Forgeable γ' reinforced superalloy with high mechanical strength

A nickel-chromium-cobalt-based alloy with controlled composition addresses the limitations of existing γ'-reinforced alloys by achieving superior low-cycle fatigue, creep strength, and thermal stability for high-temperature gas turbine components, particularly turbine cases.

JP2026538977APending Publication Date: 2026-11-19HAYNES INTERNATIONAL
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
JP2026522023
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-10-24
Filing Date
2024-10-25
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing forgeable γ'-reinforced alloys do not possess adequate low-cycle fatigue strength, creep strength, and thermal stability at temperatures above 1400°F (760°C), limiting their application in high-temperature gas turbine components like turbine cases.

Method used

A nickel-chromium-cobalt-based alloy with specific compositional ranges of chromium, cobalt, molybdenum, tungsten, aluminum, titanium, niobium, tantalum, and trace elements, along with controlled γ'-forming and solid solution strengthening agents, to achieve high containment performance, thermal stability, and mechanical strength.

Benefits of technology

The alloy exhibits improved low-cycle fatigue strength, creep strength, and thermal stability at 1500°F (816°C), with enhanced containment properties and weldability, surpassing the performance of existing alloys like Waspaloy.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026538977000001_ABST
    Figure 2026538977000001_ABST
Patent Text Reader

Abstract

A forged, age-hardenable nickel-chromium-cobalt-based alloy composition suitable for use in high-temperature gas turbine cases, possessing higher mechanical strength, toughness / containment performance, and thermal stability compared to currently available alloys, along with an acceptable containment coefficient, comprising 16-20 wt% chromium, 8-13 wt% cobalt, 4-8.5 wt% molybdenum, 8 wt% or less tungsten, 2.1-4.1 wt% aluminum, 1.9 wt% or less titanium, 3.7 wt% or less niobium, 5 wt% or less iron, greater than 0 and 0.15 wt% carbon, 0.015 wt% or less boron, 7.1 wt% or less tantalum, 0.13 wt% or less silicon, 1 wt% or less manganese, and 0.06 wt% or less zirconium, with the remainder being nickel and impurities. The amounts of specific alloying elements must be carefully controlled according to the three compositional relationships disclosed herein.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This invention relates to a forgeable high-strength alloy for use at high temperatures. In particular, this invention relates to an alloy having sufficient mechanical strength, toughness / containment performance, and thermal stability for use in gas turbine cases and other gas turbine components. [Background technology]

[0002] To meet the demand for improved operational efficiency, gas turbine engine designers want to adopt higher operating temperatures. However, the ability to increase operating temperatures is often limited by material properties. One application where such limitations are problematic is the gas turbine case. The turbine case encloses and protects the turbine section of the engine. Since turbine cases are usually manufactured as forgings, good forgeability is required. In many cases, γ'-reinforced alloys are used for turbine cases due to their mechanical strength at high temperatures. These alloys require particularly high low-cycle fatigue (LCF) strength and high creep strength. High LCF strength is considered a good indicator of the alloy's resistance to thermal fatigue caused by the cycling of engine temperatures throughout the engine's lifespan. However, currently available forgeable γ'-reinforced alloys do not possess adequate LCF strength at temperatures above approximately 1400°F (760°C). High creep strength is an indicator of the alloy's ability to withstand prolonged loading at medium to high temperatures.

[0003] Forged γ'-reinforced alloys are often nickel-chromium-cobalt based, but other base systems are also used. These alloys typically contain one or more elements from aluminum, titanium, niobium, and tantalum, which contribute to the formation of the γ' phase, Ni3(X) (X = Ti, Al, Nb, Ta, etc.). Age-hardening heat treatment is used to precipitate the γ' phase within the alloy microstructure. This heat treatment is usually performed when the alloy is annealed. The presence of the γ' phase significantly strengthens the alloy over a wide temperature range. Other elements that may be added include molybdenum or tungsten for solid solution strengthening, carbon for carbide formation, and boron for improved high-temperature ductility. Certain amounts of iron are tolerated in these alloys and are usually present as a result of the manufacturing process.

