Edge bonding material, semiconductor package, and method for manufacturing a semiconductor package

The edge bonding material with specific resin and filler compositions addresses the issue of communication delays and thermal cycle resistance in semiconductor packages, ensuring efficient radio wave transmission and stress relief.

JP2026182866APending Publication Date: 2026-11-19RESONAC CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026180109
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2020-11-19
Filing Date
2026-07-29
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional resin materials used in semiconductor packages reduce the transmission efficiency of high-frequency radio waves, leading to communication delays, and there is a lack of knowledge on resin compositions with excellent thermal cycle resistance.

Method used

An edge bonding material containing a curable resin with a thixotropic index of 1.0 or higher, comprising an epoxy resin, a curing agent, an inorganic filler, and cyclic carbodiimide, with a glass transition temperature of 130°C or higher and thermal expansion coefficients of 25 ppm/°C or less at 10°C to 30°C and 80 ppm/°C or less at 180°C to 220°C.

Benefits of technology

The material enhances thermal cycling resistance and maintains high-frequency radio wave transmission efficiency by reducing stress on semiconductor components and allowing selective material selection for different application areas.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026182866000005
    Figure 2026182866000005
  • Figure 2026182866000006
    Figure 2026182866000006
  • Figure 2026182866000007
    Figure 2026182866000007
Patent Text Reader

Abstract

The present invention provides a resin material capable of achieving good thermal cycling resistance, as well as a semiconductor package using the same and a method for manufacturing the same. [Solution] An edge bond material that satisfies at least one of the following (1) to (3): (1) Contains a curable resin and has a thixotropic index of 1.0 or higher at 25°C to 50°C; (2) Contains epoxy resin, a curing agent, an inorganic filler, and a cyclic carbodiimide; (3) Contains epoxy resin, a curing agent, and an inorganic filler, and in the cured product of the edge bond material, the glass transition temperature measured by thermomechanical analysis is 130°C or higher, the coefficient of thermal expansion at 10°C to 30°C is 25 ppm / °C or lower, and the coefficient of thermal expansion at 180°C to 220°C is 80 ppm / °C or lower.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an edge bond material, a semiconductor package, and a method for manufacturing the semiconductor package.

Background Art

[0002] In semiconductor package mounting technology, resin materials called underfill materials for filling gaps between a substrate and an element, molding materials for covering the outer periphery of the element, and the like are used. Improvements in the physical properties of these resin materials are being studied to meet requirements corresponding to their intended use. For example, Japanese Patent Laid-Open No. 2019-011409 describes an underfill material that contains an aminophenol-type epoxy resin, thereby achieving both suppression of an increase in the coefficient of thermal expansion after curing and reduction in viscosity during filling.

Summary of Invention

Problems to be Solved by the Invention

[0003] In recent years, with the spread of 5th generation mobile communication standard (5G) technology, new problems have arisen in the mounting technology for semiconductor packages used in communication devices and the like. For example, it has been pointed out that conventionally used resin materials may reduce the transmission efficiency of high-frequency radio waves, leading to the occurrence of communication delays and the like.

[0004] In view of the above circumstances, an embodiment of the present disclosure has an object to provide a resin material for use in new semiconductor package mounting technology, as well as a semiconductor package using the same and a method for manufacturing the same.

[0005] Resin materials used for mounting semiconductor elements are required to withstand temperature cycles during mounting (thermal cycle resistance). In studies conducted in related research, it has been found that the coefficient of thermal expansion and glass transition temperature of the resin material greatly contribute to thermal cycle resistance. However, knowledge relating to the specific composition of resin materials having excellent thermal cycle resistance has not been obtained.

[0006] In view of the above circumstances, one embodiment of the present disclosure aims to provide a resin material capable of achieving good thermal cycling properties, as well as a semiconductor package using the same and a method for manufacturing the same. [Means for solving the problem]

[0007] The means for accomplishing the above objectives include the following embodiments. <1> An edge bonding material containing a curable resin and having a thixotropic index of 1.0 or higher at 25°C to 50°C. <2> The curable resin includes an epoxy resin and a curing agent. <1> The edge bonding material described above. <3> The epoxy resin comprises an epoxy resin that is liquid at 25°C, and the curing agent comprises a curing agent that is solid at 25°C. <2> The edge bonding material described above. <4> An edge bonding material containing epoxy resin, a hardener, an inorganic filler, and cyclic carbodiimide. <5> It contains epoxy resin, a hardener, and an inorganic filler. An edge bond material in which the cured product has a glass transition temperature of 130°C or higher as measured by thermomechanical analysis, a thermal expansion coefficient of 25 ppm / °C or less at 10°C to 30°C, and a thermal expansion coefficient of 80 ppm / °C or less at 180°C to 220°C. <6> The epoxy resin contains 30% by mass or more of a trifunctional or more epoxy resin relative to the total mass of the epoxy resin. <4> or <5> The edge bonding material described above. <7> The epoxy resin includes a bisphenol F type epoxy resin and a glycidylamine type epoxy resin. <4> ~ <6> An edge bond material as described in any one of the items. <8> The curing agent contains an aliphatic polyamine. <4> ~ <7> An edge bond material as described in any one of the items. <9> A support, a semiconductor element, and an object disposed at the periphery of the space between the support and the semiconductor element. <1> ~ <8> A semiconductor package comprising a cured product of an edge bond material as described in any one of the items. <10> At the periphery of the space between the support and the semiconductor element <1> ~ <8> A method for manufacturing a semiconductor package, comprising the steps of: arranging an edge bond material as described in any one of the items; and curing the edge bond material. [Effects of the Invention]

[0008] According to one embodiment of the present disclosure, a resin material for use in a new semiconductor package mounting technology, as well as a semiconductor package using the same and a method for manufacturing the same are provided. According to one embodiment of the present disclosure, a resin material that can be used in a new semiconductor package mounting technology and that can achieve good thermal cycling resistance is provided, as well as a semiconductor package using the same and a method for manufacturing the same. [Brief explanation of the drawing]

[0009] [Figure 1] This is a schematic cross-sectional view showing a specific example of the shape of a cured edge bond material. [Figure 2] This is a schematic cross-sectional view showing a specific example of the shape of a cured edge bond material. [Figure 3] This is a schematic cross-sectional view showing a specific example of the shape of a cured edge bond material. [Figure 4] This is a schematic plan view illustrating a specific example of the shape of a cured edge bond material. [Figure 5] This is a schematic plan view illustrating a specific example of the shape of a cured edge bond material. [Modes for carrying out the invention]

[0010] The embodiments for carrying out the present invention will be described in detail below. However, the present invention is not limited to the following embodiments. In the following embodiments, the components (including elemental steps, etc.) are not essential unless otherwise specified. The same applies to numerical values ​​and their ranges, and they do not limit the present invention.

