Adhesive composition, adhesive film, and surface protective film for polarizing plates

The surface protective film with a crosslinked adhesive composition balances adhesive strength and antistatic properties, addressing the challenges of conventional films by ensuring easy peeling and reworkability while preventing residue.

JP2026183005APending Publication Date: 2026-11-19ZACROS CORP
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
JP2026202915
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2026-09-09
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional surface protective films for optical components in liquid crystal displays struggle to simultaneously balance adhesive strength in low-speed and high-speed peeling regions, prevent adhesive residue, exhibit excellent antistatic performance, and ensure reworkability, despite individual performances being achievable in prior art.

Method used

A surface protective film with an adhesive layer formed by crosslinking an adhesive composition containing specific monomers, a trifunctional isocyanate compound, crosslinking retarder, crosslinking catalyst, antistatic agent, and polyether-modified siloxane compound, achieving balanced adhesive strength and antistatic properties.

Benefits of technology

The film achieves excellent antistatic performance, prevents adhesive residue, and ensures easy peeling with minimal force, maintaining adhesive strength consistency across peeling speeds, and enhances durability and reworkability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026183005000001
    Figure 2026183005000001
  • Figure 2026183005000002
    Figure 2026183005000002
  • Figure 2026183005000003
    Figure 2026183005000003
Patent Text Reader

Abstract

The present invention provides an adhesive composition, adhesive film, and surface protective film for polarizing plates that possess antistatic properties, have an excellent balance of adhesive strength between low-speed and high-speed peeling regions, and further exhibit excellent durability, reworkability, and antistatic properties. [Solution] An adhesive composition comprising (A) a (meth)acrylic acid ester monomer having C4 to C10 C atoms in the alkyl group, (B) a copolymerizable monomer containing a hydroxyl group, (C) a copolymerizable monomer containing a carboxyl group, and (D) a copolymer containing a polyalkylene glycol mono(meth)acrylic acid ester monomer, further comprising (E) a trifunctional or more isocyanate compound, (H) an antistatic agent, and (I) a polyether-modified siloxane compound, wherein the weight ratios are (A) 100 to (B) 0.1 to 5.0, (C) 0.35 to 1.0, (D) 1 to 20, and (E) 0.5 to 5.0 and (I) 0.01 to 0.5 per 100 copolymer.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a surface protection film used in the manufacturing process of liquid crystal displays. More specifically, it relates to a surface protection film used to protect the surface of optical components such as polarizing plates and phase difference plates that constitute liquid crystal displays by being attached to the surface of such optical components. [Background technology]

[0002] Conventionally, in the manufacturing process of optical components such as polarizers and phase difference plates, which are components of liquid crystal displays, a surface protection film is applied to temporarily protect the surface of the optical components. Such surface protection films are used only in the manufacturing process of the optical components and are peeled off and removed when the optical components are assembled into the liquid crystal display. Because such surface protection films for protecting the surface of optical components are used only in the manufacturing process, they are sometimes commonly referred to as process films.

[0003] In the process of manufacturing optical components, the surface protection film used is an optically transparent polyethylene terephthalate (PET) resin film with an adhesive layer formed on one side. However, a release film, which has been treated to protect the adhesive layer, is laminated on top of the adhesive layer until it is bonded to the optical component. Furthermore, optical components such as polarizing plates and phase difference plates undergo product inspections that include optical evaluations of the liquid crystal display's display capability, hue, contrast, and foreign matter contamination while the surface protective film is attached. Therefore, the required performance of the surface protective film is that the adhesive layer is free of air bubbles and foreign matter. Furthermore, in recent years, there have been concerns that the static electricity generated when peeling the adhesive layer off optical components such as polarizing plates and phase difference plates may affect the electrical control circuits of liquid crystal displays, leading to a demand for adhesive layers with superior antistatic properties. Furthermore, when bonding surface protective films to optical components such as polarizers and phase difference plates, it is sometimes necessary to peel off the surface protective film and reapply it for various reasons. In such cases, ease of removal from the optical component (reworkability) is required. Furthermore, when the surface protective film is finally peeled off from optical components such as polarizers and phase difference plates, it is required that it can be peeled off quickly. In other words, even with high-speed peeling, it is required that the adhesive strength does not change much with the peeling speed so that it can be peeled off quickly.

[0004] Thus, in recent years, the required performance of the adhesive layer constituting surface protective films has been to include (1) balancing adhesive strength in the low-speed and high-speed peeling regions, (2) preventing the generation of adhesive residue, (3) excellent antistatic performance, and (4) reworkability, all of which are desirable in terms of ease of use when using surface protective films. However, while it was possible to satisfy each of the individual performance requirements (1) to (4) for the adhesive layer constituting the surface protective film, simultaneously satisfying all of the performance requirements (1) to (4) for the adhesive layer of the surface protective film was an extremely difficult challenge.

[0005] For example, the following suggestions are known regarding (1) balancing the adhesive strength in the low-speed peeling region and the high-speed peeling region, and (2) preventing the generation of adhesive residue.

[0006] Acrylic adhesive layers, primarily composed of a copolymer of an alkyl (meth)acrylate having an alkyl group with 7 or fewer carbon atoms and a copolymerizable compound containing a carboxyl group, and crosslinked with a crosslinking agent, have the problem that the adhesive transfers to the adherend when bonded for a long period of time, and that the adhesive strength to the adherend increases significantly over time. To avoid this, an adhesive layer is known in which a copolymer of an alkyl (meth)acrylate having an alkyl group with 8 to 10 carbon atoms and a copolymerizable compound having an alcoholic hydroxyl group is used, and this copolymer is crosslinked with a crosslinking agent (Patent Document 1). Furthermore, it has been proposed that a small amount of copolymer of (meth)acrylate alkyl ester and a carboxyl group-containing copolymerizable compound is added to the copolymer similar to the above, and that this copolymer is crosslinked with a crosslinking agent to form an adhesive layer. However, when these are used for surface protection of plastic sheets with low surface tension and smooth surfaces, problems such as peeling due to heating during processing or storage, and poor re-peelability when peeled off at high speeds, which is the domain of manual work, have been reported.