[0004] Many gas turbine engine components (including turbine cases) require high mechanical strength at high temperatures. Depending on the operating temperature and nature of the load on the component, there are several types of strength that may be required. At high temperatures, these strengths include low-cycle fatigue strength, creep strength, and tensile strength. Another important property in turbine cases and other specific components is the toughness of the material. Toughness is an indicator of an alloy's ability to absorb energy before fracture. Both strength and ductility contribute to the toughness of an alloy. As will be further discussed later in this specification, alloys with high toughness are also said to have high containment capabilities.

[0005] Thermal stability is an indicator of how well an alloy's microstructure is maintained when exposed to heat. Many high-temperature alloys can form brittle intermetallic or carbide phases upon thermal exposure. The presence of these phases can significantly reduce the material's ductility at room temperature. This reduction in ductility can be effectively assessed using a standard room-temperature tensile test.

[0006] In addition to the material properties required for gas turbine engine alloys during operation, alloys must also possess properties necessary to enable the manufacture of complex components. These properties may include qualities such as hot forgeability, cold formability, and weldability. In the case of γ'-reinforced alloys, weldability often limits their applicability or necessitates high manufacturing costs. The weldability of γ'-reinforced alloys is closely related to their resistance to strain aging cracking, as will be discussed later in this specification.

[0007] Many forged gamma-reinforced alloys are available on the market today. Rene-41 or R-41 alloy (Patent Document 1) was developed by General Electric in the 1950s for use in turbine engines. This alloy has excellent creep strength but is limited by its poor thermal stability and resistance to strain aging cracking. A similar General Electric alloy, M-252 alloy (Patent Document 2), was also developed in the 1950s. M-252 alloy has excellent creep strength and resistance to strain aging cracking but is limited by its poor thermal stability, similar to the R-41 alloy. Another gamma-reinforced alloy developed by Pratt & Whitney, commercially known as WASPALOY alloy (likely not covered by US patents), is intended for use in turbine engines and is available as a sheet material. However, this alloy has insufficient LCF strength at 1500°F (816°C), insufficient creep strength, and only moderate resistance to strain aging cracking. The alloy commercially known as alloy 263 (Patent Document 3) was developed in the late 1950s and introduced by Rolls-Royce in 1960. This alloy possesses excellent thermal stability and resistance to strain aging cracking, but its LCF strength and creep strength at 1500°F (816°C) are very low. Haynes 282 alloy (Patent Document 4) was introduced in 2005. This alloy combines resistance to strain aging cracking, excellent thermal stability, and good creep strength. However, its LCF strength at 1500°F (816°C) is insufficient for certain advanced turbine case applications. Haynes 233 alloy (Patent Document 5) was introduced in 2016. This alloy combines excellent oxidation resistance, good creep strength, good thermal stability, and good workability. However, like Waspaloy and 282 alloys, the LCF strength of 233 alloy is not sufficient for advanced turbine casing applications at 1500°F (816°C).

[0008] As these examples suggest, established commercial alloys commonly considered for turbine casing applications do not possess sufficiently high mechanical strength (LCF and / or creep) at 1500°F (816°C) while combining high containment performance and good thermal stability to meet the increasing demands of next-generation gas turbine engines.

[0009] Patent document 6 discloses alloys suitable for use in the manufacture of gas turbine engines. However, the claims of this UK patent include compositions that, based on the relationships disclosed by the present invention, are not expected to have at least one of the three important properties of the turbine case described above. The range of aluminum content in the compositions disclosed in this patent publication does not overlap with the range of aluminum for the compositions of the present invention. Furthermore, this publication does not disclose a method for controlling the composition to obtain these desired properties. Finally, the alloy examples described in that publication do not fall within the preferred scope of the present invention.

[0010] Patent Document 7 discloses alloys for manufacturing engineering components capable of withstanding high stress at high temperatures, including blades or other components in an internal combustion gas turbine. However, the claims of this UK patent include compositions that, based on the relationships disclosed by the present invention, are not expected to possess at least one of the three important properties of the turbine case described above. For example, the commercially available alloys Waspaloy and Haynes 282, as well as experimental alloys 3 and 7, are among the compositions disclosed in this patent publication that do not necessarily possess all of the important properties. Furthermore, this publication does not disclose a method for controlling the composition to obtain these desired properties. Finally, the alloy examples described in this publication do not fall within the preferred scope of the present invention.