[0011] In the present disclosure, the term "step" includes not only a step independent from other steps, but also a step that cannot be clearly distinguished from other steps, as long as the purpose of that step is achieved. In the present disclosure, the numerical ranges indicated by "~" include the numerical values stated before and after "~" as the minimum value and the maximum value, respectively. In the numerical ranges described stepwise in the present disclosure, the upper limit value or the lower limit value described in one numerical range may be replaced with the upper limit value or the lower limit value of another stepwise described numerical range. Further, in the numerical ranges described in the present disclosure, the upper limit value or the lower limit value of the numerical range may be replaced with the values shown in the Examples. In the present disclosure, each component may contain a plurality of corresponding substances. When a plurality of substances corresponding to each component are present in the composition, the content rate or content amount of each component means the total content rate or total content amount of the plurality of such substances present in the composition, unless otherwise specified. In the present disclosure, a plurality of types of particles corresponding to each component may be included. When a plurality of types of particles corresponding to each component are present in the composition, the particle size of each component means a value for the mixture of the plurality of types of particles present in the composition, unless otherwise specified.

[0012] <Edge Bond Material> The edge bond material according to the present disclosure satisfies at least one of the following (1) to (3). (1) Contains a curable resin, and has a thixotropic index of 1.0 or more at 25°C to 50°C (2) Contains an epoxy resin, a curing agent, an inorganic filler, and a cyclic carbodiimide (3) Contains an epoxy resin, a curing agent, and an inorganic filler, and in a cured product of the edge bond material, the glass transition temperature measured by thermomechanical analysis is 130°C or higher, the coefficient of thermal expansion at 10°C to 30°C is 25ppm / °C or less, and the coefficient of thermal expansion at 180°C to 220°C is 80ppm / °C or less

[0013] In the present disclosure, the edge bond material satisfying (1) may be referred to as the first embodiment, the edge bond material satisfying (2) as the second embodiment, and the edge bond material satisfying (3) as the third embodiment, respectively.

[0014] The edge bond material according to the first embodiment may have the properties that either or both of the second embodiment and the third embodiment have, the edge bond material according to the second embodiment may have the properties that either or both of the first embodiment and the third embodiment have, and the edge bond material according to the third embodiment may have the properties that either or both of the first embodiment and the second embodiment have.

[0015] In the present disclosure, the term "edge bond material" means a material that is provided at the peripheral edge of the space between opposing members (for example, between a substrate and a semiconductor element) to join the members to each other. In the present disclosure, the "peripheral edge of the space between opposing members" means a portion corresponding to the outline of the region sandwiched by the opposing members or the vicinity thereof (which may be either or both of the inside and the outside of the region).

[0016] By using the edge bond material in the manufacture of semiconductor packages, for example, the following effects can be expected. (1) If a structure is adopted in which the peripheral edge of the space between opposing members is joined with the edge bond material and the inner side thereof is not filled with resin, the inner side of the peripheral edge is filled with air having a lower dielectric constant than the resin. As a result, the transmission efficiency of high-frequency radio waves is less likely to decrease, and the occurrence of communication delays and the like is suppressed. (2) Inside a semiconductor package, larger stress tends to be applied to the peripheral edge than to the central portion of the opposing members. By disposing the cured product of the edge bond material at the peripheral edge, the cured product of the edge bond material functions as a cushioning material, and the stress applied to the peripheral edge is effectively relieved. (3) Edge bonding material can be used for the periphery of the space between opposing members, and a different material can be used for the interior filling. This makes it possible to select materials according to the part between opposing members. For example, the mechanical properties can be considered when selecting materials for the periphery of the space between opposing members, and the dielectric constant can be considered when selecting materials for the interior filling.

[0017] (First Embodiment) The edge bond material according to the first embodiment has a thixotropic index of 1.0 or higher at 25°C to 50°C. Therefore, the shape immediately after applying the edge bond material to a desired area at the periphery of the space between members does not change easily even if the viscosity decreases during the heating process for curing, and a cured product with a shape close to that immediately after application can be obtained. In addition, the process of applying the edge bond material can be carried out at room temperature, and it is easy to handle. In this disclosure, "the thixotropic index is 1.0 or higher at 25°C to 50°C" means that the thixotropic index is 1.0 or higher at any temperature between 25°C and 50°C.

[0018] From the viewpoint of shape retention, the thixotropic index of the edge bond material in the range of 25°C to 50°C is preferably 1.2 or higher, more preferably 1.5 or higher, and even more preferably 1.7 or higher. There is no specific upper limit specified for the thixotropic index of edge bond materials in the 25°C to 50°C range. For example, it may be 5.0 or less.

[0019] The thixotropic index of the edge bond material is measured by the method described in the examples.

[0020] The type of curable resin included in the edge bond material is not particularly limited and can be selected according to the application of the edge bond material. Specific examples of curable resins include thermosetting resins such as epoxy resins, phenolic resins, melamine resins, and unsaturated polyester resins, and UV-curable resins such as acrylic resins. Among these, epoxy resins are preferred.

[0021] (Second and third embodiments) The edge bond material according to the second embodiment contains an epoxy resin, a hardening agent, an inorganic filler, and a cyclic carbodiimide. The edge bond material according to the third embodiment contains an epoxy resin, a curing agent, and an inorganic filler, and the cured product of the edge bond material has a glass transition temperature of 130°C or higher as measured by thermomechanical analysis, a thermal expansion coefficient of 25 ppm / °C or less at 10°C to 30°C, and a thermal expansion coefficient of 80 ppm / °C or less at 180°C to 220°C.

