Composite cathode active material, cathode, and lithium secondary battery
A composite cathode active material with lithium iron phosphate, lithium manganese iron phosphate, and lithium nickel composite oxide addresses the low capacity and energy density of lithium iron phosphate, enhancing energy density and low-temperature performance while maintaining cost-effectiveness.
Patent Information
- Application Number
- JP2026078093
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2026-04-30
- Filing Date
- 2026-05-07
- Publication Date
- 2026-11-19
AI Technical Summary
Lithium iron phosphate compounds in lithium secondary batteries offer superior lifespan characteristics but suffer from low capacity and energy density, while mixtures with lithium nickel-based composite oxides improve energy density but compromise low-temperature performance.
A composite cathode active material comprising lithium iron phosphate, lithium manganese iron phosphate, and lithium nickel composite oxide, with specific weight and volume ratios and particle size distributions, to balance energy density, lifespan, and low-temperature performance.
The composite cathode active material achieves high pellet density, improved capacity and energy density, excellent lifespan characteristics, and stable operation in low-temperature environments, maintaining price competitiveness.
Smart Images

Figure 2026182824000001_ABST
Abstract
Description
[Technical Field]
[0001] This relates to composite cathode active materials, cathodes, and lithium secondary batteries. [Background technology]
[0002] Lithium-ion batteries, which offer high energy density while remaining portable, are primarily used as power sources for mobile information terminals such as mobile phones, laptops, and smartphones. Recently, research has been actively conducted on using high-energy-density lithium-ion batteries as power sources or energy storage sources for hybrid and electric vehicles.
[0003] Known positive electrode active materials used in lithium secondary batteries include lithium cobalt oxides such as lithium cobalt oxide (LiCoO2), lithium nickel-based composite oxides such as lithium nickel-cobalt-manganese oxide (NCM) and lithium nickel-cobalt-aluminum oxide (NCA), and lithium iron phosphate compounds. Among these, due to the high prices of nickel (Ni) and cobalt (Co), low-cost lithium iron phosphate compounds and lithium manganese iron phosphate compounds, which mainly consist of relatively inexpensive iron (Fe) raw materials, are attracting attention.
[0004] Lithium iron phosphate and lithium manganese iron phosphate compounds have an olivine structure and exhibit superior lifespan characteristics compared to other cathode materials, but they have the disadvantage of low capacity and energy density. [Overview of the Initiative] [Problems that the invention aims to solve]
[0005] To provide a composite cathode active material, cathode, and lithium secondary battery that maintain price competitiveness while achieving high pellet density, excellent lifespan characteristics, superior low-temperature performance, low resistance, and improved capacity and energy density. [Means for solving the problem]
[0006] One embodiment provides a composite positive electrode active material comprising: a first positive electrode active material in the form of a granular material containing a lithium iron phosphate compound and in which a plurality of primary particles are aggregated; a second positive electrode active material in the form of a granular material containing a lithium manganese iron phosphate compound and in which a plurality of primary particles are aggregated; and a third positive electrode active material containing a lithium nickel composite oxide, wherein the weight ratio of the first positive electrode active material to the second positive electrode active material is 5:1 to 1:1, the third positive electrode active material is contained in an amount of 5% to 25% by weight based on 100% by weight of the total composite positive electrode active material, and granules with a particle size of 10 μm or more are contained in an amount of 30% by volume or more based on 100% by volume of the total of the first positive electrode active material and the second positive electrode active material.
[0007] Other embodiments include a positive electrode current collector and a positive electrode active material layer located on the positive electrode current collector, wherein the positive electrode active material layer includes the aforementioned composite positive electrode active material.
[0008] Another embodiment provides a lithium secondary battery comprising the aforementioned positive electrode, negative electrode, and electrolyte. [Effects of the Invention]
[0009] A composite cathode active material according to one embodiment ensures price competitiveness while exhibiting high pellet density, high initial charge / discharge capacity and efficiency, improved average voltage, excellent lifetime characteristics and high-rate lifetime characteristics, improved low-temperature characteristics (e.g., low-temperature capacity and / or low-temperature storage characteristics), and low resistance while maintaining high capacity per unit volume and high energy density. [Brief explanation of the drawing]
[0010] [Figure 1] This is a schematic perspective view showing a section of a cylindrical lithium-ion secondary battery that has been cut open. [Figure 2] This is a schematic cross-sectional view of a prismatic lithium-ion secondary battery. [Figure 3] This is a schematic disassembled perspective view of a pouch-type lithium secondary battery. [Figure 4]This is a schematic disassembled perspective view of a pouch-type lithium secondary battery. [Modes for carrying out the invention]
[0011] The following describes specific embodiments in detail so that they can be easily implemented by those with ordinary skill in the art. However, the present invention can be realized in a variety of different forms and is not limited to the embodiments described herein.
[0012] The terms used herein are used solely to describe exemplary embodiments and are not intended to limit the invention. Singular expressions include plural expressions unless the context clearly indicates otherwise.
[0013] Here, "these combinations" refers to mixtures of components, laminates, composites, copolymers, alloys, blends, reaction products, etc.
[0014] Here, terms such as “include,” “equip,” or “possess” are intended to specify the existence of the implemented features, figures, stages, components, or combinations thereof, and should be understood not to preemptively exclude the existence or possibility of adding one or more other features, figures, stages, components, or combinations thereof.
[0015] To clearly represent various layers and regions in the drawings, thicknesses are shown enlarged, and similar parts are given the same drawing reference numerals throughout the specification. When a layer, film, region, plate, or other part is said to be "on top of" or "on" another part, this includes not only when it is "directly on top of" another part, but also when there is another part in between. Conversely, when a part is said to be "directly on top of" another part, it means that there is no other part in between.
[0016] Furthermore, the term "layer" here includes not only the shapes formed on the entire surface when observed in a plan view, but also the shapes formed on a portion of the surface.
[0017] The average particle size can be measured by methods widely known to those skilled in the art, for example, by a particle size analyzer, or by transmission electron microscope images or scanning electron microscope images. Alternatively, it can be measured using dynamic light scattering, and the average particle size value can be calculated after counting the number of particles for each particle size range through data analysis. Unless otherwise defined, the average particle size is the diameter (D) of the particle whose cumulative volume in the particle size distribution is 50% by volume. 50 ) can mean. Also, unless otherwise defined, the average particle size is the diameter (D) of the particle whose cumulative volume in the particle size distribution is 50% by volume, obtained by measuring the size (diameter or length of the long axis) of more than 20 randomly selected particles in a scanning electron microscope image. 50 This could be the average particle size taken from ).
[0018] Here, "or" is not interpreted as having an exclusive meaning; for example, "A or B" is interpreted as including A, B, A+B, etc.
[0019] The term "metal" is interpreted as encompassing general metals, transition metals, and metalloids.
[0020] Composite positive electrode active material One embodiment provides a composite positive electrode active material comprising: a first positive electrode active material in the form of a granular material containing a lithium iron phosphate compound and aggregated from a plurality of primary particles; a second positive electrode active material in the form of a granular material containing a lithium manganese iron phosphate compound and aggregated from a plurality of primary particles; and a third positive electrode active material containing a lithium nickel composite oxide, wherein the weight ratio of the first positive electrode active material to the second positive electrode active material is 5:1 to 1:1, the third positive electrode active material is present in an amount of 5% to 25% by weight based on 100% by weight of the total composite positive electrode active material, and granules with a particle size of 10 μm or more are present in an amount of 30% by volume or more based on 100% by volume of the total of the first and second positive electrode active materials. The first to third positive electrode active materials may be different from each other. The lithium iron phosphate compound, the lithium manganese iron phosphate compound, and the lithium nickel composite oxide may be different from each other.
[0021] Recently, lithium iron phosphate compounds have been attracting attention due to their excellent structural stability, high heat resistance, and competitive pricing. However, while lithium iron phosphate compounds have excellent lifespan characteristics, they suffer from the disadvantages of low capacity and energy density.
[0022] To compensate for this, there have been attempts to use a mixture of lithium iron phosphate-based compounds and lithium nickel-based composite oxides to increase capacity. However, while this allows for high energy density, it can result in inferior low-temperature performance.
[0023] Conventional lithium-ion secondary batteries experience a rapid decline in performance at sub-zero temperatures (e.g., below -20°C), with reduced discharge capacity and increased internal resistance making normal operation difficult. Furthermore, low temperatures can decrease the diffusion rate of lithium ions within the electrodes, increasing electrolyte viscosity and reducing output, potentially shortening battery life in the long term. Improving low-temperature performance to address these issues would enable stable use in extreme environments such as military equipment, polar research equipment, and satellites, significantly improving their applicability. Therefore, developing a secondary battery with excellent lifespan characteristics, high capacity and energy density, and improved low-temperature performance is a crucial research challenge. To this end, one embodiment proposes the following composite cathode active material.
[0024] One embodiment of the composite cathode active material includes a first cathode active material containing a lithium iron phosphate compound and having a granular form in which multiple primary particles are aggregated. It also includes a second cathode active material containing a lithium manganese iron phosphate compound and having a granular form in which multiple primary particles are aggregated. At this time, granules with a particle size of 10 μm or more are present in an amount of 30% by volume or more, based on 100% by volume of the total of the first and second cathode active materials. Furthermore, in order to achieve high energy density, a third cathode active material containing a lithium nickel-based composite oxide is included. At this time, the weight ratio of the first cathode active material to the second cathode active material is 5:1 to 1:1, and the third cathode active material is present in an amount of 5% to 25% by weight, based on 100% by weight of the total composite cathode active material.
[0025] Specifically, the weight ratio of the first positive electrode active material to the second positive electrode active material is 5:1 to 1:1. For example, the weight ratio of the first positive electrode active material to the second positive electrode active material may be 4.5:1 to 1:1, 4.0:1 to 1:1, 3.5:1 to 1:1, 3.0:1 to 1:1, 3.0:1 to 1.1:1, 3.0:1 to 1.2:1, 2.8:1 to 1.3:1, 2.6:1 to 1.4:1, or 2.4:1 to 1.4:1. In addition, the third positive electrode active material is included in an amount of 5% to 25% by weight based on 100% by weight of the total composite positive electrode active material, for example, 10% to 20% by weight, 15% to 25% by weight, 5% to 15% by weight, or 13% to 18% by weight. Within the aforementioned composition range, the battery's lifespan characteristics are maintained to be excellent, while its initial capacity and energy density can be improved. Furthermore, it can operate stably even in low-temperature environments, and in particular, it exhibits improved low-temperature capacity.
