Double cold-rolled non-oriented electrical steel and method for manufacturing the non-oriented electrical steel.
A double cold-rolled non-oriented electrical steel sheet with optimized elemental composition and microstructure addresses the balance of eddy current loss and mechanical properties, enhancing efficiency and suitability for industrial applications.
Patent Information
- Application Number
- JP2025546231
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-15
- Filing Date
- 2024-11-14
- Publication Date
- 2026-11-19
AI Technical Summary
Existing non-oriented electrical steel sheets face challenges in achieving a balance between low eddy current loss, magnetic permeability, thermal conductivity, tensile strength, and yield strength, particularly in high-speed motors for electric vehicles, with previous methods either reducing thickness or adding alloying elements leading to limitations in torque, rigidity, and magnetic properties.
A double cold-rolled non-oriented electrical steel sheet with specific elemental composition and microstructure, including controlled thickness and recrystallization, achieving magnetic polarization of 1.66T to 1.70T, eddy current loss of 40% to 50%, and mechanical properties like ultimate tensile strength, yield strength, and total elongation, while being suitable for conventional industrial applications.
The solution provides a steel sheet with enhanced mechanical and magnetic properties, ensuring high efficiency, punchability, and coating suitability, while maintaining compatibility with industrial processes and resisting manufacturing parameter changes.
Smart Images

Figure 2025104658000001 
Figure 2025104658000002 
Figure 2025104658000003
Abstract
Description
Technical Field
[0001] The present invention relates to a double cold-rolled non-oriented electrical steel sheet and a method for manufacturing the same. Specifically, the present invention relates to a double cold-rolled non-oriented electrical steel sheet that has excellent mechanical properties while having low iron loss, specifically low eddy current loss, and a method for manufacturing the same.
Background Art
[0002] Accordingly, vigorous research and development efforts are being invested, and due to the global increase in the achievement of energy saving for electrical appliances, higher performance characteristics are required for using non-oriented electrical steel sheets as core materials for electrical machines. In recent years, in particular, demand for small, high-output motors used in applications such as electric vehicles has been increasing. Such electric vehicle motors are designed to enable high-speed rotation, thereby obtaining high torque while having the minimum possible loss. This requires a light, highly efficient non-oriented electrical steel that has low loss as its main characteristic. Finding a balance between loss, magnetic permeability, polarization, thermal conductivity, tensile strength and yield strength is essential for non-oriented electrical steel.
[0003] The lower the iron loss in an electrical machine, the higher the efficiency of the electrical machine, and thus to reduce the amount of iron loss in the electrical machine, electrical machine manufacturers have several options, and their main option is to reduce either hysteresis loss or eddy current loss to improve the efficiency of the electrical machine. Progress is often achieved by a combination of these two approaches. The present invention relates to the second option, namely the reduction of eddy current loss for electrical machines. There are two options to reduce eddy current loss.
[0004] The first approach involves reducing the thickness of the steel plates used in electrical machinery, such as having a thickness of less than 0.35 mm or thinner. Unfortunately, this solution has limitations due to the reduction in the lamination ratio, which decreases the torque achievable for a given machine height, as well as a very significant decrease in the rigidity of certain automotive parts, and the emergence of acoustic problems that cause discomfort to the occupants.
[0005] The second method involves optimizing the elemental composition of the steel sheet by increasing the amount of alloying elements to limit eddy current losses. Among these alloying elements, aluminum and manganese, for example, have attractive mechanical and magnetic properties while significantly reducing eddy current losses. However, beyond a certain percentage, the presence of alloying elements affects hysteresis losses and magnetic polarization, so the addition of alloying elements can be limited.
[0006] Previous research and development in the field of high-strength non-oriented electrical steel have resulted in several methods for producing high-strength non-oriented electrical steel, some of which are listed herein for a thorough understanding of the present invention.
