Electrochemical apparatus and electronic apparatus
By using a tungsten-containing positive electrode active material and fluoroethylene carbonate electrolyte, the low-temperature rate and safety issues of lithium-ion batteries are addressed, resulting in improved performance and safety.
Patent Information
- Application Number
- JP2026130396
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2026-07-02
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional lithium-ion batteries face safety issues under extreme operating conditions, particularly low-temperature performance degradation, high-rate discharge limitations, and potential for thermal runaway due to delayed heat dissipation, along with risks from overcharging.
Incorporating a positive electrode active material containing a tungsten element and an electrolyte with fluoroethylene carbonate, which enhances lattice stability and reduces ionic resistance, thereby improving low-temperature rate characteristics and safety.
The combination significantly improves the low-temperature rate performance and safety of lithium-ion batteries by suppressing lattice distortion and reducing surface defects, enhancing interfacial stability and thermal abuse resistance.
Smart Images

Figure 2026182864000001 
Figure 2026182864000002 
Figure 2026182864000003
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to the field of energy storage, and specifically relates to electrochemical devices and electronic apparatuses, in particular to lithium ion batteries. BACKGROUND ART
[0002] With the development of technology and the increasing demand for mobile devices, the demand for electrochemical devices (e.g., lithium ion batteries) under different use conditions has increased significantly, which puts forward higher requirements for the properties of lithium ion batteries, such as high capacity, desirable cycle life, good high-temperature properties, good low-temperature properties, good high-rate discharge properties, overcharge resistance and safety.
[0003] Since the potential difference between the positive electrode active material and the negative electrode active material used in lithium ion batteries is generally 2V or more, only organic solvent electrolyte systems with a wider electrochemical window can be selected. However, these lithium ion batteries are not suitable for use under extreme operating conditions (e.g., low temperature) and have potential safety issues.
[0004] In view of this point, there is a need to provide electrochemical devices and electronic apparatuses with improved low-temperature properties and safety. SUMMARY OF THE INVENTION
[0005] The embodiments of the present invention solve the problems existing in the prior art to a certain extent by providing electrochemical devices and electronic apparatuses with improved low-temperature properties and safety.
[0006] In one aspect of the present invention, the present invention provides an electrochemical device comprising a positive electrode, a negative electrode and an electrolyte, wherein the positive electrode comprises a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, the positive electrode active material layer comprises a positive electrode active material, the positive electrode active material comprises a tungsten element, and the electrolyte comprises fluoroethylene carbonate.
[0007] According to an embodiment of the present invention, if the content of tungsten element is x% with respect to the mass of the positive electrode active material, and the content of fluoroethylene carbonate is a% with respect to the mass of the electrolyte, then x and a satisfy 1 ≤ a / x ≤ 70.
[0008] According to an embodiment of the present invention, if the content of the tungsten element is x% with respect to the mass of the positive electrode active material, then x satisfies 0.05 ≤ x ≤ 1.
[0009] According to an embodiment of the present invention, if the content of fluoroethylene carbonate relative to the mass of the electrolyte is a%, then a satisfies 0.1 ≤ a ≤ 7.
[0010] According to embodiments of the present invention, the electrolyte further contains a compound having a sulfur-oxygen double bond, and the content of the compound having a sulfur-oxygen double bond relative to the mass of the electrolyte is b%, where b satisfies 0.01 ≤ b ≤ 5.
[0011] According to an embodiment of the present invention, if the tungsten content is x% with respect to the mass of the positive electrode active material, then b and x satisfy 1 ≤ b / x ≤ 50.
[0012] According to an embodiment of the present invention, the positive electrode further includes an insulating layer, wherein the insulating layer is formed on the positive electrode current collector and overlaps with the positive electrode active material layer in a portion of the region, or the insulating layer is formed on the positive electrode current collector and does not overlap with the positive electrode active material layer.
[0013] According to an embodiment of the present invention, the insulating layer contains a compound containing an aluminum element, and the content of the aluminum element relative to the mass of the insulating layer is y1%, and the content of the tungsten element relative to the mass of the positive electrode active material is x%, then y1 and x satisfy 50 ≤ y1 / x ≤ 650.
[0014] According to the embodiment of the present invention, the value of y1 is in the range of 30 to 65.
[0015] According to an embodiment of the present invention, the positive electrode further includes an undercoat layer formed between the positive electrode current collector and the positive electrode active material layer.
[0016] According to an embodiment of the present invention, the undercoat layer contains an aluminum element, and the content of the aluminum element relative to the mass of the undercoat layer is y2%, and the content of the tungsten element relative to the mass of the positive electrode active material is x%, then y2 and x satisfy 20 ≤ y2 / x ≤ 550.
[0017] According to the embodiment of the present invention, the value of y2 is in the range of 20 to 50.
[0018] According to embodiments of the present invention, the electrolyte further comprises at least one of succinonitrile, adiponitrile, ethylene glycol bis(2-cyanoethyl) ether, 1,3,6-hexanetricarbonitride, 1,2,3-tris(2-cyanoethoxy)propane, 1,3-propanesultone, ethylene sulfate, vinylene carbonate, and 1-propyl phosphate cyclic anhydride.
[0019] According to an embodiment of the present invention, the positive electrode active material includes lithium nickel cobalt manganese oxide.
[0020] In another embodiment of the present invention, the present invention provides an electronic apparatus including an electrochemical apparatus according to the present invention.
[0021] The tungsten-containing positive electrode active material used in the present invention has high lattice stability and can significantly improve the safety of electrochemical devices at high temperatures and pressures. At the same time, by using an electrolyte containing fluoroethylene carbonate in combination, the low-temperature rate characteristics of the electrochemical device can be significantly improved.
[0022] Further embodiments and advantages of the present invention are described, indicated, or construed in part in the following description. [Modes for carrying out the invention]
[0023] The embodiments of the present invention will be described in detail below. The embodiments of the present invention should not be construed as limiting the present invention.
[0024] Unless otherwise explicitly stated, the following terms used in this specification have the meanings set forth below.
[0025] In the embodiments and claims for carrying out the invention, a list of items connected by the phrase "at least one of" can mean any combination of the listed items. For example, if item A and item B are listed, the phrase "at least one of A and B" means A only, B only, or A and B. In other examples, if items A, B, and C are listed, the phrase "at least one of A, B, and C" means A only, B only, C only, A and B (excluding C), A and C (excluding B), B and C (excluding A), or all of A, B, and C. Item A may contain a single element or more elements. Item B may contain a single element or more elements. Item C may contain a single element or more elements. The phrase "at least one of" has the same meaning as the phrase "at least one of".
[0026] Organic solvent electrolyte systems used in conventional electrochemical devices (e.g., lithium-ion batteries) are prone to combustion under extreme operating conditions (e.g., overcharge and overdischarge, overheating, or overcooling), which poses serious safety risks. In addition, the negative electrode active materials of lithium-ion batteries are generally graphite-based materials, silicon-carbon composite materials, or silicon monoxide materials. These materials have poor kinetic properties under low-temperature operating conditions or high-rate operating conditions, which severely degrades the performance of lithium-ion batteries. Furthermore, conventional lithium-ion batteries have poor low-temperature discharge performance; their performance drops sharply at temperatures below -10°C, and they may even fail to discharge. Conventional lithium-ion batteries also have poor high-rate performance. When discharging continuously at a 5C rate, delayed heat dissipation leads to a high temperature rise, creating a risk of thermal runaway. Moreover, misuse of user terminals may also cause overcharging of lithium-ion batteries, which may further lead to safety accidents such as combustion and explosion.
[0027] Adding additives such as aromatic compounds like fluorobenzene and biphenyl to the electrolyte is one of the means to solve the safety problems of lithium-ion batteries, but these additives not only increase the impedance of the battery, but also cause degradation of low-temperature performance. Safety can also be improved by providing an inorganic coating layer on the surface of the electrode sheet, but this still leads to loss of energy density or degradation of low-temperature performance. In the industry, tungsten element is sometimes added to positive electrode materials to modify the surface energy of the microscopic structure of the material and significantly improve the cycle stability of the material. However, there are still no reports that safety can be improved by adding tungsten element to positive electrode materials. In addition, it is generally believed that the use of fluoroethylene carbonate in the electrolyte is to form a film on the negative electrode and reduce side reactions between the negative electrode and the electrolyte. Based on existing knowledge, it is impossible to predict how the simultaneous use of a positive electrode active material containing tungsten element and an electrolyte containing fluoroethylene carbonate will affect the low-temperature rate performance and safety characteristics of electrochemical devices.
