Method for producing ethylene-vinyl alcohol copolymer film
The method addresses film whitening in EVOH resin films by maintaining an alcohol-rich solvent composition and temperature during spray coating, improving productivity and reducing capital costs.
Patent Information
- Application Number
- JP2026075046
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2025-05-09
- Filing Date
- 2026-04-28
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional methods for forming ethylene-vinyl alcohol copolymer (EVOH) films using spray coating result in film whitening due to solvent composition imbalances, particularly when alcohol with a lower boiling point preferentially volatilizes, and require preheating, leading to high capital investment and reduced productivity.
A method for producing EVOH resin films through spray coating with an ethylene-vinyl alcohol copolymer solution having a specific composition and temperature, ensuring the solution remains alcohol-rich, suppressing film whitening and eliminating the need for preheating.
The method effectively suppresses film whitening during spray coating, reduces capital investment, and enhances productivity by avoiding preheating, making it suitable for various packaging applications.
Smart Images

Figure 2026182791000001
Abstract
Description
Technical Field
[0001] The present invention relates to a method for producing an ethylene-vinyl alcohol copolymer film.
Background Art
[0002] Films obtained from an ethylene-vinyl alcohol copolymer (hereinafter sometimes referred to as "EVOH resin") are excellent in transparency, gas barrier properties against oxygen and the like, and are useful as various packaging materials for foods, medical products, industrial chemicals and the like, or as composite materials laminated with plastic films, paper, and metal foils.
[0003] When forming an EVOH resin film, any method can be used, but a solution coating method has attracted attention, in which a solution of EVOH resin dissolved in a solvent or an aqueous dispersion of EVOH resin dispersed in water is applied to a substrate, in view of the fact that a relatively thin film can be formed, a film can be easily formed even on a substrate having a complicated shape such as a hollow container, and the coating operation can be performed with a relatively simple apparatus.
[0004] However, when a film is formed using an EVOH resin, there are few known good solvents used in the coating step, and when a solution prepared using such a solvent is applied to a substrate and dried, a whitened film is likely to be obtained.
[0005] Accordingly, as a method for forming an EVOH resin film, for example, Patent Document 1 discloses a method for forming an EVOH resin film, in which the EVOH resin is dissolved using a solvent obtained by mixing a specific alcohol and water at a specific ratio, and coating and drying are performed under coating conditions where the solution temperature is 50°C or higher, whereby whitening of the EVOH resin film can be suppressed.
Prior Art Documents
Patent Documents
[0006]
Patent Document 1
Summary of the Invention
[0007] However, while the technology disclosed in Patent Document 1 can suppress film whitening in coating methods such as bar coating and dip coating, when spray coating is used, if the solvent composition of water and alcohol is 1:1, the surface area of the solution increases, causing the alcohol, which has a lower boiling point, to preferentially volatilize. When the solution adheres to the object, the solvent composition becomes water-rich, resulting in film whitening. In particular, when the solution temperature is high (50°C or higher), the volatilization of the alcohol is accelerated, and the effect of whitening becomes more pronounced. Furthermore, since solutions are typically stored at room temperature (around 20°C), conventional technologies require preheating, and the coater also requires heating equipment, resulting in high capital investment costs and reduced productivity.
[0008] Therefore, against this background, the present invention aims to provide a method for producing an EVOH resin film that can suppress whitening of the film when an EVOH resin solution is formed during spray coating. [Means for solving the problem]
[0009] In view of these circumstances, the inventors conducted extensive research and, as a result, discovered that by making the solution composition richer in alcohol than the usual optimal composition range, the solution composition remains within a suitable range for EVOH resin even when alcohol evaporates during spray coating, thus completing the present invention.
