Packaging substrate and semiconductor package including the same

The packaging substrate with a glass core and composite insulating layers addresses warpage and delamination issues by stabilizing the glass core and supporting wiring layers, ensuring reliable electrical connections and reduced signal loss.

JP2026182774APending Publication Date: 2026-11-19ABSOLICS INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2026069689
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-05-08
Filing Date
2026-04-20
Publication Date
2026-11-19

Smart Images

  • Figure 2026182774000001_ABST
    Figure 2026182774000001_ABST
Patent Text Reader

Abstract

This provides a packaging substrate that suppresses excessive warpage and offers excellent electrical reliability. [Solution] The packaging substrate 100 includes a glass core 10 and a first composite insulating layer 20 disposed on the glass core. The first composite insulating layer includes an elastic insulating layer 21 and a base insulating layer 22 disposed on the elastic insulating layer. The ratio of the thickness of the glass core to the thickness of the first composite insulating layer is 8 to 30. The glass transition temperature of the elastic insulating layer is 30°C to 85°C. This makes it possible to provide a packaging substrate with excellent electrical reliability without the glass core 10 easily warping during the process of forming the insulating layer on the glass core 10.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The specific examples relate to packaging substrates and semiconductor packages containing them. [Background technology]

[0002] In the manufacturing of electronic components, the process of creating circuits on semiconductor wafers is called the front-end process (FE), and the process of assembling the wafers into a state where they can be used in actual products is called the back-end process (BE), and the packaging process is included in this back-end process.

[0003] The four core technologies of the semiconductor industry that have enabled the rapid development of recent electronic products are semiconductor technology, semiconductor packaging technology, manufacturing process technology, and software technology. Semiconductor technology has evolved into various forms such as line widths in the nanoscale (below the micron), cells exceeding 10 million, high-speed operation, and significant heat dissipation, but relatively speaking, the technology to perfectly package these is not yet supported. Therefore, the electrical performance of a semiconductor is sometimes determined more by the packaging technology and the resulting electrical connections than by the performance of the semiconductor technology itself.

[0004] Ceramics or resins are used as materials for packaging substrates. In the case of ceramic substrates, it is not easy to mount high-performance high-frequency semiconductor elements due to their high resistance or dielectric constant. In the case of resin substrates, it is relatively possible to mount high-performance high-frequency semiconductor elements, but there are limitations to the reduction of the wiring pitch.

[0005] Recently, research has been progressing on applying silicon and glass to high-end packaging substrates. By forming through-holes in silicon or glass substrates and applying conductive materials to these holes, the wiring length between the device and the motherboard can be shortened, resulting in superior electrical characteristics. [Prior art documents] [Patent Documents]

[0006] [Patent Document 1] Korean Registered Patent No. 10-1396700 [Overview of the Initiative] [Problems that the invention aims to solve]

[0007] The objective of this embodiment is to provide a packaging substrate with superior electrical reliability by suppressing the occurrence of excessive warpage. [Means for solving the problem]

[0008] A packaging substrate according to one embodiment of this specification includes a glass core and a first composite insulating layer disposed on the glass core.

[0009] The first composite insulating layer includes an elastic insulating layer and a base insulating layer disposed on the elastic insulating layer.

[0010] The ratio of the thickness of the glass core to the thickness of the first composite insulating layer is 8 to 30.

[0011] The glass transition temperature of the elastic insulating layer is 30°C to 85°C.

[0012] The Dcp value, which is the deviation of the thermal expansion characteristics of the first composite insulating layer according to the following formula 1, may be 4 ppm / °C to 15 ppm / °C.

[0013] [Formula 1] JPEG2026182774000002.jpg553

[0014] In the above formula 1, the Tr b This is the ratio of the thickness of the base insulating layer to the thickness of the first composite insulating layer, and the CTE b This is the thermal expansion coefficient (unit: ppm / °C) of the base insulating layer measured at 25°C to 150°C, and the Tr e This is the ratio of the thickness of the elastic insulating layer to the thickness of the first composite insulating layer, and the CTEe is the coefficient of thermal expansion (unit: ppm / °C) of the elastic insulating layer measured at 25°C to 150°C.

[0015] The elongation rate of the elastic insulating layer may be 25% or more.

[0016] The ratio of the thickness of the elastic insulating layer to the thickness of the base insulating layer may be 0.05 to 0.3.

[0017] The thickness of the elastic insulating layer may be 1 μm to 15 μm.

[0018] The elastic insulating layer may be disposed in contact with at least a part of the upper surface of the glass core.

[0019] The dielectric constant Dk of the base insulating layer at a frequency of 5.8 GHz may be 4 or less.

[0020] The dielectric loss factor Df of the base insulating layer at a frequency of 5.8 GHz may be 0.01 or less.

[0021] The elastic insulating layer may contain a bismaleimide resin.

[0022] The packaging substrate may include two or more layers of the first composite insulating layer.

[0023] The packaging substrate may further include a wiring layer disposed between the first composite insulating layers.

[0024] The upper surface of the wiring layer may be disposed in contact with the lower surface of the first composite insulating layer disposed on the wiring layer.

[0025] The 90° peel strength of the wiring layer relative to the first composite insulating layer disposed on the wiring layer may be 1 kgf / cm or more. [[ID=47】Effects of the Invention

[0026] The packaging substrate in this example can suppress the generation of excessive wattage and have excellent electrical reliability. [Brief explanation of the drawing]

[0027] [Figure 1] This is a cross-sectional view illustrating a packaging substrate according to one embodiment of the actual product. [Figure 2] This is a cross-sectional view illustrating a packaging substrate according to another embodiment of the concrete example. [Figure 3] This is a cross-sectional view illustrating a packaging substrate according to yet another embodiment of the concrete example. [Best Mode for Carrying Out the Invention]

[0028] Hereinafter, embodiments will be described in detail with reference to the accompanying drawings so that they can be easily implemented by a person with ordinary skill in the art to which the present invention pertains. However, the present invention can be realized in a variety of different forms and is not limited to the embodiments described herein. Similar parts are denoted by the same reference numerals throughout the specification.

[0029] Throughout this specification, the term “these combinations” as used in any expression in Markush form means one or more mixtures or combinations selected from the group of components described in the Markush form, and includes one or more of those components.

[0030] Throughout this specification, terms such as “First,” “Second,” or “A,” “B” are used to distinguish identical terms from one another. Furthermore, singular expressions include plural expressions unless the context clearly indicates otherwise.

[0031] In this specification, "~system" may mean that the compound contains a compound corresponding to "~" or a derivative of "~".

[0032] In this specification, the meaning of B being located on A means either B being in direct contact with A, or B being located on A with other layers located between them, and is not limited to B being in contact with the surface of A.

[0033] In this specification, the meaning of B being connected to A means either that A and B are directly connected, or that A and B are connected through other components between them, and is not limited to the direct connection of A and B unless otherwise specified.

