Lithium-ion secondary battery comprising inorganic oxide powder and electrodes containing the same

JP2026183089APending Publication Date: 2026-11-19OHARA INC
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2026206359
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Filing Date
2026-09-15
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Lithium-ion secondary batteries experience a decrease in discharge capacity due to side reactions of the electrolyte component, leading to a reduction in discharge capacity retention rate upon repeated charging and discharging.

Method used

Incorporating an inorganic oxide powder with specific component compositions and properties, including Li2O, Al2O3, TiO2, and P2O5, into the electrodes, which captures hydrogen fluoride generated in the electrolyte, thereby maintaining high discharge capacity retention.

Benefits of technology

The inorganic oxide powder enhances the discharge capacity retention rate of lithium-ion secondary batteries to more than 70% after 300 cycles by effectively trapping hydrogen fluoride, thus stabilizing battery performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026183089000001_ABST
    Figure 2026183089000001_ABST
Patent Text Reader

Abstract

This material makes it possible to obtain lithium-ion secondary batteries with excellent discharge capacity retention. [Solution] The material contains 4.0-6.0% Li2O, 3.0-9.0% Al2O3, 31.0-40.0% TiO2, and 49.0-57.0% P2O5 by mass percentage in terms of oxides, with a BET specific surface area of ​​8 m². 2 / g or more 35m 2 The above problem is solved by using an inorganic oxide powder that has a density of less than / g and an HF trapping capacity of 2.0 to 9.0.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a lithium-ion secondary battery comprising an inorganic oxide powder and an electrode containing the same. [Background technology]

[0002] Lithium-ion rechargeable batteries, which have high energy density and can be charged and discharged, are widely used in applications such as power supplies for electric vehicles and mobile phone terminals. Most lithium-ion secondary batteries currently on the market use a liquid electrolyte to achieve high energy density. This electrolyte is typically a non-aqueous solution, such as a lithium salt dissolved in an organic solvent. The battery structure mainly consists of a separator between the positive and negative electrodes, with the electrolyte filling the cavity. Furthermore, lithium-ion secondary batteries (lithium-ion polymer secondary batteries) that use a polymer compound containing electrolyte components (lithium-ion conductive polymer) as the electrolyte layer have also been developed and are commercially available.

[0003] In lithium-ion secondary batteries, as described above, the discharge capacity tends to decrease when repeatedly charged and discharged due to side reactions of the lithium salt, which is an electrolyte component. Therefore, technological development is underway to maintain a high discharge capacity even after repeated charging and discharging.

[0004] For example, Patent Document 1 discloses an electrode for a lithium-ion battery that includes a sulfonic acid compound comprising a sulfonic acid anion represented by a predetermined formula and a Mn cation, which is capable of maintaining a higher discharge capacity after repeated charging and discharging of the lithium-ion battery at high temperatures. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2023-176985 SUMMARY OF THE INVENTION PROBLEMS TO BE SOLVED BY THE INVENTION

[0006] However, the lithium ion secondary battery as described above still has room for further improvement in terms of discharge capacity retention (suppression of reduction in discharge capacity retention rate) when charge and discharge are repeated.

[0007] Accordingly, an object of the present invention is to provide a material capable of obtaining a lithium ion secondary battery having an excellent discharge capacity retention rate. MEANS FOR SOLVING THE PROBLEMS

[0008] In order to solve the above problems, the present inventors conducted intensive studies, and found that the discharge capacity retention rate of the lithium ion secondary battery as described above correlates with the ability of the electrode and the like thereof to capture hydrogen fluoride generated in the electrolyte (HF trapping ability). Furthermore, the present inventors also found that this HF trapping ability is related to the component composition of the used material, the BET specific surface area, and the like, and conducted further studies, and found that, in mass% in terms of oxide, the material contains 4.0 to 6.0% of Li2O component, 3.0 to 9.0% of Al2O3 component, 31.0 to 40.0% of TiO2 component, and 49.0 to 57.0% of P2O5 component, and has a BET specific surface area of 8 m 2 / g or more and 35 m 2 / g or less, and by incorporating inorganic oxide powder having an HF trapping ability of 2.0 or more and 9.0 or less into an electrode together with an electrode active material, when a lithium ion secondary battery provided with the electrode is repeatedly charged and discharged, the inorganic oxide powder captures hydrogen fluoride generated in the electrolyte, so that the discharge capacity retention rate can be kept high, and the present invention has been completed.

[0009] That is, the present invention includes the following embodiments <1> to <9>. <1>In mass% in terms of oxide, the Li2O component is 4.0 to 6.0%, the Al2O3 component is 3.0 to 9.0%, the TiO2 component is 31.0 to 40.0%, P2O5 component: 49.0-57.0% Contains, BET specific surface area 8m 2 / g or more 35m 2 It is less than / g The HF trapping capability is between 2.0 and 9.0. Inorganic oxide powder. <2> The product of the BET specific surface area and the Al2O3 content (BET × Al2O3) is 30 or more and 300 or less. <1> The inorganic oxide powder described above. <3> The average particle size (D) of the inorganic oxide powder 50 The ratio of the BET specific surface area to the (BET / average particle diameter) is 10 or more. <1> or <2> The inorganic oxide powder described above. <4> The Al2O3 component content is 5.0% or more, and the TiO2 component content is 33.0% or more. <1> ~ <3> An inorganic oxide powder as described in any one of the following. <5> The Al2O3 component content is 5.0% or more, and the sum of the content of the Li2O component, the Al2O3 component, and the TiO2 component (Li2O + Al2O3 + TiO2) is 45.5% or more. <1> ~ <4> An inorganic oxide powder as described in any one of the following. <6> It is glass powder. <1> ~ <5> An inorganic oxide powder as described in any one of the following. <7> It is a glass-ceramic powder or ceramic powder containing LATP crystals. <1> ~ <5> An inorganic oxide powder as described in any one of the following. <8> <1> ~ <7> The electrode comprises an electrode containing an inorganic oxide powder as described in any one of the above, and an electrolyte layer containing a lithium salt containing fluorine as an electrolyte component. Lithium-ion rechargeable battery. <9> The device comprises the aforementioned electrode and a non-aqueous electrolyte containing LiPF6 as an electrolyte component, and has a discharge capacity retention rate of more than 70% after 300 cycles. <8> Lithium-ion secondary batteries as described above. [Effects of the Invention]

