SiC substrates and SiC epitaxial wafers
By employing controlled manufacturing processes, SiC substrates with large diameters and minimal micropipes are produced, addressing the challenge of defect-induced yield loss in SiC devices, resulting in improved device production efficiency.
Patent Information
- Application Number
- JP2026206264
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2026-09-15
- Publication Date
- 2026-11-19
AI Technical Summary
Existing SiC substrates and epitaxial wafers face challenges in achieving large diameters while minimizing micropipes, which are defects that negatively impact device performance and yield.
The production of SiC substrates with diameters of 195 mm or more and micropipe densities of 0.01 pieces/cm² or less is achieved through controlled manufacturing processes, including seed crystal preparation, crucible coating, precise raw material placement, and controlled crystal growth to minimize micropipe formation.
This approach results in SiC substrates and epitaxial wafers with reduced micropipes, enabling the production of a higher number of functional devices per wafer by ensuring micropipe-free regions, thereby enhancing the yield and quality of SiC devices.
Smart Images

Figure 2026183084000001_ABST
Abstract
Description
[Technical Field]
[0001] This invention relates to a SiC substrate and a SiC epitaxial wafer. [Background technology]
[0002] Silicon carbide (SiC) has a dielectric breakdown field that is an order of magnitude larger and a band gap that is three times larger than that of silicon (Si). Furthermore, SiC has properties such as a thermal conductivity that is approximately three times higher than that of silicon (Si). Therefore, SiC is expected to have applications in power devices, high-frequency devices, and high-temperature operating devices. For this reason, SiC epitaxial wafers have recently come into use in semiconductor devices such as those mentioned above.
[0003] SiC epitaxial wafers are obtained by laminating SiC epitaxial layers onto the surface of a SiC substrate. Hereinafter, the substrate before lamination of the SiC epitaxial layers will be referred to as a SiC substrate, and the substrate after lamination of the SiC epitaxial layers will be referred to as a SiC epitaxial wafer. SiC substrates are manufactured by cutting them from a SiC ingot. SiC devices such as power devices, high-frequency devices, and high-temperature operating devices are obtained by forming devices on the SiC epitaxial layer of a SiC epitaxial wafer and then chipping the SiC epitaxial wafer.
[0004] To increase the number of SiC devices that can be obtained from a single SiC epitaxial wafer, there is a need to increase the diameter of SiC substrates and SiC epitaxial wafers. However, increasing the diameter of SiC substrates and SiC epitaxial wafers is not easy. For example, Non-Patent Literature 1 states that as the diameter of SiC substrates and SiC epitaxial wafers increases, the number of defects increases significantly.
[0005] Another type of defect found in SiC substrates is micropipes (see, for example, Patent Document 1). Micropipes are killer defects that negatively impact subsequent processes and SiC devices. For example, micropipes can cause breakdown voltage failure in SiC devices. Micropipes are hollow crystal defects with a diameter ranging from sub-μm to several μm, propagating in the c-axis direction of hexagonal silicon carbide. It is believed that micropipes are formed when helical dislocations with large Burgers vectors relieve strain energy. [Prior art documents] [Patent Documents]
[0006] [Patent Document 1] Japanese Patent Publication No. 2016-127201 [Non-patent literature]
[0007] [Non-Patent Document 1] N. Piluso, E. Carria, R. Anzalone, A Severino. Microelectronic Engineering 273 (2023) 111962. [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] As described in Patent Document 1, micropipes are a defect that is difficult to completely eliminate. Furthermore, this tendency becomes more pronounced when the SiC substrate is large in diameter.
[0009] The present invention has been made in view of the above problems, and aims to provide a SiC substrate and a SiC epitaxial wafer that have a large diameter and few micropipes. [Means for solving the problem]
[0010] The present inventors fabricated a SiC substrate and a SiC epitaxial wafer that have a large diameter and few micropipes.
[0011] (1) The SiC substrate according to the first aspect has a diameter of 195 mm or more, and a micropipe density of 0.01 pieces / cm 2 or less.
[0012] (2) In the SiC substrate according to the above aspect, the number of micropipes in the effective region excluding the edge exclusion region within 3 mm from the outer periphery may be 3 or less.
