Back-illuminated sensor and method for manufacturing the same

By integrating a p-type SiGe layer and anti-reflective coating with a boron layer, the image sensor addresses reflection and absorption losses, achieving enhanced photon absorption and stability for DUV and VUV applications.

JP2026538951APending Publication Date: 2026-11-19KLA CORP
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
JP2026518687
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-10-28
Filing Date
2024-10-29
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing image sensors face challenges in achieving high sensitivity and stability for detecting defects in miniaturized features due to reflection and absorption losses at DUV and VUV wavelengths, and high photon flux requirements for high SNR, which are not adequately addressed by current boron-coated silicon sensors.

Method used

Incorporating a p-type SiGe layer between the boron layer and silicon layer to reduce refractive index mismatch and using an anti-reflective coating to enhance photon absorption efficiency, along with a boron layer to improve radiation resistance and electron transport.

Benefits of technology

The resulting image sensor achieves a 20-90% increase in VUV/DUV photon absorption efficiency and improved long-term radiation stability, enhancing sensitivity and reliability for inspection systems.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026538951000001_ABST
    Figure 2026538951000001_ABST
Patent Text Reader

Abstract

The image sensor includes a p-type silicon layer, a silicon layer disposed on the p-type silicon layer, a p-type SiGe layer disposed on the p-type silicon layer, a boron layer disposed on the p-type SiGe layer, and an anti-reflective film disposed on the boron layer. A trench can be formed within the image sensor so that the boron layer is located within the trench.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] This application claims priority to provisional patent application filed on October 31, 2023 and assigned U.S. Application No. 63 / 546,530, the disclosure of which is incorporated herein by reference in its entirety.

[0002] The present disclosure relates to image sensors.

BACKGROUND ART

[0003] In the integrated circuit industry, inspection tools with higher resolution and sensitivity are required to resolve increasingly miniaturized features and higher-density integrated circuits, reticles (photomasks), solar cells, or charge-coupled devices, as well as to detect defects with sizes equal to or smaller than the size of these features.

[0004] Inspection systems operating at short wavelengths (e.g., wavelengths less than about 250 nm) can often provide such resolution. For reticle and wafer inspection, it may be desirable to perform inspection using the wavelength of lithography (i.e., near 193.4 nm for immersion lithography, near 13.5 nm for extreme ultraviolet lithography) and wavelengths equal to or close to the feature size, since the phase shift of inspection light caused by the pattern is the same as or similar to that occurring during lithography. When inspecting semiconductor patterned wafers, inspection systems operating over a relatively wide wavelength range, including the near ultraviolet (UV), deep ultraviolet (DUV), and / or vacuum ultraviolet (VUV) ranges, may be advantageous because the wide wavelength range provides operational flexibility to deliver high sensitivity for different process layers and pattern dimensions.

[0005] Detecting small defects and particles on reticles and semiconductor wafers requires a high signal-to-noise ratio (SNR). For high-speed inspection, the statistical variation in the arrival of individual photons (Poisson noise) becomes a fundamental limiting factor for the SNR; therefore, a high photon flux density is necessary to ensure a high SNR. In many cases, more than 100,000 photons per pixel are required. Sensors used in inspection systems are typically exposed to large amounts of radiation after only a few months of 24-hour inspection operation. Radiation resistance is one of the requirements for sensors used in inspection systems to maintain stable performance.

[0006] High spectral sensitivity is another requirement for sensors used in inspection, measurement, and related applications. As mentioned above, a high signal-to-noise ratio is required. If the sensor does not convert most of the incident photons into a signal, a brighter light source is needed to maintain the same inspection or measurement speed compared to an inspection or measurement system with a more efficient sensor. Adopting a brighter light source can cause damage or degradation to the instrument's optics and the sample being inspected over time. Also, brighter light sources can be more expensive or may not be available, especially at DUV and VUV wavelengths.

[0007] The strong surface absorption of DUV and VUV radiation by silicon poses a challenge for sensors used for inspection at these wavelengths. While visible or extreme ultraviolet (EUV) wavelengths are absorbed over approximately 100 nm and beyond within silicon, such wavelengths can be largely absorbed within approximately 10 nm or even tens of nm of the silicon surface. The high density of inherent surface defects on silicon (such as dangling bonds, vacancies, or interstitial atoms) affects conductivity and recombination processes within the semiconductor, potentially posing a problem for sensors intended to operate at DUV or VUV wavelengths. The efficiency of sensors operating at DUV or VUV wavelengths may depend on how much of the photoelectrons generated near the silicon surface can be collected before carrier recombination or carrier trapping occurs.