[0026] In this case, granules with a particle size of 10 μm or larger are included in an amount of 30 volume% or more, based on a total of 100 volume% of the first positive electrode active material and the second positive electrode active material. For example, the granules with a particle size of 10 μm or larger may be included in amounts of 30 volume% to 80 volume%, 40 volume% to 70 volume%, 40 volume% to 60 volume%, or 40 volume% to 50 volume%, based on a total of 100 volume% of the first positive electrode active material and the second positive electrode active material. Within this range, the compressibility between positive electrode active material particles is improved, increasing electrode density and thereby increasing energy density. Furthermore, structural stability is improved, and excellent lifetime characteristics can be achieved simultaneously with the increase in energy density. A method for measuring the proportion of granules with a particle size of 10 μm or larger may be, for example, by putting the positive electrode active material powder into a particle size analyzer, obtaining a particle size distribution curve, and measuring the volume ratio of particles with a particle size of 10 μm or larger. The particle size analyzer used was a Beckman Coulter counter LS13 320, and the measurement method was laser diffraction. The solvent used for the measurement was isopropyl alcohol (refractive index 1.377).
[0027] The aforementioned composite cathode active material exhibits the excellent cycle life characteristics of lithium iron phosphate compounds, the excellent low-temperature performance of lithium iron manganese phosphate compounds, and the excellent capacity and energy density characteristics of lithium nickel composite oxides. As a result, stable output characteristics and lifetime characteristics can be ensured even in low-temperature environments. Furthermore, by adjusting the particle size distribution and the composition ratio of each cathode active material, a balance can be achieved between energy density, lifetime characteristics, and low-temperature performance, thereby simultaneously ensuring high performance and price competitiveness.
[0028] The first positive electrode active material, the second positive electrode active material, and the third positive electrode active material will be described in detail below.
[0029] First positive electrode active material The first positive electrode active material includes a lithium iron phosphate compound. By including a lithium iron phosphate compound as the first positive electrode active material, the composite positive electrode active material can achieve excellent structural stability and thermal stability while maintaining price competitiveness.
[0030] The aforementioned lithium iron phosphate compound can be represented by chemical formula 1.
[0031] [Chemical formula 1] Li a1 Fe (1-x1) M 1 x1 PO4 In chemical formula 1, 0.90 ≤ a1 ≤ 1.5 and 0 ≤ x1 ≤ 0.4, and M 1 a1 is one or more elements from Al, B, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr. Here, 0.90 ≤ a1 ≤ 1.5 may also be true, for example, 0.90 ≤ a1 ≤ 1.2 or 0.95 ≤ a1 ≤ 1.1. Also, 0 ≤ x1 ≤ 0.4, 0 ≤ x1 ≤ 0.3, 0 ≤ x1 ≤ 0.2, 0 ≤ x1 ≤ 0.1, or 0.001 ≤ x1 ≤ 0.05.
[0032] Specifically, the lithium iron phosphate compound may include, but is not limited to, LiFePO4.
[0033] The lithium iron phosphate compound may further contain one or more elements from Al, Mg, Ti, and V as a doping element, and the one or more elements from Al, Mg, Ti, and V may be present in the lithium iron phosphate compound in an amount of 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium, in which case the rate characteristics and lifetime characteristics are improved.
[0034] As an example, the lithium iron phosphate compound further contains one or more elements from Ti and Al as doping elements, and the Ti content may be 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium, and the Al content may be 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium. In this case, the rate characteristics and lifetime characteristics are improved.
[0035] As an example, M in the above chemical formula 1 1 The formula may contain one or more elements from Al, Mg, Ti, and V, in which case the lifetime characteristics of the lithium iron phosphate positive electrode active material can be improved. In chemical formula 1, one or more elements from Al, Mg, Ti, and V may be present in amounts of 0.1 mol% to 0.5 mol%, or 0.1 mol% to 0.3 mol%, based on 100 mol% of the total metal excluding lithium, in which case the lifetime characteristics of the lithium iron phosphate positive electrode active material can be improved. For example, in chemical formula 1, 0.001 ≤ x1 ≤ 0.005, or 0.001 ≤ x1 ≤ 0.003 may be present.
[0036] As an example, the lithium iron phosphate-based compound of the first positive electrode active material, unlike the lithium manganese iron phosphate-based compound of the second positive electrode active material, may contain no manganese or contain manganese in a very small amount. Based on 100 mol% of all metals excluding lithium in the lithium iron phosphate-based compound, the manganese content may be 0 to 0.01 mol%, or as an example, may be 0 mol%. At this time, in Chemical Formula 1, M 1 may be one or more elements selected from Al, B, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr. According to an embodiment, by mixing the first positive electrode active material including the lithium iron phosphate-based compound containing no manganese and the second positive electrode active material including the lithium manganese iron phosphate-based compound containing manganese, it is possible to improve low-temperature characteristics while enhancing capacity, efficiency, and lifespan characteristics at the same time.
[0037] The first positive electrode active material is in the form of particles, and may be secondary particles in which a plurality of primary particles are aggregated. The secondary particles may have a spherical or elliptical spherical shape as the primary particles are closely aggregated with each other. The secondary particles can be referred to as granulated bodies. The composite positive electrode active material according to an embodiment can improve capacity and lifespan characteristics by including the first positive electrode active material in the form of granulated bodies.
[0038] The average particle diameter (D 50 ) of the secondary particles may be, for example, 5 μm to 25 μm, 7 μm to 20 μm, 8 μm to 15 μm, 8 μm to 12 μm, 8 μm to 10 μm, or 8 μm to 9 μm. The average particle diameter (D 50 ) of the primary particles forming the secondary particles may be 0.01 μm to 2 μm, 0.1 μm to 1.2 μm, or 0.5 μm to 0.9 μm, may be 500 nm or less as an example, and may be, for example, 10 nm to 400 nm, 20 nm to 300 nm, or 50 nm to 200 nm. When the average particle diameters of the secondary particles and the primary particles forming the same satisfy the above ranges, lifespan characteristics and energy density are improved.
[0039] The average particle size (D) of the secondary particles 50 ) For example, by arbitrarily selecting more than 30 particles from electron microscope images of the first positive electrode active material and measuring their particle size, the diameter (D) of the particle whose cumulative volume in the particle size distribution is 50% is determined. 50 ) may be taken as the average particle size. The average particle size of the primary particles forming the secondary particles is determined by measuring the size of more than 30 primary particles in an electron microscope image of the surface or cross-section of the particles, and taking the diameter (D) of the particle whose cumulative volume in the particle size distribution is 50% by volume. 50 This could be the average particle size taken from ).
[0040] The secondary particles may contain voids inside, and the porosity, which is the ratio of the area occupied by voids to the cross-sectional area of the secondary particles, may be about 20% to about 50%, for example, 20% to 40%, 20% to 30%, or 20% to 25%. As an example, the porosity may be measured by using an image analysis program such as Image J on a scanning electron microscope image of the cross-section of the secondary particles to measure the ratio of the area occupied by the voids inside the secondary particles to the cross-sectional area of the secondary particles. When the porosity inside the secondary particles satisfies the above range, primary particles can fill the voids during rolling, improving the pellet density, thereby improving the volume characteristics.
[0041] In this case, the granules of the first positive electrode active material having a particle size of 10 μm or more may be present in an amount of 30% or more by volume, based on 100% by volume of the total first positive electrode active material. For example, the granules of the first positive electrode active material having a particle size of 10 μm or more may be present in an amount of 30% to 80% by volume, 40% to 70% by volume, 40% to 60% by volume, or 40% to 50% by volume, based on 100% by volume of the total first positive electrode active material. Within this range, it can be seen that the energy density of the electrode is high and the lifetime characteristics are improved. A method for measuring the proportion of granules with a particle size of 10 μm or more may be, for example, by putting the first positive electrode active material powder into a particle size analyzer, obtaining a particle size distribution curve, and measuring the volume ratio of particles with a particle size of 10 μm or more. The particle size analyzer used in this case was a Beckman Coulter counter LS13 320, and the measurement method was laser diffraction. The solvent used for the measurement was isopropyl alcohol (refractive index 1.377).
[0042] The first positive electrode active material may further include a carbon coating layer. The carbon coating layer can improve the electrical conductivity of the lithium iron phosphate compound and reduce the resistance of the positive electrode. The carbon coating layer can be formed using one or more raw materials from, for example, glucose, sucrose, lactose, starch, oligosaccharides, polyoligosaccharides, fructose, cellulose, polymers of furfuryl alcohol, block copolymers of ethylene and ethylene oxide, vinyl resins, cellulose resins, phenolic resins, pitch resins, and tar resins. Specifically, the carbon coating layer can be formed by placing the raw materials on the surface of the lithium iron phosphate compound particles and then firing them.
[0043] For example, the first positive electrode active material may further include a carbon coating layer located on the surface of the secondary particles and / or on the surface of the primary particles forming the secondary particles. The carbon coating layer may be as described above.
[0044] The first positive electrode active material may further include single particle forms in addition to the secondary particle forms described above. The average particle size (D) of the single particles containing the lithium iron phosphate compound. 50 The average particle size (D) of a single particle may be 2 μm or less, for example, 100 nm to 2 μm, 200 nm to 1.5 μm, 300 nm to 1.2 μm, or 400 nm to 1.0 μm. 50 ) is the average particle size (D) of the secondary particles mentioned above. 50 ) may be smaller than the average particle size (D) of the primary particles that form the secondary particles. 50 ) may be the same as or even larger. The average particle size of a single particle can be measured by arbitrarily selecting more than 30 single particles from an electron microscope image of the first positive electrode active material and determining the particle size of the particle whose cumulative volume in the particle size distribution is 50% by volume (D 50 This could be the average particle size taken from ).
[0045] Second positive electrode active material The second positive electrode active material includes a lithium manganese iron phosphate compound. By including a lithium manganese iron phosphate compound as the second positive electrode active material, the composite positive electrode active material can maintain price competitiveness while also exhibiting excellent rate characteristics and low-temperature performance.
[0046] The aforementioned lithium manganese iron phosphate compound can be represented by chemical formula 2.