[0010] In other words, the present invention has the following aspects. [1] A method for producing an ethylene-vinyl alcohol copolymer film by spray coating with an ethylene-vinyl alcohol copolymer solution, The ethylene-vinyl alcohol copolymer solution comprises an ethylene-vinyl alcohol copolymer and a water-alcohol mixed solvent. The solution composition of the ethylene-vinyl alcohol copolymer solution satisfies the following formula (1): The concentration of the ethylene-vinyl alcohol copolymer in the ethylene-vinyl alcohol copolymer solution is less than 10% by mass. A method for producing an ethylene-vinyl alcohol copolymer film, wherein the solution temperature of the ethylene-vinyl alcohol copolymer solution is less than 50°C. ·Solution composition: 26+X <n<0.5X+65···(1) [X: Percentage of ethylene structural units in ethylene-vinyl alcohol copolymer (mol%), n: Alcohol concentration in water-alcohol mixed solvent (mass%)] [2] The method for producing an ethylene-vinyl alcohol copolymer film according to [1], wherein the content of ethylene structural units in the ethylene-vinyl alcohol copolymer is 25 to 44 mol%. [3] The method for producing an ethylene-vinyl alcohol copolymer film according to [1] or [2], wherein the viscosity of the ethylene-vinyl alcohol copolymer solution, as measured with a B-type viscometer at a solution temperature of 20°C, is 200 mPa·s or less. [Effects of the Invention]
[0011] The manufacturing method of the present invention can suppress film whitening when forming an EVOH resin solution film during spray coating. Furthermore, since the manufacturing method of the present invention does not require preheating of the solution, capital investment can be reduced and productivity can be improved. [Modes for carrying out the invention]
[0012] The present invention will be described below based on examples of embodiments for carrying out the present invention. However, the present invention is not limited to the embodiments described below.
[0013] In this specification, "x and / or y (where x and y are any combination)" means at least one of x and y, and can mean x only, y only, or x and y. When the expression "X to Y" (X and Y are any numbers) is used, unless otherwise specified, it means "X or more and Y or less", and also includes the meanings of "preferably more than X" or "preferably less than Y". When the expression "X or more" (X is any number) or "Y or less" (Y is any number) is used, it also includes the meanings of "preferably more than X" or "preferably less than Y". With regard to the numerical ranges described stepwise in the present specification, the upper limit value or lower limit value of a numerical range in a certain step can be arbitrarily combined with the upper limit value or lower limit value of a numerical range in another step. In addition, in the numerical ranges described in the present specification, the upper limit value or lower limit value of the numerical range can also be replaced with the values shown in the Examples. In the present specification, a combination of preferred embodiments is a more preferred embodiment. In the present specification, room temperature as well as various physical property values and characteristic values are at 20°C unless otherwise specified. In the present specification, the term "layer" has a meaning that includes not only a thick layer but also relatively thin layers such as "film", "tape", and "sheet". When describing measurement methods and the like based on standards in the present specification, unless otherwise specified, they are based on the relevant standard as of the filing date of the present application (or the priority date if a priority date is claimed). If the relevant standard has been abolished at that time, it shall be based on the standard as of the abolition date.
[0014] The method for producing an EVOH resin film according to one embodiment of the present invention (hereinafter sometimes referred to as "the present production method") is obtained by spray-coating an EVOH resin solution. Hereinafter, before describing the present production method, the EVOH resin solution will be described.
[0015] <EVOH Resin Solution> The EVOH resin solution used in the present production method is obtained by dissolving an EVOH resin in a water-alcohol mixed solvent.
[0016] [EVOH Resin] The EVOH resin is usually a resin obtained by saponifying an ethylene-vinyl ester copolymer, which is a copolymer of ethylene and a vinyl ester monomer, and is a water-insoluble thermoplastic resin.
[0017] As the vinyl ester monomer used for the EVOH resin, vinyl acetate is typically used from the viewpoints of good commercial availability and high impurity treatment efficiency during production. Examples of other vinyl ester monomers include aliphatic vinyl esters such as vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, and vinyl versatate, and aromatic vinyl esters such as vinyl benzoate. Usually, aliphatic vinyl esters having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, particularly preferably 4 to 7 carbon atoms can be used. These can be used alone or in combination of two or more.
[0018] As the polymerization method of ethylene and the vinyl ester monomer, any known polymerization method such as solution polymerization, suspension polymerization, or emulsion polymerization can be used, and solution polymerization using methanol as a solvent is generally employed. Saponification of the obtained ethylene-vinyl ester copolymer can also be carried out by a known method. The EVOH resin produced in this manner is mainly composed of ethylene-derived structural units and vinyl alcohol structural units, and usually contains a small amount of residual vinyl ester structural units that are not saponified.
