Recycling of catalyst coating film components

The method of solvent treatment, forced filtration, and selective acid leaching effectively recycles catalyst-coated membranes by recovering platinum group metals and ionomers in high yield, addressing the environmental hazards of incineration and preserving component integrity.

JP2026538963APending Publication Date: 2026-11-19JOHNSON MATTHEY PLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026520519
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-13
Filing Date
2024-09-03
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Current methods for recycling catalyst-coated membranes (CCMs) from fuel cells and hydrogen-generating water electrolyzers involve incineration, which releases harmful gases and destroys ionomer components, necessitating a cleaner and more environmentally friendly process to recover both platinum group metals (PGMs) and ionomers.

Method used

A method involving solvent treatment, forced filtration, and selective acid leaching to separate and recover platinum group metals and ionomers in high yield, using techniques like centrifugal filtration and controlled acid leaching to preserve the integrity of carbon catalyst-supported and membrane-reinforced materials.

Benefits of technology

Achieves high recovery yields of PGMs and ionomers while minimizing environmental impact by reducing harmful emissions and maintaining the integrity of other components, ensuring safe and efficient recycling.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026538963000001_ABST
    Figure 2026538963000001_ABST
Patent Text Reader

Abstract

A method for recycling waste ionomer material comprising at least one ionomer, at least one platinum group metal, and one or more of a metal catalyst material, a carbon catalyst support material, and a film reinforcing material, comprising: (a) treating the waste ionomer material with a solvent to disperse the ionomer and form an ionomer dispersion containing one or more of a metal catalyst material, a carbon catalyst support material, and a film reinforcing material; and (b) subjecting the ionomer dispersion to a forced filtration technique in which force is actively applied to the ionomer dispersion to push out the metal catalyst material, carbon catalyst support material, A method comprising: (c) producing a filter cake on a filter containing one or more of the and membrane reinforcing materials, and a filtrate of an ionomer dispersion; and (c) extracting platinum group metals using one or more acid leaches, wherein (i) one or more acid leaches are applied to waste ionomer material before forming the ionomer dispersion in step (a) to extract platinum group metals from the waste ionomer material, or (ii) one or more acid leaches are applied to the filter cake material after step (b) to extract platinum group metals from the filter cake material.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] The present specification relates to a method for recycling components of catalyst-coated membranes, such as those used in fuel cells and hydrogen-generating water electrolyzers. BACKGROUND ART

[0002] As investments are made in the global hydrogen economy, the production of fuel cells and hydrogen-generating water electrolyzers is expected to grow rapidly. The catalyst coated membrane (CCM) is a major functional component of both fuel cells and electrolyzers. Such CCMs generally comprise an electrically conductive polymer membrane coated on both sides by catalyst-containing layers. The CCM is configured to drive oxidation and reduction reactions and support proton and electron transport, and these processes are required for fuel cell and electrolyzer technologies to function.

[0003] While variations exist in the materials and configurations of CCM components according to functional performance requirements in end-use applications, they generally contain several useful components including one or more platinum group metal (PGM) catalysts and one or more proton-conductive polymers.

[0004] Typically, the membrane is formed from one or more ionomers, such as perfluorosulfonic-acid (PFSA) ionomers. Ionomers may also be provided in one or both of the catalyst layers. The ionomer in the catalyst layer may be the same as or different from the ionomer in the main membrane component and / or in the other catalyst layer.

[0005] The CCM may contain two different catalysts, one for driving an oxidation reaction on one side of the CCM and the other for driving a reduction reaction on the other side of the CCM. The CCM may also contain a recombination catalyst provided to catalyze the recombination of hydrogen and oxygen to form water, reducing the amount of hydrogen passing through the membrane and mixing with oxygen to form a potentially explosive mixture. The CCM may also contain a metal oxide (e.g., CeO2) as a peroxide scavenger.

[0006] CCM catalysts can be based on platinum group metals such as platinum, ruthenium, iridium, palladium, or mixtures thereof. Platinum group metals may be provided in elemental (metallic) form, compound form (e.g., oxides such as iridium oxide catalysts), or PGM-based metal alloys (e.g., PtCo). Furthermore, the PGM catalyst material may be supported on a substrate material (e.g., carbon such as a platinum-supported carbon catalyst or PtCo-supported carbon containing carbon particles on which platinum is arranged).

[0007] The catalyst coating (CCM) can also be provided in combination with additional functional layers to form a membrane electrode assembly (MEA). Such an MEA may have, for example, 3, 5, or 7 layers.

