Method for manufacturing martensitic precipitation-hardening stainless steel and martensitic precipitation-hardening stainless steel products
The described method enhances the low-temperature toughness of martensitic precipitation-hardening stainless steels through tailored heat treatments, achieving improved mechanical properties suitable for extreme cold conditions.
Patent Information
- Application Number
- JP2026066216
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-07
- Filing Date
- 2026-04-14
- Publication Date
- 2026-11-19
AI Technical Summary
Existing martensitic precipitation-hardening stainless steels, such as 17-4PH equivalent steels, do not achieve sufficient low-temperature toughness in extremely cold environments, particularly when exposed to liquefied gases, necessitating improvements in mechanical properties for applications in such conditions.
A method involving specific composition and heat treatment processes, including solution treatment at 1020-1060°C, first aging at 750-770°C, second aging at 610-630°C, and a subsequent toughness-enhancing heat treatment at 580-620°C, to enhance the low-temperature toughness without altering standard conditions, promoting retained austenite and coarsening of the precipitation-hardened phase.
The method significantly improves low-temperature toughness, achieving absorbed energies of 21.0 J or more in a Charpy impact test at -196°C, with potential increases up to 25.0 J or more, maintaining mechanical properties and enabling use in extreme cold environments.
Smart Images

Figure 2026182767000001 
Figure 2026182767000002 
Figure 2026182767000003
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a method for producing martensitic precipitation hardening stainless steel and a martensitic precipitation hardening stainless steel product.
BACKGROUND ART
[0002] Martensitic precipitation hardening stainless steel is added with Cu, Nb, Ti, Al, Mo and the like as precipitation hardening elements, and precipitates are formed by aging treatment after solution treatment, so that a high-strength product can be obtained. Products made of martensitic precipitation hardening stainless steel have excellent corrosion resistance and high strength, and are used in a wide range of applications such as shafts, bolts, gears, valves, turbine components, and aircraft components.
[0003] In martensitic precipitation hardening stainless steel, the precipitation state of the precipitation hardening phase can be adjusted by aging treatment after solution treatment according to the mechanical properties required for the product. For example, 17-4PH is an alloy containing Cu as a precipitation hardening element, and the precipitation state of the Cu phase can be adjusted by aging treatment. For SUS630 registered in the JIS-G-4303 standard as a martensitic precipitation hardening stainless steel equivalent to 17-4PH (hereinafter also referred to as 17-4PH equivalent steel), after performing a solution treatment of heating to 1020 to 1060°C, holding, and then cooling, the conditions for various subsequent aging treatments (referred to as "precipitation hardening treatment") are specified. In addition, for type 630 registered in the ASTM-F593 standard as 17-4PH equivalent steel, ASTM-A564 specifies that after performing a solution treatment of heating to 1040°C ±15°C, holding, and then cooling, the conditions for various subsequent aging treatments are specified.
[0004] For 17-4PH equivalent steels, when particularly toughness improvement is required, ASTM-A564, for example, standardizes the above aging treatment with conditions H1150M, which consists of a first aging treatment of heating to 760°C followed by cooling, and a second aging treatment of heating to 620°C followed by cooling. Furthermore, a method for improving low-temperature toughness has been proposed to accommodate the use of 17-4PH equivalent steels in low-temperature environments (Patent Document 1). According to Patent Document 1, such martensitic precipitation-hardening stainless steel can be used for applications such as (a) a rotor and stator that rotate by the hydraulic power of a fluid in a drilling drill, (b) a drive shaft that transmits the rotation of the rotor and stator, (c) a bearing structural member that holds the drive shaft, (d) a structural member of a MWD that measures the drilling depth, inclination angle and azimuth angle of the drill string of a drilling drill, (e) a structural member of a LWD that performs geological analysis, and (f) a housing member of an MWD or LWD, as well as steam turbine blades, aerospace structural members, and high-strength fasteners. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2021-123792 [Overview of the Initiative] [Problems that the invention aims to solve]
