Method for manufacturing a TiO2-containing silica glass substrate
The described manufacturing method for TiO2-containing silica glass addresses striations and thermal expansion issues, producing a substrate with ultra-high smoothness and low CTE-slope, suitable for optical applications.
Patent Information
- Application Number
- JP2026205839
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2021-09-08
- Filing Date
- 2026-09-14
- Publication Date
- 2026-11-19
AI Technical Summary
Existing methods for producing TiO2-containing silica glass struggle with periodic striations and uneven thermal expansion, making it difficult to achieve ultra-smooth surfaces and precise thermal expansion characteristics, especially in optical applications.
A manufacturing method involving the preparation of raw material powder, molding, and firing, with slurry dehydration and filtration, followed by calcination, to produce a TiO2-containing silica glass substrate with controlled TiO2 concentration and low CTE-slope, ensuring no striations on both main and end surfaces.
The method results in a TiO2-containing silica glass substrate with ultra-high smoothness and low thermal expansion, meeting strict optical application requirements by eliminating striations and achieving a CTE-slope of 1.40 ppb/K/K or less.
Smart Images

Figure 2026183069000002 
Figure 2026183069000003 
Figure 2026183069000004
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a TiO2-containing silica glass substrate.
BACKGROUND ART
[0002] Silica glass containing TiO2 is known as an ultra-low thermal expansion material, and the coefficient of thermal expansion can be adjusted by regulating the TiO2 content, making it possible to achieve a substantially zero coefficient of thermal expansion within a specific temperature range, that is, to realize zero expansion. For this reason, TiO2-containing silica glass has drawn attention as a suitable material for applications where low thermal expansion property and smoothness are strictly required, for example, precision component materials such as optical component materials, large-sized reflector substrate materials, and reference gauges for precision measurement, as well as optical materials for exposure apparatuses for EUV (Extreme Ultra Violet) lithography.
[0003] As methods for producing TiO2-containing silica glass, a vapor phase method (for example, Patent Documents 1 and 2) and a liquid phase method (for example, Patent Document 3) are known. The vapor phase method includes a direct method and an indirect method. The direct method is a production method for obtaining TiO2-containing silica glass, in which TiO2-containing silica glass fine particles (soot) obtained by subjecting a glass raw material to flame hydrolysis or thermal decomposition are deposited on a base material and simultaneously vitrified into a transparent glass. The indirect method is a production method for obtaining TiO2-containing silica glass, in which TiO2-containing silica glass fine particles (soot) obtained by subjecting a glass raw material to flame hydrolysis or thermal decomposition are deposited and grown on a base material to obtain a porous TiO2-containing silica glass, which is then heated to a temperature equal to or higher than the transparent vitrification temperature to obtain the TiO2-containing silica glass. The liquid phase method is a production method in which glass raw material powder is made into a slurry, which is then dried and subjected to heat treatment to be vitrified into a transparent glass.
PRIOR ART DOCUMENTS
PATENT DOCUMENTS
[0004]
PATENT DOCUMENT 1
PATENT DOCUMENT 2
[0005] In the vapor phase process, periodic fluctuations (streaks) occur in the TiO2 / SiO2 composition ratio of the glass due to the thermal history during the manufacturing process. The presence of these striaks makes it difficult to obtain a surface with ultra-high smoothness even by mirror polishing, which is undesirable for optical applications. Therefore, various methods have been investigated to suppress these striaks (Patent Documents 1 and 2). However, none of these methods can fundamentally eliminate pulse patterns; they merely suppress them. In the Qi physiognomy method, it is difficult to completely prevent the generation of pulse patterns.
[0006] On the other hand, in the liquid-phase method disclosed in Patent Document 3, the periodic striations on the glass surface described above are thought to be suppressed more than in the gas-phase method. Here, in order to suppress changes in the shape of the substrate caused by temperature changes during use, it is desirable that the rate of change of the thermal expansion coefficient of the glass (CTE-Slope) be low. For example, when the glass substrate expands in volume during exposure, distortion occurs in the image and the exposure characteristics deteriorate. However, if raw materials with an average particle size as shown in Patent Document 3 are used, it is difficult to control the OH concentration in the glass, and as a result it becomes extremely difficult to achieve a low CTE-Slope. Furthermore, the particle size of the raw materials is also likely to affect the homogeneity of the TiO2 concentration in the glass.