[0007] U.S. Patent Application Publication No. 2021 / 371948 describes a non-oriented electrical steel sheet, 4.5 × 10 -6 The following steel slabs, having the average magnetostriction λp-p at 400 Hz and 1.0 T, and an area ratio of recrystallized crystal grains in the cross-section of the steel sheet in the rolling direction of the sheet of 40-95%, and containing, by mass%, C: 0.005% or less, Si: 2.8-6.5%, Mn: 0.05-2.0%, Al: 3.0% or less, P: 0.20% or less, S: 0.005% or less, N: 0.005% or less, Ti: 0.003% or less, V: 0.005% or less, and Nb: 0.005% or less, and satisfying Si-2A1-Mn≧0, are subjected to hot rolling, hot-rolled sheet annealing, appropriate cold rolling and finish annealing conditions, resulting in an average thickness of 10-40 microns. particle sizeThis is a non-oriented electrical steel sheet from which a motor core is manufactured. U.S. Patent Application Publication No. 2021 / 371948 does not demonstrate total elongation and eddy current losses at all. European Patent Application Publication No. 4265749 discloses a non-oriented electrical steel sheet and a method for producing it, which involves appropriately adding Mo, Ti, Nb, and V, and controlling the time within a specific temperature range during the cooling process after final annealing to suppress the formation of fine carbonitrides. As a result, it discloses a non-oriented electrical steel sheet and a method for producing it that are excellent in both magnetism and strength. European Patent Application Publication No. 4079893 relates to non-oriented electrical steel sheets and methods for manufacturing the same, and specifically discloses non-oriented electrical steel sheets and methods for manufacturing the same in which the magnetic properties are improved by appropriately adding As and P to improve the texture. European Patent Application Publication No. 4265745 discloses a non-oriented electrical steel sheet and a method for manufacturing the same, which appropriately add Mo, Ti, and Nb to suppress the formation of fine carbides by bubbling during the molten steel manufacturing process. As a result, it discloses a non-oriented electrical steel sheet and a method for manufacturing the same that improve the cleanliness of the steel and improve magnetization properties by facilitating magnetic domain wall movement. European Patent Application Publication No. 3173503 discloses a non-oriented electrical steel sheet suitable for use as a core material for electrical equipment and a method for manufacturing the same. [Prior art documents] [Patent Documents]
[0008] [Patent Document 1] U.S. Patent Application Publication No. 2021 / 371948 [Patent Document 2] European Patent Application Publication No. 4265749 [Patent Document 3] European Patent Application Publication No. 4079893 [Patent Document 4] European Patent Application Publication No. 4265745 [Patent Document 5] European Patent Application Publication No. 3173503 [Overview of the Initiative] [Problems that the invention aims to solve]
[0009] The object of the present invention is to solve these problems by producing a double cold-rolled non-oriented electrical steel sheet that simultaneously has a magnetic polarization of 1.66T to 1.70T at 5000 A / m (J50), preferably 1.665T to 1.690T at 5000 A / m (J50), more preferably 1.670T to 1.690T at 5000 A / m (J50), and a percentage of eddy current loss in total iron loss of 40 to 50%, preferably 40% to 50%, more preferably 43% to 48%, when calculated according to the Bertotti method.
[0010] In preferred embodiments, the following additional properties can also be achieved, either alone or in combination: • Ultimate tensile strength of 490 MPa or more in both the direction perpendicular to rolling and the rolling direction, preferably exceeding 520 MPa in both the direction perpendicular to rolling and the rolling direction. • Yield strength of 380 MPa or more in both the direction perpendicular to rolling and the rolling direction, preferably 390 MPa or more in both the direction perpendicular to rolling and the rolling direction. • Total elongation of 15% or more in both the direction perpendicular to rolling and the rolling direction, preferably 17% or more in both the direction perpendicular to rolling and the rolling direction. • Total losses of 15-18 W / kg, preferably 16-18 W / kg, when measured at 1T and 400Hz.
