Powder and method for manufacturing powder

A powder with high sphericity and negative thermal expansion properties is produced using spray-drying and secondary calcination, addressing thermal expansion challenges in precision equipment by suppressing thermal expansion in composite materials.

JP2026183151APending Publication Date: 2026-11-19MISARIO CO LTD
View PDF 1 Cites 0 Cited by

Patent Information

Application Number
JP2026208051
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2025-10-14
Filing Date
2026-09-17
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing materials face challenges in achieving low thermal expansion while maintaining processability, particularly in precision equipment where slight thermal expansion can cause functional issues, and combining materials with different thermal expansion coefficients leads to problems like interfacial delamination and disconnection.

Method used

A powder containing a negative thermal expansion material with a sphericity of 0.2 or higher is produced through a method involving spray-drying and secondary calcination at 1000°C or lower, and a secondary calcination time of 10 minutes or more, ensuring small particle sizes and rounded shapes.

Benefits of technology

The resulting powder exhibits excellent negative thermal expansion properties, effectively suppressing thermal expansion in composite materials, reducing mechanical load, and maintaining precision in applications like semiconductor manufacturing.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026183151000001_ABST
    Figure 2026183151000001_ABST
Patent Text Reader

Abstract

To provide a powder material with excellent negative thermal expansion properties. [Solution] The powder contains a material that undergoes negative thermal expansion and has a sphericity of 0.2 or higher.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This disclosure relates to a powder containing a negative thermal expansion material and a method for producing the powder. [Background technology]

[0002] Generally, composite materials can exhibit functions that cannot be achieved with individual materials. For example, by combining a resin material with high thermal expansion with an inorganic powder filler with low thermal expansion, such as silica, as a thermal expansion inhibitor, it is possible to achieve low thermal expansion that cannot be achieved with a single resin while maintaining the high processability that is a characteristic of resin materials.

[0003] It is generally known that materials expand with increasing temperature, but recent advances in industrial technology demand control even over thermal expansion, which is an inherent characteristic of solid materials. -5 Even a small rate of change, such as a small one from a general perspective, can be a serious problem in fields such as semiconductor device manufacturing, where nanometer-level precision is required, or in precision equipment where even slight distortion of components can have a significant impact on functionality. Furthermore, in devices that combine multiple materials, differences in the thermal expansion of each constituent material can lead to other problems such as interfacial delamination and disconnection.

[0004] On the other hand, negative thermal expansion materials are also known, in which the lattice volume decreases with increasing temperature (having a negative coefficient of thermal expansion). For example, β-Cu with a monoclinic crystal structure exhibits large negative thermal expansion over a wide temperature range. 1.8 Zn 0.2 V2O7 is known (see Patent Document 1). These negative thermal expansion materials are effective, for example, in suppressing the thermal expansion of resin materials. [Prior art documents] [Patent Documents]

[0005] [Patent Document 1] Japanese Patent Publication No. 2019-210198 [Overview of the Initiative] [Problems that the invention aims to solve]

[0006] A promising method for obtaining low-expansion materials useful in fields such as electronic devices and optical instruments is to compound a resin with a negatively thermally expanding powder filler. The inventors recognized that this requires not only small particle sizes for the powder filler, but also rounded particle shapes, i.e., high sphericity, and thus conceived the technology disclosed herein.

[0007] This disclosure is made in view of these circumstances, and one of its objectives is to provide a powder of a negative thermal expansion material having excellent properties. [Means for solving the problem]

[0008] To solve the above problems, a powder according to one embodiment of the present disclosure contains a negative thermal expansion material and has a sphericity of 0.2 or higher.

[0009] Another aspect of the present disclosure is a method for producing powder. This method comprises the steps of spray-drying a solution containing raw materials for a negative thermal expansion material to produce powder, and secondary calcining the produced powder, wherein the temperature of the secondary calcination is 1000°C or lower.

[0010] A further aspect of this disclosure is a method for producing a powder. This method comprises the steps of spray-drying a solution containing raw materials for a negative thermal expansion material to produce a powder, and secondary calcining the produced powder, wherein the secondary calcination time is 10 minutes or more.

[0011] A further aspect of this disclosure is a method for producing a powder. This method comprises the steps of introducing a powder of a negative thermal expansion material into a flow channel and heating the powder while dispersing it inside the flow channel, wherein the powder remains in the flow channel for 1 second or more. [Effects of the Invention]

[0012] According to this disclosure, it is possible to provide a powder material of negative thermal expansion having excellent properties. [Brief explanation of the drawing]

[0013] [Figure 1] This figure schematically shows the configuration of a powder manufacturing apparatus according to an embodiment of the present disclosure. [Figure 2A] This figure schematically shows the definitions of the major axis DL and minor axis DS used in calculating sphericity according to the embodiments of this disclosure. [Figure 2B] This is another diagram schematically showing the definitions of the major axis DL and minor axis DS used in calculating sphericity according to the embodiment of this disclosure. [Figure 2C] This is yet another figure schematically illustrating the definitions of the major axis DL and minor axis DS used in calculating sphericity according to the embodiments of this disclosure. [Figure 3] This figure shows the chemical composition, final firing temperature, volume frequency central particle size, volume frequency 90% diameter, sphericity, and linear expansion coefficient of the powder calculated based on the composite rule for Examples 1 to 10. [Figure 4A] This is an electron microscope image of the negative thermal expansion material of Example 1, taken at 5000x magnification. [Figure 4B] Figure 4A is a magnified view of a portion of the electron microscope image of the negative thermal expansion material of Example 1. [Figure 5A] This figure shows the volume frequency particle size distribution of the negative thermal expansion material in Example 1. [Figure 5B] This figure shows the linear thermal expansion of the composite material of the negative thermal expansion material and epoxy resin of Example 1, along with the linear thermal expansion of the epoxy resin alone. [Figure 6A] This is an electron microscope image of the negative thermal expansion material of Example 2, taken at 5000x magnification. [Figure 6B] This is an electron microscope image of the negative thermal expansion material of Example 2, taken at 10,000x magnification. [Figure 7A] This figure shows the volume frequency particle size distribution of the negative thermal expansion material in Example 2. [Figure 7B]This figure shows the linear thermal expansion of the composite material of the negative thermal expansion material and epoxy resin in Example 2, along with the linear thermal expansion of the epoxy resin alone. [Figure 8A] This is an electron microscope image of the negative thermal expansion material of Example 3, taken at 5000x magnification. [Figure 8B] This figure shows the linear thermal expansion of the composite material of the negative thermal expansion material and epoxy resin in Example 3, along with the linear thermal expansion of the epoxy resin alone. [Figure 9A] This is an electron microscope image of the powder from Example 4, taken at 20,000x magnification. [Figure 9B] Figure 9A is a partially enlarged view of an electron microscope image of the powder from Example 4 shown in Figure 9A. [Figure 10A] This is an electron microscope image of the negative thermal expansion material of Example 5, taken at 10,000x magnification. [Figure 10B] Figure 10A is a magnified view of a portion of the electron microscope image of the negative thermal expansion material of Example 5. [Figure 11A] This figure shows the volume frequency particle size distribution of the negative thermal expansion material in Example 5. [Figure 11B] This figure shows the linear thermal expansion of the composite material of the negative thermal expansion material and epoxy resin in Example 5, along with the linear thermal expansion of the epoxy resin alone. [Figure 12A] This is an electron microscope image of the negative thermal expansion material of Example 6, taken at 10,000x magnification. [Figure 12B] Figure 12A is a magnified view of a portion of the electron microscope image of the negative thermal expansion material of Example 6. [Figure 13A] This figure shows the volume frequency particle size distribution of the negative thermal expansion material in Example 6. [Figure 13B] This figure shows the linear thermal expansion of the composite material of the negative thermal expansion material and epoxy resin in Example 6, along with the linear thermal expansion of the epoxy resin alone. [Figure 14A] This is an electron microscope image taken at 10,000x magnification of the negative thermal expansion material shown as Example 7. [Figure 14B] This figure shows the volume frequency particle size distribution of the negative thermal expansion material in Example 7. [Figure 15A]This is an electron microscope image taken at 10,000x magnification of the negative thermal expansion material shown as Example 8. [Figure 15B] This figure shows the volume frequency particle size distribution of the negative thermal expansion material in Example 8. [Figure 16] This is an electron microscope image taken at 2000x magnification of the negative thermal expansion material shown as Example 9. [Figure 17A] This figure shows the volume frequency particle size distribution of the negative thermal expansion material in Example 9. [Figure 17B] This figure shows the linear thermal expansion of the composite material of the negative thermal expansion material and epoxy resin in Example 9, along with the linear thermal expansion of the epoxy resin alone. [Figure 18A] This is an electron microscope image taken at 2000x magnification of the negative thermal expansion material shown as Example 10. [Figure 18B] This figure shows the volume frequency particle size distribution of the negative thermal expansion material in Example 10. [Figure 19A] This is an electron microscope image of the negative thermal expansion material of Example 11, taken at 10,000x magnification. [Figure 19B] This figure shows the volume frequency particle size distribution of the negative thermal expansion material in Example 11. [Figure 20A] This is an electron microscope image of the negative thermal expansion material of Example 12, taken at 10,000x magnification. [Figure 20B] This figure shows the linear thermal expansion of the composite material of the negative thermal expansion material and epoxy resin in Example 12, along with the linear thermal expansion of the epoxy resin alone. [Modes for carrying out the invention]

[0014] (First Embodiment) As a first embodiment of this disclosure, a technology for manufacturing powders will be described. As a second embodiment of this disclosure, the sphericity of powders will be described. As a third embodiment of this disclosure, a composite material containing an inorganic powder filler will be described.