[0047] [Chemical formula 2] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO4 In chemical formula 2, 0.90 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² ≤ 0.9, and 0.1 ≤ x² + y² < 1, and M 2a² is one or more elements from Al, B, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr. Here, 0.90 ≤ a² ≤ 1.5 may also be true, for example, 0.90 ≤ a² ≤ 1.2 or 0.95 ≤ a² ≤ 1.1. Also, 0.1 ≤ x² ≤ 0.9, 0.3 ≤ x² ≤ 0.9 or 0.4 ≤ x² ≤ 0.8 may be true, and 0 ≤ y² ≤ 0.4, 0 ≤ y² ≤ 0.3, 0 ≤ y² ≤ 0.2, 0 ≤ y² ≤ 0.1 or 0 ≤ y² ≤ 0.05 may be true. Specifically, the lithium manganese iron phosphate compound is LiMn 0.7 Fe 0.3 PO4, LiMn 0.6 Fe 0.4 PO4, LiMn 0.5 Fe 0.5 PO4, LiMn 0.4 Fe 0.6 PO4 and LiMn 0.3 Fe 0.7 The PO4 compound may or may not contain one or more compounds.
[0048] The lithium manganese iron phosphate compound may further contain one or more elements from Al, Mg, Ti, and V as a doping element, and the amount of one or more of Al, Mg, Ti, and V in the lithium manganese iron phosphate compound may be 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium, in which case the rate characteristics and lifetime characteristics are improved.
[0049] As an example, the lithium manganese iron phosphate compound further contains one or more elements from Ti and Al as doping elements, and the Ti content may be 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium, and the Al content may be 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium. In this case, the rate characteristics and lifetime characteristics are improved.
[0050] M in chemical formula 2 2The compound may contain one or more elements from Al, Mg, Ti, and V, in which case the lifetime characteristics of the lithium iron manganese phosphate-based cathode active material can be improved. For example, the compound may have a ratio of 0.001 ≤ x² ≤ 0.005 or 0.001 ≤ x² ≤ 0.003 in chemical formula 2, in which case the lifetime characteristics of the lithium iron manganese phosphate-based cathode active material can be improved.
[0051] The second positive electrode active material is in particulate form and may be secondary particles formed by the aggregation of multiple primary particles. The secondary particles may be spherical or ellipsoidal in shape due to the close aggregation of primary particles. The secondary particles can be described as a granule. The average particle size (D) of the secondary particles 50 The average particle size (D) of the primary particles forming the secondary particles may be, for example, 5 μm to 25 μm, 7 μm to 20 μm, or 8 μm to 15 μm, 9 μm to 12 μm, or 9 μm to 10 μm. 50 The particle size may be 0.01 μm to 2 μm, 0.1 μm to 1.2 μm, or 0.5 μm to 0.9 μm, and may be 500 nm or less, for example, 10 nm to 400 nm, 20 nm to 300 nm, or 50 nm to 200 nm. When the average particle size of the secondary particles and the primary particles forming them satisfies the above range, the lifetime characteristics and energy density are improved.
[0052] The average particle size (D) of the secondary particles 50 As an example, the particle size of a particle whose cumulative volume in the particle size distribution is 50% by volume is determined by arbitrarily selecting more than 30 particles from electron microscope images of the second positive electrode active material and measuring their particle size. 50 ) may be taken as the average particle size. The average particle size of the primary particles forming the secondary particles is determined by measuring the size of more than 30 primary particles in an electron microscope image of the surface or cross-section of the particles, and taking the diameter (D) of the particle whose cumulative volume in the particle size distribution is 50% by volume. 50 This could be the average particle size taken from ).
[0053] The secondary particles may contain voids inside, and the porosity, which is the ratio of the area occupied by voids to the cross-sectional area of the secondary particles, may be about 20% to about 50%, for example, 20% to 40%, 20% to 30%, or 20% to 25%. As an example, the porosity may be measured by using an image analysis program such as Image J on a scanning electron microscope image of the cross-section of the secondary particles to measure the ratio of the area occupied by voids within the secondary particles to the cross-sectional area of the secondary particles. When the porosity within the secondary particles satisfies the above range, primary particles can fill the voids during rolling, improving the pellet density, thereby improving the volume characteristics.
[0054] At this time, the granules of the second positive electrode active material having a particle size of 10 μm or more are present in an amount of 30 volume% or more based on 100 volume% of the total second positive electrode active material. For example, the granules of the second positive electrode active material having a particle size of 10 μm or more may be present in an amount of 30 volume% to 80 volume%, 35 volume% to 70 volume%, 40 volume% to 60 volume%, or 40 volume% to 50 volume%, based on 100 volume% of the total second positive electrode active material. Within this range, the energy density of the electrode is high and the lifetime characteristics are improved. A method for measuring the proportion of granules with a particle size of 10 μm or more may be, for example, by putting the second positive electrode active material powder into a particle size analyzer, obtaining a particle size distribution curve, and measuring the volume ratio of particles with a particle size of 10 μm or more. The particle size analyzer used at this time was a Beckman Coulter counter LS13 320, and the measurement method was laser diffraction. The solvent used for the measurement was isopropyl alcohol (refractive index 1.377).
[0055] The second cathode active material may further include a carbon coating layer. The carbon coating layer can be formed in the same manner as the first cathode active material described above.
[0056] The second positive electrode active material may further include single particle forms in addition to the secondary particle forms described above. The average particle size (D) of the single particles containing the lithium manganese iron phosphate compound. 50The average particle size (D) of a single particle may be 2 μm or less, for example, 100 nm to 2 μm, 200 nm to 1.5 μm, 300 nm to 1.2 μm, or 400 nm to 1.0 μm. 50 ) is the average particle size (D) of the secondary particles mentioned above. 50 ) may be smaller than the average particle size (D) of the primary particles that form the secondary particles. 50 ) may be the same as or even larger. The average particle size of a single particle is, as an example, determined by arbitrarily selecting more than 30 single particles from an electron microscope image of the second positive electrode active material, measuring their particle size, and determining the diameter of the particle whose cumulative volume in the particle size distribution is 50% by volume (D 50 This could be the average particle size taken from ).
[0057] Third positive electrode active material The third positive electrode active material according to one embodiment contains a lithium nickel-based composite oxide. By containing the lithium nickel-based composite oxide, the composite positive electrode active material can have increased capacity and be driven at high voltages. Specifically, the lithium nickel-based composite oxide can be represented by the following chemical formula 3.
[0058] [Chemical formula 3] Li a3 Ni x3 M 3 y3 M 4 z3 O 2-b3 X b3 In chemical formula 3, 0.9 ≤ a³ ≤ 1.8, 0.3 ≤ x³ ≤ 1, 0 ≤ y³ ≤ 0.7, 0 ≤ z³ ≤ 0.7, 0.9 ≤ x³ + y³ + z³ ≤ 1.1, and 0 ≤ b³ ≤ 0.1, M 3 and M 4 Each of the following elements is independently one or more of the elements Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more of the elements F, P, and S.
[0059] In chemical formula 3, either 0.6 ≤ x³ ≤ 1, 0 ≤ y³ ≤ 0.4, and 0 ≤ z³ ≤ 0.4, or 0.8 ≤ x³ ≤ 1, 0 ≤ y³ ≤ 0.2, and 0 ≤ z³ ≤ 0.2, or 0.9 ≤ x³ < 1, 0 <y3≦0.1、および0≦z3≦0.1であってもよい。
[0060] The aforementioned lithium nickel-based composite oxide can be represented by chemical formula 4 or chemical formula 5 below as a specific example.
[0061] [Chemical formula 4] Li a4 Ni x4 Co y4 M 5 z4 O 2-b4 X b4 In the above chemical formula 4, 0.9 ≤ a4 ≤ 1.2, 0.3 ≤ x4 < 1, 0 <y4≦0.7、0≦z4≦0.7、0.9≦x4+y4+z4≦1.1、および0≦b4≦0.1であり、M 5 X is one or more elements from Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more elements from F, P, and S.
[0062] In the aforementioned chemical formula 4, 0.3≦x4≦0.8, 0.1≦y4≦0.6, and 0.1≦z4≦0.6 may be true, or 0.3≦x4≦0.6, 0.2≦y4≦0.5, and 0.2≦z4≦0.5 may be true, or 0.7≦x4<1, 0.05≦y4≦0.3, and 0.001≦z4≦0.02 may be true, or 0.8≦x4≦0.9, 0.1≦y4≦0.2, and 0.008≦z4≦0.012 may be true.
[0063] [Chemical formula 5] Li a5 Ni x5 Co y5 M 6 z5 M 7 w5 O 2-b5 X b5 In the above chemical formula 5, 0.9≦a5≦1.2, 0.3≦x5≦0.98, 0.01≦y5≦0.69, 0.01≦z5≦0.69, 0≦w5≦0.68, 0.9≦x5+y5+z5+w5≦1.1, and 0≦b5≦0.1, M 6 is one or more elements from Al and Mn, and M 7 X is one or more elements from B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more elements from F, P, and S.
[0064] In the aforementioned chemical formula 5, 0.3 ≤ x 5 ≤ 0.8, 0.1 ≤ y 5 ≤ 0.6, 0.1 ≤ z 5 ≤ 0.6, and 0 ≤ w 5 ≤ 0.5, or 0.3 ≤ x 5 ≤ 0.6, 0.2 ≤ y 5 ≤ 0.5, 0.2 ≤ z 5 ≤ 0.5, and 0 ≤ w 5 ≤ 0.3.
[0065] The lithium-nickel composite oxide may also be a high-nickel cathode active material. For example, in the lithium-nickel composite oxide, the nickel content may be 80 mol% or more based on 100 mol% of the total metal excluding lithium, and may be, for example, 85 mol% or more, 90 mol% or more, 91 mol% or more, 94 mol% or more, or 99 mol% or less. Such a high-nickel cathode active material can achieve high capacity and high performance.
[0066] The third positive electrode active material containing the lithium nickel-based composite oxide is in particulate form and may include first particles, second particles, or a combination thereof.
[0067] The first particle may be a secondary particle formed by the aggregation of multiple primary particles, and the second particle may be a secondary particle, a single particle, or a combination thereof. The secondary particle and single particle may be spherical, ellipsoidal, polyhedronal, or irregular in shape, and the primary particles forming the secondary particle may be spherical, ellipsoidal, plate-shaped, or a combination thereof.