[0013] (3) In the SiC substrate according to the above aspect, the number of micropipes in the effective region excluding the edge exclusion region within 3 mm from the outer periphery may be 1 or less.
[0014] (4) In the SiC substrate according to the above aspect, 7209 or more of the plurality of first regions, which are obtained by dividing the surface into squares each having an area of 4 mm 2 , may have no micropipes.
[0015] (5) In the SiC substrate according to the above aspect, 3168 or more of the plurality of second regions, which are obtained by dividing the surface into squares each having an area of 9 mm 2 , may have no micropipes.
[0016] (6) In the SiC substrate according to the above aspect, 1764 or more of the plurality of third regions, which are obtained by dividing the surface into squares each having an area of 16 mm 2 , may have no micropipes.
[0017] (7) In the SiC substrate according to the above aspect, 1116 or more of the plurality of fourth regions, which are obtained by dividing the surface into squares each having an area of 25 mm 2 , may have no micropipes.
[0018] (8) In the SiC substrate according to the above aspect, the surface is divided into squares each having an area of 36 mm 2Among the plurality of fifth regions divided by squares, 764 or more of the fifth regions may be free of micropipes.
[0019] (9) The SiC substrate according to the above aspect may have a surface divided by squares each having an area of 49 mm 2 Among the plurality of sixth regions thus divided, 556 or more of the sixth regions may be free of micropipes.
[0020] (10) The SiC substrate according to the above aspect may have a surface divided by squares each having an area of 64 mm 2 Among the plurality of seventh regions thus divided, 421 or more of the seventh regions may be free of micropipes.
[0021] (11) The SiC substrate according to the above aspect may have a surface divided by squares each having an area of 81 mm 2 Among the plurality of eighth regions thus divided, 329 or more of the eighth regions may be free of micropipes.
[0022] (12) The SiC substrate according to the above aspect may have a surface divided by squares each having an area of 100 mm 2 Among the plurality of ninth regions thus divided, 262 or more of the ninth regions may be free of micropipes.
[0023] (13) The SiC substrate according to the above aspect may have a surface divided by squares each having an area of 225 mm 2 Among the plurality of tenth regions thus divided, 112 or more of the tenth regions may be free of micropipes.
[0024] (14) The SiC substrate according to the above aspect may have a surface divided by squares each having an area of 400 mm 2 Among the plurality of eleventh regions thus divided, 58 or more of the eleventh regions may be free of micropipes.
[0025] (15) The SiC substrate according to the above aspect may have a diameter of 205 mm or less.
[0026] (16) A SiC epitaxial wafer according to a second embodiment comprises a SiC substrate according to the above embodiment and a SiC epitaxial layer laminated on the SiC substrate. [Effects of the Invention]
[0027] The SiC substrate and SiC epitaxial wafer according to the above embodiment have a large diameter and few micropipes. [Brief explanation of the drawing]
[0028] [Figure 1] This is a plan view of the SiC substrate according to this embodiment. [Figure 2] This is a magnified view of the vicinity of the center of the SiC substrate according to this embodiment. [Figure 3] This figure illustrates the manufacturing method of the SiC substrate according to this embodiment. [Figure 4] This is a cross-sectional view of a SiC epitaxial wafer according to this embodiment. [Modes for carrying out the invention]
[0029] The SiC substrate and SiC epitaxial wafer according to this embodiment will be described in detail below, with reference to the figures as appropriate. In the drawings used in the following description, characteristic parts may be enlarged for convenience in order to make the features of this embodiment easier to understand, and the dimensional ratios of each component may differ from those of the actual product. The materials, dimensions, etc. exemplified in the following description are examples only, and the present invention is not limited to them, and can be implemented with appropriate modifications without changing the essence of the invention.
[0030] In this specification, individual orientations are indicated by [] and collective orientations by <>. While crystallographic conventions dictate that negative exponents should be preceded by a "-" (bar), in this specification, the negative sign is placed before the number.