[0015] In the powder manufacturing method of this disclosure, by spray drying and thermal decomposition of the raw material solution, a powder with small particle size, a narrow particle size distribution, and high sphericity can be obtained.

[0016] The powder manufacturing apparatus 1 shown in Figure 1 includes a mist generator (not shown) that generates mist 10 (aerosol) from a raw material solution, a flow passage 2 through which a carrier gas CG containing the mist 10 flows, a drying furnace 3 that heats and dries the mist 10, a pyrolysis furnace 4 that heats and thermally decomposes the dried mist 13, and a recovery unit (not shown) that recovers the fine particles 16 produced as a result of the thermal decomposition.

[0017] Next, the raw material compounds can be oxides such as copper oxide, zinc oxide, vanadium pentoxide, and magnesium oxide, or salts such as ammonium dihydrogen phosphate. The salts may be salts of organic acids and alkalis, or salts of inorganic acids and alkalis. Examples of salts that can be used include metal nitrates, metal acetates, metal sulfates, metal chlorides, and metal fatty acids. Examples of organometallic compounds that can be used include metal alkoxides and metal acetylacetonates.

[0018] The solution may be an aqueous solution containing an acid. The acid may be an organic acid or an inorganic acid. Examples of organic acids include citric acid and acetic acid. In addition, examples of inorganic salt aqueous solutions and organometallic compound aqueous solutions include metal nitrates, metal acetates, metal sulfates, metal chlorides, metal fatty acids, metal alkoxides, and metal acetylacetonates. Alternatively, aqueous solutions in which metals are dissolved in nitric acid, hydrochloric acid, sulfuric acid, etc., may also be used. Alternatively, colloidal solutions or sol solutions containing silica SiO2, zirconia ZrO2, yttria-stabilized zirconia (YSZ), etc., or inorganic salt aqueous solutions may be used. Commercially available colloidal solutions and sol solutions can also be used.

[0019] When preparing the raw material solution, the target compound itself may be dissolved, or the raw material of the target compound may be dissolved. The raw material aqueous solution containing at least one of the target compound and its raw material, along with at least one of an acid, salt, and organometallic compound, can also be spray-dried or thermally decomposed.

[0020] The solution obtained in the preparation step is atomized into mist 10 using a mist generator such as an ultrasonic transducer or a two-fluid nozzle (misting step). The diameter of the droplets that make up mist 10 is adjusted by changing the mist generation method, etc.

[0021] The mist 10 generated in the atomization process is heated in a temperature range of 150°C to 400°C while flowing through the heating space in the flow passage 2 corresponding to the drying oven 3 using a carrier gas CG (drying process). As the mist 10 flowing through the heating space of the drying oven 3 is heated in a temperature range of 150°C to 400°C, it is gradually dried into mist 11, mist 12, and mist 13. Air is used as the carrier gas CG through which mist 10 to 13 flows. Instead of air, a gas mixture of oxygen and nitrogen in any ratio may be used. Other than these, inert gases such as nitrogen gas and argon gas, or reducing gases such as hydrogen gas can also be used.

[0022] Next, the heating space corresponding to the pyrolysis furnace 4 within the flow passage 2 is heated in a temperature range of 600°C to 1200°C while carrier gas CG is flowed through it (heating process). The dried product 14 flowing through the heating space of the pyrolysis furnace 4 is further heated in a temperature range of 600°C to 1200°C, undergoing pyrolysis and solid-phase reaction, and most of the particles 15 undergoing pyrolysis become fine particles 16 after pyrolysis.

[0023] Next, the product obtained in the heating step is subjected to further heat treatment (calcination) at a temperature range of, for example, 500°C to 1200°C (secondary calcination step). The secondary calcination step is carried out in a predetermined atmosphere using an electric furnace or the like. This decomposes the dried product 14 that has not yet undergone thermal decomposition and the particles 15 that are undergoing thermal decomposition, i.e., the organic acid salt particles, into fine particles 16, which are then recovered as a group of fine particles.

[0024] Furthermore, a secondary calcination process is not always necessary. For example, by securing a larger heating space corresponding to the pyrolysis furnace 4 in the heating process and adjusting the flow rate of the carrier gas CG, it is possible to obtain the same fine particles 16 as when a secondary calcination process is performed, without going through a secondary calcination process. In this case, since it becomes a single process, manufacturing costs can be reduced compared to when a secondary calcination process is performed separately from the heating process.

[0025] Furthermore, by adjusting the temperature during spray pyrolysis, the flow rate of the carrier gas CG, the residence time in the mist furnace, the concentration of the raw material solution, etc., fine particles 16 with a desired composition, microstructure, internal structure, and particle size can be obtained.

[0026] The drying oven 3 may heat the mist 10 to a temperature of preferably 100°C to 600°C, more preferably 200°C to 500°C. The heating temperature of the mist 10 may be 100°C or higher, 120°C or higher, 150°C or higher, 200°C or higher, 300°C or higher, 400°C or higher, 500°C or higher, 600°C or higher, or 700°C or higher. The heating temperature of the mist 10 may be 1000°C or lower, 900°C or lower, 800°C or lower, 700°C or lower, 600°C or lower, 500°C or lower, 400°C or lower, or 300°C or lower.

[0027] The pyrolysis furnace 4 may heat the mist 13, which has been dried to preferably 500°C to 1200°C, more preferably 600°C to 110°C. The heating temperature of the dried mist 13 may be 150°C or higher, 600°C or higher, 700°C or higher, 800°C or higher, or 900°C or higher. The heating temperature of the dried mist 13 may be 1300°C or lower, 1200°C or lower, 1100°C or lower, 1000°C or lower, 900°C or lower, or 800°C or lower.

[0028] The spray drying method yields particles with smaller particle sizes, a narrower particle size distribution, and an isotropic shape compared to conventional solid-phase reaction methods. This allows for powder pulverization with significantly less mechanical load compared to pulverizing large crystals obtained with conventional solid-phase reaction methods, resulting in a group of fine particles that maintain negative thermal expansion properties. Further adjustments to particle size and particle size distribution can be made by incorporating classification processes such as sieving or jet milling.

[0029] The drying furnace 3 and the pyrolysis furnace 4 can be integrated, allowing drying and pyrolysis to be performed in a single furnace. In this case, the temperature of the drying furnace and the temperature of the pyrolysis furnace can be considered to be the same. Alternatively, drying and pyrolysis can be performed within a single furnace with a temperature gradient. In this case, the lower temperature side can be considered to correspond to the drying furnace temperature, and the higher temperature side to the pyrolysis furnace temperature.

[0030] In Figure 1, the powder manufacturing apparatus 1 is depicted with the flow passage 2 installed horizontally, but the orientation of the flow passage can be changed as appropriate. For example, the flow passage 2 can be installed vertically with the drying oven 3 at the bottom, and the mist 10 can be introduced from below. In this case, an upward airflow is generated because the drying oven 3 and the pyrolysis oven 4 heat the mist, which allows for smooth movement of the dried mist 11, 12, 13, the drying result 14, the particles undergoing pyrolysis 15, and the generated fine particles 16.

[0031] The powder produced by the powder manufacturing equipment has a volume frequency and central particle size (median diameter) D, determined by the laser diffraction / scattering particle size distribution evaluation method. 50 This may be an aggregate of fine particles having a diameter of 30 nm or more and less than 10 μm. Here, "fine particles" includes aggregates of even smaller single crystal grains. In the following, "volume frequency median particle size (median diameter) obtained by laser diffraction / scattering particle size distribution evaluation method" may simply be referred to as "particle size". The particle size of the powder can be changed as appropriate by changing the manufacturing conditions. For example, the volume frequency median particle size D of the powder 50may be 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, 5 μm or less, 4 μm or less, 3 μm or less, 2 μm or less, 1.3 μm or less, 1.2 μm or less, 1.1 μm or less, 1 μm or less, 0.9 μm or less, 0.8 μm or less, 0.7 μm or less, 0.6 μm or less, 0.5 μm or less, 0.4 μm or less, 0.3 μm or less, 0.2 μm or less, or 0.1 μm or less. In addition, the 90% volume frequency diameter D90 of the powder may be 20 μm or less, 18 μm or less, 16 μm or less, 14 μm or less, 12 μm or less, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, 5 μm or less, 4 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, 0.9 μm or less, or 0.8 μm or less. As the laser diffraction / scattering particle size distribution evaluation apparatus, for example, LA-950V2 manufactured by Horiba, Ltd. can be used. In addition, particle size information can also be obtained from scanning electron micrographs, and by comparing with the numerical values obtained by the laser diffraction / scattering particle size distribution evaluation method, the particle size can be examined from multiple perspectives.

[0032] The powder may include a low thermal expansion material or a negative thermal expansion material. Alternatively, it may function as a thermal expansion inhibitor.