[0007] To solve these problems, an adhesive composition has been proposed in which a copolymer of monomer mixtures is obtained by adding 100 parts by weight of an alkyl (meth)acrylate mainly composed of an alkyl (meth)acrylate having an alkyl group having 8 to 10 carbon atoms, 1 to 15 parts by weight of a copolymerizable compound containing a carboxyl group, and 3 to 100 parts by weight of a vinyl ester of an aliphatic carboxylic acid having 1 to 5 carbon atoms, and a crosslinking agent in an amount equivalent to or greater than the carboxyl group of component b) above is added (Patent Document 2). The adhesive composition described in Patent Document 2 does not exhibit peeling phenomena such as lifting during processing or storage, and furthermore, it has a small increase in adhesive strength over time and excellent re-peelability, and can be re-peeled with little force even after long-term storage, especially in a high-temperature atmosphere, without leaving any adhesive residue on the adherend, and can also be re-peeled with little force even when peeled at high speed.

[0008] Furthermore, (3) regarding excellent antistatic performance, methods for imparting antistatic properties to a surface protective film include kneading an antistatic agent into the base film, and examples of antistatic agents disclosed include (a) various cationic antistatic agents having cationic groups such as quaternary ammonium salts, pyridinium salts, and primary to tertiary amino groups, (b) anionic antistatic agents having anionic groups such as sulfonic acid bases, sulfate ester bases, phosphate ester bases, and phosphonic acid bases, (c) amphoteric antistatic agents such as amino acid-based and aminosulfate ester-based agents, (d) nonionic antistatic agents such as amino alcohol-based, glycerin-based, and polyethylene glycol-based agents, and (e) polymer-type antistatic agents with high molecular weights, such as the above-mentioned antistatic agents (Patent Document 3). Furthermore, in recent years, it has been proposed to incorporate such antistatic agents into the base film, or to directly incorporate them into the adhesive layer rather than applying them to the surface of the base film.

[0009] Furthermore, (4) Regarding rework performance, for example, an adhesive composition has been proposed in which an isocyanate compound curing agent and a specific silicate oligomer are blended in an acrylic resin at a concentration of 0.0001 to 10 parts by weight per 100 parts by weight of the acrylic resin (Patent Document 4). Patent Document 4 states that the main monomer component may be an alkyl acrylate with an alkyl group having 2 to 12 carbon atoms, or an alkyl methacrylate with an alkyl group having 4 to 12 carbon atoms, and that other functional group-containing monomer components, such as a carboxyl group-containing monomer, may also be included. Generally, it is preferable to contain 50% by weight or more of the above main monomer, and it is desirable that the content of the functional group-containing monomer component be 0.001 to 50% by weight, preferably 0.001 to 25% by weight, and more preferably 0.01 to 25% by weight. The adhesive composition described in Patent Document 4 is said to have reworkability because it exhibits little change in cohesive force and adhesive force over time even at high temperatures or high temperature and high humidity, and also shows excellent effect on curved surface adhesion. In general, when the pressure-sensitive adhesive layer is made to have a soft property, adhesive residue tends to occur easily, and reworkability tends to deteriorate. That is, when bonded by mistake, it is difficult to peel off, and re-bonding tends to be difficult. For this reason, it is considered necessary to crosslink a monomer having a functional group such as a carboxyl group with the main agent to make the pressure-sensitive adhesive layer have a certain hardness in order to impart reworkability.

Prior Art Document

Patent Document

[0010]

Patent Document 1

Patent Document 2

Patent Document 3

Patent Document 4

Summary of Invention

Problem to be Solved by the Invention

[0011] In the prior art, as the required performance for the pressure-sensitive adhesive layer constituting the surface protective film, balancing the adhesive force between the low-speed peeling region and the high-speed peeling region, excellent antistatic performance, rework performance and the like have been demanded. However, although individual required performances could be satisfied respectively, it was not possible to satisfy all the required performances demanded for the pressure-sensitive adhesive layer of the surface protective film.

[0012] The present invention has been made in view of the above circumstances, and an object of the present invention is to provide a surface protective film that has antistatic performance, has an excellent balance of adhesive force between a low-speed peeling region and a high-speed peeling region, and is further excellent in durability, reworkability and antistatic property.

Means for Solving the Problem

[0013] To solve the above problems, the present invention provides a surface protective film comprising a surface protective film formed on one side of a resin film, wherein the adhesive layer is formed by crosslinking an adhesive composition containing an acrylic copolymer, an antistatic agent, and a crosslinking agent, and the acrylic copolymer is formed by copolymerizing (A) 100 parts by weight of one or more (meth)acrylic acid ester monomers having C4 to C10 alkyl groups, (B) 0.1 to 5.0 parts by weight of one or more copolymerizable monomers containing hydroxyl groups, (C) 0.35 to 1.0 parts by weight of one or more copolymerizable monomers containing carboxyl groups, and (D) 1 to 20 parts by weight of one or more polyalkylene glycol mono(meth)acrylic acid ester monomers. The present invention provides a surface protection film comprising a copolymer, wherein the adhesive composition contains (E) a trifunctional or greater isocyanate compound, (F) a crosslinking retarder, (G) a crosslinking catalyst, (H) an antistatic agent, and (I) a polyether-modified siloxane compound having an HLB value of 7 to 12, wherein the adhesive composition contains 0.5 to 5.0 parts by weight of the (E) trifunctional or greater isocyanate compound per 100 parts by weight of the acrylic copolymer, and the adhesive layer has an adhesive strength of 0.05 to 0.1 N / 25 mm in the low-speed peeling region of 0.3 m / min and an adhesive strength of 1.0 N / 25 mm or less in the high-speed peeling region of 30 m / min.

[0014] Preferably, the copolymerizable monomer containing the hydroxyl group (B) is at least one selected from the group of compounds consisting of 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, N-hydroxy(meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-hydroxyethyl (meth)acrylamide, and the total amount of 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate from the copolymerizable monomer containing the hydroxyl group (B) is 0 to 0.9 parts by weight per 100 parts by weight of the (meth)acrylic acid ester monomer having C4 to C10 carbon atoms in the alkyl group (A) (meth)acrylate (B) (it is also acceptable if 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate are not included).

