Phosphorus-containing flame retardants, resin compositions, prepregs, and metal foil-clad laminates

A phosphorus-containing flame retardant with specific structural segments chemically bonds with resin materials, addressing low glass transition temperature issues and enhancing dielectric and thermal stability in printed circuit boards.

JP2026182829APending Publication Date: 2026-11-19CHANG CHUN PLASTICS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026078354
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2026-04-30
Filing Date
2026-05-07
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing phosphorus-containing flame retardants for printed circuit boards do not form chemical bonds with resin materials, leading to low glass transition temperature and reduced cost-effectiveness at high concentrations, affecting the inherent properties of the resin composition.

Method used

A phosphorus-containing flame retardant with specific structural segments, such as benzocyclobutene-derived compounds, forms chemical bonds with resin materials, providing stable and long-lasting flame retardancy at low addition levels, enhancing dielectric properties, thermal stability, and reducing water absorption.

Benefits of technology

The solution achieves excellent dielectric properties, chemical stability, low thermal expansion, and low water absorption in printed circuit boards while maintaining effective flame retardancy without compromising resin composition integrity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182829000001
    Figure 2026182829000001
  • Figure 2026182829000002
    Figure 2026182829000002
  • Figure 2026182829000003
    Figure 2026182829000003
Patent Text Reader

Abstract

The present invention provides a phosphorus-containing flame retardant containing a phosphorus-containing compound. [Solution] A phosphorus-containing flame retardant comprising a phosphorus-containing compound, wherein the phosphorus-containing compound comprises a first structural segment selected from the group consisting of the following formulas, and the phosphorus content of the phosphorus-containing flame retardant is 8% to 10% by weight relative to the total weight of the phosphorus-containing flame retardant. 1 In the H-NMR spectrum, the signal in the range of 7.80 ppm to 8.10 ppm has an integrated area A, and the signal in the range of 3.00 ppm to 4.50 ppm has an integrated area B, with the ratio of A to B (A / B) being 0.40 to 0.70. 1 The 1H-NMR spectrum was obtained by measuring the spectrum using deuterated chloroform as the solvent and tetramethylsilane as the reference substance. This invention provides a phosphorus-containing flame retardant. JPEG2026182829000020.jpg2588
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to phosphorus-containing flame retardants, and more particularly to phosphorus-containing flame retardants comprising phosphorus-containing compounds having specific structural segments. The present invention also relates to resin compositions comprising the phosphorus-containing flame retardant, and to prepregs and metal foil-clad laminates obtained from the resin compositions. [Background technology]

[0002] Printed circuit boards (PCBs) are circuit boards for electronic devices, mounting other electronic components, providing electrical communication between these components, and ensuring a stable circuit operating environment. PCBs are generally manufactured using copper-clad laminates (CCLs). Copper-clad laminates are primarily composed of resin, reinforcing materials, and copper foil. Common resins include epoxy resin, phenolic resin, polyphenylene ether resin, polyaminoformaldehyde, silicone, and polytetrafluoroethylene. Common reinforcing materials include glass fiber cloth, glass fiber mat, and insulating paper.

[0003] Generally, printed circuit boards are manufactured by the following method: A reinforcing material is impregnated into a resin composition, and then the reinforcing material containing the impregnated resin composition is cured to a semi-cured state (i.e., stage B) to obtain a prepreg. Subsequently, the prepregs are laminated, and metal foil is laminated on the outside to form a laminate, and the laminate is subjected to a thermocompression treatment (i.e., stage C) to obtain a metal foil-clad laminate. The metal foil on the surface of the metal foil-clad laminate is etched to form a specific circuit pattern, holes are made in the metal foil-clad laminate, and conductive material is plated into the holes to form via holes, thereby completing the manufacture of the printed circuit board.

[0004] When manufacturing printed circuit boards using resin compositions, various flame retardants, such as halogen-containing flame retardants and phosphorus-containing flame retardants, are usually added to impart flame retardancy to the electronic materials. However, the use of halogen-containing flame retardants is restricted from an environmental protection standpoint. Existing phosphorus-containing flame retardants are typically additive-type phosphorus-containing flame retardants that are physically mixed (blended) into the composition. Examples include phosphorus nitride compounds (such as SPB-100 from Otsuka Chemical Co., Ltd.) and condensed phosphorus esters (such as PX-200 from Daihachi Chemical Industry Co., Ltd.). However, because additive-type phosphorus-containing flame retardants do not form chemical bonds with the resin material, the glass transition temperature (Tg) of the resulting electronic material is generally low. Furthermore, while the amount of additive-type phosphorus-containing flame retardant used needs to reach a certain level to obtain the desired flame retardant effect, adding high concentrations of flame retardants not only reduces cost-effectiveness but also affects the inherent properties of the resin composition. [Overview of the Initiative] [Problems that the invention aims to solve]

[0005] In view of the aforementioned technical problems, the present invention provides a phosphorus-containing flame retardant comprising a phosphorus-containing compound, wherein the phosphorus-containing compound comprises a specific structural segment, thereby forming a reactive phosphorus-containing compound that can chemically bond with a resin material and provide stable and long-lasting flame retardancy at low addition levels. The phosphorus-containing flame retardant of the present invention is particularly suitable for addition to dielectric layer materials of printed circuit boards, and the printed circuit board can have excellent dielectric properties, chemical stability, thermal stability, a low coefficient of thermal expansion, and low water absorption.

[0006] Therefore, one object of the present invention is a phosphorus-containing flame retardant comprising a phosphorus-containing compound, wherein the phosphorus-containing compound is [ka] The phosphorus-containing flame retardant comprises a first structural segment selected from the group, wherein the phosphorus content of the phosphorus-containing flame retardant is 8% to 10% by weight relative to the total weight of the phosphorus-containing flame retardant.1 In the 1H-NMR spectrum, the signal in the range of 7.80 ppm to 8.10 ppm has an integrated area A, and the signal in the range of 3.00 ppm to 4.50 ppm has an integrated area B, with the ratio of A to B (A / B) being 0.40 to 0.70. 1 The 1H-NMR spectrum was obtained by measuring the spectrum using deuterated chloroform as the solvent and tetramethylsilane as the reference substance. The objective is to provide a phosphorus-containing flame retardant.

[0007] In one embodiment of the present invention, 1 The H-NMR spectrum was obtained by measuring it using a nuclear magnetic resonance spectrometer under the following conditions: probe diameter 5 mm, resonance frequency 500 megahertz (MHz), pulse width 10 μs, pulse delay time 2 seconds, and number of integrations 32 times, with the tetramethylsilane signal set to 0 ppm.

