Method for determining the length of non-standard cast slabs, and continuous casting method.
By analyzing molten steel flow and component concentration in the tundish, the method accurately determines the length of off-spec slabs in continuous casting, minimizing yield loss by precise cutting.
Patent Information
- Application Number
- JP2026206977
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2026-09-16
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional methods for determining the length of non-conforming slabs in continuous casting of different steel grades inaccurately estimate the off-spec slab length due to assuming uniform component concentration within the tundish, leading to yield loss.
A method that analyzes the flow of molten steel in the tundish during the mixing of different steel charges, calculates the component concentration over time, and determines the slab length when the concentration meets the standard value, using either transient numerical analysis or an approximate formula based on operational variables.
Accurately estimates the length of off-spec slabs, reducing yield loss by precisely identifying and cutting non-conforming portions.
Smart Images

Figure 2026183111000001_ABST
Abstract
Description
TECHNICAL FIELD
[0001] The present invention relates to a non-conforming slab length determination method for determining the length of a non-conforming slab at the joint portion of a continuously cast slab produced by supplying post-charge molten steel with different components to a tundish in which pre-charge molten steel remains, and a continuous casting method.
BACKGROUND ART
[0002] In continuous casting of different steel grades, in which molten steels of different components are cast continuously, the joint portion of the slab where the pre-charge molten steel and the post-charge molten steel are mixed is usually cut to a uniform fixed length and discarded, regardless of the component range or operating conditions. This is based on the viewpoint of quality assurance, and is because the component concentration at the joint portion often satisfies neither the specification values of the slab cast from the pre-charge molten steel nor the specification values of the slab cast from the post-charge molten steel. However, if the joint portion of the slab is cut to a uniform fixed length, there is a possibility that portions that actually satisfy the specification values of the slab cast from the post-charge molten steel are also cut and discarded, resulting in yield loss. For this reason, conventionally, in the continuous casting of different steel grades, it has been studied to accurately determine the slab length of the joint portion whose component concentration is out of specification (hereinafter also referred to as "non-conforming slab length") to suppress yield loss.
[0003] For example, Patent Document 1 discloses a method for processing a joint portion slab in continuous casting of different steel grades, in which molten steel having a different composition from the preceding charge is poured as the succeeding charge into a tundish in which the preceding charge molten steel remains, and the preceding charge and the succeeding charge are continuously cast in sequence. In this method, the slab position corresponding to the molten steel level position in the mold at the time when the succeeding charge is poured into the tundish is taken as the reference position, and from the reference position, the succeeding charge slab up to the range of the slab length calculated in consideration of the weight of the preceding charge molten steel remaining in the tundish and the cross-sectional area of the slab is subjected to scrap processing.
[0004] Furthermore, Patent Document 2 discloses a method for determining the component mixing length when performing continuous casting by continuously supplying molten metal of a subsequent charge with a different composition to an intermediate container while leaving molten metal from a previous charge in the intermediate container. In this method, the weight of the molten metal in the intermediate container and the slab withdrawal speed are continuously measured, and the injection speed into the intermediate container and the injection speed from the intermediate container to the mold are continuously calculated. Then, a component mixing simulation is performed based on these measured and calculated values, the slab size, the component values of the preceding and succeeding ladles, and the allowable component ranges. The length of the portion where the slab component values in the simulation result fall outside the molten metal component range of the preceding and succeeding charges is defined as the component mixing length. [Prior art documents] [Patent Documents]
[0005] [Patent Document 1] Japanese Patent Publication No. 2009-72800 [Patent Document 2] Japanese Patent Application Publication No. 1-258857 [Overview of the project] [Problems that the invention aims to solve]
[0006] However, it is presumed that the methods described in Patent Documents 1 and 2 above calculate the length of the off-spec slab at the joint based on a fully mixed tank model in which molten steel flowing into the tundish is completely mixed with the molten steel already inside the tundish the moment it enters the tundish. The fully mixed tank model assumes that the component concentration of the molten steel inside the tundish is uniform regardless of location. However, in reality, the molten steel inside the tundish flows over time, and the component concentration of the molten steel is not uniform at different locations within the tundish. For this reason, it is possible that conventional methods cannot accurately estimate the length of the off-spec slab at the joint.
