Semiconductor equipment

The semiconductor device with a layered structure and specific fabrication processes addresses mobility and reliability issues, achieving high on-current and low power consumption for high-definition displays.

JP2026182820APending Publication Date: 2026-11-19SEMICON ENERGY LAB CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2026078036
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-02-10
Filing Date
2026-05-07
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing semiconductor devices face challenges in achieving high field-effect mobility, large on-current, small size, short channel length, good electrical characteristics, high-speed operation, low power consumption, and high reliability, particularly in high-definition display devices.

Method used

A semiconductor device with a layered structure comprising a semiconductor layer with multiple metal oxide layers and insulating layers, including silicon and hydrogen, oxygen, and nitrogen, is fabricated using specific deposition and heat treatment processes to enhance film density and crystallization.

Benefits of technology

The solution results in a semiconductor device with high field-effect mobility, large on-current, small size, and low power consumption, enabling high-definition display devices with reduced footprint and improved reliability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182820000001_ABST
    Figure 2026182820000001_ABST
Patent Text Reader

Abstract

The present invention provides a semiconductor device having a transistor with high field-effect mobility. [Solution] A semiconductor device having a semiconductor layer, a first insulating layer, a second insulating layer, and a conductive layer. The semiconductor layer is located on the first insulating layer. The second insulating layer is located on the semiconductor layer. The semiconductor layer has a region that overlaps with the conductive layer via the second insulating layer. The semiconductor layer has a first metal oxide layer and a second metal oxide layer on the first metal oxide layer. The first metal oxide layer and the second metal oxide layer each contain indium and oxygen. The film density of the first metal oxide layer is higher than that of the second metal oxide layer. The first insulating layer contains silicon, oxygen, and hydrogen. The second insulating layer contains silicon and oxygen.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] One aspect of the present invention relates to a semiconductor device and a method for manufacturing the same. Another aspect of the present invention relates to a transistor and a method for manufacturing the same. Another aspect of the present invention relates to a semiconductor device having a transistor.

[0002] It should be noted that one aspect of the present invention is not limited to the above-mentioned technical field. Examples of technical fields of one aspect of the present invention include semiconductor devices, display devices, light-emitting devices, energy storage devices, memory devices, electronic devices, lighting devices, input devices (e.g., touch sensors), input / output devices (e.g., touch panels), methods for driving them, or methods for manufacturing them.

[0003] In this specification, a semiconductor device refers to a device that utilizes semiconductor properties, including circuits containing semiconductor elements (transistors, diodes, photodiodes, etc.), devices having such circuits, etc. It also refers to any device that can function by utilizing semiconductor properties. For example, integrated circuits, chips equipped with integrated circuits, and electronic components with chips housed in packages are examples of semiconductor devices. Furthermore, memory devices, display devices, light-emitting devices, lighting devices, and electronic devices are themselves semiconductor devices, and may each have semiconductor devices. [Background technology]

[0004] In recent years, there has been a growing demand for high-resolution display devices. Devices requiring high-resolution displays include those for virtual reality (VR), augmented reality (AR), substitutional reality (SR), and mixed reality (MR), for which development is actively underway.

[0005] Examples of display devices include display devices having liquid crystal elements and display devices having light-emitting elements (also called light-emitting devices). Examples of light-emitting elements include organic EL (Electro-Luminescence) elements and light-emitting diodes (LEDs). Patent Document 1 discloses a high-definition display device using an organic EL element.

[0006] Technology related to transistors using semiconductor thin films is attracting attention. These transistors are widely applied in electronic devices such as integrated circuits (ICs) and display devices. While silicon-based semiconductor materials are widely known as semiconductor materials applicable to transistors, oxide semiconductors are also attracting attention as other materials.

[0007] Examples of oxide semiconductors applicable to transistors include indium oxide and indium gallium zinc oxide. Non-patent documents 1, 2, and 3 disclose thin-film transistors using indium oxide. [Prior art documents] [Patent Documents]

[0008] [Patent Document 1] International Publication No. 2016 / 038508 [Non-patent literature]

[0009] [Non-Patent Document 1] Y. Magari et al., “High-mobility hydrogenated polycrystalline In2O3(In2O3:H) thin-film transistors”, nature COMMUNICATIONS, 13, 1078 (2022) [Non-Patent Document 2] Dhananjay and CW Chu, “Realization of In2O3 thin film transistors through reactive evaporation process” Appl. Phys. Lett. 91, 132111 (2007). [Non-Patent Document 3] JYLin et al., “First Demonstration of Top-Gate Enhancement-Mode ALD In2O3 FETs With High Thermal Budget of 600℃ for DRAM Applications”, IEEE Electron Device Letters, 45, 10, pp. 1851-1854 (2024) [Non-Patent Document 4] Takashi Koida, "High-Mobility Transparent Conductive Film," National Institute of Advanced Industrial Science and Technology (AIST), AIST Photovoltaic Power Generation Research Results Presentation 2019, Internet<URL:https: / / unit.aist.go.jp / rpd-envene / PV / ja / results / 2019 / oral / T13.pdf> [Overview of the Initiative] [Problems that the invention aims to solve]

[0010] One aspect of the present invention aims to provide a semiconductor device having a transistor with high field-effect mobility. Alternatively, it aims to provide a semiconductor device having a transistor with a large on-current. Alternatively, it aims to provide a semiconductor device having a transistor of a very small size. Alternatively, it aims to provide a semiconductor device having a transistor with a short channel length. Alternatively, it aims to provide a semiconductor device having a transistor with good electrical characteristics. Alternatively, it aims to provide a semiconductor device that operates at high speed. Alternatively, it aims to provide a semiconductor device with a small footprint. Alternatively, it aims to provide a semiconductor device with low wiring resistance. Alternatively, it aims to provide a semiconductor device or display device with low power consumption. Alternatively, it aims to provide a transistor, semiconductor device, or display device with high reliability. Alternatively, it aims to provide a high-definition display device. Alternatively, it aims to provide a method for manufacturing the aforementioned transistor, semiconductor device, or display device. Alternatively, it aims to provide a method for manufacturing a transistor, semiconductor device, or display device with high productivity. Alternatively, it aims to provide a novel transistor, semiconductor device, display device, or method for manufacturing the same.

[0011] Furthermore, the description of these problems does not preclude the existence of other problems. One aspect of the present invention does not necessarily have to solve all of these problems. It is possible to extract other problems from the description in the specification, drawings, and claims. [Means for solving the problem]

[0012] One aspect of the present invention is a semiconductor device having a semiconductor layer, a first insulating layer, a second insulating layer, and a conductive layer. The semiconductor layer is located on the first insulating layer. The second insulating layer is located on the semiconductor layer. The semiconductor layer has a region that overlaps with the conductive layer via the second insulating layer. The semiconductor layer has a first metal oxide layer and a second metal oxide layer on the first metal oxide layer. The first metal oxide layer and the second metal oxide layer each contain indium and oxygen. The film density of the first metal oxide layer is higher than that of the second metal oxide layer. The first insulating layer contains silicon, oxygen, and hydrogen. The second insulating layer contains silicon and oxygen.

[0013] One aspect of the present invention is a semiconductor device having a semiconductor layer, a first insulating layer, a second insulating layer, and a conductive layer. The semiconductor layer is located on the first insulating layer. The second insulating layer is located on the semiconductor layer. The semiconductor layer has a region that overlaps with the conductive layer via the second insulating layer. The semiconductor layer has a first metal oxide layer, a second metal oxide layer on the first metal oxide layer, and a third metal oxide layer on the second metal oxide layer. The first metal oxide layer, the second metal oxide layer, and the third metal oxide layer each contain indium and oxygen. The film density of the first metal oxide layer is higher than that of the second metal oxide layer. The film density of the third metal oxide layer is higher than that of the second metal oxide layer. The first insulating layer contains silicon, oxygen, and hydrogen. The second insulating layer contains silicon and oxygen.

[0014] In the aforementioned semiconductor device, it is preferable to have a third insulating layer. The third insulating layer preferably has a region that overlaps with the semiconductor layer via the first insulating layer. The third insulating layer preferably contains silicon and nitrogen.

[0015] In the aforementioned semiconductor device, the third insulating layer preferably contains hydrogen. The third insulating layer preferably has a region with a higher hydrogen concentration than the first insulating layer.

[0016] One aspect of the present invention is a semiconductor device having a semiconductor layer, a first insulating layer, a second insulating layer, a third insulating layer, a fourth insulating layer, and a conductive layer. The second insulating layer is located on the first insulating layer. The semiconductor layer is located on the second insulating layer. The third insulating layer is located on the semiconductor layer. The semiconductor layer has a region that overlaps with the conductive layer via the third insulating layer. The fourth insulating layer is located on the semiconductor layer, the third insulating layer, and the conductive layer. The semiconductor layer has a first metal oxide layer, a second metal oxide layer on the first metal oxide layer, and a third metal oxide layer on the second metal oxide layer. The first metal oxide layer, the second metal oxide layer, and the third metal oxide layer each contain indium and oxygen. The film density of the first metal oxide layer is higher than that of the second metal oxide layer. The film density of the third metal oxide layer is higher than that of the second metal oxide layer. The second insulating layer comprises silicon, oxygen, and hydrogen. The third insulating layer comprises silicon and oxygen. The first and fourth insulating layers each comprise silicon and nitrogen.

[0017] In the semiconductor device described above, the semiconductor layer preferably has a first region that overlaps with the conductive layer via a second insulating layer, and a pair of second regions that sandwich the first region. The fourth insulating layer preferably has a region that is in contact with the second region.

[0018] In the semiconductor device described above, the first insulating layer preferably contains hydrogen. The first insulating layer preferably has a region with a higher hydrogen concentration than the second insulating layer.

[0019] One aspect of the present invention is a method for manufacturing a semiconductor device, comprising depositing a first insulating layer, depositing a semiconductor layer on the first insulating layer, and performing a first heat treatment on the first insulating layer and the semiconductor layer. The first insulating layer is deposited using a gas containing silicon, oxygen, and hydrogen. The semiconductor layer is deposited in the order of a first metal oxide layer and a second metal oxide layer. The first metal oxide layer and the second metal oxide layer are each deposited by sputtering. The deposition of the first metal oxide layer and the second metal oxide layer is performed using an indium oxide target, and oxygen and argon are used as the deposition gas, respectively. The power density during deposition of the first metal oxide layer is higher than the power density during deposition of the second metal oxide layer. The temperature of the first heat treatment is 150°C or higher and 670°C or lower.

[0020] In the aforementioned method for manufacturing a semiconductor device, it is preferable not to use a gas containing hydrogen as the film-forming gas for depositing the first metal oxide layer and the second metal oxide layer.

[0021] In the aforementioned method for manufacturing a semiconductor device, it is preferable that the film-forming gas used in the deposition of the first metal oxide layer and the second metal oxide layer consists of oxygen and argon.

[0022] In the aforementioned method for manufacturing a semiconductor device, it is preferable not to heat the first insulating layer during the deposition of the first metal oxide layer and the second metal oxide layer.

[0023] In the aforementioned method for manufacturing a semiconductor device, it is preferable to crystallize the semiconductor layer by the first heat treatment.

[0024] In the aforementioned method for fabricating a semiconductor device, it is preferable that the pressure used for depositing the first metal oxide layer is lower than the pressure used for depositing the second metal oxide layer.

[0025] In the aforementioned method for manufacturing a semiconductor device, it is preferable to deposit a second insulating layer before depositing a first insulating layer. The second insulating layer is preferably deposited using a gas containing silicon and nitrogen.

[0026] In the aforementioned method for manufacturing a semiconductor device, it is preferable to deposit a third insulating layer on the semiconductor layer after the first heat treatment. It is preferable to perform the second heat treatment on the first insulating layer, the second insulating layer, the third insulating layer, and the semiconductor layer. It is preferable that the third insulating layer is deposited using a gas containing silicon, oxygen, and hydrogen. The temperature of the second heat treatment is preferably 300°C or higher and 500°C or lower.

[0027] In the aforementioned method for manufacturing a semiconductor device, it is preferable to form a conductive layer on the third insulating layer after the second heat treatment. It is also preferable to form a fourth insulating layer on the semiconductor layer, the third insulating layer, and the conductive layer. The fourth insulating layer is preferably formed using a gas containing silicon and nitrogen.

[0028] In the aforementioned method for fabricating a semiconductor device, the semiconductor layer is preferably formed in the order of a first metal oxide layer, a second metal oxide layer, and a third metal oxide layer. The third metal oxide layer is preferably formed by sputtering. For the formation of the third metal oxide layer, an indium oxide target is preferably used, and oxygen and argon are preferably used as the deposition gas. The power density during the formation of the third metal oxide layer is preferably higher than the power density during the formation of the second metal oxide layer.

[0029] In the aforementioned method for fabricating a semiconductor device, it is preferable that the pressure used for depositing the third metal oxide layer is lower than the pressure used for depositing the second metal oxide layer.

[0030] One aspect of the present invention is a semiconductor device having a semiconductor layer, a first insulating layer, a second insulating layer, and a conductive layer. The semiconductor layer has a region in contact with the upper surface of the first insulating layer. The second insulating layer is located on the semiconductor layer. The semiconductor layer has a region that overlaps with the conductive layer via the second insulating layer. The semiconductor layer contains indium and oxygen. The first insulating layer contains silicon, oxygen, and hydrogen. In a temperature-controlled desorption gas analysis method in which the surface temperature of the first insulating layer is in the range of 50°C to 350°C, the amount of hydrogen molecules desorbed is 1.2 × 10⁻¹⁴. 13 molecular / cm² 2 The above 8.0 x 10 13 molecular / cm² 2 The following applies:

[0031] In the semiconductor device described above, the semiconductor layer preferably comprises a first metal oxide layer and a second metal oxide layer on the first metal oxide layer. The film density of the first metal oxide layer is preferably higher than that of the second metal oxide layer.

[0032] In the semiconductor device described above, it is preferable that the semiconductor layer comprises a first metal oxide layer, a second metal oxide layer on the first metal oxide layer, and a third metal oxide layer on the second metal oxide layer. It is preferable that the film density of the first metal oxide layer is higher than that of the second metal oxide layer. It is preferable that the film density of the third metal oxide layer is higher than that of the second metal oxide layer.

[0033] One aspect of the present invention is a method for manufacturing a semiconductor device, comprising forming a first insulating layer, forming a semiconductor layer on the first insulating layer, and performing a first heat treatment on the first insulating layer and the semiconductor layer. The first insulating layer is formed using a gas containing silicon, oxygen, and hydrogen. In a temperature-controlled desorption gas analysis method in which the surface temperature of the first insulating layer is in the range of 50°C to 350°C, the amount of hydrogen molecules desorbed is 1.2 × 10⁻¹⁶. 13 molecular / cm² 2 The above 8.0 x 10 13 molecular / cm² 2The following applies: The semiconductor layer is deposited by sputtering. An indium oxide target is used for deposition of the semiconductor layer, and oxygen and argon are used as deposition gases. The temperature of the first heat treatment is between 150°C and 670°C.

[0034] In the aforementioned method for manufacturing semiconductor devices, it is preferable not to use a gas containing hydrogen as the film-forming gas for depositing the semiconductor layer.

[0035] In the aforementioned method for fabricating a semiconductor device, the deposition gas used in forming the semiconductor layer is preferably composed of oxygen and argon.

[0036] In the aforementioned method for manufacturing a semiconductor device, it is preferable to crystallize the semiconductor layer by the first heat treatment.

[0037] In the aforementioned method for manufacturing a semiconductor device, it is preferable to perform a second heat treatment on the first insulating layer before forming the semiconductor layer. The temperature of the second heat treatment is preferably between 150°C and 670°C.

[0038] In the aforementioned method for manufacturing a semiconductor device, it is preferable that the semiconductor layer is formed in the order of a first metal oxide layer and a second metal oxide layer. It is preferable that the power density during the formation of the first metal oxide layer is higher than the power density during the formation of the second metal oxide layer.

[0039] In the aforementioned method for fabricating a semiconductor device, it is preferable that the pressure used for depositing the first metal oxide layer is lower than the pressure used for depositing the second metal oxide layer.

[0040] In the aforementioned method for manufacturing a semiconductor device, it is preferable that the semiconductor layer is formed in the order of a first metal oxide layer, a second metal oxide layer, and a third metal oxide layer. It is preferable that the power density during the formation of the third metal oxide layer is higher than the power density during the formation of the second metal oxide layer.

[0041] In the aforementioned method for fabricating a semiconductor device, it is preferable that the pressure used for depositing the third metal oxide layer is lower than the pressure used for depositing the second metal oxide layer. [Effects of the Invention]

[0042] One aspect of the present invention can provide a semiconductor device having a transistor with high field-effect mobility. Or, a semiconductor device having a transistor with high on-current can be provided. Or, a semiconductor device having a transistor of a very small size can be provided. Or, a semiconductor device having a transistor with a short channel length can be provided. Or, a semiconductor device having a transistor with good electrical characteristics can be provided. Or, a semiconductor device that operates at high speed can be provided. Or, a semiconductor device with a small footprint can be provided. Or, a semiconductor device with low wiring resistance can be provided. Or, a semiconductor device or display device with low power consumption can be provided. Or, a transistor, semiconductor device, or display device with high reliability can be provided. Or, a high-definition display device can be provided. Or, a method for manufacturing the aforementioned transistor, semiconductor device, or display device can be provided. Or, a method for manufacturing a transistor, semiconductor device, or display device with high productivity can be provided. Or, a novel transistor, semiconductor device, display device, or method for manufacturing them can be provided.

[0043] Furthermore, the description of these effects does not preclude the existence of other effects. One aspect of the present invention does not necessarily have to possess all of these effects. Other effects can be extracted from the description, drawings, and claims. [Brief explanation of the drawing]

[0044] [Figure 1] Figure 1(A) is a top view showing an example of a semiconductor device. Figures 1(B) and 1(C) are cross-sectional views showing an example of a semiconductor device. [Figure 2] Figures 2(A) and 2(B) are cross-sectional views showing an example of a semiconductor device. [Figure 3] Figures 3(A) to 3(C) are cross-sectional views showing an example of a semiconductor device. [Figure 4] Figures 4(A) and 4(B) are cross-sectional views showing an example of a semiconductor device. [Figure 5] Figures 5(A) and 5(B) are cross-sectional views showing an example of a semiconductor device. [Figure 6] Figures 6(A) to 6(D) are cross-sectional views showing an example of a semiconductor device. [Figure 7] Figure 7(A) is a top view showing an example of a semiconductor device. Figure 7(B) is a cross-sectional view showing an example of a semiconductor device. [Figure 8] Figure 8(A) is a top view showing an example of a semiconductor device. Figures 8(B) and 8(C) are cross-sectional views showing an example of a semiconductor device. [Figure 9] Figures 9(A) to 9(E) are cross-sectional views showing an example of a method for manufacturing a semiconductor device. [Figure 10] Figures 10(A) to 10(D) are cross-sectional views showing an example of a method for manufacturing a semiconductor device. [Figure 11] Figure 11 is a cross-sectional view showing an example of a semiconductor device manufacturing method. [Figure 12] Figures 12(A) and 12(B) illustrate the carrier concentration dependence of hole mobility. Figure 12(C) is a cross-sectional view illustrating an indium oxide film. [Figure 13] Figure 13(A) is a perspective view showing an example of a display device. Figures 13(B) and 13(C) are circuit diagrams showing an example of a sub-pixel. [Figure 14] Figures 14(A) and 14(B) are circuit diagrams showing an example of a sub-pixel. [Figure 15] Figures 15(A) and 15(B) are cross-sectional views showing an example of a display device. [Figure 16] Figure 16 is a cross-sectional view showing an example of a display device. [Figure 17] Figure 17 is a cross-sectional view showing an example of a display device. [Figure 18] Figures 18(A) to 18(C) are cross-sectional views showing an example of a display device. [Figure 19]Figures 19(A) and 19(B) are cross-sectional views showing an example of a display device. [Figure 20] Figures 20(A) and 20(B) are cross-sectional views showing an example of a display device. [Figure 21] Figure 21 is a cross-sectional view showing an example of a display device. [Figure 22] Figure 22 is a cross-sectional view showing an example of a display device. [Figure 23] Figure 23 is a cross-sectional view showing an example of a display device. [Figure 24] Figures 24(A) to 24(D) show examples of electronic devices. [Figure 25] Figures 25(A) through 25(F) show examples of electronic devices. [Figure 26] Figures 26(A) to 26(G) show examples of electronic devices. [Figure 27] Figures 27(A) and 27(B) show the Id-Vg characteristics of the transistor according to the embodiment. [Figure 28] Figures 28(A) and 28(B) show the Id-Vg characteristics of the transistor according to the embodiment. [Figure 29] Figures 29(A) and 29(B) show the Id-Vg characteristics of the transistor according to the embodiment. [Figure 30] Figure 30 shows the reliability of the transistor according to the embodiment. [Figure 31] Figures 31(A) to 31(C) show the TDS measurement results of the samples according to the examples. [Figure 32] Figures 32(A) and 32(B) show the TDS measurement results of the samples according to the examples. [Figure 33] Figures 33(A) and 33(B) show the Id-Vg characteristics of the transistor according to the embodiment. [Figure 34] Figures 34(A) to 34(D) show the SIMS measurement results of the samples according to the examples. [Figure 35] Figure 35 shows the SIMS measurement results of the sample according to the example. [Modes for carrying out the invention]

[0045] Embodiments will be described in detail with reference to the drawings. However, it will be readily apparent to those skilled in the art that the present invention is not limited to the following description, and that its form and details can be modified in various ways without departing from the spirit and scope of the present invention. Accordingly, the present invention shall not be construed as being limited to the descriptions of the embodiments shown below.

[0046] In the configuration of the invention described below, the same reference numerals are used in common across different drawings for parts that are identical or have similar functions, and repeated explanations are omitted. In addition, when referring to similar functions, the hatching patterns are the same, and reference numerals may not be assigned.

[0047] The position, size, and scope of each component shown in the drawings may not represent the actual position, size, and scope for the sake of ease of understanding. Therefore, the disclosed invention is not necessarily limited to the position, size, and scope disclosed in the drawings.

[0048] In this specification, ordinal numbers such as "first," "second," etc., are used to avoid confusion of components and do not limit the number of components or the order of components (e.g., process order or layering order). Furthermore, even if a term does not have an ordinal number in this specification, an ordinal number may be added in the claims to avoid confusion of components. Even if a term has an ordinal number in this specification, a different ordinal number may be added in the claims. Even if a term has an ordinal number in this specification, an ordinal number may be omitted in the claims.

[0049] In this specification and drawings, when the same reference numeral is used for multiple elements, and especially when it is necessary to distinguish them, an identifying code such as "_1", "[n]", or "[m,n]" may be added to the reference numeral. Conversely, when describing a common matter for multiple elements with identifying codes, or when it is not necessary to distinguish them, the identifying codes may be omitted.

[0050] The words "film" and "layer" can be interchanged depending on the context or situation. For example, the term "conductive layer" can be changed to "conductive film." Or, for example, the term "insulating film" can be changed to "insulating layer."

[0051] A transistor is a type of semiconductor device that can perform functions such as amplifying current or voltage, and switching operations that control conduction or non-conductivity. Transistors as used herein include IGFETs (Insulated Gate Field Effect Transistors) and Thin Film Transistors (TFTs).

[0052] The functions of "source" and "drain" may be reversed when transistors with different polarities are used, or when the direction of current changes during circuit operation. For this reason, in this specification, the terms "source" and "drain" may be used interchangeably. Furthermore, the names of the source and drain of a transistor can be appropriately rephrased as source terminal and drain terminal, or source electrode and drain electrode, depending on the situation.

[0053] The terms "gate" and "back gate" are interchangeable. Therefore, in this specification, the terms "gate" and "back gate" may be used interchangeably. Furthermore, the names of the gate and back gate of a transistor can be appropriately rephrased as gate electrode and back gate electrode, etc., depending on the context.

[0054] In this specification, "connection" includes, for example, "electrical connection." The term "electrical connection" is sometimes used to define the connection relationship of circuit elements as a physical object. Furthermore, "electrical connection" includes both "direct connection" and "indirect connection." "A and B are directly connected" means that A and B are connected without the use of circuit elements (e.g., transistors, switches, etc.; wiring is not considered a circuit element). On the other hand, "A and B are indirectly connected" means that A and B are connected through one or more circuit elements. A and B refer to objects such as elements, circuits, wiring, electrodes, terminals, semiconductor layers, and conductive layers.

[0055] For example, assuming a circuit containing A and B is in operation, if there is a timing during the circuit's operation when electrical signals are exchanged or potential interactions occur between A and B, then it can be defined that "A and B are indirectly connected" as physical objects. Furthermore, even if there is a timing during the circuit's operation when no electrical signals are exchanged or potential interactions occur between A and B, if there is a timing during the circuit's operation when electrical signals are exchanged or potential interactions occur between A and B, then it can be defined that "A and B are indirectly connected."

[0056] An example of a case where "A and B are indirectly connected" is when A and B are connected via the source and drain of one or more transistors. On the other hand, an example of a case where "A and B are not indirectly connected" is when an insulator is interposed in the path from A to B. Specifically, this includes cases where a capacitive element is connected between A and B, or where a transistor gate insulating film is interposed between A and B. Therefore, it cannot be said that "the gate (A) of a transistor and the source or drain (B) of a transistor are indirectly connected."

[0057] Another example of a situation where it cannot be said that "A and B are indirectly connected" is when multiple transistors are connected via source and drain in the path from A to B, and a constant potential V is supplied to the nodes between the transistors from a power supply, GND, etc.

[0058] In this specification, unless otherwise specified, on-current refers to the drain current (also called the conduction state) when the transistor is in the on state. Unless otherwise specified, the on state refers to the state in an n-channel transistor where the voltage between the gate and source (gate voltage, also called Vg or Vgs) is equal to or greater than the threshold voltage (also called Vth), and in a p-channel transistor where it is less than or equal to the threshold voltage.

[0059] In this specification, unless otherwise specified, off-current refers to the source-drain leakage current when the transistor is in the off state (also called the non-conducting state or cutoff state). Unless otherwise specified, the off state refers to the state in an n-channel transistor where the voltage between the gate and source is lower than the threshold voltage, and in a p-channel transistor where it is higher than the threshold voltage.

[0060] In this specification, "parallel" means that two lines are positioned at an angle of -10 degrees or more and 10 degrees or less. Therefore, the case of -5 degrees or more and 5 degrees or less is also included. Furthermore, "approximately parallel" means that two lines are positioned at an angle of -30 degrees or more and 30 degrees or less. Furthermore, "perpendicular" means that two lines are positioned at an angle of 80 degrees or more and 100 degrees or less. Therefore, the case of 85 degrees or more and 95 degrees or less is also included. Furthermore, "approximately perpendicular" means that two lines are positioned at an angle of 60 degrees or more and 120 degrees or less.

[0061] In this specification, the top surface shape of a component refers to the contour shape of the component when viewed from above (also called a plan view). Furthermore, a top view refers to viewing from the direction normal to the surface on which the component is formed, or to the surface of the support (e.g., substrate) on which the component is formed.

[0062] In this specification, "matching or roughly matching top shapes" means that at least a portion of the contours overlap between stacked layers. For example, this includes cases where the upper and lower layers are processed with the same mask pattern, or partially with the same mask pattern. However, strictly speaking, the contours may not overlap, and the upper layer may be located inside the lower layer, or the upper layer may be located outside the lower layer; in this case, it may also be said that the "matching or roughly matching top shapes" apply. Furthermore, when the top shapes match or roughly match, it can also be said that the "edges match or roughly match," or "the edges are aligned or roughly aligned."

[0063] In this specification, a tapered shape refers to a shape in which at least a portion of the side surface of a structure is inclined with respect to the substrate surface or the surface to be formed. The angle formed between the inclined side surface and the substrate surface or the surface to be formed is sometimes referred to as the taper angle.

[0064] In this specification, "step breakage" refers to the phenomenon in which a layer, film, or electrode is divided due to the shape of the surface on which it is formed (e.g., a step).

[0065] In this specification, "island-like" refers to a state in which two or more layers made of the same material and formed in the same process are physically separated. For example, an island-like metal oxide layer refers to a state in which the metal oxide layer and adjacent metal oxide layers are physically separated.

[0066] In this specification, devices fabricated using a metal mask or an FMM (Fine Metal Mask, a high-resolution metal mask) may be referred to as MM (Metal Mask) structured devices. Furthermore, in this specification, devices fabricated without using a metal mask or an FMM may be referred to as MML (Metal Maskless) structured devices.

[0067] In this specification, a structure in which different light-emitting layers are created using light-emitting devices with different emission wavelengths may be referred to as an SBS (Side By Side) structure.

[0068] In this specification, holes or electrons may be referred to as "carriers." For example, in a light-emitting element, a hole injection layer or electron injection layer may be called a "carrier injection layer," a hole transport layer or electron transport layer may be called a "carrier transport layer," and a hole blocking layer or electron blocking layer may be called a "carrier blocking layer." Note that the above-mentioned carrier injection layer, carrier transport layer, and carrier blocking layer may not always be clearly distinguishable. Furthermore, a single layer may combine the functions of two or three of the carrier injection layer, carrier transport layer, and carrier blocking layer.

[0069] In this specification, a light-emitting element has an EL layer between a pair of electrodes (a first electrode and a second electrode). The light-emitting element includes a first electrode, an EL layer on the first electrode, and a second electrode on the EL layer. The EL layer has at least a light-emitting layer. Examples of layers (also called functional layers) that the EL layer has include a light-emitting layer, a carrier injection layer (hole injection layer and electron injection layer), a carrier transport layer (hole transport layer and electron transport layer), and a carrier blocking layer (hole blocking layer and electron blocking layer). In this specification, a photodetector (also called a photodetector device) has at least an active layer that functions as a photoelectric conversion layer between a pair of electrodes. In this specification, one of the first electrode and the second electrode may be referred to as a pixel electrode, and the other as a common electrode.

[0070] In this specification, flexibility refers to the property of an object being flexible and able to bend. It is the property of an object being able to deform in response to an external force applied to it, regardless of whether it is elastic or able to return to its original shape.

[0071] For example, flexible electronic devices, flexible display devices (also called flexible displays, etc.), flexible batteries (also called flexible batteries, etc.), and flexible substrates (also called flexible substrates, etc.) can each be deformed in response to external forces. Flexible electronic devices, flexible display devices, flexible batteries, and flexible substrates can each be used fixed in a deformed state, used after repeated deformation, or used in an undeformed state. The phrase "deforms in response to external forces" above means that it can be deformed by the average adult's hand without requiring excessive force. Flexibleness can be evaluated using testing machines capable of stress-strain measurement (tensile testing machines, compression testing machines, etc.). In stress-strain measurement, the flexibility of an object can be quantified by applying an external force to the object and measuring the strain of the object caused by the resulting stress.

