electrode
The electrode with a PTC polymer layer addresses the risk of short circuits in secondary batteries by maintaining stability under normal conditions and preventing hazards through increased resistance in abnormal states.
Patent Information
- Application Number
- JP2026199531
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2022-10-19
- Filing Date
- 2026-09-02
- Publication Date
- 2026-11-19
AI Technical Summary
Secondary batteries are prone to fire or explosion due to short circuits caused by direct contact between positive and negative electrodes, which can occur during overcharging, high-temperature exposure, or external impact, leading to internal heat generation and gas formation.
An electrode design incorporating a polymer layer that exhibits a positive temperature coefficient (PTC) effect and controlled oxidation potential, ensuring stable performance under normal conditions while increasing resistance in abnormal states to prevent short circuits.
The electrode maintains stable electrical characteristics under normal conditions and ensures safety by preventing short circuits and potential hazards under abnormal conditions, such as overcharging or external impacts.
Smart Images

Figure 2026182977000001_ABST
Abstract
Description
[Technical Field]
[0001] This application claims priority based on Republic of Korea Patent Application No. 10-2022-0135150 dated October 19, 2022, and all contents of the literature of said patent application are included as part of this specification.
[0002] This specification discloses electrodes and their applications. [Background technology]
[0003] Energy storage technology is seeing expanding applications to include mobile phones, tablets, laptops, and electric vehicles.
[0004] As the data processing speed of mobile devices such as cell phones and tablets increases and their usage time lengthens, the development of secondary batteries with high energy density and operating potential, long cycle life, and low self-discharge rates is progressing.
[0005] Furthermore, as major developed countries reduce the production of internal combustion engine-driven vehicles to combat global warming and air pollution, major automakers are also developing a variety of electric vehicles, and the importance of secondary batteries with high energy density, high discharge voltage, and output stability as their power source is increasing.
[0006] However, in line with the aforementioned trend, the frequency of fire or explosion accidents in devices and automobiles that use secondary batteries as an energy source, caused by overcharging, high-temperature exposure, or external impact, is also increasing.
[0007] The main cause of such accidents is known to be a short circuit, which occurs when the positive and negative electrodes inside the electrode assembly come into direct contact due to external stimuli. When a secondary battery is overcharged, exposed to high temperatures or external stimuli, the aforementioned short circuit can occur due to the contraction of the separator membrane caused by the rise in the internal temperature of the secondary battery, or damage to the internal structure of the secondary battery due to external impact.
[0008] When a short circuit phenomenon occurs, the movement of lithium ions and electrons concentrates through the site where the positive electrode and the negative electrode are in direct contact, which can promote internal heat generation. It is known that this generates gas and the like inside the battery, causes the volume to expand, and increases the risk of ignition. Summary of the Invention Problems to be Solved by the Invention
[0009] The present specification discloses an electrode and uses thereof. An object of the present specification is to disclose an electrode including a polymer layer that exhibits a positive temperature coefficient (PTC) effect and an oxidation potential controlled to meet the intended purpose. Such an electrode exhibits excellent electrical characteristics such as low resistance in a normal state, does not affect or even improves the performance and operation of a secondary battery, and can ensure stability in an abnormal state. Another object of the present specification is to disclose uses of the electrode. Means for Solving the Problems
[0010] As used herein, the term "normal temperature" refers to the natural unmodified temperature that is not heated or cooled, and may be, for example, any temperature within the range of 10°C to 30°C, or a temperature of about 23°C or about 25°C.
[0011] Among the physical properties referred to in the present specification, when the measurement temperature affects the physical property, the physical property is the physical property measured at normal temperature, unless otherwise specifically specified.
[0012] Unless otherwise specifically specified, the unit of temperature in the present specification is degree Celsius (°C).
[0013] As used herein, the term "normal pressure" refers to the natural unmodified pressure that is not pressurized or depressurized, and may generally mean a pressure of about 730 mmHg to 790 mmHg. Among the physical properties referred to in the present specification, when the measurement pressure affects the physical property, the physical property is the physical property measured at normal pressure, unless otherwise specifically specified.
[0014] In this specification, if the measured humidity affects the results of any physical property mentioned herein, unless otherwise specified, the physical property shall be measured at standard humidity conditions.
[0015] Standard humidity refers to a relative humidity within the range of 40% to 60%, for example, a relative humidity of around 55% or 60%.
[0016] In this specification, the term "normal state" means the normal operating state (e.g., the normal charging or discharging state of the secondary battery) or storage state of the secondary battery.
[0017] In this specification, the term "abnormal condition" means a hazardous condition in which an abnormal flow of electric charge, abnormal heat generation or explosion occurs due to an external shock and / or short circuit, or in which the likelihood of such an abnormal condition occurring is increased.
[0018] This specification discloses electrodes.
[0019] The electrode may include a current collector, an active material layer formed on the current collector, and a polymer layer formed between the current collector and the active material layer. Figure 1 is a cross-sectional view of an exemplary electrode that sequentially includes the current collector 100, the polymer layer 200, and the active material layer 300. As shown in the drawing, the current collector 100, the polymer layer 200, and the active material layer 300 may be in contact with each other. If necessary, other elements may be present between the current collector 100 and the polymer layer 200 and / or between the polymer layer 200 and the active material layer 300. Although the drawing shows a case where the active material layer 300 is present on only one side of the current collector 100, the active material layer 300 may be present on both sides of the current collector 100. In such a case, the polymer layer 200 may be present in two layers between each of the active material layers 300 present on both sides of the current collector 100 and the current collector 100, or it may be present in one layer between any one of the active material layers 300 present on both sides and the current collector 100.
[0020] The electrode may be, for example, a negative electrode (anode) or a positive electrode (cathode) applied to a secondary battery.
[0021] The polymer layer contained in the electrode is a layer containing a polymer. Such a polymer may be a conductive polymer, as described later.
[0022] In the electrode, the polymer layer is provided to exhibit a controlled PTC (Positive Temperature Coefficient) effect. As is well known, the PTC effect is the effect in which resistance increases with temperature. The polymer layer is provided so that the PTC effect is exhibited at the abnormal temperature. Therefore, the electrode exhibits stable performance under normal conditions due to the excellent electrical properties of the polymer layer, and stability can be ensured under abnormal conditions through the increase in resistance of the polymer layer.
[0023] The polymer layer at the electrode can exhibit an oxidation potential adjusted in relation to the active material layer.
[0024] For example, in the electrode, the polymer layer or the conductive polymer contained therein can have a low oxidation potential relative to the electrode active material or the active material layer. Through such adjustments, stable performance can be maintained even when repeated charging and discharging, or fast charging and / or fast discharging, is performed on the secondary battery to which the electrode is applied.
[0025] The oxidation potential of the conductive polymer or polymer layer is the oxidation potential for lithium, and the oxidation potential for lithium and lithium ions (Li / Li + It is a standard and can be measured using the method described in "4. Method for Measuring Oxidation Potential (Conductive Polymer / Polymer Layer)" of the Examples section of this specification.
[0026] The oxidation potential of the electrode active material or active material layer is the oxidation potential for lithium, and the oxidation potential for lithium and lithium ions (Li / Li +It is a standard and can be measured by the method described in "5. Method for Measuring Oxidation Potential (Electrode Active Material)" of the Examples section of this specification.
[0027] For example, the electrode may be designed such that the RV in the following Equation 1 falls within a predetermined range.
[0028] [Formula 1] RV = 100 × Va / Vs
[0029] In Equation 1, Va is the oxidation potential of the electrode active material or the active material layer, and Vs is the oxidation potential of the conductive polymer or the polymer layer.
[0030] The lower limit of RV in Equation 1 may be approximately 100, 100.5, 101, 101.5, 102, or 102.5, and its upper limit may be approximately 200, 195, 190, 185, 180, 175, 170, 165, 160, 155, 150, 145, 140, 135, 130, 125, 120, 115, 110, 109, 108, 107, 106, 105, 104, or 103. The RV may be within a range that is greater than or greater than any of the lower limits mentioned above; or it may be less than or equal to any of the upper limits mentioned above, while being greater than or greater than any of the lower limits mentioned above.
[0031] In Equation 1, the oxidation potential Va is determined by the type of electrode active material and is not particularly limited. For example, the lower limit of the oxidation potential Va may be around 2.0V, 2.1V, 2.2V, 2.3V, 2.4V, 2.5V, 2.6V, 2.7V, 2.8V, 2.9V, 3V, 3.1V, 3.2V, 3.3V, 3.4V, 3.5V, 3.6V, 3.7V, 3.8V, 3.9V, or 4.0V, and its upper limit may be 5V, 4.9V, 4.8V, 4. The oxidation potential Va may be approximately 7V, 4.6V, 4.5V, 4.4V, 4.3V, 4.2V, 4.1V, 4.0V, 3.9V, 3.8V, 3.7V, 3.6V, 3.5V, 3.4V, 3.3V, 3.2V, 3.1V, 3.0V, 2.9V, 2.8V, 2.7V, 2.6V, 2.5V, 2.4V, 2.3V, 2.2V, 2.1V, or 2.0V. The oxidation potential Va may be within a range that is above or above any of the lower limits mentioned above; or within a range that is below or below any of the upper limits mentioned above; or within a range that is below or below any of the upper limits mentioned above, while being above or above any of the lower limits mentioned above.