[0011] Preferably, such steel can have good punchability and coating properties, and excellent suitability for rolling.
[0012] Preferably a hardness of 185 HV or higher, preferably 195 HV or higher.
[0013] Another object of the present invention is also to make available a method for manufacturing these sheets that is compatible with conventional industrial applications and at the same time robust against changes in manufacturing parameters. Means for Solving the Problems
[0014] The above objects and other advantages of the present invention will become more apparent by describing the preferred embodiments of the present invention in detail. Modes for Carrying Out the Invention
[0015] The chemical composition of the non-oriented electrical steel includes the following elements in weight percent: The carbon present in the steel of the present invention is 0.0001% to 0.007%. Since carbon is a precipitate-forming element, it is detrimental to the magnetic properties of the present steel. Therefore, the presence of carbon in the present steel is 0.0001% to 0.007%. Since carbon promotes magnetic aging, the preferable content of carbon according to the present invention is 0.002% to 0.007%, more preferably 0.002% to 0.006%.
[0016] The manganese content of the steel of the present invention is 0.1% to 0.3%. Manganese This results in solid solution strengthening. reduces iron loss by increasing the specific resistivity of low Reduce ers. If the added amount of manganese exceeds 0.3%, the magnetic flux density may be significantly reduced, and recrystallization of the steel is inhibited during annealing. The preferable limits for the presence of manganese are 0.1% to 0.25%, more preferably 0.1% to 0.2%.
[0017] The silicon content of the steel of the present invention is 3.1% to 3.8%. Silicon is an element that contributes to increasing strength by solid solution strengthening, and is a central element for reducing the eddy current loss of iron loss by increasing the specific resistivity of the steel. The above-mentioned effect requires a minimum silicon content of at least 3.1%. However, if the silicon content exceeds 3.8%, rolling becomes difficult, and the steel Magnetic flux densityis significantly reduced. The preferable limit for the presence of silicon is 3.2% to 3.7%, more preferably 3.2% to 3.6%.
[0018] The aluminum content is 0.6% to 0.8%. Aluminum can increase the electrical resistivity of the material and effectively reduce the iron loss of the steel. If the aluminum content is present in excess of 0.8%, the steel's Magnetic flux density is significantly reduced, which is also detrimental to the cold rolling rollability of the steel of the present invention. The preferable limit for the presence of aluminum is 0.6% to 0.75%, more preferably 0.6% to 0.7%.
[0019] Sulfur is not an essential element, but may be contained as an impurity in the steel. From the viewpoint of the present invention, the sulfur content is preferably as low as possible, but from the viewpoint of production cost, it is 0.006% or less. Furthermore, when higher sulfur is present in the steel, sulfur combines to form sulfides that are detrimental to the magnetic properties of the present invention.
[0020] The phosphorus component of the steel of the present invention is 0% to 0.15%, and phosphorus reduces hot and cold ductility due to its tendency to segregate, especially at grain boundaries, or its tendency to cosegregate with manganese. For these reasons, its content is limited to 0.15%, preferably less than 0.09%.
[0021] Nitrogen is limited to 0.09% to minimize the precipitation of aluminum nitride during solidification, which is detrimental to the magnetic properties of the steel.
[0022] Titanium is an optional element, and when added to the steel of the present invention, it is 0% to 0.1%. Titanium forms titanium nitride that appears during solidification of the casting. For this reason, the amount of titanium is limited to 0.1% to avoid the formation of titanium nitride that is detrimental to the magnetic properties of the steel of the present invention. When the titanium content is less than 0.001%, it does not exert any influence on the steel of the present invention.
[0023] Niobium is present in the steel of the present invention at a concentration of 0% to 0.1% and is suitable for forming carbonitrides to increase the strength of the steel of the present invention through precipitation hardening. Niobium also precipitates as carbonitrides, resulting in fine particles. organization It affects the size of the components. However, niobium content exceeding 0.1% is not economically interesting due to the saturation effect.