[0011] Patent Document 8 discloses a nickel-based alloy that is said to have excellent hot workability. This publication discloses that zirconium improves the hot workability of the alloy and should be present in an amount of 0.02% to 0.1% by weight. However, such levels of zirconium may cause hot cracking problems during welding of the alloy. This patent application also discloses that tungsten is necessary for high-temperature toughness, but only very small amounts of tungsten can be used, although it has been found that tungsten can exist as a partial substitute for molybdenum according to certain relationships. Furthermore, the composition range of the claims in Patent Document 8 includes alloys that are expected to lack one or more of the important properties of a gas turbine case based on the relationships disclosed by the present invention. Finally, the alloy examples described in that publication are not within the preferred scope of the present invention.

[0012] Patent Document 9 discloses a nickel-chromium-cobalt-molybdenum alloy containing 8-12 wt% molybdenum. However, this patent (issued in the 1990s) appears to claim the compositions of earlier patented alloys, such as R-41 alloy and M-252 alloy (mentioned above in this publication). This reference does not recognize that molybdenum levels exceeding 8.5 wt% are detrimental and may lead to decreased thermal stability, reduced LCF strength, and / or reduced containment performance of this type of alloy. The composition range claimed in this Japanese reference includes compositions that are not expected to possess all of the important properties mentioned above. The HAYNES 282 alloy and experimental alloys 2, 4, and 5 in Table 1 below contain small amounts of iron (levels considered typical for iron impurities in this type of commercially produced alloy) and do not possess all the important properties. Removing the iron would produce alloys within the composition range of the alloys disclosed in Patent Document 9. However, removing the iron is not expected to significantly alter the important properties of these alloys. Furthermore, this publication does not disclose a method for controlling the composition to obtain these desired properties. Finally, the alloy examples described in the publication are not within the preferred scope of the present invention.

[0013] Therefore, an alloy is needed that combines excellent mechanical strength, high containment performance, and good thermal stability at an intermediate temperature of 1500°F (816°C). Furthermore, for certain applications, it would be beneficial if the alloy possessed good weldability, particularly good resistance to strain aging cracking. [Prior art documents] [Patent Documents]

[0014] [Patent Document 1] U.S. Patent No. 2,945,758 [Patent Document 2] U.S. Patent No. 2,747,993 [Patent Document 3] U.S. Patent No. 3,222,165 [Patent Document 4] U.S. Patent No. 8,066,938 [Patent Document 5] U.S. Patent No. 10,577,680 [Patent Document 6] UK Patent Application Publication No. 1029609 [Patent Document 7] UK Patent Application Publication No. 2712498 [Patent Document 8] Japanese Patent Application Publication No. 01-129942 [Patent Document 9] Japanese Patent Application Publication No. 06-172900 [Overview of the Initiative] [Problems that the invention aims to solve]

[0015] The main objective of the present invention is to provide a new forgeable, age-hardenable nickel-chromium-cobalt-based alloy suitable for use in high-temperature gas turbine cases and other gas turbine components, having higher low-cycle fatigue strength, good thermal stability, and an acceptable containment coefficient. [Means for solving the problem]

[0016] It has been found that this object can be achieved by an alloy comprising chromium and cobalt within a certain range, solid solution strengthening agents (molybdenum and tungsten) within a certain range, and γ' formers (aluminum, titanium, niobium, and tantalum) within a certain range, with the balance being nickel and various trace elements and impurities.

