Red metallic latex products

JP2026531367A5Pending Publication Date: 2026-11-20SUN CHEMICAL CORP +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026510074
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-08-17
Filing Date
2024-08-16
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing methods for achieving a true red metallic luster in latex products, such as gloves and balloons, fail to produce the desired color without complex procedures and higher costs, as aluminum pigments shift colors to bluish-red tones.

Method used

A formulation using iron oxide-coated aluminum in combination with red, purple, or orange pigments in a single-layer latex product, achieving a true red metallic luster with specific color dimensions and flop index values.

Benefits of technology

The solution provides a cost-effective and efficient method to achieve a true red metallic luster in latex products, reducing production complexity and costs while maintaining color stability.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2025037020000001
    Figure 2025037020000001
  • Figure 2025037020000002
    Figure 2025037020000002
  • Figure 2025037020000003
    Figure 2025037020000003
Patent Text Reader

Abstract

The present application relates to a latex or a latex product having a red metallic surface finish, wherein the red metallic surface finish embedded in the latex product at least on the surface thereof is (a) one or more metallic fillers comprising metal and / or metal oxide particles, and (b) one or more red, violet and / or orange absorbing pigment particles comprising said metallic surface finish has a red metallic effect having the following properties: a * = 25 to 80 (at 45°) b * = 10 to 40 (at 45°) Flop index (FI) according to formula (1): FI≧9.0.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a latex product having a red metallic surface finish and a method for manufacturing the same. [Background technology]

[0002] Latex product manufacturers want to differentiate their products, such as gloves, balloons, and other elastomer consumer products, for decorative or functional purposes. A metallic appearance is particularly desirable for many of these latex products, and this metallic appearance can be achieved in a variety of colors. These colors are obtained by combining aluminum pigments and absorbent pigments. A preferred method involves mixing an organic pigment dispersion of the desired color with an aluminum pigment preparation in a latex vat, and then using this mixture in a typical molding process for the desired latex product. The resulting latex product retains its metallic luster along with its absorbent color once fully cured. However, this method does not work for reddish tones. The blue reflection of aluminum shifts the color to a very bluish-red, resulting in a magenta appearance regardless of the pigment's hue. To achieve a true red, latex product manufacturers need to produce a two-layer product. By using an aluminum metallic layer as the inner layer and a red layer as the outer layer, blue reflection is minimized, making it possible to obtain a true red. However, compared to single-layer processes, such processes impose more complex procedures, longer production times, and higher costs on latex product manufacturers. One area where this problem is particularly evident is the manufacture and decoration of latex balloons, but this application is also applicable to other latex products. Other applications of the present invention include erasers, condoms and pessaries, rubber household gloves, medical gloves, beach toys and other novelty items, catheters, dental products (wedges, orthodontic rubber bands), and elastic for clothing.

[0003] US2019 / 0192984 discloses an inflatable balloon made from a latex composition. Said composition comprises latex, passivated flakes made from metals such as aluminum, nickel, iron, copper, lead, zinc, chromium, tin, or metal alloys, and a metal chelate complex.

PRIOR ART DOCUMENT

PATENT DOCUMENT

[0004]

Patent Document 1

Summary of the Invention

Problem to be Solved by the Invention

[0005] Conventionally, it has been impossible to achieve true red using aluminum in latex products. In order to solve this problem, the present inventors have found that a true red metallic luster effect can be obtained by using iron oxide-coated aluminum in combination with a red pigment. The present application provides a formulation that achieves true red with metallic luster demanded by latex product manufacturers.

Means for Solving the Problem

[0006] Accordingly, the present invention relates to a latex product having a red metallic surface finish, wherein the red metallic surface finish, embedded in the latex product at least on the surface thereof, comprises: (a) one or more metallic fillers comprising metal and / or metal oxide particles, and (b) one or more red, purple and / or orange color-absorbing pigment particles comprising The metallic surface finish has a red metallic effect having the following characteristics: a * = 25 to 80 (at 45°) b * = 10 to 40 (at 45°) Flop index (FI) according to formula (1): FI≧9.0

Numerical Formula

[0007] The Lab color system is an opponent color space that comprises a dimension L representing lightness, and opponent color dimensions a * and b * representing red-green and blue-yellow, respectively.

[0008] L * 15, L * 110, L * 45 are color measurement values at respective viewing angles, measured by "BYK-mac i", and the FI value is automatically calculated using the above formula.

[0009] BYK-mac i objectively measures color tone, sparkle and graininess under different viewing angles. It further detects and quantifies fluorescent light in the visible light range, and has the following features: Overall color impression: - 5-angle color measurement for light-dark difference evaluation: 15° / 25° / 45° / 75° / 110° - Additional color measurement behind the glossy surface for analyzing color flop: -15° - Sparkle and graininess measurement for flake characteristic evaluation - Detection and quantification of fluorescent light excited in the visible light range (luminescence intensity) Color measurement: Color geometry 45° illumination; -15°, 15°, 25°, 45°, 75°, 110° diffuse viewing Measurement area: 23 mm in diameter Spectral range: colorimetric measurement 400~700 nm, resolution 10 nm Measurement range: reflectance 0~600% Color reproducibility: 0.01ΔE * (10 consecutive measurements on white) Color reproducibility gray BCRA II tile: average ΔE *<0.10, Chromaticity BCRA II Tile: Average ΔE * <0.25 Color scale: ΔE * ;ΔE CMC;ΔE 94;ΔE 2000;ΔE 99;ΔE DIN6175-2019 and customer specification scale Color index: Flop, Int-Em Light source:A;C;D50;D65;F2;F7;F11;F12;CIE 015:2018 LED Observer 2°, 10° Effectiveness measurement: Effect geometry: 15°, 45°, 75°, and diffuse illumination; vertical observation by camera. Effect parameters: ΔS; ΔS_a; ΔS_i; ΔG Reproducibility effect: S_a / S_i: 5% or >0.50 / G = ±0.05 Reproducibility effect: S_a / S_i: 10% or >1.00 / G = ±0.15.