[0022] As mentioned above, the thermal expansion coefficient and glass transition temperature greatly contribute to the thermal cycling resistance of resin materials. In the second embodiment, it was found that by incorporating cyclic carbodiimide into the edge bond material, a cured product with a high glass transition temperature and a suppressed coefficient of thermal expansion could be obtained. This is thought to achieve good thermal cycling resistance. In the third embodiment, it was found that good thermal cycling resistance could be obtained by setting the glass transition temperature and thermal expansion coefficient of the cured edge bond material within the above range. The reason for this is not entirely clear, but it is thought that because the temperature cycle is performed in a range below the glass transition temperature of the cured material, the change in the thermal expansion coefficient becomes small, and the stress on components such as packages is reduced.

[0023] The thermal expansion coefficient and glass transition temperature of the cured edge bond material are measured by the method described in the examples.

[0024] The components contained in the edge bond material related to this disclosure are described below.

[0025] [Epoxy resin] The type of epoxy resin included in the edge bond material is not particularly limited. Examples include bisphenol-type epoxy resins, naphthalene-type epoxy resins, glycidylamine-type epoxy resins, hydrogenated bisphenol-type epoxy resins, alicyclic epoxy resins, alcohol ether-type epoxy resins, cyclic aliphatic epoxy resins, fluorene-type epoxy resins, and siloxane-based epoxy resins. One type of epoxy resin may be used alone, or two or more types may be used in combination.

[0026] Among the epoxy resins mentioned above, bisphenol-type epoxy resins and glycidylamine-type epoxy resins are preferred from the viewpoint of balancing the properties of the edge bonding material.

[0027] Examples of bisphenol-type epoxy resins include bisphenol A type epoxy resin, bisphenol F type epoxy resin, and bisphenol AD ​​type epoxy resin. Among these, bisphenol-type epoxy resins that are liquid at 25°C are preferred, and bisphenol F type epoxy resins that are liquid at 25°C are more preferred. A commercially available example of a liquid bisphenol F type epoxy resin at 25°C is "Epotote YDF-8170C" from Nippon Steel Chemical & Material Chemicals Co., Ltd.

[0028] When the edge bonding material contains a bisphenol-type epoxy resin, the proportion of the epoxy resin in the total epoxy resin is not particularly limited and can be selected according to the desired properties of the edge bonding material. In the first embodiment, the proportion of the bisphenol-type epoxy resin to the total epoxy resin may be 30% to 100% by mass, 40% to 90% by mass, or 50% to 70% by mass. In the second and third embodiments, the proportion of the bisphenol-type epoxy resin to the total epoxy resin may be 10% to 100% by mass, 10% to 90% by mass, 20% to 80% by mass, 20% to 50% by mass, or 20% to 40% by mass.

[0029] Specific examples of glycidylamine-type epoxy resins include diglycidylamine-type epoxy resins and trifunctional or higher glycidylamine-type epoxy resins. Among these, glycidylamine-type epoxy resins that are liquid at 25°C are preferred, and trifunctional or higher glycidylamine-type epoxy resins that are liquid at 25°C are more preferred.

[0030] Triglycidyl-p-aminophenol is an example of a glycidylamine-type epoxy resin that is liquid at 25°C. Commercially available triglycidyl-p-aminophenol products include "jER-630" and "jER-630LSD" from Mitsubishi Chemical Corporation, and "EP-3950S" from ADEKA Corporation.

[0031] When the edge bonding material contains a glycidylamine-type epoxy resin, the proportion of that resin in the total epoxy resin is not particularly limited and can be selected according to the desired properties of the edge bonding material. In the first embodiment, the proportion of the glycidylamine-type epoxy resin to the total epoxy resin may be 10% to 100% by mass, 20% to 70% by mass, or 30% to 50% by mass. In the second and third embodiments, the proportion of the glycidylamine-type epoxy resin to the total epoxy resin may be 10% to 100% by mass, 20% to 90% by mass, 30% to 80% by mass, 40% to 80% by mass, 50% to 80% by mass, or 60% to 80% by mass.

[0032] The epoxy resin may include a trifunctional or tetrafunctional epoxy resin (i.e., an epoxy resin having three or more epoxy groups in one molecule). Examples of trifunctional or tetrafunctional epoxy resins include trifunctional or tetrafunctional epoxy resins, and from the viewpoint of balancing the elastic modulus of the cured product with the glass transition temperature, a trifunctional epoxy resin is preferred.

[0033] If the epoxy resin contains a trifunctional or higher epoxy resin, the content of the trifunctional or higher epoxy resin may be 30% by mass or more, 40% by mass or more, 50% by mass or more, or 60% by mass or more, based on the total mass of the epoxy resin. Generally, incorporating a large amount of trifunctional or higher epoxy resin tends to increase the elastic modulus of the cured product excessively. However, it has been found that with the edge bond material of this disclosure, good physical properties can be ensured even when trifunctional or higher epoxy resin is incorporated in the above proportion relative to the total mass of epoxy resin. Furthermore, it has been found that when trifunctional or higher epoxy resin is used in combination with cyclic carbodiimide, a particularly high glass transition temperature tends to be achieved. From the viewpoint of preventing the elastic modulus from increasing too much, the content of the trifunctional or more epoxy resin may be 90% by mass or less, 80% by mass or less, or 70% by mass or less, relative to the total mass of the epoxy resin. From this viewpoint, the content of the trifunctional or more epoxy resin may be 30% to 90% by mass, 40% to 90% by mass, 50% to 80% by mass, or 60% to 70% by mass, relative to the total mass of the epoxy resin.