[0032] The Vs in Equation 1 is not particularly limited as long as it is controlled so that the range of RV is satisfied depending on the oxidation potential of the applied electrode active material or active material layer. For example, the lower limit of the oxidation potential Vs is 0V, 0.1V, 0.2V, 0.3V, 0.4V, 0.5V, 0.6V, 0.7V, 0.8V, 0.9V, 1.0V, 1.1V, 1.2V, 1.3V, 1.4V, 1.5V, 1.6V, 1.7V, 1.8V, 1.9V, 2.0V, 2.1V, 2.2V, 2.3V, 2.4V, 2.5V, 2.6V, 2.7V, 2.8V, 2.9V, 3V, 3.1V, 3.2V, 3.3V, 3.4V, 3.5V, 3.6V, It may be around 3.7V, 3.8V, 3.9V, or 4.0V, and its upper limit may be around 5V, 4.9V, 4.8V, 4.7V, 4.6V, 4.5V, 4.4V, 4.3V, 4.2V, 4.1V, 4.0V, 3.9V, 3.8V, 3.7V, 3.6V, 3.5V, 3.4V, 3.3V, 3.2V, 3.1V, 3.0V, 2.9V, 2.8V, 2.7V, 2.6V, 2.5V, 2.4V, 2.3V, 2.2V, 2.1V, or 2.0V. The oxidation potential Vs may be within a range that is greater than or greater than any of the lower limits mentioned above; or within a range that is less than or equal to any of the upper limits mentioned above; or within a range that is less than or equal to any of the upper limits mentioned above, but greater than or equal to any of the lower limits mentioned above.
[0033] The upper limits of the DC resistance of the polymer layer at 25°C for the electrodes are 10,000 Ω·cm, 9,500 Ω·cm, 9,000 Ω·cm, 8,500 Ω·cm, 8,000 Ω·cm, 7,500 Ω·cm, 7,000 Ω·cm, 6,500 Ω·cm, 6,000 Ω·cm, 5,500 Ω·cm, 5,000 Ω·cm, 4,500 Ω·cm, 4,000 Ω·cm, 3,500 Ω·cm, 3,000 Ω·cm, 2,500 Ω·cm, 2,000 Ω·cm, 1,500 Ω·cm, 1,000 Ω·cm, and 950 Ω·cm. The DC resistance may be approximately 900Ω·cm, 850Ω·cm, 800Ω·cm, 750Ω·cm, 700Ω·cm, 650Ω·cm, 600Ω·cm, 550Ω·cm, 500Ω·cm, 450Ω·cm, 400Ω·cm, or 350Ω·cm, with its lower limit being approximately 10Ω·cm, 50Ω·cm, 100Ω·cm, 150Ω·cm, 200Ω·cm, 250Ω·cm, 300Ω·cm, 350Ω·cm, 400Ω·cm, 450Ω·cm, 500Ω·cm, 550Ω·cm, or 600Ω·cm. The DC resistance may be within or below any of the upper limits mentioned above; or it may be within or below any of the upper limits mentioned above, while being above or above any of the lower limits mentioned above. The DC resistance was measured using the method described in "6. Method for Measuring DC Resistance" of the Examples in this Specification.
[0034] The upper limit of the AC impedance resistance of the polymer layer in the electrode may be approximately 1,000Ω, 950Ω, 900Ω, 850Ω, 800Ω, 750Ω, 700Ω, 650Ω, 600Ω, 550Ω, 500Ω, 450Ω, 400Ω, 350Ω, 300Ω, 250Ω, 200Ω, 150Ω, 100Ω, 95Ω, 90Ω, 85Ω, 80Ω, 75Ω, 70Ω, 65Ω, 60Ω, 55Ω, or 50Ω, and the lower limit may be approximately 10Ω, 15Ω, 20Ω, 25Ω, 30Ω, 35Ω, 40Ω, 45Ω, 50Ω, 55Ω, 60Ω, 65Ω, 70Ω, 75Ω, 80Ω, or 85Ω. The AC impedance resistance may be within a range of any upper limit or less than any of the upper limits described above; or it may be within a range of any lower limit or greater than any of the lower limits described above, while being below or less than any of the upper limits described above. The AC impedance resistance is measured by the method described in "7. Interface Resistance (AC Impedance Resistance)" of the Examples of this Specification.
[0035] Because the polymer layer exhibits the DC resistance and / or AC impedance resistance, the electrode or the secondary battery or electrode assembly to which the electrode is applied can operate or be stored stably under normal conditions.
[0036] The polymer layer can exhibit a PTC effect designed to suit the purpose.
[0037] For example, the polymer layer can exhibit properties such that △R1 in the following equation 2 is within a predetermined range.
[0038] [Formula 2] △R1=Max{(R n+5 / R n ) / 5}
[0039] In Equation 1, R n R is the DC resistance at any temperature n°C within the range of 25°C to 135°C. n+5 This is the DC resistance at a temperature 5°C higher than the aforementioned temperature n°C ((n+5)°C), and Max{(R n+5 / R n) / 5} was confirmed within the temperature range of 25°C to 135°C (R n+5 / R n ) / 5 is the maximum value among the values.
[0040] ΔR1 in Formula 2 is measured on a coin cell to which the polymer layer is applied, and the specific method thereof is described in "8. Maximum Resistance Change Rate Measurement (DC Resistance)" in the Examples. In the method for confirming the ΔR1, the initial temperature is 25°C and the final temperature is 135°C. While increasing the temperature by 5°C starting from the initial temperature of 25°C, the DC resistance is measured at each temperature to obtain the R n+5 and R n are confirmed. For example, when n is 90, R 95 / R 90 is the ratio of the DC resistance at 95°C to the DC resistance at 90°C. For example, that ΔR1 is 100Ω·cm / °C or more at any temperature within the temperature range of 25°C to 135°C means that the resistance of the polymer layer increases relatively sharply at any temperature within the aforementioned temperature range.
[0041] The lower limit of the ΔR1 may be about 40, 45, 50, 55, 60, 65, 70, 75, 80, 90, 100, 150, 200, 250, 300, 350 or 400, and the upper limit thereof may be about 1,000, 950, 900, 850, 800, 750, 700, 650, 600, 550, 500, 450, 400, 350, 300, 250, 200 or 150. The unit of the ΔR1 is Ω·cm / °C. The ΔR1 may be in a range that is equal to or greater than any one of the aforementioned lower limits; or may have a range that is equal to or less than any one of the aforementioned upper limits or less than any one of the aforementioned upper limits, while being equal to or greater than any one of the aforementioned lower limits or exceeding any one of the aforementioned lower limits. Through the aforementioned characteristics, the electrode can ensure the stability of secondary batteries and the like in an abnormal state.
[0042] The temperature at which the ΔR1 is confirmed, that is, R nThe lower limit of the temperature may be around 70°C, 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, or 95°C, and the upper limit may be around 200°C, 190°C, 180°C, 170°C, 160°C, 150°C, 140°C, 130°C, 120°C, 110°C, 100°C, or 90°C. The temperature may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or more than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, but within a range of any lower limit or more than any of the lower limits mentioned above. The temperature is adjusted to a temperature at which an abnormal condition occurs or is likely to occur. When a polymer layer exhibiting the aforementioned characteristics is applied, the electrode, electrode assembly, or secondary battery can maintain stable performance under abnormal conditions, while also maintaining stable performance under normal storage conditions at relatively high temperatures, and under high-temperature charging and discharging conditions.
[0043] The polymer can exhibit the characteristic that △R2 in the following formula 3 is within a predetermined range.
[0044] [Formula 3] △R² = Max{(R z+5 / R z ) / 5}
[0045] In equation 2, R z R is the AC impedance resistance at any temperature n°C within the range of 25°C to 135°C. z+5 This is the AC impedance resistance at a temperature 5°C higher than the aforementioned temperature n°C ((n+5)°C), and Max{(R z+5 / R z ) / 5} was confirmed within the temperature range of 25℃ to 135℃ (R z+5 / R z ) / 5 is the maximum value among them.
[0046] The ΔR2 in Equation 3 is measured for a coin cell to which the polymer layer is applied, and the specific method is described in "9. Measurement of Maximum Resistance Change Rate (AC Impedance)" of the Examples. In the method for confirming ΔR2, the initial temperature is 25°C and the final temperature is 135°C. The AC impedance resistance is measured at each temperature while increasing the temperature by 5°C at the initial temperature of 25°C, and the ΔR2 is determined. z+5 and R z Check this. For example, if n is 90, then R 95 / R 90 This is the ratio of the AC impedance resistance at 95°C to the AC impedance resistance at 90°C. For example, if ΔR2 is 10Ω / °C or higher at any temperature within the temperature range of 25°C to 135°C, it means that the resistance of the polymer layer increases relatively rapidly at any temperature within that temperature range.
[0047] The lower limit of ΔR2 may be approximately 8, 10, 12, 14, 16, 18, 20, 22, 24, 26, 28, 30, 33, 34, 36, 38, 40, 42, or 44, and its upper limit may be approximately 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 18, or 16. The unit of ΔR2 is Ω / ℃. ΔR2 may be less than or equal to any of the upper limits mentioned above, greater than or equal to any of the lower limits mentioned above, or less than or equal to any of the upper limits mentioned above while being greater than or equal to any of the lower limits mentioned above. Through these characteristics, electrodes to which the polymer layer is applied can ensure the stability of secondary batteries and the like under abnormal conditions.
[0048] The temperature at which ΔR2 in the aforementioned range is observed, i.e., R zThe lower limit of the temperature may be around 80°C, 81°C, 82°C, 83°C, 84°C, 85°C, 86°C, 87°C, 88°C, 89°C, 90°C, 91°C, 92°C, 93°C, 94°C, or 95°C, and the upper limit may be around 200°C, 190°C, 180°C, 170°C, 160°C, 150°C, 140°C, 130°C, 120°C, 110°C, 100°C, or 90°C. The temperature may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or more than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, while being above or more than any lower limit or more than any of the lower limits mentioned above. The temperature is adjusted to a temperature at which an abnormal condition occurs or is likely to occur. When a polymer layer exhibiting the aforementioned characteristics is applied, the electrode, electrode assembly, or secondary battery can maintain stable performance under abnormal conditions, while also maintaining stable performance under normal storage conditions at relatively high temperatures, and under high-temperature charging and discharging conditions.
[0049] The conductive polymer forming the polymer layer can be controlled so that the polymer layer exhibits the controlled oxidation potential and PTC effect as described above.