[0033] The negative thermal expansion material of the present disclosure is represented by the general formula (1) Cu x1 T x2 V y1 A y2 O z(T comprises at least one element selected from Li, Na, K, Mg, Ca, Sr, Ba, Al, Si, Ti, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ta, W, and Bi; A comprises at least one element selected from Li, Mg, Ca, Al, Si, P, Ti, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ta, W, and Bi; and 0≦x2<2, 0≦y2≦2, 1.7≦x1+x2≦2.3, 1.7≦y1+y2≦2.3, and 6≦z≦8 are satisfied.) The composition may comprise a compound represented by It is more preferable that T comprises at least two of the elements mentioned above. The negative thermal expansion material of the present disclosure may comprise two or more compounds represented by general formula (1). That is, the material may comprise two or more compounds that differ in at least one of T, x1, x2, A, y1, and y2 in general formula (1).

[0034] x in general formula (1) may satisfy 0<x2≦2, 0≦x2<2, or 0<x2<2. x2 may be 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, 1 or more, 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, or 1.6 or more. x2 may be 1.9 or less, 1.8 or less, 1.7 or less, 1.6 or less, 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, 1.1 or less, 1 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, or 0.1 or less.

[0035] y2 in general formula (1) may be 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, 1 or more, 1.1 or more, 1.2 or more, 1.3 or more, 1.4 or more, 1.5 or more, or 1.6 or more. y2 may be 1.9 or less, 1.8 or less, 1.7 or less, 1.6 or less, 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, 1.1 or less, 1 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, or 0.1 or less.

[0036] In general formula (1), z may be 6.5 or greater, 6.8 or greater, or 6.9 or greater. z may also be 7.5 or less, 7.2 or less, or 7.1 or less. Even if there are generally possible compositional fluctuations, z=7 is also acceptable.

[0037] The negative thermal expansion material disclosed herein is Zn (2) x1 T x2 P y1 A y2 O z The compound may also include the following: (T contains at least one element selected from Li, Mg, Al, Si, Ca, Sr, Ba, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ce, Ta, W, Bi, B, Na, K, F, Cl, Br, I, Hf, Y, Yb, S, Mo, Te, Pb, Cd, Te, Nd, Sm, Eu, Tb, Dy, Ho, and A contains at least one element selected from Li, Ca, Sr, Ba, Al, Si, V, Ge, Sn, La, Ce, Y, Pr, Nd, Sm, and satisfies 0≦x²<2, 0≦y²≦2, 1.7≦x¹+x²≦2.3, 1.7≦y¹+y²≦2.3, and 6≦z≦8.) It is even more preferable that T contains at least two of the elements mentioned above. The negative thermal expansion material of this disclosure may contain two or more compounds represented by general formula (2). That is, it may contain two or more compounds in which at least one of T, x1, x2, A, y1, and y2 of general formula (2) is different.

[0038] x2 in the general formula (2) may satisfy 0<x2≦1.6. More preferably, x2 is 0.05 to 1.6. x2 may be 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, or 1 or more. x2 may be 1.6 or less, 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, 1.1 or less, 1 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, or 0.1 or less.

[0039] y2 in the general formula (2) may satisfy 0≦y2≦1.8. More preferably, y2 is 0≦y2≦1.6, and still more preferably, y2 is 0 to 1.2. y2 may be 0.1 or more, 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, 0.8 or more, 0.9 or more, or 1 or more. y2 may be 1.8 or less, 1.7 or less, 1.6 or less, 1.5 or less, 1.4 or less, 1.3 or less, 1.2 or less, 1.1 or less, 1 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, 0.3 or less, 0.2 or less, or 0.1 or less.

[0040] z in the general formula (2) may be 6.5 or more, 6.8 or more, or 6.9 or more. z may be 7.5 or less, 7.2 or less, or 7.1 or less. In general, z may be 7, including possible fluctuations in the composition that are commonly acceptable.

[0041] Pyrophosphates are known to have many stoichiometric compositions, such as Mg2P2O7, Ca2P2O7, Mn2P2O7, Fe2P2O7, Co2P2O7, Ni2P2O7, Cu2P2O7, and Zn2P2O7, and have a flexible crystal structure. For this reason, many elements close to Zn on the periodic table are preferable as T in the general formula (2). For example, Mg, Al, Ti, Mn, Fe, Cu, Zr, and Ba are preferable as T.

[0042] A negative thermal expansion material represented by general formula (2) exhibits a structural phase transition in the negative thermal expansion temperature range, resulting in negative thermal expansion because the volume of the lower temperature phase is larger than that of the higher temperature phase. In the temperature range exhibiting negative thermal expansion, the high-temperature and low-temperature phases coexist, and their ratio is thought to change with temperature. The space group of the low-temperature phase structure (called the α phase) is I2 / c, and the space group of the high-temperature phase structure (called the β phase) is C2 / m. Therefore, materials with a high ratio of the α phase at temperatures below the negative thermal expansion temperature range and a high ratio of the β phase at higher temperatures exhibit good, large negative thermal expansion. In particular, a high ratio of I2 / c in the low-temperature phase and a high ratio of C2 / m in the high-temperature phase are preferable, but the material is not limited to this.

[0043] Previously known literature has reported that, for example, Zn2P2O7 has a space group Ic in its low-temperature phase, so the negative thermal expansion material of this disclosure may include a compound of general formula (2) having a space group Ic. Also, for example, Mg2P2O7 has been reported to have a space group B21 / c or P21 / c in its low-temperature phase, so the negative thermal expansion material of this disclosure may include a compound of general formula (2) having a space group B21 / c or P21 / c. Furthermore, for example, Cu2P2O7 has been reported to have a space group C2 / c in its low-temperature phase, so the negative thermal expansion material of this disclosure may include a compound of general formula (2) having a space group C2 / c.

[0044] Furthermore, the negative thermal expansion material contained in the powder of this disclosure may include impurities that are mixed in when using general raw materials and synthesis methods. Since the effect of negative thermal expansion is proportional to the volume, if the negative thermal expansion material of this disclosure is included, it will exhibit negative thermal expansion in proportion to its content, and can therefore be used as a thermal expansion inhibitor or a negative thermal expansion material. Accordingly, even if a mixture contains impurities, if it contains the negative thermal expansion material of this disclosure, it is within the scope of this disclosure.

[0045] The negative thermal expansion material of this disclosure may include a compound represented by general formula (1) and a compound represented by general formula (2).

[0046] The negative thermal expansion material of this disclosure has a negative linear expansion coefficient at the above particle size in at least a portion of the temperature range from 200K to 400K, preferably having a linear expansion coefficient of α = -3.5 ppm / K or less, more preferably α = -6 ppm / K or less, even more preferably α = -10 ppm / K or less, and even more preferably -20 ppm / K or less. The linear expansion coefficient of the powder may be -1 ppm / K or less, -2 ppm / K or less, -3 ppm / K or less, -4 ppm / K or less, -5 ppm / K or less, -7 ppm / K or less, -8 ppm / K or less, -9 ppm / K or less, -12 ppm / K or less, -15 ppm / K or less, -30 ppm / K or less, or -40 ppm / K or less. It is sufficient that the negative coefficient of linear expansion is present in at least a portion of the temperature range between 200K and 400K, but it is not necessary that it be present in at least a portion of the temperature range between 200K and 400K. "At least a portion of the temperature range" can be any temperature range, for example, 1K, or 10K, 20K, 30K, 40K, 50K, 70K, 100K, or 120K.

[0047] In this disclosure, the linear expansion coefficient of the powder is evaluated as follows. Measuring the thermal expansion characteristics of a single fine particle is technically difficult, and attempting to measure the thermal expansion characteristics of sintered fine particles may result in alteration of the negative thermal expansion material during the sintering process. Considering that negative thermal expansion materials are primarily used to suppress thermal expansion by compounding them with materials such as resins, it is reasonable to evaluate the linear expansion coefficient of the powder by measuring the extent to which thermal expansion is suppressed in a composite material in which the powder is compounded with a general resin such as epoxy resin. Therefore, in this disclosure, the linear expansion coefficient of the powder is evaluated according to a composite rule that predicts the linear expansion coefficient of the composite material by apportioning the thermal expansion coefficients of the respective components based on the volume ratio of the base material and the powder dispersed in the base material.

[0048] The combined rule is that the volume ratio of the base and the coefficient of linear expansion are given by ν. m , α m The volume ratio and linear expansion coefficient of the fine particles are respectively ν f , α fThe coefficient of linear thermal expansion of the composite material is α c as, α c =ν m α m +ν f α f The linear thermal expansion of composite materials is predicted from the following relationship: Here, ν m +ν f = 1. Based on this equation, α f =( α c -ν m α m ) / ν f The coefficient of linear expansion of the powder is evaluated. α f All other parameters can be easily measured. According to this method, the linear expansion coefficient α of the powder can be determined regardless of the type of base material. f Since the same value can be obtained as the coefficient of linear expansion α m Any material can be used as a base material as long as its properties are known or measurable. However, when using metals or ceramics as a base material, the heat treatment temperature for composite formation is higher than that of resins, so the negative thermal expansion material may be altered during the composite formation process, resulting in a lower value than the negative thermal expansion value that would normally be shown. This has been reported in past literature (e.g., "Matrix-filler interfaces and physical properties of metal matrix composites with negative thermal expansion manganese nitride," K. Takenaka, K. Kuzuoka, and N. Sugimoto, J. Appl. Phys. 118, 084902 (2015)), and is therefore undesirable for the purpose of evaluating the linear thermal expansion coefficient of powders. For this reason, it is preferable to use epoxy resin as a base material. In the examples described below, the linear thermal expansion coefficient of powders was evaluated using composite materials formed by compounding powders with epoxy resin as a base material. α at 250K~350K fThe average value of α is taken as the linear thermal expansion coefficient of the powder in the range of 250K to 350K. Since the temperature range in which the powder exhibits large negative thermal expansion can vary depending on the chemical composition, the temperature range for evaluating thermal expansion may be appropriately changed in order to properly evaluate the powder's ability to suppress thermal expansion. For example, ranges such as 200K to 350K, 250K to 380K, and 300K to 400K may be preferred. α at both ends of the temperature range f The average value may be used as the coefficient of linear expansion of the powder within that temperature range.