[0010] According to the present invention, it is possible to provide an inorganic oxide powder that can be used to obtain a lithium-ion secondary battery with excellent discharge capacity retention, and furthermore, it is possible to provide a lithium-ion secondary battery with excellent discharge capacity retention that includes this powder in the electrodes. [Brief explanation of the drawing]

[0011] [Figure 1] This graph shows the relationship between BET / average particle size and HF trapping capacity for inorganic oxide powders in the examples and comparative examples. [Figure 2] This graph shows the relationship between BET×Al2O3 and HF trapping capacity for inorganic oxide powders in the examples and comparative examples. [Figure 3] This graph shows the relationship between the HF trapping ability of inorganic oxide powders in the examples and comparative examples and the discharge capacity retention rate of lithium-ion secondary batteries equipped with a positive electrode containing them after 300 cycles. [Figure 4] This graph shows the relationship between the number of cycles and the discharge capacity retention rate in a lithium-ion secondary battery equipped with a positive electrode containing inorganic oxide powder according to Example 2 or Comparative Example 3. [Modes for carrying out the invention]

[0012] The present invention will now be described. This invention contains, by mass percent on an oxide basis, 4.0-6.0% Li2O, 3.0-9.0% Al2O3, 31.0-40.0% TiO2, and 49.0-57.0% P2O5, with a BET specific surface area of ​​8 m². 2 / g or more 35m 2 The lithium-ion secondary battery comprises an inorganic oxide powder having a density of 2.0 or less per gram and an HF trapping capacity of 9.0 or more (hereinafter, this may also be referred to as "the inorganic oxide powder of the present invention"), an electrode containing this inorganic oxide powder, and an electrolyte layer containing a lithium salt containing fluorine as an electrolyte component.

[0013] First, the components (essential components, optional components), their form, physical properties, etc., that constitute the inorganic oxide powder of the present invention will be described in detail.

[0014] The content of each component in the inorganic oxide powder of the present invention is expressed in mass % (wt%) in terms of oxide unless otherwise specified (hereinafter, when simply % is used to refer to the content of a component, it means mass % in terms of oxide unless otherwise specified). The content expressed as "mass % in terms of oxide" is determined by analyzing the inorganic oxide powder of the present invention by performing ICP emission spectroscopy (inductively coupled plasma emission spectroscopy) on the Li component and XRF analysis (X-ray fluorescence analysis) on the other components. Based on the analysis values, the total mass assuming all components are oxides is set to 100% by mass, and the oxide content of each component in the inorganic oxide powder of the present invention is expressed in mass %.

[0015] The Li2O component is an essential component for imparting lithium ion conductivity to the inorganic oxide powder of the present invention. It also becomes a constituent component of LATP crystals. Therefore, the Li2O content should be 4.0 to 6.0%. From the viewpoint of lithium ion conductivity and LATP crystal formation (glass ceramic powder or ceramic powder), the lower limit is more preferably 4.3% or more, even more preferably 4.4% or more, and even more preferably 4.5% or more. The upper limit is more preferably 5.8% or less, even more preferably 5.5% or less, even more preferably 5.2% or less, and even more preferably 5.0% or less, from the viewpoint of easily suppressing the generation of by-products during crystallization and easily achieving high HF trapping ability. Furthermore, in cases such as when using glass powder, this upper limit may be set to 5.1% or less, or even 4.6% or less, in order to easily suppress the formation of heterogeneous crystals.

[0016] The Al2O3 component is an essential component necessary for the inorganic oxide powder of the present invention to have lithium ion conductivity and high HF trapping capacity. It also becomes a component of LATP crystals. Therefore, the Al2O3 content should be 3.0 to 9.0%. From the viewpoint of the above effects, the lower limit is more preferably 4.0% or more, even more preferably 5.0% or more, even more preferably 6.0% or more, even more preferably 6.5% or more, and even more preferably 7.0% or more. From similar viewpoints and the ease of LATP crystal formation (glass ceramic powder or ceramic powder), the upper limit is more preferably 8.8% or less, even more preferably 8.7% or less, and even more preferably 8.5% or less. In the case of glass powder, the lower limit may be set to 6.8% or more, even more preferably 7.5% or more, even more preferably 8.0% or more, and even more preferably 8.4% or more, from the viewpoint of glass formation, the stability of the glass itself, and pulverability.

[0017] The TiO2 component is also an essential component necessary for the inorganic oxide powder of the present invention to have lithium ion conductivity and high HF trapping capacity. It also becomes a component of the LATP crystal. Therefore, the TiO2 content should be 31.0 to 40.0%. From the viewpoint of the above effects, the lower limit is more preferably 33.0% or more, and even more preferably 34.0% or more. The upper limit is more preferably 38.0% or less, even more preferably 37.0% or less, and even more preferably 35.0% or less, as it makes it easier to suppress the formation of by-products during crystallization and to achieve high HF trapping capacity.

[0018] The P2O5 component is also an essential component necessary for the inorganic oxide powder of the present invention to have lithium ion conductivity and high HF trapping capacity. It also becomes a component of LATP crystals. Therefore, the P2O5 content is set to 49.0-57.0%. From the viewpoint of the above effects, the lower limit is more preferably 49.5% or more, and even more preferably 50.0% or more. For similar reasons, as well as to suppress the generation of by-products during crystallization, and for ease of pulverization, the upper limit is more preferably 56.5% or less, even more preferably 56.0% or less, even more preferably 55.5% or less, even more preferably 55.0% or less, even more preferably 54.5% or less, even more preferably 54.0% or less, even more preferably 53.5% or less, even more preferably 53.0% or less, even more preferably 52.5% or less, even more preferably 52.0% or less, even more preferably 51.5% or less, and even more preferably 51.0% or less.

[0019] Furthermore, to facilitate the expression of the present invention, it is preferable that the inorganic oxide powder of the present invention has an Al2O3 component content of 5.0% or more and a TiO2 component content of 33.0% or more. Moreover, the Al2O3 component content may be 6.0% or more and the TiO2 component content may be 34.0% or more. The Al2O3 component content may also be 6.5% or more. For similar reasons, the inorganic oxide powder of the present invention preferably has an Al2O3 component content of 5.0% or more, and the sum of the content of the Li2O component, Al2O3 component, and TiO2 component (total of Li2O component content, Al2O3 component content, and TiO2 component content, Li2O + Al2O3 + TiO2) is 45.5% or more. Furthermore, the lower limit of this sum of content is more preferably 46.0% or more, and even more preferably 46.5% or more. The lower limit of the content of the Al2O3 component may also be within the above range (for example, 6.0% or more, and even more preferably 6.5% or more). The upper limit of the above sum of content may be, for example, 51.0% or less, and may also be 50.0% or less.