[0034] Epoxy resin may be liquid or solid at 25°C. The edge bond material may contain both a liquid component at 25°C and a solid component at 25°C as the epoxy resin and curing agent. For example, the edge bond material may contain both a liquid epoxy resin at 25°C and a solid curing agent at 25°C. By using both a liquid component at 25°C and a solid component at 25°C as the epoxy resin and curing agent, it is easier to obtain an edge bond material with a thixotropic index of 1.0 or higher in the range of 25°C to 50°C.

[0035] [Hardening agent] The type of curing agent included in the edge bond material is not particularly limited. Examples include amine curing agents, phenol curing agents, acid anhydride curing agents, polymer captan curing agents, polyaminoamide curing agents, isocyanate curing agents, and blocked isocyanate curing agents. The curing agent may be used alone or in combination of two or more types.

[0036] Among the curing agents mentioned above, amine curing agents are preferred from the viewpoint of balancing the properties of the edge bond material. Examples of amine curing agents include aliphatic amine compounds such as diethylenetriamine, triethylenetetramine, n-propylamine, 2-hydroxyethylaminopropylamine, cyclohexylamine, and 4,4'-diamino-dicyclohexylmethane; aromatic amine compounds such as diethyltoluenediamine, 3,3'-diethyl-4,4'-diaminodiphenylmethane, and 2-methylaniline; imidazole compounds such as imidazole, 2-methylimidazole, 2-ethylimidazole, and 2-isopropylimidazole; and imidazoline compounds such as imidazoline, 2-methylimidazolin, and 2-ethylimidazolin.

[0037] The hardener used in edge bond material may be liquid or solid at 25°C. From the viewpoint of balancing ease of application by dispenser, etc., and shape retention, it is preferable to use a hardener that is solid at 25°C, and more preferable to use an amine hardener that is solid at 25°C.

[0038] Examples of amine curing agents that are solid at 25°C include the aliphatic amine compounds mentioned above. Examples of commercially available amine curing agents that are solid at 25°C include "Fujicure FXR-1020", "Fujicure FXR-1030", "Fujicure FXR-1081", and "Fujicure FXR-1121" from T&K TOKA Corporation.

[0039] The curing agent may contain an aliphatic polyamine. Studies have shown that the use of aliphatic polyamines tends to enable rapid curing even at low temperatures. Furthermore, the use of aliphatic polyamines has been shown to maintain good cured material properties even when curing edge bond materials at low temperatures. Therefore, the use of aliphatic polyamines is particularly useful in applications where low-temperature curing is desirable, such as edge bond materials for secondary mounting.

[0040] In this disclosure, an aliphatic polyamine means an aliphatic compound having at least two amino groups, each having at least one active hydrogen atom. An aliphatic polyamine may be an aliphatic polyamine in which all of the amino groups are primary amino groups, or an aliphatic polyamine in which at least one of the amino groups is a secondary polyamine. In one embodiment, it is preferable that the aliphatic polyamine is an aliphatic polyamine containing at least one secondary polyamine among the amino groups, -(R-NH) n It is more preferable that the aliphatic polyamine has multiple amine units represented by -. Here, R represents a divalent aliphatic hydrocarbon group, and n represents the number of alkyleneamine units.

[0041] The curing agent may include a latent curing agent. A latent curing agent is a curing agent that exhibits a curing acceleration function under specific conditions (temperature, etc.). Examples of latent curing agents include ordinary curing accelerators protected by microcapsules, etc., and those with a structure in which a curing accelerator and various compounds form a salt. With a latent curing agent, for example, when a certain temperature is exceeded, the curing accelerator is released into the system from the microcapsules, salt, etc., and exhibits a curing acceleration function.

[0042] Examples of latent curing agents include reaction products of amine compounds and epoxy resins (also called amine-epoxy adduct curing agents) and reaction products of amine compounds and isocyanate compounds or urea compounds (also called urea-type adduct curing agents). Among these, reaction products of epoxy resins and amine compounds are preferred from the viewpoint of low-temperature, short-time curing. In one embodiment, an aliphatic polyamine, which is a latent curing agent, may be used.

[0043] In one embodiment, the edge bond material may contain an aliphatic polyamine and be curable at temperatures of 130°C or lower, 120°C or lower, 110°C or lower, 100°C or lower, or 90°C or lower, and may be curable at the above temperatures within 100 minutes, 60 minutes or 30 minutes.

[0044] The mixing ratio of epoxy resin and curing agent contained in the edge bond material is preferably set so that the ratio of the number of functional groups of the curing agent (active hydrogen in the case of amine curing agents) to the number of epoxy groups of the epoxy resin (number of functional groups of curing agent / number of epoxy groups of epoxy resin) is within the range of 0.5 to 2.0, more preferably within the range of 0.6 to 1.3, and even more preferably within the range of 0.8 to 1.2, in order to minimize the amount of unreacted components of each.

[0045] [Inorganic filler] The edge bond material may contain inorganic fillers. Including inorganic fillers makes it possible to reduce the thermal expansion coefficient of the cured edge bond material and improve its thermal conductivity.

[0046] Examples of inorganic fillers include silica, alumina, calcium carbonate, zirconium silicate, calcium silicate, silicon nitride, aluminum nitride, boron nitride, beryllia, zirconia, zircon, fossilite, steatite, spinel, mullite, titania, talc, clay, mica, and others.

[0047] Among the inorganic fillers mentioned above, silica is preferred from the viewpoint of reducing the coefficient of thermal expansion, and alumina is preferred from the viewpoint of improving thermal conductivity. One type of inorganic filler may be used alone, or two or more types may be used in combination.

[0048] The inorganic filler content in the edge bond material is not particularly limited. From the viewpoint of reducing the thermal expansion coefficient and improving the thermal conductivity of the cured product, the inorganic filler content is preferably 40% by mass or more of the total edge bond material, more preferably 50% by mass or more, and even more preferably 60% by mass or more. From the viewpoint of suppressing the viscosity increase of the edge bond material, the inorganic filler content is preferably 90% by mass or less of the total edge bond material, more preferably 80% by mass or less, and even more preferably 75% by mass or less. When the edge bond material contains inorganic filler as a thixotropic agent, the inorganic filler content refers to the content including the inorganic filler as a thixotropic agent.