[0006] In the case of 17-4PH equivalent steel, applying the aforementioned ASTM-A564 H1150M to the aging treatment conditions can improve the toughness after aging. Furthermore, in the case of martensitic precipitation-hardening stainless steel described in Patent Document 1, an absorbed energy of 20 J or more can be achieved in a Charpy impact test using a 2 mm V-notch specimen at a test temperature of minus 40°C, making it suitable for use in cold regions. However, if we consider its use not only in natural environments but also in extremely cold environments (for example, in environments where it comes into contact with various liquefied gases), achieving sufficient absorbed energy at test temperatures lower than minus 40°C could lead to further improvements in low-temperature toughness. The object of the present invention is to provide a method for producing martensitic precipitation-hardening stainless steel that is effective in improving the low-temperature toughness of 17-4PH equivalent steel, and to provide a martensitic precipitation-hardening stainless steel product produced by this method. [Means for solving the problem]
[0007] The present invention relates to a method for producing martensitic precipitation-hardening stainless steel, in which a heat-treated material having a composition of C: 0.10% or less, Si: 1.00% or less, Mn: 1.00% or less, P: 0.04% or less, S: 0.03% or less, Cr: 14.00~18.00%, Ni: 3.00~6.00%, Cu: 1.00~5.00%, Nb: 0.50% or less, Mo: 1.00% or less, N: 0.10% or less, the remainder being Fe and impurities is subjected to a solution treatment in which a heat-treated material is heated and held at 1020~1060°C and then cooled, and an aging treatment consisting of a first aging treatment in which a heat-treated material is heated and held at 750~770°C and then cooled, and a second aging treatment in which a heat-treated material is heated and held at 610~630°C and then cooled, and the heat-treated material is subjected to a solution treatment in which a heat-treated material has a composition of C: 0.10% or less, Si: 1.00% or less, Mn: 1.00% or less, P: 0.04% or less, S: 0.03% or less, Cr: 14.00~18.00%, Ni: 3.00~6.00%, Cu: 1.00~5.00%, Nb: 0.50% or less, Mo: 1.00% or less, N: 0.10% or less, the remainder being Fe and impurities, by performing an aging treatment. This is a method for manufacturing martensitic precipitation-hardening stainless steel, which involves further toughness-enhancing heat treatment by heating and holding at 580-620°C followed by cooling, after the aging treatment described above. In this case, it is preferable that the heating and holding temperature for the second aging treatment described above be 615°C or higher. The product is a martensitic precipitation-hardening stainless steel product manufactured by this manufacturing method. [Effects of the Invention]
[0008] According to the present invention, the low-temperature toughness of martensitic precipitation-hardening stainless steel can be improved. [Modes for carrying out the invention]
[0009] The distinguishing feature of this invention is that, for martensitic precipitation-hardening stainless steel equivalent to 17-4PH, improvement in low-temperature toughness can be achieved without changing the standardized solution treatment and aging treatment conditions. This is advantageous in terms of manufacturing efficiency, as, for example, when improving the low-temperature toughness of 17-4PH equivalent steel, it can be placed in the same heating furnace as other 17-4PH equivalent steels. The requirements of this invention will be described below.
[0010] (1) The component composition of the martensitic precipitation-hardening stainless steel according to the present invention is as follows, in mass% (hereinafter also simply referred to as "%): C: 0.10% or less, Si: 1.00% or less, Mn: 1.00% or less, P: 0.04% or less, S: 0.03% or less, Cr: 14.00~18.00%, Ni: 3.00~6.00%, Cu: 1.00~5.00%, Nb: 0.50% or less, Mo: 1.00% or less, N: 0.10% or less, the remainder being Fe and impurities.
[0011] ·C: 0.10% or less If the amount of carbon (C) is too high, it will form a large number of chromium carbides at the grain boundaries, leading to a deficiency of chromium near the grain boundaries and reducing corrosion resistance. Therefore, the amount of carbon should be 0.10% or less. Preferably, it should be 0.08% or less, more preferably 0.07% or less, and even more preferably 0.06% or less. Furthermore, carbon (C) is also an effective element for reducing the amount of δ-ferrite phase remaining in the product structure after aging treatment. Therefore, it can be included in a concentration of 0.01% or more. More preferably, it can be 0.02% or more, and even more preferably 0.03% or more.