[0008] In one embodiment of the present invention, the integral area B is between 2.85 and 5.00.

[0009] In one embodiment of the present invention, the phosphorus-containing flame retardant has a melting point of 135°C to 190°C as measured by differential scanning calorimetry (DSC).

[0010] In one embodiment of the present invention, in the infrared absorption spectrum obtained by Fourier transform infrared spectroscopy (FTIR) using a thin-film method on a KBr tablet, at 1400 cm⁻¹ -1 ~1405cm -1 It has a characteristic peak, or 1456cm -1 ~1461cm -1 It has a characteristic peak.

[0011] In one embodiment of the present invention, the phosphorus-containing compound [ka] further comprising a second structural segment selected from the group consisting of, wherein the second structural segment directly connects its * part to the * part of the first structural segment.

[0012] Another object of the present invention is to provide a resin composition comprising a first reactive component selected from the group consisting of polyphenylene ether resins having olefinic carbon-carbon unsaturated double bonds, allyl group-containing compounds, epoxy resins, phenolic resins, benzoxazine resins, elastomers having olefinic carbon-carbon unsaturated double bonds, maleimide resins, and combinations thereof, as well as the aforementioned phosphorus-containing flame retardant.

[0013] In one embodiment of the present invention, based on the total weight of the first reactive component and the phosphorus-containing flame retardant, the content of the phosphorus-containing flame retardant is 10 wt% to 30 wt%.

[0014] In one embodiment of the present invention, the polyphenylene ether resin having an olefinic carbon-carbon unsaturated double bond is selected from the group consisting of dihydroxypolyphenylene ether resins, methacrylic acid polyphenylene ether resins, vinyl group-containing polyphenylene ether resins, and combinations thereof.

[0015] In one embodiment of the present invention, the resin composition further comprises a component selected from the group consisting of fillers, catalysts, elastomers not having olefinic carbon-carbon unsaturated double bonds, dispersants, toughening agents, viscosity modifiers, plasticizers, coupling agents, and combinations thereof.

[0016] Still another object of the present invention is to provide a prepreg obtained by impregnating or coating a substrate with the aforementioned resin composition, and drying the impregnated or coated substrate.

[0017] A still further object of the present invention is to provide a metal foil-clad laminate obtained by laminating the aforementioned prepreg and a metal foil, or a metal foil-clad laminate obtained by applying the aforementioned resin composition to a metal foil and drying the coated metal foil.

[0018] To make the above-mentioned objects, technical features and advantages of the present invention clearer and easier to understand, some specific embodiments are described in detail below. MODE FOR CARRYING OUT THE INVENTION

[0019] Some specific embodiments according to the present invention are described in detail below. However, the present invention may be implemented in various different forms of embodiments, and the protection scope of the present invention should not be limited to the aforesaid specific embodiments.

[0020] Unless otherwise specifically stated, the terms "a", "the" and similar terms used in this specification and the claims shall be understood to include both the singular and the plural forms.

[0021] Unless otherwise specifically stated, the terms "first", "second" and similar terms used in this specification and the claims are intended to distinguish the described components or constituents, have no special meaning per se, and do not indicate any order.

[0022] Unless otherwise specifically stated, the constituents contained in the solutions, mixtures, or compositions described in this specification and the claims do not include the weight of the solvent.

[0023] Numerical ranges (for example, from 5 to 100) used in this specification and the claims are to be understood to include all rational numbers within the aforesaid range and ranges composed of any rational numbers within the aforesaid range, so the numerical ranges used in this specification include all possible combinations of the numerical values between the listed minimum and maximum values.

[0024] The advantage of the present invention over the prior art is to provide a phosphorus-containing flame retardant comprising a phosphorus-containing compound, wherein the phosphorus-containing compound comprises a specific structural segment, thereby enabling the formation of a chemical bond with a resin material. The phosphorus-containing flame retardant is particularly suitable for addition to the dielectric layer material of printed circuit boards, and the manufactured printed circuit boards have excellent dielectric properties, chemical stability, thermal stability, a low coefficient of thermal expansion, and low water absorption.

[0025] 1. Phosphorus-containing flame retardant

[0026] The phosphorus-containing flame retardant of the present invention comprises a phosphorus-containing compound, wherein the phosphorus-containing compound is [ka] It comprises a first structural segment selected from the group, and a phosphorus-containing segment linked to the first structural segment.

[0027] The first structural segment is derived from benzocyclobutene (BCB) and possesses a reactive cyclobutene functional group. It can induce a ring-opening reaction by heat, light, or mechanical action to form highly active o-quinodimethane, which can then undergo addition polymerization with other reactive components. Therefore, the phosphorus-containing flame retardant of the present invention functions as a reactive phosphorus-containing flame retardant.

[0028] The selection of the phosphorus-containing segment is characterized in that the phosphorus content of the phosphorus-containing flame retardant is 8.0% by weight to 10.0% by weight relative to the total weight of the phosphorus-containing flame retardant, and is within the range of, for example, 8.0% by weight, 8.1% by weight, 8.2% by weight, 8.3% by weight, 8.4% by weight, 8.5% by weight, 8.6% by weight, 8.7% by weight, 8.8% by weight, 8.9% by weight, 9.0% by weight, 9.1% by weight, 9.2% by weight, 9.3% by weight, 9.4% by weight, 9.5% by weight, 9.6% by weight, 9.7% by weight, 9.8% by weight, 9.9% by weight, or 10.0% by weight, or any two of the above values.

[0029] The example of the phosphorus-containing segment is as follows: [ka] It includes a second structural segment selected from a larger group. The second structural segment directly connects its * portion to the * portion of the first structural segment.

[0030] Therefore, specific examples of phosphorus-containing compounds of the present invention include the following group. [ka]

[0031] The second structural segment is derived from 9,10-dihydro-9-oxa-10-phosphaphenanthrene-10-oxide (DOPO), aromatic phosphate esters, or aromatic phosphate oxides. In one preferred embodiment of the present invention, the phosphorus-containing compound comprises a second structural segment derived from DOPO, i.e. [ka] Includes.

[0032] The phosphorus-containing flame retardant of the present invention satisfies the following conditions. 1In the H-NMR spectrum, when the integrated area of the signal from 7.80 ppm to 8.10 ppm is denoted as A, and the integrated area of the signal from 3.00 ppm to 4.50 ppm is denoted as B, the ratio of A to B (A / B) is 0.40 to 0.70, more specifically 0.49 to 0.61. For example, the ratio is 0.40, 0.41, 0.42, 0.43, 0.44, 0.45, 0.46, 0.47, 0.48, 0.49, 0.50, 0.51, 0.52, 0.53, 0.54, 0.55, 0.56, 0.57, 0.58, 0.59, 0.60, 0.61, 0.62, 0.63, 0.64, 0.65, 0.66, 0.67, 0.68, 0.69, or 0.70, or falls within a range constituted by any two of the aforementioned numerical values. By controlling the value of A / B within the specified range, the phosphorus-containing flame retardant of the present invention can simultaneously improve the dielectric properties, flame retardancy and heat resistance of the obtained electronic material.