[0049] In the powder manufacturing method of this disclosure, the fluid may be a gas or a liquid. The fluid may not react with the substances contained in the powder, or have low reactivity, in the temperature range from room temperature to the temperature inside the pyrolysis furnace 4. The gas may be air or oxygen, or an inert gas such as nitrogen or a noble gas. The noble gas may be helium, neon, argon, xenon, etc. The liquid may not dissolve the substances contained in the powder, or have low solubility, in the temperature range from room temperature to the temperature inside the pyrolysis furnace 4. The liquid may be an inorganic solvent or an organic solvent. The liquid may be a polar solvent such as water, methanol, ethanol, propanol, formic acid, acetic acid, tetrahydrofuran, acetone, acetonitrile, or dimethyl sulfoxide, or a nonpolar solvent such as hexane, diethyl ether, benzene, or ethyl acetate.

[0050] The powders of this disclosure may be produced by a method of recrystallizing powders obtained by micronizing bulk material or coarse powder. In this case, the powder is heated while being dispersed by flowing a fluid containing the powder obtained by micronizing bulk material or coarse powder into a flow passage 2 heated in a drying oven 3 and a pyrolysis oven 4. This improves the deterioration of properties caused by crystal strain and defects introduced during micronization. Furthermore, it is possible to promote the recrystallization of the powder while suppressing the bonding of the fine particles together. As a result, it is possible to produce fine particle powders that have the excellent properties of the bulk material or coarse powder while suppressing effects such as increased particle size and non-uniformity.

[0051] To promote the recrystallization of powders, heating the powder is advantageous. Traditionally, powders were heated in containers such as crucibles. However, heating powders can cause problems such as the bonding of fine particles, leading to increased particle size and unevenness. Such increases in particle size and unevenness can contribute to a decrease in the powder's properties.

[0052] Here, "fluid" refers to a continuous body that has fluidity, such as a gas or liquid, and does not generate shear stress in a static state, regardless of whether it is in a flowing state or not. Therefore, the powder manufacturing method of this disclosure includes both cases in which a non-flowing fluid is made to flow and cases in which a flowing fluid is kept flowing.

[0053] The powder manufacturing apparatus of this disclosure may, if necessary, include an inlet flow rate adjustment mechanism, a powder introduction section, and a powder delivery section upstream of the drying furnace 3. Furthermore, an outlet flow rate adjustment section and a cooling mechanism may be placed downstream of the pyrolysis furnace 4. A control unit for controlling these components may also be included.

[0054] The inlet-side flow rate adjustment unit adjusts the flow rate of the fluid flowing into the flow passage 2. The outlet-side flow rate adjustment unit adjusts the flow rate of the fluid discharged from the flow passage 2. The inlet-side and outlet-side flow rate adjustment units may be composed of valves with adjustable opening degrees or orifices with adjustable inner diameters. The inlet-side and outlet-side flow rate adjustment units may be controlled by a control unit to adjust the fluid velocity and fluidity inside the flow passage 2, or to adjust the time (heating time) that the powder remains inside the drying oven 3 and the pyrolysis oven 4.

[0055] The drying furnace 3 and the pyrolysis furnace 4 have a space capable of containing powder and heat the powder present in the space. The drying furnace 3 and the pyrolysis furnace 4 may be composed of any type of electric furnace, flame furnace, etc. The drying furnace 3 and the pyrolysis furnace 4 may also be composed of a container and electric heating wires or gas burners provided on the inner wall or inside of the container.

[0056] The powder introduced into the flow passage 2 is heated and recrystallized in the drying oven 3 and the pyrolysis oven 4. This makes it possible to produce powder with a higher degree of crystallinity than the powder before heating. The powder introduced into the flow passage 2 is dispersed by the flow of the fluid inserted into the flow passage 2, so the bonding of fine particles is suppressed. This makes it possible to produce powder with small particle sizes and uniform particle size. The fluid delivery unit functions as a flow generating unit that causes the fluid inside the flow passage 2 to flow.

[0057] The fluid inside the flow passage 2 also flows due to convection caused by heating. Therefore, the flow passage 2 also functions as a flow generating section. If the bonding of fine particles is sufficiently suppressed by the fluid flow due to convection alone, the fluid delivery section may deliver fluid at a flow rate sufficient to introduce the powder into the flow passage 2.

[0058] An inlet for introducing powder and fluid into the flow passage 2 may be provided at the bottom of the flow passage 2, and an outlet for discharging powder and fluid from the flow passage 2 may be provided at the top of the flow passage 2. This allows the powder to be discharged from the upper outlet along with the heated and rising fluid without the need to suck fluid from outside the flow passage 2, thus simplifying the configuration of the powder manufacturing apparatus 1. A suction unit for sucking fluid from inside the flow passage 2 may also be provided. In this case, the suction unit may function as a flow generation unit.

[0059] The drying oven 3 and the pyrolysis furnace 4 may heat the powder to a temperature lower than the melting point of the substances contained in the powder. This suppresses the melting of the substances contained in the powder and the bonding of the fine particles together. The drying oven 3 and the pyrolysis furnace 4 may heat the powder to a temperature near the melting point of the substances contained in the powder. This further promotes the recrystallization of the powder, thus shortening the heating time. The drying oven 3 and the pyrolysis furnace 4 may heat the powder to a temperature slightly higher than the melting point of the substances contained in the powder. This melts the substances on the surface of the fine particles, causing them to become spherical due to surface tension, thereby improving the sphericity of the powder. Furthermore, the drying oven 3 and the pyrolysis furnace 4 may heat the powder to a temperature higher than the melting point of the substances contained in the powder. This allows the fine particles to melt into droplets and then be cooled as they are transported downstream of the flow passage 2 by the CG, thus producing spherical fine particles.

[0060] The cooling section cools the powder heated by the drying oven 3 and the pyrolysis oven 4. The cooling section may cool the powder by methods such as air cooling or water cooling. Part of the flow path from the outlet of the flow passage 2 to the powder recovery section may be open to the atmosphere. The powder recovery section recovers the powder cooled by the cooling section.

[0061] The control unit controls the flow generation unit to cause the fluid in which the powder is dispersed to flow when the powder is heated inside the flow passage 2. For example, the control unit controls the fluid delivery unit, the inlet flow rate adjustment unit, and the outlet flow rate adjustment unit to control the fluid flow rate so that the fluid flows inside the flow passage 2.

[0062] The above describes a case in which powder is continuously introduced into the flow passage 2 and powder is manufactured using a continuous operation method, but powder may also be manufactured using a batch operation method. In this case, the fluid delivery section, inlet flow rate adjustment section, and outlet flow rate adjustment section do not need to be provided. As a flow generation section that causes the fluid inside the flow passage 2 to flow, a stirring blade or fan may be provided to agitate the fluid inside the flow passage 2.

[0063] The powder manufacturing method of this disclosure may include a step of grinding the recrystallized powder as described above. The step of grinding the powder may be performed by grinding the powder using a jet mill, which finely grinds the material by causing it to collide with each other using compressed air or high-pressure gas. This makes the particle size of the powder even smaller and more uniform.

[0064] The powders of this disclosure may be produced by a solid-phase reaction method. In this case, powders of raw materials such as oxides containing the constituent elements of the compounds represented by general formulas (1) to (2) are weighed in a specified molar ratio, mixed in an agate mortar and pestle, and then calcined in an alumina crucible.

[0065] The powder manufacturing technology disclosed herein enables the production of inexpensive negative thermal expansion material powders that exhibit significant negative thermal expansion at or near room temperature. Furthermore, by using this negative thermal expansion material powder, precise control of thermal expansion in minute components and localized areas at the 1 μm level becomes possible. In addition, when the negative thermal expansion material powder is dispersed in a base material such as resin, sedimentation of the negative thermal expansion material powder can be suppressed, thereby achieving homogeneous dispersion. Moreover, since the median diameter of the negative thermal expansion material powder is equivalent to or smaller than the wavelength of visible light (300 nm to 800 nm), the transmittance of visible light can be maintained even when the negative thermal expansion material powder is blended into transparent or translucent materials such as glass or acrylic.

[0066] The powders of this disclosure include a negative thermal expansion material having a negative coefficient of linear expansion in at least a portion of the temperature range, and the volume frequency central particle size (median diameter) D as measured by a laser diffraction / scattering particle size distribution evaluation device. 50 It is 20 μm or less. D 50The particle size may be 15 μm or less, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, 5 μm or less, 4 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, 0.9 μm or less, 0.8 μm or less, 0.7 μm or less, 0.6 μm or less, 0.5 μm or less, 0.4 μm or less, 0.3 μm or less, 0.2 μm or less, 0.1 μm or less, 0.09 μm or less, 0.08 μm or less, 0.07 μm or less, 0.06 μm or less, 0.05 μm or less, 0.04 μm or less, 0.03 μm or less, 0.02 μm or less, or 0.01 μm or less. This makes it possible to provide powder with a small particle size.