[0034] In this specification, unless otherwise specified, singular expressions are interpreted to include singular or plural, as interpreted in the context.

[0035] In this specification, the form, relative size, angles, etc., of each component in the drawings are illustrative and may be exaggerated for illustrative purposes, and the rights shall not be construed as being limited to the drawings.

[0036] In this specification, "adjacent to A and B" means that A and B are located touching each other, or that A and B are not touching but are located close to each other. In this specification, the expression "adjacent to A and B" is not construed to mean that A and B are located touching each other unless otherwise specified.

[0037] In this specification, unless otherwise specified, the physical properties of each component within the packaging substrate are assumed to have been measured at room temperature. Room temperature is defined as 20°C to 25°C.

[0038] The following provides a detailed explanation of specific examples.

[0039] Figure 1 is a cross-sectional view illustrating a packaging substrate according to one embodiment of the actual example. The actual example will be described below with reference to Figure 1.

[0040] glass core The packaging substrate 100 in this example may include a glass core 10.

[0041] The glass core 10 may have the shape of a glass substrate. For example, the glass core 10 may be made of alkali borosilicate glass, alkali-free borosilicate glass, alkali-free alkaline earth borosilicate glass, etc., and any glass plate used as an electronic component is applicable. The glass core 10 may be made of glass substrates for electronic devices, and for example, those manufactured by Schott, AGC, Corning, etc. may be used, but are not limited to these.

[0042] The glass core 10 may include through vias (not shown) that penetrate in the thickness direction of the glass core 10.

[0043] A through via consists of an internal space (not shown) and an inner diameter surface of the via (not shown) surrounding the internal space. The internal space refers to an empty space, and the inner diameter surface of the via refers to the surface of the glass core 10 formed inside the through via.

[0044] The through via may have a diameter that varies in the thickness direction of the glass core 10. The through via may have a substantially uniform diameter in the thickness direction of the glass core 10.

[0045] The surface of the glass core 10 may include an upper surface and a side surface connected to the upper surface and formed in the thickness direction of the glass core 10. The surface of the glass core 10 may also include a lower surface facing the upper surface.

[0046] The statement that the side surface is formed in the thickness direction of the glass core 10 is interpreted to mean not only that the side surface is perpendicular to the upper surface of the glass core 10, but also that at least a portion of the side surface forms an angle (angle of inclination) other than 90° with the upper surface.

[0047] The aforementioned side surface may be flat or curved.

[0048] The glass core 10 may include a cavity (not shown), which is a space formed by a recess inside.

[0049] The cavity may be formed by a recess in the upper / lower side of the glass core 10 in the thickness direction of the glass core 10, or it may penetrate through the glass core 10 in the thickness direction.

[0050] The element is mounted in the cavity, and the packaging substrate 100 and the element can be electrically connected. The element may be a semiconductor element such as a CPU, GPU, or memory chip, as well as a capacitor element, a transistor element, an impedance element, or other modules. In other words, any semiconductor element that can be mounted on a semiconductor device can be used as the element without limitation.

[0051] The thickness of the glass core 10 may be 100 μm or more. The thickness may be 200 μm or more. The thickness may be 300 μm or more. The thickness may be 3000 μm or less. The thickness may be 2000 μm or less. The thickness may be 1000 μm or less. In such cases, the glass core 10 does not easily warp during the process of forming an insulating layer on the glass core 10, which contributes to providing a thinner packaging substrate 100.

[0052] Physical properties and structure of composite insulating layers The packaging substrate 100 includes a first composite insulating layer 20 disposed on the glass core 10. The first composite insulating layer 20 includes an elastic insulating layer 21 and a base insulating layer 22 disposed on the elastic insulating layer 21.

[0053] The elastic insulating layer 21 is a layer that has insulating properties and is even more elastic than the base insulating layer 22. The elastic insulating layer 21 can function as a buffer layer that relieves stress acting on the glass core 10 in an atmosphere where the temperature repeatedly rises and falls.

[0054] The base insulating layer 22 has insulating properties and is a layer that supports the wiring layer placed on the first composite insulating layer 20.

[0055] The first composite insulating layer 20 may be positioned in contact with at least a portion of the upper surface of the glass core 10. If other components such as a wiring layer are formed on the upper surface of the glass core 10, the first composite insulating layer 20 may be positioned in contact with the upper surface of the glass core 10 that is not covered by the wiring layer or the like.

[0056] The elastic insulating layer 21 may be positioned in contact with at least a portion of the upper surface of the glass core 10. If other components, such as a wiring layer, are formed on the upper surface of the glass core 10, the elastic insulating layer 21 may be positioned in contact with the upper surface of the glass core 10 that is not covered by the wiring layer or the like.

[0057] At least a portion of the base insulating layer 22 may be placed in contact with the elastic insulating layer 21. The base insulating layer 22 may be placed in contact with the elastic insulating layer 21. The entire lower surface of the base insulating layer 22 may be placed in contact with the upper surface of the elastic insulating layer 21. That is, no other components may be placed between the elastic insulating layer 21 and the base insulating layer 22 within the first composite insulating layer 20.

[0058] One concrete example is controlling the thickness ratio of the first composite insulating layer 20 to the glass core 10, thereby preventing the glass core 10 from easily warping due to stress generated during the curing process of the first composite insulating layer 20.

[0059] The ratio of the thickness of the glass core 10 to the thickness of the first composite insulating layer 20 can be 8 to 30. The ratio may be 10 or more. The ratio may be 13 or more. The ratio may be 25 or less. The ratio may be 22 or less. The ratio may be 20 or less. A packaging substrate having such characteristics, while having a thin thickness, prevents the glass core 10 from easily warping during the lamination and curing process of the first composite insulating layer 20.

[0060] The thickness of the first composite insulating layer 20 refers to the thickness of a single layer of the first composite insulating layer 20.

[0061] The first composite insulating layer 20 may include an elastic insulating layer 21 whose glass transition temperature is controlled within a range predetermined in the embodiment. When the first composite insulating layer 20 has the above characteristics, the elastic insulating layer 21 can have sufficient elasticity to function as a buffer layer for reducing stress on the glass core 10 within the first composite insulating layer 20. Specifically, when the base insulating layer 22 is formed through a curing process or the like, the elastic insulating layer 21 can stably reduce the force that the base insulating layer 22 applies to the glass core 10.

[0062] The glass transition temperature of the elastic insulating layer 21 may be 30°C to 85°C. The glass transition temperature may be 35°C or higher. The glass transition temperature may be 40°C or higher. The glass transition temperature may be 80°C or lower. The glass transition temperature may be 75°C or lower. In such cases, the glass core 10 can stably maintain excellent flatness.