[0017] Specifically, the required ranges are 16 to 20 wt% chromium, 8 to 13 wt% cobalt, 4 to 8.5 wt% molybdenum, 8 wt% or less tungsten, 2.1 to 4.1 wt% aluminum, 1.9 wt% or less titanium, 3.7 wt% or less niobium, 5 wt% or less iron, more than 0 and 0.15 wt% or less carbon, 0.015 wt% or less boron, 7.1 wt% or less tantalum, 0.13 wt% or less silicon, 1.0 wt% or less manganese, 0.06 wt% or less zirconium, with the balance being nickel and impurities. In addition, specific compositional relationships are required that impose limits on the total and relative amounts of both the γ' formers and the solid solution strengthening agents. As a result, there are certain experimental alloys that meet all the individual element requirements but are not considered part of the present invention because they do not satisfy one of the aforementioned compositional relationships. Such alloys fail to meet one or more critical property targets. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] [Figure 1] It is a graph of the low cycle fatigue life at 1500°F (816°C) in a fully reversed strain-controlled test with a total strain range of 0.6% for several forged age-hardenable nickel-chromium-cobalt base alloys. [Figure 2] It is a graph of the containment factor at 1400°F (760°C) for several forged age-hardenable nickel-chromium-cobalt base alloys. [Figure 3] It is a graph of the thermal stability of several forged age-hardenable nickel-chromium-cobalt base alloys, as indicated by ductility in a standard room temperature tensile test after 1000 hours of thermal exposure at 1400°F (760°C). [Figure 4]This graph shows the creep strength of several forged age-hardenable nickel-chromium-cobalt alloys, measured by 1% creep life in a creep test applied at 1500°F (816°C) with a stress of 30 ksi (207 MPa). [Figure 5] This graph shows the weldability of several forging age-hardenable nickel-chromium-cobalt alloys, measured by CHRT ductility in a heating rate-controlled tensile test at 1450°F (788°C). [Figure 6] This figure illustrates the R, G, and T factors and the limits of these factors as defined by the compositional relationships discovered in this invention. The figure also shows the compositions of numerous experimental, commercial, and predictive alloys described herein. [Modes for carrying out the invention]

[0019] Ni-Cr-Co-(Mo,W)-(Al,Ti,Nb,Ta) alloys are provided, comprising 16-20 wt% chromium, 8-13 wt% cobalt, 4-8.5 wt% molybdenum, 8 wt% or less tungsten, 2.1-4.1 wt% aluminum, 1.9 wt% or less titanium, 3.7 wt% or less niobium, 7.1 wt% or less tantalum, additives of specific trace elements along with typical impurities, and the remainder nickel, and possessing properties useful for various gas turbine engine components such as turbine cases, according to the specific composition relationships defined and disclosed herein. Based on an understanding of the turbine case requirements for future gas turbine engines, alloys with the following properties would be highly desirable: 1) high containment performance at intermediate operating temperatures such as 1200-1500°F (649-816°C), 2) good thermal stability at intermediate operating temperatures, and 3) excellent mechanical strength at intermediate operating temperatures. For many applications, moderate to high weldability would also be desirable. Currently, no commercially available alloy possessing all of these qualities is available on the market. One of the more commonly used turbine case alloys is Waspaloy. While Waspaloy offers high containment performance and good thermal stability, its mechanical strength (both LCF and creep) at 1500°F (816°C) is considerably low, limiting the upper limit of the alloy's operating temperature. As will be shown below, the alloy of the present invention provides significantly improved mechanical strength compared to Waspaloy at 1500°F (816°C).

[0020] Forty-one experimental alloys having the compositions shown in Table 1 were tested. All experimental alloys were nickel-based, with chromium content ranging from 16.80 to 19.65 wt%, cobalt content from 9.28 to 10.81 wt%, molybdenum content from 3.73 to 8.59 wt%, aluminum content from 1.35 to 3.90 wt%, and iron content from 0.87 to 9.93 wt. Some alloys contained titanium, ranging from less than 0.01 wt% to 2.96 wt%. Some alloys contained niobium, ranging from less than 0.02 wt% to 5.33 wt%. Some alloys contained tantalum, ranging from less than 0.01 wt% to 2.01 wt%. Some alloys contained tungsten, ranging from less than 0.01 wt% to 8.43 wt%. Silicon was present as an impurity in some alloys and intentionally added in others, ranging from 0.01 to 0.17 wt%. Manganese was intentionally added to some alloys, ranging from less than 0.01 wt% to 0.24 wt% or less. Small amounts of carbon and boron were also added to the experimental alloys, present at a maximum of 0.081 wt% and 0.006 wt% or less, respectively. Zirconium was not intentionally added to any of the alloys. As a result, the measured zirconium levels in all experimental alloys were less than 0.02 wt% (for brevity, these results are not included in Table 1).

