Nonwoven fabrics, their manufacturing methods, and uses
A nonwoven fabric using a resin composition with a rigid biodegradable resin, plasticizer, and antiblocking agent addresses flexibility and moldability issues, maintaining biodegradability and enhancing water resistance.
Patent Information
- Application Number
- JP2026024728
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-08
- Filing Date
- 2026-02-18
- Publication Date
- 2026-11-19
AI Technical Summary
Existing nonwoven fabrics made from rigid biodegradable resins like polylactic acid lack flexibility and moldability, and blending with aliphatic polyester copolymers compromises degradability and increases costs, while softening with plasticizers leads to adhesion issues during manufacturing.
A nonwoven fabric composed of biodegradable fibers formed from a resin composition containing a rigid biodegradable resin, a plasticizer, and an antiblocking agent, with 98.3 mol% or more of the resin being in the D-form or L-form, which enhances moldability and flexibility, and includes specific proportions of plasticizer and antiblocking agent to improve water resistance.
The nonwoven fabric achieves both moldability and flexibility, maintains biodegradability, and exhibits improved water resistance, making it suitable for applications like sanitary materials.
Smart Images

Figure 2026182736000003 
Figure 2026182736000004 
Figure 2026182736000001
Abstract
Description
Technical Field
[0001] The present invention relates to a nonwoven fabric comprising fibers formed from a rigid biodegradable resin composition, as well as a production method and use thereof.
Background Art
[0002] Efforts toward realizing a "low-carbon society" through reduction of greenhouse gas emissions and an "environmentally-friendly resource recycling society" are strongly demanded, and the spread of a new material "bioplastic" is accelerating to achieve these societies. In recent years, due to concerns over the depletion of petroleum resources, demand for biomass fuels is increasing more and more, and attempts to convert biomass plastics such as polylactic acid made from renewable resources into biogas containing methane by methane fermentation are attracting attention.
[0003] Among them, polylactic acid is widely used as a plant-derived and biodegradable resin, but polylactic acid is a rigid resin, and when a nonwoven fabric is produced from polylactic acid alone, the flexibility is insufficient, resulting in limited applicable uses.
[0004] Japanese Translation of PCT Application No. 2017-527706 (Patent Document 1) discloses a spunbond electret web that is a through-air bonded web comprising charged fibers in which at least a portion of the polylactic acid fibers contain about 0.1 to 6 mass% of a charging additive.
[0005] Japanese Unexamined Patent Application Publication No. 2009-203599 (Patent Document 2) discloses a polylactic acid-based nonwoven fabric formed by a spunbond method using composite fibers as constituent units, the composite fibers containing a polylactic acid-based resin with a melting point of 160°C or higher and an aliphatic polyester resin having a melting point 50°C or more lower than that of the polylactic acid-based resin.
Prior Art Documents
Patent Documents
[0006]
Patent Document 1
[0007] However, while Patent Document 1 describes the successful production of an electret web using polylactic acid via the spunbond method, there is no mention of flexibility, suggesting that it is a rigid nonwoven fabric.
[0008] On the other hand, Patent Document 2 describes the successful production of a flexible nonwoven fabric by blending polylactic acid with an aliphatic polyester copolymer. However, in the nonwoven fabric described in Patent Document 2, blending polylactic acid with an aliphatic polyester copolymer reduces the degradability of the resin composition and increases manufacturing costs.
[0009] Furthermore, the inventors attempted to manufacture nonwoven fabrics by softening rigid biodegradable resins such as polylactic acid with plasticizers and spinning them using methods such as spunbonding. However, the nonwoven fabric adhered to the rolls during the manufacturing process, making it impossible to obtain a uniform nonwoven fabric. In other words, it was difficult to achieve both moldability and flexibility in nonwoven fabrics formed from fibers containing rigid biodegradable resins.
[0010] Therefore, the object of the present invention is to provide a nonwoven fabric and a method for producing the same that can achieve both moldability and flexibility even when formed from a rigid biodegradable resin.
[0011] Another object of the present invention is to provide a nonwoven fabric and a method for producing the same that can further improve water resistance. [Means for solving the problem]
[0012] As a result of diligent research to achieve the above objectives, the present inventors have discovered that by including rigid biodegradable fibers formed from a resin composition containing a rigid biodegradable resin (A), a plasticizer (B), and an antiblocking agent (C), and by making 98.3 mol% or more of the constituent units of the rigid biodegradable resin (A) either the D-form or the L-form, it is possible to achieve both moldability and flexibility even when formed from a rigid biodegradable resin such as a polylactic acid-based resin, thus completing the present invention.
[0013] In other words, the present invention includes the following embodiments.
[0014] Embodiment [1]: A nonwoven fabric comprising biodegradable fibers formed from a resin composition comprising a rigid biodegradable resin (A), a plasticizer (B), and an antiblocking agent (C), wherein 98.3 mol% or more of the constituent units of the rigid biodegradable resin (A) are either the D-form or the L-form.
[0015] Embodiment [2]: The nonwoven fabric according to Embodiment [1], wherein the rigid biodegradable resin (A) is a polylactic acid resin.
[0016] Embodiment [3]: The nonwoven fabric according to Embodiment [2], wherein the polylactic acid resin is polylactic acid.
[0017] Embodiment [4]: The nonwoven fabric according to any of Embodiments [1] to [3], wherein the melting point of the hard biodegradable resin (A) is 165°C or higher.
[0018] Embodiment [5]: The nonwoven fabric according to any one of Embodiments [1] to [4], wherein the plasticizer (B) is an ester-based plasticizer.
[0019] Embodiment [6]: The nonwoven fabric according to any one of Embodiments [1] to [5], wherein the antiblocking agent (C) is inorganic particles with an average particle diameter of 10 μm or less.
[0020] Embodiment [7]: The nonwoven fabric according to any one of Embodiments [1] to [6], wherein the proportion of the plasticizer (B) is 5 to 20 parts by mass per 100 parts by mass of the hard biodegradable resin (A).
[0021] Embodiment [8]: The nonwoven fabric according to any one of Embodiments [1] to [7], wherein the proportion of the antiblocking agent (C) is 0.5 to 1.5 parts by mass per 100 parts by mass of the hard biodegradable resin (A).
[0022] Embodiment [9]: The nonwoven fabric according to any of Embodiments [1] to [8], wherein the average fiber diameter of the biodegradable fibers is 5 to 20 μm.
[0023] Embodiment
[10] : A nonwoven fabric according to any of Embodiments [1] to [9], which is a spunbond nonwoven fabric. Embodiment
[11] : The nonwoven fabric according to any of Embodiments [1] to
[10] , further comprising a lubricant (D).
[0024] Embodiment
[12] : The nonwoven fabric according to Embodiment
[11] , wherein the lubricant (D) is a fatty acid amide having 12 or more carbon atoms.
[0025] Embodiment
[13] : The nonwoven fabric according to Embodiment
[11] or
[12] , wherein the proportion of the lubricant (D) is 0.1 to 5 parts by mass per 100 parts by mass of the hard biodegradable resin (A).
[0026] Embodiment
[14] : A nonwoven fabric according to any of Embodiments [1] to
[13] , wherein the rigidity is 10 mN·cm or less and the water resistance is 150 mm or more.
[0027] Embodiment
[15] : A method for producing a nonwoven fabric according to any one of Embodiments [1] to
[14] , comprising a melt spinning step of melt spinning a resin composition comprising a rigid biodegradable resin (A), a plasticizer (B), and an antiblocking agent (C) to form biodegradable fibers.
[0028] Embodiment
[16] : The method according to Embodiment
[15] , further comprising a web formation step of stretching and collecting the biodegradable fibers obtained in the melt spinning step to form a web, and a heat-sealing step of heat-sealing the web to form a nonwoven fabric.
[0029] Embodiment
[17] : A sanitary material formed from a nonwoven fabric according to any of Embodiments [1] to
[14] .
[0030] Embodiment
[18] : A method of using the nonwoven fabric described in any of Embodiments [1] to
[14] by bringing it into contact with the human body.
[0031] In this specification and in the claims, the number of carbon atoms in substituents, etc., is defined as C1, C6, C 10 It is sometimes indicated in these ways. For example, "C1 alkyl group" means an alkyl group with 1 carbon atom, and "C 6-10 The term "aryl group" refers to an aryl group with 6 to 10 carbon atoms.
[0032] In this specification and in the claims, when "X~Y" is used to indicate a numerical range, it is used to mean that the end numbers X and Y are included.
[0033] In this specification and in the claims, the term "carboxylic acid component," such as lactic acid component, is used to include not only carboxylic acids but also their reactive derivatives.