[0008] Boron has been considered to address some of these problems in sensor design. However, reflection losses from interfaces (i.e., boron-silicon interface and air-boron interface), and absorption losses in the boron layer, hinder boron-coated silicon sensors from achieving higher quantum efficiency at VUV and DUV wavelengths. Reflection losses from interfaces are due to the large refractive index mismatch between silicon and boron at these wavelengths. Due to optical losses, the upper limit of the percentage of photons transmitted into silicon with a 2 nm thick boron overlayer is approximately 0.2–0.3 at VUV and DUV. Therefore, about 70% of incident photons are lost and do not contribute to photocarrier generation within silicon. [Prior art documents] [Patent Documents]

[0009] [Patent Document 1] U.S. Patent Application Publication No. 2019 / 0131465 [Patent Document 2] U.S. Patent Application Publication No. 2019 / 0386054 [Overview of the Initiative] [Problems that the invention aims to solve]

[0010] Improved sensors and manufacturing methods are needed. [Means for solving the problem]

[0011] In a first embodiment, an image sensor is provided. The image sensor includes a p-type silicon layer, a silicon layer disposed on the p-type silicon layer, a p-type SiGe layer disposed on the p-type silicon layer, a boron layer disposed on the p-type SiGe layer, and an anti-reflective film disposed on the boron layer.

[0012] The image sensor may preferably further include a polysilicon layer disposed on the side of the p-type silicon layer opposite to the silicon layer.

[0013] The image sensor may, for example, further include a metal layer disposed on the polysilicon layer.

[0014] The p-type SiGe layer may be a continuous layer.

[0015] The boron layer may be a continuous layer.

[0016] The p-type SiGe layer may have a thickness of 20 to 50 nm.

[0017] The boron layer may have a thickness of 2 to 20 nm.

[0018] The p-type SiGe layer may be disposed directly on the p-type silicon layer and the silicon layer.

[0019] The boron layer may be disposed directly on the p-type SiGe layer.

[0020] In one embodiment, the silicon layer defines a trench that exposes the p-type silicon layer at the bottom of the trench. The p-type SiGe layer is disposed at the bottom of the trench so as to be disposed on the silicon layer forming the trench and on the p-type silicon layer. The boron layer is disposed on the p-type SiGe layer within the trench.

[0021] The image sensor may preferably further include a second silicon handle substrate disposed on the p-type silicon layer on the side opposite to the p-type SiGe layer.

[0022] The image sensor may, for example, further include an oxide layer disposed between the p-type silicon layer and the silicon layer.

[0023] The inspection system may include an embodiment of the image sensor.

[0024] In the second embodiment, a method for manufacturing an image sensor is provided. The method includes forming a p-type silicon layer over a silicon layer. A p-type SiGe layer is formed over the p-type silicon layer. The p-type SiGe layer is covered with a boron layer. An anti-reflective coating is formed over the boron layer.

[0025] The method may preferably further include forming a polysilicon layer on a side of the p-type silicon layer opposite to the silicon layer.

[0026] The method may for example further include performing a metallization process, thereby adding a metal layer over the polysilicon layer.

[0027] The p-type silicon layer or the p-type SiGe layer may be formed using epitaxial growth.

[0028] The method may more preferably further include an annealing step in which, after the boron layer is formed, boron from the boron layer is introduced into the p-type SiGe layer. In one example, the annealing step is at a temperature ranging from 450°C to 950°C.

[0029] In one embodiment, the method includes etching a trench in the silicon layer. The trench exposes the p-type silicon layer at the bottom of the trench. The p-type SiGe layer is disposed on the p-type silicon layer at the bottom of the trench and on the silicon layer forming the sidewalls of the trench. Brief Description of the Drawings