[0019] The content ratio (X) of the ethylene structural unit in the EVOH resin is usually 25 to 44 mol%, preferably 26 to 40 mol%, more preferably 27 to 38 mol%, and particularly preferably 28 to 35 mol%. When the content ratio is at or above the lower limit, the gas barrier property under high humidity tends to be excellent, while when it is at or below the upper limit, the gas barrier property tends to be excellent. The content ratio of the ethylene structural unit can be controlled by the pressure of ethylene when copolymerizing the vinyl ester monomer and ethylene. The content ratio (X) of such ethylene structural units is usually, 1 It is measured by 1H-NMR. For example, 1 A measurement method is used that employs 1H-NMR, with DMSO-d6 as the measurement solvent and a measurement temperature of 50°C.
[0020] The degree of saponification of the EVOH resin is typically 90-100 mol%, preferably 95-100 mol%, and more preferably 99-100 mol%. The degree of saponification can be controlled by the amount of saponification catalyst (usually an alkaline catalyst such as sodium hydroxide) used to saponify the ethylene-vinyl ester copolymer, the temperature, the time, etc. When the degree of saponification is above the lower limit, the resin tends to exhibit excellent gas barrier properties. The degree of saponification of such EVOH resin is typically, 1 It is measured by 1H-NMR. For example, 1 A measurement method using 1H-NMR is employed, with DMSO-d6 as the measurement solvent and a measurement temperature of 50°C.
[0021] The melt flow rate (MFR) (210°C, 2160g load) of the EVOH resin is typically 0.5 to 100 g / 10 min, preferably 1 to 50 g / 10 min, and more preferably 3 to 35 g / 10 min. Within this MFR range, the resin tends to exhibit excellent coating properties. The aforementioned MFR is an indicator of the degree of polymerization of the EVOH resin and can be adjusted by the amount of polymerization initiator and solvent used when copolymerizing ethylene and vinyl ester monomers.
[0022] Furthermore, the EVOH resin may contain structural units derived from the following comonomers, to the extent that they do not impede the effects of the present invention (for example, 10 mol% or less of the EVOH resin). Examples of the comonomers include olefins such as propylene, 1-butene, and isobutene; hydroxyl group-containing α-olefins such as 3-buten-1-ol, 3-buten-1,2-diol, 4-penten-1-ol, and 5-hexen-1,2-diol, and their esterified and acylated derivatives; hydroxyalkylvinylidenes such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1,3-diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, and 1,3-dibutyl Hydroxyalkylvinylidene diacetates such as hydroxy-2-methylenepropane; unsaturated acids such as acrylic acid, methacrylic acid, crotonic acid, (anhydride) phthalic acid, (anhydride) maleic acid, (anhydride) itaconic acid, or their salts, or mono or dialkyl esters with 1 to 18 carbon atoms in the alkyl group; acrylamide, N-alkylacrylamide with 1 to 18 carbon atoms in the alkyl group, N,N-dimethylacrylamide, 2-acrylamidopropanesulfonic acid or its salts, acrylamidopropyldimethylamine or its salts or its quaternary salts Acrylamides such as methacrylamide, N-alkylmethacrylamide with 1 to 18 C1 of the alkyl group, N,N-dimethylmethacrylamide, 2-methacrylamidepropanesulfonic acid or its salts, methacrylamidopropyldimethylamine or its salts or its quaternary salts, and other methacrylamides; N-vinylamides such as N-vinylpyrrolidone, N-vinylformamide, N-vinylacetamide; vinyl cyanides such as acrylonitrile, methacrylnitrile, and other alkyl vinyl ethers with 1 to 18 C1 of the alkyl group, hydro Examples include vinyl ethers such as xyalkyl vinyl ethers and alkoxyalkyl vinyl ethers; vinyl halogenated compounds such as vinyl chloride, vinylidene chloride, vinyl fluoride, vinylidene fluoride, and vinyl bromide; vinyl silanes such as trimethoxyvinylsilane; allyl halogenated compounds such as allyl acetate and allyl chloride; allyl alcohols such as allyl alcohol and dimethoxyallyl alcohol; and comonomers such as trimethyl-(3-acrylamido-3-dimethylpropyl)-ammonium chloride and acrylamide-2-methylpropanesulfonic acid.These can be used individually or in combination of two or more types.