[0008] With the increase in CCM production for fuel cells and electrolytic cells, there is also a corresponding increase in CCM waste material, including large amounts of scrap material generated during CCM production (e.g., due to quality control failures), and an increase in end-of-life (EoL) CCM. Since CCM contains several rare and / or valuable components, including platinum group metals (particularly Pt, Pd, Ir, and Ru) and ionomers (in both membrane and catalyst layers), there is a growing demand for methods to recycle such components from waste CCM material.

[0009] One current method for recovering PGMs from production scrap and end-of-life CCM materials involves incineration. The incineration process produces PGM-rich ash (typically Pt and Ir) that is processed through conventional PGM refining routes. However, the incineration process releases harmful and toxic gases such as CO2 and HF from the polymers that are part of the membrane. Both of these gases have adverse effects as they pollute the atmosphere, increase the greenhouse effect, and / or have harmful effects on human health. Therefore, cleaner methods are needed to reduce or eliminate the emissions of these gases.

[0010] In addition to the above, incineration methods destroy ionomer components, which are of equally important value. Therefore, it is desirable to provide a process that can recover both PGMs and ionomer components, as well as a process that is cleaner, safer, and more environmentally friendly. Processes for recovering perfluorosulfonic acid ionomers are known. See, for example, International Publication WO2016 / 156815 and U.S. Patent No. 7255798. Furthermore, processes for recovering individual PGM catalyst components are known. See, for example, U.S. Patent No. 7709135. However, in order to enable fuel cells and electrolytic cells to become more sustainable technologies, there is a need for commercially viable and environmentally friendly routes for recovering, separating, and recycling both PGMs and ionomer components from waste CCM materials, including production scrap and end-of-life materials.

[0011] The purpose of this specification is to address this problem. [Overview of the Initiative]

[0012] This specification relates to a method for recycling waste ionomer materials that enables the separation and recovery of both platinum group metal components and ionomer components in a purified form in high yield, while also ensuring that other component materials in the waste ionomer material, such as metal catalyst materials, carbon catalyst supported materials, and / or film reinforcing materials, are separated and recovered during processing.

[0013] This specification provides a method for recycling waste ionomer material, comprising at least one ionomer, at least one platinum group metal, and one or more of the following: a metal catalyst material (e.g., containing a platinum group metal), a carbon catalyst supporting material, and a film reinforcing material. (a) Treating waste ionomer material with a solvent to disperse the ionomer and form an ionomer dispersion containing one or more of the following: a metal catalyst material, a carbon catalyst supporting material, and a film reinforcing material. (b) Subjecting the ionomer dispersion to a forced filtration technique in which force is actively applied to the ionomer dispersion to push it through a filter, thereby producing a filter cake on the filter containing one or more of a metal catalyst material, a carbon catalyst supported material, and a membrane reinforcing material, as well as a filtrate of the ionomer dispersion. (c) A method for extracting platinum group metals using one or more acid leachings, wherein (i) one or more acid leachings are applied to waste ionomer material before forming an ionomer dispersion in step (a) to extract platinum group metals from the waste ionomer material, or (ii) one or more acid leachings are applied to filter cake material after step (b) to extract platinum group metals from the filter cake material.

[0014] Forced filtration techniques can be selected from centrifugal filtration, negative pressure (i.e., vacuum) filtration, and positive pressure filtration. Centrifugal filtration has been found to be particularly effective in separating ionsomers from carbon catalyst-supported materials and membrane-reinforced materials to produce high-purity ionomer dispersions in high yield. It can be noted that while filtration has been used previously, forced filtration techniques such as centrifugal filtration have been found to be significantly more effective in producing high-purity ionomer dispersions in high yield. It can also be noted that while centrifugation of ionomer materials has also been disclosed previously, it is not in combination with filtration to provide a centrifugal filtration process. For example, U.S. Patent No. 7,255,798 uses centrifugation to separate ionsomers from platinum-supported carbon catalyst materials, but does not consider the use of centrifugal filtration to collect solids such as carbon catalyst-supported materials and membrane-reinforced materials. International Publication No. WO2016156815 also mentions centrifugation, but does not disclose centrifugal filtration for separating ionomer dispersions and collecting solids such as carbon catalyst-supported materials and membrane-reinforced materials.

[0015] The waste ionomer material may additionally include one or both of the sealing material and the gas diffusion layer material, in which case the filter cake formed in step (b) includes one or both of the sealing material and the gas diffusion layer material.

[0016] After separating the ionomer dispersion by forced filtration, the filter cake material is processed to separate and recover one or more of the following: metal catalyst material, carbon catalyst supported material, membrane reinforcement material, sealing material, and gas diffusion layer material. For example, the filter cake material can be processed to separate and recover one or more of the following: metal catalyst material, carbon catalyst supported material, membrane reinforcement material, sealing material, and gas diffusion layer material, by forming a slurry of the filter cake material and performing one or more filters of the slurry, optionally forced filtration, to achieve separation based on different particle sizes of the materials. Typically, the carbon catalyst supported material and / or metal catalyst material have smaller particle sizes than the membrane reinforcement material, and a suitable filter is selected such that the filtration of the slurry yields a filtrate containing the carbon catalyst material and / or metal catalyst material with membrane reinforcement material trapped on the filter.