[0030] [Figure 1] A cross-sectional side view of a method for manufacturing an image sensor according to an embodiment of the present disclosure is shown. [Figure 2] A cross-sectional side view of a method for manufacturing an image sensor according to an embodiment of the present disclosure is shown. [Figure 3] A cross-sectional side view of a method for manufacturing an image sensor according to an embodiment of the present disclosure is shown. [Figure 4] A cross-sectional side view of a method for manufacturing an image sensor according to an embodiment of the present disclosure is shown. [Figure 5] A cross-sectional side view of a method for manufacturing an image sensor according to one embodiment of the present disclosure is shown. [Figure 6] A cross-sectional side view of a method for manufacturing an image sensor according to one embodiment of the present disclosure is shown. [Figure 7] The calculation of the percentage of photons transmitted through boron and anti-reflective overlayers into silicon and silicon-germanium substrates at VUV and DUV wavelengths is shown. [Figure 8] An exemplary testing system is shown. [Figure 9] This is a schematic diagram of an image sensor comprising boron-coated silicon germanium according to the present disclosure, where the gray gradient background in the p+ SiGe epitaxial layer and the p- Si epitaxial layer indicates doping concentration, and the dark gray indicates a higher doping concentration. [Figure 10] This shows a cross-sectional side view of another exemplary process for manufacturing an image sensor on a silicon substrate using partial wafer thinning. [Figure 11] A cross-sectional side view follows Figure 10. [Figure 12] A cross-sectional side view follows Figure 11. [Figure 13] A cross-sectional side view follows Figure 12. [Figure 14] A cross-sectional side view follows Figure 13. [Figure 15] A cross-sectional side view follows Figure 14. [Figure 16] A cross-sectional side view follows Figure 15. [Figure 17] This shows a cross-sectional side view of another exemplary process for manufacturing an image sensor on a silicon substrate using complete wafer thinning. [Figure 18] A cross-sectional side view follows Figure 17. [Figure 19] A cross-sectional side view follows Figure 18. [Figure 20] A cross-sectional side view follows Figure 19. [Figure 21] A cross-sectional side view follows Figure 20. [Figure 22]A cross-sectional side view follows Figure 21. [Figure 23] A cross-sectional side view follows Figure 22. [Figure 24] This shows a cross-sectional side view of another exemplary process for manufacturing an image sensor on an SOI substrate using partial wafer thinning. [Figure 25] A cross-sectional side view follows Figure 24. [Figure 26] A cross-sectional side view follows Figure 25. [Figure 27] A cross-sectional side view follows Figure 26. [Figure 28] A cross-sectional side view follows Figure 27. [Figure 29] A cross-sectional side view follows Figure 28. [Figure 30] This shows a cross-sectional side view of another exemplary process for manufacturing an image sensor on an SOI substrate using complete wafer thinning. [Figure 31] A cross-sectional side view follows Figure 30. [Figure 32] A cross-sectional side view follows Figure 31. [Figure 33] A cross-sectional side view follows Figure 32. [Figure 34] A cross-sectional side view follows Figure 33. [Figure 35] A cross-sectional side view follows Figure 34. [Figure 36] A cross-sectional side view follows Figure 35. [Modes for carrying out the invention]

[0031] While the claimed subject matter is described in relation to specific embodiments, other embodiments, including those that do not provide all of the advantages and features described herein, are also within the scope of this disclosure. Various structural, logical, process steps, and electronic modifications can be made without departing from the scope of this disclosure. Accordingly, the scope of this disclosure is defined solely by reference to the appended claims.

[0032] Embodiments disclosed herein include a silicon-germanium (SiGe) epitaxial layer between the boron layer and silicon to improve VUV and DUV sensitivity while maintaining the long-term stability provided by boron. The resulting image sensor can be used in DUV and VUV applications. The resulting image sensor is suitable for use in wafer and reticle inspection systems, as well as other measurement applications.

[0033] While an optional anti-reflective coating on the boron layer can improve reflection losses from the air-boron interface, it has been found that adding an intermediate layer between boron and silicon with an intermediate refractive index at VUV and DUV wavelengths can improve losses from the boron-silicon interface. In addition to providing an appropriate refractive index, the role of the intermediate layer is to ensure its electronic compatibility with silicon. The energy barrier to electron transport between the intermediate layer and silicon can be negligible in order to maintain efficient charge transfer and collection.