[0020] The inorganic oxide powder of the present invention may further contain, as an optional component, one or more components selected from the group consisting of SiO2, GeO2, ZrO2, SnO2, B2O3, Y2O3, Sc2O3, ZnO, Na2O, K2O, and transition metal oxides such as Co, Ni, Mn, and Fe. However, embodiments that substantially do not contain any of these optional components (a configuration consisting of the essential components described above) are also acceptable. The following explains this optional component.

[0021] The SiO2 component is an optional component that facilitates glass formation when the inorganic oxide powder of the present invention is used as glass powder or glass ceramic powder. When used as glass ceramic powder or ceramic powder, it also becomes a component of the LATP crystal, substituting at the P site of the PO4 skeleton in the LATP crystal, causing skeleton distortion, thereby increasing lithium ion conductivity, and further enhancing HF trapping ability. In addition, this SiO2 component can also increase the mechanical strength of the inorganic oxide powder of the present invention. The content of the SiO2 component is preferably 5.0% or less, more preferably 3.0% or less. The lower limit may be greater than 0%, 0.1% or more, or 0.2% or more.

[0022] The GeO2 component is an optional component that facilitates crystal formation when the inorganic oxide powder of the present invention is made into a glass ceramic powder or ceramic powder. It also becomes a component of the LATP crystal, and by substituting into the Ti sites in the LATP crystal and increasing the lithium ion content in the LATP crystal, it can enhance lithium ion conductivity. The GeO2 component content is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably 1.0% or less.

[0023] The ZrO2 component is an optional component that can contribute to improving the chemical durability of the inorganic oxide powder of the present invention. Furthermore, this ZrO2 component can also enhance the water resistance of the inorganic oxide powder of the present invention. The ZrO2 content is preferably 5.0% or less, more preferably 3.0% or less, even more preferably 1.0% or less, and even more preferably 0.5% or less.

[0024] The SnO2 component is also an optional component that facilitates crystal formation when the inorganic oxide powder of the present invention is a glass ceramic powder or a ceramic powder. The SnO2 content is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably 1.0% or less.

[0025] The B2O3 component is also an optional component that facilitates glass formation when the inorganic oxide powder of the present invention is made into glass powder or glass ceramic powder. Furthermore, this B2O3 component can be substituted for a portion of the Al2O3 component and is also a component that can adjust the lithium ion conductivity of the inorganic oxide powder of the present invention. The content of the B2O3 component is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably 1.0% or less.

[0026] The Sc2O3 and Y2O3 components can also be substituted for a portion of the Al2O3 component and are optional components that can adjust the lithium ion conductivity of the inorganic oxide powder of the present invention. The content of each of these components is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably 1.0% or less.

[0027] The ZnO component can substitute for a portion of the TiO2 component and is an optional component that can adjust the lithium ion conductivity of the inorganic oxide powder of the present invention. The ZnO content is preferably 5.0% or less, more preferably 3.0% or less, and even more preferably 1.0% or less.

[0028] The Na2O and K2O components are also optional components that can adjust the lithium ion conductivity of the inorganic oxide powder of the present invention. The content of each of these components is preferably 5.0% or less, more preferably 3.0% or less, even more preferably 1.0% or less, and even more preferably 0.5% or less.

[0029] Transition metals such as Co, Ni, Mn, and Fe are optional components that can suppress the elution of transition metals and other elements contained in the electrode active material (especially the positive electrode active material) into the electrolyte. The total content of these transition metal oxides is preferably 5.0% or less, more preferably 3.0% or less, even more preferably 1.0% or less, and even more preferably 0.5% or less.

[0030] Furthermore, it is preferable to minimize the sulfur (S) content in the inorganic oxide powder of the present invention (for example, less than 0.5%, and even less than 0.1%), and more preferably to omit it altogether. This is because reducing the S component reduces the possibility of generating harmful gases such as hydrogen sulfide in lithium-ion secondary batteries and the like that equipped with electrodes containing the inorganic oxide powder of the present invention. Similarly, it is preferable to minimize the content of arsenic (As), antimony (Sb), and lead (Pb), and more preferably to omit them altogether, because they are harmful substances. In addition, it is preferable to minimize the content of bismuth (Bi) and tellurium (Te), and more preferably to omit them altogether.

[0031] Then, the inorganic oxide powder of the present invention having the above component composition may be a glass powder (amorphous powder) obtained by using the raw material as a glass melt melted at a predetermined temperature, or may be a glass-ceramic powder obtained by vitrifying the raw material and then crystallizing it by heat treatment or the like. Further, this glass-ceramic powder may be one obtained by subjecting the aforementioned glass powder or the like to heat treatment or the like. Furthermore, it may be a ceramic powder obtained by sintering the raw material or the like. When the inorganic oxide powder of the present invention is made into a glass-ceramic powder or a ceramic powder, in either case, it shall contain LATP crystals, and it is more preferable that the LATP crystals are the main crystal phase (more than 50 mass%, preferably 70 mass% or more, more preferably 90 mass% or more, further preferably 95 mass% or more, still more preferably 99 mass% or more of all crystal phases are LATP crystals). However, embodiments partially containing crystals other than LATP crystals (for example, other NASICON-type lithium ion conductive crystals, lithium ion conductive crystals of other structures such as LISICON-type, perovskite-type, garnet-type, and other by-product crystals, etc.) are also acceptable. Here, this "LATP crystal" refers to Li 1+x+y Al x Ti 2-x Si y P 3-y O 12 It is a NASICON-type lithium ion conductive oxide crystal represented by the composition formula (0≦x≦0.4, 0≦y≦0.6). In this formula, from the viewpoint of lithium ion conductivity and the like, the lower limit of X is preferably more than 0, more preferably 0.05 or more, further preferably 0.08 or more, and still more preferably 0.10 or more. The upper limit is preferably 0.35 or less, more preferably 0.30 or less. From the same viewpoint, the lower limit of Y is preferably more than 0, more preferably 0.025 or more, further preferably 0.04 or more, and still more preferably 0.06 or more. The upper limit is preferably 0.50 or less, more preferably 0.40 or less, and further preferably 0.30 or less.