[0012] ·Si: 1.00% or less Excessive addition of Si can cause the δ-ferrite phase to remain, adversely affecting the properties. Therefore, the Si content should be 1.00% or less. Preferably, it should be 0.70% or less, and more preferably 0.50% or less. Furthermore, Si is effective as a deoxidizing element, and it can be included in a concentration of 0.10% or more. More preferably, it can be 0.20% or more, and even more preferably 0.30% or more.
[0013] ·Mn: 1.00% or less When manganese is added in excess, it forms MnS, and in the product after aging treatment, MnS becomes the starting point for pitting corrosion, reducing corrosion resistance. Therefore, the amount of manganese should be 1.00% or less. Preferably, it should be 0.80% or less, and more preferably 0.60% or less. Furthermore, Mn is effective as a deoxidizing element, and it can be included in a concentration of 0.10% or more. More preferably, it can be 0.20% or more, and even more preferably 0.30% or more.
[0014] ·P:0.04% or less P tends to segregate at grain boundaries, which can cause grain boundary embrittlement and thus adversely affect mechanical properties. Therefore, its content should be 0.04% or less. Preferably, it should be 0.03% or less.
[0015] ·S: 0.03% or less S forms sulfides, which adversely affects mechanical properties. Therefore, its content should be 0.03% or less. Preferably, it should be 0.02% or less. More preferably, it should be 0.01% or less. Even more preferably, it should be 0.005% or less.
[0016] • Cr: 14.00~18.00% Cr is an element that contributes to the corrosion resistance of the product, and an appropriate addition amount is required. To achieve good corrosion resistance, the content is set to 14.00% or more. On the other hand, if Cr is added excessively, it causes the δ ferrite phase to remain, which adversely affects the properties, so the content is set to 18.00% or less. The content is preferably 14.50% or more, more preferably 15.00% or more. Also, the content is preferably 17.50% or less, more preferably 17.00% or less, even more preferably 16.50% or less, and still more preferably 16.00% or less.
[0017] ·Ni: 3.00 to 6.00% Ni is an element effective in reducing the amount of remaining δ ferrite phase. It is also an element effective in improving corrosion resistance, so the content is set to 3.00% or more. On the other hand, if Ni is added excessively, a large amount of residual austenite will be present, and the strength will be significantly reduced, so the content is set to 6.00% or less. The content is preferably 3.50% or more, more preferably 4.00% or more. Also, the content is preferably 5.50% or less, more preferably 5.00% or less.
[0018] ·Cu: 1.00 to 5.00% Cu is an element that forms a precipitation hardening phase, and the content is set to 1.00% or more for sufficient strengthening. On the other hand, if Cu is added excessively, a large amount of residual austenite will be present, and the strength will be significantly reduced, so the content is set to 5.00% or less. The content is preferably 1.50% or more, more preferably 2.00% or more, even more preferably 2.50% or more, and still more preferably 3.00% or more. Also, the content is preferably 4.50% or less, more preferably 4.00% or less.
[0019] ·Nb: 0.50% or less If Nb is contained excessively, it causes the δ-ferrite phase to remain, which adversely affects the properties. Therefore, the Nb content is set to 0.50% or less, preferably 0.45% or less, more preferably 0.40% or less, and still more preferably 0.35% or less. Note that Nb forms carbonitrides and suppresses coarsening of crystal grains during solution treatment. Thus, when contained, the Nb content is preferably 0.10% or more, more preferably 0.15% or more, and still more preferably 0.20% or more.
[0020] The component composition of the martensitic precipitation hardening stainless steel of the present invention can be, for example, that of the aforementioned 17-4PH equivalent steel. Further, for example, Mo and N can be optionally contained.
[0021] ·Mo: 1.00% or less If Mo is contained excessively, it causes the δ-ferrite phase to remain and adversely affects the properties, so even when contained, the Mo content is set to 1.00% or less, preferably 0.80% or less, more preferably 0.60% or less, still more preferably 0.40% or less, and even more preferably 0.30% or less. Note that Mo is an element effective for improving corrosion resistance. In this respect, the Mo content can preferably be 0.05% or more, more preferably 0.07% or more, and still more preferably 0.09% or more.