[0007] Therefore, the present invention has been made in view of the above problems, and the object of the present invention is to provide a method for determining the length of an out-of-spec cast slab and a continuous casting method that can more accurately estimate the length of an out-of-spec cast slab at a joint in continuous casting of different types of steel, and suppress yield loss due to cutting and discarding the cast slab. [Means for solving the problem]
[0008] To solve the above problems, according to one aspect of the present invention, a method for determining the length of an out-of-spec cast slab at the joint of a cast slab that is continuously cast by supplying molten steel of a later charge with a different composition to a tundish in which molten steel of a earlier charge remains is provided. The method involves analyzing the flow of molten steel in the tundish when casting a joint where molten steel of a earlier charge and molten steel of a later charge are mixed, calculating the component concentration of the molten steel of the earlier charge contained in the molten steel flowing from the tundish to the mold at each time point of the continuous casting operation, and determining the length of the cast slab from the start of tapping molten steel from the tundish until the component concentration of the molten steel at the joint, calculated based on the component concentration of the molten steel of the earlier charge, meets the standard value, as the length of the cast slab, and determining this as the length of the cast slab.
[0009] The shape of the tundish, the shape of the sliding nozzle, the amount of molten steel from the pre-charge remaining in the tundish, the supply flow rate of the molten steel from the post-charge, and the casting speed may be set, and the flow of molten steel within the tundish may be analyzed.
[0010] Furthermore, in order to solve the above problems, according to another aspect of the present invention, there is a method for determining the length of an out-of-spec cast slab at the joint of a cast slab that is continuously cast by supplying molten steel of a later charge with a different composition to a tundish in which molten steel of a previous charge remains, wherein for each of several operating conditions that are expected to be implemented, a dataset is prepared in advance of the mass fraction of molten steel of the previous charge contained in the molten steel flowing from the tundish to the mold calculated based on the operating conditions and the operating variables included in the operating conditions, an approximate formula representing the relationship between the operating variables and the mass fraction of molten steel of the previous charge contained in the molten steel flowing from the tundish to the mold is generated using the multiple datasets, the component concentration of the molten steel at the joint to be analyzed is calculated using the approximate formula, and the length of the cast slab from the start of tapping molten steel from the tundish until the component concentration of the molten steel at the joint satisfies the standard value is determined as the length of the out-of-spec cast slab.
[0011] When the mass fraction of the molten steel in the first charge is F, the mass fraction of the molten steel in the second charge is 1-F, the component concentration of the molten steel in the first charge is A, and the component concentration of the molten steel in the second charge is B, the component concentration of the molten steel at the joint flowing from the tundish to the mold may be expressed as FA + (1-F)B.
[0012] Furthermore, in order to solve the above problems, according to another aspect of the present invention, a continuous casting method is provided for continuously casting slabs by supplying molten steel of a later charge with a different composition to a tundish in which molten steel of a previous charge remains, wherein when casting the joint portion of a slab in which the molten steel of the previous charge and the molten steel of the later charge are mixed, the flow of molten steel in the tundish is analyzed to calculate the component concentration of the molten steel of the previous charge contained in the molten steel flowing from the tundish to the mold at each time of the continuous casting operation, the length of the slab from the start of tapping molten steel from the tundish until the component concentration of the molten steel at the joint portion, calculated based on the component concentration of the molten steel of the previous charge, meets the standard value, is determined as the off-spec slab length, and the portion corresponding to the off-spec slab length is cut and separated from the joint portion as an off-spec slab.
[0013] The shape of the tundish, the shape of the sliding nozzle, the amount of molten steel from the pre-charge remaining in the tundish, the supply flow rate of the molten steel from the post-charge, and the casting speed may be set, and the flow of molten steel within the tundish may be analyzed.
[0014] Furthermore, in order to solve the above problems, according to another aspect of the present invention, a continuous casting method is provided for continuously casting slabs by supplying molten steel of a later charge with a different composition to a tundish in which molten steel of a previous charge remains, wherein, before continuously casting the slabs, a dataset is prepared in advance for each of several operating conditions that are expected to be implemented, consisting of the mass fraction of molten steel of the previous charge contained in the molten steel flowing from the tundish to the mold calculated based on the operating conditions, and the operating variables included in the operating conditions, and an approximate formula is generated using the multiple datasets to represent the relationship between the operating variables and the mass fraction of molten steel of the previous charge contained in the molten steel flowing from the tundish to the mold, the component concentration of the molten steel at the joint to be analyzed is calculated using the approximate formula, the length of the slab from the start of tapping molten steel from the tundish until the component concentration of the molten steel at the joint meets the standard value is determined as the off-spec slab length, and the portion corresponding to the off-spec slab length is cut and separated from the joint as an off-spec slab.
