Structures for optical devices, methods for fabricating the same, and photocurable siloxane resin compositions therefor

A photocurable siloxane resin composition with controlled viscosity and a photoacid generator addresses the issues of conventional encapsulants by forming a protective layer that enhances optical properties and seals LED chips, improving brightness and contrast ratio.

JP2026183053APending Publication Date: 2026-11-19DUPONT SPECIALTY MATERIALS KOREA LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026205126
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2021-11-30
Filing Date
2026-09-11
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional encapsulants for LED chips face issues with heat control during curing, leading to shape reproduction difficulties, long curing times, and potential discoloration, while also failing to enhance optical properties like brightness and contrast ratio due to uncontrolled heat flow and the use of platinum catalysts.

Method used

A photocurable siloxane resin composition with controlled viscosity and solvent-free formulation, using a photoacid generator instead of a thermal acid generator, forms a protective layer that improves optical properties by shortening curing time and preventing discoloration, while maintaining excellent pattern reproducibility and light diffusion.

Benefits of technology

The protective layer effectively seals LED chips from heat and moisture, enhances brightness and contrast ratio through light diffusion, and achieves a desirable diameter-to-thickness ratio, overcoming the limitations of conventional encapsulants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026183053000001_ABST
    Figure 2026183053000001_ABST
Patent Text Reader

Abstract

The present invention provides structures for optical devices, methods for fabricating them, and photocurable siloxane resin compositions for the same. [Solution] The structure for the optical device according to the embodiment includes a protective layer formed from a photocurable siloxane resin composition, which not only protects or seals light-emitting elements such as mini-LED chips from external heat or moisture, but also helps to improve optical properties such as brightness and contrast ratio of the light emitted from the light-emitting elements through a light diffusion effect.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to structures for optical devices, methods for manufacturing the same, and photocurable siloxane resin compositions therefor. [Background technology]

[0002] Optical devices refer to light-emitting elements that convert electrical signals into optical signals. Typically, light-emitting diodes (LEDs) are used due to their advantages such as high light energy conversion efficiency, miniaturization, weight reduction, and low power consumption. In recent years, the size of LED chips has been gradually decreasing. For example, mini-LEDs with chip sizes of 100 μm to 200 μm and micro-LEDs with chip sizes of less than 100 μm have been developed. Since each LED chip within mini-LEDs and micro-LEDs functions individually as a pixel or light source, the limitations on the size and shape of the display are removed, and clearer image characteristics can be achieved than those of conventional light sources.

[0003] Among the above, mini-LEDs are based on intermediate technology between general-purpose LEDs and micro-LEDs. They have the advantage of being able to utilize existing LED production lines, thus increasing profitability while extending the lifespan of existing production plants and technologies. In particular, mini-LEDs are thinner than organic light-emitting diodes (OLEDs), which are widely used today, and can offer improved power efficiency and resolution, while also mitigating the burn-in phenomenon that is a disadvantage of OLEDs.

[0004] LED chips are encased in a encapsulant for protection, which helps protect the LED chips from external heat or moisture. Conventional encapsulants are generally obtained by curing epoxy with the introduction of a thermal acid generator or thermal base generator, or by crosslinking double bonds in the presence of a platinum catalyst. However, these conventional methods have problems in that the heat flow is not controlled during the process, making it difficult to reproduce the shape of the cured product, and that curing takes a long time or discoloration may occur depending on the amount of platinum catalyst used.

[0005] In addition, in composite LEDs, lenses for diffusing light are formed on the encapsulating material, and such lenses must be formed within a dome structure having a specific thickness to promote light diffusion. In particular, since mini-LEDs have light-emitting components that are smaller than those of general LEDs, it is necessary to improve the brightness or contrast ratio of the light generated from the LED chip through the light diffusion effect of the lens.

[0006] In recent years, methods have been developed to encapsulate LED chips using LED encapsulating agents to form lenses. For this purpose, the encapsulating agent must possess both LED encapsulating agent and lens properties simultaneously. However, conventional encapsulating agents have problems in that the heat generated by the LED chip raises the temperature of the LED packaging, which reduces the adhesion of the encapsulating agent or lowers the light efficiency due to burnout or reduced transmittance.

[0007] [Prior art document] (Patent Document 1) Korean Patent Application Publication No. 2014-0078655 Specification [Overview of the Initiative] [Problems that the invention aims to solve]

[0008] As a result of research conducted by the present inventors, a functional group that reacts with acid is introduced into the polysiloxane, a photoacid generator is used instead of a thermal acid generator, and a solvent-free photocurable siloxane resin composition with controlled viscosity is used, thereby enabling the acquisition of a protective layer with excellent pattern reproducibility and light diffusion properties while shortening the curing time.

[0009] Therefore, the object of the present invention is to provide a structure for an optical device equipped with a protective layer that can serve not only to protect or seal light-emitting elements such as mini LED chips from external heat or moisture, but also as a lens that improves optical properties such as brightness and contrast ratio of light emitted from the light-emitting elements through a light diffusion effect. [Means for solving the problem]

[0010] To achieve the above objectives, the present invention provides a structure for an optical device comprising a substrate layer, a light-emitting element formed on the substrate layer, and a protective layer surrounding the light-emitting element, wherein the protective layer comprises a photocured material of a photocurable siloxane resin composition.

[0011] A method for fabricating a structure for an optical device includes the steps of fabricating a substrate layer and a light-emitting element formed on the substrate layer, applying a photocurable siloxane resin composition to the light-emitting element, and irradiating the photocurable siloxane resin composition with light to form a protective layer surrounding the light-emitting element.

[0012] The photocurable siloxane resin composition comprises (A) a polysiloxane having a functional group that reacts with acid, (B) a photoacid generator, and (C) a solvent-free diluent having a functional group that reacts with acid. The viscosity of the polysiloxane is 10,000 cP to 50,000 cP at 25°C, and the solvent content in the composition is less than 4.0% by weight.