[0022] ·N: 0.10% or less If N is contained excessively, it reduces toughness, so even when contained, the N content is set to 0.10% or less, preferably 0.08% or less, more preferably 0.06% or less, and still more preferably 0.05% or less. Note that N is an element effective for improving strength by solid solution strengthening. In this respect, the N content can preferably be 0.01% or more, and more preferably 0.02% or more.
[0023] ·Balance: Fe and impurities The martensitic precipitation-hardening stainless steel according to the present invention may consist of Fe and impurities as the remainder, excluding the above-mentioned constituent elements. In this case, even if the content of impurities exceeds the detection limits of the above-mentioned constituent elements and other elements excluding Fe, these other elements can be treated as impurities if, for example, the content of each element is less than 1.00%. Preferably, the total content of these other elements is less than 3.00%. A typical component composition of the martensitic precipitation-hardening stainless steel according to the present invention is, for example, 17-4PH equivalent steel.
[0024] (2) The solution treatment according to the present invention involves heating a martensitic precipitation-hardening stainless steel material having the above-mentioned component composition to 1020-1060°C, holding it thereafter, and then cooling it. The martensitic precipitation-hardening stainless steel according to the present invention is a steel whose Ms point (martensitization initiation temperature) is above room temperature and which exhibits a martensitic structure after solution treatment. In this solution treatment, it is important to dissolve precipitation-hardening elements into the matrix phase in order to promote precipitation hardening in the subsequent aging treatment. Therefore, the solution treatment according to the present invention has a heating and holding temperature of 1020°C or higher. Preferably, it is 1025°C or higher, and more preferably 1030°C or higher. On the other hand, if the heating and holding temperature during the solution treatment is too high, a δ-ferrite phase is formed, which adversely affects the mechanical properties. Therefore, the above heating and holding temperature is 1060°C or lower. Preferably, it is 1055°C or lower, and more preferably 1050°C or lower.
[0025] There are no specific regulations regarding the heating and holding time. As long as the precipitate-hardening elements can be sufficiently dissolved in the matrix phase, conventional methods can be followed, such as 30 minutes or more, or 1 hour or more. The upper limit can also be determined according to the state of solid solution of the precipitate-hardening elements, such as 20 hours or less, 15 hours or less, 10 hours or less, or 5 hours or less. After the heating and holding described above, it is preferable to perform rapid cooling, for example, in order to obtain a martensitic structure while the precipitated hardening elements remain dissolved in the matrix phase. This rapid cooling can follow conventional cooling methods, such as oil cooling, water cooling, air cooling, or blast cooling.
[0026] Regarding the solution treatment of 17-4PH equivalent steel, for example, JIS-G-4303 specifies that the treatment should be heated to 1020-1060°C and then rapidly cooled. ASTM-A564 also specifies that the treatment should be heated to 1045°C ± 15°C and then cooled to 32°C or below.
[0027] (3) The aging treatment according to the present invention consists of a first aging treatment in which the material is heated to 750 to 770°C and then cooled, and a second aging treatment in which the material is heated to 610 to 630°C and then cooled. When aging martensitic precipitation-hardening stainless steel after solution treatment, if toughness is a priority, it is advantageous to set a higher treatment temperature. For example, in the case of aging treatment of 17-4PH equivalent steel, JIS-G-4303 specifies that the heat treatment symbol H1150 involves heating to 610-630°C followed by cooling. ASTM-A564 also specifies that the same condition H1150 involves heating to 620°C followed by cooling.
[0028] Furthermore, in this invention, in order to further improve the toughness of 17-4PH equivalent steel products, a "first" aging treatment with a higher heating and holding temperature is performed before the aging treatment of heating and holding at 610-630°C followed by cooling. By raising the temperature of the first aging treatment, retained austenite is more likely to be present in the microstructure after aging treatment, improving the toughness of the 17-4PH equivalent steel product. In addition, raising the aging treatment temperature leads to over-aging, making the precipitation-hardened phase coarser and improving toughness. Furthermore, by setting an upper limit on the first aging treatment temperature, the excessive release of alloying elements dissolved in the martensite generated by the solution treatment due to aging treatment is suppressed, and the original strengthening mechanism by martensite can be maintained.