[0028] The present invention solves the problems related to the low-temperature rate and safety characteristics of electrochemical devices by using a positive electrode active material containing a tungsten element and an electrolyte containing fluoroethylene carbonate. Doping the positive electrode active material with the tungsten element can effectively suppress lattice distortion and improve the stability of the lattice, thereby suppressing the volume change of particles during charge-discharge cycles under high-temperature or low-temperature conditions so as to reduce particle cracking and collapse, and improving the interfacial stability. Using the electrolyte containing fluoroethylene carbonate can significantly reduce the ionic resistance and electronic resistance on the surface of the positive electrode active material. The specific combination of the positive electrode active material and the electrolyte of the present invention can not only effectively improve the low-temperature rate characteristics of the electrochemical device, but also significantly improve the safety of the electrochemical device (such as short-circuit safety, thermal abuse safety, etc.).
[0029] I. Positive Electrode The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode active material layer may be a single layer or a plurality of layers. The positive electrode active material layer contains a positive electrode active material, and each layer in the plurality of positive electrode active material layers may contain the same or different positive electrode active materials.
[0030] One main feature of the electrochemical device of the present invention is that the positive electrode active material contains a tungsten element.
[0031] In some embodiments, relative to the mass of the positive electrode active material, when the content of the tungsten element is x%, x satisfies 0.05≦x≦1. In some embodiments, x satisfies 0.01≦x≦0.5. In some embodiments, x may be 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, or 1. Alternatively, x may be in a range consisting of any two of the above numerical values. When the content of the tungsten element in the positive electrode active material is within the above range, the low-temperature rate characteristics and high-temperature high-voltage safety of the electrochemical device can be further improved.
[0032] In some embodiments, the positive electrode further includes an insulating layer, wherein the insulating layer is formed on the positive electrode current collector and overlaps with the positive electrode active material layer in some areas, or the insulating layer is formed on the positive electrode current collector and does not overlap with the positive electrode active material layer.
[0033] In some embodiments, the insulating layer comprises a compound containing aluminum. In some embodiments, the compound containing aluminum comprises alumina ceramics. When the insulating layer comprises a compound containing aluminum, the low-temperature rate characteristics and high-temperature and high-pressure safety of the electrochemical apparatus can be further improved.
[0034] In some embodiments, when the content of the aluminum element is y1% of the mass of the insulating layer, y1 and x satisfy 50 ≤ y1 / x ≤ 650. In some embodiments, y1 and x satisfy 60 ≤ y1 / x ≤ 600. In some embodiments, y1 and x satisfy 100 ≤ y1 / x ≤ 500. In some embodiments, y1 and x satisfy 200 ≤ y1 / x ≤ 400. In some embodiments, y1 / x may be 50, 60, 70, 80, 90, 100, 150, 200, 250, 300, 350, 400, 450, 500, 550, 600, or 650. Alternatively, y1 / x may be within the range of any two of the above values. When the aluminum content in the insulating layer and the tungsten content in the positive electrode active material satisfy the above relationship, surface defects in the crystal structure of the positive electrode active material can be reduced, effectively suppressing the sustained breakdown of the surface passivation layer of the positive electrode active material during the charge-discharge cycle of the electrochemical apparatus and reducing the number of repairs required. As a result, the interfacial stability of the positive electrode active material layer can be sufficiently improved, further improving the low-temperature rate characteristics and high-temperature and high-pressure safety of the electrochemical apparatus.
[0035] In some embodiments, the value of y1 is in the range of 30 to 65. In some embodiments, the value of y1 is in the range of 40 to 60. In some embodiments, y1 may be 30, 35, 40, 45, 50, 55, 60, or 65. Alternatively, y1 may be in the range of any two of the above values. When the content of aluminum element in the insulating layer is within the above range, the low-temperature rate characteristics and high-temperature and high-pressure safety of the electrochemical apparatus can be further improved.
[0036] In some embodiments, the positive electrode further includes an undercoat layer formed between the positive electrode current collector and the positive electrode active material layer.
[0037] In some embodiments, the undercoat layer contains an aluminum element. In some embodiments, the undercoat layer contains alumina ceramics. When the undercoat layer contains a compound containing an aluminum element, the low-temperature rate characteristics and high-temperature and high-pressure safety of the electrochemical apparatus can be further improved.
[0038] In some embodiments, when the content of the aluminum element is y2% of the mass of the undercoat layer, y2 and x satisfy 20 ≤ y2 / x ≤ 550. In some embodiments, y2 and x satisfy 50 ≤ y2 / x ≤ 500. In some embodiments, y2 and x satisfy 100 ≤ y2 / x ≤ 400. In some embodiments, y2 and x satisfy 200 ≤ y2 / x ≤ 400. In some embodiments, y2 / x may be 20, 30, 40, 50, 100, 150, 200, 250, 300, 350, 400, 450, 500, or 550. Alternatively, y2 / x may be within the range of any two of the above values. When the aluminum content in the undercoat layer and the tungsten content in the positive electrode active material satisfy the above relationship, the stability of the positive electrode interface during the charge-discharge cycle of the electrochemical apparatus can be effectively improved, resulting in further improvements to the low-temperature rate characteristics and high-temperature, high-pressure safety of the electrochemical apparatus.
[0039] In some embodiments, the value of y2 is in the range of 20 to 50. In some embodiments, the value of y2 is in the range of 20 to 35. In some embodiments, y2 may be 20, 25, 30, 35, 40, 45, or 50. Alternatively, y2 may be in the range of any two of the above values. When the aluminum element content in the undercoat layer is within the above range, the low-temperature rate characteristics and high-temperature / high-pressure safety of the electrochemical apparatus can be further improved.
[0040] In some embodiments, the positive electrode active material includes lithium cobalt oxide. In some embodiments, the positive electrode active material includes lithium nickel cobalt manganese oxide. Compared to lithium cobalt oxide, doping lithium nickel cobalt manganese oxide with tungsten results in a more stable crystal structure and a more significant improvement in the low-temperature rate characteristics and high-temperature / high-pressure safety of the electrochemical apparatus.
[0041] In some embodiments, a substance of a different composition may be attached to the surface of the positive electrode active material. Examples of surface-attached substances include, but are not limited to, oxides such as alumina, silica, titania, zirconia, magnesia, calcium oxide, boron oxide, antimony oxide, and bismuth oxide; sulfates such as lithium sulfate, sodium sulfate, potassium sulfate, magnesium sulfate, calcium sulfate, and aluminum sulfate; carbonates such as lithium carbonate, calcium carbonate, and magnesium carbonate; and carbon. By attaching a substance to the surface of the positive electrode active material, the oxidation reaction of the electrolyte on the surface of the positive electrode active material can be suppressed, thereby increasing the lifespan of the electrochemical apparatus. If the amount of substance attached to the surface is too small, the effect may not be fully observed. If the amount of substance attached to the surface is too large, the movement of lithium ions may be inhibited, which may increase resistance. In the present invention, a positive electrode active material on which a substance of a different composition is attached to the surface is also referred to as the "positive electrode active material".
[0042] In some embodiments, the shape of the positive electrode active material particles includes, but is not limited to, block-shaped, polyhedral, spherical, ellipsoidal, plate-shaped, needle-shaped, and columnar. In some embodiments, the positive electrode active material particles include primary particles, secondary particles, or a combination thereof. In some embodiments, primary particles may aggregate to form secondary particles.
[0043] There are no restrictions on the type of positive electrode conductive material, and any known conductive material may be used. Examples of positive electrode conductive materials include, but are not limited to, graphite such as natural graphite and artificial graphite; carbon black such as acetylene black; carbon materials such as amorphous carbon such as needle-shaped coke; carbon nanotubes; and graphene. The positive electrode conductive materials may be used alone or in any combination.