[0034] Silicon-germanium alloys are emerging as promising intermediate layer materials sandwiched between silicon epitaxial and (amorphous) boron layers in boron-coated sensors for inspection systems at near-UV, DUV, and / or VUV wavelengths. SiGe exhibits a higher refractive index compared to silicon at these wavelengths, but lower than that of boron. The refractive index of SiGe can also be tuned by adjusting the proportion of germanium. In terms of electronic compatibility, there is a small conduction band at the silicon-silicon-germanium interface, which can be beneficial for efficient electron transport across the heterojunction. For example, in the case of silicon-germanium containing 50% germanium, the offset may be less than 0.05 eV compared to silicon. In addition to the optical and electronic advantages, dislocation-free SiGe layers can be epitaxially grown on silicon substrates using chemical vapor deposition (CVD) or molecular beam epitaxy (MBE) techniques. High-quality SiGe layers can minimize crystal defects or electron traps that could affect electron transport.

[0035] Figures 1 to 6 illustrate a method for manufacturing the image sensor 100. Figure 1 shows a silicon layer 101. In one embodiment, the silicon layer 101 may be a silicon substrate. The silicon layer 101 is 1 e 18 cm². -3 It may also be highly p-doped (i.e., p+), exceeding . The image sensor 100 may have a thickness of 0.5 mm to 1 mm. For example, the silicon layer 101 may have a thickness of 675 ± 20 μm on a 6-inch wafer and 750 ± 25 μm on an 8-inch wafer.

[0036] In Figure 2, a p-type silicon layer 102 is formed on the silicon layer 101. Optionally, a polysilicon layer 103 is formed on the side of the p-type silicon layer 102 opposite to the silicon layer 101. The p-type silicon layer 102 can be formed using epitaxial growth or other techniques. The side of the image sensor 100 having the polysilicon layer 103 may be referred to as the front end.

[0037] Circuit elements for CCD sensors, CMOS sensors, or photodiodes can be fabricated within the polysilicon layer 103. This may include one or more steps of doping the polysilicon layer 103 in a specific region, dielectric deposition and patterning, polysilicon contact deposition, and patterning for forming the front die circuit elements.

[0038] In Figure 3, a trench 104 is etched into the silicon layer 101. The trench 104 exposes the p-type silicon layer 102 at its bottom. The trench also includes side walls formed from the silicon layer 101. The trench 104 can be formed by etching. In one example, the etching is wet etching. Grinding can also be used, with or without etching, to form the trench 104. Grinding can thin the side of the image sensor opposite to the p-type silicon layer 102, for example, by thinning the silicon layer 101. The side of the image sensor 100 with the trench 104 is sometimes referred to as the back surface. In one example, grinding is performed on the silicon layer 101 to a thickness of approximately 300 μm, followed by wet etching to open the trench 104 to expose the light-receiving area of ​​the p-type silicon layer 102.

[0039] In Figure 4, a p-type SiGe layer 105 is formed within a trench 104. The p-type SiGe layer 105 is formed at the bottom of the trench 104 (i.e., on the p-type silicon 102) and on the sidewall of the trench 104 (i.e., on the silicon layer 101). The p-type SiGe layer 105 can also be formed on the surface of the silicon layer 101 opposite the p-type silicon layer 102 on the outside of the trench 104. The p-type SiGe layer 105 can be formed using epitaxial growth, chemical vapor deposition, molecular beam epitaxy, or other techniques. Epitaxial growth may be carried out at temperatures from 500°C to 850°C (e.g., 550°C to 700°C). The p-type SiGe layer 105 may have a thickness of less than 50 nm (e.g., 20-50 nm or less than 20 nm). In another example, the p-type SiGe layer 105 has a thickness of less than 100 nm.

[0040] In Figure 5, the p-type SiGe layer 105 is coated with a boron layer 106. The boron layer 106 may have a thickness of less than 100 nm, for example, less than 20 nm or about 2 to 20 nm. The boron layer 106 may be pure boron. The boron layer 106 may be present on both the bottom and side walls of the trench 104. The boron layer 106 may also be on other surfaces, such as across the surface of the silicon layer 101 adjacent to the trench 104. The boron layer 106 may be deposited using a CVD process, such as using B2H6 as a precursor gas along with H2 and / or N2 carrier gases. Other possible techniques include MBE, atomic layer deposition (ALD), or physical vapor deposition (PVD).

[0041] The SiGe layer 105 can reduce the refractive index mismatch between the boron layer 106 and the silicon layer 101 or p-type silicon layer 102. Refractive index mismatch is an optical property based on how the atoms are arranged and the resulting electromagnetic properties.

