed on the ferroelectric storage layer and is in direct contact with the ferroelectric storage layer. The doped regions are formed in the semiconductor substrate on both sides of the gate.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present invention relates to semiconductor memory technology, and in particular to a hybrid memory device. BACKGROUND ART

[0002] Flash memory is a type of non-volatile memory, and currently occupies a leading position in the field of non-volatile memory. Despite significant progress, flash memory has the drawbacks of high operating voltage (>20V) and slow operating speed (approximately 1ms).

[0003] On the other hand, ferroelectric field-effect transistor (FeFET) memory is a type of non-volatile memory that is seeing new developments, and not only has excellent energy efficiency and CMOS compatibility, but also demonstrates potential for applications in the areas of associative search and memory computing acceleration. However, FeFET memory has the problem that the post-write read delay cannot be reduced.

[0004] Therefore, there is an urgent current need to develop non-volatile memory that solves the aforementioned respective problems. SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION

[0005] The present invention provides a hybrid memory device that can reduce the operating voltage and improve the operating speed, and at the same time can achieve excellent effects in terms of read speed and reliability. MEANS FOR SOLVING THE PROBLEMS

[0006] The hybrid memory element of the present invention includes a semiconductor substrate, a tunnel layer, a ferroelectric storage layer, a gate, and a plurality of doped regions. The tunnel layer is placed on the semiconductor substrate. The ferroelectric storage layer is placed on the tunnel layer and enhances the electric field of the tunnel layer, and the ferroelectric storage layer contains a ferroelectric material. The gate is placed on the ferroelectric storage layer and is in direct contact with the ferroelectric storage layer. The doped regions are formed in the semiconductor substrate on both sides of the gate.

[0007] In the embodiments of the present invention, the ferroelectric material includes metal-doped hafnium oxide.

[0008] In embodiments of the present invention, the semiconductor substrate includes a silicon substrate or a germanium substrate.

[0009] In embodiments of the present invention, the tunnel layer includes a single-layer or multi-layer structure.

[0010] In embodiments of the present invention, the gate includes a metal gate or a titanium nitride gate.

[0011] In embodiments of the present invention, the tunnel layer comprises a high-dielectric constant (high-k) material. [Effects of the Invention]

[0012] Based on the above, the present invention overcomes the limitations of conventional flash memory, namely its excessively high operating voltage and slow operating speed, by employing a ferroelectric material as the charge trapping layer of the flash memory. Furthermore, it overcomes the limitations in read operation and reliability of current FeFET ferroelectric memories. The hybrid memory of the present invention is expected to enable multi-bit storage operations of two or more bits and to have the capability for future application to computation-in-memory (CIM).

[0013] To make the above-mentioned features and advantages of the present invention easier to understand, examples are given below and will be described in detail together with the accompanying drawings. Brief Description of the Drawings

[0014] [Figure 1] It is a schematic cross-sectional view of the hybrid memory device according to the first embodiment of the present invention. [Figure 2] It is a polarization-voltage (P-V) curve diagram of the comparative example, Experimental Example 1 and Experimental Example 2. [Figure 3] It is an ID-VGS curve diagram of the comparative example, Experimental Example 1 and Experimental Example 2. [Figure 4] It is an energy band diagram when the gate in the devices of the comparative example and Experimental Example 1 is subjected to a positive bias. [Figure 5] It is an energy band diagram when the gate in the devices of the comparative example and Experimental Example 1 is subjected to a negative bias. [Figure 6] It is a threshold voltage (Vt) curve diagram accompanying a change in pulse width of the devices of the comparative example and Experimental Example 1. [Figure 7] It is a switchable polarization curve diagram accompanying a change in pulse width of the device of Experimental Example 1. [Figure 8] It is a short-term delay curve diagram of Read-after-write in the devices of the comparative example and Experimental Example 1. [Figure 9] It is a long-term delay curve diagram of read operation in the devices of the comparative example and Experimental Example 1. [Figure 10] It is a Vt curve diagram after the durability test of the devices of the comparative example and Experimental Example 1. [Figure 11] It is a retention characteristic diagram of the device of Experimental Example 1 in different Vt states after 10⁵ cycles. [Figure 12] It is a Vt distribution diagram of the device of Experimental Example 1 in different Vt states after 10⁵ cycles. [Figure 13] It is an excitatory postsynaptic current (EPSC) curve diagram of the device of Experimental Example 1. [Figure 14]This is a graph of the inhibitory postsynaptic current (IPSC) curve of the device of Experimental Example 1. [Mode for Carrying Out the Invention]