[0015] When the mass fraction of the molten steel in the first charge is F, the mass fraction of the molten steel in the second charge is 1-F, the component concentration of the molten steel in the first charge is A, and the component concentration of the molten steel in the second charge is B, the component concentration of the molten steel at the joint flowing from the tundish to the mold may be expressed as FA + (1-F)B. [Effects of the Invention]
[0016] As described above, according to the present invention, in continuous casting of different types of steel, the length of the off-spec cast slab at the joint can be estimated more accurately, and yield loss due to cutting and discarding the cast slab can be suppressed. [Brief explanation of the drawing]
[0017] [Figure 1] This is an explanatory diagram showing the schematic configuration of a continuous casting equipment according to one embodiment of the present invention. [Figure 2A] This is an explanatory diagram showing an example of the flow of continuous casting of different steel types. [Figure 2B] This is an explanatory diagram showing another example of the flow of continuous casting of different steel types. [Figure 3] This is a flowchart showing the method for determining the length of non-standard cast slabs according to the present embodiment, illustrating a case where the molten steel flow in the tundish is predicted by unsteady numerical analysis. [Figure 4] This is a graph showing an example of the temporal transition of the component concentration of molten steel at the joint portion. [Figure 5] This is a flowchart showing the method for determining the length of non-standard cast slabs according to the present embodiment, illustrating a case where the molten steel flow in the tundish is predicted using an approximate expression. [Figure 6] This is a graph showing an example of the measured values and the calculated values based on the approximate expression for the temporal transition of the component concentration of molten steel at the joint portion. [Mode for Carrying Out the Invention]
[0018] Hereinafter, preferred embodiments of the present invention will be described in detail with reference to the accompanying drawings. Note that in the present specification and the drawings, components having substantially the same functional configuration are denoted by the same reference numerals, thereby omitting redundant description.
[0019] [1. Configuration of Continuous Casting Equipment] First, the schematic configuration of the continuous casting equipment according to an embodiment of the present invention will be described based on FIG. 1. FIG. 1 is an explanatory diagram showing the schematic configuration of the continuous casting equipment 1 according to the present embodiment.
[0020] The continuous casting equipment 1 according to the present embodiment is an apparatus for continuously casting molten steel 2 using a continuous casting mold 10 to produce cast slabs 3. Although the continuous casting equipment 1 shown in FIG. 1 is a vertical bending type continuous casting equipment 1, the present invention is not limited to such an example, and is applicable to various other continuous casting equipment such as a curved type or a vertical type. The continuous casting equipment 1 includes a mold (casting mold) 10, a ladle 4, a tundish 5, an immersion nozzle 6, and a secondary cooling device 7.
[0021] The ladle 4 is a movable container for transporting molten steel 2 from the outside to the tundish 5. The ladle 4 is positioned above the tundish 5, and the molten steel 2 in the ladle 4 is supplied to the tundish 5. The tundish 5 is positioned above the mold 10, and stores the molten steel 2 and removes inclusions from it. The immersion nozzle 6 extends downward from the lower end of the tundish 5 toward the mold 10, and its tip is immersed in the molten steel 2 in the mold 10. The immersion nozzle 6 continuously supplies the molten steel 2 from which inclusions have been removed in the tundish 5 into the mold 10.
[0022] The mold 10 is a rectangular cylindrical mold formed according to the width and thickness of the cast slab 3. The mold 10 is composed of, for example, a pair of short copper plates and a pair of long copper plates. The copper plates constituting the mold 10 are, for example, water-cooled copper plates. The molten steel 2 in contact with the inner surface of these copper plates is cooled, and a cast slab 3 containing an unsolidified portion 3b inside the solidified outer shell 3a is produced. As the solidified shell 3a moves downward in the mold 10, the solidification of the unsolidified portion 3b inside progresses, and the thickness of the solidified outer shell 3a gradually increases. The cast slab 3 containing the solidified shell 3a and the unsolidified portion 3b is then withdrawn from the lower end of the mold 10.