[0017] According to a particular preferred method, one or more acid leachings are applied to waste ionomer material to form an ionomer dispersion and to extract platinum group metals from the waste ionomer material before treating the ionomer dispersion through a forced filtration process. In this case, it has been found that the platinum group metals can be acid-leaded while retaining the carbon catalyst-supported material and membrane-reinforced material in a solid form with sufficient particle size, and after the ionomer is dispersed, the carbon catalyst-supported material and membrane-reinforced material can be efficiently separated by forced filtration.

[0018] In alternative methodologies, ionomer dispersion and forced filtration are performed before acid leaching to extract the platinum group metal material. In this case, during forced filtration, the carbon catalyst-supported material and / or metal catalyst material being filtered contains the platinum group metal catalyst material. Acid leaching is then applied to the filter cake material to extract the platinum group metals from the filter cake material. Acid leaching may still be applied to a filter cake material that still contains a mixture of the carbon catalyst-supported material, the membrane-reinforced material, and optionally the sealing material and / or the gas diffusion layer material. Alternatively, the filter cake material can be treated first to separate the platinum group metal catalyst material, optionally including the carbon catalyst-supported material, and then only that portion of the filter cake material is subjected to acid leaching. That is, according to a different version of the methodology of the present invention, acid leaching may be applied to the filter cake material before or after the filter cake material has been treated to separate and recover one or more of the metal catalyst material, carbon catalyst-supported material, membrane-reinforced material, sealing material, and gas diffusion layer material.

[0019] For waste ionomer materials containing platinum, palladium, and / or ruthenium, acid leaching may include acid leaching using a heated solution containing an acid and an oxidizing agent, in which case the platinum, palladium, and / or ruthenium are leached into the solution.

[0020] For waste ionomer materials containing iridium, acid leaching may include acid leaching using a heated solution containing an acid and a reducing agent, and the iridium will leach into the solution.

[0021] For waste ionomer materials containing both platinum, palladium, and / or ruthenium, as well as iridium, acid leaching may include both the oxidative and reductive leaching methods described above. While these two leaching methods can be performed in either order, oxidative leaching has been found to be selective for platinum, palladium, and / or ruthenium, with virtually no iridium being leached. In contrast, reductive iridium leaching also leaches some of the platinum, palladium, and / or ruthenium. While the mixed solution of iridium and platinum, palladium, and / or ruthenium can be further treated to separate the PGMs, it is advantageous to perform oxidative leaching first, followed by reductive leaching, thereby pre-separating platinum, palladium, and / or ruthenium from iridium in the process. This improves process efficiency and reduces downstream separation requirements.

[0022] From the above viewpoint, it is preferable that oxidative acid leaching be carried out before reducing acid leaching. This methodology also includes treating the waste ionomer material with a heated solvent to disperse the ionomer, which is preferably carried out after oxidative and reducing leaching. This is because it has been found that if the ionomer dispersion step is carried out while the PGM catalyst material is still present, the PGM catalyst can promote the decomposition of the ionomer during dispersion. Therefore, it is preferable that the PGM material be removed before the ionomer dispersion step.

[0023] The solvent used to disperse the ionomer can be selected from water, a basic aqueous solution, an organic solvent, an alcohol, or a mixture of alcohol and water. Furthermore, the solvent used to disperse the ionomer can be heated to a temperature within the range defined by at least 150°C, 180°C, 200°C, 220°C, 230°C, or 240°C; 400°C or less, 300°C or less, 275°C or less, or 250°C or less; or any combination of the aforementioned lower and upper limits. Moreover, it is preferable that the ionomer be treated with a base to convert it into a salt form before dispersing it in the solvent. These conditions have been found to achieve a highly dispersed ionomer while retaining the carbon catalyst-supported material and membrane-reinforced material in a solid form with sufficient particle size so that the carbon catalyst-supported material and membrane-reinforced material can be efficiently separated from the highly dispersed ionomer via forced filtration. Subsequently, after forced filtration, the ionomer dispersion can be subjected to an ion exchange process to reprotonate the ionomer. [Brief explanation of the drawing]