[0032] The above-mentioned glass powder is composed of an amorphous phase, and does not substantially contain a crystalline phase. In addition, the above-mentioned glass ceramic powder includes a crystalline phase containing LATP crystals formed by heat treatment (for example, LATP crystals as the main crystalline phase and other by-product crystalline phases) and an amorphous phase. That is, it is a mixture of ceramics and glass. Furthermore, the above-mentioned ceramic powder is composed of a crystalline phase containing LATP crystals (for example, LATP crystals as the main crystalline phase and other by-product crystalline phases), and does not substantially contain an amorphous phase.

[0033] <BET specific surface area> The inorganic oxide powder of the present invention has the above-described component composition and form, and has a BET specific surface area of 8 m 2 / g or more and 35 m 2 / g or less. As a result, it has a high HF trapping capability, and when it is contained in an electrode of a predetermined lithium ion secondary battery, the discharge capacity retention rate thereof can be kept high. This lower limit is more preferably 9 m from the viewpoints of easily enhancing the HF trapping capability and easily keeping the average particle diameter small 2 / g or more, still more preferably 10 m 2 / g or more, still more preferably 11 m 2 / g or more, still more preferably 12 m 2 / g or more, still more preferably 15 m 2 / g or more. The upper limit is more preferably 32 m from the viewpoints of wettability with the electrolytic solution and grindability of the powder particles 2 / g or less, still more preferably 31 m 2 / g or less, still more preferably 30 m 2 / g or less, still more preferably 27 m 2 / g or less. This can be adjusted by the composition, firing conditions, conditions during pulverization or particle size regulation, and the like. Here, this BET specific surface area means the average value of values measured twice by the BET one-point method using a fully automatic specific surface area analyzer Macsorb HM-1201 manufactured by MOUNTECH Co., Ltd.

[0034] Further, in the inorganic oxide powder of the present invention, since the effects of the present invention can be more easily exerted, this BET specific surface area (m 2 / g) and the above-mentioned content of the Al2O3 component (mass% in terms of oxide) (BET×Al2O3) is more preferably 30 or more and 300 or less. This lower limit is more preferably 45 or more, further preferably 60 or more, further preferably 75 or more, further preferably 90 or more, further preferably 130 or more, and further preferably 150 or more. The upper limit is more preferably 280 or less, further preferably 260 or less.

[0035] <HF trapping capacity> Since the inorganic oxide powder of the present invention has the above-described component composition, morphology, BET specific surface area, etc., its HF trapping capacity (capacity to capture hydrogen fluoride) is 2.0 or more and 9.0 or less. Accordingly, when the inorganic oxide powder of the present invention is contained in an electrode of a predetermined lithium ion secondary battery, hydrogen fluoride that may be generated in the electrolyte layer (generated mainly by a side reaction between a fluorine-containing lithium salt and a trace amount of moisture contained in the electrolyte layer (for example, a side reaction such as LiPF6+H2O→LiF+2HF+POF3)) can be efficiently captured to reduce the concentration of hydrogen fluoride contained in the lithium ion secondary battery, so that the discharge capacity retention rate can be kept high even after repeated charge and discharge cycles. This lower limit is more preferably 2.3 or more, further preferably 3.0 or more, further preferably 4.0 or more, further preferably 5.0 or more, further preferably 6.0 or more, further preferably 6.5 or more, and further preferably 7.0 or more. The upper limit may be, for example, 8.0 or less. This HF trapping capacity is measured and calculated by the following procedure.

[0036] 60 g of an electrolyte containing 1 ppm to 40 ppm of HF (hydrogen fluoride) and 20 ppm or less of water (electrolyte component: 1 mol / L LiPF6, solvent: ethylene carbonate:ethyl methyl carbonate = 3:7, where "ppm" is the volume ratio of the amount of the component to the total volume of the electrolyte) is mixed with 2 g of the inorganic oxide powder of the present invention (pre-dried under vacuum at 160°C for 24 hours using a glass tube oven (manufactured by Nippon Buch Co., Ltd., B-585)) and sealed with aluminum laminate. After storing this in a constant temperature bath at 60°C for one week, the electrolyte is extracted to obtain a sample for HF concentration measurement. This sample is diluted with pure water and neutralization titration is performed using a 0.01 mol / L sodium hydroxide solution in an automatic titrator. Then, assuming that all the acids contained in the electrolyte are HF, the HF trapping capacity is calculated from the HF concentration using the following formula.

[0037] HF concentration=(DB)×K×F×M×1000 / S D: Titration volume of sodium hydroxide solution to the endpoint (mL) B: Titration volume (mL) of blank sodium hydroxide solution K:HF molecular weight (20.0063) F: Sodium hydroxide solution factor M: Sodium hydroxide concentration (0.01 mol / L) S: Sample amount (g) HF trapping capacity = 100 × (1 / HF concentration)

[0038] <Lithium-ion conductivity> The inorganic oxide powder of the present invention is a lithium-ion conductive inorganic oxide powder (lithium-ion conductive inorganic material), and is not limited thereto, but its lithium-ion conductivity at 25°C is 1.0 × 10⁻⁶. -7 Preferably, the lithium ion conductivity is (1.0E-07) S / cm or higher, and if the inorganic oxide powder of the present invention is a glass ceramic powder or ceramic powder containing LATP crystals, its lithium ion conductivity at 25°C is 1.0 × 10⁻⁶. -5 (1.0E-05)S / cm or more is more preferable, and 1.0 × 10 -4It is even more preferable that the value is (1.0E-04)S / cm or higher. Here, the lithium-ion conductivity is calculated by forming a gold electrode as a blocking electrode on the object to be measured using a magnetron sputtering apparatus, and then measuring the impedance using an electrochemical evaluation apparatus at 25°C under the conditions of a frequency of 0.1 Hz to 7 MHz, an amplitude voltage of 10 mV, and an open-circuit voltage. In this measurement, the object to be measured is a solid material before powdering (before pulverization) on which a gold electrode can be formed on the surface.

[0039] <Average particle size> The inorganic oxide powder of the present invention has an average particle size (D 50 A particle size of 0.1 μm or more and 2.0 μm or less is preferable from the viewpoint of the effects of the present invention and ease of use in electrodes. The lower limit may be 0.2 μm or more, and the upper limit may be 1.5 μm or less, further 1.0 μm or less, further 0.7 μm or less, further 0.6 μm or less, further 0.5 μm or less, and further 0.4 μm or less. This can be adjusted by conditions during grinding and sizing. Here, this "average particle diameter (D 50 )" refers to the average particle diameter based on volume (50% diameter (D) measured by a laser diffraction / scattering particle size distribution analyzer. 50 )) is.