[0023] The secondary cooling device 7 is installed in the secondary cooling zone 9 below the mold 10 and cools the cast slab 3 as it is withdrawn from the lower end of the mold 10 while supporting and transporting it. The secondary cooling device 7 has a plurality of pairs of support rolls 8 arranged on both sides of the thickness direction of the cast slab 3, and a plurality of spray nozzles (not shown) that spray cooling water onto the cast slab 3. The support rolls 8 provided in the secondary cooling device 7 are arranged in pairs on both sides of the thickness direction of the cast slab 3 and function as a support and transport means that supports and transports the cast slab 3. By supporting the cast slab 3 from both sides of the thickness direction with these support rolls 8, breakout and bulging of the cast slab 3 during solidification can be prevented in the secondary cooling zone 9.
[0024] The support rolls 8 form the transport path (pass line) for the cast slab 3 in the secondary cooling zone 9. As shown in Figure 1, this pass line is vertical directly below the mold 10 (vertical zone 9A), then curves in a curved shape (curved zone 9B), and finally becomes horizontal (horizontal zone 9C). The support rolls 8 consist of a support roll provided in the vertical zone 9A to support the cast slab 3 immediately after it is withdrawn from the mold 10, a pinch roll which is a driven roll that withdraws the cast slab 3 from the mold 10, and segment rolls provided in the curved zone 9B and horizontal zone 9C to support and guide the cast slab 3 along the pass line.
[0025] After passing through the secondary cooling zone 9, the cast slab 3 is cut to a predetermined length by a cast slab cutting machine (not shown) installed downstream of the horizontal zone 9C. The cut cast slab 3 moves along a table roll and is transported to the equipment for the next process.
[0026] [2. Continuous casting of different types of steel] In continuous casting of dissimilar steel grades, molten steel from a pre-charge and molten steel from a post-charge, each with different component concentrations, are cast in succession. Continuous casting of dissimilar steel grades is carried out, for example, in the flow shown in Figure 2A or Figure 2B. Figures 2A and 2B are explanatory diagrams showing an example of the flow in continuous casting of dissimilar steel grades.
[0027] For example, in the continuous casting of different steel types shown in Figure 2A, as shown in the upper part of Figure 2A, once the supply of the pre-charge molten steel 2a from the ladle 4a to the tundish 5 is complete, the tapping of steel from the tundish 5 to the mold 10 is stopped. The molten steel 2a from the pre-charge remains in the tundish 5. Next, the ladle 4a that contained the pre-charge molten steel 2a is moved from above the mold 10, and as shown in the center of Figure 2A, the ladle 4b containing the next charge (post-charge) molten steel 2b is moved above the tundish 5. Then, the post-charge molten steel 2b from the ladle 4b is supplied to the tundish 5 via the sliding nozzle 15. After that, as shown in the lower part of Figure 2A, once a predetermined amount of molten steel 2 has been supplied to the tundish 5, the molten steel 2 is supplied to the mold 10 from the tapping port 5a of the tundish 5, and casting begins. Even after tapping begins, molten steel 2b continues to be supplied to tundish 5 from ladle 4b.
[0028] As shown in the center of Figure 2A, the molten steel 2b from the later charge is supplied into the tundish 5 where the molten steel 2a from the earlier charge remains. For this reason, for a while after the start of tapping from the tundish 5 shown at the bottom of Figure 2A, molten steel 2, which is a mixture of the molten steel 2a from the earlier charge and the molten steel 2b from the later charge, is supplied to the mold 10, and slabs that do not meet the standard values for the component concentration of the slabs cast from the molten steel from the later charge are cast. Subsequently, as the proportion of the molten steel 2b from the later charge increases in the molten steel 2 in the tundish 5, the component concentration of the slabs will meet the standard values, and the casting of slabs that can be used as products will begin.
[0029] Furthermore, as shown in Figure 2B, different types of steel can be continuously cast without stopping the tapping from the tundish 5. As shown in the upper part of Figure 2B, first, the molten steel 2a of the previous charge is supplied from the ladle 4a to the tundish 5 via the sliding nozzle 15. Once the supply of the molten steel 2a of the previous charge from the ladle 4a to the tundish 5 is complete, as shown in the center of Figure 2B, the ladle 4a that contained the molten steel 2a of the previous charge is moved from above the tundish 5 while continuing to tap the steel from the tundish 5 to the mold 10. Then, the ladle 4b containing the molten steel 2b of the next charge (post-charge) is moved above the tundish 5. After that, as shown in the lower part of Figure 2B, the molten steel 2b of the post-charge is supplied from the ladle 4b to the tundish 5 via the sliding nozzle 15.