[0034] In this specification and in the claims, spunbond nonwoven fabric means a nonwoven fabric obtained by the spunbond method. [Effects of the Invention]
[0035] In this invention, the nonwoven fabric contains fibers formed from a resin composition comprising a rigid biodegradable resin (A), a plasticizer (B), and an antiblocking agent (C), and by making 98.3 mol% or more of the constituent units of the rigid biodegradable resin (A) either the D-form or the L-form, both moldability and flexibility can be achieved even when formed from a rigid biodegradable resin. In particular, because the content of either the D-form or the L-form in the constituent units of the rigid biodegradable resin (A) is adjusted to 98.3 mol% or more, a uniform nonwoven fabric can be produced even if the nonwoven fabric is a spunbond nonwoven fabric, and the moldability of the nonwoven fabric can be improved. Furthermore, the nonwoven fabric of this invention also has improved water resistance, making it suitable as a sanitary material such as diapers. Moreover, by using a polylactic acid-based resin (especially polylactic acid) as the rigid biodegradable resin (A), the excellent biodegradability characteristic of polylactic acid-based resins can be maintained. [Brief explanation of the drawing]
[0036] [Figure 1] Figure 1 is a schematic diagram illustrating the method for manufacturing nonwoven fabric using the spunbond method. [Figure 2] Figure 2 is a scanning electron microscope (SEM) image (1000x magnification) of the spunbond nonwoven fabric obtained in Example 2. [Modes for carrying out the invention]
[0037] [Resin composition] The biodegradable fibers contained in the nonwoven fabric of the present invention are formed from a resin composition comprising a rigid biodegradable resin (A), a plasticizer (B), and an antiblocking agent (C).
[0038] (A) Hard biodegradable resin The rigid biodegradable resin (A) can be any resin conventionally known as a rigid biodegradable resin, for example, a resin with a flexural modulus of 1000 MPa or more.
[0039] In this specification and in the claims, the flexural modulus of the rigid biodegradable resin (A) can be measured in accordance with ISO 178.
[0040] The hard biodegradable resin (A) contains C, such as glycolic acid, lactic acid, and hydroxybutyric acid. 2-4 Hydroxymonocarboxylic acids; such as malic acid and tartaric acid. 3-5 The resin may be a biodegradable resin containing hydroxypolycarboxylic acid or the like as a polymerization component. Examples of rigid biodegradable resins include polyglycolic acid-based resins, polylactic acid-based resins, and polyhydroxybutyric acid-based resins. These rigid biodegradable resins can be used alone or in combination of two or more types, and may also be alloy resins formed by combining two or more types (or polymerization compositions) of rigid biodegradable resins, but a single type of resin is preferred. Of these, polylactic acid-based resins are preferred in terms of storage stability and versatility.
[0041] A polylactic acid-based resin can be any resin (polymer) that contains a lactic acid component as a polymerization component. The lactic acid component may be lactic acid (2-hydroxypropanoic acid or 2-hydroxypropionic acid), or a reactive derivative of lactic acid.
[0042] Lactic acid may be in the form of optical isomers (D-form, L-form) or a racemic mixture (DL-form). However, from the viewpoint of moldability of the nonwoven fabric, either the L-form (L-lactic acid) or the D-form (D-lactic acid) (especially the L-form) may be present in an amount of 98.3 mol% or more of lactic acid (lactic acid component), preferably 98.5 mol% or more, more preferably 98.7 mol% or more, more preferably 98.9 mol% or more, and most preferably 99 mol% or more.
[0043] Reactive derivatives of lactic acid include lactide (lactic acid dimer), acid anhydride, methyl ester, etc. 1-3 Examples include alkyl esters and acid halides such as acid chlorides.
[0044] These lactic acid components can be used individually or in combination of two or more. Of these lactic acid components, those containing L-lactic acid [(S)-2-hydroxypropanoic acid] or its reactive derivatives are preferred, and a combination of L-lactic acid and D-lactic acid [(R)-2-hydroxypropanoic acid] is particularly preferred.
[0045] The polylactic acid-based resin is preferably a polymer containing a lactic acid component as the main polymerization component, and may be a homopolymer of the lactic acid component (for example, poly-D-lactic acid, poly-L-lactic acid, poly-D,L-lactic acid, etc.), or a copolymer of the lactic acid component and a copolymerizable component.
[0046] Examples of the copolymerizable component that can copolymerize with the lactic acid component include diols, dicarboxylic acid components, hydroxycarboxylic acid components, and lactones.
[0047] The diol is not particularly limited, and may be any of an aliphatic diol, an alicyclic diol, and an aromatic diol, with aliphatic diols being preferred from the viewpoints of biodegradability and the like. Examples of the aliphatic diol include C such as ethylene glycol, propylene glycol, trimethylene glycol, 1,4-butanediol, 1,3-butanediol, neopentyl glycol, hexanediol, and octamethylene glycol 2-10 aliphatic diols. These diols can be used alone or in combination of two or more kinds.
[0048] Among these diols, C 2-8 aliphatic diols are preferred, and C such as ethylene glycol, 1,4-butanediol, and neopentyl glycol 2-6 alkanediols are particularly preferred.
[0049] The dicarboxylic acid component is not particularly limited, and examples thereof include aliphatic dicarboxylic acid components, alicyclic dicarboxylic acid components, and aromatic dicarboxylic acid components.
[0050] Examples of the aliphatic dicarboxylic acid include C such as oxalic acid, succinic acid, adipic acid, pimelic acid, suberic acid, azelaic acid, and sebacic acid 2-12 aliphatic dicarboxylic acids.
[0051] Examples of the alicyclic dicarboxylic acid include C such as cyclohexanedicarboxylic acid 5-10Examples include cycloalkane-dicarboxylic acids, such as decalindicarboxylic acid, norbornanedicarboxylic acid, and adamantanedicarboxylic acid, as well as di or tricycloalkanedicarboxylic acids.
[0052] Examples of aromatic dicarboxylic acids include terephthalic acid, isophthalic acid, phthalic acid, 2,6-naphthalenedicarboxylic acid, 1,8-naphthalenedicarboxylic acid, anthracenedicarboxylic acid, phenantradicarboxylic acid, etc. 6-14 Examples include arene-dicarboxylic acids.
[0053] Reactive derivatives of these dicarboxylic acids include acid anhydrides, methyl esters, and other C compounds. 1-3 Examples include alkyl esters and acid halides such as acid chlorides. These dicarboxylic acid components can be used individually or in combination of two or more.
[0054] Of these dicarboxylic acid components, C 2-8 Aliphatic dicarboxylic acids or their reactive derivatives are preferred, such as oxalic acid, succinic acid, and adipic acid. 2-6 Alkanedicarboxylic acids or their reactive derivatives are particularly preferred.
[0055] Examples of hydroxycarboxylic acid components include hydroxyaliphatic carboxylic acid components, hydroxyalicyclic carboxylic acid components, and hydroxyaromatic carboxylic acid components. Any of these may be used as the hydroxycarboxylic acid component, but hydroxyaliphatic carboxylic acid components are preferred from the standpoint of biodegradability and other factors.
[0056] The hydroxyaliphatic carboxylic acid component may be a hydroxyaliphatic carboxylic acid itself, or a reactive derivative of a hydroxyaliphatic carboxylic acid.
[0057] Examples of hydroxyaliphatic carboxylic acids include glycolic acid, 3-hydroxypropanoic acid (3HP), 2-hydroxybutyric acid (2-hydroxybutanoic acid or 2HB), 3-hydroxybutyric acid (3HB), 4-hydroxybutyric acid (4HB), 3-hydroxy-3-methylbutyric acid, 2-hydroxyvaleric acid (2-hydroxypentanoic acid), 3-hydroxyvaleric acid (3HV), 4-hydroxyvaleric acid, 5-hydroxyvaleric acid, 2-hydroxy-2-methylvaleric acid, 3-hydroxyhexanoic acid, 6-hydroxyheptanoic acid, 3-hydroxyheptanoic acid, 7-hydroxyheptanoic acid, 3-hydroxyoctanoic acid, 8-hydroxyoctanoic acid, 3-hydroxynonanoic acid, 9-hydroxynonanoic acid, 3-hydroxydecanoic acid, 10-hydroxydecanoic acid, etc. 1-6 Hydroxy C which may have an alkyl group 2-15 Examples include alkanic acids.
[0058] Examples of reactive derivatives of hydroxyaliphatic carboxylic acids include acid anhydrides, methyl esters, etc. 1-3 Examples include alkyl esters, acid halides such as acid chlorides, and lactones corresponding to hydroxyaliphatic carboxylic acids.
[0059] Examples of lactones include diC14, such as glycolide, β-propiolactone, β-dimethylpropiolactone, γ-butyrolactone, γ-dimethylbutyrolactone, δ-valerolactone, and ε-caprolactone. 1-6 C may have an alkyl group 3-15 Lactones are an example. These lactones can be used alone or in combination of two or more. Of these lactones, C 3-10 Lactones are preferred, such as glycosides, propiolactones, and caprolactones. 3-8 Lactones are particularly preferred.
[0060] These hydroxycarboxylic acid components can be used individually or in combination of two or more.
[0061] Of these hydroxycarboxylic acid components, hydroxyC2-10 Alkanic acid or its reactive derivatives are preferred, and hydroxy C 2-8 Alkanic acid or its reactive derivatives are more preferred, such as glycolic acid, 3-hydroxypropanoic acid, and other hydroxy-C 2-6 Alkanic acid or its reactive derivatives are more preferred.