[0015] Figure 1 is a schematic cross-sectional view of the hybrid memory device according to the first embodiment of the present invention.

[0016] Referring to Figure 1, the hybrid memory device 10 of the first embodiment includes a semiconductor substrate 100, a tunnel layer 102, a ferroelectric storage layer 104, a gate 106, and a plurality of doped regions 108. The tunnel layer 102 is disposed on the semiconductor substrate 100. The ferroelectric storage layer 104 is disposed on the tunnel layer 102 to enhance the electric field of the tunnel layer 102, and the ferroelectric storage layer 104 includes a ferroelectric material. The gate 106 is disposed on the ferroelectric storage layer 106, and the gate 106 is in direct contact with the underlying ferroelectric storage layer 104. The doped regions 108 are formed in the semiconductor substrate 100 on both sides of the gate 106, act as the source and drain of the hybrid memory device 10, and make the operation of the hybrid memory device 10 follow the operation mode of a flash memory.

[0017] In some embodiments, the ferroelectric material in the ferroelectric storage layer 104 may be metal-doped hafnium oxide, including hafnium zirconium oxide (HZO), hafnium aluminum oxide (HAO), hafnium silicon oxide (HSO), or hafnium oxide doped with other metals. Usable dopants include scandium (Sc), lanthanum (La), calcium (Ca), barium (Ba), yttrium (Y), strontium (Sr), and / or gadolinium (Gd). In some other embodiments, the above-mentioned ferroelectric material may include lead zirconate titanate (PZT), lanthanum-doped lead zirconate titanate (PLZT), lead zirconate (PBT), barium titanate (BaTiO3), lead titanate (PbTiO3), lead metaniobate (PbNb2O6), lithium niobate (LiNbO3), lithium tantalate (LiTaO3), magnesium lead niobate (PMN), scandium lead tantalate (PST), strontium bismuth tantalate (SBT), sodium bismuth titanate (BNT), scandium aluminum nitride (AlScN), or aluminum nitride (AlN). Because the ferroelectric material in the ferroelectric storage layer 104 has a dipole effect, it stores electrons and has ferroelectric properties, thereby reducing the electric field distribution. That is, the electric field applied to the gate 106 makes it easier to apply a voltage to this thin film layer, allowing for a lower operating voltage and improved operating speed.

