hardened material
A multi-layered cured product with varying filler content surfaces addresses appearance and resolution issues in solder resist technologies, ensuring high elasticity and low thermal expansion.
Patent Information
- Application Number
- JP2026196332
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2026-08-28
- Publication Date
- 2026-11-19
AI Technical Summary
Existing solder resist technologies face issues with impaired appearance due to linear defects and reduced resolution when film thickness is increased, leading to difficulties in fine patterning.
A cured product with multiple resin layers, each containing a high and low filler content surface, laminated in a specific pattern to achieve uniform filler distribution and improved resolution, while maintaining elasticity and low thermal expansion.
The solution provides a cured product with excellent appearance and resolution, even when thickened, reducing warping and enhancing concealment of circuits.
Smart Images

Figure 2026182897000001_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a cured product. BACKGROUND ART
[0002] In recent years, along with the miniaturization and higher performance of electronic devices, insulating materials (solder resists) used for circuit boards are required to have properties such as high elasticity, low coefficient of thermal expansion, and hiding power in addition to good appearance. As a means for achieving these properties, increasing the film thickness of the solder resist is known.
[0003] For example, a solder resist formed by laminating a plurality of coating films made of a white curable composition containing titanium oxide is disclosed (see Patent Document 1). Further, a method of forming a thick-film resist by performing exposure each time a plurality of photosensitive films are laminated, and developing after lamination is disclosed (see Patent Document 2). PRIOR ART DOCUMENTS PATENT DOCUMENTS
[0004] PATENT DOCUMENT 1 Japanese Unexamined Patent Application Publication No. 2015-5784 PATENT DOCUMENT 2 Japanese Unexamined Patent Application Publication No. 2004-157422 SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION
[0005] However, with the techniques of Patent Document 1 or Patent Document 2, although the generation of holes (pinholes) formed due to influences such as light shielding by foreign matter can be suppressed, the appearance is impaired by unevenness caused by linear defects (coating streaks) formed due to the concentration difference of the curable resin composition. In addition, when the film thickness of the solder resist is increased, fine patterning becomes difficult during exposure of a curable resin layer such as a coating film or a dry film made of the curable resin composition in the process of forming the solder resist, which causes the problem of reduced resolution.
[0006] This invention addresses the above-mentioned problems and aims to provide a cured product that has excellent appearance and excellent resolution even when thickened. [Means for solving the problem]
[0007] One aspect of the present invention is a cured product. The cured product is a cured product in which two or more resin cured layers are laminated, wherein the filler content in each resin cured layer is 30% by mass or more on a basis of total solid content, and each resin cured layer has a filler-high surface area which is a surface region with a relatively high filler content and a filler-low surface area which is a surface region with a relatively low filler content, and in a pair of adjacent resin cured layers, the filler-high surface of one resin cured layer and the filler-low surface of the other resin cured layer are laminated.
[0008] In the cured product according to the above embodiment, it is preferable that the filler content in each resin cured layer is 50 to 90% by mass on a basis of total solid content.
[0009] In the cured product according to the above embodiment, it is preferable that the filler is silica.
[0010] In the cured product according to any of the above embodiments, it is preferable that the resin cured layer is laminated in two to seven layers, the thickness of each resin cured layer is 3 μm to 25 μm, and the thickness of the cured product is 15 μm to 65 μm.
[0011] In the cured product according to any of the above embodiments, it is preferable that the filler is silica, the silica content in each resin cured layer is 50 to 90% by mass on a basis of total solid content, the resin cured layers are stacked in layers of 2 to 7, the thickness of each resin cured layer is 3 μm to 25 μm, and the thickness of the cured product is 15 μm to 65 μm.
[0012] In a cured product according to any of the above embodiments, after the curable resin layers are stacked, vacuum lamination is performed using a vacuum laminator under first lamination conditions of pressurization conditions of 0.1 to 1.0 MPa, heating conditions of 40 to 80°C, and lamination time of 20 to 40 seconds, followed by pressurization conditions of 5 to 10 kgf / cm². 2 Preferably, the laminated material is formed by laminating it under second lamination conditions, which consist of a heating temperature of 40-100°C and a lamination time of 50-70 seconds. [Effects of the Invention]
[0013] According to the present invention, it is possible to provide a cured product that has excellent appearance and excellent resolution even when thickened. [Brief explanation of the drawing]
[0014] [Figure 1] Figure 1 is a schematic cross-sectional view of the cured product according to this embodiment. [Figure 2] Figure 2 is a schematic cross-sectional view of the dry film according to this embodiment. [Figure 3] Figures 3(a) to 3(c) are cross-sectional views illustrating the manufacturing process (lamination process) of the curable resin laminate according to this embodiment. [Modes for carrying out the invention]
[0015] Embodiments of the present invention will be described in detail below. In this specification, unless otherwise specified, the notation "a~b" in the description of numerical ranges means a or greater and b or less.
[0016] If isomers exist for the compound described, all possible isomers can be used in this invention unless otherwise specified.
[0017] In this specification, "(meth)acrylic" means both "acrylic" and "methacrylic." Similarly, "(meth)acrylate" means both "acrylate" and "methacrylate."
[0018] The weight average molecular weight can be measured by a known measurement method, for example, using a gel permeation chromatography (GPC) method as a polystyrene-equivalent molecular weight.
[0019] In the present specification, "resin composition" may be used to mean "curable resin composition". Further, "resin layer" may be used to mean "curable resin layer".
[0020] In the present specification, the "curable resin laminate" refers to the state before curing of the "cured product", and the "curable resin layer" refers to the state before curing of the "cured resin layer".
[0021] In the present specification, the term "process" and "step" refer to work performed to achieve the purpose of that process or step, regardless of whether the content thereof can be clearly distinguished from other processes or steps.
[0022] In the present specification, when the upper limit value and the lower limit value of a numerical range are described separately, all combinations of each lower limit value and each upper limit value are substantially described within a non-contradictory range.
[0023] 1. Cured Product 1-1. Configuration Figure 1 is a schematic cross-sectional view of a cured product 10 according to the present embodiment. As shown in Figure 1, the cured product 10 of the present embodiment is configured by laminating a plurality of cured resin layers 11 to 14.
[0024] The present embodiment (Figure 1) shows an example in which four cured resin layers 11 to 14 are laminated, but the present embodiment is not limited thereto. The number of laminated cured resin layers may be any number as long as it is 2 or more. For example, the number of cured resin layers is preferably 2 or more and 7 or less, more preferably 3 or more and 6 or less, and even more preferably 4. By setting the number of laminated cured resin layers within the above range, it is possible to form the cured product 10 that is excellent in resolution while maintaining high elasticity, low thermal expansion coefficient, and hiding properties.
[0025] 1-1-1. Resin hardening layer Each of the resin curing layers 11-14 contains a filler. The shades of color in the filled areas of each resin curing layer 11-14 in Figure 1 indicate the filler distribution. Darker areas indicate a relatively high filler content, while lighter areas indicate a relatively low filler content. The filler distribution changes stepwise in the lamination direction of each resin curing layer 11-14. That is, the filler is distributed in a stepwise manner in the lamination direction of each resin curing layer 11-14.