[0072] In this specification, when an object is described as having flexibility, it means that at least a part of the object is flexible. In other words, a flexible object may have parts that are not flexible.

[0073] (Embodiment 1) In this embodiment, a semiconductor device according to one aspect of the present invention will be described with reference to Figures 1(A) to 11. This semiconductor device according to one aspect of the present invention can be suitably used, for example, in one or both of the pixel circuit and / or drive circuit of a display device.

[0074] <Configuration Example 1> Figure 1(A) shows a top view (also called a plan view) of a semiconductor device 10 according to one aspect of the present invention. Figure 1(B) shows a cross-sectional view of the section along the dashed-dotted line A1-A2 in Figure 1(A), and Figure 1(C) shows a cross-sectional view of the section along the dashed-dotted line B1-B2. Note that in Figure 1(A), some components of the semiconductor device 10 (such as the gate insulating layer) are omitted. In subsequent drawings, as in Figure 1(A), some components of the top view of the semiconductor device will also be omitted.

[0075] The semiconductor device 10 has a transistor 100. The transistor 100 has a conductive layer 103 on a substrate 102, an insulating layer 105 on the conductive layer 103, a semiconductor layer 108 on the insulating layer 105, an insulating layer 106 on the semiconductor layer 108, and a conductive layer 104 on the insulating layer 106. The conductive layer 104 has a region that overlaps with the semiconductor layer 108 via the insulating layer 106. In the transistor 100, the conductive layer 104 functions as a first gate electrode, and the insulating layer 106 functions as a first gate insulating layer. The conductive layer 103 has a region that overlaps with the semiconductor layer 108 via the insulating layer 105. In addition, the conductive layer 103 has a region that overlaps with the conductive layer 104 via the insulating layer 105, the semiconductor layer 108, and the insulating layer 106. In the transistor 100, the conductive layer 103 functions as a second gate electrode, and the insulating layer 105 functions as a second gate insulating layer. Furthermore, a configuration without the conductive layer 103 is also possible.

[0076] The semiconductor layer 108 has a region 108i that overlaps with the conductive layer 104 via the insulating layer 106, and a pair of regions (region 108P and region 108Q) that sandwich region 108i. Regions 108P and 108Q do not overlap with the conductive layer 104. In the transistor 100, region 108i functions as a channel formation region, region 108P functions as either a source region or a drain region, and region 108Q functions as the other source region or drain region.

[0077] In the semiconductor layer 108, the length of the region located between the source region and the drain region and overlapping with the conductive layer 104 via the insulating layer 106 becomes the channel length of the transistor 100. Furthermore, the width of the region where the semiconductor layer 108 and the conductive layer 104 overlap in a direction perpendicular to the channel length direction becomes the channel width of the transistor 100.

[0078] Furthermore, in the semiconductor layer 108, the region overlapping with at least one of the conductive layer 104 and the conductive layer 103 functions as a channel-forming region. For the sake of simplicity, the region of the semiconductor layer 108 that overlaps with the conductive layer 104 is sometimes referred to as the channel-forming region, but a region that does not overlap with the conductive layer 104 but overlaps with the conductive layer 103 can also function as a channel-forming region.

[0079] Transistor 100 has gate electrodes (a first gate electrode and a second gate electrode) on both sides of the channel formation region, and can be described as a dual-gate transistor. Note that one of the first and second gate electrodes may be referred to as the front gate electrode (or simply as the gate electrode), and the other as the back gate electrode. Furthermore, one of the first and second gate insulating layers may be referred to as the front gate insulating layer (or simply as the gate insulating layer), and the other as the back gate insulating layer.

[0080] Preferably, the conductive layer 103 has a region that protrudes from the edge of the conductive layer 104. This enhances the effect (also called the electric field shielding effect) of the conductive layer 103 shielding electric fields generated outside the transistor and making it difficult for externally generated electric fields to act on the channel formation region.

[0081] By providing a back gate electrode, the potential on the back gate electrode side (also called the back channel side) of semiconductor layer 108 is fixed, which can improve the saturation in the Id-Vd characteristics. Furthermore, by fixing the potential on the back channel side of semiconductor layer 108, the threshold voltage shift can be suppressed. As a result, the drain current (hereinafter also referred to as the cutoff current) that flows when the gate voltage (Vg) is 0V can be reduced, making it possible to create a normally-off transistor. Therefore, a semiconductor device with low power consumption can be created. In the following, conductive layer 104 may be described as the gate electrode and conductive layer 103 as the back gate electrode.

[0082] The semiconductor layer 108 preferably has a metal oxide (also called an oxide semiconductor) that exhibits semiconductor properties. Examples of metal oxides include indium oxide, gallium oxide, and zinc oxide. The band gap of the metal oxide is preferably 2.0 eV or more, and more preferably 2.5 eV or more. Transistors using oxide semiconductors (hereinafter also referred to as OS transistors) have extremely high field-effect mobility compared to transistors using amorphous silicon. Furthermore, OS transistors have a remarkably low off-current, and can retain the charge stored in a capacitor connected in series with the transistor for a long period of time. In addition, the power consumption of the semiconductor device can be reduced by applying an OS transistor. When an oxide semiconductor is used for the semiconductor layer, the semiconductor layer can be called an oxide semiconductor layer or a metal oxide layer.

[0083] The metal oxide preferably contains at least indium. Furthermore, a high indium content in the metal oxide is preferable. By using a metal oxide with a high indium content in the semiconductor layer, a transistor with a large on-current can be obtained. Therefore, a high-speed semiconductor device can be produced. When a semiconductor device according to one aspect of the present invention is applied to a display device, a high-speed, high-resolution display device can be produced. Also, because transistors using metal oxides with a high indium content have high field-effect mobility, a large on-current can be obtained even with a small channel width. Therefore, the area occupied by the transistor can be reduced, and thus the area occupied by the semiconductor device can be reduced. When a semiconductor device according to one aspect of the present invention is applied to the pixel circuit of a display device, the area occupied by the pixel circuit can be reduced, resulting in a high-definition display device. Furthermore, when a semiconductor device according to one aspect of the present invention is applied to the drive circuit of a display device (for example, one or both of the gate line drive circuit and the source line drive circuit), the area occupied by the drive circuit can be reduced, resulting in a narrow-bezel display device.

[0084] In this specification, the ratio of the number of indium atoms to the sum of the total number of atoms of all contained metal elements may be referred to as the indium content. The same applies to other metal elements.

[0085] The semiconductor layer 108 preferably contains indium and oxygen. For example, indium oxide (also written as IO) can be suitably used for the semiconductor layer 108.

[0086] The crystallinity of the semiconductor material used in the semiconductor layer 108 is not particularly limited, and any amorphous semiconductor, single-crystal semiconductor, or semiconductor having crystallinity other than single crystal (microcrystalline semiconductor, polycrystalline semiconductor, or semiconductor having a crystalline region in part) can be used.

[0087] The semiconductor layer 108 is preferably crystalline. Using a crystalline oxide semiconductor for the semiconductor layer 108 is preferable because it suppresses the degradation of transistor characteristics. The semiconductor layer 108 is preferably highly crystalline, and preferably polycrystalline or monocrystalline. For example, it is preferable to use a polycrystalline indium oxide film as the semiconductor layer 108, and more preferably a monocrystalline indium oxide film. Note that indium oxide having crystal grains may be referred to as crystalline indium oxide (crystal IO) or crystalline indium oxide (crystalline IO). In addition, the crystal structure of In2O3 is typically cubic (bixbite type).

[0088] Single-crystal films are particularly preferred because they do not have grain boundaries, thus suppressing carrier scattering at grain boundaries and enabling transistors with high field-effect mobility. Compared to microcrystalline and amorphous films, polycrystalline films can reduce carrier scattering and enable transistors with high field-effect mobility. When a polycrystalline film is used for semiconductor layer 108, it is preferable that the grain size of the crystal grains contained in semiconductor layer 108 (hereinafter also referred to as grain size) is large. By using a polycrystalline film with a large grain size, the number of grain boundaries located in the channel formation region can be reduced, and the length of the grain boundaries located in the channel formation region can be shortened, thus enabling transistors with high field-effect mobility. Furthermore, it is preferable that there are few grain boundaries in the channel formation region that intersect with the direction in which the drain current flows (also known as the channel length direction). Note that even with a polycrystalline film, if there are no grain boundaries located in the channel formation region, the same effects as a single-crystal film can be achieved.

[0089] When a non-single-crystal (e.g., polycrystalline) film is used as the semiconductor layer 108, it is preferable that the barrier height at the grain boundaries is low. A low barrier height at the grain boundaries reduces the effect of grain boundary scattering, thus enabling a transistor with high field-effect mobility. Generally, the barrier height at the grain boundaries of low-temperature polysilicon (LTPS) is 60 meV to 80 meV. When a polycrystalline metal oxide is used for the semiconductor layer 108, it is preferable that the barrier height at the grain boundaries is lower than that of LTPS. For example, the barrier height at the grain boundaries of a metal oxide is preferably greater than 0 meV and less than 60 meV, more preferably greater than 0 meV and 55 meV or less, and even more preferably greater than 0 meV and 50 meV or less. Note that the barrier height at the grain boundaries of a metal oxide is not limited to the above range. Also, transistors using silicon in the channel formation region are sometimes referred to as Si transistors, and transistors using LTPS are sometimes referred to as LTPS transistors.

[0090] For example, Kelvin Probe Force Microscopy (KFM) can be used to measure the barrier height at grain boundaries. KFM is a type of scanning probe microscopy (SPM) measurement mode in which the potential distribution on the sample surface can be evaluated by scanning the sample surface with a conductive probe and detecting the electrostatic force between the probe and the sample surface.

[0091] Due to the low barrier height at the grain boundaries of metal oxides, OS transistors have high field-effect mobility and can operate at high speeds. Furthermore, OS transistors have high saturation (also known as high constant current) and low electrical hysteresis. Therefore, OS transistors can be suitably used as both selector and drive transistors in pixel circuits. By using OS transistors with high saturation and high current controllability as drive transistors, a display device with high display quality can be created. Additionally, using OS transistors with low hysteresis can further enhance display quality.

[0092] In this specification, the term "high saturation" may be used to describe a transistor's Id-Vd characteristics where the current change in the saturation region is small.

[0093] The crystallinity of semiconductor layer 108 can be analyzed, for example, by X-ray diffraction (XRD), transmission electron microscopy (TEM), or electron diffraction (ED). Alternatively, a combination of these methods can be used for analysis.

[0094] It is preferable that the insulating layer 106 and the insulating layer 105 each have one or more inorganic insulating layers. Examples of materials that can be used for the inorganic insulating layer include oxides, nitrides, oxidized nitrides, and nitride oxides. Examples of oxides include silicon oxide, aluminum oxide, magnesium oxide, gallium oxide, germanium oxide, yttrium oxide, zirconium oxide, lanthanum oxide, neodymium oxide, hafnium oxide, tantalum oxide, cerium oxide, zinc gallium oxide, and hafnium aluminate. Examples of nitrides include silicon nitride and aluminum nitride. Examples of oxidized nitrides include silicon oxidized nitride, aluminum oxidized nitride, gallium oxidized nitride, yttrium oxidized nitride, and hafnium oxidized nitride. Examples of nitride oxides include silicon nitride and aluminum nitride.

[0095] In this specification, the term "oxidogenic nitride" refers to a material whose composition contains more oxygen than nitrogen. The term "nitride oxide" refers to a material whose composition contains more nitrogen than oxygen.

[0096] The insulating layer 105 and the insulating layer 106 each have a region in contact with the semiconductor layer 108. When a metal oxide is used for the semiconductor layer 108, it is preferable that at least a portion of the region of the insulating layer 106 in contact with the semiconductor layer 108 contains oxygen in order to improve the interfacial properties between the semiconductor layer 108 and the insulating layer 106. Specifically, it is preferable that the region of the insulating layer 106 in contact with the channel-forming region contains oxygen. One or more oxides and oxidized nitrides can be suitably used in the region of the insulating layer 106 in contact with the channel-forming region. The same applies to the insulating layer 105. For example, it is preferable that the insulating layer 106 and the insulating layer 105 each contain silicon and oxygen, respectively. Silicon oxide or silicon oxidized nitride can be suitably used for the insulating layer 106 and the insulating layer 105, respectively.

[0097] The insulating layer 106 and insulating layer 105 can be deposited using sputtering, atomic layer deposition (ALD), or chemical vapor deposition (CVD), respectively. CVD methods include plasma enhanced chemical vapor deposition (PECVD) and thermal CVD. One type of thermal CVD is metal-organic chemical vapor deposition (MOCVD). Plasma CVD is preferably used for depositing the insulating layer 106 and insulating layer 105.

[0098] The insulating layer 105, which is the layer to be formed on the semiconductor layer 108, preferably contains hydrogen. The insulating layer 105 preferably contains, for example, silicon, oxygen, and hydrogen. The insulating layer 105 can preferably be silicon oxynitride containing hydrogen, or silicon oxide containing hydrogen. The insulating layer 105 is preferably formed using a method that uses a gas containing the element hydrogen as the film-forming gas. This allows for the formation of an insulating layer 105 containing hydrogen.

[0099] When using plasma CVD, a depositing gas containing silicon and an oxidizing gas can be used as the deposition gas for silicon oxidizide films and silicon oxide films. Examples of depositing gases containing silicon include silane (SiH4), disilane (Si2H6), trisilane (Si3H8), and TEOS (Tetraethoxysilane, Si(OC2H5)4). These depositing gases contain hydrogen along with silicon, making them suitable for use as the deposition gas for the insulating layer 105. As an oxidizing gas, a gas containing oxygen can be used. Examples of oxidizing gases include oxygen (O2), ozone (O3), nitrous oxide (N2O), nitric oxide (NO), and nitrogen dioxide (NO2). When depositing a silicon oxidizide film containing hydrogen, a deposition gas containing silicon, oxygen, nitrogen, and hydrogen can be used. Typically, SiH4 and N2O can be suitably used as the film-forming gas for a hydrogen-containing silicon oxidizide film. When using SiH4, using N2O as the oxidizing gas is preferable because it reduces the amount of particles compared to using O2. Furthermore, when forming a hydrogen-containing silicon oxide film, a film-forming gas containing silicon, oxygen, and hydrogen elements can be used. Typically, TEOS and O2 can be suitably used as the film-forming gas for a hydrogen-containing silicon oxide film. The type of film-forming gas for the insulating layer 105 is not particularly limited.

[0100] A semiconductor layer 108 can be formed by depositing a metal oxide film over the insulating layer 105 and processing the metal oxide film into an island shape. The metal oxide film can be deposited by a sputtering method, an atomic layer deposition (ALD) method, or a chemical vapor deposition (CVD) method. Note that in the case where the metal oxide film is deposited by a sputtering method, the composition of the metal oxide film after deposition may differ from the composition of a sputtering target. In particular, the content rate of zinc in the metal oxide film after deposition may decrease to approximately 50% of the content rate in the sputtering target. Similarly for other elements, the content rate in the metal oxide film after deposition may differ from the content rate in the sputtering target.

[0101] Heat treatment is preferably performed before the metal oxide film is processed into an island shape or after the metal oxide film is processed into an island shape. By the heat treatment, the crystallinity of the semiconductor layer 108 can be increased and defects can be reduced. In addition, impurities contained in the semiconductor layer 108 or adsorbed on the surface thereof can be removed by the heat treatment.

[0102] The crystallinity of the metal oxide film after deposition is preferably low, and particularly preferably amorphous. By performing heat treatment on the metal oxide film with low crystallinity, the metal oxide film can be crystallized to increase its crystallinity. In addition, the grain size of crystal grains contained in the semiconductor layer 108 can be increased. For example, when the metal oxide film contains hydrogen, generation of crystal nuclei and crystal growth are suppressed, whereby the metal oxide film with low crystallinity can be deposited.

[0103] Here, when the hydrogen concentration of the metal oxide film at the stage after deposition is too high, the hydrogen concentration in the semiconductor layer 108 is increased, which may cause oxygen vacancies (V O ) in the channel formation region to increase. In addition, a defect in which hydrogen enters an oxygen vacancy (hereinafter referred to as V OH (also written as H) can function as a donor and generate carrier electrons. This can cause a shift in the transistor's threshold voltage. It can also reduce the reliability of the transistor. This is especially true in transistors with short channel lengths, where oxygen deficiencies and V in the channel formation region can be problematic. O The effect of H on the electrical characteristics is greater, and it is more likely to become normally-on. Also, as mentioned above, by using a metal oxide with a high indium content in the semiconductor layer 108, it is possible to create a transistor with high field-effect mobility. However, metal oxides with a high indium content are prone to oxygen vacancies, and oxygen vacancies and V in the semiconductor layer 108 and V O There are cases where the amount of H becomes excessive.

[0104] By using a gas containing hydrogen (e.g., H2) as the deposition gas for metal oxide films, a metal oxide film containing hydrogen can be formed. In this case, it is preferable to reduce the flow rate of the gas containing hydrogen. However, even if the flow rate of the gas containing hydrogen is reduced, the hydrogen concentration in the metal oxide film will increase, resulting in oxygen vacancies and V in the semiconductor layer 108. O In some cases, the amount of H may become excessive. Also, if the flow rate is small, it may be difficult to control that flow rate.

[0105] It is preferable to deposit metal oxide films using a method that does not use a hydrogen-containing gas (e.g., H2) as the deposition gas. This suppresses the increase in hydrogen concentration in the metal oxide film. Sputtering is preferred for depositing metal oxide films. It is preferable to deposit metal oxide films using a metal target or a sputtering method using a metal oxide target. Furthermore, noble gases (e.g., helium gas, argon gas, xenon gas, etc.) can be used as the deposition gas when depositing metal oxide films. Since H2 gas is flammable, explosion-proof measures are required when using it. Not using H2 gas is preferable because it eliminates the need for capital investment related to explosion-proof measures.

[0106] When using sputtering to deposit a metal oxide film, the deposition gas (e.g., argon) is ionized, and these ions collide with a sputtering target. The sputtered particles ejected from the sputtering target reach the layer to be formed (in this case, the insulating layer 105), thereby depositing the metal oxide film. A high power density is preferable during metal oxide film deposition. A low pressure is also preferable. As a result, the sputtered particles reach the surface of the insulating layer 105 with high kinetic energy, causing some of the hydrogen contained in the insulating layer 105 to desorb. The hydrogen desorbed from the insulating layer 105 then diffuses into the metal oxide film. In this way, a gas containing hydrogen is not used as the deposition gas for the metal oxide film; instead, hydrogen is desorbed from the insulating layer 105 during deposition and diffused into the metal oxide film. This allows the metal oxide film to contain hydrogen while preventing the hydrogen concentration in the metal oxide film from becoming too high. Finally, crystallization can be achieved by heat treatment, resulting in a metal oxide film with a large grain size.

[0107] It is preferable that hydrogen is desorbed from the insulating layer 105 when heat is applied. When a metal oxide film is formed on the insulating layer 105, the application of heat causes hydrogen (e.g., hydrogen molecules) to desorb from the insulating layer 105, and this hydrogen diffuses into the metal oxide film. As a result, the crystallinity of the metal oxide film after formation is reduced, allowing for a metal oxide film with a larger grain size through subsequent heat treatment. Furthermore, when heat treatment is performed after the metal oxide film has been formed, hydrogen is desorbed from the insulating layer 105, and this hydrogen diffuses into the metal oxide film. By performing heat treatment while the metal oxide film contains hydrogen, the number of crystal nuclei formed in the metal oxide film is reduced, allowing for a metal oxide film with a larger grain size. In this way, supplying hydrogen from the insulating layer 105 to the metal oxide film can suppress the hydrogen concentration in the metal oxide film from becoming too high, and a metal oxide film with a larger grain size can be obtained. Note that the desorption of a substance from a layer may be described as the release of that substance.

[0108] The insulating layer 105 exhibits a hydrogen molecule desorption rate of 1.0 × 10⁻¹⁰ when its surface temperature is between 50°C and 350°C. 13 molecular / cm² 2 More than 1.0 × 10 14 molecular / cm² 2 Less than is preferable, and even more preferably 1.2 × 10 13 molecular / cm² 2 The above 8.0 x 10 13 molecular / cm² 2 The following is preferable. The amount of hydrogen molecules desorbed as described above is the total amount in the temperature range of 50°C to 350°C on the surface of the insulating layer 105.

[0109] If a large amount of hydrogen molecules are removed from the insulating layer 105, the hydrogen concentration in the metal oxide film may become high. In such cases, it is preferable to perform a treatment to remove hydrogen from the insulating layer 105 after it has been formed but before the metal oxide film has been formed, thereby lowering the hydrogen concentration in the insulating layer 105. This reduces the amount of hydrogen that diffuses into the metal oxide film and suppresses an increase in the hydrogen concentration in the metal oxide film. For example, heat treatment can be suitably used as this treatment. It is preferable to set the conditions of the treatment so that the amount of hydrogen molecules removed from the insulating layer 105 after the treatment to lower the hydrogen concentration in the insulating layer 105 falls within the aforementioned range. Typically, the hydrogen concentration in the insulating layer 105 can be adjusted by adjusting the temperature of the heat treatment. For example, by increasing the temperature of the heat treatment, the hydrogen concentration in the insulating layer 105 can be lowered, and the amount of hydrogen that diffuses into the metal oxide film can be reduced.

[0110] If the amount of hydrogen molecules desorbed from the insulating layer 105 is small, the crystallinity of the metal oxide film after deposition may increase, resulting in a smaller grain size. In such cases, it is preferable to supply hydrogen to the insulating layer 105 after deposition of the insulating layer 105 but before deposition of the metal oxide film, thereby increasing the hydrogen concentration in the insulating layer 105. This increases the amount of hydrogen diffusing into the metal oxide film, thereby lowering the crystallinity of the metal oxide film after deposition. Plasma treatment can be suitably used as this treatment. It is preferable to perform the plasma treatment in an atmosphere containing a hydrogen-containing gas (e.g., H2). It is preferable to set the conditions of the treatment so that the amount of hydrogen molecules desorbed from the insulating layer 105 after the treatment to increase the hydrogen concentration in the insulating layer 105 falls within the aforementioned range. Typically, the hydrogen concentration in the insulating layer 105 can be adjusted by adjusting the plasma treatment time. For example, by increasing the plasma treatment time, the hydrogen concentration in the insulating layer 105 can be increased, thereby increasing the amount of hydrogen diffusing into the metal oxide film.

[0111] The insulating layer 105 can also be formed using a method that does not use a gas containing hydrogen as the deposition gas. For example, when forming a silicon oxide film as the insulating layer 105, a reactive sputtering method using a silicon target or a sputtering method using a silicon oxide target can be used, and oxygen and argon can be used as the deposition gas. When forming the insulating layer 105 using a method that does not use a gas containing hydrogen as the deposition gas, the hydrogen concentration in the insulating layer 105 after formation is low, so it is preferable to perform a treatment to increase the hydrogen concentration in the insulating layer 105.

[0112] The amount of hydrogen molecules desorbed can be evaluated, for example, by thermal desorption spectroscopy (TDS), using the amount of H2 (m / z (also called mass-to-charge ratio) = 2) desorbed. In TDS, the amount of desorption can be quantified from the detection intensity (here, the current value) of the mass spectrometer. To convert from detection intensity to desorption amount, for example, a standard sample with a known amount of H2 (m / z=2) desorption can be used. The lower limit of quantification in TDS is 1.0 × 10⁻⁶. 13 molecular / cm² 2 It is to that extent. Furthermore, the amount of hydrogen molecules desorbed from the insulating layer 105 is not limited to the aforementioned range.

[0113] When performing TDS on the semiconductor device 10, it is preferable to remove the layer above the insulating layer 105 to expose the insulating layer 105. In this embodiment, the heating rate of the sample surface temperature during TDS is set to approximately 16°C / min. The heating rate of the stage on which the sample is placed can be, for example, approximately 32°C / min. During the manufacturing process of the semiconductor device 10, hydrogen may diffuse from the insulating layer 105 to the metal oxide film or semiconductor layer 108, and in the semiconductor device 10 after the manufacturing process, the amount of hydrogen that can be desorbed from the insulating layer 105 may be small. Therefore, when performing TDS on the semiconductor device 10, the amount of hydrogen molecules desorbed may be small.

[0114] For analyzing the hydrogen concentration in the semiconductor layer 108 and the insulating layer 105, for example, secondary ion mass spectrometry (SIMS) can be used. However, the hydrogen concentration in the semiconductor layer 108 may not be uniform. The same applies to the insulating layer 105.

[0115] By using oxygen gas as the deposition gas for the metal oxide film, the occurrence of oxygen vacancies in the metal oxide film can be suppressed. Furthermore, oxygen can be supplied to the insulating layer 105 during the deposition of the metal oxide film. This allows oxygen to be supplied from the insulating layer 105 to the semiconductor layer 108 in subsequent processes, thus suppressing oxygen vacancies and V OH can be reduced. However, if the ratio of oxygen gas flow rate to the total deposition gas flow rate when depositing the metal oxide film (hereinafter also referred to as the oxygen flow rate ratio) is too high, the number of crystal grains contained in the metal oxide film will increase at the stage of deposition, and the grain size of the crystal grains contained in the semiconductor layer 108 may decrease. Also, if the amount of oxygen contained in the semiconductor layer 108 is too high, shallow defect levels (sDOS: shallow level Density of States) may be formed in the metal oxide. If the amount of sDOS increases, the S value (Subthreshold Swing, also referred to as SS) of the transistor will increase, and there is a risk that the field effect mobility will decrease. The oxygen flow rate ratio is preferably higher than 0% and 10% or less, more preferably higher than 0% and 5% or less, and even more preferably higher than 0% and 3% or less. By setting the oxygen flow rate ratio within the above range, oxygen vacancies and V in the semiconductor layer 108 can be reduced. O This method reduces H and lowers the crystallinity of the metal oxide film after deposition. Furthermore, it enables the creation of transistors with a small S value and high field-effect mobility. Note that the oxygen flow rate ratio is not limited to the aforementioned range.

[0116] Noble gases and oxygen gases can be used to form metal oxide films. As mentioned above, it is preferable not to use gases containing hydrogen in the formation of metal oxide films. It is preferable that a portion of the film-forming gas for metal oxide films is a noble gas (typically argon), and the rest is oxygen gas.

[0117] The thickness T108 in the channel formation region of the semiconductor layer 108 is preferably 1 nm to 50 nm, more preferably 1 nm to 40 nm, more preferably 1 nm to 30 nm, more preferably 1 nm to 20 nm, and more preferably 1 nm to 10 nm. Increasing the thickness T108 can increase the on-current of the transistor. However, if the thickness T108 is too thick, oxygen vacancies and V in the semiconductor layer 108 will occur. OIf the amount of H increases, the transistor may become normally-on. Furthermore, reliability may decrease. The grain size of the crystal grains contained in the semiconductor layer 108 may also decrease. By setting the thickness T108 within the aforementioned range, a transistor with good electrical characteristics and high reliability can be obtained. The thickness T108 can be defined as the shortest distance between the surface of the semiconductor layer 108 where it overlaps with the conductive layer 104 (in this case, the upper surface of the insulating layer 105) and the upper surface of the semiconductor layer 108 in a cross-sectional view. In Figure 1(C), the thickness T108 is indicated by a solid arrow. Note that the thickness T108 is not limited to the aforementioned range.

[0118] The grain size of the crystal grains contained in semiconductor layer 108 can be analyzed, for example, by transmission electron microscopy (TEM), scanning transmission electron microscopy (STEM), or electron backscatter diffraction (EBSD or EBSP). Alternatively, a combination of these methods can be used for analysis. For example, the average grain size of multiple crystal grains can be used as the grain size. Furthermore, the grain size of a crystal grain can be defined as, for example, the diameter of a circle with the same area as the crystal grain. This diameter is sometimes called the equivalent diameter of a circle. The crystal structure of cubic In2O3 belongs to space group Ia-3 (space group number 206), for example.

[0119] In this specification, a grain boundary refers to, for example, the boundary between adjacent grains with different crystal orientations. Therefore, in this specification, boundaries between adjacent grains with the same crystal orientation are not included in grain boundaries. For example, even if a boundary is observed between two grains in a TEM image, if the crystal orientations of those two grains are the same or approximately the same, the boundary may not be called a grain boundary. Also, in EBSD, if the difference in crystal orientation between adjacent measurement points is small (for example, if the difference in crystal orientation is less than 5 degrees), these measurement points can be considered to belong to the same grain.

[0120] In this specification, space groups are denoted using international notation (or Hermann-Mauguin notation) in short form. In addition, space group numbers from the International Tables for Crystallography Volume A (hereinafter also referred to as ITA) may be included. Crystal planes and crystal directions are indicated using Miller indices. While crystallographic notation uses a bar above the number for space groups, crystal planes, and crystal directions, due to formatting constraints in this specification, a minus sign (-) may be placed before the number instead. Individual orientations within a crystal are indicated by [ ], collective orientations showing all equivalent directions are indicated by < >, individual crystal planes are indicated by ( ), and collective planes with equivalent symmetry are indicated by {}. Note that even with the same space group number, the notation of the space group may differ depending on the choice of crystal axes.

[0121] The grain size of the crystal grains can also be confirmed, for example, using an optical microscope or a scanning electron microscope (SEM). Furthermore, by creating surface irregularities on the semiconductor layer 108 using etchants with different etching rates depending on the crystal plane or crystallinity, the crystal grains can be more easily observed using an optical microscope or SEM. When an indium oxide film is used as the semiconductor layer 108, the crystal grains of the indium oxide can be more easily observed by using an etchant containing an acid. Examples of such acids include one or more types of phosphoric acid, oxalic acid, hydrofluoric acid, nitric acid, and hydrochloric acid. However, if the etching amount is too large, a portion of the semiconductor layer 108 may disappear, making it difficult to observe the crystal grains. Therefore, it is preferable to adjust the etching amount by the type, concentration, temperature, and processing time of the etchant so that the semiconductor layer 108 does not disappear but its thickness is reduced (also called half-etching). Half-etching allows for easy observation of the crystal grains.

[0122] Furthermore, if the thickness T108 is thin, it may be difficult to evaluate the crystallinity and grain size of the semiconductor layer 108.