[0018] In some embodiments, the semiconductor substrate 100 includes a silicon (Si) substrate or a germanium (Ge) substrate. In embodiments where the semiconductor substrate 100 is a silicon substrate, the tunnel layer 102 has a single-layer structure (not shown), and the single-layer structure is, for example, a silicon oxide layer or a silicon oxynitride layer, but is not limited thereto. The silicon substrate can also be combined with a multilayer tunnel layer 102, for example, an oxide layer-silicon nitride-oxide layer (ONO) structure. In an example where the semiconductor substrate 100 is a germanium substrate, the tunnel layer 102 may have a multilayer structure, for example, a germanium oxide layer 110 adjacent to the germanium substrate and a high-dielectric constant (high-k) material layer 112 interposed between the germanium oxide layer 110 and the ferroelectric storage layer 104. Because there are defects on the surface of the germanium substrate, the interface between the semiconductor substrate 100 and its upper layer can be improved by growing the germanium oxide layer 110 first. The high-k material layer 112 formed on the germanium oxide layer 110 has a larger energy gap, so electrons do not easily escape after being stored. In this text, "high-k material" refers to a material having a higher dielectric constant compared to silicon dioxide, and is usually a material with a dielectric constant greater than about 3.9, but may also be a material with a dielectric constant greater than about 7.0. In some examples, the material of the high-k material layer 112 includes metal oxides or metal nitrides, such as zirconium oxide, aluminum oxide, hafnium oxide, silicon nitride, silicon oxynitride, hafnium nitride (HfN), titanium oxide, tantalum oxide, zirconium oxide, zirconium silicon oxide, lanthanum oxide, yttrium oxide, strontium titanate, barium titanate, barium zirconate, lanthanum silicon oxide, aluminum silicon oxide, hafnium tantalum oxide, hafnium titanium oxide, or a combination thereof. Germanium channels formed within a germanium substrate have more thermally excited free carriers than channels formed within a silicon substrate, thus reducing the depolarization field and increasing the memory window (MW). In some embodiments, when the semiconductor substrate 100 is a p-type substrate, the doped region 108 is an n-type region.In some other embodiments, the semiconductor substrate 100 is an n-type substrate, and the doped region 108 is a p-type region.

[0019] In some embodiments, the gate 106 includes a metal gate or a gate containing a metal, and the material of the gate 106 includes, but is not limited to, titanium (Ti), titanium nitride (TiN), tantalum (Ta), tantalum nitride (TaN), tungsten (W), tungsten nitride (WN), platinum (Pt), copper (Cu), aluminum (Al), iron (Fe), nickel (Ni), cobalt (Co), chromium (Cr), beryllium (Be), antimony (Sb), iridium (Ir), molybdenum (Mo), ruthenium (Ru), osmium (Os), thorium (Th), vanadium (V), or alloys thereof. In some embodiments, if the gate 106 is selected to be a metal gate (e.g., a tungsten gate), the ferroelectric properties can be enhanced. The ferroelectric storage layer 104, which functions as a charge trapping layer, is ferroelectric, and its electric dipole can more effectively store trapped electrons. Therefore, there is no need to install a blocking layer such as an oxide layer between the gate 106 and the ferroelectric storage layer 104 below it, thus maintaining excellent data endurance and further reducing the operating voltage.

[0020] Continuing to refer to Figure 1, although the layer structure of the hybrid memory element 10 is not depicted in proportion, the relative thickness of each layer can be seen in the drawing. For example, the ferroelectric storage layer 104 is thicker than the tunnel layer 102, and the gate 106 is thicker than the ferroelectric storage layer 104. On the other hand, the germanium oxide layer 110 and the high-k material layer 112 in the tunnel layer 102 are both only a few nanometers thick, and the thickness of the germanium oxide layer 110 is not greater than the thickness of the high-k material layer 112.

[0021] Since each layer in the hybrid memory element 10 can be formed by atomic layer deposition (ALD), the hybrid memory element 10 can essentially be manufactured in the same apparatus. However, the present invention is not limited to this. In some embodiments, each layer in the hybrid memory element 10 can be deposited by different processes.

[0022] The effects of implementing the present invention will be verified by providing experimental examples below, but the present invention is not limited to the following.

[0023] <Experimental Example 1>

[0024] On a p-type Ge substrate, a 0.5 nm thick germanium oxide (GeO2) layer, a 1.2 nm thick aluminum oxide (Al2O3) layer, and a 6.5 nm thick HZO layer were continuously grown / deposited using an ALD (Advanced Laser Deposition) system. The germanium oxide and aluminum oxide layers were used as tunnel layers, and the HZO layer was used as a ferroelectric storage layer.

