Inkjet printable UV-curable composition
Patent Information
- Application Number
- JP2026514953
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Filing Date
- 2023-09-14
- Publication Date
- 2026-11-24
AI Technical Summary
Existing UV-curable compositions for OLED displays face challenges in achieving low viscosity for inkjet printing while maintaining high refractive index and optical clarity, often requiring inorganic nanoparticles that increase viscosity and decrease clarity, and involve sulfur-containing monomers and solvents.
A solvent-free, UV-curable composition comprising aromatic (meth)acrylate compounds, bifunctional methacrylate compounds, and zirconium dioxide nanoparticles, with specific concentrations to achieve a viscosity of 10-25 mPa at 25°C, refractive index of at least 1.63, and high optical clarity, free from sulfur-containing monomers.
The composition maintains low viscosity and high refractive index, ensuring excellent optical clarity and durability, suitable for microlens structures in OLED displays, with over 95% transmittance after aging.
Abstract
Description
Field of Invention
[0001] The present invention relates to a substantially solvent-free, inkjet-printable, UV-curable composition. This composition comprises aromatic (meth)acrylate compounds and bifunctional methacrylate compounds. [Background technology]
[0002] Organic light-emitting diode (OLED) technology is replacing liquid crystal display (LCD) technology in the display market. However, the requirements for OLED materials suitable for the complex optical designs of current displays impose challenging demands on OLED materials. For example, the light extraction microlens design of OLED displays requires a UV-curable and inkjet-printable composition that is optically transparent and hardens into a coating having a high refractive index (RI) of at least 1.63, preferably greater than 1.630, at a wavelength of light of 633 nanometers.
[0003] One way to increase the RI of a composition is to include inorganic nanoparticles, as discussed in U.S. Publication No. 2020 / 0216697 ('697). '697 provides a curable high refractive index composition that is also inkjet printable. As described in '697, challenges associated with adding inorganic nanoparticles include an increase in viscosity to the point where the composition is no longer inkjet printable, and a decrease in the optical clarity of the resulting cured composition. '697 uses inorganic nanoparticles treated with a silane surface modifier, and the ability to obtain low viscosity and clarity is attributed to these surface modifiers. However, '697 is 30 millipascals in the range from room temperature to 60 degrees Celsius (°C). * seconds (mPa) * The target viscosity for inkjet printing is less than s. A more desirable but stringent viscosity target for inkjet printing is 10-25 mPa at a temperature of 25°C. * Examples of '697' containing more than 10 wt% inorganic nanoparticles (see IE13 and IE31 of '697) are 10-25 mPa.* It has a viscosity value well above the more challenging target of s. 10-25 mPa at 25°C. * It is desirable to provide a curable high refractive index composition having a viscosity in the range of less than s and also containing more than 10% by weight of inorganic nanoparticles.
[0004] Several references, including International Publication No. WO2018122748 and Chinese Patent No. 109952663, disclose photocurable compositions that require sulfur-containing photocurable monomers. It is desirable to avoid the need to use sulfur-containing photocurable monomers, and if this can be done, the art will advance.
[0005] Furthermore, in order to reduce or eliminate volatile organic compounds during processing, it is desirable to minimize or eliminate the presence of solvents in the photocurable composition. [Overview of the project]
[0006] This invention relates to 10-25 mPa at 25°C. * The present invention provides a substantially solvent-free, inkjet-printable, UV-curable composition having a viscosity in the range of less than s, containing 20% by weight or more of inorganic nanoparticles, substantially free of sulfur-containing photocurable monomers, curing to a composition having an RI value of at least 1.63, typically greater than 1.630, using light at a wavelength of 633 nm, and exhibiting an aged average transmittance (%T) of at least 95% through a 20-micrometer thick film over a wavelength range of 380-780 nm, even after aging for 500 hours at 85°C and 85% relative humidity. The composition may be substantially free, or even completely free, of sulfur-containing photocurable monomers.