[0015] Preferably, the copolymerizable monomer containing the (C) carboxyl group is at least one selected from the group of compounds consisting of (meth)acrylic acid, carboxyethyl (meth)acrylate, and carboxypentyl (meth)acrylate.

[0016] Preferably, the (D) polyalkylene glycol mono(meth)acrylic acid ester monomer is at least one selected from the group of compounds consisting of polyalkylene glycol mono(meth)acrylate, methoxypolyalkylene glycol (meth)acrylate, and ethoxypolyalkylene glycol (meth)acrylate.

[0017] It is preferable that the (E) isocyanate compound with three or more functions is selected from the group of compounds consisting of isocyanurate forms of hexamethylene diisocyanate compounds, isocyanurate forms of isophorone diisocyanate compounds, adduct forms of hexamethylene diisocyanate compounds, adduct forms of isophorone diisocyanate compounds, burette forms of hexamethylene diisocyanate compounds, and burette forms of isophorone diisocyanate compounds, and at least one of these compounds.

[0018] It is preferable that the (H) antistatic agent is an ionic compound with a melting point of 30 to 80°C, contained in an amount of 0.1 to 5.0 parts by weight per 100 parts by weight of the copolymer, or a quaternary ammonium salt type acrylic monomer with a melting point of 30 to 80°C copolymerized in an amount of 0.1 to 5.0% by weight in the copolymer.

[0019] The (I) polyether-modified siloxane compound is a polyether-modified siloxane compound having an HLB value of 7 to 12, and it is preferable that the (I) polyether-modified siloxane compound is present in an amount of 0.01 to 0.5 parts by weight per 100 parts by weight of the copolymer.

[0020] The (F) crosslinking retarder is preferably a ketoenol tautomer compound, and the (F) crosslinking retarder is preferably present in an amount of 1.0 to 5.0 parts by weight per 100 parts by weight of the copolymer.

[0021] The (G) crosslinking catalyst is preferably an organotin compound, and preferably the (G) crosslinking catalyst is present in an amount of 0.01 to 0.5 parts by weight per 100 parts by weight of the copolymer.

[0022] Preferably, the adhesive layer formed by crosslinking the aforementioned adhesive composition has an adhesive strength of 0.05 to 0.1 N / 25 mm in the low-speed peeling region of 0.3 m / min and an adhesive strength of 1.0 N / 25 mm or less in the high-speed peeling region of 30 m / min.

[0023] The adhesive layer formed by crosslinking the aforementioned adhesive composition has a surface resistance value of 5.0 × 10+10 It is preferable that the impedance is Ω / □ or less and the stripping band voltage is ±0 to 1kV.

[0024] Furthermore, the present invention provides an adhesive film characterized by having an adhesive layer formed on one or both sides of a resin film, which is obtained by crosslinking the above-mentioned adhesive composition.

[0025] Furthermore, the present invention provides a surface protection film comprising an adhesive layer formed on one side of a resin film by crosslinking the above-mentioned adhesive composition, characterized in that there is no contamination transfer to the adherend after tracing over the surface protection film with a ballpoint pen via the adhesive layer.

[0026] The aforementioned surface protection film can be used as a surface protection film for polarizing plates.

[0027] Preferably, the side of the resin film opposite to the side on which the adhesive layer is formed is treated with an antistatic and anti-fouling coating. [Effects of the Invention]

[0028] According to the present invention, it is possible to satisfy all the performance requirements for the adhesive layer of a surface protective film, which could not be solved with conventional technology, and to obtain excellent antistatic performance and adhesive residue prevention performance. Specifically, it is possible to reduce the amount of antistatic agent added while maintaining antistatic performance, and to further improve adhesive residue prevention performance. [Modes for carrying out the invention]

[0029] The present invention will be described below based on preferred embodiments. The adhesive composition of the present invention is characterized in that its main component comprises (A) a (meth)acrylic acid ester monomer having C4 to C10 C atoms in the alkyl group, (B) a copolymerizable monomer containing a hydroxyl group, (C) a copolymerizable monomer containing a carboxyl group, and (D) a copolymer containing a polyalkylene glycol mono(meth)acrylic acid ester monomer, and further comprises (E) a trifunctional or more isocyanate compound, (F) a crosslinking retarder, (G) a crosslinking catalyst, (H) an antistatic agent, and (I) a polyether-modified siloxane compound.

[0030] (A) Examples of (meth)acrylic acid ester monomers having C4 to C10 carbon atoms in the alkyl group include butyl (meth)acrylate, isobutyl (meth)acrylate, pentyl (meth)acrylate, hexyl (meth)acrylate, heptyl (meth)acrylate, octyl (meth)acrylate, isooctyl (meth)acrylate, 2-ethylhexyl (meth)acrylate, nonyl (meth)acrylate, isononyl (meth)acrylate, and decyl (meth)acrylate.

[0031] (B) Examples of copolymerizable monomers containing hydroxyl groups include hydroxyalkyl (meth)acrylates such as 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, and 2-hydroxyethyl (meth)acrylate, as well as hydroxyl group-containing (meth)acrylamides such as N-hydroxy (meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-hydroxyethyl (meth)acrylamide. Preferably, it is at least one compound selected from the group consisting of 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, 4-hydroxybutyl (meth)acrylate, 2-hydroxyethyl (meth)acrylate, N-hydroxy(meth)acrylamide, N-hydroxymethyl (meth)acrylamide, and N-hydroxyethyl (meth)acrylamide. (A) Preferably, the copolymerizable monomer containing a hydroxyl group (B) is included in 0.1 to 5.0 parts by weight per 100 parts by weight of (meth)acrylic acid ester monomer having C4 to C10 in the alkyl group. Furthermore, (B) of the copolymerizable monomers containing hydroxyl groups, the total amount of 8-hydroxyoctyl (meth)acrylate, 6-hydroxyhexyl (meth)acrylate, and 4-hydroxybutyl (meth)acrylate is preferably less than 1 part by weight (it is also acceptable if they are not included), and preferably 0 to 0.9 parts by weight.