[0029] Accordingly, the aging treatment according to the present invention involves a first aging treatment in which the material is heated and held at 750-770°C and then cooled, followed by a second aging treatment in which the material is heated and held at 610-630°C and then cooled. In this case, the heating and holding temperature for the second aging treatment is preferably 615°C or higher, more preferably 620°C or higher, and even more preferably 625°C or higher. There are no special restrictions on the heating and holding time at the aging treatment temperature for each aging treatment; for example, the first aging treatment can be 60 minutes or more, or 180 minutes or less. Similarly, the second aging treatment can be 180 minutes or more, or 540 minutes or less. The heating and holding time for the second aging treatment is preferably 200 minutes or more, and more preferably 220 minutes or more. In each aging treatment, the cooling after heating and holding can follow conventional cooling methods, such as air cooling or blast cooling.
[0030] Regarding the aging treatment of 17-4PH equivalent steel, for example, ASTM-A564 specifies that a first aging treatment is performed under the condition H1150M, consisting of heating and holding at 760°C for 2 hours followed by air cooling, and then a second aging treatment is performed at 620°C for 4 hours followed by air cooling. In the present invention, improvement in low-temperature toughness can be achieved without changing these standardized aging treatment conditions. Furthermore, these standardized conditions can be modified to improve various mechanical properties.
[0031] (4) The present invention provides a method for producing martensitic precipitation-hardening stainless steel, which involves performing a toughness-enhancing heat treatment after the aging treatment described above, by heating and holding at 580-620°C and then cooling to obtain a heat-treated material. Furthermore, according to various standards, conventionally, the material would be considered the final heat-treated material (i.e., the product) after completing the above-mentioned second aging treatment. However, in the present invention, this material is subjected to an additional special heat treatment to become the final heat-treated material. In other words, in the case of the present invention, the amount of retained austenite in the microstructure of the 17-4PH equivalent steel is increased by the above-mentioned first and second aging treatments. Further, by performing a "toughness-enhancing heat treatment" with controlled treatment temperature, an increase in the amount of austenite due to reverse transformation and coarsening of the precipitation-hardened phase due to overaging are promoted, thereby improving toughness.
[0032] Furthermore, by controlling the above-mentioned processing temperature (heating and holding temperature) within the range of 580 to 620°C, an improvement in toughness can be expected even in low-temperature environments such as -196°C. In other words, a clear improvement in toughness is observed when this processing temperature is 580°C or higher. Preferably, it is 590°C or higher, more preferably 600°C or higher, and even more preferably 610°C or higher. By setting an upper limit on this processing temperature, the excessive release of alloying elements dissolved in the martensite can be suppressed, and the original strengthening mechanism by martensite can be maintained, so the upper limit is set at 620°C. Preferably, the upper limit is set at 615°C.
[0033] There are no special restrictions on the heating and holding time in the toughness-improving heat treatment described above; for example, it can be 60 minutes or more, or 500 minutes or less. Further improvement in toughness can be expected by increasing the heating and holding time. More preferably, it is 90 minutes or more, even more preferably 120 minutes or more, and even more preferably 200 minutes or more. Setting an upper limit on the heating and holding time is effective in maintaining the strengthening mechanism by martensite. It also contributes to reducing energy costs by shortening the heating and holding time. More preferably, it is 450 minutes or less, even more preferably 350 minutes or less, and even more preferably 250 minutes or less. Cooling after heating and holding can follow conventional cooling methods, such as air cooling or blast cooling. Furthermore, air cooling can be used in accordance with various standards and regulations.