[0007] In the first aspect, the present invention is substantially solvent-free, UV-curable, and curable at 10-25 mPa at 25°C. * A composition having a viscosity in the range of less than s, and an aromatic (meth)acrylate material having the following structure (I): H2C=C(R 1 )C(O)-OR2 -CH2-R (I) (wherein R is a biphenyl group or a naphthyl group, R 1 is hydrogen or a methyl group, and R 2 is selected from the group consisting of a single bond, C 2~10 divalent hydrocarbon, C 2~10 polyethylene, and C 3~10 polypropylene); and (b) 10 to 25 weight percent of a difunctional methyl acrylate having the following structure (II): H2C=C(CH3)C(O)-O-R 3 -O-C(O)C(CH3)=CH2 (II) (wherein R 3 is selected from the group consisting of a single bond, C 2~10 divalent hydrocarbon, C 2~10 polyethylene, and C 3~10 polypropylene); and (c) zirconium dioxide nanoparticles having an average particle size in the range of 1 to 20 nanometers as determined by dynamic light scattering, and present at a concentration of 20 weight percent or more, with the proviso that the concentration of zirconium dioxide nanoparticles in the composition is within the weight percent range bounded by (i) 1.23 (weight percent of difunctional methyl acrylate (b)) + 1.60 weight percent and (ii) 1.09 (weight percent of difunctional methyl acrylate (b)) + 26.02 weight percent; and (d) 0.1 to 6.0 weight percent of a photoinitiator; and (e) 0 to 6.0 weight percent of a trifunctional methyl acrylate; and (f) 0 to 1.0 weight percent of a surfactant; a composition comprising the above components, wherein the weight percent values are based on the weight of the composition.
[0008] In a second aspect, the present invention is a method of applying the composition according to any one of the claims, comprising depositing the composition according to any one of the claims onto a substrate by inkjet deposition.
[0009] The composition of the present invention is suitable for use as a component in a microlens structure for light extraction in an OLED layer structure. Mode for Carrying Out the Invention
[0010] Unless a date is indicated together with the number of a test method, the test method refers to the latest test method as of the priority date of the present document. References to a test method include both references to the testing association and the test method number. As used herein, the following abbreviations and identifiers for test methods apply: ASTM refers to test methods of the American Society for Testing and Materials, EN refers to European Norm, DIN refers to Deutsches Institut fur Normung, ISO refers to the International Organization for Standards, and UL refers to Underwriters Laboratory.
[0011] Products identified by trade names refer to compositions available under those trade names as of the priority date of the present document.
[0012] "Multiple" means two or more. "And / or" means "and, or as an alternative". All ranges include endpoints unless otherwise specifically indicated.
[0013] C x~y type names refer to having from x to y carbon atoms.
[0014] "Substantially free" means that the content of the specified component is less than 5 weight percent (wt%), preferably less than 4 wt%, more preferably less than 3 wt%, less than 2 wt%, less than 1 wt%, less than 0.5 wt%, wherein the weight percentage is based on the weight of the composition. "Substantially free" does not require that the specified component is completely absent.
[0015] Unless otherwise specified, weight percent (wt%) in the present specification is based on the weight of the composition.
[0016] "Solvent" refers to a non-polymerizable organic material having a boiling point of 120°C or lower at a pressure of 101 kilopascals.
[0017] "(Meth)acrylate" refers to acrylate, methacrylate, or a combination of an acrylate compound and a methacrylate compound.
[0018] In a first aspect, the present invention provides a composition that is substantially free of solvents, is ultraviolet-curable, and has a viscosity at 25°C in the range of 10 to 25 millipascals * second (mPa * s) of less than
[0019] "Substantially free of solvent" means that the composition contains less than 5% by weight, preferably less than 4% by weight, more preferably less than 3% by weight, less than 2% by weight, less than 1% by weight, and less than 0.5% by weight of non-polymerizable organic material having a boiling point of 120°C or lower at a pressure of 101 kilopascals, and may contain none. Wt% is based on the weight of the composition.
[0020] "Ultraviolet-curable" means that components in the composition undergo a crosslinking reaction when exposed to ultraviolet light. It is desirable to achieve more than 90%, preferably 95% or more curing after exposure to 365 nm light at a dose of 2 joules per square centimeter.