[0123] Figure 1(B), etc., shows a configuration in which the edge of the insulating layer 106 coincides with the edge of the conductive layer 104. The edge of the insulating layer 106 is located on the semiconductor layer 108. Furthermore, the insulating layer 106 does not overlap with either region 108P or region 108Q. It can also be said that the top surface shape of the insulating layer 106 coincides with, or roughly coincides with, the conductive layer 104. The insulating layer 106 can be formed, for example, by processing it using a resist mask for processing the conductive layer 104. Note that it is also possible to have a configuration in which the edge of the insulating layer 106 does not coincide with the edge of the conductive layer 104.

[0124] An insulating layer 195 is provided on the semiconductor layer 108, the insulating layer 106, and the conductive layer 104. The insulating layer 195 has regions that are in contact with the top and side surfaces of the semiconductor layer 108, the side surfaces of the insulating layer 106, and the top and side surfaces of the conductive layer 104. The insulating layer 195 has regions that are in contact with region 108P and region 108Q, and has an opening 147a that reaches region 108P and an opening 147b that reaches region 108Q. Conductive layers 112a and 112b are formed so as to cover the openings 147a and 147b. Conductive layer 112a is in contact with region 108P at the opening 147a and is connected to region 108P. Conductive layer 112b is in contact with region 108Q at the opening 147b and is connected to region 108Q. The conductive layer 112a functions as one of the source and drain electrodes of the transistor 100, and the conductive layer 112b functions as the other of the source and drain electrodes.

[0125] The conductive layer 104 is located above the semiconductor layer 108 and can be described as a top gate. Furthermore, by using the conductive layer 104 as a mask and supplying impurities to the semiconductor layer 108, regions 108P and 108Q, which function as the source and drain regions in a self-aligned manner, can be formed. Transistor 100 can be described as a TGSA (Top Gate Self-Aligned) type transistor.

[0126] In a TGSA-type transistor, the physical distance between the conductive layers 112a and 112b, which function as the source and drain electrodes, and the conductive layer 104, which functions as the gate electrode, can be increased, thereby reducing the parasitic capacitance between them.

[0127] Furthermore, the conductive layer 103 can be configured to be connected to either the conductive layer 112a or the conductive layer 112b. For example, by providing openings in the insulating layer 195, insulating layer 106, and insulating layer 105 that reach the conductive layer 103, and providing the conductive layer 112a so as to cover these openings, the conductive layer 103 and the conductive layer 112a can be in contact. By connecting the conductive layer 112a and the conductive layer 103, the source electrode and the drain electrode and the back gate electrode can be brought to the same potential. For example, when the conductive layer 112a functions as the source electrode, a shift in the threshold voltage of the transistor 100 can be suppressed. In addition, the reliability of the transistor 100 can be improved.

[0128] Alternatively, the conductive layer 103 can be configured to be connected to the conductive layer 104. For example, by providing openings in the insulating layer 106 and the insulating layer 105 that reach the conductive layer 103, and providing the conductive layer 104 so as to cover the openings, the conductive layer 103 and the conductive layer 104 can be in contact. By connecting the gate electrode and the back gate electrode, the back gate electrode and the gate electrode can be brought to the same potential, and the on-current of the transistor 100 can be increased.

[0129] Regions 108P and 108Q contain impurities. By supplying impurities to the semiconductor layer 108, the electrical resistance of regions 108P and 108Q can be lowered. The elements contained in the impurities (hereinafter also referred to as the first element or impurity element) can be hydrogen, boron, carbon, nitrogen, fluorine, phosphorus, sulfur, arsenic, aluminum, magnesium, silicon, and one or more noble gases. Representative examples of noble gases include helium, neon, argon, krypton, and xenon. It is particularly preferable to use one or more of hydrogen, boron, phosphorus, and fluorine as the first element. The concentration of the first element in regions 108P and 108Q is higher than the concentration of the first element in region 108i.

[0130] For analyzing the concentration of the first element in semiconductor layer 108, for example, SIMS or X-ray photoelectron spectroscopy (XPS) can be used. XPS is sometimes also called ESCA (Electron Spectrometry for Chemical Analysis). Furthermore, multiple analytical methods can be used. For example, a combined analysis using both SIMS and XPS can be performed. The same applies to other analyses.

[0131] By supplying the first element, an oxygen vacancy is created in the semiconductor layer 108. Furthermore, V OThe generation of H allows for the formation of regions 108P and 108Q, which have low electrical resistance. Furthermore, when an element that readily bonds with oxygen is used as the first element, the first element removes oxygen from the semiconductor layer 108 and exists in a state bonded with oxygen. When an element that becomes stable when bonded with oxygen is used as the first element, the first element in the semiconductor layer 108 exists stably in an oxidized state, making it less susceptible to desorption due to heat applied during the semiconductor device manufacturing process, thus keeping the electrical resistance of regions 108P and 108Q low. For this reason, it is preferable to use an element as the first element whose oxide can exist as a solid at least at the temperature during the manufacturing process. Boron and phosphorus, or both, can be suitably used as the first element.

[0132] When boron is used as the first element, boron in regions 108P and 108Q can exist bonded to oxygen. This can be confirmed by the observation of peaks attributable to the B2O3 bond in XPS analysis. In addition, in XPS analysis, peaks attributable to the element boron existing in its pure form may not be observed, or the peak intensity may be extremely low, almost at background levels.

[0133] Hydrogen, when supplied, causes an oxygen deficiency, and when it enters the oxygen deficiency, V O Because H is generated, the electrical resistance in regions 108P and 108Q can be efficiently reduced. Therefore, hydrogen can be suitably used as the first element.

[0134] In supplying the first element, it is preferable to adjust the supply conditions so that the concentration of the first element is highest on the surface of the semiconductor layer 108 or in a region close to the surface.

[0135] For supplying the first element, the raw material can be, for example, a gas containing the first element. When supplying boron, typically one or more of B2H6 gas or BF3 gas can be used. Similarly, when supplying phosphorus, typically PH3 gas can be used. Furthermore, these raw material gases can be diluted with noble gases. Note that the raw material is not limited to gases; solids or liquids can also be vaporized and used.

[0136] As a method for supplying the first element, for example, ion implantation or plasma treatment can be used.

[0137] Ion implantation allows for highly precise control of the concentration profile in the depth direction by adjusting the ion acceleration energy and dose. The acceleration energy can be adjusted by the acceleration voltage during ion implantation. Furthermore, by using an ion implantation method that ionizes the source gas and supplies the ions by mass separation, it is possible to supply ions of a specific mass and increase the purity of the supplied ions. Alternatively, productivity can be increased by using an ion implantation method that supplies ions without mass separation. Unless otherwise specified in this specification, the presence or absence of mass separation is not limited. Note that the method of supplying ions by mass separation is sometimes called ion implantation, and the method of supplying ions without mass separation is sometimes called ion doping. By using a gas containing a first element as the source gas, the first element can be supplied. The amount of the first element supplied can be adjusted, for example, by adjusting the ion acceleration energy and dose.

[0138] When using ion implantation to supply the first element, it is preferable to set conditions such as acceleration voltage and dose amount considering the composition, density, and thickness of the insulating layer 106 and the semiconductor layer 108. Furthermore, since the first element is supplied to regions of the insulating layer 105 that do not overlap with the conductive layer 104, these regions may also contain the first element.

[0139] The method of supplying the first element is not particularly limited; for example, plasma treatment or treatment utilizing thermal diffusion by heating can be used. For plasma treatment, a device that generates plasma from a gas using high-frequency power can be suitably used. Examples of such devices include plasma CVD devices, plasma etching devices, and plasma ashing devices. In the case of plasma treatment, the first element can be supplied by generating plasma in a gas atmosphere containing the first element to be supplied and performing plasma treatment.

[0140] A plasma CVD apparatus can be used for supplying the first element to regions 108P and 108Q, and for depositing the insulating layer 195. This allows the supply of the first element and the deposition of the insulating layer 195 to be performed continuously within the plasma CVD apparatus, thereby increasing productivity. Furthermore, it is preferable to perform these processes continuously in the same processing chamber of the same plasma CVD apparatus. For example, by performing plasma treatment in an atmosphere containing a hydrogen-containing gas (e.g., NH3) using a plasma CVD apparatus, hydrogen can be supplied as the first element to a region of the semiconductor layer 108 that does not overlap with the conductive layer 104. Subsequently, the insulating layer 195 can be deposited in the same processing chamber as the supply of the first element.

[0141] An insulating layer 218 is provided on the conductive layer 112a, the conductive layer 112b, and the insulating layer 195. The insulating layer 195 and the insulating layer 218 each function as protective layers for the transistor 100.

[0142] [Semiconductor layer 108] The metal oxides that can be used in the semiconductor layer 108 will be described in detail. As mentioned above, the metal oxide preferably contains at least indium. Indium oxide can be suitably used as the metal oxide. Alternatively, the metal oxide preferably contains one or both of indium and element M. Alternatively, the metal oxide preferably contains one or both of indium and zinc. Alternatively, the metal oxide preferably has one or more elements selected from indium, element M, and zinc. Element M is a metallic or metalloid element with a high bond energy with oxygen, for example, a metallic or metalloid element with a higher bond energy with oxygen than indium. Specific examples of element M include aluminum, gallium, tin, yttrium, titanium, vanadium, chromium, manganese, iron, cobalt, nickel, zirconium, molybdenum, hafnium, tantalum, tungsten, lanthanum, cerium, neodymium, magnesium, calcium, strontium, barium, boron, silicon, germanium, and antimony. The element M present in the metal oxide is preferably one or more of the above elements, more preferably one or more selected from gallium, aluminum, tin, and yttrium, and even more preferably one or more of gallium, aluminum, and tin. These elements are more preferred because they have high bonding energy with oxygen and their ionic radii are similar to those of indium or zinc. Furthermore, tin is more preferred because its tetravalent state can increase carrier mobility. In this specification, metallic elements and metalloid elements are sometimes collectively referred to as "metallic elements," and the "metallic elements" described herein may include metalloid elements.

[0143] The semiconductor layer 108 is, for example, made of indium oxide (IO), gallium oxide, zinc oxide, indium zinc oxide (In-Zn oxide, also known as IZO®), indium tin oxide (In-Sn oxide, also known as ITO), indium titanium oxide (In-Ti oxide), indium gallium oxide (In-Ga oxide, also known as IGO), indium tungsten oxide (In-W oxide, also known as IWO), indium gallium aluminum oxide (In-Ga-Al oxide), indium gallium tin oxide (In-Ga-Sn oxide, also known as IGTO), gallium zinc oxide (Ga-Zn oxide, also known as GZO), aluminum Indium zinc oxide (Al-Zn oxide, also written as AZO), indium aluminum zinc oxide (In-Al-Zn oxide, also written as IAZO), indium tin zinc oxide (In-Sn-Zn oxide, also written as ITZO®), indium titanium zinc oxide (In-Ti-Zn oxide), indium gallium zinc oxide (In-Ga-Zn oxide, also written as IGZO), indium gallium tin zinc oxide (In-Ga-Sn-Zn oxide, also written as IGZTO), indium gallium aluminum zinc oxide (In-Ga-Al-Zn oxide, also written as IGAZO, IGZAO, or IAGZO), etc., can be used. Alternatively, silicon-containing indium tin oxide (In-Sn-Si oxide, also written as ITSO), gallium tin oxide (Ga-Sn oxide), aluminum tin oxide (Al-Sn oxide), etc., can be used.

[0144] Furthermore, the metal oxide can be composed of one or more metal elements with high periodic numbers in the periodic table, either in place of indium or in addition to indium. The greater the overlap of the metal element orbitals, the greater the carrier conduction in the metal oxide tends to be. Therefore, by including metal elements with high periodic numbers, the field-effect mobility of the transistor can be increased. Examples of metal elements with high periodic numbers include those belonging to the 5th period and those belonging to the 6th period. Specifically, these metal elements include yttrium, zirconium, silver, cadmium, tin, antimony, barium, lead, bismuth, lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium. Lanthanum, cerium, praseodymium, neodymium, promethium, samarium, and europium are called light rare earth elements.

[0145] Metal oxides may contain one or more nonmetallic elements. The presence of nonmetallic elements in metal oxides can increase carrier concentration or reduce the band gap, potentially improving the field-effect mobility of transistors. Examples of nonmetallic elements include carbon, nitrogen, phosphorus, sulfur, selenium, fluorine, chlorine, bromine, and hydrogen.

[0146] A metal oxide containing indium and element M can be used for the semiconductor layer 108. The presence of element M allows for oxygen vacancies (V) in the metal oxide. O The formation of ) is suppressed, and carrier generation due to oxygen vacancies is suppressed. As a result, the threshold voltage of the transistor is not shifted, the cutoff current can be reduced, and a normally-off transistor can be made. In addition, a transistor with a small off current can be made. Fluctuations in the electrical characteristics of the transistor are suppressed, and reliability can be improved. For example, fluctuations in electrical characteristics due to photo-negative bias (hereinafter also referred to as photo-negative bias degradation) can be suppressed.

[0147] However, if the content of element M in the metal oxide is too high, the content of indium will decrease, which may result in a low field-effect mobility. Therefore, it is preferable that the atomic ratio of element M in the metal oxide is less than or equal to the atomic ratio of indium.

[0148] The atomic ratio of indium in the metal oxide is preferably equal to or greater than the atomic ratio of element M. Furthermore, the indium content in the metal oxide is preferably 50% to 100%, more preferably 60% to 100%, more preferably 60% to 99%, more preferably 70% to 99%, more preferably 80% to 99%, more preferably 80% to 98%, more preferably 80% to 96%, more preferably 86% to 94%, and more preferably 80% to 92%. However, the indium content is not limited to the above ranges.

[0149] The composition of the metal oxide applied to the semiconductor layer 108 can affect the electrical characteristics and reliability of the transistor. Therefore, it is preferable to select the content of indium and element M according to the electrical characteristics and reliability required for the transistor. Typically, it is preferable to use indium gallium oxide with an indium content of 60% to 99% for the semiconductor layer 108. This makes it possible to create a transistor that achieves both high field-effect mobility and high reliability.

[0150] When the metal oxide is an In-M oxide, it is preferable to use metal oxides with atomic ratios of the metal elements such as In:M=99:1, In:M=98:2 (49:1), In:M=97:3, In:M=95:5 (19:1), In:M=10:1, In:M=5:1, In:M=4:1, In:M=3:1, In:M=2:1, or close to these. Typically, metal oxides with any of these atomic ratios and in which element M is Ga can be suitably used.

[0151] If element M contains multiple elements, the content of element M can be defined as the sum of the ratios of the number of atoms of element M to the sum of the total number of atoms of all contained metal elements.

[0152] By increasing the zinc content in a metal oxide, a highly crystalline metal oxide is obtained, which suppresses the diffusion of impurities within the metal oxide. Therefore, fluctuations in the electrical characteristics of the transistor are suppressed, and its reliability can be improved.

[0153] When the metal oxide is an In-M-Zn oxide, it is preferable that the atomic ratio of In in the In-M-Zn oxide is equal to or greater than the atomic ratio of element M. Examples of such atomic ratios of metal elements in an In-M-Zn oxide include In:M:Zn=1:1:1, In:M:Zn=1:1:1.2, In:M:Zn=2:1:3, In:M:Zn=3:1:1, In:M:Zn=3:1:2, In:M:Zn=4:2:3, In:M:Zn=4:2:4.1, In:M:Zn=5:1:3, In:M:Zn=5:1:6, In:M:Zn=5:1:7, In:M:Zn=5:1:8, and In:M Compositions such as Zn=5:1:9, In:M:Zn=6:1:6, In:M:Zn=10:1:1, In:M:Zn=10:1:3, In:M:Zn=10:1:4, In:M:Zn=10:1:6, In:M:Zn=10:1:7, In:M:Zn=10:1:8, In:M:Zn=5:2:5, In:M:Zn=10:1:10, In:M:Zn=20:1:10, In:M:Zn=40:1:10, and compositions near these. In this specification, "nearby composition" includes a range of ±30% of the desired atomic ratio. Increasing the atomic ratio of indium in a metal oxide can increase the on-current or field-effect mobility of a transistor.

[0154] The atomic ratio of In in an In-M-Zn oxide can be less than the atomic ratio of element M. Examples of such atomic ratios of metal elements in In-M-Zn oxides include In:M:Zn=1:3:2, In:M:Zn=1:3:3, In:M:Zn=1:3:4, In:M:Zn=1:3:6, and compositions close to these. Increasing the proportion of M atoms in the metal oxide can suppress the formation of oxygen vacancies.

[0155] A metal oxide that does not contain element M can be applied to the semiconductor layer 108. When the metal oxide is an In-Zn oxide, examples of atomic ratios of the metal elements include In:Zn=1:1, In:Zn=2:1, In:Zn=1:2, In:Zn=3:1, In:Zn=3:2, In:Zn=2:3, In:Zn=4:1, In:Zn=4:3, In:Zn=5:1, In:Zn=5:2, In:Zn=5:3, In:Zn=5:4, In:Zn=5:6, In:Zn=5:7, In:Zn=5:8, In:Zn=5:9, In:Zn=7:1, In:Zn=10:1, In:Zn=10:3, In:Zn=10:7, and compositions near these. Furthermore, it is more preferable that the atomic ratio of In is greater than or equal to the atomic ratio of Zn. By increasing the atomic ratio of indium in a metal oxide, the on-current or field-effect mobility of a transistor can be increased.

[0156] When the metal oxide is an In-M-Zn oxide, it is preferable to use a metal oxide with an atomic ratio of metal elements of, for example, In:M:Zn = 40:1:10, or close to that ratio. Typically, a metal oxide with any of these atomic ratios and in which element M is Ga can be suitably used.

[0157] For analyzing the composition of the semiconductor layer 108, for example, energy dispersive X-ray spectroscopy (EDX), X-ray photoelectron spectroscopy (XPS), inductively coupled plasma mass spectrometry (ICP-MS), or inductively coupled plasma atomic emission spectroscopy (ICP-AES) can be used. Alternatively, a combination of these methods can be used for analysis. It is preferable to separate the peaks of the spectrum obtained by the analysis and then identify and quantify the elements. Note that for elements with low content, the actual content may differ from the content obtained by the analysis due to the effect of analytical accuracy. For example, if the content of element M is low, the content of element M obtained by the analysis may be lower than the actual content, it may be difficult to quantify the content of element M, or element M may be below the detection limit.

[0158] The semiconductor layer 108 can be a single layer or a stacked structure of two or more layers. When the semiconductor layer 108 is a stacked structure, the aforementioned metal oxides can be suitably used in each layer of the semiconductor layer 108. The same material can be used for each layer of the semiconductor layer 108. Alternatively, different materials can be used for one or more layers of the semiconductor layer 108.

[0159] In this specification, "different materials" means materials in which some or all of the constituent elements are different, or materials in which the constituent elements are the same but the composition is different.

[0160] It is preferable to use a crystalline metal oxide for the semiconductor layer 108. Examples of crystalline metal oxide structures include CAAC (c-axis aligned crystal) structure, polycrystalline structure, microcrystalline structure, and nanocrystalline (nc) structure. By using a crystalline metal oxide, the defect level density in the semiconductor layer 108 can be reduced, resulting in a highly reliable transistor. Therefore, a highly reliable semiconductor device can be realized.

[0161] It is preferable to use CAAC-OS or nc-OS for the semiconductor layer 108.

[0162] CAAC-OS has multiple layered crystals. The c-axis of these crystals is oriented in the direction normal to the surface to be formed. Preferably, the semiconductor layer 108 has layered crystals that are parallel or approximately parallel to the surface to be formed. Preferably, the semiconductor layer 108 has layered crystals that are parallel or approximately parallel to the upper surface of the insulating layer 105, which is the surface to be formed. With this configuration, the layered crystals of the semiconductor layer 108 are formed parallel or approximately parallel to the channel length direction of the transistor 100, so that a transistor with a large on-current can be made.

[0163] OS transistors exhibit minimal fluctuations in electrical properties due to radiation exposure, meaning they have high radiation resistance, making them suitable for use in environments where radiation may be incident. OS transistors can also be said to have high reliability against radiation. For example, OS transistors are suitable for use in the pixel circuits of X-ray flat panel detectors. Furthermore, OS transistors are suitable for use in semiconductor devices used in outer space. Examples of radiation include electromagnetic radiation (e.g., X-rays and gamma rays) and particle radiation (e.g., alpha rays, beta rays, protons, and neutrons).

[0164] The semiconductor layer 108 may have a layered material that functions as a semiconductor. A layered material is a general term for a group of materials that have a layered crystal structure. Layered materials have high electrical conductivity within a unit layer, that is, high two-dimensional electrical conductivity. By using a material that functions as a semiconductor and has high two-dimensional electrical conductivity in the channel formation region, a transistor with a large on-current can be provided.

[0165] Examples of the above-mentioned layered materials include graphene, silicene, and chalcogenides. Chalcogenides are compounds containing chalcogens (elements belonging to Group 16). Examples of chalcogenides include transition metal chalcogenides and Group 13 chalcogenides. Specific examples of transition metal chalcogenides applicable as channel-forming regions include molybdenum sulfide (typically MoS2), molybdenum selenide (typically MoSe2), molybdenum tellurium (typically MoTe2), tungsten sulfide (typically WS2), tungsten selenide (typically WSe2), tungsten tellurium (typically WTe2), hafnium sulfide (typically HfS2), hafnium selenide (typically HfSe2), zirconium sulfide (typically ZrS2), and zirconium selenide (typically ZrSe2).

[0166] [Insulating layer 106, insulating layer 105] The materials that can be used for insulating layer 106 and insulating layer 105 can be found in the description above. Note that in miniature transistors, if the thickness of the gate insulating layer is reduced, the leakage current may increase. By using a material with a high dielectric constant (also called a high-k material) for the gate insulating layer, it is possible to reduce the voltage during transistor operation while maintaining the physical film thickness. Examples of high-k materials that can be used for insulating layer 106 include gallium oxide, hafnium oxide, zirconium oxide, oxides having aluminum and hafnium, oxidized nitrides having aluminum and hafnium, oxides having silicon and hafnium, oxidized nitrides having silicon and hafnium, and nitrides having silicon and hafnium.

[0167] In Figure 1(B), etc., the insulating layer 106 and insulating layer 105 are shown as single-layer structures, but the present invention is not limited to this. One or both of the insulating layer 106 and insulating layer 105 can be made into a laminated structure of two or more layers. When the insulating layer 106 is made into a laminated structure, it is preferable that the insulating layer on the semiconductor layer 108 side has an oxide or oxidizride. Similarly, when the insulating layer 105 is made into a laminated structure, it is preferable that the insulating layer on the semiconductor layer 108 side has an oxide or oxidizride. For example, one or more of silicon oxide, silicon oxidizride, or aluminum oxide can be suitably used for the insulating layer on the semiconductor layer 108 side. Non-patent document 3 discloses a configuration in which hafnium oxide is used for the insulating layer in contact with the lower surface of the indium oxide layer, which is a semiconductor layer, and aluminum oxide is used for the insulating layer in contact with the upper surface of the indium oxide layer.

[0168] It is preferable to use a material that is impermeable to substances in one or more of the layers constituting the insulating layer 106. This layer can also be said to function as a barrier film. By providing a layer that functions as a barrier film, it is possible to suppress the diffusion of metal components contained in the conductive layer 104 and impurities (e.g., water and hydrogen) contained in the layers formed on the transistor 100 into the semiconductor layer 108 via the insulating layer 106. Furthermore, it is possible to suppress the diffusion of oxygen contained in the semiconductor layer 108 into the conductive layer 104 side via the insulating layer 106. This suppresses the formation of oxygen vacancies in the semiconductor layer 108. In addition, it is possible to suppress the oxidation of the conductive layer 104 by the oxygen contained in the semiconductor layer 108, which increases the electrical resistance of the conductive layer 104. As a result, a transistor with good electrical characteristics and high reliability can be obtained. Similarly, it is preferable to provide a layer that functions as a barrier film in one or more of the layers constituting the insulating layer 105.

[0169] In this specification, the term "barrier film" refers to a film that possesses barrier properties. Barrier properties refer to one or both of the following functions: a function that makes it difficult for the target substance to diffuse, thereby suppressing the permeation of the substance through the film (also known as low permeability), and a function that captures or fixes the substance (also known as gettering).

[0170] The barrier film can be, for example, one or more oxides having aluminum and / or hafnium, an oxide having magnesium, an oxide having gallium, a nitride having silicon, an oxidized nitride having silicon, and an oxide nitride having silicon. Typically, the barrier film can be preferably made from one or more aluminum oxide, hafnium oxide, hafnium aluminate, magnesium oxide, gallium oxide, zinc gallium oxide, silicon nitride, silicon oxidized nitride, and silicon oxide nitride. The barrier film of the insulating layer 106 can be made from one or more oxides and oxidized nitrides, for example, aluminum oxide can be preferably used. The barrier film of the insulating layer 105 can be made from one or more nitrides and oxide nitrides, for example, silicon nitride can be preferably used.

[0171] The insulating layer 106 can, for example, be a laminated structure of a silicon oxidizide film and a silicon nitride film on the silicon oxidizide film. Alternatively, the insulating layer 106 can be a laminated structure of a silicon oxidizide film and an aluminum oxide film on the silicon oxidizide film. Alternatively, the insulating layer 106 can be a laminated structure of an aluminum oxide film and a silicon oxidizide film on the aluminum oxide film. Alternatively, the insulating layer 106 can be a laminated structure of an aluminum oxide film and a silicon nitride film on the aluminum oxide film. Here, an example is shown in which the insulating layer 106 has a two-layer laminated structure, but the present invention is not limited to this. The insulating layer 106 can also have a laminated structure of three or more layers.

[0172] Examples of insulating layers 105 having a laminated structure are shown in Figures 2(A) and 2(B). The top views of the semiconductor device 10A shown in Figures 2(A) and 2(B) can be found by referring to Figure 1(A). Figure 2(A) is a cross-sectional view of the section along the dashed-dotted line A1-A2 shown in Figure 1(A), and Figure 2(B) is a cross-sectional view of the section along the dashed-dotted line B1-B2.

[0173] The semiconductor device 10A has a transistor 100A. Figures 2(A) and 2(B) show an example in which the insulating layer 105 has an insulating layer 105a and an insulating layer 105b on the insulating layer 105a.

[0174] As mentioned above, the insulating layer 105b in contact with the semiconductor layer 108 preferably contains oxygen. The insulating layer 105a located on the substrate 102 and conductive layer 103 side preferably functions as a barrier film. By providing a barrier film, the diffusion of components (e.g., metals) contained in the substrate 102 and conductive layer 103 into the semiconductor layer 108 can be suppressed, resulting in a highly reliable semiconductor device. For details on the barrier film, please refer to the above description. The insulating layer 105a preferably contains nitrogen.

[0175] The insulating layer 105a preferably contains silicon and nitrogen. The insulating layer 105b preferably contains silicon and oxygen. For example, silicon nitride can be suitably used for the insulating layer 105a and silicon oxynitride can be suitably used for the insulating layer 105b.

[0176] When the insulating layer 105 has a laminated structure, it is preferable that one or more layers of the insulating layer 105 contain hydrogen. In particular, it is preferable that the insulating layer 105b, which is the layer to be formed on the semiconductor layer 108, contains hydrogen. The insulating layer 105b preferably contains, for example, silicon, oxygen, and hydrogen. For example, silicon oxidnitride containing hydrogen or silicon oxide containing hydrogen can be suitably used as the insulating layer 105b. It is preferable to form the insulating layer 105b using a method that uses a gas containing the element hydrogen as the film-forming gas. For silicon oxidnitride films containing hydrogen and silicon oxide films containing hydrogen, refer to the above description.

[0177] The insulating layer 105a can also be configured to contain hydrogen. The hydrogen contained in the insulating layer 105a diffuses into the insulating layer 105b, allowing the metal oxide film to contain hydrogen when it is formed on the insulating layer 105. The insulating layer 105a preferably contains, for example, silicon, nitrogen, and hydrogen. For example, silicon nitride containing hydrogen can be used for the insulating layer 105a. As the film-forming gas for the silicon nitride film, a depositing gas containing silicon and a nitriding gas can be used. As the nitriding gas, a gas containing nitrogen can be used. For example, one or more of nitrogen (N2) and ammonia (NH3) can be used as the nitriding gas. Since NH3 contains hydrogen along with nitrogen, it can be suitably used as the film-forming gas for the insulating layer 105a. Typically, SiH4, N2, and NH3 can be suitably used as film-forming gases for a silicon nitride film containing hydrogen. Furthermore, the hydrogen concentration of the silicon nitride film can be controlled by the ratio of ammonia gas flow rate to the total film deposition gas flow rate (hereinafter also referred to as the ammonia flow rate ratio). Specifically, increasing the ammonia flow rate ratio can increase the hydrogen concentration of the silicon nitride film, while decreasing the ammonia flow rate ratio can decrease the hydrogen concentration. In addition, the stress on the silicon nitride film can sometimes be controlled by the ammonia flow rate ratio. By reducing the stress, defects caused by stress (for example, film delamination) can be suppressed.

[0178] Here, an example is shown in which the insulating layer 105 has a two-layer laminated structure, but the present invention is not limited to this. The insulating layer 105 can also have a three-layer or more laminated structure.

[0179] [Conductive layer 112a, conductive layer 112b, conductive layer 104, conductive layer 103] The conductive layers 112a, 112b, 104, and 103 can each be a single-layer structure or a laminated structure of two or more layers. Materials that can be used for the conductive layers 112a, 112b, 104, and 103 include, for example, one or more of chromium, copper, aluminum, gold, silver, zinc, tantalum, titanium, tungsten, manganese, nickel, iron, cobalt, molybdenum, and niobium, as well as alloys comprising one or more of the aforementioned metals. Conductive materials with low electrical resistivity, containing one or more of copper, silver, gold, and aluminum, can be suitably used for the conductive layers 112a, 112b, 104, and 103, respectively. Copper or aluminum are particularly preferred due to their excellent mass-productivity.

[0180] Conductive layers 112a, 112b, 104, and 103 can each be made of a conductive metal oxide (also called an oxide conductor (OC)). Examples of oxide conductors include indium oxide, zinc oxide, ITO, In-Zn oxide, In-W oxide, In-W-Zn oxide, In-Ti oxide, In-Ti-Sn oxide, ITSO, In-Sn-Zn oxide, Ga-Zn oxide, and In-Ga-Zn oxide. Oxide conductors containing indium are particularly preferred due to their high conductivity.

[0181] When oxygen vacancies are formed in a metal oxide with semiconductor properties, and hydrogen is added to these vacancies, donor levels are formed near the conduction band. As a result, the metal oxide becomes highly conductive and turns into a conductor. A metal oxide that has become conductive can also be called an oxide conductor.

