Method for manufacturing a resist pattern-containing laminate, conductive film
By controlling light exposure and development processes with specific line width and substrate thickness relationships, the method addresses back-exposure reflection issues, enabling the production of a resist pattern-containing laminate with desired shapes and conductive nanowires.
Patent Information
- Application Number
- JP2023159381
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-09-25
- Publication Date
- 2026-11-20
AI Technical Summary
The formation of a resist pattern on a conductive film is hindered by back-exposure reflection caused by fine metal wires on the opposite surface of the base material, making it difficult to achieve a desired shape.
A method involving specific exposure and development steps with light irradiation and resist film formation, ensuring the line widths and substrate thickness satisfy certain relationships to suppress back-exposure reflection, allowing for the creation of a resist pattern-containing laminate.
This method enables the production of a resist pattern-containing laminate with a desired shape by suppressing back-facing of the resist film, facilitating the formation of thin and conductive nanowires with excellent conductivity.
Smart Images

Figure 2026183168000007 
Figure 2026183168000008 
Figure 2026183168000009
Abstract
Description
[Technical Field]
[0001] The present invention relates to a method for manufacturing a resist pattern-containing laminate and a conductive film. [Background technology]
[0002] Flexible substrates having conductive nanowires (fine wire-shaped wiring exhibiting conductivity) (hereinafter also referred to as "conductive films") are widely used in various applications such as touch panels, solar cells, and EL (electroluminescent) elements. In particular, the adoption rate of touch panels in mobile phones and portable game devices has been increasing in recent years, and the demand for conductive films for capacitive touch panels capable of multi-point detection is rapidly expanding. Various methods have been proposed for manufacturing conductive nanowires. For example, as shown in Patent Document 1, a method for manufacturing conductive nanowires by a semi-additive method is described, which includes the steps of using a negative-type photoresist to provide a plating resist pattern for a metal wiring pattern on the surface of a first metal layer, performing electroplating, peeling off the plating resist pattern, and then removing the first metal layer. [Prior art documents] [Patent Documents]
[0003] [Patent Document 1] Japanese Patent Publication No. 2007-287953 [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] The present inventors studied a new method for producing a resist pattern-containing laminate with reference to the technology related to the production of conductive films described in Patent Document 1 and the like, and found that when a resist film is disposed on one surface side of a laminate in which fine metal wires are arranged on both sides of a base material and an attempt is made to form a pattern on the resist film, back-exposure reflection on the resist film caused by the fine metal wires disposed on the other surface side of the base material occurs, which may make it difficult to form a resist pattern of a desired shape.
[0005] In view of the above circumstances, the present invention has an object to provide a method for producing a resist pattern-containing laminate, in which back-exposure reflection on a resist film disposed on one surface side of a base material caused by fine metal wires disposed on the other surface side is suppressed, and a resist pattern of a desired shape can be produced. Another object of the present invention is to provide a conductive film. [Means for Solving the Problems]
[0006] As a result of intensive studies to solve the above problems, the present inventors have completed the present invention. That is, the inventors have found that the above problems can be solved by the following configurations.
[0007] [1] An exposure step of irradiating a laminate having a base material, a first metal pattern disposed on one surface side of the base material and composed of first fine metal wires, a first resist film disposed on the first metal pattern, and a second metal pattern disposed on the other surface side of the base material and composed of second fine metal wires with light from the other surface side of the base material to expose the first resist film, and a development step of developing the first resist film to form a first resist pattern to obtain a resist pattern-containing laminate, wherein the line width w2 of the second fine metal wires and the thickness d of the base material satisfy the relationship of formula (1) described later, the method for producing a resist pattern-containing laminate. [2] A method for manufacturing a resist pattern-containing laminate according to [1], further comprising: a second resist film formation step of forming a second resist film on the surface side of the substrate on which the second metal pattern is arranged after the development step described above; a second exposure step of irradiating the second resist film with light from one of the surfaces of the substrate to expose the second resist film; and a second development step of developing the second resist film to form a second resist pattern and obtain a resist pattern-containing laminate, wherein the line width w1 of the first metal nanowire and the thickness d of the substrate satisfy the relationship of formula (2) described below. [3] A method for manufacturing a resist pattern-containing laminate according to [1] or [2], further comprising a conductive wire forming step of forming an upper conductive layer on the exposed first metal nanowire and on the exposed second metal nanowire of the resist pattern-containing laminate obtained in the second developing step to obtain a conductive nanowire. [4] The method for manufacturing a resist pattern-containing laminate according to [3], wherein the conductive fine wire formation step is a step of performing a plating treatment on the resist pattern-containing laminate obtained in the second development step. [5] The method for manufacturing a resist pattern-containing laminate according to [4], wherein the above plating treatment is electroless plating. [6] A method for manufacturing a resist pattern-containing laminate according to any one of [1] to [5], wherein the line width w2 of the second fine metal wire is 3.0 μm or less. [7] A method for manufacturing a resist pattern-containing laminate according to any one of [1] to [6], wherein the line width w1 of the first metal nanowire is 3.0 μm or less. [8] A method for manufacturing a resist pattern-containing laminate according to any one of [1] to [7], further comprising a first resist film forming step, before the exposure step, in which a first resist film is formed on the surface side of the substrate on which the first metal pattern is arranged, in a precursor laminate having the substrate, the first metal pattern, and the second metal pattern, to obtain the laminate. [9] The method for manufacturing a resist pattern-containing laminate according to [8], wherein the first resist film formation step is a step of transferring the resist film to the surface side of the substrate on which the first metal pattern is arranged, using a dry film resist having a temporary substrate and a resist film.
[10] A method for manufacturing a resist pattern-containing laminate according to any one of [1] to [9], further comprising a first conductive wire forming step of forming a metal pattern on the first metal wire after the above developing step to obtain a conductive wire.
[11] The material comprises a substrate, a first conductive nanowire disposed on one surface of the substrate, a first insulating film disposed on the one surface of the substrate in a region where the first conductive nanowire is not disposed, a second conductive nanowire disposed on the other surface of the substrate, and a second insulating film disposed on the other surface of the substrate in a region where the second conductive nanowire is not disposed, wherein the line width v1 of the first conductive nanowire and the thickness d of the substrate satisfy the relationship of equation (X1) described below, and the height h1 of the first conductive nanowire and the line width v1 of the first conductive nanowire A conductive film wherein the following relationship is satisfied by equation (Y1) described below, the line width v2 of the second conductive nanowire and the thickness d of the substrate satisfy the following relationship by equation (X2) described below, the height h2 of the second conductive nanowire and the line width v2 of the second conductive nanowire satisfy the following relationship by equation (Y2) described below, the metal density of the lower region of the first conductive nanowire on the substrate side is lower than the metal density of the upper region of the first conductive nanowire other than the lower region, and the metal density of the lower region of the second conductive nanowire on the substrate side is lower than the metal density of the upper region of the second conductive nanowire other than the lower region.
[12] The conductive film according to
[11] , wherein the line width v2 of the second conductive nanowire is 3.0 μm or less.
[13] The conductive film according to
[11] or
[12] , wherein the line width v1 of the first conductive nanowire is 3.0 μm or less.
[14] A conductive film comprising a substrate, a first conductive nanowire disposed on one surface side of the substrate, a first insulating film disposed on the one surface side of the substrate in a region where the first conductive nanowire is not disposed, and a second metal pattern disposed on the other surface side of the substrate and composed of a second metal nanowire, wherein the line width w2 of the second metal pattern and the thickness d of the substrate satisfy the relationship of formula (1) described below, the height h1 of the first conductive nanowire and the line width v1 of the first conductive nanowire satisfy the relationship of formula (Y1) described below, and the metal density of the lower region of the first conductive nanowire on the substrate side is lower than the metal density of the upper region of the first conductive nanowire other than the lower region.
[15] The conductive film according to
[14] , wherein the line width w2 of the second metal pattern described above is 3.0 μm or less.
[16] The conductive film according to
[14] or
[15] , wherein the line width v1 of the first conductive nanowire is 3.0 μm or less. [Effects of the Invention]
[0008] According to the present invention, a method for manufacturing a resist pattern-containing laminate is provided, which suppresses back-facing of a resist film placed on one surface of the substrate by a metal fine wire placed on the other surface, and enables the production of a resist pattern of a desired shape. Furthermore, according to the present invention, a conductive film can be provided. [Brief explanation of the drawing]
[0009] [Figure 1] This figure shows an example of the structure of a laminate used in the manufacturing method of the present invention. [Figure 2] This figure shows an example of the structure of a laminate obtained in the exposure step of the manufacturing method of the present invention. [Figure 3] This figure shows an example of the structure of a resist pattern-containing laminate manufactured by the manufacturing method of the present invention. [Figure 4] This is a plan view showing an example of a mesh-like metal pattern. [Figure 5]This figure shows an example of the configuration of a precursor laminate used in the resist film formation step of the manufacturing method of the present invention. [Figure 6] This figure shows another example of the configuration of a resist pattern-containing laminate manufactured by the manufacturing method of the present invention. [Figure 7] This figure shows another example of the configuration of a resist pattern-containing laminate manufactured by the manufacturing method of the present invention. [Figure 8] This is a diagram illustrating a manufacturing method according to the first embodiment of the present invention. [Figure 9] This is a diagram illustrating a manufacturing method according to a second embodiment of the present invention. [Figure 10] This is a diagram illustrating a manufacturing method according to a second embodiment of the present invention. [Figure 11] This is a diagram illustrating a manufacturing method according to a third embodiment of the present invention. [Figure 12] This is a diagram illustrating a manufacturing method according to a third embodiment of the present invention. [Modes for carrying out the invention]
[0010] The present invention will be described in detail below with reference to the drawings. The following description of the constituent elements may be based on typical embodiments of the present invention, but the present invention is not limited to such embodiments. Furthermore, the following figures are illustrative for illustrating the present invention, and the present invention is not limited by these figures.
[0011] The following definitions are used within this specification. In this specification, a numerical range represented by "~" means a range that includes the numbers written before and after "~" as the lower and upper limits, respectively. In this specification, if two or more components are present, the "content" of those components means the total content of those two or more components. In this specification, "g" and "mg" represent "mass in g" and "mass in mg," respectively. In this specification, angles expressed as specific numerical values, as well as angle-related terms such as "parallel," "perpendicular," and "orthogonal," shall include the generally acceptable margin of error in the relevant art unless otherwise specified. For example, "orthogonal" or "perpendicular" means within the range of 90° ± 5°, and "parallel" means within the range of 0° ± 5°. Similarly, for other specific angles, unless otherwise specified, it means that the difference from the exact angle is within 5 degrees. The above angle difference is preferably within 4 degrees, and more preferably within 3 degrees.
[0012] In this specification, "polymer" or "polymer compound" means a compound having a weight-average molecular weight of 2000 or more. Here, the weight-average molecular weight is defined as the polystyrene equivalent value measured using gel permeation chromatography (GPC) under the following conditions. • Equipment: HLC-8320GPC manufactured by Tosoh Corporation • Column: TSK-GEL G3000PWXL manufactured by Tosoh Corporation • Column temperature: 35℃ ·Flow rate: 0.5mL / min • Calibration curve: POLY SODIUM ACRYLATE STANDARD, manufactured by Sowa Kagaku Co., Ltd. • Eluent: A solution prepared by diluting a mixture of sodium dihydrogen phosphate dodecahydrate and disodium hydrogen phosphate dihydrate (34.5g / 46.2g) with pure water to 5000g.
[0013] [Method for manufacturing a laminate containing a resist pattern] The present invention provides a method for manufacturing a resist pattern-containing laminate (hereinafter also referred to as "this manufacturing method"), which comprises a substrate, a first metal pattern composed of first metal nanowires arranged on one surface side of the substrate, a first resist film arranged on the first metal pattern, and a second metal pattern composed of second metal nanowires arranged on the other surface side of the substrate (hereinafter also referred to as "laminated body A"), and includes an exposure step of irradiating the substrate with light from the other surface side to expose the first resist film, and a development step of developing the first resist film to form a first resist pattern and obtain a resist pattern-containing laminate. Furthermore, in this manufacturing method, the line width w2 of the second metal nanowire and the thickness d of the substrate satisfy the relationship given by equation (1). Formula (1) d / w2≧3.0 The following describes each step in this manufacturing method.
[0014] <Exposure process> This manufacturing method includes an exposure step in which the laminate A is exposed by irradiating it with light from the other surface side of the substrate, i.e., the surface side on which the second metal pattern is arranged. Figure 1 shows an example of the configuration of laminate A used in the exposure process of this manufacturing method. The laminate 11 shown in Figure 1 comprises a substrate 20, a first metal nanowire 31 disposed on one surface 21 of the substrate 20, a first resist film 40 disposed on the first metal nanowire 31, and a second metal nanowire 32 disposed on the other surface 22 of the substrate 20. Here, the first metal nanowire 31 constitutes a first metal pattern (not shown), and the second metal nanowire 32 constitutes a second metal pattern (not shown). As shown in the figure, in the laminate 11, the first metal wire 31 (first metal pattern) and the second metal wire 32 (second metal pattern) are arranged facing each other with the base material 20 in between.
[0015] Although Figure 1 shows two first metal wires 31 and one second metal wire 32 extending perpendicular to the plane of the paper, Figure 1 is only a part of the overall structure of the laminate 11, and the arrangement and number of each metal wire in the laminate A are not particularly limited. The arrangement and number of metal wires, upper conductive layers, and conductive wires shown in each of the following drawings are the same as described above.
[0016] In the exposure process, light is shone onto the entire surface of the substrate 20 from the other surface 22 side of the substrate, and the first resist film 40 is exposed using the first metal pattern as a mask. Figure 2 shows an example of the structure of the laminate A obtained by the exposure process. In the laminate 12 shown in Figure 2, the substrate 20, the first metal nanowire 31, and the second metal nanowire 32 are the same as those in the laminate 11 shown in Figure 1. On the other hand, the first resist film 40 of the laminate 11 is divided into an exposed portion 41 and an unexposed portion 42 in the laminate 12. When light is irradiated onto the first resist film 40 from the other surface 22 of the substrate 20 through the substrate 20, the area on one surface 21 where the first metal nanowires 31 are not placed becomes an exposed area 41, and the area where the first metal nanowires 31 are placed becomes an unexposed area 42. In this way, the first metal pattern composed of the first metal nanowires 31 functions as a mask for the first resist film 40, and exposed areas 41 and unexposed areas 42 with shapes corresponding to the first metal pattern are formed.
[0017] The wavelength of light used in the exposure process is not particularly limited as long as it can expose the first resist film and penetrate the substrate. Examples of light and light sources used in the exposure process include g-line (wavelength 436 nm), i-line (365 nm), KrF excimer laser (248 nm), ArF excimer laser (193 nm), and F2 excimer laser (157 nm). When using a laser as the light source, the exposure can be performed by scanning the laser so that the entire surface of the substrate is irradiated with light. The exposure amount in the exposure process can be adjusted as needed, but is generally between 50 and 2000 mJ / cm². 2 Preferably, 100-1000 mJ / cm² 2 More preferably, 200-500 mJ / cm² 2 That is even more preferable.
[0018] In the exposure process, the first resist film may be heated (pre-baked) before exposure, or heated (post-baked) after exposure. The heating can be adjusted as appropriate depending on the first resist film used, but examples of heating conditions include heating at 60 to 150°C for 10 to 300 seconds.
[0019] <Developing process> This manufacturing method includes a developing step (first developing step) in which an exposed first resist film is developed to form a first resist pattern. In the development process, the first resist film is developed, which removes the first resist film located in the region corresponding to the first metal pattern, and forms a first resist pattern having openings with a shape corresponding to the first metal pattern.
[0020] Figure 3 shows an example of the structure of a resist pattern-containing laminate (hereinafter also referred to as "laminated laminate B") produced by this manufacturing method, which is obtained by developing the first resist film of laminate A in a development step after the exposure step. The laminate 13 shown in Figure 3 comprises a substrate 20, a first metal nanowire 31 disposed on one surface 21 of the substrate 20, a first resist pattern 43 disposed on one surface 21 of the substrate in an area where the first metal nanowire 31 is not disposed, and a second metal nanowire 32 disposed on the other surface 22 of the substrate 20. In the laminate 13 shown in Figure 3, the base material 20, the first metal wire 31, and the second metal wire 32 are the same as those in the laminate 11 shown in Figure 1. Meanwhile, the developing process removes the unexposed portion 42 of the laminate 12, forming a first resist pattern 43 that covers only the areas where the first metal wires 31 are not placed. In addition, an opening 44 is formed in the area that was occupied by the unexposed portion 42 of the laminate 12, that is, the area on one surface 21 of the substrate 20 where the first metal wires 31 were placed.