[0062] These copolymer components can be used individually or in combination of two or more. Among these copolymer components, C such as ethylene glycol... 2-4 Alkanediols, adipic acid, etc. 2-6 Alkanedicarboxylic acid components, glycolic acid, and other hydroxy C 2-4 Alkanic acid components, such as glycosides and caprolactone. 4-6 Lactones are preferred. The copolymer components may be copolymer components excluding the 3-hydroxybutyric acid component.
[0063] In polylactic acid resins, the proportion of the lactic acid monomer may be the largest proportion of all constituent monomers, for example, 50 mol% or more of all constituent monomers (e.g., about 50 to 99.5 mol%), preferably 70 mol% or more (e.g., about 70 to 99 mol%), more preferably 80 mol% or more (e.g., about 80 to 98 mol%), more preferably 90 mol% or more, and most preferably 95 mol% or more. The polylactic acid resin may consist only of the lactic acid component, with polylactic acid being the most preferred. If the proportion of the lactic acid component is too low, the biodegradability of the resin composition may decrease.
[0064] The polylactic acid resin may be an alloy resin obtained by combining two or more different types (or polymerization compositions) of polylactic acid resins, but a single type of polylactic acid resin is preferred.
[0065] The polylactic acid resin (especially polylactic acid) may be present in the rigid biodegradable resin (A) in an amount of 50% by mass or more, preferably 70% by mass or more, more preferably 80% by mass or more, more preferably 90% by mass or more, and most preferably 100% by mass.
[0066] The constituent units of the rigid biodegradable resin (A) contain either the D-form or the L-form in high purity; specifically, they contain either the D-form or the L-form in an amount of 98.3 mol% or more of the total units. The content of either the D-form or the L-form in the constituent units (D-form or L-form content) greatly affects the melting point and crystallization rate. In this invention, by adjusting the D-form or L-form content in the rigid biodegradable resin (A) to a predetermined content or higher, the moldability of the nonwoven fabric can be improved, and in particular, the moldability can be greatly improved when manufacturing the nonwoven fabric by the spunbond method. The D-form or L-form content is preferably 98.5 mol% or more, more preferably 98.7 mol% or more, more preferably 98.9 mol% or more, and most preferably 99 mol% or more. If the D-form or L-form content is too low, the moldability of the nonwoven fabric decreases.
[0067] In particular, the D-isomer or L-isomer content in the rigid biodegradable resin (A) is preferably the content of polylactic acid-based resin (especially polylactic acid). When the content is polylactic acid-based resin (especially polylactic acid), the D-isomer or L-isomer content within the above range may be either the D-isomer or the L-isomer content, but from the viewpoint of biodegradability, it is preferable that the L-isomer content is (i.e., that the L-isomer is of high purity).
[0068] In this specification and in the claims, the D-isomer or L-isomer content in the constituent units of the rigid biodegradable resin (A) can be directly measured by hydrolyzing a freeze-dried resin (especially a polylactic acid-based resin such as polylactic acid) under alkaline conditions and analyzing the monomer component peak (lactic acid in the case of polylactic acid) using high-performance liquid chromatography (HPLC) and an optical isomer separation column.
[0069] The melt flow rate (MFR) of rigid biodegradable resin (A) (particularly polylactic acid-based resins such as polylactic acid) is, for example, 1 to 100 g / 10 min, preferably 10 to 50 g / 10 min, more preferably 15 to 45 g / 10 min, more preferably 20 to 40 g / 10 min, and most preferably 25 to 35 g / 10 min, under conditions of a temperature of 190°C and a load of 2.16 kgf. If the MFR is too low, the moldability of the resin composition may decrease, and conversely, if it is too high, the mechanical properties of the resin composition may decrease.
[0070] The weight-average molecular weight Mw of the rigid biodegradable resin (A) (especially polylactic acid-based resins such as polylactic acid) can be selected from the range of 1,000 to 1,000,000, for example, 5,000 to 1,000,000, preferably 10,000 to 800,000, more preferably 20,000 to 700,000, more preferably 30,000 to 600,000, and most preferably 50,000 to 500,000.
[0071] In this specification and in the claims, the weight-average molecular weight Mw of the rigid biodegradable resin (A) can be measured using gel permeation chromatography (GPC) by the polystyrene equivalent method.
[0072] The glass transition temperature (Tg) of the rigid biodegradable resin (A) (especially polylactic acid-based resins such as polylactic acid) is, for example, 40 to 80°C, preferably 45 to 75°C, more preferably 50 to 70°C, more preferably 55 to 65°C, and most preferably 57 to 62°C. If the glass transition temperature is too low, the heat resistance and mechanical properties of the resin composition may decrease, and conversely, if it is too high, the biodegradability and moldability of the resin composition may decrease. The rigid biodegradable resin (A) (especially polylactic acid-based resins) may be crystalline.
[0073] The melting point of rigid biodegradable resin (A) (especially polylactic acid-based resins such as polylactic acid) is, for example, 100°C or higher (e.g., 100-250°C), preferably 150°C or higher (e.g., 150-200°C), more preferably 160°C or higher (e.g., 160-180°C), more preferably 165°C or higher (e.g., 165-175°C), and most preferably 167°C or higher (e.g., 167-173°C). If the melting point is too low, the moldability and heat resistance of the resin composition may decrease, and conversely, if it is too high, the moldability of the resin composition may decrease.
[0074] In this specification and in the claims, the glass transition temperature and melting point of resins such as rigid biodegradable resin (A) can be measured using a differential scanning calorimeter (DSC).
[0075] The acid value of the rigid biodegradable resin (A) (especially polylactic acid-based resins such as polylactic acid) may be, for example, 0 to 100 mg KOH / g (e.g., 0.1 to 80 mg KOH / g), preferably 0.2 to 80 mg KOH / g, more preferably 0.3 to 60 mg KOH / g, and especially around 0.5 to 30 mg KOH / g. If the acid value is too high, hydrolysis may occur easily. The hydroxyl value of the rigid biodegradable resin (A) (especially polylactic acid-based resins) can also be selected from a range similar to that of the acid value.
[0076] The proportion of rigid biodegradable resin (A) (especially polylactic acid-based resins such as polylactic acid) may be 30% by mass or more (especially 50% by mass or more) in the resin composition, for example, 50-99% by mass, preferably 70-95% by mass, more preferably 75-93% by mass, more preferably 80-90% by mass, and most preferably 83-87% by mass. If the proportion of rigid biodegradable resin (A) is too low, there is a risk that the biodegradability and other properties will decrease.
[0077] (B) Plasticizer The resin composition further contains a plasticizer (B) to improve flexibility. The plasticizer (B) can be selected from conventional plasticizers depending on the type of rigid biodegradable resin (A), and if the rigid biodegradable resin (A) is a polylactic acid-based resin, it may be a conventional plasticizer used for polyester-based resins.
[0078] Conventional plasticizers include ester-based plasticizers such as aliphatic dicarboxylic acid esters, aromatic dicarboxylic acid esters, oxycarboxylic acid esters, and polyhydric alcohol fatty acid esters; phosphate ester-based plasticizers such as aliphatic phosphate esters, aromatic phosphate esters, and condensed phosphate esters; epoxy-based plasticizers such as alkyl epoxy stearates; amide-based plasticizers such as sulfonamides; and oligomeric plasticizers such as ester oligomers and amide oligomers. These plasticizers can be used individually or in combination of two or more.
[0079] Of these plasticizers, ester-based plasticizers and oligomeric plasticizers such as ester oligomers are preferred, and ester-based plasticizers are particularly preferred, from the viewpoint of compatibility with hard biodegradable resin (A).
[0080] Preferred ester-based plasticizers include polycarboxylic acid esters and polyhydric alcohol esters.
[0081] The polycarboxylic acid ester may also be a dicarboxylic acid ester, or a polycarboxylic acid ester having three or more carboxyl groups.
[0082] Examples of dicarboxylic acid esters include aliphatic dicarboxylic acid esters and aromatic dicarboxylic acid esters.
[0083] Examples of aliphatic dicarboxylic acid esters include aliphatic dialkyl dicarboxylic acids, diesters of aliphatic dicarboxylic acids with glycol ethers, and diesters of aliphatic dicarboxylic acids with aralkyl alcohols and (poly)alkylene glycol monoalkyl ethers.
[0084] Examples of aliphatic dialkyl dicarboxylates include dibutyl adipate, dioctyl adipate, di-2-ethylhexyl adipate, isononyl adipate, diisodecyl adipate, dibutyl sebacate, dioctyl sebacate, diethyl azelaate, dibutyl azelaate, and di-2-ethylhexyl azelaate. 2-10 Aliphatic dicarboxylic acid diC 1-18 Alkyl (especially C 4-10 Alkanedicarboxylic acid diC 4-14 Examples include alkyl esters.