[0021] All alloy tests were performed on sheet material with thicknesses of 0.065–0.125 inches (1.6–3.2 mm). The experimental alloys were vacuum induction melted and then electroslag remelted at a heat intensity of 30–50 pounds (13.6–27.2 kg). The ingots were hot forged on an open die press with little difficulty to obtain slabs. The slabs were then hot-rolled to intermediate gauges. Sheets were annealed, water-cooled, and cold-rolled to produce sheets of the desired gauge. Intermediate annealing of cold-rolled sheets was necessary during the production of 0.065-inch sheets (1.6 mm). Cold-rolled sheets were annealed as needed to produce a fully recrystallized equiaxed grain structure with an ASTM grain size typically between 4–5. Sheet samples were water-cooled or rapidly air-cooled after annealing. For specific tests, annealed samples were subjected to age-hardening heat treatments appropriate for the specific alloy prior to testing. Details of the age-curing heat treatment will be described later in this specification.

[0022] [Table 1]

[0023] Up to five different tests were performed on the experimental alloys to evaluate critical properties (containment performance, thermal stability, and mechanical strength) and secondary properties (weldability) to establish their suitability for the intended application. The results of these tests are described in the following section. In addition, to provide comparative information, critical and secondary properties were tested on three commercial alloys (282 alloy, Waspaloy alloy, and 233 alloy). Table 2 shows the measured compositions of the commercial alloy samples tested. Note that the chemical properties of the commercial alloy samples are taken from actual samples of the commercial alloys and are considered representative, but may not correspond to the same temperatures tested in this program.

[0024] [Table 2]

[0025] The first important property of the alloy of the present invention is its containment performance. In certain components of gas turbine engines, particularly aircraft engines, it is desirable to have high containment performance (or toughness) at high operating temperatures. These components, which may include certain cases and rings, may require high containment properties in the event of engine failure. Such containment properties depend largely on the ductility of the alloy at operating temperatures, in addition to high strength. While containment properties are best measured by expensive special high-strain-rate tests, a reasonable measure of containment properties can be obtained by considering the ductility (elongation) values ​​obtained from standard tensile tests at the relevant temperatures. The yield strength (YS) and ultimate tensile strength (UTS) values ​​from the tensile tests are also considered. The containment coefficient CF can be calculated from the results of the tensile tests and is defined as CF = 1 / 2 × (YS + UTS) × (elongation). (Note: In conventional units, the containment coefficient is calculated using YS and UTS in ksi units, and elongation is expressed in %, therefore the unit of the containment coefficient is lbf-in / in) 3 ×10 -1 This is the result. For the sake of brevity, in the remainder of this specification, this unit descriptor is not added to the containment coefficient value, and unless otherwise specified, lbf-in / in 3 ×10 -1 It is assumed that CF is in meters (MJ / m 3 To convert to ), multiply by 0.06895. For applications requiring containment properties, a high CF value is desirable. When comparing the CF values ​​of various alloys, it is important to use similar product shapes and sizes and identical sample shapes, as tensile properties can be highly dependent on the shape and size of the product, as well as the shape of the test sample. Given that the underlying tensile properties are usually temperature-dependent, the containment coefficient is temperature-dependent. For applications where containment properties are important, the operating temperature may fall within an "intermediate range" of approximately 1200°F to 1500°F (649 to 816°C). For this reason, a temperature of 1400°F (760°C) was selected for the test.

[0026] Forty-one experimental alloys and three commercially available alloys (HAYNES 282 alloy, HAYNES 233 alloy, and Waspaloy alloy) were subjected to tensile tests at 1400°F (760°C) to measure their strength and ductility. The results, along with the calculated containment factors, are shown in Table 3. Note that all samples were tested in the as-heat-treated state as defined in Table 4.