[0021] In this manufacturing method, during the exposure process, light is irradiated from the other surface of the substrate to expose the first resist film using the first metal pattern as a mask. Therefore, during the development process, a resist pattern is formed having a desired pattern shape that is self-aligned with the first metal pattern, with the shape of the openings corresponding to the shape of the first metal pattern. By applying the conductive nanowire formation process described later to the laminate B having such a resist pattern, conductive nanowires with a desired line width that does not exceed the width of the openings can be formed. In addition, since the shape of the conductive nanowire corresponds to the shape of the openings in the resist pattern, by increasing the aspect ratio (ratio of depth to width) of the opening shape, conductive nanowires that are thin and also have excellent conductivity can be formed more easily. Unless otherwise specified, any description including the simple notation "conductive nanowire" applies to both the first conductive nanowire formed on one surface of the substrate and the second conductive nanowire formed on the other surface of the substrate, without distinction.
[0022] Furthermore, this manufacturing method makes it possible to suppress back-image reflection from a metal fine wire placed on one surface of the substrate onto a resist film placed on the other surface. In this specification, "back-facing" refers to the phenomenon in which, when a resist film placed on one surface of a substrate is exposed by irradiating it with light from the other surface of the substrate, film defects such as depressions and holes occur in the region of the exposed resist film that is facing the metal wires placed on the other surface of the substrate, with the substrate in between. The mechanism by which the present invention can suppress back-facing of the resist film due to the metal nanowire is not entirely clear, but the inventors speculate as follows: That is, if the thickness d of the substrate does not satisfy the relationship of equation (1) with respect to the line width w2 of the second metal nanowire, and the thickness d of the substrate is thin, then when light is irradiated from the other surface side of the substrate, the light is blocked by the second metal nanowire, and the region of the first resist film facing the second metal nanowire across the substrate is not sufficiently exposed, resulting in back-facing of the first resist film. On the other hand, if the thickness d of the substrate satisfies the relationship of equation (1) with respect to the line width w2 of the second metal nanowire, then when light is irradiated in the same way, it is speculated that the light that passes outside the width direction of the second metal nanowire and is diffracted by the second metal nanowire reaches the region of the first resist film corresponding to the second metal nanowire while passing through the substrate which has sufficient thickness d. As a result, the region of the first resist film corresponding to the second metal nanowire was also exposed, and it is believed that the back exposure caused by the second metal nanowire was suppressed in the first resist film. Based on the above, it is considered that this manufacturing method suppresses the back-facing of metal fine lines onto the resist film, and makes it possible to manufacture a resist pattern-containing laminate having a resist pattern of a desired shape.
[0023] In the development process, known developers can be used, and the developer should be selected according to the type of first resist film. Examples of developers include alkaline developers and organic solvent developers. Furthermore, in the developing process, rinsing with a rinsing solution may be performed after development. The rinsing solution may be the same as that used in the developing solution, or a different rinsing solution may be used. Examples of other rinsing solutions include water (preferably deionized water or ultrapure water). In the development process, the first resist pattern formed preferably has a rectangular shape in a cross-section perpendicular to the direction in which the first metal nanowires constituting the first metal pattern extend.
[0024] The following provides a more detailed explanation of the components used in this manufacturing method and any processes that this manufacturing method may include.
[0025] <Laminate A> Laminate A comprises at least a substrate, a first metal pattern disposed on one surface of the substrate and composed of first metal nanowires, a first resist film disposed on the first metal pattern, and a second metal pattern disposed on the other surface of the substrate and composed of second metal nanowires. Laminate A may have other components as long as they do not interfere with the exposure process and development process described later and can be used to manufacture the target laminate B. For example, in the laminate 11 shown in Figure 1, the area on the other surface 22 of the substrate 20 where the second metal fine wire 32 is not placed is exposed, but the laminate A may have a second resist pattern placed in the area on the other surface of the substrate where the second metal pattern is not placed.
[0026] Each component of laminate A will be described in detail.
[0027] (base material) The substrate is not particularly limited in type, as long as it is a material that can support each metal wire and transmit the exposure light used in the exposure process. Examples of substrates include plastic substrates and glass substrates, with plastic substrates being preferred. The substrate material should be selected to match the wavelength of the exposure light used in the exposure process. The transmittance of the substrate at the wavelength of the exposure light used in the exposure process is preferably 30% or more, more preferably 50% or more, and even more preferably 70% or more. There is no particular upper limit, and 100% is an example. The above transmittance can be measured with a commercially available spectrophotometer.
[0028] The substrate is preferably flexible in that the resulting conductive film has excellent bendability. A flexible substrate means a substrate that can be bent, and specifically means a substrate that does not crack even when bent with a bending radius of curvature of 2 mm. The flexible substrate has processability that allows it to form a three-dimensional shape. The above-mentioned plastic substrate is an example of a flexible substrate.
[0029] The materials constituting the base material are preferably resins with a melting point of approximately 290°C or lower, such as polyethylene terephthalate (PET) (258°C), polycycloolefin (134°C), polycarbonate (250°C), acrylic film (128°C), polyethylene naphthalate (269°C), polyethylene (135°C), polypropylene (163°C), polystyrene (230°C), polyvinyl chloride (180°C), polyvinylidene chloride (212°C), and triacetylcellulose (290°C). PET, polycycloolefin, or polycarbonate are more preferred. Among these, PET is even more preferred due to its excellent adhesion to each metal pattern. The values in parentheses above are the melting point or glass transition temperature. Furthermore, polyimide may be selected as the base material, as long as it allows the exposure light used in the exposure process to pass through it. The total light transmittance of the substrate is preferably 85-100%. The total light transmittance is measured using the method specified in JIS (Japanese Industrial Standards) K 7375:2008, "Plastics - Method for determining total light transmittance and total light reflectance."
[0030] The thickness d of the substrate is not particularly limited as long as the wire width w2 of the second metal nanowire of the laminate A and the thickness d of the substrate satisfy the relationship given by equation (1). For example, it is more than 10 μm and 300 μm or less, and 20 to 200 μm is preferred, and 30 to 150 μm is more preferred, in terms of having better flexibility of the conductive film.
[0031] A primer layer may be applied to the surface of the substrate. The undercoat layer preferably contains a specific polymer, as described later. Using this undercoat layer further improves the adhesion of each metal wire to the substrate. The method for forming the undercoat layer is not particularly limited. For example, an undercoat layer-forming composition containing a specific polymer, as described later, can be applied to a substrate and subjected to heat treatment as necessary. The undercoat layer-forming composition may optionally contain a solvent. The type of solvent is not particularly limited, and examples include solvents used in the photosensitive layer-forming composition described later. In addition, a latex containing particles of the specific polymer may be used as the undercoat layer-forming composition containing the specific polymer. The thickness of the undercoat layer is not particularly limited, but 0.02 to 0.3 μm is preferred, and 0.03 to 0.2 μm is more preferred, as it provides better adhesion of each metal wire to the substrate.
[0032] (1st metal thin wire, 2nd metal thin wire) In laminate A, the first metal nanowire constituting the first metal pattern and the second metal nanowire constituting the second metal pattern are arranged on one surface side and the other surface side of the substrate, respectively.
[0033] In this manufacturing method, the wire width w2 of the second metal fine wire and the thickness d of the base material satisfy the relationship given by equation (1). Formula (1) d / w2≧3.0 The ratio d / w2 of the wire width w2 of the second metal fine wire to the thickness d of the base material is preferably 5.0 or greater, and more preferably 15.0 or greater, in terms of achieving superior effects of the present invention. There is no particular upper limit, but it is preferably 300.0 or less, and more preferably 150.0 or less.
[0034] The wire width w2 of the second metal nanowire is not particularly limited as long as the relationship between the thickness d of the base material and formula (1) above is satisfied. However, in terms of superior effects of the present invention and the fact that the formed conductive nanowire is less visible, it is preferably 5.0 μm or less, more preferably 3.0 μm or less, and even more preferably 2.0 μm or less. The lower limit is not particularly limited, but it is preferably 0.1 μm or more, and more preferably 0.5 μm or more. The thickness of the second metal wire is not particularly limited, but is preferably 0.1 to 3.0 μm, and more preferably 0.1 to 2.0 μm, in terms of superior adhesion to the substrate and conductivity of the conductive film.
[0035] In laminate A, it is preferable that the wire width w1 of the first metal nanowire and the thickness d of the base material satisfy the relationship given by equation (2). Formula (2) d / w1≧3.0 If laminate A does not have a second resist pattern on the other surface side of the substrate, a second resist film is formed on the other surface side of the substrate, and when light is irradiated from one surface side of the substrate to expose the second resist film and form a second resist pattern, back reflection by the first metal nanowire in the resulting second resist pattern can be suppressed. The ratio d / w1 of the wire width w1 of the first metal fine wire to the thickness d of the base material is more preferably 0.5 or greater, and even more preferably 15.0 or greater, in terms of achieving the above-mentioned effects more favorably. There is no particular upper limit, but it is preferably 300.0 or less, and more preferably 150.0 or less.
[0036] The preferred embodiment of the wire width w1 and thickness of the first metal thin wire is the same as the preferred embodiment of the wire width w2 and thickness of the second metal thin wire.
[0037] Unless otherwise specified, any description including the simple term "metallic wire" below applies to both the first and second metallic wires, without distinction.
[0038] The wire width and thickness of a thin metal wire are obtained by the following method. When a metal wire is exposed on the surface of a substrate, the wire width and thickness of the metal wire can be measured using a digital microscope (for example, the VHX-5000 microscope manufactured by Keyence Corporation). On the other hand, if the metal wire is not exposed on the surface of the substrate, the wire width and thickness of the metal wire can be measured by observation using a scanning electron microscope (SEM). Taking a conductive film obtained by forming an upper conductive layer on a metal wire in laminate B as an example, the conductive film is cut along a cross section perpendicular to the direction in which the metal wire extends, and the resulting cross section is observed with an SEM. The maximum value in the width direction of the metal wire is measured from the obtained observation image. The above cross-sectional observation and measurement using an SEM is performed at 10 arbitrary locations on the conductive film where the metal wire is arranged, and the average value obtained by arithmetic meaning the obtained measurements is taken as the wire width of the metal wire. The thickness of the metal wire can also be measured in accordance with the above method for measuring the wire width.
[0039] Metal wires contain metal as a conductive material. Examples of metals included in the metal wires are individual metals selected from the group consisting of silver, copper, gold, nickel, and palladium, as well as mixtures (alloys) of two or more metals selected from the above group. The metal contained in the metal wire is preferably at least one of silver and copper, with silver being more preferred, due to its superior conductivity. The silver contained in the metal wire may be pure silver or a mixture of silver and another metal (silver alloy). Among the metals included in the metal wires, pure silver or an alloy of silver and copper is more preferred, and pure silver is even more preferred.
[0040] The metal (preferably metallic silver) contained in the metal nanowire is often in the form of solid parts. The average particle size of the metal is preferably 10 to 1000 nm in terms of equivalent spherical diameter, and more preferably 10 to 200 nm. A value of 50 to 150 nm is even more preferable because it results in a smaller change in the resistance value of the conductive nanowire under humid heat conditions. The equivalent spherical diameter is the diameter of spherical particles having the same volume, and the average particle size of the metal particles (preferably metallic silver particles) and the silver halide particles described later is obtained by measuring the equivalent spherical diameter of 100 objects and taking the arithmetic mean of those values. The shape of the metal particles is not particularly limited and may include, for example, spherical, cubic, plate-like, octahedral, and tetrahedral shapes. Furthermore, the metal particles may be partially or entirely bonded together by fusion.
[0041] The metal nanowire may have a structure in which multiple metals are dispersed in a polymer compound, as described later, or the metals may aggregate within the polymer compound to form aggregates. Furthermore, at least some of the multiple metals contained in the metal nanowire may be joined together by metals derived from metal ions used in the plating process described later. The metal content in the metal nanowire is not particularly limited, but in terms of superior conductivity of the conductive film, the metal content per unit area of the region on the substrate surface where the metal nanowire is located is 1.0 to 20.0 g / m². 2 Preferably, it is 2.0 to 10.0 g / m 2 It is preferable that it be so.
[0042] The metal fine wire preferably contains a polymer compound, as this provides superior bending resistance for the conductive film. The type of polymer compound included in the metal nanowire is not particularly limited, and known polymer compounds can be used. Among these, polymer compounds different from gelatin (hereinafter also referred to as "specific polymers") are preferred because they can form a silver-containing layer and metal nanowire with superior strength. The specific polymers contained in the metal wires will be discussed later.
[0043] The metal wire may contain gelatin as a polymer compound. The type of gelatin is not particularly limited; for example, lime-treated gelatin and acid-treated gelatin can be used. Furthermore, compounds selected from the group consisting of gelatin hydrolysates, gelatin enzymatic hydrolysates, and gelatin modified with amino and / or carboxyl groups (phthalated gelatin and acetylated gelatin) may also be used.
[0044] The metal wire may also contain other materials besides those described above, as needed. Other materials may include a photosensitive layer, as described later, as needed.
[0045] (First metal pattern, second metal pattern) In laminate A, the arrangement of the first metal pattern, which is composed of first metal wires, on one surface of the substrate, and the arrangement of the second metal pattern, which is composed of second metal wires, on the other surface of the substrate are not particularly limited. Unless otherwise specified, any description including the simple term "metal pattern" below applies to both the first and second metal patterns, without distinction.
[0046] The pattern shape of the metal pattern is not particularly limited, and is preferably a geometric figure such as an equilateral triangle, isosceles triangle, or right triangle; a quadrilateral such as a square, rectangle, rhombus, parallelogram, or trapezoid; a regular n-gon such as a regular hexagon or octagon; a circle, ellipse, or star; or a geometric figure formed by combining these figures, and is more preferably a mesh pattern.
[0047] Figure 4 is a plan view showing an example of a mesh-like metal pattern. A mesh pattern, as shown in Figure 4, refers to a shape that includes multiple non-fine wire sections (grids) 33 composed of intersecting metal fine wires 30, each spaced apart from the others. In Figure 4, the non-fine wire sections 33 have a square shape with side length L, but the non-fine wire sections of the mesh pattern may have other shapes as long as they are regions demarcated by metal fine wires, such as polygons (e.g., triangles, quadrilaterals (rhombuses, rectangles, etc.), hexagons, and random polygons). The shape of the edges may also be curved shapes other than straight lines, or they may be arc-shaped. If they are arc-shaped, for example, two opposing sides may be outwardly convex arcs, and the other two opposing sides may be inwardly convex arcs. Alternatively, the shape of each edge may be a wavy line shape consisting of a continuous outwardly convex arc and an inwardly convex arc. Of course, the shape of each edge may also be a sine curve.
[0048] The length L of one side of the non-fine line portion 33, which is a square grid, is not particularly limited, but is preferably 1500 μm or less, more preferably 1300 μm or less, and even more preferably 1000 μm or less. The lower limit of the length L is not particularly limited, but is preferably 5 μm or more, more preferably 30 μm or more, and even more preferably 80 μm or more. When the length of one side of the non-fine line portion is within the above range, it is also possible to maintain good transparency, and when the conductive film described later is attached to the front of the display device, the display can be viewed without any discomfort.
[0049] In terms of visible light transmittance, the aperture ratio of the metal pattern formed by the metal fine wires is preferably 90% or more, more preferably 95% or more, and even more preferably 99% or more. There is no particular upper limit, but it is less than 100%. The aperture ratio refers to the ratio (area ratio) of the area of the region where the metal pattern is not placed to the total surface area of the substrate on which the metal pattern is placed.
[0050] (First resist film) The first resist film of the laminate A is located on one surface side of the substrate and is positioned on the first metal pattern. As the first resist film, a negative-type resist is preferred in which the exposed portion is insoluble in the developer used in the developing process. Known negative-type resists can be used as the negative-type resist. Among these, a negative-type resist whose solubility in alkaline developer decreases upon exposure is preferred.
[0051] The thickness of the first resist film is not particularly limited and can be adjusted as appropriate according to the height (thickness) of the upper metal layer and conductive nanowire formed by the conductive nanowire formation process described later. The thickness of the first resist film is, for example, 0.5 to 100.0 μm, and preferably 1.0 to 30.0 μm. The thickness of the first resist film can be measured in accordance with the method for measuring the line width and thickness of a metal nanowire.
[0052] (Resist film formation process) Laminate A can be manufactured, for example, by preparing a precursor laminate having at least a substrate, a first metal pattern disposed on one surface side of the substrate and composed of first metal nanowires, and a second metal pattern disposed on the other surface side of the substrate and composed of second metal nanowires, and then forming a first resist film on the surface side (one surface side) of the substrate where the first metal pattern is disposed in the prepared precursor laminate. In other words, it is preferable that the present manufacturing method further includes a resist film formation step (first resist film formation step) to obtain the laminate A by forming a first resist film on the surface side (one surface side) of the precursor laminate on which the first metal pattern of the substrate is arranged, before the exposure step.