[0067] Volume frequency of the powder in this disclosure, center particle size D 50 These particles may be 0.01 μm or larger, 0.05 μm or larger, 0.1 μm or larger, 0.2 μm or larger, 0.3 μm or larger, 0.4 μm or larger, 0.5 μm or larger, 0.6 μm or larger, 0.7 μm or larger, 0.8 μm or larger, 0.9 μm or larger, 1 μm or larger, 2 μm or larger, 3 μm or larger, 4 μm or larger, 5 μm or larger, 6 μm or larger, 7 μm or larger, 8 μm or larger, 9 μm or larger, or 10 μm or larger.

[0068] The powders of this disclosure include a negative thermal expansion material having a negative coefficient of linear expansion in at least a portion of the temperature range, and the volume frequency of the 90% diameter D is determined by a laser diffraction / scattering particle size distribution evaluation device. 90 It is 50 μm or less. D 90 The particle size may be 45 μm or less, 40 μm or less, 35 μm or less, 30 μm or less, 25 μm or less, 20 μm or less, 19 μm or less, 18 μm or less, 17 μm or less, 16 μm or less, 15 μm or less, 14 μm or less, 13 μm or less, 12 μm or less, 11 μm or less, 10 μm or less, 9 μm or less, 8 μm or less, 7 μm or less, 6 μm or less, 5 μm or less, 4 μm or less, 3 μm or less, 2 μm or less, 1 μm or less, 0.9 μm or less, 0.8 μm or less, 0.7 μm or less, 0.6 μm or less, 0.5 μm or less, 0.4 μm or less, 0.3 μm or less, 0.2 μm or less, or 0.1 μm or less. This makes it possible to provide a powder with a small particle size and containing almost no large particles.

[0069] The powder disclosed herein has a volume frequency of 90% and a particle size of D 90The particle size may be 0.01 μm or larger, 0.05 μm or larger, 0.1 μm or larger, 0.2 μm or larger, 0.3 μm or larger, 0.4 μm or larger, 0.5 μm or larger, 0.6 μm or larger, 0.7 μm or larger, 0.8 μm or larger, 0.9 μm or larger, 1 μm or larger, 1.5 μm or larger, 2 μm or larger, 2.5 μm or larger, 3 μm or larger, 3.5 μm or larger, 4 μm or larger, 4.5 μm or larger, 5 μm or larger, 5.5 μm or larger, 6 μm or larger, 6.5 μm or larger, 7 μm or larger, 7.5 μm or larger, 8 μm or larger, 8.5 μm or larger, 9 μm or larger, 9.5 μm or larger, or 10 μm or larger.

[0070] The above numerical ranges may be any combination as long as the lower limit of the 90% volume frequency particle size is smaller than the upper limit of the 90% volume frequency particle size, the lower limit of the central volume frequency particle size is smaller than the upper limit of the central volume frequency particle size, the upper limit of the central volume frequency particle size is smaller than the upper limit of the 90% volume frequency particle size, and the lower limit of the central volume frequency particle size is smaller than the lower limit of the 90% volume frequency particle size.

[0071] The powders of this disclosure may contain any compound. For example, the powders of this disclosure may contain negative thermal expansion materials such as compounds represented by the general formulas (1) to (2) above. The powder manufacturing technology of this disclosure is particularly suitable for manufacturing powders in which the properties of the bulk material deteriorate upon micronization.

[0072] The negative thermal expansion material of this disclosure may be manufactured by a solid-phase reaction method or a spray drying method, or by grinding a powder manufactured by a solid-phase reaction method or a spray drying method using a planetary ball mill or a jet mill.

[0073] The negative thermal expansion material of this disclosure has excellent negative thermal expansion properties even in the form of a fine powder. Therefore, it can effectively suppress the thermal expansion of components such as resin films, adhesives, interlayer fillers, and substrates that are expected to be used in the field of electronic devices at a size of several micrometers.

[0074] (Second Embodiment) The powder according to the second embodiment of this disclosure may contain at least one of the compounds represented by the above general formulas (1) and (2). Furthermore, the powder according to the second embodiment of this disclosure may also contain negative thermal expansion materials other than the compounds represented by the above general formulas (1) and (2).

[0075] To suppress thermal expansion in minute components, it is necessary not only for the particle size of the negative thermal expansion material powder to be small, but also for the particle shape to be rounded, that is, to have high sphericity. From this viewpoint, the inventors conceived that it is appropriate to define the negative thermal expansion material powder by a numerical value of sphericity.

[0076] The sphericity of the powder according to the second embodiment of this disclosure is 0.2 or higher. The sphericity may be 0.3 or higher, 0.4 or higher, 0.5 or higher, 0.6 or higher, 0.7 or higher, 0.8 or higher, or 0.9 or higher.

[0077] The sphericity of the powder according to the second embodiment of this disclosure is 1 or less. The sphericity may be less than 1, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, 0.5 or less, 0.4 or less, or 0.3 or less.

[0078] The above numerical ranges may be arbitrarily combined, as long as the lower limit of sphericity is smaller than the upper limit of sphericity.

[0079] In this disclosure, the sphericity of the powder is evaluated as follows: An electron microscope is used to take images at magnifications ranging from 1,000 to 250,000 times to obtain a photographic projection. From this photographic projection, 30 arbitrary particles are selected, and their major axis DL and minor axis DS are measured. The ratio (DS / DL) is then calculated. The average value of these ratios is defined as the sphericity. Here, DL is defined as the smallest circumscribed diameter for each selected particle, and DS is defined as the largest inscribed diameter. Figures 2A, 2B, and 2C show examples of the definitions of DL and DS.

[0080] The powders of this disclosure may contain any compound. For example, the powders of this disclosure may contain negative thermal expansion materials such as compounds represented by the above general formulas (1) to (2).

[0081] The powder of this disclosure may be manufactured by the manufacturing method described in the first embodiment. To increase the sphericity of the powder, it is preferable to lower the temperature of the secondary firing process, lengthen the duration of the secondary firing process, and lengthen the time the powder remains in the flow passage 2 during recrystallization. The temperature of the secondary firing process may be 1000°C or less, 950°C or less, 900°C or less, 850°C or less, 800°C or less, 750°C or less, 700°C or less, 650°C or less, 600°C or less, 550°C or less, 500°C or less, 450°C or less, or 400°C or less, and is preferably 650°C or less. The duration of the secondary firing process may be 10 minutes or more, 20 minutes or more, 30 minutes or more, 40 minutes or more, 50 minutes or more, 1 hour or more, 2 hours or more, 3 hours or more, 4 hours or more, or 5 hours or more, and is preferably 1 hour or more. The time the powder remains in the flow path 2 during recrystallization may be 1 second or more, 1.5 seconds or more, 2 seconds or more, 2.5 seconds or more, 3 seconds or more, 3.5 seconds or more, 4 seconds or more, 4.5 seconds or more, 5 seconds or more, or 7 seconds or more, but it is preferably 3 seconds or more.

[0082] (Third embodiment) As a third embodiment of this disclosure, a composite material obtained by mixing a powder containing the negative thermal expansion material described in the first and second embodiments with a resin will be described.

[0083] The composite material of the third embodiment of this disclosure may contain at least one of the compounds represented by the above general formulas (1) and (2). The composite material of the fourth embodiment of this disclosure may contain negative thermal expansion materials other than the compounds represented by the above general formulas (1) and (2). It may also contain powders of various materials that do not exhibit negative thermal expansion, such as alumina, zirconia, and silica.

[0084] If a composite material contains powder of a negative thermal expansion material, its thermal expansion can be controlled. Furthermore, if it contains powder of a material with high thermal conductivity, such as alumina, its thermal conductivity can be improved. Therefore, by simultaneously incorporating various materials, including the compounds represented by the general formulas (1) and (2) above, it is possible to control not only the thermal expansion of the composite material but also other properties such as thermal conductivity. Additionally, by simultaneously incorporating materials that change shape in response to the application of magnetic or electric fields, it is possible to simultaneously control thermal expansion and improve dimensional accuracy in actuator materials that change shape in response to electric or magnetic fields. The negative thermal expansion material represented by general formula (1) can also be used as an actuator material in a similar manner.

[0085] In the composite material of the third embodiment of this disclosure, a negative thermal expansion material is dispersed in the base resin. Since the resin has high resistance, a high electric field can be applied to the composite material. This improves the performance as an actuator.

[0086] In the composite material of the third embodiment of this disclosure, the resin may be any type of thermoplastic resin, thermosetting resin, etc. The resin may also include epoxy resin, phenolic resin, fluororesin, acrylic resin, acrylonitrile butadiene resin, polycarbonate, polyimide, polyamideimide, polypropylene, polyamide, polyethylene, polyethylene terephthalate, etc.