[0063] The glass transition temperature of the base insulating layer 22 may be 100°C or higher. The glass transition temperature may be 110°C or higher. The glass transition temperature may be 120°C or higher. The glass transition temperature may be 130°C or higher. The glass transition temperature may be 140°C or higher. The glass transition temperature may be 230°C or lower. The glass transition temperature may be 220°C or lower. The glass transition temperature may be 210°C or lower. The glass transition temperature may be 200°C or lower. The glass transition temperature may be 190°C or lower. In such cases, the wiring layer placed on the base insulating layer 22 can be stably fixed and maintained even in a high-temperature atmosphere.

[0064] The glass transition temperatures of the elastic insulating layer 21 and the base insulating layer 22 are measured using a thermomechanical analyzer (TMA) with JIS-C6481 as the standard. During the measurement, the tensile method is implemented in accordance with the method specified in IPC-TM650, and a heating rate of 10°C / min is applied. The glass transition temperature is measured within the range of 25°C to 150°C.

[0065] The Dcp value, which is the deviation of the thermal expansion property of the following Formula 1 of the first composite insulating layer 20, may be 4ppm / °C to 15ppm / °C.

[0066] [Formula 1] JPEG2026182774000003.jpg553

[0067] In the Formula 1, the Tr b is the ratio of the thickness of the base insulating layer 22 to the thickness of the first composite insulating layer 20, and the CTE b is the thermal expansion coefficient (unit: ppm / °C) of the base insulating layer 22 measured at 25°C to 150°C, and the Tr e is the ratio of the thickness of the elastic insulating layer 21 to the thickness of the first composite insulating layer 20, and the CTE e is the thermal expansion coefficient (unit: ppm / °C) of the elastic insulating layer 21 measured at 25°C to 150°C.

[0068] The thermal expansion coefficient is the thermal expansion coefficient in the x-y direction (CTE x-y ).

[0069] The thermal expansion coefficient is the thermal expansion coefficient in the x-y direction measured within the range of 25°C to 150°C.

[0070] In the process of forming two or more first composite insulating layers 20 on the glass core 10, the packaging substrate 100 may be repeatedly exposed to an atmosphere in which the temperature rises and falls. In this case, if the first composite insulating layer 20 expands excessively in a high-temperature atmosphere, a problem may arise in which the wiring layers formed within the first composite insulating layer 20 (particularly the wiring layers formed in the via patterns within the first composite insulating layer 20) are damaged. In addition, in a high-temperature atmosphere, repeated thermal expansion of each layer constituting the first composite insulating layer 20 may cause the base insulating layer 22 and the elastic insulating layer 21 to delaminate from each other.

[0071] In practice, the Dcp value, which is the deviation of the thermal expansion characteristics of the first composite insulating layer 20, can be controlled within a specific range. In such a case, the thermal expansion characteristics of the entire first composite insulating layer 20 can be controlled to a certain level or lower, thereby suppressing the delamination of the base insulating layer 22 from the elastic insulating layer 21 in a high-temperature atmosphere. At the same time, the strength of the force acting on the glass core due to the formation of the first composite insulating layer can be effectively reduced.

[0072] The thermal expansion coefficients of the elastic insulating layer 21 and the base insulating layer 22 are measured using a thermomechanical analyzer (TMA) according to JIS-C6481. During measurement, the tensile method is carried out according to the method specified in IPC-TM650, and a heating rate of 10°C / min is applied. The thermal expansion coefficients are measured within the range of 25°C to 150°C.

[0073] The Dcp value, which is the deviation of the thermal expansion characteristics of the first composite insulating layer 20 according to formula 1, may be 4 ppm / °C to 15 ppm / °C. The Dcp value may be 13 ppm / °C or less. The Dcp value may be 11 ppm / °C or less. The Dcp value may be 9 ppm / °C or less. The Dcp value may be 4.5 ppm / °C or more. The Dcp value may be 5 ppm / °C or more. The Dcp value may be 5.5 ppm / °C or more. The Dcp value may be 6 ppm / °C or more. In such cases, even if an elastic insulating layer 21 with sufficient elasticity is applied to the first composite insulating layer 20, it is possible to suppress delamination within the first composite insulating layer 20 and damage to electrical connections in a high-temperature atmosphere.

[0074] The thermal expansion coefficient in the x and y directions of the elastic insulating layer 21, measured within the range of 25°C to 150°C, may be 40 ppm / °C or higher. The thermal expansion coefficient may be 50 ppm / °C or higher. The thermal expansion coefficient may be 60 ppm / °C or higher. The thermal expansion coefficient may be 120 ppm / °C or lower. The thermal expansion coefficient may be 110 ppm / °C or lower. The thermal expansion coefficient may be 100 ppm / °C or lower. In such cases, the influence of the thermal expansion behavior of the elastic insulating layer 21 on the reliability of electrical connections within the packaging substrate 100 can be reduced to below a certain level.

[0075] The thermal expansion coefficient in the x and y directions of the base insulating layer 22, measured within the range of 25°C to 150°C, may be 50 ppm / °C or less. The thermal expansion coefficient may be 40 ppm / °C or less. The thermal expansion coefficient may be 30 ppm / °C or less. The thermal expansion coefficient may be 5 ppm / °C or more. In such cases, the first composite insulating layer 20 can contribute to stably supporting and fixing the wiring layer even in a high-temperature atmosphere.

[0076] The elongation rate of the elastic insulating layer 21 may be 25% or more. The elongation rate of the elastic insulating layer 21 may be 35% or more. The elongation rate of the elastic insulating layer 21 may be 45% or more. The elongation rate of the elastic insulating layer 21 may be 55% or more. The elongation rate of the elastic insulating layer 21 may be 120% or less. The elongation rate of the elastic insulating layer 21 may be 100% or less. The elongation rate of the elastic insulating layer 21 may be 80% or less. An elastic insulating layer 21 having such characteristics can effectively reduce the force acting on the glass core 10 when forming multiple layers of the first composite insulating layer 20, and can contribute to suppressing separation of the base insulating layer 22 and the elastic insulating layer 21, or damage to the elastic insulating layer 21.

[0077] The elongation of the elastic insulating layer 21 is measured using a Universal Testing Machine (UTM) at 23°C in pull mode. During measurement, the tensile speed is 1 mm / min, and the measurement is performed under average conditions of N=5.

[0078] The ratio of the thickness of the elastic insulating layer 21 to the thickness of the base insulating layer 22 may be 0.05 to 0.3. The ratio may be 0.25 or less. The ratio may be 0.22 or less. The ratio may be 0.2 or less. The ratio may be 0.18 or less. The ratio may be 0.07 or more. The ratio may be 0.1 or more. In such cases, the thermal expansion characteristics of the first composite insulating layer 20 can be stably maintained, and the elastic insulating layer 21 can effectively relieve the stress acting on the glass core 10 as a stress buffer layer.