[0023] Among these, hydroxyl group-containing α-olefins are preferred, and 3-butene-1,2-diol and 5-hexene-1,2-diol are particularly preferred. When the hydroxyl group-containing α-olefins are copolymerized, the resulting EVOH resin has primary hydroxyl groups in its side chains. Such EVOH resins having primary hydroxyl groups in their side chains, and especially EVOH resins having a 1,2-diol structure in their side chains, are preferred because they maintain gas barrier properties while exhibiting good flexibility.
[0024] When the EVOH resin has a primary hydroxyl group in its side chain, the content of structural units derived from monomers having the primary hydroxyl group is typically 0.1 to 20 mol%, preferably 0.5 to 15 mol%, and particularly preferably 1 to 10 mol% of the EVOH resin.
[0025] Furthermore, as the EVOH resin, EVOH resins that have undergone "post-modification" such as esterification, urethaneization, acetalization, cyanoethylation, or oxyalkyleneization can also be used.
[0026] When using the post-modified EVOH resin described above, the modification rate is usually 10 mol% or less, preferably 4 mol% or less. The lower limit is 0.1 mol%. If the modification rate of such EVOH resin is too high, it tends to be susceptible to thermal degradation, and if it is too low, it tends to have reduced long-run performance.
[0027] The EVOH resin may be a mixture of EVOH resins with different ethylene structural unit content, degree of saponification, degree of polymerization, copolymer components, etc.
[0028] The concentration of EVOH resin in the EVOH resin solution is less than 10% by mass, preferably 8% by mass or less, and more preferably 6% by mass or less. The lower limit is 0.1% by mass or more. When the EVOH concentration is within the above range, the film-forming properties tend to be excellent, as does the gas barrier properties.
[0029] [Water-alcohol mixed solvent] The aforementioned water-alcohol mixed solvent refers to a mixed solvent of water and alcohol. The aforementioned alcohol is not particularly limited as long as it can dissolve the EVOH resin, but examples include monohydric alcohols such as methyl alcohol, ethyl alcohol, propyl alcohol, and butyl alcohol; dihydric alcohols such as ethylene glycol and propylene glycol; trihydric alcohols such as glycerin; and phenols such as phenol and cresol. These can be used individually or in combination of two or more. Among these, n-propyl alcohol, isopropyl alcohol, and methyl alcohol are preferred, with n-propyl alcohol being more preferred.
[0030] The alcohol concentration (n) in the aforementioned water-alcohol mixed solvent is preferably more than 50% by mass and 90% by mass or less, more preferably 52% by mass or more and 85% by mass or less, and even more preferably 54% by mass or more and 82% by mass or less. When the alcohol concentration (n) is within the above range, the EVOH resin solution becomes alcohol-rich, and even if the alcohol with a lower boiling point preferentially volatilizes when sprayed during spray coating, the solution composition remains within a suitable range for EVOH resin, which tends to suppress resin precipitation and also tends to suppress whitening of the EVOH resin film.
[0031] Furthermore, the water / alcohol mixing ratio (mass ratio) of the water-alcohol mixed solvent is appropriately selected depending on the type of alcohol and the type of EVOH resin to be dissolved, but it is preferably 2 / 8 to 3 / 7.
[0032] The content of the water-alcohol mixed solvent is preferably 90% by mass or more, more preferably 92% by mass or more, and even more preferably 95% by mass or more, relative to the EVOH resin solution. The upper limit is usually 99% by mass. When the content ratio falls within the above range, it tends to exhibit excellent film-forming properties.
[0033] [Other compounding agents] Furthermore, it is preferable to incorporate boron compounds into the EVOH resin solution to improve its stability. Examples of such boron compounds include boric acid or its metal salts, calcium borate, cobalt borate, zinc borate (zinc tetraborate, zinc metaborate, etc.), aluminum potassium borate, ammonium borate (ammonium metaborate, ammonium tetraborate, ammonium pentaborate, ammonium octaborate, etc.), cadmium borate (cadmium orthoborate, cadmium tetraborate, etc.), and potassium borate (potassium metaborate). (Potassium tetraborate, potassium pentaborate, potassium hexaborate, potassium octaborate, etc.), silver borate (silver metaborate, silver tetraborate, etc.), copper borate (copper dicorate, copper metaborate, copper tetraborate, etc.), sodium borate (sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, sodium octaborate, etc.), lead borate (lead metaborate, lead hexaborate, etc.), nickel borate (ortho) Nickel borate, nickel diborate, nickel tetraborate, nickel octaborate, etc.), barium borate (barium orthoborate, barium metaborate, barium diborate, barium tetraborate, etc.), bismuth borate, magnesium borate (magnesium orthoborate, magnesium diborate, magnesium metaborate, trimagnesium tetraborate, pentamagnesium tetraborate, etc.), manganese borate (manganese borate I, magnesium metaborate) Examples of suitable materials include manganese tetraborate (such as manganese tetraborate), lithium borate (such as lithium metaborate, lithium tetraborate, and lithium pentaborate), as well as borate minerals such as borax, carnite, inyoite, kotoite, syuanite, and zyberite. Preferably, boric acid and sodium borate (such as sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, and sodium octaborate) are used.