[0034] The martensitic precipitation-hardening stainless steel products of the present invention can maintain sufficient mechanical properties as specified in various standards. For example, in terms of hardness, they can maintain a room-temperature hardness of approximately 20-40 HRC on the Rockwell hardness scale. Furthermore, they can be used in low-temperature environments at various temperatures. The low-temperature toughness achieved by the present invention can be evaluated as an indicator of its effectiveness, for example, by the absorbed energy at a test temperature of -196°C in a 2mm V-notch test specimen. In this case, the specific value of the absorbed energy varies depending on the condition (manufacturing history) of the heat-treated material. When evaluated using heat-treated materials in the same condition, the absorbed energy achieved by the present invention can increase by, for example, 2.0 J or more compared to a heat-treated material that has not undergone the toughness-enhancing heat treatment according to the present invention. Preferably, the increase is 2.5 J or more, and more preferably 3.0 J or more. Furthermore, regarding the specific values themselves, it is possible to achieve absorbed energies of 21.0 J or more, 22.0 J or more, even 23.0 J or more, 24.0 J or more, and even 25.0 J or more. And because the absorbed energy at -196°C achieves the above values, improved low-temperature toughness can be obtained even in low-temperature environments at temperatures higher than -196°C. [Examples]
[0035] A steel ingot equivalent to 17-4PH with the component composition shown in Table 1 was hot-worked to form a steel rod with a diameter of 85 mm. The remaining impurities include unavoidable impurities that may have been introduced during the manufacturing process. This component composition can be analyzed using combustion-infrared absorption spectroscopy, X-ray fluorescence spectroscopy, and spark discharge emission spectroscopy. The analysis method should be appropriately changed depending on the timing of specimen sampling.
[0036] [Table 1]
[0037] Using the above-mentioned steel material as the heat treatment material, first, a solution treatment was performed on this steel material by heating and holding at 1040°C for 40 minutes, followed by oil cooling. Then, a first aging treatment was performed on the steel material after this solution treatment, which involved heating and holding at 760°C for 2 hours (120 minutes), followed by air cooling. A test piece for evaluation was taken from the circumferential surface of this steel material at a position D / 4 toward the center of the diameter (where D represents the diameter), and a second aging treatment was performed on this test piece by heating and holding, followed by air cooling, under the conditions shown in Table 2.
[0038] Then, the test specimens after the aging treatments described above (the first and second aging treatments) were subjected to a further heat treatment (toughness-enhancing heat treatment as defined in this invention) by heating, holding, and then air-cooling under the conditions shown in Table 2 to obtain martensitic precipitation-hardening stainless steel, and the mechanical properties of this heat-treated martensitic precipitation-hardening stainless steel were evaluated. The mechanical properties were evaluated using the room-temperature tensile test according to JIS Z2241 and the Charpy impact test according to JIS Z2242. The test specimens for the Charpy impact test were 2 mm V-notched, the test temperature was -196°C, and the absorbed energy was the average of the results of two tests. The sampling procedure for the test specimens followed JIS G0416. The sampling direction of the test specimens was axial (parallel) to the length of the rod-shaped steel material. The room-temperature hardness of the martensitic precipitation-hardening stainless steel was also measured. The results of these mechanical properties are also shown in Table 2.
[0039] [Table 2]
[0040] As shown in Table 2, all test specimens of the present invention obtained an absorbed energy of 25.0 J or more. Furthermore, the absorbed energy was increased by 2.5 J or more compared to the comparative example No. 1 test specimen. In the case of the heat treatment material prepared under the conditions of Example 1, the absorbed energy at -196°C of No. 1, which did not undergo the toughness-enhancing heat treatment according to the present invention, was 22.4 J, while the absorbed energy at -196°C of No. 2, which underwent the toughness-enhancing heat treatment according to the present invention, improved to 26.2 J. In addition, other mechanical properties were maintained at sufficient values as described in various standards. Furthermore, by adjusting the heating and holding conditions of the second aging treatment performed on No. 2, the absorbed energy at -196°C could be further improved, and in particular, an improvement effect was confirmed when the heating and holding temperature of the second aging treatment was increased. Furthermore, absorbed energies of 27.0 J or more were obtained for Nos. 4 to 7. Furthermore, the absorbed energy was increased by 5.0 J or more compared to the comparative example No. 1. [Examples]
[0041] Steel ingots equivalent to 17-4PH steel with the component composition shown in Table 3 were hot-worked to form 55mm diameter steel rods. The remaining impurities include unavoidable impurities that may have been introduced during the manufacturing process. This component composition can be analyzed using combustion-infrared absorption spectroscopy, X-ray fluorescence spectroscopy, and spark discharge emission spectroscopy. The analysis method should be appropriately changed depending on the timing of specimen sampling.