[0079] The thickness of the elastic insulating layer 21 may be 1 μm or more. The thickness may be 2 μm or more. The thickness may be 3 μm or more. The thickness may be 15 μm or less. The thickness may be 12 μm or less. The thickness may be 10 μm or less. In such cases, the elastic insulating layer 21 can have a thickness suitable for functioning as a stress buffer layer.

[0080] The thickness of the base insulating layer 22 may be 15 μm or more. The thickness may be 18 μm or more. The thickness may be 20 μm or more. The thickness may be 23 μm or more. The thickness may be 25 μm or more. The thickness may be 28 μm or more. The thickness may be 30 μm or more. The thickness may be 50 μm or less. In such cases, the first composite insulating layer 20 can stably support the wiring layer.

[0081] If the entire surface of a wiring layer is surrounded by an insulating layer with high dielectric properties, there is a risk of significant signal loss during signal transmission through the wiring layer. In one concrete example, by surrounding a portion of the surface of the wiring layer with a base insulating layer 22 having controlled dielectric properties, smooth signal transmission through the wiring layer can be enabled.

[0082] The dielectric constant Dk of the base insulating layer 22 at a frequency of 5.8 GHz may be 4 or less. The Dk value may be 3.8 or less. The Dk value may be 3.6 or less. The Dk value may be 3.4 or less. The Dk value may be 1 or more.

[0083] The dielectric loss rate Df of the base insulating layer 22 at a frequency of 5.8 GHz may be 0.01 or less. The Df value may be 0.008 or less. The Df value may be 0.006 or less. The Df value may be 0.004 or less. The Df value may be 0.001 or more. The Df value may be 0.002 or more.

[0084] In such cases, stable signal transmission is possible without excessive signal loss through the wiring layer formed on the first composite insulating layer 20.

[0085] The Dk and Df values ​​of the base insulating layer 22 are measured at room temperature using a dielectric constant meter.

[0086] In this embodiment, the ratio of the thickness of the base insulating layer 22 and the elastic insulating layer 21 within the first composite insulating layer 20 can be adjusted. In this case, the elastic insulating layer 21 can suppress excessive thermal expansion of the first composite insulating layer 20 in the thickness direction, thereby suppressing damage to the electrical connections formed in the through vias within the first composite insulating layer 20.

[0087] Figure 2 is a cross-sectional view illustrating a packaging substrate according to another embodiment of the concrete example. The concrete example will be described below with reference to Figure 2.

[0088] The packaging substrate 100 includes a glass core 10 and a first composite insulating layer 20 disposed on the glass core 10. The components of the packaging substrate 100 are the same as those described in Figure 1 above. The differences will be explained below.

[0089] The packaging substrate 100 may further include a wiring layer 30, which is a conductor for transmitting electrical signals. The wiring layer 30 may be electrically connected to terminals and / or elements within the packaging substrate 100.

[0090] The wiring layer 30 may contain an electrically conductive material. For example, the wiring layer 30 may contain at least one of copper, nickel, aluminum, gold, and silver. Copper or the like may be used as the material for the wiring layer 30.

[0091] The packaging substrate 100 may include a wiring layer 30 disposed on the first composite insulating layer 20. The packaging substrate 100 may further include a wiring layer 30 disposed in contact with the upper surface of the glass core 10. The first composite insulating layer 20 may include through vias (not shown). The packaging substrate 100 may further include a wiring layer 30 disposed within the through vias.

[0092] The packaging substrate 100 may include two or more first composite insulating layers 20. The packaging substrate 100 may further include wiring layers 30 disposed between the first composite insulating layers 20.

[0093] The wiring layer 30 may be arranged in combination with the first composite insulating layer 20 arranged on the wiring layer 30. The wiring layer 30 may be arranged in a form embedded within the first composite insulating layer 20 arranged on the wiring layer 30. The first composite insulating layer 20 arranged on the wiring layer 30 may surround at least a portion of the top surface and / or side surface of the wiring layer 30.

[0094] The upper surface of the wiring layer 30 may be in contact with the lower surface of the first composite insulating layer 20, which is placed on the wiring layer 30. The lower surface of the wiring layer 30 may be in contact with the upper surface of the first composite insulating layer 20, which is placed below the wiring layer 30.

[0095] The 90° peel strength of the wiring layer 30 relative to the first composite insulating layer 20 placed on the wiring layer 30 may be 1 kgf / cm or more. The peel strength may be 1.2 kgf / cm or more. The peel strength may be 1.4 kgf / cm or more. The peel strength may be 3 kgf / cm or less.

[0096] The upper surface of the wiring layer 30 can be in contact with the lower surface of the elastic insulating layer 21 placed on the wiring layer 30. The 90° peel strength of the wiring layer 30 relative to the elastic insulating layer 21 placed on the wiring layer 30 may be 1 kgf / cm or more. The peel strength may be 1.2 kgf / cm or more. The peel strength may be 1.4 kgf / cm or more. The peel strength may be 3 kgf / cm or less.

[0097] In such cases, the wiring layer 30 is stably supported and fixed within the packaging substrate 100, and can have stable electrical reliability.

[0098] The peel strength of the wiring layer 30 is measured by the following method.

[0099] The multilayer film, which includes a wiring layer 30 and a first composite insulating layer 20 placed in contact with the wiring layer 30, is peeled off from the first composite insulating layer 20 located beneath the wiring layer 30. The multilayer film is then turned over, and the peel strength of the wiring layer 30 is measured while peeling the wiring layer 30 within the multilayer film from the first composite insulating layer 20. The peel strength of the wiring layer 30 is measured using a bond tester by a 90° peel test. The measurement speed (peel speed) is set to 10 mm / s, and the measurement distance (peel distance) is set to [value missing]. For example, the value of the peel strength can be measured using a Condor Sigma bond tester from XYZ TEC.

[0100] Figure 3 is a cross-sectional view illustrating a packaging substrate according to yet another embodiment of the concrete example. The concrete example will be described below with reference to Figure 3.

[0101] The packaging substrate 100 includes a glass core 10 and a first composite insulating layer 20 disposed on the glass core 10. The components of the packaging substrate 100 are the same as those described in Figure 2 above. The differences will be explained below.

[0102] The packaging substrate 100 may further include a second composite insulating layer 23 disposed beneath the glass core 10. The second composite insulating layer 23 may include the elastic insulating layer 21 and the base insulating layer 22 disposed beneath the elastic insulating layer 21. The elastic insulating layer 21 and the base insulating layer 22 included in the second composite insulating layer 23 correspond to the elastic insulating layer 21 and the base insulating layer 22 described above, respectively. A description of the elastic insulating layer 21 and the base insulating layer 22 included in the second composite insulating layer 23 will be omitted as it will overlap with the content described above.

[0103] The packaging substrate 100 may further include a wiring layer (not shown) positioned in contact with the lower surface of the glass core 10. The packaging substrate 100 may further include a wiring layer (not shown) positioned beneath the second composite insulating layer 23.