[0024] For a better understanding of the present invention and to illustrate how it can be implemented, certain embodiments of the present invention are described hereby by reference only to the accompanying drawings. [Figure 1] This specification outlines the waste CCM recycling process. [Figure 2] The waste CCM recycling process, including platinum leaching, followed by iridium leaching, and then ionomer dispersion, is illustrated. [Figure 3]A more detailed example illustrating a spent CCM recycling process is provided, which includes the following steps in the stated order: (i) recovering platinum by oxidative acid leaching; (ii) recovering iridium by reductive acid leaching; (iii) treating the remaining solid ionomer material with a base to form a solid ionomer salt material; (iv) heating the solid ionomer salt material in a solvent to disperse and recover the ionomer material; (v) separating the ionomer dispersion from other components including carbon catalyst support material and / or membrane reinforcement material via a forced filtration technique; and (vi) subjecting the ionomer dispersion to an ion exchange process to reprotonate the ionomer material. [Figure 4] FTIR data is shown for the fluorinated polymer membrane material (301), the fluorinated polymer salt material (303) formed after treatment in water and base, and the fluorinated polymer salt material (304) formed after treatment in water and base and subsequently washed with water. [Figure 5] An example of process steps (before autoclaving) is shown, comprising refluxing a fluorinated polymer membrane in a basic LiOH solution to form a fluorinated polymer salt without dispersing the membrane, followed by washing with water. [Figure 6] This is a photograph showing the membrane before (left side) and after (right side) the process step of refluxing the membrane in a basic LiOH solution and washing with water. [Figure 7] A further step is shown of subjecting the membrane to an autoclave treatment following the treatment process illustrated in Figure 3, in order to disperse the membrane in water. [Figure 8] A further ion exchange step (after autoclaving) is shown for converting the dispersed polymer salt back to the protonated acid form. DETAILED DESCRIPTION OF EMBODIMENTS

[0025] As described in the Overview section and illustrated in Figure 1, this specification provides a method for recycling waste ionomer material, comprising at least one ionomer, at least one platinum group metal, and one or more of the following: a metal catalyst material (e.g., including a platinum group metal), a carbon catalyst supporting material, and / or a film reinforcing material. (a) Treating waste ionomer material with a solvent to disperse the ionomer and form an ionomer dispersion containing one or more of the following: a metal catalyst material, a carbon catalyst supporting material, and / or a film reinforcing material. (b) Subjecting the ionomer dispersion to a forced filtration technique in which force is actively applied to the ionomer dispersion to push it through a filter, thereby producing a filter cake on the filter containing one or more of a metal catalyst material, a carbon catalyst supported material, and / or a membrane reinforcing material, as well as a filtrate of the ionomer dispersion. (c) A method for extracting platinum group metals using one or more acid leachings, wherein (i) one or more acid leachings are applied to waste ionomer material before forming an ionomer dispersion in step (a) to extract platinum group metals from the waste ionomer material, or (ii) one or more acid leachings are applied to filter cake material after step (b) to extract platinum group metals from the filter cake material.

[0026] Forced filtration techniques can be selected from centrifugal filtration, negative pressure (i.e., vacuum) filtration, and positive pressure filtration. Centrifugal filtration has been found to be particularly effective in separating ionomers from carbon catalyst-supported materials and membrane-reinforced materials to produce high-purity ionomer dispersions in high yield.

[0027] The waste ionomer material may additionally include one or both of the sealing material and the gas diffusion layer material, in which case the filter cake formed in step (b) includes one or both of the sealing material and the gas diffusion layer material. After separating the ionomer dispersion by forced filtration technique, the filter cake material is processed to separate and recover one or more of the carbon catalyst supporting material, membrane reinforcing material, sealing material, and gas diffusion layer material. For example, the filter cake material can be processed to separate and recover one or more of the carbon catalyst supporting material, membrane reinforcing material, sealing material, and gas diffusion layer material by forming a slurry of the filter cake material and performing one or more filters of the slurry, optionally forced filtration, to achieve separation based on different particle sizes of the materials. Typically, the carbon catalyst supporting material has a smaller particle size than the membrane reinforcing material, and a suitable filter is selected such that the filtration of the slurry yields a filtrate containing the carbon catalyst supporting material with membrane reinforcing material capture on the filter.

[0028] According to a particular preferred method, one or more acid leachings are applied to waste ionomer material to form an ionomer dispersion and to extract platinum group metals from the waste ionomer material before treating the ionomer dispersion through a forced filtration process. In this case, it has been found that the platinum group metals can be acid-leaded while retaining the carbon catalyst-supported material and membrane-reinforced material in a solid form with sufficient particle size, and after the ionomer is dispersed, the carbon catalyst-supported material and membrane-reinforced material can be efficiently separated by forced filtration.

[0029] In alternative methodologies, ionomer dispersion and forced filtration are performed before acid leaching to extract the platinum group metal material. In this case, acid leaching is applied to the filter cake material to extract the platinum group metal from the filter cake material.