[0026] For example, the resin cured layer 11 has a high-filler content surface 11a, which is a surface region with a relatively high filler content, and a low-filler content surface 11b, which is a surface region with a relatively low filler content. In other words, the filler content on the high-filler content surface 11a is higher than the filler content on the low-filler content surface 11b. Preferably, the filler content increases as you approach the high-filler content surface 11a and decreases as you approach the low-filler content surface 11b. In other words, preferably, the filler is distributed in greater quantities as you approach the high-filler content surface 11a and less as you approach the low-filler content surface 11b.
[0027] Similar to the resin cured layer 11 described above, each resin cured layer 12 to 14 also has a high filler content surface 12a to 14a and a low filler content surface 12b to 14b, respectively. In other words, the filler content in the high filler content surface 12a to 14a is higher than the filler content in the low filler content surface 12b to 14b. Preferably, the filler content is higher as you approach the high filler content surface 12a to 14a and lower as you approach the low filler content surface 12b to 14b. In other words, preferably, the filler is distributed in greater quantities as you approach the high filler content surface 12a to 14a and less as you approach the low filler content surface 12b to 14b.
[0028] In this embodiment, the cured product 10 has a pair of adjacent resin cured layers, with a high filler content surface of one resin cured layer and a low filler content surface of the other resin cured layer laminated together.
[0029] More specifically, a pair of adjacent resin-cured layers, resin-cured layer 11 and resin-cured layer 12, are laminated such that the filler-high-content surface 11a of resin-cured layer 11 and the filler-low-content surface 12b of resin-cured layer 12 are in contact. Similarly, resin-cured layer 12 and resin-cured layer 13 are laminated such that the filler-high-content surface 12a of resin-cured layer 12 and the filler-low-content surface 13b of resin-cured layer 13 are in contact. Resin-cured layer 13 and resin-cured layer 14 are laminated such that the filler-high-content surface 13a of resin-cured layer 13 and the filler-low-content surface 14b of resin-cured layer 14 are in contact.
[0030] In this embodiment, since the cured product 10 has resin curing layers 11 to 14 each containing fillers, the elastic modulus of the cured product 10 can be improved and the coefficient of thermal expansion can be reduced compared to conventional products.
[0031] In this embodiment, the cured product 10 is constructed by laminating resin curing layers 11 to 14, and the distribution of filler in each layer changes stepwise in the lamination direction, resulting in a uniform distribution of filler throughout the cured product 10. As a result, the cured product 10 of this embodiment can achieve improved resolution compared to the case where a single layer is formed into a thick film. Furthermore, since the difference in thermal expansion coefficient between the cured product 10 and the substrate is reduced, warping of the cured product 10 can be further reduced when manufacturing printed circuit boards and the like. Moreover, even if pinholes occur in each resin curing layer 11 to 14, since multiple layers are laminated, the pinholes in each layer are filled in by the other layers, thus suppressing damage to the appearance of the cured product 10 as a whole due to pinholes.
[0032] 1-2. Thickness 1-2-1. Cured product The thickness of the cured product 10 is preferably 10 μm or more, 15 μm or more, 20 μm or more, and also preferably 65 μm or less, 60 μm or less, 55 μm or less.
[0033] If the thickness of the cured material 10 is within the above range, the cured material 10 becomes thicker, and therefore the cured material 10 becomes more elastic. As a result, when formed on a printed circuit board or the like, the displacement of the board can be further suppressed. In addition, the concealment of circuits and scratches can be further improved. The thermal expansion coefficient of the cured material 10 can be further reduced.
[0034] 1-2-2. Resin hardening layer The thickness of each resin cured layer 11 to 14 is preferably 3 μm or more, 5 μm or more, 8 μm or more, and also preferably 25 μm or less, 20 μm or less, 15 μm or less.
[0035] By setting the thickness of the resin curing layers 11 to 14 within the above range, the overall distribution of fillers in the cured product 10 becomes more uniform, thereby further improving resolution.
[0036] In this embodiment (Figure 1), an example is shown in which the thicknesses of the resin cured layers 11 to 14 are formed to be substantially the same. However, this embodiment is not limited to this, and the thicknesses of the resin cured layers 11 to 14 may be different. Furthermore, the filler content in each resin cured layer, the filler content on the high-filler-content side, the filler content on the low-filler-content side, and the presence or degree of a filler concentration gradient (in the thickness direction) in the resin cured layer may be the same or different among the multiple resin cured layers.
[0037] 2. Dry film Figure 2 is a schematic cross-sectional view of the dry film D1 of this embodiment. As shown in Figure 2, the dry film D1 has a curable resin layer 21 and a first film P1. To prevent dust and other particles from adhering to the dry film D1, a peelable second film (not shown) may be further laminated on the surface of the curable resin layer 21 opposite to the first film P1. The dry film D1 is used in the manufacturing process of the cured product 10, which will be described later.
[0038] The structure and manufacturing method of the dry film D1 of this embodiment will be described below with reference to Figure 2.
[0039] 2-1. Composition 2-1-1. Curable resin layer The curable resin layer 21 is formed when a curable resin composition, described later, is applied to the first film P1, and the organic solvent contained in the formed curable resin composition layer evaporates and dries. The curable resin composition contains a filler.
[0040] The shades of color in the curable resin layer 21 in Figure 2 represent the distribution of filler. Darker areas indicate a relatively high filler content, while lighter areas indicate a relatively low filler content. The filler content changes stepwise in the lamination direction within the curable resin layer 21. That is, the filler is distributed in the curable resin layer 21 in a stepwise manner in the lamination direction.
[0041] For example, the curable resin layer 21 has a high-filler content surface 21a, which is a surface region with a relatively high filler content, and a low-filler content surface 21b, which is a surface region with a relatively low filler content. In other words, the filler content on the high-filler content surface 21a is higher than the filler content on the low-filler content surface 21b. Preferably, the filler content increases as you approach the high-filler content surface 21a and decreases as you approach the low-filler content surface 21b. In other words, preferably, the filler is distributed in greater quantities as you approach the high-filler content surface 21a and less as you approach the low-filler content surface 21b.
[0042] Typically, fillers contained in a curable resin composition have a higher specific gravity than other components in the curable resin composition. Therefore, when the curable resin composition is applied to the first film P1 to form a curable resin composition layer, the fillers are thought to gradually settle towards the first film P1 side due to gravity. Subsequently, the organic solvent contained in the curable resin composition layer is evaporated and dried to obtain a dry film D1 having the first film P1 and the curable resin layer 21. As a result, the curable resin layer 21 is formed in a state where the distribution of fillers in the curable resin layer 21 changes stepwise in the direction of gravity (a state where the filler content is progressively higher towards the first film P1 side). Consequently, the curable resin layer 21 has a high-filler content surface area 21a, which is a surface area with a relatively high filler content, and a low-filler content surface area 21b, which is a surface area with a relatively low filler content (see Figure 2).