[0042] After the boron layer 106 is formed, an optional annealing step may be performed. During annealing, boron from the boron layer 106 can be introduced into the p-type SiGe layer 105. Annealing may be performed at a temperature higher than 400°C, for example, 450°C to 950°C (e.g., 450°C to 700°C or 450°C to 850°C). Since the boron layer 106 may also be formed at these temperatures, these temperatures can be applied during the formation of the boron layer 106.

[0043] One advantage of increasing the boron deposition temperature (e.g., between 600°C and 900°C) is that at such temperatures, boron readily diffuses into the silicon, resulting in a highly p-doped layer. P-type doping creates a high static electric field gradient near the surface, accelerating the separation of electrons from the surface to the silicon layer for charge collection, thus ensuring high quantum efficiency against DUV and VUV radiation. The boron layer 106 can passivate the light-receiving back surface of the image sensor from oxidative attack on the silicon and degradation under heavy DUV and / or VUV radiation.

[0044] The p-type SiGe layer 105 can be doped with boron. This can be done during the deposition of growing SiGe by introducing B2H6 gas into the mixed gas of the CVD process. In another example, a drive-in step can be added after boron deposition by heating the wafer at over 700°C for less than 5 minutes, allowing some of the boron from the boron layer 106 to diffuse into the p-type SiGe layer 105. The p-type SiGe layer 105 can be monotonically p-doped using boron from the boron layer 106, from the surface toward the bulk of the p-type SiGe layer 105. The boron doping profile can be adjusted so that the concentration is highest near the surface and decreases monotonically toward the bulk to create a high electric field for charge collection.

[0045] In one embodiment, the drive-in decreases monotonically toward the bulk at less than 100 nm (1E19 cm²). -3 This provides a surface concentration of over 20 nm due to the high surface electric field. Since boron is less mobile below this temperature, the typical drive-in temperature is above 700°C. Temperatures below 700°C can also be used for narrow doping profiles, for example, less than 20 nm. Since boron is typically deposited at 675°C, intrinsic doping may exist. This intrinsic doping may be sufficient without requiring an additional annealing step.

[0046] In one example, the p-type SiGe layer 105 is strained. Because the SiGe layer can be thin (e.g., less than 50 nm), the strain can cause several crystal defects in the SiGe. High boron doping can compensate for the strain and counteract carrier recombination in the SiGe by creating a high electric field on the surface.

[0047] The p-type SiGe layer 105 has a composition factor x ranging from 0 to 1. X Ge 1-XThe composition may include the composition factor x. The value of the composition factor x depends on the processing conditions. In another example, the composition factor x can vary continuously from 0 below the boron layer 106 to 1 above the silicon layer 101.

[0048] The p-type SiGe layer 105 may be an active layer for photogeneration. For photogeneration, monotonic boron doping may be present, with a thickness of less than 50 nm, on the back / irradiated surface of the image sensor, and decreasing from the surface toward the bulk. In one example, for a high electric field and efficient charge collection, doping may be 1e19cm at the surface. -3 Ultra-high bulk concentration 1e14cm -3 It can vary to less than [a certain value]. SiGe, together with the p-type silicon layer 102, forms the active layer. A portion of the light tail that is not absorbed by SiGe is absorbed by the p-type silicon layer 102 for photogeneration.

[0049] In Figure 6, an anti-reflective coating 107 is formed on the boron layer 106 within the trench 104. Although only the trench 104 is disclosed in Figure 6, the anti-reflective coating 107 may also be formed on other surfaces of the boron layer 106. The anti-reflective coating 107 can improve the performance of the image sensor 100. The anti-reflective coating 107 may be made from, for example, a metal fluoride (such as MgF2), SiO2, Al2O3, or a combination thereof. The anti-reflective coating 107 may be a single layer or a multilayer.

[0050] In one example, the anti-reflective coating 107 may be deposited over the entire back surface. This can be done after the metallization of the surface. Since some processes on the surface may affect the anti-reflective coating 107, the anti-reflective coating 107 may be applied before dicing.

[0051] The metal layer 108 can be added to the polysilicon layer 103 using a metallization process. Metallization may be carried out at a temperature of approximately 450°C. Metallization may be carried out before the formation of the anti-reflective film 107. The metal layer 108 may be used in conjunction with the interconnection of a CMOS sensor, a CCD sensor, or a photodiode circuit element. The metal layer 108 may have a multilayer structure with interlayer dielectrics that separate the metal layers to prevent short circuits.