[0030] The leaching and dispersion steps may be carried out in any order, but one preferred methodology is shown in Figure 2, which illustrates a waste CCM recycling process including platinum leaching, followed by iridium leaching, and then ionomer dispersion. This example provides a method for recycling waste catalyst coating material comprising an ionomer film and at least one catalyst including platinum (e.g., platinum-supported carbon catalyst), palladium, and / or ruthenium, and at least one catalyst including iridium (e.g., iridium oxide catalyst). This method is (a) A treatment in which the waste catalyst coating material is treated with a solution containing an acid and an oxidizing agent, wherein platinum, palladium and / or ruthenium are leached from the waste catalyst coating material into the solution, and the solution is separated from the remaining solid components of the waste catalyst coating material. (b) After step (a), iridium is leached from the waste catalyst coating material using a heated solution containing an acid and a reducing agent, and the solution containing the leached iridium is separated from the remaining solid components of the waste catalyst coating material. (c) After steps (a) and (b), the waste catalyst coating material is treated with a heated solvent to disperse the ionomer film, and the ionomer dispersion is recovered.

[0031] By carrying out the above-described steps in the order described, it is possible to recover platinum, palladium, and / or ruthenium, iridium, and the ionomer material separately without significantly degrading the ionomer, ensuring that substantially all (e.g., at least 97%) of the PGMs are recovered and that platinum and iridium are separated beforehand in the process.

[0032] The acid used in either or both iridium leaching and / or platinum leaching is preferably hydrochloric acid and optionally does not contain nitric acid. Furthermore, either or both of the solutions used for platinum leaching and / or iridium leaching are preferably heated to a temperature within the range defined by at least 50°C, 60°C, or 70°C; 160°C or less, 120°C or less, 100°C or less, or 90°C or less; or any combination of the aforementioned lower and upper limits, and if the solution is heated above 100°C, this is done in a pressurized vessel. Exemplary temperatures are about 70°C for platinum leaching and about 105°C for iridium leaching. The solution is heated to increase the leaching rate of the PGM.

[0033] The oxidizing agent may include, for example, a sodium chlorate solution, hydrogen peroxide, or a chlorate such as chlorine gas. According to one preferred option, the acid used in the leaching of platinum, palladium, and / or ruthenium is hydrochloric acid, and the oxidizing agent is chlorine gas produced in situ from hydrochloric acid electrolytically. The oxidizing agent may be added to the hydrochloric acid solution or produced in situ after heating to the aforementioned temperature. Alternatively, the oxidizing agent may be added to multiple aliquots during heating. For example, the oxidizing agent may be added to a series of aliquots during heating. The solution for leaching platinum may have an oxidizing agent concentration (e.g., a total oxidizing agent concentration in the range of 0.01 to 0.10 mol / l) within the range defined by at least 0.001, 0.005, or 0.01 mol / l; 1 or less, 0.5 or less, or 0.10 mol / l or less; or any combination of the aforementioned lower and upper limits. Either or both of the solutions used for platinum leaching and / or iridium leaching have an acid concentration within the range defined by 4M or more, 5M or more, 5.5M or more, or 6M or more; 15M or less, 12M or less, 10M or less, or 7M or less; or any combination of the aforementioned lower and upper limits.

[0034] The separation of the solution containing leached platinum can be achieved by filtration or centrifugation. The separated solution may be concentrated by boiling to a suitable platinum concentration for further processing. Alternatively, the leachate can be recirculated to leach platinum from further waste catalyst coating material, and the recirculation is repeated as needed until a suitable or target concentration of platinum is reached. For example, after separating the solution containing leached platinum from the remaining solid components of the waste catalyst coating material, the solution can be concentrated to obtain chloroplatinic acid containing at least 30% by weight of Pt.

[0035] One advantage of the aforementioned process is that it achieves high recovery yields for platinum, palladium, and / or ruthenium. For example, at least 97% by weight of platinum in the waste catalyst coating can be recovered.

[0036] Another advantage of the aforementioned process is that, using these conditions, fluorine is not substantially leached from the fluoropolymer film into the leachate. This is advantageous for two reasons. Firstly, the ionomer remains intact and can be recycled separately. Secondly, fluorine leaching into an acidic leachate can lead to the formation of HF, which can pose serious environmental health and safety risks as well as damage to downstream processing equipment. Therefore, avoiding HF formation provides a safer and more environmentally friendly process.

[0037] Another advantage of the process described above is that, for CCMs containing both platinum and iridium oxide catalysts (a useful combination of catalysts for the cathode and anode catalysts, respectively, in a hydrogen-producing water electrolyzer), the leaching conditions are selective for platinum and do not leach iridium to any significant degree. Therefore, this process represents an efficient method for separating platinum from other components of such waste CCMs while leaving the remaining CCM components intact and processing them separately.