[0024] Vanadium is present in the steel of the present invention at a concentration of 0% to 0.1%, and is effective in increasing the strength of the steel by forming carbides or carbonitrides. From an economic standpoint, the upper limit is 0.1%.
[0025] Chromium is the element used in the steel of this invention, present in an amount of 0.01% to 1%. Chromium provides strength to the steel through solid solution strengthening, but using more than 1% impairs the magnetic properties of the steel.
[0026] Molybdenum is an optional element that constitutes 0% to 0.5% of the steel of the present invention.
[0027] Mo has the effect of reducing iron loss by coarsening carbides. When Mo exceeds 0.5%, the effect of improving iron loss saturates.
[0028] Tungsten is an optional element that constitutes 0% to 0.1% of the steel of the present invention. Like Mo, tungsten has the effect of coarsening carbides and reducing iron loss. However, if the amount added is less than 0.001% by mass, the above effect cannot be fully obtained, while if the amount added exceeds 0.1% by weight, the effect of improving iron loss saturates.
[0029] Cobalt is an optional element that constitutes 0% to 1% of the steel of the present invention. Cobalt is an element that increases the magnetic moment of Fe alloys, thereby increasing magnetic flux density and reducing iron loss. However, if the amount added is less than 0.01% by weight, the above effects cannot be fully obtained, while if the amount added exceeds 1% by weight, the raw material costs increase significantly.
[0030] Arsenic is an optional element that constitutes 0% to 0.05% of the steel of the present invention. As is a grain boundary segregation element that improves texture and thereby reduces iron loss. The above effect is obtained by adding 0.001% by weight or more. However, As is an element that causes grain boundary embrittlement, and this adverse effect becomes particularly pronounced when added in amounts exceeding 0.05% by weight. Therefore, it is preferable that As be added in the range of 0.001 to 0.05% by weight.
[0031] Nickel is an optional element and is present in an amount of 0.001% to 0.01% to increase the strength of the steel of the present invention and to improve its strength and elongation. In preferred embodiments, the nickel content is kept below 0.04%.
[0032] Copper may be added as an element in an amount of 0.01% to 1% to increase the strength and elongation of the steel of the present invention. However, if the content exceeds 1%, copper may degrade the surface morphology.
[0033] Boron is an optional element for the steel of the present invention and may be present in amounts of 0% to 0.05%. Boron forms boronitrides, and when added in an amount of at least 0.0001%, it imparts further strength to the steel of the present invention.
[0034] Calcium may be optionally present in the steel of the present invention, in amounts ranging from 0.001% to 0.01%. Calcium contributes to the refining of the steel by binding harmful sulfur-containing substances in a spherical manner, thereby delaying the harmful effects of sulfur.
[0035] Other elements such as Sn, Pb, or Sb can be added individually or in combination in the following proportions: Sn ≤ 0.2%, Pb ≤ 0.2%, and Sb ≤ 0.2%. Up to the indicated maximum content levels, these elements allow for grain refinement during solidification. In preferred embodiments, the Sn content is less than 0.04%.
[0036] The remainder of the steel's composition is iron and processIt consists of unavoidable impurities that arise from it.
[0037] Here, the micro-grain of non-oriented electrical steel organization This will be explained in detail, but all percentages are area fractions.
[0038] micro organization It is made from ferrite. The steel of this invention has an average thickness of 20 to 110 microns. particle size The crystal grains have a recrystallization fineness of 80% to 100% in area fraction. organization It has a region. Recrystallization with a high degree of recrystallization. organization This is due to homogeneous silicon enrichment that improves the magnetic properties of the steel of the present invention. particle size This ensures the mechanical properties in both the direction of rolling and perpendicular to the rolling direction. The preferred degree of recrystallization is 90% to 100%. Preferred average for the present invention particle size The micron size is 20 to 100 microns, more preferably 20 to 90 microns.