[0182] The conductive layers 112a, 112b, 104, and 103 can each be a laminated structure of a conductive film containing the aforementioned oxide conductor (metal oxide) and a conductive film containing a metal or alloy. By using a conductive film containing a metal or alloy, the wiring resistance can be reduced.

[0183] Conductive layers 112a, 112b, 104, and 103 can each be made of nitride conductors. Examples of nitride conductors include tantalum nitride and titanium nitride.

[0184] Conductive layers 112a, 112b, 104, and 103 can each be made of a Cu-X alloy film (where X is Mn, Ni, Cr, Fe, Co, Mo, Ta, or Ti). Using a Cu-X alloy film allows for processing by wet etching, thus reducing manufacturing costs.

[0185] The conductive layer 104 has a work function (φ M It is preferable to use a material with a large work function. It is preferable that the work function of the conductive layer 104 is greater than the electron affinity of the semiconductor layer 108. An OS transistor using a metal oxide containing indium is a storage-type transistor with electrons as the majority carrier. By using a material with a large work function for the conductive layer 104 which functions as the gate electrode of the transistor, it is possible to shift the threshold voltage of the transistor. Furthermore, normally-off becomes possible. Therefore, a transistor with good electrical characteristics can be provided.

[0186] As the conductive layer 104, for example, a conductive material having a work function of 4.5 eV or more, preferably 5.0 eV or more, can be used. Examples of such conductive materials include metals such as platinum, nickel, copper, cobalt, molybdenum, chromium, and tungsten. Examples of such conductive materials include oxide conductors, nitrogen-containing oxide conductors, and nitride conductors. Examples of such oxide conductors include ITO, ITSO, In-Zn oxide, tungsten-containing indium tin oxide (In-Sn-W oxide), In-Ti oxide, and indium zirconium oxide (In-Zr oxide). Examples of such nitrogen-containing oxide conductors include nitrogen-containing In-Ga-Zn oxide, nitrogen-containing indium tin oxide, nitrogen-containing indium gallium oxide, nitrogen-containing indium zinc oxide, nitrogen-containing tin oxide, and nitrogen-containing indium oxide. Examples of such nitride conductors include titanium nitride, indium nitride, and tin nitride.

[0187] Note that conductive layers 112a, 112b, 104, and 103 can be made of the same material. Alternatively, at least one of them can be made of a different material.

[0188] [Insulating layer 195] The insulating layer 195 preferably has one or more inorganic insulating layers. Refer to the above description for details regarding the inorganic insulating layers.

[0189] The insulating layer 195 preferably functions as a barrier film. This effectively suppresses the diffusion of impurities (e.g., water and hydrogen) into the transistor from the outside, thereby improving the reliability of the semiconductor device. For example, one or more of silicon nitride, silicon oxide nitride, and silicon oxynitride can be suitably used as the insulating layer 195. For details regarding the barrier film, please refer to the above description.

[0190] It is preferable to provide barrier films above and below the semiconductor layer 108. It is preferable that each of these barrier films has a region that overlaps with the semiconductor layer 108. This suppresses both the diffusion of impurities into the semiconductor layer 108 from above and from below. Therefore, fluctuations in the electrical characteristics of the transistor are suppressed, and reliability can be improved. For example, it is preferable to provide barrier films on both the insulating layer 195 and the insulating layer 105. For the insulating layer 105, refer to the description above. Typically, silicon nitride can be used for the insulating layer 105a and silicon nitride oxide can be used for the insulating layer 195. Alternatively, silicon nitride can be used for the insulating layer 105a and silicon oxynitride oxide can be used for the insulating layer 195. For the laminated structure of the insulating layer 105, refer to the description in Figures 2(A) and 2(B).

[0191] [Insulating layer 218] As the insulating layer 218, either an inorganic insulating layer or an organic insulating layer, or both, can be used. The inorganic insulating layer can be made from the materials listed for insulating layer 106 and insulating layer 105. Examples of materials that can be used for the organic insulating layer include acrylic resin and polyimide resin. The organic insulating layer functions as a planarizing layer that reduces irregularities caused by the transistor.

[0192] [Circuit board 102] There are no major restrictions on the material of the substrate 102, but it must have at least enough heat resistance to withstand subsequent heat treatments. For example, single-crystal semiconductor substrates, polycrystalline semiconductor substrates, compound semiconductor substrates such as silicon germanium, SOI substrates, glass substrates, quartz substrates, sapphire substrates, ceramic substrates, or resin substrates made of silicon or silicon carbide can be used as the substrate 102. Furthermore, a substrate on which a semiconductor element is provided can be used as the substrate 102. A substrate with an insulating film formed on its surface can also be used as the substrate 102. The shape of the substrate 102 is not particularly limited and can be, for example, circular or rectangular.

[0193] A flexible substrate can be used as the substrate 102, and transistors 100, etc., can be formed directly on the flexible substrate. Alternatively, a release layer can be provided between the substrate 102 and the transistors 100, etc. By providing a release layer, part or all of the semiconductor device can be formed on it, then separated from the substrate 102 and transferred to another substrate. In this case, the transistors 100, etc., can also be transferred to a substrate with low heat resistance or a flexible substrate.

[0194] The following describes a configuration example that differs in some aspects from the aforementioned <Configuration Example 1>. Note that in the following, explanations of parts that overlap with <Configuration Example 1> may be omitted. Also, in the drawings shown below, parts having the same function as those in <Configuration Example 1> may use the same hatching pattern and may not be labeled.

[0195] Furthermore, the structure of the transistor that can be applied to a semiconductor device according to one aspect of the present invention is not particularly limited.

[0196] <Configuration Example 2> Figures 3(A) and 3(B) show cross-sectional views of a semiconductor device 10B, which is one embodiment of the present invention. A top view of the semiconductor device 10B can be found in Figure 1(A). Figure 3(A) is a cross-sectional view of the section along the dashed line A1-A2 shown in Figure 1(A), and Figure 3(B) is a cross-sectional view of the section along the dashed line B1-B2.

[0197] The semiconductor device 10B has a transistor 100B. Transistor 100B differs from transistor 100 shown in Figure 1(B), etc., in that its semiconductor layer 108 has a stacked structure.

[0198] Figure 3(B), etc., shows a configuration in which the semiconductor layer 108 has a three-layer structure consisting of semiconductor layer 108a, semiconductor layer 108b on semiconductor layer 108a, and semiconductor layer 108c on semiconductor layer 108b. Semiconductor layer 108b is in contact with and sandwiched between semiconductor layers 108a and 108c.

[0199] The semiconductor layers 108a, 108b, and 108c can each be made from the materials listed for semiconductor layer 108. The semiconductor layers 108a, 108b, and 108c can each be made from the same material. Indium oxide can be suitably used for each of the semiconductor layers 108a, 108b, and 108c. Alternatively, one or more of the semiconductor layers 108a, 108b, and 108c can be made from different materials.

[0200] In some cases, the boundaries between semiconductor layer 108a and semiconductor layer 108b, and between semiconductor layer 108b and semiconductor layer 108c, cannot be clearly identified. Therefore, in Figure 3(B), etc., these boundaries are shown with dashed lines. In some cases, one or both of these boundaries can be identified.

[0201] It is preferable that the conductivity of semiconductor layer 108b is higher than that of either semiconductor layer 108a or semiconductor layer 108c. This ensures that the main current path in transistor 100B is semiconductor layer 108b. On the other hand, in semiconductor layer 108, it is preferable that semiconductor layer 108a in contact with insulating layer 105 and semiconductor layer 108c in contact with insulating layer 106 are denser and have fewer defects than semiconductor layer 108b.

[0202] Trap levels due to impurities or defects may form at the interface between the insulating layer 106, which functions as a gate insulating layer, and the semiconductor layer 108, and at the interface between the insulating layer 105, which functions as a back gate insulating layer, and the semiconductor layer 108, and at the interface at the interface at the interface. Furthermore, when the insulating layer 106 is deposited, damage may be inflicted on the interface between the insulating layer 106 and the semiconductor layer 108, causing trap levels to form at the interface at the interface at the interface. By sandwiching the semiconductor layer 108b, which is the main current path, between semiconductor layers 108a and 108c, the semiconductor layer 108b can be moved away from the interface between the semiconductor layer 108 and the insulating layer, thereby reducing the trap level density at and near the interface of the semiconductor layer 108b. This makes it possible to create a transistor with high field-effect mobility.

[0203] Here, when a high potential is applied to the conductive layer 104 functioning as a gate electrode, trap levels can be formed at and in the vicinity of the interface between the insulating layer 106 and the semiconductor layer 108. Similarly, when a high potential is applied to the conductive layer 103 functioning as a back gate electrode, trap levels can be formed at and in the vicinity of the interface between the insulating layer 105 and the semiconductor layer 108. When electrons are trapped in these trap levels, the threshold voltage of the transistor shifts to the positive side, which may reduce reliability. By providing the semiconductor layer 108c with few defects in contact with the insulating layer 106, formation of trap levels at and in the vicinity of the interface between the insulating layer 106 and the semiconductor layer 108 can be suppressed. Similarly, by providing the semiconductor layer 108a with few defects in contact with the insulating layer 105, formation of trap levels at and in the vicinity of the interface between the insulating layer 105 and the semiconductor layer 108 can be suppressed. Accordingly, a transistor with high reliability can be obtained.

[0204] In this manner, by sandwiching the semiconductor layer 108b with high conductivity between the semiconductor layer 108a and the semiconductor layer 108c each having few defects, a transistor that achieves both high field-effect mobility and high reliability can be obtained. Accordingly, a semiconductor device that achieves both high-speed operation and high reliability can be obtained.

[0205] In the channel formation region, the carrier mobility of the semiconductor layer 108b is preferably higher than that of the semiconductor layer 108a and the semiconductor layer 108c. Here, in the case where a non-single-crystal (e.g., polycrystalline) metal oxide is used for the semiconductor layer, the carrier mobility can sometimes be increased by increasing the carrier concentration. The carrier concentration of the semiconductor layer 108b is preferably higher than that of the semiconductor layer 108a and the semiconductor layer 108c. Accordingly, the conductivity of the semiconductor layer 108b, which is the main current path, is increased, and a transistor with high field-effect mobility can be obtained.

[0206] It is preferable that semiconductor layer 108a, semiconductor layer 108b, and semiconductor layer 108c each have an element that increases the carrier concentration (hereinafter also referred to as the second element). For example, one or more of hydrogen, carbon, and nitrogen can be used as the second element. Hydrogen can be suitably used as the second element. Hydrogen reacts with oxygen bonded to the metal atoms of the metal oxide to form water, thereby forming oxygen vacancies in the metal oxide. Furthermore, a defect (V) is formed when hydrogen enters the oxygen vacancy. O H) functions as a donor, generating electrons, which are carriers, thereby increasing the carrier concentration in the metal oxide. Note that in the following explanation, hydrogen may be used as an example of the second element.

[0207] In the channel formation region, it is preferable that semiconductor layer 108b has a region with a higher concentration of the second element compared to semiconductor layer 108a and semiconductor layer 108c. Typically, it is preferable that semiconductor layer 108b has a region with a higher hydrogen concentration compared to semiconductor layer 108a and semiconductor layer 108c. This increases the carrier concentration in semiconductor layer 108b, thereby increasing the carrier mobility. On the other hand, if the hydrogen concentration in semiconductor layer 108a and semiconductor layer 108c is too high, there is a risk of an increase in defects. Therefore, in the channel formation region, it is preferable that semiconductor layer 108a and semiconductor layer 108c each have a region with a lower concentration of the second element compared to semiconductor layer 108b.

[0208] For the analysis of the concentration of the second element in the semiconductor layer 108, for example, SIMS or XPS can be used. For example, SIMS can be suitably used for the analysis of hydrogen concentration. However, the reliability of the measured values ​​may be low at the interface between the semiconductor layer 108 and the layer in contact with the semiconductor layer 108, and in its vicinity, due to the matrix effect. For example, when measurements are taken in the direction from the insulating layer 106 towards the semiconductor layer 108, the reliability of the measured values ​​may be low at the interface between the insulating layer 106 and the semiconductor layer 108, and in its vicinity. Measured values ​​in areas with low reliability should not be treated as the concentration of the second element in the semiconductor layer 108. Furthermore, the accuracy of the analysis of the concentration of the second element in the semiconductor layer 108 can sometimes be improved by combining measurements taken in the direction from the insulating layer 106 towards the semiconductor layer 108 with measurements taken in the direction from the insulating layer 105 towards the semiconductor layer 108.

[0209] In concentration analysis, the intensity of the constituent elements of the metal oxide can sometimes be used to infer the location of the interface between the insulating layer 106 and the semiconductor layer 108, and the location of the interface between the insulating layer 105 and the semiconductor layer 108. For example, the range in which the intensity of the constituent elements of the metal oxide present in the semiconductor layer 108 is 1 / 2 or more of its maximum value can be defined as the semiconductor layer 108. When a metal oxide containing indium is used for the semiconductor layer 108, and SIMS is used for the concentration analysis of the second element, the range in which the secondary ion intensity of indium is 1 / 2 or more of its maximum value can be defined as the semiconductor layer 108, and the range in which it is less than 1 / 2 of its maximum value can be defined as layers other than the semiconductor layer 108 (e.g., insulating layer 105 and insulating layer 106). Alternatively, the range in which the secondary ion intensity of an indium-containing cluster (e.g., an indium-oxygen cluster) is 1 / 2 or more of its maximum value can be defined as the semiconductor layer 108, and the range in which it is less than 1 / 2 of its maximum value can be defined as layers other than the semiconductor layer 108 (e.g., insulating layer 105 and insulating layer 106).

[0210] It is preferable that the film density of semiconductor layer 108a and semiconductor layer 108c is higher than that of semiconductor layer 108b. This reduces defects in semiconductor layer 108a and semiconductor layer 108c. Furthermore, by providing a semiconductor layer 108c with a high film density on semiconductor layer 108b, damage to semiconductor layer 108b during the deposition of the insulating layer 106 can be suppressed. Film density can be evaluated using, for example, Rutherford backscattering spectrometry (RBS) or X-ray reflectivity (XRR).

[0211] Differences in film density can sometimes be evaluated using a cross-sectional transmission electron microscope (TEM) image. In TEM observation, a high film density results in a darker transmission electron (TE) image, while a low film density results in a lighter (brighter) transmission electron (TE) image. Therefore, even when the same material, such as indium oxide, is used for semiconductor layers 108a, 108b, and 108c, differences in film density among these layers can sometimes be observed as differences in contrast in cross-sectional TEM observations. Specifically, in the TE image, semiconductor layers 108a and 108c may have darker regions compared to semiconductor layer 108b. Also, semiconductor layer 108b may have lighter (brighter) regions compared to semiconductor layers 108a and 108c.

[0212] Furthermore, the film densities of semiconductor layer 108a and semiconductor layer 108c can be the same as, or lower than, the film densities of semiconductor layer 108b, respectively.

[0213] Even when using the same material, the etching rate may be slower if the film is denser and has a higher film density. It is preferable that the etching rate at one etchant of semiconductor layer 108a and semiconductor layer 108c is slower than the etching rate of semiconductor layer 108b. It is also preferable to provide a semiconductor layer 108c with a slow etching rate on top of semiconductor layer 108b. This makes it possible to suppress the disappearance of semiconductor layer 108c in the etching process after the formation of semiconductor layer 108, and to suppress the thinning of the thickness of semiconductor layer 108.

[0214] When the semiconductor layer 108 has a three-layer structure consisting of semiconductor layer 108a, semiconductor layer 108b, and semiconductor layer 108c, the metal oxide films are deposited in the following order: a first metal oxide film to become semiconductor layer 108a, a second metal oxide film to become semiconductor layer 108b, and a third metal oxide film to become semiconductor layer 108c.

[0215] The first, second, and third metal oxide films are preferably deposited by sputtering using a metal target or a metal oxide target. Alternatively, the first, second, and third metal oxide films are preferably deposited by ALD (Advanced Laser Deposition) method. Since the deposition rate of the ALD method is easy to control, thin films can be deposited with a high yield. Therefore, the ALD method is particularly suitable when the metal oxide film is thin. Alternatively, the CVD method can also be used.

[0216] Examples of power supplies used in sputtering equipment include DC (Direct Current) power supplies, RF (Radio Frequency) power supplies, and AC (Alternating Current) power supplies. A pulsed DC power supply, which applies a pulsed voltage to the target, can also be used. Furthermore, the magnetron sputtering method, which utilizes the magnetic field of a magnet, offers a high deposition rate, thus increasing productivity. The deposition of the first, second, and third metal oxide films can be preferably performed using sputtering methods, particularly magnetron sputtering. In the following explanation, the magnetron sputtering method may be used as an example to describe the deposition methods for the first, second, and third metal oxide films.

[0217] It is preferable to deposit a second metal oxide film in a vacuum after depositing a first metal oxide film, without exposing the surface of the first metal oxide film to the atmosphere. Similarly, it is preferable to deposit a third metal oxide film in a vacuum after depositing a second metal oxide film, without exposing the surface of the second metal oxide film to the atmosphere. By depositing the first, second, and third metal oxide films in succession, it is possible to suppress the adhesion of airborne impurities to the surfaces of the first and second metal oxide films. Examples of such impurities include water and organic matter.

[0218] When using the same material for two or more of the first, second, and third metal oxide films, the films can be deposited using the same sputtering target and in the same processing chamber.

[0219] It is preferable that semiconductor layers 108a, 108b, and 108c use the same material. The first metal oxide film, the second metal oxide film, and the third metal oxide film can be deposited continuously in the same processing chamber using the same sputtering target. This increases the productivity of semiconductor devices and reduces manufacturing costs. Furthermore, it is possible to suppress the adhesion of airborne impurities to the surfaces of the first metal oxide film and the second metal oxide film.

[0220] Alternatively, it is preferable to use one or more different materials for semiconductor layer 108a, semiconductor layer 108b, and semiconductor layer 108c. Two or more sputtering targets can be used to deposit the first metal oxide film, the second metal oxide film, and the third metal oxide film. In this case as well, it is preferable to deposit the metal oxide films continuously in a vacuum within the same apparatus without exposing the surface of the metal oxide films to the atmosphere. For example, it is preferable to deposit each metal oxide film in different processing chambers continuously in a vacuum within the same apparatus.

[0221] As mentioned above, the boundaries between semiconductor layer 108a and semiconductor layer 108b, and between semiconductor layer 108b and semiconductor layer 108c, may not be clearly identifiable. In particular, in configurations where the same material is used for semiconductor layer 108a, semiconductor layer 108b, and semiconductor layer 108c, these boundaries may not be clearly identifiable. Furthermore, by continuously depositing the first metal oxide film, the second metal oxide film, and the third metal oxide film in a vacuum, no interface may be formed between each metal oxide film, and these boundaries may not be identifiable. In such cases, semiconductor layer 108a, semiconductor layer 108b, and semiconductor layer 108c can be read as the first region, the second region, and the third region. Semiconductor layer 108 has a first region (corresponding to semiconductor layer 108a) on the insulating layer 105 side, a third region (corresponding to semiconductor layer 108c) on the insulating layer 106 side, and a second region (corresponding to semiconductor layer 108b) between the first region and the third region.

[0222] Preferably, the concentration of the second element in the second region is higher than the concentration of the second element in the first region and higher than the concentration of the second element in the third region. The concentration of the second element in the second region can be determined by referring to the description of the concentration of the second element in semiconductor layer 108b described above. The concentrations of the second element in the first region and the third region can be determined by referring to the descriptions of the concentrations of the second element in semiconductor layer 108a and semiconductor layer 108c described above, respectively. Note that the concentrations of the second element in the first region, the second region, and the third region are not limited to the ranges described above.

[0223] Preferably, the film density of the first region and the third region is higher than the film density of the second region. When observing the cross-section of the semiconductor layer 108 using TEM, the first and third regions may have darker areas in the TE image compared to the second region. Also, the second region may have lighter areas compared to the first and third regions.

[0224] Here, by varying the deposition conditions for the metal oxide film, the film quality of the metal oxide film (later the semiconductor layer) can be varied. Examples of film quality include conductivity, band gap, defect amount, impurity concentration, and crystallinity. Examples of deposition conditions include power density, pressure, gas type, gas flow rate, substrate temperature, and the distance between the sputtering target and the substrate (TS distance, also called TS distance). When varying the deposition conditions, one or more of the power density, pressure, gas type, gas flow rate, substrate temperature, and TS distance can be varied. Note that changing the substrate temperature and the TS distance may take time. Therefore, when depositing two or more metal oxide films in the same processing chamber, it is preferable to keep the substrate temperature and TS distance the same. Note that even when using the same material, the band gap may differ by varying the deposition conditions.

[0225] The deposition conditions for the first metal oxide film (hereinafter also referred to as the first deposition conditions) are preferably different from the deposition conditions for the second metal oxide film (hereinafter also referred to as the second deposition conditions). The deposition conditions for the third metal oxide film (hereinafter also referred to as the third deposition conditions) are preferably different from the second deposition conditions. For example, one or both of the power density and pressure under the first deposition conditions are preferably different from the power density and pressure under the second deposition conditions. Similarly, one or both of the power density and pressure under the third deposition conditions are preferably different from the power density and pressure under the second deposition conditions. It is particularly preferable that the power density and pressure under the first deposition conditions are different from the power density and pressure under the second deposition conditions, and the power density and pressure under the third deposition conditions are different from the power density and pressure under the second deposition conditions.

[0226] The power density under each of the first deposition conditions and the third deposition conditions is preferably higher than the power density under the second deposition conditions. By increasing the power density, the semiconductor layer 108a and the semiconductor layer 108c that are dense and have few defects can be obtained. The power density under each of the first deposition conditions and the third deposition conditions is 0.3 W / cm 2 or more and 2 W / cm 2 or less, more preferably 0.4 W / cm 2 or more and 2 W / cm 2 or less, more preferably 0.5 W / cm 2 or more and 2 W / cm 2 or less, more preferably 0.6 W / cm 2 or more and 2 W / cm 2 or less, more preferably 0.6 W / cm 2 or more and 1 W / cm 2The following is preferable. If the power density is too low, there is a risk of an increase in defects in the semiconductor layer 108a and semiconductor layer 108c, while if the power density is too high, there is a risk of an increased load on the device. By setting the power density in the first and third film deposition conditions within the aforementioned range, it is possible to obtain dense semiconductor layers 108a and 108c with few defects, while also reducing the load on the device. Note that the power density in the first and third film deposition conditions is not limited to the aforementioned ranges.

[0227] Power density is calculated by dividing the power applied to the substrate by the magnet area. The magnet area is the area of ​​the surface of the magnet that faces the sputtering target.

[0228] The power density under the second film deposition condition was 0.1 W / cm². 2 More than 1W / cm 2 The following are preferred, and moreover, 0.2 W / cm² 2 More than 1W / cm 2 The following are preferred, and moreover, 0.2 W / cm² 2 More than 0.8W / cm 2 The following are preferred, and moreover, 0.2 W / cm² 2 More than 0.6W / cm 2 The following are preferred, and moreover, 0.3 W / cm². 2 More than 0.6W / cm 2 The following is preferable. Furthermore, it is preferable that the power density under the second film deposition condition is lower than the power density under the first and third film deposition conditions. If the power density is too high, the conductivity of the semiconductor layer 108b may be low, while if the power density is too low, the film deposition rate will be slow, which may reduce productivity. Also, if the power density is too low, the discharge may become unstable. By setting the power density under the second film deposition condition within the aforementioned range, it is possible to obtain a semiconductor layer 108b with high conductivity and to increase productivity. Note that the power density under the second film deposition condition is not limited to the aforementioned range.

[0229] The pressure in the first and third film deposition conditions is preferably lower than the pressure in the second film deposition condition. By lowering the pressure, dense semiconductor layers 108a and 108c with few defects can be obtained. The pressure in the first and third film deposition conditions is preferably 0.1 Pa or more and 0.8 Pa or less, more preferably 0.1 Pa or more and 0.6 Pa or less, more preferably 0.1 Pa or more and 0.4 Pa or less, and more preferably 0.1 Pa or more and 0.3 Pa or less. If the pressure is too high, there is a risk of an increase in defects in semiconductor layers 108a and 108c, while if the pressure is too low, it may take a long time to adjust the pressure in the processing chamber, potentially reducing productivity. Also, if the pressure is too low, arcing may occur, making discharge difficult. By setting the pressure in the first and third film deposition conditions within the above range, dense semiconductor layers 108a and 108c with few defects can be obtained, and productivity can be increased. Furthermore, the pressures in the first and third film deposition conditions are not limited to the ranges described above.

[0230] The pressure in the second film deposition condition is preferably 0.2 Pa or more and 1 Pa or less, more preferably 0.3 Pa or more and 1 Pa or less, more preferably 0.4 Pa or more and 1 Pa or less, and more preferably 0.4 Pa or more and 0.8 Pa or less. Furthermore, the pressure in the second film deposition condition is preferably higher than the pressure in the first and third film deposition conditions. If the pressure is too low, the conductivity of the semiconductor layer 108b may be low. On the other hand, if the pressure is too high, the film deposition rate will be slow, which may reduce productivity. Also, if the pressure is too high, discharge may become difficult. By setting the pressure in the second film deposition condition within the above range, it is possible to obtain a semiconductor layer 108b with high conductivity and increase productivity. Note that the pressure in the second film deposition condition is not limited to the above range.

[0231] It is particularly preferable that the power density under the first and third film deposition conditions is higher than the power density under the second film deposition condition, and that the pressure under the first and third film deposition conditions is lower than the pressure under the second film deposition condition. This makes it possible to increase the conductivity of the semiconductor layer 108b and to make the semiconductor layers 108a and 108c denser and reduce defects.

[0232] Here, a configuration is shown in which the power density and pressure in the first and third film deposition conditions are different from those in the second film deposition condition; however, the present invention is not limited to this. It is also possible to differ other parameters (for example, gas flow rate) between the first and third film deposition conditions and the second film deposition condition.

[0233] Furthermore, the first and third film deposition conditions can be the same or different. By making the first and third film deposition conditions the same, that is, by making the film quality of semiconductor layer 108a and semiconductor layer 108c the same, the number of film types that need to be controlled in the manufacturing of semiconductor devices can be reduced. This can increase productivity. Alternatively, the first and third film deposition conditions can be different, that is, by making the film quality of semiconductor layer 108a and semiconductor layer 108c different. Since damage may occur to the semiconductor layer 108c when depositing the insulating layer 106, it is preferable that the third film deposition conditions be denser and less prone to defects compared to the first film deposition conditions. For example, one or both of the power density and pressure in the third film deposition conditions can be different from the power density and pressure in the first film deposition conditions. Specifically, the power density under the third film deposition condition can be made higher than the power density under the first film deposition condition. Furthermore, the pressure under the third film deposition condition can be made lower than the pressure under the first film deposition condition.

[0234] Figure 3(C) shows an enlarged view of the semiconductor layer 108 and its vicinity, as shown in Figure 3(B). In Figure 3(C), the thicknesses T108a of semiconductor layer 108a, T108b of semiconductor layer 108b, and T108c of semiconductor layer 108c are indicated by solid arrows. Thicknesses T108a, T108b, and T108c are the thicknesses of each layer in the region where semiconductor layer 108 overlaps with conductive layer 104 in a cross-sectional view. Note that thicknesses T108a, T108b, and T108c can be controlled by the processing time (also referred to as deposition time) during the deposition of semiconductor layers 108a, 108b, and 108c, respectively.

[0235] A thickness T108b is preferable. A thickness T108b is preferable to both thickness T108a and thickness T108c. By increasing the thickness T108b of the semiconductor layer 108b, which is the main current path, a transistor with a large on-current can be made. However, if the thickness T108b is too thick, oxygen vacancies and V in the semiconductor layer 108b may occur. O An increase in the amount of H can cause a shift in the transistor's threshold voltage, potentially leading to a larger cutoff current. The thickness T108b is preferably 1 nm to 30 nm, more preferably 2 nm to 30 nm, more preferably 2 nm to 20 nm, more preferably 4 nm to 20 nm, and more preferably 4 nm to 10 nm. By setting the thickness T108b within the above range, a transistor with a large on-current can be made. Furthermore, by suppressing the shift in the threshold voltage, the cutoff current can be reduced, resulting in a normally-off transistor. Note that the thickness T108b is not limited to the above range.

[0236] It is preferable that thicknesses T108a and T108c are each thinner than thickness T108b. Furthermore, thicknesses T108a and T108c are preferably 0.5 nm to 10 nm, more preferably 0.5 nm to 6 nm, more preferably 0.5 nm to 4 nm, more preferably 0.5 nm to 3 nm, and more preferably 1 nm to 3 nm. If thickness T108c is too thick, the physical distance between the conductive layer 104, which functions as the first gate electrode, and the semiconductor layer 108b becomes longer, which may result in a decrease in field-effect mobility. On the other hand, if thickness T108c is too thin, the physical distance between the interface and vicinity of the interface between the insulating layer 106 and the semiconductor layer 108, where trap levels can be formed, and the semiconductor layer 108b, which is the main current path, becomes shorter, which may result in a decrease in field-effect mobility. In addition, reliability may decrease. The same applies to thickness T108a. By setting the thicknesses T108a and T108c within the aforementioned ranges, a transistor with high field-effect mobility and high reliability can be obtained. Note that the thicknesses T108a and T108c are not limited to the aforementioned ranges.

[0237] Here, the semiconductor layer 108 is shown as a three-layer stacked structure, but the present invention is not limited to this. The semiconductor layer 108 can be a single layer, a two-layer, or a four-layer or more stacked structure. When the semiconductor layer 108 has a stacked structure, it is preferable that the semiconductor layer 108 has at least one semiconductor layer 108b.

[0238] Figures 4(A) and 4(B) show cross-sectional views of a semiconductor device 10C, which is one embodiment of the present invention. A top view of the semiconductor device 10C can be found in Figure 1(A). Figure 4(A) is a cross-sectional view of the section along the dashed line A1-A2 shown in Figure 1(A), and Figure 4(B) is a cross-sectional view of the section along the dashed line B1-B2.

[0239] The semiconductor device 10C has a transistor 100C. Transistor 100C differs from transistor 100B shown in Figure 3(A), etc., in that its semiconductor layer 108 has a two-layer structure consisting of semiconductor layer 108a and semiconductor layer 108b. By omitting the semiconductor layer 108c, the manufacturing process can be simplified and productivity can be increased.

[0240] Figures 5(A) and 5(B) show cross-sectional views of a semiconductor device 10D according to one embodiment of the present invention. A top view of the semiconductor device 10D can be found in Figure 1(A). Figure 5(A) is a cross-sectional view of the section along the dashed line A1-A2 shown in Figure 1(A), and Figure 5(B) is a cross-sectional view of the section along the dashed line B1-B2.