[0044] There are no particular restrictions on the type of positive electrode binder used in the manufacture of the positive electrode active material layer; in the case of the coating method, any material that can be dissolved or dispersed in the liquid medium used during electrode manufacture is acceptable. Examples of positive electrode binders include resin polymers such as polyethylene, polypropylene, polyethylene terephthalate, polymethyl methacrylate, polyimide, aromatic polyamide, cellulose, and cellulose nitrate; rubbery polymers such as styrene-butadiene rubber (SBR), nitrile rubber (NBR), fluororubber, isoprene rubber, butadiene rubber, and ethylene-propylene rubber; styrene-butadiene-styrene block copolymer or its hydride, ethylene-propylene-diene ternary copolymer (EPDM), styrene-ethylene-butadiene-ethylene copolymer, and styrene-isoprene- The positive electrode binder may include, but is not limited to, one or more of the following: thermoplastic elastomer polymers such as ethylene block copolymers or their hydrides; soft resin-like polymers such as syndiotactic-1,2-polybutadiene, polyvinyl acetate, ethylene-vinyl acetate copolymer, and propylene-α-olefin copolymer; fluorine-based polymers such as polyvinylidene fluoride (PVDF), polytetrafluoroethylene, fluorinated polyvinylidene fluoride, and polytetrafluoroethylene-ethylene copolymer; and ion-conducting polymer compositions having alkali metal ions (especially lithium ions). The positive electrode binder may be used alone or in any combination.
[0045] The type of solvent used to form the positive electrode slurry is not limited; any solvent capable of dissolving or dispersing the positive electrode active material, conductive material, positive electrode binder, and any thickener used as needed is acceptable. Examples of solvents used to form the positive electrode slurry may include either aqueous solvents or organic solvents. Examples of aqueous media may include, but are not limited to, water and mixed media of alcohol and water. Examples of organic media may include, but are not limited to, aliphatic hydrocarbons such as hexane; aromatic hydrocarbons such as benzene, toluene, xylene, and methylnaphthalene; heterocyclic compounds such as quinoline and pyridine; ketones such as acetone, methyl ethyl ketone, and cyclohexanone; esters such as methyl acetate and methyl acrylate; amines such as diethylenetriamine and N,N-dimethylaminopropylamine; ethers such as diethyl ether, propylene oxide, and tetrahydrofuran (THF); amides such as N-methylpyrrolidone (NMP), dimethylformamide, and dimethylacetamide; and aprotic polar solvents such as hexamethylphosphamide and dimethyl sulfoxide.
[0046] Thickeners are typically used to adjust the viscosity of a slurry. When using an aqueous medium, a slurry can be formed using a thickener and a styrene-butadiene rubber (SBR) emulsion. The type of thickener is not particularly limited and may include, but is not limited to, carboxymethylcellulose, methylcellulose, hydroxymethylcellulose, ethylcellulose, polyvinyl alcohol, oxidized starch, phosphorylated starch, casein, and salts thereof. The thickeners may be used alone or in any combination.
[0047] The type of positive electrode current collector is not particularly limited and may be any known material suitable for use as a positive electrode current collector. Examples of positive electrode current collectors include, but are not limited to, metallic materials such as aluminum, stainless steel, nickel plating, titanium, and tantalum; and carbon materials such as carbon cloth and carbon paper. In some embodiments, the positive electrode current collector is a metallic material. In some embodiments, the positive electrode current collector is aluminum.
[0048] To reduce the electrical contact resistance between the positive electrode current collector and the positive electrode active material layer, the surface of the positive electrode current collector may contain a conductive additive. Examples of conductive additives include, but are not limited to, carbon and precious metals such as gold, platinum, and silver.
[0049] A positive electrode can be manufactured by forming a positive electrode active material layer containing positive electrode active material and a binder on a current collector. The manufacture of a positive electrode using positive electrode active material can be carried out by conventional methods. Specifically, the positive electrode active material, binder, and optionally conductive material and thickener are dry-mixed to form a sheet, and the resulting sheet is pressed onto the positive electrode current collector; or these materials are dissolved or dispersed in a liquid medium to form a slurry, and this slurry is applied to the positive electrode current collector and dried to form a positive electrode active material layer on the current collector. This allows a positive electrode to be obtained.
[0050] In some embodiments, the mass fraction of the positive electrode active material in the positive electrode active material layer is 95%, preferably 96%, and more preferably 97%. In some embodiments, the mass fraction of the positive electrode active material in the positive electrode active material layer is 98%. In some embodiments, the mass fraction of the positive electrode active material in the positive electrode active material layer is 99%. When the mass fraction of the positive electrode active material in the positive electrode active material layer is within the above range, the energy density of the electrochemical apparatus can be significantly increased.
[0051] If the positive electrode active material consists of primary particles, the average particle diameter of the positive electrode active material refers to the primary particle diameter of the positive electrode active material particles. If the primary particles of the positive electrode active material aggregate to form secondary particles, the average particle diameter of the positive electrode active material particles refers to the secondary particle diameter of the positive electrode active material particles.
[0052] In some embodiments, when the average particle size of the positive electrode active material is D μm, the value of D is in the range of 5 to 30. In some embodiments, the value of D is in the range of 10 to 25. In some embodiments, the value of D is in the range of 12 to 20. In some embodiments, D may be 5, 7, 9, 10, 12, 15, 18, 20, 25, or 30. Alternatively, D may be in the range of any two of the above values.
[0053] When the average particle size of the positive electrode active material falls within the above range, a positive electrode active material with a high tap density can be obtained, which can suppress the deterioration of the characteristics of the electrochemical apparatus. Furthermore, problems such as streaking can be prevented during the preparation process of the positive electrode of the electrochemical apparatus (i.e., when the positive electrode active material, conductive material, binder, etc., are slurryed with a solvent and applied in a film form). By mixing two or more positive electrode active materials having different average particle sizes, the packing performance during positive electrode preparation can be further improved.
[0054] The average particle size of the positive electrode active material can be measured using a laser diffraction / scattering particle size distribution analyzer. When using the HORIBA LA-920 particle size distribution analyzer, a 0.1% sodium hexametaphosphate aqueous solution is used as the dispersion medium during measurement, and after 5 minutes of ultrasonic dispersion, the measurement refractive index is set to 1.24. The average particle size of the positive electrode active material can also be measured using a laser diffraction particle size distribution analyzer (Shimadzu Corporation SALD-2300) and a scanning electron microscope (ZEISS EV018, with a sample size of 100 or more).
[0055] II, electrolyte The electrolyte used in the electrochemical apparatus of the present invention comprises an electrolyte and a solvent for dissolving the electrolyte. Another key feature of the electrochemical apparatus of the present invention is that the electrolyte contains fluoroethylene carbonate.
[0056] In some embodiments, when the content of fluoroethylene carbonate relative to the mass of the electrolyte is a%, x and a satisfy 1 ≤ a / x ≤ 70. In some embodiments, x and a satisfy 2 ≤ a / x ≤ 60. In some embodiments, x and a satisfy 5 ≤ a / x ≤ 50. In some embodiments, x and a satisfy 10 ≤ a / x ≤ 30. In some embodiments, a / x may be 1, 2, 3, 5, 8, 10, 20, 30, 40, 50, 60, or 70. Alternatively, a / x may be within the range of any two of the above values. When the fluoroethylene carbonate content in the electrolyte and the tungsten content in the positive electrode active material satisfy the above relationship, surface defects in the crystal structure of the positive electrode active material can be reduced, effectively suppressing the sustained breakdown of the surface passivation layer of the positive electrode active material during the charge-discharge cycle of the electrochemical apparatus and reducing the number of repairs required. As a result, the interfacial stability of the positive electrode active material layer can be sufficiently improved, further improving the low-temperature rate characteristics and high-temperature / high-pressure safety of the electrochemical apparatus.
[0057] In some embodiments, a satisfies 0.1 ≤ a ≤ 7. In some embodiments, a satisfies 0.1 ≤ a ≤ 5. In some embodiments, a satisfies 0.5 ≤ a ≤ 3. In some embodiments, a satisfies 1 ≤ a ≤ 2. In some embodiments, a may be 0.1, 0.2, 0.5, 1, 2, 3, 4, 5, 6, or 7. Alternatively, a may be within the range of any two of the above values. When the fluoroethylene carbonate content in the electrolyte is within the above range, the low-temperature rate characteristics and high-temperature / high-pressure safety of the electrochemical apparatus can be further improved.
[0058] In some embodiments, the electrolyte further comprises a compound having a sulfur-oxygen double bond.
[0059] In some embodiments, if the content of the compound having a sulfur-oxygen double bond relative to the mass of the electrolyte is b%, then b satisfies 0.01 ≤ b ≤ 5. In some embodiments, b satisfies 0.01 ≤ b ≤ 2. In some embodiments, b satisfies 0.05 ≤ b ≤ 1. In some embodiments, b satisfies 0.1 ≤ b ≤ 0.5. In some embodiments, b may be 0.01, 0.02, 0.05, 0.1, 0.2, 0.3, 0.4, 0.5, 0.6, 0.7, 0.8, 0.9, 1, 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or 5. Alternatively, b may be within the range of any two of the above values. When the content of the compound having a sulfur-oxygen double bond in the electrolyte is within the above range, the low-temperature rate characteristics and high-temperature / high-pressure safety of the electrochemical apparatus can be further improved.