[0053] The resist film formation process can be carried out using a known resist film formation method. Examples of the resist film formation process include a method of applying a resist composition containing components of the first resist film to the surface of the substrate on which the first metal pattern is arranged, and curing the coating film as necessary, and a method of transferring the resist film to the surface of the substrate on which the first metal pattern is arranged using a dry film resist. In particular, the method of transferring the resist film using a dry film resist is preferred because it can suppress deformation of the first metal pattern. A more specific method for transferring a resist film is, for example, to attach a dry film resist having a temporary substrate and a resist film to the surface side of the substrate where the first metal pattern is placed, and then transfer the resist film by peeling the temporary substrate away from the resist film.
[0054] Furthermore, when the first and second resist patterns described later are not removed and the material is used as an insulating film (permanent resist) in a conductive film, it is preferable that the resulting insulating film exhibits minimal changes in haze and retardation over time. Examples of resist materials that can form a resist film usable as the above insulating film include Dow Chemical's "ATN1021" negative-type acrylic resist, the liquid negative resist material "ZPN1150" (manufactured by Nippon Zeon Co., Ltd.), and negative-type dry film resist (Asahi Kasei Electronics Corporation, "Sunfort"). Furthermore, in a laminate containing a resist pattern, the resist pattern may be removed after the conductive nanowire formation process described later is carried out. One method for removing the resist pattern is to use a stripping solution that has high affinity with the material constituting the resist pattern. A known stripping solution can be used.
[0055] (Precursor laminate) The precursor laminate used in the resist film formation process will be explained in more detail. Figure 5 is a schematic cross-sectional view showing an example of the structure of a precursor laminate. The precursor laminate 10 shown in Figure 5 comprises a base material 20, a first metal nanowire 31 arranged on one surface 21 of the base material 20, and a second metal nanowire 32 arranged on the other surface 22 of the base material 20. Here, the first metal nanowire 31 constitutes a first metal pattern (not shown), and the second metal nanowire 32 constitutes a second metal pattern (not shown).
[0056] Furthermore, the precursor laminate 10 shown in Figure 5 has, in this order, a second metal nanowire 32 constituting the second metal pattern, a base material 20, and a first metal nanowire 31 constituting the first metal pattern, while the area on the other surface 22 side of the base material 20 where the second metal nanowire 32 is not arranged is exposed. The precursor laminate used in the resist film formation process may have components other than those of the precursor laminate 10 shown in Figure 5, as long as the laminate A can be manufactured by the resist film formation process. For example, the precursor laminate may be a laminate having a second metal pattern, a substrate, and a first metal pattern in that order, and further having a second resist pattern arranged in a region on the other surface side of the substrate where the second metal pattern is not located.
[0057] The substrate, first metal wire, and second metal wire of the precursor laminate are the same as those of laminate A, including in preferred embodiments. Next, the method for manufacturing the precursor laminate will be explained using the precursor laminate 10 shown in Figure 5 as an example.
[0058] <<Method for manufacturing the precursor laminate>> The method for manufacturing the precursor laminate is not particularly limited as long as it can form metal nanowires (first metal nanowire and second metal nanowire) having the above configuration on both sides of the substrate, and known methods can be used. Methods for forming metal nanowires include, for example, a method in which a silver halide-containing layer containing silver halide particles is provided on the surface of a substrate, and then the silver halide particles are reduced to form metal nanowires (photographic method); a method in which a metal-containing layer containing metal is formed over the entire surface of a substrate, and then the metal-containing layer is partially removed using a resist pattern to form metal nanowires; and a method in which a metal-containing composition is ejected onto a substrate by a known printing method such as inkjet printing to form metal nanowires.
[0059] Among these, the photographic method of forming metal nanowires by reducing silver halide particles is preferred because it offers superior productivity and conductivity of the conductive film. Examples of photographic methods include the following methods (a) and (b), with method (a) being preferred. (a) A method for forming a layer containing silver halide on the surface of a substrate, reducing the silver halide by pattern exposure of the formed silver halide-containing layer, and then forming a patterned fine metal wire by development. (b) A method in which a physically developing nucleus layer and a layer containing silver halide are formed on a substrate in this order, the silver layer is deposited on the physically developing nucleus by pattern exposure, and then the unwanted layer containing silver halide is washed off with water (silver complex salt diffusion transfer method).
[0060] A more specific method for manufacturing a precursor laminate using photographic methods is to carry out the following steps A to E in that order. Process A: A process of forming a silver halide-free layer on both sides of the substrate, which contains a dye that is decolorized with a developing solution, gelatin, and a specific polymer. Step B: A step of forming a silver halide-containing photosensitive layer (hereinafter also referred to as the "photosensitive layer") containing silver halide, gelatin, and a specific polymer on each silver halide-free layer formed on both sides of the substrate. Step C: A step in which a photosensitive layer formed on both sides of the substrate is exposed, and then developed to form a fine, wire-like silver-containing layer containing metallic silver, gelatin, and a specific polymer. Process D: A process in which the silver-containing layer obtained in process C is subjected to heat treatment. Step E: A step to remove the gelatin from the silver-containing layer obtained in Step D and form a metal wire. The following describes processes A through E.
[0061] -Process A- A method for manufacturing a precursor laminate includes, for example, step A, forming a silver halide-free layer on both sides of a substrate containing a dye that is decolorized with a developing solution, gelatin, and a specific polymer. By performing step A, an anti-halation layer consisting of a silver halide-free layer is formed between the substrate and the silver halide-containing photosensitive layer. This prevents the photosensitive layer on one surface from being exposed by light irradiated onto the other surface during the exposure treatment in step C described later. Furthermore, since the dye is decolorized by the developer during the development treatment in step C described later, the effective reduction in exposure amount during the exposure process of this manufacturing method can be suppressed. In addition, this silver halide-free layer also contributes to improving the adhesion between the conductive fine wire and the substrate.
[0062] The substrate used in the manufacture of the precursor laminate is as previously described, including preferred embodiments.
[0063] The silver halide-free layer contains a dye that is decolorized by the developer described above, gelatin, and a specific polymer. On the other hand, the silver halide-free layer does not contain silver halide. In the silver halide-free layer, the ratio of the mass of the specific polymer to the mass of gelatin (mass of specific polymer / mass of gelatin) is not particularly limited, but is preferably 0.1 to 5.0, and more preferably 1.0 to 3.0. The content of specific polymers in the silver halide-free layer is not particularly limited, up to 0.03 g / m². 2 In many cases, the above is true, and 0.5g / m² offers superior adhesion to the conductive fine wire portion. 2 The above is preferable. There is no particular upper limit, but 2.0 g / m 2 The following are common cases. The dyes that are decolorized by the developer contained in the silver halide-free layer are not particularly limited as long as they are dyes that are decolorized by the developer (preferably an alkaline developer) used in the developing process of step C, and examples include cyanine dyes, pyryllium dyes, and aminium dyes. The content of the above dye in the silver halide-free layer is preferably 0.01 to 10% by mass, and more preferably 0.1 to 5% by mass, relative to the total solid content of the silver halide-free layer, from the viewpoint of anti-halation effect and decrease in sensitivity due to increased addition.
[0064] The method for forming the silver halide-free layer is not particularly limited. For example, a layer-forming composition containing the above-mentioned dye, gelatin, and a specific polymer is applied to a substrate, and heat treatment is performed as necessary. The layer-forming composition may optionally contain a solvent. Examples of solvents include those used in the photosensitive layer-forming composition described later. The thickness of the silver halide-free layer is not particularly limited, but is often 0.05 μm or more. A thickness of more than 1.0 μm is preferred, and 1.5 μm or more is more preferred, as it provides better adhesion to the conductive fine wire portion. There is no particular upper limit, but less than 3.0 μm is preferred. The optical density of the silver halide-free layer at a wavelength of 360 nm before the development process in step C is preferably 0.5 or higher, and more preferably 0.7 or higher, in that it provides a superior anti-halation layer effect. There is no particular upper limit to the above optical density, but 3.0 or lower is preferred. The optical density of the silver halide-free layer can be adjusted, for example, by the type and content of the above dye. The optical density of the silver halide-free layer can be determined by measuring the transmittance of the silver halide-free layer at a wavelength of 360 nm using a UV spectrophotometer (for example, "UV-1800" manufactured by Shimadzu Corporation) and converting it to optical density. The composition and physical properties of the silver halide-free layers formed on both sides of the substrate may be the same or different.
[0065] -Process B- Step B is a process of forming a photosensitive layer (silver halide-containing photosensitive layer) containing silver halide, gelatin, and a specific polymer (a polymer compound different from gelatin) on each silver halide-free layer formed on both sides of the substrate. Step B produces a substrate with a photosensitive layer that will undergo the exposure treatment described later. First, we will describe the materials (silver halides, gelatin, and specific polymers) that are preferably used in the manufacture of photosensitive substrates, and then we will describe the procedure of step B in detail.
[0066] (Silver halide) The halogen atoms contained in silver halide may be chlorine atoms, bromine atoms, iodine atoms, and fluorine atoms, or a combination thereof. For example, silver halide mainly composed of silver chloride, silver bromide, or silver iodide is preferred, and silver halide mainly composed of silver chloride or silver bromide is more preferred. Silver bromide salt, silver bromide iodide, or silver iobromide are also preferably used. Here, for example, "silver halide mainly composed of silver chloride" refers to a silver halide in which the mole fraction of chloride ions in the total halide ions is 50% or more. This silver halide mainly composed of silver chloride may also contain bromide ions and / or iodide ions in addition to chloride ions.
[0067] Silver halides are usually in the form of solid particulate matter, and the average particle size of silver halides is preferably 10 to 1000 nm in terms of spherical equivalent diameter, more preferably 10 to 200 nm, and even more preferably 50 to 150 nm, as this results in less change in the resistance value of the conductive nanowires formed under a humid and hot environment. The equivalent spherical diameter is the diameter of a spherical particle having the same volume. The "equivalent spherical diameter" used as the average particle size of silver halide mentioned above is an average value, calculated by measuring the equivalent spherical diameters of 100 silver halides and taking their arithmetic mean.
[0068] The shape of the silver halide particles is not particularly limited and can be spherical, cubic, plate-shaped (hexagonal plate-shaped, triangular plate-shaped, quadrilateral plate-shaped, etc.), octahedral, or tetrahedral.
[0069] (gelatin) The type of gelatin is not particularly limited; for example, lime-treated gelatin and acid-treated gelatin can be used. In addition, hydrolyzed gelatin, enzymatically hydrolyzed gelatin, and gelatin modified with amino groups and / or carboxyl groups (phthalated gelatin and acetylated gelatin) may be used.
[0070] (Specific polymer) The specific polymer is a polymer compound different from the above-mentioned gelatin. When the photosensitive layer contains the specific polymer, the strength of the fine metal wires formed from the photosensitive layer can be easily improved. The type of the specific polymer is not particularly limited as long as it is a compound different from gelatin, and a polymer compound that decomposes gelatin described later and does not decompose with a proteolytic enzyme or an oxidizing agent is preferable. Examples of the specific polymer include hydrophobic polymers (water-insoluble polymers), for example, (meth)acrylic resins, styrene resins, vinyl resins, polyolefin resins, polyester resins, polyurethane resins, polyamide resins, polycarbonate resins, polydiene resins, epoxy resins, silicone resins, cellulose polymers, and at least one resin selected from the group consisting of chitosan polymers, or copolymers composed of monomers constituting these resins, and the like. Further, the specific polymer preferably has a reactive group that reacts with a crosslinking agent described later. The specific polymer is preferably in the form of particles. That is, the fine metal wires preferably contain particles of the specific polymer.
[0071] As the specific polymer, a polymer (copolymer) represented by the following general formula (1) is preferable. General formula (1): -(A) x -(B) y -(C) z -(D) w - In the general formula (1), A, B, C, and D each represent a repeating unit represented by the following general formulas (A) to (D).
[0072] [Chemical Formula]
[0073] R 11 represents a methyl group or a halogen atom, and a methyl group, a chlorine atom, or a bromine atom is preferable. p represents an integer of 0 to 2, preferably 0 or 1, and more preferably 0. R 12This represents a methyl group or an ethyl group, with a methyl group being preferred. R 13 represents a hydrogen atom or a methyl group, with a hydrogen atom being preferred. L represents a divalent linking group, and a group represented by the following general formula (2) is preferred. General formula (2):-(CO-X 1 )rX 2 - In general formula (2), X 1 is an oxygen atom or NR 30 - represents this. Here R 30 R represents a hydrogen atom, an alkyl group, an aryl group, or an acyl group, and each may have substituents (e.g., a halogen atom, a nitro group, and a hydroxyl group). 30 Preferred members are hydrogen atoms, C1-C10 alkyl groups (e.g., methyl group, ethyl group, n-butyl group, and n-octyl group), or acyl groups (e.g., acetyl group and benzoyl group). 1 As such, oxygen atoms or NH- are preferred. X 2 represents an alkylene group, arylene group, alkylene arylene group, arylene alkylene group, or alkylene arylene alkylene group, and these groups include -O-, -S-, -CO-, -COO-, -NH-, -SO2-, -N(R 31 )-, or -N(R 31 )SO2- etc. may be inserted in between. 31 X represents a linear or branched alkyl group having 1 to 6 carbon atoms. 2 Preferred members include dimethylene, trimethylene, tetramethylene, o-phenylene, m-phenylene, p-phenylene, -CH2CH2OCOCH2CH2-, or -CH2CH2OCO(C6H4)-. r represents either 0 or 1. q represents either 0 or 1, with 0 being preferred.
[0074] R 14 represents an alkyl group, an alkenyl group, or an alkynyl group, with alkyl groups having 5 to 50 carbon atoms being preferred, alkyl groups having 5 to 30 carbon atoms being more preferred, and alkyl groups having 5 to 20 carbon atoms being even more preferred. R 15 is a hydrogen atom, a methyl group, an ethyl group, a halogen atom, or -CH2COOR 16 It represents a hydrogen atom, a methyl group, a halogen atom, or -CH2COOR 16 Preferably, a hydrogen atom, a methyl group, or -CH2COOR 16 This is more preferable, and a hydrogen atom is even more preferable. R 16 R represents a hydrogen atom or an alkyl group having 1 to 80 carbon atoms. 14 It can be the same or different, R 16 The number of carbon atoms is preferably 1 to 70, and more preferably 1 to 60.
[0075] In general formula (1), x, y, z, and w represent the molar ratios of each repeating unit. x is 3 to 60 mol%, preferably 3 to 50 mol%, and more preferably 3 to 40 mol%. y is 30-96 mol%, preferably 35-95 mol%, and more preferably 40-90 mol%. z is 0.5 to 25 mol%, preferably 0.5 to 20 mol%, and more preferably 1 to 20 mol%. w is 0.5 to 40 mol%, and preferably 0.5 to 30 mol%. In general formula (1), it is preferable that x is 3-40 mol%, y is 40-90 mol%, z is 0.5-20 mol%, and w is 0.5-10 mol%.
[0076] As the polymer represented by general formula (1), the polymer represented by general formula (2) below is preferred.
[0077] [ka]
[0078] In general formula (2), x, y, z, and w are as defined above.
[0079] The polymer represented by general formula (1) may contain other repeating units other than those represented by general formulas (A) to (D) above. Examples of monomers for forming other repeating units include acrylic acid esters, methacrylic acid esters, vinyl esters, olefins, crotonic acid esters, itaconic acid diesters, maleic acid diesters, fumaric acid diesters, acrylamides, unsaturated carboxylic acids, allyl compounds, vinyl ethers, vinyl ketones, vinyl heterocyclic compounds, glycidyl esters, and unsaturated nitriles. These monomers are also described in paragraphs 0010 to 0022 of Japanese Patent No. 3754745. From the viewpoint of hydrophobicity, acrylic acid esters or methacrylic acid esters are preferred, and hydroxyalkyl methacrylate or hydroxyalkyl acrylate is more preferred. The polymer represented by general formula (1) preferably contains repeating units represented by general formula (E).
[0080] [ka]
[0081] In the above formula, L E represents an alkylene group, preferably an alkylene group having 1 to 10 carbon atoms, more preferably an alkylene group having 2 to 6 carbon atoms, and even more preferably an alkylene group having 2 to 4 carbon atoms.
[0082] Of the polymers represented by general formula (1), the polymer represented by general formula (3) below is particularly preferred.