[0021] Viscosity relating to the composition refers to the viscosity of the composition before curing. The viscosity of the composition is determined using an AR2000ex rheometer manufactured by TA Instruments, with a 40 millimeter aluminum plate, a shear rate of 100 s -1 , a temperature range of 20 to 50°C, and a heating rate of 3°C per minute. Unless otherwise specified, viscosity values herein correspond to the viscosity at 25°C.
[0022] The composition of the present invention comprises (a) an aromatic (meth)acrylate material, (b) a bifunctional methacrylate, (c) zirconium dioxide (ZrO2) nanoparticles, (d) a photoinitiator, optionally (e) a trifunctional methyl acrylate, and optionally (f) a surfactant. Preferably, the composition of the present invention is substantially free of sulfur-containing photocurable components, and preferably does not contain any sulfur-containing substances. The composition may be completely free of sulfur-containing substances.
[0023] (a) Aromatic (meth)acrylate materials Aromatic (meth)acrylate materials have chemical structure (I): H2C=C(R 1 )C(O)-OR 2 -CH2-R (I) (In the formula, R is a biphenyl group or a naphthyl group, R 1 R is a hydrogen or methyl group, 2 C is a single bond. 2~10 Divalent hydrocarbons, C 2~10 Polyethylene, and C 3~10 (Selected from the group consisting of polypropylene).
[0024] The aromatic (meth)acrylate material may be either 4-biphenylmethyl acrylate or naphthalene-1-ylmethyl acrylate, or both. The composition may not contain α-naphthyl acrylate.
[0025] Typically, the concentration of aromatic (meth)acrylate material is 70% by weight or less, 60% by weight or less, 50% by weight or less, and even 40% by weight or less, based on the weight of the composition, but at the same time, it is typically 25% by weight or more, preferably 30% by weight or more, 40% by weight or more, and even 50% by weight or more.
[0026] (b) Difunctional methacrylate The bifunctional methacrylate has chemical composition (II): H2C=C(CH3)C(O)-OR 3-OC(O)C(CH3)=CH2(II) (In the formula, R 3 C is a single bond. 2~10 Divalent hydrocarbons, C 2~10 Polyethylene, and C 3~10 (Selected from the group consisting of polypropylene). An example of a suitable bifunctional methacrylate is ethylene glycol dimethacrylate.
[0027] The concentration of the bifunctional methacrylate is typically 10% by weight or more, preferably 12% by weight or more, and may be 15% by weight or more, 17% by weight or more, or even 20% by weight or more, relative to the weight of the composition, but at the same time, it is typically 25% by weight or less, and may be 22% by weight or less, 20% by weight or less, or even 18% by weight or less.
[0028] (c) Zirconium dioxide nanoparticles Zirconium dioxide (ZrO2) nanoparticles, as determined by dynamic light scattering, have an average particle size of 1 nanometer (nm) or larger, preferably 2 nm or larger, 3 nm or larger, 4 nm or larger, 5 nm or larger, 6 nm or larger, 7 nm or larger, and even 8 nm or larger, 9 nm or larger, and even 10 nm or larger, while typically being 20 nm or smaller, 18 nm or smaller, 16 nm or smaller, 14 nm or smaller, 12 nm or smaller, and even 10 nm or smaller. Generally, ZrO2 nanoparticles can have any shape, but are preferably spherical.
[0029] The concentration of ZrO2 nanoparticles in the composition is 20% by weight or more, and may be 30% by weight or more, 35% by weight or more, and even 40% by weight or more, but at the same time, it is typically 50% by weight or less, and may be 45% by weight or less, 40% by weight or less, 35% by weight or less, and even 30% by weight or less, however, the concentration of ZrO2 nanoparticles is (i) 1.23 (weight percent of difunctional methyl acrylate (b)) + 1.60 weight percent, and (ii) The range enclosed by 1.09 (weight percent of difunctional methyl acrylate (b)) + 26.02 weight percent, preferably the range is (i) 1.23 (weight percent of difunctional methyl acrylate (b)) + 2.94 weight percent, and (ii) 1.09 (weight percent of difunctional methyl acrylate (b)) + 26.02 weight percent, The weight percentage is relative to the weight of the composition. When the concentration of ZrO2 nanoparticles exceeds 1.09 (weight percentage of difunctional methyl acrylate (b)) + 26.02 weight percent, the viscosity of the composition is 25 mPa. * There is a tendency for the refractive index to exceed s. When the concentration of ZrO2 nanoparticles is less than 1.23 (weight percent of difunctional methyl acrylate (b)) + 1.60 weight percent, the refractive index of the composition tends to be less than 1.63. When the concentration of ZrO2 nanoparticles is less than 1.23 (weight percent of difunctional methyl acrylate (b)) + 2.94 weight percent, the refractive index of the composition tends to be less than 1.630.