[0010] Furthermore, the object of the present invention is achieved by a method for producing a latex product having a red metallic surface finish as described in any of the prior claims, the method being A liquid or fluid natural and / or synthetic latex is mixed with (a) one or more metal fillers containing metal and / or metal oxide particles, and (b) one or more red, purple and / or orange color-absorbing pigment particles to form a red metallic surface finish, or a particulate composition containing (a) and (b), and a latex product is formed from the mixture obtained thereby, so that the red metallic surface finish is embedded in the latex product at least on its surface and has a red metallic effect. Alternatively, a latex product is first formed from a liquid or fluid natural and / or synthetic latex, and then the dried product is coated with a mixture of the liquid or fluid natural and / or synthetic latex and (a) one or more metal fillers containing metal and / or metal oxide particles, and (b) a red metallic surface finish containing one or more red, purple and / or orange color-absorbing pigment particles, or a particle composition containing (a) and (b), and a latex coating is formed on the latex product from the mixture, so that the red metallic surface finish is embedded in the latex product at least on its surface and has a red metallic effect. It is carried out by [the specified method].

[0011] Preferably, the particulate composition comprising a liquid or fluid latex and / or (a) and (b) is preferably in water and comprises water and one or more auxiliary agents, the auxiliary agents being selected from the group consisting of non-silicone defoamers, polyalkylene glycols, nonionic surfactants, preferably alcohol ethoxylates, rheology modifiers, and preferably acrylic polymers and / or acrylic copolymer emulsions.

[0012] The object of the present invention is further achieved by the red metal latex product obtained by the above method.

[0013] The object of the present invention is further, (a) One or more metal fillers comprising metal and / or metal oxide particles as defined in any one of claims 1 to 11, and (b) One or more red, purple and / or orange absorbing pigment particles as defined in any one of claims 1 to 11 This is achieved by a particle composition containing, Here, the particle composition produces a red metallic surface finish on at least the surface of a latex product containing the particle composition, and the metallic surface finish in the latex product has the following characteristics: a * =25~80 (at 45°) b *=10~40 (at 45°) The flop exponent (FI) according to equation (1) is FI ≥ 9.0.

number

[0014] Furthermore, the object of the present invention is achieved by a method of using the particle composition as a red metallic surface finish on at least a portion of the surface of a latex product, and by using the above-defined particle or pigment dispersion for coloring photosensitive resist formulations for the manufacture of color filters, printing inks, liquid inks, coating compositions, paints, plastics, films or fibers, wherein the metallic surface finish on the latex product exhibits a red metallic effect having the above-described properties.

[0015] Furthermore, the object of the present invention is achieved by a particle or pigment dispersion comprising the particle composition defined above, and further comprising a polymer dispersant.

[0016] The Paliochrome lineup includes two types of aluminum flakes: one is the "cornflake type," and the other is the "silver dollar type."

[0017] Regarding particle size, D50 is 10 to 22 microns, preferably 20 microns. PALIOCROM GOLD L2158 (NV 72.5%) has a particle size D50 of 17 microns, and the paste composition is aluminum (approximately 28%), silicon dioxide (approximately 13%), iron oxide (approximately 32%), and solvent (approximately 27%). [Modes for carrying out the invention]

[0018] The inventors have discovered that true red can be achieved in a single-layer latex material by changing the metallic hue from a silvery aluminum pigment to a metallic pigment in the gold, red, or orange color space, preferably in a multilayer structure. Such pigments, which are component (a) metal and / or metal oxide particles according to the present invention, are preferably designed in combination with a substrate material and a substrate material coated with one or more metal oxides having a refractive index different from that of the substrate, or include such a substrate material. For example, by coating an aluminum substrate with iron oxide (Fe2O3), particles (a) can be given black, brown, gold, red, orange, or yellow. Alternatively, or preferably additionally, one or more other coating layers may be present, such as SiO2, TiO2, SnO2, ZnO, Al2O3, and / or other metal oxides well known to those skilled in the art. Other substrates can also be used, such as mica, glass, Al2O3, copper, silver, nickel, stainless steel, and alloys of various metals such as zinc and copper. The coating is preferably 5 to 95, more preferably 10 to 80, and most preferably 20 to 70% by mass, based on the coated pigment (a) or the substrate of the coated pigment (a).

[0019] The shape of pigment (a) can be freely selected. Preferably, the pigment is thinner in one direction than in the other two directions. Preferably, the shape is sheet-like, coin-like, (corn) flake-like, or confetti-like. Silver coin-like and (corn) flake-like shapes are particularly preferred.

[0020] The particle size D50 is preferably 5 to 100, more preferably 10 to 50, most preferably 10 to 35 microns, for example 10 to 22 microns, preferably 15 to 22, most preferably 17 to 20 microns (micrometers).

[0021] The production of latex for balloons, gloves, and other products is typically carried out in aqueous latex tanks. Before forming the latex product in a mold, the pigment must be completely dispersed in the latex tank. This formation is achieved by immersing the mold in the latex solution. The color of the pigment in the latex solution must remain stable over a long period. Therefore, the pigment is supplied as a preparation that maximizes the color tone of the final latex product.

[0022] The pigment of type (a) described above must be compatible with the latex solution and other components in the tank. Furthermore, the pigment should maintain its color value after being added to the tank. For this purpose, surface treatment with stabilizers is preferred to extend the stability of the pigment in the latex solution. Such stabilizer surface treatments include, but are not limited to, polymer encapsulation, silica encapsulation, and passivation with molybdic acid, vanadium, chromium, phosphate esters, phosphonic acid, and other chemicals well known to those skilled in the art. Other useful passivation chemicals include amines, carboxylic acids, organophosphate esters, and polymers having groups that form complexes with iron oxides.

[0023] Optionally, the pigment may be provided as a pre-prepared formulation or concentrate. The pigment formulation may be solid or liquid, with a preferred form being a liquid dispersion of the pigment, particularly a dispersion in water. Liquid preparations may be prepared by adding dispersants such as nonionic surfactants, anionic surfactants, polymer dispersants, or mixtures thereof. Combinations of surfactants, or combinations of surfactants and polymers, may also be used in the preparation. Examples of surfactants include alcohol ethoxylates, fatty acid ethoxylates, polyglycol ethers, and alkylbenzene sulfonates.