[0087] In the actuator material of the third embodiment of this disclosure, the mixture of the resin and the powder of the negative thermal expansion material contains 10% by volume or more of powder based on the total volume of the mixture. The mixture may also contain 1% by volume or more, 5% by volume or more, 10% by volume or more, 20% by volume or more, 30% by volume or more, 40% by volume or more, 50% by volume or more, 60% by volume or more, 70% by volume or more, 80% by volume or more, or 90% by volume or more of powder based on the total volume of the mixture. The mixture may also contain 99% by volume or less, 95% by volume or less, 90% by volume or less, 80% by volume or less, 70% by volume or less, 60% by volume or less, 50% by volume or less, 40% by volume or less, 30% by volume or less, 20% by volume or less, or 10% by volume or less of powder based on the total volume of the mixture.

[0088] The electrical resistivity of the composite material in the third embodiment of this disclosure may be 107 Ωcm or more. Depending on the mixing ratio and the types of materials included, this value may be 105 Ωcm or more, 1010 Ωcm or more, or 1012 Ωcm or more.

[0089] The properties of the composite material in the third embodiment of this disclosure, such as the coefficient of thermal expansion, electrical resistivity, electrostriction constant, and whether or not it is flexible, may be adjusted according to the specifications.

[0090] A method for producing a composite material according to a third embodiment of the present disclosure includes the step of molding a mixture of a powder containing a negative thermal expansion material and a resin.

[0091] The method for molding the mixture may be any method for molding resin. For example, the mixture containing resin and a negative thermal expansion material may be molded using an extruder or injection molder, or it may be molded using a 3D printer.

[0092] (Examples) Based on the method for producing negative thermal expansion materials described in the above embodiments, powders containing negative thermal expansion materials represented by general formulas (1) and (2) were prepared. Figure 3 shows the chemical composition, final calcination temperature, volume frequency central particle size, volume frequency 90% diameter, sphericity, and linear expansion coefficient of the powders calculated based on the composite rule for Examples 1 to 10.

[0093] (Examples 1 and 2) Based on the method for manufacturing a negative thermal expansion material described in the above embodiment, Cu 1.8 Zn 0.2 A group of V2O7 microparticles was prepared. Figures 4A to 7B show the measurements for Examples 1 and 2.

[0094] The raw material reagents (powder) of CuO, ZnO, and V2O5, weighed in stoichiometric ratios, were mixed in a mortar and calcined in air at 670°C for 10 hours. The resulting powder was ground in a mortar and dissolved in pure water with anhydrous citric acid. At this time, 3 g of anhydrous citric acid and 100 mL of pure water were added for every 1 g of sample powder, and the mixture was stirred using a magnetic stirrer until the sample powder was dissolved. Note that V2O3 may be used instead of V2O5. The resulting aqueous solution was atomized and heated under the conditions of a drying oven temperature of 400°C, a pyrolysis oven temperature of 600°C, a carrier gas flow rate of CG of 3.8 L / min, and a residence time in the mist oven of 7 sec to produce particles of the negative thermal expansion material. Next, the obtained particles were subjected to secondary calcination at 580°C for 4 hours or at 670°C for 10 minutes to obtain the negative thermal expansion material fine particles of Example 1 and Example 2, respectively.

[0095] Figure 4A is an electron microscope image of the powder of Example 1 taken at 5000x magnification, and Figure 4B is a magnified view of a portion of the electron microscope image of the negative thermal expansion material of Example 1 shown in Figure 4A. The sphericity of the powder of Example 1 was 0.85. Figure 6A is an electron microscope image of the powder of Example 2 taken at 5000x magnification, and Figure 6B is an electron microscope image of the powder of Example 2 taken at 10000x magnification. The sphericity of the powder of Example 2 was 0.77. The sphericity was estimated from the analysis of electron microscope images, as explained in the second embodiment. From these results, it can be seen that lowering the temperature and increasing the time of secondary firing leads to an improvement in sphericity.

[0096] Figure 5A shows the particle size distribution of the powder in Example 1. Volume frequency central particle size D of the powder in Example 1 50 It is 3.59 μm, and the volume frequency is 90% diameter D 90The size was 5.93 μm. Figure 7A shows the particle size distribution of the powder in Example 2. Volume frequency central particle size D of the powder in Example 2 50 It is 2.27 μm, and the volume frequency is 90% diameter D 90 The length was 4.47 μm. Figure 5B shows the linear thermal expansion of the powder of Example 1. Figure 7B shows the linear thermal expansion of the powder of Example 2. In both figures, the solid circles represent the linear thermal expansion of a composite material in which the powder of the example was blended with epoxy resin (Adeka® EP-4100E / EH-105L) at a volume ratio of 30%, and the solid lines represent the linear thermal expansion of the epoxy resin alone. The thermal expansion of solid materials is evaluated by the linear thermal expansion ΔL / L. The linear thermal expansion ΔL / L on the vertical axis of Figures 5B and 7B is the change in length relative to the length L at 100K. The change in length was measured using a laser thermal expansion meter (LIX-2: manufactured by ULVAC, Inc.). The slope of the linear thermal expansion, i.e., the temperature derivative, is the coefficient of linear expansion. In the case of isotropic materials that do not depend on direction, the linear thermal expansion essentially represents the volume thermal expansion, and the relationship ΔV / V = 3ΔL / L holds (V is volume). The linear expansion coefficient α of the powder in Example 1 f The coefficient of linear expansion α of the powder in Example 2 is -30.0 ppm / K. f The coefficient of thermal expansion is -37.9 ppm / K. The coefficient of thermal expansion was estimated by assuming a composite law based on the linear thermal expansion measurement results of the epoxy resin containing the powder, as described in the first embodiment.

[0097] (Example 3) Based on the method for manufacturing a negative thermal expansion material described in the above embodiment, Cu 1.8 Zn 0.2 V 1.5 P 0.5 A group of O7 microparticles was prepared. Figures 8A and 8B show the measurements taken for Example 3.

[0098] The raw material reagents (powder) of CuO, ZnO, V2O5, and NH4H2PO4, weighed in stoichiometric ratios, were mixed in a mortar and calcined in air at 670°C for 10 hours. The resulting powder was ground in a mortar and dissolved in pure water with anhydrous citric acid. At this time, 3 g of anhydrous citric acid and 100 mL of pure water were added for every 1 g of sample powder, and the mixture was stirred using a magnetic stirrer until the sample powder was dissolved. The resulting aqueous solution was atomized and heated under the conditions of a drying oven temperature of 400°C, a pyrolysis oven temperature of 600°C, a carrier gas flow rate of CG of 3.8 L / min, and a residence time in the mist oven of 7 sec to produce particles of negative thermal expansion material. Next, the obtained particles were subjected to secondary calcination at 670°C for 10 minutes to obtain a group of negative thermal expansion material fine particles.

[0099] Figure 8A is an electron microscope image of the powder of Example 3 taken at 5000x magnification, and the sphericity of the powder of Example 3 was 0.75. The sphericity was estimated from the analysis of the electron microscope image, as described in the second embodiment. Figure 8B shows the linear thermal expansion of the powder of Example 3. The solid circles show the linear thermal expansion of a composite material in which the powder of Example 3 was blended with epoxy resin (Adeka® EP-4100E / EH-105L) at a volume ratio of 30%, and the solid line shows the linear thermal expansion of the epoxy resin alone. The linear thermal expansion coefficient α of this powder f The coefficient of thermal expansion is -22.4 ppm / K. The coefficient of thermal expansion was estimated by assuming a composite law based on the linear thermal expansion measurement results of the epoxy resin containing the powder, as described in the first embodiment.

[0100] (Example 4) Based on the powder manufacturing method described in the above embodiment, a group of fine particles with a weight ratio of SiO2:YSZ = 85:15 was prepared. Figures 9A and 9B show the measurements for Example 4.

[0101] Based on the preparation method described in the above embodiment, the raw material solution was heated under the following conditions: spray pyrolysis temperature of 800°C, carrier gas CG flow rate of 5 L / min, residence time in the mist furnace of 8 sec, and raw material solution concentration of 0.075 M to produce inorganic fillers with an average particle size of 300 nm. Next, the obtained particles were subjected to secondary calcination at 1100°C for 2 hours.

[0102] Figure 9A is an electron microscope image of the powder of Example 4 taken at 20,000x magnification, and Figure 9B is a magnified view of a portion of the electron microscope image of the powder of Example 4 shown in Figure 9A. The sphericity of the powder of Example 4 was 0.95. The sphericity was estimated from the analysis of the electron microscope image, as described in the second embodiment.

[0103] (Examples 5 and 6) Based on the method for producing a negative thermal expansion material described in the above embodiment, Zn 1.6 Mg 0.4 A group of P2O7 fine particles was prepared. Figures 10A to 13B show the measurements taken for Examples 5 and 6.

[0104] First, as part of the preparation process, the raw material reagents (powder) of ZnO, MgO, and NH4H2PO4, weighed in stoichiometric ratios, were mixed in a mortar and calcined in an alumina crucible at 800-850°C in air for 2-6 hours. After calcination, the mixture was removed and mixed again in an agate mortar and pestle, then calcined in an alumina crucible at 850-900°C in air for 2-10 hours. The prepared powder was further ground in a planetary ball mill for approximately 10 minutes to 6 hours. This allowed the median diameter to be reduced to less than 1 μm.