[0007] Thus, even with the liquid-phase method, obtaining homogeneous glass is difficult, and there was room for improvement in completely suppressing the occurrence of striations. Furthermore, striations are not necessarily parallel to the main surface; they can also exist in the direction of the end face. In view of the above, the present invention aims to provide a TiO2-containing silica glass substrate that has a low CTE-Slope and is free of striations on any surface, including not only the main surface but also the end surfaces. [Means for solving the problem]
[0008] The present invention provides a method for manufacturing a silica glass substrate that solves the above problems, as described below. [1] A method for manufacturing a TiO2-containing silica glass substrate, comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it, To prepare a slurry containing the aforementioned raw material powder, and The slurry is dehydrated and filtered, and then calcined. The TiO2-containing silica glass substrate has a TiO2 concentration distribution of 0.01% by mass or less. A method for manufacturing a TiO2-containing silica glass substrate, wherein the TiO2-containing silica glass substrate contains 6.7 to 12% by mass of TiO2 on an oxide-based mass percentage basis, has a CTE-slope of 1.40 ppb / K / K or less, and shows no striations in striation evaluation according to JOGIS-11 (2008) on at least one main surface and at least one end surface. [2] A method for manufacturing a TiO2-containing silica glass substrate, comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it, To prepare a slurry containing the aforementioned raw material powder, and The slurry is dehydrated and filtered, and then calcined. The TiO2-containing silica glass substrate has a TiO2 concentration distribution of 0.01% by mass or less. The TiO2-containing silica glass substrate is characterized by containing 6.7 to 12% by mass of TiO2 on an oxide-based mass percentage basis, having a CTE-slope of 1.40 ppb / K / K or less, and having a striation strength on at least one main surface and at least one end surface that conforms to Class A of the US military standard: MIL-G174B. [3] A method for manufacturing a TiO2-containing silica glass substrate, comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it, To prepare a slurry containing the aforementioned raw material powder, and The process includes dispersing the slurry using at least one of a wet jet mill, a ball mill, or a bead mill. The TiO2-containing silica glass substrate has a TiO2 concentration distribution of 0.01% by mass or less. A method for manufacturing a TiO2-containing silica glass substrate, wherein the TiO2-containing silica glass substrate contains 6.7 to 12% by mass of TiO2 on an oxide-based mass percentage basis, has a CTE-slope of 1.40 ppb / K / K or less, and shows no striations in striation evaluation according to JOGIS-11 (2008) on at least one main surface and at least one end surface. [4] A method for manufacturing a TiO2-containing silica glass substrate, comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it, To prepare a slurry containing the aforementioned raw material powder, and The process includes dispersing the slurry using at least one of a wet jet mill, a ball mill, or a bead mill. The TiO2-containing silica glass substrate has a TiO2 concentration distribution of 0.01% by mass or less. The TiO2-containing silica glass substrate is characterized by containing 6.7 to 12% by mass of TiO2 on an oxide-based mass percentage basis, having a CTE-slope of 1.40 ppb / K / K or less, and having a striation strength on at least one main surface and at least one end surface that conforms to Class A of the US military standard: MIL-G174B. [5] A method for manufacturing a TiO2-containing silica glass substrate, comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it, This includes preparing a slurry containing the aforementioned raw material powder and a binder. The TiO2-containing silica glass substrate has a TiO2 concentration distribution of 0.01% by mass or less. A method for producing a TiO2-containing silica glass substrate, wherein the TiO2-containing silica glass substrate contains 6.7 to 12 mass% of TiO2 in terms of mass percentage on an oxide basis, has a CTE-slope of 1.40 ppb / K / K or less, and no striae are observed in striae evaluation in accordance with JOGIS-11 (2008) on at least one main surface and at least one end surface. [6] A method for producing a TiO2-containing silica glass substrate, comprising the steps of preparing a raw material powder, shaping the raw material powder, and then firing the shaped raw material powder, wherein the method comprises preparing a slurry containing the raw material powder and a binder, the TiO2-containing silica glass substrate has a TiO2 concentration distribution of 0.01 mass% or less, A method for producing a TiO2-containing silica glass substrate, wherein the TiO2-containing silica glass substrate contains 6.7 to 12 mass% of TiO2 in terms of mass percentage on an oxide basis, has a CTE-slope of 1.40 ppb / K / K or less, and the striae intensity on at least one main surface and at least one end surface falls under Class A of US Military Standard: MIL-G174B. [Effects of the Invention]
[0009] The TiO2-containing silica glass substrate of the present invention has a low CTE-Slope, and no striae are observed on any surface including not only the main surfaces but also the end surfaces. Therefore, the TiO2-containing silica glass substrate of the present invention has low thermal expansion, and a surface with ultra-high smoothness can be easily obtained by mirror polishing. [Brief Description of the Drawings]
[0010] [Figure 1] Figure 1 shows the striae evaluation results of a standard sample in accordance with JOGIS. [Figure 2] Figure 2 shows the striae evaluation results in accordance with JOGIS in the end surface direction of Example 1. [Figure 3] Figure 3 shows the striae evaluation results in accordance with JOGIS in the end surface direction of Example 3. [Figure 4] Figure 4 shows the class evaluation results of a standard sample in accordance with US Military Standard. [Figure 5] Figure 5 shows the class evaluation results according to U.S. military standards for the end face direction in Example 1. [Figure 6] Figure 6 shows the class evaluation results according to U.S. military standards for the end face direction in Example 3. [Modes for carrying out the invention]
[0011] The embodiments of the present invention will be described in detail below. However, the present invention is not limited to the embodiments described below.