[0030] (d) Photoinitiator In the broadest scope of the present invention, the photoinitiator may be any one photoinitiator useful for curing using ultraviolet light, any combination of photoinitiators, or more than one photoinitiator.
[0031] The photoinitiator may be, for example, one component selected from the group consisting of benzophenone and benzophenone derivatives, acetophenone and acetophenone derivatives, benzoin and its alkyl esters, phosphine oxide derivatives, xanthone derivatives, oxime ester derivatives, and camphorquinone, or a combination of one or more components.Suitable commercially available photopolymerization initiators include 2,6-bis(4-azidobenzylidene)cyclohexanone, 2,6-bis(4-azidobenzylidene)-4-methylcyclohexanone, 1-hydroxyl-cyclohexyl-phenyl-ketone (available under the name OMNIRAD® 184), 2-methyl-1[4-(methylthio)phenyl]-2-morpholinopropan-1-one (available under the name OMNIRAD® 907), 2-hydroxy-2methyl-1-phenyl-propan-1-one (available under the name OMNIRAD® 1173), 2-hydroxy-1-[4-(2-hydroxyethoxy)phenyl]-2-methyl-1-propanone (available under the name OMNIRAD® 2959), and methylbenzoylformate (OMNIRAD® Available under the name MBF, α,α-dimethoxy-α-phenylacetophenone (available under the name OMNIRAD651), 2-benzyl-2-(dimethylamino)-1-[4-(4-morpholinyl)phenyl]-1-butanone (available under the name OMNIRAD369), diphenyl(2,4,6-trimethylbenzoyl)phosphine oxide (available under the name OMNIRAD TPO), ethyl(2,4,6-trimethylbenzoyl)phenylphosphineate (available under the name OMNIRAD TPO-L), and oxime ester compounds (Adeka Examples include any one or more combinations selected from the following (available from the Corporation as products N-1919, NCI-831, NCI-930, NCI-730 and NCI-100): 12-thioxanthene-9-one, 10-methylphenothiazine, isopropyl-9H-thioxanthene-9-one; 2,4-diethyl-9H-thioxanthene-9-one, 2-chlorothioxanthene-9-one; 1-chloro-4-propoxy-9H-thioxanthene-9-one; 2-methyl-4'-(methylthio)-2-morpholinopropiophenone, 2-isopropylthioxanthone, 1-[4-(phenylthio)phenyl]-1,2-octanedione 2-(o-benzoyloxime), and 2-hydroxy-2-methylpropiophenone. OMNIRAD is a trademark of IGM Group BV.
[0032] The concentration of the photoinitiator in the composition is typically 0.1% by weight or more, and may be 0.2% by weight or more, 0.3% by weight or more, 0.4% by weight or more, 0.5% by weight or more, 0.6% by weight or more, 0.8% by weight or more, 0.9% by weight or more, 1.0% by weight or more, 1.2% by weight or more, 1.4% by weight or more, 1.6% by weight or more, 1.8% by weight or more, 2.0% by weight or more, 2.5% by weight or more, 3.0% by weight or more, 3.5% by weight or more, 4.0% by weight or more, 4.5% by weight or more, and even 5.0% by weight or more. At the same time, it is typically 6.0% by weight or less, and may be 5.0% by weight or less, 4.0% by weight or less, 3.0% by weight or less, 2.0% by weight or less, 1.5% by weight or less, 1.0% by weight or less, and even 0.9% by weight or less, where weight percent is relative to the weight of the composition.