[0032] (C) Preferably, the copolymerizable monomer containing a carboxyl group is at least one selected from the group of compounds consisting of (meth)acrylic acid, carboxyethyl (meth)acrylate, and carboxypentyl (meth)acrylate. (A) Preferably, the mixture contains 0.35 to 1.0 parts by weight of copolymerizable monomer containing a carboxyl group per 100 parts by weight of (meth)acrylic acid ester monomer having C4 to C10 in the alkyl group.

[0033] (D) The polyalkylene glycol mono(meth)acrylic acid ester monomer can be any compound in which one of the multiple hydroxyl groups of the polyalkylene glycol is esterified as a (meth)acrylic acid ester. Since the (meth)acrylic acid ester group is a polymerizable group, it can be copolymerized with the main polymer. The other hydroxyl groups may remain as OH groups, or they may be alkyl ethers such as methyl ether or ethyl ether, or saturated carboxylic acid esters such as acetate esters, etc. The alkylene groups in polyalkylene glycol include, but are not limited to, ethylene groups, propylene groups, and butylene groups. The polyalkylene glycol may be a copolymer of two or more polyalkylene glycols, such as polyethylene glycol, polypropylene glycol, and polybutylene glycol. Examples of polyalkylene glycol copolymers include polyethylene glycol-polypropylene glycol, polyethylene glycol-polybutylene glycol, polypropylene glycol-polybutylene glycol, and polyethylene glycol-polypropylene glycol-polybutylene glycol, and the copolymer may be a block copolymer or a random copolymer.

[0034] (D) The polyalkylene glycol mono(meth)acrylic acid ester monomer is preferably at least one selected from the group of compounds consisting of polyalkylene glycol mono(meth)acrylate, methoxypolyalkylene glycol (meth)acrylate, and ethoxypolyalkylene glycol (meth)acrylate. More specifically, polyethylene glycol-mono(meth)acrylate, polypropylene glycol-mono(meth)acrylate, polybutylene glycol-mono(meth)acrylate, polyethylene glycol-polypropylene glycol-mono(meth)acrylate, polyethylene glycol-polybutylene glycol-mono(meth)acrylate, polypropylene glycol-polybutylene glycol-mono(meth)acrylate, polyethylene glycol-polypropylene glycol-polybutylene glycol-mono(meth)acrylate; methoxypolyethylene glycol-(meth)acrylate, methoxypolypropylene glycol-(meth)acrylate, methoxypolybutylene glycol-(meth)acrylate, methoxypolyethylene glycol Examples include polybutylene glycol-(meth)acrylate, methoxy-polypropylene glycol-polybutylene glycol-(meth)acrylate, methoxy-polyethylene glycol-polypropylene glycol-polybutylene glycol-(meth)acrylate; ethoxypolyethylene glycol-(meth)acrylate, ethoxypolypropylene glycol-(meth)acrylate, ethoxypolybutylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polypropylene glycol-(meth)acrylate, ethoxy-polyethylene glycol-polybutylene glycol-(meth)acrylate, ethoxy-polypropylene glycol-polybutylene glycol-(meth)acrylate, and ethoxypolyethylene glycol-polypropylene glycol-polybutylene glycol-(meth)acrylate. (A) Preferably, the mixture contains 1 to 20 parts by weight of (D) polyalkylene glycol mono(meth)acrylic acid monomer per 100 parts by weight of (meth)acrylic acid monomer having C4 to C10 in the alkyl group.

[0035] (E) As isocyanate compounds with three or more functions, any polyisocyanate compound having at least three isocyanate (NCO) groups in one molecule is acceptable, and examples include biuret-modified and isocyanurate-modified diisocyanates (compounds having two NCO groups in one molecule) such as hexamethylene diisocyanate, isophorone diisocyanate, diphenylmethane diisocyanate, tolylene diisocyanate, and xylylene diisocyanate, as well as adducts (polyol-modified) with trivalent or higher polyols (compounds having at least three OH groups in one molecule) such as trimethylolpropane and glycerin. (E) The isocyanate compound with three or more functions is a polyisocyanate compound having at least three isocyanate (NCO) groups in one molecule, and it is preferable that it is at least one selected from the group of compounds consisting of isocyanurate forms of hexamethylene diisocyanate compounds, isocyanurate forms of isophorone diisocyanate compounds, adduct forms of hexamethylene diisocyanate compounds, adduct forms of isophorone diisocyanate compounds, burette forms of hexamethylene diisocyanate compounds, and burette forms of isophorone diisocyanate compounds. (E) The isocyanate compound with three or more functions is preferably contained in an amount of 0.5 to 5.0 parts by weight per 100 parts by weight of the copolymer.

[0036] (F) Examples of crosslinking retarders include β-ketoesters such as methyl acetoacetate, ethyl acetoacetate, octyl acetoacetate, oleyl acetoacetate, lauryl acetoacetate, and stearyl acetoacetate, as well as β-diketones such as acetylacetone, 2,4-hexanedione, and benzoylacetone. These are ketoenol tautomer compounds, and in adhesive compositions using polyisocyanate compounds as crosslinking agents, they block the isocyanate groups of the crosslinking agent, thereby suppressing excessive viscosity increase and gelation of the adhesive composition after the addition of the crosslinking agent, and extending the pot life of the adhesive composition. (F) The crosslinking retarder is preferably a ketoenol tautomer compound, and more preferably at least one selected from the group of compounds consisting of acetylacetone and acetateethyl. (F) The crosslinking retarder is preferably present in an amount of 1.0 to 5.0 parts by weight per 100 parts by weight of the copolymer.