[0012] The silica glass substrate of this embodiment (hereinafter also simply referred to as "the glass substrate of this embodiment") has a TiO2 content of 6.7 to 12% by mass on an oxide basis, has a CTE-slope of 1.40 ppb / K / K or less, and is a silica glass substrate in which striations are not observed in striation evaluation in accordance with JOGIS-11 (2008) on at least one main surface and at least one end surface. Furthermore, the silica glass substrate of this embodiment has a TiO2 content of 6.7 to 12% by mass on an oxide basis, has a CTE-slope of 1.40 ppb / K / K or less, and is a silica glass substrate that conforms to MIL-G174B Class A on at least one main surface and at least one end surface. The glass substrate in question will be described in detail below.
[0013] If the TiO2 content of the glass substrate in this embodiment is too high, the coefficient of thermal expansion may become too large, and if it is too low, the coefficient of thermal expansion may become negative. In either case, zero expansion may not be achievable. Therefore, the TiO2 content of the glass substrate in this embodiment is 6.7% by mass or more, preferably 7.0% by mass or more, more preferably 7.5% by mass or more, and also 12% by mass or less, preferably 11% by mass or less, more preferably 10% by mass or less.
[0014] The remainder of the glass substrate in this embodiment mainly consists of SiO2. The SiO2 content of the glass substrate in this embodiment is, for example, 88% by mass or more, preferably 89% by mass or more, more preferably 90% by mass or more, and also, for example, 93.3% by mass or less, preferably 93% by mass or less, more preferably 92.5% by mass or less.
[0015] Furthermore, the glass substrate of this embodiment may contain components other than SiO2 and TiO2, as long as they do not impair the effects of the present invention. For example, the glass substrate of this embodiment may contain oxides of Ce, B, P, Ge, Zr, etc.
[0016] In this embodiment, the glass substrate preferably has a TiO2 concentration distribution of 0.1% by mass or less. Having a TiO2 concentration distribution within the substrate within this range ensures stable thermal expansion characteristics. The TiO2 concentration distribution of the glass substrate can be measured using X-ray fluorescence.
[0017] In this embodiment, the glass substrate preferably has an OH group concentration of 600 ppm by mass or more. An OH group concentration of 600 ppm by mass or more in the glass substrate makes it possible to reduce the gradient of the CTE-slope. More preferably, the OH group concentration is 700 ppm by mass or more, and even more preferably 800 ppm by mass or more. Furthermore, if the OH group concentration is 1200 ppm by mass or less, the effect on glass hardness is small, and it is less likely to lead to an increase in defects during polishing. Preferably, it is 1100 ppm by mass or less, and more preferably 1000 ppm by mass or less.
[0018] The OH concentration of the glass substrate depends heavily on the particle size of the silica raw material. This is thought to be due to the presence of isolated silanol groups on the surface of the silica raw material. The smaller the particle size of the raw material, the higher the sintering rate, and as a result, the desorption of silanol groups is suppressed. Therefore, it was observed that the OH concentration of the glass substrate tends to increase with a larger specific surface area of the raw material. By using raw material with a BET particle size of less than 30 nm, it is possible to achieve an OH concentration of 600 ppm by mass or more in the glass substrate. While it is possible to increase the OH concentration of the glass substrate by reducing the particle size of the raw material, it becomes very difficult to increase the solid content concentration in the liquid when it is formed into a slurry, making it unsuitable for manufacturing methods that involve adding a gelling agent to induce gelation, such as the sol-gel method.
[0019] Furthermore, the OH concentration can be measured using known methods. For example, the OH concentration can be determined from the absorption peak at a wavelength of 2.7 μm by measuring with an infrared spectrophotometer (JP Williams et.al., American Ceramic Science Bulletin, 55(5), 524, 1976).
[0020] The glass substrate of this embodiment has a CTE-slope of 1.40 ppb / K / K or less. CTE-slope refers to the slope of the CTE at the temperature (COT) where the coefficient of thermal expansion (CTE) is 0 ppb / K. A smaller CTE-slope is preferable because it indicates better thermal expansion characteristics. The glass substrate of this embodiment preferably has a CTE-slope of 1.30 ppb / K / K or less. Furthermore, in order to achieve a CTE-slope of 1.40 ppb / K / K or less, it is preferable that the OH concentration of the glass substrate is 600 ppm or more. CTE-slope can be measured using an interferometric thermal expander.
[0021] In this embodiment, no striations are observed on at least one main surface and at least one end surface of the glass substrate in the striation evaluation according to the Nippon Optical Glass Manufacturers Association standard JOGIS-11 (2008). In this embodiment, no striations are observed not only on at least one main surface but also on at least one end surface; in other words, it is a highly homogeneous glass substrate. Furthermore, the absence of visible striations means that, in an environment where shadows of 10nm steps projected onto a screen can be observed, shadows caused by striations are not observed. The striation evaluation will be performed in accordance with JOGIS-11 (2008). The sample to be measured will be placed between the projection device and the screen, and the striations will be observed and evaluated by projecting the image onto the screen. The illuminance on the screen will be kept at 50 lux or higher. In addition, the illuminance on the screen will be adjusted using a striation standard sample during measurement. The striation standard sample can be prepared using methods such as vapor deposition or etching. The degree of striations will be evaluated by comparing the projected image of the sample to the projected image of the striation standard sample.