[0085] Diesters of aliphatic dicarboxylic acids and glycol ethers include diesters of aliphatic dicarboxylic acids and (poly)alkylene glycol monoalkyl ethers, such as bis(methyldiethylene glycol) adipate [or di(methoxyethoxyethyl) adipate], bis(butyldiethylene glycol) adipate, bis(methyldiethylene glycol) succinate, methyldiethylene glycol ethyl diethylene glycol adipate (or methoxyethoxyethyl / ethoxyethoxyethyl adipate), methyldiethylene glycol butyldiethylene glycol adipate, etc. 2-10 Aliphatic dicarboxylic acids and di or tetraC 2-4 Alkylene glycol mono C 1-4 Examples include diesters with alkyl ethers.
[0086] Examples of diesters of aliphatic dicarboxylic acids with aralkyl alcohols and (poly)alkylene glycol monoalkyl ethers include benzyl methyl diethylene glycol adipate (or methoxyethoxyethyl benzyl adipate), benzyl ethyl diethylene glycol adipate, benzyl butyl diethylene glycol adipate, benzyl methyl diglycol succinate, benzyl butyl diglycol succinate, and other C21 compounds. 2-10 Aliphatic dicarboxylic acids and C 6-10 Aryl C 1-4 Alkyl alcohols and C2-4 Alkylene glycol mono C 1-4 Examples include diesters with alkyl ethers.
[0087] Examples of aromatic dicarboxylic acid esters include dialkyl aromatic dicarboxylic acids, alkyl aralkyl aromatic dicarboxylic acid esters, and diesters of aromatic dicarboxylic acids and glycol ethers.
[0088] Examples of dialkyl aromatic dicarboxylates include dimethyl phthalate, diethyl phthalate, dibutyl phthalate, dihexyl phthalate, dioctyl phthalate, di-2-ethylhexyl phthalate, and diisodecyl phthalate. 8-14 Allene dicarboxylate diC 1-12 Alkyl esters (especially benzenedicarboxylic acid C) 4-8 Examples include alkyl esters.
[0089] Examples of aromatic alkyl dicarboxylates include C14, such as butyl benzyl phthalate. 8-14 Allenedicarboxylic acid C 1-12 Alkyl C 6-10 Aryl C 1-4 Examples include alkyl esters.
[0090] Diesters of aromatic dicarboxylic acids and glycol ethers include diesters of aromatic dicarboxylic acids and (poly)alkylene glycol monoalkyl ethers, such as bis(methyldiethylene glycol) phthalate (or di(methoxyethyl) phthalate). 8-14 Allene dicarboxylic acid (especially C 8-12 (alenedicarboxylic acid) and di or tetraC 2-4 Alkylene glycol mono C 1-4 Examples include diesters with alkyl ethers.
[0091] Polycarboxylic acid esters having three or more carboxyl groups may also be esters of aliphatic or aromatic carboxylic acids having approximately 3 to 8 (particularly 3 to 6) carboxyl groups. Examples of such polycarboxylic acid esters include citrate esters such as tributyl citrate, tributyl acetyl citrate, and tri-2-ethylhexyl acetyl citrate; trimellitic acid esters such as trimethyl trimellitic acid, triethyl trimellitic acid, trioctyl trimellitic acid, and tri-2-ethylhexyl trimellitic acid; and pyromellitic acid esters such as tetraoctyl pyromellitic acid.
[0092] The polyhydric alcohol ester may be an ester of a polyhydric alcohol having three or more hydroxyl groups and a fatty acid. Examples of the polyhydric alcohol include alcohols having about 3 to 6 hydroxyl groups, such as sucrose, glycerin, diglycerin, trimethylolethane, trimethylolpropane, pentaerythritol, dipentaerythritol, and sorbitol. An example of the polyhydric alcohol fatty acid ester is glycerin diacetate mono-C. 8-10 (Poly)C such as alkyl esters, triacetin, diglycerin tetraacetate 3-10 Alkane polyol mono or hexa C 2-10 Examples include alcanoates.
[0093] These ester-based plasticizers can be used individually or in combination of two or more. Among these ester-based plasticizers, aliphatic dicarboxylic acid esters are preferred from the viewpoint of biodegradability, etc. Furthermore, among aliphatic dicarboxylic acid esters, C such as adipic acid esters are preferred. 4-8 Alkanedicarboxylic acid esters are preferred, as they easily achieve both flexibility and hydrolysis resistance in the hard biodegradable resin (A), C 4-8 Alkanedicarboxylic acids and C 6-10 Aryl C 1-4 Alkyl alcohols and mono- or tri-C alcohols 2-4 Alkylene glycol mono C 1-4 Diesterification with alkyl ether is even more preferred, C 5-7Alkanedicarboxylic acids and phenyl C 1-3 Alkyl alcohols and mono or diC 2-3 Alkylene glycol mono C 1-3 Diesterification with alkyl ether is even more preferred, C 5-7 Alkanedicarboxylic acids and phenyl C 1-2 Alkyl alcohols and diethylene glycol monoC 1-2 Diesterification with alkyl ether is most preferred.
[0094] The weight-average molecular weight Mw of the plasticizer (B) may be less than 2000 (particularly 1500 or less), for example, 100 to 1500, preferably 200 to 1000, more preferably 300 to 800, and more preferably 400 to 500.
[0095] In this specification and in the claims, the weight-average molecular weight Mw of the plasticizer (B) can be measured by the polystyrene-to-polystyrene method using gel permeation chromatography (GPC).
[0096] The proportion of plasticizer (B) can be selected from a range of about 1 to 50 parts by mass per 100 parts by mass of hard biodegradable resin (A) (especially polylactic acid-based resins such as polylactic acid), for example, 3 to 30 parts by mass, preferably 5 to 20 parts by mass, more preferably 10 to 20 parts by mass, more preferably 13 to 18 parts by mass, and most preferably 14 to 17 parts by mass. If the proportion of plasticizer (B) is too low, the flexibility of the nonwoven fabric may decrease, and if it is too high, the biodegradability and strength of the nonwoven fabric may decrease.
[0097] The proportion of plasticizer (B) may be 1 to 35% by mass in the resin composition, preferably 3 to 30% by mass, more preferably 5 to 25% by mass, more preferably 8 to 20% by mass, and most preferably 10 to 15% by mass.
[0098] (C) Anti-blocking agent (blocking prevention agent) The resin composition further contains an antiblocking agent (C) to improve the moldability and water resistance of the nonwoven fabric. The antiblocking agent (C) can be any particles formed from a component having a melting point or softening point higher than the melt spinning temperature, and is added to prevent blocking between fibers and improve the moldability of the nonwoven fabric. Surprisingly, in this invention, in addition to the moldability of the nonwoven fabric, the water resistance can also be improved.
[0099] Examples of antiblocking agents (C) include inorganic particles such as silica, alumina, talc, mica, titanium dioxide, and calcium carbonate; organic particles such as high heat-resistant thermoplastic resin particles like engineering plastics, crosslinked resin particles (such as crosslinked acrylic resin particles and crosslinked melamine resin particles), and thermosetting resin particles. These antiblocking agents can be used alone or in combination of two or more. Of these, inorganic particles such as silica are preferred.
[0100] Examples of the antiblocking agent (C) include spherical (perfectly spherical or nearly spherical), ellipsoidal, rod-shaped or rod-shaped, cylindrical or conical, polyhedral [for example, polygonal prisms such as cubes and rectangular prisms; polygonal pyramidal shapes such as triangular pyramidal and square pyramidal pyramidal shapes], flake-shaped, fibrous, dendritic, and irregular shapes. Of these, granular shapes such as spherical and irregular shapes are commonly used, and spherical shapes are preferred, with perfectly spherical shapes being particularly preferred, as they can improve the moldability of the nonwoven fabric.
[0101] The average particle size of the antiblocking agent (C) may be 20 μm or less (particularly 10 μm or less), for example, 0.1 to 20 μm, preferably 1 to 15 μm, more preferably 3 to 10 μm, more preferably 4 to 8 μm, and most preferably 5 to 7 μm. If the average particle size of the antiblocking agent (C) is too small, the moldability and water resistance of the nonwoven fabric may decrease, and if it is too large, the mechanical properties of the nonwoven fabric may decrease.
[0102] In this specification and in the claims, the average particle size of the antiblocking agent (C) can be measured by the Coulter counter method.
[0103] The average particle size of the antiblocking agent (C) is preferably 1 or less (particularly 0.8 or less) of the average fiber diameter of the biodegradable fibers, for example, 0.03 to 1, preferably 0.05 to 0.9, more preferably 0.1 to 0.8, more preferably 0.2 to 0.7, and most preferably 0.3 to 0.6. If this ratio is too small, the moldability and water resistance of the nonwoven fabric may decrease, and if it is too large, the mechanical properties of the nonwoven fabric may decrease.