[0039] The steel of the present invention has a non-recrystallized fine particle content of 0% to 20% in area fraction. organization It may have regions, and the preferred degree of non-recrystallization is 0% to 10%, more preferably 0% to 5%.
[0040] The above fine organization In addition, the microstructure of non-oriented electrical steel consists of fine elements such as martensite, bainite, pearlite, and cementite. organization It does not contain any ingredients.
[0041] The steel according to the present invention can be manufactured by any suitable method. However, as a non-limiting example, it is preferable to use the method according to the present invention, which is detailed below.
[0042] Such a preferred method lies in providing a semi-finished casting of steel having the chemical composition of steel according to the present invention. The casting can be in the form of an ingot, or in the form of a continuous thin slab or thin strip, i.e., about 240 mm for any form of the casting. below The thickness can be within this range.
[0043] For example, a casting in the form of a slab is cast with the chemical composition according to the present invention and then reheated, with the slab reheating temperature being between 1000°C and 1250°C until the temperature is uniform throughout the slab. Below 1000°C, rolling becomes difficult and the force on the mill becomes too high. Above 1200°C, the high-silicon grade becomes very soft and may exhibit some deflection, making it difficult to handle. Preferably, the slab reheating temperature is between 1040°C and 1220°C, more preferably between 1060°C and 1200°C.
[0044] The reheated slab is hot-rolled to a final hot-rolled fineness. organization It plays a role in the process and is subjected to hot rolling at 840°C to 950°C. If the finish rolling temperature falls below 840°C, recrystallization is restricted, resulting in a finer grain. organization The material undergoes significant deformation. Temperatures exceeding 950°C mean that the amount of impurities in the solid solution increases, which can result in precipitation and deterioration of magnetic properties. Preferably, the finish rolling temperature is 840°C to 940°C, more preferably 845°C to 930°C.
[0045] Next, the hot-rolled steel sheet obtained in this manner is immediately cooled at a cooling rate of at least 10°C / second to the winding temperature of the hot-rolled steel sheet, which also serves the same purpose as the hot-rolled steel sheet, and the winding is performed at 500°C to 750°C. Winding at temperatures below 500°C does not result in a suitable distribution and size for the steel precipitates of the present invention. Above 750°C, a thick oxide layer appears, causing difficulties in subsequent processing steps such as cold rolling and / or pickling. Preferably, the cooling rate is 200°C / second or less, and more preferably, the cooling rate is 12°C / second to 75°C / second. Preferably, the winding temperature is 600°C to 725°C, and more preferably, 625°C to 725°C.
[0046] Next, the rolled hot-rolled steel sheet is cooled to room temperature and then subjected to hot-rolled sheet annealing.
[0047] The hot-rolled steel sheet may be subjected to an optional descaling process to remove scale formed during hot rolling, prior to optional hot-rolled sheet annealing. The hot-rolled sheet is then subjected to an optional hot-rolled sheet annealing, which is carried out at a temperature of 780°C to 1000°C, preferably for at least 10 seconds and 96 hours or less, and the temperature is preferably maintained at 790°C to 980°C, more preferably 800°C to 950°C. Subsequently, the optional descaling process of the hot-rolled steel sheet may be carried out, for example, by pickling such a sheet.
[0048] Therefore, the resulting hot-rolled steel sheet may have a thickness of any choice between 0.8 mm and 3.5 mm, preferably between 0.9 mm and 3 mm, and more preferably between 1 mm and 2.8 mm.
[0049] Next, the hot-rolled steel sheet is subjected to a first cold rolling to obtain an intermediate cold-rolled steel sheet having a thickness reduction of 60-95%. Preferably, a thickness reduction of 65-95%, more preferably 70-95%, results in an intermediate thickness of less than 1 mm.
[0050] Subsequently, the intermediate cold-rolled steel sheet is heat-treated, and the heat treatment is performed to acquire the mechanical properties and fine grain required for the steel of the present invention. organization Grant it.