[0030] The molten steel 2b from the later charge is supplied into the tundish 5 where the molten steel 2a from the earlier charge remains. For a while after the supply of the molten steel 2b from the later charge begins, molten steel 2, which is a mixture of the molten steel 2a from the earlier charge and the molten steel 2b from the later charge, is supplied to the mold 10, and slabs that do not meet the standard values for the component concentration of the slabs to be cast from the molten steel 2b from the later charge are cast. Subsequently, as the proportion of the molten steel 2b from the later charge increases in the molten steel 2 in the tundish 5, the component concentration of the slabs will meet the standard values, and the casting of slabs that can be used as products will begin.
[0031] Here, at the joint between the pre-charge and post-charge of the slab, any portion that does not meet the standard value for the component concentration of the slab cast from the molten steel of the post-charge is cut off, separated, and discarded as an off-spec slab. If the length of this off-spec slab can be accurately predicted, excessive slab waste can be avoided, and yield loss can be suppressed.
[0032] Therefore, in the method for determining the length of an out-of-spec cast slab according to this embodiment, the flow of molten steel in the tundish 5 when the molten steel 2a from the pre-charge and the molten steel 2b from the post-charge are mixed is analyzed, as shown in the center of Figure 2A, the lower part of Figure 2A, and the lower part of Figure 2B, and the time course of the component concentration contained in the molten steel 2 flowing from the tap 5a of the tundish 5 to the mold 10 is predicted. As a result, the component concentration of the molten steel in the tundish can be predicted with greater accuracy compared to when it is determined based on a complete mixing tank model that assumes the component concentration of the molten steel in the tundish is uniform regardless of location, and the length of the out-of-spec cast slab at the joint can be accurately estimated. The method for determining the length of an out-of-spec cast slab according to this embodiment will be described in detail below.
[0033] [3. Method for determining the length of non-standard cast slabs] [3-1. Prediction of molten steel flow in a tundish using transient numerical analysis] First, based on Figure 3, a method for determining the length of an out-of-spec slab when predicting the molten steel flow in a tundish using transient numerical analysis will be explained. Figure 3 is a flowchart showing the method for determining the length of an out-of-spec slab according to this embodiment, and shows the case where the molten steel flow in a tundish is predicted using transient numerical analysis. In transient numerical analysis, computational fluid dynamics software is used to simulate the shape of the actual tundish and analyze the molten steel flow in the tundish. The program of the computational fluid dynamics software is executed by an information processing device such as a computer.
[0034] First, as shown in Figure 3, the initial settings for the analysis conditions necessary for performing transient numerical analysis are performed (S100). For transient numerical analysis, the shape of the tundish and the shape of the sliding nozzle are set as initial settings. The shape of the tundish is defined by size information necessary to identify the shape of the tundish, such as the length, width, and depth, as well as the shape of the tapping port, the number of tapping ports, and the position of the tapping ports on the tundish. The shape of the sliding nozzle is defined by the nozzle cross-sectional shape, and its installation position relative to the tundish is also set. Initial settings are performed by the operator inputting various information into the information processing device.
[0035] Next, the operating conditions for performing transient numerical analysis are input (S110). In this embodiment, the operating conditions input are the amount of molten steel from the pre-charge remaining in the tundish, the supply flow rate of the molten steel from the post-charge supplied to the tundish via the sliding nozzle, and the casting speed. The operator inputs the operating conditions into the information processing device.
[0036] Once the analysis conditions are set in steps S100 and S110, the information processing device executes the computational fluid dynamics software program to analyze the molten steel flow in the tundish. Based on the transient numerical analysis results, the concentration of pre-charge molten steel components in the molten steel flowing from the tundish to the mold at each time point in the continuous casting operation is calculated (S120). In transient numerical analysis, the entire analysis is divided into predetermined unit time periods, and the phenomenon at the next time point is determined by gradually advancing the time, thereby identifying the state of the molten steel flow process and obtaining the changes until the final state (in this embodiment, the state in which only the post-charge molten steel components remain). In other words, the time progression of the concentration of pre-charge molten steel components in the molten steel flowing from the tundish to the mold is obtained.
[0037] Transstational numerical analysis only needs to be performed on at least one of the various components contained in the molten steel. When obtaining the time course of a specific component concentration, it may be necessary to obtain data on components whose concentrations differ significantly between the molten steel from the previous charge and the molten steel from the subsequent charge. This allows for a clear capture of the change in the ratio of molten steel from the previous charge to the molten steel from the subsequent charge at the joint.