[0043] The thickness of the curable resin layer 21 can be appropriately set within a range such as preferably 3 to 25 μm, more preferably 3 to 20 μm, and even more preferably 3 to 15 μm.
[0044] 2-1-2. The first film The first film P1 in this embodiment has the role of supporting each curable resin layer 21. The first film P1 can be used without particular limitations as long as it is known, and for example, films made of thermoplastic resins such as polyester films such as polyethylene terephthalate and polyethylene naphthalate, polyimide films, polyamide-imide films, polypropylene films, and polystyrene films can be suitably used. Among these, polyester films are preferred from the viewpoint of heat resistance, mechanical strength, and handling. A laminate of these films can also be used as the first film.
[0045] Furthermore, from the viewpoint of improving mechanical strength, the thermoplastic resin film described above is preferably a film stretched in one or two axes.
[0046] The thickness of the first film is not particularly limited and can be, for example, 10 μm to 150 μm.
[0047] 2-1-3. The second film The second film in this embodiment serves to protect the surface of the curable resin layer 21. The second film only needs to have an adhesive strength less than that between the curable resin layer 21 and the first film P1 when the second film is peeled off. For example, polyethylene film, polytetrafluoroethylene film, polypropylene film, surface-treated paper, etc., can be used.
[0048] The thickness of the second film is not particularly limited and is generally selected as appropriate depending on the application, within the range of 10 to 150 μm. The surface of the second film that is in contact with the curable resin layer 21 may be treated with a release agent.
[0049] 2-2. Method for manufacturing dry film The method for manufacturing the dry film of this embodiment includes a preparation step of preparing a curable resin composition; and a manufacturing step of producing a dry film having a first film and a curable resin layer. Each step will be described below.
[0050] 2-2-1. Preparation process In the preparation process, the various raw materials for the curable resin composition, described later, are mixed and stirred to prepare the product.
[0051] 2-2-1-1. Curable resin composition A curable resin composition is a resin composition that constitutes a curable resin layer. The curable resin composition includes an alkali-soluble resin, a photopolymerization initiator, a filler, and, if necessary, other components (additives). The individual components included in the curable resin composition are described below.
[0052] 2-2-1-1-1. Alkali-soluble resins The alkali-soluble resin in this embodiment is not particularly limited, and known materials can be used. Furthermore, the alkali-soluble resin in this embodiment may be either negative or positive type, with the negative type being more preferred. Examples include compounds having two or more phenolic hydroxyl groups, carboxyl group-containing resins, compounds having both phenolic hydroxyl groups and carboxyl groups, and compounds having two or more thiol groups.
[0053] Of these, carboxyl group-containing resins or phenolic resins are preferred because they have excellent adhesion to the substrate. Furthermore, carboxyl group-containing resins are even more preferred because they have excellent developability. The carboxyl group-containing resin may be a carboxyl group-containing photosensitive resin having ethylenically unsaturated groups, or a carboxyl group-containing resin without ethylenically unsaturated groups.
[0054] Specific examples of carboxyl group-containing resins include the following compounds (which may be either oligomers or polymers):
[0055] (1) A carboxyl group-containing resin obtained by copolymerization of an unsaturated carboxylic acid such as (meth)acrylic acid and an unsaturated group-containing compound such as styrene, α-methylstyrene, lower alkyl (meth)acrylate, or isobutylene.
[0056] (2) A carboxyl group-containing urethane resin obtained by polyaddition reaction of diisocyanates such as aliphatic diisocyanates, branched aliphatic diisocyanates, alicyclic diisocyanates, and aromatic diisocyanates with carboxyl group-containing dialcohol compounds such as dimethylolpropionic acid and dimethylolbutanoic acid, and diol compounds such as polycarbonate polyols, polyether polyols, polyester polyols, polyolefin polyols, acrylic polyols, bisphenol A alkylene oxide adduct diols, compounds having phenolic hydroxyl groups, and compounds having alcoholic hydroxyl groups.
[0057] (3) A urethane resin containing terminal carboxyl groups, obtained by reacting an acid anhydride at the ends of a urethane resin by a polyaddition reaction of a diisocyanate compound such as aliphatic diisocyanate, branched aliphatic diisocyanate, alicyclic diisocyanate, or aromatic diisocyanate with a diol compound such as a polycarbonate polyol, polyether polyol, polyester polyol, polyolefin polyol, acrylic polyol, bisphenol A alkylene oxide adduct diol, a compound having a phenolic hydroxyl group, or an alcoholic hydroxyl group.
[0058] (4) A carboxyl group-containing urethane resin obtained by polyaddition reaction of diisocyanate with (meth)acrylate or partially acid anhydride-modified product thereof of a bifunctional epoxy resin such as bisphenol A type epoxy resin, hydrogenated bisphenol A type epoxy resin, bisphenol F type epoxy resin, bisphenol S type epoxy resin, bixylenol type epoxy resin, or biphenol type epoxy resin, a carboxyl group-containing dialcohol compound, and a diol compound.
[0059] (5) A carboxyl group-containing urethane resin obtained by adding a compound having one hydroxyl group and one or more (meth)acryloyl groups in its molecule, such as hydroxyalkyl (meth)acrylate, during the synthesis of the resin of (2) or (4) above, and then (meth)acrylizing the terminal (meth)acrylic.
[0060] (6) A carboxyl group-containing urethane resin obtained by adding a compound having one isocyanate group and one or more (meth)acryloyl groups in its molecule, such as a reaction product of isophorone diisocyanate and pentaerythritol triacrylate, to the synthesis of the resin of (2) or (4) above, and then (meth)acrylicating the terminals.
[0061] (7) A carboxyl group-containing resin obtained by reacting a polyfunctional epoxy resin with (meth)acrylic acid and adding dibasic acid anhydrides such as phthalic anhydride, tetrahydrophthalic anhydride, and hexahydrophthalic anhydride to the hydroxyl groups present in the side chain.
[0062] (8) A carboxyl group-containing resin obtained by reacting a polyfunctional epoxy resin, in which the hydroxyl groups of a bifunctional epoxy resin are further epoxidized with epichlorohydrin, with (meth)acrylic acid, and then adding a dibasic acid anhydride to the resulting hydroxyl groups.
[0063] (9) A carboxyl group-containing polyester resin obtained by reacting a polyfunctional oxetane resin with a dicarboxylic acid and adding a dibasic acid anhydride to the resulting primary hydroxyl group.
[0064] (10) A carboxyl group-containing resin obtained by reacting a reaction product obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with an alkylene oxide such as ethylene oxide or propylene oxide with an unsaturated group-containing monocarboxylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.
[0065] (11) A carboxyl group-containing resin obtained by reacting a reaction product obtained by reacting a compound having multiple phenolic hydroxyl groups in one molecule with a cyclic carbonate compound such as ethylene carbonate or propylene carbonate with an unsaturated group-containing monocarboxylic acid, and then reacting the resulting reaction product with a polybasic acid anhydride.