[0060] In some embodiments, b and x satisfy 1 ≤ b / x ≤ 50. In some embodiments, b and x satisfy 2 ≤ b / x ≤ 20. In some embodiments, b and x satisfy 5 ≤ b / x ≤ 10. In some embodiments, b / x may be 1, 2, 3, 5, 8, 10, 20, 30, 40, or 50. Alternatively, b / x may be within the range of any two of the above values. When the content of compounds having sulfur-oxygen double bonds in the electrolyte and the content of tungsten in the positive electrode active material satisfy the above relationship, surface defects in the crystal structure of the positive electrode active material can be reduced, effectively suppressing the sustained breakdown of the surface passivation layer of the positive electrode active material during the charge-discharge cycle of the electrochemical apparatus and reducing the number of repairs. As a result, the interfacial stability of the positive electrode active material layer can be sufficiently improved, further improving the low-temperature rate characteristics and high-temperature / high-pressure safety of the electrochemical apparatus.
[0061] In some examples, the compound having a sulfur-oxygen double bond includes at least one of cyclic sulfuric acid esters, linear sulfuric acid esters, linear sulfonic acid esters, cyclic sulfonic acid esters, linear sulfite esters, and cyclic sulfite esters.
[0062] In some examples, the cyclic sulfate ester includes, but is not limited to, one or more of the following: 1,2-ethylene sulfate, 1,2-propylene sulfate, 1,3-propylene sulfate, 1,2-butylene sulfate, 1,3-butylene sulfate, 1,4-butylene sulfate, 1,2-pentylene sulfate, 1,3-pentylene sulfate, 1,4-pentylene sulfate, and 1,5-pentylene sulfate.
[0063] In some examples, the chain-like sulfate ester includes, but is not limited to, one or more of the following: dimethyl sulfate, methyl ethyl sulfate, and diethyl sulfate.
[0064] In some examples, the chain-like sulfonic acid ester includes, but is not limited to, one or more of the following: fluorosulfonic acid esters such as methyl fluorosulfonate and ethyl fluorosulfonate, methyl methanesulfonate, ethyl methanesulfonate, butyl dimethylsulfonate, methyl 2-(methanesulfonyloxy)propionate, and ethyl 2-(methanesulfonyloxy)propionate.
[0065] In some examples, the cyclic sulfonic acid ester is 1,3-propanesultone, 1-fluoro-1,3-propanesultone, 2-fluoro-1,3-propanesultone, 3-fluoro-1,3-propanesultone, 1-methyl-1,3-propanesultone, 2-methyl-1,3-propanesultone, 3-methyl-1,3-propanesultone, 1-propene-1,3-sultone, 2-propylene-1,3-sultone, 1-fluoro-1-propene-1,3-sultone, 2-fluoro-1-propene-1,3-sultone, 3-fluoro-1-propene-1,3-sultone, 1-fluoro-2-propene This includes, but is not limited to, one or more of the following: n-1,3-sultone, 2-fluoro-2-propene-1,3-sultone, 3-fluoro-2-propene-1,3-sultone, 1-methyl-1-propene-1,3-sultone, 2-methyl-1-propene-1,3-sultone, 3-methyl-1-propene-1,3-sultone, 1-methyl-2-propene-1,3-sultone, 2-methyl-2-propene-1,3-sultone, 3-methyl-2-propene-1,3-sultone, 1,4-butanesultone, 1,5-pentanesultone, methylene methanedisulfonate, and ethylene methanedisulfonate.
[0066] In some examples, the chain-like sulfite ester includes, but is not limited to, one or more of the following: dimethyl sulfite, methyl ethyl sulfite, and diethyl sulfite.
[0067] In some examples, the cyclic sulfite ester includes, but is not limited to, one or more of the following: 1,2-ethylene sulfite, 1,2-propylene sulfite, 1,3-propylene sulfite, 1,2-butylene sulfite, 1,3-butylene sulfite, 1,4-butylene sulfite, 1,2-pentylene sulfite, 1,3-pentylene sulfite, 1,4-pentylene sulfite, and 1,5-pentylene sulfite.
[0068] In some examples, the compound having a sulfur-oxygen double bond includes the compound of formula I, [ka] Here, W is [ka] Selected from, L is independently either a single bond or a methylene group. m is 1, 2, 3, or 4. n is 0, 1, or 2, and p is 0, 1, 2, 3, 4, 5, or 6.
[0069] In some examples, the compound of formula I is [ka] It includes at least one of the following.
[0070] In some examples, the dicyclosultone comprises the compound of formula II, [ka] Here, A1, A2, A3, and A4 are each independently selected from substituted or unsubstituted C1-3 alkylene groups, and if substituted, the substituent is selected from C1-5 alkyl groups, halogens, and halogenated C1-5 alkyl groups.
[0071] In some examples, the compound of formula II is [ka] It includes at least one of the following.
[0072] In some examples, the electrolyte further comprises at least one of succinonitrile, adiponitrile, ethylene glycol bis(2-cyanoethyl) ether, 1,3,6-hexanetricarbonitric acid, 1,2,3-tris(2-cyanoethoxy)propane, 1,3-propanesultone, ethylene sulfate, vinylene carbonate, and 1-propyl phosphate cyclic anhydride. In some examples, the content of the compound is 0.1% to 6% of the mass of the electrolyte. In some examples, the content of the compound is 0.5% to 5% of the mass of the electrolyte. In some examples, the content of the compound is 1% to 3% of the mass of the electrolyte. These compounds help to stabilize the interface between the positive electrode and the electrolyte, thereby further improving the overcharge resistance and safety of the electrochemical apparatus at high temperature and high pressure.
[0073] In some embodiments, the electrolyte further comprises any non-aqueous solvent that can be used as a solvent for electrolytes known in the prior art.
[0074] In some examples, the non-aqueous solvent includes, but is not limited to, one or more of the following: cyclic carbonate esters, linear carbonate esters, cyclic carboxylic acid esters, linear carboxylic acid esters, cyclic ethers, linear ethers, phosphorus-containing organic solvents, sulfur-containing organic solvents, and aromatic fluorine-containing solvents.
[0075] In some examples, the cyclic carbonate ester may include, but is not limited to, one or more of ethylene carbonate (EC), propylene carbonate (PC), and butylene carbonate. In some examples, the cyclic carbonate ester has 3 to 6 carbon atoms.
[0076] In some examples, the chain-like carbonate ester may include, but is not limited to, one or more chain-like carbonate esters such as dimethyl carbonate, methyl ethyl carbonate, diethyl carbonate (DEC), methyl-n-propyl carbonate, ethyl-n-propyl carbonate, and di-n-propyl carbonate. The fluorine-substituted chain-like carbonate ester may include, but is not limited to, one or more chain-like carbonates such as bis(fluoromethyl) carbonate, bis(difluoromethyl) carbonate, bis(trifluoromethyl) carbonate, bis(2-fluoroethyl) carbonate, bis(2,2-difluoroethyl) carbonate, bis(2,2,2-trifluoroethyl) carbonate, 2-fluoroethylmethyl carbonate, 2,2-difluoroethylmethyl carbonate, and 2,2,2-trifluoroethylmethyl carbonate.
[0077] In some examples, the cyclic carboxylic acid ester may include, but is not limited to, one or more of γ-butyrolactone and γ-valerolactone. In some examples, some of the hydrogen atoms of the cyclic carboxylic acid ester may be substituted with fluorine.
[0078] In some examples, the chain-like carboxylic acid ester may include, but is not limited to, one or more of the following: methyl acetate, ethyl acetate, propyl acetate, isopropyl acetate, butyl acetate, sec-butyl acetate, isobutyl acetate, tert-butyl acetate, methyl propionate, ethyl propionate, propyl propionate, isopropyl propionate, methyl butyrate, ethyl butyrate, propyl butyrate, methyl isobutyrate, ethyl isobutyrate, methyl valerate, ethyl valerate, methyl pivalate, and ethyl pivalate. In some examples, some of the hydrogen atoms of the chain-like carboxylic acid ester may be substituted with fluorine. In some examples, the fluorine-substituted chain-like carboxylic acid ester may include, but is not limited to, methyl trifluoroacetate, ethyl trifluoroacetate, propyl trifluoroacetate, butyl trifluoroacetate, and 2,2,2-trifluoroethyl trifluoroacetate.