[0033] In one embodiment of the present invention, when the integrated area A is normalized to 2.00, the integrated area B is 2.85 to 5.00, for example 2.85, 2.90, 2.95, 3.00, 3.05, 3.10, 3.15, 3.20, 3.25, 3.30, 3.31, 3.35, 3.40, 3.45, 3.50, 3.55, 3.60, 3.65, 3.70, 3.75, 3.80, 3.85, 3.90, 3.95, 4.00, 4.05, 4.06, 4.10, 4.15, 4.20, 4.25, 4.30, 4.35, 4.40, 4.45, 4.50, 4.55, 4.60, 4.65, 4.70, 4.75, 4.80, 4.85, 4.90, 4.95, or 5.00, or is a range constituted by any two of the aforementioned numerical values.

[0034] Of the phosphorus-containing flame retardant of the present invention 1The H-NMR spectrum was obtained by measuring using a nuclear magnetic resonance spectrometer under the following conditions, with deuterated chloroform as the solvent and tetramethylsilane as the reference substance: probe diameter 5 mm, resonance frequency 500 megahertz, pulse width 10 μs, pulse delay time 2 seconds, number of integrations 32, and tetramethylsilane signal set to 0 ppm. The detailed measurement method is as follows: First, a phosphorus-containing flame retardant is dissolved in deuterated chloroform to obtain a test sample solution. Next, the test sample solution is placed in the sample loader of the nuclear magnetic resonance spectrometer, and a magnetic field homogenization (shimming) operation is performed to ensure magnetic field uniformity. Then, using a 5 mm diameter probe, the test sample solution is analyzed under the following parameter conditions. 1 A 1H-NMR spectrum was obtained. The resonance frequency was set to 500 megahertz, the pulse width to 10 μs, the pulse delay time to 2 seconds, the number of integrations to 32, and the tetramethylsilane signal to 0 ppm.

[0035] In one embodiment of the present invention, the phosphorus-containing flame retardant has a melting point of 135°C to 190°C as measured by differential scanning calorimetry. For example, 135°C, 136°C, 137°C, 138°C, 139°C, 140°C, 141°C, 142°C, 143°C, 144°C, 145°C, 146°C, 147°C, 148°C, 149°C, 150°C, 151°C, 152°C, 153°C, 154°C, 155°C, 156°C, 157°C, 158°C, 159°C, 160°C, 161°C, 162°C, 163°C, 164°C, 165°C The range consists of ℃, 166℃, 167℃, 168℃, 169℃, 170℃, 171℃, 172℃, 173℃, 174℃, 175℃, 176℃, 177℃, 178℃, 179℃, 180℃, 181℃, 182℃, 183℃, 184℃, 185℃, 186℃, 187℃, 188℃, 189℃, or 190℃, or any two of the above values.

[0036] In one embodiment of the present invention, the phosphorus-containing flame retardant, in the infrared absorption spectrum obtained by FTIR using the film method on KBr tablets, showed an absorption of 1400 cm⁻¹. -1 ~1405cm -1 It has a characteristic peak at 1456 cm. -1 ~1461cm-1 It has a characteristic peak at 1400cm. -1 ~1405cm -1 Features of the peak or 1456cm -1 ~1461cm -1 The characteristic peak corresponds to the characteristic vibration of the four-membered ring in benzocyclobutene, confirming the presence of the four-membered ring structure of benzocyclobutene in phosphorus-containing flame retardants.

[0037] In a more preferred embodiment of the present invention, the content of the phosphorus-containing compound relative to the total weight of the phosphorus-containing flame retardant is 86.0% by weight to 99.9% by weight, for example, 86.0% by weight, 87.0% by weight, 88.0% by weight, 89.0% by weight, 90.0% by weight, 91.0% by weight, 92.0% by weight, 93.0% by weight, 94.0% by weight, 95.0% by weight, 96.0% by weight, 97.0% by weight, 98.0% by weight, 99.0% by weight, or 99.9% by weight, or any two of the above values.

[0038] The phosphorus-containing flame retardant of the present invention is prepared by the following method. First, DOPO or aromatic phosphate esters, halogenated benzocyclobutene, and a first organic base are dissolved in a first organic solvent to obtain a mixed solution. Next, a catalyst is added to the mixed solution, and the mixed solution is refluxed under a nitrogen atmosphere for 5 to 10 hours to carry out the reaction and obtain a crude product solution. Then, the crude product solution is filtered using diatomaceous earth, and the obtained filtrate is concentrated under reduced pressure and purified to obtain the phosphorus-containing flame retardant of the present invention. Examples of halogenated benzocyclobutene include, but are not limited to, bromobenzocyclobutene, fluorobenzocyclobutene, and chlorobenzocyclobutene. Examples of first organic bases include, but are not limited to, triethylamine, trimethylamine, diisopropylethylamine, N-methylpiperidine, and pyridine. Each of the first organic bases may be used alone or in combination. Examples of first organic solvents include, but are not limited to, acetonitrile, acetone, tetrahydrofuran, and dimethylformamide. Each of the first organic solvents may be used alone or in combination.

[0039] Alternatively, the phosphorus-containing flame retardant may be prepared by the following method. First, DOPO or aromatic phosphate esters, halogenated benzocyclobutene, and a second organic base are dissolved in a second organic solvent to obtain a mixed solution. Next, the mixed solution is stirred at room temperature under a nitrogen atmosphere for 12 to 36 hours to carry out the reaction and obtain a crude product solution. After that, the crude product is precipitated using water and the crude product is purified to obtain the phosphorus-containing flame retardant of the present invention. Examples of second organic bases include, but are not limited to, sodium methanol, sodium ethanol, and tertiary butyl potassium. Each of the above second organic bases may be used alone or in combination. Examples of second organic solvents include, but are not limited to, methanol, ethanol, and isopropanol. Each of the above second organic solvents may be used alone or in combination.

[0040] 2.Resin composition

[0041] Since the phosphorus-containing flame retardant of the present invention is applicable to the production of resin compositions for electronic materials, the present invention also provides a resin composition that includes a first reactive component and the phosphorus-containing flame retardant as essential components, and also includes other components selected as needed.