[0050] The conductive polymer contained in the polymer layer may be polythiophene or a thiophene polymer. In this specification, the terms "polythiophene" or "thiophene polymer" mean a polymer containing a certain level or more of thiophene units. The thiophene unit means a monomer unit formed by polymerization of monomers of the thiophene series, and the monomers of the thiophene series mean monomers containing a thiophene skeleton.
[0051] The aforementioned term "monomer unit" refers to a structure in which monomers are polymerized and contained within a polymer.
[0052] In the polythiophene or thiophene polymer, the lower limit of the ratio of thiophene units is approximately 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, 85 mol%, and 90 mol%, based on the total number of moles of monomer units in the polythiophene or thiophene polymer. The amount may be approximately % or 95 mol%, with upper limits being approximately 99 mol%, 97 mol%, 95 mol%, 93 mol%, 91 mol%, 89 mol%, 87 mol%, 85 mol%, 83 mol%, 81 mol%, 79 mol%, 77 mol%, 75 mol%, 73 mol%, 71 mol%, 69 mol%, 67 mol%, 65 mol%, 63 mol%, 61 mol%, 59 mol%, 57 mol%, 55 mol%, 53 mol%, or 51 mol%. The ratio of thiophene units may be within a range that is greater than or greater than any of the lower limits mentioned above; or it may be less than or less than any of the upper limits mentioned above, while being greater than or greater than any of the lower limits mentioned above.
[0053] The thiophene units included in the polythiophene may be thiophene units having hydrocarbon functional groups.
[0054] In this specification, the term "hydrocarbon functional group" means a monovalent hydrocarbon group (i.e., a monovalent functional group consisting of carbon and hydrogen) or a monovalent functional group containing such a monovalent hydrocarbon group. Therefore, the hydrocarbon functional group may contain other atoms in addition to carbon and hydrogen. Examples of the monovalent hydrocarbon group include alkyl groups, alkynyl groups, or alkenyl groups, and examples of monovalent functional groups containing such a monovalent hydrocarbon group include alkoxy groups, alkylcarbonyl groups, or alkylcarbonyloxy groups, but the types of hydrocarbon functional groups are not limited to these.
[0055] The lower limit of the number of carbon atoms in the hydrocarbon functional group may be approximately 3, 4, 5, 6, 7, 8, 9, 10, 11, or 12, and the upper limit may be approximately 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, 10, 9, 8, 7, 6, 5, 4, or 3. The number of carbon atoms may be within a range that is greater than or greater than any of the lower limits mentioned above; or within a range that is less than or equal to any of the upper limits mentioned above; or within a range that is less than or equal to any of the upper limits mentioned above, while being greater than or equal to any of the lower limits mentioned above.
[0056] The carbon number may be the total number of carbon atoms in the hydrocarbon functional group or the monovalent hydrocarbon group contained therein, or the number of carbon atoms in the longest linear hydrocarbon chain contained in the hydrocarbon functional group or the monovalent hydrocarbon group contained therein. That is, the hydrocarbon functional group or monovalent hydrocarbon group may have a linear or branched structure, but even in the case of a branched structure, the number of carbon atoms constituting the longest linear chain in that branched structure may be within the range described above. For example, if the branched structure is a 2-ethylhexyl group, the number of carbon atoms constituting the longest chain is 6.
[0057] The hydrocarbon functional group, which is an alkyl group, alkenyl group, alkynyl group, alkoxy group, alkylcarbonyl group, or alkylcarbonyloxy, may optionally be substituted with one or more substituents.
[0058] In the conductive polymer, the lower limit of the ratio of moles of thiophene units having hydrocarbon functional groups may be approximately 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, or 85 mol%, and the upper limit may be approximately 95 mol%, 90 mol%, 85 mol%, 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, or 45 mol%. The ratios are based on the total number of moles of monomer units contained in the polymer. The ratio may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or greater than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, but within a range of any lower limit or greater than any of the lower limits mentioned above.
[0059] By including the thiophene units in the conductive polymer, the polymer or the polymer layer containing it exhibits an appropriate PTC (Positive Temperature Coefficient) effect, its surface properties are adjusted to ensure excellent adhesion to electrodes or current collectors, and it can exhibit an appropriate level of oxidation potential.
[0060] The hydrocarbon functional group is a functional group that can impart appropriate fluidity (mobility) to the polymerization process of the conductive polymer or to the conductive polymer itself. Such a functional group imparts appropriate fluidity to the monomer mixture and allows polymerization to occur with excellent efficiency by diffusing within the monomer mixture. Furthermore, the conductive polymer having the functional group can ensure that a stable and uniform polymer layer is formed between the current collector and the active material layer through appropriate fluidity.
[0061] The hydrocarbon functional groups may be appropriately oriented during the drying or annealing (heat treatment) process applied in the polymer layer formation process to impart PTC effect and oxidation potential characteristics suitable for the polymer.
[0062] When a certain amount of thermal energy is applied to the hydrocarbon functional group, it vibrates due to the heat. This vibration (thermal vibration) promotes the dedoping of anions bonded to the polymer, thereby inducing an increase in resistance. The temperature at which the thermal vibration occurs can be controlled by the length and / or amount of the hydrocarbon functional group. For example, at the same temperature, the thermal vibration of a relatively long chain is greater than that of a relatively short chain, and consequently, the longer chain can induce a resistance increase effect at a relatively lower temperature. Therefore, the desired PTC effect can be set by controlling the length and / or ratio of the hydrocarbon functional group.
[0063] The thiophene units of the hydrocarbon functional group may include a first thiophene unit having a long-chain hydrocarbon functional group and a second thiophene unit having a short-chain hydrocarbon functional group.
[0064] The term "long-chain hydrocarbon functional group" refers to a hydrocarbon functional group as described above, but specifically one in which the number of carbon atoms has been adjusted to a certain level or higher.
[0065] The term "short-chain hydrocarbon functional group" refers to a hydrocarbon functional group as described above, but specifically one in which the number of carbon atoms has been adjusted to a certain level or lower.
[0066] The lower limit of the carbon number of the long-chain hydrocarbon functional group may be around 10, 11, or 12, and the upper limit may be around 20, 19, 18, 17, 16, 15, 14, 13, 12, 11, or 10. The carbon number of the long-chain hydrocarbon functional group may be within a range of being above or above any of the lower limits mentioned above; or it may be below or below any of the upper limits mentioned above, while being above or above any of the lower limits mentioned above.
[0067] The lower limit of the number of carbon atoms in the short-chain hydrocarbon functional group may be approximately 3, 4, 5, 6, 7, or 8, and the upper limit may be approximately 9, 8, 7, or 6. The number of carbon atoms in the short-chain hydrocarbon functional group may be within or below any of the upper limits mentioned above; or it may be within or below any of the upper limits mentioned above, while being above or above any of the lower limits mentioned above.
[0068] The specific descriptions of the long-chain and short-chain hydrocarbon functional groups are as described for the hydrocarbon functional groups, except for the number of carbon atoms.
[0069] In the conductive polymer, the lower limit of the ratio of the total number of moles of the first and second thiophene units may be approximately 10 mol%, 15 mol%, 20 mol%, 25 mol%, 30 mol%, 35 mol%, 40 mol%, 45 mol%, 50 mol%, 55 mol%, 60 mol%, 65 mol%, 70 mol%, 75 mol%, 80 mol%, or 85 mol%, and the upper limit may be approximately 95 mol%, 90 mol%, 85 mol%, 80 mol%, 75 mol%, 70 mol%, 65 mol%, 60 mol%, 55 mol%, 50 mol%, or 45 mol%. The ratio is based on the total number of moles of monomer units contained in the polymer. The ratio may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or greater than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, but within a range of any lower limit or greater than any of the lower limits mentioned above.
[0070] The lower limit of the ratio (M2 / M1) of the number of moles of the second thiophene units (M2) to the number of moles of the first thiophene units (M1) in the conductive polymer may be approximately 0.01, 0.05, 0.1, 0.5, 1, 1.5, or 2, and the upper limit may be approximately 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 9, 8, 7, 6, 5, 4, 3, 2, 1, 0.8, 0.7, 0.6, or 0.55. The ratio may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or more than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, while being above or more than any of the lower limits mentioned above.
[0071] Under such ratios, the conductive polymer or the polymer layer exhibits an appropriate PTC (Positive Temperature Coefficient) effect, and its surface properties are adjusted to ensure excellent adhesion to the electrode or current collector.
[0072] The polymer may further include, as the thiophene units, thiophene units having polar functional groups in addition to the thiophene units having hydrocarbon functional groups.
[0073] The term "polar functional group" refers to a functional group that contains one or more polar atoms, such as oxygen and / or nitrogen. Examples of such polar functional groups include, but are not limited to, carboxyl groups, hydroxyl groups, amino groups, cyano groups, nitro groups, ether groups, or the functional group of chemical formula 1 below.
[0074] [ka]
[0075] In chemical formula 1, L3 is a single bond, an alkylene group, or an alkylidene group; L4 is an alkylene group or an alkylidene group; R8 is a hydrogen atom or an alkyl group; and n is any number.
[0076] In chemical formula 1, L3 being a single bond means that L3 is absent, and the oxygen atom between L4 and L3 is directly linked to the monomer or polymer backbone.
[0077] In this specification, the term "alkylene group" refers to a divalent functional group in an alkane formed by the removal of hydrogen atoms from two different carbon atoms, while the term "alkylidene group" refers to a divalent functional group in an alkane formed by the removal of two hydrogen atoms from one carbon atom.
[0078] In this specification, the term "alkylene group" may refer to an alkylene group having 2 to 20 carbon atoms, 2 to 16 carbon atoms, 2 to 12 carbon atoms, 2 to 8 carbon atoms, or 2 to 4 carbon atoms, unless otherwise specified. The alkylene group may be linear, branched, or cyclic, and may be optionally substituted with one or more substituents.