[0024] Therefore, the pigment (a) dispersion preferably contains pigment (a), a liquid dispersion medium (preferably water), and at least one dispersant preferably selected from nonionic surfactants, anionic surfactants, polymer dispersants, or mixtures thereof. The amount of dispersant is preferably 0.1 to 10, more preferably 0.5 to 5, and most preferably 0.5 to 3% by mass, based on the pigment (a) dispersion.

[0025] Alternatively, solid preparations that are readily dispersible or agitable in water are also acceptable. Such solid preparations comprise a pigment (a) and a solid support compatible with the aqueous system. Examples of supports include phosphates, phosphate esters, and phosphonic acids, which, due to their degree of hydrophilicity, allow for easy integration of the product into the aqueous solution of latex. The pigment concentration is typically in the range of 40–95% by mass. The support is typically present at a concentration of 5–60% by mass.

[0026] The process for manufacturing latex products consists of a molding process that includes a pre-dispersion process, a dispersion process, and a drying process. In the pre-dispersion process, a pH-adjusted pigment (a) dispersion and natural latex are thoroughly mixed. Further, natural latex and coloring pigment (b) are added to the pre-dispersion and mixed well. The molded body, such as balloons or gloves, is immersed in a coagulant such as calcium nitrate and dried. After immersing the dried molded body in a natural latex solution, it is fired at 60-120°C, preferably 80-100°C, until curing is complete.

[0027] In this invention, a metal pigment (a) coated with 1 to 5% by mass of iron oxide, such as Paliocrom (Sun Chemical), Stellar (CQV), Zenexo (Schlenk), Meoxal (Merck), preferably aluminum; and an organic pigment (b) of 0.1 to 5.0% by mass are blended with natural latex to obtain the following red metallic target colors: a * =25~80 (at 45°) b * =10~40 (at 45°) The flop exponent (FI) according to equation (1) is FI ≥ 9.0.

number

[0028] Flop refers to the change in brightness, hue, and saturation that occurs when a dried ink, paint, or other colored finish is viewed from different angles. For example, a color may match well to a test panel when viewed from the front, but the color may change when viewed from a 45 or 60-degree angle to the left or right.

[0029] Paliocrom offers two types of aluminum flakes: one is the "cornflake type," and the other is the "silver dollar type." In terms of particle size, D50 is 10-22 microns, preferably 20 microns.

[0030] [Table 1]

[0031] PALIOCROM GOLD L2158 (NV 72.5%) has a particle size D50 of 17 microns, and the paste composition is aluminum (approximately 28%), silicon dioxide (approximately 13%), iron oxide (approximately 32%), and solvent (approximately 27%).

[0032] Red, purple, and / or orange absorbing pigment particles (b) reflect red, purple, and / or orange. Preferably, the red absorbing pigment (b) can be an inorganic pigment, preferably an organic pigment, or a mixture of two or more of these. Preferably, it is selected from the group consisting of quinacridone, diketopyrrolopyrrolidone, azored, azoorange, dioxazine, naphthal, diallyl, perylene, diazoorange, benzimidazolon, pyrazolone, perinone, azomethine, anthraquinone, triarylcarbonium, thioindogo, isoindoline, substitutions of general chemical structures, inorganic mixed metal and mixed metal oxide red pigments, and mixtures thereof. More preferably, the red absorbing pigment is selected from the group consisting of pigment red 122, pigment red 202, pigment red 188, pigment red 269, pigment red 254, pigment red 57:1, pigment red 48:2, pigment violet 23, and mixtures thereof.

[0033] The average particle size of the red, purple, and / or orange absorbing pigment particles (b) is freely selectable, but is often in the nanometer range. In other embodiments, the particles may have an average diameter of 0.1 to 200 nanometers, or 0.1 to 15 nanometers. The particle size can be measured with a camcorder or other optical instrument.

[0034] The amounts and mass ratios of components (a) and (b) in the latex or latex product can be freely selected according to the desired final color effect and depth or density of color. The amount of component (a) in the latex is preferably 0.1 to 20% by mass, more preferably 0.5 to 10% by mass, and most preferably 1 to 5% by mass, based on the final latex which is 100% by mass.

[0035] The amount of component (b) in the latex is preferably 0.01 to 20% by mass, more preferably 0.1 to 10% by mass, and most preferably 0.25 to 7.5% by mass, based on the final latex which is 100% by mass.

[0036] The appropriate or preferred mass ratio of pigment (b) to (a) is evident from the following examples.

[0037] No citation or specification of any document in this application constitutes prior art to the present invention.

[0038] Embodiment The present invention is further described by the following series of sections and embodiments, as well as combinations of sections and embodiments arising from the given dependencies and backreferences. In particular, where the scope of an embodiment is referred to in each case, for example, in the context of the term "the method according to any one of claims 1 to 5," it is intended that all embodiments within that scope are expressly disclosed to those skilled in the art, that is, the wording of this term should be understood by those skilled in the art as synonymous with "the method according to any one of embodiments 1, 2, 3, 4 and 5." Furthermore, it is explicitly noted that the following series of sections and embodiments are not claims defining the scope of protection, but rather appropriate components of the description relating to general and specific aspects of the present invention.

[0039] 1. A method for providing a latex product having a red metallic finish, comprising a printing ink containing one or more metal fillers and one or more red, purple, or orange absorbing pigments, wherein the metallic finish has the following characteristics: a * =25~80 (at 45°) b * =10~40 (at 45°) The flop exponent (FI) according to equation (1) is FI ≥ 9.0. A method having a red metallic effect.

[0040] 2. The method according to Embodiment 1, wherein the metal filler comprises one or more layers of metal or metal oxide.

[0041] 3. The method according to Embodiment 2, wherein the mass of the metal filler is 0.5 to 10% by mass.

[0042] 4. The method according to any one of Embodiments 1 to 3, wherein the metal filler comprises one or more layers of metal or metal oxide and one or more layers of iron oxide.