[0083] [ka]
[0084] In the above formula, a1, b1, c1, d1, and e1 represent the molar ratio of each repeating unit, where a1 is 3-60 (mol%), b1 is 30-95 (mol%), c1 is 0.5-25 (mol%), d1 is 0.5-40 (mol%), and e1 is 1-10 (mol%). The preferred range for a1 is the same as the preferred range for x described above, the preferred range for b1 is the same as the preferred range for y described above, the preferred range for c1 is the same as the preferred range for z described above, and the preferred range for d1 is the same as the preferred range for w described above. e1 is 1 to 10 mol%, preferably 2 to 9 mol%, and more preferably 2 to 8 mol%.
[0085] Specific polymers can be synthesized by referring, for example, to Japanese Patent Publication No. 3305459 and Japanese Patent Publication No. 3754745. The weight-average molecular weight of the specific polymer is not particularly limited, but is preferably 1,000 to 1,000,000, more preferably 2,000 to 750,000, and even more preferably 3,000 to 500,000.
[0086] (Other materials) The photosensitive layer may contain other materials besides those described above, if necessary. Other materials include, for example, metal compounds belonging to Group 8 or 9, such as rhodium compounds and iridium compounds, which are used to stabilize and increase the sensitivity of silver halides. Other materials include antistatic agents, nucleation accelerators, spectral sensitizing dyes, surfactants, anti-fogging agents, hardening agents, black spot inhibitors, redox compounds, monomethine compounds, and dihydroxybenzenes, as described in paragraphs
[0220] to
[0241] of Japanese Patent Publication No. 2009-004348. In photographic manufacturing, when using method (b) above, other materials may include physical developing nuclei. Examples of materials for physical developing nuclei include colloids such as gold and silver, and metal sulfides obtained by mixing water-soluble salts such as palladium and zinc with sulfides.
[0087] Furthermore, the photosensitive layer may contain a crosslinking agent used to crosslink the specific polymers mentioned above. The inclusion of the crosslinking agent promotes crosslinking between the specific polymers, and even when the gelatin is decomposed and removed, the linkage between the metallic silver particles in the layer formed by the photosensitive layer is maintained.
[0088] Furthermore, when using the method described in (b) above in the photographic manufacturing process, a physical development nucleus layer containing physical development nuclei may be provided between the substrate and the photosensitive layer. The physical development nuclei contained in the physical development nucleus layer are as described above. For information on how to form the physical development nucleus layer, refer to paragraphs
[0007] to
[0016] of Japanese Patent Publication No. 5-265162.
[0089] (Step B procedure) The method for forming the photosensitive layer containing the above-mentioned components in step B is not particularly limited, but from the viewpoint of productivity, a method is preferred in which a photosensitive layer-forming composition containing silver halide, gelatin, and a specific polymer is brought into contact with the surface of the silver halide-free layer, and the photosensitive layer is formed on the silver halide-free layer. The form of the photosensitive layer-forming composition used in this method will be described in detail below, followed by a detailed description of the process steps.
[0090] (Materials included in photosensitive layer-forming compositions) The photosensitive layer-forming composition includes the aforementioned silver halide, gelatin, and a specific polymer. If necessary, the specific polymer may be included in the photosensitive layer-forming composition in particulate form. The photosensitive layer-forming composition may optionally contain a solvent. Examples of solvents include water, organic solvents (e.g., alcohols, ketones, amides, sulfoxides, esters, and ethers), ionic liquids, and mixtures thereof.
[0091] The method for bringing the photosensitive layer-forming composition into contact with the surface of the silver halide-free layer is not particularly limited. Examples include applying the photosensitive layer-forming composition to the surface of the silver halide-free layer, and immersing a substrate with a silver halide-free layer in the photosensitive layer-forming composition. When forming a photosensitive layer by applying the photosensitive layer-forming composition, it may be applied to both surfaces simultaneously, or it may be applied to one surface first and then to the other surface. Furthermore, if necessary, drying may be performed after the above-mentioned processing.
[0092] (Silver halide-containing photosensitive layer) The photosensitive layer (silver halide-containing photosensitive layer) formed by the above procedure contains silver halide, gelatin, and a specific polymer. The content of silver halide in the photosensitive layer is not particularly limited, but in the exposure process described later, it functions as a self-aligning mask pattern and suppresses variations in the line width of the fine metal lines formed after the development process described later. Therefore, a silver equivalent of 1.0 to 10.0 g / m² is recommended. 2 Preferably, 2.0 to 7.0 g / m 2 This is more preferable. "Silver equivalent" means converting to the mass of silver produced when all the silver halides are reduced. The content of specific polymers in the photosensitive layer is not particularly limited, but 0.04 to 2.0 g / m² is preferable in terms of superior formation of the upper conductive layer on the metal nanowire and the flexibility of the conductive nanowire. 2 Preferably, 0.08 to 1.0 g / m 2 This is preferable. The composition and physical properties of the photosensitive layers formed on both sides of the substrate may be the same or different.
[0093] Steps A and B described above may be carried out simultaneously by simultaneous multi-layer coating. That is, the silver halide-free layer-forming composition and the photosensitive layer-forming composition may be applied to the surface of the substrate to simultaneously form the silver halide-free layer and the photosensitive layer in order from the surface side of the substrate.
[0094] -Process C- Step C is a process in which the photosensitive layer is exposed and then developed to form a fine, wire-like silver-containing layer containing metallic silver, gelatin, and a specific polymer.
[0095] By applying an exposure treatment to the photosensitive layer, a latent image is formed in the exposed area. Exposure may be performed in a pattern. For example, to obtain a mesh pattern consisting of conductive fine wires as described later, methods include exposure through a mask having a mesh-like aperture pattern, and exposure in a mesh pattern by scanning with laser light. The type of light used during exposure is not particularly limited; any light capable of forming a latent image in silver halide is acceptable, such as visible light, ultraviolet light, and X-rays. The exposure process may be performed simultaneously on the photosensitive layers on both sides of the substrate, or one photosensitive layer may be exposed first, followed by the other photosensitive layer.
[0096] By developing the exposed photosensitive layer, metallic silver is deposited in the exposed area (the area where the latent image is formed). The development process is not particularly limited and includes known methods used for silver halide photographic film, photographic paper, printing platemaking film, and emulsion masks for photomasks. In the developing process, a developer is typically used. The type of developer is not particularly limited, and examples include PQ (phenidone hydroquinone) developer, MQ (methol hydroquinone) developer, and MAA (methol ascorbic acid) developer. The developability of a photosensitive layer is determined by the wavelength and intensity of the light source, as well as the sensitivity characteristics of the photosensitive layer.
[0097] Step C may further include a fixing process performed for the purpose of removing and stabilizing the unexposed silver halide. Fixing is performed simultaneously with and / or after development. The fixing method is not particularly limited and includes, for example, methods used for silver halide photographic film, photographic paper, printing plate film, and emulsion masks for photomasks. Fixing typically involves the use of a fixing solution. The type of fixing solution is not particularly limited; for example, the fixing solutions described on page 321 of "The Chemistry of Photography" (by Sasai, Photo Industry Publishing Co., Ltd.) are examples.
[0098] By performing the above-described process, a fine, wire-like silver-containing layer is formed, which contains metallic silver, gelatin, and a specific polymer. One method for adjusting the width of the silver-containing layer is to adjust the aperture width of the mask used during exposure. Furthermore, when using a mask during exposure, the width of the formed silver-containing layer can be adjusted by adjusting the exposure amount. For example, if the aperture width of the mask is narrower than the target width of the silver-containing layer, the width of the region where the latent image is formed can be adjusted by increasing the exposure amount. In other words, the line width of the silver-containing layer and the formed conductive nanowire can be adjusted by the exposure amount. Furthermore, when using laser light, the exposure area can be adjusted by adjusting the focusing range and / or scanning range of the laser light.
[0099] The width of the silver-containing layer is adjusted as appropriate according to the wire width w2 of the target second metal nanowire and the wire width w1 of the first metal nanowire, but is preferably less than 5.0 μm, more preferably 3.0 μm or less, and even more preferably 2.0 μm or less. There is no particular lower limit, but is preferably 0.1 μm or more, and more preferably 0.5 μm or more. Furthermore, the silver-containing layer obtained by the procedure described above is in the form of a fine wire, and the width of the silver-containing layer refers to the length (width) of the silver-containing layer in a direction perpendicular to the direction in which the fine wire-like silver-containing layer extends.
[0100] -Process D- Step D is a process in which the silver-containing layer obtained in step C is subjected to heat treatment. By performing this step, fusion between specific polymers in the silver-containing layer is promoted, and the strength of the silver-containing layer is improved.
[0101] The method of heat treatment is not particularly limited, and examples include contacting the silver-containing layer with superheated steam and heating with a temperature control device (e.g., a heater), with the method of contacting the silver-containing layer with superheated steam being preferred.
[0102] The superheated steam can be superheated water steam or a mixture of superheated water steam and other gases. The contact time between the superheated steam and the silver-containing layer is not particularly limited, but 10 to 70 seconds is preferred. The supply rate of superheated steam is 500-600 g / m³. 3 Preferably, the superheated steam temperature is 100 to 160°C (preferably 100 to 120°C) at 1 atmosphere.
[0103] In the method of heating the silver-containing layer with a temperature control device, the preferred heating conditions are 100 to 200°C (preferably 100 to 150°C) for 1 to 240 minutes (preferably 60 to 150 minutes).
[0104] -Process E- Step E is a step to remove gelatin from the silver-containing layer obtained in step D. By performing this step, gelatin is removed from the silver-containing layer, and a space is formed within the silver-containing layer.
[0105] The method for removing gelatin is not particularly limited and includes, for example, a method using a proteolytic enzyme (hereinafter also referred to as "Method 1") and a method of decomposing and removing gelatin using an oxidizing agent (hereinafter also referred to as "Method 2").
[0106] The proteolytic enzyme used in Method 1 is a known plant or animal enzyme capable of hydrolyzing proteins such as gelatin. Examples of proteolytic enzymes include pepsin, rennin, trypsin, chymotrypsin, cathepsin, papain, ficin, thrombin, renin, collagenase, bromelain, and bacterial proteases, with trypsin, papain, ficin, or bacterial proteases being preferred. The procedure in Method 1 can be any method of bringing the silver-containing layer into contact with the proteolytic enzyme described above. For example, this could involve bringing the silver-containing layer into contact with a treatment solution containing the proteolytic enzyme (hereinafter also referred to as the "enzyme solution"). Methods of contact include immersing the silver-containing layer in the enzyme solution and applying the enzyme solution onto the silver-containing layer. The amount of proteolytic enzyme in the enzyme solution is not particularly limited, but it is preferably 0.05 to 20% by mass, and more preferably 0.5 to 10% by mass, relative to the total amount of the enzyme solution, as this allows for easy control of the degree of gelatin degradation and removal. Enzyme solutions often contain water in addition to the protein-digesting enzymes mentioned above. The enzyme solution may contain other additives as needed (e.g., pH buffers, antimicrobial compounds, wetting agents, and preservatives). The pH of the enzyme solution is chosen to maximize the enzyme's activity, but generally, a range of 5 to 9 is preferred. The enzyme solution should ideally be at a temperature that enhances enzyme activity. Specifically, 25-45°C is preferred.
[0107] If necessary, a washing process may be performed after treatment with the enzyme solution, in which the resulting silver-containing layer is washed with warm water. The cleaning method is not particularly limited, but a method of bringing the silver-containing layer into contact with hot water is preferred. Examples include immersing the silver-containing layer in hot water and applying hot water to the silver-containing layer. The temperature of the hot water is appropriately selected according to the type of proteolytic enzyme used, and from the standpoint of productivity, 20 to 80°C is preferred, and 40 to 60°C is more preferred. The contact time (washing time) between the hot water and the silver-containing layer is not particularly limited, but from a productivity standpoint, 1 to 600 seconds is preferred, and 30 to 360 seconds is more preferred.
[0108] The oxidizing agent used in Method 2 can be any oxidizing agent capable of decomposing gelatin, and an oxidizing agent with a standard electrode potential of +1.5V or higher is preferred. Here, the standard electrode potential refers to the standard electrode potential of the oxidizing agent in an aqueous solution relative to a standard hydrogen electrode (at 25°C, E0 ) is intended. Examples of the oxidizing agents mentioned above include persulfuric acid, percarbonate, superphosphate, hypoperchloric acid, peracetic acid, metachloroperbenzoic acid, hydrogen peroxide, perchloric acid, periodic acid, potassium permanganate, ammonium persulfate, ozone, hypochlorous acid or its salts. However, from the viewpoint of productivity and economic efficiency, hydrogen peroxide (standard electrode potential: 1.76V), hypochlorous acid or its salts are preferred, and sodium hypochlorite is more preferred.
[0109] The procedure in Method 2 may involve any method of bringing the silver-containing layer into contact with the oxidizing agent described above. For example, this could involve bringing the silver-containing layer into contact with a treatment solution containing the oxidizing agent (hereinafter also referred to as the "oxidizing agent solution"). Methods of contact include immersing the silver-containing layer in the oxidizing agent solution and applying the oxidizing agent solution onto the silver-containing layer. The type of solvent included in the oxidizing agent solution is not particularly limited, and examples include water and organic solvents.
[0110] -Process F- The manufacturing method for the precursor laminate may include a step F in which a smoothing treatment is performed after step E. By performing step F, a conductive nanowire with superior handling resistance (film strength) can be obtained. The method of smoothing is not particularly limited, but a calendering process is preferred in which a substrate having a silver-containing layer is passed between at least one pair of rolls under pressure. Hereinafter, the smoothing process using calendering rolls will be referred to as calendering. Examples of rolls used in calendering include plastic rolls and metal rolls, with plastic rolls being preferred from the standpoint of preventing wrinkles. The pressure between the rolls is not particularly limited, but is preferably 2 MPa or higher, more preferably 4 MPa or higher, and preferably 120 MPa or lower. The pressure between the rolls can be measured using a Fujifilm Prescale (for high pressure). The temperature for the smoothing process is not particularly limited, but is preferably 10 to 100°C, and more preferably 10 to 50°C.
[0111] [Laminate containing resist pattern] The resist pattern-containing laminate produced by this manufacturing method comprises at least a substrate, a first metal pattern disposed on one surface side of the substrate and composed of first metal nanowires, a first resist pattern disposed on one surface side of the substrate and in a region where the first metal nanowires are not disposed, and a second metal pattern disposed on the other surface side of the substrate and composed of second metal nanowires. The resist pattern-containing laminate produced by this manufacturing method has the function of a conductive film.
[0112] An example of the configuration of a resist pattern-containing laminate is the laminate 13 shown in Figure 3, which has already been described. The resist pattern-containing laminate produced by this manufacturing method is not limited to the embodiment shown in Figure 3, and may have components other than the substrate, the first metal pattern, the first resist pattern, and the second metal pattern.
[0113] <Second Resist Pattern> The resist pattern-containing laminate may, for example, have a second resist pattern located on the other surface side of the substrate, in an area where the second conductive nanowire is not located. Figure 6 shows another example of the configuration of a resist pattern-containing laminate manufactured by this manufacturing method. The laminate (resist pattern-containing laminate) 16 shown in Figure 6 comprises a substrate 20, a first metal nanowire 31 disposed on one surface 21 of the substrate 20, a first resist pattern 43 disposed on one surface 21 of the substrate and in an area where the first metal nanowire 31 is not disposed, a second metal nanowire 32 disposed on the other surface 22 of the substrate 20, and a second resist pattern 53 disposed on the other surface 22 of the substrate and in an area where the second metal nanowire 32 is not disposed.
[0114] In the laminate 16 shown in Figure 6, the substrate 20, the first metal nanowire 31, the second metal nanowire 32, and the first resist pattern 43 are the same as those in the laminate 13 shown in Figure 3. Furthermore, the second resist pattern 53 of the laminate 16 has the same configuration as the first resist pattern 43, except that it is located on the other surface 22 side of the substrate in an area where the second metal wire 32 is not arranged, and the preferred embodiment is also the same.
[0115] The method for forming the second resist pattern is not particularly limited and can be formed, for example, by performing the same steps as in the first resist pattern formation step. That is, the second resist pattern can be formed by forming a second resist film on the other surface side of the substrate in the precursor laminate according to the method described in the resist film formation step, exposing the second resist film by irradiating light from one surface side of the substrate according to the method described in the exposure step, and developing the exposed second resist film according to the method described in the development step. Preferred embodiments of each step, the precursor laminate, and the resist film are also the same as preferred embodiments in the first resist pattern formation step.