[0104] The packaging substrate 100 may include two or more layers each of the first composite insulating layer 20 and the second composite insulating layer 23. In one example, the first composite insulating layer 20 and the second composite insulating layer 23, to which the elastic insulating layer 21 is applied, can be laminated in multiple layers above and below the glass core 10. In this case, even if multiple insulating layers are laminated on the glass core 10, excessive warping of the glass core 10 can be suppressed.

[0105] The ratio of the sum of the total thicknesses of the first composite insulating layer 20 and the second composite insulating layer 23 to the thickness of the glass core 10 may be 0.7 or more. The ratio may be 0.75 or more. The ratio may be 0.8 or more. The ratio may be 2 or less. The ratio may be 1.8 or less. The packaging substrate 100 of the embodiment can have stable flatness even when such ratios are applied.

[0106] Composition of the composite insulating layer The elastic insulating layer 21 may contain bismaleimide resin. Bismaleimide resin can impart elastic properties suitable for the elastic insulating layer 21 to function as a stress buffer layer within the composite insulating layer. Furthermore, by ensuring that the elastic insulating layer 21 has excellent bonding strength to the wiring layer 30, the wiring layer 30 can be stably fixed to the elastic insulating layer 21 without excessive surface roughening treatment of the wiring layer 30. In this case, when the packaging substrate 100 is driven by applying high-frequency power, the signal loss is significantly less compared to the packaging substrate 100 with an excessively roughened wiring layer 30.

[0107] The number average molecular weight of the bismaleimide resin may be 4,000 or more. The number average molecular weight may be 7,000 or more. The number average molecular weight may be 10,000 or more. The number average molecular weight may be 15,000 or more. The number average molecular weight may be 50,000 or less. The number average molecular weight may be 45,000 or less. The number average molecular weight may be 40,000 or less. The number average molecular weight may be 35,000 or less.

[0108] The number-average molecular weight of bismaleimide resin is measured by gel permeation chromatography (GPC).

[0109] Bismaleimide resins may have a dimer acid skeleton. Bismaleimide resins may be resins formed through the reaction of acid anhydrides and diamines.

[0110] The elastic insulating layer 21 may further contain an epoxy resin. The elastic insulating layer 21 may further contain a cured epoxy resin. The epoxy resin may be any one selected from the group consisting of bisphenol-type epoxy resin, novolac-type epoxy resin, biphenyl-type epoxy resin, arylalkylene-type epoxy resin, tetraphenyloleethane-type epoxy resin, naphthalene-type epoxy resin, anthracene-type epoxy resin, phenoxy-type epoxy resin, dicyclopentadiene-type epoxy resin, norbornene-type epoxy resin, and combinations thereof.

[0111] The elastic insulating layer 21 may contain 0.1 parts by weight or more of epoxy resin per 100 parts by weight of bismaleimide resin. The elastic insulating layer 21 may contain 1 part by weight or more of epoxy resin per 100 parts by weight of bismaleimide resin. The elastic insulating layer 21 may contain 5 parts by weight or more of epoxy resin per 100 parts by weight of bismaleimide resin. The elastic insulating layer 21 may contain 15 parts by weight or less of epoxy resin per 100 parts by weight of bismaleimide resin. The elastic insulating layer 21 may contain 10 parts by weight or less of epoxy resin per 100 parts by weight of bismaleimide resin. In such cases, the elastic insulating layer 21 may have flexibility suitable for application to the first composite insulating layer 20, etc., and bonding strength to the wiring layer 30.

[0112] The elastic insulating layer 21 may further contain a filler. The filler may include an inorganic filler. The inorganic filler may be any one selected from the group consisting of barium sulfate, silica, talc, clay, magnesium carbonate, calcium carbonate, aluminum oxide, aluminum hydroxide, silicon nitride, aluminum nitride, titanium oxide, and combinations thereof.

[0113] The elastic insulating layer 21 may further contain other additives in addition to the components described above. The additives are not limited as long as they are commonly used in the field of packaging substrates. Examples of additives include curing agents, colorants, and defoamers.

[0114] The base insulating layer 22 may contain epoxy resin and filler. The base insulating layer 22 may also contain cured epoxy resin and filler.

[0115] The epoxy resin mentioned above may be used. A detailed explanation of epoxy resins will be omitted as it will overlap with the previously mentioned content.

[0116] The base insulating layer 22 may contain 10% by weight or more of epoxy resin. The base insulating layer 22 may contain 15% by weight or more of epoxy resin. The base insulating layer 22 may contain 20% by weight or more of epoxy resin. The base insulating layer 22 may contain 50% by weight or less of epoxy resin. The base insulating layer 22 may contain 45% by weight or less of epoxy resin. The base insulating layer 22 may contain 40% by weight or less of epoxy resin.

[0117] The base insulating layer 22 may contain fillers. The base insulating layer 22 may contain the fillers mentioned above. The explanation of fillers will be omitted as it will be redundant with the explanation given above.

[0118] The base insulating layer 22 may further contain other additives in addition to the components described above. The additives are not limited to those commonly used in the field of packaging substrates. Examples of additives include curing agents, colorants, and defoamers.

[0119] Semiconductor packages A semiconductor package according to yet another embodiment of the embodiment includes a packaging substrate and an element electrically connected to the packaging substrate.

[0120] The packaging board can be mounted on the main board and electrically connected to the main board.

[0121] The explanation of the packaging substrate and components will be omitted as it will overlap with the content described above.

[0122] Manufacturing method for packaging substrates A further embodiment of the embodiment is a method for manufacturing a packaging substrate that includes a composite insulating layer formation step of forming a composite insulating layer on a glass core.

[0123] The explanation of the glass core will be omitted as it will overlap with what was previously mentioned.

[0124] If necessary, a glass core with a wiring layer formed on its upper surface can be provided.

[0125] The composite insulating layer formation step may include an elastic insulating layer formation process in which an elastic insulating layer is formed on a glass core, and a base insulating layer formation process in which a base insulating layer is formed on the elastic insulating layer.

[0126] The process for forming the elastic insulating layer can be carried out by laminating an elastic insulating layer-forming film onto a glass core and curing it, or by applying an elastic insulating layer-forming composition onto a glass core and then curing it.

[0127] The film or composition for forming an elastic insulating layer may contain a bismaleimide resin. The number average molecular weight of the bismaleimide resin may be 4,000 or more. The number average molecular weight may be 7,000 or more. The number average molecular weight may be 10,000 or more. The number average molecular weight may be 15,000 or more. The number average molecular weight may be 50,000 or less. The number average molecular weight may be 45,000 or less. The number average molecular weight may be 40,000 or less. The number average molecular weight may be 35,000 or less.

[0128] The number-average molecular weight of bismaleimide resin is measured by gel permeation chromatography (GPC).