[0031] Figure 1 is a plan view of the SiC substrate 10 according to this embodiment. Figure 1 shows the SiC substrate <0001> This is a view from a specific direction. The SiC substrate 10 is made of, for example, n-type SiC. The polytype of the SiC substrate 10 is not particularly limited and can be any of 2H, 3C, 4H, or 6H. The SiC substrate 10 is, for example, 4H-SiC.
[0032] The SiC substrate 10 has a roughly circular shape in plan view. The SiC substrate 10 may have notches 3 for determining the direction of the crystal axes. Alternatively, the SiC substrate 10 may have orientation flats instead of notches 3.
[0033] The diameter of the SiC substrate 10 is, for example, 195 mm or more, preferably 199 mm or more. Furthermore, the diameter of the SiC substrate 10 is preferably 205 mm or less, more preferably 201 mm or less.
[0034] The SiC substrate 10 has an effective region 1 and an edge exclusion region 2. The effective region 1 is the region used for device acquisition and is the region of the SiC substrate 10 excluding the edge exclusion region 2. The edge exclusion region 2 is the region within 3 mm from the outer edge. The edge exclusion region 2 is generally a region that is not used for device fabrication.
[0035] The SiC substrate 10 according to this embodiment has a micropipe density of 0.01 particles / cm². 2 The following applies. In addition, the SiC substrate 10 according to this embodiment has 3 or fewer micropipes, preferably 1 or fewer, and more preferably 0. Also, the number of micropipes in the effective region 1 is, for example, 3 or fewer, preferably 1 or fewer, and more preferably 0.
[0036] Micropipes are hollow defects exposed on the surface of the SiC substrate 10 with a diameter greater than 1 μm. Micropipes can be identified by transmission X-ray topography. Micropipes have strong distortion and a dense, point-like contrast. Therefore, in transmission X-ray topography, micropipes can be distinguished by utilizing the difference in contrast with other defects. For example, when micropipes are identified by transmission X-ray topography, the contrast of point-like defects caused by the distortion of the micropipe is more than three times greater than the contrast of point-like defects caused by penetrating dislocations.
[0037] In addition to transmission X-ray topography, micropipes may also be evaluated using optical microscopy and photoluminescence. Micropipes are observed as surface irregularities under an optical microscope. Micropipes are also observed as dark spots with bright points using photoluminescence. Observing micropipes using multiple evaluation methods can further improve the accuracy of micropipe identification.
[0038] Following the procedure described above, after distinguishing between micropipes and other defects, the number of micropipes can be counted to determine the micropipe density and the number of micropipes in the SiC substrate 10. The position coordinates of the micropipes can be calculated from the position coordinates of the full-frame image of the transmission X-ray topography. Furthermore, the micropipe density can be calculated by dividing the number of micropipes by the area of the substrate.
[0039] The SiC substrate 10 is cut into multiple chips when acquiring a device. For example, the SiC substrate 10 is divided into multiple regions according to the size of the chips. Figure 2 is an enlarged view of the vicinity of the center C of the SiC substrate 10 according to this embodiment. For example, the surface of the SiC substrate 10 is divided into multiple regions A. Each region A consists of a square with side length a. Regions A are laid out without gaps on the surface of the SiC substrate 10. The center of one of the multiple regions A coincides with the center C of the SiC substrate 10. Each region A corresponds to each individual chip, and each becomes a SiC device.
[0040] The size of region A varies depending on the required size of the device. The area of region A varies depending on the length a of one side. Length a is 2 mm and area is 4 mm 2 The square region is called the first region. Length a is 3 mm and area is 9 mm 2 The square region is called the second region. Length a is 4 mm and area is 16 mm 2 The square region is called the third region. Length a is 5 mm and area is 25 mm 2 The square region is called the fourth region. Length a is 6 mm and area is 36 mm 2 The square region is called the fifth region. Length a is 7 mm and area is 49 mm 2 The square region is called the sixth region. Length a is 8 mm and area is 64 mm² 2 The square region is called the seventh region. Length a is 9 mm and area is 81 mm² 2 The square region is called the eighth region. Length 'a' is 10 mm and area is 100 mm² 2 The square region is called the 9th region. Length a is 15 mm and area is 225 mm² 2 The square region is referred to as the 10th region. Length 'a' is 20 mm and area is 400 mm² 2 The square region is called the 11th region.