[0042] 2.1. Primary Reactive Components

[0043] In the resin composition of the present invention, the first reactive component includes one or more of the following: polyphenylene ether resin having an olefin-type carbon-carbon unsaturated double bond, allyl group-containing compound, epoxy resin, phenol resin, benzoxazine resin, elastomer having an olefin-type carbon-carbon unsaturated double bond, and maleimide resin.

[0044] In this specification, polyphenylene ether resin having an olefin-type carbon-carbon unsaturated double bond means having repeating units in the molecular backbone [ka] This refers to a thermosetting resin containing and having an olefin-type carbon-carbon unsaturated double bond at its terminus, where R is independently hydrogen or an alkyl group having 1 to 5 carbon atoms, and v is an integer from 1 to 100. The olefin-type carbon-carbon unsaturated double bond can undergo addition polymerization reactions with other reactive components (e.g., the phosphorus-containing flame retardant of the present invention). Examples of the olefin-type carbon-carbon unsaturated double bond include, but are not limited to, vinyl, vinyl benzyl, allyl, acrylic, and methacrylic groups. Examples of polyphenylene ether resins having an olefin-type carbon-carbon unsaturated double bond include, but are not limited to, dihydroxypolyphenylene ether resins, methacrylic acid polyphenylene ether resins, and vinyl group polyphenylene ether resins. Each of the polyphenylene ether resins having an olefin-type carbon-carbon unsaturated double bond may be used individually or in combination of multiple types. Commercially available olefin-type polyphenylene ether resins having carbon-carbon unsaturated double bonds include, but are not limited to, methacrylic acid polyphenylene ether resins (e.g., product SA9000 from Saudi Basic Industries), vinyl group polyphenylene ether resins (e.g., product OPE-2st 2200 from Mitsubishi Gas Chemical Company, Inc.), and dihydroxy polyphenylene ether resins (e.g., product SA90 from Saudi Basic Industries Corporation).

[0045] In this specification, an allyl group-containing compound is a polyfunctional allyl group-containing compound, that is, a compound having at least two allyl groups. Examples of polyfunctional allyl group-containing compounds include, but are not limited to, triallyl cyanurate (TAC), triallyl isocyanurate (TAIC), diallyl phthalate, diallyl isophthalate, triallyl trimellitate, and prepolymers of the said compounds.

[0046] In this specification, epoxy resin refers to a thermosetting resin having at least two epoxy functional groups in one molecule, and includes, for example, difunctional epoxy resins, tetrafunctional epoxy resins, octafunctional epoxy resins, or linear phenolic resin epoxy resins, with no particular limitations on the type.

[0047] In this specification, "phenol resin" refers to a resin obtained by the condensation of a phenol compound and an aldehyde compound. Specific examples include, but are not limited to, phenol-formaldehyde resin, cresol-formaldehyde resin, and resorcinol-formaldehyde resin.

[0048] In this specification, a benzoxazine resin refers to a compound having at least one benzoxazine structure, and a benzoxazine structure refers to a bicyclic heterocyclic structure formed by the condensation of a benzene ring and an oxazine ring. Examples of benzoxazine resins include, but are not limited to, phenol-type benzoxazine resins and bisphenol A-type benzoxazine resins.

[0049] In this specification, an elastomer having an olefin-type carbon-carbon unsaturated double bond refers to a polymer that has an olefin-type carbon-carbon unsaturated double bond and is viscoelastic. Specific examples of elastomers having an olefin-type carbon-carbon unsaturated double bond include, but are not limited to, but butadiene-based elastomers having an olefin-type carbon-carbon unsaturated double bond and styrene-based elastomers having an olefin-type carbon-carbon unsaturated double bond. Commercially available elastomers having an olefin-type carbon-carbon unsaturated double bond include, but are not limited to, the RICON series products from Cray Valley, Inc., the B1000 series products from Nippon Soda Co., Ltd., and the TUFPRENE and ASAPRENE T series products from Asahi Kasei Corporation.

[0050] In this specification, maleimide resin refers to a thermosetting resin having a maleimide functional group, and the maleimide functional group means an unsaturated imide functional group having a reactive double bond. Components having a maleimide functional group can react with other components having a reactive double bond because they have a reactive double bond. Commercially available maleimide resins include products with model numbers BMI-1000, BMI-1000H, BMI-1100, BMI-1100H, BMI-2000, BMI-2300, BMI-3000, BMI-3000H, BMI-4000H, BMI-5000, BMI-5100, BMI-7000 and BMI-7000H available from Yamato Chemical Industries, Ltd., products with model numbers BMI-70 and BMI-80 available from K.I. Chemicals, Ltd., product with model number MIR-3000 available from Nippon Kayaku Co., Ltd., and products with model numbers X9-470, NE-X-9470S and NE-X-9480 available from DIC Corporation.

[0051] The content of the first reactive component can be adjusted as needed. Generally, the content of the first reactive component is 50% to 90% by weight, more specifically 55% to 85% by weight, relative to the total weight of the first reactive component and the phosphorus-containing flame retardant. For example, the content of the first reactive component relative to the total weight of the first reactive component and the phosphorus-containing flame retardant may be 55% by weight, 56% by weight, 57% by weight, 58% by weight, 59% by weight, 60% by weight, 61% by weight, 62% by weight, 63% by weight, 64% by weight, 65% by weight, 66% by weight, 67% by weight, 68% by weight, 69% by weight, 70% by weight, 71% by weight, 72% by weight, 73% by weight, 74% by weight, 75% by weight, 76% by weight, 77% by weight, 78% by weight, 79% by weight, 80% by weight, 81% by weight, 82% by weight, 83% by weight, 84% by weight, or 85% by weight, or within the range of any two of the above values, but the present invention is not limited thereto.

[0052] 2.2. Phosphorus-containing flame retardants

[0053] The phosphorus-containing flame retardant is the phosphorus-containing flame retardant of the present invention described above. The content of the phosphorus-containing flame retardant in the resin composition can be adjusted as needed. Generally, the content of the phosphorus-containing flame retardant is 1% to 35% by weight, more preferably 10% to 30% by weight, and even more preferably 13% to 25% by weight, relative to the total weight of the first reactive component and the phosphorus-containing flame retardant. For example, the content of the phosphorus-containing flame retardant is 10%, 11%, 12%, 13%, 14%, 15%, 16%, 17%, 18%, 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, or 30% by weight, or within the range of any two of the above values, but the present invention is not limited thereto.