[0027] [Table 3]

[0028] [Table 4]

[0029] The containment coefficients at 1400°F (760°C) for three commercially available alloys are 2305, 2924, and 3634 (159, 202, and 251 MJ / m³) for 282 alloy, 233 alloy, and Waspaloy alloy, respectively. 3 It was found that ). For turbine case alloys, it is desirable to have a containment coefficient of 1400°F (760°C) equivalent to or higher than that of alloy 282, so this was used as the target of the present invention. Of the 41 experimental alloys, 33 had a containment coefficient of 1400°F (760°C) higher than that of alloy 282, i.e., CF ≥ 2305 (159 MJ / m). 3 It was found that it has a containment coefficient of 2305 (159 MJ / m³) at 1400°F (760°C). 3 The eight alloys with a coefficient of less than ) were experimental alloys 3, 4, 7, 12, 13, 14, 18, and 19. Therefore, these eight alloys are considered to be outside the scope of the present invention.

[0030] Figure 2 is a graph of the containment coefficients for alloy 282, Waspaloy alloy, and 233 alloy, as well as experimental alloys 8, 9, 17, 22, 23, and 30 in Table 1. The graph shows that all of these experimental alloys have a higher containment coefficient than alloy 282. Experimental alloys 8, 9, 17, 22, 23, and 30 are not all but some of the experimental alloys of the present invention disclosed herein and can be considered representative of the alloys of the present invention.

[0031] The second important property of the alloy of the present invention is thermal stability. For applications such as turbine cases, where high temperatures and prolonged use are required, the thermal stability of the constituent materials is extremely important. The thermal stability of experimental and commercially available alloys was tested by exposure to heat at 1400°F (760°C) for 1000 hours. Note that for all alloys, the thermal exposure was applied to age-hardened samples. Next, the room temperature (RT) tensile properties of the heat-exposed samples were measured. The residual RT yield strength and residual RT tensile elongation (ductility) after thermal exposure are measures of the alloy's thermal stability. These measurement results are shown in Table 5. The exposure temperature of 1400°F (760°C) was chosen because many nickel-based alloys exhibit the lowest thermal stability around this temperature range, making it suitable for turbine case applications. To obtain acceptable thermal stability for the target applications, the residual RT yield strength must be equal to or greater than that of the 282 alloy, i.e., 104.1 ksi (718 MPa) or higher, and the residual RT ductility must be at least 10%. Table 5 shows the results for 41 experimental alloys and 3 commercially available alloys. Of the 41 experimental alloys, 39 were found to have a holding yield strength exceeding 104.1 ksi (718 MPa). Only experimental alloys 5 and 18 did not have a holding yield strength sufficient to be considered part of the present invention. Both alloy 233 and Waspaloy alloy were found to have a holding yield strength exceeding 104.1 ksi (718 MPa). Considering holding ductility, 36 of the 41 experimental alloys were found to have a value exceeding 10%. The five experimental alloys with holding ductility of less than 10% were experimental alloys 11, 14, 15, 32, and 33, and these alloys are not considered part of the present invention. All three commercially available alloys had holding ductility exceeding 20%.

[0032] Figure 3 shows graphs of thermal stability, measured by room-temperature ductility, for alloys 282, Waspaloy, and 233, as well as experimental alloys 8, 9, 17, 22, 23, and 30 in Table 1. All of these alloys maintain room-temperature ductility above the target of 10%, and in fact all exceed 15%, with some exceeding 20%.

[0033] [Table 5]

[0034] A third important property of the alloys of the present invention is high mechanical strength, particularly high LCF strength and / or creep strength. A common test for evaluating LCF strength is a strain-controlled test in which a sample is periodically strained to a constant strain level until it breaks, and the number of cycles until breakage (also called LCF lifetime) is considered a measure of LCF strength. In this specification, LCF test results at 1500°F (816°C) are provided for most experimental alloys and all three commercially available alloys. The tests were performed under strain-controlled bipolar conditions (R=-1) with a triangular waveform and a frequency of 20 cycles / min (0.33 Hz). Most tests were performed at a total strain range (TSR) of 0.6%. The results are shown in Table 6. Note that not all experimental alloys were LCF tested due to the labor and cost involved in such tests.