[0049] When the inorganic filler is in particulate form, its average particle size is not particularly limited. For example, the volume average particle size of the inorganic filler is preferably 60 μm or less, more preferably 40 μm or less, even more preferably 20 μm or less, and particularly preferably 15 μm or less. When the volume average particle size of the inorganic filler is 60 μm or less, the discharge performance tends to improve when applying the edge bond material using a coating needle or the like. The volume-average particle size of the inorganic filler is preferably 0.05 μm or larger, and more preferably 0.1 μm or larger. When the volume-average particle size of the inorganic filler is 0.05 μm or larger, the increase in viscosity of the edge bond material tends to be suppressed.

[0050] The volume-average particle diameter of the inorganic filler is defined as the particle diameter (D50) at which the cumulative volume from the smaller diameter side reaches 50% in the volume-based particle size distribution obtained by a laser scattering diffraction particle size distribution analyzer.

[0051] [Cyclic carbodiimide] Cyclic carbodiimides are compounds having a cyclic structure in which one or more carbodiimide groups (-N=C=N-) are present in the molecule, and the two nitrogen atoms constituting the carbodiimide group are linked by a linking group. Cyclic carbodiimides may be used individually or in combination of two or more. Cured edge bond materials containing cyclic carbodiimides exhibit good thermal expansion coefficients and glass transition temperatures. Furthermore, incorporating cyclic carbodiimides into edge bonds tends to achieve desired cured product properties while maintaining good thixotropy of the edge bond material.

[0052] From the viewpoint of improving the heat resistance of the edge bond material when it is cured, it is preferable that the cyclic carbodiimide contains two or more carbodiimide groups in its molecule.

[0053] The cyclic structure in a cyclic carbodiimide may be one or more. When there are two or more cyclic structures, they may share two or more atoms, such as in a bicyclo or tricyclo structure, or they may share one atom, such as in a spiro structure. Furthermore, the atoms constituting the cyclic structures may have cyclic groups as substituents, resulting in a structure with two or more cyclic structures.

[0054] The linking group that connects the two nitrogen atoms constituting the carbodiimide group (hereinafter referred to as X) is a linking group with a valency of 2 or higher. If X is a linking group with a valency of 3 or higher, X may be bonded to the polymer or to other cyclic structures. The linking group represented by X includes carbon atoms and hydrogen atoms, and may also include heteroatoms. Examples of heteroatoms include oxygen atoms, nitrogen atoms, sulfur atoms, phosphorus atoms, and the like.

[0055] The number of atoms (member count) in the cyclic structure comprising the carbodiimide group and X is not particularly limited, but is preferably 8 to 50, more preferably 10 to 30, and even more preferably 10 to 20. The number of members referred to here does not include the number of substituent atoms.

[0056] Examples of linking groups represented by X include aliphatic hydrocarbon groups, alicyclic hydrocarbon groups, aromatic hydrocarbon groups, combinations thereof, or combinations of these with heteroatoms.

[0057] Examples of aliphatic hydrocarbon groups represented by X include alkylene groups with 1 to 20 carbon atoms, alkanetriyl groups with 1 to 20 carbon atoms, and alkanetetrayl groups with 1 to 20 carbon atoms. The aliphatic hydrocarbon group may or may not have substituents. Examples of substituents include aryl groups with 6 to 15 carbon atoms, halogen atoms, nitro groups, amide groups, hydroxyl groups, ester groups, ether groups, and aldehyde groups.

[0058] Examples of alicyclic hydrocarbon groups represented by X include cycloalkylene groups having 3 to 20 carbon atoms, cycloalkanetriyl groups having 3 to 20 carbon atoms, and cycloalkanetetrayl groups having 3 to 20 carbon atoms. Alicyclic hydrocarbon groups may or may not have substituents. Examples of substituents include alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 15 carbon atoms, halogen atoms, nitro groups, amide groups, hydroxyl groups, ester groups, ether groups, and aldehyde groups.

[0059] Examples of aromatic hydrocarbon groups represented by X include arylene groups having 5 to 15 carbon atoms, arenetriyl groups having 5 to 15 carbon atoms, and arenetetrayl groups having 5 to 15 carbon atoms. Aromatic hydrocarbon groups may or may not have substituents. Examples of substituents include alkyl groups having 1 to 20 carbon atoms, aryl groups having 6 to 15 carbon atoms, halogen atoms, nitro groups, amide groups, hydroxyl groups, ester groups, ether groups, and aldehyde groups.

[0060] The molecular weight of the cyclic carbodiimide is preferably 100 to 1000, more preferably 100 to 750, and even more preferably 250 to 750.

[0061] The cyclic carbodiimide may be solid or liquid at 25°C. If the cyclic carbodiimide is solid, its form may be any form, including particulate. When the cyclic carbodiimide is in particulate form, the volume-average particle size of the particles is preferably 200 μm or less, more preferably 100 μm or less, even more preferably 20 μm or less, particularly preferably 10 μm or less, and extremely preferably 8 μm or less. Furthermore, the volume-average particle size of the cyclic carbodiimide is preferably 0.1 μm or more, more preferably 0.5 μm or more, and even more preferably 0.8 μm or more.

[0062] The volume-average particle size of cyclic carbodiimide refers to the particle size (D50) at which the cumulative total from the smaller diameter side reaches 50% in the volume-based particle size distribution curve obtained by laser diffraction scattering.

[0063] When the cyclic carbodiimide is in particulate form, the maximum particle size (Dmax) is preferably 2 mm or less, more preferably 800 μm or less, even more preferably 100 μm or less, and particularly preferably 50 μm or less. Furthermore, the maximum particle size (Dmax) of the cyclic carbodiimide is preferably 1 μm or more, more preferably 3 μm or more, and even more preferably 5 μm or more.

[0064] The maximum particle size (Dmax) of cyclic carbodiimide is determined by calculating the volume-based particle size distribution curve using laser diffraction scattering, and represents the maximum particle size on this curve.

[0065] When a cyclic carbodiimide has a spiro structure, examples of cyclic carbodiimides include compounds represented by the following general formula (1).