[0034] The content of such compounding agents is usually 30% by mass or less, preferably 20% by mass or less, and particularly preferably 10% by mass or less, of the EVOH resin solution, with the lower limit usually being 0% by mass.
[0035] [Method for producing EVOH resin solution] The mixing of the EVOH resin and the water-alcohol mixed solvent can be carried out by a known method. For example, the EVOH resin may be mixed into the water-alcohol mixed solvent, and the mixture may be mixed and stirred under heating at 50 to 100°C using a stirrer equipped with stirring blades such as turbine-type or ribbon-type stirring blades at a rotation speed of 10 to 1000 rpm.
[0036] The EVOH resin solution obtained by the above production method satisfies the following formula (1). ·Solution composition: 26+X<n<0.5X+65···(1) [X: Content ratio (mol%) of ethylene structural units in the ethylene-vinyl alcohol copolymer, n: Alcohol concentration (mass%) in the water-alcohol mixed solvent]
[0037] Further, the viscosity of the EVOH resin solution measured with a Brookfield viscometer at a solution temperature of 20°C is preferably 200 mPa·s or less, more preferably 150 mPa·s or less, and even more preferably 100 mPa·s or less. The lower limit is usually 50 mPa·s. When such viscosity falls within the above range, the solution tends to be easily atomized during spraying in spray coating, and is less likely to drip from the nozzle of the sprayer. Such viscosity refers to a value measured using a Brookfield viscometer in accordance with JIS Z8803:2011.
[0038] <Method for producing EVOH resin film> This production method relates to a method for producing an EVOH resin film, which comprises spray-coating the EVOH resin solution. More specifically, the EVOH resin solution can be applied to an object to be coated by spray coating using a sprayer or the like, and then dried, whereby the EVOH resin film can be produced.
[0039] In this manufacturing method, the temperature of the EVOH resin solution during spray coating can be at room temperature (20°C), preferably less than 50°C, more preferably 45°C or lower, more preferably 40°C or lower, and even more preferably 35°C or lower. The lower limit is 10°C. Normally, EVOH resin solutions are stored at room temperature (around 20°C), so they need to be heated to over 50°C for spray coating. However, this manufacturing method allows spray coating without prior heating, resulting in lower equipment investment costs and a tendency towards superior productivity.
[0040] Methods of application using spray coating include air spraying, airless spraying, electrostatic spraying, and HVLP spraying. Among these, air spraying is preferred because it provides a smooth finish without unevenness and requires less equipment investment.
[0041] The droplet size of the EVOH resin solution discharged from the nozzle is preferably 0.1 μm to 100 μm, the discharge volume is preferably 0.2 to 10 g / min, the coating speed is preferably 30 to 300 mm / second, and the atomizing air pressure in the case of the air spray method is preferably 0.03 to 0.2 MPa.
[0042] The distance between the nozzle and the object to be coated is preferably, for example, 20 to 300 mm. The distance between the nozzle and the object to be coated refers to the distance from the nozzle to the surface of the object to be coated.
[0043] The drying temperature of the EVOH resin solution can be, for example, 70°C or higher and 150°C or lower, and the drying time can be, for example, 1 minute or more and 600 minutes or less.
[0044] The thickness of the EVOH resin film is not particularly limited, but is preferably in the range of 5 to 600 μm, more preferably in the range of 10 to 500 μm, and even more preferably in the range of 12 to 400 μm. When the thickness of the EVOH resin film is above the lower limit, it tends to be easier to manufacture, and when it is below the upper limit, it tends to be advantageous in terms of cost.