[0033] (e) Trifunctional methyl acrylate The composition may contain one or more trifunctional methyl acrylates. Trifunctional methyl acrylates can increase the curing amount while keeping the viscosity of the composition low. An example of a suitable trifunctional methyl acrylate is trimethylolpropane trimethacrylate. The concentration of the trifunctional methyl acrylate may be 0% by weight or more, 0.5% by weight or more, 1.0% by weight or more, 1.5% by weight or more, 2.0% by weight or more, 3.0% by weight or more, 4.0% by weight or more, and even 5.0% by weight or more, based on the weight of the composition, but at the same time typically 6.0% by weight or less, 5.0% by weight or less, 4.0% by weight or less, 3.0% by weight or less, 2.0% by weight or less, and even 1.0% by weight or less.
[0034] (f) Surfactants The composition may consist of one surfactant or any combination of one or more surfactants. Surfactants are useful for increasing the film-forming and leveling properties of the composition on the substrate. Preferably, the surfactant is selected from the group consisting of silicone polyether surfactants and acrylate-modified silicone polyether surfactants. Examples of suitable surfactants include those commercially available from BYK as BYK-378 and BYK-UV3575. The concentration of the surfactant is 0% by weight or more, and may be 0.1% by weight or more, 0.2% by weight or more, 0.3% by weight or more, 0.4% by weight or more, 0.5% by weight or more, 0.6% by weight or more, 0.7% by weight or more, 0.8% by weight or more, and even 0.9% by weight or more, but at the same time, it is typically 1.0% by weight or less, and may be 0.9% by weight or less, 0.8% by weight or less, 0.7% by weight or less, 0.6% by weight or less, 0.5% by weight or less, 0.4% by weight or less, 0.3% by weight or less, 0.2% by weight or less, or even 0.1% by weight or less.
[0035] In a second aspect, the present invention is a method for use in a composition of the first aspect of the present invention. The method of the present invention is a method of coating the composition of the present invention by arranging it on a substrate by inkjet deposition (inkjet printing). This method may further include curing the composition on the substrate by exposing it to ultraviolet light. [Examples]
[0036] Table 1 lists the components used in the preparation of the following examples.
[0037] [Table 1]
[0038] PixClear is a trademark of Pt SPE Subco, LLC.
[0039] Synthesis of naphthalene-1-ylmethyl acrylate In a 500 ml (mL) round-bottom, three-necked flask equipped with a stirrer, 15.82 g of 1-naphthalenemethanol (Sigma Aldrich) was dissolved in 200 mL of dichloromethane (Sigma Aldrich). The contents of the flask were cooled to 0°C while constantly stirring. 20.9 mL of triethylamine (MilliporeSigma) was added. 12.2 mL of acryloyl chloride (Sigma Aldrich) was added dropwise over 30 minutes with stirring. The contents of the flask were warmed to 25°C over 12 hours. The contents of the flask were washed with water. The resulting organic phase was dried over sodium sulfate (Sigma Aldrich) and concentrated under vacuum. The resulting product was purified by column chromatography to produce naphthalene-1-yl methyl acrylate, a colorless liquid product.
[0040] Synthesis of α-naphthyl acrylate In a 500 mL round-bottomed, three-necked glass flask equipped with a stirrer, 14.42 g of 1-naphthol (MilliporeSigma) was dissolved in 200 mL of dichloromethane (Sigma Aldrich). The contents of the flask were cooled to 0°C while constantly stirring. 20.9 mL of triethylamine (MilliporeSigma) was added. 12.2 mL of acryloyl chloride (Sigma Aldrich) was added dropwise over 30 minutes with stirring. The contents of the flask were warmed to 25°C over 12 hours. The contents of the flask were washed with water. The resulting organic phase was dried over sodium sulfate (Sigma Aldrich) and concentrated under vacuum. The resulting product was purified by column chromatography to produce α-naphthyl acrylate, a colorless liquid product.
[0041] Isolation of ZrO2 nanoparticles ZrO2 nanoparticles are isolated from the ethyl acetate in which they are dispersed as PCPB-2-50-ETA by removing the ethyl acetate under vacuum for 20-30 minutes.