[0043] 5. The method according to Embodiment 4, wherein the metal filler contains 30 to 250 times (by mass) iron oxide relative to the metal or metal oxide substrate.

[0044] 6. The method according to any one of Embodiments 1 to 5, wherein the red absorbing pigment is selected from the group consisting of quinacridone, diketopyrrolopyrrolidone, azored, azoorange, dioxazine, naphthal, diallyl, perylene, diazoorange, benzimidazolon, pyrazolone, perinone, azomethine, anthraquinone, triarylcarbonium, thioindogo, isoindoline, substituted derivatives of general chemical structures, inorganic mixed metal and mixed metal oxide red pigments, and mixtures thereof.

[0045] 7. The method according to any one of Embodiments 1 to 6, wherein the red absorbing pigment is selected from the group consisting of pigment red 122, pigment red 202, pigment red 188, pigment red 269, pigment red 254, pigment red 57:1, pigment red 48:2, pigment violet 23, and mixtures thereof.

[0046] 8. The method according to any one of Embodiments 1 to 7, wherein the latex product is selected from the group consisting of balloons, gloves, and erasers.

[0047] 9. A red metallic latex product that can or can be obtained by the method described in any one of Embodiments 1 to 7.

[0048] 10. Latex or latex product having a red metallic surface finish, wherein the red metallic surface finish is embedded in the latex product at least on its surface, and (a) one or more metallic fillers including metal and / or metal oxide particles, (b) One or more red, purple and / or orange color-absorbing pigment particles Includes, The aforementioned metal surface finish has a red metallic effect with the following characteristics: a * =25~80 (at 45°) b * =10~40 (at 45°) The flop exponent (FI) according to equation (1) is FI ≥ 9.0.

number

[0049] 11. The latex or latex product according to Embodiment 10, wherein the metal filler (a) comprises one or more metal and / or metal oxide surface layers (a2).

[0050] 12. The latex or latex product according to Embodiment 10 or 11, wherein the amount of metal filler (a) in the latex or latex product is 0.5 to 10% by mass, based on the latex or latex product having a red metal surface finish.

[0051] 13. The latex or latex product according to any one of Embodiments 10 to 12, wherein the metal filler (a) includes, as a base material (a1), a selection from the group consisting of metal oxides, preferably mica, glass, and Al2O3, and / or a metal, preferably aluminum, copper, silver, nickel, zinc, stainless steel, or an alloy of two or more of these metals.

[0052] 14. The latex or latex product according to Embodiment 13, wherein the metal filler (a) comprises one or more surface layers (a2) on the substrate (a1) selected from one or more surface layers of a metal or metal oxide different from iron oxide and / or one or more surface layers of iron oxide, and the metal and metal oxide are different from the metal and metal oxide of the substrate.

[0053] 15. The latex or latex product according to Embodiment 14, wherein the metal filler (a) has a mass amount of iron oxide in the surface layer (a2) that is 30 to 250 times the mass amount of the metal and / or metal oxide substrate (a1).

[0054] 16. The latex or latex product according to any one of Embodiments 10 to 15, wherein the red absorbing pigment (b) is selected from the group consisting of quinacridone, diketopyrrolopyrrolidone, azored, azoorange, dioxazine, naphthal, diallyl, perylene, diazoorange, benzimidazolon, pyrazolone, perinone, azomethine, anthraquinone, triarylcarbonium, thioindogo, isoindoline, substitutions of general chemical structures, inorganic mixed metal and / or mixed metal oxide red pigments, and mixtures thereof.

[0055] 17. The red absorbing pigment (b) is selected from the group consisting of pigment red 122, pigment red 202, pigment red 188, pigment red 269, pigment red 254, pigment red 57:1, pigment red 48:2, pigment violet 23, and mixtures thereof, as described in any one of Embodiments 10 to 16, the latex or latex product.

[0056] 18. The latex or latex product according to any one of Embodiments 10 to 17, wherein the latex is selected from the group consisting of natural rubber latex and / or synthetic rubber latex.

[0057] 19. The latex or latex product according to any one of Embodiments 10 to 18, wherein the latex product is selected from the group consisting of balloons, gloves, preferably rubber household gloves and medical gloves, condoms and pessaries, beach toys, catheters, dental products, preferably wedges and orthodontic rubber bands, and clothing rubber.

[0058] 20. The latex or latex product according to any one of embodiments 10 to 19, wherein the red metallic surface finish, comprising one or more metal fillers (a) containing metal and / or metal oxide particles, and one or more red, purple and / or orange absorbent pigment particles (b), is part of a printing ink used to give the latex or latex product a red metallic surface finish.

[0059] 21. A method for manufacturing a latex product according to any one of embodiments 10 to 20 having a red metallic surface finish, comprising the following steps: A step of mixing liquid-dispersed natural and / or synthetic latex with a red metallic surface finish comprising one or more metal fillers (a) containing metal and / or metal oxide particles and one or more red, purple and / or orange absorbent pigment particles (b), thereby forming a latex product from the mixture, wherein the red metallic surface finish is embedded in the latex product at least on its surface, and the product has a red metallic effect. Alternatively, a process comprising first forming a latex product from liquid-dispersed natural and / or synthetic latex, then coating the dried product with a mixture of liquid-dispersed natural and / or synthetic latex having a red metallic surface finish, comprising one or more metal fillers (a) containing metal and / or metal oxide particles and one or more red, purple and / or orange absorbent pigment particles (b), thereby forming a latex coating on an article from the mixture, wherein the red metallic surface finish is embedded in the latex product at least on its surface, thereby having a red metallic effect. Methods that include...

[0060] 22. The method according to Embodiment 21, wherein the latex and / or mixture preferably comprises water and one or more auxiliary agents, the auxiliary agents being selected from the group consisting of non-silicone defoamers, polyalkylene glycols, nonionic surfactants, preferably alcohol ethoxylates, rheology modifiers, and preferably acrylic polymers and / or acrylic copolymer emulsions.

[0061] 23. A red metal latex product that can or can be obtained by the method described in Embodiment 21 or 22.