[0013] Advantageous effects of the invention The structure for an optical device according to the present invention includes a protective layer formed from a photocurable siloxane resin composition, and the protective layer can serve not only to protect or seal light-emitting elements such as mini LED chips from external heat or moisture, but also to improve optical properties such as the luminance and contrast ratio of light emitted from the light-emitting elements through the light diffusion effect brought by the improved refractive index.

[0014] Specifically, in the photocurable siloxane resin composition used for producing the protective layer, functional groups that react with an acid are introduced into polysiloxane, and a photoacid generator is used instead of a thermal acid generator that requires a long time for curing, thereby shortening the curing time and satisfying pattern reproducibility and physical properties. In addition, the photocurable siloxane resin composition is a solvent-free type, and the acid generated by light acts as a catalyst that shortens the process time. Since it does not require the use of a platinum catalyst, problems related to discoloration caused by platinum adsorption during the process do not occur. Furthermore, the photocurable siloxane resin composition has a controlled viscosity, which solves the problem that it is difficult for conventional compositions to increase the thickness due to thermal flow in the direction of gravity. It is also possible to obtain a structure for an optical device provided with a protective layer having an excellent diameter-to-thickness ratio. [Brief Description of the Drawings]

[0015] [Figure 1] A cross-sectional view of a structure for an optical device according to an embodiment is shown. [Figure 2] The diameter and thickness of the protective layer of the structure for an optical device according to the embodiment are shown. [Figure 3] A method for fabricating a structure for an optical device according to an embodiment is shown. [Figure 4] Figure 4a is a photograph of the protective layer of the example having an excellent diameter-to-thickness ratio in the test example. Figure 4b is a photograph of the protective layer of the comparative example having an insufficient diameter-to-thickness ratio in the test example. [Figure 5]Figure 5a is a photograph of the protective layer of an example having an excellent yellowness index (Y.I.) in a test example. Figure 5b is a photograph of the protective layer of a comparative example having an insufficient yellowness index in a test example. [Description of Embodiments]

[0016] The present invention is not limited to what is described below. Rather, it may be modified into various forms as long as the gist of the present invention is not altered.

[0017] Throughout the present specification, when a part is said to "comprise" an element, it is understood that other elements may be included, rather than excluding other elements, unless otherwise specifically stated. In addition, all numbers and expressions relating to the amounts of components, reaction conditions and the like used in the present specification should be understood as being modified by the term "about" unless otherwise specifically stated.

[0018] Structure for Optical Device Figure 1 shows a cross-sectional view of a structure for an optical device according to an embodiment. Referring to Figure 1, the structure for an optical device according to the present invention includes a base material layer (100), a light-emitting element (200) formed on the base material layer (100), and a protective layer (300) surrounding the light-emitting element (200).

[0019] The base material layer may be, for example, a circuit board. Specifically, the base material layer may include a circuit composed of a conductive material such as aluminum or copper. In addition, the base material layer may further include an insulating material. The insulating material may include, for example, polymers such as polyimide, epoxy, and polyester, and ceramics such as aluminum nitride, boron nitride, silicon nitride, alumina, or glass.

[0020] One or more light-emitting elements are formed on the base material layer. For example, the light-emitting elements can be provided on the base material layer by die bonding. In addition, the light-emitting elements can be electrically connected to the circuit of the base material layer by a conductor, for example, a bonding wire.

[0021] The light-emitting element may be a light-emitting diode (LED) chip. For example, the light-emitting element may be a mini-LED chip, and its size may be specifically 1 mm or less, 500 μm or less, 300 μm or less, or 200 μm or less, more specifically 100 μm to 200 μm. As another example, the light-emitting element may be a micro-LED chip, and its size may be specifically less than 100 μm, more specifically 5 μm to less than 100 μm.

[0022] A protective layer is formed on the substrate layer to surround the light-emitting element. Therefore, the protective layer serves as an encasing agent for the light-emitting element to protect it from external heat or moisture. The shape of the protective layer is not particularly limited, but it can have a hemispherical shape, such as a dome.

[0023] In particular, the protective layer may have a lens shape to diffuse light. Therefore, the protective layer can function simultaneously as both a encapsulant and a lens.

[0024] According to the examples, the protective layer may have a specific diameter-to-thickness ratio to further enhance its function as a lens.

[0025] Figure 2 shows the diameter (D) and thickness (t) of the protective layer of a structure for an optical device. Referring to Figure 2, the protective layer may satisfy the following relationship (1). 7.0 > D / t(1) Here, D is the diameter of the protective layer (mm), and t is the thickness of the protective layer (mm).

[0026] The value of D / t in relation (1) can be, for example, less than 7.0, 6.5 or less, 6.0 or less, less than 6.0, 5.5 or less, or 5.0 or less. In addition, the value of D / t in relation (1) can be at least a specific level, for example, 1.0 or more, 2.0 or more, 3.0 or more, 4.0 or more, 4.5 or more, 5.0 or more, 5.5 or more, or 6.0 or more. In addition, the protective layer may have a refractive index of at least a certain level. For example, it may have a refractive index of 1.2 or higher, 1.3 or higher, 1.4 or higher, or 1.5 or higher. Specifically, the protective layer may have a refractive index of 1.5 or higher.

[0027] In addition, the refractive index of the protective layer may be 3.0 or less, 2.5 or less, 2.0 or less, 1.7 or less, or 1.6 or less.

[0028] The protective layer not only protects or seals optical devices such as mini-LED chips from external heat or moisture, but can also help improve optical properties such as brightness and contrast ratio of the light emitted from the LED through a light diffusion effect caused by improved refractive index.