[0104] The proportion of the antiblocking agent (C) may be 5 parts by mass or less (particularly 3 parts by mass or less) per 100 parts by mass of the hard biodegradable resin (A) (especially polylactic acid-based resins such as polylactic acid), and can be selected from a range of about 0.1 to 5 parts by mass, for example 0.1 to 2 parts by mass, preferably 0.3 to 1.7 parts by mass, more preferably 0.5 to 1.5 parts by mass, more preferably 0.7 to 1.4 parts by mass, and most preferably 0.8 to 1.2 parts by mass. If the proportion of the antiblocking agent (C) is too low, the moldability and water resistance of the nonwoven fabric may decrease, and if it is too high, the biodegradability and strength of the nonwoven fabric may decrease.
[0105] The proportion of the antiblocking agent (C) may be 0.1 to 3% by mass in the resin composition, preferably 0.2 to 2% by mass, more preferably 0.3 to 1.7% by mass, more preferably 0.5 to 1.5% by mass, and most preferably 0.7 to 1.4% by mass.
[0106] (D) Lubricant (slip agent) The resin composition preferably further contains a lubricant (D) to improve the water resistance of the nonwoven fabric. Lubricants (or slip agents) are usually added to reduce friction and improve moldability, but in this invention, surprisingly, the water resistance of the nonwoven fabric can be improved by adding a lubricant (D). In particular, the water resistance of the nonwoven fabric tends to decrease when a plasticizer (B) is added, but the water resistance of the nonwoven fabric can be improved when a lubricant (D) is added. Therefore, by combining a plasticizer (B), an antiblocking agent (C), and a lubricant (D), it is possible to produce a nonwoven fabric that simultaneously satisfies moldability, flexibility, and water resistance.
[0107] Examples of lubricants (D) include fatty acids or their derivatives, such as stearic acid and coconut oil fatty acids; silicon dioxide, such as hydrated silicon dioxide and silicon dioxide; polyorganosiloxanes, such as dimethylpolysiloxane; oils and fats, such as hydrogenated oil and cocoa butter; and waxes, such as beeswax, bleached beeswax, carnauba wax, lanolin, paraffin, and petrolatum. These lubricants can be used alone or in combination of two or more. Among these lubricants, fatty acids or their derivatives are preferred, and higher fatty acids or their derivatives are particularly preferred, as they easily improve the water resistance of the nonwoven fabric.
[0108] The higher fatty acid may be a fatty acid with 12 or more carbon atoms. The carbon number of the higher fatty acid is, for example, 12 to 30, preferably 14 to 28, more preferably 16 to 26, more preferably 18 to 24, and most preferably 20 to 23. If the carbon number of the higher fatty acid is too small, the water resistance of the nonwoven fabric may decrease.
[0109] Examples of higher fatty acids include lauric acid, myristic acid, palmitic acid, stearic acid, hydroxystearic acid, arachidic acid, behenic acid, lignoceric acid, cerotic acid, and montanic acid. 12-30 Saturated fatty acids; such as dodeca-9-enoic acid (9-dodecenoic acid), myristoleic acid, palmitoleic acid, petroseric acid, oleic acid, vaccenic acid, linoleic acid, linolenic acid, eleostearic acid, gatolenic acid, arachidonic acid, erucic acid (erucic acid), etc. 12-30Examples include unsaturated fatty acids. These higher fatty acids can be used individually or in combination of two or more. Of these, C 18-26 Fatty acids are preferred, C 20-24 Fatty acids are particularly preferred.
[0110] Examples of derivatives of higher fatty acids include higher fatty acid metal salts, higher fatty acid alkyl esters, and higher fatty acid amides. Among higher fatty acids and their derivatives, higher fatty acid metal salts, higher fatty acid alkyl esters, and higher fatty acid amides are preferred, with higher fatty acid amides being particularly preferred, because they easily improve the water resistance of nonwoven fabrics.
[0111] Preferred higher fatty acid amides include C such as stearic acid amide. 14-28 Saturated fatty acid amide (preferably C 16-28 Saturated fatty acid amide, more preferably C 18-26 Saturated fatty acid amides, more preferably C 20-24 C (saturated fatty acid amides), oleic acid amides, erucic acid amides, etc. 14-28 Unsaturated fatty acid amides (preferably C 16-28 Unsaturated fatty acid amides, more preferably C 18-26 Unsaturated fatty acid amides, more preferably C 20-24 Examples include unsaturated fatty acid amides.
[0112] The proportion of lubricant (D) may be 5 parts by mass or less (particularly 3 parts by mass or less) per 100 parts by mass of hard biodegradable resin (A) (especially polylactic acid-based resins such as polylactic acid), and can be selected from a range of about 0.01 to 5 parts by mass, for example 0.05 to 3 parts by mass, preferably 0.1 to 2 parts by mass, more preferably 0.2 to 1.5 parts by mass, more preferably 0.3 to 1 part by mass, and most preferably 0.4 to 0.7 parts by mass. If the proportion of lubricant (D) is too low, the water resistance of the nonwoven fabric may decrease, and if it is too high, the biodegradability and strength of the nonwoven fabric may decrease.
[0113] The proportion of lubricant (D) may be 0.05 to 3% by mass in the resin composition, preferably 0.1 to 2% by mass, more preferably 0.2 to 1.5% by mass, more preferably 0.3 to 1% by mass, and most preferably 0.4 to 0.7% by mass.
[0114] (E) Other ingredients The resin composition may further contain conventional additives that are incorporated into the fibers as other components. Examples of conventional additives include stabilizers (anti-aging agents, antioxidants, ozone degradation inhibitors, ultraviolet absorbers, light stabilizers, heat stabilizers such as copper compounds, etc.), flame retardants (phosphorus-based flame retardants, halogen-based flame retardants, inorganic flame retardants, etc.), flame retardant enhancers, impact resistance improvers, lubricants, matting agents, heat storage agents, fragrances, fluorescent whitening agents, wetting agents, flowability improvers, leveling agents, thickeners, defoaming agents, mold release agents, color improvers, dispersants, compatibilizers, stress reduction agents, antistatic agents, crystal nucleating agents, colorants such as dyes and pigments, antibacterial agents, preservatives, insecticides and mite repellents, and fungicides. These additives can be used individually or in combination of two or more.
[0115] The total proportion of the other components may be 100 parts by mass or less (for example, 0.1 to 100 parts by mass) per 100 parts by mass of the hard biodegradable resin (A) (especially polylactic acid-based resins such as polylactic acid), preferably 50 parts by mass or less (for example, 1 to 50 parts by mass), more preferably 30 parts by mass or less, more preferably 10 parts by mass or less, and most preferably 5 parts by mass or less.
[0116] (F) Properties of the resin composition The resin composition contains a plasticizer (B) and therefore exhibits excellent melt flowability. The melt flow rate (MFR) of the resin composition, under conditions of a temperature of 190°C and a load of 2.16 kgf, is, for example, 30 to 200 g / 10 min, preferably 50 to 150 g / 10 min, more preferably 100 to 140 g / 10 min, more preferably 120 to 135 g / 10 min, and most preferably 125 to 130 g / 10 min. If the MFR is too low, spinnability may decrease, and conversely, if it is too high, the mechanical properties of the biodegradable fiber may decrease.
[0117] [Non-woven fabric] The nonwoven fabric of the present invention includes biodegradable fibers formed from the resin composition. The cross-sectional shape of the biodegradable fibers (the cross-sectional shape perpendicular to the length direction of the fibers) is not limited to a general solid cross-sectional shape such as a round cross-section or an irregular cross-section [flat, elliptical, polygonal, etc.], but may also be a hollow cross-sectional shape, but a solid round cross-sectional shape is preferred.
[0118] The average fiber diameter of the biodegradable fibers can be selected from a range of approximately 1 to 100 μm, for example, 3 to 50 μm, preferably 5 to 20 μm, more preferably 7 to 18 μm, more preferably 8 to 16 μm, and most preferably 10 to 15 μm. If the average fiber diameter of the biodegradable fibers is too small, the strength of the nonwoven fabric may decrease, and if it is too large, the flexibility may decrease.
[0119] In this specification and in the claims, the average fiber diameter of biodegradable fibers is the average value of fiber diameters measured at any 10 locations based on photographs observed with a scanning electron microscope (SEM).
[0120] Biodegradable fibers may be short fibers with an average fiber length of about 10 to 100 mm, but from the standpoint of the strength of the nonwoven fabric, long fibers (substantially continuous filaments) with an average fiber length of more than 100 mm are preferred.
[0121] In addition to biodegradable fibers, the nonwoven fabric may further contain other fibers, provided that they do not impair the effects of the present invention. Examples of other fibers include soft biodegradable fibers formed from soft biodegradable resins, polyolefin fibers (e.g., polyethylene fibers, polypropylene fibers, etc.), vinyl alcohol fibers (e.g., ethylene-vinyl alcohol copolymer fibers, etc.), acrylic fibers (e.g., acrylonitrile fibers, etc.), polyester fibers (e.g., polyethylene terephthalate fibers, polybutylene terephthalate fibers, etc.), polyamide fibers (e.g., polyamide 6 fibers, polyamide 66 fibers, etc.), polyurethane fibers (e.g., polyester polyol type urethane fibers, etc.), cellulose fibers [e.g., natural fibers (cotton, wool, silk, hemp, etc.), semi-synthetic fibers (acetate fibers such as triacetate fibers, etc.), regenerated fibers (rayon, polynosic, cupro, lyocell (e.g., registered trademark name: "Tencel"), etc.)]. These other fibers can be used individually or in combination of two or more types. Of these, soft biodegradable fibers and cellulose fibers are preferred due to their excellent biodegradability.