[0066] (12) A carboxyl group-containing resin obtained by reacting an epoxy compound having multiple epoxy groups in one molecule with a compound having at least one alcoholic hydroxyl group and one phenolic hydroxyl group in one molecule, such as p-hydroxyphenethyl alcohol, and an unsaturated group-containing monocarboxylic acid such as (meth)acrylic acid, and then reacting the alcoholic hydroxyl group of the reaction product with a polybasic acid anhydride such as maleic anhydride, tetrahydrophthalic anhydride, trimellitic anhydride, pyromellitic anhydride, or adipic anhydride.
[0067] (13) A carboxyl group-containing resin obtained by adding a compound having one epoxy group and one or more (meth)acryloyl groups in the molecule, such as glycidyl (meth)acrylate or α-methylglycidyl (meth)acrylate, to the carboxyl group-containing resin described in (1) to (12) above.
[0068] It is preferable that the carboxyl group-containing resin contains at least one of the carboxyl group-containing resins described in (7), (8), (10), (11), and (13), and it is more preferable to include the carboxyl group-containing resin described in (10) or (11) from the viewpoint of further improving insulation reliability.
[0069] The acid value of the alkali-soluble resin is not particularly limited as long as it does not hinder the effects of the present invention, and is, for example, 20 to 200 mg KOH / g, preferably 40 to 150 mg KOH / g. When the acid value of the alkali-soluble resin is within this range, development of the curable resin laminate with an alkaline aqueous solution after exposure becomes easier, and the drawing of a normal cured product pattern becomes easier.
[0070] The weight-average molecular weight of the alkali-soluble resin varies depending on the resin skeleton, but can be between 1,500 and 150,000, preferably between 1,500 and 100,000, more preferably between 1,500 and 50,000, and particularly preferably between 1,500 and 30,000. When the weight-average molecular weight is within this range, it exhibits excellent tack-free performance, storage stability, moisture resistance of the curable resin laminate after exposure, and developability, and further suppresses film thinning during development and a decrease in resolution.
[0071] Alkali-soluble resins can be used alone or in combination.
[0072] 2-2-1-1-2. Photopolymerization Initiators The photopolymerization initiator in this embodiment is not particularly limited, and any photopolymerization initiator known as a photopolymerization initiator or photoradical generator can be used.
[0073] Examples of photopolymerization initiators include bis-(2,6-dichlorobenzoyl)phenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-2,5-dimethylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-4-propylphenylphosphine oxide, bis-(2,6-dichlorobenzoyl)-1-naphthylphosphine oxide, bis-(2,6-dimethoxybenzoyl)phenylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,4,4-trimethylpentylphosphine oxide, bis-(2,6-dimethoxybenzoyl)-2,5-dimethylphenylphosphine oxide, and bis-(2,4,6-trimethylbenzoyl)-phenylphosphine oxide, among other bisacylphosphine oxides; Monoacyl phosphine oxides such as 2,6-dimethoxybenzoyldiphenylphosphine oxide, 2,6-dichlorobenzoyldiphenylphosphine oxide, 2,4,6-trimethylbenzoylphenylphosphate methyl ester, 2-methylbenzoyldiphenylphosphine oxide, pivaloylphenylphosphate isopropyl ester, and 2,4,6-trimethylbenzoyldiphenylphosphine oxide; Hydroxyacetophenones such as 1-hydroxycyclohexylphenyl ketone, 1-[4-(2-hydroxyethoxy)-phenyl]-2-hydroxy-2-methyl-1-propan-1-one, 2-hydroxy-1-{4-[4-(2-hydroxy-2-methylpropionyl)-benzyl]phenyl}-2-methyl-propan-1-one, and 2-hydroxy-2-methyl-1-phenylpropan-1-one; Benzoin compounds such as benzoin, benzyl benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin n-propyl ether, benzoin isopropyl ether, and benzoin n-butyl ether; Benzoin alkyl ethers; Benzophenones such as benzophenone, p-methylbenzophenone, Michler ketone, methylbenzophenone, 4,4'-dichlorobenzophenone, and 4,4'-bisdiethylaminobenzophenone; Acetophenones such as acetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2-phenylacetophenone, 1,1-dichloroacetophenone, 1-hydroxycyclohexylphenyl ketone, 2-methyl-1-[4-(methylthio)phenyl]-2-morpholino-1-propanone, 2-benzyl-2-dimethylamino-1-(4-morpholinophenyl)-butanone-1, 2-(dimethylamino)-2-[(4-methylphenyl)methyl]-1-[4-(4-morpholinyl)phenyl]-1-butanone, and N,N-dimethylaminoacetophenone; Thioxanthones such as thioxanthone, 2-ethylthioxanthone, 2-isopropylthioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, 2-chlorothioxanthone, and 2,4-diisopropylthioxanthone; Anthraquinones such as anthraquinone, chloroanthraquinone, 2-methylanthraquinone, 2-ethylanthraquinone, 2-tert-butylanthraquinone, 1-chloroanthraquinone, 2-amylanthraquinone, and 2-aminoanthraquinone; Ketals such as acetophenone dimethyl ketal and benzyl dimethyl ketal; Benzoate esters such as ethyl-4-dimethylaminobenzoate, 2-(dimethylamino)ethylbenzoate, and p-dimethylbenzoate ethyl ester; Oxime esters such as 1,2-octanedione, 1-[4-(phenylthio)-2-(O-benzoyl oxime)], ethanone, and 1-[9-ethyl-6-(2-methylbenzoyl)-9H-carbazole-3-yl]-1-(O-acetyl oxime); Titanocenes such as bis(η5-2,4-cyclopentadien-1-yl)-bis(2,6-difluoro-3-(1H-pyrrole-1-yl)phenyl)titanium and bis(cyclopentadienyl)-bis[2,6-difluoro-3-(2-(1-pyrrole-1-yl)ethyl)phenyl]titanium; Examples include phenyl disulfide 2-nitrofluorene, butyroine, anisoin ethyl ether, azobisisobutyronitrile, and tetramethylthiuram disulfide. These can be used individually or in combination.
[0074] The amount of photopolymerization initiator is not particularly limited, but for example, 0.5 to 20% by mass is preferred based on 100% by mass of the alkali-soluble resin. When the amount of photopolymerization initiator is within this range, a curable resin composition and cured product can be obtained that has superior surface curability, is less prone to halation, and has better resolution.
[0075] 2-2-1-1-3. Filler Examples of fillers include inorganic fillers and organic fillers.
[0076] Inorganic fillers that can be used include metal oxides such as silica, alumina, and titanium oxide; metal hydroxides such as aluminum hydroxide and magnesium hydroxide; clay minerals such as talc and mica; fillers with a ferrobskite-type crystal structure such as barium titanate and strontium titanate; and boron nitride, aluminum borate, barium sulfate, and calcium carbonate.