[0038] Iridium (which may be in the form of iridium oxide, mixed iridium oxide, or supported iridium oxide) can be extracted separately using an acid leaching process. This differs from the process used for leaching platinum. In particular, reducing agents (e.g., hydrazine) rather than oxidizing agents are used for iridium leaching. Optionally, the reducing agent is first added to the waste catalyst coating material, followed by the addition of the acid.

[0039] One advantage of the aforementioned process is that it achieves a high recovery yield for iridium. For example, at least 95% by weight of iridium in the waste catalyst coating can be recovered.

[0040] Another advantage of the aforementioned process is that, using these conditions, fluorine is not substantially leached from the fluoropolymer film into the leachate. This is advantageous for two reasons. Firstly, the ionomer remains intact and can be recycled separately. Secondly, fluorine leaching into an acidic leachate can lead to the formation of HF, which can pose serious environmental health and safety risks as well as damage to downstream processing equipment. Therefore, avoiding HF formation provides a safer and more environmentally friendly process.

[0041] As mentioned above, the iridium leaching conditions are such that a significant amount of platinum (e.g., 20-40% of Pt) also leaches out, if it is still present in the waste catalyst coating material. Therefore, according to the methodology of the present invention, Pt (and / or palladium and / or ruthenium) is first removed by oxidative leaching before reductive leaching is applied to recover iridium.

[0042] After platinum and iridium are recovered from the waste catalyst coating, they may be treated with a heating solvent to disperse the ionomer film and recover the ionomer dispersion. The solvent used to disperse the ionomer may be selected from water, basic aqueous solutions, organic solvents, alcohols, or mixtures of alcohol and water. The solvent used to disperse the ionomer may be heated to a temperature within the range defined by at least 150°C, 180°C, 200°C, 220°C, 230°C, or 240°C; 400°C or less, 300°C or less, 275°C or less, or 250°C or less; or any combination of the aforementioned lower and upper limits.

[0043] In one preferred methodology, the ionomers are treated with a base to convert them into a salt form before being dispersed in a solvent. Subsequently, after dispersion of the ionomers, the ionomer dispersion can be subjected to an ion exchange process to reprotonate the ionomers in the dispersion. This methodology has been found to be advantageous in achieving good dispersion of ionomer materials without damaging the ionomer materials, as long as the PGM material is removed before the ionomer dispersion process. Therefore, the preferred process flow illustrated in Figure 3 is as follows: (i) recover platinum (and / or palladium and / or ruthenium) by oxidizing acid leaching; (ii) recover iridium by reducing acid leaching; (iii) form a solid ionomer salt material by treating the remaining solid ionomer material with a base; (iv) disperse and recover the ionomer material by heating the solid ionomer salt material in a solvent; (v) separate the ionomer dispersion from other components (carbon and / or membrane reinforcing material) by forced filtration; and (vi) reprotonate the ionomer material by subjecting the ionomer dispersion to an ion exchange process. [Examples]

[0044] PMD Recovery Regarding the water electrolysis cell materials, Ir was recovered by reductive leaching, but this also resulted in varying levels of Pt recovery. To minimize this mixing of Pt and Ir chloride species, Pt oxidation leaching was attempted first, followed by reductive Ir leaching. For reliability, this experiment was repeated twice.

[0045] Pt oxidation leaching Five water electrolytic cell CCMs were shredded into pieces measuring 1 cm x 2 cm. The total mass of the CCMs was 21.23 g.

[0046] A flanged container equipped with an overhead agitator, a condenser with cooling water, a temperature probe, and plugs on all empty ports was placed on a hot plate. CCM was added to it, and 395 mL of 12 M HCl was added to it, causing the solution to immediately turn yellow. This was set to be stirred at 200 rpm and heated to 70°C.

[0047] When the temperature was reached, 1.25 mL of 30% peroxide was added to the container via a Watson-Marlow peristaltic pump at 1 rpm for the first minute, and then at 7 rpm for the remainder. The reaction was continued by heating for a further 50 minutes. After completion, heating was stopped and the reaction mixture was allowed to cool. This was filtered under vacuum using cellulose nitrate filter paper.

[0048] Ir reduction leaching The leached CCM was suspended in 90 mL of desalted water in a beaker, and 1.8 mL of 35% hydrazine was added dropwise while stirring. The CCM turned gray where it came into direct contact with the hydrazine. This suspension was sonicated in an ultrasonic bath at room temperature for 5 minutes.