[0025] Next, a 50nm thick TiN layer was deposited, and a TiN metal gate was formed by patterning. Subsequently, phosphorus (P) implantation was performed to form source / drain layers in the p-type Ge substrate on both sides of the TiN metal gate. Finally, rapid thermal annealing (RTA) was performed at 500°C to activate the dopant and simultaneously crystallize the HZO, ultimately completing the hybrid memory device (labeled AlO / HZO) of Experimental Example 1.

[0026] <Experimental Example 2>

[0027] The same process as in Experimental Example 1 was used, but the aluminum oxide layer was replaced with an HfN layer. The final completed hybrid memory element of Experimental Example 2 was denoted as HfN / HZO.

[0028] <Comparative Example>

[0029] The same process as in Experimental Example 1 was used, but the HZO layer was replaced with a hafnium oxide (HfO2) layer. The final memory element of the comparative example was denoted as AlO / HfO.

[0030] <Performance Evaluation>

[0031] Figure 2 shows the PV curves for all the above elements. Among them, the AlO / HZO element (Experimental Example 1) and the HfN / HZO element (Experimental Example 2) showed a clear change in polarization amount (Pr), while the AlO / HfO element (Comparative Example) did not exhibit ferroelectric properties.

[0032] Figure 3 shows the result of applying a 5V / -3V pulse for 1μs to all of the above elements. D -V GS This is a curve diagram. As can be seen from Figure 3, the positive Vt shift of +5V in the AlO / HZO element (Experimental Example 1) and the HfN / HZO element (Experimental Example 2) indicates that the memory operation mechanism of HZO is electron trapping and not electric dipole direction switching. In other words, the operation of Experimental Examples 1 and 2 is similar to flash memory and not conventional ferroelectric memory. Furthermore, the maximum MW of Experimental Example 1 was 2.2V, which was significantly higher than that of the AlO / HfO element (Comparative Example). These results indicate that even when both HZO and HfO2 act as charge trapping layers, the presence of ferroelectricity has a significant impact on memory performance.

[0033] Figures 4 and 5 are simulation diagrams of the energy bands when the gates in Experimental Example 1 and the Comparative Example are subjected to positive and negative biases, respectively.

[0034] In Figure 4, a higher Pr value can enhance the electric field of the tunnel oxide layer, promote electron injection from the substrate to the HZO layer, shorten the electron tunneling distance, and improve charge trapping efficiency. In the erasure operation shown in Figure 5, the enhanced electric field is also advantageous for electron emission from the HZO layer to the substrate.

[0035] Figure 6 shows the threshold voltage (Vt) curves associated with the change in 5V / -3V pulse width for Experimental Example 1 and the Comparative Example. As can be seen from Figure 6, under the same pulse conditions, Experimental Example 1 showed a higher Vt shift than similar devices. Under a 1μs 5V / -3V pulse, Experimental Example 1 showed a Vt shift of approximately 2.2V, which means that the negative bias can improve the operating speed and that a larger Vt change allows for a larger MW. Figure 7 shows the switching polarization curve of Experimental Example 1 associated with the change in 5V / -3V pulse width, where 16.4μC / cm was obtained under a 1μs 5V / -3V pulse. 2 Switching polarization can be obtained.

[0036] Figure 8 shows the short-term retention results for Experimental Example 1 and the comparative example. Figure 9 shows the long-term retention results for Experimental Example 1 and the comparative example.

[0037] As can be seen in Figure 8, 10 -5 Even within the short delay time of s, both types of elements exhibited stable Vt. Furthermore, the delay time in Experimental Example 1 is far shorter than the 1s to 0.1s readout delay required by current n-FeFETs.

[0038] As can be seen from Figure 9, Experimental Example 1 maintains excellent data durability even without a blocking layer. This is because the charge trapping layer in Experimental Example 1 has ferroelectric properties, and its electric dipole can more effectively store trapped electrons, resulting in a clear MW of 1.6V even when extrapolating to the 10-year line. On the other hand, the long-term retention capability of the comparative example is insufficient.