[0038] In step S120, when the component concentrations of the pre-charge molten steel contained in the molten steel flowing from the tundish to the mold at each time point of the continuous casting operation are calculated, the information processing device calculates the component concentration of the molten steel at the joint flowing from the tundish to the mold (S130). When the mass fraction of the pre-charge molten steel is F, the mass fraction of the post-charge molten steel is 1-F, the component concentration of the pre-charge molten steel is A, and the component concentration of the post-charge molten steel is B, the component concentration of the molten steel at the joint can be expressed by the following formula (1).
[0039] The concentration of molten steel components at the joint = F × A + (1 - F) × B ... (1)
[0040] The information processing device calculates the component concentration of the molten steel at the joint at each time point, based on the above formula (1).
[0041] Subsequently, based on the time progression of the component concentration of the molten steel at the joint calculated in step S130, the length of the slab from the start of tapping the molten steel from the tundish until the component concentration of the molten steel at the joint meets the standard value is determined as the out-of-spec slab length (S140). The standard value is set based on the component concentration of the molten steel in the subsequent charge, and may, for example, be a value within the range of acceptable component concentration for the molten steel in the subsequent charge. When the component concentration of the molten steel at the joint calculated in step S130 meets the standard value, it can be determined that the joint has transitioned from the molten steel of the previous charge to the molten steel of the subsequent charge. Therefore, the length of the slab from the start of tapping the molten steel from the tundish until the component concentration of the molten steel at the joint meets the standard value is determined as the out-of-spec slab length. The out-of-spec slab length may be determined by the information processing device based on a pre-set standard value, or it may be determined by the operator by checking the time progression of the component concentration of the molten steel at the joint calculated in step S130.
[0042] The above describes a method for determining the length of off-spec cast slabs when predicting molten steel flow in a tundish using transient numerical analysis. This method allows for accurate prediction of the component concentration of the molten steel in the tundish by performing transient numerical analysis based on computational fluid dynamics, thereby enabling precise estimation of the length of off-spec cast slabs at the joints. As a result, slab yield loss can be suppressed.
[0043] Figure 4 shows an example of the time course of the component concentrations of the molten steel at the joint calculated in step S130. In Figure 4, we focus on Mn among the components contained in the molten steel and show the time course of Mn concentration, including measured values, calculated values from transient numerical analysis, and calculated values based on a complete mixing tank model. The casting length is defined as the length of the cast slab from the tapping port, with the time when tapping from the tundish begins set to 0.
[0044] In the transient numerical analysis and calculations based on the fully mixed tank model, the scenario assumed continuous casting of different steel types in the flow shown in Figure 2A. With 8 tons of molten steel from the previous charge remaining in the tundish, molten steel from the next charge was supplied to the tundish from the ladle at a rate of 20 tons / min, and tapping began when the amount of molten steel in the tundish reached 37 tons. After tapping began, molten steel from the next charge was supplied to the tundish at a rate of 5.88 tons / min. The casting speed was set to the same rate as the operation when the measured value of the target casting speed of 1.2 m / min was obtained.
[0045] As shown in Figure 4, the measured values and the calculated values from transient numerical analysis are generally consistent. In contrast, the calculated values from the fully mixed tank model are close to the measured values, but the prediction results show that even parts of the slab where the measured values fall outside the specified range meet the specified range. The fully mixed tank model predicts the concentration of molten steel in the tundish by assuming that the molten steel flowing into the tundish is completely mixed with the molten steel already in the tundish the moment it enters, and that the concentration of components in the molten steel within the tundish is uniform regardless of location. Therefore, the fully mixed tank model can determine the concentration of molten steel without considering the shape of the tundish or the shape of the sliding nozzle. However, in reality, the molten steel in the tundish flows over time, and the concentration of components in the molten steel at different locations within the tundish is not uniform. For this reason, it is presumed that the calculated values from the fully mixed tank model deviate from the measured values.
[0046] [3-2. Prediction of molten steel flow in a tundish using an approximation formula] Next, a method for determining the length of an off-spec cast slab when predicting the molten steel flow in a tundish using an approximate formula will be described based on Figure 5. Figure 5 is a flowchart showing the method for determining the length of an off-spec cast slab according to this embodiment, and shows the case where the molten steel flow in a tundish is predicted using an approximate formula. The approximate formula used to predict the molten steel flow in a tundish can be obtained using an information processing device such as a computer.