[0037] (G) The crosslinking catalyst can be any substance that functions as a catalyst for the reaction (crosslinking reaction) between the copolymer and the crosslinking agent when a polyisocyanate compound is used as the crosslinking agent, and examples include amine compounds such as tertiary amines, organotin compounds, organolead compounds, organozinc compounds and other organometallic compounds. Examples of tertiary amines include trialkylamines, N,N,N',N'-tetraalkyldiamines, N,N-dialkylamino alcohols, triethylenediamines, morpholine derivatives, and piperazine derivatives. Examples of organotin compounds include dialkyltin oxides, fatty acid salts of dialkyltin, and fatty acid salts of stannous tin. (G) The crosslinking catalyst is preferably an organotin compound, and more preferably at least one selected from the group of compounds consisting of dioctyl tin oxide and dioctyl tin dilaurate. (G) The crosslinking catalyst is preferably present in an amount of 0.01 to 0.5 parts by weight per 100 parts by weight of the copolymer.

[0038] (H) The antistatic agent is preferably solid at room temperature (e.g., 30°C), and more specifically, it is preferably an ionic compound with a melting point of 30 to 80°C, contained in an amount of 0.1 to 5.0 parts by weight per 100 parts by weight of the copolymer, or a quaternary ammonium salt type acrylic monomer with a melting point of 30 to 80°C copolymerized in the copolymer at an amount of 0.1 to 5.0% by weight. In the present invention, as the (H) antistatic agent, (H1) an ionic compound with a melting point of 30 to 80°C is added to the copolymer, or (H2) a quaternary ammonium salt type acrylic monomer with a melting point of 30 to 80°C is copolymerized into the copolymer. These (H) antistatic agents are presumed to have high affinity with acrylic copolymers because they have low melting points and long-chain alkyl groups.

[0039] (H1) Ionic compounds with a melting point of 30-80°C include ionic compounds having a cation and anion, wherein the cation is a nitrogen-containing onium cation such as pyridinium cation, imidazolium cation, pyrimidinium cation, pyrazolium cation, pyrrolidinium cation, ammonium cation, phosphonium cation, sulfonium cation, etc., and the anion is hexafluoride phosphate (PF6) - ), thiocyanate (SCN - ), alkylbenzene sulfonate (RC6H4SO3 - ), perchlorate (ClO4 - ), tetrafluoroborate (BF4 - Examples include inorganic or organic anion compounds such as ). By selecting the chain length of the alkyl group, the position and number of substituents, compounds with a melting point of 30 to 80°C can be obtained. The cation is preferably a quaternary nitrogen-containing onium cation, and examples include quaternary pyridinium cations such as 1-alkylpyridinium (the carbon atoms at positions 2 to 6 may have substituents or be unsubstituted), quaternary imidazolium cations such as 1,3-dialkylimidazolium (the carbon atoms at positions 2, 4, and 5 may have substituents or be unsubstituted), and quaternary ammonium cations such as tetraalkylammonium.

[0040] (H2) Examples of the quaternary ammonium salt type acrylic monomer having a melting point of 30 to 80°C include ionic compounds having a cation and an anion, where the cation is a (meth)acryloyloxyalkyltrialkylammonium [R₃N + -C n H 2n -OCOCQ=CH₂, where Q=H or CH₃, R=alkyl] or other (meth)acrylic group-containing quaternary ammonium, and the anion is an inorganic or organic anion such as hexafluorophosphate (PF₆ - ), thiocyanate (SCN - ), organic sulfonate (RSO₃ - ), perchlorate (ClO₄ - ), tetrafluoroborate (BF₄ - ) and the like. (H) Specific examples of the antistatic agent are not particularly limited, and include 1-octylpyridinium hexafluorophosphate, 1-nonylpyridinium hexafluorophosphate, 2-methyl-1-dodecylpyridinium hexafluorophosphate, 1-octylpyridinium dodecylbenzenesulfonate, 1-dodecylpyridinium thiocyanate, 1-dodecylpyridinium dodecylbenzenesulfonate, 4-methyl-1-octylpyridinium hexafluorophosphate, dimethylaminomethyl acrylate methyl hexafluorophosphate salt [(CH₃)₃N + CH₂OCOCH=CH₂·PF₆ - and the like.

[0041] (I) The polyether-modified siloxane compound is a siloxane compound having a polyether group, and in addition to the usual siloxane unit [-SiR 1 ₂-O-], it has a siloxane unit having a polyether group [-SiR 1 (R 2 O(R 3 O) n R 4 )-O-]. Here, R 1 is one or more alkyl groups or aryl groups, R 2 and R 3 are one or more alkylene groups, R 4This represents one or more alkyl groups or acyl groups (terminal groups). Examples of polyether groups include polyoxyethylene groups [(C2H4O)] n ] or polyoxypropylene group [(C3H6O) n Examples of polyoxyalkylene groups include the following: (I) The polyether-modified siloxane compound is a polyether-modified siloxane compound having an HLB value of 7 to 12, and it is preferable that the (I) polyether-modified siloxane compound is present in an amount of 0.01 to 0.5 parts by weight per 100 parts by weight of the copolymer. More preferably, it is 0.1 to 0.5 parts by weight. HLB refers to the hydrophilic-lipophilic balance (hydrophilic-lipophilic ratio) as defined in standards such as JIS K3211 (Terminology for Surfactants). Polyether-modified siloxane compounds can be obtained, for example, by grafting an organic compound having unsaturated bonds and polyoxyalkylene groups onto a polyorganosiloxane main chain having silicon hydride groups via a hydrosilylation reaction. Specifically, examples include dimethylsiloxane-methyl(polyoxyethylene)siloxane copolymers, dimethylsiloxane-methyl(polyoxyethylene)siloxane-methyl(polyoxypropylene)siloxane copolymers, and dimethylsiloxane-methyl(polyoxypropylene)siloxane polymers. (I) By incorporating a polyether-modified siloxane compound into the adhesive composition, the adhesive strength and rework performance of the adhesive can be improved.

[0042] Furthermore, other known additives containing alkylene oxides, such as copolymerizable (meth)acrylic monomers, (meth)acrylamide monomers, dialkyl-substituted acrylamide monomers, surfactants, curing accelerators, plasticizers, fillers, curing retarders, processing aids, anti-aging agents, and antioxidants, can be appropriately blended as other components. These can be used individually or in combination of two or more.