[0039] Figure 10 shows the durability test results for the comparative example and Experimental Example 1. The aforementioned tests were performed on AlO / HZO elements and AlO / HfO elements under bipolar operating conditions of +5V / 1μs and -3V / 1μs. As can be seen from Figure 10, the AlO / HZO element was 10 7 Even after repeated cycles, the MW can be maintained at 2.0V. On the other hand, AlO / HfO elements have a small initial MW, and 10 5After repeated cycles, only 0.39V remains in MW.

[0040] In the age of artificial intelligence, high-density memory capable of realizing multi-level cells (MLCs) and mimicking synaptic activity is necessary. To verify that the present invention is applicable to MLC memory, AlO / HZO elements were subjected to 10 different Vt states. 5 After the cycle, we obtained the results shown in Figure 11 and the statistics shown in Figure 12.

[0041] As can be seen from Figures 11 and 12, the AlO / HZO element has stable multi-bit storage capability and not only realizes four clearly distinguishable Vt states, but also 10 5 Even after repeated cycles, a stable and consistent Vt readout range can be maintained, and there is no overlap in the distribution between each state, ensuring its identifiability.

[0042] Furthermore, when a continuous 1μs, 1.5V / -1.5V pulse was applied to the gate (corresponding to the presynaptic neuron) in Experimental Example 1, a corresponding current change was observed in the drain (corresponding to the postsynaptic neuron), which was recorded in Figures 13 and 14.

[0043] Figure 13 shows the change in excitatory postsynaptic current (EPSC), and Figure 14 shows the change in inhibitory postsynaptic current (IPSC). From Figures 13 and 14, we can observe EPSC / IPSC similar to those in the nervous system, demonstrating that the hybrid memory element of the present invention has potential application value in neuromorphic computing.

[0044] As described above, by utilizing a ferroelectric material as a charge trapping layer in flash memory, the present invention not only improves the operating speed of flash memory and effectively reduces the operating voltage, but also eliminates the need for a blocking oxide layer required in conventional flash memory, thereby further reducing the operating voltage. Compared with current ferroelectric memories, the hybrid memory element of the present invention avoids the limitations of read delay, has a larger memory window and multi-bit storage capability, and possesses long-term retention capability, excellent durability, and negligible read delay.

[0045] Although the present invention is disclosed by the above embodiments, these do not limit the invention, and any person with ordinary skill in the art may make some changes and modifications without departing from the spirit and scope of the invention. Therefore, the scope of protection of the present invention shall be determined by the appended claims. [Industrial applicability]

[0046] The hybrid memory element of the present invention can be used in a memory-driven neuromorphic computing device. [Explanation of symbols]

[0047] 10: Hybrid memory element 100: Semiconductor substrate 102: Tunnel layer 104: Ferroelectric storage layer 106: Gate 108: Doping Area 110: Germanium oxide layer 112:High-k material layer

Claims

1. Semiconductor substrate and A tunnel layer installed on the semiconductor substrate, Installed on the tunnel layer, enhancing the electric field of the tunnel layer, and comprising a ferroelectric storage layer containing a ferroelectric material, A gate is placed on the ferroelectric storage layer and is in direct contact with the ferroelectric storage layer, A hybrid memory element comprising a plurality of doped regions formed in the semiconductor substrate on both sides of the gate.

2. The hybrid memory element according to claim 1, wherein the ferroelectric material includes metal-doped hafnium oxide.

3. The hybrid memory element according to claim 1, wherein the semiconductor substrate includes a silicon substrate or a germanium substrate.

4. The hybrid memory element according to claim 1, wherein the tunnel layer includes a single-layer or multi-layer structure.

5. The hybrid memory element according to claim 1, wherein the gate includes a metal gate or a titanium nitride gate.

6. The hybrid memory element according to claim 1, wherein the tunnel layer comprises a high dielectric constant (high-k) material.