[0079] In some examples, the cyclic ether may include, but is not limited to, one or more of tetrahydrofuran, 2-methyltetrahydrofuran, 1,3-dioxolane, 2-methyl-1,3-dioxolane, 4-methyl-1,3-dioxolane, 1,3-dioxane, 1,4-dioxane, and dimethoxypropane.
[0080] In some examples, the chain ether may include, but is not limited to, one or more of the following: dimethoxymethane, 1,1-dimethoxyethane, 1,2-dimethoxyethane, diethoxymethane, 1,1-diethoxyethane, 1,2-diethoxyethane, ethoxymethoxymethane, 1,1-ethoxymethoxyethane, and 1,2-ethoxymethoxyethane.
[0081] In some examples, the phosphorus-containing organic solvent may include, but is not limited to, one or more of the following: trimethyl phosphate, triethyl phosphate, dimethylethyl phosphate, methyldiethyl phosphate, ethylenemethyl phosphate, ethyleneethyl phosphate, triphenyl phosphate, trimethyl phosphate, triethyl phosphate, triphenyl phosphate, tri(2,2,2-trifluoroethyl) phosphate, and tri(2,2,3,3,3-pentafluoropropyl) phosphate.
[0082] In some examples, the sulfur-containing organic solvent may include, but is not limited to, one or more of the following: sulfolane, 2-methylsulfolane, 3-methylsulfolane, dimethylsulfone, diethylsulfone, ethylmethylsulfone, methylpropylsulfone, dimethyl sulfoxide, methyl methanesulfonate, ethyl methanesulfonate, methyl ethanesulfonate, ethyl ethanesulfonate, dimethyl sulfate, diethyl sulfate, and dibutyl sulfate. In some examples, some of the hydrogen atoms in the sulfur-containing organic solvent may be substituted with fluorine.
[0083] In some examples, the aromatic fluorine-containing solvent includes, but is not limited to, one or more of fluorobenzene, difluorobenzene, trifluorobenzene, tetrafluorobenzene, pentafluorobenzene, hexafluorobenzene, and trifluoromethylbenzene.
[0084] In some examples, the solvent used in the electrolyte of the present invention includes cyclic carbonate esters, linear carbonate esters, cyclic carboxylic acid esters, linear carboxylic acid esters, and combinations thereof. In some examples, the solvent used in the electrolyte of the present invention includes organic solvents selected from the group consisting of ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate, n-propyl acetate, ethyl acetate, and combinations thereof. In some examples, the solvent used in the electrolyte of the present invention includes ethylene carbonate, propylene carbonate, diethyl carbonate, ethyl propionate, propyl propionate, γ-butyrolactone, and combinations thereof.
[0085] In some embodiments, the electrolyte is not particularly limited, and any known electrolyte can be used. In the case of lithium secondary batteries, lithium salts are usually used.Examples of electrolytes include inorganic lithium salts such as LiPF6, LiBF4, LiClO4, LiAlF4, LiSbF6, and LiWF7; lithium tungstates such as LiWOF5; lithium carboxylate salts such as HCO2Li, CH3CO2Li, CH2FCO2Li, CHF2CO2Li, CF3CO2Li, CF3CH2CO2Li, CF3CF2CO2Li, CF3CF2CF2CO2Li, and CF3CF2CF2CF2CO2Li; and FSO3Li, CH3SO3Li, CH2FSO3Li, CHF2SO3Li, CF3SO3Li, and CF3CF2SO3Li. Lithium sulfonate salts such as 3Li, CF3CF2CF2SO3Li, CF3CF2CF2CF2SO3Li; Limidolithium salts such as LiN(FCO)2, LiN(FCO)(FSO2), LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,2-perfluoroethanebissulfonyliimide lithium, cyclic 1,3-perfluoropropanebissulfonyliimide lithium, LiN(CF3SO2)(C4F9SO2); LiC(FSO2)3, LiC(CF3SO2)3 , methylated lithium salts such as LiC(C2F5SO2)3; lithium (malonite) borate salts such as lithium bis(malonite)borate and lithium difluoro(malonite)borate; lithium (malonite) phosphate salts such as lithium tris(malonite)phosphate, lithium difluorobis(malonite)phosphate, and lithium tetrafluoro(malonite)phosphate; and LiPF4(CF3)2, LiPF4(C2F5)2, LiPF4(CF3SO2)2, LiPF4(C2F5SO2)2, LiBF3CF3, LiBF3C2F5, LiB This may include, but is not limited to, fluorine-containing organolithium salts such as F3C3F7, LiBF2(CF3)2, LiBF2(C2F5)2, LiBF2(CF3SO2)2, and LiBF2(C2F5SO2)2; lithium oxalate borate salts such as lithium difluoro(oxalate)borate and lithium bis(oxalate)borate; and lithium oxalate phosphate salts such as lithium tetrafluoro(oxalate)phosphate, lithium difluorobis(oxalate)phosphate, and lithium tris(oxalate)phosphate.
[0086] In some examples, the electrolyte has been selected from LiPF6, LiSbF6, FSO3Li, CF3SO3Li, LiN(FSO2)2, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,2-perfluoroethanebissulfonyliimide lithium, cyclic 1,3-perfluoropropanebissulfonyliimide lithium, LiC(FSO2)3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiBF3CF3, LiBF3C2F5, LiPF3(CF3)3, LiPF3(C2F5)3, lithium difluoro(oxalate) borate, lithium bis(oxalate) borate, and lithium difluorobis(oxalate) phosphate, which helps to improve the output characteristics, high-rate charge-discharge characteristics, high-temperature storage characteristics, and cycle characteristics of electrochemical devices.
[0087] The electrolyte content is not particularly limited as long as it does not impair the effects of the present invention. In some examples, the total molar concentration of lithium in the electrolyte is greater than 0.3 mol / L, greater than 0.4 mol / L, or greater than 0.5 mol / L. In some examples, the total molar concentration of lithium in the electrolyte is less than 3 mol / L, less than 2.5 mol / L, or less than 2.0 mol / L. In some examples, the total molar concentration of lithium in the electrolyte is within the range of any two of the above values. When the electrolyte concentration is within the above range, there is no too little lithium, which is a charged particle, and the viscosity can be kept within an appropriate range, making it easier to ensure good electrical conductivity.
[0088] When two or more electrolytes are used, the electrolyte contains at least one salt selected from the group consisting of monofluorophosphates, borates, oxalates, and fluorosulfonates. In some examples, the electrolyte contains a salt selected from the group consisting of monofluorophosphates, oxalates, and fluorosulfonates. In some examples, the electrolyte contains a lithium salt. In some examples, the content of a salt selected from the group consisting of monofluorophosphates, borates, oxalates, and fluorosulfonates is greater than 0.01% or greater than 0.1% of the weight of the electrolyte. In some examples, the content of a salt selected from the group consisting of monofluorophosphates, borates, oxalates, and fluorosulfonates is less than 20% or less than 10% of the weight of the electrolyte. In some examples, the content of a salt selected from the group consisting of monofluorophosphates, borates, oxalates, and fluorosulfonates is within the range of any two of the above values.
[0089] In some examples, the electrolyte comprises one or more salts selected from the group consisting of monofluorophosphates, borates, oxalates, and fluorosulfonates, and one or more other salts. Examples of other salts include the lithium salts exemplified above. In some examples, the other salts are LiPF6, LiN(FSO2)(CF3SO2), LiN(CF3SO2)2, LiN(C2F5SO2)2, cyclic 1,2-perfluoroethanebissulfonyliimide lithium, cyclic 1,3-perfluoropropanebissulfonyliimide lithium, LiC(FSO2)3, LiC(CF3SO2)3, LiC(C2F5SO2)3, LiBF3CF3, LiBF3C2F5, LiPF3(CF3)3, and LiPF3(C2F5)3. In some examples, the other salt is LiPF6.
[0090] In some examples, the content of other salts relative to the weight of the electrolyte is greater than 0.01% or greater than 0.1%. In some examples, the content of other salts relative to the weight of the electrolyte is less than 20%, less than 15%, or less than 10%. In some examples, the content of other salts is within the range of any two of the above values. Other salts having the above content help to balance the electrical conductivity and viscosity of the electrolyte.
[0091] III, negative electrode The negative electrode comprises a negative electrode current collector and a negative electrode active material layer provided on one or both surfaces of the negative electrode current collector, the negative electrode active material layer comprising a negative electrode active material. The negative electrode active material layer may be a single layer or multiple layers, and each layer of the multiple negative electrode active material may contain the same or different negative electrode active material. The negative electrode active material is any material capable of reversibly intercalating and releasing metal ions such as lithium ions. In some embodiments, the rechargeable capacity of the negative electrode active material is greater than the discharge capacity of the positive electrode active material in order to prevent unintended deposition of lithium metal on the negative electrode during charging.