[0052] In addition to the metal layer 108, a gate layer can be formed on the p-type silicon layer 102. The gate layer can be formed before the polysilicon layer 103 and before thinning. The gate layer may include one or more layers of dielectric material such as SiO2 or Si3N4. Circuit elements can be formed on this gate layer using polysilicon and dielectric material. The circuit elements may include transistors, diodes, resistors, capacitors, or electrical interconnects that enable the operation of the photodetector. The circuit elements may be isolated by dielectric material to avoid short circuits.

[0053] The substrate equipped with the image sensor 100 may be diced and packaged into individual image sensors 100 or sensor chips after the metal layer 108 and anti-reflective film 107 have been applied.

[0054] The resulting image sensor 100 includes a p-type silicon layer 102 and a silicon layer 101 disposed on the p-type silicon layer 102. The silicon layer 101 defines a trench 104 that exposes the p-type silicon layer 102 at the bottom of the trench 104. A p-type SiGe layer 105 is disposed at the bottom of the trench 104 and on the silicon layer 101 that forms the trench 104. A boron layer 106 is disposed on the p-type SiGe layer 105 within the trench 104. An anti-reflective coating 107 is disposed on the boron layer 106 within the trench. The anti-reflective coating 107 may be located only within the trench 104 or elsewhere on the surface of the image sensor 100. The anti-reflective coating 107 may be located on the boron layer 106, the SiGe layer 105, and the low-doped p-type silicon layer 102. This is where light reaches. These layers typically extend across the entire back surface (sidewalls and unetched areas). The polysilicon layer 103 or multilayer structure may be located on the opposite side of the p-type silicon layer 102 from the silicon layer 101. The metal layer 108 is located on top of the polysilicon layer 103.

[0055] The various layers within the image sensor 100 may be continuous. For example, the p-type SiGe layer 105 and the boron layer 106 may be continuous. The side walls and back surface may be inactive in terms of light reception.

[0056] The various layers within the image sensor 100 may be formed directly on each other (i.e., without other intervening layers). For example, the p-type SiGe layer 105 may be formed directly on the p-type silicon layer 102 and the silicon layer 101. In another example, the boron layer 106 may be formed directly on the p-type SiGe layer 105.

[0057] The image sensor 100 contains boron-coated SiGe, which is located on top of a silicon layer 101. Compared to boron-coated Si, the image sensor 100 shows a 20% to 90% increase in VUV / DUV photon absorption efficiency. The presence of the boron layer 106 improves quantum efficiency and long-term radiation stability in the image sensor 100. An anti-reflective coating 107 can provide further improvements in quantum efficiency. In one example, the image sensor 100 is configured for DUV and VUV wavelengths.

[0058] The image sensor 100, equipped with boron-coated SiGe, reduces reflection losses from the boron-SiGe interface, which can result in an approximately 1.5 to 2-fold increase in VUV photon absorption efficiency. The VUV and DUV photon absorption efficiencies of the image sensor are approximately 0.3 to 0.4, which is higher than that of the boron-free structure. Higher photon absorption efficiency can potentially lead to increased VUV and DUV photodetection sensitivity. Figure 7 shows the calculation of the percentage of photons transmitted through the boron and anti-reflective overlayer into the silicon and silicon-germanium substrates at VUV and DUV wavelengths.

[0059] In a particular embodiment, the image sensor 100 is a back-illuminated image sensor comprising a silicon membrane epitaxially grown with circuit elements on its surface, a p-doped SiGe layer less than 100 nm thick epitaxially grown on its back surface, a pure boron layer less than 20 nm thick deposited on the SiGe layer, and an anti-reflective overlayer or overlayer.

[0060] The resulting sensor module array, equipped with an image sensor 100, may be a time-delay integral (TDI) sensor module. In one embodiment, each TDI sensor module may include local drive and signal processing circuitry. This circuitry may include a TDI sensor (central block), processing circuitry for processing signals from the TDI sensor, timing and serial drive circuitry, and pixel gate driver circuitry. The drive / processing circuitry is arranged around the TDI sensor. Thus, TDI sensors in adjacent rows can be aligned so that at least 100% image coverage is achieved when used in a continuous scan configuration.