[0066] [ka]

[0067] In formula (1), Ar 1 ~Ar 4 Each of these independently represents a substituted or unsubstituted orthophenylene group or a 1,2-naphthalene-diyl group. Substituents include C1-C20 alkyl groups, C6-C15 aryl groups, halogen atoms, nitro groups, amide groups, hydroxyl groups, ester groups, ether groups, aldehyde groups, etc. 1 ~Ar 4 Each of these elements may independently have a heterocyclic structure containing a heteroatom. Examples of heteroatoms include oxygen, nitrogen, sulfur, and phosphorus atoms.

[0068] A specific example of a compound represented by general formula (1) is Ar 1 ~Ar 4 Examples of compounds in which all of the groups are substituted or unsubstituted orthophenylene groups, preferably unsubstituted orthophenylene groups.

[0069] These cyclic carbodiimides can be manufactured by methods well known from various documents, patent publications, etc.

[0070] Commercially available cyclic carbodiimides include Carbodista (registered trademark, trade name, Teijin Limited), such as Carbodista TCC-FP10M.

[0071] The content of cyclic carbodiimide in the edge bond material is not particularly limited. From the viewpoint of heat cycle resistance, it is preferable to have 1 part by mass or more, more preferably 5 parts by mass or more, and even more preferably 10 parts by mass or more, per 100 parts by mass of epoxy resin. From the viewpoint of suppressing viscosity increase of the edge bond material, the content of cyclic carbodiimide is preferably 30 parts by mass or less, more preferably 25 parts by mass or less, and even more preferably 20 parts by mass or less, per 100 parts by mass of epoxy resin. From this viewpoint, the content of cyclic carbodiimide is preferably 1 to 30 parts by mass, more preferably 5 to 25 parts by mass, and even more preferably 10 to 20 parts by mass, per 100 parts by mass of epoxy resin.

[0072] [Various additives] In addition to the components mentioned above, the edge bond material may also contain various additives such as thixotropic agents, curing accelerators, stress relaxants, coupling agents, and colorants. If the edge bond material contains components other than epoxy resin, hardener, and inorganic filler, the total content of these components is preferably 10% by mass or less of the total edge bond material, and more preferably 5% by mass or less.

[0073] The edge bond material may contain silica as a thixotropic agent, with a volume-average primary particle diameter of 0.1 nm to 100 nm, preferably 1 nm to 50 nm, and more preferably 10 nm to 30 nm. Such fine particles tend to readily form hydrogen bonds on their surface and exhibit thixotropic properties. When the edge bonding material contains silica with a volume-average primary particle diameter of 0.1 nm to 100 nm as a thixotropic agent, its content is preferably 0.1% to 10% by mass, and more preferably 1% to 5% by mass, relative to the total mass of the edge bonding material.

[0074] (Properties) The edge bonding material is preferably liquid in the range of 25°C to 50°C. In this case, when manufacturing a semiconductor package, it is easy to apply the edge bonding material to a desired area on the periphery of the region between opposing members. Furthermore, by heating and curing it after application, a structure can be easily formed in which the periphery of the region between members is joined with the cured edge bonding material. In this disclosure, "liquid in the range of 25°C to 50°C" means that the substance is liquid at any temperature between 25°C and 50°C.

[0075] (viscosity) The viscosity of the edge bond material in the range of 25°C to 50°C is preferably 10 Pa·s or higher, more preferably 20 Pa·s or higher, and even more preferably 30 Pa·s or higher. When the viscosity of the edge bond material in the range of 25°C to 50°C is 10 Pa·s or higher, the original shape is more easily maintained even after being left to stand after the edge bond material has been applied to a desired part of a substrate or the like. The viscosity of the edge bond material in the range of 25°C to 50°C is preferably 300 Pa·s or less, more preferably 250 Pa·s or less, and even more preferably 230 Pa·s or less. When the viscosity of the edge bond material at 25°C is 300 Pa·s or less, the edge bond material can be applied to desired parts of the substrate, etc., using a dispenser, screen printing machine, inkjet printing machine, etc., resulting in excellent workability. When the viscosity of the edge bond material in the range of 25°C to 50°C is stated as being within the above range, it means that the viscosity of the edge bond material is within the above range at any temperature between 25°C and 50°C.

[0076] The viscosity of the edge bond material at 25°C is preferably 300 Pa·s or less, more preferably 250 Pa·s or less, and even more preferably 230 Pa·s or less. When the viscosity of the edge bond material at 25°C is 300 Pa·s or less, the edge bond material can be applied to desired areas of the substrate, etc., using a dispenser, screen printing machine, inkjet printing machine, etc., resulting in excellent workability.

[0077] The viscosity of the edge bond material at 50°C may be, for example, 200 Pa·s or less, 150 Pa·s or less, or 100 Pa·s or less.

[0078] The viscosity of the edge bond material is measured using a dynamic viscoelasticity measuring device (e.g., AR-2000, manufactured by T.A. Instruments Corporation) at a speed of 10 rpm (revolutions / minute).

[0079] (curing temperature) The curing temperature of the edge bond material is not particularly limited, but from the viewpoint of workability, it is preferably 200°C or lower, more preferably 170°C or lower, and even more preferably 150°C or lower. In addition, depending on the application of the edge bond material, curing at a low temperature may be desired. From the viewpoint of suitability for such applications, the curing temperature of the edge bond material may be 130°C or lower, 120°C or lower, or 110°C or lower. Furthermore, the curing temperature may be 70°C or higher, 80°C or higher, 90°C or higher, or 100°C or higher. From this viewpoint, the curing temperature of the edge bond material may be 70°C to 200°C, 70°C to 170°C, 70°C to 150°C, 70°C to 130°C, 80°C to 120°C, or 90°C to 110°C. The curing temperature of edge bond material is defined as the temperature of the exothermic peak in differential scanning calorimetry (DSC).

[0080] <Semiconductor Packages> The semiconductor package according to this disclosure comprises a support, a semiconductor element, and a cured product of the edge bond material described above, which is disposed at the periphery of the space between the support and the semiconductor element.