[0054] 2.3. Selected Ingredients

[0055] In addition to the components described above, the resin composition of the present invention may further contain selected components, provided that they do not contradict the technical principles of the present invention. For example, it may contain additives well known in the art, thereby improving the physicochemical properties of the metal foil laminate obtained from the resin composition and the processability of the resin composition during the manufacturing process. Examples of such well known additives include, but are not limited to, fillers, catalysts, olefin-type carbon-carbon unsaturated double bond-less elastomers, dispersants, toughening agents, viscosity modifiers, plasticizers, and coupling agents. These additives may be used alone or in combination. The use of such additives can be carried out as needed by a person with ordinary skill in the art to which the present invention belongs, with reference to the disclosures herein, and is not a technical feature of the present invention, so it will not be described in detail here.

[0056] 2.4. Preparation of resin composition

[0057] The resin composition of the present invention is manufactured in a clear lacquer form by uniformly mixing the components of the resin composition, which include a first reactive component, a phosphorus-containing flame retardant, and other optional components, using a stirrer, and dissolving or dispersing them in a third organic solvent, for use in subsequent processing. The third organic solvent is an inert solvent that can dissolve or disperse the components of the resin composition and does not react with these components. Specific examples of third organic solvents used to dissolve or disperse the components of the resin composition include, but are not limited to, toluene, γ-butyrolactone, methyl ethyl ketone, cyclohexanone, butyl ketone, acetone, xylene, methyl isobutyl ketone, N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), and N-methylpyrrolidone (NMP). Each third organic solvent may be used alone or in combination. There are no special restrictions on the amount of third organic solvent used; in principle, any amount sufficient is enough to uniformly dissolve or disperse the components of the resin composition.

[0058] 3. Prepregs and metal foil-clad laminates

[0059] The present invention also provides a prepreg obtained from the resin composition. The prepreg is manufactured by impregnating a substrate with the resin composition or by coating a substrate with the resin composition and drying the impregnated or coated substrate. The substrate is a reinforcing material commonly used in the field of printed circuit board technology, and specific examples include, but are not limited to, paper, cloth, or felt made of glass fibers. In one embodiment of the present invention, a 2116 glass fiber cloth is used as the substrate and a semi-cured prepreg is obtained by heating and drying it at 170°C.

[0060] The present invention provides a metal foil-clad laminate obtained by laminating a prepreg and a metal foil. Specifically, the metal foil-clad laminate of the present invention includes a dielectric layer and a metal layer, the dielectric layer being formed from the prepreg. A metal foil-clad laminate can be obtained by laminating multiple layers of the prepreg to form a dielectric layer, laminating a metal foil (e.g., copper foil, as a metal layer) onto at least one outer surface of the dielectric layer to form a laminate, and then subjecting the laminate to a thermocompression bonding treatment. Alternatively, a metal foil-clad laminate can be obtained by directly applying the resin composition of the present invention to a metal foil and drying the applied metal foil.

[0061] The outer metal foil of the metal foil-clad laminate is further patterned to obtain a printed circuit board. The patterning method includes, but is not limited to, etching. [Examples]

[0062] 4. Examples

[0063] 4.1. Explanation of Measurement Method

[0064] The present invention will be further described below with reference to specific embodiments. The measuring devices and methods employed are as follows.

[0065] [ 1 H-NMR analysis]

[0066] 15 milligrams of phosphorus-containing flame retardant were dissolved in 750 microliters of deuterated chloroform to obtain a test sample solution. Next, the test sample solution was placed in the sample loader of a nuclear magnetic resonance spectrometer (model: AVANCE-500, manufactured by Bruker, Germany), and a magnetic field homogenization procedure was performed to ensure magnetic field uniformity. Subsequently, the test sample solution was analyzed using a 5 mm diameter probe (type: BBFO Smart probe) under the following parameter conditions. 1¹H-NMR spectra were acquired. The resonance frequency was set to 500 megahertz, the pulse width to 10 μs, the pulse delay time to 2 seconds, and the number of integrations to 32. The signal of tetramethylsilane (CAS No. 75~76~3) was set to 0 ppm as the reference substance.

[0067] [ 13 C-NMR analysis]

[0068] A test sample solution was obtained by dissolving 15 milligrams of phosphorus-containing flame retardant in 750 microliters of deuterated chloroform. Next, the test sample solution was placed in the sample loader of the AVANCE-500 nuclear magnetic resonance spectrometer, and a magnetic field uniformity procedure was performed to ensure magnetic field uniformity. Subsequently, the test sample solution was analyzed using a 5 mm diameter probe (Type: BBFO Smart probe) under the following parameter conditions. 1 ¹H-NMR spectra were acquired. The resonance frequency was set to 125 megahertz, the pulse width to 10 μs, the pulse delay time to 2 seconds, the number of integrations to 1024, and the signal of tetramethylsilane (CAS No. 75~76~3) as the reference substance was set to 0 ppm.

[0069] [Phosphorus content measurement]

[0070] A test sample was prepared by dissolving 500 milligrams of phosphorus-containing flame retardant in 2.5 grams of dimethylphosphine. Next, the test sample was pretreated according to the U.S. Environmental Protection Agency's certification method EPA 3050B (1996 edition). Subsequently, the phosphorus content of the test sample was analyzed using an inductively coupled plasma atomic emission spectrometer (model: Optima 8300, Perkin Elmer).

[0071] [Melting point measurement]

[0072] Four milligrams of phosphorus-containing flame retardant were prepared as a test sample. Next, the melting point of the test sample was measured using a differential scanning calorimetry (DSC) (model: Q200, manufactured by TA Instruments) under the following conditions. First, the test sample was equilibrated at 50°C, and then heated from 50°C to 300°C at a heating rate of 10°C / min. Then, the melting point, exothermic onset temperature, and exothermic termination temperature were calculated using the software attached to the DSC.

[0073] [FTIR measurement]

[0074] First, 5 milligrams of phosphorus-containing flame retardant were applied to KBr tablets with a diameter of 13 mm and a thickness of 1 mm using a film method. Next, the KBr tablets coated with the phosphorus-containing flame retardant were placed in a Fourier transform infrared spectrometer (model: Spotlight 200i, manufactured by PerkinElmer) and exposed to light at 400 cm². -1 ~4000cm -1 Infrared spectra were measured in the following range. The measurement conditions were as follows: measurements were performed using the transmission method, with a resolution of 1 cm. -1 The number of integration cycles was 16. Spectral intensity was expressed as absorbance (in arbitrary units) at each wavelength.