[0047] First, as shown in Figure 5, for each of the multiple operating conditions that are expected to be implemented, a dataset is prepared in advance containing the mass fraction of pre-charged molten steel included in the molten steel flowing from the tundish to the mold, calculated based on the operating conditions, and the operating variables included in those operating conditions (S200).
[0048] The mass fraction of pre-charge molten steel contained in the molten steel flowing from the tundish to the mold, calculated based on operating conditions, can be determined, for example, by transient numerical analysis using computational fluid dynamics software, as explained in Figure 3. While the operating variables to be included in the dataset can be arbitrarily selected, it is preferable to select those that affect the molten steel flow within the tundish. For example, the amount of pre-charge molten steel remaining in the tundish, the supply flow rate of post-charge molten steel supplied to the tundish via the sliding nozzle, and the casting rate should be included in the dataset.
[0049] Since the flow of molten steel within the tundish depends on the shape of the tundish and the sliding nozzle, it is desirable to prepare a group consisting of multiple data sets for each continuous casting facility. There is no particular limit to the number of data sets in one group, but about ten to several dozen would suffice.
[0050] Next, using the multiple datasets prepared in step S200, an approximate formula is generated that represents the relationship between the operational variables and the mass fraction of pre-charge molten steel contained in the molten steel flowing from the tundish to the mold (S210). That is, an approximate formula is generated that takes the operational variables as arguments and represents the mass fraction of pre-charge molten steel contained in the molten steel flowing from the tundish to the mold. The method for generating the approximate formula is not particularly limited and may be generated by statistical analysis, for example, or by machine learning. The operational variables used as arguments may be one or more operational variables such as the amount of pre-charge molten steel remaining in the tundish, the supply flow rate of post-charge molten steel supplied to the tundish via the sliding nozzle, the casting rate, etc.
[0051] In step S210, an approximation formula is generated, and the component concentrations of the molten steel at the joint to be analyzed are calculated using this approximation formula (S220). First, by inputting the value of the operational variable used as an argument at a certain point in time into the approximation formula for the operation to be analyzed, the mass fraction of the pre-charged molten steel contained in the molten steel flowing from the tundish to the mold at that time can be obtained. Once the mass fraction of the pre-charged molten steel is obtained, the component concentrations of the molten steel at the joint to be analyzed can be determined from the above formula (1).
[0052] Subsequently, based on the component concentration of the molten steel at the joint calculated in step S220, the length of the cast slab from the start of tapping the molten steel from the tundish until the component concentration of the molten steel at the joint meets the standard value is determined as the off-spec cast slab length (S230). The process in step S230 can be carried out in the same way as in step S140 in Figure 3.
[0053] The above describes a method for determining the length of off-spec slabs when predicting molten steel flow in a tundish using an approximate formula. The mass fraction of pre-charge molten steel contained in the molten steel flowing from the tundish to the mold can also be accurately calculated by the transient numerical analysis described in Figure 3. On the other hand, transient numerical analysis has a high computational load, and it may take about a month to obtain the calculation results shown in Figure 4, for example. In contrast, if the mass fraction of pre-charge molten steel contained in the molten steel flowing from the tundish to the mold is expressed in advance by an approximate formula, it becomes possible to calculate this value instantaneously. For example, if the approximate formula generated in step S210 is implemented in a process computer, the mass fraction of pre-charge molten steel contained in the molten steel flowing from the tundish to the mold can be obtained by inputting the values of the operational variables used as arguments into the approximate formula in real time during continuous casting operation. As a result, the component concentration of the molten steel at the current joint can be obtained. Therefore, the length of off-spec slabs can be identified in real time.
[0054] Furthermore, since multiple datasets for creating approximation formulas are prepared from the analysis results of transient numerical analysis, the accuracy of predicting the component concentration of molten steel in the tundish using transient numerical analysis can be maintained, and the length of the off-spec cast slab at the joint can be accurately estimated.
[0055] For example, suppose that based on the calculated values obtained by transient numerical analysis shown in Figure 4, an approximate formula representing the relationship between the casting length and the mass fraction of the pre-charge molten steel contained in the molten steel flowing from the tundish to the mold is obtained as equation (2) below.