[0051] Next, the intermediate cold-rolled steel sheet is subjected to a first annealing, with heating starting from room temperature, and the intermediate cold-rolled steel sheet is heated to a first annealing temperature TA1, which is 900°C to 1100°C, preferably 920°C to 1080°C, more preferably 940°C to 1070°C, at a heating rate HR1 of at least 1°C / second. In a preferred embodiment, the heating rate HR1 for heating is at least 2°C / second, more preferably at least 5°C / second. The intermediate cold-rolled steel sheet is kept at TA1 for 10 seconds to 5000 seconds to serve both the role of recrystallizing the intermediate cold-rolled steel with 80% to 100% recrystallization after the first cold rolling and the role of improving the magnetic properties of the steel of the present invention by dissolving carbides precipitated during sheet cooling and winding after hot rolling.
[0052] Next, the intermediate cold-rolled steel sheet is cooled, starting from TA1, and the intermediate cold-rolled steel sheet is cooled to a temperature T1 in the range of 20°C to 300°C at a cooling rate CR1 of 1°C / sec to 150°C / sec. In a preferred embodiment, the cooling rate CR1 is 3°C / sec to 120°C / sec. A preferred T1 temperature is 20°C to 200°C. At the end of cooling, a cold-rolled steel sheet that has undergone the first annealing is obtained.
[0053] Subsequently, the cold-rolled steel sheet that underwent the first annealing process was It is subjected to a second cold rolling process. 50-95% thickness Reduction ratio Cold-rolled steel sheet obtained The thickness reduction ratio is Preferably 60% to 95%, more preferably 75% to 95% %。
[0054] Subsequently, the cold-rolled steel sheet is subjected to a second annealing, in which heating begins at room temperature and the cold-rolled steel sheet is heated to a second annealing temperature TA2, which is 900°C to 1100°C, preferably 920°C to 1080°C, more preferably 940°C to 1070°C, at a heating rate HR2 of at least 1°C / second. In a preferred embodiment, the heating rate HR2 for heating is at least 2°C / second, more preferably at least 5°C / second.
[0055] Cold-rolled steel sheets are maintained at TA2 for 10 to 5000 seconds to ensure 80% to 100% recrystallization.
[0056] Next, the cold-rolled steel sheet is cooled, starting from TA2, and the cold-rolled steel sheet is cooled to a temperature T2 in the range of 20°C to 300°C at a cooling rate CR2 of 1°C / sec to 150°C / sec. In a preferred embodiment, the cooling rate CR2 is 3°C / sec to 120°C / sec. A preferred T2 temperature is 20°C to 100°C.
[0057] The cold-rolled steel sheet obtained in this manner has a thickness of 0.3 mm to 0.38 mm, preferably 0.31 mm to 0.37 mm, and more preferably 0.33 mm to 0.37 mm.
[0058] Subsequently, the cold-rolled steel sheet is cooled to room temperature to obtain a double cold-rolled non-oriented electrical steel sheet.
[0059] The double cold-rolled non-oriented electrical steel sheet of the present invention may be optionally coated with an insulating material, an organic coating, an inorganic coating, or a combination thereof, in order to improve its insulating properties. [Examples]
[0060] The following tests, examples, symbolic illustrations, and tables presented herein are not limiting in nature and should be considered for illustrative purposes only, and illustrate advantageous features of the present invention.
[0061] Table 1 summarizes steel sheets made from steel with different compositions, and each steel sheet is manufactured according to the process parameters specified in Table 2. Subsequently, Table 3 summarizes the results of the evaluation of the obtained properties.
[0062] All steels in Table 1 had a nitrogen content of less than 0.09%.