[0075] [Flame retardancy test]

[0076] Copper foil-clad laminates were etched to remove the copper foil from both sides, obtaining uncopper-clad laminates with a thickness of 0.45 mm to 0.55 mm. The uncopper-clad laminates were cut into test samples measuring 125 mm in length and 13 mm in width. The test samples were subjected to flame retardancy tests based on the UL 94 flame retardancy test standard. The V0 grade result indicated that after two 10-second flame tests on the test sample, combustion stopped within 10 seconds and no combustion dripping occurred. The V1 grade indicated that after two 10-second flame tests under the test conditions, combustion stopped within 30 seconds and no combustion dripping occurred. The V2 grade indicated that after two 10-second flame tests under the test conditions, combustion stopped within 30 seconds, but combustion dripping occurred. Therefore, the flame retardancy ranking was V0 superior to V1, and V1 superior to V2. In this study, five test samples were taken from each resin composition, and five UL 94 flame retardancy tests were performed. Each test involved re-measuring the flame retardancy using a new test sample, and the worst result was recorded.

[0077] [Glass transition temperature (Tg) measurement]

[0078] First, copper foil was removed from both sides of a copper foil-clad laminate by etching, and uncopper-clad laminates with a thickness of 0.45 mm to 0.55 mm were obtained as test samples. The Tg of the test samples was measured using a dynamic mechanical analyzer (DMA, model number: Q800, manufactured by TA Instruments) according to IPC-TM-650-2.4.24.4. The measurement conditions were as follows: A three-point bending jig module was used, the frequency was 1 Hz, and the heating rate was 2 °C / min. Dynamic viscoelasticity was measured during the heating process from 50 °C to 400 °C. Tg was defined as the temperature at which tanδ in the obtained viscoelastic curve showed its maximum value.

[0079] [Measurement of dielectric constant (Dk) and dielectric loss tangent (Df)]

[0080] First, the copper foil on both sides of the copper foil-clad laminate was removed by etching to obtain uncopper-clad laminates with a thickness of 0.45 mm to 0.55 mm as test samples. Using a split post-dielectric resonator (SPDR), the Dk and Df of the test samples were measured at 25°C and an operating frequency of 10 GHz, in accordance with IEC 61189-2-721.

[0081] 4.2. Preparation of phosphorus-containing flame retardants

[0082] [Synthesis Example 1]

[0083] 300 ml of acetonitrile (CAS No. 75-05-8) was added to a 1000 ml reaction vessel, and 32.4 g of DOPO (CAS No. 35948-25-5), 45 g of triethylamine (CAS No. 121-44-8), and 30 g of 4-bromobenzocyclobutene (CAS No. 1073-39-8) were dissolved to obtain a mixed solution. Next, 2.7 g of palladium acetate (CAS No. 3375-31-3) was added to the mixed solution, and the reaction was carried out under reflux for 7 hours under a nitrogen atmosphere to obtain a crude product solution. Subsequently, the crude product solution was filtered using diatomaceous earth, and the obtained filtrate was concentrated under reduced pressure and purified to obtain a phosphorus-containing flame retardant FR1 containing phosphorus-containing compound P1 having the following structural formula. The content of phosphorus-containing compound P1 relative to the total weight of phosphorus-containing flame retardant FR1 was 98% by weight. [ka]

[0084] [Synthesis Example 2]

[0085] 300 ml of methanol was added to a 1000 ml reaction vessel, and 51 g of DOPO, 65 g of 30 w / w% sodium methanol (CAS No. 124-41-4), and 54 g of 1-bromobenzocyclobutene (CAS No. 21120-91-2) were dissolved to obtain a mixed solution. Next, the mixed solution was stirred under a nitrogen atmosphere at room temperature for 24 hours to carry out the reaction and obtain a crude product solution. Subsequently, the crude product was precipitated using water, and the crude product was purified to obtain a phosphorus-containing flame retardant FR2 containing phosphorus-containing compound P2 having the following structural formula. The content of phosphorus-containing compound P2 relative to the total weight of the phosphorus-containing flame retardant FR2 was 98% by weight. [ka]

[0086] [Comparative Synthesis Example 1]

[0087] 300 ml of acetonitrile was added to a 1000 ml reaction vessel, and 32.4 g of DOPO, 45 g of triethylamine, and 45 g of 4-bromobenzocyclobutene were dissolved to obtain a mixed solution. Next, 2.7 g of palladium acetate was added to the mixed solution, and the reaction was carried out under reflux for 7 hours under a nitrogen atmosphere to obtain a crude product solution. Subsequently, the crude product solution was filtered using diatomaceous earth, and the resulting filtrate was concentrated under reduced pressure to obtain comparative example phosphorus-containing flame retardant CFR1 containing phosphorus-containing compound P1 having the following structural formula. The content of phosphorus-containing compound P1 relative to the total weight of comparative example phosphorus-containing flame retardant CFR1 was 85% by weight. [ka]

[0088] [Comparative Synthesis Example 2]

[0089] 300 ml of acetonitrile was added to a 1000 ml reaction vessel, and 42.1 g of DOPO, 45 g of triethylamine, and 30 g of 4-bromobenzocyclobutene were dissolved to obtain a mixed solution. Next, 2.7 g of palladium acetate was added to the mixed solution, and the reaction was carried out under reflux for 7 hours under a nitrogen atmosphere to obtain a crude product solution. Subsequently, the crude product solution was filtered using diatomaceous earth, and the resulting filtrate was concentrated under reduced pressure to obtain comparative example phosphorus-containing flame retardant CFR2, which contains phosphorus-containing compound P1 having the following structural formula. The content of phosphorus-containing compound P1 relative to the total weight of comparative example phosphorus-containing flame retardant CFR2 was 85% by weight. [ka]

[0090] [Comparative Synthesis Example 3]

[0091] 300 ml of methanol was added to a 1000 ml reaction vessel, and 51 g of DOPO, 65 g of 30 w / w% sodium methanol, and 31 g of 4-chloromethylstyrene (CAS No. 1592-20-7) were dissolved to obtain a mixed solution. Next, the mixed solution was stirred under a nitrogen atmosphere at room temperature for 24 hours to carry out the reaction and obtain a crude product solution. Subsequently, the crude product was precipitated using water, and the crude product was purified to obtain comparative example phosphorus-containing flame retardant CFR3, which contains comparative phosphorus-containing compound CP3 having the following structural formula. The content of comparative example phosphorus-containing compound CP3 was 98% by weight relative to the total weight of comparative example phosphorus-containing flame retardant CFR3. [ka]

[0092] [Comparative Synthesis Example 4]

[0093] 300 ml of tetrahydrofuran was added to a 1000 ml reaction vessel, and 19.5 g of magnesium ribbon (CAS No. 7439-95-4) and 128.1 g of 4-bromobenzocyclobutene were added to obtain a mixed solution. Next, the mixed solution was stirred under a nitrogen atmosphere and refluxed for 2 hours. Then, the temperature was lowered to 0°C, and 67.9 g of phenylphosphonic dichloride (CAS No. 824-72-6) was added dropwise. The reaction was carried out by stirring at room temperature for 16 hours to obtain a crude product solution. Next, the crude product solution was extracted and purified to obtain comparative example phosphorus-containing flame retardant CFR4, which contains comparative example phosphorus-containing compound CP4 having the following structural formula. The content of comparative example phosphorus-containing compound CP4 was 98% by weight of the total weight of comparative example phosphorus-containing flame retardant CFR4. [ka]

[0094] According to the method described above, various properties of phosphorus-containing flame retardants FR1 to FR2 and comparative example phosphorus-containing flame retardants CFR1 to CFR4 were measured. The measurement items were: 1 H-NMR analysis, 13 The analysis included 13C-NMR analysis, FTIR analysis, melting point, exothermic onset temperature, exothermic termination temperature, and phosphorus content. The measurement results are recorded in Tables 1-1 and 1-2.