[0035] [Table 6]

[0036] As shown in Table 6, the LCF life of the three commercially available alloys under these test conditions was 6446, 6344, and 9507 cycles for alloy 282, Waspaloy alloy, and 233 alloy, respectively. Since the design of the new gas turbine engine requires a significantly improved LCF strength compared to currently available alloys, a minimum of 10,000 cycles, representing an improvement of 57% or more over Waspaloy, was selected as the desirable target for the alloys of the present invention. Considering this 10,000-cycle target, Table 6 shows that of the 28 experimental alloys tested, only 18 met the target, while 10 failed to do so. The alloys that met the target were experimental alloys 3, 7, 8-10, 16, 17, 20, 22-25, 27, and 30-34. The alloys that failed to meet the target were experimental alloys 2, 12-14, 18, 19, 21, 26, 28, and 29. The 16 alloys that were not tested were experimental alloys 1, 4-6, 11, 15, 31-33, and 35-41.

[0037] Figure 1 shows graphs of the low-cycle fatigue life of alloys 282, Waspaloy, and 233, as well as experimental alloys 8, 9, 17, 22, 23, and 30 in Table 1, at 1500°F (816°C) and TSR=0.6%. While the low-cycle fatigue life of commercially available alloys is less than 10,000 cycles, all experimental alloys have low-cycle fatigue lives exceeding 10,000 cycles. The low-cycle fatigue lives of experimental alloys 9, 17, and 30 exceed 19,500 cycles.

[0038] In addition to the LCF tests described above, LCF tests were also performed on eight experimental alloys at a low TSR value of 0.5%. These tests are time-consuming and costly, but in a sense, they allow for a more accurate prediction of the long-term fatigue strength of the alloys. Temperature and other test conditions were all kept the same as in the TSR=0.6% tests. The results are shown in Table 7 below.

[0039] [Table 7]

[0040] As shown in Table 7, the LCF lives of the three commercial alloys under these test conditions were 13,130, 31,520, and 39,957 cycles for alloy 282, Waspaloy, and alloy 233, respectively. At this TSR level, a target LCF life of 40,000 cycles was selected, representing a 27% increase over Waspaloy. Of the eight experimental alloys tested under these conditions, three (alloys 1, 5, and 6) failed to meet the target, while five (alloys 7, 8, 23, 30, and 36) did. None of the three commercial alloys tested met the target LCF life.

[0041] The creep strength of 15 experimental alloys and Waspaloy was measured in creep tests at 1500°F (816°C) with a stress of 30 ksi (207 MPa). The 1% creep life (i.e., the time to reach 1% elongation) was recorded for each test, and the results are shown in Table 8. The 1% creep life of Waspaloy was 49.5 hours. We selected a target of 70 hours for the 1% creep life of the alloys of the present invention, which represents a 41% improvement over Waspaloy. All 15 experimental alloys (3, 9, 17, 20, 22-23, 30-31, 35-41) subjected to creep tests at 1500°F (816°C) and 30 ksi (207 MPa) were found to meet this target.

[0042] [Table 8]

[0043] Figure 4 is a graph of the 1% creep life of Waspaloy alloy and experimental alloys 9, 17, 22, 23, 30, 31, 37, and 41 in Table 1, measured during creep tests with a stress of 30 ksi (207 MPa) at 1500°F (816°C). The graph shows that the 1% creep lives of all these experimental alloys are longer than those of Waspaloy alloy, and that the lives of alloys 9, 17, 23, 30, 31, and 41 are considerably longer. Experimental alloys 9, 17, 22, 23, 30, 31, 37, and 41 are not all, but some, of the experimental alloys of the present invention disclosed herein and can be considered representative of the alloys of the present invention.

[0044] When all three important properties (containment performance, thermal stability, and mechanical strength) were considered together, 21 experimental alloys were found to meet all three important property targets and be considered alloys of the present invention. These were experimental alloys 8-10, 16, 17, 20, 22-25, 27, 30, 31, and 34-41, listed in Table 9. Note that not all mechanical tests were performed on each alloy; therefore, alloys that met the targets in one or more of the three tests (i.e., two LCF test conditions and a creep test) were counted as having satisfactory mechanical strength. Table 9 also shows that all 20 experimental alloys and 3 commercially available alloys failed to meet one or more of the important property targets and are therefore not part of the present invention.