[0040] Furthermore, in the inorganic oxide powder of the present invention, this average particle size (D 50 The aforementioned BET specific surface area (m²) relative to μm. 2It is preferable that the ratio of (BET / average particle size) ( / g) be 10 or greater, and more preferably 25 or greater. This is because the particle shape of the powder becomes more uneven or porous, which increases the contact area with the electrolyte, and thus increases the HF trapping capacity. In particular, for glass ceramic powder or ceramic powder, it is preferable that the above ratio be 40 or greater. The lower limit is more preferably 45 or greater, and even more preferably 50 or greater. This ratio can be adjusted by adjusting the crystallization and firing conditions to reduce the crystal size of LATP crystals, etc., making it easier to pulverize into such shapes, or by reducing the amount of media relative to the pulverizing material and adopting pulverizing conditions that increase the BET specific surface area without making the particle size too small. The upper limit is not particularly limited, but for example it may be 200 or less, or 150 or less.

[0041] The present invention provides a method for producing inorganic oxide powders using general methods in the production of inorganic materials, such as calcination (pre-calcination), melting, vitrification, crystallization, and sintering, or modified methods thereof. While not limited to these methods, when producing glass powder, an example is to melt the raw materials at a predetermined temperature (for example, 1000°C or higher, and even 1200°C to 1600°C, with a particularly favorable rapid heating rate of 100°C / min or higher), cast the resulting glass melt onto a metal casting plate or drop it into flowing water to obtain glass particles, and then further crush them into glass powder by coarse crushing, fine crushing, and pulverizing through a classification device. Furthermore, when producing glass ceramic powder, an example is to vitrify the raw materials (melt and rapidly cool), then heat-treat them (for example, to 900°C or higher, or even 900°C to 1200°C, with a heating rate of 10°C / min or higher being particularly preferable) to crystallize them, cool them (cooling at a cooling rate of 10°C / min or higher is particularly preferable) to obtain glass ceramic particles, and then further crush them, finely grind them, and pulverize them through a classification device to produce glass ceramic powder. Furthermore, when producing ceramic powder, an example is to mix and mold the raw materials, perform solid-phase reaction sintering (for example, to 700°C to 1300°C, with a heating rate of 30°C / min or higher for calcination and 10°C / min or higher for final calcination), cool them (cooling at a cooling rate of 10°C / min or higher is particularly preferable) to obtain a ceramic body, and then further crush them, finely grind them, and pulverize them through a classification device to produce ceramic powder. These methods share a common characteristic: by appropriately adjusting the homogeneity of heating and cooling, the heating rate, the heating temperature and time, the cooling rate, the cooling temperature and time, the grinding conditions (material, quantity, and diameter of the media, the type and quantity of solvent in the case of wet grinding, grinding time, etc.), and the grinding equipment, the inorganic oxide powder of the present invention can be obtained.

[0042] <Lithium-ion rechargeable battery> Next, a lithium-ion secondary battery comprising an electrode containing the inorganic oxide powder of the present invention and an electrolyte layer containing a fluorine-containing lithium salt as an electrolyte component will be described in detail.

[0043] As described above, this lithium-ion secondary battery comprises an electrode containing the inorganic oxide powder of the present invention (an electrode containing the inorganic oxide powder of the present invention together with the electrode active material) and an electrolyte layer containing a fluorine-containing lithium salt as an electrolyte component (a non-aqueous electrolyte or a lithium-ion conductive polymer electrolyte), and has excellent discharge capacity retention (high discharge capacity is maintained when repeatedly charged and discharged, for example, a discharge capacity retention rate of more than 70% after 300 cycles under predetermined conditions). For example, an electrode (positive or negative electrode) can be formed by mixing and molding the inorganic oxide powder of the present invention with a positive electrode material (positive electrode active material) or a negative electrode material (negative electrode active material) and, if necessary, a conductive additive, a binder, etc., and combining the electrode (positive and negative electrode) containing this with a non-aqueous electrolyte solution in which a lithium salt containing fluorine is dissolved as an electrolyte component in an aprotic organic solvent, and a separator (placed between the positive and negative electrodes) to form the lithium-ion secondary battery described above. Alternatively, at least a portion of the surface of the positive electrode material or the negative electrode material may be coated with the inorganic oxide powder of the present invention and used to form the electrode, or both the mixing and this coating may be performed. It is also possible to include the inorganic oxide powder of the present invention in only one of the positive or negative electrodes, or in both of them, but it is more preferable that at least the positive electrode contains the inorganic oxide powder of the present invention, as this makes it easier to exhibit the effects of the present invention. Furthermore, when a lithium-ion conductive polymer electrolyte is used as the electrolyte layer, the inorganic oxide powder of the present invention may also be blended into this polymer electrolyte. Generally, incorporating materials other than the electrode active material into the electrodes of a lithium-ion secondary battery tends to lead to a decrease in discharge capacity and discharge capacity retention rate. However, one of the major features of the inorganic oxide powder of the present invention is that by incorporating it together with the electrode active material into the electrodes of a lithium-ion secondary battery, it is possible to maintain the discharge capacity (suppress the decrease in discharge capacity retention rate).

[0044] As the positive electrode active material for the positive electrode material, a transition metal compound capable of intercalating and releasing lithium can be used. For example, a transition metal oxide containing at least one selected from the group consisting of manganese, cobalt, nickel, vanadium, niobium, molybdenum, iron, and titanium (specifically, LiCoO2, etc.) can be used. As the negative electrode active material for the negative electrode material, examples include metallic lithium, lithium-aluminum alloys, lithium-indium alloys and other alloys capable of intercalating and releasing lithium, transition metal oxides such as titanium and vanadium, and carbon-based materials such as graphite (specifically, artificial graphite, etc.). Furthermore, as a conductive additive, carbon-based materials such as acetylene black can be used. Furthermore, as a binder, examples include fluororesins such as Pvdf (polyvinylidene fluoride) and rubber materials such as SBR (styrene-butadiene rubber). In addition, thickeners such as CMC (carboxymethylcellulose sodium) can also be used.