[0022] The glass substrate of this embodiment has striation strength on at least one main surface and at least one end surface that meets the US military standard MIL-G174B Class A. This means that, as described above, the glass substrate of this embodiment is a highly homogeneous glass substrate in which no striations are observed not only on at least one main surface but also on at least one end surface. In striation evaluation based on the US military standard MIL-G174B, parallel light from a monochromatic light source is shone onto the sample through a collimating lens, and the shading of the striations in the sample is evaluated by comparing it with that of a striation standard sample. The striation standard sample can be prepared using methods such as vapor deposition or etching.
[0023] Methods for obtaining a glass substrate in which striations are not observed on either the main surface or the edge surface include, for example, liquid-phase methods such as the sol-gel method described later in the manufacturing process, and zone melting, in which a portion of the glass obtained by the gas-phase method is heated and subjected to homogenization while shearing. However, although zone melting is considered an effective method for reducing striations, it is thought to be extremely difficult to completely remove the striations within a realistic manufacturing timeframe.
[0024] In this embodiment, the glass substrate has at least one main surface and at least one end surface in which the in-plane refractive index variation range Δn is 5 × 10 -5 The following is preferable: Here, the refractive index corresponds to the bias in the TiO2 / SiO2 composition ratio. In a TiO2-containing silica glass substrate, if there is a large bias in the TiO2 / SiO2 composition ratio, it becomes very difficult to obtain ultra-high smoothness even by mirror polishing. This is because, in a TiO2-containing silica glass substrate, the polishing rate is not constant because the mechanical and chemical properties of the glass differ depending on the composition ratio in areas where the TiO2 / SiO2 composition ratio is different. Since the refractive index also differs when the TiO2 / SiO2 composition ratio is different, the bias in the TiO2 / SiO2 composition ratio can be evaluated by the refractive index. The glass substrate in this embodiment is homogeneous, and therefore, the fluctuation in the refractive index within the plane is small, regardless of whether the measurement is taken from the main surface side or the edge surface side.
[0025] The range of refractive index variation Δn in the plane is preferably 5 × 10⁻⁶. -5 The following is true: The glass substrate of this embodiment has a small refractive index variation Δn on both the main surface and the edge surface, meaning it is a homogeneous glass with little bias in the TiO2 / SiO2 composition ratio, and therefore ultra-high smoothness can be easily obtained by mirror polishing.
[0026] The refractive index variation range (Δn) refers to the range of refractive index variation measured relative to the measurement surface of a measurement sample cut from a glass substrate, which has a measurement surface of a predetermined size. The measurement sample is cut so that the measurement surface of the sample is parallel to the surface being measured for Δn. That is, when measuring Δn on the main surface of a glass substrate, a measurement sample with a measurement surface parallel to the main surface is cut and measured. When measuring Δn on an edge surface of a glass substrate, a measurement sample with a measurement surface parallel to the edge surface is cut and measured. The size of the measurement sample is not particularly limited, but it should be sized such that the measurement surface provides a measurement area large enough to adequately detect changes in refractive index.
[0027] The method for measuring the refractive index fluctuation range Δn differs depending on whether the fluctuation range is Δn1 over a small area or Δn2 over a wide area, as shown below.
[0028] The range of refractive index variation Δn1 in a small region is measured as follows. A measurement sample (e.g., 6mm x 30mm x 1mm) is cut from a glass substrate, sized to ensure a measurement area (e.g., 3mm x 3mm) large enough to adequately detect refractive index fluctuations in a small region. Using a Fizeau interferometer, a helium-neon laser beam is shone perpendicularly onto the measurement area (e.g., 3mm x 3mm) of the measurement surface of this sample to examine the refractive index distribution within the plane and determine the refractive index fluctuation range Δn1, i.e., the difference between the maximum and minimum refractive index values within the plane. Furthermore, depending on the number of effective pixels in the interferometer's CCD, the size of one pixel may not be sufficiently small compared to the width of the striae, potentially making it impossible to detect the striae. In this case, the measurement area is divided into multiple minute regions, and the refractive index variation Δn in each minute region is measured. 1x The value is measured, and its maximum value is defined as the refractive index variation range Δn1.
[0029] The range of refractive index variation Δn2 over a wide area, such as the surface (main surface) irradiated with EUV light used for exposure, is measured by cutting a measurement sample from a glass substrate that is large enough to secure a measurement area (for example, a measurement area of 100 mm x 100 mm) that can sufficiently detect the refractive index variation over a wide area, and performing the measurement in the same manner. Furthermore, if Δn1 measured on the same surface is greater than Δn2, Δn1 is taken as Δn, and if Δn2 is greater than or equal to Δn1, Δn2 is taken as Δn.
[0030] Furthermore, the TiO2 content can be measured using an electron beam microanalyzer (EPMA), and the refractive index can be determined using the following formula (A). Formula (A) is valid for TiO2-containing silica glass when the TiO2 content is 12% by mass or less. Refractive index = 3.27 × 10⁻⁶ -3 ×TiO2 content (mass%) + 1.459 (A)
[0031] The thickness of the glass substrate and the dimensions of the main surface in this embodiment are not particularly limited, but it is preferable that, for example, the length of each side forming the main surface is 150 mm or more and the thickness is 6.0 mm or more.