[0241] The semiconductor device 10D has a transistor 100D. Transistor 100D differs from transistor 100B shown in Figure 3(A), etc., mainly in that its semiconductor layer 108 has a two-layer structure consisting of semiconductor layer 108b and semiconductor layer 108c. By omitting the semiconductor layer 108a, the manufacturing process can be simplified and productivity can be increased.

[0242] As mentioned above, the layers of the semiconductor layer 108 can be made of the same material, or one or more layers of the semiconductor layer 108 can be made of different materials.

[0243] An example of a configuration in which one or more layers of the semiconductor layer 108 are made of different materials will be described.

[0244] In the semiconductor layer 108 shown in Figures 3(A) to 5(B), it is preferable that semiconductor layer 108a and semiconductor layer 108c each contain indium, element M, and oxygen. It is preferable that semiconductor layer 108b contains indium and oxygen. It is preferable that the content of element M in semiconductor layer 108a and semiconductor layer 108c is higher than the content of element M in semiconductor layer 108b. For example, In-M oxide can be suitably used in semiconductor layer 108a and semiconductor layer 108c, and indium oxide can be suitably used in semiconductor layer 108b. For element M, please refer to the above description. For example, gallium can be suitably used as element M. In the following, gallium may be used as an example of element M in the explanation.

[0245] It is preferable that semiconductor layer 108a and semiconductor layer 108c each contain indium, gallium, and oxygen. It is preferable that semiconductor layer 108b contains indium and oxygen. It is preferable that the gallium content in semiconductor layer 108a and semiconductor layer 108c is higher than the gallium content in semiconductor layer 108b. For example, In-Ga oxide can be suitably used for semiconductor layer 108a and semiconductor layer 108c, and indium oxide can be suitably used for semiconductor layer 108b.

[0246] Because the semiconductor layer 108c has element M with a high bonding energy with oxygen, oxygen vacancies and V are formed in the semiconductor layer 108. O The increase in H can be suppressed. On the conductive layer 104 side which functions as the gate electrode, oxygen deficiency and V O By providing a semiconductor layer 108c with low H content, a highly reliable transistor can be made. Similarly, on the conductive layer 103 side which functions as the back gate electrode, oxygen deficiency and V O By providing a semiconductor layer 108a with a low H content, a highly reliable transistor can be created.

[0247] When forming an insulating layer 106 on a semiconductor layer 108, damage is inflicted on the semiconductor layer 108, resulting in oxygen vacancies and V OH can be generated. This may cause the threshold voltage of the transistor to shift. Also, the reliability of the transistor may decrease. By using a metal oxide containing element M in the semiconductor layer 108c that has a region in contact with the insulating layer 106, oxygen vacancies and V can be introduced into the semiconductor layer 108. O This suppresses the increase in H. As a result, even transistors with short channel lengths can be made normally off. Furthermore, it can suppress threshold voltage variations due to drain-induced barrier lowering (DIBL), resulting in a more reliable transistor.

[0248] It is preferable that the indium content in semiconductor layer 108b is higher than that in semiconductor layers 108a and 108c. By increasing the indium content in semiconductor layer 108b, which is the main current path, a transistor with high field-effect mobility can be made.

[0249] When using sputtering to deposit a first metal oxide film that becomes semiconductor layer 108a, a second metal oxide film that becomes semiconductor layer 108b, and a third metal oxide film that becomes semiconductor layer 108c, it is preferable to use different sputtering targets and deposit the metal oxide films continuously in a vacuum within the same apparatus without exposing the surface of the metal oxide films to the atmosphere. For example, it is preferable to deposit each metal oxide film in different processing chambers continuously in a vacuum within the same apparatus. For example, a sputtering target having indium, element M, and oxygen can be used to deposit the first and third metal oxide films. For example, an In-M oxide sputtering target can be used as the sputtering target. A sputtering target having indium and oxygen can be used to deposit the second metal oxide film. For example, an indium oxide sputtering target can be used as the sputtering target.

[0250] Alternatively, the first, second, and third metal oxide films can be deposited using the same sputtering target, and then element M (e.g., gallium) can be supplied to the first and third metal oxide films. For supplying element M, for example, ion implantation can be used. For details on ion implantation, please refer to the previous description. For example, an indium oxide sputtering target can be used to deposit the first, second, and third metal oxide films. Since the first, second, and third metal oxide films can be deposited continuously in the same processing chamber using the same sputtering target, the productivity of semiconductor devices can be increased.

[0251] In supplying element M to semiconductor layer 108a, it is preferable to set the acceleration energy for supplying element M so that the concentration of element M is highest in semiconductor layer 108a, or at or near the interface between insulating layer 105 and semiconductor layer 108a. Similarly, in supplying element M to semiconductor layer 108c, it is preferable to set the acceleration energy for supplying element M so that the concentration of element M is highest in semiconductor layer 108c, or at or near the interface between insulating layer 106 and semiconductor layer 108c.

[0252] By supplying element M to the first and third metal oxide films, element M is also supplied to the second metal oxide film, and semiconductor layer 108b may also contain element M. In this case, it is preferable that the content of element M in semiconductor layer 108b is lower than that of semiconductor layers 108a and 108c. It is also possible to supply element M after the first metal oxide film has been formed, and then form the second metal oxide film. Note that the supply of element M is not limited to ion implantation.

[0253] <Configuration Example 3> Figures 6(A) and 6(B) show cross-sectional views of a semiconductor device 10E, which is one embodiment of the present invention. A top view of the semiconductor device 10E can be found in Figure 1(A). Figure 6(A) is a cross-sectional view of the section along the dashed line A1-A2 shown in Figure 1(A), and Figure 6(B) is a cross-sectional view of the section along the dashed line B1-B2.

[0254] The semiconductor device 10E has a transistor 100E. Transistor 100E differs from transistor 100 shown in Figure 1(B), etc., in that the insulating layer 106 has regions in contact with regions 108P and 108Q.

[0255] The insulating layer 106 has regions that are in contact with the upper and side surfaces of the semiconductor layer 108, and the upper surface of the insulating layer 105. An insulating layer 195 is provided on the insulating layer 106 and the conductive layer 104. The insulating layer 195 and the insulating layer 106 have openings 147a and 147b. Conductive layers 112a and 112b are formed to cover openings 147a and 147b.

[0256] Region 108i overlaps with the conductive layer 104 via the insulating layer 106. Regions 108P and 108Q overlap with the insulating layer 106 but do not overlap with the conductive layer 104.

[0257] After forming a conductive layer 104 on an insulating layer 106, the conductive layer 104 can be used as a mask to supply the first element to the semiconductor layer 108 via the insulating layer 106. In this case, the first element may be supplied to regions of the insulating layer 106 that do not overlap with the conductive layer 104, thereby resulting in those regions containing the first element. For example, ion implantation can be suitably used to supply the first element.

[0258] <Configuration Example 4> Figures 6(C) and 6(D) show cross-sectional views of a semiconductor device 10F according to one aspect of the present invention. A top view of the semiconductor device 10F can be found in Figure 1(A). Figure 6(C) is a cross-sectional view of the section along the dashed line A1-A2 shown in Figure 1(A), and Figure 6(D) is a cross-sectional view of the section along the dashed line B1-B2.

[0259] The semiconductor device 10F has a transistor 100F. Transistor 100F differs from transistor 100 shown in Figure 1(B), etc., in that the insulating layer 106 has a region that protrudes more than the conductive layer 104.

[0260] The edges of the insulating layer 106 are located on the semiconductor layer 108, and the edges of the conductive layer 104 are located on the insulating layer 106. It can also be said that the edges of the insulating layer 106 are located outside the edges of the conductive layer 104. The insulating layer 106 has a region that overlaps with the conductive layer 104 and a region that does not overlap with the conductive layer 104 on the semiconductor layer 108.

[0261] The semiconductor layer 108 has region 108i, a pair of regions (region 108R and region 108S) flanking region 108i, and a pair of regions (region 108P and region 108Q) located outside of these. Regions 108R and 108S overlap with the insulating layer 106 but do not overlap with the conductive layer 104. Region 108R is located between region 108i and region 108P, and region 108S is located between region 108i and region 108Q.

[0262] Regions 108R and 108S function as buffer regions to mitigate the drain electric field. Since regions 108R and 108S do not overlap with the conductive layer 104, channels are hardly formed in these regions even when a gate voltage is applied to the conductive layer 104. It is preferable that the carrier concentration in regions 108R and 108S is higher than that in the channel formation region. This allows regions 108R and 108S to function as LDD (Lightly Doped Drain) regions.

[0263] Regions 108R and 108S can also be described as regions with similar or lower electrical resistance, similar or higher carrier concentration, similar or higher oxygen deficiency density, and similar or higher concentration of the first element compared to the channel-forming region.

[0264] Regions 108R and 108S can also be described as regions with similar or higher electrical resistance, similar or lower carrier concentration, similar or lower oxygen deficiency density, and similar or lower concentration of the first element, compared to regions 108P and 108Q.

[0265] The insulating layer 195 has regions that are in contact with the upper and side surfaces of the semiconductor layer 108, the upper and side surfaces of the insulating layer 106, and the upper and side surfaces of the conductive layer 104.

[0266] <Configuration Example 5> Figure 7(A) shows a top view of a semiconductor device 10G, which is one embodiment of the present invention. Figure 7(B) shows a cross-sectional view of the section along the dashed line A1-A2 shown in Figure 7(A). For a cross-sectional view of the section along the dashed line B1-B2, please refer to Figure 6(B).

[0267] The semiconductor device 10G has a transistor 100G. Transistor 100G differs from transistor 100F shown in Figure 6(C), etc., in that conductive layers 112a and 112b are formed in the same process as conductive layer 104.

[0268] The insulating layer 106 has openings 147a and 147b that reach the semiconductor layer 108. Conductive layers 112a and 112b are provided so as to cover a portion of opening 147a and a portion of opening 147b. Conductive layer 112a has a region that contacts the semiconductor layer 108 at opening 147a, and conductive layer 112b has a region that contacts the semiconductor layer 108 at opening 147b.

[0269] Conductive layers 104, 112a, and 112b can be formed using the same material and the same process. For example, an insulating film is deposited on a semiconductor layer 108, and the insulating film is processed to form an insulating layer 106 having openings 147a and 147b. Then, a conductive film is deposited to cover the insulating layer 106, openings 147a and 147b, and the conductive film is processed to form conductive layers 104, 112a, and 112b. By forming conductive layers 112a and 112b using the same process as conductive layer 104, the number of processes can be reduced.

[0270] By supplying the first element to the semiconductor layer 108 using conductive layers 104, 112a, and 112b as masks, regions 108P and 108Q can be formed self-aligned. Regions 108P and 108Q are formed in regions of the semiconductor layer 108 that do not overlap with conductive layers 104, 112a, 112b, or the insulating layer 106. In addition, regions 108R and 108S are formed in regions of the semiconductor layer 108 that do not overlap with conductive layers 104, 112a, or 112b, but overlap with the insulating layer 106.

[0271] The region of the semiconductor layer 108 that is in contact with the conductive layer 112a, and the region 108P in contact with said region, function as one of the source region and the drain region. The region of the semiconductor layer 108 that is in contact with the conductive layer 112b, and the region 108Q in contact with said region, function as the other of the source region and the drain region.

[0272] An insulating layer 195 is provided on the transistor 100G. Although Figure 7(B) shows an example configuration in which an insulating layer 218 is not provided, the present invention is not limited to this. An insulating layer 218 can also be provided on the insulating layer 195.

[0273] <Configuration Example 6> Figure 8(A) shows a top view of a semiconductor device 10H, which is one embodiment of the present invention. Figure 8(B) shows a cross-sectional view of the section along the dashed-dotted line A1-A2 shown in Figure 8(A). For a cross-sectional view of the section along the dashed-dotted line B1-B2, please refer to Figure 6(D).

[0274] The semiconductor device 10H differs from the semiconductor device 10F shown in Figure 6(C), etc., in that it has layers 121a and 121b. The semiconductor device 10H includes a transistor 100H, layer 121a, and layer 121b.

[0275] Layers 121a and 121b are provided between the semiconductor layer 108 and the insulating layer 105, respectively. The semiconductor layer 108 has regions that are in contact with layers 121a, 121b, and the insulating layer 105.

[0276] The semiconductor layer 108 has region 108i, a pair of regions (regions 108X and 108Y) flanking region 108i, and a pair of regions (regions 108P and 108Q) located outside of these. Region 108i overlaps with the conductive layer 104 via the insulating layer 106 and does not contact either layer 121a or layer 121b. Regions 108P and 108Q do not overlap with either the conductive layer 104 or the insulating layer 106, respectively. It is also preferable that regions 108P and 108Q contact either layer 121a or layer 121b, respectively. Regions 108X and 108Y contact the insulating layer 106 and either layer 121a or layer 121b, respectively. In transistor 100H, region 108P functions as one of the source region and drain region, and region 108Q functions as the other of the source region and drain region.

[0277] A conductive layer can be used as layer 121a and layer 121b. The conductive layer can be made from the materials listed for conductive layer 104, conductive layer 112a, and conductive layer 112b. Oxide conductors can preferably be used as layer 121a and layer 121b. By using an oxide conductor, the contact resistance between layer 121a and semiconductor layer 108, and the contact resistance between layer 121b and semiconductor layer 108 can be further reduced. Alternatively, a semiconductor layer can be used as layer 121a and layer 121b. The semiconductor layer can be made from the materials listed for semiconductor layer 108. Typically, ITO, ITSO, or In-Sn-Zn oxide can preferably be used as layer 121a and layer 121b.

[0278] It is preferable that the thicknesses of layers 121a and 121b are greater than the thickness T108 of the semiconductor layer 108. This allows for lower electrical resistance of layers 121a and 121b. However, if the thickness T108 of the semiconductor layer 108 is thin, the electrical resistance of regions 108P and 108Q may become high. Nevertheless, by lowering the electrical resistance of layers 121a and 121b, the electrical resistance of the source and drain regions can be lowered even when the thickness T108 is thin.

[0279] Figure 8(B), etc., shows a configuration in which layers 121a and 121b each have regions that overlap with the conductive layer 104. That is, regions 108X and 108Y each have regions that overlap with the conductive layer 104. In regions 108X and 108Y, the regions that overlap with the conductive layer 104 may function as channel-forming regions. Furthermore, if the electrical resistance of these regions is lower than that of the channel-forming regions, these regions can function as buffer regions to mitigate the drain electric field.

[0280] As shown in Figure 8(C), the openings 147a and 147b can also be configured to penetrate the semiconductor layer 108 and reach layers 121a and 121b. The conductive layer 112a has a region in contact with layer 121a and region 108P at the opening 147a. The conductive layer 112b has a region in contact with layer 121b and region 108Q at the opening 147b. This makes it possible to lower the contact resistance between the source electrode and the source region, and the contact resistance between the drain electrode and the drain region, even when the thickness T108 is thin.

[0281] In addition, while Figures 8(A) to 8(C) show configurations in which layers 121a and 121b each have regions that overlap with the conductive layer 104, the present invention is not limited to these. It is also possible to have a configuration in which one or both of layers 121a and 121b do not overlap with the conductive layer 104.

[0282] A method for manufacturing a semiconductor device according to one aspect of the present invention will be described. Note that explanations regarding the materials and formation methods of each element may be omitted if they have already been described.

[0283] Thin films (insulating films, semiconductor films, and conductive films, etc.) that constitute semiconductor devices can be deposited using sputtering, chemical vapor deposition (CVD), vacuum deposition, pulsed laser deposition (PLD), ALD, and other methods.

[0284] Thin films (insulating films, semiconductor films, conductive films, etc.) that constitute semiconductor devices can be formed by wet deposition methods such as spin coating, dip coating, spray coating, inkjet printing, dispensing, screen printing, offset printing, doctor knife method, slit coating, roll coating, curtain coating, or knife coating.

[0285] When processing thin films that constitute semiconductor devices, lithography or similar methods can be used. Alternatively, thin films can be processed by nanoimprint lithography, sandblasting, lift-off methods, etc. Furthermore, island-shaped thin films can be directly formed by deposition methods using shielding masks such as metal masks.

[0286] There are two main methods of lithography. One method involves forming a resist mask on the thin film to be processed, then processing the thin film by etching or other means, and finally removing the resist mask. The other method involves forming a photosensitive thin film, then exposing and developing it to process the thin film into the desired shape.

[0287] In lithography, the light used for exposure can be, for example, i-line (wavelength 365 nm), g-line (wavelength 436 nm), h-line (wavelength 405 nm), or a mixture thereof. Other options include ultraviolet light, KrF laser light, or ArF laser light. Exposure can also be performed using immersion lithography. Furthermore, extreme ultraviolet (EUV) light or X-rays can be used for exposure. An electron beam can also be used instead of light for exposure. Using extreme ultraviolet light, X-rays, or an electron beam is preferable because it allows for extremely fine processing. Note that a photomask is not required when exposure is performed by scanning a beam such as an electron beam.

[0288] For etching thin films, one or more of the following methods can be used: dry etching, wet etching, and sandblasting.

[0289] <Example of manufacturing method 1> Here, an example of a method for manufacturing the semiconductor device 10B shown in Figures 3(A) and 3(B) will be explained using Figures 9(A) to 10(D). Figures 9(A) to 10(D) show side by side the cross-sectional view between the dashed lines A1 and A2 shown in Figure 3(A) and the cross-sectional view between the dashed lines B1 and B2 shown in Figure 3(B).

[0290] First, a conductive film is formed on the substrate 102, and the conductive film is processed to form a conductive layer 103. The conductive film can be suitably formed using a sputtering method.

[0291] Next, an insulating layer 105 is formed on the conductive layer 103 and the substrate 102 (Figure 9(A)). The insulating layer 105 can preferably be formed by sputtering or plasma CVD.

[0292] Next, a metal oxide film 108f, which will become the semiconductor layer 108, is deposited on the insulating layer 105 (Figure 9(C)). The metal oxide film 108f is preferably deposited by sputtering using a metal target or a metal oxide target. Alternatively, the metal oxide film 108f is preferably deposited by the ALD method. The ALD method allows for easy control of the deposition rate, enabling the deposition of thin films with a high yield. Therefore, the ALD method is particularly suitable when the thickness of the metal oxide film 108f is thin. Furthermore, the CVD method can be used to deposit the metal oxide film 108f.

[0293] If the substrate temperature during the deposition of the metal oxide film 108f is too high, the indium content in the metal oxide film 108f may decrease. The substrate temperature during the deposition of the metal oxide film 108f is preferably between room temperature (e.g., 25°C) and 200°C, more preferably between room temperature and 150°C, more preferably between room temperature and 120°C, and more preferably between room temperature and 100°C. However, the substrate temperature during the deposition of the metal oxide film 108f is not limited to the above range.

[0294] By increasing the substrate temperature when forming the metal oxide film 108f, the crystallinity of the metal oxide film 108f is increased, and defects can be reduced. This results in a transistor with high field-effect mobility and high reliability. Typically, the substrate temperature can be set to 100°C.

[0295] By lowering the substrate temperature during the deposition of the metal oxide film 108f, the crystallinity of the metal oxide film 108f can be reduced. This allows for a larger grain size during subsequent heat treatment. In particular, it is preferable to deposit the metal oxide film 108f at room temperature or without heating the substrate.

[0296] Here, as the metal oxide film 108f, a metal oxide film 108af that becomes the semiconductor layer 108a, a metal oxide film 108bf that becomes the semiconductor layer 108b, and a metal oxide film 108cf that becomes the semiconductor layer 108c are deposited. Sputtering is preferably used for depositing the metal oxide film 108af, metal oxide film 108bf, and metal oxide film 108cf. For the metal oxide film 108af, metal oxide film 108bf, and metal oxide film 108cf, refer to the descriptions of the first, second, and third metal oxide films mentioned above.

[0297] As mentioned above, it is preferable to have a high power density and low pressure during the deposition of the metal oxide film 108af (first metal oxide film). This increases the kinetic energy of the sputtered particles during the deposition of the metal oxide film 108af, allowing some of the hydrogen contained in the insulating layer 105 to be desorbed. This hydrogen then diffuses into the metal oxide film 108f, resulting in a metal oxide film 108f containing hydrogen. Figure 9(B) schematically shows the desorption of hydrogen from the insulating layer 105 using dashed arrows.

[0298] When using the ALD method, it is preferable to use a film deposition method such as the thermal ALD method or PEALD (Plasma Enhanced ALD). The thermal ALD method is preferred because it exhibits extremely high coverage. The PEALD method is preferred because, in addition to exhibiting high coverage, it allows for low-temperature film deposition.

[0299] The metal oxide films 108af, 108bf, and 108cf can each be formed by the ALD method using, for example, a precursor containing the constituent metal elements and an oxidizing agent.

[0300] For example, when depositing an indium oxide film, an indium-containing precursor can be used. When depositing an In-Ga oxide film, two types of precursors can be used: one containing indium and another containing gallium. Alternatively, a precursor containing both indium and gallium can be used.

[0301] Examples of indium precursors include triethylindium, trimethylindium, tris(2,2,6,6-tetramethyl-3,5-heptanedionic acid)indium, cyclopentadienylindium, indium(III) chloride, (3-(dimethylamino)propyl)dimethylindium, and [1,1,1-trimethyl-N-(trimethylsilyl)amide]indium.

[0302] Examples of gallium-containing precursors include trimethylgallium, triethylgallium, gallium(III) chloride, tris(dimethylamide)gallium(III), gallium(III) acetylacetonate, tris(2,2,6,6-tetramethyl-3,5-heptanedionic acid)gallium, dimethylchlorogallium, and diethylchlorogallium.

[0303] Examples of aluminum-containing precursors include aluminum chloride and trimethylaluminum.

[0304] Examples of tin-containing precursors include tin(IV) chloride and tetrakis(dimethylamide)tin.

[0305] Examples of zinc-containing precursors include zinc dimethyl, zinc diethyl, zinc bis(2,2,6,6-tetramethyl-3,5-heptanedione), and zinc chloride.

[0306] Examples of oxidizing agents include ozone, oxygen, hydrogen peroxide, and water.

[0307] Methods for controlling the composition of the resulting film include adjusting one or more of the type of raw material gas, the flow rate ratio of the raw material gases, the duration for which the raw material gases are flowed, and the order in which the raw material gases are flowed. By adjusting these factors, the composition of the metal oxide films 108af, 108bf, and 108cf can be controlled. Furthermore, by adjusting these factors, it is also possible to deposit a metal oxide film 108f with a continuously changing composition.

[0308] Before forming the metal oxide film 108f, it is preferable to perform at least one of the following: a treatment to desorb water, hydrogen, and organic matter adsorbed on the surface of the insulating layer 105, and a treatment to supply oxygen into the insulating layer 105. For example, a heat treatment can be performed in a vacuum at a temperature of 70°C to 200°C. Alternatively, a plasma treatment can be performed in an atmosphere containing oxygen. Alternatively, oxygen can be supplied to the insulating layer 105 by plasma treatment in an atmosphere containing an oxidizing gas such as nitrous oxide (N2O). Plasma treatment in an atmosphere containing nitrous oxide can suitably remove organic matter from the surface of the insulating layer 105 while supplying oxygen. After such treatment, it is preferable to continuously form the metal oxide film 108f without exposing the surface of the insulating layer 105 to the atmosphere.

[0309] Next, the metal oxide film 108f is processed into island-like structures to form the semiconductor layer 108 (Figure 9(D)). The semiconductor layer 108 can preferably be formed using a wet etching method. In this case, a portion of the region of the insulating layer 105 that does not overlap with the semiconductor layer 108 may be etched, resulting in a reduction in the thickness of that region. However, by using a material with a high selectivity ratio for the insulating layer 105 during the etching of the metal oxide film 108f, the reduction in the thickness of the insulating layer 105 can be suppressed.

[0310] A heat treatment (hereinafter also referred to as the first heat treatment) is performed before or after processing the metal oxide film 108f into island shapes. The first heat treatment can improve the crystallinity of the semiconductor layer 108 and reduce defects. In addition, the heat treatment can remove impurities contained in or adsorbed on the surface of the semiconductor layer 108. Furthermore, the first heat treatment can supply oxygen from the insulating layer 105 to the metal oxide film 108f or the semiconductor layer 108.

[0311] By performing the first heat treatment on a metal oxide film 108f with low crystallinity, crystallization can be induced and its crystallinity increased. Furthermore, the grain size of the crystal grains contained in the semiconductor layer 108 can be increased. Hydrogen contained in the metal oxide film is detached from the metal oxide film during crystallization. As a result, the hydrogen concentration in the metal oxide film after the first heat treatment decreases, and the hydrogen concentration in the semiconductor layer 108 can be reduced.

[0312] For the first heat treatment, a device that heats by heat conduction or thermal radiation from a heating element can be used. For the first heat treatment, an oven or a rapid thermal annealing (RTA) device can be used. As the RTA device, an LRTA (Lamp RTA) device that heats the workpiece by radiation of light (electromagnetic waves) emitted from a lamp can be used. Examples of such lamps include halogen lamps, metal halide lamps, xenon arc lamps, carbon arc lamps, high-pressure sodium lamps, and high-pressure mercury lamps. Alternatively, as the RTA device, a GRTA (Gas RTA) device that heats the workpiece using high-temperature gas can be used.

[0313] The temperature for the first heat treatment is preferably 100°C or higher but below the strain point of the substrate, more preferably 150°C or higher but 670°C or lower, more preferably 100°C or higher but 450°C or lower, more preferably 150°C or higher but 450°C or lower, more preferably 200°C or higher but 450°C or lower, more preferably 300°C or higher but 450°C or lower, and more preferably 350°C or higher but 450°C or lower. When an oven is used for the first heat treatment, a typical heat treatment at 350°C for 1 hour can be used. Furthermore, the processing time can be shortened by using an RTA device. The processing time is preferably 1 minute or more but 10 minutes or lower, more preferably 3 minutes or more but 10 minutes or lower, and more preferably 5 minutes or more but 10 minutes or lower. When using an RTA device and a short processing time is required, the heating temperature can be set to be above the strain point of the substrate. This can further shorten the processing time. When a GRTA device is used for the first heat treatment, a typical heat treatment at 650°C for 6 minutes can be used. In the first heat treatment, it is preferable that the substrate temperature falls within the aforementioned temperature range. However, the temperature in the first heat treatment is not limited to the aforementioned range.

[0314] The first heat treatment can be carried out in an atmosphere containing one or more noble gases, nitrogen, or oxygen. Dry air (CDA: Clean Dry Air) can be used as the atmosphere containing nitrogen or oxygen. It is preferable to carry out the first heat treatment in an atmosphere containing oxygen. Performing the first heat treatment in an atmosphere containing oxygen may enhance effects such as defect reduction and increased grain size. CDA can be suitably used as the atmosphere for the first heat treatment. It is preferable that the content of hydrogen, water, etc. in the atmosphere be kept to a minimum. It is preferable to use a high-purity gas with a dew point of -60°C or lower, preferably -100°C or lower, as the atmosphere. By using an atmosphere with a very low content of hydrogen, water, etc., it is possible to prevent hydrogen, water, etc. from being incorporated into the semiconductor layer 108 as much as possible.

[0315] Note that no heat treatment is performed at this stage; it can be combined with a heat treatment performed in a later step. Furthermore, a heat treatment in a later step (for example, a film deposition process) may also serve as the first heat treatment.

[0316] Next, an insulating film 106f is formed to cover the semiconductor layer 108 and the insulating layer 105, becoming the insulating layer 106 (Figure 9(E)). For the formation of the insulating film 106f, plasma CVD, sputtering, or ALD methods can be suitably used, for example.

[0317] By increasing the temperature during the formation of the insulating film 106f, a gate insulating layer with fewer defects can be obtained. However, if the temperature during the formation of the insulating film 106f is high, oxygen will be detached from the semiconductor layer 108, resulting in oxygen vacancies and V in the semiconductor layer 108. O In some cases, the amount of H may increase. The substrate temperature when forming the insulating layer 106 is preferably 180°C to 450°C, more preferably 200°C to 450°C, more preferably 250°C to 450°C, more preferably 300°C to 450°C, and more preferably 300°C to 400°C. By setting the substrate temperature when forming the insulating film 106f within the above range, defects in the insulating layer 106 can be reduced, and the detachment of oxygen from the semiconductor layer 108 can be suppressed. Therefore, a transistor with good electrical characteristics and high reliability can be obtained.

[0318] Before depositing the insulating film 106f, the surface of the semiconductor layer 108 can be subjected to plasma treatment. This plasma treatment can reduce impurities such as water adsorbed on the surface of the semiconductor layer 108. This reduces impurities at the interface between the semiconductor layer 108 and the insulating layer 106, enabling the realization of a highly reliable transistor. This is particularly suitable when the surface of the semiconductor layer 108 is exposed to the atmosphere between the formation of the semiconductor layer 108 and the deposition of the insulating film 106f. The plasma treatment can be performed in an atmosphere such as oxygen, ozone, nitrogen, nitrous oxide, or argon. Furthermore, it is preferable that the plasma treatment and the deposition of the insulating film 106f are performed continuously without exposure to the atmosphere.

[0319] After forming the insulating film 106f, a heat treatment (hereinafter also referred to as the second heat treatment) is performed. The second heat treatment can reduce defects in the insulating layer 106. In addition, the second heat treatment can remove impurities contained in or adsorbed on the surface of the insulating layer 106. For details on the second heat treatment, refer to the description of the first heat treatment. When an oven is used for the second heat treatment, the temperature of the second heat treatment is preferably 300°C to 500°C, and typically a heat treatment at 350°C for 1 hour can be used.

[0320] In the semiconductor layer 108, regions with low crystallinity (e.g., amorphous regions) may exist between crystal grains. In particular, if regions with low crystallinity exist in the channel formation region, there is a risk that the field-effect mobility of the transistor will decrease due to carrier scattering. By performing multiple heat treatments (here, the first heat treatment and the second heat treatment), the grain size of the crystal grains can be increased, and the regions with low crystallinity between crystal grains can be reduced. This makes it possible to create a transistor with high field-effect mobility. Furthermore, by performing multiple heat treatments, defects in the semiconductor layer 108 can be further reduced. In addition, impurities contained in the semiconductor layer 108 or adsorbed on its surface can be efficiently removed.

[0321] After the insulating film 106f is formed, oxygen can be supplied to the insulating film 106f. As a method of supplying oxygen, for example, ion implantation or plasma treatment can be used. Plasma treatment is preferably performed in an atmosphere containing oxygen. For example, plasma treatment is preferably performed in an atmosphere containing one or more of oxygen, nitrous oxide (N2O), nitrogen dioxide (NO2), carbon monoxide, and carbon dioxide. The amount of oxygen supplied can be adjusted, for example, by the power and treatment time in the plasma treatment.