[0077] Organic fillers that can be used include fluoropolymer fillers such as polytetrafluoroethylene (PTFE), tetrafluoroethylene / ethylene copolymer (ETFE), tetrafluoroethylene / perfluoroalkyl vinyl ether copolymer (PFA), tetrafluoroethylene / hexafluoropropylene copolymer (FEP), polychlorotrifluoroethylene (PCTFE), polyvinylidene fluoride (PVDF), and polyvinyl fluoride (PVF); and hydrocarbon resin fillers such as cycloolefin polymer (COP) and cycloolefin copolymer (COC).
[0078] Inorganic fillers are preferred as fillers. From the viewpoint of further improving the heat resistance and mechanical properties of the cured product, silica is more preferred. The average particle size of silica is preferably 0.01 to 5 μm, more preferably 0.01 to 1 μm. Here, the average particle size can be determined as the median diameter (d50, volume basis) based on the cumulative distribution from the measured particle size distribution by the laser diffraction and scattering method using a commercially available laser diffraction and scattering particle size distribution analyzer. Furthermore, the average particle size of silica refers to the value measured in the above manner from the powder before the resin composition is prepared (pre-mixed, kneaded).
[0079] It is preferable that silica be incorporated in slurry form. Incorporating silica in slurry form makes it easier to achieve higher dispersion and suppress aggregation, thus making it easier to handle silica with an average particle size within the specified range. Furthermore, incorporating silica in slurry form makes it easier to maintain the accuracy (in units of 1 μm) of the resin layer's film thickness.
[0080] The filler is preferably a surface-treated filler (surface-treated filler). By surface-treating the filler, a cured product with higher elasticity and lower thermal expansion can be obtained without impairing resolution.
[0081] The filler content in the curable resin composition is preferably 30% by mass or more based on the total solids content, preferably 30 to 90% by mass, and more preferably 50 to 90% by mass. By setting the filler content within the above range, the elastic modulus of the cured product can be further improved, and the thermal expansion coefficient of the cured product can be further reduced.
[0082] 2-2-1-1-4. Organic solvents The organic solvent is not particularly limited, but examples include chloroform, methylene chloride, and toluene. Other solvents that may be used include N-methyl-2-pyrrolidone (NMP), tetrahydrofuran (THF), cyclohexanone, propylene glycol monomethyl ether acetate (PMA), diethylene glycol monoethyl ether acetate (CA), methyl ethyl ketone, ethyl acetate, and anisole. One organic solvent may be used, or two or more may be used.
[0083] 2-2-1-1-5. Other ingredients / additives Other components may include photocurable compounds and thermosetting compounds other than the alkali-soluble resins mentioned above. Additives may also include colorants, anti-settling agents, polymerization inhibitors, UV absorbers, silane coupling agents, plasticizers, flame retardants, antistatic agents, anti-aging agents, antioxidants, antibacterial and antifungal agents, defoamers, leveling agents, thickeners, adhesion promoters, thixotropic agents, photoinitiator aids, sensitizers, photobase generators, thermoplastic resins, elastomers, organic fillers, release agents, surface treatment agents, dispersants, dispersion aids, surface modifiers, stabilizers, phosphors, and the like. These can be used individually or in combination.
[0084] 2-2-2. Manufacturing Process In the manufacturing process, the curable resin composition prepared in the preparation process is applied to the first film P1 to form a curable resin composition layer, and then the organic solvent is evaporated and dried to produce a dry film D1 having the first film P1 and the curable resin layer 21.
[0085] In the preparation step, the curable resin composition, adjusted to an appropriate viscosity with an organic solvent, is applied to the first film P1 to a uniform thickness using a comma coater, blade coater, lip coater, rod coater, squeeze coater, reverse coater, transfer roll coater, gravure coater, spray coater, etc., in the manufacturing step. The applied curable resin composition forms a curable resin composition layer. Subsequently, the organic solvent contained in the curable resin composition layer is evaporated and dried, usually at a temperature of 50 to 130°C for 1 to 30 minutes, thereby converting the curable resin composition layer into a curable resin layer 21. Through this operation, a dry film D1 having the first film P1 and the curable resin layer 21 is obtained (see Figure 2).
[0086] In this embodiment, in the manufacturing process of the cured product 10 described later, at least the same number of dry films as the number of resin curing layers 11 to 14 of the cured product 10 are required. For example, in the cured product 10 of this embodiment, four layers of resin curing layers 11 to 14 are laminated. Therefore, it is preferable to produce at least four dry films. That is, it is preferable to produce at least four dry films D1 to D4, such as dry film D1 having the first film P1 and curable resin layer 21 (see Figure 2), dry film D2 having the first film P2 and curable resin layer 22, dry film D3 having the first film P3 and curable resin layer 23, and dry film D4 having the first film P4 and curable resin layer 24. Since dry films D2 to D4 have the same configuration and manufacturing method as dry film D1, they are not shown or described.
[0087] 3. Method for manufacturing cured products The cured product 10 of this embodiment is manufactured by sequentially laminating curable resin layers onto a substrate to form a curable resin laminate, and then curing the curable resin laminate. The manufacturing method of the cured product 10 of this embodiment includes a lamination step of laminating curable resin layers onto a substrate using the dry film described above to obtain a curable resin laminate; and a curing step of curing the curable resin laminate to obtain the cured product 10. Each step will be described below.
[0088] 3-1.Lamination process Figures 3(a) to 3(c) are cross-sectional views showing the manufacturing process (lamination process) of the curable resin laminate 20 according to this embodiment. The lamination process involves laminating curable resin layers 21 to 24 onto a substrate Q using the dry films D1 to D4 described above to obtain the curable resin laminate 20. The lamination process includes a bonding step and a lamination step, which will be described later. Each step will be explained below with reference to Figure 3.
[0089] 3-1-1. Bonding Step Figure 3(a) is a cross-sectional view of the process after the dry film D1 described above has been laminated onto the substrate Q. As shown in Figure 3(a), in the lamination step, the dry film D1 is laminated onto the substrate Q by lamination so that the curable resin layer 21 and the substrate Q face each other.
[0090] Specifically, first, the second film is peeled off from the dry film D1, which is laminated in the order of the first film P1, the curable resin layer 21, and the second film (not shown). Then, with the curable resin layer 21 and the substrate Q facing each other, the dry film D1 is bonded onto the substrate Q using a vacuum laminator at a temperature of 80-110°C and a pressure of 0.5 MPa {see Figure 3(a)}.
[0091] The substrate Q is not particularly limited and can be any printed circuit board or flexible printed circuit board with circuits pre-formed using copper or the like, or any material such as copper-clad laminates for high-frequency circuits using paper phenol, paper epoxy, glass cloth epoxy, glass polyimide, glass cloth / nonwoven epoxy, glass cloth / paper epoxy, synthetic fiber epoxy, fluororesin / polyethylene / polyphenylene ether, polyphenylene oxide / cyanate, etc., including copper-clad laminates of all grades (FR-4, etc.), as well as metal substrates, polyimide films, PET films, polyethylene naphthalate (PEN) films, glass substrates, ceramic substrates, wafers, etc. The substrate Q may be one that has undergone known pretreatment, such as chemical polishing. Examples of such pretreatments include etching (e.g., etching with organic acids; 1 μm etching), discoloration prevention treatment, water washing treatment, and drying treatment. From the viewpoint of adhesion with the cured product, it is preferable to use a substrate Q that has undergone pretreatment, and among these, it is more preferable to use one that has undergone chemical polishing treatment.