[0079] In this specification, the term "alkylidene group" may refer to alkylidene groups having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, unless otherwise specified. The alkylidene group may be linear, branched, or cyclic, and may be optionally substituted with one or more substituents.
[0080] The alkyl group R8 in Chemical Formula 1 may, for example, be an alkyl group having 1 to 20 carbon atoms, 1 to 16 carbon atoms, 1 to 12 carbon atoms, 1 to 8 carbon atoms, or 1 to 4 carbon atoms, or it may be a methyl group or an ethyl group. The alkyl group may be linear, branched, or cyclic, and may appropriately be linear or branched.
[0081] In chemical formula 1, the lower limit of n may be approximately 1, 2, 3, or 4, and its upper limit may be approximately 10, 9, 8, 7, 6, 5, 4, or 3. The n may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or greater than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, while being above or greater than any of the lower limits mentioned above.
[0082] Through the application of the aforementioned polar functional groups, a polymer layer containing a conductive polymer can be bonded to other layers with appropriate bonding force, and such a uniform layer of conductive polymer can be formed to efficiently achieve the desired protective function.
[0083] When thiophene units having the polar functional group are present in a conductive polymer, the thiophene units having the polar functional group can be present such that the total number of moles of thiophene units having the hydrocarbon functional group is within a predetermined range per mole of thiophene units having the polar functional group.
[0084] For example, the lower limit of the ratio (i.e., M / M3) of the total number of moles (M) of thiophene units having the hydrocarbon functional group to the number of moles (M3) of thiophene units having the polar functional group may be around 1, 2, 3, 4, 5, 6, 8 moles or 8.5 moles, and the upper limit may be around 500, 450, 400, 350, 300, 250, 200, 150, 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 15, 10, 9.5 moles or 9 moles. The ratio may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or more than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, while being within a range of any lower limit or more than any of the lower limits mentioned above.
[0085] The thiophene unit described above may be, for example, the unit shown in Chemical Formula 2 below.
[0086] [ka]
[0087] In chemical formula 2, R1 and R2 can each be independently hydrogen, the polar functional group, or the hydrocarbon functional group.
[0088] In other examples, R1 and R2 of chemical formula 1 may be linked together to form the divalent functional group of chemical formula 3 shown below.
[0089] [ka]
[0090] In chemical formula 3, L1 and L2 are independently a single bond, an alkylene group, or an alkylidene group, and R3 and R4 are independently hydrogen, the polar functional group, or the hydrocarbon functional group.
[0091] For example, if the unit of chemical formula 2 is a thiophene unit having the aforementioned hydrocarbon functional group, then one or more of R1 and R2 may be the hydrocarbon functional group (if R1 and R2 are not linked), and one or more of R3 and R4 may be the hydrocarbon functional group (if R1 and R2 are not linked).
[0092] For example, if the unit of chemical formula 2 is a thiophene unit having the aforementioned polar functional group, then one or more of R1 and R2 may be the aforementioned polar functional group (when R1 and R2 are not linked), and one or more of R3 and R4 may be the aforementioned polar functional group (when R1 and R2 are not linked).
[0093] For example, if the unit of chemical formula 2 is the aforementioned first thiophene unit, then one or more of R1 and R2 may be the aforementioned long-chain hydrocarbon functional group (if R1 and R2 are not linked), and one or more of R3 and R4 may be the aforementioned long-chain hydrocarbon functional group (if R1 and R2 are not linked).
[0094] For example, if the unit of chemical formula 2 is the aforementioned second thiophene unit, then one or more of R1 and R2 may be the aforementioned short-chain hydrocarbon functional group (when R1 and R2 are not linked), and one or more of R3 and R4 may be the aforementioned short-chain hydrocarbon functional group (when R1 and R2 are not linked).
[0095] A detailed explanation of the aforementioned hydrocarbon functional groups, polar functional groups, long-chain hydrocarbon functional groups, and short-chain hydrocarbon functional groups is as described above.
[0096] Furthermore, a detailed explanation of the alkylene group and alkylidene group in chemical formula 3 is as described in chemical formula 1.
[0097] The polymer may contain additional monomeric units along with the thiophene units. For example, additional monomers may be included to adjust the oxidation potential of the polymer. For instance, units exhibiting a lower or higher oxidation potential relative to the thiophene units may be included in the conductive polymer as needed.
[0098] The polymer may have a weight-average molecular weight (Mw) within a predetermined range. The lower limit of the weight-average molecular weight of the polymer is 10,000 g / mol, 11,000 g / mol, 12,000 g / mol, 13,000 g / mol, 14,000 g / mol, 15,000 g / mol, 16,000 g / mol, 17,000 g / mol, 18,000 g / mol, 19,000 g / mol, 20,000 g / mol, 21,000 g / mol, 22,000 g / mol, 23,000 g / mol, 24,000 g / mol, 25,000 g / mol, 26,000 g / mol, and 27,000 g / mol. Possible concentrations include 28,000 g / mol, 29,000 g / mol, 30,000 g / mol, 31,000 g / mol, 32,000 g / mol, 33,000 g / mol, 34,000 g / mol, 35,000 g / mol, 36,000 g / mol, 37,000 g / mol, 38,000 g / mol, 39,000 g / mol, or approximately 40,000 g / mol, with upper limits being 2,000,000 g / mol, 1,500,000 g / mol, 1,000,000 g / mol, 900,000 g / mol, and 800,000 g / mol. 00g / mol, 700,000g / mol, 600,000g / mol, 500,000g / mol, 400,000g / mol, 300,000g / mol, 295,000g / mol, 290,000g / mol, 285,000g / mol, 280, 000g / mol, 275,000g / mol, 270,000g / mol, 265,000g / mol, 260,000g / mol, 255,000g / mol, 250,000g / mol, 245,000g / mol, 240,000g / mol, 235, 000g / mol, 230,000g / mol, 225,000g / mol, 220,000g / mol, 215,000g / mol, 210,000g / mol, 205,000g / mol, 200,000g / mol, 195,000g / mol, 190, 000g / mol, 185,000g / mol, 180,000g / mol, 175,000g / mol, 170,000g / mol, 165,000g / mol, 160,000g / mol, 155,000g / mol, 150,000g / mol, 145,The weight-average molecular weight may be approximately 000 g / mol, 140,000 g / mol, 135,000 g / mol, 130,000 g / mol, 125,000 g / mol, 120,000 g / mol, 115,000 g / mol, 110,000 g / mol, 105,000 g / mol, or 100,000 g / mol. The weight-average molecular weight may be within a range of any upper limit or less than any of the upper limits mentioned above; within a range of any lower limit or greater than any of the lower limits mentioned above; or within a range of any upper limit or less, while being above or greater than any lower limit or greater than any of the lower limits mentioned above.
[0099] The molecular weight distribution of the polymer, i.e., the ratio of weight-average molecular weight (Mw) to number-average molecular weight (Mn), may be within a predetermined range. The lower limit of the molecular weight distribution may be approximately 2, 2.5, 3, 3.5, or 4, and the upper limit may be approximately 8, 7.5, 7, 6.5, 6, 5.5, 5, 4.5, 4, or 3.5. The molecular weight distribution may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or more than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, while being above or above any one of the lower limits mentioned above.
[0100] The weight-average molecular weight and molecular weight distribution are measured using the method described in "2. GPC (Gel Permeation Chromatograph)" of the Examples section of this specification.
[0101] The polymer layer may contain the polymer. The polymer layer may consist of the polymer alone, or it may contain any other necessary additives in addition to the polymer. By using the polymer, the desired electrode can be effectively formed. In one example, the lower limit of the polymer content in the polymer layer may be around 30% by weight, 35% by weight, 40% by weight, 45% by weight, 50% by weight, 55% by weight, 60% by weight, 65% by weight, 70% by weight, 75% by weight, 80% by weight, 85% by weight, 90% by weight, or 95% by weight, and the upper limit may be around 100% by weight, 95% by weight, 90% by weight, or 85% by weight based on the total weight of the polymer layer. The ratios are based on the total weight of the polymer layer. The range of the ratios may be within or below any of the upper limits mentioned above; or within or above any of the lower limits mentioned above; or within or below any of the upper limits mentioned above, while being within or above any of the lower limits mentioned above.
[0102] The thickness of the polymer layer can be appropriately controlled depending on the purpose. For example, the lower limit of the thickness may be around 10 nm, 50 nm, 100 nm, 150 nm, 200 nm, 250 nm, 300 nm, 350 nm, 400 nm, 450 nm, or 500 nm, and the upper limit may be around 2 μm, 1.5 μm, 1 μm, 950 nm, 900 nm, 850 nm, 800 nm, 750 nm, 700 nm, 650 nm, 600 nm, 550 nm, 500 nm, 450 nm, 400 nm, 350 nm, or 300 nm. The thickness may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or more than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, while being above or above any of the lower limits mentioned above. The aforementioned thickness can be measured by the method described in "3. Thickness Measurement" of the Examples section of this specification.
[0103] The current collector included in the electrode can be any current collector that is normally used as a positive or negative electrode current collector, without any particular restrictions.
[0104] The type, size, and shape of the current collector are not particularly limited, as long as it does not induce chemical changes in the application device such as a secondary battery and is conductive. Examples of materials that can be used as the current collector include copper, aluminum, stainless steel, nickel, titanium, or calcined carbon, or materials whose surface is treated with carbon, nickel, titanium, or silver, etc. The current collector may be in the form of a film, sheet, foil, net, porous body, foam, or nonwoven fabric containing the material. In some cases, the surface of the current collector may be subjected to a known surface treatment to improve adhesion to other layers such as a polymer layer or an active material layer.
[0105] Such current collectors can typically have a thickness in the range of 3 μm to 500 μm, but are not limited to this range.
[0106] The active material layer can also be a layer that is normally applied.
[0107] Typically, the active material layer includes an electrode active material. There are no particular restrictions on the specific type of electrode active material; typically, a material that forms the positive or negative electrode can be used.