[0105] The crushed raw material powder was introduced into the powder manufacturing apparatus 1 and recrystallized. For the powder of Example 5, the temperature of both the drying oven 3 and the pyrolysis oven 4 was set to 1050°C, and 93.5g of raw material powder was introduced into the flow passage 2 over 4.5 hours, resulting in the recovery of 73.5g of powder. The yield was 16.3g per hour, and the time the powder remained in the flow passage 2 was 2 seconds. For the powder of Example 6, the temperature of both the drying oven 3 and the pyrolysis oven 4 was set to 1050°C, and 46.8g of raw material powder was introduced into the flow passage 2 over 4.5 hours, resulting in the recovery of 27.8g of powder. The yield was 6.2g per hour, and the time the powder remained in the flow passage 2 was approximately 5 seconds.

[0106] The pulverized raw material powder was introduced into powder manufacturing apparatus 1 for recrystallization, and then pulverized using a jet mill pulverizer (CO-JET system α MARK III, manufactured by Seishin Corporation) to produce the powders of Examples 5 and 6. The powder was pulverized using the jet mill pulverizer with compressed air at 0.1 to 0.69 MPa.

[0107] Figure 10A is an electron microscope image of the negative thermal expansion material of Example 5 taken at 10,000x magnification, and Figure 10B is a magnified view of a portion of the electron microscope image of the negative thermal expansion material of Example 5 shown in Figure 10A. The sphericity of the powder of Example 5 was 0.59. Figure 12A is an electron microscope image of the negative thermal expansion material of Example 6 taken at 10,000x magnification, and Figure 12B is a magnified view of a portion of the electron microscope image of the negative thermal expansion material of Example 6 shown in Figure 12A. The sphericity of the powder of Example 6 was 0.65. The sphericity was estimated from the analysis of electron microscope images, as explained in the second embodiment. From these results, it can be seen that increasing the time the material remains in the flow channel 2 leads to an improvement in sphericity.

[0108] Figure 11A shows the particle size distribution of the powder in Example 5. Volume frequency central particle size D of the powder in Example 5. 50 It is 0.62 μm, and the volume frequency is 90% diameter D 90The coefficient of linear thermal expansion of the powder in Example 5 was 1.22 μm. Figure 11B shows the linear thermal expansion of the powder in Example 5. The solid circles represent the linear thermal expansion of a composite material in which the powder in Example 5 was blended with epoxy resin (Adeka® EP-4100E / EH-105L) at a volume ratio of 30%, and the solid line represents the linear thermal expansion of the epoxy resin alone. Linear thermal expansion coefficient α of the powder in Example 5 f The value is -49.0 ppm / K. Figure 13A shows the particle size distribution of the powder in Example 6. Volume frequency central particle size D of the powder in Example 6 50 It is 0.66 μm, and the volume frequency is 90% diameter D 90 The coefficient of linear thermal expansion of the powder in Example 5 was 1.20 μm. Figure 13B shows the linear thermal expansion of the powder in Example 5. The solid circles represent the linear thermal expansion of the composite material obtained by blending the powder in Example 6 with epoxy resin at a volume ratio of 30%, and the solid line represents the linear thermal expansion of the epoxy resin alone. The coefficient of linear thermal expansion of the powder in Example 6 is α. f The coefficient of thermal expansion is -58.7 ppm / K. The coefficient of thermal expansion was estimated by assuming a composite law based on the linear thermal expansion measurement results of the epoxy resin containing the powder, as described in the first embodiment.

[0109] (Examples 7-10) Negative thermal expansion powders can also be obtained by solid-phase reaction and pulverization. First, as a preparation step, raw material reagents (powder) of ZnO, MgO, and NH4H2PO4, weighed in stoichiometric ratios, were mixed in a mortar and calcined in an alumina crucible at 800-850°C in air for 2-6 hours. After calcination, the mixture was removed, mixed again in an agate mortar and pestle, and then calcined in an alumina crucible at 850-900°C in air for 2-10 hours. The prepared powder was further pulverized in a planetary ball mill for about 10 minutes to 6 hours. In Example 7, the final calcination temperature was 875°C. In Examples 8-10, in addition to ZnO, MgO, and NH4H2PO4, Al2O3 was used as a raw material, and the final calcination temperature was 875°C. Figures 14A-18B show the measurements for Examples 7-10.

[0110] Figure 14A is an electron microscope image taken at 10,000x magnification of the negative thermal expansion material shown as Example 7. The sphericity of the powder in Example 7 was 0.44. Figure 15A is an electron microscope image taken at 10,000x magnification of the negative thermal expansion material shown as Example 8. The sphericity of the powder in Example 8 was 0.34. Figure 16 is an electron microscope image taken at 2,000x magnification of the negative thermal expansion material shown as Example 9. The sphericity of the powder in Example 9 was 0.51. Figure 18A is an electron microscope image taken at 2,000x magnification of the negative thermal expansion material shown as Example 10. The sphericity of the powder in Example 10 was 0.38. The sphericity was estimated from the analysis of electron microscope images, as described in the second embodiment.

[0111] Figure 14B shows the particle size distribution of the powder in Example 7. Volume frequency central particle size D of the powder in Example 7. 50 It is 2.79 μm, and the volume frequency is 90% diameter D 90 The particle size was 5.68 μm. Figure 15B shows the particle size distribution of the powder in Example 8. Volume frequency central particle size D of the powder in Example 8 50 It is 1.42 μm, and the volume frequency is 90% diameter D 90 The size was 3.21 μm. Figure 17A shows the particle size distribution of the powder in Example 9. Volume frequency central particle size D of the powder in Example 9 50 It is 15.93 μm, and the volume frequency is 90% diameter D 90 The coefficient of linear thermal expansion of the powder of Example 9 was 29.42 μm. Figure 17B shows the linear thermal expansion of the powder of Example 9. The solid circles represent the linear thermal expansion of a composite material in which the powder of Example 9 was blended with epoxy resin (Adeka® EP-4100E / EH-105L) at a volume ratio of 30%, and the solid line represents the linear thermal expansion of the epoxy resin alone. Linear thermal expansion coefficient α of the powder of Example 9 f The value is -57.5 ppm / K. Figure 18B shows the particle size distribution of the powder in Example 10. Volume frequency central particle size D of the powder in Example 10 50 It is 14.87 μm, and the volume frequency is 90% diameter D 90 The value was 30.12 μm. The coefficient of thermal expansion was estimated by assuming a composite law based on the linear thermal expansion measurement results of the epoxy resin containing the powder, as described in the first embodiment.

[0112] (Examples 11 and 12) The raw material reagents (powder) of ZnO, MgO, and NH4H2PO4, weighed in stoichiometric ratios, were stirred with anhydrous citric acid in pure water using a magnetic stirrer until dissolved. The raw material solution prepared according to the preparation method described in the above embodiment was atomized and heated under the conditions of a drying oven temperature of 800°C, a pyrolysis oven temperature of 1100°C, a carrier gas flow rate of CG of 20 L / min, and a residence time in the mist oven of 2 sec to obtain the powder of Example 11. Next, the obtained powder was further calcined at 800°C for 20 min to obtain the powder of Example 12.

[0113] Figure 19A is an electron microscope image of the powder of Example 11 taken at 10,000x magnification. The sphericity of the powder of Example 11 was 0.95. The sphericity was estimated from the analysis of the electron microscope image, as described in the second embodiment. Figure 19B shows the particle size distribution of the powder of Example 11. Volume frequency median particle size D of the powder of Example 11 50 It is 3.74 μm, and the volume frequency is 90% diameter D 90 It was 9.03 μm.

[0114] Figure 20A is an electron microscope image of the powder of Example 12 taken at 10,000x magnification. The sphericity of the powder of Example 12 was 0.58. The sphericity was estimated from the analysis of the electron microscope image, as described in the second embodiment. Figure 20B shows the linear thermal expansion of the powder of Example 12. The solid circles represent the linear thermal expansion of a composite material in which the powder of Example 12 was blended with epoxy resin (Adeka® EP-4100E / EH-105L) at a volume ratio of 30%, and the solid line represents the linear thermal expansion of the epoxy resin alone. The linear thermal expansion coefficient α of this powder f The coefficient of thermal expansion is -89.8 ppm / K. The coefficient of thermal expansion was estimated by assuming a composite law based on the linear thermal expansion measurement results of the epoxy resin containing the powder, as described in the first embodiment.

[0115] The sphericity of the powder containing the negative thermal expansion material represented by general formula (1) may be 1 or less, less than 1, 0.95 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, or 0.5 or less. Further, the sphericity of the powder containing the negative thermal expansion material represented by general formula (1) may be 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, or 0.8 or more. The sphericity of the powder containing the negative thermal expansion material represented by general formula (2) may be 1 or less, less than 1, 0.95 or less, 0.9 or less, 0.8 or less, 0.7 or less, 0.6 or less, or 0.5 or less. Further, the sphericity of the powder containing the negative thermal expansion material represented by general formula (2) may be 0.2 or more, 0.3 or more, 0.4 or more, 0.5 or more, 0.6 or more, 0.7 or more, or 0.8 or more. The above numerical ranges may be arbitrarily combined as long as the lower limit value of the sphericity is smaller than the upper limit value of the sphericity.

[0116] Hereinafter, preferred examples of the negative thermal expansion material included in the present invention will be listed. It goes without saying that the negative thermal expansion material included in the present invention is not limited to these. Furthermore, those in which part of the oxygen atoms contained in the negative thermal expansion materials described below are deficient or contained in excess can also be cited as preferred examples. In addition, those having compositional fluctuations that may occur when using common raw materials and production methods can also be cited as preferred examples.