[0116] <Upper conductive layer> Furthermore, the resist pattern-containing laminate may have an upper conductive layer containing a conductive material such as metal, which is disposed on the surface side of at least one of the first metal pattern composed of first metal nanowires and the second metal pattern composed of second metal nanowires. In a resist pattern-containing laminate, the upper conductive layer is arranged on a metal nanowire (metal pattern), and a conductive nanowire consisting of a laminated structure including the metal nanowire and the upper conductive layer is formed, thereby allowing the resist pattern-containing laminate to be used as a conductive film with superior conductivity.
[0117] Figure 7 shows another example of the configuration of a resist pattern-containing laminate manufactured by this manufacturing method. The laminate (resist pattern-containing laminate) 1 shown in Figure 7 comprises a substrate 20, a first metal nanowire 31 disposed on one surface 21 of the substrate 20, an upper conductive layer 61 disposed on the first metal nanowire 31, a first resist pattern 43 disposed on one surface 21 of the substrate and in an area where the first metal nanowire 31 is not disposed, a second metal nanowire 32 disposed on the other surface 22 of the substrate 20, an upper conductive layer 62 disposed on the second metal nanowire 32, and a second resist pattern 53 disposed on the other surface 22 of the substrate and in an area where the second metal nanowire 32 is not disposed. In the laminate 1 shown in Figure 7, the substrate 20, the first metal nanowire 31, the second metal nanowire 32, the first resist pattern 43, and the second resist pattern 53 are the same as those in the laminate 16 shown in Figure 6.
[0118] The resist pattern-containing laminate having an upper conductive layer is not limited to the configuration shown in Figure 7, and the upper conductive layer may be arranged only on one surface side of the first metal nanowire (first metal pattern) and the second metal nanowire (second metal pattern). It is more preferable to have an upper conductive layer on the surface side of both the first and second metal nanowires in terms of superior conductivity. Furthermore, in a resist pattern-containing laminate, it is preferable that the upper conductive layer is not located in a region on the surface side of the substrate where metal nanowires are not arranged, i.e., in a region where the first resist pattern or the second resist pattern is arranged. In this case, the conductive nanowire, which consists of a laminated structure including metal nanowires and an upper conductive layer, forms a conductive pattern having a pattern shape similar to that of the metal pattern formed by the metal nanowires. The pattern shape of the conductive pattern consisting of conductive fine wires may be the same as the pattern shape of the metal pattern, including in preferred embodiments.
[0119] The upper conductive layer contains a conductive material such as a metal, and preferably contains a metal. Examples of metals included in the upper conductive layer include individual metals selected from the group consisting of silver, copper, gold, nickel, cobalt, and palladium, as well as mixtures (alloys) of two or more metals selected from the above group. Among these, at least one of silver and copper is preferred in terms of superior conductivity, with elemental silver or an alloy of silver and copper being more preferred, and elemental silver being even more preferred.
[0120] The upper conductive layer preferably contains metal as its main component. The statement that the upper conductive layer "contains metal as a main component" means that the metal content is 50% by mass or more of the total mass of the upper conductive layer. Preferably, the metal content in the upper conductive layer is 90% by mass or more, and more preferably 95% by mass or more, of the total mass of the upper conductive layer. There is no particular upper limit, and it may be 100% by mass of the total mass of the upper conductive layer.
[0121] The resist pattern-containing laminate may have a blackened layer as the conductive layer furthest from the substrate among the conductive layers constituting the upper conductive layer. The blackened layer has the function of preventing light reflection on the surface of the conductive fine wire and further improving visibility. Examples of known black plating layers include a black chromium plating layer, a black nickel plating layer, and a black anodized aluminum plating layer. These blackened layers can be formed by a plating process using known black metallic materials.
[0122] The line width of the upper conductive layer is preferably 5.0 μm or less, more preferably 3.0 μm or less, and even more preferably 2.0 μm or less, in such a way that the conductive fine wires are not easily visible. There is no particular lower limit, but in such a way that conductivity is better, it is preferably 0.1 μm or more, and more preferably 0.5 μm or more. The height of the upper conductive layer is preferably 1.0 μm or more, and more preferably 2.0 μm or more, in terms of superior conductivity. There is no particular upper limit, but it is preferably 20.0 μm or less, and more preferably 10.0 μm or less, in terms of the conductivity of the conductive wires being less visible and the flexibility of the conductive film being superior. The wire width and height of the upper conductive layer can be measured by performing the same measurement method as the method for measuring the wire width and thickness of the fine metal wire described above.
[0123] The resist pattern-containing laminate preferably has a conductive pattern on at least one surface side of the substrate, composed of conductive nanowires having a laminated structure including a metal nanowire and an upper conductive layer; more preferably has a first conductive pattern on one surface side of the substrate, composed of a first conductive nanowire having a laminated structure including a first metal nanowire and an upper conductive layer, and a second conductive pattern on the other surface side of the substrate, composed of a second conductive nanowire having a laminated structure including a second metal nanowire and an upper conductive layer.
[0124] <Conductive thin wire formation process> The method for obtaining a conductive nanowire by forming an upper conductive layer on the surface side of a metal nanowire is not particularly limited as long as it is a method that can form a conductive nanowire by laminating a conductive material such as metal on the surface side of a metal nanowire, but a method of forming a plated metal layer by plating is preferred. In other words, the present manufacturing method may further include a conductive wire formation step in which, after forming a resist pattern according to the method described in the development step above, an upper conductive layer is formed on a metal wire exposed at the openings of the obtained resist pattern to obtain a conductive wire. Preferably, in the conductive wire formation step, a plating treatment is performed on the metal wire as a seed layer to form a plated metal layer as an upper conductive layer on the metal wire.
[0125] The plating method is not particularly limited and may be electroless plating (chemical reduction plating, displacement plating, etc.) or electroplating, but electroless plating is preferred. Known electroless plating techniques can be used as the electroless plating treatment. Examples of plating treatments include silver plating, copper plating, nickel plating, and cobalt plating. Silver plating or copper plating is preferred, and silver plating is more preferred, as it provides superior conductivity to the conductive fine wires.
[0126] The components contained in the plating solution used in the plating process are not particularly limited, but typically, in addition to a solvent (e.g., water), it mainly contains: 1. metal ions for plating, 2. a reducing agent, 3. an additive (stabilizer) to improve the stability of the metal ions, and 4. a pH adjuster. In addition to these, the plating solution may also contain known additives such as a stabilizer for the plating solution. The type of metal ions used for plating contained in the plating solution can be appropriately selected depending on the type of metal to be deposited. Examples include silver ions, copper ions, nickel ions, and cobalt ions. A commercially available plating solution may be used.
[0127] The plating procedure described above is not particularly limited and any method of bringing the metal pattern into contact with the plating solution is acceptable. Examples include immersing the metal pattern in the plating solution and applying the plating solution to the metal pattern. The contact time between the metal pattern and the plating solution is not particularly limited, but 20 seconds to 30 minutes is preferred from the standpoint of achieving better conductivity for conductive fine wires and productivity.
[0128] When forming a conductive nanowire having a blackened layer at the position furthest from the substrate, the blackened layer can be formed by performing a plating treatment using the blackened metal material described above during the conductive nanowire formation process.
[0129] Furthermore, after the conductive nanowire formation process, a heat treatment may be applied. By applying the heat treatment, a conductive nanowire with superior conductivity can be obtained. The method for applying the heat treatment to the conductive nanowire is not particularly limited, and the method described in step D above is one example.
[0130] <Conductive film> As described above, the resist pattern-containing laminate produced by this manufacturing method can be suitably used as a conductive film. In particular, a conductive film in which the first resist pattern and the second resist pattern function as an insulating film is preferred.
[0131] As an example of a preferred embodiment of a conductive film made of a resist pattern-containing laminate manufactured by this manufacturing method, a conductive film is provided which comprises a substrate, a first conductive nanowire disposed on one surface side of the substrate, a first insulating film disposed on one surface side of the substrate and in a region where the first conductive nanowire is not disposed, a second conductive nanowire disposed on the other surface side of the substrate, and a second insulating film disposed on the other surface side of the substrate and in a region where the second conductive nanowire is not disposed, wherein the line width v2 of the second conductive nanowire and the thickness d of the substrate satisfy the relationship of formula (X2). Formula (X2) d / v2≧3.0
[0132] In the conductive film, the ratio d / v2 of the thickness d of the substrate to the width v2 of the second conductive fine wire is preferably 5.0 or greater, and more preferably 15.0 or greater, in terms of achieving superior effects of the present invention. There is no particular upper limit, but it is preferably 300.0 or less, and more preferably 150.0 or less.
[0133] Furthermore, in the conductive film, the line width v1 of the first conductive nanowire and the thickness d of the substrate are preferably such that the conductive film is obtained in which back reflection by the first metal nanowire in the second insulating film is suppressed, and the following formula (X1) is satisfied. Formula (X1) d / v1≧3.0 Furthermore, the ratio d / v1 of the thickness d of the substrate to the width v1 of the first conductive nanowire is more preferably 5.0 or greater, and even more preferably 15.0 or greater. There is no particular upper limit, but it is preferably 300.0 or less, and more preferably 150.0 or less.
[0134] The wire width v2 of the second conductive nanowire is not particularly limited as long as the relationship of formula (X2) above is satisfied, but for example it is 5.0 μm or less, more preferably 3.0 μm or less, and even more preferably 2.0 μm or less, in that the conductive nanowire is difficult to see. The lower limit is not particularly limited, but 0.1 μm or more is preferred, and 0.5 μm or more is more preferred in that conductivity is better.
[0135] The height h2 of the second conductive nanowire is not particularly limited, but is preferably 1.0 μm or more, and more preferably 2.0 μm or more, in terms of superior conductivity. The upper limit is not particularly limited, but is preferably 20.0 μm or less, and more preferably 10.0 μm or less, in terms of the conductivity of the conductive nanowire being less visible and the flexibility of the conductive film being superior.
[0136] Furthermore, in terms of superior conductivity, the ratio of the height h2 of the second conductive nanowire to the width v2 of the second conductive nanowire, h2 / v2, is preferably 1.0 or greater, more preferably 2.0 or greater, and even more preferably 2.5 or greater. There is no particular upper limit, but in terms of making the conductive nanowire less visible and the flexibility of the conductive film better, it is preferably 20.0 or less, and more preferably 10.0 or less. In other words, it is more preferable that the height h2 of the second conductive nanowire and the width v2 of the second conductive nanowire satisfy the relationship shown in the following equation (Y2). Formula (Y2) h2 / v2≧2.0
[0137] Preferred embodiments of the line width v1 and height h1 of the first conductive nanowire, and the ratio h1 / v1 of the height h1 of the first conductive nanowire to the line width v1 of the first conductive nanowire, are the same as preferred embodiments of the first conductive nanowire. In particular, it is more preferable that the height h1 of the first conductive nanowire and the width v1 of the first conductive nanowire satisfy the relationship given by the following equation (Y1). Formula (Y1) h1 / v1≧2.0
[0138] The wire width and height of the conductive nanowire can be measured by the same measurement method as the method for measuring the wire width and thickness of the metal nanowire described above. A more detailed measurement method will be described in the examples below. The height of the conductive nanowire is the sum of the thickness of the metal nanowire and the height of the upper conductive layer. The wire width and height of the conductive nanowire can be adjusted by the wire width of the metal nanowire, the thickness of the resist pattern (resist film), and the plating time in the conductive nanowire formation process.
[0139] Furthermore, another example of a preferred embodiment of a conductive film comprising a resist pattern-containing laminate manufactured by this manufacturing method is a conductive film having a substrate, a first conductive nanowire disposed on one surface side of the substrate, a first insulating film disposed on one surface side of the substrate and in a region where the first conductive nanowire is not disposed, and a second metal pattern disposed on the other surface side of the substrate and composed of second metal nanowires, wherein the line width w2 of the second metal nanowire and the thickness d of the substrate satisfy the following equation (1). Formula (1) d / w2≧3.0 Preferred embodiments of the first conductive nanowire, first insulating film, second metal nanowire, and second metal pattern provided in the conductive film described above have already been explained.
[0140] In conductive nanowires of a conductive film, it is preferable that the metal density of the lower region on the substrate side is lower than the metal density of the upper region other than the lower region of the conductive nanowire. When conductive nanowires have a lower metal density in the lower region and a higher metal density in the upper region, the bending resistance of the conductive film can be improved. Note that the above-mentioned metal density refers to the weight of metal contained in a unit volume of conductive nanowire.
[0141] For conductive nanowires in which the metal density of the lower region is lower than that of the upper region, examples include a method in which a metal nanowire is formed by carrying out steps B to E in that order, and then forming the upper conductive layer by a plating process, and a method in which a metal nanowire is formed using a metal with a lower density (such as copper and copper alloys), and the upper conductive layer is formed using a metal with a higher density (such as pure silver).
[0142] The metal density of conductive nanowires contained in a conductive film can be determined, for example, by measuring the relative metal content in the cross-section of the conductive nanowire using time-of-flight secondary ion mass spectrometry (TOF-SIMS). By measuring the metal density of the conductive nanowire described above, it is possible to distinguish between the upper and lower regions of the conductive nanowire.
[0143] Specifically, a conductive film is cut along a direction intersecting the extension direction of the conductive nanowire using a microtome or similar instrument, and the local concentration of metal at the cut surface of the resulting conductive nanowire is analyzed using the TOF-SIMS method. The TOF-SIMS method is Ga + and In + This method measures the amount of compounds present on the surface of a solid sample by detecting secondary ions such as molecular ions and fragment ions emitted from molecules in the sample upon irradiation with primary ions. While both positive and negative ions can be detected by the TOF-SIMS method, in this embodiment, positive ions are selected, and the entire secondary ion image with masses from 0 to 1000 amu (atom mass units) is measured in raw data format in the same region of the cross-section of a conductive nanowire. It is preferable to use an electron gun (flood gun) to neutralize the charge buildup on the sample surface during measurement. When analyzing the local concentration of conductive nanowires, the cross-section of the conductive nanowire is divided into fine regions (apertures) with a diameter of approximately 10 to 50 nm, and the signal intensity originating from the metal is measured within these aperture sizes. By mapping the measured signal intensity originating from the metal in these fine regions across the entire cross-section of the conductive nanowire, a compositional distribution is obtained that shows the relative local concentrations of the metal present at each position on the cross-section of the conductive nanowire, with the thickness and width directions as coordinates. Based on the differences in local concentrations of metals shown in the obtained composition distribution, the lower and upper regions of the conductive nanowire can be distinguished. Furthermore, when the thickness of the conductive nanowire is thin (for example, several times the thickness of the aperture), it is preferable to increase the resolution of mapping within the conductive nanowire by changing the cutting direction of the conductive film from the normal direction to the main surface of the conductive film (90°) to an oblique direction (1 to less than 90° to the main surface of the conductive film) to increase the area of the cut surface. Furthermore, if the conductive nanowire contains multiple types of metals, the local concentration of each metal can be measured using the TOF-SIMS method, and the sum of the local concentrations of each metal can be calculated to distinguish between the lower and upper regions.
[0144] The first insulating film and the second insulating film of the conductive film are preferably transparent. In this specification, "transparent" means that the average transmittance of visible light with wavelengths of 400 to 700 nm is 80% or higher. The average transmittance of the insulating film with visible light is preferably 90% or higher. There is no particular upper limit, for example, 99% or less. The transmittance can be measured using a spectrophotometer.
[0145] The resist pattern-containing laminate and conductive film produced by this manufacturing method may have other components besides the above-mentioned substrate, conductive nanowires (metal nanowires and upper conductive layer), and insulating film. Other components that the resist pattern-containing laminate and conductive film may have include, for example, conductive parts with a different configuration from conductive nanowires.
[0146] The following describes specific embodiments of this manufacturing method with reference to the drawings. However, this manufacturing method, the resist pattern-containing laminate produced by this manufacturing method, and the conductive film are not limited to the specific embodiments described below.
[0147] [First Embodiment] The method for manufacturing a resist pattern-containing laminate according to the first embodiment comprises at least steps (1-1) to (1-5). (1-1) A first exposure step in which a laminate having a second metal pattern, a substrate, a first metal pattern, and a first resist film in this order is exposed by irradiating light from the other surface side of the substrate. (1-2) A first development step in which the exposed first resist film is developed to form a first resist pattern. (1-3) A second resist film formation step, in which a second resist film is formed on the other surface side of the substrate (the surface side on which the second metal pattern is arranged) after the first development step (1-2). (1-4) A second exposure step in which the second resist film is exposed by irradiating it with light from one surface side of the substrate, i.e., the surface side on which the first metal pattern is arranged. (1-5) A second development step in which the exposed second resist film is developed to form a second resist pattern and obtain a laminate containing the resist pattern.
[0148] The manufacturing method according to this embodiment preferably includes the following first resist film formation step (1-0) before step (1-1). (1-0) A first resist film forming step to obtain a laminate, in which a first resist film is formed on the surface side of the substrate on which the first metal pattern is arranged, in a precursor laminate having a second metal pattern, a substrate and a first metal pattern in this order.