[0092] Any known current collector can be used as the current collector that maintains the negative electrode active material. Examples of negative electrode current collectors include, but are not limited to, metallic materials such as aluminum, copper, nickel, stainless steel, and nickel-plated steel. In some embodiments, the negative electrode current collector is copper.
[0093] When the negative electrode current collector is made of a metallic material, the form of the negative electrode current collector may include, but is not limited to, metal foil, metal cylinder, metal strip roll, metal plate, metal film, metal lath, punched metal, foamed metal, etc. In some embodiments, the negative electrode current collector is a metal film. In some embodiments, the negative electrode current collector is copper foil. In some embodiments, the negative electrode current collector is rolled copper foil produced by a rolling method, or electrolytic copper foil produced by an electrolytic method.
[0094] In some embodiments, the thickness of the negative electrode current collector is greater than 1 μm or greater than 5 μm. In some embodiments, the thickness of the negative electrode current collector is less than 100 μm or less than 50 μm. In some embodiments, the thickness of the negative electrode current collector is within the range of any two of the above values.
[0095] The negative electrode active material is not particularly limited, as long as it can reversibly intercept and release lithium ions. Examples of negative electrode active materials include, but are not limited to, carbon materials such as natural graphite and artificial graphite, metals such as silicon (Si) and tin (Sn), or oxides of metallic elements such as Si and Sn. The negative electrode active material may be used alone or in any combination.
[0096] The negative electrode active material layer may further contain a negative electrode binder. The negative electrode binder can improve the bonding between negative electrode active material particles and the bonding between the negative electrode active material and the current collector. There are no particular restrictions on the type of negative electrode binder; any material that is stable to the solvent used in the manufacture of the electrolyte and electrodes is acceptable. In some examples, the negative electrode binder includes a resin binder. Examples of resin binders include, but are not limited to, fluororesins, polyacrylonitrile (PAN), polyimide resins, acrylic acid resins, and polyolefin resins. When preparing a negative electrode mixture slurry using an aqueous solvent, the negative electrode binder includes, but is not limited to, carboxymethylcellulose (CMC) or its salts, styrene-butadiene rubber (SBR), polyacrylic acid (PAA) or its salts, and polyvinyl alcohol.
[0097] The negative electrode can be prepared by applying a negative electrode mixture slurry containing negative electrode active material and a resin binder to a negative electrode current collector, drying it, and then rolling it to form a negative electrode active material layer on both sides of the negative electrode current collector.
[0098] IV, Separator To prevent short circuits, a separator is usually provided between the positive and negative electrodes. In this case, the electrolyte of the present invention is typically used by permeating the separator.
[0099] The material and shape of the separator are not particularly limited, as long as they do not significantly impair the effects of the present invention. The separator may be a resin, glass fiber, inorganic material, or the like, made of a material stable with respect to the electrolyte of the present invention. In some embodiments, the separator includes a porous sheet or a nonwoven fabric-like material with excellent liquid retention properties. Examples of materials for the resin or glass fiber separator may include, but are not limited to, polyolefins, aromatic polyamides, polytetrafluoroethylene, and polyethersulfone. In some embodiments, the polyolefin is polyethylene or polypropylene. In some embodiments, the polyolefin is polypropylene. The materials of the separator may be used individually or in any combination.
[0100] The separator may be a material formed by laminating the aforementioned materials, and examples include, but are not limited to, a three-layer separator formed by laminating polypropylene, polyethylene, and polypropylene in that order.
[0101] Examples of inorganic materials may include, but are not limited to, oxides such as alumina and silica, nitrides such as aluminum nitride and silicon nitride, and sulfates (e.g., barium sulfate, calcium sulfate, etc.). The form of the inorganic material may include, but is not limited to, particulate or fibrous forms.
[0102] The separator may be in the form of a film, and examples include, but are not limited to, nonwoven fabrics, woven fabrics, and microporous films. In the form of a film, the separator has a pore size of 0.01 μm to 1 μm and a thickness of 5 μm to 50 μm. In addition to the independent film-like separator described above, a separator formed by using a resin-based binder to form a composite porous layer containing the inorganic particles on the surfaces of the positive and / or negative electrodes can also be used. For example, a separator formed by using a fluororesin as a binder to form a porous layer on both sides of the positive electrode with alumina particles having a 90% particle size of less than 1 μm.
[0103] The thickness of the separator is arbitrary. In some embodiments, the thickness of the separator is greater than 1 μm, greater than 5 μm, or greater than 8 μm. In some embodiments, the thickness of the separator is less than 50 μm, less than 40 μm, or less than 30 μm. In some embodiments, the thickness of the separator is within the range of any two of the above values. When the thickness of the separator is within the above range, insulation and mechanical strength are ensured, and the rate characteristics and energy density of the electrochemical apparatus are ensured.
[0104] When a porous material such as a porous sheet or nonwoven fabric is used as the separator, the porosity of the separator is arbitrary. In some embodiments, the porosity of the separator is greater than 10%, greater than 15%, or greater than 20%. In some embodiments, the porosity of the separator is less than 60%, less than 50%, or less than 45%. In some embodiments, the porosity of the separator is within the range of any two of the above values. When the porosity of the separator is within the above range, insulation and mechanical strength are ensured, sheet resistance is suppressed, and the electrochemical apparatus has good safety characteristics.
[0105] The average pore diameter of the separator is also arbitrary. In some embodiments, the average pore diameter of the separator is less than 0.5 μm or less than 0.2 μm. In some embodiments, the average pore diameter of the separator is greater than 0.05 μm. In some embodiments, the average pore diameter of the separator is within the range of any two of the above values. If the average pore diameter of the separator exceeds the above range, short circuits are more likely to occur. If the average pore diameter of the separator is within the above range, the electrochemical apparatus will have good safety characteristics.
[0106] V, Electrochemical apparatus assembly The electrochemical apparatus assembly includes electrode groups, current collection structures, outer casings, and protective elements.
[0107] The electrode group may be either a laminated structure in which the positive electrode and the negative electrode are stacked with the separator in between, or a structure in which the positive electrode and the negative electrode are wound in a spiral shape with the separator in between. In some embodiments, the ratio of the mass of the electrode group to the internal volume of the battery (electrode group occupancy rate) is greater than 40% or greater than 50%. In some embodiments, the electrode group occupancy rate is less than 90% or less than 80%. In some embodiments, the electrode group occupancy rate is within the range of any two of the above values. When the electrode group occupancy rate is within the above range, the capacity of the electrochemical device can be secured, and the deterioration of characteristics such as repeated charge-discharge characteristics and high-temperature storage due to the increase in internal pressure can be suppressed.
[0108] There are no particular limitations on the current collection structure. In some embodiments, the current collection structure is designed to reduce the resistance of the wiring and connection parts. When the electrode group has a laminated structure, a structure formed by bundling the metal core portions of each electrode layer and welding them to a terminal is preferably used. When the electrode area is large, the internal resistance increases, so it is also preferable to provide two or more terminals within the electrode to reduce the resistance. When the electrode group has a wound structure, the internal resistance can be reduced by providing two or more lead structures for both the positive and negative electrodes and bundling them to a terminal.
[0109] The material of the outer casing is not particularly limited and can be any substance that is stable with respect to the electrolyte used. The outer casing may be made of metals such as nickel-plated steel, stainless steel, aluminum or aluminum alloy, magnesium alloy, or a laminated film of resin and aluminum foil, but is not limited to these. In some embodiments, the outer casing is made of aluminum or an aluminum alloy, or a laminated film.
[0110] The metal outer casing includes, but is not limited to, a sealed structure formed by welding metals together by laser welding, resistance welding, or ultrasonic welding, or a rivet structure using the metals via a resin gasket. The outer casing using the laminated film includes, but is not limited to, a sealed structure formed by heat-fusing resin layers together. To improve sealing performance, a resin different from the resin used in the laminated film may be interposed between the resin layers. When a sealed structure is formed by heat-fusing resin layers via a current collector terminal, the metal is joined to the resin, so a resin having polar groups or a modified resin with polar groups introduced is used as the interposed resin. The shape of the outer casing is also arbitrary, and may be any one of the following, for example, cylindrical, rectangular, laminated, button-shaped, or large.