[0042] [Table 3]
[0043] Using the above-mentioned steel material as the heat treatment material, first, a solution treatment was performed on this steel material by heating and holding at 1040°C for 40 minutes, followed by oil cooling. After this solution treatment, a test piece for evaluation was taken from the circumferential surface of the steel material at a position D / 4 toward the center of the diameter (where D represents the diameter). This test piece was subjected to a first aging treatment by heating and holding at 760°C for 2 hours (120 minutes), followed by air cooling, and then a second aging treatment by heating and holding at 620°C for 4 hours (240 minutes), followed by air cooling.
[0044] Then, the test specimens after the aging treatments described in the first and second aging treatments were subjected to a toughness-enhancing heat treatment, which involved heating, holding, and air cooling under the conditions shown in Table 4, to obtain martensitic precipitation-hardening stainless steel. The mechanical properties of this martensitic precipitation-hardening stainless steel after toughness-enhancing heat treatment were then evaluated. The mechanical properties were evaluated using the room-temperature tensile test according to JIS Z2241 and the Charpy impact test according to JIS Z2242. The test specimens for the Charpy impact test were 2 mm V-notched, the test temperature was -196°C, and the absorbed energy was the average of the results of two tests. The sampling procedure for the test specimens followed JIS G0416. The sampling direction of the test specimens was axial (parallel) to the length of the rod-shaped steel material. The room-temperature hardness of the martensitic precipitation-hardening stainless steel was also measured. The results of these mechanical properties are also shown in Table 4.
[0045] [Table 4]
[0046] As shown in Table 4, all test specimens in the present invention examples obtained an absorbed energy of 21.0 J or more. In the case of the heat treatment material prepared under the conditions of Example 2, although the toughness was generally lower compared to the results of Example 1 (Table 2) due to its smaller diameter and the high hardness, 0.2% yield strength, and tensile strength after the toughness-enhancing heat treatment, the absorbed energy at -196°C for No. 11, which underwent the toughness-enhancing heat treatment according to the present invention, which involved heating and holding at 580°C for 2 hours (120 minutes) followed by air cooling, was 21.4 J. At this time, other mechanical properties maintained sufficient values as described in various standards. Furthermore, by adjusting the heating and holding temperature and time of the toughness-enhancing heat treatment performed on No. 11 (for example, by raising the heating and holding temperature to 600°C or higher, or by extending the heating and holding time to 200 minutes or higher), the absorbed energy at -196°C could be further improved. Absorbed energies of 23.0 J or more were obtained for Nos. 13, 14, 16, and 17. [Examples]
[0047] Steel ingots equivalent to 17-4PH steel with the component composition shown in Table 5 were hot-worked to form 115 mm diameter steel rods. The remaining impurities include unavoidable impurities that may have been introduced during the manufacturing process. This component composition can be analyzed using combustion-infrared absorption spectroscopy, X-ray fluorescence analysis, and spark discharge emission spectroscopy. The analysis method should be appropriately changed depending on the timing of specimen sampling.
[0048] [Table 5]
[0049] Using the above-mentioned steel material as the heat treatment material, a test specimen for evaluation was taken from the circumferential surface of the steel material at a position D / 4 toward the center of the diameter (where D represents the diameter). This test specimen underwent a solution treatment by heating and holding at 1040°C for 60 minutes, followed by oil cooling. Next, a first aging treatment was performed by heating and holding at 760°C for 2 hours (120 minutes), followed by air cooling. Then, a second aging treatment was performed by heating and holding, followed by air cooling, under the conditions shown in Table 6. In the present invention example, the test specimen after the aging treatments consisting of the first and second aging treatments was further subjected to a toughness-enhancing heat treatment by heating and holding at 580°C for 4 hours (240 minutes), followed by air cooling to obtain martensitic precipitation-hardening stainless steel for the present invention example and comparative example, and their mechanical properties were evaluated.
[0050] Mechanical properties were evaluated using the Charpy impact test according to JIS Z2242. The test specimens were 2 mm V-notched, and the test temperatures were -50°C, -100°C, and -150°C. The absorbed energy was calculated by averaging the results of two tests. The specimen sampling procedure followed JIS G0416. The specimens were sampled axially (parallel to) the length of the rod-shaped steel material. Room temperature hardness was also measured. The results of these mechanical property tests are shown in Table 6.