[0041] Here, an example of region A is shown, but the size of the region is not limited to these. For example, the length of one side could be 11mm, 12mm, 13mm, 14mm, 15mm, 16mm, 17mm, 18mm, or 19mm, and the length of one side is not limited to an integer.
[0042] If region A is the first region, it is preferable that 7209 or more of the multiple first regions contained in the SiC substrate 10 do not have micropipes. The number of first regions belonging to effective region 1 is 7209, and if all of these do not have micropipes, the maximum number of SiC devices can be obtained from a single SiC substrate 10.
[0043] If region A is a second region, it is preferable that 3168 or more of the multiple second regions included in the SiC substrate 10 do not have micropipes. The number of second regions belonging to effective region 1 is 3168.
[0044] If region A is a third region, it is preferable that 1764 or more of the multiple third regions included in the SiC substrate 10 do not have micropipes. The number of third regions belonging to effective region 1 is 1764.
[0045] If region A is the fourth region, it is preferable that 1116 or more of the multiple fourth regions included in the SiC substrate 10 do not have micropipes. The number of fourth regions belonging to effective region 1 is 1116.
[0046] If region A is the fifth region, it is preferable that 764 or more of the multiple fifth regions included in the SiC substrate 10 do not have micropipes. The number of fifth regions belonging to effective region 1 is 764.
[0047] If region A is the sixth region, it is preferable that 556 or more of the multiple sixth regions included in the SiC substrate 10 do not have micropipes. The number of sixth regions belonging to effective region 1 is 556.
[0048] If region A is the seventh region, it is preferable that 421 or more of the seventh regions included in the SiC substrate 10 do not have micropipes. The number of seventh regions belonging to effective region 1 is 421.
[0049] If region A is the eighth region, it is preferable that 329 or more of the eighth regions included in the SiC substrate 10 do not have micropipes. The number of eighth regions belonging to effective region 1 is 329.
[0050] If region A is the ninth region, it is preferable that 262 or more of the multiple ninth regions included in the SiC substrate 10 do not have micropipes. The number of ninth regions belonging to effective region 1 is 262.
[0051] If region A is the 10th region, it is preferable that 112 or more of the multiple 10th regions included in the SiC substrate 10 do not have micropipes. The number of 10th regions belonging to effective region 1 is 112.
[0052] If region A is the 11th region, it is preferable that 58 or more of the multiple 11th regions included in the SiC substrate 10 do not have micropipes. The number of 11th regions belonging to effective region 1 is 58.
[0053] Next, a method for manufacturing the SiC substrate 10 according to this embodiment will be described. Figure 3 is a diagram illustrating the method for manufacturing the SiC substrate 10 according to this embodiment. The SiC substrate 10 comprises a seed crystal preparation step, a crucible preparation step, a seed crystal placement step, a raw material placement step, a crystal growth step, and a slicing step.
[0054] First, in the seed crystal preparation step, seed crystal 11 is prepared. Seed crystal 11 is prepared as a crystal that does not contain micropipes. Seed crystal 11 that does not contain micropipes can be prepared, for example, using the RAF (Repeated a-face) method.
[0055] Next, in the crucible preparation step, a crucible 12 to be used for crystal growth is prepared. The crucible 12 is made of graphite, and a portion of its inner wall surface 12A is covered with a coating film 13. The coating film 13 is made of TaC. The coating film 13 covers an area of 10% to 50% of the inner wall surface 12A of the crucible 12. Here, the inner wall surface 12A refers to the inner surface of the crucible that is not filled with raw material 15 and is exposed to the growth space.
[0056] If the coverage area of the coating film 13 is too small, carbon dust generated from the inner wall surface 12A of the crucible 12 is more easily incorporated into the growing crystal. Carbon inclusions incorporated into the crystal cause the formation of micropipes. Conversely, if the coverage area of the coating film 13 is too large, the supply of carbon gas from the inner wall surface 12A of the crucible 12 is reduced, making it easier for heterogeneous polytype SiC to form within the growing crystal. Heterogeneous polytype SiC also causes the formation of micropipes. Covering a predetermined area of the inner wall surface 12A of the crucible 12 with the coating film 13 is one way to prevent the formation of micropipes in the SiC substrate 10.