[0111] As protective elements, a positive temperature coefficient (PTC) whose resistance increases when abnormal heat is generated or excessive current flows, a thermal fuse, a thermistor, and a current interruption valve that interrupts the current flowing through the electrical circuit by rapidly increasing the internal pressure or internal temperature of the battery when abnormal heat is generated are used. The protective elements can be selected to be non-functional during normal use at high currents, or the system can be designed in such a way that abnormal heat generation or thermal runaway does not occur even without protective elements.
[0112] The electrochemical apparatus of the present invention includes any apparatus in which an electrochemical reaction occurs, and specific examples include a lithium metal secondary battery or a lithium ion secondary battery.
[0113] The present invention further provides an electronic apparatus including the electrochemical apparatus described in the present invention.
[0114] The applications of the electrochemical apparatus of the present invention are not particularly limited and can be used in any electronic device known in the prior art. In some embodiments, the electrochemical apparatus of the present invention can be used in, but is not limited to, laptop computers, pen-input computers, mobile computers, e-book players, mobile phones, portable facsimile machines, portable copiers, portable printers, stereo headsets, video recorders, LCD televisions, portable cleaners, portable CD players, mini CDs, transceivers, electronic notebooks, calculators, memory cards, portable tape recorders, radios, backup power supplies, motors, automobiles, motorcycles, auxiliary bicycles, bicycles, lighting fixtures, toys, game consoles, clocks, power tools, flashlights, cameras, large household storage batteries, and lithium-ion capacitors.
[0115] In the following, the preparation of a lithium-ion battery will be explained using a lithium-ion battery as an example and referring to specific examples. Those skilled in the art should understand that the preparation method described in the present invention is merely illustrative, and that any other suitable preparation method is within the scope of the present invention. Examples
[0116] 1. Preparation of lithium-ion batteries 1. Preparation of the negative electrode Artificial graphite, styrene-butadiene rubber, and sodium carboxymethylcellulose were mixed with deionized water in a mass ratio of 96%:2%:2%, and uniformly stirred to obtain a negative electrode slurry. This negative electrode slurry was applied to a 9 μm copper foil, dried, cold-rolled, punched out, and tabs were welded to obtain a negative electrode.
[0117] 2. Preparation of the positive electrode (1) Preparation of lithium nickel-cobalt-manganate containing tungsten as the positive electrode active material Anhydrous ethanol and deionized water were mixed in a volume ratio of 7:3, and 0.05 moles of nickel nitrate hexahydrate, 0.02 moles of cobalt nitrate hexahydrate, and 0.03 moles of manganese acetate tetrahydrate were added and stirred ultrasonically until completely dissolved. The mixture was transferred to a 500 mL autoclave, 0.6 moles of ammonium bicarbonate were added, and the mixture was heated to 120°C, held for 8 hours, cooled, centrifuged, and the precipitate was collected. The precipitate was washed three times with anhydrous ethanol and vacuum-dried at 60°C for 8 hours to obtain a nickel-cobalt-manganese hydroxide precursor. Subsequently, lithium carbonate, tungsten oxide, and the prepared nickel-cobalt-manganese hydroxide precursor were thoroughly mixed and ground, calcined in a tubular furnace at 900°C for 20 hours, cooled, and ground again to obtain lithium nickel-cobalt-manganate containing the tungsten element, which is the positive electrode active material.
[0118] (2) Preparation of lithium cobalt oxide containing tungsten, which is the positive electrode active material. A certain amount of Co3O4 and LiOH powder were weighed out, thoroughly mixed in an agate mortar, and ground. The mixture was then calcined at 900°C for 10 hours. A predetermined amount of sodium tungstate was added to the calcined mixture, and the mixture was ball-milled in ethanol as a solvent for 10 hours. Finally, it was calcined at 800°C for 10 hours to obtain lithium cobalt oxide containing tungsten, which is the positive electrode active material.
[0119] Alumina, carbon nanotubes, and polypropionate were mixed with deionized water in a mass ratio of 65:25:10 and uniformly stirred to obtain an insulating layer or undercoat layer slurry. This insulating layer or undercoat layer slurry was applied to a 12 μm aluminum foil.
[0120] A cathode active material, carbon nanotubes, and polyvinylidene fluoride were mixed with N-methylpyrrolidone (NMP) in a mass ratio of 97:1:2 and uniformly stirred to obtain a cathode active material layer slurry. This cathode active material layer slurry was applied to an undercoat layer or aluminum foil, dried, cold-rolled, punched out, and tabs were welded to obtain a cathode.
[0121] 3. Preparation of the electrolyte In a dry argon gas atmosphere, EC, PC, PP, and DEC (weight ratio 1:1:1:1) were mixed, LiPF6 was added, and the mixture was homogenized to form a base electrolyte with a LiPF6 concentration of 12.5%. By adding additives with different concentrations to the base electrolyte, electrolytes for different examples and comparative examples were obtained.
[0122] The abbreviations and names of the components in the electrolyte are shown in the table below.
[0123] [Table 1A]
[0124] 4. Preparation of the separator A porous polyethylene polymer film was used as the separator.
[0125] 5. Preparation of lithium-ion batteries The obtained positive electrode, separator, and negative electrode were wound in sequence, placed in an outer foil, and an electrolyte injection port was left open. The electrolyte was injected through the injection port, packaged, and then subjected to further processes such as formation and capacity grading to manufacture the lithium-ion battery.
[0126] 2.Measurement method 1. Method for measuring the overcharge deformation rate of lithium-ion batteries At 25°C, the lithium-ion battery was left standing for 30 minutes, then charged with a constant current at a rate of 0.5C to 4.45V, and further charged with a constant voltage at 4.45V to 0.05C. After standing for 60 minutes, the thickness 1 was measured. Subsequently, the process of constant current charging at a rate of 0.1C for 60 minutes, followed by standing for 30 minutes, was repeated five times to bring the lithium-ion battery to a 150% charge state (SOC), and the thickness 2 was measured. The overcharge deformation rate of the lithium-ion battery was calculated using the following formula.
[0127]
number
[0128] 2. Method for measuring the high-temperature short-circuit deformation rate of lithium-ion batteries At 25°C, the lithium-ion battery was left standing for 30 minutes, then charged with a constant current at a rate of 0.5C up to 4.7V, and further charged with a constant voltage at 4.7V down to 0.05C. After standing for 60 minutes, the thickness T1 of the lithium-ion battery was measured. Next, the lithium-ion battery was short-circuited with a 100mΩ resistor for 10 seconds, and the thickness T2 of the lithium-ion battery was measured. The high-temperature short-circuit deformation rate of the lithium-ion battery was calculated using the following formula.
[0129]
number
[0130] 3. Method for measuring the low-temperature rate characteristics of lithium-ion batteries At -20°C, the lithium-ion battery was discharged to 3.0V at 0.2C, allowed to stand for 5 minutes, charged to 4.7V at 0.5C, then charged at a constant voltage to 0.05C, allowed to stand for 5 minutes, and then discharge measurements were performed at 0.2C and 5.0C respectively to obtain discharge capacity 1 and discharge capacity 2. The low-temperature rate of the lithium-ion battery was calculated using the following formula.
[0131]
number
[0132] 3. Measurement results Table 1B shows the effects of the positive electrode active material and electrolyte on the low-temperature rate characteristics and high-temperature / high-pressure safety of lithium-ion batteries. Examples 1-1 to 1-19 and Comparative Examples 1-1 to 1-3 used lithium nickel cobalt manganese oxide with or without tungsten as the positive electrode active material. Examples 1-20 and Comparative Examples 1-4, 1-5, and 1-6 used lithium cobalt oxide with or without tungsten as the positive electrode active material.
[0133] [Table 1B]
[0134] As shown in Comparative Example 1-1, when the positive electrode active material is undoped lithium nickel-cobalt-manganate and the electrolyte does not contain FEC, the lithium-ion battery exhibits high overcharge deformation rates and short-circuit deformation rates, and low low-temperature rates. As shown in Comparative Example 1-2, when the positive electrode active material is lithium nickel-cobalt-manganate containing tungsten, but the electrolyte does not contain FEC, the lithium-ion battery exhibits high overcharge deformation rates and short-circuit deformation rates, and low low-temperature rates. As shown in Comparative Example 1-3, when the electrolyte contains FEC, but the positive electrode active material is undoped lithium nickel-cobalt-manganate, the lithium-ion battery exhibits high overcharge deformation rates and short-circuit deformation rates, and low low-temperature rates.