[0108] For example, if the active material layer is a positive electrode active material layer, the electrode active material may be a layered compound such as lithium cobalt oxide (LiCoO2), lithium nickel oxide (LiNiO2), or a compound substituted with one or more transition metals; lithium iron oxide such as LiFe3O4; or a compound with the chemical formula Li 1+C1 Mn 2-c1 Lithium manganese oxides such as O4 (0 ≤ c1 ≤ 0.33), LiMnO3, LiMn2O3, or LiMnO2; lithium copper oxide (Li2CuO2); vanadium oxides such as LiV3O8, V2O5, or Cu2V2O7; chemical formula LiNi1-c2 M c2 O2 (wherein M is at least one selected from the group consisting of Co, Mn, Al, Cu, Fe, Mg, B and Ga, and satisfies 0.01≦c2≦0.3), a Ni-site type lithium nickel oxide represented by; a chemical formula LiMn 2-c3 M c3 O2 (wherein M is at least one selected from the group consisting of Co, Ni, Fe, Cr, Zn and Ta, and satisfies 0.01≦c3≦0.1) or Li2Mn3MO8 (wherein M is at least one selected from the group consisting of Fe, Co, Ni, Cu and Zn), a lithium manganese composite oxide represented by; lithium nickel cobalt manganese (NCM) composite oxide, lithium nickel cobalt manganese aluminum (NCMA) composite oxide, and LiMn2O4 in which part of Li in the chemical formula is substituted with an alkaline earth metal ion, and the like, but are not limited thereto.
[0109] When the active material layer is a negative electrode active material layer, a compound capable of reversible intercalation and deintercalation of lithium may be used as the electrode active material. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloy, Sn alloy, or Al alloy; SiO a (0<a<2), SnO2, vanadium oxide, metal oxides capable of doping and dedoping lithium such as lithium vanadium oxide; or composites containing the aforementioned metallic compound and carbonaceous material such as Si-C composite or Sn-C composite, and the like, and any one or a mixture of two or more thereof may be used.
[0110] A lithium thin film may be used as the negative electrode active material, and low-crystalline carbon and high-crystalline carbon may be used as the carbon material. Typical low-crystalline carbons include soft carbon and hard carbon, while typical high-crystalline carbons include amorphous, plate-like, flake-like, spherical or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, mesocarbon microbeads, mesophase pitches, and high-temperature calcined carbon such as petroleum or coal tar pitch-derived cokes.
[0111] The electrode active material may be present in the active material layer in an amount of approximately 80% to 99.5% by weight or 88% to 99% by weight relative to the total weight of the active material layer, but the ratio can be changed depending on the application and design of the electrode.
[0112] The active material layer may additionally contain a binder. The binder plays a role in improving adhesion between the active materials and between the active material layer and the current collector. Examples of the binder are not particularly limited and include, for example, PVDF (Poly(vinylidene fluoride)), PVA (poly(vinyl alcohol)), SBR (styrene butadiene rubber), PEO (poly(ethylene oxide)), CMC (carboxyl methyl cellulose), cellulose acetate, cellulose acetate butylate, cellulose acetate propionate, cyanoethyl pullulan, cyanoethyl polyvinyl alcohol, cyanoethyl cellulose, and cyanoethyl sucrose. One or more substances may be selected and used from the group consisting of sucrose, pullulan, polymethyl methacrylate, polybutylacrylate, polyacrylonitrile, polyvinylpyrrolidone, polyvinylacetate, polyethylene-co-vinyl acetate, and polyarylate.
[0113] The binder may, for example, be included in the active material layer in an amount of 0.1 to 10 parts by weight or 0.5 to 5 parts by weight per 100 parts by weight of the electrode active material, but is not limited thereto.
[0114] The active material layer may optionally contain additional conductive materials. Any known conductive material can be used without particular limitation, as long as it does not induce chemical changes in the secondary battery and is conductive. For example, graphite such as natural graphite or artificial graphite; carbon black such as carbon black, acetylene black, Kechen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes (CNTs); metal powders such as fluorocarbon, aluminum, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide and / or polyphenylene derivatives; and other conductive materials.
[0115] The conductive material may, for example, be included in an amount of 0.1 to 20 parts by weight or 0.3 to 10 parts by weight per 100 parts by weight of the electrode active material, but may also be included in the active material layer, although it is not limited to this.
[0116] The active material layer may also contain additional known components as needed, in addition to the components described above.
[0117] This specification also discloses a method for manufacturing the electrode.
[0118] The manufacturing method may include the step of forming the polymer layer on the current collector, and may also include the step of forming the active material layer on the polymer layer.
[0119] There are no particular restrictions on the method of forming the polymer layer on the current collector. For example, the polymer layer can be formed by diluting the conductive polymer and, if necessary, other additives in a suitable solvent to produce a coating solution, coating the current collector with this solution, and then drying it.
[0120] In another example, the monomers forming the conductive polymer may be directly polymerized on the current collector to form the polymer layer.
[0121] The method for producing the coating composition for forming the polymer layer and the coating method are not particularly limited, and known coating methods can be applied. Similarly, the method for polymerizing the conductive polymer is not particularly limited, and known methods can be applied. For example, methods utilizing oxidative polymerization reactions and radical reactions are known for producing polythiophene, and such methods can also be applied to the process of forming the conductive polymer in the present invention.
[0122] A polymer layer can be formed on a current collector using the manufactured coating composition. This process typically includes the steps of coating the current collector with the coating composition and heat-treating the coated coating composition. The properties of the polymer layer can also be controlled by the conditions of the heat treatment during this process.
[0123] For example, the temperature T and / or time H of the heat treatment can be adjusted.
[0124] For example, the lower limit of the temperature T could be around 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, or 140°C, and its upper limit could be 300°C, 295°C, 290°C, 285°C, 280°C, 275°C, 270°C, 265°C, 260°C, 255°C, or 250°C. The temperature may be approximately 245°C, 240°C, 235°C, 230°C, 225°C, 220°C, 215°C, 210°C, 205°C, 200°C, 195°C, 190°C, 185°C, 180°C, 175°C, 170°C, 165°C, 160°C, 155°C, 150°C, 145°C, 140°C, 135°C, 130°C, 125°C, 120°C, 115°C, 110°C, 105°C, 100°C, 95°C, or 90°C. The temperature may be within the range of any upper limit or less than any of the upper limits mentioned above; or within the range of any lower limit or more than any of the lower limits mentioned above; or within the range of any upper limit or less than any of the upper limits mentioned above, but within the range of any lower limit or more than any of the lower limits mentioned above. Within this range, the alignment of hydrocarbon groups in the conductive polymer can be appropriately adjusted, thereby ensuring the desired properties.
[0125] The product of the heat treatment temperature T and time H (T × H) can be adjusted to achieve the objective.For example, the lower limit of the product (T×H) of the heat treatment temperature T and the time H may be on the order of 0.01°C·hour, 0.05°C·hour, 0.1°C·hour, 0.2°C·hour, 0.3°C·hour, 0.5°C·hour, 1°C·hour, 5°C·hour, 10°C·hour, 15°C·hour, 20°C·hour, 25°C·hour, 30°C·hour, 35°C·hour, 40°C·hour, 45°C·hour, 50°C·hour, 75°C·hour, 100°C·hour, 110°C·hour, 120°C·hour or 130°C·hour, and the upper limit thereof may be on the order of 100000°C·hour, 95000°C·hour, 90000°C·hour, 85000°C·hour, 80000°C·hour, 75000°C·hour, 70000°C·hour, 65000°C·hour, 60000°C·hour, 55000°C·hour, 50000°C·hour, 45000°C·hour, 40000°C·hour, 35000°C·hour, 30000°C·hour, 25000°C·hour, 20000°C·hour, 15000°C·hour, 10000°C·hour, 9500°C·hour, 9000°C·hour, 8500°C·hour, 8000°C·hour, 7500°C·hour, 7000°C·hour, 6500°C·hour, 6000°C·hour, 5500°C·hour, 5000°C·hour, 4500°C·hour, 4000°C·hour, 3500°C·hour, 3000°C·hour, 2500°C·hour, 2000°C·hour, 1500°C·hour, 1400°C·hour, 1300°C·hour, 1200°C·hour, 1100°C·hour, 1000°C·hour, 900°C·hour, 800°C·hour, 700°C·hour, 600°C·hour, 500°C·hour, 400°C·hour, 300°C·hour, 200°C·hour, 100°C·hour, 90°C·hour, 80°C·hour, 70°C·hour, 60°C·hour, 50°C·hour, 45°C·hour, 40°C·hour, 35°C·hour, 30°C·hour, 25°C·hour, 20°C·hour, 15°C·hour, 10°C·hour, 5°C·hour, 4°C·hour, 3°C·hour, 2°C·hour, 1°C·hour or 0.5°C·hour.The aforementioned product (T × H) may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or greater than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, but within a range of any lower limit or greater than any of the lower limits mentioned above. Within such a range, the alignment state of the hydrocarbon groups of the conductive polymer can be appropriately adjusted, and the desired properties can be ensured accordingly.
[0126] To more effectively ensure the desired properties, the heat treatment may be carried out in two stages.
[0127] For example, the heat treatment may include a step of primary heat treatment of the coating composition at a first temperature T1 for a first time H1 and a step of secondary heat treatment at a second temperature T2 for a second time H2, where the temperatures T1 and T2 are different from each other, and / or the times H1 and H2 are different from each other.
[0128] For example, the lower limit of the temperature T1 could be around 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, or 140°C, and its upper limit could be 300°C, 295°C, 290°C, 285°C, 280°C, or 275°C. The temperature may be approximately 270°C, 265°C, 260°C, 255°C, 250°C, 245°C, 240°C, 235°C, 230°C, 225°C, 220°C, 215°C, 210°C, 205°C, 200°C, 195°C, 190°C, 185°C, 180°C, 175°C, 170°C, 165°C, 160°C, 155°C, 150°C, 145°C, or 140°C. The temperature may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or more than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, but within a range of any lower limit or more than any of the lower limits mentioned above. Within such a range, the alignment of hydrocarbon groups in the conductive polymer can be appropriately adjusted, and the desired properties can be ensured accordingly.