[0032] The glass substrate of this embodiment preferably does not contain air bubbles larger than 10 μm. Air bubbles larger than 10 μm affect the flatness during polishing, so it is preferable that they not be present. One method to prevent the inclusion of air bubbles larger than 10 μm is to use a slurry with a sharp particle size distribution that does not contain coarse particles. It has been confirmed that coarse particles in the slurry form a heterogeneous layer when forming a wet cake, and remain as bubbles after densification.
[0033] In glass substrates with striations, even after mirror polishing, undulations with a pitch similar to the striation pitch occur on the surface, making it extremely difficult to achieve the low level of smoothness described above. On the other hand, since the glass of this embodiment is homogeneous, the low level of smoothness described above can be easily obtained by mirror polishing. The smoothness of the main surface of a glass substrate can be measured, for example, using a non-contact surface shape measuring instrument (Zygo NewView5032).
[0034] [Manufacturing method for silica glass substrates] Next, as an example of a method for manufacturing the glass substrate of this embodiment, a liquid-phase method (sol-gel method) will be described. Note that the method for manufacturing the glass substrate of this embodiment is not limited to the method described below.
[0035] The method for producing TiO2-containing silica glass according to this embodiment using the liquid phase method (hereinafter also referred to as "this manufacturing method") comprises the following steps (1) to (5). (1) Slurry manufacturing process (2) Dispersion process (3) Dehydration filtration process (4) Drying process (5) Heat treatment process Furthermore, this manufacturing method may include steps other than those described in (1) to (5) above. For example, it may include a step of processing to a desired dimension after the heat treatment step, or a step of mirror polishing.
[0036] <Slurry Manufacturing Process> The slurry manufacturing process is a process for producing a raw material slurry in which raw material powders are dispersed as primary particles in a dispersion medium. Silica powder and titania powder are used as raw material powders, and these are mixed to achieve the desired TiO2 / SiO2 composition ratio. When water is used as the dispersion medium, it is preferable to use titania-containing silica powder to prevent titanium aggregation and precipitation. To obtain uniform glass, the BET diameter of the raw material powder (i.e., silica powder and titania powder) is preferably small, for example, 150 nm or less is preferred, 100 nm or less is more preferred, 40 nm or less is even more preferred, and 30 nm or less is particularly preferred. On the other hand, if the particle size of the raw material is too small, it will lead to a decrease in the solid content concentration in the slurry, an increase in filtration resistance during dewatering filtration, and as a result, a significant decrease in productivity. Therefore, it is preferable that the BET diameter of the raw material powder be 10 nm or more. The dispersion medium is not particularly limited, but water can be used, for example. Furthermore, additives such as pH adjusters, surfactants, dispersants, and binders may be added to the raw material slurry as appropriate. These raw material powders and additives are dispersed in a dispersion medium to obtain a raw material slurry. By using a slurry with a sharp particle size distribution that does not contain coarse particles, a glass substrate free of air bubbles can be obtained after densification. To obtain a slurry free of coarse particles, it is preferable to remove coarse particles as needed. Methods for removing coarse particles include filtering the slurry using a filter with a desired mesh size. Furthermore, from the viewpoint of suppressing bubbles and internal defects, it is preferable to perform precise dispersion during dispersion. Coarse particles refer to silica aggregates of about 1 μm. By selecting an appropriate filter, coarse particles of 1 μm or larger can be removed. The dispersion equipment used for precise dispersion is not particularly limited, but examples include wet jet mills, ball mills, and bead mills.
[0037] <Dehydration filtration process> In the dehydration and filtration process, solid-liquid separation is performed on the raw material slurry by dehydration and filtration to obtain a wet cake. In the dehydration and filtration process, the slurry, which is homogeneously dispersed on the nano-order, is deposited while maintaining its dispersion state, forming a wet cake (gel). Here, the homogeneity of the wet cake is due to the dispersibility of the slurry. In conventional technology, a method is known in which a wet cake is obtained by adding a gelling agent to the raw material slurry and allowing it to precipitate. In such a method, secondary and tertiary particles are easily formed in the slurry, and the dispersibility of the slurry tends to decrease, so the homogeneity of the resulting wet cake is also thought to be low.
[0038] In this invention, the method of dewatering filtration is not particularly limited, and an appropriate method can be selected; either vacuum filtration or pressure filtration is possible. Vacuum filtration has a simple apparatus structure, but the filtration speed is slow. Pressure filtration uses a pressure vessel, so the apparatus structure is more complex, but it is possible to increase the back pressure, resulting in a faster filtration speed and higher productivity. From a productivity standpoint, pressurized filtration is preferable. While wet cake formation is possible with reduced pressure filtration, the deposition rate is slow, so pressurized filtration is preferable for producing large sizes. Especially when the glass substrate is large, insufficient removal of the dispersion medium during the dewatering and filtration process can lead to cracking or shrinkage of the glass substrate during the drying and heat treatment processes. To prevent such problems, methods such as solvent removal by filtering can be used. One method of solvent removal by filtering involves filling a pressure vessel with slurry and performing solid-liquid separation using a membrane filter. The back pressure can be selected arbitrarily. Higher back pressure increases the filtration rate, but tends to increase desorption from the membrane filter. The mesh size of the membrane filter can also be determined according to the dispersion state of the slurry.