[0029] In the structure for the optical device of the present invention, the protective layer comprises a photocured material of a photocurable siloxane resin composition.

[0030] According to the embodiment, the photocurable siloxane resin composition contains a polysiloxane into which functional groups that react with acid have been introduced, uses a photoacid generator instead of a thermal acid generator, and is a solvent-free type with controlled viscosity, thereby enabling the production of a protective layer with excellent pattern reproducibility and light diffusion properties while shortening the curing time.

[0031] In contrast, conventional protective layers are generally obtained by curing epoxy with the introduction of a thermal acid generator or thermal base generator, or by crosslinking double bonds in the presence of a platinum catalyst. However, in these conventional methods, the heat flow is not controlled during the process, making it difficult to reproduce the shape of the cured material, and problems arise such as the long curing time or discoloration depending on the amount of platinum catalyst used.

[0032] Figure 3 shows a method for fabricating a structure for an optical device according to an embodiment.

[0033] Referring to Figure 3, in a structure for an optical device, a photocurable siloxane resin composition (301) is applied to a light-emitting element (200) formed on a substrate layer (100), and photocured (for example by ultraviolet irradiation) to form a protective layer surrounding the light-emitting element.

[0034] A method for fabricating a structure for an optical device according to an embodiment includes the steps of (1) fabricating a substrate layer and a light-emitting element formed on the substrate layer, (2) applying a photocurable siloxane resin composition to the light-emitting element, and (3) irradiating the photocurable siloxane resin composition with light to form a protective layer surrounding the light-emitting element.

[0035] Light irradiation should last from 5 to 30 seconds, for example, at approximately 10 mJ / cm². 2 ~5,000 mJ / cm 2 This may be done by irradiating with ultraviolet light (e.g., UV-A, UV-B, UV-C) in the specified dose.

[0036] Photocurable siloxane resin composition The photocurable siloxane resin composition comprises (A) a polysiloxane having a functional group that reacts with an acid, (B) a photoacid generator, and (C) a solvent-free diluent having a functional group that reacts with an acid. The photocurable siloxane resin composition may optionally further contain (D) an adhesion aid or other additives.

[0037] Polysiloxanes can have at least a certain level of refractive index. For example, they can have a refractive index of 1.2 or higher, 1.3 or higher, 1.4 or higher, or 1.5 or higher. On the other hand, the refractive index of polysiloxanes can be 3.0 or lower, 2.5 or lower, 2.0 or lower, 1.7 or lower, or 1.6 or lower. In addition, photocurable siloxane resin compositions can also have the same or similar refractive index as their main component, polysiloxane.

[0038] According to the embodiment, the polysiloxane has a viscosity of 10,000 cP to 50,000 cP at 25°C. For example, the viscosity of the polysiloxane may be 10,000 cP or more, 15,000 cP or more, 20,000 cP or more, 25,000 cP or more, or 30,000 cP or more at 25°C, and also 50,000 cP or less, 45,000 cP or less, 40,000 cP or less, or 35,000 cP or less. The viscosity may be the value of the polysiloxane measured with a Brookfield viscometer. When the viscosity is within the above range, it is advantageous to adjust the viscosity of the entire composition to a preferred range to obtain a reproducible structure by improving problems caused by layers being pulled up or flowing during intermittent operations in the process.

[0039] The photocurable siloxane resin composition is prepared as a solvent-free type. For example, the solvent content in the composition of the present invention may be less than 4.0% by weight, specifically less than 3.0% by weight, less than 2.0% by weight, or less than 1.0% by weight. If the solvent content is outside the above range, bubbles may be generated by solvent vapor during the process of using the composition, making it difficult to form a uniformly shaped pattern and potentially causing problems in the process. On the other hand, any solvent that may be present in trace amounts in the composition of the present invention may be residual solvent that cannot be removed during the synthesis of the raw materials.

[0040] The composition of the present invention does not use a solvent, but a diluent having a functional group that reacts with an acid is used to sufficiently dissolve the photoacid generator and the like, and adjust the viscosity.

[0041] In addition, the viscosity of a photocurable siloxane resin composition may be affected by the viscosity of components contained therein, such as polysiloxane. For example, the viscosity of a photocurable siloxane resin composition may be 10,000 cP or higher, 15,000 cP or higher, 20,000 cP or higher, 25,000 cP or higher, or 30,000 cP or higher at 25°C, and also 50,000 cP or lower, 45,000 cP or lower, 40,000 cP or lower, or 35,000 cP or lower. Specifically, a photocurable siloxane resin composition can have a viscosity of 20,000 cP to 40,000 cP at 25°C.

[0042] In the photocurable siloxane resin composition, functional groups that react with acid are introduced into the polysiloxane, and a photoacid generator is used instead of a thermal acid generator, which takes a long time to cure, thereby shortening the curing time and satisfying pattern reproducibility and physical properties. In addition, the photocurable siloxane resin composition is solvent-free, and the acid generated by light acts as a catalyst to shorten the process time. Since it does not require the use of a platinum catalyst, the problem of discoloration due to platinum adsorption during the process does not occur. Furthermore, the photocurable siloxane resin composition has a controlled viscosity, thereby solving the problem that conventional compositions have difficulty increasing in thickness due to heat flow in the direction of gravity. It is also possible to achieve an excellent diameter-to-thickness ratio.

[0043] In this specification, the components of the photocurable siloxane resin composition are described in detail below.

[0044] (A) Polysiloxane The photocurable siloxane resin composition contains a polysiloxane having a functional group that reacts with acid.

[0045] For example, polysiloxane is expressed by the following formula 1: [Formula 1] R 1 p R 2 q SiO (4-p-q) / 2 It can have an average structure represented by [this].