[0122] The proportion of other fibers may be 100 parts by mass or less per 100 parts by mass of biodegradable fiber, preferably 50 parts by mass or less, more preferably 30 parts by mass or less, more preferably 10 parts by mass or less, and most preferably 5 parts by mass or less.
[0123] The proportion of biodegradable fibers may be 50% by mass or more in the nonwoven fabric, preferably 80% by mass or more, more preferably 90% by mass or more, more preferably 95% by mass or more, and most preferably 99% by mass or more. The nonwoven fabric may be made up solely of biodegradable fibers.
[0124] Examples of nonwoven fabrics of the present invention include long-fiber nonwoven fabrics such as spunbond nonwoven fabrics, meltblown nonwoven fabrics, and flash-spun nonwoven fabrics; and short-fiber nonwoven fabrics such as spunlace nonwoven fabrics, airlace nonwoven fabrics, thermal-bonded nonwoven fabrics, needle-punched nonwoven fabrics, and chemical-bonded nonwoven fabrics. Of these, long-fiber nonwoven fabrics are preferred, and spunbond nonwoven fabrics are particularly preferred, as they offer the greatest benefits of the present invention.
[0125] The nonwoven fabric of the present invention has excellent flexibility, and its rigidity may be 10 mN·cm or less (for example, 0.01 to 10 mN·cm), preferably 8 mN·cm or less (for example, 0.03 to 8 mN·cm), more preferably 6 mN·cm or less (for example, 0.05 to 6 mN·cm), and more preferably 5 mN·cm or less (for example, 0.1 to 5 mN·cm). If the rigidity of the nonwoven fabric is too high, there is a risk that the flexibility of the nonwoven fabric will decrease.
[0126] When the nonwoven fabric of the present invention is a spunbond nonwoven fabric, the stiffness of the nonwoven fabric in the MD direction (fiber stretching direction and web transport direction) is, for example, 5 mN·cm or less (e.g., 0.01 to 5 mN·cm), preferably 1 mN·cm or less (e.g., 0.05 to 1 mN·cm), and more preferably 0.5 mN·cm or less (e.g., 0.1 to 0.5 mN·cm). The stiffness of the nonwoven fabric in the TD direction (direction perpendicular to the stretching direction and transport direction) is, for example, 12 mN·cm or less (e.g., 0.5 to 12 mN·cm), preferably 10 mN·cm or less (e.g., 1 to 10 mN·cm), and more preferably 8 mN·cm or less (e.g., 3 to 8 mN·cm).
[0127] In this specification and in the claims, the rigidity of the nonwoven fabric can be measured in accordance with ISO 9073-7, and in detail, it can be measured by the method described in the examples below.
[0128] The tensile elongation of the nonwoven fabric of the present invention is, for example, 5% or more (e.g., 5-100%), preferably 8% or more (e.g., 8-70%), and more preferably 10% or more (e.g., 10-50%). If the tensile elongation of the nonwoven fabric is too low, the flexibility of the nonwoven fabric may decrease.
[0129] When the nonwoven fabric of the present invention is a spunbond nonwoven fabric, the tensile elongation of the nonwoven fabric in the MD direction is, for example, 5% or more (e.g., 5-50%), preferably 8% or more (e.g., 8-30%), and more preferably 10% or more (e.g., 10-20%). The tensile elongation of the nonwoven fabric in the TD direction is, for example, 10% or more (e.g., 10-70%), preferably 15% or more (e.g., 15-50%), and more preferably 20% or more (e.g., 20-40%).
[0130] The tensile strength of the nonwoven fabric of the present invention is, for example, 3N or more (e.g., 3 to 100N), preferably 5N or more (e.g., 5 to 80N), and more preferably 8N or more (e.g., 8 to 70N). If the tensile strength of the nonwoven fabric is too low, there is a risk that the mechanical properties of the nonwoven fabric will deteriorate.
[0131] When the nonwoven fabric of the present invention is a spunbond nonwoven fabric, the tensile strength of the nonwoven fabric in the MD direction is, for example, 10N or more (e.g., 10 to 100N), preferably 30N or more (e.g., 30 to 80N), and more preferably 50N or more (e.g., 50 to 70N). The tensile strength of the nonwoven fabric in the TD direction is, for example, 3N or more (e.g., 3 to 30N), preferably 5N or more (e.g., 5 to 20N), and more preferably 8N or more (e.g., 8 to 10N).
[0132] In this specification and in the claims, the tensile strength and tensile elongation of the nonwoven fabric can be measured in accordance with the JIS L 1096A method (cut-slip method), and in detail, they can be measured by the method described in the examples below.
[0133] The tear strength of the nonwoven fabric of the present invention is, for example, 1N or more (e.g., 1 to 100N), preferably 2N or more (e.g., 2 to 50N), and more preferably 3N or more (e.g., 3 to 30N). The nonwoven fabric of the present invention can achieve both flexibility and tear strength. If the tear strength of the nonwoven fabric is too low, there is a risk that the mechanical properties of the nonwoven fabric will deteriorate.
[0134] When the nonwoven fabric of the present invention is a spunbond nonwoven fabric, the tear strength of the nonwoven fabric in the MD direction is, for example, 1N or more (e.g., 1 to 20N), preferably 2N or more (e.g., 2 to 10N), and more preferably 3N or more (e.g., 3 to 8N). The tear strength of the nonwoven fabric in the TD direction is, for example, 5N or more (e.g., 5 to 100N), preferably 10N or more (e.g., 10 to 50N), and more preferably 15N or more (e.g., 15 to 30N).
[0135] In this specification and in the claims, the tear strength of the nonwoven fabric can be measured in accordance with the trapezoid method of JIS L 1913, and in detail, it can be measured by the method described in the examples below.
[0136] The water resistance of the nonwoven fabric of the present invention is 110 mm or more (e.g., 110 to 1000 mm), preferably 130 mm or more (e.g., 130 to 500 mm), more preferably 150 mm or more (e.g., 150 to 300 mm), more preferably 170 mm or more (e.g., 170 to 250 mm), and most preferably 180 mm or more (e.g., 180 to 230 mm). If the water resistance of the nonwoven fabric is too low, there is a risk that the water resistance of the nonwoven fabric will decrease.
[0137] In this specification and in the claims, the water resistance of the nonwoven fabric can be measured in accordance with the JIS L 1092A method.
[0138] The basis weight of the nonwoven fabric of the present invention can be appropriately selected depending on the application, for example, 5 to 10,000 g / m². 2 You can choose from a range of degrees, for example, 7-1000 g / m². 2 Preferably 8-500 g / m² 2 More preferably 10-100 g / m² 2 Comfortably 15-50g / m 2 Most preferably 18-30 g / m² 2 That is the case.
[0139] The apparent density of the nonwoven fabric of the present invention is, for example, 0.0001 to 0.1 g / cm³. 3 Preferably 0.0005 to 0.05 g / cm³ 3More preferably 0.001 to 0.01 g / cm³ 3 That is the case.
[0140] The thickness of the nonwoven fabric of the present invention is, for example, 0.01 to 2 mm, preferably 0.02 to 1 mm, and more preferably 0.05 to 0.5 mm.
[0141] [Manufacturing method for nonwoven fabrics] The method for producing the nonwoven fabric of the present invention is any method that includes a melt-spinning step to form biodegradable fibers by melt-spinning a resin composition containing a rigid biodegradable resin (A), a plasticizer (B), and an antiblocking agent (C) (or a resin composition further containing additives such as a lubricant (D) as needed), and can be produced by conventional methods depending on the type of nonwoven fabric.
[0142] If the nonwoven fabric of the present invention is a spunbond nonwoven fabric, the method for manufacturing the nonwoven fabric of the present invention may include the melt spinning step, the web formation step of stretching and collecting the biodegradable fibers obtained in the melt spinning step to form a web, and the heat-sealing step of heat-sealing the web to form a nonwoven fabric.
[0143] An example of the spunbond method for manufacturing spunbond nonwoven fabrics will be explained using Figure 1.
[0144] The resin composition for forming biodegradable fibers is usually in pellet form and is melt-kneaded using an extruder or the like before being supplied to the spinneret 1. As shown in Figure 1, the melted resin composition supplied to the spinneret 1 is extruded from the spinneret 1 as biodegradable fibers 2 in the melt-spinning process and then cooled.