[0061] Figure 8 shows an exemplary inspection system 200 configured to measure a sample 204, such as a wafer, reticle, or photomask. The sample 204 is placed on a stage 205 to facilitate movement of the sample 204 to different regions below the optical system 202. The stage 205 can move in one or more axial directions and / or rotate. In one embodiment, the stage 205 can adjust the height of the sample 204 during inspection to maintain focus. In other embodiments, the objective lens 203 can be adjusted to maintain focus.

[0062] The illumination source 201 may include one or more lasers and / or broadband light sources. The illumination source 201 may emit DUV and / or VUV radiation. An optical system 202, including an objective lens 203, can direct the radiation toward the sample 204 and focus it onto the sample. The optical system 203 may also include mirrors, lenses, and / or beam splitters. Light reflected or scattered from the sample 204 is collected, guided, and focused by the optical system 202 and sent to the detector 206 in the detector assembly 207.

[0063] The detector 206 may include one or more of the image sensors described herein, including CCD sensors, CMOS sensors, and electron shock image sensors incorporating image sensors. The detector 206 may also include a two-dimensional array sensor or a one-dimensional line sensor. In one embodiment, the output of the detector 206 is provided to a processor 208, which analyzes its output. The processor 208 may be configured by program instructions that can be stored on a carrier medium (not shown).

[0064] In one embodiment, the illumination source 201 may be a continuous light source such as an arc lamp, a laser-excited plasma light source, or a CW laser. In another embodiment, the illumination source 201 may be a pulsed light source such as a mode-locked laser, a Q-switched laser, or a plasma light source excited by a Q-switched laser. In an embodiment of the inspection system 200 incorporating a Q-switched laser, the image sensor in the detector 206 is synchronized with the laser pulse. In this embodiment, the image sensor operates in TDI mode during the laser pulse, and data can then be read out through multiple outputs on both sides of the sensor during the laser pulse.

[0065] One embodiment of the inspection system 200 illuminates a line on the sample 204 and collects scattered and / or reflected light in one or more dark-field and / or bright-field acquisition channels. In such an embodiment, the image sensor may be a line sensor or an electronic impact line sensor.

[0066] One embodiment of the inspection system 200 illuminates multiple spots on a sample 204 and collects scattered and / or reflected light in one or more dark-field and / or bright-field acquisition channels. In such an embodiment, the image sensor may be a two-dimensional array sensor or an electron impact two-dimensional array sensor.

[0067] Figure 9 is a schematic diagram of one embodiment of an image sensor equipped with boron-coated silicon germanium. The gray gradient background in the p+ SiGe epitaxial layer and the p- Si epitaxial layer indicates doping concentration, with darker gray indicating higher doping concentration. Figure 9 shows exemplary interconnects and circuit elements.

[0068] Figures 10–16 show cross-sectional side view flow diagrams of another exemplary process for manufacturing an image sensor on a silicon substrate using partial wafer thinning. Figures 10–16 may correspond to the steps shown in Figures 1–6. The capping layer may correspond to the anti-reflective coating 107. The capping layer in Figure 16 extends over a larger portion of the surface. Embodiments in Figures 10–16 also include the circuit elements and surface metals generally described in Figures 1–6.

[0069] Figures 17–23 show cross-sectional side view flow diagrams of another exemplary process for manufacturing an image sensor on a silicon substrate using complete wafer thinning. In Figure 19, a second handle substrate is placed on top of a protective layer on the surface circuit elements. In Figure 20, the p+ silicon substrate is etched to form regions near blind vias. A p+ SiGe layer can be applied epitaxially as shown in Figure 21. In Figure 23, a boron layer is applied to the p+ SiGe layer. In Figure 23, a capping layer (e.g., an anti-reflective coating) is applied to the boron layer.

[0070] Figures 24–29 show cross-sectional side view flow diagrams of another exemplary process for manufacturing an image sensor on a silicon-on-insulator (SOI) substrate using partial wafer thinning. As shown in Figure 24, an oxide layer is included between the silicon substrate and the upper silicon layer. The trench formed in Figure 26 extends through the silicon substrate and the oxide layer so that the upper silicon layer is exposed. In Figure 27, a p+ SiGe layer is applied within the trench. In Figure 28, a boron layer is applied to the p+ SiGe layer. In Figure 29, a capping layer (e.g., an anti-reflective coating) is applied to the boron layer.