[0049] The flanged vessel was set up in the same manner as before using Pt leaching. The CCM suspension was added to the flanged vessel. 250 mL of 12 M HCl was gradually added while stirring at 200 rpm. The CCM fragments began to break apart at this point. A sample was taken. The vessel was heated to 105°C. Once the temperature was reached, a timer was started, and samples were taken every 1.5 hours for a total of 4.5 hours. After this, the reaction vessel was cooled, and the suspension was vacuum filtered. All samples were filtered under vacuum and then syringe filtered.

[0050] Pt oxidation leaching (repeated) For the repeated experiments, the same method was used for oxidative leaching, but the sonication step was omitted for reductive leaching. The mass of CCM was 21.27 g, and 400 mL of 12 M acid was used, heated to 75°C, and 1.5 mL of hydrogen peroxide was added. As before, heating was carried out for 50 minutes.

[0051] Ir reduction leaching (repeated) The flanged vessel was set up as before. CCM was added to the vessel along with 90 mL of demineralized water. The mixture was stirred at 130 rpm, during which 1.8 mL of hydrazine was added dropwise. This was stirred for 5 minutes. 250 mL of 12 M HCl was slowly added while stirring at 300 rpm. The vessel was heated to 105°C as before. Once the temperature was reached, the timer was started, and samples were taken every 1.5 hours for a total of 4.5 hours. After this, the reaction vessel was cooled, and the suspension was vacuum filtered. All samples were filtered under vacuum and then syringe filtered.

[0052] Results, Discussion, and Conclusion When selective oxidative leaching was performed on CCM, it showed a good recovery rate of Pt (approximately 100% within the experimental margin of error). Subsequently, reductive leaching showed a good recovery rate of Ir, and in repeated experiments, it showed an even higher recovery rate (over 95%). Overall, over 97% of PGM was recovered from the CCM material.

[0053] Ionomer recovery Anhydrous LiOH (6.0 g) was added to water (250 g) to dissolve the LiOH in the water. The membrane fragment was submerged in the LiOH solution and heated under reflux for 1 hour. The resulting mixture was washed with (4 × 100 mL) of water. The remaining water was decanted to leave a (moistened) membrane fragment. Water (250 g) was added to the (moistened) membrane fragment and heated under reflux for 1 hour. The water was then decanted and the solid product was dried under vacuum.

[0054] Figure 4 shows FTIR data indicating salt formation. FTIR data was collected for the untreated fluorinated polymer film material 301, the fluorinated polymer salt material 303 formed after treatment in an aqueous LiOH solution, and the fluorinated polymer salt material formed after treatment in an aqueous LiOH solution, followed by water washing 304.

[0055] Figure 5 shows an example of the process steps (before autoclaving). The film was brownish in color as shown in the figure. After refluxing the film in lithium hydroxide solution, the film became colorless and was converted to a salt form, as confirmed by spectroscopic analysis. The conversion was achieved without dispersing the film, and the film remained in a solid, non-dispersible form. In the final step before autoclaving, shown in Figure 4, the solid polymer salt film material was washed with water to remove all residual LiOH solution.

[0056] Figure 6 shows photographs of the film before (left) and after (right) the process of refluxing the film in a basic LiOH solution and washing it with water. It illustrates the change in film color from brown to colorless, and the fact that the film remains in a non-dispersed solid state. Spectroscopic analysis confirmed that the colorless film was in salt form.

[0057] Figure 7 shows a further step of autoclaving the membrane following the processing steps shown in Figure 4, in order to disperse the membrane in water. A colorless solid, undispersed polymer salt membrane was autoclaved in water under nitrogen at 250°C and a self-sustaining pressure of 40 bar (4000 kPa). This yielded a (non-basic) aqueous dispersion of the polymer salt.

[0058] Next, the aqueous dispersion of the polymer (ionomer) salt was subjected to centrifugal filtration to separate the ionomer dispersion from the solid carbon catalyst support and the solid polytetrafluoroethylene membrane reinforcing material. For example, the recycled dispersion containing the ionomer, solid carbon catalyst support, and solid polytetrafluoroethylene was added to a centrifuge tube containing a 0.45 μm PVDF filter. The tube was centrifuged for 2 × 6 minutes with a relative centrifugal force of approximately 3000 g to produce a solid cake on the filter consisting of black (carbon) and white (PTFE) solids, as well as a dispersion containing the ionomer at the bottom of the tube.

[0059] Figure 8 shows a further subsequent ion exchange step to convert the dispersed polymer salt back into a protonated acid form. An ion exchange column containing Amberlyst® 15(H) resin was used in this process step. The dispersion of (protonated)fluorinated polymer may be reused to produce a new membrane or may be dried and stored for future use.