[0129] For example, the lower limit of the product of the temperature T1 and time H1 (T1 × H1) in the primary heat treatment could be around 0.01°C / hour, 0.05°C / hour, 0.1°C / hour, 0.2°C / hour, or 0.3°C / hour, and its upper limit could be 1000°C / hour, 900°C / hour, 800°C / hour, 700°C / hour, 600°C / hour, 500°C / hour, 400°C / hour, 300°C / hour, or 200°C / hour. r may be approximately 100°C.hour, 90°C.hour, 80°C.hour, 70°C.hour, 60°C.hour, 50°C.hour, 45°C.hour, 40°C.hour, 35°C.hour, 30°C.hour, 25°C.hour, 20°C.hour, 15°C.hour, 10°C.hour, 5°C.hour, 4°C.hour, 3°C.hour, 2°C.hour, 1°C.hour, or 0.5°C.hour. The product (T1 × H1) may be within the range of any upper limit or less than any of the upper limits mentioned above; or within the range of any lower limit or greater than any of the lower limits mentioned above; or within the range of any upper limit or less than any of the upper limits mentioned above, while being above or greater than any lower limit or greater than any of the lower limits mentioned above. Within such a range, the alignment state of the hydrocarbon groups of the conductive polymer can be appropriately adjusted, and the desired properties can be ensured accordingly.
[0130] For example, the lower limit of the heat treatment temperature T2 for the secondary heat treatment could be around 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, or 130°C, and its upper limit could be 300°C, 295°C, 290°C, 285°C, 280°C, 275°C, or 270°C. The temperature may be approximately 265°C, 260°C, 255°C, 250°C, 245°C, 240°C, 235°C, 230°C, 225°C, 220°C, 215°C, 210°C, 205°C, 200°C, 195°C, 190°C, 185°C, 180°C, 175°C, 170°C, 165°C, 160°C, 155°C, 150°C, 145°C, 140°C, 135°C, or 130°C. The temperature may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or more than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, but within a range of any lower limit or more than any of the lower limits mentioned above. Within such a range, the alignment state of the hydrocarbon groups of the conductive polymer can be appropriately adjusted, and the desired properties can be ensured accordingly.
[0131] The product of the secondary heat treatment temperature T2 and time H2 (T2 × H2) can be adjusted. For example, the lower limit of the product of the heat treatment temperature T and time H (T² × H²) may be around 10°C / hour, 15°C / hour, 20°C / hour, 25°C / hour, 30°C / hour, 35°C / hour, 40°C / hour, 45°C / hour, 50°C / hour, 75°C / hour, 100°C / hour, 110°C / hour, 120°C / hour, or 130°C / hour, and its upper limit may be around 1000°C / hour, 900°C / hour, 800°C / hour, 700°C / hour, 600°C / hour, 500°C / hour, 400°C / hour, 300°C / hour, 200°C / hour, 180°C / hour, 160°C / hour, 150°C / hour, 145°C / hour, 140°C / hour, 135°C / hour, or 130°C / hour. The aforementioned product (T2 × H2) may be within a range of any upper limit or less than any of the upper limits mentioned above; or within a range of any lower limit or greater than any of the lower limits mentioned above; or within a range of any upper limit or less than any of the upper limits mentioned above, but within a range of any lower limit or greater than any of the lower limits mentioned above. Within such a range, the alignment state of the hydrocarbon groups of the conductive polymer can be appropriately adjusted, and the desired properties can be ensured accordingly.
[0132] In the above case, the lower limit of the ratio T1 / T2 between the primary heat treatment temperature T1 and the secondary heat treatment temperature T2 may be approximately 0.1, 0.3, 0.5, 0.7, 0.9, 0.95, 1, 1.01, 1.02, 1.03, 1.04, 1.05, 1.06, or 1.07, and the upper limit may be approximately 10, 9, 8, 7, 6, 5, 4, 3, 2, 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3, 1.2, or 1.1. The ratio T1 / T2 may be within the range of any upper limit or less than any of the upper limits mentioned above; or within the range of any lower limit or more than any of the lower limits mentioned above; or within the range of any upper limit or less than any of the upper limits mentioned above, while being above or more than any of the lower limits mentioned above. Within this range, the alignment of hydrocarbon groups in the conductive polymer can be appropriately adjusted, thereby ensuring the desired properties.
[0133] In the above case, the lower limit of the ratio H2 / H1 between the primary heat treatment time H1 and the secondary heat treatment time H2 may be around 0.5, 1, 3, 5, 7, 9, 10, 11, 12, 13, 14, 14.5, or 15, and the upper limit may be around 100, 95, 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 20, 19, 18, 17, 16, 15.5, or 15. The ratio H2 / H1 may be within the range of any upper limit or less than any of the upper limits mentioned above; or within the range of any lower limit or more than any of the lower limits mentioned above; or within the range of any upper limit or less than any of the upper limits mentioned above, but within the range of any lower limit or more than any of the lower limits mentioned above. Within such a range, the alignment state of the hydrocarbon groups of the conductive polymer can be appropriately adjusted, and the desired properties can be ensured accordingly.
[0134] In the manufacturing process, additional post-processing steps, such as a suitable drying step, may be carried out following the coating and / or polymerization process.
[0135] There are no particular restrictions on the method for forming the active material layer on the polymer layer. Typically, the active material layer is formed by coating a slurry containing the electrode active material, binder, and conductive material onto the current collector (polymer layer), drying, and then rolling it. Such known methods can also be applied in the present invention.
[0136] This specification also introduces electrode assemblies or electrochemical elements, such as secondary batteries, that include the electrodes. The electrode assemblies and electrochemical elements are not specifically limited in their other configurations, as long as they include the electrodes described above. For example, the electrode assembly may include a positive electrode, a negative electrode, and a separator membrane between the positive and negative electrodes, in which case one or both of the positive and negative electrodes may be the electrodes described above. Furthermore, the electrochemical element, such as a secondary battery, may include the electrodes or the electrode assembly and an electrolyte, etc. [Effects of the Invention]
[0137] This specification discloses electrodes and their applications. The electrodes include a polymer layer exhibiting a controlled positive temperature coefficient (PTC) effect and oxidation potential for a particular purpose. Such electrodes, under normal conditions, exhibit excellent electrical properties such as low resistance, thus not affecting, or even improving, the performance and operation of secondary batteries, while ensuring stability under abnormal conditions. This specification also discloses applications of such electrodes. [Brief explanation of the drawing]
[0138] [Figure 1] This is an illustrative cross-sectional view of an electrode. [Figure 2] This is the NMR analysis result of monomers produced in the manufacturing example. [Figure 3] This shows the performance evaluation results for the electrode of Example 1. [Figure 4] This shows the performance evaluation results for the electrode of Example 1. [Figure 5] This shows the performance evaluation results for the electrode of Comparative Example 1. [Figure 6]These are the performance evaluation results for the electrode of Comparative Example 1. DESCRIPTION OF EMBODIMENTS
[0139] Hereinafter, the electrodes and the like disclosed in the present specification will be specifically described through Examples and Comparative Examples, but the scope of the electrodes and the like is not limited by the following Examples.
[0140] 1. NMR Analysis Method 1 1H-NMR analysis was performed at room temperature using an NMR spectrometer including a Bruker UltraShield spectrometer (300 MHz) equipped with a triple-resonance 5 mm probe. The sample was diluted to a concentration of about 10 mg / ml in an NMR measurement solvent (CDCl3) for use, and the chemical shift was expressed in ppm.
[0141] 2. GPC (Gel Permeation Chromatography) Molecular weight characteristics were measured using GPC (Gel Permeation Chromatography). A sample is placed in a 5 mL vial and diluted with chloroform to a concentration of about 1 mg / mL. Thereafter, the calibration standard sample and the sample to be analyzed were filtered through a syringe filter (pore size: 0.45 μm) and then measured. Using Waters' Empower 3 as the analysis program, the elution time of the sample was compared with the calibration curve to determine the weight average molecular weight (Mw) and the number average molecular weight (Mn) respectively, and the molecular weight distribution (PDI) was calculated from the ratio (Mw / Mn). The GPC measurement conditions are as follows.
[0142] <GPC Measurement Conditions> Apparatus: Waters 2414 Columns: 3 Waters Styragel columns used Solvent: THF (Tetrahydrofuran) Column temperature: 35℃ Sample concentration: 1 mg / mL, 1 μL injection Standard sample: Polystyrene (Mp: 3,900,000, 723,000, 316,500, 52,200, 31,400, 7,200, 3,940, 485)
[0143] 3. Thickness measurement The thickness of the polymer layer and other components was measured by cross-sectioning the electrode using an ion milling device (Hitachi, IM5000) and then capturing an image with a scanning electron microscope (SEM) (JEOL, JSM-7200F). The cross-section formation conditions for ion milling were set to cross-section milling mode, with a speed (reciprocation / min) of 3, an acceleration voltage of 6.0kV, a discharge voltage of 15kV, a current of 150μA, and a time of 4 hours.
[0144] 4. Method for measuring oxidation potential (conductive polymer / polymer layer) The oxidation potential was measured using the following method. A layer approximately 10 μm thick (hereinafter referred to as the polymer layer) was formed on an aluminum foil (Al Foil) with a thickness of approximately 15 μm using a conductive polymer for which the oxidation potential was to be measured. The polymer layer was formed by applying the same method as that used in Example 1 below.
[0145] Subsequently, a separation membrane and a lithium film were laminated onto the polymer layer to produce a laminate consisting of aluminum foil / polymer layer / separation membrane / lithium film, and this laminate was punched out into a circular shape with a diameter of approximately 1.4 cm. A coin cell was manufactured using the circularly punched laminate and electrolyte (using a Welcos CR2032 coin cell kit).