[0092] 3-1-2. Lamination Step In the lamination step, the first film P1 is peeled off from the dry film D1 that was bonded to the substrate Q in the bonding step, and another dry film D2 is used to laminate a curable resin layer 22 onto the side of the curable resin layer 21 opposite to the substrate Q. The curable resin layers 23 and 24 are laminated in the same manner to obtain a curable resin laminate 20.
[0093] Specifically, the first film P1 is peeled off from the dry film D1 (see Figure 3(a)) having a curable resin layer 21 that was bonded to the substrate Q in the bonding step. Meanwhile, the second film is peeled off from the dry film D2, in which the first film P2, the curable resin layer 22, and the second film (not shown) are laminated in this order. The dry film D2 having the curable resin layer 22 is bonded to the dry film D2 having the curable resin layer 22 using a laminator or the like so that the curable resin layer 21 and the curable resin layer 22 face each other. Through this operation, the curable resin layer 22 is laminated on the side of the curable resin layer 21 opposite to the substrate Q (see Figure 3(b)). The same operation as described above for the curable resin layer 22 is repeated for the curable resin layers 23 and 24, and they are sequentially laminated by lamination to produce a curable resin laminate 20 (see Figure 3(c)).
[0094] Figure 3(c) is a schematic cross-sectional view of the curable resin laminate 20 obtained by laminating the curable resin layers 21-24 of this embodiment onto a substrate Q, that is, the curable resin laminate 20 at the stage when the lamination process is completed. As shown in Figure 3(c), at the end of the lamination step, the curable resin layer 24, which is laminated by bonding the dry film D4, is positioned at the position furthest from the substrate Q of the curable resin laminate 20 (outermost layer). In the state of the curable resin laminate 20 after the lamination step is completed, the first film P4 has not been peeled off from the dry film D4 having the curable resin layer 24 laminated as the outermost layer, and the first film P4 is attached to the curable resin laminate 20 (curable resin layer 24). In this state, the exposure step (irradiation with active energy rays included in the curing process), which will be described later, is performed. The first film P4 is peeled off after the exposure step is completed.
[0095] The lamination step is preferably performed under at least the following different conditions, namely, a first lamination condition and a second lamination condition.
[0096] 3-1-2-1. First Lamination Conditions In the first lamination condition, it is preferable to use a vacuum laminator and perform vacuum lamination under pressure and heat. The preferred pressure conditions are 0.1 to 1.0 MPa, the preferred heating conditions are 40 to 80°C, and the preferred lamination time is 20 to 40 seconds.
[0097] By performing vacuum lamination, when a circuit-formed substrate is used as the base material, even if the surface of the circuit board has irregularities, the dry film adheres closely to the circuit board, preventing the inclusion of air bubbles and further improving the ability to fill in depressions on the substrate surface.
[0098] 3-1-2-2. Second Lamination Conditions Under the second lamination condition, it is preferable to perform lamination under the following pressure and heating conditions. The pressure conditions are 5-10 kgf / cm². 2 The heating conditions are preferably 40-100°C, and the lamination time is preferably 50-70 seconds.
[0099] By using the above heating conditions in both the first and second lamination conditions, the curable resin composition can maintain a higher viscosity. As a result, the flow of fillers and resins in each curable resin layer 21-24 is further suppressed, and the curable resin laminate 20 can be formed on the substrate Q while maintaining the filler distribution and layer structure.
[0100] As described above, in this embodiment, the curable resin layers 21 to 24 are laminated by laminating the dry films D1 to D4, making it easier to maintain the layer structure. Furthermore, since the flow of fillers within the curable resin layers is relatively suppressed, the filler distribution can be cured in a state where it changes stepwise in the lamination direction. As a result, the filler distribution is made uniform throughout the cured product 10, and the resolution can be further improved.
[0101] In contrast, conventional methods such as screen printing, which involve applying the coating in multiple layers, are prone to over-drying, making it difficult to maintain the layer structure. Furthermore, even when fillers are included, they tend to settle within the layers, resulting in an uneven distribution of fillers, making it impossible to achieve a uniform filler distribution throughout the cured product.
[0102] 3-2.Curing process In the curing step, the curable resin laminate 20 produced in the lamination step is cured to obtain a cured product 10. The curing step includes the exposure step, development step, and finishing step, which will be described later. Each step will be described below.
[0103] 3-2-1. Exposure Step In the exposure step, the curable resin laminate 20 produced in the lamination process is irradiated (exposed) with active energy rays.
[0104] Specifically, after creating a curable resin laminate 20 in the lamination process, the entire curable resin laminate 20 is selectively irradiated (exposed) with active energy rays through a photomask with a predetermined pattern. At this time, it is preferable to expose each curable resin layer 21 to 24 contained in the curable resin laminate 20 simultaneously (single exposure). After exposure, it is preferable to leave it at room temperature for 10 to 180 minutes. After that, the first film P4 attached to the curable resin layer 24, which is the outermost layer of the curable resin laminate 20, is peeled off.
[0105] By exposing the entire curable resin laminate 20 in a single exposure, and simultaneously exposing each curable resin layer 21-24 contained in the curable resin laminate 20, pattern development can be formed in a shorter time than when each layer is exposed individually. Furthermore, finer patterning becomes possible compared to when each curable resin layer 21-24 is exposed after being laminated.
[0106] The exposure machine used for active energy ray irradiation can be any device equipped with a high-pressure mercury lamp, ultra-high-pressure mercury lamp, metal halide lamp, mercury short-arc lamp, etc., that irradiates active energy rays in the range of 350 to 450 nm. Furthermore, a direct imaging device (for example, a laser direct imaging device that directly draws images with a laser using CAD data from a computer) can also be used. The lamp light source or laser light source of the direct imaging device can have a maximum wavelength in the range of 350 to 450 nm. The exposure amount for image formation varies depending on the film thickness, etc., but is generally 10 to 1000 mJ / cm². 2 Preferably 20-800 mJ / cm² 2 It can be within the range of
[0107] 3-2-2. Development Step In the developing step, the unexposed areas are developed with an alkaline aqueous solution.
[0108] Specifically, the unexposed portion of the curable resin laminate 20 from which the first film P4 has been peeled off in the exposure step described above is developed (for example, for 60 to 90 seconds) with a dilute alkaline aqueous solution (for example, 0.3 to 3% by mass sodium carbonate aqueous solution or potassium carbonate aqueous solution) to form a pattern on the curable resin laminate 20. After pattern formation, it may be washed with a washing solution.