[0046] In Formula 1, p and q satisfy 1≦p+q≦3 and 0≦q, p:q is 3:1 to 1:0, and R 1 contains a cyclic ether group having 2 to 6 carbon atoms, and R 2 contains an aryl group or aralkyl group having 6 to 15 carbon atoms.

[0047] For example, in Formula 1, p can be 0.75 or more or 1 or more, and 3 or less or 2.5 or less. q can be 0 or more or 0.25 or more, and 0.75 or less or 0.5 or less. Specifically, in Formula 1, p can be 0.75 to 3, and q can be 0 to 0.75.

[0048] The cyclic ether group can have 2 to 6 carbon atoms, and can contain an oxygen atom between carbon chains. The number of carbon atoms in the cyclic ether group can be 2 to 6, 2 to 5, or 2 to 4. It can contain 1 to 3 oxygen atoms. R containing the cyclic ether group 1 Specific examples of include epoxy, glycidyl, glycidoxy, glycidoxymethyl, glycidoxyethyl, glycidoxypropyl, 3,4-epoxycyclohexylethyl and the like.

[0049] The aryl group or aralkyl group can have 6 to 15 carbon atoms, and includes an aromatic hydrocarbon. The number of carbon atoms in the aryl group or aralkyl group can be 6 to 15, 6 to 12, 6 to 10, or 6 to 8. Specific examples of the aryl group or aralkyl group may include phenyl, benzyl, phenethyl, tolyl, naphthyl, naphthylmethyl, naphthylethyl and the like. These may be unsubstituted, or substituted with one or more halogen, amino, alkyl and the like.

[0050] In Formula 1, R 1 to R 2 The molar ratio of can be 75:25 to 100:0, 75:25 to 90:10, 75:25 to 80:20, 80:20 to 100:0, 85:15 to 100:0, or 80:20 to 90:10.

[0051] Specifically, the polysiloxane may contain (a-1) structural units derived from a silane compound containing a cyclic ether group, and (a-2) structural units derived from a silane compound containing an aryl group or an aralkyl group.

[0052] (a-1) Structural unit derived from a silane compound containing a cyclic ether group Structural unit (a-1) contains a cyclic ether group, which helps form a network structure through reaction with acid during curing, thereby enhancing durability and optical properties.

[0053] The structural unit (a-1) is derived from a silane compound containing a cyclic ether group. Silane compounds containing a cyclic ether group are represented by the following formula 2a: [Formula 2a] R 1 a Si(OR 3 ) 4-a It may be at least one silane compound represented by or a hydrolysate thereof.

[0054] In equation 2a, a is an integer from 1 to 3, and R 1 Each contains a cyclic ether group having 2 to 6 carbon atoms, R 3 It is an alkyl group having 1 to 6 carbon atoms.

[0055] A cyclic ether group can have 2 to 6 carbon atoms and can contain oxygen atoms between the carbon chains. The number of carbon atoms in a cyclic ether group can be 2 to 6, 2 to 5, or 2 to 4. It can contain 1 to 3 oxygen atoms. R containing a cyclic ether group 1 Specific examples include epoxy, glycidyl, glycidoxy, glycidoxymethyl, glycidoxyethyl, glycidoxypropyl, and 3,4-epoxycyclohexylethyl.

[0056] Alkyl groups can have 1 to 6 carbon atoms, for example, 1 to 5, 1 to 4, or 1 to 3 carbon atoms. Specific examples of alkyl groups may include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, t-butyl, pentyl, and hexyl.

[0057] In formula 2a, the compound may be a tetrafunctional silane compound (wherein a is 0), a trifunctional silane compound (wherein a is 1), a bifunctional silane compound (wherein a is 2), or a monofunctional silane compound (wherein a is 3).

[0058] Specific examples of silane compounds containing a cyclic ether group include 3-glycidoxypropyl-trimethoxysilane (γ-glycidoxypropyl-trimethoxysilane), 3-glycidoxypropyl-methyldimethoxysilane, 3-glycidoxypropyl-triethoxysilane, 3-glycidoxypropyl-methyldiethoxysilane, and β-(3,4-epoxycyclohexyl)ethyl-trimethoxysilane.

[0059] The amount of structural unit (a-1) can be 51 to 100 mol%, preferably 75 to 100 mol%, based on the total number of moles of structural units constituting the polysiloxane. Within the above content range, it is advantageous for having sufficient adhesion and hardness.

[0060] (a-2) Structural units derived from silane compounds containing an aryl group or an aralkyl group Structural unit (a-2) contains an aryl group or an aralkyl group, which can increase the refractive index and thereby enhance the light diffusion properties.

[0061] The structural unit (a-2) is derived from a silane compound containing an aryl group or an aralkyl group. Silane compounds containing an aryl group or an aralkyl group are defined by the following formula 2b: [Formula 2b] R 2 b Si(OR 3 ) 4-b It may be at least one silane compound represented by or a hydrolysate thereof.

[0062] In equation 2b, b is an integer from 1 to 3, and R 2 Each contains an aryl group or aralkyl group having 6 to 15 carbon atoms, and R 3 It is an alkyl group having 1 to 6 carbon atoms.

[0063] Aryl or aralkyl groups can have 6 to 15 carbon atoms and include aromatic hydrocarbons. The number of carbon atoms in an aryl or aralkyl group can be 6 to 15, 6 to 12, 6 to 10, or 6 to 8. Specific examples of aryl or aralkyl groups may include phenyl, benzyl, phenethyl, tolyl, naphthyl, naphthylmethyl, naphthylethyl, etc. These may be unsubstituted or substituted with one or more halogens, aminos, alkyls, etc.

[0064] Alkyl groups can have 1 to 6 carbon atoms, for example, 1 to 5, 1 to 4, or 1 to 3 carbon atoms. Specific examples of alkyl groups may include methyl, ethyl, n-propyl, i-propyl, n-butyl, i-butyl, t-butyl, pentyl, and hexyl.