[0057] Furthermore, the coating film 13 is installed on the inner wall surface 12A at a position close to the seed crystal. For example, if the crucible 12 has a guide member 16, a part of the guide member 16 is covered with the coating film 13. Specifically, the surface of the guide member 16 is covered with the coating film 13 from a position 5 mm away from the first end 16a of the guide member 16 to a position 100 mm away. Here, the first end 16a is the end of the guide member 16 on the seed crystal 11 side. By partially covering the guide member 16 with the coating film 13, dust generation can be suppressed while also suppressing the generation of different polytypes. The state of micropipe generation on the SiC substrate 10 also changes depending on the installation position of the coating film 13.
[0058] Next, in the seed crystal placement process, the seed crystal 11 is placed in the crucible 12. The seed crystal 11 may be placed on the inner wall surface 12A of the crucible 12, or it may be placed on a base installed on the inner wall surface 12A. The base is made of the same material as the crucible 12, for example.
[0059] The seed crystal 11 is placed in the crucible 12, for example, with adhesive 14. In this case, the crucible 12 is positioned on the seed crystal 11 such that the shortest distance D between the back surface of the seed crystal 11 and the installation surface of the seed crystal 11 is 30 μm or less at any position in the in-plane direction of the seed crystal 11. The installation surface is the inner wall surface 12A of the crucible 12 when the seed crystal 11 is placed directly in the crucible 12, and the exposed surface of the base when the seed crystal 11 is placed on a base. The in-plane direction of the seed crystal 11 is the in-plane direction in which the seed crystal 11 expands, and coincides with the direction in which the plane perpendicular to the line connecting the seed crystal 11 and the raw material 15 by the shortest distance expands. The shortest distance D between the back surface of the seed crystal 11 and the installation surface of the seed crystal 11 does not change significantly before and after heating during crystal growth, so it can be measured either before or after heating. Note that the adhesive 14 carbonizes when heated. A gap may form between the surface of the carbonized adhesive 14 and the seed crystal 11. The thickness of this gap (the shortest distance between the carbonized surface of the adhesive 14 and the seed crystal 11) should be 10 μm or less.
[0060] As the distance between the seed crystal 11 and the mounting surface increases, the seed crystal 11 is relatively closer to the raw material 15. The temperature is higher closer to the raw material 15, and etching of the seed crystal 11 is more likely to occur in a high-temperature environment. When the seed crystal 11 is etched, the adhesive 14 or the mounting surface is exposed. SiC polycrystals are likely to grow in the exposed areas of the adhesive 14 or the mounting surface. Micropipes are likely to form in the SiC polycrystalline structure. By appropriately controlling the distance between the seed crystal 11 and the mounting surface, the formation of micropipes in the SiC substrate 10 can be suppressed. In addition, the gap between the surface of the carbonized adhesive 14 and the seed crystal 11 disrupts the temperature uniformity within the plane during crystal growth, causing a temperature rise. In areas that become locally hot, etching is accelerated, and the adhesive 14 or the mounting surface is exposed. Therefore, by preventing the formation of a gap between the surface of the adhesive 14 and the seed crystal 11, or by making it sufficiently narrow, the formation of micropipes in the SiC substrate 10 can be further suppressed.
[0061] Next, in the raw material placement process, raw material 15 is placed at the bottom of the crucible 12. Raw material 15 is, for example, SiC powder. In the raw material placement process, raw material 15 is placed so that the shortest distance between the outermost surface of raw material 15 and the seed crystal 11 is 150 mm or more. By increasing the distance between the raw material and the seed crystal, the risk of the seed crystal becoming hot and being etched can be reduced.
[0062] Next, the crystal growth process is carried out by sublimation. In the sublimation method, the crucible 12 is heated to supply sublimated gas, which is produced from the raw materials 15 inside the crucible 12, to the seed crystal 11, causing the seed crystal 11 to grow into a larger SiC ingot. The SiC ingot grows on the seed crystal 11.