[0135] As shown in Examples 1-1 to 1-19, when the positive electrode active material is lithium nickel cobalt manganese oxide containing tungsten, and the electrolyte contains FEC, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be significantly reduced, and the low-temperature rate can be significantly increased.
[0136] When the FEC content in the electrolyte (a%) and the tungsten element content in the positive electrode active material (x%) satisfy 1 ≤ a / x ≤ 70, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced, and the low-temperature rate can be significantly increased.
[0137] When the FEC content in the electrolyte is in the range of 0.1% to 7%, the overcharge deformation rate and short-circuit deformation rate of lithium-ion batteries can be further reduced, and the low-temperature rate can be significantly increased.
[0138] When the tungsten content in the positive electrode active material is 0.05% to 1%, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced, and the low-temperature rate can be significantly increased.
[0139] Furthermore, as shown in Comparative Examples 1-4 to 1-6 and Example 1-20, when the positive electrode active material is lithium cobalt oxide containing tungsten and the electrolyte contains FEC, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be significantly reduced, and the low-temperature rate can be significantly increased. Compared to lithium cobalt oxide containing tungsten, lithium nickel cobalt manganese oxide containing tungsten has a more evident effect in improving the properties of lithium-ion batteries.
[0140] Table 2 shows the effects of compounds containing sulfur-oxygen double bonds in the electrolyte, and their relationship to the tungsten content in the positive electrode active material, on the low-temperature rate characteristics and high-temperature / high-pressure safety of lithium-ion batteries. Except for the parameters listed in Table 2, Examples 2-1 to 2-25 had the same settings as Example 1-1.
[0141] [Table 2]
[0142] As the results show, by adding 0.01% to 5% of a compound containing a sulfur-oxygen double bond to the electrolyte, in addition to the presence of FEC, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced, and the low-temperature rate can be significantly increased.
[0143] When the content of a compound having a sulfur-oxygen double bond in the electrolyte (b%) and the content of tungsten element in the positive electrode active material (x%) satisfy 1 ≤ b / x ≤ 50, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced, and the low-temperature rate can be significantly increased.
[0144] Table 3 shows the effects of the aluminum content in the insulating layer and the tungsten content in the positive electrode active material on the low-temperature rate characteristics and high-temperature / high-pressure safety of the lithium-ion battery. Except for the parameters listed in Table 3, Examples 3-1 to 3-16 had the same settings as Example 1-1.
[0145] [Table 3]
[0146] As can be seen from the results, when the aluminum content y1% in the positive electrode insulating layer and the tungsten content x% in the positive electrode active material satisfy 50 ≤ y1 / x ≤ 650, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced, and the low-temperature rate can be further significantly increased.
[0147] When the aluminum content in the positive electrode insulating layer is 30% to 65%, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced, and the low-temperature rate can be significantly increased.
[0148] Table 4 shows the effects of the aluminum content in the undercoat layer and the tungsten content in the positive electrode active material on the low-temperature rate characteristics and high-temperature / high-pressure safety of the lithium-ion battery. Except for the parameters listed in Table 4, Examples 4-1 to 4-15 had the same settings as Example 1-1.
[0149] [Table 4]
[0150] As can be seen from the results, when the aluminum element content y2% in the positive electrode undercoat layer and the tungsten element content x% in the positive electrode active material satisfy 20 ≤ y2 / x ≤ 550, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced, and the low-temperature rate can be further significantly increased.
[0151] When the aluminum element content in the positive electrode undercoat layer is 20% to 50%, the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery can be further reduced, and the low-temperature rate can be significantly increased.
[0152] Table 5 shows the effects of adding additional compounds to the electrolyte on the low-temperature rate characteristics and high-temperature / high-pressure safety of the lithium-ion battery. Except for the parameters listed in Table 5, Examples 5-1 to 5-15 had the same settings as Example 1-1.
[0153] [Table 5]
[0154] As can be seen from the results, in addition to the electrolyte containing dinitrile compounds, the addition of at least one of succinonitrile, adiponitrile, ethylene glycol bis(2-cyanoethyl) ether, 1,3,6-hexanetricarbonitride, 1,2,3-tris(2-cyanoethoxy)propane, 1,3-propanesultone, ethylene sulfate, vinylene carbonate, and 1-propyl phosphate cyclic anhydride can further reduce the overcharge deformation rate and short-circuit deformation rate of the lithium-ion battery while improving the low-temperature rate.
[0155] Throughout this specification, any reference by “Example,” “Part of an Example,” “One Example,” “Another Example,” “Example,” “Specific Example,” or “Part of an Example” means that at least one example or example of the present invention includes the specific features, structures, materials, or properties described in that example or example. Therefore, any reference by “In some examples,” “In an example,” “In one example,” “In another example,” “In one example,” “In a particular example,” or “Example” found anywhere in this specification does not necessarily refer to the same example or example in the present invention. Furthermore, the specific features, structures, materials, or properties described herein can be combined in any preferred manner in one or more examples or examples.
[0156] While exemplary embodiments have been described and explained, those skilled in the art should understand that the embodiments described above are not intended to limit the present invention, and that modifications, substitutions, and changes to the embodiments are permitted as long as they do not depart from the spirit, principles, and scope of the invention.
Claims
1. An electrochemical apparatus comprising a positive electrode, a negative electrode, and an electrolyte, The positive electrode includes a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector. The positive electrode active material layer includes a positive electrode active material, The positive electrode active material contains tungsten, and The electrochemical apparatus contains fluoroethylene carbonate as the electrolyte.
2. The electrochemical apparatus according to claim 1, wherein the content of the tungsten element is x% with respect to the mass of the positive electrode active material, and the content of the fluoroethylene carbonate is a% with respect to the mass of the electrolyte, such that x and a satisfy 1 ≤ a / x ≤ 70.
3. The electrochemical apparatus according to claim 1, wherein, with respect to the mass of the positive electrode active material, the content of the tungsten element is x%, and x satisfies 0.05 ≤ x ≤ 1.
4. The electrochemical apparatus according to claim 1, wherein, with respect to the mass of the electrolyte, the content of fluoroethylene carbonate is a%, and a satisfies 0.1 ≤ a ≤ 7.
5. The electrochemical apparatus according to claim 1, wherein the electrolyte further contains a compound having a sulfur-oxygen double bond, and the content of the compound having a sulfur-oxygen double bond relative to the mass of the electrolyte is b%, where b satisfies 0.01 ≤ b ≤ 5.
6. The electrochemical apparatus according to claim 5, wherein, with respect to the mass of the positive electrode active material, the content of the tungsten element is x%, and b and x satisfy 1 ≤ b / x ≤ 50.
7. The positive electrode further includes an insulating layer, and The insulating layer is formed on the positive electrode current collector and overlaps with the positive electrode active material layer in some areas, or The electrochemical apparatus according to claim 1, wherein the insulating layer is formed on the positive electrode current collector and does not overlap with the positive electrode active material layer.
8. The insulating layer comprises a compound containing an aluminum element, With respect to the mass of the insulating layer, the content of the aluminum element is y 1 If the content of the tungsten element is x% relative to the mass of the positive electrode active material, then y 1 And x is 50 ≤ y 1 The electrochemical apparatus according to claim 7, satisfying / x ≤ 650.
9. y 1 The electrochemical apparatus according to claim 8, wherein the value of is in the range of 30 to 65.
10. The electrochemical apparatus according to claim 1, wherein the positive electrode further includes an undercoat layer formed between the positive electrode current collector and the positive electrode active material layer.
11. The undercoat layer contains an aluminum element, With respect to the mass of the undercoat layer, the content of the aluminum element is y 2 If the content of the tungsten element is x% relative to the mass of the positive electrode active material, then y 2 And x is 20 ≤ y 2 The electrochemical apparatus according to claim 10, satisfying / x ≤ 550.
12. y 2 The electrochemical apparatus according to claim 11, wherein the value of is in the range of 20 to 50.
13. The electrochemical apparatus according to claim 1, wherein the electrolyte further comprises at least one of succinonitrile, adiponitrile, ethylene glycol bis(2-cyanoethyl) ether, 1,3,6-hexanetricarbonitride, 1,2,3-tris(2-cyanoethoxy)propane, 1,3-propanesultone, ethylene sulfate, vinylene carbonate, and 1-propyl phosphate cyclic anhydride.
14. The electrochemical apparatus according to claim 1, wherein the positive electrode active material comprises lithium nickel cobalt manganese oxide.
15. An electronic apparatus comprising an electrochemical apparatus as described in any one of claims 1 to 14.