[0129] Bismaleimide resins may have a dimer acid skeleton. Bismaleimide resins may be resins formed through the reaction of acid anhydrides and diamines.

[0130] The film or composition for forming an elastic insulating layer may further contain an epoxy resin. The epoxy resin may be any one selected from the group consisting of bisphenol-type epoxy resins, novolac-type epoxy resins, biphenyl-type epoxy resins, arylalkylene-type epoxy resins, tetraphenyloleethane-type epoxy resins, naphthalene-type epoxy resins, anthracene-type epoxy resins, phenoxy-type epoxy resins, dicyclopentadiene-type epoxy resins, norbornene-type epoxy resins, and combinations thereof.

[0131] The film or composition for forming an elastic insulating layer may contain 0.1 parts by weight or more of epoxy resin per 100 parts by weight of bismaleimide resin. The film or composition for forming an elastic insulating layer may contain 1 part by weight or more of epoxy resin per 100 parts by weight of bismaleimide resin. The film or composition for forming an elastic insulating layer may contain 5 parts by weight or more of epoxy resin per 100 parts by weight of bismaleimide resin. The film or composition for forming an elastic insulating layer may contain 15 parts by weight or less of epoxy resin per 100 parts by weight of bismaleimide resin. The film or composition for forming an elastic insulating layer may contain 10 parts by weight or less of epoxy resin per 100 parts by weight of bismaleimide resin. In such cases, the elastic insulating layer may function as a stress buffer layer to reduce stress on the glass core and may have physical properties suitable for fixing the wiring layer.

[0132] The film or composition for forming an elastic insulating layer may further contain fillers. The elastic insulating layer may also contain the aforementioned fillers. A description of the fillers in the elastic insulating layer is omitted as it will be redundant with the previous description.

[0133] The film or composition for forming an elastic insulating layer may further contain other additives in addition to the components described above. The additives are not limited as long as they are commonly used in the field of packaging substrates. Examples of additives include curing agents, colorants, and defoamers.

[0134] An elastic insulating layer can be formed by laminating a film for forming an elastic insulating layer onto a glass core and curing the film.

[0135] Specifically, the film for forming the elastic insulating layer can be vacuum-bonded to the upper surface of the glass core, and then laminated by hot-pressing.

[0136] Vacuum sealing of the film for forming the elastic insulating layer may be performed for 10 seconds or more. Vacuum sealing of the film for forming the elastic insulating layer may be performed for 20 seconds or more. Vacuum sealing of the film for forming the elastic insulating layer may be performed for 120 seconds or less.

[0137] Vacuum bonding of the film for forming the elastic insulating layer may be carried out in an atmosphere of 50°C or higher. Vacuum bonding of the film for forming the elastic insulating layer may be carried out in an atmosphere of 60°C or higher. Vacuum bonding of the film for forming the elastic insulating layer may be carried out in an atmosphere of 150°C or lower. Vacuum bonding of the film for forming the elastic insulating layer may be carried out in an atmosphere of 140°C or lower.

[0138] The press pressure during vacuum adhesion of the film for forming the elastic insulating layer may be 0.05 MPa or higher. The press pressure may be 0.1 MPa or higher. The press pressure may be 1 MPa or lower.

[0139] When hot-pressing the film for forming the elastic insulating layer, the hot-press temperature may be 70°C or higher. The hot-press temperature may be 80°C or higher. The hot-press temperature may be 200°C or lower. The hot-press temperature may be 180°C or lower.

[0140] The pressure applied when hot-pressing the film for forming the elastic insulating layer is 1 kgf / cm². 2 The above pressure may also be greater than 3 kgf / cm². 2 The pressure may be greater than or equal to 10 kgf / cm². 2 The following is also acceptable.

[0141] The hot-press adhesion of the film for forming the elastic insulating layer may be performed for 10 seconds or more. The hot-press adhesion of the film for forming the elastic insulating layer may be performed for 20 seconds or more. The hot-press adhesion of the film for forming the elastic insulating layer may be performed for 90 seconds or less.

[0142] An elastic insulating layer can be formed by curing a laminated film for forming an elastic insulating layer.

[0143] The curing of the film for forming the elastic insulating layer can be carried out through two or more heat treatment steps.

[0144] In the primary heat treatment process, the ambient temperature may be 90°C or higher. The ambient temperature may be 100°C or higher. The ambient temperature may be 110°C or higher. The ambient temperature may be 150°C or lower.

[0145] The primary heat treatment process may be carried out for 10 minutes or more. The primary heat treatment process may be carried out for 15 minutes or more. The primary heat treatment process may be carried out for 20 minutes or more. The primary heat treatment process may be carried out for 60 minutes or less.

[0146] In the secondary heat treatment process, the ambient temperature may be 110°C or higher. The ambient temperature may be 120°C or higher. The ambient temperature may be 130°C or higher. The ambient temperature may be 200°C or lower.

[0147] The secondary heat treatment process may be carried out for 10 minutes or more. The secondary heat treatment process may be carried out for 15 minutes or more. The secondary heat treatment process may be carried out for 20 minutes or more. The secondary heat treatment process may be carried out for 60 minutes or less.

[0148] The base insulating layer can be formed by laminating a film for forming the base insulating layer onto an elastic insulating layer or a film for manufacturing an elastic insulating layer, or by applying a composition for forming the base insulating layer and then curing the film or composition.

[0149] The film or composition for manufacturing the base insulating layer may contain epoxy resin and fillers.

[0150] The epoxy resin mentioned above may be used. A detailed explanation of epoxy resins will be omitted as it will overlap with the previously mentioned content.

[0151] The film for manufacturing the base insulating layer may contain 10% by weight or more of epoxy resin. The film for manufacturing the base insulating layer may contain 15% by weight or more of epoxy resin. The film for manufacturing the base insulating layer may contain 20% by weight or more of epoxy resin. The film for manufacturing the base insulating layer may contain 50% by weight or less of epoxy resin. The film for manufacturing the base insulating layer may contain 45% by weight or less of epoxy resin. The film for manufacturing the base insulating layer may contain 40% by weight or less of epoxy resin.

[0152] The film for manufacturing the base insulating layer may contain fillers. The film for manufacturing the base insulating layer may contain the fillers mentioned above. The explanation of fillers is omitted as it will be redundant with the explanation above.

[0153] The film for manufacturing the base insulating layer may further contain other additives in addition to the components described above. The additives are not limited as long as they are those commonly used in the field of build-up films. Examples of additives include curing agents, colorants, and defoamers.

[0154] A base insulating layer can be formed by laminating a film for forming a base insulating layer onto an elastic insulating layer or a film for manufacturing an elastic insulating layer, and then curing the film.

[0155] A film for forming the base insulating layer can be placed in the area to be formed, the film can be vacuum-bonded to the surface, and then laminated by hot pressing.