[0068] The average particle size (D) of the first particle 50 The average particle size (D) of the second particle may be, for example, 10 μm to 25 μm, or 12 μm to 18 μm. 50 The average particle size (D) of the third positive electrode active material may be, for example, 1 μm to 8 μm, or 2 μm to 5 μm. 50 The particle size may be 1 μm to 20 μm, 5 μm to 20 μm, or 8 μm to 18 μm. Here, the average particle size (D 50 The particle size can be determined by randomly measuring the size (diameter or length of the major axis) of more than 20 particles in a scanning electron microscope image of the positive electrode active material, obtaining a particle size distribution, and taking the diameter of the particle whose cumulative volume is 50% by volume in the particle size distribution as the average particle size.
[0069] The third positive electrode active material may contain 40% to 95% by weight of the first particles and 5% to 60% by weight of the second particles, based on a total of 100% by weight of the first and second particles. For example, it may contain 60% to 80% by weight of the first particles and 20% to 40% by weight of the second particles. When the first and second particles are mixed in the third positive electrode active material within the above range, the energy density and output performance can be improved compared to when using existing single-particle-size third positive electrode active materials, improving cycle life and maximizing the efficiency of the lithium secondary battery.
[0070] The first positive electrode active material may be included in amounts of 37.5% to 70% by weight, 40% to 70% by weight, or 50% to 60% by weight, based on 100% by weight of the entire composite positive electrode active material, and the second positive electrode active material may be included in amounts of 20% to 47.5% by weight, 25% to 45% by weight, 30% to 45% by weight, or 35% to 45% by weight, based on 100% by weight of the entire composite positive electrode active material. In this case, the weight ratio of the first positive electrode active material to the second positive electrode active material is 5:1 to 1:1, and may be, for example, 4.5:1 to 1:1, 4.0:1 to 1:1, 3.5:1 to 1:1, 3.0:1 to 1:1, 3.0:1 to 1.1:1, 3.0:1 to 1.2:1, 2.8:1 to 1.3:1, 2.6:1 to 1.4:1, or 2.4:1 to 1.4:1. The third positive electrode active material may be included in an amount of 5% to 20% by weight, 5% to 10% by weight, or 10% to 20% by weight, based on 100% by weight of the total composite positive electrode active material. Within this range, the composite positive electrode active material can be driven stably at high voltage while being price-competitive, its energy density can be maximized, its low-temperature characteristics and life characteristics can be improved, and a high-capacity and high-density battery can be realized.
[0071] The pellet density of the composite positive electrode active material according to one embodiment may be 2.2 g / cc to 3.0 g / cc, for example, 2.2 g / cc to 2.5 g / cc, 2.2 g / cc to 2.40 g / cc, 2.3 g / cc to 2.40 g / cc, or 2.34 g / cc to 2.40 g / cc. When the pellet density of the composite positive electrode active material satisfies the above range, high charge-discharge efficiency can be achieved while realizing high capacity per unit volume. The pellet density is determined by molding 3 g of the composite positive electrode active material (area: 1.298 cm²). 2 The measurement may have been taken after the mold bar was placed in the mold body, the mold set was placed in a hydraulic press, and then pressurized at a pressure of 4.0 tons for 30 seconds to pelletize the material.
[0072] positive electrode A positive electrode according to one embodiment includes a positive electrode current collector and a positive electrode active material layer located on the positive electrode current collector, which includes the aforementioned composite positive electrode active material. The positive electrode according to one embodiment includes the aforementioned composite positive electrode active material, which improves overall battery performance, specifically by improving low-temperature performance, and enabling high capacity, high efficiency, high energy density, and excellent lifespan characteristics.
[0073] positive electrode current collector The positive electrode current collector is not particularly limited as long as it is conductive without inducing a chemical change in the lithium secondary battery, and may be aluminum foil or stainless steel foil with a thickness of 10 μm to 15 μm.
[0074] Cathode active material layer The positive electrode active material layer includes the aforementioned composite positive electrode active material.
[0075] The specific details regarding the positive electrode active material are as described above.
[0076] The content of the composite positive electrode active material may be 60% to 99.9% by weight, 70% to 99.8% by weight, 80% to 99% by weight, or 90% to 98% by weight, based on 100% by weight of the positive electrode active material layer.
[0077] The positive electrode active material layer may further selectively include a binder, a conductive material, or a combination thereof.
[0078] The binder can effectively adhere the positive electrode active material particles to each other and to the positive electrode active material to the current collector. Typical examples of binders include, but are not limited to, polyvinyl alcohol, carboxymethylcellulose, hydroxypropylcellulose, diacetylcellulose, polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, polymers containing ethylene oxide, polyvinylpyrrolidone, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, epoxy resin, (meth)acrylic resin, polyester resin, and nylon.
[0079] The conductive material is used to impart conductivity to the electrodes, and any electronically conductive material that does not cause chemical changes within the battery can be used. Examples of conductive materials include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjenblack, carbon fibers, carbon nanofibers, and carbon nanotubes; metallic materials containing copper, nickel, aluminum, silver, etc., in the form of metal powders or metal fibers; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0080] In the positive electrode active material layer, the binder content may be approximately 0.1% to 5% by weight based on 100% by weight of the entire positive electrode active material layer, and the conductive material content may be 0.1% to 5% by weight based on 100% by weight of the entire positive electrode active material layer.
[0081] The density of the positive electrode active material layer may be between 2.2 g / cc and 3.0 g / cc, for example, 2.2 g / cc to 2.5 g / cc, 2.2 g / cc to 2.40 g / cc, 2.3 g / cc to 2.40 g / cc, or 2.34 g / cc to 2.40 g / cc. When the density of the positive electrode active material layer satisfies the above range, high charge and discharge efficiency can be achieved while realizing high capacity per unit volume. The density of the positive electrode active material layer refers to the ratio of the weight of the positive electrode active material layer to its volume in a rolled positive electrode. The density of the positive electrode active material layer can be determined by measuring the cross-sectional area, thickness, and weight of the positive electrode active material layer excluding the positive electrode current collector, calculating the volume by multiplying the cross-sectional area and thickness, and then dividing the weight by the volume.
[0082] Lithium-ion battery A lithium secondary battery according to one embodiment includes the positive electrode, negative electrode, and electrolyte described above. The lithium secondary battery may include the positive electrode, negative electrode, a separator located between the positive electrode and the negative electrode, and an electrolyte.
[0083] Lithium-ion batteries are classified into cylindrical, prismatic, pouch-type, and coin-type based on their form. Figures 1 to 4 are schematic diagrams showing a lithium-ion battery according to one embodiment, with Figure 1 being cylindrical, Figure 2 being prismatic, and Figures 3 and 4 being pouch-type batteries. Specifically, Figure 1 is a schematic perspective view showing a part of a cylindrical lithium-ion battery cut off, Figure 2 is a schematic cross-sectional view showing a prismatic lithium-ion battery, and Figures 3 and 4 are schematic exploded perspective views of a pouch-type lithium-ion battery.
[0084] Referring to Figures 1 to 4, the lithium secondary battery 100 may include an electrode assembly 40 with a separator 30 interposed between a positive electrode 10 and a negative electrode 20, and a case 50 in which the electrode assembly 40 is housed. The positive electrode 10, the negative electrode 20, and the separator 30 may be impregnated with an electrolyte (not shown). The lithium secondary battery 100 may include a sealing member 60 that seals the case 50, as shown in Figure 1. Also in Figure 2, the lithium secondary battery 100 may include a positive electrode lead tap 11 and a positive electrode terminal 12, a negative electrode lead tap 21 and a negative electrode terminal 22. As shown in Figures 3 and 4, the lithium secondary battery 100 may include electrode taps 70, namely a positive electrode tap 71 and a negative electrode tap 72, which serve as electrical pathways for guiding the current formed in the electrode assembly 40 to the outside.
[0085] negative electrode A negative electrode for a lithium secondary battery includes a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector. The negative electrode active material layer comprises a negative electrode active material and may further optionally include a binder, a conductive material, or a combination thereof.
[0086] The negative electrode current collector is not particularly limited as long as it is conductive without inducing a chemical change in the lithium secondary battery, and may be copper foil with a thickness of 10 μm to 15 μm.
[0087] The negative electrode active material includes a substance capable of reversibly intercalating / deintercalating lithium ions, lithium metal, an alloy of lithium metal, a substance that can be doped and dedoped with lithium, or a transition metal oxide.
[0088] Examples of the substance capable of reversibly intercalating / deintercalating the lithium ions include carbon-based negative electrode active materials, which may include, for example, crystalline carbon, amorphous carbon, or a combination thereof. Examples of the crystalline carbon include graphite such as amorphous, plate-like, flake, spherical or fibrous natural graphite or artificial graphite, and examples of the amorphous carbon include soft carbon or hard carbon, mesophase pitch carbide, calcined coke, and the like.
[0089] As the lithium metal alloy, an alloy of lithium and a metal selected from Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, and Sn can be used.
[0090] As the substance capable of being doped and dedoped with lithium, a Si-based negative electrode active material or a Sn-based negative electrode active material can be used. Examples of the Si-based negative electrode active material include silicon, a silicon-carbon composite, SiO x (0<x≦2), a Si-Q alloy (where Q is an element selected from alkali metals, alkaline earth metals, Group 13 elements, Group 14 elements (excluding Si), Group 15 elements, Group 16 elements, transition metals, rare earth elements, and combinations thereof, for example, selected from Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db, Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Tl, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof), or a combination thereof. The Sn-based negative electrode active material may be Sn, SnO2, a Sn alloy, or a combination thereof.
[0091] The silicon-carbon composite may be a composite of silicon and amorphous carbon. The average particle diameter (D of the silicon-carbon composite particles 50The particle size may be, for example, 0.5 μm to 20 μm. According to one embodiment, the silicon-carbon composite may be in the form of silicon particles and amorphous carbon coating on the surface of the silicon particles. For example, it may include secondary particles (core) formed by granulating primary silicon particles, and an amorphous carbon coating layer (shell) located on the surface of these secondary particles. The amorphous carbon may also be located between the primary silicon particles, for example, the primary silicon particles may be coated with amorphous carbon. The secondary particles may be dispersed in the amorphous carbon matrix.
[0092] The silicon-carbon composite may further contain crystalline carbon. For example, the silicon-carbon composite may include a core containing crystalline carbon and silicon particles and an amorphous carbon coating layer located on the surface of this core. The crystalline carbon may be artificial graphite, natural graphite, or a combination thereof. The amorphous carbon may be soft carbon or hard carbon, mesophase pitch carbide, calcined coke, etc.