[0045] Furthermore, a non-aqueous electrolyte is an electrolyte in which an electrolyte component containing a fluorine-containing lithium salt is dissolved in a liquid non-aqueous solvent. Examples of this liquid non-aqueous solvent include aprotic organic solvents (for example, mixed solvents of cyclic carbonates and / or linear carbonates such as ethylene carbonate, propylene carbonate, butylene carbonate, vinylene carbonate, fluoroethylene carbonate, ethyl methyl carbonate, diethyl carbonate, and dimethyl carbonate). Examples of the electrolyte component include lithium salts such as lithium hexafluoride phosphate (LiPF6) and lithium bisfluorosulfonimide (LiFSI). Furthermore, examples of lithium-ion conductive polymer electrolytes include those obtained by impregnating a polymer compound (such as a polymer gel, e.g., polyvinylidene fluororide, polyacrylonitrile, etc.) with an electrolyte component containing a fluorine-containing lithium salt. In addition, a non-aqueous liquid solvent as described above may also be impregnated. Furthermore, lithium-ion conductive inorganic materials may be further included. Furthermore, it is also possible to use this non-aqueous electrolyte or lithium-ion conductive polymer electrolyte in combination with other electrolyte components that do not contain fluorine.

[0046] <Discharge capacity maintenance rate> As described above, the lithium-ion secondary battery comprising an electrode containing the inorganic oxide powder of the present invention and an electrolyte layer containing a fluorine-containing lithium salt as an electrolyte component exhibits excellent discharge capacity retention. For example, in the case of a lithium-ion secondary battery comprising an electrode (especially the positive electrode) containing the inorganic oxide powder of the present invention and a non-aqueous electrolyte containing LiPF6 as an electrolyte component, the discharge capacity retention rate after 300 cycles can be more than 70%. In other words, the discharge capacity after 300 cycles of repeated charging and discharging (discharge capacity at the 300th cycle) can be maintained at more than 70% compared to the discharge capacity at the first cycle, which is set at 100%. Furthermore, this discharge capacity retention rate can be 72% or more, even 75% or more, even 78% or more, and even 80% or more.

[0047] The discharge capacity retention rate over 300 cycles can be measured as follows: Specifically, first, a positive electrode is prepared by coating an Al foil, which is the positive electrode current collector, with a positive electrode mixture containing 0-10 wt% of the inorganic oxide powder of the present invention and drying it. A negative electrode is prepared by coating a Cu foil, which is the negative electrode current collector, with a negative electrode mixture containing 0-10 wt% of the inorganic oxide powder of the present invention and drying it (the inorganic oxide powder of the present invention is mixed into either the positive electrode mixture or the negative electrode mixture, or both, and it is particularly preferable to mix it into the positive electrode mixture). A lithium-ion secondary battery is then prepared by combining a non-aqueous electrolyte solution with LiPF6 as the electrolyte component, the above-mentioned positive and negative electrodes, and a separator. Then, using a charge / discharge device, known chemical treatment and known aging are performed in this order, and the following cycle test is conducted to confirm the discharge capacity in a predetermined number of cycles, and the maintenance rate of the discharge capacity (mAh / g) at 300 cycles relative to the discharge capacity (mAh / g) at 1 cycle is calculated. Cycle test: A test in which CC-CV charging (1.0C, 4.4V - 0.05C cutoff, 25℃) and CC discharging (1.0C, 3.0V cutoff, 25℃) are repeated as one cycle.

[0048] The embodiments described above are merely examples to facilitate understanding of the present invention and do not limit it. In other words, the components and the like described above can be changed or improved without departing from the spirit of the present invention, and of course, the present invention includes equivalents thereof.

[0049] The following describes embodiments of the present invention, but the present invention is not limited to the following embodiments, and various modifications are possible within the technical concept of the present invention. [Examples]

[0050] We fabricated various inorganic oxide powders with lithium-ion conductivity and evaluated them, as well as lithium-ion secondary batteries equipped with electrodes containing these powders.

[0051] <Preparation of lithium-ion conductive inorganic oxide powders> As raw materials, LiCO3, H3PO4, TiO2, and Al(PO3)3, along with SiO2 as needed, were weighed and uniformly mixed to achieve the composition shown in Table 1 below, expressed as mass percent in oxide terms, for the final product's component analysis. The mixture was then placed in a platinum pot and rapidly heated (at a heating rate of 200-800°C / min), and heated and melted in an electric furnace at 1500°C for 4 hours while stirring. The resulting glass melt was then rapidly cooled by dropping it into running water to obtain flake-shaped glass. This flake-shaped glass was quickly recovered from the water, spread on a flat plate, and dried in a 100°C constant temperature bath for 12 hours or more to remove moisture. For Example 4, this glass was crushed and sizing to obtain glass powder. For Examples 1-3 and 7, the dried flake-like glass obtained above was heated at a heating rate of 10-100°C / min, and then heat-treated at 950°C for 6-12 hours according to the conditions for each powder to crystallize. Furthermore, it was cooled to room temperature at a cooling rate of 10-20°C / min to obtain glass ceramics, which were similarly crushed and sizing to obtain glass ceramic powder. The crushing and sizing conditions were determined based on the target BET specific surface area and average particle size (D 50 The composition and firing conditions were adjusted to achieve this result.

[0052] On the other hand, for Examples 5-6, LiCO3, Li3PO4, H3PO4, TiO2, and Al(PO3)3 were used as raw materials. The final product was weighed and uniformly mixed so that the composition was as shown in Table 1 below, expressed in mass % on an oxide basis. The mixture was then formed into pellets approximately 15 mm in diameter and 5 mm thick, placed in a platinum crucible, covered with a lid of the same material, and heated in an electric furnace at a heating rate of 50°C / min, followed by calcination at 1000°C for 10 hours. After cooling to room temperature, the pellets were removed, dry-ground to approximately 100 μm or less, and then formed into pellets again in the same manner. The crucible and lid were then placed in an electric furnace at a heating rate of 10°C / min, followed by final calcination (sintering) at 1200°C for 4 hours, and then cooled to room temperature at 20°C / min to obtain ceramics. These were then ground and sized to obtain ceramic powder. Furthermore, for Comparative Examples 1-2, the component composition, BET specific surface area, and average particle size (D 50 The ceramic powder was prepared in the same manner as above, except that the ) was changed. In all cases, the grinding conditions and sizing conditions were set to the target BET specific surface area and average particle size (D 50 The composition and firing conditions were adjusted to achieve this result. Furthermore, as Comparative Example 3, Li manufactured by Toyoshima Seisakusho Co., Ltd. 6.75 La3Zr 1.75 Nb 0.25 O 12 (100 wt% concentration, LLZ ceramic powder) was also prepared.