[0065] Specific examples of structural units (a-2) include phenyltrimethoxysilane, phenyltriethoxysilane, diethoxydiphenylsilane, dimethoxydiphenylsilane, N-phenyl-3-aminopropyltrimethoxysilane, p-chlorophenyltrimethoxysilane, p-bromophenyltrimethoxysilane, diethoxymethylphenylsilane, dimethoxymethylphenylsilane, triethoxytolylsilane, 1-naphthyltrimethoxysilane, and m-aminophenyltrimethoxysilane.

[0066] The amount of structural unit (a-2) can be 0 to 49 mol%, preferably 0 to 25 mol%, based on the total number of moles of structural units constituting the polysiloxane. Within this range, it is advantageous for increasing the refractive index, improving the yellowness index (YI) value, and for UV stability.

[0067] Preparation and properties of polysiloxanes A silane compound containing a cyclic ether group, as illustrated above, and a silane compound containing an aryl group or an aralkyl group can be used in combination in the preparation of polysiloxanes. Specifically, a silane compound of formula 2a and a silane compound of formula 2b can be used in combination in the preparation of polysiloxanes.

[0068] The conditions for obtaining hydrolysates or condensates of these silane compounds for the preparation of polysiloxanes are not particularly limited. For example, the silane compounds of formula 2a and formula 2b are optionally diluted with a solvent, such as ethanol, 2-propanol, acetone, butyl acetate, etc., and water, and an acid (e.g., hydrochloric acid, acetic acid, nitric acid, etc.) or a base (e.g., ammonia, triethylamine, cyclohexylamine, tetramethylammonium hydroxide, etc.) is added as a catalyst, and the mixture is then stirred to obtain the desired hydrolysate or condensate.

[0069] The type and amount of solvent or acid or base catalyst are not particularly limited. Furthermore, the hydrolysis polymerization reaction may be carried out at low temperatures of 20°C or below. Alternatively, the reaction may be accelerated by heating or reflux.

[0070] The required reaction time can be adjusted depending on the type and concentration of the silane compound, the reaction temperature, and so on. For example, the reaction typically takes 15 minutes to 30 days to proceed until the molecular weight of the resulting condensate is approximately 500 to 50,000. However, it is not limited to these times.

[0071] The weight-average molecular weight (Mw) of the polysiloxane may be in the range of 2,000 to 10,000, preferably 3,000 to 5,000. Within this molecular weight range, it is advantageous to achieve the desired viscosity when preparing the composition without using a solvent.

[0072] In this specification, weight-average molecular weight refers to the weight-average molecular weight measured by gel permeation chromatography (GPC, eluent: tetrahydrofuran) with respect to a polystyrene standard. Typically, it is unitless but can be understood to have units of g / mol or Da.

[0073] The solid content of the polysiloxane, excluding the solvent, can be 96% to 99.9% by weight. Within this range, it is advantageous to control the solvent content in the total composition to a preferred range for preparing it as a solvent-free type.

[0074] Polysiloxanes can have viscosities of 10,000 cP to 50,000 cP at 25°C. Viscosity may be the value of the polysiloxane measured with a Brookfield viscometer. When the viscosity is within the above range, the viscosity of the entire composition can be adjusted to a preferred range, which is advantageous for obtaining reproducible structures by improving problems caused by layers being pulled up or flowing during intermittent operations in the process.

[0075] The polysiloxane content may be 70 to 99% by weight, preferably 80 to 95% by weight, based on the total weight of the photocurable siloxane resin composition. The content can be based on the content excluding the solvent. Within the above content range, it is advantageous to obtain structures with excellent optical properties and high curing.

[0076] (B) Photoacid generator A photocurable siloxane resin composition containing a photoacid generator.

[0077] The photoacid generator generates acid when irradiated with light, and crosslinks polysiloxanes that have functional groups that react with the acid.

[0078] In addition, photoacid generators help initiate the polymerization of monomers that can be cured by visible light, ultraviolet light, deep ultraviolet light, etc.

[0079] Examples of photoacid generators include, but are not limited to, onium salt compounds, halogen-containing compounds, diazoketone compounds, diazomethane compounds, sulfone compounds, sulfone ester compounds, and sulfonimide compounds.

[0080] Examples of onium salt compounds include iodonium salts, sulfonium salts, phosphonium salts, diazonium salts, and pyridinium salts. Specific examples of onium salt compounds include at least one selected from the group consisting of diphenyliodonium triflate, diphenyliodonium pyrene sulfonate, diphenyliodonium dodecylbenzene sulfonate, triphenylsulfonium triflate, triphenylsulfonium hexafluoroantimonate, and triphenylsulfonium naphthalene sulfonate.

[0081] Examples of halogen-containing compounds include haloalkyl group-containing hydrocarbon compounds and haloalkyl group-containing heterocyclic compounds. Specific examples of halogen-containing compounds include 1,10-dibromo-n-decane, 1,1-bis(4-chlorophenyl)-2,2,2-trichloroethane, phenyl-bis(trichloromethyl)-s-triazine, 4-methoxyphenyl-bis(trichloromethyl)-s-triazine, styryl-bis(trichloromethyl)-s-triazine, and naphthyl-bis(trichloromethyl)-s-triazine.

[0082] Specific examples of diazomethane compounds include bis(trifluoromethylsulfonyl)diazomethane, bis(cyclohexylsulfonyl)diazomethane, and bis(phenylsulfonyl)diazomethane.

[0083] Specific examples of sulfonate ester compounds include alkyl sulfonates, haloalkyl sulfonates, aryl sulfonates, and iminosulfonates. Specific examples of preferred sulfonate compounds include benzointosylate, pyrogallol trifluoromethanesulfonate, o-nitrobenzyl trifluoromethanesulfonate, and o-nitrobenzyl p-toluenesulfonate.