[0060] summary This specification provides a method for recycling waste ionomer materials that allows for the separation and recovery of both platinum group metal components and ionomer components in a purified form with high yield, while also ensuring that other component materials within the waste ionomer material, such as carbon catalyst supporting materials and film reinforcing materials, are separated and recovered during processing.

[0061] Although the present invention has been specifically illustrated and described with reference to certain examples, it will be understood by those skilled in the art that various modifications of form and detail can be made without departing from the scope of the invention as defined by the appended claims.

Claims

1. A method for recycling waste ionomer material, comprising at least one ionomer, at least one platinum group metal, and one or more of a metal catalyst material, a carbon catalyst supporting material, and a film reinforcing material, (a) Treating the waste ionomer material with a solvent to disperse the ionomer and form an ionomer dispersion containing one or more of the metal catalyst material, the carbon catalyst supporting material, and the film reinforcing material, (b) Subjecting the ionomer dispersion to a forced filtration technique in which force is actively applied to the ionomer dispersion to push it through a filter, thereby producing a filter cake on the filter containing one or more of the metal catalyst material, the carbon catalyst supporting material, and the membrane reinforcing material, and a filtrate of the ionomer dispersion, (c) A method for extracting the platinum group metals using one or more acid leachings, wherein (i) the one or more acid leachings are applied to the waste ionomer material before forming the ionomer dispersion in step (a) to extract the platinum group metals from the waste ionomer material, or (ii) the one or more acid leachings are applied to the filter cake material after step (b) to extract the platinum group metals from the filter cake material.

2. The method according to claim 1, wherein the forced filtration technique is selected from one of centrifugal filtration, negative pressure filtration, positive pressure filtration, cross-flow filtration, dead-end filtration, and vacuum filtration.

3. The method according to claim 1 or 2, wherein the waste ionomer material further comprises one or both of the sealing material and the gas diffusion layer material, and the filter cake formed in step (b) comprises one or both of the sealing material and the gas diffusion layer material.

4. The method according to any one of claims 1 to 3, wherein after separating the ionomer dispersion by the forced filtration technique, the filter cake material is processed to separate and recover one or more of the metal catalyst material, the carbon catalyst supporting material, the membrane reinforcing material, the sealing material, and the gas diffusion layer material.

5. The method according to claim 4, wherein the filter cake material is processed to separate and recover one or more of the metal catalyst material, the carbon catalyst supported material, the membrane reinforcing material, the sealing material, and the gas diffusion layer material by performing one or more filters of the slurry based on different particle sizes of the material.

6. The method according to claim 5, wherein the carbon catalyst-supported material and / or the metal catalyst material has a particle size smaller than the film-reinforcement material, and a suitable filter is selected such that the filtration of the slurry yields a filtrate containing the carbon catalyst-supported material and / or the metal catalyst material having the film-reinforcement material trapped on the filter.

7. The method according to claim 4, 5, or 6, wherein step c(ii) is used in claim 1, thereby applying the one or more acid leachings to the filter cake material to extract the platinum group metals from the filter cake material, and the one or more acid leachings are applied before or after processing the filter cake material to separate and recover one or more of the metal catalyst material, the carbon catalyst supporting material, the film reinforcing material, the sealing material, and the gas diffusion layer material.

8. The method according to any one of claims 1 to 7, wherein step (c) comprises acid leaching using a heated solution containing an acid and an oxidizing agent, wherein platinum, palladium, and / or ruthenium are leached into the solution.

9. The method according to any one of claims 1 to 8, wherein step (c) comprises acid leaching using a heated solution containing an acid and a reducing agent, wherein iridium is leached into the solution.

10. The method according to any one of claims 1 to 9, wherein step (a) includes treating the waste ionomer material with a heated solvent to disperse the ionomer.

11. The method according to any one of claims 8 to 10, wherein the oxidizing acid leaching described in claim 12 is performed before the reducing acid leaching described in claim 13.

12. The method according to claim 10 or 11, wherein the solvent used to disperse the ionomer is selected from water, a basic aqueous solution, an organic solvent, an alcohol, or a mixture of alcohol and water.

13. The method according to any one of claims 10 to 12, wherein the solvent used to disperse the ionomer is heated to a temperature within the range defined by at least 150°C, 180°C, 200°C, 220°C, 230°C, or 240°C; 400°C or less, 300°C or less, 275°C or less, or 250°C or less; or any combination of the aforementioned lower and upper limits.

14. The method according to any one of claims 10 to 13, wherein, before dispersing the ionomer in the solvent, the ionomer is treated with a base to convert the ionomer into a salt form.

15. The method according to claim 14, wherein the ionomer dispersion is subjected to an ion exchange process to reprotonate the ionomer after the ionomer has been separated from other materials by the forced filtration of the ionomer dispersion.