[0146] As the separation membrane, we used the WL20C model from DoubleScope Korea, and as the lithium film, we used a film with a thickness of approximately 100 μm. As the electrolyte, we used a 1M LiPF6 solution from Enchem (solvent: EC / DMC / EMC = 3 / 4 / 3 (mass ratio), EC: ethylene carbonate, DMC: dimethyl carbonate, EMC: ethyl methyl carbonate).
[0147] The oxidation potential of the coin cell was measured at 25°C using an electrochemical measuring instrument (potentiostat) (Princeton Applied Research, PARASTAT-MC). The oxidation potential was measured by measuring the CV (Cyclic Voltammetry) in the range of 1.5V to 5.5V at a scan speed of 0.17mV / sec to 0.5mV / sec. The oxidation potential is the oxidation potential with respect to lithium, and is the oxidation potential between lithium and lithium ions (Li / Li + This measurement was taken based on the standard.
[0148] 5. Oxidation potential measurement method (electrode active material) The oxidation potential of the electrode active material was measured for a coin cell manufactured using an electrode made with the electrode active material.
[0149] A slurry was prepared by blending the electrode active material, conductive material (ECP (Ketjen Black) 0.5%, SFG (Trimrex graphite) 0.4%, DB (Denka Black) 0.4%), PVDF (poly(vinylidene fluoride)), and NMP (N-Methyl-2-pyrrolidone) in a weight ratio of 75:1:1:23 (electrode active material:conductive material:PVDF:NMP). The slurry was applied to a current collector with a doctor blade, dried at room temperature (approximately 25°C), maintained in a drying oven at 130°C for about 30 minutes, and then rolled to form an electrode active material layer with a thickness of approximately 53 μm, thereby producing an electrode.
[0150] The electrode active material used was the electrode active material that was the subject of the measurement.
[0151] The rolling process was carried out so that the porosity of the active material layer was approximately 25%. The porosity of the active material layer was calculated by comparing the ratio of the difference between the actual density and the density after rolling, and this method of determining porosity is well known.
[0152] As the current collector, aluminum foil with a thickness of approximately 15 μm was used.
[0153] Subsequently, a separation membrane and a lithium film were laminated onto the electrode active material layer of the electrode to produce a laminate consisting of the electrode, separation membrane, and lithium film. This laminate was then punched out in a circular shape with a diameter of approximately 1.4 cm. A coin cell was manufactured using the circularly punched laminate and electrolyte (using a Welcos CR2032 coin cell kit).
[0154] As the separation membrane, we used the WL20C model from DoubleScope Korea, and as the lithium fill, we used a film with a thickness of approximately 100 μm. As the electrolyte, we used a 1M LiPF6 solution from Enchem (solvent: EC / DMC / EMC = 3 / 4 / 3 (mass ratio), EC: ethylene carbonate, DMC: dimethyl carbonate, EMC: ethyl methyl carbonate).
[0155] The oxidation potential of the coin cell was measured at 25°C using an electrochemical measuring instrument (potentiostat) (Princeton Applied Research, PARASTAT-MC). The oxidation potential was measured by measuring the cyclic voltage (CV) in the range of 1.5V to 5.5V at a scan speed of 0.17mV / sec to 0.5mV / sec.
[0156] The oxidation potential is the oxidation potential for lithium, and is the oxidation potential for lithium and lithium ions (Li / Li + This measurement was taken based on the standard.
[0157] 6. Method for measuring DC resistance DC resistance was evaluated using the same coin cell as described in "4. Oxidation Potential Measurement Method (Conductive Polymer / Polymer Layer)" above. However, the thickness of the polymer layer in the coin cell was set to approximately 200 nm. A voltage of 4.3 eV was applied to the coin cell at room temperature (25°C) for 10 minutes, and the DC resistance was measured using a Fluke digital multimeter (FLUKE-87-5).
[0158] 7. Interface resistance (AC impedance resistance) The interfacial resistance was evaluated using EIS (Electrochemical Impedance Spectronization) with the same coin cell used in "4. Oxidation Potential Measurement Method (Conductive Polymer / Polymer Layer)" described above. However, the thickness of the polymer layer in the coin cell was set to approximately 200 nm. A voltage of 4.3 V was applied to the coin cell at room temperature (25°C) for 10 minutes, and the interfacial resistance obtained in the high-frequency region was measured using the Nyquist plot obtained by the EIS measurement method at 50,000 Hz to 0.1 Hz. An electrochemical measuring instrument (potentiostat) (Princeton Applied Research, PARASTAT-MC) was used as the EIS measuring instrument.
[0159] 8. Measurement of maximum resistance change rate (DC resistance) The maximum resistance change rate △R1 is determined by the following equation 1.
[0160] <Expression 1> △R1=Max{(R n+5 / R n ) / 5}
[0161] The aforementioned △R1 is measured using the following method.
[0162] A coin cell for measuring DC resistance (the coin cell used in "6. Method for Measuring DC Resistance" above) is placed in the center of a convection oven (JOTECH, OF3-05W), and the oven temperature is set to increase by 5°C per minute from an initial temperature of 25°C to a final temperature of 135°C. The coin cell is connected to a multimeter for resistance measurement outside the oven (Fluke digital multimeter (FLUKE-87-5)) so that resistance measurement is possible. Subsequently, the DC resistance is measured at each temperature as the temperature increases as set. Specifically, the DC resistance is measured at 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, and 130°C. Each temperature is maintained for one minute according to the set settings, and the DC resistance is measured when one minute has elapsed at that temperature. The DC resistance at each temperature is R in Equation 1. n The DC resistance at a temperature 5°C higher than the temperature in question is given by R in Equation 1. n+5 The DC resistances measured at 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, and 125°C are respectively R n Then, in the temperature range of 25℃ to 130℃, 21 values (R n+5 / R n After calculating ) / 5, the maximum value among them is given by Max{(R n+5 / R n ) / 5}(=△R1), and the maximum value of (R n+5 / R n Set the temperature n°C at ) / 5 to the On-Set temperature.
[0163] 9. Measurement of maximum resistance change rate (AC impedance) The maximum resistance change rate △R2 is determined by the following equation 2.
[0164] <Expression 2> △R² = Max{(R z+5 / R z ) / 5}
[0165] The aforementioned △R2 is measured using the following method.
[0166] A coin cell for measuring AC impedance resistance (the coin cell used in "7. Interface Resistance (AC Impedance Resistance)" above) is placed in the center of a convection oven (JOTECH, OF3-05W), and the oven temperature is set to increase by 5°C per minute from an initial temperature of 25°C to a final temperature of 135°C. The coin cell is connected to an external resistance measuring device (the measuring device used in "7. Interface Resistance (AC Impedance Resistance)" above) so that resistance measurement is possible. Subsequently, the temperature is increased as set, and the AC impedance resistance is measured at each temperature. Specifically, the AC impedance resistance is measured at 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, and 130°C. Each temperature is maintained for one minute according to the set configuration, and the AC impedance resistance is measured after one minute has elapsed at that temperature.
[0167] The AC impedance resistance at each temperature is R in Equation 2 above. z The AC impedance resistance at a temperature 5°C higher than the temperature in question is given by R in equation 2. z+5 The AC impedance resistance measured is R at 25°C, 30°C, 35°C, 40°C, 45°C, 50°C, 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, and 125°C. z Then, in the temperature range of 25℃ to 130℃, 21 values (R z+5 / R z After calculating ) / 5, the maximum value among them is given by Max{(R z+5 / R z) / 5}(=△R2), and the maximum value of (R z+5 / R z Set the temperature z°C at ) / 5 to the On-Set temperature.
[0168] The aforementioned AC impedance resistor was determined by applying a voltage of 4.3V for 10 minutes and obtaining a Nyquist plot using the EIS measurement method at 50,000Hz to 0.1Hz. The resistance was determined to be the semicircle in the high-frequency region.
[0169] Manufacturing Example 1. Synthesis of Monomer (A) The monomer of chemical formula A below was synthesized by the following method.
[0170] [ka]
[0171] 1.372 g (12.02 mmol, 1 eq) of 3-methoxythiophene and 3 g (16.83 mmol, 1.4 eq) of triethylene glycol monomethyl ether were dissolved in 100 ml of toluene with 230 mg of p-toluenesulfonic acid (p-TsOH) and mixed. The mixture was reacted under reflux at 120°C, and methanol produced by the reaction (transetherification) was removed using a soxhlet extractor with a charged 4A type molecular sieve. After refluxing the reaction product for 24 hours, it was quenched with water, extracted with ethyl acetate, washed with brine, and dried on magnesium sulfate (MgSO4). The solvent was removed using a rotary evaporator, and the residue was purified by column chromatography using methylene chloride / hexane (2:1) elution to obtain the target compound (monomer (A)). The NMR analysis results for the target compound (monomer (A)) are shown in Figure 2.
[0172] Manufacturing Example 2. Synthesis of conductive polymer (polythiophene(A)) Polythiophene (A) was prepared by dissolving 3.20 g (19.71 mmol, 3 eq) of iron(III) chloride in 150 ml of methylene chloride, then adding 1 g (3.94 mmol, 0.6 eq) of 3-dodecylthiophene, 0.33 g (1.97 mmol, 0.3 eq) of 3-hexylthiophene, and 0.16 g (0.66 mmol, 0.1 eq) of monomer (A) from Production Example 1, and polymerizing at 30°C for 24 hours. In conductive polymer (A), the molar ratio of 3-dodecylthiophene units (I), 3-hexylthiophene units (II), and monomer (A) units (III) from Production Example 1 is approximately 3.94:1.97:0.66 (I:II:III).
[0173] The polymerization solution was placed in a permeable membrane with a molecular weight of cut-off (MWCO) of 5000, and then immersed in 200 ml of acetonitrile solvent to remove unreacted iron(III) chloride, monomers, and low molecular weight oligomers. The residue precipitated inside the permeable membrane was washed with methanol and dried at 60°C for 12 hours to obtain polythiophene (A).