[0056]
number
[0057] Here, X is the casting length [m]. The casting length X can be expressed as the product of the operating variable casting speed, the area of the tundish tap, and time. Also, α = 1.84376 and β = 0.439307. By substituting the value of the mass fraction of pre-charged molten steel contained in the molten steel flowing from the tundish to the mold, calculated by equation (2), into equation (1), the Mn concentration of the molten steel can be determined. For example, if the Mn concentration of the molten steel is calculated every 500 mm of casting length, the time course of the Mn concentration of the molten steel can be obtained, as shown in Figure 6. Comparing this with the two measured values under the same casting conditions shown in Figure 6, the Mn concentration obtained based on the approximation formula is in general agreement with the measured value. From these results, it can be seen that even when using an approximation formula, the accuracy of predicting the component concentration of molten steel in the tundish by transient numerical analysis can be maintained, and the length of the off-spec cast slab at the joint can be accurately estimated.
[0058] Although preferred embodiments of the present invention have been described in detail above with reference to the attached drawings, the present invention is not limited to these examples. It is clear to any person with ordinary skill in the art to which the present invention belongs that various modifications or alterations can be conceived within the scope of the technical idea described in the claims, and these are also understood to fall within the technical scope of the present invention. [Explanation of Symbols]
[0059] 1. Continuous casting equipment 2 Molten steel 2a Molten steel from the previous charge 2b Molten steel after charge 3 cast slabs 3a Solidified shell 3b Unsolidified area 4 Ladle 4a Ladle (pre-charge) 4b Ladle (recharge after use) 5 Tan Dish 5a Steel tapping port 6. Immersion nozzle 7 Secondary cooling device 8 support rolls 9. Secondary cooling zone 9A Vertical band 9B Curved Zone 9C Horizontal band 10 molds 15 Sliding Nozzles
Claims
1. A method for determining the length of an out-of-spec cast slab at the joint of a cast slab that is continuously cast by supplying molten steel of a later charge with a different composition to a tundish in which molten steel of a previous charge remains, For each of the multiple operating conditions that are expected to be implemented, a dataset is prepared in advance containing the mass fraction of the pre-charged molten steel included in the molten steel flowing from the tundish to the mold, calculated based on the said operating conditions, and the operating variables included in said operating conditions. Using multiple datasets, an approximate formula is generated that represents the relationship between the operating variables and the mass fraction of the pre-charged molten steel contained in the molten steel flowing from the tundish to the mold. A method for determining the length of an out-of-spec cast slab, comprising: calculating the component concentration of the molten steel at the joint to be analyzed using the aforementioned approximation formula; and determining the length of the cast slab from the start of tapping the molten steel from the tundish until the component concentration of the molten steel at the joint meets the standard value as the out-of-spec cast slab length.
2. The method for determining the length of an off-spec cast slab according to claim 1, wherein, when the mass fraction of the molten steel in the pre-charge is F, the mass fraction of the molten steel in the post-charge is 1-F, the component concentration of the molten steel in the pre-charge is A, and the component concentration of the molten steel in the post-charge is B, the component concentration of the molten steel in the joint flowing from the tundish to the mold is expressed as FA + (1-F)B.
3. A continuous casting method in which molten steel of a different composition is supplied to a tundish containing molten steel from a previous charge, thereby continuously casting slabs. Before the continuous casting of the aforementioned slab, For each of the multiple operating conditions that are expected to be implemented, a dataset is prepared in advance containing the mass fraction of the pre-charged molten steel included in the molten steel flowing from the tundish to the mold, calculated based on the said operating conditions, and the operating variables included in said operating conditions. Using multiple datasets, an approximate formula is generated that represents the relationship between the operating variables and the mass fraction of the pre-charged molten steel contained in the molten steel flowing from the tundish to the mold. Using the aforementioned approximation formula, the component concentrations of the molten steel at the joint to be analyzed are calculated, and the length of the cast slab from the start of tapping the molten steel from the tundish until the component concentration of the molten steel at the joint meets the standard value is determined as the length of the non-standard cast slab. A continuous casting method comprising cutting and separating the portion corresponding to the non-standard cast slab length from the aforementioned joint portion as a non-standard cast slab.
4. The continuous casting method according to claim 3, wherein, when the mass fraction of the molten steel in the pre-charge is F, the mass fraction of the molten steel in the post-charge is 1-F, the component concentration of the molten steel in the pre-charge is A, and the component concentration of the molten steel in the post-charge is B, the component concentration of the molten steel in the joint flowing from the tundish to the mold is expressed as FA + (1-F)B.
Citation Information
Patent Citations
Method for deciding length of component mixture in continuous casting
JP1989258857A