[0062] 24. (a) One or more metal filler particles containing metal and / or metal oxide particles, and (b) One or more red, purple and / or orange absorbing pigment particles as defined in any one of Embodiments 10 to 20 A particle composition containing, The particle composition produces a red metallic surface finish on at least the surface of a latex product containing a pigment composition, and the metallic surface finish in the latex product has the following characteristics: a * =25~80 (at 45°) b * =10~40 (at 45°) The flop exponent (FI) according to equation (1) is FI ≥ 9.0.

number

[0063] 25. (a) One or more metal fillers containing metal and / or metal oxide particles, (b) One or more red, purple and / or orange absorbing pigment particles as defined in any one of Embodiments 10 to 20 A method for using a particle composition containing the above as a red metallic surface finish on a latex product, at least on its surface, In the aforementioned latex product, the metal surface finish has a red metallic effect having the following characteristics: a * =25~80 (at 45°) b * =10~40 (at 45°) The flop exponent (FI) according to equation (1) is FI ≥ 9.0.

number

[0064] The particle (pigment) composition of the present invention can be appropriately dispersed using a polymer dispersant to form a pigment dispersion.

[0065] Therefore, in a further embodiment, the present invention is 26. A particle or pigment dispersion comprising the particle composition defined in Embodiment 24 and a polymer dispersant. Regarding.

[0066] Furthermore, it is possible to add two or more polymer dispersants.

[0067] A suitable polymer dispersant improves pigment dispersion and reduces interparticle attractive forces within the dispersion. Improved dispersion means a smaller average particle size (or a reduction in particle size achieved with shorter grinding times) and a narrower particle size distribution. The dispersion is significantly more stable against flocculation and aggregation than those produced by conventional methods. A suitable polymer dispersant has a two-component structure containing polymer chains and anchor groups. A specific combination of these components produces the desired effect.

[0068] The polymer dispersant can be statistical (e.g., random), alternating, gradient, graft, or block copolymer. The polymer dispersant is generally added in an amount of 1 to 50% by mass, preferably up to 35% by mass, based on the particles (a) and pigment (b) and any further pigments.

[0069] Suitable polymer dispersant copolymers include, for example, cationic copolymers, anionic copolymers, amphoteric copolymers, or nonionic copolymers.

[0070] The copolymer may have repeating units derived, for example, from polymerizable or condensable acids, esters, glycols, nitriles, amides, imides, olefins, epoxides, or aziridines, such as acrylic acid or methacrylic acid or their esters, amides, nitriles, terephthalic acid esters, caprolactam, ethylene, propylene, isobutylene, styrene, ethylene oxide, or ethyleneimine. Graft copolymers and block copolymers are preferred.

[0071] Examples of cationic, anionic, amphoteric, or nonionic copolymers include commercially available Disperbyk® 111, 160, 161, 162, 163, 164, 166, 170, 171, 182, 2000, 2001, 2070, 2150, 2163; EFKA® PX 4300, PX 4310, PX 4320, PX 4330, PX 4340, PX 4350, PA 4400, PA 4401, PA 4402, PA 4403, PA 4450, PX 4700, PX 4701, PX 4731, PX 4732, and Dispex® Ultra 4585, Solsperse® 24000, 32550, Ajisper® PB-821, PB-822, PB-823, and combinations thereof may be used.

[0072] Polymer dispersants typically affect the viscosity of pigment dispersions. Therefore, it is preferable to use polymer dispersants that lower the viscosity of the particle / pigment dispersion, such as amphoteric, and especially cationic copolymers.

[0073] Particles or pigment dispersions can be prepared in various ways. For example, a pigment composition, solvent, polymer dispersant, and optionally further pigment synergenizers are dispersed in predetermined amounts by a dispersion process. The dispersion process can be carried out using a paint conditioner, sand grinder, ball mill, roll mill, stone mill, jet mill, or homogenizer. Further colorants may also be added, if present. If necessary, other suitable additives or binder resins of the composition to be used in the final application may be present during the dispersion process. The binder resin may be added partially or completely. The dispersion time can be appropriately adjusted depending on the equipment used. The dispersion temperature can be varied, for example, above 0°C, to room temperature, or up to 100°C.

[0074] The particle / pigment composition or particle / pigment dispersion of the present invention can be used in a variety of applications, such as coloring any organic material of natural or synthetic origin, photosensitive resist compositions for the manufacture of color filters, printing inks, liquid inks, coating compositions, paints, plastics, films, or fibers.

[0075] Therefore, in a further embodiment, the present invention 27. A method for using the particle composition defined in Embodiment 24, or the particle or pigment dispersion defined in Embodiment 26, for coloring photosensitive resist compositions for manufacturing color filters, printing inks, liquid inks, coating compositions, paints, plastics, films, or fibers. Regarding.

[0076] Based on the organic material to be colored, the particle / pigment composition is typically used in amounts ranging from 0.01% to 30% by mass.

[0077] The present invention has been described in detail, including various embodiments. However, those skilled in the art will understand that improvements and / or enhancements to the present invention, which fall within the scope and spirit of the invention, can be made by considering the present disclosure. [Examples]

[0078] The present invention can be further illustrated by the following non-limiting embodiments, which are intended to further illustrate the invention and are not intended to limit the scope of the invention, nor should they be construed as such.

[0079] The following compositions were used in the examples: Compal WS4468 (Al 88.0%): D50 15μm PR122 dispersion Sunsperse QPD0122 (40.2% by mass of PR122) PR269 dispersion RPD-2690 (37.61% by mass of PR269) PR57:1 dispersion RFD-9587 (38.0% by mass of PR57:1) PR254 dispersion RFD-0254 (48.10% by mass of PR254) PV23 dispersion VFD-1157 (46.90% by mass of PV23) Compal WS4468 Metallic Pigment (Sun Chemical) (88.0% Al) All of the following examples were prepared stepwise according to the described procedure.