[0109] Developing with an alkaline aqueous solution can be done using methods such as dipping, showering, spraying, or brushing. Suitable developers include alkaline aqueous solutions of potassium hydroxide, sodium hydroxide, sodium carbonate, potassium carbonate, sodium phosphate, sodium silicate, ammonia, and amines. These can also be mixed.
[0110] 3-2-3. Finishing Steps In the finishing step, the curable resin laminate 20, which has a pattern formed in the development step described above, is irradiated with active energy rays and then heat-cured (for example, at 100-220°C). In the finishing step, the curable resin laminate 20 is completely cured, forming the cured product 10. [Examples]
[0111] The present invention will be described below with reference to examples and comparative examples, but the present invention is not limited to the following.
[0112] (Synthesis of alkali-soluble resin solution) In an autoclave equipped with a thermometer, a nitrogen introduction device / alkylene oxide introduction device, and a stirring device, 119.4 parts by mass of novolac-type cresol resin (Showa Denko Corporation, Schoenol CRG951, OH equivalent: 119.4), 1.19 parts by mass of potassium hydroxide, and 119.4 parts of toluene were introduced. The system was then heated and the temperature increased while stirring and purging with nitrogen. Next, 63.8 parts of propylene oxide were gradually added dropwise to 125-132°C and 0-4.8 kg / cm³. 2The mixture was reacted for 16 hours. After cooling to room temperature, 1.56 parts of 89% phosphoric acid were added to the reaction solution and mixed to neutralize the potassium hydroxide, yielding a propylene oxide reaction solution of novolac-type cresol resin with a non-volatile content of 62.1% and a hydroxyl value of 182.2 mg KOH / g (307.9 g / eq.). This solution had an average of 1.08 moles of propylene oxide added per equivalent of phenolic hydroxyl groups. 293.0 parts of the obtained propylene oxide reaction solution of novolac-type cresol resin, 43.2 parts of acrylic acid, 11.53 parts of methanesulfonic acid, 0.18 parts of methylhydroquinone, and 252.9 parts of toluene were introduced into a reactor equipped with a stirrer, thermometer, and air blowing tube, and the mixture was reacted at 110°C for 12 hours while blowing air at a rate of 10 ml / min and stirring. The water produced by the reaction was distilled off as an azeotropic mixture with toluene, with 12.6 parts of water being removed. The mixture was then cooled to room temperature, neutralized with 35.35 parts of 15% aqueous sodium hydroxide solution, and then washed with water. Toluene was then removed by distillation in an evaporator while substituting with 118.1 parts of diethylene glycol monoethyl ether acetate to obtain a novolac-type acrylate resin solution. Next, 332.5 parts of the obtained novolac-type acrylate resin solution and 1.22 parts of triphenylphosphine were introduced into a reactor equipped with a stirrer, thermometer, and air blowing tube. Air was blown in at a rate of 10 ml / min, and while stirring, 60.8 parts of tetrahydrophthalic anhydride were gradually added, and the mixture was reacted at 95-101°C for 6 hours. After cooling, the mixture was removed. In this way, a carboxyl group-containing alkali-soluble resin solution with a non-volatile content of 65% and a solid acid value of 87.7 mgKOH / g was obtained.
[0113] (Preparation of surface-treated filler (methacrylate silane-treated silica)) A silica solvent dispersion was obtained by uniformly dispersing 70 g of spherical silica (SFP-30M, manufactured by Denka Co., Ltd.), 28 g of PMA (propylene glycol monomethyl ether acetate) as a solvent, and 2 g of KBM-503, manufactured by Shin-Etsu Chemical Co., Ltd., as a silane coupling agent.
[0114] <Preparation of curable resin composition> Each component was mixed according to the formulations shown in the examples A to C in Table 1 below, and pre-mixed using a stirrer. Then, the mixture was dispersed in a bead mill and kneaded to prepare the curable resin compositions of formulations A to C.
[0115] [Table 1]
[0116] The amounts in Table 1 are shown in parts by mass. The details of each component in Table 1 are as follows: *1: Alkali-soluble resin solution having ethylenically unsaturated groups synthesized as described above. *2: Irgacure TPO (2,4,6-trimethylbenzoyl-diphenyl-phosphine oxide) manufactured by BASF Japan *3: JMT784 (titanocene photopolymerization initiator) manufactured by Yueyang Jin Maotai Technology Co., Ltd. *4: Epiclon N-730A (phenol novolac type epoxy resin) manufactured by DIC Corporation *5: Epiclon N-870 (Bisphenol A novolac type epoxy resin) manufactured by DIC Corporation *6: Solvent dispersion of silica surface-treated with methacrylate silane, prepared as described above. *7: Benton 38 manufactured by Toshin Kasei Co., Ltd. *8: EASTMAN CAP-504-0.2DPM30 *9: Melamine manufactured by Nissan Chemical Industries, Ltd. *10: Kayacure DETX-S (2,4-diethylthioxanthone) manufactured by Nippon Kayaku Co., Ltd. *11: Blue pigment and yellow pigment
[0117] [Examples 1-9, Comparative Examples 1-7] <Fabrication of evaluation board> Evaluation substrates for each example and comparative example were prepared according to the following procedure, so as to have the layer structure and thickness of each layer shown in Tables 2 and 3.
[0118] The above curable resin composition was applied to a polyethylene terephthalate film (hereinafter also referred to as PET film) (manufactured by Toyobo Co., Ltd., E5041) (first film) measuring 300 mm x 130 mm and 25 μm thick, so that the film thickness after drying was as shown in Table 2. The film was then heated and dried to form the first curable resin layer. Next, a polypropylene film (manufactured by Oji F-Tex Co., Ltd., MA411) (second film) measuring 300 mm x 100 mm and 15 μm thick was laminated onto the curable resin layer to form a dry film. The same procedure was repeated to produce dry films having each of the subsequent curable resin layers, in the number of layers required for lamination.
[0119] A double-sided printed circuit board measuring 150 mm x 95 mm with a thickness of 0.4 mm was used as the substrate, and chemical polishing equivalent to 1.0 μm was performed using MEC Etchbond CZ-8100 manufactured by MEC Corporation. A dry film having the first curable resin layer was cut to 150 mm x 90 mm, and after peeling off the polypropylene film (second film), the dry film was laminated to the substrate after the above pretreatment using a two-chamber vacuum laminator CVP-600 (manufactured by Nikko Materials Co., Ltd.) under the following conditions, so that the curable resin layer and the substrate faced each other. Laminating temperature: 80℃ Vacuuming: 30 seconds, 3 hPa Lamination: 30 seconds, 0.5 MPa
[0120] From the first layer of dry film laminated onto the substrate, the first film was peeled off to expose the curable resin layer. A dry film with a second curable resin layer was then cut to 150 mm x 90 mm, and after peeling off the second film, the second curable resin layer was laminated so that it faced the first curable resin layer. Similarly, subsequent curable resin layers were sequentially laminated to create a curable resin laminate on the substrate. The outermost PET film of the created curable resin laminate was not peeled off, and the PET film remained attached (curable resin laminate with PET film). The lamination of the second and subsequent curable resin layers was performed under the following two different conditions.