[0043] The copolymer of the main component used in the adhesive composition of the present invention can be synthesized by polymerizing (A) a (meth)acrylic acid ester monomer having C4 to C10 C10 alkyl groups, (B) a copolymerizable monomer containing a hydroxyl group, (C) a copolymerizable monomer containing a carboxyl group, and (D) a polyalkylene glycol mono(meth)acrylic acid ester monomer. The polymerization method of the copolymer is not particularly limited, and any suitable polymerization method such as solution polymerization or emulsion polymerization can be used. (H) When a quaternary ammonium salt type acrylic monomer of (H2) is used as an antistatic agent, the copolymer of the main component used in the adhesive composition of the present invention can be synthesized by polymerizing (A) a (meth)acrylic acid ester monomer having C4 to C10 C atoms in the alkyl group, (B) a copolymerizable monomer containing a hydroxyl group, (C) a copolymerizable monomer containing a carboxyl group, (D) a polyalkylene glycol mono(meth)acrylic acid ester monomer, and a quaternary ammonium salt type acrylic monomer of (H2). The adhesive composition of the present invention can be prepared by blending the above copolymer with (E) a trifunctional or more isocyanate compound, (F) a crosslinking retarder, (G) a crosslinking catalyst, (H) an antistatic agent, (I) a polyether-modified siloxane compound, and any other additives as appropriate. Note that when (H2) a quaternary ammonium salt type acrylic monomer with a melting point of 30-80°C is polymerized into the copolymer as the main component, (H) an antistatic agent may or may not be added to the copolymer.

[0044] Preferably, the adhesive layer formed by crosslinking the aforementioned adhesive composition has an adhesive strength of 0.05 to 0.1 N / 25 mm in the low-speed peeling region of 0.3 m / min and an adhesive strength of 1.0 N / 25 mm or less in the high-speed peeling region of 30 m / min. This results in a performance where the adhesive strength does not change much with the peeling speed, and it becomes possible to peel it off quickly even at high speeds. Furthermore, when peeling off the surface protective film for reapplication, it does not require excessive force and is easy to peel off from the adherend.

[0045] The adhesive layer formed by crosslinking the aforementioned adhesive composition has a surface resistance value of 5.0 × 10 +10 The surface resistance is preferably Ω / □ or less, and the peel band voltage is preferably ±0 to 1kV. In this invention, "±0 to 1kV" means 0 to -1kV and 0 to +1kV, i.e., -1 to +1kV. If the surface resistance is large, the performance of dissipating static electricity generated by charging during peeling is poor. By making the surface resistance sufficiently small, the peel band voltage generated by static electricity when the adhesive layer is peeled off by the adherend is reduced, and it is possible to suppress the effect on the electrical control circuit of the adherend, etc.

[0046] The gel fraction of the adhesive layer (adhesive after crosslinking) obtained by crosslinking the adhesive composition of the present invention is preferably 95 to 100%. This high gel fraction prevents excessive adhesion in the low-speed peel region, reduces the elution of unpolymerized monomers or oligomers from the copolymer, improves reworkability and durability at high temperatures and humidity, and suppresses contamination of the adherend.

[0047] The adhesive film of the present invention is formed by creating an adhesive layer on one or both sides of a resin film, which is formed by crosslinking the adhesive composition of the present invention. The surface protection film of the present invention is a surface protection film formed on one side of a resin film, which is formed by creating an adhesive layer on one side of a resin film, which is formed by crosslinking the adhesive composition of the present invention. Because the adhesive composition of the present invention contains a well-balanced blend of the above components (A) to (I), it has antistatic properties, excellent balance of adhesive strength between low-speed peeling regions and high-speed peeling regions, and also excellent durability, reworkability (no contamination transfer to the adherend after tracing the surface protection film with a ballpoint pen via the adhesive layer), and antistatic properties. For this reason, it can be suitably used as a surface protection film for polarizing plates.

[0048] For the base film of the adhesive layer and the release film (separator) that protects the adhesive surface, resin films such as polyester film can be used. The base film can be treated with antifouling treatments such as silicone-based or fluorine-based release agents or coatings, silica microparticles, etc., on the side opposite to the side where the adhesive layer of the resin film is formed, or with antistatic treatments such as application or mixing of antistatic agents. The release film is treated with a release agent, such as a silicone-based or fluorine-based release agent, on the side that comes into contact with the adhesive surface of the adhesive layer. [Examples]

[0049] The present invention will be specifically described below with reference to examples.

[0050] <Manufacturing of acrylic copolymers> [Example 1] Nitrogen gas was introduced into a reactor equipped with a stirrer, thermometer, reflux condenser, and nitrogen inlet tube to replace the air in the reactor with nitrogen gas. Then, 100 parts by weight of 2-ethylhexyl acrylate, 0.9 parts by weight of 8-hydroxyoctyl acrylate, 0.5 parts by weight of acrylic acid, and 3 parts by weight of polyethylene glycol monoacrylate were added to the reactor along with 60 parts of solvent (ethyl acetate). Subsequently, 0.1 parts by weight of azobisisobutyronitrile was added dropwise over 2 hours as a polymerization initiator, and the reaction was carried out at 65°C for 6 hours to obtain acrylic copolymer solution 1 used in Example 1, with a weight-average molecular weight of 500,000. [Examples 2-9 and Comparative Examples 1-9] Except for the monomer compositions being as described in (A) to (D) of Table 1, the acrylic copolymer solutions used in Examples 2 to 9 and Comparative Examples 1 to 9 were obtained in the same manner as acrylic copolymer solution 1 used in Example 1 above.