[0095] [Table 1-1]

[0096] [Table 1-2]

[0097] 4.3. Preparation of resin composition

[0098] [Example 1]

[0099] 13 grams of polyphenylene ether methacrylate resin (model number: SA9000, purchased from Saudi Basic Industries), 38 grams of vinyl group polyphenylene ether resin (model number: OPE-2st 2200, purchased from Mitsubishi Gas Chemical), 25 grams of TAIC (CAS No. 1025-15-6), 12 grams of butadiene-styrene copolymer (model number: R-100, purchased from Cray Valley), 0.1 grams of benzoyl peroxide (CAS No. 94-36-0), 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker and heated to 90°C using an electromagnetic stirrer. Next, 15 grams of phosphorus-containing flame retardant FR1 was added to the beaker and stirred until clear to prepare the resin composition of Example 1.

[0100] [Example 2]

[0101] 13 grams of methacrylate polyphenylene ether resin SA9000, 38 grams of vinyl group polyphenylene ether resin OPE-2st 2200, 25 grams of TAIC, 12 grams of butadiene-styrene copolymer R-100, 0.1 grams of benzoyl peroxide, 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker and heated and stirred to 90°C using an electromagnetic stirrer. Next, 22.5 grams of phosphorus-containing flame retardant FR1 was added to the beaker and stirred until clear to obtain the resin composition of Example 2.

[0102] [Example 3]

[0103] 13 grams of methacrylate polyphenylene ether resin SA9000, 38 grams of vinyl group polyphenylene ether resin OPE-2st 2200, 25 grams of TAIC, 12 grams of butadiene-styrene copolymer R-100, 0.1 grams of benzoyl peroxide, 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker and heated and stirred to 90°C using an electromagnetic stirrer. Next, 22.5 grams of phosphorus-containing flame retardant FR2 was added to the beaker and stirred until clear to prepare the resin composition of Example 3.

[0104] [Example 4]

[0105] 13 grams of methacrylate polyphenylene ether resin SA9000, 38 grams of vinyl group polyphenylene ether resin OPE-2st 2200, 25 grams of TAIC, 12 grams of butadiene-styrene copolymer R-100, 0.1 grams of benzoyl peroxide, 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker and heated and stirred to 90°C using an electromagnetic stirrer. Next, 30 grams of phosphorus-containing flame retardant FR1 was added to the beaker and stirred until clear to prepare the resin composition of Example 4.

[0106] [Example 5]

[0107] 25 grams of methacrylate polyphenylene ether resin SA9000, 25 grams of vinyl group polyphenylene ether resin OPE-2st 2200, 25 grams of TAIC, 12 grams of butadiene-styrene copolymer R-100, 0.1 grams of benzoyl peroxide, 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker and heated to 90°C using an electromagnetic stirrer. Next, 22.5 grams of phosphorus-containing flame retardant FR1 was added to the beaker and stirred until clear to prepare the resin composition of Example 5.

[0108] [Comparative Example 1]

[0109] 13 grams of methacrylate polyphenylene ether resin SA9000, 38 grams of vinyl group polyphenylene ether resin OPE-2st 2200, 25 grams of TAIC, 12 grams of butadiene-styrene copolymer R-100, 0.1 grams of benzoyl peroxide, 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker and heated to 90°C using an electromagnetic stirrer. Next, 22.5 grams of comparative example phosphorus-containing flame retardant CFR1 were added to the beaker and stirred until clear to prepare the resin composition of Comparative Example 1.

[0110] [Comparative Example 2]

[0111] 13 grams of methacrylate polyphenylene ether resin SA9000, 38 grams of vinyl group polyphenylene ether resin OPE-2st 2200, 25 grams of TAIC, 12 grams of butadiene-styrene copolymer R-100, 0.1 grams of benzoyl peroxide, 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker and heated to 90°C using an electromagnetic stirrer. Next, 22.5 grams of comparative example phosphorus-containing flame retardant CFR2 were added to the beaker and stirred until clear, thereby obtaining the resin composition of comparative example 2.

[0112] [Comparative Example 3]

[0113] 13 grams of methacrylate polyphenylene ether resin SA9000, 38 grams of vinyl group polyphenylene ether resin OPE-2st 2200, 25 grams of TAIC, 12 grams of butadiene-styrene copolymer R-100, 0.1 grams of benzoyl peroxide, 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker and heated to 90°C using an electromagnetic stirrer. Next, 22.5 grams of comparative phosphorus-containing flame retardant CFR3 were added to the beaker and stirred until clear, after which the resin composition of Comparative Example 3 was prepared.

[0114] [Comparative Example 4]

[0115] 13 grams of methacrylate polyphenylene ether resin SA9000, 38 grams of vinyl group polyphenylene ether resin OPE-2st 2200, 25 grams of TAIC, 12 grams of butadiene-styrene copolymer R-100, 0.1 grams of benzoyl peroxide, 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker and heated and stirred to 90°C using an electromagnetic stirrer. Next, 22.5 grams of comparative example phosphorus-containing flame retardant CFR4 were added to the beaker and stirred until clear to prepare the resin composition of Comparative Example 4.

[0116] [Comparative Example 5]

[0117] 13 grams of methacrylate polyphenylene ether resin SA9000, 38 grams of vinyl group polyphenylene ether resin OPE-2st 2200, 25 grams of TAIC, 12 grams of butadiene-styrene copolymer R-100, 0.1 grams of benzoyl peroxide, 32 grams of toluene, and 30 grams of methyl ethyl ketone were added to a beaker, heated to 90°C using an electromagnetic stirrer, stirred until clear, and then the resin composition of Comparative Example 5 was prepared.