[0063] In the crystal growth process, the SiC ingot is grown to a diameter of 10 mm or more. The diameter expansion of the SiC ingot relative to the seed crystal 11 is set to be between 5 mm and 10 mm. The diameter expansion is the value obtained by subtracting the diameter of the seed crystal 11 from the maximum diameter of the SiC ingot. The diameter expansion of the SiC ingot can be obtained by adjusting the shape of the guide member 16 that widens the flow of sublimation gas. By adjusting the growth rate of the SiC ingot according to the shape of the guide member 16, the diameter expansion can be set to be between 5 mm and 10 mm. With a diameter expansion of 5 mm or less, it is necessary to repeat the diameter expansion process multiple times to obtain a large-diameter crystal, making it difficult to produce a large-diameter crystal.
[0064] On the other hand, if the crystal diameter is increased too much during crystal growth, stress is generated within the crystal. If the diameter increase during crystal growth is too large, stress concentration occurs, and cracks may form within the crystal. These cracks are the cause of micropipe defects. By controlling the crystal diameter increase to 10 mm or less during the crystal growth process, the generation of micropipes in the SiC substrate 10 can be suppressed.
[0065] Next, in the slicing process, the SiC substrate 10 is cut from the SiC ingot. For example, the SiC ingot is hollowed out into a cylinder of a predetermined diameter, and the cylinder is sliced to produce the SiC substrate 10. Slicing may be performed using a laser or a wire saw.
[0066] As described above, by controlling each step—seed crystal preparation, crucible preparation, seed crystal placement, raw material placement, crystal growth, and slicing—it is possible to produce a SiC substrate 10 with a large diameter and few micropipes.
[0067] The SiC substrate 10 according to this embodiment has a large diameter but few micropipes. Therefore, many good SiC devices can be obtained from the SiC substrate 10 according to this embodiment. SiC devices are obtained by chipping the SiC epitaxial wafer into regions A. Figure 4 is a cross-sectional view of the SiC epitaxial wafer 100 according to this embodiment. The SiC epitaxial wafer 100 has a SiC substrate 10 and a SiC epitaxial layer 20. Devices are formed on the SiC epitaxial layer 20.
[0068] Although preferred embodiments of the present invention have been described in detail above, the present invention is not limited to any particular embodiment, and various modifications and changes are possible within the scope of the gist of the present invention as described in the claims. [Examples]
[0069] "Example 1" First, a seed crystal was prepared. A 4H-SiC single crystal with a diameter of 197 mm was prepared as the seed crystal.
[0070] Next, a crucible was prepared. The crucible used had 39% of its inner wall surface coated with TaC. The TaC coating was formed on a portion of the inner surface of the guide member near the seed crystal of the crucible. Specifically, the area from 5 mm away from the first end of the guide member on the seed crystal side to 100 mm away was coated with TaC.
[0071] Next, a seed crystal was placed on the inner wall surface of the crucible. The seed crystal was attached to the inner wall surface using an adhesive. A carbon adhesive with a thickness of 20 μm was used. After the seed crystal was placed, the distance between the back surface of the seed crystal and the surface on which it was attached remained at 20 μm because there was no peeling of the adhesive, and no gap was formed between the carbonized adhesive and the seed crystal.
[0072] Next, the raw material was packed into the bottom of the crucible. SiC powder was used as the raw material. The distance between the outermost surface of the raw material and the surface of the seed crystal was set to 200 mm.
[0073] Next, a SiC ingot was grown on a seed crystal using the sublimation method. The crystal growth amount (thickness of the SiC ingot) was 25 mm. The diameter increase of the SiC ingot relative to the seed crystal was 8 mm.
[0074] Next, the fabricated SiC ingot was sliced, and the (0001) surface of the cut substrate was polished in the following order: grinding, mechanical polishing (MP), and chemical mechanical polishing (CMP) to obtain a SiC substrate. The surface of the SiC substrate was measured using transmission X-ray topography to determine the number of micropipes contained within the SiC substrate.