[0063] Table 2 summarizes the hot rolling and annealing process parameters performed on cold-rolled steel sheets to impart the mechanical and magnetic properties necessary to become non-oriented electrical steel to the steels in Table 1. All steels of the present invention from I1 to I6 are cooled at a cooling rate of 15°C / second after hot rolling. Furthermore, in the embodiments of the present invention, the heating rate HR1 to TA1 temperature is 5°C / second. For all embodiments of the present invention, the T1 temperature is 25°C, and the cooling rate CR1 is 5°C / second. For all embodiments of the present invention, the heating rate HR2 to TA2 temperature is 5°C / second. For all embodiments of the present invention, the T2 temperature is 25°C, and the cooling rate CR2 is 5°C / second.
[0064] All steels manufactured according to the parameters in Table 2 exhibited over 95% recrystallization and a thickness of 20-110 μm. particle size Recrystallized fine particles organization This was shown.
[0065] [Table 1]
[0066] [Table 2]
[0067] Table 3 The results of various mechanical tests conducted in accordance with the standards are compiled. Ultimate tensile strength, total elongation, and yield strength were measured according to the NF EN ISO 6892-1 standard, and J50 magnetic properties and total iron loss at 1T and 400Hz were measured according to the IEC 60404-2 standard. Eddy current loss was measured in Giorgio, published in IEEE TRANSACTIONS ON MAGNETICS, Vol.24, No.1, January 1988. Bertotti The calculation is performed according to the Bertotti method, as published in the paper entitled "General Properties of Power Losses in Soft Ferromagnetic Materials". Equation 2 is what is called eddy current loss in this invention (P class Identify the classical loss represented by ).
[0068] Recrystallization fine organization Average particle size It is measured using the linear intercept method in accordance with the ASTM E112 96(02) standard.
[0069] [Table 3]
Claims
1. A double cold-rolled non-oriented electrical steel sheet having a thickness of 0.3 mm to 0.38 mm and having a composition consisting of the following elements, expressed in weight percent: 0.0001% ≤ Carbon ≤ 0.007% 0.1% ≤ Manganese ≤ 0.3% 3.1% ≤ Silicon ≤ 3.8% 0.6% ≤ Aluminum ≤ 0.8% Phosphorus ≤ 0.15% Sulfur ≤ 0.006% 0.01% ≤ Chromium ≤ 0.0335% 0.01%≦Copper≦0.0215% The remaining composition consists of iron and unavoidable impurities caused by the process, and the microstructure of the steel sheet is made from ferrite and consists of 80% to 100% recrystallized microstructure and 0% to 20% non-recrystallized microstructure in area fraction, with the grain size of the recrystallized microstructure being 20 to 110 microns, and also includes what is called eddy current loss, specified by Equation 2 of the Bertotti method, as described in Giorgio Bertotti's paper entitled "General Properties of Power Losses in Soft Ferromagnetic Materials" published in IEEE TRANSACTIONS ON MAGNETICS, Vol. 24, No. 1 in January 1988 (P class It has a percentage of eddy current loss in total iron loss measured at 1T and 400Hz according to the IEC 60404-2 standard, which is 40-50% when calculated according to the classical loss expressed by ), and simultaneously has magnetic polarization at 5000 A / m (J50) of 1.66T to 1.7T, and Double cold-rolled non-oriented electrical steel sheet having an ultimate tensile strength of at least 490 MPa in both the direction perpendicular to rolling and the rolling direction, as measured according to the NF EN ISO 6892-1 standard, a yield strength of at least 380 MPa in both the direction perpendicular to rolling and the rolling direction, as measured according to the NF EN ISO 6892-1 standard, a total elongation of at least 15% in both the direction perpendicular to rolling and the rolling direction, and a total loss of 15 to 18 W / kg when measured at 1 T and 400 Hz.
2. The double cold-rolled non-oriented electrical steel sheet according to claim 1, wherein the composition contains 3.2% to 3.7% silicon.
3. The double cold-rolled non-oriented electrical steel sheet according to claim 1, wherein the composition contains 0.002% to 0.007% carbon.
4. The double cold-rolled non-oriented electrical steel sheet according to claim 1, wherein the composition contains 0.6% to 0.75% aluminum.