[0118] 4.4. Manufacturing and property measurement of metal foil-clad laminates

[0119] Metal foil-clad laminates were manufactured using the resin compositions of Examples 1-5 and Comparative Examples 1-5. First, glass fiber cloth (model number: 2116) was impregnated with the resin compositions of Examples 1-5 and Comparative Examples 1-5, respectively. Next, the impregnated glass fiber cloth was heated and dried in a 170°C dryer for 3 minutes to obtain a semi-cured (stage B) prepreg. Two copper foils were prepared, and a laminate was obtained by laminating one copper foil, four prepregs, and one copper foil in that order. Next, the laminate was hot-pressed under vacuum at a temperature range of 200°C to 220°C for 2 hours to obtain a metal foil-clad laminate.

[0120] According to the measurement method described above, various properties, flame retardancy, Dk, Df, and Tg were measured for the metal foil-clad laminates of Examples 1-5 and Comparative Examples 1-5, and the results were recorded in Tables 2-1 and 2-2.

[0121] [Table 2-1]

[0122] [Table 2-2]

[0123] As shown in Table 2-1, the metal foil-clad laminate produced from the resin composition containing the phosphorus-containing flame retardant of the present invention simultaneously possessed excellent flame retardancy, excellent heat resistance (high Tg), and good dielectric properties (low Dk and low Df). Examples 2, 3, and 5 demonstrated that when the resin composition contained the phosphorus-containing flame retardant of the present invention within an appropriate content range, the resulting electronic material had optimal flame retardancy, heat resistance, and dielectric properties. Furthermore, the reason for the slightly inferior flame retardancy performance in Example 1 was the insufficient amount of phosphorus-containing flame retardant used. The results of Example 4 showed that excessive addition of phosphorus-containing flame retardant affected the inherent properties of the resin composition, resulting in a deterioration of the electrical properties and heat resistance of the resulting electronic material.

[0124] In contrast, as shown in Table 2-2, metal foil-clad laminates that did not use the resin composition containing the phosphorus-containing flame retardant of the present invention did not simultaneously possess excellent flame retardancy, heat resistance, and dielectric properties. Specifically, in a comparison between Examples 2, 3, and 5 and Comparative Examples 1 to 4, even when the amount of phosphorus-containing flame retardant used was the same, metal foil-clad laminates manufactured using the resin composition without the phosphorus-containing flame retardant of the present invention did not simultaneously possess excellent flame retardancy, heat resistance, and dielectric properties. Furthermore, Comparative Example 5 showed that when the resin composition did not contain any phosphorus-containing flame retardant, the resulting metal foil-clad laminate did not exhibit good flame retardancy or heat resistance.

[0125] The above embodiments exemplify the principles and effects of the present invention and disclose the technical features of the present invention, and are not intended to limit the scope of protection of the present invention. Any modifications or arrangements that can be easily made by a person familiar with the art, provided they do not violate the technical principles of the present invention, fall within the scope claimed by this application. Accordingly, the scope of protection of the present invention is as described in the appended claims.

Claims

1. A phosphorus-containing flame retardant containing a phosphorus-containing compound, The phosphorus-containing compound is 【Chemistry 1】 It includes a first structural segment selected from a group of, The phosphorus content of the phosphorus-containing flame retardant is 8% to 10% by weight relative to the total weight of the phosphorus-containing flame retardant. The phosphorus-containing flame retardant 1 In the 1H-NMR spectrum, signals from 7.80 ppm to 8.10 ppm have an integrated area A, signals from 3.00 ppm to 4.50 ppm have an integrated area B, and the ratio of A to B (A / B) is 0.40 to 0.

70. The aforementioned 1 The 1H-NMR spectrum was obtained by measuring with deuterated chloroform as the solvent and tetramethylsilane as the reference substance; this is a phosphorus-containing flame retardant.

2. The aforementioned 1 The phosphorus-containing flame retardant according to claim 1, wherein the H-NMR spectrum is obtained by measuring it using a nuclear magnetic resonance spectrometer under the following conditions: probe diameter of 5 mm, resonance frequency of 500 megahertz (MHz), pulse width of 10 μs, pulse delay time of 2 seconds, and number of integrations of 32, with the signal of tetramethylsilane set to 0 ppm.

3. The phosphorus-containing flame retardant according to claim 1, wherein the integral area B is 2.85 to 5.

00.

4. The phosphorus-containing flame retardant according to any one of claims 1 to 3, wherein the phosphorus-containing flame retardant has a melting point of 135°C to 190°C as measured by differential scanning calorimetry (DSC).

5. The phosphorus-containing flame retardant was found to have a phosphorus content of 1400 cm⁻¹ in its infrared absorption spectrum obtained by Fourier transform infrared spectroscopy (FTIR) using a thin-film method on a KBr tablet. -1 ~1405cm -1 It has a characteristic peak, or 1456 cm -1 ~1461cm -1 A phosphorus-containing flame retardant according to any one of claims 1 to 3, having a characteristic peak.

6. The phosphorus-containing compound is 【Chemistry 2】 Further including a second structural segment selected from a larger group, The phosphorus-containing flame retardant according to any one of claims 1 to 3, wherein the second structural segment is directly connected to the * portion of the first structural segment.

7. A resin composition comprising a polyphenylene ether resin having an olefin-type carbon-carbon unsaturated double bond, an allyl group-containing compound, an epoxy resin, a phenolic resin, a benzoxazine resin, an elastomer having an olefin-type carbon-carbon unsaturated double bond, a maleimide resin, and a first reactive component selected from the group of combinations thereof, and a phosphorus-containing flame retardant according to any one of claims 1 to 3.

8. The resin composition according to claim 7, wherein the content of the phosphorus-containing flame retardant is 10% to 30% by weight relative to the total weight of the first reactive component and the phosphorus-containing flame retardant.

9. The resin composition according to claim 7, wherein the olefin-type carbon-carbon unsaturated double bond-having polyphenylene ether resin is selected from the group consisting of dihydroxypolyphenylene ether resin, methacrylate polyphenylene ether resin, vinyl group polyphenylene ether resin, and combinations thereof.

10. The resin composition according to claim 7, further comprising a component selected from the group consisting of a filler, a catalyst, an olefin-type carbon-carbon unsaturated double bond-less elastomer, a dispersant, a toughening agent, a viscosity modifier, a plasticizer, a coupling agent, and combinations thereof.

11. A prepreg obtained by impregnating or coating a substrate with the resin composition described in claim 7, and drying the impregnated or coated substrate.

12. A metal foil-clad laminate manufactured by laminating the prepreg described in claim 11 with a metal foil.

13. A metal foil laminate obtained by applying the resin composition according to claim 7 to a metal foil and drying the applied metal foil.