[0093] When the silicon-carbon composite contains silicon and amorphous carbon, the silicon content may be 10% to 50% by weight per 100% by weight of the silicon-carbon composite, and the amorphous carbon content may be 50% to 90% by weight. Furthermore, when the silicon-carbon composite contains silicon, amorphous carbon, and crystalline carbon, the silicon content may be 10% to 50% by weight per 100% by weight of the silicon-carbon composite, the crystalline carbon content may be 10% to 70% by weight, and the amorphous carbon content may be 20% to 40% by weight.
[0094] Furthermore, the thickness of the amorphous carbon coating layer may be 5 nm to 100 nm. The average particle size (D) of the silicon particles (primary particles) 50 The size of the silicon particles may be 10 nm to 1 μm, or 10 nm to 200 nm. The silicon particles may exist as silicon alone, as a silicon alloy, or as an oxidized form. The oxidized form of silicon is SiO xcan be expressed as (0<x≦2). At this time, the atomic content ratio of Si:O indicating the degree of oxidation may be 99:1 to 33:67. In the present specification, unless otherwise defined, the average particle diameter (D 50 ) means the diameter of particles at a cumulative volume of 50% by volume in the particle size distribution.
[0095] The Si-based negative electrode active material or Sn-based negative electrode active material may be used by mixing with a carbon-based negative electrode active material. When the Si-based negative electrode active material or Sn-based negative electrode active material is mixed with the carbon-based negative electrode active material for use, the mixing ratio thereof may be 1:99 to 90:10 by weight.
[0096] The negative electrode active material may be included in an amount of 90 wt% to 99.8 wt%, or 94 wt% to 99 wt%, based on 100 wt% of the negative electrode active material layer.
[0097] The binder serves to make the negative electrode active material particles adhere well to each other and to make the negative electrode active material adhere well to the current collector. As the binder, a non-aqueous binder, an aqueous binder, a dry binder, or a combination thereof may be used.
[0098] Examples of the non-aqueous binder include polyvinyl chloride, carboxylated polyvinyl chloride, polyvinyl fluoride, ethylene-propylene copolymer, polystyrene, polyurethane, polytetrafluoroethylene, polyvinylidene fluoride, polyethylene, polypropylene, polyamideimide, polyimide, or combinations thereof.
[0099] The aqueous binder may be selected from styrene-butadiene rubber, (meth)acrylated styrene-butadiene rubber, (meth)acrylonitrile-butadiene rubber, (meth)acrylic rubber, butyl rubber, fluororubber, polyethylene oxide, polyvinylpyrrolidone, polyepichlorohydrin, polyphosphazene, poly(meth)acrylonitrile, ethylene propylene diene copolymer, polyvinylpyridine, chlorosulfonated polyethylene, latex, polyester resin, (meth)acrylic resin, phenolic resin, epoxy resin, polyvinyl alcohol, and combinations thereof.
[0100] When an aqueous binder is used as the negative electrode binder, it may further contain a cellulosic compound that can impart viscosity. This cellulosic compound can be a mixture of one or more carboxymethylcellulose, hydroxypropylmethylcellulose, methylcellulose, or alkali metal salts thereof. The alkali metal can be Na, K, or Li.
[0101] The dry binder is a polymeric substance that can be formed into fibers, and may be, for example, polytetrafluoroethylene, polyvinylidene fluoride, polyvinylidene fluoride-hexafluoropropylene copolymer, polyethylene oxide, or a combination thereof.
[0102] The conductive material is used to impart conductivity to the electrodes, and any electronically conductive material that does not cause chemical changes in the battery can be used. Specific examples include carbon-based materials such as natural graphite, artificial graphite, carbon black, acetylene black, Ketjenblack, carbon fibers, carbon nanofibers, and carbon nanotubes; metallic materials in the form of metal powders or metal fibers containing copper, nickel, aluminum, silver, etc.; conductive polymers such as polyphenylene derivatives; or mixtures thereof.
[0103] The content of the binder may be 0.1% to 5% by weight relative to 100% by weight of the negative electrode active material layer, and the content of the conductive material may be 0.1% to 5% by weight relative to 100% by weight of the negative electrode active material layer.
[0104] electrolyte The electrolyte for lithium secondary batteries may be, for example, an electrolyte solution, which contains a non-aqueous organic solvent and a lithium salt.
[0105] The non-aqueous organic solvent serves as a medium through which ions involved in the electrochemical reaction of the battery can move. The non-aqueous organic solvent may be a carbonate-based, ester-based, ether-based, ketone-based, or alcohol-based solvent, an aprotic solvent, or a combination thereof.
[0106] Examples of carbonate-based solvents that can be used include dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate (DPC), methyl propyl carbonate (MPC), ethyl propyl carbonate (EPC), methyl ethyl carbonate (MEC), ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate (BC). Examples of ester-based solvents that can be used include methyl acetate, ethyl acetate, n-propyl acetate, t-butyl acetate, methyl propionate, ethyl propionate, decanolide, mevalonolactone, valerolactone, and caprolactone. As ether-based solvents, dibutyl ether, tetraglyme, diglyme, dimethoxyethane, 2-methyltetrahydrofuran, 2,5-dimethyltetrahydrofuran, and tetrahydrofuran can be used. As ketone-based solvents, cyclohexanone can be used. As alcohol-based solvents, ethyl alcohol and isopropyl alcohol can be used, and as aprotic solvents, nitriles such as R-CN (where R is a linear, branched, or cyclic hydrocarbon group with 2 to 20 carbon atoms, and can include double bonds, aromatic rings, or ether groups); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane and 1,4-dioxolane; and sulfolanes can be used.
[0107] Non-aqueous organic solvents can be used alone or in combination of two or more, and the mixing ratio when using two or more can be appropriately adjusted according to the desired battery performance, which should be widely understood by those working in this field.
[0108] When using carbonate-based solvents, cyclic carbonates and linear carbonates can be mixed, and the cyclic carbonates and linear carbonates can be mixed in a volume ratio of 1:1 to 1:9.
[0109] The non-aqueous organic solvent may further contain an aromatic hydrocarbon organic solvent. For example, the carbonate solvent and the aromatic hydrocarbon organic solvent can be mixed and used in a volume ratio of 1:1 to 30:1.
[0110] The electrolyte may further contain vinylethylene carbonate, vinylene carbonate, or an ethylene carbonate-based compound to improve battery life.
[0111] Typical examples of the aforementioned ethylene carbonate compounds include fluoroethylene carbonate, difluoroethylene carbonate, chloroethylene carbonate, dichloroethylene carbonate, bromoethylene carbonate, dibromoethylene carbonate, nitroethylene carbonate, and cyanoethylene carbonate.
[0112] Lithium salts are substances that dissolve in organic solvents and act as a source of lithium ions in batteries, enabling the operation of basic lithium secondary batteries and facilitating the movement of lithium ions between the positive and negative electrodes. Typical examples of lithium salts include LiPF6, LiBF4, LiSbF6, LiAsF6, LiClO4, LiAlO2, LiAlCl4, LiPO2F2, LiCl, LiI, LiN(SO2C2F5)2, Li(FSO2)2N (lithium bis(fluorosulfonyl)imide; LiFSI), LiC4F9SO3, and LiN(C x F 2x+1 SO2)(C y F 2y+1 It may contain one or more selected from SO2) (where x and y are integers from 1 to 20), lithium trifluoromethanesulfonate, lithium tetrafluoroethanesulfonate, lithium difluorobis(oxalate)phosphate (LiDFOB), and lithium bis(oxalate) borate (LiBOB).
[0113] It is preferable to use lithium salts within a concentration range of 0.1 M to 2.0 M. When the lithium salt concentration falls within this range, the electrolyte has appropriate ionic conductivity and viscosity, resulting in excellent performance and effective lithium ion movement.
[0114] Separator Depending on the type of lithium secondary battery, a separator may be present between the positive and negative electrodes. Such separators can be made of polyethylene, polypropylene, polyvinylidene fluoride, or multilayer films of two or more layers of these materials. Mixed multilayer films such as polyethylene / polypropylene two-layer separators, polyethylene / polypropylene / polyethylene three-layer separators, and polypropylene / polyethylene / polypropylene three-layer separators can also be used.
[0115] The separator may include a porous substrate and a coating layer comprising organic, inorganic, or a combination thereof located on one or both sides of the porous substrate.
[0116] The porous substrate may be a polymer film formed from one polymer selected from polyethylene, polyolefins such as polypropylene, polyesters such as polyethylene terephthalate and polybutylene terephthalate, polyacetal, polyamide, polyimide, polycarbonate, polyetherketone, polyaryletherketone, polyetherimide, polyamideimide, polybenzimidazole, polyethersulfone, polyphenylene oxide, cyclic olefin copolymer, polyphenylene sulfide, polyethylene naphthalate, and polytetrafluoroethylene (e.g., Teflon®), or from a copolymer or mixture of two or more of these polymers. The porous substrate may contain glass fibers or a composite film of polymer and glass fibers.
[0117] The porous substrate may have a thickness of about 1 μm to 40 μm, for example, a thickness of 1 μm to 30 μm, 1 μm to 20 μm, 5 μm to 15 μm, or 10 μm to 15 μm.
[0118] The organic substance may include a (meth)acrylic copolymer comprising a first structural unit derived from (meth)acrylamide, and a second structural unit comprising at least one selected from a structural unit derived from (meth)acrylic acid or (meth)acrylate and a structural unit derived from (meth)acrylamidesulfonic acid or a salt thereof.
[0119] The inorganic substance may include, but is not limited to, inorganic particles selected from Al₂O₃, SiO₂, TiO₂, SnO₂, CeO₂, MgO, NiO, CaO, Ga₂O₃, ZnO, ZrO₂, Y₂O₃, SrTiO₃, BaTiO₃, Mg(OH)₂, boehmite, and combinations thereof. The average particle diameter (D 50 ) of the inorganic particles may be 1 nm to 2000 nm, for example, 100 nm to 1000 nm, or 100 nm to 700 nm.
[0120] The organic substance and the inorganic substance may be present in a mixed state in a single coating layer, or may be present in a form in which a coating layer containing the organic substance and a coating layer containing the inorganic substance are laminated.
[0121] The thickness of each of the coating layers may be 0.5 μm to 20 μm, for example, 1 μm to 10 μm, or 1 μm to 5 μm.