[0051] [Table 6]
[0052] As shown in the results in Table 6, for the heat treatment material prepared under the conditions of Example 3, the absorbed energy of No. 22, which underwent the toughness-enhancing heat treatment according to the present invention, was improved at each temperature compared to No. 21, which did not undergo the toughness-enhancing heat treatment according to the present invention. Furthermore, by adjusting the heating and holding conditions of the second aging treatment performed on No. 22, the absorbed energy at each temperature could be further improved, and in particular, an improvement effect was confirmed at relatively low test temperatures when the heating and holding temperature of the second aging treatment was increased. Absorbed energy of 50.0 J or more was obtained for all test pieces of the present invention example at a test temperature of -150°C. In addition, an increase of 3.5 J or more was obtained compared to the comparative example test piece No. 21. [Examples]
[0053] The test specimens treated with solution in Example 3 were subjected to a first aging treatment, which involved heating and holding at 760°C for 2 hours (120 minutes) followed by air cooling. Then, a second aging treatment was performed, which involved heating and holding followed by air cooling under the conditions shown in Table 7, and a toughness-enhancing heat treatment was also performed, which involved heating and holding followed by air cooling (including specimen No. 22 in Example 3). This resulted in martensitic precipitation-hardening stainless steel, and the mechanical properties of this toughness-enhancing heat-treated martensitic precipitation-hardening stainless steel were evaluated. Mechanical properties were evaluated using the Charpy impact test according to JIS Z2242. The test specimens were 2 mm V-notched, and the test temperatures were -50°C, -100°C, and -150°C. The absorbed energy was calculated by averaging the results of two tests. The specimen sampling procedure followed JIS G0416. The specimens were sampled axially (parallel to) the length of the steel rod. Room temperature hardness was also measured. The results of these mechanical property tests are shown in Table 7.
[0054] [Table 7]
[0055] As shown in Table 7, for the heat treatment material prepared under the conditions of Example 4, the absorbed energy at each temperature could be further improved by further adjusting the heating and holding conditions of the second aging treatment and toughness-enhancing heat treatment compared to the absorbed energy of No. 22, which underwent the toughness-enhancing heat treatment according to the present invention. In particular, an improvement effect was confirmed at relatively low test temperatures when the heating and holding temperature of the second aging treatment and toughness-enhancing heat treatment was increased. Absorbed energies of 55.0 J or more were obtained for test pieces No. 31 and 32 at a test temperature of -150°C. Furthermore, an increase of 7.0 J or more was obtained compared to the absorbed energy of test piece No. 21 in Table 6, which is a comparative example.
Claims
1. In mass percent, C: 0.10% or less, Si: 1.00% or less, Mn: 1.00% or less, P: 0.04% or less, S: 0.03% or less, Cr: 14.00-18.00%, Ni: 3.00-6.00%, Cu: 1.00-5.00%, Nb: 0.50% or less, Mo: 1.00% or less N: 0.10% or less, Remainder: Fe and impurities A heat treatment material having the following component composition, A solution treatment is performed by heating and holding at 1020-1060°C followed by cooling. The aging treatment consists of a first aging treatment in which the material is heated and held at 750-770°C and then cooled, and a second aging treatment in which the material is heated and held at 610-630°C and then cooled. In a method for producing martensitic precipitation-hardening stainless steel that is heat-treated, The process is characterized by further heat treatment to improve toughness, which involves heating and holding the temperature to 580-620°C followed by cooling, after the aforementioned aging treatment. A method for producing martensitic precipitation-hardening stainless steel.
2. A method for producing martensitic precipitation-hardening stainless steel according to claim 1, characterized in that the heating and holding temperature of the second aging treatment is 615°C or higher.
3. A martensitic precipitation-hardening stainless steel product, characterized by being manufactured by the method for manufacturing martensitic precipitation-hardening stainless steel described in claim 1.
Citation Information
Patent Citations
Precipitation hardening martensitic stainless steel