[0121] (First lamination condition) Laminating temperature: 80℃ Vacuuming: 30 seconds, 3 hPa Lamination: 30 seconds, 0.5 MPa
[0122] (Second lamination conditions) Laminating temperature: 100℃ Press: 60 seconds, 8 kgf / cm 2
[0123] The curable resin laminate with PET film, obtained on the substrate, was subjected to a single exposure using a DI exposure apparatus (Mms60, manufactured by Oak Manufacturing Co., Ltd.) through a photomask with aperture patterns of Φ80 μm and Φ100 μm (exposure dose: 300 mJ / cm²). 2 The PET film was then left at room temperature for 10 minutes before being peeled off. Development was then carried out using a 1% by mass Na2CO3 aqueous solution at 30°C and a spray pressure of 0.2 MPa for 90 seconds to form a curable resin laminate having opening patterns of Φ80 μm and Φ100 μm. The curable resin laminate was washed with a washing solution at 25°C and a spray pressure of 0.1 MPa for 90 seconds, and after exposure (exposure amount: 1000 mJ / cm²), 2 The material was heated at 170°C for 60 minutes to allow it to fully cure. An evaluation substrate was prepared with the cured material formed on the substrate. The properties of the obtained evaluation substrate were evaluated as follows. The results are shown in Tables 2 and 3.
[0124] <Exterior Evaluation> Pinholes and unevenness were visually observed on the evaluation substrates of each example and comparative example. The evaluation of each item was carried out according to the following criteria.
[0125] (Pinhole) ○: No pinholes ×: Pinhole present
[0126] (mura) ○: No coating streaks ×: Painting streaks present
[0127] <Preparation of samples for opacity evaluation> In the above-described "Preparation of evaluation substrates," the same procedure was followed as described above, except that a substrate measuring 150 mm x 95 mm with a thickness of 0.4 mm on both sides was used as the base material, with scratches 5 μm deep and 10 mm long made on the circuit surface using a utility knife. Samples for opacity evaluation of each example and comparative example were prepared using this method. The opacity of the samples used for opacity evaluation in each example and comparative example was observed visually and evaluated according to the following criteria.
[0128] (Concealing ability) ◎: No scratches ○: Slightly damaged ×: Damaged
[0129] (Measurement of linear thermal expansion coefficient (CTE)) The cured material was peeled off the evaluation substrates of each example and comparative example, and samples were cut out to obtain a measurement size (3 mm x 10 mm) to be used as measurement samples. The CTE of each measurement sample was measured using a Hitachi High-Tec TMA6100. The measurement conditions were a test load of 5 g, and the sample was heated from room temperature in tensile mode at a heating rate of 10°C / min, repeating this process twice. The average linear thermal expansion coefficient (α2) calculated in the range of 200°C to 250°C during the second measurement was determined.
[0130] (resolution) In the evaluation substrates of each example and comparative example, the diameter of the opening end (Top) at φ80 μm and φ100 μm was measured using a SEM (JEOL Ltd., JSM6610LV) at a measurement magnification of 1,000x, and the rate of change T from the design value was calculated using the following formula. The rate of change for a diameter of φ80μm is T = 100 - diameter / 80 × 100 φ100μm change rate T=100-diameter / 100×100
[0131] In the evaluation substrates of each example and comparative example, the diameter of the bottom of the opening at φ80 μm and φ100 μm was measured using a SEM (JEOL Ltd., JSM6610LV) at a magnification of 1,000x, and the rate of change B relative to the design value was calculated using the following formula. The rate of change for a diameter of φ80μm is B = 100 - diameter / 80 × 100 The rate of change for a diameter of φ100μm is B = 100 - diameter / 100 × 100
[0132] [Table 2]
[0133] [Table 3]
[0134] Comparative Examples 1 and 2, being thin films, exhibited excellent resolution, but pinholes occurred. Comparative Examples 3-7, being thicker films than Comparative Examples 1 and 2, suppressed the occurrence of pinholes, but unevenness occurred, resulting in reduced resolution.
[0135] On the other hand, in Example 1, although the thickness was similar to that of Comparative Example 2, not only was the resolution superior, but the occurrence of pinholes was also suppressed. Furthermore, the linear thermal expansion coefficient results were satisfactory, indicating that a low thermal expansion coefficient could be achieved. In addition, in Example 2-9, which was thicker than Example 1, the occurrence of unevenness was suppressed, and the resolution was also superior. Furthermore, although the thickness was similar to that of Comparative Example 3-7, the linear thermal expansion coefficient was reduced, and the thermal expansion coefficient was further reduced. From the above, it was shown that the manufacturing method according to each example makes it easy to suppress the occurrence of pinholes and unevenness, and to obtain a cured product that has good resolution even when thickened. [Industrial applicability]
[0136] This invention provides a cured product that has excellent appearance and excellent resolution even when thickened, and can therefore be used in miniaturized, high-performance electronic devices and the like. [Explanation of Symbols]
[0137] 10 Cured product 20 Curable resin laminate P1 First Film P4 First Film D1 Dry Film D4 Dry Film Q Base material
Claims
1. A cured product having two or more resin curing layers laminated together, The filler content in each resin cured layer is 30% by mass or more based on the total solid content. Each of the aforementioned resin cured layers has a high-filler content surface area, which is a surface area with a relatively high filler content, and a low-filler content surface area, which is a surface area with a relatively low filler content. A cured product in which a pair of adjacent resin cured layers are laminated, with the filler-high content surface of one resin cured layer and the filler-low content surface of the other resin cured layer.
2. The cured product according to claim 1, wherein the filler content in each of the aforementioned resin cured layers is 50 to 90% by mass on a basis of total solid content.
3. The cured product according to claim 2, wherein the filler is silica.
4. The cured product according to claim 1, wherein the resin curing layer is laminated in two to seven layers, the thickness of each resin curing layer is 3 μm to 25 μm, and the thickness of the cured product is 15 μm to 65 μm.
5. The filler is silica, The silica content in each of the aforementioned resin cured layers is 50 to 90% by mass on a basis of total solid content. The cured product according to claim 1, wherein the resin curing layer is laminated in two to seven layers, the thickness of each resin curing layer is 3 μm to 25 μm, and the thickness of the cured product is 15 μm to 65 μm.
6. After the curable resin layers are stacked, vacuum lamination is performed using a vacuum laminator under the first lamination conditions of a pressure of 0.1 to 1.0 MPa, a heating condition of 40 to 80°C, and a lamination time of 20 to 40 seconds. Subsequently, a pressure of 5 to 10 kgf / cm² is applied. 2 The cured product according to claim 1, which is laminated by laminating under second lamination conditions of heating conditions of 40 to 100°C and lamination time of 50 to 70 seconds.
Citation Information
Patent Citations
Method for forming pattern
JP2004157422A
White coating film layer, method of forming the same, and printed circuit board
JP2015005784A