[0039] <Drying process> In the drying process, the wet cake is dried to obtain a dried product. The drying method is not particularly limited, and any suitable method can be used. For example, a dried product can be obtained over approximately 30 days in a constant temperature and humidity environment of 30°C and 60rh%.
[0040] <Heat treatment process> In the heat treatment process, the dried material is subjected to heat treatment. In the heat treatment process, it is preferable to perform heat treatment as shown below, for example. (air firing) First, the dried material is calcined in the atmosphere to burn off any organic matter (binders, etc.) contained within it. The heating temperature and time for the atmospheric calcination are not particularly limited as long as they are sufficient to burn off the contained organic matter, but the heating temperature is typically around 100-800°C and the heating time around 1-100 hours. (Vacuum firing) Next, the dried material from which the organic matter has been burned is subjected to heat treatment under a vacuum atmosphere to vitrify it. The heating temperature and heating time for vacuum firing are not particularly limited as long as they are the temperature and time at which vitrification proceeds, but the heating temperature is, for example, 1250 to 1300°C and the heating time is, for example, 1 to 100 hours. (High-temperature firing) Next, the glass is subjected to further heat treatment at a higher temperature to melt the titania crystals and obtain a uniform glass. The heating temperature and heating time for high-temperature firing are not particularly limited as long as they are sufficient to melt the titania crystals, but the heating temperature is, for example, 1500 to 1700°C and the heating time is, for example, 1 to 100 hours.
[0041] As described above, this specification discloses the following TiO2-containing silica glass substrates. [1] A TiO2-containing silica glass substrate containing 6.7 to 12% by mass of TiO2 on an oxide basis, having a CTE-slope of 1.40 ppb / K / K or less, and in which no striations are observed in striation evaluation in accordance with JOGIS-11 (2008) on at least one main surface and at least one end surface. [2] A TiO2-containing silica glass substrate containing 6.7 to 12% by mass of TiO2 on an oxide basis, having a CTE-slope of 1.40 ppb / K / K or less, and having striation strength on at least one main surface and at least one end surface that conforms to Class A of the US military standard: MIL-G174B. [3] In the at least one main surface and the at least one end surface, the range of variation Δn of the refractive index in the plane is 5 × 10 -5 The TiO2-containing silica glass substrate described in [1] or [2] below. [4] A TiO2-containing silica glass substrate according to any one of [1] to [3], wherein the concentration distribution of TiO2 is 0.1% by mass or less. [5] A TiO2-containing silica glass substrate according to any of [1] to [4], wherein the OH group concentration is 600 ppm by mass or more. [6] A TiO2-containing silica glass substrate according to any of [1] to [5], wherein the length of each side forming the main surface is 150 mm or more and the thickness is 6.0 mm or more. [7] A TiO2-containing silica glass substrate as described in any of [1] to [6], which does not contain bubbles larger than 10 μm. [Examples]
[0042] Hereinafter, the present invention will be specifically described with reference to Examples, but the present invention is not limited thereto.
[0043] <Production of TiO2-containing silica glass substrate> (Example 1) (Slurry production step) 30000 g of commercially available fumed silica powder (BET diameter: 30 nm) and 3500 g of commercially available titania-containing silica powder (BET diameter: 30 nm) were mixed, and further 6500 g of a dispersant (TEAH) and 120000 g of pure water were mixed to produce a raw material slurry. (Dispersion step) The obtained slurry was roughly dispersed with an ultrasonic homogenizer, then subjected to dispersion treatment with a wet jet mill, and coarse particles were removed using a filter with an opening of 1 μm. (Dehydration filtration step) The raw material slurry after the dispersion step was subjected to dehydration filtration under the following conditions to obtain a wet cake. Apparatus: Pressure filter A wet cake was obtained by subjecting the raw material slurry to dehydration filtration. The dehydration filtration was performed by pumping the slurry pressurized to 0.8 MPa into a filter chamber with an internal dimension of φ230 × 30, and a wet cake of Φ230 × 23 mm was obtained. (Drying step) The obtained wet cake was formed into a plate shape of Φ230 mm × 23 mm, and dried for 720 hours in an environment of 30°C and 60% RH. (Heat treatment step) Firing was performed in the air at 600°C for 10 hours to remove the dispersant and the binder. Further, firing was performed in a vacuum atmosphere at 1280°C for 2 hours to perform vitrification. Then, heat treatment was performed in an argon atmosphere at 1600°C for 10 hours to dissolve titania crystals, thereby obtaining a glass substrate.
[0044] (Example 2) A glass substrate of Example 2 was obtained in the same manner as in Example 1, except that a commercially available fumed silica powder having a BET diameter of 40 nm was used as the fumed silica powder.