[0122] Hereinafter, Examples and Comparative Examples of the present invention will be described. However, the following Examples are merely illustrative of the present invention, and the present invention is not limited to the following Examples. [Examples]
[0123] Production example 1-1: Production of first positive electrode active material A slurry was prepared by wet grinding using FePO4 as an iron phosphate precursor, Li2CO3 as a lithium raw material, and water as a solvent. At this time, FePO4 and Li2CO3 were mixed so that the molar ratio of Fe:Li was 1:1. The wet-ground slurry was fed into a spray device at an input rate of 0.5 kg / min based on the total amount of raw materials (iron phosphate precursor and lithium raw material), spray-dried at a temperature of 250°C, and calcined at a temperature of 750°C for 8 hours to produce a calcined product. The calcined product was ground using a jet mill at a grinding speed of 5000 rpm, and then filtered to remove iron and packaged to produce the first positive electrode active material.
[0124] At this time, the first positive electrode active material consists of multiple primary particles (average particle size of the primary particles (D 50 The lithium iron phosphate compound (LiFePO4) is in the form of a granular material in which particles of approximately 100 nm to 300 nm are aggregated, and the average particle size of the first positive electrode active material is D 50 The particle size is 8 μm. At this time, particles with a particle size of 10 μm or larger are present in the first positive electrode active material at a concentration of 30 volume% relative to 100 volume% of the total first positive electrode active material. A method for measuring the proportion of granules with a particle size of 10 μm or larger may be, for example, to put the first positive electrode active material powder into a particle size analyzer, obtain a particle size distribution curve, and measure the volume ratio of particles with a particle size of 10 μm or larger. The particle size analyzer used at this time was a Beckman Coulter counter LS13 320, and the measurement method was laser diffraction. The solvent used for the measurement was isopropyl alcohol (refractive index 1.377).
[0125] Manufacturing Example 1-2: Manufacturing of the First Cathode Active Material The first positive electrode active material is a lithium iron phosphate compound (LiFePO4) in the form of a granular material in which multiple primary particles are aggregated, and the average particle size (D) of the first positive electrode active material is adjusted by controlling the spray pressure during spray drying. 50 The first positive electrode active material is manufactured in the same manner as in Manufacturing Example 1-1, except that the particle size of the first positive electrode active material is 8.3 μm, and particles with a particle size of 10 μm or more are included in 40% by volume based on 100% by volume of the total first positive electrode active material.
[0126] Manufacturing Example 1-3: Manufacturing of the First Cathode Active Material The first positive electrode active material is a lithium iron phosphate compound (LiFePO4) in the form of a granular material in which multiple primary particles are aggregated, and the average particle size (D) of the first positive electrode active material is adjusted by controlling the spray pressure during spray drying. 50 The first positive electrode active material is manufactured in the same manner as in Manufacturing Example 1-1, except that the particle size is 10 μm, and particles with a particle size of 10 μm or more in the first positive electrode active material are included in 50% by volume based on 100% by volume of the total first positive electrode active material.
[0127] Comparative Manufacturing Example 1-4: Manufacturing of the First Cathode Active Material The first positive electrode active material is a lithium iron phosphate compound (LiFePO4) in the form of a granular material in which multiple primary particles are aggregated, and the average particle size (D) of the first positive electrode active material is adjusted by controlling the spray pressure during spray drying. 50 The first positive electrode active material is manufactured in the same manner as in Manufacturing Example 1-1, except that the particle size of the first positive electrode active material is 7.6 μm, and particles with a particle size of 10 μm or more are included in 20% by volume based on 100% by volume of the total first positive electrode active material.
[0128] Manufacturing Example 2-1: Manufacturing of the second positive electrode active material A slurry was prepared by wet grinding using FePO4 as an iron phosphate precursor, MnCO3 as a manganese raw material, Li2CO3 as a lithium raw material, and water as a solvent. At this time, FePO4, MnCO3, and Li2CO3 were mixed so that the molar ratio of Fe:Mn:Li was 1:1:1. The wet-ground slurry was fed into a spray device at an input rate of 0.5 kg / min based on the total amount of raw materials (iron phosphate precursor, manganese raw material, and lithium raw material), spray-dried at a temperature of 250°C, and calcined at a temperature of 750°C for 8 hours to produce a calcined product. The calcined product was ground using a jet mill grinding device at a grinding speed of 5000 rpm, and then filtered to remove iron and packaged to produce the second positive electrode active material.
[0129] At this time, the second positive electrode active material consists of multiple primary particles (average particle size of the primary particles (D 50): about 50 nm to about 150 nm) are aggregated, which is a lithium manganese iron phosphate-based compound (LiMnFePO4) in the form of granulated particles, and the average particle diameter (D 50 ) of the second positive electrode active material is 9 μm. At this time, particles having a particle diameter of 10 μm or more in the second positive electrode active material are contained in an amount of 30% by volume based on 100% by volume of the entire second positive electrode active material.
[0130] Manufacturing Example 2-2: Manufacturing of the Second Cathode Active Material The second positive electrode active material is a lithium manganese iron phosphate-based compound (LiMnFePO4) in the form of granulated particles formed by aggregating a plurality of primary particles, and the spray pressure during spray drying is adjusted to control the average particle diameter (D 50 ) of the second positive electrode active material to 9.3 μm. A second positive electrode active material is produced in the same manner as in Production Example 2-1, except that particles having a particle diameter of 10 μm or more in the second positive electrode active material are contained in an amount of 40% by volume based on 100% by volume of the entire second positive electrode active material.
[0131] Manufacturing Example 2-3: Manufacturing of the Second Cathode Active Material The second positive electrode active material is a lithium manganese iron phosphate-based compound (LiMnFePO4) in the form of granulated particles formed by aggregating a plurality of primary particles, and the spray pressure during spray drying is adjusted to control the average particle diameter (D 50 ) of the second positive electrode active material to 10 μm. A second positive electrode active material is produced in the same manner as in Production Example 2-1, except that particles having a particle diameter of 10 μm or more in the second positive electrode active material are contained in an amount of 50% by volume based on 100% by volume of the entire second positive electrode active material.
[0132] Comparative Manufacturing Example 2-4: Manufacturing of the Second Cathode Active Material The second positive electrode active material is a lithium manganese iron phosphate-based compound (LiMnFePO4) in the form of granulated particles formed by aggregating a plurality of primary particles, and the spray pressure during spray drying is adjusted to control the average particle diameter (D 50 ) of the second positive electrode active material to 8.7 μm. A second positive electrode active material is produced in the same manner as in Production Example 2-1, except that particles having a particle diameter of 10 μm or more in the second positive electrode active material are contained in an amount of 20% by volume based on 100% by volume of the entire second positive electrode active material.
[0133] Manufacturing Example 3: Manufacturing of the third positive electrode active material Composition is Li 1.05 Ni 0.85 Co 0.14 Al 0.01 O2 and average particle size (D 50 ) is 15 μm, and the first particle is a secondary particle form in which multiple primary particles are aggregated, and the composition is Li 1.05 Ni 0.85 Co 0.14 Al 0.01 O2 and average particle size (D 50 The third positive electrode active material (lithium nickel-based composite oxide) is produced by mixing a second particle, which is 4 μm in size and in single-particle form, in a 7:3 weight ratio.
[0134] Example 1 (1) Manufacturing of the positive electrode The first cathode active material contains a lithium iron phosphate compound from Production Example 1-2, the second cathode active material contains a lithium manganese iron phosphate compound from Production Example 2-2, and the third cathode active material contains a lithium nickel-based composite oxide from Production Example 3. In this case, the composite cathode active material was produced by mixing the first cathode active material at 60% by weight, the second cathode active material at 25% by weight, and the third cathode active material at 15% by weight, based on 100% by weight of the total composite cathode active material.
[0135] A cathode active material composition was prepared by mixing the aforementioned composite cathode active material, polyvinylidene fluoride as a binder, and carbon nanotubes as a conductive material in a weight ratio of 97:1:2 (cathode active material:binder:conductive material). This was dispersed in N-methylpyrrolidone solvent to produce a cathode active material slurry, which was then coated onto a 13.5 μm thick Al foil, dried, and rolled to produce a cathode.
[0136] (2) Manufacturing of lithium secondary batteries A negative electrode active material slurry was prepared by dispersing 97.5% by weight of graphite as the negative electrode active material, 1.5% by weight of carboxymethylcellulose and 1% by weight of styrene-butadiene rubber as binders in distilled water. This slurry was coated onto a 10 μm thick Cu foil, dried, and rolled to produce the negative electrode.
[0137] An electrode assembly was manufactured by interposing a 10 μm thick polyethylene separator between the positive and negative electrodes, inserting it into a case, and then injecting an electrolyte to produce a lithium secondary battery (100 mAh level pouch cell). As the electrolyte, a solution of 1.15 M LiPF6 dissolved in a solvent mixed with EC (ethylene carbonate):EMC (ethyl methyl carbonate):DMC (dimethyl carbonate) in a volume ratio of 2:4:4 was used.
[0138] Example 2 The first positive electrode active material includes the lithium iron phosphate compound from Production Example 1-2, the second positive electrode active material includes the lithium manganese iron phosphate compound from Production Example 2-2, and the third positive electrode active material includes the lithium nickel composite oxide from Production Example 3. In this case, the positive electrode and lithium secondary battery were manufactured in the same manner as in Example 1, except that the composite positive electrode active material was manufactured by mixing the first positive electrode active material in amounts of 50% by weight, the second positive electrode active material in amounts of 35% by weight, and the third positive electrode active material in amounts of 15% by weight, based on 100% by weight of the total composite positive electrode active material.
[0139] Comparative Example 1 The first positive electrode active material includes the lithium iron phosphate compound from Production Example 1-2, and the third positive electrode active material includes the lithium nickel-based composite oxide from Production Example 3. In this case, the positive electrode and lithium secondary battery were manufactured in the same manner as in Example 1, except that the composite positive electrode active material was manufactured by mixing 85% by weight of the first positive electrode active material and 15% by weight of the third positive electrode active material, based on 100% by weight of the total composite positive electrode active material.
[0140] Comparative Example 2 The second positive electrode active material includes the lithium manganese iron phosphate compound from Production Example 2-2, and the third positive electrode active material includes the lithium nickel composite oxide from Production Example 3. In this case, the positive electrode and lithium secondary battery were manufactured in the same manner as in Example 1, except that the composite positive electrode active material was manufactured by mixing 85% by weight of the second positive electrode active material and 15% by weight of the third positive electrode active material, based on 100% by weight of the total composite positive electrode active material.