[0042] Preparation and characterization of samples of curable compositions To prepare the following samples, first isolate the ZrO2 nanoparticles from ethyl acetate and weigh out the specified amount of the sample. Add the other components for the specific sample and mix to form a clear solution of the curable composition.
[0043] First, a cured sample of the composition is prepared by spin-coating the curable composition onto bare glass at a speed of 500 revolutions per minute (RPM) for 20 seconds, or onto a single-crystal silicon wafer at a speed of 6000 RPM for 20 seconds. Next, the spin-coated sample is exposed to 365 nm light at a dose of 2 joules / cm² to cure the composition.
[0044] The obtained samples are characterized using four methods.
[0045] (i)UV curing ability The ability to cure using ultraviolet (UV) light is determined by curing the spin-coated film of the sample as described above, and then determining the degree of curing. For satisfactory curing, more than 90% of the composition needs to be cured. The degree of curing is evaluated by Fourier transform infrared spectroscopy (FTIR) using a Perkin Elmer Spectrum Frontier with a Diamond ATR. The sample to be analyzed is placed on a diamond / ZnSe crystal, sufficient pressure is applied to obtain contact, and then an ATR-FTIR spectrum is collected over 400–650 wavenumbers. Each sample is scanned eight times, and the spectra are averaged. The FTIR setup is 4.0 wavenumber resolution, "strong" apodization, a scanning speed of 0.20 cm / second, and an MIR TGS detector.
[0046] The peak in the wavenumber range of 1644–1627 is C=C. The peak in the wavenumber range of 1766–1658 is C=O. Using FTIR software, the peak areas are calculated in the wavenumber ranges of 1646–1625 and 1768–1654, respectively, as baselines for C=C and C=O. Since the signal of the C=C group decreases during UV curing, while the signal of the C=O group remains unchanged, the ratio of the peak areas of C=C and C=O provides an indicator of the curing percentage. Therefore, the curing percentage can be calculated by dividing the peak area of C=C by the peak area of C=O and multiplying by 100.
[0047] UV curing ability is reported as a curing percentage, and curing percentages exceeding 90% are acceptable.
[0048] (ii) Viscosity at 25°C The viscosity of the sample composition before curing was determined using a TA Instrument AR20000ex rheometer (shape: 40 mm aluminum plate, shear rate of 100 s⁻¹). Viscosity was measured at 25°C. The result was 25 mPa. * Less than s, preferably 10-25 mPa * Viscosities in the range of less than s are acceptable.
[0049] (iii) Refractive index at 633 nm light Spin coating and curing should yield a cured film with a thickness of approximately 20 micrometers. The thickness will be determined by examining the cross-section of the cured film using a Hitachi S-34000N scanning electron microscope. The film thickness will be determined using the scanning electron microscope's operating software.
[0050] The refractive index (RI) is determined using 633nm light and a HORIBA UVISEL Plus ellipsometer. An RI value of at least 1.63, preferably 1.630 or higher, is acceptable.
[0051] (iv) Transmittance %.
[0052] After aging the sample at 85°C for 500 hours, the transmittance %(%T) of the spin-coated, cured sample with a thickness of 20 micrometers is determined. Using a Shimadzu UV3600 spectrophotometer, %T is measured through the aged sample over a wavelength range of 350–800 nm. The %T is averaged over light wavelengths of 380–780 nm and reported as the sample's %T. A %T exceeding 95% is acceptable.
[0053] result Tables 2 and 3 show the formulations of the curable composition samples, with the amounts of each component in grams. Tables 2 and 3 also show the results of the characterization of the samples.
[0054] A comparison of samples 1-4 and sample 22 revealed that acceptable curing can be obtained when the photoinitiator concentration is 0.1-6.0% by weight relative to the weight of the composition, but unacceptable when the concentration is less than 0.1% by weight.
[0055] Comparison of samples 13 and 14 with samples 23 to 25 revealed that ZrO2 nanoparticles, bifunctional methacrylate, or aromatic (meth)acrylate materials are necessary to achieve the desired viscosity and RI. Sample 23 shows that the sample without ZrO2 nanoparticles has an RI of less than the desired value of 1.63. Sample 24 shows that the sample without bifunctional methacrylate has an RI of less than the desired 25 mPa. * This indicates that the viscosity is greater than less than s. Sample 25 revealed that samples without aromatic (meth)acrylate materials have the desired RI value of less than 1.63. In contrast, samples 13 and 14, which have similar compositions to samples 23 to 25, achieve the desired viscosity and RI value.