[0045] (Example 3) A commercially available silica-titania doped low-expansion glass material was used as the glass substrate of Example 3.
[0046] (Example 4) A glass substrate of Example 4 was obtained in the same manner as Example 1, except that in the dispersion step, a slurry subjected only to rough dispersion by an ultrasonic homogenizer was used without performing the fine dispersion treatment by a wet jet mill.
[0047] The evaluations shown below were performed on the glass substrates of each example. The results are shown in the table described later. Note that Example 1 and Example 4 are working examples, and Example 2 and Example 3 are comparative examples.
[0048] <TiO₂ Concentration Distribution> For the TiO₂ concentration distribution, 81 points in a 9×9 in-plane arrangement were measured using a fluorescent X-ray measuring apparatus (primus400) manufactured by Rigaku Corporation, and the PV value was calculated.
[0049] <OH Group Concentration> Evaluation was performed using an FT-IR apparatus.
[0050] <cte-slope> A measurement sample with a cross-section of 35 mm × 10 mm and a length of 100 mm was cut out from each glass substrate, and its CTE in the longitudinal direction was precisely measured in the range of -150 to +200°C using a laser heterodyne interference type thermal dilatometer. Then, the value of CTE-Slope was calculated from the measurement results.
[0051] <Refractive index variation range> From each glass substrate, 6 mm × 30 mm × 1 mm measurement samples were cut out for the main surface and the end surface respectively. The measurement samples were cut out such that the 6 mm × 30 mm surface (measurement surface) was parallel to the main surface or the end surface. Within a 3 mm × 3 mm range on the measurement surface of the measurement sample, the in-plane refractive index variation range (Δn) was measured using a two-beam interferometer (transmission two-beam interference microscope (TD series) manufactured by Mizojiri Optical Co., Ltd.).
[0052] <Presence or absence of bubbles of 10 μm or larger> The bubble evaluation was carried out by visual inspection.
[0053] <Striae evaluation> Striae evaluation of the main surface and end surface of each glass substrate was performed in accordance with JOGIS-11 2008. Using a striae standard sample with an optical path difference of 6 nm, the main surface and end surface of the glass substrate were evaluated after confirming that shadows were generated when irradiated onto a screen. It was evaluated that striae existed when a shadow was projected on the screen, and it was evaluated that no striae existed when no shadow was projected. For the standard sample, a sample having a spike-like refractive index difference was prepared by varying the input raw material during the hydrolysis reaction using a vapor phase method. Figure 1 shows the striae evaluation results in the end surface direction of the standard sample, Figure 2 shows those of Example 1, and Figure 3 shows those of Example 3, respectively.
[0054] <MIL-G174B class evaluation> Similar to the striae evaluation of JOGIS, a striae standard sample with an optical path difference of 10 nm was prepared, and class evaluation of the main surface and end surface was performed. Figure 4 shows the class evaluation results in the end surface direction of the standard sample, Figure 5 shows those of Example 1, and Figure 6 shows those of Example 3, respectively.
[0055] [Table 1]
[0056] Based on the above results, the glass substrates of Example 1 and Example 4 showed no striations on the main surface and edge surface in both JOGIS and US military standards evaluations, and the CTE-Slope was sufficiently low. Furthermore, no bubbles larger than 10 μm were observed in the glass substrate of Example 1, resulting in a homogeneous glass. In Example 2, the glass substrate had a high CTE-Slope, while in Example 3, striations were observed at the edge. In Example 4, the glass substrate showed results similar to Example 1 regarding striations, but multiple air bubbles were found to remain within the substrate.
[0057] Although the present invention has been described in detail and with reference to specific embodiments, it will be apparent to those skilled in the art that various changes and modifications can be made without departing from the spirit and scope of the invention. This application is based on Japanese Patent Application No. 2021-146400, filed on 8 September 2021, the contents of which are incorporated herein by reference.
Claims
1. A TiO2 process comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it. 2 A method for manufacturing a silica glass substrate containing silica, To prepare a slurry containing the aforementioned raw material powder, and The slurry is dehydrated and filtered, and then calcined. The TiO 2 The silica glass substrate contains TiO 2 The concentration distribution is 0.01% by mass or less. The TiO 2 The silica glass substrate contains 6.7 to 12% by mass of TiO2, expressed as a mass percentage based on oxide. 2 It contains TiO2, has a CTE-slope of 1.40 ppb / K / K or less, and on at least one main surface and at least one end surface, no striations are observed in striation evaluation according to JOGIS-11 (2008). 2 A method for manufacturing a silica-containing glass substrate.
2. A TiO2 process comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it. 2 A method for manufacturing a silica glass substrate containing silica, To prepare a slurry containing the aforementioned raw material powder, and The slurry is dehydrated and filtered, and then calcined. The aforementioned TiO 2 The silica glass substrate containing TiO has a TiO 2 concentration distribution of 0.01 mass% or less, The TiO 2 The silica glass substrate contains 6.7 to 12% by mass of TiO2, expressed as a mass percentage based on oxide. 2 It contains TiO2, has a CTE-slope of 1.40 ppb / K / K or less, and on at least one main surface and at least one end surface, the striation strength corresponds to Class A of the US military standard: MIL-G174B. 2 A method for manufacturing a silica-containing glass substrate.