[0141] Comparative Example 3 The first positive electrode active material includes the lithium iron phosphate compound from Comparative Production Examples 1-4, the second positive electrode active material includes the lithium manganese iron phosphate compound from Comparative Production Examples 2-4, and the third positive electrode active material includes the lithium nickel-based composite oxide from Production Example 3. In this case, the positive electrode and lithium secondary battery were manufactured in the same manner as in Example 1, except that the mixture consisted of 60% by weight of the first positive electrode active material, 25% by weight of the second positive electrode active material, and 15% by weight of the third positive electrode active material, based on 100% by weight of the total composite positive electrode active material.
[0142] Comparative Example 4 The first positive electrode active material includes the lithium iron phosphate compound from Production Example 1-2, the second positive electrode active material includes the lithium manganese iron phosphate compound from Production Example 2-2, and the third positive electrode active material includes the lithium nickel composite oxide from Production Example 3. In this case, the positive electrode and lithium secondary battery were manufactured in the same manner as in Example 1, except that the composite positive electrode active material was manufactured by mixing the first positive electrode active material in amounts of 40% by weight, the second positive electrode active material in amounts of 45% by weight, and the third positive electrode active material in amounts of 15% by weight, based on 100% by weight of the total composite positive electrode active material.
[0143] Comparative Example 5 The first positive electrode active material includes the lithium iron phosphate compound from Production Example 1-2, the second positive electrode active material includes the lithium manganese iron phosphate compound from Production Example 2-2, and the third positive electrode active material includes the lithium nickel composite oxide from Production Example 3. In this case, the positive electrode and lithium secondary battery were manufactured in the same manner as in Example 1, except that the composite positive electrode active material was manufactured by mixing the first positive electrode active material in amounts of 30% by weight, the second positive electrode active material in amounts of 55% by weight, and the third positive electrode active material in amounts of 15% by weight, based on 100% by weight of the total composite positive electrode active material.
[0144] Comparative Example 6 The first positive electrode active material includes the lithium iron phosphate compound from Production Example 1-2, the second positive electrode active material includes the lithium manganese iron phosphate compound from Production Example 2-2, and the third positive electrode active material includes the lithium nickel-based composite oxide from Production Example 3. In this case, the positive electrode and lithium secondary battery were manufactured in the same manner as in Example 1, except that the composite positive electrode active material was manufactured by mixing the first positive electrode active material in amounts of 65% by weight, the second positive electrode active material in amounts of 20% by weight, and the third positive electrode active material in amounts of 15% by weight, based on 100% by weight of the total composite positive electrode active material.
[0145] Evaluation Example 1: Performance Evaluation of the First Positive Electrode Active Material Battery The performance of lithium secondary batteries (hereinafter referred to as the lithium secondary batteries of Manufacturing Example 1-1, Manufacturing Example 1-2, Manufacturing Example 1-3, and Comparative Manufacturing Example 1-4) was evaluated using positive electrodes containing 100% by weight of the first positive electrode active material. At this time, the positive electrode and lithium secondary battery were manufactured in the same manner as in Example 1, except that they contained 100% by weight of the first positive electrode active material.
[0146] (1) Initial charge / discharge capacity and efficiency evaluation Lithium secondary batteries containing the first positive electrode active material of Manufacturing Example 1-1, Manufacturing Example 1-2, Manufacturing Example 1-3, and Comparative Manufacturing Example 1-4 were charged at 25°C at a 0.2C rate until the battery voltage reached 3.8V, and then discharged at a 0.2C rate to a cutoff voltage of 2.5V. The initial charge / discharge capacity was measured, and the initial efficiency was calculated using the following formula 1. The results are shown in Table 1 below. [Formula 1] Initial efficiency [%] = [1 st Discharge capacity per cycle / 1 st [Charging capacity per cycle] × 100 (2) Average voltage and energy density
[0147] The average voltage at an initial discharge state of charge (SOC) of 50% for lithium secondary batteries containing the first positive electrode active material of Manufacturing Example 1-1, Manufacturing Example 1-2, Manufacturing Example 1-3, and Comparative Manufacturing Example 1-4 was measured, and the energy density was calculated using Equation 2, as shown in Table 1 below. The current density in Equation 2 is expressed as milliampere-hours (mAh / cm²). 2 The value was calculated from the total current passing through the battery divided by the geometric area of the battery's electrodes. [Formula 2] Energy density (Wh / L) = [(Current density at the positive electrode / Total cell thickness) × Average voltage]
[0148] (3) Low-temperature capacity evaluation Lithium secondary batteries containing the first positive electrode active material of Manufacturing Example 1-1, Manufacturing Example 1-2, Manufacturing Example 1-3, and Comparative Manufacturing Example 1-4 were charged at 25°C at a rate of 0.2C until the battery voltage reached 3.8V. After that, they were discharged at a rate of 0.2C to a cutoff voltage of 2.5V in an environment with a constant temperature bath set to -20°C, and the low-temperature discharge capacity at this time was measured. The results are shown in Table 1 below.
[0149] (4) Evaluation of life characteristics As described above, for the lithium secondary batteries of Manufacturing Example 1-1, Manufacturing Example 1-2, Manufacturing Example 1-3, and Comparative Manufacturing Example 1-4, which contain the first positive electrode active material, the initial charge-discharge cycle (i.e., the first cycle) was performed, and then the charge-discharge cycle was repeated 49 or more times under the same conditions as the initial charge-discharge (i.e., at 25°C, charging to 3.8V at a 0.2C rate and discharging to a cutoff voltage of 2.5V at a 0.2C rate was repeated 49 or more times). This resulted in a total of 50 or more charge-discharge cycles, including the first cycle. Next, the lifespan was calculated as the ratio of the discharge capacity after 50 cycles to the initial discharge capacity using the following formula 3, and the results are shown in Table 1 below. [Formula 3] Lifespan [%]=[50 th Discharge capacity per cycle / 1 st [Discharge capacity per cycle] × 100
[0150] (5) DC Internal Resistance Evaluation (DC-IR) For lithium secondary batteries containing the first positive electrode active material of Manufacturing Example 1-1, Manufacturing Example 1-2, Manufacturing Example 1-3, and Comparative Manufacturing Example 1-4, after charging to 50% SOC, charging and discharging are performed at a 1C rate for 10 seconds to obtain the charging voltage and discharging voltage, and the DC-IR value is calculated from these.
[0151] [Table 1]
[0152] Referring to Table 1, it can be seen that lithium secondary batteries containing Manufacturing Examples 1-1, 1-2, and 1-3, in which particles with a particle size of 10 μm or larger in the first positive electrode active material constitute 30% or more by volume based on 100% by volume of the total first positive electrode active material, show higher initial charge capacity and initial discharge capacity, improved initial efficiency, superior lifespan, improved energy density, improved low-temperature capacity, reduced internal resistance, and overall improved battery performance. Therefore, it can be seen that when manufacturing composite positive electrode active materials, a first positive electrode active material containing particles with a particle size of 10 μm or larger in the first positive electrode active material constitutes 30% or more by volume based on 100% by volume of the total first positive electrode active material, which can improve battery performance.
[0153] Evaluation Example 2: Performance Evaluation of a Second Positive Electrode Active Material Battery The performance of lithium secondary batteries (hereinafter referred to as the lithium secondary batteries of Manufacturing Example 2-1, Manufacturing Example 2-2, Manufacturing Example 2-3, and Comparative Manufacturing Example 2-4) was evaluated using positive electrodes containing 100% by weight of the second positive electrode active material. At this time, the positive electrode and lithium secondary battery were manufactured in the same manner as in Example 1, except that they contained 100% by weight of the second positive electrode active material.
[0154] At this time, the initial charge / discharge capacity, initial efficiency, average voltage, energy density, low-temperature capacity, lifetime characteristics, and DC internal resistance of lithium secondary batteries containing the second positive electrode active material for manufacturing examples 2-1, 2-2, 2-3, and comparative manufacturing example 2-4 were evaluated using the same method as in evaluation example 1, except that instead of charging the lithium secondary battery at 25°C at a 0.2C rate to a voltage of 3.8V and discharging it to a cutoff voltage of 2.5V at a 0.2C rate, the battery was charged at 25°C at a 0.2C rate until the battery voltage reached 4.45V and then discharged to a cutoff voltage of 2.5V at a 0.2C rate. The results are shown in Table 2.
[0155] [Table 2]
[0156] Referring to Table 2, it can be seen that in manufacturing examples 2-1, 2-2, and 2-3, in which particles with a particle size of 10 μm or larger in the second positive electrode active material account for 30% or more by volume relative to 100% of the total second positive electrode active material, the charging capacity and initial discharge capacity are high, the initial efficiency is improved, the lifespan is excellent, the energy density is improved, the internal resistance is reduced, and the low-temperature performance is excellent, resulting in an overall improvement in battery performance. Therefore, it can be seen that when manufacturing composite positive electrode active materials, a second positive electrode active material containing particles with a particle size of 10 μm or larger accounted for 30% or more by volume relative to 100% of the total second positive electrode active material can improve low-temperature performance and thus improve battery performance.
[0157] Evaluation Example 3: Pellet Density Evaluation The pellet density of the positive electrode active material produced in Examples 1 and 2 was measured and is shown in Table 3 below. The pellet density was calculated from the pellet thickness and mold diameter after placing 3g of positive electrode active material in a pellet manufacturing mold and maintaining it at 4.0 tons for 30 seconds, and is shown in Table 3.
[0158] [Table 3]
[0159] Referring to Table 3, the pellet densities measured in Examples 1 and 2 were 2.40 g / cc and 2.34 g / cc, respectively. It can be seen that the pellet density was improved compared to Production Examples 1-1 to 1-3, shown in Tables 1 and 2, which were obtained using the same method as when the first positive electrode active material was used alone to obtain the pellet densities of Examples 1 and 2, and Production Examples 2-1 to 2-3, which were used when the second positive electrode active material was used alone.