[0045] The material to be coated is not particularly limited, but may include linear low-density polyethylene, low-density polyethylene, medium-density polyethylene, high-density polyethylene, ethylene-vinyl acetate copolymer, ionomer, ethylene-propylene copolymer, ethylene-acrylic acid ester copolymer, polypropylene, propylene-α-olefin (α-olefin with 4 to 20 carbon atoms) copolymer, polybutene, polypentene, and other olefins, either alone or in copolymer form, or these olefins, either alone or in copolymer form, graft-modified with unsaturated carboxylic acids or their esters, etc., in the broad sense of polyolefin-based materials. Examples of suitable substrates include stretched or unstretched films, sheets, hollow containers, paper, cellophane, cellulose, cellulose acetate, natural rubber, synthetic rubber, metal foil, woven fabric, nonwoven fabric, metal cotton strips, and wood surfaces, all made from various plastics such as fats, polystyrene resins, polyesters, polyamides, copolymerized polyamides, polyvinyl chloride, polyvinylidene chloride, acrylic resins, vinyl ester resins, polyester elastomers, polyurethane elastomers, chlorinated polyethylene, chlorinated polypropylene, and EVOH resins. The appropriate film thickness for such substrates is approximately 10 to 1000 μm. [Examples]
[0046] The present invention will be described in more detail below with reference to examples, but the present invention is not limited to the following examples unless it exceeds the gist of the invention. In the examples, "parts" and "%" refer to mass.
[0047] <Example 1> An EVOH resin containing 29 mol% ethylene structural units was added to a mixed solvent of water and n-propyl alcohol (water / alcohol = 4 / 6 (mass ratio)), and refluxed using a hot stirrer (80°C) to obtain an EVOH resin solution (EVOH resin concentration 5%). The obtained EVOH resin solution was left to stand in a constant temperature and humidity chamber and cooled to 20°C (room temperature). The prepared EVOH resin solution was spray-coated onto a 12 μm thick polyethylene terephthalate (PET) film cut to A4 size using a sprayer (manufactured by Asahi Paint Co., Ltd.). The PET film was then placed in an 80°C oven and dried for 5 minutes to form a 2 μm thick EVOH resin film on the PET substrate.
[0048] <Example 2> An EVOH resin film was fabricated in the same manner as in Example 1, except that the EVOH resin concentration was changed to 3%.
[0049] <Example 3> In Example 1, an EVOH resin film was fabricated in the same manner as in Example 1, except that the temperature of the EVOH resin solution was set to 30°C.
[0050] <Example 4> An EVOH resin film was fabricated in the same manner as in Example 1, except that the composition of the mixed solvent of water and n-propyl alcohol was changed to water / alcohol = 3 / 7 (mass ratio).
[0051] <Example 5> An EVOH resin film was fabricated in the same manner as in Example 1, except that the EVOH resin was changed to an EVOH resin with an ethylene structural unit content of 32 mol%.
[0052] <Comparative Example 1> An EVOH resin film was fabricated in the same manner as in Example 1, except that the composition of the mixed solvent of water and n-propyl alcohol was changed to water / alcohol = 5 / 5 (mass ratio).
[0053] <Comparative Example 2> In Example 2, an EVOH resin film was fabricated in the same manner as in Example 2, except that the composition of the mixed solvent of water and n-propyl alcohol was changed to water / alcohol = 5 / 5 (mass ratio).
[0054] <Comparative Example 3> In Example 5, an EVOH resin film was fabricated in the same manner as in Example 5, except that the composition of the mixed solvent of water and n-propyl alcohol was changed to water / alcohol = 5 / 5 (mass ratio).
[0055] <Comparative Example 4> In Example 1, an EVOH resin film was fabricated in the same manner as in Example 1, except that the temperature of the EVOH resin solution was set to 50°C.
[0056] <Comparative Example 5> An EVOH resin film was fabricated in the same manner as in Example 1, except that the concentration of the EVOH resin was changed to 15%.
[0057] <Comparative Example 6> In Example 1, instead of spray coating, an EVOH resin solution was applied to a corona-treated 12 μm thick polyethylene terephthalate (PET) film using a wire bar #9 (bar coater), and dried at 80°C for 5 minutes to form a 2 μm thick EVOH resin film on the PET film.