[0080] Example 1 of the present invention - Dispersion & Latex Solution 1. Weigh out 502.4g of PALIOCROM GOLD L2024 (non-volatile content (NV) = 60.0%), 136.7g of non-silicone defoaming agent, 23.9g of polypropylene glycol, 215.3g of deionized water (DI water), and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR122 dispersion Sunsperse QPD0122 (40.2% by mass of PR122) shown in Table 2 to mixture #3, and mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0081] Example 2 of the present invention - Dispersion & Latex Solution 1. Weigh out 502.4g of PALIOCROM GOLD L2024 (NV=60.0%), 136.7g of non-silicone defoaming agent, 23.9g of polypropylene glycol, 215.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR269 dispersion RPD-2690 (37.61% by mass of PR269) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0082] Example 3 of the present invention - Dispersion & Latex Solution 1. Weigh out 502.4g of PALIOCROM GOLD L2024 (NV=60.0%), 136.7g of non-silicone defoaming agent, 23.9g of polypropylene glycol, 215.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR57:1 dispersion RFD-9587 (38.0% by mass of PR57:1) shown in Table 2; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0083] Example 4 of the present invention - Dispersion & Latex Solution 1. Weigh out 502.4g of PALIOCROM GOLD L2024 (NV=60.0%), 136.7g of non-silicone defoaming agent, 23.9g of polypropylene glycol, 215.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR254 dispersion RFD-0254 (48.10% by mass of PR254) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0084] Example 5 of the present invention - Dispersion & Latex Solution 1. Weigh out 415.8g of PALIOCROM GOLD L2158 (NV=72.5%), 136.7g of non-silicone defoaming agent, 32.6g of polypropylene glycol, 293.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 3.1g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR57:1 dispersion RFD-9587 (38.0% by mass of PR57:1) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0085] Example 6 of the present invention - Dispersion & Latex Solution 1. Weigh out 415.8g of PALIOCROM GOLD L2158 (NV=72.5%), 136.7g of non-silicone defoaming agent, 32.6g of polypropylene glycol, 293.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 3.1g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR269 dispersion RPD-2690 (37.61% by mass of PR269) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0086] Example 7 of the present invention - Dispersion & Latex Solution 1. Weigh out 415.8g of PALIOCROM GOLD L2158 (NV=72.5%), 136.7g of non-silicone defoaming agent, 32.6g of polypropylene glycol, 293.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR122 dispersion QPD-0122 (40.2% by mass of PR-122) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0087] Example 8 of the present invention - Dispersion & Latex Solution 1. Weigh out 415.8g of PALIOCROM GOLD L2158 (NV=72.5%), 136.7g of non-silicone defoaming agent, 32.6g of polypropylene glycol, 293.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR57:1 dispersion RFD-9587 (38.0% by mass of PR57:1) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0088] Example 9 of the present invention - Dispersion & Latex Solution 1. Weigh out 415.8g of PALIOCROM GOLD L2158 (NV=72.5%), 136.7g of non-silicone defoaming agent, 32.6g of polypropylene glycol, 293.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR269 dispersion RPD-2690 (37.61% by mass of PR269) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0089] Example 10 of the present invention - Dispersion & Latex Solution 1. Weigh out 415.8g of PALIOCROM GOLD L2158 (NV=72.5%), 136.7g of non-silicone defoaming agent, 32.6g of polypropylene glycol, 293.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 53.6g of natural latex, 0.4g of rheology modifier (acrylic copolymer emulsion in water), and 10.8g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR57:1 dispersion RFD-9587 (38.0% by mass of PR57:1) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0090] Example 11 of the present invention - Dispersion & Latex Solution 1. Weigh out 415.8g of PALIOCROM GOLD L2158 (NV=72.5%), 136.7g of non-silicone defoaming agent, 32.6g of polypropylene glycol, 293.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 53.6g of natural latex, 0.4g of rheology modifier (acrylic copolymer emulsion in water), and 10.8g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR269 dispersion RPD-2690 (37.61% by mass of PR269) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0091] Example 12 of the present invention - Dispersion & Latex Solution 1. Weigh out 405.7g of PALIOCROM RED L3258 (NV=74.3%), 136.7g of non-silicone defoaming agent, 41.2g of polypropylene glycol, 302.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 3.1g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR57:1 dispersion RFD-9587 (38.0% by mass of PR57:1) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0092] Example 13 of the present invention - Dispersion & Latex Solution 1. Weigh out 405.7g of PALIOCROM RED L3258 (NV=74.3%), 136.7g of non-silicone defoaming agent, 41.2g of polypropylene glycol, 302.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 3.1g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR269 dispersion RPD-2690 (37.61% by mass of PR269) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0093] Example 14 of the present invention - Dispersion & Latex Solution 1. Weigh out 405.7g of PALIOCROM RED L3258 (NV=74.3%), 136.7g of non-silicone defoaming agent, 41.2g of polypropylene glycol, 302.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR122 dispersion QPD-0122 (40.2% by mass of PR122) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0094] Example 15 of the present invention - Dispersion & Latex Solution 1. Weigh out 405.7g of PALIOCROM RED L3258 (NV=74.3%), 136.7g of non-silicone defoaming agent, 41.2g of polypropylene glycol, 302.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR269 dispersion RPD-2690 (37.61% by mass of PR269) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0095] Example 16 of the present invention - Dispersion & Latex Solution 1. Weigh out 405.7g of PALIOCROM RED L3258 (NV=74.3%), 136.7g of non-silicone defoaming agent, 41.2g of polypropylene glycol, 302.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR57:1 dispersion RFD-9587 (38.0% by mass of PR57:1) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0096] Example 17 of the present invention - Dispersion & Latex Solution 1. Weigh out 405.7g of PALIOCROM RED L3258 (NV=74.3%), 136.7g of non-silicone defoaming agent, 41.2g of polypropylene glycol, 302.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR254 dispersion RFD-0254 (48.10% by mass of PR254) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0097] Example 18 of the present invention - Dispersion & Latex Solution 1. Weigh out 405.7g of PALIOCROM RED L3258 (NV=74.3%), 136.7g of non-silicone defoaming agent, 41.2g of polypropylene glycol, 302.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PV23 dispersion VFD-1157 (46.90% by mass of PV23) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0098] Example 19 of the present invention - Dispersion & Latex Solution 1. Weigh out 405.7g of PALIOCROM RED L3258 (NV=74.3%), 136.7g of non-silicone defoaming agent, 32.6g of polypropylene glycol, 293.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 53.6g of natural latex, 0.4g of rheology modifier (acrylic copolymer emulsion in water), and 10.8g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR122 dispersion QPD-0122 (40.2% by mass of PR122) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0099] Example 20 of the present invention - Dispersion & Latex Solution 1. Weigh out 405.7g of PALIOCROM RED L3258 (NV=74.3%), 136.7g of non-silicone defoaming agent, 32.6g of polypropylene glycol, 293.3g of DI water, and 17.9g of alcohol ethoxylate nonionic surfactant, place them in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 53.6g of natural latex, 0.4g of rheology modifier (acrylic copolymer emulsion in water), and 10.8g of Paliocrom dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR269 dispersion RPD-2690 (37.61% by mass of PR269) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0100] Example 21 of the present invention - Dispersion & Latex Solution 1. Weigh out 301.4g of SunMICA gold 284-1219; 136.7g of non-silicone defoaming agent; 44.0g of polypropylene glycol; 396.2g of DI water; and 17.9g of alcohol ethoxylate nonionic surfactant, place in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of SunMICA dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR122 dispersion QPD-0122 (40.2% by mass of PR122) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0101] Example 22 of the present invention - Dispersion & Latex Solution 1. Weigh out 301.4g of SunMICA gold 284-1219; 136.7g of non-silicone defoaming agent; 44.0g of polypropylene glycol; 396.2g of DI water; and 17.9g of alcohol ethoxylate nonionic surfactant, place in a 2L beaker, and stir for 30 minutes; 2. Add 102.53g of acrylic emulsion and stir for 30 minutes; 3. Weigh 89.3g of natural latex, 0.7g of rheology modifier (acrylic copolymer emulsion in water), and 10.0g of SunMICA dispersion (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR269 dispersion RPD-2690 (37.61% by mass of PR269) shown in Table 2 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0102] Comparative Example 23 - Dispersion & Latex Solution (Iron Oxide Free) 1. Weigh 25.0 g of Compal WS4468 metallic effect pigment (SunChemical) (88.0% Al) and 50.0 g of DI water, place them in a 100 mL beaker, and stir for 30 minutes; 2. Adjust the pH to 9.2 using a buffer system; 3. Weigh 78.6g of natural latex, 10.0g of rheology modifier (acrylic copolymer emulsion in water), and 10.5g of premix Compal WS4468 (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR122 dispersion QPD-0122 (40.2% by mass of PR122) shown in Table 3 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0103] Comparative Example 24 - Dispersion & Latex Solution (Iron Oxide Free) 1. Weigh 25.0 g of Compal WS4468 (88.0% Al) and 50.0 g of DI water, place them in a 100 mL beaker, and stir for 30 minutes; 2. Adjust the pH to 9.2 using a buffer system; 3. Weigh 78.6g of natural latex, 10.0g of rheology modifier (acrylic copolymer emulsion in water), and 10.5g of premix Compal WS4468 (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR269 dispersion RPD-2690 (37.6% by mass of PR269) shown in Table 3 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0104] Comparative Example 25 - Dispersion & Latex Solution (Iron Oxide Free) 1. Weigh 25.0 g of Compal WS4468 (88.0% Al) and 50.0 g of DI water, place them in a 100 mL beaker, and stir for 30 minutes; 2. Adjust the pH to 9.2 using a buffer system; 3. Weigh 78.6g of natural latex, 10.0g of rheology modifier (acrylic copolymer emulsion in water), and 10.5g of premix Compal WS4468 (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR57:1 dispersion RFD-9587 (38.0% by mass of PR57:1) shown in Table 3 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0105] Comparative Example 26 - Dispersion & Latex Solution (Iron Oxide Free) 1. Weigh 25.0 g of Compal WS4468 (88.0% Al) and 50.0 g of DI water, place them in a 100 mL beaker, and stir for 30 minutes; 2. Adjust the pH to 9.2 using a buffer system; 3. Weigh 78.6g of natural latex, 10.0g of rheology modifier (acrylic copolymer emulsion in water), and 10.5g of premix Compal WS4468 (from step 1) into a separate container and stir for 30 minutes; 4. Add the amount of PR254 dispersion RFD-0254 (48.1% by mass of PR254) shown in Table 3 to mixture #3; 5. Mix at 3000 RPM for 3 minutes using a Speed ​​Mixer DAC 150 FVZ-K (Flack Tec., Inc.) to obtain the final mixture.