[0322] It is preferable to deposit a film 139 on the insulating film 106f (Figure 9(E)). Sputtering is preferably used to deposit the film 139. By depositing the film 139 in an oxygen-containing atmosphere, oxygen can be supplied to the insulating film 106f.

[0323] The film 139 preferably contains oxygen, and oxides or oxiditrides can be suitably used. The conductivity of the film 139 is not required. At least one of an insulating film, a semiconductor film, and a conductive film can be used as the film 139. For example, the film 139 can be aluminum oxide, hafnium oxide, hafnium aluminate, indium oxide, indium gallium oxide, IGZO, ITO, or ITSO.

[0324] It is preferable to use a metal oxide containing one or more of the same elements as the semiconductor layer 108 as the film 139. In particular, it is preferable to use a metal oxide that is applicable to the semiconductor layer 108. By using the same material for film 139 as for the semiconductor layer 108, the equipment used for forming film 139 and the metal oxide film 108f can be shared, thereby reducing manufacturing costs.

[0325] When forming the film 139, the higher the oxygen flow rate ratio of the film-forming gas introduced into the processing chamber of the film-forming apparatus, or the higher the oxygen partial pressure inside the processing chamber, the greater the amount of oxygen supplied to the insulating film 106f. The oxygen flow rate ratio is preferably, for example, 50% to 100%, more preferably 60% to 100%, more preferably 70% to 100%, more preferably 80% to 100%, and more preferably 90% to 100%. Typically, the oxygen flow rate ratio can be set to 100%. Note that the oxygen flow rate ratio can be interpreted as the ratio of the oxygen partial pressure to the pressure inside the processing chamber.

[0326] Thus, by depositing the film 139 by sputtering in an oxygen-containing atmosphere, oxygen can be supplied to the insulating film 106f during the deposition of the film 139, while preventing oxygen from being released from the insulating film 106f. As a result, a large amount of oxygen can be trapped in the insulating film 106f. Then, a large amount of oxygen can be supplied to the semiconductor layer 108 by subsequent heat treatment. As a result, oxygen vacancies and V in the semiconductor layer 108 can be reduced. O This allows for a reduction in H, resulting in a transistor that exhibits good electrical characteristics and is highly reliable.

[0327] Furthermore, if there is too much oxygen in the insulating layer 106, defect levels may easily form at and near the interface between the semiconductor layer 108 and the insulating layer 106. In this case, if a high potential is applied to the conductive layer 104, which functions as the gate electrode, electrons, which are carriers, may be trapped in these defect levels, causing the transistor's threshold voltage to shift to the positive side and potentially reducing reliability. In such cases, it is preferable to lower the oxygen flow rate ratio or oxygen partial pressure during film formation of the film 139 to reduce the amount of oxygen supplied to the insulating film 106f. The oxygen flow rate ratio is preferably, for example, 10% to 60%, more preferably 20% to 60%, more preferably 30% to 60%, and more preferably 30% to 50%. This suppresses fluctuations in the threshold voltage, resulting in a highly reliable transistor.

[0328] It is preferable to perform a heat treatment (hereinafter also referred to as the third heat treatment) after forming the film 139. The third heat treatment allows for effective supply of oxygen from the insulating film 106f to the semiconductor layer 108. It also allows for supply of oxygen from the film 139 to the insulating film 106f. For details on the third heat treatment, refer to the description of the first heat treatment. When using an oven for the third heat treatment, a typical heat treatment at 350°C for 1 hour can be used.

[0329] After the film 139 is formed, or after the third heat treatment, oxygen can be supplied to the insulating film 106f via the film 139. For example, ion implantation or plasma treatment can be used as methods for supplying oxygen. For plasma treatment, please refer to the previous description.

[0330] Next, film 139 is removed. Removal of film 139 exposes the insulating film 106f. There are no particular limitations on the method for removing film 139, but a wet etching method can be suitably used. By using a wet etching method, etching of the insulating film 106f during the removal of film 139 can be suppressed. This prevents the thickness of the insulating film 106f from becoming thinner, and the thickness of the insulating layer 106 can be made uniform.

[0331] The process of supplying oxygen to the insulating film 106f is not limited to the methods described above. For example, ion implantation or plasma treatment can be used. Alternatively, a film that suppresses oxygen desorption can be formed on the insulating film 106f, and then oxygen can be supplied to the insulating film 106f through this film. It is preferable to remove the film after supplying oxygen. As the film that suppresses oxygen desorption mentioned above, a conductive film or semiconductor film having one or more of indium, zinc, gallium, tin, aluminum, chromium, tantalum, titanium, molybdenum, nickel, iron, cobalt, and tungsten can be used.

[0332] Next, a conductive film is deposited on the insulating film 106f. Then, the conductive layer 104 and the insulating layer 106f are processed to form a conductive layer 104 and an insulating layer 106 (Figure 10(A)). The conductive film can be deposited using, for example, sputtering, thermal CVD (including MOCVD), or ALD.

[0333] Next, the first element is supplied to the semiconductor layer 108 using the conductive layer 104 as a mask. As a result, regions 108P and 108Q are formed in the region of the semiconductor layer 108 that does not overlap with the conductive layer 104 (Figure 10(B)). Figure 10(B) schematically shows the supply of the first element to the semiconductor layer 108 with dashed arrows. When supplying the first element, it is preferable to determine the supply conditions for the first element by considering the material and thickness of the conductive layer 104 that acts as a mask, so that the first element is supplied as little as possible to the region of the semiconductor layer 108 that overlaps with the conductive layer 104. This makes it possible to lower the concentration of the first element in region 108i of the semiconductor layer 108 that overlaps with the conductive layer 104.

[0334] Furthermore, the first element can be supplied before removing the resist mask used to form the conductive layer 104 and the insulating layer 106. By supplying the first element to the semiconductor layer 108 using the resist mask and the conductive layer 104 as a mask, regions 108P and 108Q can be formed. After that, the resist mask is removed.

[0335] In the transistor 100F shown in Figure 6(C), etc., an insulating layer 106 is provided on regions 108R and 108S, so the amount of the first element supplied to these regions is less than the amount supplied to regions 108P and 108Q. In addition, in the transistor 100E shown in Figure 6(A), etc., after forming the insulating layer 106 and the conductive layer 104, the first element can be supplied to the semiconductor layer 108 using the conductive layer 104 as a mask. In this case, the first element is supplied to regions 108P and 108Q via the insulating layer 106.

[0336] Next, an insulating film 195f is formed to cover the conductive layer 104, the insulating layer 106, and the semiconductor layer 108, forming the insulating layer 195 (Figure 10(C)). Plasma CVD can be suitably used to form the insulating film 195f.

[0337] If the deposition temperature of the insulating film 195f is too high, the first element contained in regions 108P and 108Q may diffuse into the peripheral region including the channel-forming region. Furthermore, the electrical resistance of regions 108P and 108Q may increase. Therefore, it is preferable to determine the deposition temperature of the insulating film 195f considering the diffusion of the first element.

[0338] The deposition temperature for the insulating film 195f is preferably, for example, 150°C to 400°C, more preferably 180°C to 360°C, and more preferably 200°C to 250°C. By depositing the insulating film 195f at a low temperature, a transistor with good electrical characteristics can be obtained even with a short channel length.

[0339] After the formation of the insulating film 195f, a heat treatment can be performed. This heat treatment may further reduce the electrical resistance of regions 108P and 108Q. For details on the heat treatment, please refer to the previous description. Note that if the heat treatment temperature is too high (e.g., above 500°C), the first element may diffuse into the channel formation region, potentially leading to a decrease in the electrical characteristics and reliability of the transistor. Note that heat treatment is not required at this stage. Alternatively, heat treatment can be omitted and combined with a heat treatment performed in a later step. Furthermore, if there is a heat treatment in a later step (e.g., a film deposition process), this heat treatment may also be combined with that process.

[0340] Next, a portion of the insulating film 195f is removed to form openings 147a and 147b that reach regions 108P and 108Q (Figure 10(D)). This forms the insulating layer 195. For example, a dry etching method can be suitably used to form openings 147a and 147b.

[0341] Next, conductive layers 112a and 112b are formed to cover openings 147a and 147b (Figure 10(D)).

[0342] Next, an insulating layer 218 is formed on the insulating layer 195, conductive layer 112a, and conductive layer 112b (Figures 3(A) and 3(B)). Plasma CVD can be suitably used to form the inorganic insulating layer of the insulating layer 218.

[0343] By following the above steps, a semiconductor device 10B according to one aspect of the present invention can be manufactured.

[0344] <Example of manufacturing method 2> This section describes a manufacturing method that differs from the manufacturing method example 1 described above. Note that some parts that overlap with manufacturing method example 1 may be omitted from the explanation.

[0345] First, the insulating layer 105 is formed in the same manner as in example 1 of the manufacturing method (Figure 9(A)).

[0346] As mentioned above, if the hydrogen concentration in the insulating layer 105 after film formation is high, a large amount of hydrogen will diffuse from the insulating layer 105 to the metal oxide film 108f, which may result in a high hydrogen concentration in the semiconductor layer 108. In such cases, it is preferable to perform a heat treatment (hereinafter also referred to as the fourth heat treatment) after the insulating layer 105 has been formed but before the metal oxide film 108f has been formed. This will lower the hydrogen concentration in the insulating layer 105 and reduce the amount of hydrogen that diffuses from the insulating layer 105 to the metal oxide film 108f. Furthermore, the fourth heat treatment can reduce defects in the insulating layer 105. For details on the fourth heat treatment, please refer to the description related to the first heat treatment.

[0347] The temperature of the fourth heat treatment is preferably 100°C or higher but below the strain point of the substrate, more preferably 150°C or higher but 670°C or lower, more preferably 100°C or higher but 450°C or lower, more preferably 150°C or higher but 450°C or lower, more preferably 200°C or higher but 450°C or lower, more preferably 300°C or higher but 450°C or lower, and more preferably 350°C or higher but 450°C or lower. When an oven is used for the fourth heat treatment, a typical heat treatment at 350°C for 1 hour can be used. When a GRTA apparatus is used for the fourth heat treatment, a typical heat treatment at 650°C for 6 minutes can be used. In the fourth heat treatment, it is preferable that the substrate temperature is within the above temperature range. However, the temperature in the fourth heat treatment is not limited to the above range.

[0348] Next, a metal oxide film 108f is formed on the insulating layer 105 (Figure 9(C)). For the steps after the formation of the metal oxide film 108f, please refer to the descriptions in Figures 9(C) to 10(D).

[0349] By following the above steps, a semiconductor device 10B according to one aspect of the present invention can be manufactured.

[0350] <Example of manufacturing method 3> A different manufacturing method from the aforementioned manufacturing method examples 1 and 2 will be explained using Figure 11. Figure 11 shows side by side the cross-sectional view between the dashed lines A1-A2 shown in Figure 3(A) and the cross-sectional view between the dashed lines B1-B2 shown in Figure 3(B). Note that explanations of parts that overlap with manufacturing method example 1 may be omitted.

[0351] First, the insulating layer 105 is formed in the same manner as in example 1 of the manufacturing method (Figure 9(A)).

[0352] As mentioned above, if the hydrogen concentration in the insulating layer 105 after film formation is low, less hydrogen will diffuse from the insulating layer 105 to the metal oxide film 108f, which may result in increased crystallinity of the metal oxide film 108f after film formation. In such cases, it is preferable to perform plasma treatment in an atmosphere containing a hydrogen-containing gas (e.g., H2) after the insulating layer 105 has been formed but before the metal oxide film 108f has been formed. Figure 11 schematically shows how hydrogen is supplied to the insulating layer 105 with dashed arrows. The method of supplying hydrogen is not limited to plasma treatment; ion implantation or treatment utilizing thermal diffusion by heating can also be used. For information on the hydrogen supply method, please refer to the description related to the first element supply method. For example, a plasma CVD apparatus can be used for film formation of the insulating layer 105 and for supplying hydrogen to the insulating layer 105. This allows the film formation of the insulating layer 105 and the supply of hydrogen to be performed continuously within the plasma CVD apparatus, thereby increasing productivity. For example, after forming an insulating layer 105 using a plasma CVD apparatus, hydrogen can be supplied to the insulating layer 105 by performing plasma treatment in the same processing chamber in an atmosphere containing a hydrogen element gas (e.g., H2 or NH3).

[0353] Next, a metal oxide film 108f is formed on the insulating layer 105 (Figure 9(C)). For the steps after the formation of the metal oxide film 108f, please refer to the descriptions in Figures 9(C) to 10(D).

[0354] By following the above steps, a semiconductor device 10B according to one aspect of the present invention can be manufactured.

[0355] This embodiment can be combined with other embodiments as appropriate. Furthermore, if multiple configuration examples are shown within a single embodiment in this specification, these configuration examples can be combined as appropriate.

[0356] (Embodiment 2) This embodiment describes an indium oxide film that can be used in the semiconductor layer of a transistor in a semiconductor device according to one aspect of the present invention.

[0357] In this specification, indium oxide having at least a crystalline portion or crystalline region in the film is referred to as crystalline indium oxide (crystal IO) or crystalline indium oxide (crystalline IO). Examples of crystal IO or crystalline IO include single-crystal indium oxide, polycrystalline indium oxide, and microcrystalline indium oxide.

[0358] Indium oxide is a semiconductor material with completely different physical properties from oxide semiconductors such as In-Ga-Zn oxide (hereinafter also referred to as IGZO) and zinc oxide.

[0359] This section describes the carrier concentration dependence of the hole mobility of indium oxide, silicon, and IGZO. Figure 12(A) shows silicon (Si) and indium oxide (InO X Figure 12(B) is a schematic diagram of the carrier concentration dependence of hole mobility for IGZO.

[0360] First, as indicated by the arrows in Figure 12(B), IGZO tends to exhibit higher hole mobility as the carrier concentration increases. On the other hand, as indicated by the arrows in Figure 12(A), indium oxide tends to exhibit higher hole mobility as the carrier concentration decreases (see Non-Patent Literature 4). This trend is similar to that of silicon, where the lower the concentration of dopants (impurities) in the material, the less impurity scattering occurs and the higher the hole mobility. In other words, the higher the purity and intrinsic nature of indium oxide, the higher its hole mobility. From these results, it can be said that indium oxide, unlike IGZO, is a material with physical properties similar to silicon. Note that the properties of indium oxide shown in Figure 12(A) are assumed to be those of a single crystal. Therefore, when indium oxide is not a single crystal (for example, polycrystalline), the properties may differ from those shown in Figure 12(A).

[0361] In Figure 12(A), the low carrier concentration range R1 exhibits extremely high hole mobility, making it a suitable carrier concentration range for, for example, the channel formation region of a transistor. For example, in the case of indium oxide, the range R1 is such that the carrier concentration value is 1 × 10⁻⁶. 15 cm -3 This range includes, for example, 1 × 10 14 cm -3 The above is 1 x 10 18 cm -3 The range is as follows: By sufficiently reducing the carrier concentration, the hole mobility value can be increased to 270 cm⁻¹. 2 It can be expected to be raised to the level of (V·s).

[0362] Furthermore, in indium oxide, the region where the carrier concentration is within the range R1 may contain elements that lower the carrier concentration. Examples of elements that lower the carrier concentration include magnesium, calcium, zinc, cadmium, and copper. By substituting these elements for indium, the carrier concentration can be lowered. Other elements that lower the carrier concentration include nitrogen, phosphorus, arsenic, and antimony. For example, by substituting nitrogen, phosphorus, arsenic, or antimony for oxygen, the carrier concentration can be lowered.

[0363] Elements that reduce carrier concentration can also be called elements that confer p-type properties. Adding elements that reduce carrier concentration to an indium oxide film can make the indium oxide film more easily i-type or substantially i-type. In this case, the concentration of the above-mentioned carrier-reducing element in the indium oxide film is 1 × 10⁻⁶ 16 atoms / cm 3 The above 8 x 10 20 atoms / cm 3 The following is preferable: 1 × 10 16 atoms / cm 3 The above 4 x 10 20 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 8 x 10 19 atoms / cm 3The following is more preferred, 1×10 16 atoms / cm 3 or more and 5×10 19 atoms / cm 3 or less is even more preferred. By setting such a concentration, the carrier concentration can be lowered while maintaining the crystal structure of indium oxide.

[0364] On the other hand, the high carrier concentration range R2 has low electric resistance, and can be said to be a carrier concentration range suitable for, for example, the source region and drain region of a transistor, a resistor, or a transparent conductive film. The range R2 is a range including a carrier concentration value of 1×10 20 cm -3 , and is, for example, a range of 1×10 19 cm -3 or more and 1×10 22 cm -3 or less. By making the carrier concentration sufficiently high, it is expected that the resistivity can be reduced to 1×10 -4 Ω·cm or less.

[0365] Note that in indium oxide, the region where the carrier concentration is in the range R2 can contain an element that increases the carrier concentration. For example, it is preferable to contain an element common to the source electrode and the drain electrode of the transistor. Examples of the element that increases the carrier concentration include titanium, zirconium, hafnium, tantalum, tungsten, molybdenum, tin, silicon, and boron. In particular, it is more preferable to use an element whose oxide has conductivity or semiconductivity. As a method for supplying the element that increases the carrier concentration, a method of forming a film containing the element and diffusing the element, an ion implantation method, an ion doping method, a plasma immersion ion implantation method, or plasma treatment can be used. Note that in this specification and the like, unless otherwise specified, the presence or absence of mass separation is not limited.

[0366] The element that increases the carrier concentration can also be referred to as an element that imparts n-type conductivity. The concentration of the element that increases the carrier concentration in the indium oxide film is 1×10 16 atoms / cm 3 or more and 8×1020 atoms / cm 3 or less is preferable, and 1×10 16 atoms / cm 3 or more and 4×10 20 atoms / cm 3 or less is more preferable, and 1×10 16 atoms / cm 3 or more and 8×10 19 atoms / cm 3 or less is still more preferable. By setting such a concentration, the carrier concentration can be increased while maintaining the crystal structure of indium oxide. Note that antimony may also function as an element that increases the carrier concentration. 16 atoms / cm 3 or more and 5×10 19 atoms / cm 3 or less is even more preferable. By setting such a concentration, the carrier concentration can be increased while maintaining the crystal structure of indium oxide. Note that antimony may also function as an element that increases the carrier concentration.

[0367] As described above, since indium oxide is an oxide whose valence electron can be controlled, the threshold voltage of a transistor using a semiconductor layer containing indium oxide can be controlled. Further, in indium oxide, a region with a low carrier concentration can be used for a channel formation region of a transistor, and a region with a high carrier concentration can be used for a source region and a drain region of the transistor. Note that in IGZO, strain may be formed in the source region and the drain region due to stress of an electrode in contact with IGZO, so that an n-type region may be formed. On the other hand, unlike IGZO, indium oxide allows valence electron control, so that strain does not need to be formed in the film unlike IGZO. When the strain in the film is small, improvement in reliability can be expected. For example, a so-called n-i-n junction (a junction of an n-type region, an i-type region, and an n-type region) can be formed by separately forming a region whose carrier concentration is in the range R1 shown in FIG. 12(A) and a region whose carrier concentration is in the range R2 in the indium oxide film. Note that valence electron control in a transistor using silicon is generally known. On the other hand, valence electron control in a transistor using indium oxide is a novel technical idea that cannot be usually conceived.

[0368] By applying the above technical concept, the indium oxide transistor described herein has two or more, preferably three or more, more preferably four or more, and most preferably five of the following features (1) to (5): (1) High on-current (in other words, high mobility). (2) Low off-current. (3) Normally off is possible. (4) High reliability. (5) High cutoff frequency (fT). For example, the indium oxide transistor described herein has high mobility, low off-current, and is normally off. This transistor is different from a transistor that is high mobility and normally on.

[0369] In addition, a semiconductor being i-type means that the Fermi level (Ef) and the intrinsic Fermi level (Ei) are the same (Ef=Ei). As shown in Figure 12(B), in IGZO, the lower the carrier concentration, the lower the hole mobility. Therefore, when Ef=Ei is reached, there are no carriers left (in other words, the material has properties similar to an insulator), and it may cease to function as a transistor. On the other hand, in indium oxide, as shown in Figure 12(A), the lower the carrier concentration, the higher the hole mobility, and when Ef=Ei is reached, the hole mobility is maximized. That is, transistors containing indium oxide can achieve high field-effect mobility by setting Ef=Ei. Furthermore, transistors containing indium oxide tend to be normally off due to their low carrier concentration. Therefore, transistors containing indium oxide can be normally off and achieve high field-effect mobility.

[0370] Normally off refers to the state in which no current flows through a transistor when no potential is applied to the gate or when the gate-source voltage is 0V. Normally off can be evaluated using the transistor's threshold voltage (Vth) or shift value (Vsh). Unless otherwise specified, Vth will be calculated using the constant current method. More specifically, Vth is the value of drain current (Id) × channel length (L) ÷ channel width (W) in the transistor's Id-Vg characteristic, where Vth is 1nA (1 × 10⁻¹⁰). -9 Let Vg be the gate voltage (Vg) when A) is true. Also, Vsh is defined as the tangent to the maximum slope when the drain current (Id) in the Id-Vg characteristic of the transistor is expressed logarithmically, and Id = 1pA (1 × 10⁻¹⁰). -12 Vg is the gate voltage (Vg) at the intersection with line A), or the Vg at the intersection of the line extrapolated from the two points where the slope of Id is maximized when Id is expressed logarithmically in the transistor's Id-Vg characteristic, and the line where Id = 1 pA. For example, if either Vth or Vsh, or both, are zero or positive, it can be considered a normally-off transistor.

[0371] In transistors containing indium oxide, the film configuration in contact with the indium oxide film is crucial for achieving an i-type semiconductor, i.e., Ef=Ei. For example, in transistors containing indium oxide, a film configuration can be obtained in which a silicon oxide film, a hafnium oxide film, and a silicon nitride film are stacked in contact with the indium oxide film. This film configuration allows for a semiconductor device that is both Ef=Ei and highly reliable.

[0372] Furthermore, in the above film configuration, oxygen-containing films such as silicon oxide-nitride films, silicon oxide nitride films, aluminum oxide films, and gallium oxide films can be used instead of the silicon oxide film. Also, in the above film configuration, silicon oxide nitride films, silicon oxide nitride films, etc. can be used instead of the silicon nitride film. In addition, the hafnium oxide film located on the indium oxide side of the silicon nitride film functions as a hydrogen gettering site.

[0373] The above film configuration can also be understood as a layered structure consisting of a film that can supply oxygen to the indium oxide film (e.g., a silicon oxide film), a film that can getter hydrogen (e.g., a hafnium oxide film), and a film that suppresses the intrusion of oxygen and hydrogen (e.g., a silicon nitride film), from the indium oxide film side. With this configuration, oxygen deficiencies in the indium oxide film are compensated for by oxygen in the silicon oxide film. In addition, hydrogen in the indium oxide film is captured by the hafnium oxide film through heat treatment or other means. Furthermore, by providing a silicon nitride film, the film configuration becomes one in which oxygen and hydrogen are less likely to intrude from the outside. In other words, by adopting the above film configuration, the indium oxide film can be made closer to type i. Therefore, transistors having the above indium oxide film have high field-effect mobility and high reliability.

[0374] Next, we will describe indium oxide films applied to transistors. Indium oxide films are preferably crystalline (i.e., they have crystal grains). Examples of films with crystal grains include single-crystal films, polycrystalline films, or amorphous films (also called microcrystalline films) containing crystal grains. In particular, polycrystalline films are preferred for indium oxide films, and single-crystal films are more preferred. Single-crystal films do not have crystal grain boundaries. Impurities that inhibit carrier flow (typically insulating impurities, insulating oxides, etc.) tend to segregate at crystal grain boundaries. By using a single-crystal film, carrier scattering at crystal grain boundaries can be suppressed, enabling the realization of transistors with high field-effect mobility. Furthermore, it offers excellent effects such as suppressing variations in transistor characteristics caused by these crystal grain boundaries.

[0375] Polycrystalline films are preferred over microcrystalline or amorphous films because they can reduce carrier scattering and exhibit high field-effect mobility. When using polycrystalline films, it is preferable to use films with the largest possible grain size and few grain boundaries. In a transistor to which a polycrystalline indium oxide film is applied, if there are no grain boundaries in the channel formation region, or if no grain boundaries are observed, the channel formation region is located within the single-crystal region contained in the polycrystalline film, and therefore it can be considered a transistor to which single-crystal indium oxide is applied.

[0376] In this specification, a semiconductor layer in which no grain boundaries are observed in the channel-forming region, a semiconductor layer in which the channel-forming region is contained within a single crystal grain, or a semiconductor layer in which the direction of the crystal axes is the same in at least two regions within the channel-forming region can be called a single crystal film. Furthermore, a semiconductor layer in which, within a single crystal grain in the channel-forming region, the direction of other crystal axes changes continuously with respect to a certain crystal axis or crystal orientation as the axis of rotation can also be called a single crystal film.

[0377] The channel formation region refers to the region of the semiconductor layer that overlaps with (or faces) the gate electrode via the gate insulating layer, and is located between the region in contact with the source electrode and the region in contact with the drain electrode. The current path in the channel formation region is the shortest distance between the source electrode and the drain electrode. Therefore, the crystal grains, grain boundaries, crystal axes, and crystal orientation in the channel formation region can be confirmed by cross-sectional observation in the channel length direction of the semiconductor layer (for example, cross-sectional observation including the semiconductor layer, source electrode, and drain electrode).

[0378] Furthermore, the indium oxide film may contain elements that can become trivalent cations like indium, as long as their crystals maintain a cubic crystal structure (Bixbite type). Examples include Group 13 elements of the periodic table such as gallium and aluminum, and Group 3 elements of the periodic table. Since the bonding force of these elements is stronger than that of indium and oxygen, adding these elements to the indium oxide film can reduce oxygen vacancies (V) in the indium oxide film.O This can suppress the formation of ions. Furthermore, since these elements mainly exist as trivalent cations in oxides, the carrier concentration of the indium oxide film can be kept low. Therefore, it becomes possible to shift the threshold voltage of the transistor to the positive side. Also, normally-off becomes possible. Thus, a transistor with good electrical characteristics can be provided.

[0379] The concentration of the above elements in the indium oxide film is 1 × 10⁻⁶ 16 atoms / cm 3 The above 8 x 10 20 atoms / cm 3 The following is preferable: 1 × 10 16 atoms / cm 3 The above 4 x 10 20 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 8 x 10 19 atoms / cm 3 The following is more preferable: 1 × 10 16 atoms / cm 3 The above 5 x 10 19 atoms / cm 3 The following are even more preferable.

[0380] Furthermore, the elements that impart n-type, p-type, and trivalent cations mentioned above can be added to the indium oxide film by methods such as ion doping, ion implantation, and thermal diffusion. Alternatively, the elements that impart n-type, p-type, and trivalent cations mentioned above can be added to the sputtering target, deposition gas, ALD deposition precursor, etc., when depositing the indium oxide film. Alternatively, the elements that impart n-type, p-type, and trivalent cations mentioned above can be auto-doped from the chamber used when depositing the indium oxide film. Auto-doping refers to the automatic addition of elements contained in the chamber components, etc., into the indium oxide film during deposition.

[0381] By using such an indium oxide film in a transistor, the field-effect mobility of the transistor can be increased to 50 cm². 2 / (V·s) or more, preferably 100cm 2 (V·s) or more, more preferably 150cm 2 / (V·s) or more, more preferably 200cm 2 / (V·s) or more, more preferably 250cm 2 It can be set to (V·s) or more.

[0382] One of the characteristics of indium oxide films is that they have higher oxygen permeability (diffusivity) compared to IGZO films. As shown in Figure 12(C), indium oxide films (InO X Oxygen (O) diffusing into an oxygen vacancy (V) permeates the indium oxide membrane and is released as oxygen molecules (O2). It may also be released as water molecules (H2O) by reacting with hydrogen contained in the membrane. Furthermore, oxygen vacancies (V) in the membrane... O If oxygen atoms are present, diffusing oxygen atoms will fill the oxygen deficiency. Indium oxide films can be said to be more efficient at filling oxygen deficiencies compared to IGZO films because oxygen diffuses easily.

[0383] Thus, because indium oxide films are more prone to reducing oxygen vacancies in the film compared to IGZO films, applying such indium oxide films to transistors makes it possible to realize transistors with extremely high reliability.

[0384] As shown in Figure 12(C), the indium oxide film diffuses hydrogen. Hydrogen diffusing into the indium oxide film from the outside permeates the film and is released as hydrogen molecules (H2). Alternatively, it reacts with oxygen contained in the film and is released as water molecules. The above-mentioned oxygen and hydrogen diffuse through the indium oxide film by heat treatment. The temperature of this heat treatment is 200°C to 700°C, preferably 350°C to 650°C, and more preferably 400°C to 500°C.

[0385] A transistor using an indium oxide film is a storage-type transistor that uses electrons as the majority carrier. Assuming that the carrier relaxation time is constant, the smaller the effective mass of electrons (carriers), the higher the electron mobility. In other words, by using indium oxide, which has a small effective mass of electrons, in a transistor, the on-current or field-effect mobility of the transistor can be increased.

[0386] Table 1 shows the effective masses of single-crystal indium oxide (here, In2O3) and single-crystal silicon (Si). As shown in Table 1, indium oxide is characterized by a small effective electron mass and a large effective hole mass. Furthermore, the effective electron mass of indium oxide is almost independent of the crystal orientation. Therefore, by using crystalline indium oxide in transistors, transistors with high field-effect mobility and high frequency characteristics (also called f-response) can be realized. In addition, because of the large effective hole mass, transistors with extremely low off-currents can be realized. For example, by applying an indium oxide film to a vertical transistor, the off-current per 1 μm of channel width is 1 fA (1 × 10⁻¹⁶) at 125°C. -15 A) Less than or equal to, or 1aA(1 × 10 -18 A) is less than or equal to 1aA(1 × 10) under room temperature (25°C) conditions. -18 A) Less than or equal to 1zA(1×10) -21 A) The following is possible. Furthermore, as shown in Table 1, indium oxide has a smaller effective electron mass and a larger effective hole mass than silicon, so it may be possible to realize a transistor with higher field-effect mobility and lower off-current than a Si transistor.