[0051] <Manufacturing of adhesive compositions and surface protective films> [Example 1] To the acrylic copolymer solution 1 prepared as described above (of which 100 parts by weight was acrylic copolymer), 1.5 parts by weight of 1-octylpyridinium hexafluoride phosphate, 0.1 parts by weight of KF-351A (a polyether-modified siloxane compound with HLB=12), and 2.5 parts by weight of acetylacetone were added and stirred. Then, 1.5 parts by weight of Coronate HX (an isocyanurate of a hexamethylene diisocyanate compound) and 0.02 parts by weight of dioctyl tin dilaurate were added and stirred to obtain the adhesive composition of Example 1. This adhesive composition was applied to a release film made of a silicone resin-coated polyethylene terephthalate (PET) film, and the solvent was removed by drying at 90°C to obtain an adhesive sheet with an adhesive layer thickness of 25 μm. Subsequently, an adhesive sheet was transferred to the side of a polyethylene terephthalate (PET) film that had been treated with antistatic and antifouling properties on one side, opposite to the side that had been treated with antistatic and antifouling properties, thereby obtaining the surface protection film of Example 1 having a laminated structure of "antistatic and antifouling treated PET film / adhesive layer / release film (silicone resin coated PET film)". [Examples 2-9 and Comparative Examples 1-9] Except for using additive compositions as described in (E) to (I) of Table 1, surface protective films for Examples 2 to 9 and Comparative Examples 1 to 9 were obtained in the same manner as the surface protective film for Example 1 described above.

[0052] In Table 1, the mixing ratio of each component is shown in parentheses, calculated by setting the total of group (A) to 100 parts by weight. The compound names of the abbreviated symbols used for each component in Table 1 are shown in Table 2. Note that Coronate® HX and HL are product names of Nippon Polyurethane Industry Co., Ltd., Takenate® D-140N is a product name of Mitsui Chemicals, Inc., Duranate® 24A-100 is a product name of Asahi Kasei Chemicals Corporation, and KF-351A, KF-352A, KF-353, KF-640 and X-22-6191 are product names of Shin-Etsu Chemical Co., Ltd.

[0053] [Table 1]

[0054] [Table 2]

[0055] <Test Methods and Evaluation> The surface protective films in Examples 1-9 and Comparative Examples 1-9 were aged for 7 days at 23°C and 50% RH. After that, the release film (silicone resin-coated PET film) was peeled off to expose the adhesive layer, which was used as the sample for measuring gel fraction and surface resistance. Furthermore, this surface protection film with the adhesive layer exposed was bonded to the surface of a polarizing plate attached to a liquid crystal cell via the adhesive layer, left for one day, then autoclaved at 50°C and 5 atmospheres for 20 minutes, and left at room temperature for another 12 hours. This was used as a sample for measuring adhesive strength, peel voltage, and durability.

[0056] <Gel fraction> After aging, the mass of the sample before bonding to the polarizing plate was accurately measured, and it was immersed in toluene for 24 hours and then filtered through a 200-mesh wire mesh. After drying the filtrate at 100°C for 1 hour, the mass of the residue was accurately measured, and the gel fraction of the adhesive layer (adhesive after crosslinking) was calculated using the following formula. Gel fraction (%) = Mass of insoluble portion (g) / Mass of adhesive (g) × 100

[0057] <Adhesive strength> The measurement sample obtained above (a 25 mm wide surface protective film laminated onto the surface of a polarizing plate) was peeled off in the 180° direction using a tensile testing machine at low speed (0.3 m / min) and high speed (30 m / min), and the peel strength was measured and defined as the adhesive strength.

[0058] <Surface resistance> After aging, before bonding to the polarizing plate, the release film (silicone resin-coated PET film) was peeled off to expose the adhesive layer, and the surface resistance of the adhesive layer was measured using a resistivity meter, Hi-Resta UP-HT450 (manufactured by Mitsubishi Chemical Analytec).

[0059] <Strip voltage> The voltage (band voltage) generated when the polarizing plate was charged after peeling the sample obtained above at a tensile speed of 30 m / min at 180° was measured using high-precision electrostatic sensors SK-035 and SK-200 (manufactured by Keyence Corporation), and the maximum value of the measured value was defined as the peeled band voltage.

[0060] <Reworkability> After tracing the surface protective film of the measurement sample obtained above with a ballpoint pen (load 500g, 3 back-and-forth strokes), the surface protective film was peeled off the polarizing plate and the surface of the polarizing plate was observed to confirm that there was no contamination transfer to the polarizing plate. The evaluation criteria were as follows: "○" if there was no contamination transfer to the polarizing plate, "△" if contamination transfer was confirmed at least partially along the traced path of the ballpoint pen, and "×" if contamination transfer was confirmed along the traced path of the ballpoint pen and the adhesive was also confirmed to have detached from the adhesive surface.

[0061] <Durability> The sample obtained above was left in an atmosphere of 60°C and 90% RH for 250 hours, then removed to room temperature and left for another 12 hours. The adhesive strength was then measured and confirmed to be no significant increase compared to the initial adhesive strength. The evaluation criteria were as follows: if the adhesive strength after the test was 1.5 times or less of the initial adhesive strength, it was evaluated as "○"; if it exceeded 1.5 times, it was evaluated as "×".

[0062] Table 3 shows the evaluation results. Note that the surface resistance value is "m × 10 +n This was expressed using the formula "mE+n" (where m is an arbitrary real number and n is a positive integer).

[0063] [Table 3]

[0064] The surface protective films in Examples 1-9 had an adhesive strength of 0.05-0.1 N / 25 mm in the low-speed peeling region of 0.3 m / min, an adhesive strength of 1.0 N / 25 mm or less in the high-speed peeling region of 30 m / min, and a surface resistance of 5.0 × 10⁻⁶. +10 The resistance was less than Ω / □, the peeling voltage was ±0 to 1kV, there was no contamination transfer to the substrate after tracing over the surface protective film with a ballpoint pen via the adhesive layer, and it exhibited excellent durability when left for 250 hours in an atmosphere of 60°C and 90%RH. In other words, it simultaneously satisfies all the performance requirements: (1) balancing adhesive strength in the low-speed and high-speed peeling regions, (2) preventing adhesive residue, (3) excellent antistatic performance, and (4) rework performance.