5. The double cold-rolled non-oriented electrical steel sheet according to claim 1, wherein the composition contains 0.1% to 0.25% manganese.
6. The double cold-rolled non-oriented electrical steel sheet according to claim 1, wherein the amount of non-recrystallized microstructure is 0% to 10%.
7. The double cold-rolled non-oriented electrical steel sheet according to claim 1, wherein the amount of recrystallized microstructure is 90% to 100%.
8. The following are the sequential steps: - A step of providing a semi-finished product having the steel composition described in any one of claims 1 to 5; - A process of reheating the semi-finished product to a temperature of 1000°C to 1200°C; - A process of rolling the aforementioned semi-finished product, wherein the hot rolling finishing temperature is set to 840°C to 950°C to obtain a hot-rolled steel sheet. - A process of cooling the hot-rolled sheet immediately after the hot-rolling process is completed. Next, the hot-rolled steel sheet is cooled from the hot-rolling finish to a coiling temperature range of 500°C to 750°C at a cooling rate of at least 10°C / second and no more than 200°C / second. - Subsequently, the hot-rolled steel sheet is wound up within the winding temperature range of 500°C to 750°C. - A step of optionally performing a scale removal process on the hot-rolled steel sheet; - A process in which hot-rolled steel sheets are annealed at a temperature of 780°C to 1000°C for a period of 10 seconds to 96 hours; - A step of optionally performing a scale removal process on the hot-rolled steel sheet; - A process of cold-rolling the hot-rolled steel sheet at a reduction ratio of 60% to 95% to obtain an intermediate cold-rolled steel sheet; - Subsequently, the intermediate cold-rolled steel sheet is subjected to a first annealing process, wherein the heating for the first annealing process starts from room temperature and is performed at a heating rate HR1 of at least 1°C / second until it reaches a first annealing temperature range TA1 of 900°C to 1100°C. Next, a first annealing process is carried out at the TA1 temperature for 10 to 5000 seconds. Next, the intermediate cold-rolled steel sheet is cooled starting from the TA1 temperature and at a cooling rate CR1 of 1°C / sec to 150°C / sec, until it reaches a temperature T1 of 300°C to 20°C, thereby obtaining a cold-rolled steel sheet that has undergone the first annealing process. Subsequently, the cold-rolled steel sheet that has undergone the first annealing is subjected to cold rolling at a reduction ratio of 50% to 95% to obtain a cold-rolled steel sheet; - Subsequently, the cold-rolled steel sheet is subjected to a second annealing process, wherein the heating for the second annealing starts from room temperature and is performed at a heating rate HR2 of at least 1°C / second until it reaches an annealing temperature range TA2 of 900°C to 1100°C. Next, the process involves annealing at a TA2 temperature for 10 to 5000 seconds. Next, a process of cooling the cold-rolled steel sheet, starting from the TA2 temperature and reaching a temperature T2 of 300°C to 20°C at a cooling rate CR2 of 1°C / sec to 150°C / sec. Next, the process involves cooling to room temperature to obtain a double cold-rolled non-oriented electrical steel sheet. A method for manufacturing a double cold-rolled non-oriented electrical steel sheet according to any one of claims 1 to 7.
9. The method according to claim 8, wherein the TA1 temperature for annealing is 920°C to 1080°C.
10. The method according to claim 8, wherein the temperature T1 is 200°C to 20°C.
11. The method according to claim 8, wherein the cooling rate CR1 is 3°C / sec to 120°C / sec.
Citation Information
Patent Citations
Non-oriented electrical steel sheet and manufacturing method thereof
EP3173503A1
Non-oriented electrical steel sheet and method for manufacturing same
EP4079893A2
Non-oriented electrical steel sheet and method for manufacturing same
EP4265745A1
Non-oriented electrical steel sheet and method for manufacturing same
EP4265749A1
Non-oriented electrical steel sheet and method for producing same, and motor core and method for producing same
US20210371948A1