[0387] [Table 1]

[0388] It is preferable to provide a seed layer so as to be in contact with at least a portion of the crystalline indium oxide film. It is preferable to use a material containing crystals with a small difference in lattice constant (also called lattice mismatch) with the indium oxide for the seed layer. This can improve the crystallinity of the indium oxide film. A substrate (for example, a single-crystal substrate) may be used as one of the layers in contact with at least a portion of the crystalline indium oxide film.

[0389] One method for evaluating the degree of lattice mismatch is to use the following lattice mismatch value. The lattice mismatch Δa [%] between the crystals of the seed layer and the crystals of the formed film (indium oxide film in this case) is calculated as Δa = ((L1 - L2) / L2) × 100. Here, L1 is the length of the unit cell vector or lattice constant of the crystals of the formed film, and L2 is the length of the unit cell vector or lattice constant of the crystals of the seed layer.

[0390] The lattice mismatch Δa between the seed layer and the indium oxide film is preferably small in absolute value, and most preferably 0. For example, Δa can be -5% or more and 5% or less, preferably -4% or more and 4% or less, more preferably -3% or more and 3% or less, and even more preferably -2% or more and 2% or less.

[0391] Here, the indium oxide crystal has a cubic structure (bixbite type). For example, yttria-stabilized zirconia (YSZ) crystals can have a cubic structure (fluorite type). The lattice mismatch of the indium oxide crystal with respect to the cubic YSZ crystal is in the range of -2% to 2%, and a single crystal film of indium oxide can be epitaxially grown on a YSZ substrate.

[0392] Furthermore, the crystal structure of the seed layer and the crystal structure of the indium oxide film do not necessarily have to be the same in terms of crystal system or crystal orientation. For example, a film with a hexagonal or trigonal crystal structure can be used beneath an indium oxide film with a cubic crystal structure. For instance, by setting the crystal orientation of the surface of the seed layer to

[0001] and the crystal orientation of the underside of the indium oxide film to

[0111] , the requirements related to crystal orientation necessary for epitaxial growth can be met. Examples of hexagonal or trigonal crystals include wurtzite-type structures, YbFe2O4-type structures, Yb2Fe3O7-type structures, and modified forms thereof. IGZO is an example of a crystal having a YbFe2O4-type or Yb2Fe3O7-type structure. Indium oxide single-crystal films can be formed not only on YSZ substrates but also on insulating films. On the other hand, it is difficult to form silicon single-crystal films on insulating films. Silicon crystals have a diamond structure. Thus, in terms of being a single crystal, indium oxide and silicon have similar properties. On the other hand, when comparing indium oxide and silicon from the perspective of whether they can form a single crystal on an insulating film, they have different properties.

[0393] This embodiment can be implemented in appropriate combination with other embodiments described herein, at least in part.

[0394] (Embodiment 3) In this embodiment, a display device according to one aspect of the present invention will be described with reference to Figures 13(A) to 23.

[0395] The display device of this embodiment can be a high-resolution display device or a large-screen display device. Therefore, the display device of this embodiment can be used in electronic devices with relatively large screens, such as television equipment, desktop or notebook computers, computer monitors, digital signage, and large game machines such as pachinko machines, as well as in the display units of digital cameras, digital video cameras, digital photo frames, mobile phones, portable game consoles, personal information terminals, and audio playback devices.

[0396] The display device of this embodiment can be a high-definition display device. Therefore, the display device of this embodiment can be used, for example, as a display unit for information terminals (wearable devices) such as wristwatches and bracelets, and as a display unit for wearable devices that can be worn on the head, such as VR devices such as head-mounted displays (HMDs) and AR devices such as glasses.

[0397] A semiconductor device according to one aspect of the present invention can be used as a display device or a module having said display device. Examples of modules having said display devices include a module to which a connector such as a flexible printed circuit board (FPC) or TCP (Tape Carrier Package) is attached, and a module on which an integrated circuit (IC) is mounted using the COG (Chip On Glass) method or COF (Chip On Film) method.

[0398] The display device of this embodiment may also function as a touch panel. For example, the display device can be fitted with various detection elements (also called sensor elements) that can detect the proximity or contact of an object to be detected, such as a finger.

[0399] Examples of sensor types include capacitive, resistive, surface acoustic wave, infrared, optical, and pressure-sensitive sensors.

[0400] Examples of capacitance methods include surface capacitance and projected capacitance. Furthermore, projected capacitance methods include self-capacitance and mutual capacitance. Mutual capacitance is preferable because it enables simultaneous multi-point detection.

[0401] Examples of touch panels include out-cell, on-cell, and in-cell types. An in-cell touch panel refers to a configuration in which electrodes constituting the sensing element are provided on one or both of the substrate supporting the display element and the opposing substrate.

[0402] <Example of display device configuration 1> Figure 13(A) shows a perspective view of the display device 50A.

[0403] The display device 50A has a configuration in which substrate 152 and substrate 151 are bonded together. In Figure 13(A), substrate 152 is shown with a dashed line.

[0404] The display device 50A includes a display unit 162, a connection unit 140, a circuit unit 164, a conductive layer 165, etc. Figure 13(A) shows an example in which IC 173 and FPC 172 are mounted on the display device 50A. Therefore, the configuration shown in Figure 13(A) can also be described as a display module having the display device 50A, an IC, and an FPC.

[0405] The connection portion 140 is provided on the outside of the display unit 162. The connection portion 140 can be provided along one or more sides of the display unit 162. There may be one or more connection portions 140. Figure 13(A) shows an example in which the connection portion 140 is provided so as to surround all four sides of the display unit 162. The connection portion 140 connects the common electrode of the display element to the conductive layer, and can supply potential to the common electrode.

[0406] The circuit section 164 may include, for example, a scan line drive circuit (also called a gate driver). Alternatively, the circuit section 164 may include both a scan line drive circuit and a signal line drive circuit (also called a source driver).

[0407] The circuit section 164 can utilize various circuits, including shift register circuits, level shifter circuits, inverter circuits, latch circuits, analog switch circuits, demultiplexer circuits, and logic circuits. The circuit section 164 can also utilize transistors and capacitive elements. The transistors in the circuit section 164 can be formed using the same process as the transistors in the pixel circuit.

[0408] The conductive layer 165 has the function of supplying signals and power to the display unit 162 and the circuit unit 164. These signals and power are input to the conductive layer 165 from an external source via the FPC 172, or from the IC 173.

[0409] Figure 13(A) shows an example in which IC173 is provided on the substrate 151 using the COG method. IC173 can be an IC that has, for example, one or both of a scan line drive circuit and a signal line drive circuit. Note that the display device 50A and the display module may be configured without an IC. Alternatively, the IC may be mounted on the FPC using the COF method or the like.

[0410] A semiconductor device according to one aspect of the present invention can be applied, for example, to one or both of the display unit 162 and the circuit unit 164 of a display device 50A. Oxide semiconductors (OS) can preferably be used in the channel formation region of the transistors in the display device. By using OS transistors, a display device with low power consumption can be made. Furthermore, the semiconductor device according to one aspect of the present invention can be used in both the display unit 162 and the circuit unit 164, that is, all of the transistors in the display device can be OS transistors. By making all of the transistors in the display device OS transistors in this way, the manufacturing cost can be kept low.

[0411] For example, when a semiconductor device according to one aspect of the present invention is applied to the pixel circuit of a display device, the occupied area of ​​the pixel circuit can be reduced, resulting in a high-definition display device. Also, for example, when a semiconductor device according to one aspect of the present invention is applied to the drive circuit of a display device (for example, one or both of a gate line drive circuit and a source line drive circuit), the occupied area of ​​the drive circuit can be reduced, resulting in a narrow-bezel display device. Furthermore, because the semiconductor device according to one aspect of the present invention has good electrical characteristics, its use in a display device can improve the reliability of the display device.

[0412] The display unit 162 is the area in the display device 50A that displays images, and has a plurality of pixels 201 arranged periodically. Figure 13(A) shows a magnified view of one pixel 201.

[0413] There are no particular limitations on the pixel arrangement in the display device of this embodiment, and various methods can be applied. Examples of pixel arrangements include stripe arrangements, S-stripe arrangements, matrix arrangements, delta arrangements, Bayer arrangements, and pentile arrangements.

[0414] Pixel 201, shown in Figure 13(A), has sub-pixels 11R that emit red light, sub-pixel 11G that emits green light, and sub-pixel 11B that emits blue light. Note that sub-pixels 11R, 11G, and 11B are sometimes collectively referred to as sub-pixel 11. Furthermore, the number of sub-pixels a single pixel may have is not particularly limited.

[0415] Each sub-pixel 11R, 11G, and 11B comprises a display element and a pixel circuit that controls the driving of the display element.

[0416] Various elements can be used as display elements, such as liquid crystal elements and light-emitting elements. In addition, display elements using shutter-type or optical interference-type MEMS (Micro Electro Mechanical Systems) elements, microcapsule-type, electrophoretic-type, electrowetting-type, or electronic powder fluid (registered trademark)-type elements can also be used. Furthermore, QLED (Quantum-dot LED) using a light source and color conversion technology using quantum dot materials can also be used.

[0417] Examples of display devices using liquid crystal elements include transmissive liquid crystal display devices, reflective liquid crystal display devices, and semi-transmissive liquid crystal display devices.

[0418] Modes that can be used in display devices using liquid crystal elements include, for example, Vertical Alignment (VA) mode, FFS (Fringe Field Switching) mode, IPS (In-Plane-Switching) mode, TN (Twisted Nematic) mode, ASM (Axially Symmetric aligned Micro-cell) mode, OCB (Optically Compensated Birefringence) mode, FLC (Ferroelectric Liquid Crystal) mode, AFLC (AntiFerroelectric Liquid Crystal) mode, ECB (Electrically Controlled Birefringence) mode, and guest-host mode. Examples of VA modes include MVA (Multi-Domain Vertical Alignment) mode, PVA (Patterned Vertical Alignment) mode, and ASV (Advanced Super View) mode.

[0419] Examples of liquid crystal materials that can be used in liquid crystal elements include thermotropic liquid crystals, low molecular weight liquid crystals, polymer liquid crystals, polymer dispersed liquid crystals (PDLC), polymer network liquid crystals (PNLC), ferroelectric liquid crystals, and antiferroelectric liquid crystals. Depending on the conditions, these liquid crystal materials exhibit cholesteric phases, smectic phases, cubic phases, chiral nematic phases, isotropic phases, blue phases, etc. Furthermore, either positive-type or negative-type liquid crystals may be used as the liquid crystal material, and can be selected according to the applied mode or design.

[0420] Examples of light-emitting elements include self-emissive light-emitting elements such as LEDs (Light Emitting Diodes), OLEDs (Organic LEDs), and semiconductor lasers. For example, mini-LEDs and micro-LEDs can be used as LEDs.

[0421] Examples of light-emitting materials for light-emitting devices include fluorescent materials, phosphorescent materials, thermally activated delayed fluorescence (TADF) materials, and inorganic compounds (such as quantum dot materials).

[0422] Examples of quantum dot materials include colloidal quantum dots, alloy quantum dots, core-shell quantum dots, and core quantum dots. Furthermore, quantum dot materials containing elemental groups such as Group 2 and Group 16, Group 13 and Group 15, Group 13 and Group 17, Group 11 and Group 17, or Group 14 and Group 15 can be used. Alternatively, quantum dot materials containing elements such as cadmium (Cd), selenium (Se), zinc (Zn), sulfur (S), phosphorus (P), indium (In), tellurium (Te), lead (Pb), gallium (Ga), arsenic (As), and aluminum (Al) can be used.

[0423] The light-emitting element can emit light in the following colors: infrared, red, green, blue, cyan, magenta, yellow, or white. Furthermore, the color purity can be improved by adding a microcavity structure to the light-emitting element.

[0424] Of the pair of electrodes in a light-emitting element, one electrode functions as the anode and the other electrode functions as the cathode.

[0425] Furthermore, a display device according to one aspect of the present invention may be any of the following: a top-emission type that emits light in the direction opposite to the substrate on which the light-emitting element is formed; a bottom-emission type that emits light toward the substrate on which the light-emitting element is formed; or a dual-emission type that emits light on both sides.

[0426] One embodiment of the present invention is a semiconductor device having a transistor with a high on-current. A suitable material for the channel formation region of the transistor can be an oxide semiconductor (OS), resulting in a transistor with a low off-current. This semiconductor device can be suitably used in either or both of the display unit 162 and the circuit unit 164. Furthermore, this semiconductor device can be used in both the display unit 162 and the circuit unit 164, meaning all transistors in the display device can be OS transistors. By using OS transistors for all transistors in the display device in this way, manufacturing costs can be kept low.

[0427] The transistors in the display device of this embodiment are not limited to those of one aspect of the present invention. For example, the transistors of one aspect of the present invention may be combined with transistors of other structures.

[0428] The display device of this embodiment may have, for example, one or more of planar transistors, staggered transistors, or inverse staggered transistors. The transistors in the display device of this embodiment may be top-gate or bottom-gate types. Alternatively, gates may be provided above and below the semiconductor layer in which the channel is formed.

[0429] The display device of this embodiment may have a transistor (also referred to as a Si transistor) using silicon in the channel formation region.

[0430] The transistors in the circuit unit 164 and the transistors in the display unit 162 may have the same structure or different structures. The structures of the multiple transistors in the circuit unit 164 may all be the same or there may be two or more different structures. Similarly, the structures of the multiple transistors in the display unit 162 may all be the same or there may be two or more different structures.

[0431] All transistors in the display device may be OS transistors, all transistors in the display device may be Si transistors, or some of the transistors in the display device may be OS transistors and the rest may be Si transistors. Examples of silicon include single-crystal silicon, polycrystalline silicon, microcrystalline silicon, and amorphous silicon. An example of polycrystalline silicon is low-temperature polysilicon (LTPS). Transistors using LTPS in the channel formation region (also referred to as LTPS transistors) have high field-effect mobility and can operate at high speeds.

[0432] For example, by using both LTPS transistors and OS transistors in the display unit 162, a display device with low power consumption and high driving capability can be realized. Furthermore, a configuration combining LTPS transistors and OS transistors is sometimes referred to as LTPO. A more suitable example is a configuration in which OS transistors are used for transistors that function as switches to control conduction and non-conduction between wires, and LTPS transistors are used for transistors that control current.

[0433] <Example of sub-pixel configuration> An example of the configuration of the sub-pixel 11 is shown in Figure 13(B). The sub-pixel 11 includes a pixel circuit 51 and a light-emitting device 61.

[0434] The pixel circuit 51 includes a transistor 52A, a transistor 52B, and a capacitive element 53. The pixel circuit 51 is a 2Tr1C type pixel circuit having two transistors and one capacitive element. The pixel circuit that can be applied to the display device according to one embodiment of the present invention is not particularly limited.

[0435] The anode of the light-emitting device 61 is connected to one of the source and drain electrodes of transistor 52B and one electrode of the capacitive element 53. The other source and drain of transistor 52B is connected to wiring ANO. The gate of transistor 52B is connected to one of the source and drain electrodes of transistor 52A and the other electrode of the capacitive element 53. The other source and drain of transistor 52A is connected to wiring SL. The gate of transistor 52A is connected to wiring GL. The cathode of the light-emitting device 61 is connected to wiring VCOM.

[0436] Wiring VCOM is a wire that provides a potential for supplying current to the light-emitting device 61. Transistor 52A has the function of controlling the conduction or non-conduction state between wiring SL and the gate of transistor 52B based on the potential of wiring GL. For example, wiring ANO is supplied with VDD and wiring VCOM is supplied with VSS.

[0437] In this specification, the high power supply potential VDD (also simply referred to as "VDD") refers to a power supply potential that is higher than the low power supply potential VSS. The low power supply potential VSS (also simply referred to as "VSS") refers to a power supply potential that is lower than the high power supply potential VDD. The ground potential GND (also simply referred to as "GND") can also be used as VDD or VSS. For example, if VDD is GND, then VSS is at a lower potential than GND, and if VSS is GND, then VDD is at a higher potential than GND.

[0438] Transistor 52A functions as a selection transistor for controlling the selected state of the sub-pixel 11. Transistor 52B functions as a drive transistor for controlling the amount of current flowing to the light-emitting device 61. Capacitive element 53 has the function of maintaining the gate potential of transistor 52B. The intensity of the light emitted by the light-emitting device 61 is controlled according to the image signal supplied to the gate of transistor 52B. A semiconductor device according to one aspect of the present invention can be used in the pixel circuit 51. One or both of transistors 52A and transistor 52B can preferably be one or more of the aforementioned transistors.

[0439] For the drive transistor, a transistor with high saturation and high current controllability can be suitably used. This makes it possible to create a display device with high display quality. As the drive transistor, an OS transistor with high saturation can be suitably used.

[0440] When a transistor operates in the saturation region, an OS transistor exhibits a smaller change in source-drain current in response to a change in gate-source voltage than a Si transistor. Therefore, by using an OS transistor as the driving transistor, the current flowing between the source and drain can be precisely controlled by the change in gate-source voltage, thereby allowing control of the current flowing to the light-emitting element. This allows for an increase in the number of grayscale levels in the pixel circuit.

[0441] In terms of the saturation of the current flowing when a transistor operates in the saturation region, OS transistors can supply a more stable current (saturation current) than Si transistors, even when the source-drain voltage gradually increases. Therefore, by using an OS transistor as the driving transistor, a stable current can be supplied to the light-emitting element even if there are variations in the current-voltage characteristics of the light-emitting element. In other words, when operating in the saturation region, OS transistors can stabilize the luminescence brightness of the light-emitting element because the change in source-drain current is small even when the source-drain voltage is changed.

[0442] To increase the luminescence brightness of a light-emitting element, it is necessary to increase the amount of current flowing through the element. To achieve this, the source-drain voltage of the driving transistor must be increased. OS transistors have a higher breakdown voltage between source and drain compared to Si transistors, allowing for a higher voltage to be applied to the source-drain of an OS transistor. Therefore, by using an OS transistor as the driving transistor, the amount of current flowing through the light-emitting element can be increased, thereby increasing the luminescence brightness of the element. As mentioned earlier, by using a metal oxide with a high indium content in the semiconductor layer, a transistor with a high on-current can be created. By using such a transistor as the driving transistor, the current flowing through the light-emitting element increases, resulting in a display device with high brightness.

[0443] Because OS transistors have a low off-current, they can be suitably used as selection transistors. This allows pixel gradation to be maintained even when the frame frequency is significantly low (e.g., 1 fps or less), and thus power consumption can be reduced by stopping the driver when displaying still images.

[0444] By using a transistor with high field-effect mobility as the selection transistor, the time required for charging and discharging the floating node FN can be shortened. This allows for a higher frame frequency in the display, resulting in a display device with high display quality.

[0445] By using multiple transistors and capacitive elements in a pixel circuit, a high-performance display device can be created. By applying a semiconductor device according to one aspect of the present invention, the occupied area can be reduced even if the number of transistors and capacitive elements increases, resulting in a high-performance and high-resolution display device. For example, a display device with a resolution of 300 ppi or more, 500 ppi or more, 1000 ppi or more, 2000 ppi or more, or 3000 ppi or more can be realized.

[0446] A semiconductor device according to one aspect of the present invention can reduce the occupied area, thereby increasing the aperture ratio of pixels in a bottom-emission display device. For example, a display device with an aperture ratio of 50% or more, 55% or more, or 60% or more can be realized.

[0447] In this specification, the term "aperture ratio" refers to the ratio of the area of ​​the region from which light is emitted to the area of ​​the pixel.

[0448] Figure 13(C) shows an example of a configuration different from the sub-pixel 11 shown in Figure 13(B). The sub-pixel 11 has a pixel circuit 51A and a light-emitting device 61.

[0449] Pixel circuit 51A differs from pixel circuit 51 mainly in that transistor 52B is a p-channel type transistor. One electrode of capacitive element 53 is connected to wiring ANO.

[0450] In the pixel circuit 51A, an n-channel OS transistor can be suitably used for transistor 52A, and a p-channel LTPS transistor can be suitably used for transistor 52B.

[0451] In the pixel circuit 51 shown in Figure 13(B), transistors according to one aspect of the present invention (for example, IO transistors) can be suitably used for both transistor 52A and transistor 52B. This allows transistors 52A and 52B to be formed in the same process. Therefore, compared to a configuration using LTPO, the process can be simplified and manufacturing costs can be reduced. Furthermore, as mentioned above, when increasing the luminescence brightness of the light-emitting element, it is necessary to increase the source-drain voltage of the driving transistor. When the source-drain voltage is high, the drain current of an LTPS transistor may increase due to the Kink effect. On the other hand, OS transistors show only a small increase in drain current even when the source-drain voltage is high, making them suitable for use as driving transistors. In addition, OS transistors have smaller hysteresis compared to LTPS transistors, making them suitable for use as both selection transistors and driving transistors.

[0452] Figure 14(A) shows an example of a configuration different from the sub-pixel 11 shown in Figure 13(B). The sub-pixel 11 has a pixel circuit 51B and a light-emitting device 61.

[0453] Pixel circuit 51B differs from pixel circuit 51 mainly in that it has a transistor 52C. Pixel circuit 51B has transistors 52A, 52B, 52C, and a capacitive element 53. Pixel circuit 51B is a 3Tr1C type pixel circuit having three transistors and one capacitive element.

[0454] Pixel circuit 51B has a configuration in which transistor 52C is added to pixel circuit 51 shown in Figure 13(B). One of the source and drain of transistor 52C is connected to one of the source and drain of transistor 52B. The other of the source and drain of transistor 52C is connected to wiring V0. For example, a reference potential is supplied to wiring V0. The gate of transistor 52C is connected to wiring GL. Transistor 52C has the function of controlling the conduction or non-conduction state between one of the source and drain of transistor 52B and wiring V0 based on the potential of wiring GL.

[0455] The wiring V0 can be used to obtain current values ​​that can be used to set pixel parameters. Specifically, wiring V0 can function as a monitor line to output the current flowing through transistor 52B or the current flowing through light-emitting device 61 to the outside. The current output to wiring V0 can be converted into a voltage by a source follower circuit and output to the outside. Alternatively, it can be converted into a digital signal by an AD converter and output to the outside.

[0456] Figure 14(B) shows an example of a configuration different from the sub-pixel 11 shown in Figure 14(A). The sub-pixel 11 has a pixel circuit 51C and a light-emitting device 61. The gate of transistor 52A is connected to wiring GL1. The gate of transistor 52C is connected to wiring GL2. Transistor 52C has the function of controlling the conduction or non-conduction state between the source and drain of transistor 52B and wiring V0 based on the potential of wiring GL2. By configuring the gates of transistor 52A and transistor 52C to be connected to different wirings, the operation of transistor 52A and the operation of transistor 52C can be controlled independently.

[0457] Back gates can be provided for some or all of the transistors included in the pixel circuit. For example, transistor 52B can have a back gate, and this back gate can be connected to either the source or the drain of transistor 52B. This can improve reliability. Alternatively, the back gate of transistor 52B can be connected to the gate of transistor 52B. This can increase the on-current of transistor 52B.

[0458] Figure 15(A) shows an example of a cross-section of the display device 50A when a portion of the area including the FPC 172, a portion of the circuit section 164, a portion of the display section 162, a portion of the connection section 140, and a portion of the area including the end are cut.

[0459] The display device 50A shown in Figure 15(A) has transistors 205D, 205R, 205G, 205B, light-emitting elements 130R, 130G, and 130B between substrates 151 and 152. Light-emitting element 130R is a display element of a sub-pixel 11R that emits red light, light-emitting element 130G is a display element of a sub-pixel 11G that emits green light, and light-emitting element 130B is a display element of a sub-pixel 11B that emits blue light.

[0460] The display device 50A employs an SBS structure. The SBS structure allows for the optimization of materials and configurations for each light-emitting element, thus increasing the freedom in selecting materials and configurations and making it easier to improve brightness and reliability.

[0461] The display device 50A is a top-emission type. In the top-emission type, transistors and the like can be placed overlapping with the light-emitting region of the light-emitting element, which allows for a higher aperture ratio of pixels compared to the bottom-emission type.

[0462] Transistors 205D, 205R, 205G, and 205B are all formed on substrate 151. These transistors can be manufactured using the same process. Figure 15(A) shows an example configuration in which transistors 205R, 205G, 205B, and 205D use the transistor 100 shown in Figure 1(B), etc. By using TGSA type transistors, the parasitic capacitance between the source electrode, drain electrode, and gate electrode can be reduced. Therefore, the deterioration of display quality caused by parasitic capacitance can be suppressed. Note that transistors 205D, 205R, 205G, and 205B may be transistors with different structures.

[0463] In this embodiment, an example is shown in which OS transistors are used for transistors 205D, 205R, 205G, and 205B. Transistors according to one aspect of the present invention can be used for transistors 205D, 205R, 205G, and 205B. In other words, the display device 50A has transistors according to one aspect of the present invention in both the display unit 162 and the circuit unit 164. By using transistors according to one aspect of the present invention in the display unit 162, the pixel size can be reduced, resulting in a high-definition display device. Furthermore, by using transistors according to one aspect of the present invention in the circuit unit 164, the occupied area of ​​the circuit unit 164 can be reduced, and the bezel can be narrowed. For details on the transistors according to one aspect of the present invention, refer to the description in the previous embodiment.

[0464] Specifically, transistors 205D, 205R, 205G, and 205B each have a conductive layer 104 that functions as a gate electrode, an insulating layer 106 that functions as a gate insulating layer, a conductive layer 103 that functions as a back gate electrode, an insulating layer 105 that functions as a back gate insulating layer, conductive layers 112a and 112b that function as source and drain electrodes, and a semiconductor layer 108 having a metal oxide. Here, the same hatching pattern is applied to multiple layers obtained by processing the same conductive film.

[0465] An insulating layer 218 is provided to cover transistors 205D, 205R, 205G, and 205B, and an insulating layer 235 is provided on top of the insulating layer 218. For details on the insulating layer 218, please refer to the previous description.

[0466] The insulating layer 235 preferably functions as a planarization layer, and an organic insulating layer is preferred. Alternatively, the insulating layer 235 can be a laminated structure of an organic insulating layer and an inorganic insulating layer. The outermost layer of the insulating layer 235 preferably functions as an etching protection layer. This suppresses the formation of recesses in the insulating layer 235 during processing of pixel electrodes 111R, 111G, 111B, etc. Alternatively, recesses may be provided in the insulating layer 235 during processing of pixel electrodes 111R, 111G, and 111B, etc. Note that pixel electrodes 111R, 111G, and 111B are sometimes collectively referred to as pixel electrode 111.

[0467] Light-emitting elements 130R, 130G, and 130B are provided on the insulating layer 235.

[0468] The light-emitting element 130R has a pixel electrode 111R on the insulating layer 235, an EL layer 113R on the pixel electrode 111R, and a common electrode 115 on the EL layer 113R. The light-emitting element 130R shown in Figure 15(A) emits red light (R). The EL layer 113R has a light-emitting layer that emits red light.

[0469] The light-emitting element 130G has a pixel electrode 111G on an insulating layer 235, an EL layer 113G on the pixel electrode 111G, and a common electrode 115 on the EL layer 113G. The light-emitting element 130G shown in Figure 15(A) emits green light (G). The EL layer 113G has a light-emitting layer that emits green light.

[0470] The light-emitting element 130B has a pixel electrode 111B on an insulating layer 235, an EL layer 113B on the pixel electrode 111B, and a common electrode 115 on the EL layer 113B. The light-emitting element 130B shown in Figure 15(A) emits blue light (B). The EL layer 113B has a light-emitting layer that emits blue light.

[0471] Note that in Figure 15(A), the EL layers 113R, 113G, and 113B are all shown to be the same thickness, but this is not the only option. The thicknesses of the EL layers 113R, 113G, and 113B may be different. For example, it is preferable to set the thickness of the EL layers 113R, 113G, and 113B so that the optical path length is such that the light emitted by each is intensified. This makes it possible to realize a microcavity structure and improve the color purity of the light emitted from each light-emitting element.

[0472] The pixel electrode 111R is in contact with the conductive layer 112b of the transistor 205R at an opening provided in the insulating layer 218 and the insulating layer 235, and is connected to the conductive layer 112b. Similarly, the pixel electrode 111G is connected to the conductive layer 112b of the transistor 205G, and the pixel electrode 111B is connected to the conductive layer 112b of the transistor 205B.

[0473] Each end of the pixel electrodes 111R, 111G, and 111B is covered by an insulating layer 237. The insulating layer 237 can be provided in a single-layer or multi-layer structure using one or both inorganic insulating materials and / or organic insulating materials. For example, the materials listed for insulating layer 218 and insulating layer 235 can be applied to the insulating layer 237. The insulating layer 237 provides electrical insulation between the pixel electrodes and the common electrode. Furthermore, the insulating layer 237 provides electrical insulation between adjacent light-emitting elements.

[0474] The insulating layer 237 is provided at least on the display unit 162. The insulating layer 237 may be provided not only on the display unit 162, but also on the connection unit 140 and the circuit unit 164. Furthermore, the insulating layer 237 may extend to the ends of the display device 50A.

[0475] The common electrode 115 is a continuous film provided in common to the light-emitting elements 130R, 130G, and 130B. The common electrode 115, which is shared by multiple light-emitting elements, is connected to a conductive layer 123 provided at the connection portion 140. It is preferable to use a conductive layer for the conductive layer 123 that is made of the same material and formed using the same process as the pixel electrodes 111R, 111G, and 111B.

[0476] In a display device according to one aspect of the present invention, among the pixel electrodes and common electrodes, the electrode that extracts light is preferably made of a conductive film that transmits visible light. Furthermore, it is preferable that the electrode that does not extract light is made of a conductive film that reflects visible light.

[0477] A conductive film that transmits visible light may also be used on the electrode that does not extract light. In this case, it is preferable to place the electrode between the reflective layer and the EL layer. In other words, the light emitted from the EL layer may be reflected by the reflective layer and extracted from the display device.

[0478] As the material for forming the pair of electrodes of the light-emitting element, metals, alloys, electrically conductive compounds, and mixtures thereof can be used as appropriate. Specifically, such materials include metals such as aluminum, magnesium, titanium, chromium, manganese, iron, cobalt, nickel, copper, gallium, zinc, indium, tin, molybdenum, tantalum, tungsten, palladium, gold, platinum, silver, yttrium, and neodymium, and alloys containing these in appropriate combinations. Other materials include ITO, ITSO, In-Zn oxide, and In-W-Zn oxide. Furthermore, other materials include aluminum-containing alloys such as aluminum, nickel, and lanthanum alloys (Al-Ni-La), as well as silver-containing alloys such as silver-magnesium alloys and silver-palladium-copper alloys (Ag-Pd-Cu, also written as APC). Other materials include elements belonging to Group 1 or Group 2 of the periodic table not exemplified above (e.g., lithium, cesium, calcium, strontium), rare earth metals such as europium and ytterbium, alloys containing these in appropriate combinations, graphene, and the like.