[0058] <Comparative Example 7> In Example 1, instead of spray coating, a simple gravure printing plate with a groove depth of 120 μm and a screen ruling of 100 was used to transfer the EVOH resin solution onto a polyethylene terephthalate (PET) film (gravure coater). After coating, the film was dried at 80°C for 5 minutes to form a 2 μm thick EVOH resin film on the PET film.
[0059] <Comparative Example 8> In Example 1, instead of spray coating, a polyethylene terephthalate (PET) film was immersed in an EVOH resin solution and the substrate was pulled up at a constant speed to perform coating (dip coating). This was dried at 80°C for 5 minutes to form a 5 μm thick EVOH resin film on the PET film.
[0060] <Comparative Example 9> In Example 1, instead of spray coating, 5 mL of EVOH resin solution was dropped onto a polyethylene terephthalate (PET) film. The solution spread spontaneously due to gravity and surface tension, and was dried at 80°C for 5 minutes to form a 2 μm EVOH resin film on the PET film (cast coating).
[0061] [Presence or absence of membrane whitening] The PET films obtained in Examples 1-5 and Comparative Examples 1-9 were visually observed, and evaluated as follows: "○" for those showing no whitening at all, and "×" for those showing even partial whitening. The results are shown in Table 1 below.
[0062] [Feasibility of atomization] Furthermore, in Examples 1-5 and Comparative Examples 1-5, when spray coating, the prepared EVOH resin solution was evaluated as follows: "○" indicated that it atomized when sprayed with a sprayer, and "×" indicated that it did not atomize (drip was observed from the sprayer nozzle). The results are shown in Table 1 below.
[0063] [Measurement of solution viscosity] The EVOH resin solution was heated to 20°C and measured using a Type B viscometer (TVB-10 digital viscometer, manufactured by Toki Sangyo Co., Ltd.) in accordance with JIS Z8803:2011. The results are shown in Table 1 below.
[0064] [Table 1]
[0065] As shown in Table 1 above, the EVOH resin films of Examples 1 to 5 that satisfy the specific formula showed no whitening and could be atomized. On the other hand, the EVOH resin films of Comparative Examples 1 to 3 that did not satisfy the specific formula, and the EVOH resin film of Comparative Example 4, where the solution temperature was above a specific temperature, exhibited whitening. Furthermore, Comparative Example 5, where the EVOH resin concentration was above a specific amount, could not be atomized and therefore could not be formed into a film. In addition, the EVOH resin films of Comparative Examples 6 to 9, which were formed by methods other than spray coating, exhibited whitening. [Industrial applicability]
[0066] The present invention provides a method for manufacturing EVOH resin films that, when spray-coating an EVOH resin solution, suppresses film whitening and eliminates the need for preheating of the solution. This reduces capital investment and improves productivity. Therefore, it is useful, for example, as a packaging material for various products such as food, medical products, and industrial chemicals, as a protective material for electronic and lighting equipment, or as a composite material laminated with plastic film, paper, or metal foil.
Claims
1. A method for producing an ethylene-vinyl alcohol copolymer film by spray coating with an ethylene-vinyl alcohol copolymer solution, The ethylene-vinyl alcohol copolymer solution comprises an ethylene-vinyl alcohol copolymer and a water-alcohol mixed solvent. The solution composition of the ethylene-vinyl alcohol copolymer solution satisfies the following formula (1): The concentration of the ethylene-vinyl alcohol copolymer in the ethylene-vinyl alcohol copolymer solution is less than 10% by mass. A method for producing an ethylene-vinyl alcohol copolymer film, wherein the solution temperature of the ethylene-vinyl alcohol copolymer solution is less than 50°C. ・Solution composition: 26+X<n<0.5X+65...(1) [X: Percentage of ethylene structural units in ethylene-vinyl alcohol copolymer (mol%), n: Alcohol concentration in water-alcohol mixed solvent (mass%)]
2. The method for producing an ethylene-vinyl alcohol copolymer film according to claim 1, wherein the content of ethylene structural units in the ethylene-vinyl alcohol copolymer is 25 to 44 mol%.
3. The method for producing an ethylene-vinyl alcohol copolymer film according to claim 1 or 2, wherein the viscosity of the ethylene-vinyl alcohol copolymer solution, as measured by a B-type viscometer at a solution temperature of 20°C, is 200 mPa·s or less.
Citation Information
Patent Citations
JP1972048489B