[0156] When the film for forming the base insulating layer is vacuum-bonded, the time during which the vacuum pressure is applied may be 10 seconds or more. The time may be 20 seconds or more. The time may be 90 seconds or less.

[0157] When hot-pressing the film for forming the base insulating layer, the hot-press temperature may be 70°C or higher. The hot-press temperature may be 80°C or higher. The hot-press temperature may be 200°C or lower. The hot-press temperature may be 180°C or lower.

[0158] The pressure applied when hot-pressing the film for forming the base insulating layer is 3 kgf / cm². 2 The above pressure may also be greater than 5 kgf / cm². 2 The above pressure may also be greater. 2 The following is also acceptable.

[0159] After laminating the base insulating layer film, the laminated base insulating layer film can be further hot-pressed to adhere it to the surface.

[0160] The pressure applied when hot-pressing the base insulating layer film is 1 kgf / cm². 2 The above pressure may also be greater than 3 kgf / cm². 2 The pressure may be greater than or equal to 10 kgf / cm². 2 The following is also acceptable.

[0161] When additionally hot-pressing the film for forming the base insulating layer, the hot-press temperature may be 70°C or higher. The hot-press temperature may be 80°C or higher. The hot-press temperature may be 200°C or lower. The hot-press temperature may be 180°C or lower.

[0162] When hot-pressing the base insulating layer film to adhere it, the time for which pressure is applied may be 10 seconds or more. The aforementioned time may be 20 seconds or more. The aforementioned time may be 90 seconds or less.

[0163] The base insulating layer can be formed by curing the laminated base insulating layer forming film.

[0164] The curing of the film for forming the base insulating layer can be carried out through two or more heat treatment steps.

[0165] In the primary heat treatment process, the ambient temperature may be 90°C or higher. The ambient temperature may be 100°C or higher. The ambient temperature may be 110°C or higher. The ambient temperature may be 150°C or lower.

[0166] The primary heat treatment process may be carried out for 10 minutes or more. The primary heat treatment process may be carried out for 15 minutes or more. The primary heat treatment process may be carried out for 20 minutes or more. The primary heat treatment process may be carried out for 60 minutes or less.

[0167] In the secondary heat treatment process, the ambient temperature may be 110°C or higher. The ambient temperature may be 120°C or higher. The ambient temperature may be 130°C or higher. The ambient temperature may be 200°C or lower.

[0168] The secondary heat treatment process may be carried out for 10 minutes or more. The secondary heat treatment process may be carried out for 15 minutes or more. The secondary heat treatment process may be carried out for 20 minutes or more. The secondary heat treatment process may be carried out for 60 minutes or less.

[0169] A first composite insulating layer can be formed by forming an elastic insulating layer and a base insulating layer on the elastic insulating layer.

[0170] The first composite insulating layer may be formed by laminating and curing a film for manufacturing an elastic insulating layer, and then laminating and curing a film for manufacturing a base insulating layer on the elastic insulating layer, or by laminating a film for manufacturing an elastic insulating layer and a film for manufacturing a base insulating layer, and then curing the two films simultaneously.

[0171] If necessary, after forming a wiring layer on the first composite insulating layer, another first composite insulating layer can be formed on the wiring layer so as to surround the wiring layer, thereby forming a re-wiring layer on the glass core.

[0172] The wiring layer may be formed using a dry or wet method.

[0173] The dry method is a method in which a seed layer is formed by sputtering in the area where the wiring layer will be placed, and then the wiring layer is formed by plating in the area where the seed layer has been formed. When forming the seed layer, metals such as titanium, chromium, and nickel may be sputtered, or the above metals and copper may be applied together during sputtering. Through sputtering, an anchoring effect occurs in which the surface of the glass core or the first composite insulating layer interacts with the metal particles, which can improve the adhesion of the wiring layer.

[0174] The wet method is a method in which a primer is applied to the area where the wiring layer needs to be formed, followed by seed layer formation and metal plating. The primer may contain compounds having functional groups such as amines. Depending on the desired degree of adhesion, the primer may contain both compounds having functional groups such as amines and silane coupling agents. When using a silane coupling agent, the surface to be primed can be pretreated with the silane coupling agent, and then a compound having amine groups can be applied to the pretreated area to form the primer layer.

[0175] After forming a seed layer, a wiring layer can be formed by plating with a metal. Copper plating may be applied during the formation of the wiring layer, but is not limited to this. Before metal plating, parts of the seed layer or primer layer where the wiring layer is not required can be deactivated, or parts where the wiring layer is required can be activated before plating. The activation or deactivation treatment method may include light irradiation treatment using a laser of a specific wavelength, chemical treatment, etc. However, after metal plating without applying activation or deactivation treatment, the wiring layer can be etched and patterned according to a pre-designed shape.

[0176] After forming the wiring layer, a first composite insulating layer can be formed surrounding the wiring layer. The first composite insulating layer formed on the wiring layer can be formed by the same method as described above.

[0177] If necessary, a second composite insulating layer can be formed beneath the glass core using the same method applied to the formation of the first composite insulating layer. The second composite insulating layer can be manufactured by the same method as the first composite insulating layer, except that a base insulating layer is formed beneath the elastic insulating layer. Details regarding the method for forming the second composite insulating layer are omitted as they overlap with the above.

[0178] The manufacturing method for the packaging substrate in the embodiment may further include steps of forming connection terminals, bumps, cover layers, etc., on the upper and / or lower surfaces of the packaging substrate, or mounting elements on the substrate.

[0179] The following examples will provide a more detailed explanation of the implementation through specific embodiments. These embodiments are merely illustrative to aid in understanding the implementation, and the scope of implementation is not limited to them.

[0180] Manufacturing example: Manufacturing of packaging substrates Example 1: Shin-Etsu's SLK-214 film, an elastic insulating layer formation film, was laminated onto a 650 μm thick glass substrate. Specifically, the elastic insulating layer formation film was vacuum-bonded to the substrate in a reduced-pressure atmosphere at 80°C under a pressure of 0.3 MPa for 30 seconds. Then, the elastic insulating layer formation film was subjected to a temperature of 120°C and a pressure of 3 kgf / cm². 2 The area was hot-pressed with pressure for 30 seconds.

[0181] A GL103 film from AFT, which is a base insulating layer forming film, was laminated onto a laminated elastic insulating layer forming film. After the laminated base insulating layer forming film was vacuum-bonded for 30 seconds in a reduced-pressure atmosphere, the base insulating layer forming film was subjected to a temperature of 120°C and a pressure of 7 kgf / cm². 2 Hot pressing was performed with a pressure of 5 kgf / cm². Subsequently, a temperature of 120°C and a pressure of 5 kgf / cm² were applied. 2 The film for forming the base insulating layer was subjected to hot-press adhesion for 60 seconds under pressure.