[0084] Specific examples of sulfonimide compounds include N-(trifluoromethylsulfonyloxy)succinimide, N-(trifluoromethylsulfonyloxy)phthalimide, N-(trifluoromethylsulfonyloxy)diphenylmaleimide, N-(trifluoromethylsulfonyloxy)bicyclo[2.2.1]hept-5-ene-2,3-dicarboximide, and N-(trifluoromethylsulfonyloxy)naphthylimide.

[0085] The content of the photoacid generator may be 0.01 to 10 parts by weight based on 100 parts by weight of the polysiloxane content. The content can be based on the content excluding the solvent. Within the above content range, it is advantageous to achieve optical properties such as transparency and a high degree of curing of the composition. Specifically, if the content of the photoacid generator is less than 0.01 parts by weight, the degree of curing may be insufficient. If it exceeds 10 parts by weight, discoloration or cracking of the pattern may occur due to shrinkage during curing. Preferably, the content of the photoacid generator may be 0.1 to 6 parts by weight based on 100 parts by weight of the polysiloxane content.

[0086] In addition, the amount of photoacid generator can be 0.01 to 10 parts by weight, based on the total weight of the photocurable siloxane resin composition excluding the solvent.

[0087] (C) Diluent The photocurable siloxane resin composition contains a solvent-free diluent having a functional group that reacts with acid.

[0088] The diluent helps to uniformly dissolve the photoacid generator without using a solvent while it is not vaporizing during the process.

[0089] The functional group in the diluent that reacts with the acid may be, for example, a cyclic ether group having 2 to 6 carbon atoms, such as epoxy or glycidyl.

[0090] For example, the diluent may be a monomer having an epoxy group or a glycidyl group. Specifically, the diluent may be at least one selected from the group consisting of (3,4-epoxycyclohexyl)methyl (meth)acrylate, glycidyl (meth)acrylate, and allyl glycidyl ether. More specifically, the diluent may be (3,4-epoxycyclohexyl)methyl acrylate or glycidyl methacrylate.

[0091] The diluent content may be 0.01 to 10 parts by weight based on 100 parts by weight of the polysiloxane content. The content may be based on the content excluding the solvent. Within the above content range, it is advantageous to improve the diameter-to-thickness ratio (i.e., aspect ratio) and pattern reproducibility of the composition. Specifically, if the diluent content is less than 0.01 parts by weight, the photoacid generator may not dissolve uniformly. If it exceeds 10 parts by weight, the viscosity of the composition may decrease, thereby reducing the diameter-to-thickness ratio. Preferably, the diluent content may be 0.1 to 6 parts by weight based on 100 parts by weight of the polysiloxane content.

[0092] Specifically, the diluent content may be 0.1 to 10 parts by weight based on 100 parts by weight of the polysiloxane content. It may be 30 parts by weight or more, 40 parts by weight or more, or 50 parts by weight or more based on 100 parts by weight of the total content of the photoacid generator and diluent.

[0093] In addition, the diluent content may be 0.01 to 10 parts by weight, based on the total weight of the photocurable siloxane resin composition excluding the solvent.

[0094] (D) Adhesion aid The photocurable siloxane resin composition of the present invention may further contain, if necessary, an adhesion aid to enhance adhesion to a substrate layer.

[0095] The adhesion aid may have at least one reactive group selected from the group consisting of carboxyl groups, acryloyl groups, methacryloyl groups, isocyanate groups, amino groups, mercapto groups, vinyl groups, epoxy groups, and combinations thereof.

[0096] The type of adhesion aid is not particularly limited. It may be at least one selected from the group consisting of trimethoxysilyl benzoic acid, γ-methacrylateoxypropyltrimethoxysilane, vinyltriacetoxysilane, vinyltrimethoxysilane, γ-isocyanatopropyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, N-phenylaminopropyltrimethoxysilane, and β-(3,4-epoxycyclohexyl)ethyltrimethoxysilane. Preferably, it is γ-glycidoxypropyltrimethoxysilane, γ-glycidoxypropyltriethoxysilane, or N-phenylaminopropyltrimethoxysilane, which can increase film retention and have excellent adhesion to the substrate layer.

[0097] The content of the adhesion aid may be 0.01 to 10 parts by weight based on 100 parts by weight of the polysiloxane content. The content may be based on the content excluding the solvent. Within the above content range, it is advantageous to further enhance the adhesion of the composition. Specifically, if the content of the adhesion aid is less than 0.01 parts by weight, the adhesion to the substrate layer may decrease. If it exceeds 10 parts by weight, it may decrease the degree of curing. Preferably, the content of the adhesion aid may be 0.1 to 3 parts by weight based on 100 parts by weight of the polysiloxane content.

[0098] In addition, the content of the adhesive aid may be 0.01 to 10 parts by weight, based on the total weight of the photocurable siloxane resin composition excluding the solvent.

[0099] In addition, the photocurable siloxane resin composition may further contain other additives, such as antioxidants and stabilizers, as long as they do not adversely affect the physical properties of the composition.

[0100] Embodiments of the present invention The present invention will be described in more detail hereafter with reference to the following examples. However, these examples are provided to illustrate the present invention, and the scope of the invention is not limited to these examples. [Examples]

[0101] Preparation Example 1: Preparation of Polysiloxane A-1 In a reactor equipped with a reflux condenser, 58.6 parts by weight of (3-glycidoxypropyl)trimethoxysilane, 16.4 parts by weight of phenyltrimethoxysilane, 20 parts by weight of distilled water, and 5 parts by weight of tetrahydrofuran (THF) were charged. The mixture was then refluxed and vigorously stirred for 5 hours in the presence of 0.1 parts by weight of oxalic acid catalyst.