[0065] The surface protective film of Comparative Example 1 had low adhesive strength in the low-speed peel region of 0.3 m / min and slightly inferior reworkability, possibly because it did not contain (D) polyalkylene glycol mono(meth)acrylic acid ester monomer. In the surface protective film of Comparative Example 2, (B) the amount of hydroxyl group-containing monomer was insufficient, (D) the amount of polyalkylene glycol mono(meth)acrylic acid ester monomer was insufficient, (E) the amount of isocyanate compound was excessive, and (I) the HLB value of the polyether-modified siloxane compound was insufficient. As a result, the adhesive strength in the low-speed peel region of 0.3 m / min and the high-speed peel region of 30 m / min were too high, the peel withstand voltage was high, the reworkability and durability were poor, and the gel fraction was low. In Comparative Example 3, the surface protective film had low adhesion in the low-speed peel region of 0.3 m / min, high surface resistance, high peel withstand voltage, and poor durability, possibly due to (B) excessive hydroxyl group-containing monomers, (C) excessive acid-containing monomers, (D) excessive polyalkylene glycol mono(meth)acrylic acid ester monomers, and (I) excessive HLB value of the polyether-modified siloxane compound.

[0066] In Comparative Example 4, the surface protective film had low adhesive strength in the low-speed peel region of 0.3 m / min, and poor reworkability and durability, possibly because (C) the acid-containing monomer was insufficient and (D) the polyalkylene glycol mono(meth)acrylic acid ester monomer was not present. In the surface protective film of Comparative Example 5, (B) there was an excessive amount of hydroxyl group-containing monomers, (D) there was an insufficient amount of polyalkylene glycol mono(meth)acrylic acid ester monomers, and (E) there was an insufficient amount of isocyanate compounds, resulting in excessively high adhesive strength in the low-speed peeling region of 0.3 m / min and in the high-speed peeling region of 30 m / min, a high peel withstand voltage, poor reworkability and durability, and a low gel fraction. In Comparative Example 6, the surface protective film had (F) no crosslinking retarder and (G) an excessive amount of crosslinking catalyst, which resulted in an excessively short pot life. As a result, crosslinking progressed before application, making coating impossible.

[0067] The surface protective film of Comparative Example 7 contained (A) an alkyl group-containing (meth)acrylic acid ester monomer and MA having a C1 alkyl group, (B) an excessive amount of hydroxyl group-containing monomer, (D) no polyalkylene glycol mono(meth)acrylic acid ester monomer, and (G) no crosslinking catalyst, which resulted in excessively high adhesive strength in the low-speed peel region (0.3 m / min) and high-speed peel region (30 m / min), high surface resistance, high peel withstand voltage, and poor reworkability and durability. In the surface protection film of Comparative Example 8, there was an excessive amount of (D) polyalkylene glycol mono(meth)acrylic acid ester monomer, and perhaps because (I) polyether-modified siloxane compound was not included, the adhesive strength in the low-speed peel region of 0.3 m / min and the high-speed peel region of 30 m / min was too high, the surface resistance was high, the peel withstand voltage was high, and the reworkability was somewhat poor. In the surface protection film of Comparative Example 9, (D) it did not contain polyalkylene glycol mono(meth)acrylic acid ester monomer, (H) the antistatic agent had a melting point of less than 30°C (liquid at room temperature), and (I) there was an excessive amount of polyether-modified siloxane compound, resulting in low adhesive strength in the low-speed peel region of 0.3 m / min, high peel withstand voltage, slightly poor reworkability, and poor durability. Thus, the surface protective films in Comparative Examples 1 to 9 failed to simultaneously satisfy all the required performance characteristics: (1) balancing adhesive strength in the low-speed peeling region and the high-speed peeling region, (2) preventing the generation of adhesive residue, (3) excellent antistatic performance, and (4) rework performance.

Claims

1. An adhesive composition comprising (A) a (meth)acrylic acid ester monomer having C4 to C10 C10 alkyl group, (B) a copolymerizable monomer containing a hydroxyl group, (C) a copolymerizable monomer containing a carboxyl group, and (D) a copolymer containing a polyalkylene glycol mono(meth)acrylic acid ester monomer, further comprising (E) a trifunctional or more isocyanate compound, (H) an antistatic agent, and (I) a polyether-modified siloxane compound, Each 100 parts by weight of (A) an alkyl group having C4 to C10 carbon atoms (meth)acrylic acid ester monomer contains 0.1 to 5.0 parts by weight of (B) a copolymerizable monomer containing a hydroxyl group, 0.35 to 1.0 parts by weight of (C) a copolymerizable monomer containing a carboxyl group, and 1 to 20 parts by weight of (D) a polyalkylene glycol mono(meth)acrylic acid ester monomer, and each 100 parts by weight of the copolymer contains 0.5 to 5.0 parts by weight of (E) a trifunctional or more isocyanate compound. The (E) isocyanate compound with three or more functions is at least one compound selected from the group consisting of isocyanurate derivatives of hexamethylene diisocyanate compounds, isocyanurate derivatives of isophorone diisocyanate compounds, adduct derivatives of hexamethylene diisocyanate compounds, adduct derivatives of isophorone diisocyanate compounds, burette derivatives of hexamethylene diisocyanate compounds, and burette derivatives of isophorone diisocyanate compounds. The adhesive composition is characterized in that the (I) polyether-modified siloxane compound is a polyether-modified siloxane compound having an HLB value of 7 to 12, and the (I) polyether-modified siloxane compound is present in an amount of 0.01 to 0.5 parts by weight per 100 parts by weight of the copolymer.

2. An adhesive film characterized by having an adhesive layer formed on one or both sides of a resin film, which is obtained by crosslinking the adhesive composition described in claim 1.

3. A surface protective film for a polarizing plate, characterized in that it uses the adhesive film according to claim 2, wherein the adhesive layer is formed on one side of the resin film.

Citation Information

Patent Citations

  • Pressure-sensitive adhesive

    JP1988225677A

  • Adhesive composition

    JP1996199130A

  • Surface protective film for liquid crystal display panel

    JP1999070629A

  • Pressure sensitive adhesive for surface-protecting film, and film for surface protection

    JP1999256111A