[0056] As shown in samples 26 and 27, it is important that at least one CH2 bond is present between the aromatic group and the oxygen of the (meth)acrylate group in the aromatic (meth)acrylate material. The absence of a CH2 bond (component (a)'-1) results in an unacceptable %T value, and similar examples having a structure containing at least one CH2 bond achieve the desired properties.
[0057] It is important that aromatic (meth)acrylate systems have either biphenyl or naphthyl as the aromatic group. For example, a single phenyl group does not act with biphenyl as shown in sample 28, and a tricyclic structure does not act as shown in sample 29.
[0058] As shown in Sample 6 compared to Sample 30, the composition of the bifunctional methacrylate is also important. The target properties are achieved when ethylene glycol dimethacrylate is used, but not when dipropylene glycol diacrylate is used.
[0059] [Table 2]
[0060] [Table 3] * NM means "not measured" because one of the other results was outside the desired range of values.
Claims
1. It is substantially solvent-free, UV-curable, and has a pressure of 10-25 mPa at 25°C. * A composition having a viscosity in the range of less than s, (a) Structure (I): H 2 C = C(R 1 ) C(O)-O-R 2 -CH 2 Aromatic (meth)acrylate materials having -R (I) (In the formula, R is a biphenyl group or a naphthyl group. R 1 is a hydrogen or methyl group, R 2 represents a single bond, C 2~10 divalent hydrocarbon, C 2~10 polyethylene, and C 3~10 selected from the group consisting of polypropylene), and (b) 10 to 25 weight percent of the following structure (II): H 2 C = C(CH) 3 ) C(O)-O-R 3 -O-C(O)C(CH 3 ) = CH 2 (II) Difunctional methyl acrylate (In the formula, R 3 C is a single bond. 2~10 Divalent hydrocarbons, C 2~10 Polyethylene, and C 3~10 (Selected from the group consisting of polypropylene) (c) Zirconium dioxide nanoparticles having an average particle size in the range of 1 to 20 nanometers when determined by dynamic light scattering and present at a concentration of 20 weight percent or more, provided that the concentration of zirconium dioxide nanoparticles in the composition is within the weight percent range enclosed by (i) 1.23 (weight percent of difunctional methyl acrylate (b)) + 1.60 weight percent and (ii) 1.09 (weight percent of difunctional methyl acrylate (b)) + 26.02 weight percent, (d) 0.1 to 6.0 weight percent of a photoinitiator, (e) 0 to 6.0 weight percent of a trifunctional methyl acrylate, (f) comprising 0 to 1.0 weight percent of a surfactant, The weight percentage value is relative to the weight of the composition.
2. The composition according to claim 1, wherein the composition substantially does not contain a sulfur-containing photocurable component.
3. The aforementioned composition comprises the following components: Trifunctional methyl acrylate and surfactant The composition according to claim 1 or 2, further comprising one or both of the above.
4. The composition according to any one of claims 1 to 3, wherein the trifunctional methyl acrylate is trimethylolpropanetrimethacrylate.
5. The composition according to any one of claims 1 to 4, wherein the surfactant (f) is selected from the group consisting of silicone polyether surfactants and acrylate-modified silicone polyether surfactants.
6. The composition according to any one of claims 1 to 5, wherein the difunctional methyl acrylate is ethylene glycol dimethacrylate.
7. The composition according to any one of claims 1 to 6, wherein the nanoparticles are zirconium dioxide and have an average size in the range of 1 to 10 nanometers when determined by dynamic light scattering.
8. The composition according to any one of claims 1 to 7, wherein the (meth)acrylate material is selected from 4-biphenylmethyl acrylate and naphalen-1-ylmethyl acrylate.
9. A method for applying the composition according to any one of claims 1 to 8, wherein the method comprises depositing the composition according to any one of claims 1 to 8 onto a substrate by inkjet deposition.