[0145] The spunbond method is a direct method in which the spinning process and the web formation process are directly linked. In the web formation process, the fibers 2 obtained in the spinning process are stretched by an ejector 3 to become biodegradable fibers 4 that are smaller in diameter than the fibers 2, and then accumulated on a collection net of a net conveyor 8 to form a web 5. The web 5 may also be collected from the bottom of the collection net using a suction collector (suction device).
[0146] The obtained web 5 is transported by a net conveyor 8 to a pair of heat rolls 9 and 10 and subjected to a heat-sealing process. The heat rolls 9 and 10 used in the heat-sealing process are formed by a combination of an embossed heat roll 9 with an embossed surface and a flat heat roll 10 with a smooth surface. In the heat-sealing process, the web 5 is heat-sealed by passing between the pair of heat rolls 9 and 10 to form a nonwoven fabric 6 with an embossed surface. Finally, the obtained nonwoven fabric 6 is wound up by a winder (winding machine) 11 and recovered as a roll 7.
[0147] In such spunbond methods, when using rigid biodegradable resins such as polylactic acid softened with a plasticizer, the pellets stick together at low temperatures, making them difficult to handle and hindering the efficient melt-spinning of the plasticizer-softened rigid biodegradable resin continuously. In contrast, the nonwoven fabric of the present invention contains an anti-blocking agent (C) in addition to the plasticizer (B) in the resin composition, so that the pellets do not stick together and biodegradable fibers can be produced with high productivity. However, when an anti-blocking agent is added to a rigid biodegradable resin softened with a plasticizer, the sticking of pellets together is suppressed, but in the heat-sealing process, the web tends to stick to the heat rolls, such as embossing heat rolls, making it difficult to produce a uniform nonwoven fabric. In contrast, when a rigid biodegradable resin (A) containing either the D-form or L-form in high purity is used, the sticking of the web to the heat rolls can be suppressed, and a uniform nonwoven fabric can be produced. It is presumed that by increasing the purity of the D or L form, the crystallization rate of the rigid biodegradable resin is improved, and in the web formation process, the oriented crystallization of the resin composition containing the rigid biodegradable resin (A), plasticizer (B), and antiblocking agent (C) progresses, thereby suppressing the web from sticking to the hot roll.
[0148] In this spunbond method, a resin composition containing a rigid biodegradable resin (A), a plasticizer (B), and an antiblocking agent (C) is melt-kneaded using a conventional mixer (e.g., a melt-kneading extruder) that supplies the mixture to a spinneret. The melting temperature can be selected depending on the type of rigid biodegradable resin (A), but in the case of polylactic acid-based resins such as polylactic acid, it is, for example, 150 to 250°C, preferably 150 to 220°C, and more preferably 160 to 200°C.
[0149] The resin composition, melted and kneaded by a mixer, is supplied to the spinneret of a spinneret. The spinneret typically has a row of spinning holes, with the spacing between the holes being, for example, 100 to 10,000 holes / m, preferably 500 to 7,000 holes / m, and more preferably 1,000 to 5,000 holes / m.
[0150] The single-hole discharge rate when extruding the resin composition from the spinneret is, for example, 0.01 to 5 g / (hole·min), preferably 0.1 to 3 g / (hole·min), more preferably 0.2 to 1 g / (hole·min), more preferably 0.3 to 0.8 g / (hole·min), and most preferably 0.5 to 0.7 g / (hole·min).
[0151] The spinning temperature for polylactic acid-based resins such as polylactic acid is, for example, 150 to 250°C, preferably 160 to 230°C, and more preferably 180 to 220°C.
[0152] In the heat-sealing process, the temperature of the heat roll (especially the embossing heat roll) is, for example, 60 to 180°C, preferably 80 to 160°C, more preferably 90 to 150°C, more preferably 100 to 130°C, and most preferably 110 to 120°C.
[0153] The resulting nonwoven fabric is usually in sheet form and is processed into the desired shape by cutting or other methods before use, but it may also be secondarily molded by conventional thermoforming if necessary. [Examples]
[0154] The present disclosure will be described in more detail below based on examples, but the present disclosure is not limited to these examples. The raw materials, equipment, and evaluation methods used in the examples are as follows.
[0155] [Raw materials] Polylactic acid (PLA) 1: "FY201" manufactured by Anhui Fengyuan Group Co., Ltd., melting point 165-175°C, D-isomer content less than 1 mol%, MFR (190°C, load 2.16 kgf) 25-35 g / 10 min, glass transition temperature 60°C Polylactic acid (PLA)2: "FY202" manufactured by Anhui Fengyuan Group Co., Ltd., melting point 155-165°C, D-isomer content approximately 2 mol%, MFR (190°C, load 2.16 kgf) 25-35 g / 10 min, glass transition temperature 60°C Plasticizer: "DAIFATTY-101" manufactured by Daihachi Chemical Industry Co., Ltd., adipic acid ester Antiblocking agent (AB agent): "AY603" manufactured by Tosoh Silica Co., Ltd., spherical silica, average particle size 6 μm Lubricant 1: Manufactured by Tokyo Chemical Industry Co., Ltd., erucic acid amide Lubricant 2: Oleamide, manufactured by Tokyo Chemical Industry Co., Ltd. Lubricant 3: Stearic acid amide, manufactured by Tokyo Chemical Industry Co., Ltd.
[0156] [MFR of resin composition] The MFR of the resin composition was measured in accordance with ISO 1133, under conditions of a holding time of 5 minutes, a temperature of 190°C, and a test load of 2.16 kgf.
[0157] [Adhesion of resin compositions] The pelletized resin composition was heated on a hot plate at 80°C, and it was evaluated whether the pellets stuck together.
[0158] [Moldability] When manufacturing nonwoven fabric using a spunbond nonwoven fabric manufacturing apparatus (manufactured by Kasen Nozzle Seisakusho Co., Ltd.) with pelletized resin composition as the raw material, the degree of adhesion of the nonwoven fabric to the embossing roll was checked, and the moldability of the nonwoven fabric (whether or not a uniform nonwoven fabric can be obtained) was evaluated according to the following criteria.
[0159] Good: No nonwoven fabric adheres to the embossing roll at all. Defect: Nonwoven fabric is sticking to the embossing roll.
[0160] [Rigidity and flexibility of nonwoven fabrics] The stiffness and flexibility of the nonwoven fabric were measured using the 41.5° cantilever method in accordance with ISO 9073-7. The stiffness and flexibility were measured in both the MD direction (the direction of fiber stretching and the web transport direction) and the TD direction (the direction perpendicular to the stretching and transport directions).
[0161] [Tensile strength and tensile elongation of nonwoven fabrics] The tensile strength and tensile elongation of the nonwoven fabric were measured according to the JIS L 1096A method (cut-slip method), with a tensile speed of 20 cm / min, a gripping distance of 20 cm, and a test specimen width of 5 cm. The tensile strength and tensile elongation were measured in both the MD and TD directions of the nonwoven fabric.
[0162] [Tear strength of nonwoven fabrics] The tear strength of the nonwoven fabric was measured according to the trapezoid method of JIS L 1913, with a tensile speed of 10 cm / min and a specimen width of 7.5 cm. The tear strength was measured in both the MD and TD directions of the nonwoven fabric.
[0163] [Water resistance of nonwoven fabric] The water resistance of the nonwoven fabric was measured in accordance with JIS L 1092A method.
[0164] Example 1 258g of PLA1, 42g of plasticizer, and 3g of AB agent were mixed and melt-kneaded at 180°C using a twin-screw extruder (Technovel Co., Ltd. "KZW15TW-30MG-NH(-700)") to obtain a pelletized resin composition. Using the obtained pelletized resin composition as a raw material, it was spun using a spunbond nonwoven fabric manufacturing apparatus (Kasen Nozzle Seisakusho Co., Ltd.) under the conditions of a resin temperature of 200°C, an embossing temperature of 115°C, and a single-hole discharge rate of 0.6g / (hole·minute), resulting in a basis weight of 20g / m². 2We manufactured spunbond nonwoven fabric.
[0165] Example 2 A resin composition was obtained in the same manner as in Example 1, except that 258g of PLA1, 42g of plasticizer, and 3g of AB agent were used, along with an additional 6g of lubricant 1. A spunbond nonwoven fabric was then manufactured. Figure 2 shows an SEM image (1000x magnification) of the obtained spunbond nonwoven fabric. The average fiber diameter of the biodegradable fibers constituting this spunbond nonwoven fabric was approximately 12 μm.
[0166] Example 3 A resin composition was obtained in the same manner as in Example 2, except that 270g of PLA1 and 30g of plasticizer were used instead of 258g of PLA1 and 42g of plasticizer, and then a spunbond nonwoven fabric was manufactured.
[0167] Example 4 A resin composition was obtained in the same manner as in Example 2, except that 1.5g of lubricant 1 was used instead of 6g of lubricant 1, and then a spunbond nonwoven fabric was manufactured.
[0168] Example 5 A resin composition was obtained in the same manner as in Example 2, except that 6g of lubricant 2 was used instead of 6g of lubricant 1, and then a spunbond nonwoven fabric was manufactured.