[0149] Furthermore, the manufacturing method according to this embodiment preferably includes the following conductive nanowire forming step (1-6) after step (1-5). (1-6) Conductive wire forming step of forming an upper conductive layer on a first metal nanowire exposed at an opening in a first resist pattern and on a second metal nanowire exposed at an opening in a second resist pattern to obtain a first conductive nanowire and a second conductive nanowire. In other words, the manufacturing method according to this embodiment is more preferably to include the above steps (1-0) to (1-6).
[0150] The manufacturing method of this embodiment, which has the above steps (1-0) to (1-6) in this order, will be described with reference to the drawings. Here, Figure 8 is a diagram illustrating the manufacturing method of this embodiment. Figure 8(a) is a diagram illustrating the second resist film formation step (1-3), and Figure 8(b) is a diagram illustrating the second development step (1-4).
[0151] In the first resist film formation step (1-0), the first resist film 40 is formed on one surface 21 of the substrate 20 of the precursor laminate 10 shown in Figure 5, and the laminate 11 shown in Figure 1 is obtained. In the first exposure step (1-1), light is irradiated onto the laminate 11 shown in Figure 1 from the other surface 22 side of the substrate 20, and the first resist film 40 is exposed, resulting in the laminate 12 shown in Figure 2. In the first development step (1-2), the laminate 12 shown in Figure 2 is subjected to a development process, and the unexposed portion 42 of the first resist film 40 is removed, thereby obtaining the laminate 13 shown in Figure 3.
[0152] In the second resist film formation step (1-3), the second resist film 50 is formed on the laminate 13 shown in Figure 3 so as to cover the other surface 22 side of the substrate 20 where the second metal nanowire 32 is located, and the laminate 14 shown in Figure 8(a) is obtained. The laminate (resist pattern-containing laminate) 14 shown in Figure 8(a) comprises a substrate 20, a first metal nanowire 31 disposed on one surface 21 of the substrate 20, a first resist pattern 43 disposed on one surface 21 of the substrate and in an area where the first metal nanowire 31 is not disposed, a second metal nanowire 32 disposed on the other surface 22 of the substrate 20, and a second resist film 50 disposed on the second metal nanowire 32.
[0153] In the second exposure step (1-4), light is irradiated onto the laminate 14 shown in Figure 8(a) from one surface 21 of the substrate 20, exposing the second resist film 50, and the laminate (resist pattern-containing laminate) 15 shown in Figure 8(b) is obtained. The laminate (resist pattern-containing laminate) 15 shown in Figure 8(b) comprises a substrate 20, a first metal nanowire 31 disposed on one surface 21 of the substrate 20, a first resist pattern 43 disposed on one surface 21 of the substrate and in an area where the first metal nanowire 31 is not disposed, a second metal nanowire 32 disposed on the other surface 22 of the substrate 20, and exposed portions 51 and unexposed portions 52 of a second resist film 50 (see Figure 8(a)) disposed on the second metal nanowire 32. In this way, the second exposure step (1-4) results in an exposed area 51 on the other surface 22 where the second metal nanowires 32 are not present, and an unexposed area 52 on the area where the second metal nanowires 32 are present. In this manner, the second metal pattern composed of the second metal nanowires 32 functions as a mask for the second resist film 50, and exposed areas 51 and unexposed areas 52 with shapes corresponding to the second metal pattern are formed.
[0154] In the second development step (1-5), the unexposed portion 52 of the laminate 15 shown in Figure 8(b) is removed, and a second resist pattern 53 is formed that covers only the area where the second metal nanowire 32 is not placed, resulting in the laminate 16 shown in Figure 6. The portion occupied by the unexposed portion 52 of the laminate 15, that is, the area on the other surface 22 of the substrate 20 where the second metal nanowire 32 is placed, becomes an opening 54 in the laminate 16. In the conductive nanowire formation process (1-6), upper conductive layers 61 and 62 are formed in the openings 44 and 54 of the laminate 16 shown in Figure 6, respectively, to obtain the resist pattern-containing laminate 1 (conductive film) shown in Figure 7.
[0155] [Second Embodiment] The method for manufacturing a resist pattern-containing laminate according to the second embodiment comprises the following steps (2-0) to (2-6). (2-0) A second resist film forming step to obtain a laminate, in which a second resist film is formed on the surface side of the substrate on which the second metal pattern is arranged, in a precursor laminate having a second metal pattern, a substrate and a first metal pattern in this order. (2-1) A second exposure step in which the second resist film is exposed by irradiating it with light from one surface side of the substrate. (2-2) A second development step in which the exposed second resist film is developed to form a second resist pattern and obtain a resist pattern-containing laminate. (2-3) A first resist film formation step in which a first resist film is formed on one surface side of the substrate after the second development step (2-2). (2-4) A first exposure step in which the first resist film is exposed by irradiating it with light from the other surface side of the substrate. (2-5) A first development step in which the exposed first resist film is developed to form a first resist pattern. (2-6) Conductive wire forming step of forming an upper conductive layer on a first metal nanowire exposed at an opening in a first resist pattern and on a second metal nanowire exposed at an opening in a second resist pattern to obtain a first conductive nanowire and a second conductive nanowire.
[0156] The manufacturing method of this embodiment, which has the above steps (2-0) to (2-6) in this order, will be described with reference to the drawings. Figures 9 and 10 are diagrams illustrating the manufacturing method of this embodiment. Figure 9(a) is a diagram illustrating the second resist film formation step (2-0), Figure 9(b) is a diagram illustrating the second exposure step (2-1), and Figure 9(c) is a diagram illustrating the second development step (2-2). Furthermore, Figure 10(a) is a diagram illustrating the first resist film formation step (2-3), and Figure 10(b) is a diagram illustrating the first exposure step (2-4). The components in Figures 9 and 10 are the same as the components with the same reference numerals in Figures 1-3 and 4-8; therefore, descriptions of each component are omitted.
[0157] In the second resist film formation step (2-0), the second resist film 50 is formed on the other surface 22 side of the substrate 20 of the precursor laminate 10 shown in Figure 5, and the laminate 71 shown in Figure 9(a) is obtained. In the second exposure step (2-1), light is irradiated onto the laminate 71 shown in Figure 9(a) from one surface 21 of the substrate 20, and the second resist film 50 is exposed, resulting in the laminate 72 shown in Figure 9(b). In the second development step (2-2), the laminate 72 shown in Figure 9(b) is subjected to a development process, and the unexposed portion 52 of the second resist film 50 is removed, thereby obtaining the laminate 73 shown in Figure 9(c). In the first resist film formation step (2-3), the first resist film 40 is formed on the laminate 73 shown in Figure 9(c) so as to cover the other surface 21 side of the substrate 20 where the first metal nanowire 31 is located, and the laminate 74 shown in Figure 10(a) is obtained. In the first exposure step (2-4), light is irradiated onto the laminate 74 shown in Figure 10(a) from the other surface 22 side of the substrate 20, exposing the first resist film 40, and the laminate 75 shown in Figure 10(b) is obtained. In the first development step (2-5), the laminate 75 shown in Figure 10(b) is subjected to a development process, and the unexposed portion 42 of the first resist film 40 is removed, thereby obtaining the laminate 16 shown in Figure 6. In the conductive nanowire formation step (2-6), upper conductive layers 61 and 62 are formed in the openings 44 and 54 of the laminate 16 shown in Figure 6, respectively, to obtain the resist pattern-containing laminate 1 (conductive film) shown in Figure 7.
[0158] [Third Embodiment] The method for manufacturing a resist pattern-containing laminate according to the third embodiment comprises the following steps (3-0) to (3-7). (3-0) A first resist film forming step to obtain a laminate, in which a first resist film is formed on the surface side of the substrate on which the first metal pattern is arranged, in a precursor laminate having a second metal pattern, a substrate and a first metal pattern in this order. (3-1) A first exposure step in which the first resist film is exposed by irradiating it with light from the other surface side of the substrate. (3-2) A first development step in which the exposed first resist film is developed to form a first resist pattern and obtain a laminate containing the resist pattern. (3-3) A first conductive wire formation step, in which an upper conductive layer is formed on a first metal nanowire exposed at an opening in the first resist pattern to obtain a first conductive nanowire. (3-4) A second resist film formation step in which a second resist film is formed on the other surface side of the substrate after the first conductive nanowire formation step (3-3). (3-5) A second exposure step of irradiating the second resist film with light from one surface side of the base material to expose the second resist film. (3-6) A second development step of developing the exposed second resist film to form a second resist pattern. (3-7) A second conductive thin wire forming step of forming an upper conductive layer on the second thin metal wire exposed in the opening of the second resist pattern to obtain a second conductive thin wire.
[0159] The manufacturing method of the present embodiment including the above steps (3-0) to (3-7) in this order will be described with reference to the drawings. Figure 11 and Figure 12 are drawings for explaining the manufacturing method of the present embodiment. Figure 11(a) is a drawing for explaining the first conductive thin wire forming step (3-3), Figure 11(b) is a drawing for explaining the second resist film forming step (3-4), Figure 12(a) is a drawing for explaining the second exposure step (3-5), and Figure 12(b) is a drawing for explaining the second development step (3-6). The members in Figure 11 and Figure 12 are the same as the members denoted by the same reference numerals in Figures 1 to 3 and 4 to 10, and therefore descriptions of the respective members are omitted.
[0160] The first resist film forming step (3-0), the first exposure step (3-1) and the first development step (3-2) are the same as steps (1-0) to (1-2) of the first embodiment, and the laminate 13 shown in Figure 3 is obtained by the first development step (3-2). In the first conductive thin wire forming step (3-3), the upper conductive layer 61 is formed in the opening 44 of the laminate 13 shown in Figure 3, and the resist pattern-containing laminate 81 (conductive film) shown in Figure 11(a) is obtained. In the second resist film forming step (3-4), the second resist film 50 is formed on the laminate 81 shown in Figure 11(a) so as to cover the other surface 22 side of the base material 20 on which the second thin metal wires 32 are arranged, and the laminate 82 shown in Figure 11(b) is obtained. In the second exposure step (3-5), the laminate 82 shown in Fig. 11(b) is irradiated with light from one surface 21 side of the base material 20, the second resist film 50 is exposed, and the laminate 83 shown in Fig. 11(c) is obtained. In the second development step (3-6), the laminate 83 shown in Fig. 12(a) is subjected to development processing, and the unexposed portion 52 of the second resist film 50 is removed, whereby the laminate 84 shown in Fig. 12(b) is obtained. In the second conductive fine wire forming step (3-7), the upper conductive layer 62 is formed in the opening 54 included in the laminate 84 shown in Fig. 12(b), and the resist pattern-containing laminate 1 (conductive film) shown in Fig. 7 is obtained.
[0161] <Applications of Conductive Film> The conductive film composed of the resist pattern-containing laminate obtained by the present production method can be applied to various uses, and is applicable to applications such as touch panels (or touch panel sensors), semiconductor chips, various electric wiring boards, FPCs (Flexible Printed Circuits), COFs (Chip on Film), TAB (Tape Automated Bonding), antennas, multilayer wiring boards, and motherboards. Among them, the conductive film is preferably used for a touch panel (capacitive touch panel). In a touch panel having a conductive film, the above-mentioned conductive fine wires can effectively function as detection electrodes. When the conductive film is used for a touch panel, examples of the display panel used in combination with the conductive film include a liquid crystal panel and an OLED (Organic Light Emitting Diode) panel, and a combination with an OLED panel is preferred.
[0162] Other applications of the conductive film include, for example, electromagnetic wave shields that block electromagnetic waves such as radio waves and microwaves (ultra-high frequency waves) generated from electronic devices such as personal computers and workstations, and prevent static electricity. Such an electromagnetic wave shield can be used not only in personal computer main bodies but also in electronic devices such as video photographing equipment and electronic medical equipment. Conductive films can also be used in transparent heating elements.
[0163] The conductive film may be used in the form of a laminate comprising the conductive film and other components such as an adhesive sheet and a release sheet during handling and transport. The release sheet functions as a protective sheet to prevent damage to the conductive film during transport of the laminate. Furthermore, the conductive film may be handled in the form of a composite having, for example, a conductive film, an adhesive sheet, and a protective layer in that order.
[0164] The present invention is basically configured as described above. The present invention is not limited to the embodiments described above, and various improvements or modifications may be made without departing from the spirit of the invention. [Examples]
[0165] The present invention will be described in more detail below based on examples. The materials, quantities, proportions, processing details, and processing procedures shown in the following examples can be modified as appropriate, as long as they do not depart from the spirit of the present invention. Therefore, the scope of the present invention should not be interpreted as being limited by the following examples.
[0166] In Examples 1-9 and Comparative Example 1, resist pattern-containing laminates were manufactured, and the back-facing visibility and fine line shape were evaluated as evaluation items. Examples 1-9 and Comparative Example 1 are described below.
[0167] <Example 1> [Manufacturing of Pre-Laminate P] In Example 1, a precursor laminate having a substrate, a first metal pattern consisting of first metal nanowires arranged on one surface of the substrate, and a second metal pattern consisting of second metal nanowires arranged on the other surface of the substrate was manufactured by photolithography according to the following manufacturing process (process P).
[0168] (Manufacturing of base materials) A 160 μm thick unstretched sheet was obtained by melt-extruding polyethylene terephthalate (PET) resin pellets using a T-die, and then rapidly cooling the resulting molten film while it was in close contact with a cast roll. The widthwise ends of this unstretched sheet were gripped by clips on a simultaneous biaxial stretching machine, and the unstretched sheet was simultaneously biaxially stretched to obtain a biaxially oriented film. The obtained biaxially oriented film was heat-treated, cooled, and wound on a winding machine to obtain a 12 μm thick PET film.
[0169] (Formation of the undercoat layer) The polymer latex-containing composition described above was applied to both surfaces of the obtained PET film to create a base coat layer with a thickness of 0.05 μm. This process was carried out by roll-to-roll, and each of the following processes (steps) was also carried out by roll-to-roll in the same manner. The roll width at this time was 1 m and the length was 1000 m.
[0170] (Preparation of silver halide emulsion) To a mixture of liquids 1 (maintained at 38°C and pH 4.5), 90% of each of liquids 2 and 3 were added simultaneously over 20 minutes while stirring to form 0.07 μm core particles. Subsequently, liquids 4 and 5 were added to the mixture over 8 minutes, and then the remaining 10% of liquids 2 and 3 were added over 2 minutes to grow the particles to 0.09 μm. Finally, 0.15 g of potassium iodide was added to the mixture, and it was allowed to mature for 5 minutes to complete particle formation.
[0171] 1 liquid: 750mL water Gelatin 8.6g Sodium chloride 3g 1,3-Dimethylimidazolidinedione-2-thione 20mg Sodium benzenethiosulfonate 10 mg Citric acid 0.7g 2 liquid: 300mL water Silver nitrate 150g 3 liquid: 300mL water Sodium chloride 38g Potassium bromide 32g Potassium hexachloroiridate(III) (0.005% KCl 20% aqueous solution) 5mL Ammonium hexachlororhodate (0.001% NaCl 20% aqueous solution) 7mL Solution 4: Water 100mL Silver nitrate 50g Solution 5: Water 100mL Sodium chloride 13g Potassium bromide 11g Potassium ferrocyanide 5mg
[0172] Thereafter, the grains were washed with water by a flocculation method according to a conventional procedure. Specifically, the temperature of the above mixed solution was lowered to 35°C, and sulfuric acid was used to lower the pH of the mixed solution until the silver halide grains precipitated (the pH was in the range of 3.6±0.2). Next, about 3 liters of the supernatant was removed from the mixed solution (first water washing). Further, 3 liters of distilled water was added to the mixed solution from which the supernatant had been removed, and then sulfuric acid was added until the silver halide precipitated. Again, 3 liters of the supernatant was removed from the mixed solution (second water washing). The same operation as the second water washing was repeated once more (third water washing) to complete the water washing and desalting steps. After adjusting the pH of the emulsion after water washing and desalting to 6.4 and the pAg to 7.5 respectively, 2.5 g of gelatin, 10 mg of sodium benzenethiosulfonate, 3 mg of sodium benzenethiosulfinate, 15 mg of sodium thiosulfate and 10 mg of chloroauric acid were added to the emulsion, and chemical sensitization was performed at 55°C to obtain the optimum sensitivity. Thereafter, 100 mg of 1,3,3a,7-tetraazaindene as a stabilizer and 100 mg of Proxel (trade name, manufactured by ICI Co., Ltd.) as a preservative were further added to the emulsion. The finally obtained emulsion was a silver iodochlorobromide cubic grain emulsion containing 0.08 mol% of silver iodide, having a silver chlorobromide ratio of 70 mol% silver chloride and 30 mol% silver bromide, an average grain size of 0.10 μm, and a coefficient of variation of 9%.