[0053] Furthermore, the crystalline phase of the glass ceramic powders in Examples 1-3 and 7, and the ceramic powders in Examples 5-6, was confirmed by X-ray diffraction (XRD) measurement (using an automated X-ray diffractometer, Bruker "D8 DISCOVER"), and it was confirmed that in all cases, more than 50% by mass of the total crystalline phase consisted of LATP crystals. In addition, no diffraction peaks were observed in Example 4, confirming that it was amorphous (non-crystalline).

[0054] <Evaluation of Lithium-Ion Conductive Inorganic Oxide Powders> For the obtained glass powder, glass ceramic powder, and ceramic powder, the lithium ion conductivity at 25°C, BET specific surface area, and average particle size (D) were measured. 50 The component composition and HF trapping capacity of each powder were measured and evaluated. The measurements were performed as follows. The results are summarized in Table 1 below, and Figure 1 shows a graph showing the relationship between BET / average particle size and HF trapping capacity for each powder, while Figure 2 shows a graph showing the relationship between BET×Al2O3 and HF trapping capacity for each powder.

[0055] [Lithium ion conductivity at 25°C (S / cm)] Examples 1-4 and 7 used flake-shaped glass or flake-shaped glass that had been crystallized as samples for lithium ion conductivity measurement, while Examples 5 and 6 used sintered bodies after firing as samples. Gold electrodes were formed on each sample as blocking electrodes using a magnetron sputtering apparatus (Sanyu Electronics, SC-701HMC), and impedance measurements were performed at 25°C under the conditions of a frequency of 0.1Hz to 7MHz, an amplitude voltage of 10mV, and an open-circuit voltage, and the lithium ion conductivity (S / cm) was calculated.

[0056] [BET specific surface area (m 2 / g)] For each of the above powders, use approximately 0.5g as a sample (measured at 1m²). 2Using the above adjustments, the material is crushed in an agate mortar as a pretreatment, degassed at 300°C for 30 minutes to remove surface impurities (using N2 (nitrogen) as the adsorbent gas, with a flow rate of 25 mL / min), and then the BET specific surface area (m²) is measured using the BET single-point method with a MOUNTECH Macsorb HM-1201 fully automatic specific surface area meter. 2 The value ( / g) was measured, and the average of two measurements was calculated.

[0057] [Average particle diameter (D 50 (μm) For each of the above powders, the average particle size (50% diameter (D) based on volume) was determined using a laser diffraction / scattering particle size distribution analyzer (Microtrac MT3300, manufactured by Microtrac-Bell). 50 The size (μm) was measured.

[0058] [Component composition (mass %) in terms of oxides] Each of the above powders was analyzed using an ICP emission spectrometer (Agilent Technologies, ICP-OES 5900, measurement conditions: nebulizer flow rate 0.70 L / min, Li measurement wavelength 670.783 nm) to determine the Li content of each powder, and the content (mass) was calculated in terms of Li2O. Furthermore, each of the above powders was separately analyzed using an XRF analyzer (XRF: Rigaku Corporation, Primus II 4kw tube specification, measurement conditions: FP method) to determine the content of each component other than Li. Assuming that all of these components are oxides, the Li2O content calculated from the above ICP analysis was extrapolated to the total mass, and the content of each oxide (mass %) in oxide equivalent was calculated based on this total mass (100 mass%).

[0059] [HF Trap Ability] 60 g of an electrolyte containing 1 ppm to 40 ppm of HF (hydrogen fluoride) and 20 ppm or less of water (electrolyte component: 1 mol / L LiPF6, solvent: ethylene carbonate:ethyl methyl carbonate = 3:7) was mixed with 2 g of any of the above powders (pre-dried under vacuum at 160°C for 24 hours using a glass tube oven (Buch Co., Ltd., B-585)) and sealed with aluminum laminate. After storing this in a 60°C constant temperature bath for one week, the electrolyte was extracted to prepare a sample for HF concentration measurement. This sample was diluted with pure water and neutralized using a 0.01 mol / L sodium hydroxide solution in an automatic titrator. Then, assuming that all acids in the electrolyte were HF, the HF trapping capacity was calculated from the HF concentration using the following formula.

[0060] HF concentration=(DB)×K×F×M×1000 / S D: Titration volume of sodium hydroxide solution to the endpoint (mL) B: Titration volume (mL) of blank sodium hydroxide solution K:HF molecular weight (20.0063) F: Sodium hydroxide solution factor M: Sodium hydroxide concentration (0.01 mol / L) S: Sample amount (g) HF trapping capacity = 100 × (1 / HF concentration)

[0061] <Testing with lithium-ion secondary batteries equipped with electrodes containing lithium-ion conductive inorganic oxide powder> Using the glass powder, glass-ceramic powder, and ceramic powder obtained above, electrodes (positive electrodes) were formed, and the discharge capacity retention rate was confirmed and evaluated in tests using lithium-ion secondary batteries equipped with these electrodes. Specifically, the tests were conducted as follows.

[0062] [Fabrication of electrodes and batteries] 1) Preparation of the positive electrode Using a rotation-orbit mixer (Sinky Co., Ltd., Awatori Rentaro), 98 wt% LiCoO2 was mixed as the positive electrode active material, 1 wt% acetylene black as a conductive additive, 1 wt% PVdF as a binder, and 1 wt% of any of the above powders. NMP (N-methylpyrrolidone) was added to adjust the viscosity, and the mixture was degassed to obtain a paste-like slurry. This slurry was applied to 20 μm aluminum foil using an automatic coating machine (Hosen Co., Ltd., HSCM20-800S) and dried at 120°C. The basis capacity of the electrode (discharge capacity per unit area of ​​the active material layer applied to the substrate) was 3.6 mAh / cm². 2 This was processed using a roll press machine (Housensha, HSR-60150H) to a density of 3.5 g / cm³. 3 The material was adjusted to a film thickness of 59 μm, pressed, punched out to 30 mm x 40 mm using a press cutter (manufactured by Aichi Technical Co., Ltd.), and vacuum dried at 160°C for 16 hours using a glass tube oven (manufactured by Nippon Buch Co., Ltd., B-585). 2) Fabrication of the negative electrode Using a rotation-orbit mixer (Sinky Co., Ltd., Awatori Rentaro), 97.5 wt% artificial graphite was mixed as the negative electrode active material, 1 wt% CMC as a thickener, and 1.5 wt% SBR as a binder. Ion-exchanged water was added to prepare a paste-like slurry. This slurry was applied to 16.5 μm Cu foil using an automatic coating machine (Hosen Co., Ltd., HSCM20-800S) and dried at 120°C. The basis capacitance of the electrode was 4.0 mAh / cm². 2 This was then processed using a roll press machine (Housensha, HSR-60150H) to obtain a density of 1.4 g / cm³. 3 The material was adjusted to a film thickness of 90 μm and pressed, then punched out into 30.5 mm x 40.5 mm pieces using a press cutter (manufactured by Aichi Technical Co., Ltd.), and vacuum dried at 160°C for 16 hours using a glass tube oven (manufactured by Nippon Buch Co., Ltd., B-585). 3) Making a battery In a dry room (temperature 23°C, dew point temperature below -50°C), the positive and negative electrodes obtained in 1) and 2) above were tab-welded so that the A / C ratio (volume ratio of positive electrode active material to negative electrode active material) was 1.2. These electrodes were then placed together with a separator (polypropylene, film thickness 22 μm) in a laminate resin film and heat-sealed with a sealer. An electrolyte (electrolyte component: 1 mol / L LiPF6, solvent: ethylene carbonate:ethyl methyl carbonate = 3:7) was injected to impregnate the electrodes and separator, and the battery was fabricated by vacuum sealing (vacuum degassing and sealing).