[0117] Cu 1.75~1.85 Zn 0.15~0.25 V 1.95~2 P 0~0.05 O7 Cu 1.75~1.85 Zn 0.15~0.25 V 1.4~1.6 P 0.4~0.6 O7 Zn 1.5~1.7 Mg 0.3~0.5 P2O7 Zn 1.6~1.8 Mg 0.2~0.3 Al 0.03~0.07 P2O7 Zn 1.7~1.8 Mg 0.15~0.25 Al 0.03~0.07 P2O7 Zn 1.8~1.86 Mg 0.09~0.13 Al 0.04~0.08 P2O7 Zn 1.72~1.78 Mg 0.17~0.23 Al 0.03~0.07 P2O7

[0118] In the foregoing, the present disclosure has been described based on the embodiments. These embodiments are illustrative, and it will be understood by those skilled in the art that various modifications can be made to combinations of the respective constituent elements and respective processing processes, and such modifications are also within the scope of the present disclosure.

[0119] In the powder production method of the present disclosure, the production conditions are optimized according to the physical and chemical properties of the substances constituting the obtained powder, such as melting point, vapor pressure, chemical reactivity, whether the substance decomposes and melts, and solubility in solvents such as water. Therefore, the method is not limited to the examples, and can be applied to the production of powders containing substances of various compositions represented by general formulas (1) and (2), which are considered to have similar physical and chemical properties. In addition, since this is a technology for producing fine particles while maintaining crystallinity and can suppress functional degradation, it can also be applied to other negative thermal expansion materials such as zirconium phosphate sulfate-based materials and bismuth-nickel oxide-based materials.

[0120] In the foregoing, the present disclosure has been described based on the embodiments. These embodiments are illustrative, and it will be understood by those skilled in the art that various modifications can be made to combinations of the respective constituent elements and respective processing processes, and such modifications are also within the scope of the present disclosure.

[0121] The present disclosure includes the following aspects. (Aspect 1) Comprising a negative thermal expansion material, and having a sphericity of 0.2 or higher A powder. (Aspect 2) The volume frequency median particle diameter (D 50 ) is 20 μm or less The powder according to Aspect 1. (Aspect 3) The volume frequency median particle diameter (D 50 ) is 10 μm or less The powder according to Aspect 1. (Aspect 4) The 90% volume frequency particle diameter (D90 ) is 40 μm or less The powder described in Embodiment 1. (Aspect 5) The aforementioned negative thermal expansion material is Cu (1) x1 T x2 V y1 A y2 O z (T contains at least one element selected from Li, Na, K, Mg, Ca, Sr, Ba, Al, Si, Ti, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ta, W, Bi, B, Na, K, F, Cl, Br, I, Hf, Y, Yb, S, Mo, Te, Pb, Cd, Te, Nd, Sm, Eu, Tb, Dy, Ho, and A is The compound contains at least one element selected from Li, Mg, Ca, Al, Si, P, Ti, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ta, W, Bi, Y, Pr, Nd, Sm, and satisfies 0 ≤ x² < 2, 0 ≤ y² ≤ 2, 1.7 ≤ x¹ + x² ≤ 2.3, 1.7 ≤ y¹ + y² ≤ 2.3, and 6 ≤ z ≤ 8. The powder according to any one of the embodiments 1 to 4. (Aspect 6) The aforementioned negative thermal expansion material is Zn (2) x1 T x2 P y1 A y2 O z (T contains at least one element selected from Li, Mg, Al, Si, Ca, Sr, Ba, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ce, Ta, W, Bi, B, Na, K, F, Cl, Br, I, Hf, Y, Yb, S, Mo, Te, Pb, Cd, Te, Nd, Sm, Eu, Tb, Dy, Ho, and A contains at least one element selected from Li, Ca, Sr, Ba, Al, Si, V, Ge, Sn, La, Ce, Y, Pr, Nd, Sm, and satisfies 0≦x²<2, 0≦y²≦2, 1.7≦x¹+x²≦2.3, 1.7≦y¹+y²≦2.3, and 6≦z≦8.) The powder according to any one of the embodiments 1 to 4. (Aspect 7) The aforementioned negative thermal expansion material is Zn (2) x1 T x2 P y1 A y2 O z (T contains at least two elements selected from Li, Mg, Al, Si, Ca, Sr, Ba, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ce, Ta, W, Bi, B, Na, K, F, Cl, Br, I, Hf, Y, Yb, S, Mo, Te, Pb, Cd, Te, Nd, Sm, Eu, Tb, Dy, Ho, and A contains at least one element selected from Li, Ca, Sr, Ba, Al, Si, V, Ge, Sn, La, Ce, Y, Pr, Nd, Sm, and satisfies 0≦x²<2, 0≦y²≦2, 1.7≦x¹+x²≦2.3, 1.7≦y¹+y²≦2.3, and 6≦z≦8.) The powder according to any one of the embodiments 1 to 4. (Pattern 8) The aforementioned negative thermal expansion material is Cu (1) x1 T x2 V y1 A y2 O z (T contains at least one element selected from Li, Na, K, Mg, Ca, Sr, Ba, Al, Si, Ti, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ta, W, Bi, B, Na, K, F, Cl, Br, I, Hf, Y, Yb, S, Mo, Te, Pb, Cd, Te, Nd, Sm, Eu, Tb, Dy, Ho, and A is Li It contains at least one element selected from Mg, Ca, Al, Si, P, Ti, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ta, W, Bi, Y, Pr, Nd, Sm, and satisfies 0 ≤ x² < 2, 0 ≤ y² ≤ 2, 1.7 ≤ x¹ + x² ≤ 2.3, 1.7 ≤ y¹ + y² ≤ 2.3, and 6 ≤ z ≤ 8. The powder according to any one of the embodiments 1 to 4. (Aspect 9) The aforementioned negative thermal expansion material is Zn (2) x1 Tx2 P y1 A y2 O z (T contains at least one element selected from Li, Mg, Al, Si, Ca, Sr, Ba, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ce, Ta, W, Bi, B, Na, K, F, Cl, Br, I, Hf, Y, Yb, S, Mo, Te, Pb, Cd, Te, Nd, Sm, Eu, Tb, Dy, Ho, and A contains at least one element selected from Li, Ca, Sr, Ba, Al, Si, V, Ge, Sn, La, Ce, Y, Pr, Nd, Sm, and satisfies 0≦x²<2, 0≦y²≦2, 1.7≦x¹+x²≦2.3, 1.7≦y¹+y²≦2.3, and 6≦z≦8.) This includes two or more compounds represented by The powder according to any one of the embodiments 1 to 4. (Aspect 10) The aforementioned negative thermal expansion material is General formula (1) Cu x1 T x2 V y1 A y2 O z A compound represented by (T contains at least one element selected from Li, Na, K, Mg, Ca, Sr, Ba, Al, Si, Ti, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ta, W, Bi, and A contains at least one element selected from Li, Mg, Ca, Al, Si, P, Ti, Cr, Mn, Fe, Co, Ni, Zn, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ta, W, Bi, and satisfies 0≦x²<2, 0≦y²≦2, 1.7≦x1+x²≦2.3, 1.7≦y1+y²≦2.3, 6≦z≦8) and General formula (2) Zn x1 T x2 P y1 A y2 O zA compound represented by (T contains at least one element selected from Li, Mg, Al, Si, Ca, Sr, Ba, Ti, V, Cr, Mn, Fe, Co, Ni, Cu, Ga, Ge, Zr, Nb, Mo, Ag, In, Sn, Sb, La, Ce, Ta, W, Bi, B, Na, K, F, Cl, Br, I, Hf, Y, Yb, S, Mo, Te, Pb, Cd, Te, Nd, Sm, Eu, Tb, Dy, Ho, and A contains at least one element selected from Li, Ca, Sr, Ba, Al, Si, V, Ge, Sn, La, Ce, Y, Pr, Nd, Sm, satisfying 0≦x²<2, 0≦y²≦2, 1.7≦x¹+x²≦2.3, 1.7≦y¹+y²≦2.3, 6≦z≦8), including The powder according to any one of the embodiments 1 to 4. (Aspect 11) A step of producing a powder by spray-drying a solution containing raw materials for a negative thermal expansion material, The steps include: a second calcination of the generated powder, Equipped with, The temperature for the secondary firing is 1000°C or lower. A method for manufacturing powders. (Aspect 12) A step of producing a powder by spray-drying a solution containing raw materials for a negative thermal expansion material, The steps include: a second calcination of the generated powder, Equipped with, The duration of the secondary firing is 10 minutes or more. A method for manufacturing powders. (Aspect 13) A step of introducing a powder of a negative thermal expansion material into the flow path, A step of heating the powder while dispersing it inside the flow passage, Equipped with, The time the powder remains in the flow passage is 1 second or more. A method for manufacturing powders. [Industrial applicability]

[0122] This disclosure relates to a powder containing a negative thermal expansion material and a method for producing the powder. [Explanation of Symbols]

[0123] 1: Powder manufacturing equipment, 2: Flow channel, 3: Drying oven, 4: Pyrolysis furnace, 10-13: Mist, 14: Drying result, 15: Particles during pyrolysis, 16: Fine particles

Claims

[Claim 1] It contains a material with negative thermal expansion and has a sphericity of 0.2 or higher. powder.

Citation Information

Patent Citations

  • Negative thermal expansion material and composite

    JP2019210198A