[0173] (Preparation of photosensitive layer-forming composition) The above emulsion contains 1,3,3a,7-tetraazaindene (1.2 × 10⁻¹⁰ -4 (moles / moles Ag), hydroquinone (1.2 × 10) -2 Moles / moles (Ag), citric acid (3.0 × 10 -4 The composition was obtained by adding (mol / mol Ag), 2,4-dichloro-6-hydroxy-1,3,5-triazine sodium salt (0.90 g / mol Ag), and a trace amount of hardening agent. Next, the pH of the composition was adjusted to 5.6 using citric acid. A polymer latex containing a polymer represented by (P-1) below (hereinafter also referred to as "polymer 1"), a dispersant consisting of dialkylphenyl PEO (PEO is an abbreviation for polyethylene oxide) sulfate ester, and water (the ratio of the mass of the dispersant to the mass of polymer 1 (mass of dispersant / mass of polymer 1, unit is g / g) is 0.02, and the solid content is 22% by mass) was added to the above-mentioned composition in such a way that the ratio of the mass of polymer 1 to the total mass of gelatin in the composition (mass of polymer 1 / mass of gelatin, unit is g / g) was 0.25 / 1 to obtain a polymer latex-containing composition. In this polymer latex-containing composition, the ratio of the mass of gelatin to the mass of silver derived from silver halide (mass of gelatin / mass of silver derived from silver halide, unit is g / g) was 0.11. Furthermore, EPOXY RESIN DY 022 (product name: manufactured by Nagase ChemteX Corporation) was added as a crosslinking agent. The amount of crosslinking agent added was 0.09 g / m², which corresponds to the amount of crosslinking agent in the silver halide-containing photosensitive layer described later. 2 I adjusted it so that it would be as follows. A photosensitive layer-forming composition was prepared in the manner described above. Polymer 1 was synthesized with reference to Japanese Patent Publication No. 3305459 and Japanese Patent Publication No. 3754745.
[0174] [ka]
[0175] (Process A1, Process B1) Next, the silver halide-free layer-forming composition and the above-mentioned photosensitive layer-forming composition were simultaneously applied in multiple layers to the surface of each undercoat layer formed on both surfaces of the PET film, thereby forming a silver halide-free layer (anti-halation layer) and a silver halide-containing photosensitive layer on the undercoat layer. The silver halide-free layer-forming composition contained the above-mentioned polymer latex, gelatin, and cyanine dye as a dye that is decolorized by a developer. The thickness of the silver halide-free layer is 2.0 μm, the mass ratio of polymer 1 to gelatin in the silver halide-free layer (polymer 1 / gelatin) is 2 / 1, and the polymer 1 content is 0.65 g / m². 2 Furthermore, the optical density of the silver halide-free layer, measured using the above measurement method, was approximately 1.0. Furthermore, the thickness of the silver halide-containing photosensitive layer is 2.0 μm, the mixed mass ratio of polymer 1 to gelatin in the silver halide-containing photosensitive layer (polymer 1 / gelatin) is 0.25 / 1, and the polymer 1 content is 0.15 g / m². 2 That was the case.
[0176] (Process C1) The aforementioned photosensitive layer, fabricated as described above, was simultaneously exposed to both sides of the substrate by irradiating it with parallel light from a high-pressure mercury lamp via a grid-shaped photomask. A pattern-forming mask was used as the photomask. The photosensitive layer was exposed while the photomask was in contact with it. The shape of the photomask and the exposure conditions were set so that in the laminate formed after step F1 described later, a unit square grid with an opening of side length L of 400 μm was formed, and the line width w of the metal nanowire was 4.0 μm. The exposed photosensitive layer was subjected to a developing solution, as described later, and then further processed with a fixing solution (product name: CN16X N3X-R: manufactured by Fujifilm Corporation) to perform the development process. After that, it was rinsed with pure water at 25°C and dried to obtain sample A, which had fine lines containing metallic silver formed in a mesh pattern on both sides of the substrate. In sample A, a mesh pattern area measuring 10 cm × 10 cm (corresponding to the first and second metallic patterns) was formed.
[0177] (Composition of the developing solution) One liter (L) of developer contains the following compounds: Hydroquinone 0.037 mol / L N-methylaminophenol 0.016 mol / L Sodium metaborate 0.140 mol / L Sodium hydroxide 0.360 mol / L Sodium bromide 0.031 mol / L Potassium metabisulfite 0.187 mol / L
[0178] The obtained sample A was immersed in 50°C hot water for 180 seconds. After that, the water was drained with an air shower and allowed to air dry.
[0179] (Process D1) Sample A, processed in step C1, was transferred to a 110°C superheated steam treatment tank, left to stand for 30 seconds, and then subjected to superheated steam treatment. The steam flow rate at this time was 100 kg / h.
[0180] (Process E1) Sample A, which had been processed in step D1, was immersed in a hypochlorous acid-containing aqueous solution (25°C) for 30 seconds. After removing Sample A from the aqueous solution, it was washed by immersing it in warm water (liquid temperature: 50°C) for 120 seconds. After that, the water was removed with an air shower and it was allowed to air dry. As the hypochlorous acid-containing aqueous solution mentioned above, a diluted solution prepared by diluting Kao Corporation's bleach (product name "Hyter") to twice its original volume was used.
[0181] (Process F1) Sample A, obtained in step E1, was calendered at a pressure of 30 kN using a calendering apparatus with a combination of metal and resin rollers. The calendering was performed at room temperature.
[0182] Through the above process, a precursor laminate P was obtained, which comprises a PET film as a base material, a first metal pattern consisting of first metal wires arranged on one surface side of the PET film, and a second metal pattern consisting of second metal wires arranged on the other surface side of the PET film. The wire widths w1 of the first metal nanowire and w2 of the second metal nanowire in the obtained precursor laminate P were measured using a VHX-5000 microscope manufactured by Keyence Corporation. The wire widths of each formed metal nanowire are shown in the table below.
[0183] [First resist film formation process] A liquid negative resist material "ZPN1150" (manufactured by Zeon Corporation) was applied to almost the entire surface of one of the precursor laminates P obtained in step F1 to form a first resist film. This resulted in a laminate having, in this order, a first resist film arranged on a first metal pattern, a first metal pattern, a substrate, and a second metal pattern.
[0184] [First exposure process] Next, the laminate obtained in the first resist film formation step was irradiated with a 436 nm wavelength g-ray from the other surface side of the substrate where the second metal pattern was placed, using an ultraviolet exposure apparatus. This exposed the first resist film using the first metal pattern as a self-aligning mask pattern. The exposure treatment was 320 mJ / cm². 2 After exposure with the specified UV irradiation dose, post-exposure baking (PEB) was performed at 90°C for 1 minute.
[0185] [First development step] After the first exposure step, the first resist film, which had undergone exposure treatment and PEB, was subjected to a 1-minute developing treatment using a developer ("NMD-3" manufactured by Tokyo Ohka Kogyo Co., Ltd.) to remove the unexposed areas of the first resist film. Subsequently, the laminate was washed with water to form the first resist pattern. This resulted in obtaining sample B (a resist pattern-containing laminate) having a substrate, a first metal pattern placed on one surface of the substrate, a first resist pattern placed on one surface of the substrate in an area where the first metal pattern was not placed, and a second metal pattern placed on the other surface of the substrate. The shape of the openings in the first resist pattern was almost the same as the shape of the mesh pattern of the first metal pattern. Furthermore, the opening width of the formed openings in the first resist pattern was almost the same as the line width of the first metal nanowires that constitute the mesh pattern of the first metal pattern.
[0186] [Second resist film formation process] Next, the liquid negative resist material "ZPN1150" was applied to almost the entire surface of the other surface of the substrate of sample B obtained in the first development step, where the second metal pattern was placed, to form a second resist film. This resulted in a laminate having the substrate, the first metal pattern, the first resist pattern, the second metal pattern, and the second resist film placed on the second metal pattern.
[0187] [Second freezing process] In the laminate obtained in the second resist film formation step, the second resist film was irradiated with a 436 nm wavelength g-ray from one side of the substrate where the first metal pattern and the first resist pattern were arranged, using an ultraviolet exposure apparatus. This exposed the second resist film using the second metal pattern as a self-aligning mask pattern. The exposure treatment was performed at 320 mJ / cm². 2 After exposure with the specified UV irradiation dose, post-exposure baking (PEB) was performed at 90°C for 1 minute.
[0188] [Second development process] After the second exposure step and PEB, the exposed second resist film was developed for 1 minute using the developer to remove the unexposed areas of the second resist film, and then the laminate was washed with water to form a second resist pattern. As a result, sample C was obtained having a substrate, a first metal pattern, a first resist pattern, a second metal pattern placed on the other surface side of the substrate, and a second resist pattern placed on the other surface side of the substrate in an area where the second metal pattern was not placed. The shape of the openings in the second resist pattern of sample C was almost the same as the shape of the mesh pattern of the second metal pattern. Furthermore, in sample C, the opening width of the openings in the formed second resist pattern was almost the same as the line width of the second metal nanowires that constitute the mesh pattern of the second metal pattern.
[0189] [Conductive thin wire formation process] Sample C obtained in the second development step was immersed in plating solution A (30°C), which will be described later. Then, sample C was removed from plating solution A, and subsequently, the removed sample C was washed by immersing it in warm water (liquid temperature: 50°C) for 120 seconds to wash away the plating solution adhering to sample C. In this way, the first plating film (first upper conductive layer) and the second plating film (second upper conductive layer) were formed on the first metal pattern and the second metal pattern, respectively, using each metal pattern as a seed layer. In the conductive nanowire formation process, the immersion time of sample C in plating solution A was adjusted so that the thickness of the first and second plating films was 4.0 μm. The composition of plating solution A (total volume 1200 mL) used is shown below. The amount of potassium carbonate (manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.) added was adjusted so that the pH of plating solution A was 9.5. In addition, all of the following components of plating solution A were manufactured by Fujifilm Wako Pure Chemical Industries, Ltd.
[0190] (Composition of plating solution A) AgNO3 8.8g Sodium sulfite 72g Sodium thiosulfate pentahydrate 66g • Potassium iodide 0.004g • Citric acid 12g Methylhydroquinone 3.67g • Potassium carbonate (specified amount) ·Water remainder
[0191] Through the above process, a resist pattern-containing laminate (conductive film) of Example 1 was manufactured, comprising a substrate, a first conductive nanowire, a first resist pattern, a second conductive nanowire, and a second resist pattern. Here, the first conductive nanowire is composed of a first metal pattern and a first plating film and is arranged on one surface side of the substrate, and the first resist pattern (first insulating film) is arranged on one surface of the substrate in a region where the first conductive nanowire is not arranged. Furthermore, the second conductive nanowire is composed of a second metal pattern and a second plating film and is arranged on the other surface side of the substrate, and the second resist pattern (second insulating film) is arranged on the other surface of the substrate in a region where the second conductive nanowire is not arranged.
[0192] <Examples 2-3, Comparative Example 1> The resist pattern-containing laminates of Examples 2-3 and Comparative Example 1 were manufactured in the same manner as in Example 1, except that the thickness of the PET film used as the substrate was changed to the thicknesses shown in the table below by adjusting the thickness of the molten film formed by melt extrusion and the stretching ratio of simultaneous biaxial stretching in the substrate manufacturing process.
[0193] <Examples 4-5> The resist pattern-containing laminates of Examples 4 and 5 were manufactured in the same manner as in Example 1, except that the exposure amount was changed by adjusting the exposure time for exposing the photosensitive layer in step C1, thereby changing the line width w1 of the first metal pattern and the line width w2 of the second metal pattern to the line width w shown in the table below.
[0194] <Examples 6-7> The resist pattern-containing laminates of Examples 6 and 7 were manufactured in the same manner as in Examples 4 and 5, except that, as a first resist film formation step, a negative-type dry film resist (Sunfort, manufactured by Asahi Kasei Electronics Corporation) was laminated over almost the entire surface of one of the precursor laminate P to form a first resist film, and as a second resist film formation step, the dry film resist was laminated over almost the entire surface of the other of the substrate of sample C obtained in the first development step to form a second resist film.
[0195] <Example 8> In Example 8, a precursor laminate was manufactured by the subtractive method according to the following manufacturing process (step Q). First, a substrate was prepared in the same manner as in Example 1, by applying a 0.05 μm thick undercoat layer to both surfaces of a 12 μm thick PET film. Next, a copper oxide film was formed as an adhesion layer on both surfaces of the prepared substrate. During this process, copper was used as the target, and a mixed gas of oxygen (flow rate: 90 sccm) and argon (flow rate: 270 sccm) was introduced into the sputtering apparatus while maintaining a film formation chamber pressure of 0.4 Pa and a power density of 1.7 W / cm². 2 Sputtering was performed under the condition that the roll temperature during film formation was 90°C. The thickness of the obtained copper oxide film was 20 nm.
[0196] Next, a copper film was formed on the copper oxide film on both surfaces of the substrate. Using copper as the target, argon gas (flow rate: 270 sccm) was introduced into the sputtering apparatus, with a film formation chamber pressure of 0.4 Pa and a power density of 4.2 W / cm². 2 Sputtering was performed under the condition that the roll temperature during film formation was 90°C. In the laminate obtained in this way, the thickness of each copper film was 300 nm. After forming a copper film, a rust-preventive treatment was applied to the copper film, and the copper film was patterned using photolithography. During this process, a positive-type resist was sequentially applied to each copper film to a thickness of 2 μm. Next, two glass photomasks with a mesh pattern of 4.0 μm line width corresponding to the mesh pattern shown in Figure 4 were prepared. Then, with the two glass photomasks placed on the resist films on both surfaces, each copper film was irradiated with a metal halide lamp for simultaneous exposure of both sides. Subsequently, the laminate with resist films on both surfaces was developed by immersion in a 3% sodium hydroxide aqueous solution to obtain a resist film with a pattern corresponding to the mesh pattern shown in Figure 4. Using the obtained resist film as a mask, the copper oxide film and copper film were etched using a 5% ferric chloride aqueous solution to pattern the copper oxide film and copper film placed on both surfaces of the substrate. Finally, the resist films remaining on both surfaces of the substrate were peeled off to form metal patterns (first metal pattern and second metal pattern) on both surfaces of the substrate.
[0197] Through the above process, a precursor laminate Q was obtained, having a base material, a first metal pattern composed of first metal nanowires arranged on one surface side of the base material, and a second metal pattern composed of second metal nanowires arranged on the other surface side of the base material.
[0198] Except for using the above-mentioned precursor laminate Q instead of the precursor laminate P in the first resist film formation step, the resist pattern-containing laminate of Example 8 was manufactured according to the method of Example 1, having a substrate, a first conductive nanowire, a first resist pattern (first insulating film), a second conductive nanowire, and a second resist pattern (second insulating film). The line widths of each metal wire in the obtained precursor laminate Q are shown in the table below.
[0199] <Example 9> In Example 9, a precursor laminate was manufactured by inkjet printing using conductive ink according to the following manufacturing process (process R). First, a substrate was prepared in the same manner as in Example 1, by applying a 0.05 μm thick undercoat layer to both surfaces of a 12 μm thick PET film.
[0200] Next, 60 g of dendritic electrolytic copper powder (manufactured by Mitsui Mining & Smelting Co., Ltd., product name "MF-D2", diameter 10 μm) was mixed with 100 mL of approximately 5% by mass sulfuric acid aqueous solution as washing water. The mixture was stirred at 20°C for 10 minutes, then filtered and acid washed. The washing process was repeated until the filtrate became neutral. Specifically, a total of 3 L of washing water was used for six acid washes. Next, the acid-washed raw copper powder was transferred to a 1L poly container, and an aqueous solution consisting of 31.5g of ammonium carbonate, 63g of EDTA, and 250g of water was added to prepare a copper dispersion. Then, an aqueous solution consisting of 5.25g of silver nitrate and 32.4g of water was added to this copper dispersion while stirring, and silver displacement plating (first plating step) was performed. Next, the dispersion after silver substitution plating was filtered, washed, and dried to obtain raw copper powder (first silver-plated copper powder) in which 5 parts by mass of silver were plated per 100 parts by mass of raw copper powder. The 50% particle size (D50%) of the first silver-plated copper powder was measured using a Microtrac HRA (manufactured by Nikkiso Co., Ltd.) and found to be 8.39 μm. Furthermore, the tap density of the first silver-plated copper powder was measured using the method described below and found to be 2.99 g / cm³. 3 That was the case.