[0102] After cooling the reaction solution, water was removed in a vacuum furnace at room temperature (25°C) and a minimum pressure of -760 mmHg. Next, it was transferred to a tray and further evaporated under reduced pressure at 40°C to prepare polysiloxane A-1.

[0103] The weight-average molecular weight (Mw) of the polysiloxane was measured by gel permeation chromatography (GPC), viscosity by Brookfield viscometer, and water content by volumetric KF moisture crystallization method, and these were converted to solids. These are shown in Table 1 below.

[0104] Preparation Examples 2-9: Preparation of Polysiloxanes A-2-A-9 Polysiloxanes A-2 to A-9 were prepared by repeating the procedure of Preparation Example 1 according to the monomer content ratios shown in Table 1. The weight-average molecular weight, viscosity, and solid content are shown. However, heterogeneous precipitation occurred during the synthesis of polysiloxane A-9.

[0105] Preparation Example 3: Preparation of Acrylic Copolymer A-10 Acrylic copolymer A-10 was prepared by repeating the procedure of Preparation Example 1 according to the monomer content ratios shown in Table 2 below. The weight-average molecular weight, viscosity, and solids content are shown.

[0106] [Table 1]

[0107] [Table 2]

[0108] Example 1 Step 1: Preparation of a photocurable siloxane resin composition 5.6 parts by weight of photoacid generator (B) was diluted with 5.6 parts by weight of diluent (C-1), and then added to 100 parts by weight of polysiloxane (A-1) of Preparation Example 1. The resulting mixture was mixed using a shaker for 8 hours to prepare the liquid phase composition of Example 1.

[0109] Step 2: Preparation of structures for optical devices The composition prepared in step 1 above was applied using a pipette to a small dome shape with a diameter of approximately 3 mm and a thickness of 500 μm or more on a printed circuit board (PCB) equipped with a mini LED chip. Subsequently, exposure was performed using an exposure unit (Heraeus Noblelight Benchtop Conveyor / UV-A with a standard intensity of 2,500 mW) at 3 J / cm². 2The lens-shaped protective layer was formed by fully curing it by exposure to a certain irradiation dose for 12 seconds. As a result, a structure for an optical device was obtained in which a mini LED chip on a PCB is surrounded by a lens-shaped protective layer.

[0110] Examples 2-7 and Comparative Examples 1-10 Liquid phase compositions were prepared by repeating the procedure in Step 1 of Example 1 according to the compositions of Examples 2-7 and Comparative Examples 1-10 shown in Table 3 below. Using each of the compositions thus obtained, structures for optical devices were fabricated according to the procedure in Step 2 of Example 1.

[0111] [Table 3]

[0112] [Table 4]

[0113] Test Example 1 The following tests were performed on the compositions obtained in Step 1 of the Examples and Comparative Examples.

[0114] (1) Evaluation of the viscosity of the composition The viscosity of the composition was measured at 25°C using a Brookfield viscometer.

[0115] (2) Evaluation of solvent-free preparation The composition was examined to determine if it was completely transparent when observed with the naked eye. -○: No solid objects were observed with the naked eye. -×: Solid objects were observed with the naked eye.

[0116] (3) Evaluation of refractive index The refractive index of the compositions was measured. As a result, the refractive index of all compositions in Examples 1 to 7 was measured to be 1.5 or higher.

[0117] Test Example 2 The following tests were performed on the protective layer of the structure for the optical device obtained in Step 2 of the Examples and Comparative Examples.

[0118] (1) Evaluation of bubbles The presence or absence of air bubbles in the protective layer was examined using an optical microscope. -○: No bubbles were observed. -×: Bubbles were observed.

[0119] (2) Evaluation of pattern shape The pattern shape of the protective layer was examined using an optical microscope. -○: Regular dome shape -×: Irregular dome shape

[0120] (3) Measurement of reproducibility The diameter and thickness of the five protective layers were measured using calipers, and the reproducibility was evaluated by calculating the diameter-to-thickness ratio (aspect ratio). -○: Good reproducibility -×: Poor reproducibility

[0121] (4) Measurement of degree of hardening The top of the protective layer was pressed vertically with a fingernail to check for the presence of a fingernail mark and for any rupture of the protective layer. -○: No fingernail mark was left when pressed with a fingernail. -×: When pressed with a fingernail, a fingernail mark or fracture occurs.

[0122] (5) Measurement of Yellowness Index (YI) The yellowness index (YI) of the protective layer was measured using a spectrophotometer (SD4000 manufactured by Nippon Denshoku Industries). -○: YI less than or equal to 1.0 (see Figure 5a) -×: YI greater than 1.0 (see Figure 5b)

[0123] (6) Evaluation of diameter-to-thickness ratio (aspect ratio) Referring to Figure 2, the diameter (D) and thickness (t) of the protective layer were measured using calipers, and the diameter-to-thickness ratio (D / t) was calculated based on these measurements.

[0124] In addition, the diameter-to-thickness ratio was evaluated according to the following criteria. -○: When the diameter is 3.0 ± 0.1 mm and the thickness is greater than 500 μm (see Figure 4a) -Δ: When the diameter is 3.0 ± 0.1 mm and the thickness is 200 to 500 μm -×: When the diameter is 3.0 ± 0.1 mm and the thickness is less than 200 μm (see Figure 4b)

[0125] The test results are shown in the table below.