[0174] Polythiophene (A) had a weight-average molecular weight (Mw) and a number-average molecular weight (Mn) of 118,000 g / mol and 24,500 g / mol, respectively, and an oxidation potential of approximately 3.7 V.
[0175] Example 1. An aluminum foil with a thickness of approximately 15 μm was used as the current collector. A coating solution was prepared by dispersing polythiophene (A) from Production Example 2 in a solvent (Chloroform) at a concentration of approximately 2.0% by weight. The coating solution was then coated onto the current collector using a bar coating method. Subsequently, the current collector with the coated layer was maintained in a drying oven at 140°C for about 4 minutes, and then maintained again at approximately 130°C for 1 hour to form a layer (polymer layer) with a thickness of approximately 200 nm.
[0176] Next, an active material layer was formed on the conductive polymer layer. The active material layer was formed using a slurry. The slurry was prepared by blending positive electrode active material, conductive material (ECP (Ketjen Black) 0.5%, SFG (Trimrex graphite) 0.4%, DB (Denka Black) 0.4%), PVDF (poly(vinylidene fluoride)), and NMP (N-Methyl-2-pyrrolidone) in a weight ratio of 75:1:1:23 (electrode active material: conductive material: PVDF: NMP). The slurry was applied to the conductive polymer layer with a doctor blade, dried at room temperature, maintained in a drying oven at 130°C for about 30 minutes, and then rolled to form an active material layer with a thickness of approximately 53 μm (based on an electrode active material weight of 0.03 g and a porosity of 18%).
[0177] As described above, LCO (LiCoO2) was used as the electrode active material, and the oxidation potential of the electrode active material measured using the method described in "5. Method for measuring oxidation potential (electrode active material)" was approximately 3.8V.
[0178] Comparative Example 1. When forming an active material layer on a conductive polymer layer, NCM(Li[N 0.8 Co 0.1 Mn 0.1 The electrodes were manufactured in the same manner as in Example 1, except that 2O2 was used. The oxidation potential of the electrode active material (NCM), measured using the method described in "5. Method for Measuring Oxidation Potential (Electrode Active Material)," was approximately 3.7V.
[0179] Test Example 1: Charge / Discharge Test Charge and discharge tests were performed using fabricated coin cells. The coin cells were fabricated using a CR2032 standard coin cell kit (Wellcos CR2032 coin cell kit). The electrodes fabricated in the examples or comparative examples were used as the positive electrode, and a lithium film (thickness: approximately 100 μm) was used as the negative electrode. The electrolyte used was a 1M LiPF6 solution from Enchem (solvent: EC / DMC / EMC = 3 / 4 / 3 (mass ratio), EC: ethylene carbonate, DMC: dimethyl carbonate, EMC: ethyl methyl carbonate), and the separation membrane used was a PE (poly(ethylene)) separation membrane (Double Scope Korea, WL20C model).
[0180] A charge-discharge test was conducted using the aforementioned coin cell. The test was performed over six cycles using a constant current-constant voltage (CC-CV) method, in the following order: 0.1C charge / 0.1C discharge (1 cycle), 0.2C charge / 0.2C discharge (2 cycles), 0.5C charge / 0.1C discharge (3 cycles), 0.5C charge / 0.5C discharge (4 cycles), 0.5C charge / 1C discharge (5 cycles), and 0.5C charge / 2C discharge (6 cycles).
[0181] Figures 3 and 4 show the charge-discharge curves performed on the electrode of Example 1, while Figures 5 and 6 show the charge-discharge curves resulting from the charge-discharge test performed using the electrode of Comparative Example 1.
[0182] In Figures 3 and 4, LCO(Ref) represents the charge-discharge curve from a charge-discharge test performed on an electrode manufactured using the same method as in Example 1, but without forming a conductive polymer layer, while LCO(SFL) represents the charge-discharge curve from a charge-discharge test performed on an electrode containing the current collector layer, conductive polymer layer, and active material layer manufactured in Example 1.
[0183] In Figures 5 and 6, NCM(Ref) represents the charge-discharge curve from a charge-discharge test performed on an electrode manufactured using the same method as Comparative Example 1, but without forming a conductive polymer layer, while NCM(SFL) represents the charge-discharge curve from a charge-discharge test performed on an electrode containing a current collector layer, a conductive polymer layer, and an active material layer manufactured in Comparative Example 1.
[0184] From a comparison of the drawings, it can be confirmed that in Example 1, where the oxidation potential of the conductive polymer in the conductive polymer layer (polymer layer) is lower than that of the electrode active material, the efficiency did not decrease after charging and discharging. However, in Comparative Example 1, the efficiency of the coin cell decreased after charging and discharging.
[0185] Test Example 2. PTC Efficacy Test The DC resistance, interfacial resistance, ΔR1, on-set temperature relative to ΔR1, ΔR2, and on-set temperature relative to ΔR2 were evaluated for the electrode of Example 1 among the manufactured electrodes, and the results are shown in Table 1 below.
[0186] In Table 1 below, Ref. represents the result when manufacturing coin cells to evaluate the DC resistance, interfacial resistance, ΔR1, on-set temperature for ΔR1, ΔR2, and on-set temperature for ΔR2, while only the polymer layer formation conditions were changed, and all other conditions were the same as in Example 1.
[0187] Specifically, in Table 1 below, the results for Example 1 are for a coin cell containing a polymer layer formed by coating a current collector (Al foil) with a coating solution prepared by dispersing polythiophene (A) from Production Example 2 in a solvent (Chloroform) at a concentration of approximately 2.0% by weight using a bar coating method, maintaining the current collector with the coated layer in a drying oven at 140°C for about 4 minutes, and then maintaining it at approximately 130°C for 1 hour. Ref. is the result for a coin cell containing a polymer layer formed by coating the same current collector (Al foil) with the same coating solution using a bar coating method, and maintaining the current collector with the coated layer in a drying oven at 90°C for about 20 minutes.
[0188] [Table 1]
[0189] Table 1 shows that a PTC (Positive Temperature Coefficient) effect designed to suit the purpose can be obtained through the application of specific conductive polymers, and that the PTC effect can be further controlled by the formation method even when the same conductive polymer is applied.
Claims
1. Current collector; An active material layer formed on the current collector, containing an electrode active material; and The current collector and the active material layer have a polymer layer containing a conductive polymer, An electrode in which the oxidation potential of the conductive polymer or polymer layer is lower than the oxidation potential of the electrode active material or active material layer.
2. The electrode according to claim 1, wherein RV in the following formula 1 exceeds 100: [Formula 1] RV=100×Va / Vs In Equation 1, Va is the oxidation potential of the electrode active material or the active material layer, and Vs is the oxidation potential of the conductive polymer or the polymer layer.
3. The electrode according to claim 2, wherein the oxidation potential Va is in the range of 2V to 5V.
4. The electrode according to claim 2, wherein the oxidation potential Vs is in the range of 0V to 5V.
5. The electrode according to claim 1, wherein the polymer layer has a DC resistance of 10,000 Ω·cm or less at 25°C.
6. The electrode according to claim 1, wherein the polymer layer has an AC impedance resistance of 1,000 Ω or less.
7. The electrode according to claim 1, wherein ΔR1 in the following equation 2 is 100 Ω·cm / ℃ or more: [Formula 2] △R1=Max{(R n+5 / R n ) / 5} In equation 2, R n R is the DC resistance of the polymer layer at any temperature n°C within the range of 25°C to 135°C. n+5 This is the DC resistance of the polymer layer at a temperature 5°C higher than the aforementioned temperature n°C ((n+5)°C), and Max { (R n+5 / R n ) / 5} was confirmed within the temperature range of 25°C to 135°C (R n+5 / R n ) / This is the maximum value among the five values.
8. The electrode according to claim 7, wherein the temperature at which a ΔR1 of 100 Ω·cm / ℃ or more is confirmed is 80℃ or higher.
9. The electrode according to claim 1, wherein ΔR2 in the following equation 3 is 10 Ω / °C or greater: [Formula 3] △R2=Max{(R z+5 / R z ) / 5} In equation 2, R z R is the AC impedance resistance of the polymer layer at any temperature n°C within the range of 25°C to 135°C. z+5 This is the AC impedance resistance of the polymer layer at a temperature 5°C higher than the aforementioned temperature n°C ((n+5)°C), and Max { (R z+5 / R z ) / 5} was confirmed within the temperature range of 25°C to 135°C (R z+5 / R z ) / This is the maximum value among the five values.
10. The electrode according to claim 9, wherein the temperature at which a ΔR2 of 10 Ω / °C or more is confirmed is 80°C or higher.
11. The electrode according to claim 1, wherein the conductive polymer is a polythiophene containing thiophene units having hydrocarbon functional groups.
12. The electrode according to claim 11, wherein the polythiophene comprises, as thiophene units, a first thiophene unit having a hydrocarbon functional group having 10 or more carbon atoms and a second thiophene unit having a hydrocarbon functional group having 9 or fewer carbon atoms.
13. The electrode according to claim 11, wherein the polythiophene contains 30 mol% or more of thiophene units having a hydrocarbon functional group.
14. The electrode according to claim 12, wherein the ratio M2 / M1 of the number of moles M2 of the second thiophene unit to the number of moles M1 of the first thiophene unit is in the range of 0.01 to 100.
15. The electrode according to claim 11, wherein the polythiophene further comprises thiophene units having polar functional groups.
16. The electrode according to claim 15, wherein the polythiophene comprises 1 to 500 moles of hydrocarbon functional groups per mole of polar functional group thiophene units.
17. The system includes a positive electrode, a negative electrode, and a separation membrane between the positive and negative electrodes. An electrode assembly in which the positive electrode or negative electrode is an electrode according to any one of claims 1 to 16.
18. A secondary battery comprising the electrode assembly described in claim 17.