[0106] The drawdowns from each example were applied to a primer-coated aluminum panel (4 x 6 inches) using a 25 mil applicator and baked at 80°C for 30 minutes.

[0107] Color measurements were performed using BYK-mac i. F-index (FI value): The FI value is calculated according to the following formula (1).

[0108]

number

[0109] [Table 2] TIFF2026531367000011.tif124147

[0110] * The mass percentage of red pigment refers to the actual amount of pigment in each example, not the amount of pigment dispersion (for example, 0.77 mass% of red pigment in Example 1 of the present invention requires 1.74 parts of Sunsperse QPD0122. 40.2 × 1.74 = 0.77 red pigment).

[0111] Table 2 shows that all embodiments of the present invention meet the target value for red metallic color.

[0112] [Table 3]

[0113] * The mass percentage of red pigment refers to the actual amount of pigment in each example, not the amount of pigment dispersion (for example, 0.77 mass% of red pigment in Example 1 of the present invention requires 1.74 parts of Sunsperse QPD0122. 40.2 × 1.74 = 0.77 red pigment).

[0114] Table 3 shows that the comparative example did not meet the target value for red metallic color.

Claims

1. A latex or latex product having a red metallic surface finish, wherein the red metallic surface finish is embedded in the latex product, at least on its surface, (a) one or more metal fillers containing metal and / or metal oxide particles, (b) One or more red, purple and / or orange absorbent pigment particles Includes, The aforementioned metal surface finish has a red metallic effect with the following characteristics: a * = 25-80 (at 45°) b * = 10 to 40 (at 45°) The flop exponent (FI) according to equation (1) is FI ≥ 9.