[0479] It is preferable that the light-emitting element has a microcavity structure. Therefore, it is preferable that one of the pair of electrodes in the light-emitting element is a semitransmitting / semi-reflective electrode that transmits and reflects visible light, and the other is a reflective electrode that reflects visible light. By having a microcavity structure in the light-emitting element, the light emitted from the light-emitting layer can be resonated between the two electrodes, thereby strengthening the light emitted from the light-emitting element.

[0480] The light transmittance of the transparent electrode shall be 40% or more. For example, it is preferable to use an electrode with a transmittance of 40% or more for visible light (light with a wavelength of 400 nm or more and less than 750 nm) for the transparent electrode of the light-emitting element. The visible light reflectance of the semi-transparent / semi-reflective electrode shall be 10% or more and 95% or less, preferably 30% or more and 80% or less. The visible light reflectance of the reflective electrode shall be 40% or more and 100% or less, preferably 70% or more and 100% or less. Furthermore, the electrical resistivity of these electrodes shall be 1 × 10⁻⁶ -2 A value of Ωcm or less is preferable.

[0481] The EL layers 113R, 113G, and 113B are each provided in an island-like manner. In Figure 15(A), the edges of adjacent EL layers 113R and 113G overlap, the edges of adjacent EL layers 113G and 113B overlap, and the edges of adjacent EL layers 113R and 113B overlap. When forming island-like EL layers using a fine metal mask, the edges of adjacent EL layers may overlap as shown in Figure 15(A), but this is not the only case. In other words, adjacent EL layers may not overlap and may be separated from each other. Furthermore, in a display device, there may be both regions where adjacent EL layers overlap and regions where adjacent EL layers do not overlap and are separated.

[0482] Each of the EL layers 113R, 113G, and 113B has at least one light-emitting layer. The light-emitting layer has one or more types of light-emitting materials. As the light-emitting material, a material that exhibits a light emission color such as blue, purple, blue-violet, green, yellow-green, yellow, orange, or red may be used as appropriate. In addition, a material that emits near-infrared light may be used as the light-emitting material.

[0483] The light-emitting layer may contain one or more types of organic compounds (host material, assist material, etc.) in addition to the light-emitting substance (guest material). One or more of the organic compounds may be substances with high hole transport properties (hole transport material) and / or substances with high electron transport properties (electron transport material). Alternatively, one or more of the organic compounds may be bipolar substances (substances with high electron and hole transport properties) or TADF materials.

[0484] The light-emitting layer preferably comprises, for example, a phosphorescent material and a combination of a hole-transporting material and an electron-transporting material that readily forms an excitation complex. This configuration allows for efficient emission using ExTET (Exciplex-Triplet Energy Transfer), which is energy transfer from the excitation complex to the light-emitting substance (phosphorescent material). By selecting a combination that forms an excitation complex that exhibits emission overlapping with the wavelength of the lowest-energy absorption band of the light-emitting substance, energy transfer becomes smoother, and light emission can be obtained efficiently. This configuration enables high efficiency, low-voltage operation, and a long lifespan for the light-emitting device.

[0485] The EL layer may have, in addition to the light-emitting layer, one or more of the following: a layer containing a material with high hole injection properties (hole injection layer), a layer containing a hole transport material (hole transport layer), a layer containing a material with high electron blocking properties (electron blocking layer), a layer containing a material with high electron injection properties (electron injection layer), a layer containing an electron transport material (electron transport layer), and a layer containing a material with high hole blocking properties (hole blocking layer). Furthermore, the EL layer may contain either or both a bipolar material and a TADF material.

[0486] The light-emitting element can be made of either low-molecular-weight compounds or high-molecular-weight compounds, and may also contain inorganic compounds. The layers constituting the light-emitting element can be formed by methods such as vapor deposition (including vacuum deposition), transfer, printing, inkjet, and coating.

[0487] The light-emitting element may be a single structure (a structure having only one light-emitting unit) or a tandem structure (a structure having multiple light-emitting units). Each light-emitting unit has at least one light-emitting layer. The tandem structure is a configuration in which multiple light-emitting units are connected in series via a charge generation layer. The charge generation layer has the function of injecting electrons into one of the two light-emitting units and holes into the other when a voltage is applied between a pair of electrodes. By using a tandem structure, a light-emitting element capable of high-brightness emission can be made. Furthermore, compared to a single structure, the tandem structure can reduce the current required to obtain the same brightness, thus improving reliability. The tandem structure can also be called a stacked structure.

[0488] In Figure 15(A), when a tandem light-emitting element is used, it is preferable that the EL layer 113R has a structure having multiple light-emitting units that emit red light, the EL layer 113G has a structure having multiple light-emitting units that emit green light, and the EL layer 113B has a structure having multiple light-emitting units that emit blue light.

[0489] A protective layer 131 is provided on the light-emitting elements 130R, 130G, and 130B. The protective layer 131 and the substrate 152 are bonded via an adhesive layer 142. A light-shielding layer 117 is provided on the substrate 152. For sealing the light-emitting elements, for example, a solid sealing structure or a hollow sealing structure can be applied. In Figure 15(A), the space between the substrate 152 and the substrate 151 is filled with the adhesive layer 142, and a solid sealing structure is applied. Alternatively, the space may be filled with an inert gas (such as nitrogen or argon), and a hollow sealing structure may be applied. In this case, the adhesive layer 142 may be provided in a frame shape so as not to overlap with the light-emitting elements. Furthermore, the space may be filled with a resin different from the adhesive layer 142 provided in a frame shape.

[0490] The protective layer 131 is provided at least on the display section 162, and preferably so as to cover the entire display section 162. It is preferable that the protective layer 131 covers not only the display section 162, but also the connection section 140 and the circuit section 164. Furthermore, it is preferable that the protective layer 131 extends to the edges of the display device 50A. On the other hand, in the connection section 197, there is an area where the protective layer 131 is not provided in order to connect the FPC 172 and the conductive layer 166.

[0491] By providing a protective layer 131 on the light-emitting elements 130R, 130G, and 130B, the reliability of the light-emitting elements can be improved.

[0492] The protective layer 131 can be a single layer or a laminated structure of two or more layers. Furthermore, the conductivity of the protective layer 131 is not required. At least one of an insulating film, a semiconductor film, and a conductive film can be used as the protective layer 131.

[0493] The presence of an inorganic film in the protective layer 131 prevents oxidation of the common electrode 115 and suppresses the intrusion of impurities (such as moisture and oxygen) into the light-emitting element, thereby suppressing degradation of the light-emitting element and improving the reliability of the display device.

[0494] The protective layer 131 preferably has one or more inorganic insulating layers. The protective layer 131 can be made from the materials listed for insulating layer 106 and insulating layer 105. In particular, the protective layer 131 preferably uses a nitride or nitride oxide, and more preferably uses a nitride.

[0495] The protective layer 131 may also be an inorganic film containing ITO, In-Zn oxide, Ga-Zn oxide, Al-Zn oxide, or IGZO. The inorganic film is preferably highly resistive, specifically, more resistive than the common electrode 115. The inorganic film may further contain nitrogen.

[0496] When the light emitted from a light-emitting element is extracted via a protective layer 131, it is preferable that the protective layer 131 has high transmittance to visible light. For example, ITO, IGZO, and aluminum oxide are preferred because they are inorganic materials with high transmittance to visible light.

[0497] As the protective layer 131, for example, a laminated structure of an aluminum oxide film and a silicon nitride film on the aluminum oxide film, or a laminated structure of an aluminum oxide film and an IGZO film on the aluminum oxide film can be used. By using such a laminated structure, it is possible to suppress the penetration of impurities (water, oxygen, etc.) into the EL layer.

[0498] Furthermore, the protective layer 131 may have an organic film. For example, the protective layer 131 may have both an organic film and an inorganic film. Examples of organic films that can be used for the protective layer 131 include an organic insulating layer that can be used for the insulating layer 235.

[0499] A connection portion 197 is provided in the region of substrate 151 where substrate 152 does not overlap. At the connection portion 197, the conductive layer 165 is connected to the FPC 172 via the conductive layer 166 and the connection layer 242. Figure 15(A) shows an example in which the conductive layer 165 is formed by processing the same conductive film as conductive layers 112a and 112b, and the conductive layer 166 is formed by processing the same conductive film as the pixel electrodes 111R, 111G, and 111B. The connection portion between conductive layer 165 and conductive layer 166 can be configured similarly to the connection portion between the pixel electrode 111 and conductive layer 112b. Specifically, Figure 15(A) shows an example in which an opening is provided in the upper layer of conductive layer 165, and the conductive layer 166 is in contact with the upper surface of conductive layer 165 at this opening. The conductive layer 166 is exposed on the upper surface of the connection portion 197. This allows the connection part 197 and the FPC 172 to be connected via the connection layer 242.

[0500] The display device 50A is of the top-emission type. The light emitted by the light-emitting element is emitted towards the substrate 152. It is preferable to use a material with high transmittance to visible light for the substrate 152. The pixel electrodes 111R, 111G, and 111B contain a material that reflects visible light, and the counter electrode (common electrode 115) contains a material that transmits visible light.

[0501] It is preferable to provide a light-shielding layer 117 on the surface of the substrate 152 that faces the substrate 151. The light-shielding layer 117 can be provided between adjacent light-emitting elements, in connection parts 140, and in circuit parts 164, etc.

[0502] A colored layer, such as a color filter, may be provided on the surface of the substrate 152 facing the substrate 151, or on the protective layer 131. By placing a color filter on top of the light-emitting element, the color purity of the light emitted from the pixel can be increased.

[0503] A colored layer is a colored layer that selectively transmits light in a specific wavelength range and absorbs light in other wavelength ranges. For example, a red (R) color filter that transmits light in the red wavelength range, a green (G) color filter that transmits light in the green wavelength range, and a blue (B) color filter that transmits light in the blue wavelength range can be used. One or more of the following can be used for each colored layer: metal materials, resin materials, pigments, and dyes. The colored layers are formed at the desired location using methods such as printing, inkjet printing, or etching using photolithography.

[0504] Various optical components can be placed on the outside of the substrate 152 (the side opposite to the substrate 151). Examples of optical components include polarizing plates, phase difference plates, light diffusion layers (such as diffusion films), anti-reflective layers, and light-gathering films. In addition, surface protection layers such as an antistatic film to suppress the adhesion of dust, a water-repellent film to make it difficult for dirt to adhere, a hard coat film to suppress the occurrence of scratches during use, and a shock-absorbing layer may be placed on the outside of the substrate 152. For example, a glass layer or a silica layer (SiO2) may be used as the surface protection layer. x Providing a protective layer is preferable as it can suppress surface contamination and scratching. Alternatively, materials such as DLC (diamond-like carbon), aluminum oxide, polyester-based materials, or polycarbonate-based materials may be used as the surface protective layer. It is preferable to use a material with high transmittance to visible light for the surface protective layer. Furthermore, it is preferable to use a material with high hardness for the surface protective layer.

[0505] Substrates 151 and 152 can be made of glass, quartz, ceramics, sapphire, resin, metal, alloy, semiconductor, etc., respectively. The substrate on the side that extracts light from the light-emitting element should be made of a material that transmits the light. Using flexible materials for substrates 151 and 152 increases the flexibility of the display device, enabling a flexible display. A polarizing plate may also be used as at least one of substrates 151 and 152.

[0506] As substrates 151 and 152, various materials can be used, such as polyester resins like polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyacrylonitrile resin, acrylic resin, polyimide resin, polymethyl methacrylate resin, polycarbonate (PC) resin, polyethersulfone (PES) resin, polyamide resin (nylon, aramid, etc.), polysiloxane resin, cycloolefin resin, polystyrene resin, polyamide-imide resin, polyurethane resin, polyvinyl chloride resin, polyvinylidene chloride resin, polypropylene resin, polytetrafluoroethylene (PTFE) resin, ABS resin, cellulose nanofiber, etc. At least one of substrates 151 and 152 may be made of glass of a thickness sufficient to provide flexibility.

[0507] Furthermore, when a circular polarizer is superimposed on a display device, it is preferable to use a substrate with high optical isotropy for the substrate of the display device. A substrate with high optical isotropy has low birefringence (or a small amount of birefringence). Examples of films with high optical isotropy include triacetylcellulose (TAC, also called cellulose triacetate) film, cycloolefin polymer (COP) film, cycloolefin copolymer (COC) film, and acrylic film.

[0508] Various types of curing adhesives can be used as the adhesive layer 142, including UV-curing adhesives, reaction-curing adhesives, thermosetting adhesives, and anaerobic adhesives. Examples of these adhesives include epoxy resins, acrylic resins, silicone resins, phenolic resins, polyimide resins, imide resins, PVC (polyvinyl chloride) resins, PVB (polyvinyl butyral) resins, and EVA (ethylene vinyl acetate) resins. Materials with low moisture permeability, such as epoxy resins, are particularly preferred. Two-component mixed resins may also be used. Adhesive sheets may also be used.

[0509] Anisotropic conductive film (ACF), anisotropic conductive paste (ACP), etc., can be used as the connecting layer 242.

[0510] <Example of display device configuration 2> Figure 15(B) shows an example of a cross-section of the display unit 162 of the display device 50B. The display device 50B differs from the display device 50A mainly in that each sub-pixel of each color uses a light-emitting element having a common EL layer 113 and a coloring layer (such as a color filter). The configuration shown in Figure 15(B) can be combined with the configuration of the region including the FPC 172, the circuit unit 164, the laminated structure from the substrate 151 to the insulating layer 235 of the display unit 162, the connection part 140, and the end part shown in Figure 15(A). Note that in the following description of the display device, parts that are the same as those described earlier may be omitted.

[0511] The display device 50B shown in Figure 15(B) includes light-emitting elements 130R, 130G, 130B, a colored layer 132R that transmits red light, a colored layer 132G that transmits green light, and a colored layer 132B that transmits blue light, etc.

[0512] The light-emitting element 130R includes a pixel electrode 111R, an EL layer 113 on the pixel electrode 111R, and a common electrode 115 on the EL layer 113. The light emitted from the light-emitting element 130R is extracted as red light to the outside of the display device 50B via the colored layer 132R.

[0513] The light-emitting element 130G includes a pixel electrode 111G, an EL layer 113 on the pixel electrode 111G, and a common electrode 115 on the EL layer 113. The light emitted from the light-emitting element 130G is extracted as green light to the outside of the display device 50B via the colored layer 132G.

[0514] The light-emitting element 130B includes a pixel electrode 111B, an EL layer 113 on the pixel electrode 111B, and a common electrode 115 on the EL layer 113. The light emitted from the light-emitting element 130B is extracted as blue light to the outside of the display device 50B via the colored layer 132B.

[0515] The light-emitting elements 130R, 130G, and 130B each share an EL layer 113 and a common electrode 115. Providing a common EL layer 113 for each sub-pixel of each color reduces the number of manufacturing steps compared to providing a different EL layer for each sub-pixel of each color.

[0516] For example, the light-emitting elements 130R, 130G, and 130B shown in Figure 15(B) emit white light. The white light emitted by the light-emitting elements 130R, 130G, and 130B passes through the colored layers 132R, 132G, and 132B, thereby obtaining light of a desired color.

[0517] A light-emitting element that emits white light preferably includes two or more light-emitting layers. For example, a light-emitting element may have two light-emitting layers whose emitted colors are complementary, or three or more light-emitting layers whose emitted colors combine to produce white light as a whole.

[0518] The EL layer 113 preferably has, for example, an emissive layer having a light-emitting material that emits blue light, and an emissive layer having a light-emitting material that emits visible light with a longer wavelength than blue. The EL layer 113 preferably has, for example, an emissive layer that emits yellow light and an emissive layer that emits blue light. Alternatively, the EL layer 113 preferably has, for example, an emissive layer that emits red light, an emissive layer that emits green light, and an emissive layer that emits blue light.

[0519] For light-emitting elements that emit white light, a tandem structure is preferable. Specifically, a two-stage tandem structure having a light-emitting unit that emits yellow light and a light-emitting unit that emits blue light, a two-stage tandem structure having a light-emitting unit that emits red and green light and a light-emitting unit that emits blue light, a three-stage tandem structure having a light-emitting unit that emits blue light, a light-emitting unit that emits yellow, yellow-green, or green light, and a light-emitting unit that emits blue light in that order, or a three-stage tandem structure having a light-emitting unit that emits blue light, a light-emitting unit that emits yellow, yellow-green, or green light, a light-emitting unit that emits red light, and a light-emitting unit that emits blue light in that order. For example, the number of layers and color order of the light-emitting unit can be, from the anode side, a two-layer structure of B and Y, a two-layer structure of B and light-emitting unit X, a three-layer structure of B, Y, B, or a three-layer structure of B, X, B. The number of layers and color order of the light-emitting layers in light-emitting unit X can be, from the anode side, a two-layer structure of R and Y, a two-layer structure of R and G, a two-layer structure of G and R, a three-layer structure of G, R, G, or a three-layer structure of R, G, R. In addition, other layers may be provided between the two light-emitting layers.

[0520] Furthermore, by applying a microcavity structure, a light-emitting element that normally emits white light may also emit light of specific wavelengths, such as red, green, or blue, with increased intensity.

[0521] Alternatively, for example, the light-emitting elements 130R, 130G, and 130B shown in Figure 15(B) emit blue light. In this case, the EL layer 113 has one or more light-emitting layers that emit blue light. In the sub-pixel 11B that emits blue light, the blue light emitted by the light-emitting element 130B can be extracted. In addition, in the sub-pixel 11R that emits red light and the sub-pixel 11G that emits green light, by providing a color conversion layer between the light-emitting element 130R or light-emitting element 130G and the substrate 152, the blue light emitted by the light-emitting element 130R or light-emitting element 130G can be converted into longer wavelength light, and red or green light can be extracted. It is preferable to use a quantum dot material for the color conversion layer. Furthermore, it is preferable to provide a coloring layer 132R between the color conversion layer and the substrate 152 on the light-emitting element 130R, and a coloring layer 132G between the color conversion layer and the substrate 152 on the light-emitting element 130G. Some of the light emitted by a light-emitting element may pass through without being converted by the color conversion layer. By extracting the light that has passed through the color conversion layer via a colored layer, the color of light other than the desired color can be absorbed by the colored layer, thereby increasing the color purity of the light exhibited by the subpixel.

[0522] <Example of display device configuration 3> The display device 50C shown in Figure 16 differs from the display device 50A mainly in that it has a conductive layer 234p, a conductive layer 234a, a conductive layer 234b, and an insulating layer 239.

[0523] An insulating layer 239 is provided on the insulating layer 235, and light-emitting elements 130R, 130G, and 130B are provided on the insulating layer 239.

[0524] The conductive layer 234p is provided so as to cover the openings provided in the insulating layer 218 and the insulating layer 235. The conductive layer 234p is in contact with the conductive layer 112b of the transistor 205R at the openings and is connected to the conductive layer 112b.

[0525] An insulating layer 239 is provided on the conductive layer 234p and the insulating layer 235. The insulating layer 239 can be made from the materials listed for the insulating layer 235.

[0526] The pixel electrode 111R is provided so as to cover an opening in the insulating layer 239. The pixel electrode 111R is in contact with the conductive layer 234p at the opening and is connected to the conductive layer 234p. In other words, the pixel electrode 111R is connected to the conductive layer 112b via the conductive layer 234p. The same applies to the pixel electrodes 111G and 111B.

[0527] The conductive layer 234a is provided so as to cover the openings provided in the insulating layer 218 and the insulating layer 235. The conductive layer 234a is in contact with the conductive layer 165 at the openings and is connected to the conductive layer 165.

[0528] The conductive layer 166 is provided so as to cover the opening provided in the insulating layer 239. The conductive layer 166 is in contact with the conductive layer 234a at the opening and is connected to the conductive layer 234a. In other words, the conductive layer 166 is connected to the conductive layer 165 via the conductive layer 234a.

[0529] Figure 16 shows a configuration in which the circuit section 164 has a conductive layer 234b. The conductive layer 234b can also be connected to the transistor 205D.

[0530] Conductive layers 234p, 234a, and 234b each function as wiring. Conductive layers 234p, 234a, and 234b are provided on different layers from conductive layers 112a, 112b, and 104. Therefore, wiring can be placed on each layer, increasing the flexibility of the layout and reducing the circuit's footprint.

[0531] The conductive layers 234p, 234a, and 234b can be made from the materials listed for conductive layers 112a, 112b, and 104. The conductive layers 234p, 234a, and 234b can be formed in the same process. For example, the conductive layers 234p, 234a, and 234b can be formed by depositing a conductive film and then processing the conductive film.

[0532] <Example of display device configuration 4> The display device 50D shown in Figure 17 differs from the display device 50B mainly in that it is a bottom-emission type display device.

[0533] The light emitted by the light-emitting element is emitted towards the substrate 151. It is preferable to use a material with high transmittance (also referred to as light transmission) to visible light for the substrate 151. On the other hand, the light transmission of the material used for the substrate 152 is not a requirement.

[0534] It is preferable to form a light-shielding layer 117 between the substrate 151 and the transistors. Figure 17 shows an example in which a light-shielding layer 117 is provided on the substrate 151, an insulating layer 153 is provided on the light-shielding layer 117, and transistors 205D, 205R (not shown), 205G, and 205B are provided on the insulating layer 153. In addition, a colored layer 132R, a colored layer 132G, and a colored layer 132B are provided on the insulating layer 218, and an insulating layer 235 is provided on the colored layer 132R, a colored layer 132G, and a colored layer 132B.

[0535] The light-emitting element 130R, which overlaps with the colored layer 132R, has a pixel electrode 111R, an EL layer 113, and a common electrode 115.

[0536] The light-emitting element 130G, which overlaps with the colored layer 132G, has a pixel electrode 111G, an EL layer 113, and a common electrode 115.

[0537] The light-emitting element 130B, which overlaps with the colored layer 132B, has a pixel electrode 111B, an EL layer 113, and a common electrode 115.

[0538] The pixel electrodes 111R, 111G, and 111B are made of materials with high transmittance to visible light. It is preferable to use a material that reflects visible light for the common electrode 115. In a bottom-emission type display device, a metal with low electrical resistivity can be used for the common electrode 115, thereby suppressing voltage drops caused by the electrical resistance of the common electrode 115 and achieving high display quality.

[0539] By applying a transistor according to one aspect of the present invention, the occupied area of ​​the pixel circuit can be reduced, thereby increasing the aperture ratio of the pixels or reducing the size of the pixels in a display device with a bottom emission structure.

[0540] <Example of display device configuration 5> The display device 50E shown in Figure 18(A) differs from the display device 50A mainly in that it has a light-receiving element 130S.

[0541] The display device 50E has a light-emitting element and a light-receiving element in each pixel. In the display device 50E, it is preferable to use an organic EL element as the light-emitting element and an organic photodiode as the light-receiving element. The organic EL element and the organic photodiode can be formed on the same substrate. Therefore, an organic photodiode can be incorporated into a display device using an organic EL element.

[0542] In a display device 50E having light-emitting and light-receiving elements in its pixels, the pixels have a light-receiving function, allowing for the detection of contact or proximity of an object while displaying an image. Therefore, the display unit 162 has, in addition to an image display function, one or both of an imaging function and a sensing function. For example, the display device 50E can not only display an image using all of its subpixels, but some subpixels can also emit light as a light source, some other subpixels can perform light detection, and the remaining subpixels can display an image.

[0543] Therefore, it is not necessary to provide a light receiving unit and a light source separately from the display device 50E, and the number of components in the electronic device can be reduced. For example, there is no need to separately provide a biometric authentication device or a capacitive touch panel for scrolling, etc., which are installed in the electronic device. Therefore, by using the display device 50E, it is possible to provide an electronic device with reduced manufacturing costs.

[0544] When a light-receiving element is used as an image sensor, the display device 50E can capture an image using the light-receiving element. For example, the image sensor can be used to capture images for personal authentication, such as fingerprints, palm prints, irises, pulse patterns (including vein patterns and arterial patterns), or faces.

[0545] The light-receiving element can be used in touch sensors (also called direct touch sensors) or non-contact sensors (also called hover sensors, hover touch sensors, or touchless sensors). Touch sensors can detect an object (such as a finger, hand, or pen) by making direct contact between the display device and the object. Non-contact sensors, on the other hand, can detect an object even if the object does not come into contact with the display device.

[0546] The light-receiving element 130S has a pixel electrode 111S on an insulating layer 235, a functional layer 113S on the pixel electrode 111S, and a common electrode 115 on the functional layer 113S. Light Lin is incident on the functional layer 113S from outside the display device 50E.

[0547] The pixel electrode 111S is in contact with the conductive layer 112b of the transistor 205S at an opening provided in the insulating layer 218 and the insulating layer 235, and is connected to the conductive layer 112b.

[0548] The ends of the pixel electrode 111S are covered by an insulating layer 237.

[0549] The common electrode 115 is a continuous film provided in common to the light-receiving element 130S, the light-emitting element 130R (not shown), the light-emitting element 130G, and the light-emitting element 130B. The common electrode 115, which is shared by the light-emitting element and the light-receiving element, is connected to the conductive layer 123 provided at the connection portion 140.

[0550] The functional layer 113S has at least an active layer (also called a photoelectric conversion layer). The active layer contains a semiconductor. Examples of such semiconductors include inorganic semiconductors such as silicon and organic semiconductors containing organic compounds. In this embodiment, an example is shown in which an organic semiconductor is used as the semiconductor of the active layer. Using an organic semiconductor is preferable because the light-emitting layer and the active layer can be formed by the same method (for example, vacuum deposition), and the manufacturing equipment can be shared.

[0551] The functional layer 113S may further include layers other than the active layer, such as a material with high hole transport properties, a material with high electron transport properties, or a bipolar material. Furthermore, it may also further include layers containing a material with high hole injection properties, a hole blocking material, a material with high electron injection properties, or an electron blocking material. For example, the functional layer 113S can be made from materials that can be used in the above-described light-emitting devices.

[0552] The photodetector can use either low-molecular-weight compounds or high-molecular-weight compounds, and may also contain inorganic compounds. The layers constituting the photodetector can be formed by methods such as vapor deposition (including vacuum deposition), transfer, printing, inkjet, and coating.

[0553] The display device 50E shown in Figures 18(B) and 18(C) has a layer 353 with a light-receiving element, a circuit layer 355, and a layer 357 with an light-emitting element between substrate 151 and substrate 152.

[0554] Layer 353 has, for example, a light-receiving element 130S. Layer 357 has, for example, light-emitting elements 130R, 130G, and 130B.

[0555] The circuit layer 355 includes a circuit for driving a light-receiving element and a circuit for driving a light-emitting element. The circuit layer 355 includes, for example, transistors 205R, 205G, and 205B. In addition, the circuit layer 355 may be provided with one or more of the following: switches, capacitors, resistors, wiring, and terminals.

[0556] Figure 18(B) shows an example of using the light-receiving element 130S as a touch sensor. As shown in Figure 18(B), the light emitted by the light-emitting element in layer 357 is reflected by the finger 352 that is in contact with the display device 50E, and the light-receiving element in layer 353 detects this reflected light. This makes it possible to detect that the finger 352 has come into contact with the display device 50E.

[0557] Fi...

Claims

1. It has a semiconductor layer, a first insulating layer, a second insulating layer, and a conductive layer. The semiconductor layer is located on the first insulating layer, The second insulating layer is located on the semiconductor layer, The semiconductor layer has a region that overlaps with the conductive layer via the second insulating layer, The semiconductor layer comprises a first metal oxide layer and a second metal oxide layer on the first metal oxide layer. The first metal oxide layer and the second metal oxide layer each contain indium and oxygen, The film density of the first metal oxide layer is higher than the film density of the second metal oxide layer. The first insulating layer comprises silicon, oxygen, and hydrogen. The semiconductor device comprises a second insulating layer made of silicon and oxygen.

2. It has a semiconductor layer, a first insulating layer, a second insulating layer, and a conductive layer. The semiconductor layer is located on the first insulating layer, The second insulating layer is located on the semiconductor layer, The semiconductor layer has a region that overlaps with the conductive layer via the second insulating layer, The semiconductor layer comprises a first metal oxide layer, a second metal oxide layer on the first metal oxide layer, and a third metal oxide layer on the second metal oxide layer. The first metal oxide layer, the second metal oxide layer, and the third metal oxide layer each contain indium and oxygen. The film density of the first metal oxide layer is higher than the film density of the second metal oxide layer. The film density of the third metal oxide layer is higher than that of the second metal oxide layer. The first insulating layer comprises silicon, oxygen, and hydrogen. The semiconductor device comprises a second insulating layer made of silicon and oxygen.

3. In claim 1 or claim 2, Having a third insulating layer, The third insulating layer has a region that overlaps with the semiconductor layer via the first insulating layer, The semiconductor device comprises silicon and nitrogen as the third insulating layer.

4. In claim 3, The third insulating layer contains hydrogen, The semiconductor device wherein the third insulating layer has a region with a higher hydrogen concentration than the first insulating layer.

5. It comprises a semiconductor layer, a first insulating layer, a second insulating layer, a third insulating layer, a fourth insulating layer, and a conductive layer. The second insulating layer is located on the first insulating layer, The semiconductor layer is located on the second insulating layer, The third insulating layer is located on the semiconductor layer, The semiconductor layer has a region that overlaps with the conductive layer via the third insulating layer, The fourth insulating layer is located on the semiconductor layer, the third insulating layer, and the conductive layer. The semiconductor layer comprises a first metal oxide layer, a second metal oxide layer on the first metal oxide layer, and a third metal oxide layer on the second metal oxide layer. The first metal oxide layer, the second metal oxide layer, and the third metal oxide layer each contain indium and oxygen. The film density of the first metal oxide layer is higher than the film density of the second metal oxide layer. The film density of the third metal oxide layer is higher than that of the second metal oxide layer. The second insulating layer comprises silicon, oxygen, and hydrogen. The third insulating layer comprises silicon and oxygen, A semiconductor device wherein the first insulating layer and the fourth insulating layer each consist of silicon and nitrogen.

6. In claim 5, The semiconductor layer has a first region that overlaps with the conductive layer via the second insulating layer, and a pair of second regions that sandwich the first region. The semiconductor device wherein the fourth insulating layer has a region in contact with the second region.

7. In claim 5 or claim 6, The first insulating layer contains hydrogen, A semiconductor device wherein the first insulating layer has a region with a higher hydrogen concentration than the second insulating layer.

Citation Information

Patent Citations

  • Display device

    WO2016038508A1