[0160] Evaluation Example 4: Battery Performance Evaluation The battery performance of the lithium secondary batteries manufactured in Examples 1 to 2 and Comparative Examples 1 to 6 was evaluated and is shown in Table 4. Energy density, low-temperature capacity, and DC-IR were evaluated in the same manner as in Evaluation Example 1, except that instead of charging the lithium secondary batteries at 25°C at a 0.2C rate to a voltage of 3.8V and discharging them to a cutoff voltage of 2.5V at a 0.2C rate, they were charged at 25°C at a 0.2C rate until the battery voltage reached 4.25V and then discharged to a cutoff voltage of 2.5V at a 0.2C rate.
[0161] [Table 4]
[0162] As shown in Table 4, Examples 1 and 2 exhibit superior electrochemical properties compared to Comparative Examples 1 to 6.
[0163] For example, the DC-IR internal resistance values of Example 1 and Example 2 were 10.1Ω and 10.4Ω, respectively, which are lower than the DC-IR values of Comparative Examples 1 to 6, which ranged from 10.5Ω to 20.2Ω. Furthermore, in terms of low-temperature capacity characteristics, Example 1 and Example 2 showed values of 128.6mAh / g and 132.4mAh / g, respectively, which are relatively higher than the low-temperature capacities of Comparative Examples 1 to 6, which ranged from 91.7mAh / g to 130.1mAh / g. In particular, Comparative Example 1 showed a low-temperature capacity of 91.7mAh / g, confirming that the examples provide excellent charge and discharge performance in low-temperature environments.
[0164] The energy densities of Example 1 and Example 2 were 1327 Wh / L and 1322 Wh / L, respectively, which is an improvement compared to the energy densities of Comparative Examples 1 to 6, which ranged from 1136 Wh / L to 1314 Wh / L. This indicates that the examples allowed for greater energy storage per unit volume, which is advantageous for achieving high energy density.
[0165] Thus, it can be seen that Examples 1 and 2 showed improved electrochemical properties compared to Comparative Examples 1 to 6, including reduced internal resistance, improved low-temperature performance, and increased energy density.
[0166] Although preferred embodiments of the present invention have been described above, the present invention is not limited thereto and can be implemented in various ways within the scope of the claims, the detailed description of the invention, and the attached drawings, and these also naturally fall within the scope of the present invention. [Explanation of Symbols]
[0167] 100: Lithium-ion rechargeable battery 10: Positive electrode 11: Positive lead tap 12: Positive terminal 20: Negative electrode 21: Negative lead tap 22: Negative terminal 30: Separator 40: Electrode assembly 50: Case 60: Sealing member 70: Electrode Tap 71: Positive Tap 72: Negative electrode tap
Claims
1. A composite positive electrode active material, The first positive electrode active material is a granular material containing lithium iron phosphate compounds, in which multiple primary particles are aggregated; A second positive electrode active material that contains a lithium manganese iron phosphate compound and is in the form of a granular material in which multiple primary particles are aggregated; and Third positive electrode active material containing lithium nickel-based composite oxide Includes, The weight ratio of the first positive electrode active material to the second positive electrode active material is 5:1 to 1:
1. The third positive electrode active material is present in an amount of 5% to 25% by weight, based on 100% by weight of the total composite positive electrode active material. The granules, having a particle size of 10 μm or more, are contained in an amount of 30% or more by volume, based on a total of 100% by volume of the first positive electrode active material and the second positive electrode active material. Composite positive electrode active material.
2. The composite positive electrode active material according to claim 1, wherein the first positive electrode active material contains granules having a particle size of 10 μm or more in an amount of 30 volume% or more based on 100 volume% of the total first positive electrode active material.
3. The composite positive electrode active material according to claim 1, wherein the second positive electrode active material contains granules having a particle size of 10 μm or more in an amount of 30 volume% or more based on 100 volume% of the total second positive electrode active material.
4. The first positive electrode active material is present in an amount of 37.5% to 70% by weight, based on 100% by weight of the total composite positive electrode active material. The composite positive electrode active material according to claim 1, wherein the second positive electrode active material is present in an amount of 20% to 47.5% by weight based on 100% by weight of the total composite positive electrode active material.
5. The lithium iron phosphate compound is represented by the following chemical formula 1, and is the composite cathode active material according to claim 1. [Chemical formula 1] Li a1 Fe (1-x1) M 1 x1 PO 4 (In chemical formula 1, 0.90 ≤ a1 ≤ 1.5 and 0 ≤ x1 ≤ 0.4, M 1 (It is one or more elements from Al, B, Ca, Ce, Cr, Cu, La, Mg, Mn, Mo, Nb, Ni, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr.)
6. The lithium iron phosphate compound further comprises one or more elements selected from Al, Mg, Ti, and V. The composite positive electrode active material according to claim 1, wherein one or more of the elements Al, Mg, Ti, and V are present in the lithium iron phosphate compound in an amount of 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium.
7. The lithium iron phosphate compound is LiFePO 4 The composite positive electrode active material according to claim 1.
8. The average particle diameter (D of the granulated body of the first positive electrode active material 50 ) is 5 μm to 25 μm, and the average particle diameter (D of the primary particles forming the granulated body 50 ) is 0.01 μm to 2 μm, the composite positive electrode active material according to claim 1.
9. The lithium manganese iron phosphate compound is represented by the following chemical formula 2, as described in claim 1. [Chemical formula 2] Li a2 Mn x2 Fe (1-x2-y2) M 2 y2 PO 4 (In chemical formula 2, 0.90 ≤ a² ≤ 1.5, 0.1 ≤ x² ≤ 0.9, 0 ≤ y² ≤ 0.9, and 0.1 ≤ x² + y² < 1, M 2 (It is one or more elements from Al, B, Ca, Ce, Cr, Cu, La, Mg, Mo, Nb, Ni, Sn, Si, Sr, Ti, V, W, Y, Zn, and Zr.)
10. The lithium manganese iron phosphate compound is LiMn 0.7 Fe 0.3 PO 4 LiMn 0.6 Fe 0.4 PO 4 LiMn 0.5 Fe 0.5 PO 4 LiMn 0.4 Fe 0.6 PO 4 , and LiMn 0.3 Fe 0.7 PO 4 A composite cathode active material according to claim 1, comprising one or more of the compounds.
11. The lithium manganese iron phosphate compound further comprises one or more elements selected from Al, Mg, Ti, and V. The composite positive electrode active material according to claim 1, wherein one or more of the elements Al, Mg, Ti, and V are present in the lithium manganese iron phosphate compound in an amount of 0.1 mol% to 0.5 mol% based on 100 mol% of the total metal excluding lithium.
12. The average particle size (D) of the granules of the second positive electrode active material 50 The particle size (D) of the primary particles forming the granules is 5 μm to 25 μm, and the average particle size (D) of the primary particles forming the granules is 5 μm to 25 μm. 50 The composite positive electrode active material according to claim 1, wherein the diameter is 0.01 μm to 2 μm.
13. The composite cathode active material according to claim 1, wherein the lithium nickel-based composite oxide has a nickel content of 80 mol% or more based on 100 mol% of the total metal excluding lithium.
14. The composite cathode active material according to claim 1, wherein the lithium nickel-based composite oxide is represented by the following chemical formula 3, chemical formula 4, or chemical formula 5. [Chemical formula 3] Li a3 Ni x3 M 3 y3 M 4 z3 O 2-b3 X b3 (In chemical formula 3, 0.9 ≤ a³ ≤ 1.8, 0.3 ≤ x³ ≤ 1, 0 ≤ y³ ≤ 0.7, 0 ≤ z³ ≤ 0.7, 0.9 ≤ x³ + y³ + z³ ≤ 1.1, and 0 ≤ b³ ≤ 0.1, M 3 and M 4 Each of the elements is distinct from the others and is independently one or more of the elements Al, B, Ba, Ca, Ce, Co, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, while X is one or more of the elements F, P, and S. [Chemical formula 4] Li a4 Ni x4 Co y4 M 5 z4 O 2-b4 X b4 (In chemical formula 4, 0.9 ≤ a₄ ≤ 1.2, 0.3 ≤ x₄ < 1, 0 < y₄ ≤ 0.7, 0 ≤ z₄ ≤ 0.7, 0.9 ≤ x₄ + y₄ + z₄ ≤ 1.1, and 0 ≤ b₄ ≤ 0.1, M 5 (where X is one or more elements from Al, B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mn, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more elements from F, P, and S.) [Chemical formula 5] Li a5 Ni x5 Co y5 M 6 z5 M 7 w5 O 2-b5 X b5 (In chemical formula 5, 0.9 ≤ a5 ≤ 1.2, 0.3 ≤ x5 ≤ 0.98, 0.01 ≤ y5 ≤ 0.69, 0.01 ≤ z5 ≤ 0.69, 0 ≤ w5 ≤ 0.68, 0.9 ≤ x5 + y5 + z5 + w5 ≤ 1.1, and 0 ≤ b5 ≤ 0.1, M 6 is one or more elements from Al and Mn, and M 7 (where X is one or more elements from B, Ba, Ca, Ce, Cr, Cu, Fe, Mg, Mo, Nb, Si, Sn, Sr, Ti, V, W, Y, Zn, and Zr, and X is one or more elements from F, P, and S.)
15. The average particle size (D) of the third positive electrode active material. 50 The composite positive electrode active material according to claim 1, wherein the diameter of the material is 1 μm to 20 μm.
16. The third positive electrode active material comprises a first particle, a second particle, or a combination thereof, wherein the first particle is in the form of a secondary particle formed by the aggregation of a plurality of primary particles. The average particle size (D) of the first particles of the third positive electrode active material 50 The second particle is 10 μm to 25 μm in size, and the second particle is in the form of a secondary particle, a single particle, or a combination thereof. The average particle size (D) of the second particles of the third positive electrode active material 50 The composite positive electrode active material according to claim 1, wherein the diameter of the material is 1 μm to 8 μm.
17. The third positive electrode active material includes a combination of the first and second particles, The composite positive electrode active material according to claim 16, wherein the first particles are present in an amount of 40% to 95% by weight based on the total sum (100% by weight) of the first and second particles of the third positive electrode active material, and the second particles are present in an amount of 5% to 60% by weight based on the total sum (100% by weight) of the first and second particles of the third positive electrode active material.
18. Positive electrode current collector, and Positive electrode active material layer located on the positive electrode current collector Includes, A positive electrode comprising the positive electrode active material layer according to any one of claims 1 to 17.
19. The positive electrode according to claim 18; Negative electrode; and Electrolyte; Lithium-ion batteries, including lithium-ion batteries.