[0063] [Checking the discharge capacity retention rate] For all the batteries fabricated, a charge / discharge device (Asuka Electronics Co., Ltd., ACD-M01) and a small environmental tester (Espec Corporation, SH-242) were used for temperature control. The following chemical conversion treatment, vacuum degassing and resealing (same as the vacuum sealing during the production of the cell batteries described above), and the following aging were performed in this order. After that, the following cycle tests were conducted to confirm the discharge capacity in each cycle, and the discharge capacity retention rate at 300 cycles relative to the discharge capacity at 1 cycle was determined. These results are summarized in Table 1 below. Figure 3 shows a graph illustrating the relationship between the HF trapping capacity of each powder mixed in the positive electrode and the discharge capacity retention rate of a battery equipped with that positive electrode at 300 cycles. Figure 4 shows a graph illustrating the relationship between the number of cycles and the discharge capacity retention rate for the battery using Example 2 and the battery using Comparative Example 3. Chemical treatment: CC-CV charge (0.05C, 4.4V-0.01C cutoff, 45℃), CC discharge (0.1C, 3.0V cutoff, 45℃), CC-CV charge (0.1C, 4.4V-0.05C cutoff, 45℃), CC discharge (0.1C, 3.0V cutoff, 45℃). Aging: CC-CV charging (0.2C, 4.4V-0.05C cutoff, 25℃), CC discharge (0.2C, 3.0V cutoff, 25℃). Cycle Test: This test involves repeating CC-CV charging (1.0C, 4.4V-0.05C cutoff, 25℃) and CC discharging (1.0C, 3.0V cutoff, 25℃) as one cycle, and checking the discharge capacity (mAh / g) at the first cycle and every 10 cycles up to the 300th cycle.

[0064] [Table 1]

[0065] These results show that by using glass powder, glass ceramic powder containing LATP crystals, or ceramic powder containing LATP crystals having a predetermined composition and a BET specific surface area within a predetermined range, the HF trapping capacity becomes above a predetermined level, and the discharge capacity retention rate of a predetermined lithium-ion secondary battery equipped with a positive electrode containing this was 73% or more after 300 cycles (Examples 1-7). In particular, in the glass ceramic powder or ceramic powder mentioned above, the product of the BET specific surface area and the Al2O3 component content (BET × Al2O3), or the average particle diameter (D 50 The higher the ratio of the BET specific surface area to the particle size (BET / average particle diameter), the more likely it is that the HF trapping capability will be higher, and lithium-ion secondary batteries equipped with a positive electrode containing this ratio tend to have a higher discharge capacity retention rate. On the other hand, the powders of Comparative Examples 1 and 2, whose composition and BET specific surface area were outside the specified range, had an HF trapping capacity of less than 2.0, and the discharge capacity retention rate of lithium-ion secondary batteries equipped with a positive electrode containing these powders after 300 cycles was less than 67%. Similarly, the powder of Comparative Example 3 (LLZ ceramic powder), whose composition was completely different from that of the above examples, also had an HF trapping capacity of less than 2.0, and the discharge capacity retention rate of lithium-ion secondary batteries equipped with a positive electrode containing these powders was not high, and the effects seen in the above examples were not obtained.

Claims

1. In terms of mass percentage on an oxide basis, Li 2 Component O is 4.0-6.0%, Al 2 O 3 The ingredients should be 3.0-9.0% TiO 2 The ingredients should be 31.0-40.0% P 2 O 5 Ingredients at 49.0-57.0% Contains, BET specific surface area is 8 m 2 / g or more 35m 2 / g or less, The HF trapping capacity is between 2.0 and 9.

0. Inorganic oxide powder.

2. The BET specific surface area and the Al 2 O 3 The inorganic oxide powder according to claim 1, wherein the product of the component content (BET×Al 2 O 3 ) is 30 or more and 300 or less.

3. The average particle size (D) of the inorganic oxide powder 50 The inorganic oxide powder according to claim 1 or 2, wherein the ratio of the BET specific surface area to the (BET / average particle diameter) is 10 or more.

4. The aforementioned Al 2 O 3 The content of the component is 5.0% or more, and the TiO 2 The inorganic oxide powder according to claim 1 or 2, wherein the content of the component is 33.0% or more.

5. The aforementioned Al 2 O 3 The content of the component is 5.0% or more, and the Li 2 Component O, the aforementioned Al 2 O 3 Components, and the TiO 2 Sum of component content (Li 2 O + Al 2 O 3 +TiO 2 The inorganic oxide powder according to claim 1 or 2, wherein the content of ) is 45.5% or more.

6. The inorganic oxide powder according to claim 1 or 2, wherein the inorganic oxide powder is a glass powder.

7. The inorganic oxide powder according to claim 1 or 2, which is a glass ceramic powder or ceramic powder containing LATP crystals.

8. The device comprises an electrode containing the inorganic oxide powder described in claim 1 or 2, and an electrolyte layer containing a lithium salt containing fluorine as an electrolyte component. Lithium-ion rechargeable battery.

Citation Information

Patent Citations

  • Electrode for lithium ion battery, and lithium ion battery