[0126] [Table 5]

[0127] [Table 6]

[0128] As can be seen from the above test results of the compositions prepared in Examples 1-7 using solvent-free diluents without solvents, they maintained their transparency, adjusted their viscosity within a specific range, and exhibited excellent refractive indices. In addition, in the compositions of Examples 1-7, functional groups that react with acids were introduced into the polysiloxane, and a photoacid generator was used, thereby shortening the curing time and satisfying pattern reproducibility and physical properties. Since there is no need to use a platinum catalyst, the problem of discoloration due to platinum adsorption during the process does not occur. Therefore, it was confirmed that the protective layers obtained by photocuring of the compositions of Examples 1-7 were bubble-free, had a regular and reproducible pattern shape, exhibited excellent curing degree, and had a low yellowness index. In particular, the protective layers of Examples 1-7 had an excellent diameter-to-thickness ratio, and as a result, they not only protect the mini LED chip from external heat or moisture but can also help improve optical properties such as brightness and contrast ratio of the light emitted from the LED chip through the light diffusion effect.

[0129] In contrast, the compositions prepared in Comparative Examples 1 to 10 were outside the range of the preferred structure of the present invention (i.e., the viscosity of the polysiloxane was outside a specific range, an acrylic binder was used, a thermoacid generator was used, and the diluent did not have a functional group that reacts with the acid, or the solvent was used in a content exceeding a specific level), and therefore they were insufficient in at least one test. [Explanation of Symbols]

[0130] 10 Structures for optical devices 100 Base material layer 200 luminescent elements 300 protective layer 301 Photocurable Siloxane Resin Composition D Diameter of the protective layer t Thickness of the protective layer

Claims

1. A structure for an optical device, comprising a substrate layer, a light-emitting element formed on the substrate layer, and a protective layer surrounding the light-emitting element, The protective layer comprises a photocured material of a photocurable siloxane resin composition, and The aforementioned photocurable siloxane resin composition is (A) A polysiloxane having a functional group that reacts with an acid, (B) Photoacid generator and (C) A solvent-free diluent having a functional group that reacts with an acid, A structure for an optical device, wherein the viscosity of the polysiloxane is 10,000 cP to 50,000 cP at 25°C, and the solvent content in the composition is less than 4.0% by weight.

2. The structure for an optical device according to claim 1, wherein the photocurable siloxane resin composition has a viscosity of 20,000 cP to 40,000 cP at 25°C.

3. The structure for an optical device according to claim 1, wherein the protective layer has a lens shape for diffusing light.

4. The protective layer is given by the following relation (1): 7.0>D / t (1) (In the formula, D is the diameter of the protective layer (mm), and t is the thickness of the protective layer (mm).) A structure for an optical device according to claim 3, satisfying the requirements.

5. The structure for an optical device according to claim 1, wherein the protective layer has a refractive index of 1.5 or more.

6. The polysiloxane is expressed by the following formula 1: [Formula 1] R 1 p R 2 q SiO (4-p-q)/2 (In equation 1 above, p and q satisfy 1 ≤ p + q ≤ 3 and 0 ≤ q, and p:q is 3:1 to 1:0, R 1 However, it contains a cyclic ether group having 2 to 6 carbon atoms, and R 2 (However, it contains an aryl group or aralkyl group having 6 to 15 carbon atoms.) A structure for an optical device according to claim 1, having an average structure represented by [the specified method].

7. The structure for an optical device according to claim 6, wherein the polysiloxane comprises (a-1) structural units derived from a silane compound containing a cyclic ether group and (a-2) structural units derived from a silane compound containing an aryl group or an aralkyl group.

8. The silane compound containing a cyclic ether group is given by the following formula 2a: [Formula 2a] R 1 a Si(OR 3 ) 4-a (In equation 2a, a is an integer from 1 to 3, and R 1 Each contains a cyclic ether group having 2 to 6 carbon atoms, and R 3 However, it is an alkyl group having 1 to 6 carbon atoms. A structure for an optical device according to claim 7, which is at least one silane compound represented by or a hydrolysate thereof.

9. The silane compound containing an aryl group or an aralkyl group is given by the following formula 2b: [Formula 2b] R 2 b Si(OR 3 ) 4-b (In equation 2b, b is an integer from 1 to 3, and R 2 Each contains an aryl group or aralkyl group having 6 to 15 carbon atoms, and R 3 However, it is an alkyl group having 1 to 6 carbon atoms. A structure for an optical device according to claim 7, which is at least one silane compound represented by or a hydrolysate thereof.

10. The structure for an optical device according to claim 1, wherein the content of the photoacid generator is 0.01 to 10 parts by weight based on 100 parts by weight of the polysiloxane content.

11. The structure for an optical device according to claim 1, wherein the content of the diluent is 0.01 to 10 parts by weight based on 100 parts by weight of the polysiloxane content, and 30 parts by weight or more based on 100 parts by weight of the total content of the photoacid generator and the diluent.

12. The structure for an optical device according to claim 1, wherein the diluent is a monomer having an epoxy group or a glycidyl group.

13. The structure for an optical device according to claim 1, wherein the light-emitting element includes a light-emitting diode (LED) chip.

14. A process for manufacturing a substrate layer and a light-emitting element formed on the substrate layer, A step of applying a photocurable siloxane resin composition to the light-emitting element, A method for fabricating a structure for an optical device, comprising the steps of irradiating the photocurable siloxane resin composition with light to form a protective layer surrounding the light-emitting element, A method wherein the photocurable siloxane resin composition comprises (A) a polysiloxane having a functional group that reacts with an acid, (B) a photoacid generator, and (C) a solvent-free diluent having a functional group that reacts with an acid, wherein the viscosity of the polysiloxane is 10,000 cP to 50,000 cP at 25°C, and the solvent content in the composition is less than 4.0% by weight.

15. A photocurable siloxane resin composition comprising (A) a polysiloxane having a functional group that reacts with an acid, (B) a photoacid generator, and (C) a solvent-free diluent having a functional group that reacts with an acid, The solvent-free diluent is a monomer having an epoxy group or a glycidyl group. A photocurable siloxane resin composition wherein the viscosity of the polysiloxane is 10,000 cP to 50,000 cP at 25°C, and the solvent content in the composition is less than 4.0% by weight.