3. A TiO2 process comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it. 2 A method for manufacturing a silica glass substrate containing silica, To prepare a slurry containing the aforementioned raw material powder, and The process includes dispersing the slurry using at least one of a wet jet mill, a ball mill, or a bead mill. The TiO 2 The silica glass substrate contains TiO 2 The concentration distribution is 0.01% by mass or less. The TiO 2 The silica glass substrate contains 6.7 to 12% by mass of TiO2, expressed as a mass percentage based on oxide. 2 It contains TiO2, has a CTE-slope of 1.40 ppb / K / K or less, and on at least one main surface and at least one end surface, no striations are observed in striation evaluation according to JOGIS-11 (2008). 2 A method for manufacturing a silica-containing glass substrate.
4. A TiO2 process comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it. 2 A method for manufacturing a silica glass substrate containing silica, To prepare a slurry containing the aforementioned raw material powder, and The process includes dispersing the slurry using at least one of a wet jet mill, a ball mill, or a bead mill. The TiO 2 The silica glass substrate contains TiO 2 The concentration distribution is 0.01% by mass or less. The TiO 2 The silica glass substrate contains 6.7 to 12% by mass of TiO2, expressed as a mass percentage based on oxide. 2 It contains TiO2, has a CTE-slope of 1.40 ppb / K / K or less, and on at least one main surface and at least one end surface, the striation strength corresponds to Class A of the US military standard: MIL-G174B. 2 A method for manufacturing a silica-containing glass substrate.
5. A TiO2 process comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it. 2 A method for manufacturing a silica glass substrate containing silica, This includes preparing a slurry containing the aforementioned raw material powder and a binder. The TiO 2 The silica glass substrate contains TiO 2 The concentration distribution is 0.01% by mass or less. The TiO 2 The silica glass substrate contains 6.7 to 12% by mass of TiO2, expressed as a mass percentage based on oxide. 2 It contains TiO2, has a CTE-slope of 1.40 ppb / K / K or less, and on at least one main surface and at least one end surface, no striations are observed in striation evaluation according to JOGIS-11 (2008). 2 A method for manufacturing a silica-containing glass substrate.
6. A TiO2 process comprising the steps of preparing raw material powder, molding the raw material powder, and then firing it. 2 A method for manufacturing a silica glass substrate containing silica, This includes preparing a slurry containing the aforementioned raw material powder and a binder. The TiO 2 The silica glass substrate contains TiO 2 The concentration distribution is 0.01% by mass or less. The TiO 2 The silica glass substrate contains 6.7 to 12% by mass of TiO2, expressed as a mass percentage based on oxide. 2 It contains TiO2, has a CTE-slope of 1.40 ppb / K / K or less, and on at least one main surface and at least one end surface, the striation strength corresponds to Class A of the US military standard: MIL-G174B. 2 A method for manufacturing a silica-containing glass substrate.
7. The TiO 2 A method for manufacturing a silica-containing glass substrate.
8. The TiO according to claim 3 or 4, wherein the slurry is dispersed using a wet jet mill. 2 A method for manufacturing a silica-containing glass substrate.
9. The TiO according to claim 3 or 4, wherein the slurry is dispersed using a ball mill. 2 A method for manufacturing a silica-containing glass substrate.
10. The TiO as described in claim 5 or 6, wherein the firing includes firing in air. 2 A method for manufacturing a silica-containing glass substrate.
11. The raw material powder includes titania-containing silica powder, according to any one of claims 1 to 6. 2 A method for manufacturing a silica-containing glass substrate.
12. In the at least one main surface and the at least one end surface, the in-plane refractive index variation range Δn is 5 × 10 -5 The TiO described in any of claims 1 to 6 is as follows: 2 A method for manufacturing a silica-containing glass substrate.
13. The TiO according to any one of claims 1 to 6, wherein the OH group concentration is 600 ppm by mass or more. 2 A method for manufacturing a silica-containing glass substrate.
14. The TiO according to any one of claims 1 to 6, wherein the length of each side forming the main surface is 150 mm or more, and the thickness is 6.0 mm or more. 2 A method for manufacturing a silica-containing glass substrate.
15. TiO according to any one of claims 1 to 6, which does not contain bubbles larger than 10 μm 2 A method for manufacturing a silica-containing glass substrate.
16. The TiO2 according to any one of claims 1 to 6, wherein the BET diameter of the raw material powder is 100 nm or less. 2 A method for manufacturing a silica-containing glass substrate.
17. The TiO 2 The TiO according to any one of claims 1 to 6, wherein the concentration distribution is 0.005% by mass or less. 2 A method for manufacturing a silica-containing glass substrate.
18. The TiO according to any one of claims 1 to 6, wherein the CTE-slope is 1.20 ppb / K / K or less. 2 A method for manufacturing a silica-containing glass substrate.
Citation Information
Patent Citations
Method and device for hydraulically driving pile
JP1978067204A
Method of manufacturing silica and titania extreme ultraviolet ray optical element