[0182] Using the same method, seven layers each of elastic insulating layer forming film and base insulating layer forming film were alternately laminated on a glass core, and seven layers each of elastic insulating layer forming film and base insulating layer forming film were alternately laminated below the glass core.

[0183] Subsequently, the substrate was heat-treated at 130°C for 30 minutes and then at 165°C for 30 minutes to form a first composite insulating layer and a second composite insulating layer. The substrate was then singulated to manufacture a packaging substrate. In the packaging substrate, the thickness of the elastic insulating layer was observed to be 5 μm, and the thickness of the base insulating layer was observed to be 35 μm.

[0184] Example 2: A packaging substrate was manufactured under the same conditions as in Example 1, except that Shin-Etsu's SLK-215 film was used as the film for forming the elastic insulating layer, and the ambient temperature during vacuum adhesion of the film for forming the elastic insulating layer was set to 120°C. In the said packaging substrate, the thickness of the elastic insulating layer was observed to be 5 μm, and the thickness of the base insulating layer was observed to be 35 μm.

[0185] Example 3: A 20 μm thick copper foil was prepared, with its surface roughened to have an arithmetic mean roughness Ra of 500 nm. An elastic insulating layer-forming film and a base insulating layer-forming film were laminated onto the upper surface of the copper foil under the same conditions as in Example 1. Subsequently, the copper foil laminate was heat-treated under the same conditions as in Example 1 to form the elastic insulating layer and the base insulating layer.

[0186] Comparative Example 1: A packaging substrate was manufactured under the same conditions as in Example 1, except that a film for forming an elastic insulating layer was not applied. In the packaging substrate, the thickness of the base insulating layer was observed to be 35 μm.

[0187] Evaluation example: Measurement of the physical properties of each insulating layer Test specimens were prepared by cutting the elastic insulating layer and base insulating layer from the packaging substrates of each example and comparative example. Using a thermomechanical analyzer (TMA) according to JIS-C6481, the glass transition temperature and thermal expansion coefficient of the elastic insulating layer and base insulating layer were measured for each example and comparative example, and the Dcp value was calculated. During measurement, the tensile method was carried out according to the method specified in IPC-TM650, and a heating rate of 10°C / min was applied. The glass transition temperature and thermal expansion coefficient were measured within the range of 25°C to 150°C.

[0188] Subsequently, the elongation of the elastic insulating layer for each example and comparative example was measured using a Universal Testing Machine (UTM) at 23°C in pull mode. During measurement, the tensile speed was 1 mm / min, and the elongation was measured under the average condition of N=5.

[0189] Then, using a dielectric constant meter, the dielectric constant Dk and dielectric loss rate Df of the base insulating layer for each example and comparative example were measured at room temperature at a frequency of 5.8 GHz.

[0190] In Example 3, the 90° peel strength of the copper foil from the elastic insulating layer was measured while peeling the copper foil from the elastic insulating layer. The 90° peel strength of the copper foil was measured using a Condor Sigma bond tester from XYZ TEC by a 90° peel test. The measurement speed was set to 10 mm / s and the measurement distance was set to [specify distance]. A measurement value of 1 kgf / cm or more was evaluated as Pass, and a measurement value of less than 1 kgf / cm was evaluated as Fail.

[0191] The measured values ​​and evaluation results for each insulating layer in the examples and comparative examples are shown in Table 1 below.

[0192] Evaluation example: Workpage evaluation In the manufacturing process of the packaging substrates in Examples 1 and 2 and Comparative Example 1, the wattage of the substrate was evaluated before singulation. Specifically, after placing the substrate on a flat floor surface, the height at which the edge of the substrate lifted from the floor surface was measured. The maximum measured height value is shown in Table 2 below.

[0193] [Table 1]

[0194] [Table 2]

[0195] Referring to Table 2 above, in the evaluation of the warpage, the measured values ​​were 5 mm or less in Examples 1 and 2, while the measured value exceeded 10 mm in Comparative Example 1.

[0196] Although preferred embodiments of the present invention have been described in detail above, the scope of the present invention is not limited thereto. Various modifications and improvements by those skilled in the art, utilizing the basic concepts of the present invention as defined in the appended claims, also fall within the scope of the present invention. [Explanation of Symbols]

[0197] 100 Packaging substrates 10 glass cores 20 First Composite Insulating Layer 21 Elastic insulating layer 22 Base insulating layer 23. Second composite insulating layer 30 wiring layer

Claims

1. It includes a glass core and a first composite insulating layer disposed on the glass core, The first composite insulating layer includes an elastic insulating layer and a base insulating layer disposed on the elastic insulating layer. The ratio of the thickness of the glass core to the thickness of the first composite insulating layer is 8 to 30. A packaging substrate having a glass transition temperature of 30°C to 85°C in the elastic insulating layer.

2. The packaging substrate according to claim 1, wherein the Dcp value, which is the deviation of the thermal expansion characteristics of the first composite insulating layer according to the following formula 1, is 4 ppm / °C to 15 ppm / °C. [Formula 1] (In the above formula 1, The aforementioned Tr b This is the ratio of the thickness of the base insulating layer to the thickness of the first composite insulating layer, The CTE b This is the thermal expansion coefficient (unit: ppm / °C) of the base insulating layer measured at 25°C to 150°C. The aforementioned Tr e This is the ratio of the thickness of the elastic insulating layer to the thickness of the first composite insulating layer, The CTE e This is the coefficient of thermal expansion (unit: ppm / °C) of the elastic insulating layer measured at 25°C to 150°C.

3. The packaging substrate according to claim 1, wherein the elongation rate of the elastic insulating layer is 25% or more.

4. The packaging substrate according to claim 1, wherein the ratio of the thickness of the elastic insulating layer to the thickness of the base insulating layer is 0.05 to 0.

3.

5. The packaging substrate according to claim 1, wherein the thickness of the elastic insulating layer is 1 μm to 15 μm.

6. The packaging substrate according to claim 1, wherein the elastic insulating layer is disposed in contact with at least a portion of the upper surface of the glass core.

7. The packaging substrate according to claim 1, wherein the dielectric constant Dk of the base insulating layer at a frequency of 5.8 GHz is 4 or less.

8. The packaging substrate according to claim 1, wherein the dielectric loss rate Df of the base insulating layer at a frequency of 5.8 GHz is 0.01 or less.

9. The packaging substrate according to claim 1, wherein the elastic insulating layer comprises a bismaleimide resin.

10. The first composite insulating layer comprises two or more layers, The invention further includes a wiring layer disposed between the first composite insulating layers, The upper surface of the wiring layer is in contact with the lower surface of the first composite insulating layer, which is arranged on the wiring layer. The packaging substrate according to claim 1, wherein the 90° peel strength of the wiring layer relative to the first composite insulating layer disposed on the wiring layer is 1 kgf / cm or more.

Citation Information

Patent Citations

  • Multilayered circuit board and semiconductor device

    KR101396700B1