[0201] (Method for measuring tap density) (i) Gently drop 100g of the sample (first silver-plated copper powder) into a 100mL graduated cylinder using a funnel. (ii) Place a graduated cylinder on a tap density meter and drop it 600 times at a rate of 60 times / minute with a drop distance of 20 mm to compress the sample. Measure the volume of the sample after compression. (iii) Volume after compression (cm 3 By dividing the sample mass (g) by ), the tap density (g / cm³) of the sample can be calculated. 3 ) is calculated.
[0202] Next, 0.1 parts by mass of stearic acid, a lubricant, was added to 100 parts by mass of the first silver-plated copper powder, and this was crushed in a ball mill to obtain crushed powder. The crushing conditions were 20°C, a rotation speed of 30 revolutions per minute, and a duration of 60 minutes. The 50% particle size (D50%) of the obtained pulverized powder, measured using a Microtrac HRA (manufactured by Nikkiso Co., Ltd.), was 8.04 μm. Furthermore, the tap density of the pulverized powder measured by the above method was 3.85 g / cm³. 3 That was the case.
[0203] Next, the crushed powder was transferred to a 1L poly container, and silver substitution plating (second plating step) was performed in the same manner as the first plating step described above to obtain silver-plated copper powder. In the second plating process, 5 parts by mass of silver were plated onto 100 parts by mass of copper powder. The final silver-plated copper powder was obtained by plating 10 parts by mass of silver onto 100 parts by mass of raw copper powder.
[0204] The aforementioned silver-plated copper powder (100 parts by mass), polyester resin (Toyobo Co., Ltd., trade name "Byron 550", 18 parts by mass as solids) and curing agent (block isocyanate, manufactured by Nippon Polyurethane Industry Co., Ltd., trade name "Coronate 2516", 4.5 parts by mass as solids) as a binder resin, and butyl cellosolve acetate (BCA, 286 parts by mass) as a solvent were added and premixed to ensure that the silver-plated copper powder and the other components blended well. Subsequently, this premix was dispersed in a three-roll mill to obtain a conductive ink with a solid content of 30% by mass.
[0205] The above conductive ink was filled into the ink cartridge of an inkjet recording device (product name "DMP-2831", manufactured by FUJIFILM Dimatix). The substrate was fixed to an inkjet recording device, and the conductive ink was ejected onto one surface of the substrate to form a pattern corresponding to the mesh pattern shown in Figure 4. Next, the conductive ink was ejected onto the other surface of the substrate to form a pattern corresponding to the mesh pattern shown in Figure 4, and then the substrate was heated at 120°C for 30 minutes using a hot plate. As a result, a precursor laminate R was obtained having a substrate, a first metal pattern composed of first metal nanowires arranged on one surface of the substrate, and a second metal pattern composed of second metal nanowires arranged on the other surface of the substrate. The line widths of each metal wire in the obtained precursor laminate R are shown in the table below.
[0206] Except for using the above-mentioned precursor laminate R instead of the precursor laminate P in the first resist film formation step, the resist pattern-containing laminate of Example 9 having a substrate, a first conductive nanowire, a first resist pattern (first insulating film), a second conductive nanowire, and a second resist pattern (second insulating film) was manufactured according to the method of Example 1.
[0207] <Measurement> [Width and height of conductive thin wires] In each example, the resist pattern-containing laminate was cut using an ultramicrotome along a plane perpendicular to the direction in which the conductive nanowires extended, exposing the cut surface. Next, as a pretreatment, a carbon layer 10-20 nm thick was deposited onto the exposed cut surface to prepare a test specimen for cross-sectional observation. The cross-sections of the obtained test specimens were observed using a scanning electron microscope (SEM, manufactured by Hitachi High-Technologies Corporation), and the line width and height of the conductive nanowires were measured from the obtained observation images. If the line width of the conductive nanowires differed depending on the height in a single observation image, the maximum line width was taken as the representative value of the line width in that observation image. For each resist pattern-containing laminate, the material was cut at 10 different positions of conductive nanowires. The line width and height of the conductive nanowires were measured from the observed images of the resulting cut surfaces, and the line width and height of the conductive nanowires were calculated by arithmetic mean of the 10 obtained measurements.
[0208] Test specimens with exposed cross-sections were prepared for each example of the resist pattern-containing laminate, and the metal density of the conductive nanowires at the cross-section of the test specimens was measured using the TOF-SIMS method described above. As a result, it was confirmed that the conductive nanowires in the resist pattern-containing laminate obtained in each example were located on the substrate side and had a lower region with a lower metal density, and an upper region other than the lower region with a higher metal density. It was also confirmed that the lower region corresponds to the first or second metal nanowire, and the upper region corresponds to the first or second upper conductive layer.
[0209] <Rating> The following describes the evaluation methods for the back-facing and fine-line shape of each resist pattern-containing laminate.
[0210] [Reflection on the back] The resist pattern-containing laminates produced in each example were cut using an ultramicrotome along a plane perpendicular to the direction in which the second conductive nanowire extends, exposing the cut surface including the width and thickness directions of the second conductive nanowire. Next, as a pretreatment, carbon with a thickness of 10-20 nm was deposited on the exposed cut surface to prepare a test specimen for cross-sectional observation. The cross-section of the obtained test specimen was observed using a scanning electron microscope (SEM, manufactured by Hitachi High-Technologies Corporation). The observation conditions were an acceleration voltage of 5kV, backscattered electron mode, and an observation magnification of 30,000x. Furthermore, from the cross-section of the test specimen, the observation area was selected to include at least one second conductive nanowire, the substrate, and the first resist pattern facing the second conductive nanowire across the substrate in the thickness direction. From the cross-sectional image obtained by observing the above observation area, the presence or absence of recesses and, if recesses exist, the height of the recesses (depth in the thickness direction) were measured in the region of the first resist pattern that faces the second conductive nanowire across the substrate in the thickness direction. For each resist pattern-containing laminate, test specimens were prepared at 10 arbitrarily selected locations, each having a cross-section perpendicular to the second conductive nanowire, according to the method described above. Using a scanning electron microscope (SEM), the presence and height of recesses in the region facing the second conductive nanowire in the thickness direction of the first resist pattern were measured. The arithmetic mean of the heights of the 10 recesses measured for the first resist pattern was taken, and the back-image of the second metal nanowire onto the first resist film during exposure was evaluated based on the following evaluation criteria using the average value of the resulting recesses. If no recesses were observed, the recess height was set to "0".
[0211] (Background reflection evaluation criteria) "A": No recesses were observed in any of the test specimens. "B": The average height of the recesses is greater than 0% and less than 20% of the thickness of the first resist film. "C": The average height of the recesses is 20% or more of the thickness of the first resist film.
[0212] Furthermore, for each resist pattern-containing laminate, a test specimen having a cross-section perpendicular to the first conductive nanowire was prepared according to the method described above. The presence and height of recesses in the region of the second resist pattern facing the first conductive nanowire were measured using an SEM, and the back-image of the first metal nanowire onto the second resist film during exposure was evaluated. The evaluation results were the same as those for the back-image of the second metal nanowire onto the first resist film.
[0213] [Thin line shape] The surface of the resist pattern-containing laminate manufactured in each example, where the first conductive nanowire and the first resist pattern were exposed, was observed from the normal direction of the substrate using an optical microscope. A section of the first conductive nanowire with a length of 200 μm along the direction in which the first conductive nanowire extends (hereinafter also referred to as the "length direction") was selected as the observation area. Within the above observation area, 10 equally spaced positions in the length direction, including both ends, were selected, and the position corresponding to the midpoint of the line width of the first conductive nanowire at each position in the length direction was defined as Pn (n=1~10). Next, a straight line L was drawn connecting positions P1 and P10, and the distances a2~a9 between positions P2~P9 and the straight line L were measured. The maximum value of the obtained distances a2~a9 was defined as distance a. For each resist pattern-containing laminate, the observation area was selected at five different locations of the first conductive nanowire according to the method described above, and the distance a was calculated. The arithmetic mean of the five obtained distances a was taken, and the nanowire shape of the first conductive nanowire in the resist pattern-containing laminate was evaluated from the average value of the obtained distances a based on the evaluation criteria below. A shorter average value of distance a indicates that the first conductive nanowire has a less distorted and more linear shape.
[0214] (Evaluation criteria for thin line shape) "A": The average value of distance a is 25% or less of the line width v1 of the first conductive nanowire. "B": The average value of distance a is greater than 25% of the line width v1 of the first conductive nanowire.
[0215] Furthermore, for each resist pattern-containing laminate, the surface where the second conductive nanowire and the second resist pattern were exposed was observed according to the method described above, and the average value of distance a relative to the line width v2 of the second conductive nanowire was calculated. As a result, the evaluation result of the nanowire shape of the second conductive nanowire was the same as the evaluation result of the nanowire shape of the first conductive nanowire.
[0216] <Result> The evaluation results for the above examples and comparative examples are shown in the table below. In the table, the "d[μm]" column under "Substrate" indicates the thickness (μm) of the substrate. The "w1[μm]" and "d / w1" columns show the line width w1 (μm) of the first metal nanowire of the first metal pattern and the ratio of the substrate thickness d to the line width w1, respectively. The "v1[μm]", "h1[μm]", and "h1 / v1" columns show the line width v1 (μm) of the first conductive nanowire, the height h1 of the first conductive nanowire, and the ratio of the height h1 to the line width v1, respectively. The same applies to the "w2[μm]", "d / w2", "v2[μm]", "h2[μm]", and "h2 / v2" columns. The "Precursor Laminate" column shows the manufacturing process of the precursor laminate carried out in each example. The "Resist Film" column indicates the manufacturing method for the first and second resist films in the production of each resist pattern-containing laminate. "Resist Solution" means that a resist film was formed by applying a liquid resist film-forming material, and "DFR" means that a resist film was formed by transferring a dry film resist onto a substrate.
[0217] [Table 1]
[0218] The results in Table 1 confirm that the method for manufacturing a resist pattern-containing laminate according to the present invention suppresses the back-facing of the metal nanowires onto the resist film, and allows for the production of a resist pattern with a desired pattern shape. On the other hand, in the method for manufacturing a resist pattern-containing laminate of Comparative Example 1, in which the line width w2 of the second metal nanowire and the thickness d of the substrate did not satisfy the relationship in formula (1), the back-facing of the metal nanowires onto the resist film could not be suppressed.
[0219] From a comparison of Examples 4-7 with other examples, it was confirmed that when the line width w2 of the second metal nanowire is 3.0 μm or less, the back-facing of the metal nanowire onto the resist film can be further suppressed.
[0220] A comparison of Examples 6-7 with Examples 4-5 confirmed that when a dry film resist is transferred to a surface on which a metal pattern is arranged on the substrate to form a resist film, the shape of the conductive nanowires is superior.
[0221] A comparison of Example 8 with Examples 1 and 9 confirmed that when a dry film resist is transferred to a surface on which a metal pattern is arranged on the substrate to form a resist film, the shape of the conductive nanowires is superior. [Explanation of Symbols]
[0222] 1,11,12,13,14,15,16,71,72,73,74,75,81,82,83,84 Laminate 10 Pre-laminate 20 Base material 21,22 surface 30 Fine metal wire 31 1st metal thin wire 32 Second metal thin wire 33 Non-thin line part 40 First resist film 41, 51 Exposed area 42, 52 Unexposed areas 43. First Resist Pattern 44,54 openings 50 Second resist film 53 Second Resist Pattern 61,62 Upper conductive layer
Claims
1. Substrate and A first metal pattern, composed of first metal fine wires, is arranged on one surface side of the substrate, A first resist film disposed on the first metal pattern, A laminate having a second metal pattern, which is disposed on the other surface side of the substrate and is composed of second metal fine wires, An exposure step of irradiating the substrate with light from the other surface side to expose the first resist film, The process includes a developing step of developing the first resist film to form a first resist pattern and obtain a laminate containing the resist pattern, A method for manufacturing a resist pattern-containing laminate, wherein the line width w2 of the second metal nanowire and the thickness d of the substrate satisfy the relationship of formula (1). Formula (1) d / w2≧3.0
2. A second resist film forming step is performed after the development step, in which a second resist film is formed on the surface side of the substrate on which the second metal pattern is arranged. A second exposure step involves irradiating the second resist film with light from one surface side of the substrate to expose the second resist film, The process further comprises a second developing step of developing the second resist film to form a second resist pattern and obtain a resist pattern-containing laminate, A method for manufacturing a resist pattern-containing laminate according to claim 1, wherein the line width w1 of the first metal nanowire and the thickness d of the substrate satisfy the relationship of formula (2). Formula (2) d / w1≧3.0
3. A method for manufacturing a resist pattern-containing laminate according to claim 1, further comprising a conductive wire forming step of forming an upper conductive layer on the exposed first metal nanowire and the exposed second metal nanowire of the resist pattern-containing laminate obtained in the second developing step to obtain a conductive nanowire.
4. The method for manufacturing a resist pattern-containing laminate according to claim 3, wherein the conductive fine wire formation step is a step of performing a plating treatment on the resist pattern-containing laminate obtained in the second development step.
5. The method for manufacturing a resist pattern-containing laminate according to claim 4, wherein the plating treatment is an electroless plating treatment.
6. The method for manufacturing a resist pattern-containing laminate according to claim 1, wherein the line width w2 of the second metal nanowire is 3.0 μm or less.
7. The method for manufacturing a resist pattern-containing laminate according to claim 2, wherein the line width w1 of the first metal nanowire is 3.0 μm or less.
8. A method for manufacturing a resist pattern-containing laminate according to claim 1, further comprising a first resist film forming step, in which, prior to the exposure step, a first resist film is formed on the surface side of the substrate on which the first metal pattern is arranged in a precursor laminate having the substrate, the first metal pattern, and the second metal pattern, to obtain the laminate.
9. The method for manufacturing a resist pattern-containing laminate according to claim 8, wherein the first resist film formation step is a step of transferring the resist film to the surface side of the substrate on which the first metal pattern is arranged, using a dry film resist having a temporary substrate and a resist film.
10. A method for manufacturing a resist pattern-containing laminate according to claim 1, further comprising a first conductive wire forming step of forming a metal pattern on the first metal wire after the developing step to obtain a conductive wire.
11. Substrate and A first conductive nanowire is disposed on one surface side of the substrate, A first insulating film is disposed on one of the surfaces of the substrate and in a region where the first conductive nanowire is not disposed, A second conductive nanowire is disposed on the other surface side of the substrate, The substrate comprises a second insulating film disposed on the other surface side of the substrate and in a region where the second conductive nanowire is not disposed, The wire width v1 of the first conductive nanowire and the thickness d of the substrate satisfy the relationship of equation (X1), The height h1 of the first conductive nanowire and the width v1 of the first conductive nanowire satisfy the relationship given by equation (Y1), The wire width v2 of the second conductive nanowire and the thickness d of the substrate satisfy the relationship given by equation (X2). The height h2 of the second conductive nanowire and the width v2 of the second conductive nanowire satisfy the relationship given by equation (Y2). The metal density of the lower region of the first conductive nanowire on the substrate side is lower than the metal density of the upper region of the first conductive nanowire other than the lower region. A conductive film in which the metal density of the lower region of the second conductive nanowire on the substrate side is lower than the metal density of the upper region of the second conductive nanowire other than the lower region. Formula (X1) d / v1≧3.0 Formula (Y1) h1 / v1≧2.0 Formula (X2) d / v2≧3.0 Formula (Y2) h2 / v2≧2.0
12. The conductive film according to claim 11, wherein the line width v2 of the second conductive nanowire is 3.0 μm or less.
13. The conductive film according to claim 11 or 12, wherein the line width v1 of the first conductive nanowire is 3.0 μm or less.
14. Substrate and A first conductive nanowire is disposed on one surface side of the substrate, A first insulating film is disposed on one of the surfaces of the substrate and in a region where the first conductive nanowire is not disposed, The substrate has a second metal pattern, which is arranged on the other surface side and is composed of second metal fine wires, The wire width w2 of the second metal fine wire and the thickness d of the base material satisfy the relationship in equation (1), The height h1 of the first conductive nanowire and the width v1 of the first conductive nanowire satisfy the relationship given by equation (Y1), A conductive film in which the metal density of the lower region of the first conductive nanowire on the substrate side is lower than the metal density of the upper region of the first conductive nanowire other than the lower region. Formula (1) d / w2≧3.0 Formula (Y1) h1 / v1≧2.0
15. The conductive film according to claim 14, wherein the line width w2 of the second metal pattern is 3.0 μm or less.
16. The conductive film according to claim 14 or 15, wherein the line width v1 of the first conductive nanowire is 3.0 μm or less.
Citation Information
Patent Citations
Circuit board and its production method
JP2007287953A