[0169] Example 6 A resin composition was obtained in the same manner as in Example 2, except that 6g of lubricant 3 was used instead of 6g of lubricant 1, and then a spunbond nonwoven fabric was manufactured.
[0170] Comparative Example 1 A resin composition was obtained in the same manner as in Example 1, except that plasticizers and AB agents were not added, and 300g of PLA1 was used instead of 258g of PLA1. A spunbond nonwoven fabric was then manufactured.
[0171] Comparative Example 2 A resin composition was obtained in the same manner as in Comparative Example 1, except that PLA2 was used instead of PLA1, and then a spunbond nonwoven fabric was manufactured.
[0172] Reference example 1 A resin composition was obtained in the same manner as in Example 1, except that PLA2 was used instead of PLA1, and then a spunbond nonwoven fabric was manufactured.
[0173] Comparative Example 3 A resin composition was obtained in the same manner as in Example 1, except that the AB agent was not included. The MFR of the obtained resin composition was measured and its adhesion was evaluated, but since the pellets adhered to each other, a nonwoven fabric could not be manufactured.
[0174] The evaluation results for Examples 1-6, Reference Example 1, and Comparative Examples 1-3 are shown in Tables 1 and 2. Note that in Reference Example 1, although a nonwoven fabric was obtained, its moldability was poor and only a nonwoven fabric of unevenness was obtained; therefore, the nonwoven fabric was not evaluated.
[0175] [Table 1]
[0176] [Table 2]
[0177] In Example 1, by using polylactic acid with a low D-isomer content and appropriately blending additives, adhesion between resin compositions did not occur. Furthermore, because the oriented crystallization of the resin composition progressed, it exhibited excellent moldability, and it was possible to produce a nonwoven fabric with low rigidity (excellent flexibility). However, the water resistance was too low to be measured, and the water resistance was not sufficient.
[0178] In Example 2, lubricant 1 was further added to the composition of Example 1. However, similar to Example 1, there were no problems with resin adhesion, and the moldability and flexibility were excellent, as well as improved water resistance.
[0179] In Example 3, the proportion of plasticizer was reduced compared to the composition of Example 2, but low rigidity and softness were maintained. Similar to Example 2, there were no problems with resin adhesion, and a nonwoven fabric with excellent moldability and flexibility was produced.
[0180] In Example 4, the proportion of lubricant was reduced compared to the composition of Example 2, but high water resistance was maintained, and, similar to Example 2, there were no problems with resin adhesion, and a nonwoven fabric with excellent moldability and flexibility was produced.
[0181] In Examples 5 and 6, the type of lubricant was changed from that of Example 2, but high water resistance was maintained, and, similar to Example 2, there were no problems with resin adhesion, and a nonwoven fabric with excellent moldability and flexibility was produced.
[0182] In Comparative Examples 1 and 2, while there were no problems with resin adhesion or moldability, the absence of plasticizers resulted in nonwoven fabrics with high rigidity and flexibility. The tear strength of Comparative Example 1 was similar to that of Examples 1-6. A comparison of Examples 1-6 and Comparative Example 1 revealed that Examples 1-6 showed improved flexibility while also exhibiting superior tear strength compared to Comparative Example 1. Furthermore, while Comparative Example 1 had better water resistance than Example 1 due to the absence of plasticizers, its water resistance was lower than that of Examples 2-6, possibly due to the absence of AB agents and lubricants.
[0183] In Reference Example 1, while adhesion between resin compositions did not occur due to the appropriate blending of additives, the use of a resin with a relatively high D-isomer content made it difficult for oriented crystallization to proceed during molding, and also easily resulted in stickiness due to plasticizers, leading to poor moldability and making it impossible to produce a uniform nonwoven fabric.
[0184] In Comparative Example 3, the absence of agent AB resulted in adhesion between the resin compositions, making it unsuitable for use as a raw material for nonwoven fabric. [Industrial applicability]
[0185] The nonwoven fabric of the present invention can be used as a nonwoven fabric for various applications requiring flexibility, such as electronic components (separators for insulating materials, etc.), industrial materials (oil absorbents, leather base fabrics, cement compounding materials, rubber compounding materials, various tape base materials, air filters, liquid filters, etc.), construction materials (insulating materials, sound-absorbing materials, etc.), cushioning or protective materials (automotive protective materials such as automotive cushioning materials and automotive ceiling materials, protective materials for furniture and interiors, etc.), agricultural and horticultural materials (agricultural sheets, insect-repellent sheets, light-blocking sheets, etc.), civil engineering materials (soil stabilizers, filtration materials, sand erosion prevention materials, reinforcing materials, etc.), lifestyle-related materials (wipers, printing base materials, packaging and bag materials, storage materials, lens wipes, beverage filters, etc.), medical materials [for example, wound protection materials (bandages, gauze or absorbent cotton, adhesive bandages, etc.), wound healing materials (poultices, etc.)] It can be used in medical tapes, drapes, surgical gowns, medical gowns, medical caps, sheets, surgical waste disposal materials, etc., sanitary materials [towels, masks, gloves, diapers, diaper liners, sanitary products (napkins, tampons, etc.), wet wipes, pads (sweat pads, breast pads, incontinence pads, etc.), disposable aprons, disposable hats, etc.], skincare products (or beauty products) [for example, face masks, makeup removal sheets, body cleansing sheets (sweat wipes, oil-absorbing sheets, etc.), cosmetics, etc.], wet wipes [wet wipes, various wiping sheets (cleaning paper cleaners, etc.)], and protective materials for the body such as clothing and footwear (for example, hoods, hats such as sauna caps, men's clothing, women's clothing, sportswear, underwear, bra cups, shoulder pads, shoe insole base materials, etc.).
[0186] Of these, applications that involve contact with the human body are preferred due to the importance of flexibility, and medical materials, sanitary materials, skincare products, wet wipes, and body protective materials are more preferred, while sanitary materials such as diapers and sanitary products are even more preferred due to their excellent water resistance. [Explanation of Symbols]
[0187] 1…Spinning nozzle 3… Ejector 8... Net conveyor 9... Embossing hot roll 10…Flat heat roll
Claims
1. A nonwoven fabric comprising biodegradable fibers formed from a resin composition containing a rigid biodegradable resin (A), a plasticizer (B), and an antiblocking agent (C), wherein 98.3 mol% or more of the constituent units of the rigid biodegradable resin (A) are either the D-form or the L-form.
2. The nonwoven fabric according to claim 1, wherein the rigid biodegradable resin (A) is a polylactic acid-based resin.
3. The nonwoven fabric according to claim 2, wherein the polylactic acid-based resin is polylactic acid.
4. The nonwoven fabric according to any one of claims 1 to 3, wherein the melting point of the rigid biodegradable resin (A) is 165°C or higher.
5. The nonwoven fabric according to any one of claims 1 to 3, wherein the plasticizer (B) is an ester-based plasticizer.
6. The nonwoven fabric according to any one of claims 1 to 3, wherein the antiblocking agent (C) is inorganic particles with an average particle size of 10 μm or less.
7. The nonwoven fabric according to any one of claims 1 to 3, wherein the proportion of the plasticizer (B) is 5 to 20 parts by mass per 100 parts by mass of the hard biodegradable resin (A).
8. The nonwoven fabric according to any one of claims 1 to 3, wherein the proportion of the antiblocking agent (C) is 0.5 to 1.5 parts by mass per 100 parts by mass of the hard biodegradable resin (A).
9. The nonwoven fabric according to any one of claims 1 to 3, wherein the average fiber diameter of the biodegradable fibers is 5 to 20 μm.
10. A nonwoven fabric according to any one of claims 1 to 3, which is a spunbond nonwoven fabric.
11. The nonwoven fabric according to any one of claims 1 to 3, further comprising a lubricant (D).
12. The nonwoven fabric according to claim 11, wherein the lubricant (D) is a fatty acid amide having 12 or more carbon atoms.
13. The nonwoven fabric according to claim 11, wherein the proportion of the lubricant (D) is 0.1 to 5 parts by mass per 100 parts by mass of the hard biodegradable resin (A).
14. A nonwoven fabric according to any one of claims 1 to 3, wherein the rigidity is 10 mN·cm or less and the water resistance is 150 mm or more.
15. A method for producing a nonwoven fabric according to any one of claims 1 to 3, comprising a melt spinning step of melt spinning a resin composition comprising a rigid biodegradable resin (A), a plasticizer (B), and an antiblocking agent (C) to form biodegradable fibers.
16. The method according to claim 15, further comprising a web formation step of stretching and collecting the biodegradable fibers obtained in the melt spinning step to form a web, and a heat-sealing step of heat-sealing the web to form a nonwoven fabric.
17. A sanitary material formed from a nonwoven fabric according to any one of claims 1 to 3.
18. A method of using a nonwoven fabric according to any one of claims 1 to 3 by bringing it into contact with the human body.
Citation Information
Patent Citations
Polylactic acid-based filament nonwoven fabric and method for producing the same
JP2009203599A
Spunbond web containing polylactic acid fiber
JP2017527706A