[0071] Figures 30–36 show cross-sectional side view flow diagrams of another exemplary process for manufacturing an image sensor on an SOI substrate using complete wafer thinning. As shown in Figure 30, an oxide layer is included between the silicon substrate and the upper silicon layer. In Figure 32, a second silicon handle substrate is placed on top of the protective layer for the surface circuit elements. In Figure 33, the oxide film is etched to form regions near blind vias. In Figure 34, a p+ SiGe layer is applied between the etched oxide films. In Figure 35, a boron layer is applied to the p+ SiGe layer, which can be done between the etched oxide films. In Figure 36, a capping layer (e.g., an anti-reflective coating) is applied to the boron layer.

[0072] The thickness, processing temperature, and other parameters described in Figures 1 to 6 can be applied to the embodiments shown in Figures 10 to 16, 17 to 23, 24 to 29, and 30 to 36.

[0073] In one embodiment, all or almost all of the silicon substrate is thinned. All SiGe and boron processes can be carried out at temperatures below 450°C. Metal processes can be completed before thinning.

[0074] Although this disclosure has described one or more specific embodiments, it will be understood that other embodiments of this disclosure can be made without departing from the scope of this disclosure. Accordingly, this disclosure is deemed to be limited only by the appended claims and their reasonable interpretation.

Claims

1. p-type silicon layer and A silicon layer disposed on the aforementioned p-type silicon layer, A p-type SiGe layer disposed on the aforementioned p-type silicon layer, A boron layer disposed on the aforementioned p-type SiGe layer, An anti-reflective coating disposed on the boron layer, An image sensor equipped with the following features.

2. The image sensor according to claim 1, further comprising a polysilicon layer disposed on the opposite side of the p-type silicon layer from the silicon layer.

3. The image sensor according to claim 1, further comprising a metal layer disposed on the polysilicon layer.

4. The image sensor according to claim 1, wherein the p-type SiGe layer is a continuous layer.

5. The image sensor according to claim 1, wherein the boron layer is a continuous layer.

6. The image sensor according to claim 1, wherein the p-type SiGe layer has a thickness of 20 to 50 nm.

7. The image sensor according to claim 1, wherein the boron layer has a thickness of 2 to 20 nm.

8. The image sensor according to claim 1, wherein the p-type SiGe layer is directly disposed on the p-type silicon layer and the silicon layer.

9. The image sensor according to claim 1, wherein the boron layer is directly disposed on the p-type SiGe layer.

10. The aforementioned silicon layer defines a trench at the bottom of the trench that exposes the p-type silicon layer. The p-type SiGe layer is positioned at the bottom of the trench such that the p-type SiGe layer is positioned on the p-type silicon layer and on the silicon layer forming the trench. The boron layer is arranged on the p-type SiGe layer in the trench. The image sensor according to claim 1.

11. The image sensor according to claim 1, further comprising a second silicon handle substrate disposed on the p-type silicon layer opposite to the p-type SiGe layer.

12. The image sensor according to claim 1, further comprising an oxide layer disposed between the p-type silicon layer and the silicon layer.

13. An inspection system comprising the image sensor described in claim 1.

14. Forming a p-type silicon layer on a silicon layer, Forming a p-type SiGe layer on the aforementioned p-type silicon layer, The p-type SiGe layer is coated with a boron layer, Forming an anti-reflective coating on the boron layer, A method for manufacturing an image sensor, including [the specified component].

15. The method according to claim 14, further comprising forming a polysilicon layer on the side of the p-type silicon layer opposite to the silicon layer.

16. The method according to claim 15, further comprising performing a metallization process to thereby add a metal layer on the polysilicon layer.

17. The method according to claim 14, wherein the p-type silicon layer or the p-type SiGe layer is formed using epitaxial growth.

18. The method according to claim 14, further comprising an annealing step in which, after the boron layer is formed, boron from the boron layer is introduced into the p-type SiGe layer.

19. The method according to claim 18, wherein the annealing step is performed at a temperature of 450°C to 950°C.

20. The process further includes etching trenches into the silicon layer, The trench exposes the p-type silicon layer at the bottom of the trench. The p-type SiGe layer is placed on the p-type silicon layer at the bottom of the trench and on the silicon layer forming the side wall of the trench. The method according to claim 14.

Citation Information

Patent Citations

  • Back-illuminated sensor with boron layer

    US20190131465A1

  • Back-Illuminated Sensor And A Method Of Manufacturing A Sensor

    US20190386054A1