[0075] The SiC substrate in Example 1 contained one micropipe. This single micropipe was located within the effective region, but near the edge exclusion region. Therefore, it was possible to separate the device acquisition region by excluding the micropipe from the device acquisition region.
[0076] Therefore, from the SiC substrate of Example 1, regions without micropipes could be obtained depending on the size of the region. The number of these regions corresponds to the number of devices obtained. 1st area: 7209 pieces 2nd area: 3168 pieces Third area: 1764 pieces 4th area: 1116 pieces 5th area: 764 pieces 6th area: 556 pieces 7th area: 421 pieces 8th area: 329 pieces 9th area: 262 pieces 10th area: 112 pieces Area 11: 58 pieces
[0077] As described above, in Example 1, a SiC substrate with few micropipes was obtained even with a large 8-inch diameter substrate. Example 1 was reproducible in multiple experiments. The seed crystal used in Example 1 was a crystal with few micropipes that had been enlarged multiple times in the same manner as in Example 1. [Explanation of symbols]
[0078] 1…Effective region, 2…Edge exclusion region, 3…Notch, 10…SiC substrate, A…Region, C…Center, 11…Seed crystal, 12…Crucible, 12A…Inner wall surface, 14…Adhesive, 15…Raw material, 20…SiC epitaxial layer, 100…SiC epitaxial wafer
Claims
1. The diameter is 195 mm or more. The number of micropipes in the effective region, excluding the edge exclusion region within 3 mm from the outer circumference, is 3 or less. The aforementioned micropipe was confirmed by transmission X-ray topography and is a SiC substrate.
2. The SiC substrate according to claim 1, wherein the number of micropipes in the effective region is one or less.
3. The SiC substrate according to claim 1, wherein the number of micropipes in the effective region is zero.
4. The SiC substrate according to claim 1, wherein the micropipes are observed by optical microscopy and photoluminescence in addition to transmission X-ray topography.
5. The SiC substrate according to claim 1, wherein the micropipes are exposed on the surface and are hollow defects with a diameter greater than 1 μm.
6. The SiC substrate according to claim 1, wherein in the transmission X-ray topography, the contrast of point defects caused by the distortion of the micropipe is three times or more the contrast of point defects caused by through dislocations.
7. The SiC substrate according to claim 1, wherein the diameter is 205 mm or less.
8. The surface area is 4 mm 2 The SiC substrate according to claim 1, wherein 7,209 or more of the multiple first regions divided by squares do not have micropipes.
9. The surface area is 16 mm 2 The SiC substrate according to claim 1, wherein 1,764 or more of the multiple third regions divided by squares do not have micropipes.
10. The surface area is 25 mm 2 The SiC substrate according to claim 1, wherein 1116 or more of the multiple fourth regions divided by squares do not have micropipes.
11. The surface area is 49 mm² 2 The SiC substrate according to claim 1, wherein 556 or more of the sixth regions divided by a square do not have micropipes.
12. The surface area is 100 mm 2 The SiC substrate according to claim 1, wherein 262 or more of the 9th regions divided by a square do not have micropipes.
13. The surface area is 400 mm² 2 The SiC substrate according to claim 1, wherein 58 or more of the 11th regions divided by squares do not have micropipes.
14. A SiC epitaxial wafer comprising a SiC substrate as described in claim 1 and a SiC epitaxial layer laminated on the SiC substrate.
15. A SiC epitaxial wafer comprising a SiC substrate as described in claim 3 and a SiC epitaxial layer laminated on the SiC substrate.
16. A SiC epitaxial wafer comprising a SiC substrate as described in claim 4 and a SiC epitaxial layer laminated on the SiC substrate.
17. A SiC epitaxial wafer comprising a SiC substrate as described in claim 5 and a SiC epitaxial layer laminated on the SiC substrate.
18. A SiC epitaxial wafer comprising a SiC substrate as described in claim 6 and a SiC epitaxial layer laminated on the SiC substrate.
Citation Information
Patent Citations
Method for manufacturing silicon carbide epitaxial substrate and method for manufacturing silicon carbide semiconductor device
JP2016127201A