[0081] In the semiconductor package with the above configuration, the cured edge bond material described above is placed at the periphery of the space between the support and the semiconductor element. The inside of the periphery may be filled with air or resin or the like.

[0082] The shape of the cured edge bond material, which is placed at the periphery of the space between the support and the semiconductor element, is not particularly limited. Figures 1 to 3 are schematic cross-sectional views showing specific examples of the shape of the cured edge bond material. The shape of the cured edge bond material 3 may be a shape that contacts the surface of the support 1, the side of the semiconductor element 2, and the back surface of the semiconductor element 2 (the surface on the support 1 side), as shown in Figure 1; a shape that contacts the surface of the support 1 and the side of the semiconductor element 2, as shown in Figure 2; or a shape that contacts the surface of the support 1 and the back surface of the semiconductor element 2, as shown in Figure 3.

[0083] The cured edge bond material may be placed along the entire periphery of the space between members, or partially. Figures 4 and 5 are schematic plan views showing specific examples of the shape of the cured edge bond material. The cured edge bond material 3 may be placed continuously along the periphery of the space between members, as shown in Figure 4, or discontinuously along the periphery of the space between members, as shown in Figure 5.

[0084] The distance between the support and the semiconductor element (or the distance at the periphery of the space if the distance is not constant) is not particularly limited and can be selected according to the size and type of the semiconductor package. For example, it can be selected from a range of 50 μm to 1000 μm.

[0085] The properties of the cured edge bond material are not particularly limited and can be selected according to the application of the semiconductor package, etc.

[0086] (Coefficient of thermal expansion) From a reliability standpoint, the coefficient of thermal expansion (CTE1) of the cured edge bond material is preferably 25 ppm / °C or less, more preferably 22 ppm / °C or less, and even more preferably 20 ppm / °C or less. Furthermore, the coefficient of thermal expansion (CTE2) of the cured edge bond material is preferably 80 ppm / °C or less, more preferably 75 ppm / °C or less, and even more preferably 70 ppm / °C or less.

[0087] (Glass transition temperature) From the viewpoint of heat resistance, the glass transition temperature (Tg) of the cured edge bond material is preferably 100°C or higher, more preferably 120°C or higher, even more preferably 130°C or higher, particularly preferably 140°C or higher, and most preferably 150°C or higher.

[0088] To determine whether the edge bond material has the above properties before curing, the determination should be made using a cured product obtained under sufficient curing conditions (for example, 15 minutes at 120°C or 15 minutes at 140°C, depending on the composition of the edge bond material).

[0089] Methods for adjusting the glass transition temperature of the cured edge bond material include adjusting the type of epoxy resin contained in the edge bond material and incorporating cyclic carbodiimide into the edge bond material. For example, using a trifunctional or higher epoxy resin tends to increase the glass transition temperature of the cured product. Methods for adjusting the thermal expansion coefficient of the cured edge bond material to the above range include adjusting the type of resin contained in the edge bond material, and adjusting the type or content of the inorganic filler contained in the edge bond material. For example, using silica as the inorganic filler and increasing its content tends to decrease the thermal expansion coefficient of the cured edge bond material.

[0090] The types of support and semiconductor element are not particularly limited and can be selected from those commonly used in the field of semiconductor packaging. The method of placing the edge bond material around the periphery of the space between the semiconductor element and the support is not particularly limited. For example, it can be done by known methods using a dispenser, screen printing machine, inkjet printing machine, etc.

[0091] <Manufacturing method for semiconductor packages> The semiconductor package manufacturing method of this disclosure is a semiconductor package manufacturing method comprising the steps of: placing the above-mentioned edge bond material on the periphery of the space between a support and a semiconductor element; and curing the edge bond material.

[0092] The type of support, semiconductor element, and support used in the above method are not particularly limited and can be selected from those commonly used in the field of semiconductor packaging. The method of placing the edge bond material at the periphery of the space between the semiconductor element and the support is not particularly limited. For example, it can be done by a known method using a dispenser or the like. Furthermore, the semiconductor element may be placed on the support after the edge bond material is placed on it, or the edge bond material may be placed on the support after the semiconductor element is placed on it. [Examples]

[0093] The present disclosure will be described in detail below with reference to examples, but the scope of the present disclosure is not limited to these examples.

[0094] <Examples 1-1 to 1-3, Comparative Example 1-1> The components shown in Table 1 were mixed in the amounts (parts by mass) shown in Table 1 to prepare the resin material. Details of each component are as follows. The mixing ratio of epoxy resin to curing agent was set so that the number of epoxy groups in the epoxy resin and the number of active hydrogens in the curing agent were equal.

[0095] Epoxy resin 1…Bisphenol F type epoxy resin, which is liquid at 25°C. Epoxy resin 2... Triglycidyl-p-aminophenol is liquid at 25°C.

[0096] Hardening agent 1: Aliphatic amine that is solid at 25°C. Hardener 2: Diethyltoluenediamine, liquid at 25°C. Hardener 3: 3,3'-diethyl-4,4'-diaminodiphenylmethane (liquid at 25°C)

[0097] Thixotropic agent: Aerosilica with a volume-average primary particle size of 10 nm to 20 nm. Inorganic filler: Spherical silica with a volume-average particle size of 30 μm. Coloring agent: Carbon black

[0098] [Table 1]

[0099] (Viscosity measurement) Under specified temperature conditions, the viscosity of the resin material was measured at 10 rpm (revolutions / minute) using a dynamic viscoelasticity measuring device (AR-2000, manufactured by T.A. Instruments).

[0100] (Measurement of thixotropic index) Under specified temperature conditions, the viscosity of the resin material at 2.5 rpm (revolutions / min) and at 10 rpm (revolutions / min) was measured using a dynamic viscoelasticity measuring device (AR-2000, manufactured by T.A. Instruments Co., Ltd.). The thixotropic index was calculated by dividing the viscosity measurement at 2.5 rpm (revolutions / minute) by the viscosity measurement at 10 rpm (revolutions / minute).