0. [Math 1] (In the formula, L * 15. L * 110, L * 45 is the color measurement value at each viewing angle, a * and b * (where is the color dimension of the Lab color system at 45°), latex or latex products.

2. The latex or latex product according to claim 1, wherein the metal filler (a) comprises one or more metal and / or metal oxide surface layers (a2).

3. The latex or latex product according to claim 1 or 2, wherein the amount of metal filler (a) in the latex or latex product is 0.5 to 10% by mass, based on the latex or latex product having a red metal surface finish.

4. The metal filler (a) according to the above uses a metal oxide, preferably mica, glass, Al as the base material (a1) 2 O 3 selected from the group consisting of, and / or a metal, preferably selected from the group consisting of aluminum, copper, silver, nickel, zinc, stainless steel, or alloys of two or more of these metals, the latex or latex product according to claim 1 or 2.

5. The latex or latex product according to claim 4, wherein the metal filler (a) comprises one or more surface layers (a2) on the substrate (a1) selected from the group consisting of one or more surface layers of a metal or metal oxide different from iron oxide and / or one or more surface layers of iron oxide, and the metal and metal oxide are different from the metal and metal oxide of the substrate.

6. The latex or latex product according to claim 5, wherein the metal filler (a) has a mass amount of iron oxide in the surface layer (a2) that is 30 to 250 times the mass amount of the metal and / or metal oxide substrate (a1).

7. The latex or latex product according to claim 1 or 2, wherein the red absorbent pigment (b) is selected from the group consisting of quinacridone, diketopyrrolopyrrolidone, azored, azoorange, dioxazine, naphthal, diallyl, perylene, diazoorange, benzimidazolon, pyrazolone, perinone, azomethine, anthraquinone, triarylcarbonium, thioindogo, isoindoline, substituted derivatives of the above general chemical structures, inorganic mixed metal and / or mixed metal oxide red pigments, and mixtures thereof.

8. The latex or latex product according to claim 1 or 2, wherein the red absorbing pigment (b) is selected from the group consisting of pigment red 122, pigment red 202, pigment red 188, pigment red 269, pigment red 254, pigment red 57:1, pigment red 48:2, pigment violet 23, and mixtures thereof.

9. The latex or latex product according to claim 1 or 2, wherein the latex is selected from the group consisting of natural rubber latex and / or synthetic rubber latex.

10. The latex or latex product according to claim 1 or 2, wherein the latex product is selected from the group consisting of balloons, gloves, preferably rubber household gloves and medical gloves, condoms and pessaries, beach toys, catheters, dental products, preferably wedges and orthodontic rubber bands, and clothing rubber.

11. The latex or latex product according to claim 1 or 2, wherein the red metallic surface finish, comprising one or more metal fillers (a) containing metal and / or metal oxide particles, and one or more red, purple and / or orange absorbent pigment particles (b), is part of a printing ink used to give the latex or latex product a red metallic surface finish.

12. A method for producing a latex product according to claim 1 or 2, having a red metallic surface finish, comprising the following steps: A step of mixing liquid or fluid natural and / or synthetic latex with a red metallic surface finish comprising one or more metal fillers (a) containing metal and / or metal oxide particles and one or more red, purple and / or orange absorbent pigment particles (b), or a particle composition comprising (a) and (b), thereby forming a latex product from the mixture obtained, wherein the red metallic surface finish is embedded in the latex product at least on its surface, and has a red metallic effect, Alternatively, a process comprising first forming a latex product from liquid or fluid natural and / or synthetic latex, then drying the product and coating it with a mixture of liquid or fluid natural and / or synthetic latex and a red metallic surface finish comprising one or more metal fillers (a) containing metal and / or metal oxide particles and one or more red, purple and / or orange absorbent pigment particles (b), or with a particle composition comprising (a) and (b), thereby forming a latex coating on the latex article from the mixture, wherein the red metallic surface finish is embedded in the latex product at least on its surface, thereby having a red metallic effect. Methods that include...

13. The method according to claim 12, wherein the particulate composition comprising the liquid or fluid latex and / or (a) and (b) preferably comprises water and one or more auxiliary agents, the auxiliary agent being selected from the group consisting of a non-silicone defoamer, a polyalkylene glycol, a nonionic surfactant, preferably an alcohol ethoxylate, a rheology modifier, preferably an acrylic polymer and / or an acrylic copolymer emulsion.

14. A red metal latex product that can be obtained or is obtained by the method described in claim 12.

15. (a) One or more metal fillers comprising metal and / or metal oxide particles as defined in claim 1, and (b) One or more red, purple and / or orange absorbing pigment particles as defined in claim 1 A particle composition containing, The particle composition produces a red metallic surface finish on at least the surface of a latex product containing the particle composition, and the metallic surface finish in the latex product has the following characteristics: a * = 25-80 (at 45°) b * = 10 to 40 (at 45°) The flop exponent (FI) according to equation (1) is FI ≥ 9.

0. [Math 2] (In the formula, L * 15. L * 110, L * 45 is the color measurement value at each viewing angle, a * and b * (where is the color dimension of the Lab color system at 45°), particle composition.

16. (a) One or more metal fillers comprising metal and / or metal oxide particles as defined in claim 1, and (b) One or more red, purple and / or orange absorbing pigment particles as defined in claim 1 A method for using a particle composition containing the above as a red metallic surface finish on a latex product, at least on its surface, In the aforementioned latex product, the metal surface finish has a red metallic effect having the following characteristics: a * = 25-80 (at 45°) b * = 10 to 40 (at 45°) The flop exponent (FI) according to equation (1) is FI ≥ 9.

0. [Math 3] (In the formula, L * 15. L * 110, L * 45 is the color measurement value at each viewing angle, a * and b * (This is the color dimension of the Lab color system at 45°), and how to use it.

17. A particle or pigment dispersion comprising a particle composition as defined in claim 15, further comprising a polymer dispersant.

18. A method for using the particle composition defined in claim 15, or the particle or pigment dispersion defined in claim 17, for coloring photosensitive resist formulations for the manufacture of color filters, printing inks, liquid inks, coating compositions, paints, plastics, films, or fibers.