[0101] (Creation of evaluation structures) A silicon substrate and a semiconductor chip (10mm x 10mm, 400μm thick) were prepared. A resin material (25°C) was applied at 25°C to the outer periphery of a semiconductor chip (gap: 150 μm) placed on a silicon substrate using a dispenser (needle diameter 0.82 mm). In this state, the resin material was cured by heating at 120°C for 15 minutes.

[0102] When structures made using the resin materials prepared in Examples 1-1 to 1-3 were cut and the cross-sections were observed with an electron microscope, it was observed that the cured resin material was positioned at the periphery of the space between the silicon substrate and the semiconductor chip. The shape of the cured material was almost the same as immediately after it was applied with the dispenser. The resin material prepared in Comparative Example 1-1 spread in the plane of the silicon substrate immediately after being applied to the silicon substrate using the dispenser and was unable to maintain its shape.

[0103] From these results, it was found that resin materials with a thixotropic index of 1.0 or higher in the range of 25°C to 50°C are useful as edge bonding materials.

[0104] <Examples 2-1 to 2-9, Comparative Examples 2-1 to 2-8> The components shown in Tables 2 and 3 were mixed in the amounts indicated in each table to prepare the resin material. Details of each component are as follows. The mixing ratio of epoxy resin to curing agent was set so that the number of epoxy groups in the epoxy resin and the number of active hydrogens in the curing agent were equal.

[0105] • Epoxy resin 1…Bisphenol F type epoxy resin, which is liquid at 25°C • Epoxy resin 2…Liquid triglycidyl-p-aminophenol at 25°C • Hardener 1: Aliphatic amine that is solid at 25°C • Hardener 2: Diethyltoluenediamine, which is liquid at 25°C. • Hardener 3: 3,3'-diethyl-4,4'-diaminodiphenylmethane, liquid at 25°C • Thixotropic agent: Aerosilica with a volume-average primary particle size of 10nm to 20nm. • Cyclic carbodiimide…Product name: Carbodista (registered trademark) TCC-FP10M, Teijin Limited • Inorganic filler: Spherical silica with a volume-average particle size of 30 μm. • Coloring agent: Carbon black

[0106] 〔evaluation〕 The physical properties of the cured resin materials were evaluated according to the following procedure. In Examples 2-1 to 2-4 and Comparative Example 2-1, the resin materials were cured at 120°C for 15 minutes to obtain the cured products. In Examples 2-5 to 2-9 and Comparative Examples 2-2 to 2-8, the cured products were obtained under the curing conditions described in Table 3.

[0107] (Evaluation of thermal expansion coefficient and glass transition temperature) The cured material was cut into pieces with a diameter of 8 mm and a length of 20 mm to prepare measurement samples. Using a thermomechanical analyzer (TMA2940, TA instruments), the change in length of the measurement samples (coefficient of linear expansion) was measured when the temperature was increased from 0°C to 240°C at a rate of 5°C / min using the compression method. The average value of the coefficient of linear expansion in the measurement temperature range of 10°C to 30°C was defined as CTE1, and the average value of the coefficient of linear expansion in the measurement temperature range of 180°C to 200°C was defined as CTE2. In addition, the temperature corresponding to the intersection of the tangents at 100°C and 200°C was determined as the glass transition temperature.

[0108] (Storage modulus) The cured material was cut into 60mm x 10mm x 3mm pieces to prepare measurement samples. Using a viscoelasticity analyzer (RSA III, TA Instruments), the material was heated from 20°C to 300°C at a rate of 5°C / min using the three-point bending method under conditions of a span distance of 40mm and a frequency of 1Hz, and the storage modulus (GPa) at 25°C was measured.

[0109] [Table 2]

[0110] [Table 3]

[0111] In the table, "Inorganic Filler Content" refers to the total content of inorganic fillers and thixotropic agents. In Comparative Example 2-2, the curing agents were formulated such that the ratio of the total number of active hydrogens in the curing agent to the number of epoxy groups in the epoxy resin was 1:1, and the ratio of the number of active hydrogens in curing agent 2 to curing agent 3 was 1:1.

[0112] From these results, it was found that the cured products obtained from the resin materials of the examples have a high glass transition temperature and maintain a good coefficient of thermal expansion. Furthermore, it was found that the resin materials of Examples 2-5 to 2-9 maintain a good glass transition temperature and storage modulus even when cured at relatively low temperatures. Based on these results, the resin materials of the examples are considered suitable as edge bonding materials with excellent heat cycle resistance.

[0113] The disclosures of Japanese Patent Applications Nos. 2020-169384 and 2020-192662 are incorporated herein by reference in their entirety. All documents, patent applications, and technical standards described herein are incorporated by reference to the same extent as if each individual document, patent application, and technical standard were specifically and individually noted as being incorporated by reference.

Claims

1. An edge bonding material containing epoxy resin, a hardener, an inorganic filler, and cyclic carbodiimide.

2. It contains epoxy resin, a hardener, and an inorganic filler. An edge bond material in which the cured product has a glass transition temperature of 130°C or higher as measured by thermomechanical analysis, a thermal expansion coefficient of 25 ppm / °C or less between 10°C and 30°C, and a thermal expansion coefficient of 80 ppm / °C or less between 180°C and 220°C.

3. The edge bonding material according to claim 1 or claim 2, wherein the epoxy resin contains 30% by mass or more of a trifunctional or more epoxy resin relative to the total mass of the epoxy resin.

4. The edge bonding material according to any one of claims 1 to 3, wherein the epoxy resin comprises a bisphenol F type epoxy resin and a glycidylamine type epoxy resin.

5. The edge bond material according to any one of claims 1 to 4, wherein the curing agent comprises an aliphatic polyamine.

6. A semiconductor package comprising a support, a semiconductor element, and a cured product of an edge bond material according to any one of claims 1 to 5, disposed at the periphery of the space between the support and the semiconductor element.

7. A method for manufacturing a semiconductor package, comprising the steps of: placing an edge bond material according to any one of claims 1 to 5 at the periphery of the space between a support and a semiconductor element; and curing the edge bond material.