[0045] [Table 9]

[0046] It was found that the main alloying elements of acceptable alloys are within a specific compositional range as shown in Table 10, and that acceptable alloys follow three additional compositional relationships disclosed herein. (Note: The range of trace alloying elements is discussed later in this specification.) The first two compositional relationships relate to γ'-forming elements (aluminum, titanium, niobium, and tantalum). As suggested, these elements form a strengthened γ' phase (Ni3X, X=Al, Ti, Nb, and / or Ta) when subjected to age-hardening heat treatment as detailed in Table 4. Since these elements can have a significant impact on all three important properties, it is important to control the amounts of these elements in the alloys of the present invention. It was found that the γ'-forming elements need to be controlled using the following equation (units of elemental composition are weight %).

number

number

[0047] It should be noted that, by definition, the upper limit of the R factor is 1. It is important to state that the important role that the R and G factors play in determining which alloy composition provides a unique combination of the three key properties of the alloy of this invention was an unexpected and surprising discovery.

[0048] The third compositional relationship concerns the solid solution strengthening elements molybdenum and tungsten. Too much of these elements may result in the presence of undesirable phases, which can affect thermal stability and many alloy properties, including but not limited to LCF. Conversely, too little of the solid solution strengthening elements is undesirable, as high mechanical strength is important for the alloys of the present invention. This requires upper and lower limits for the sum of these two elements, as shown by the following formula, in addition to the individual tolerance limits for these elements (listed in Table 10) (elemental composition is given in weight %).

number

[0049] [Table 10]

[0050] In Table 10, the upper limits for titanium, niobium, and tantalum are 1.9 wt%, 3.7 wt%, and 7.1 wt%, respectively. These values ​​were calculated from Equations 1 and 2, and the range of 2.1–4.1 wt% for aluminum. While the range for aluminum is well supported by the example alloy, the calculated upper limits for titanium, niobium, and tantalum are significantly higher than the satisfactory upper limits for the example alloy, which are 0.50 wt%, 2.20 wt%, and 2.01 wt%, respectively. Considering this fact and the general tolerances for these elements in actual melting, more conservative upper limits for these elements would be 1 wt%, 2.7 wt%, and 2.5 wt% for titanium, niobium, and tantalum, respectively.

[0051] [Table 11]

[0052] Considering the compositional requirements for the alloys of the present invention (Table 10 and Formulas 1, 2, and 3), it was found that 21 experimental alloys (experimental alloys 8-10, 16-17, 20, 22-25, 27, 30-31, and 34-41) that met all three important property objectives also met all compositional requirements. Conversely, 20 experimental alloys that failed to meet one or more important property objectives, and all three commercially available alloys (experimental alloys 1-7, 11-15, 18-19, 21, 26, 28-29, 32, and 33, and commercially available alloys 282, Waspaloy, and 233) did not meet one or more compositional requirements.

[0053] Certain gas turbine components may require additional secondary property targets. For example, if the component requires welding, it would be desirable to have good weldability. In the case of γ'-phase strengthened alloys, weldability can be adversely affected by an effect known as strain aging cracking. This phenomenon usually occurs when the welded component is exposed to high temperatures for the first time after welding. Often, this occurs during the post-weld annealing process, which is performed on most welded γ' alloys. Cracking occurs as a result of the formation of the γ' phase during heating to the annealing temperature. Cracking often occurs due to the formation of the strengthening γ' phase combined with the low ductility that many of these alloys have at intermediate temperatures, as well as the mechanical constraints usually imposed by the welding process. As the material thickness increases, the mechanical constraints increase, so the problem of strain aging cracking may limit the usable alloys to certain thicknesses.

[0054] The resistance of experimental and commercially available alloys to strain aging cracking was measured using a modified CHRT test described by Metzler in the Welding Journal Supplement (October 2008, pp. 249-256). This test was developed to determine the relative resistance of alloys to strain aging cracking. It is a modification of the test described in Rowe's paper published in U.S. Patent No. 8,066,938 and the Welding Journal Supplement (February 2006, pp. 27-34). The CHRT test was originally developed in the late 1960s as a method to measure the susceptibility of Rene41 (R-41) alloys to strain aging cracking under various thermal conditions (Fawley, RW, Prager, M., Carlton, JB, Sines, G. 1970, WRC Bulletin No. 150, Welding Research Council, NY). In the CHRT test, a solution-treated tensile specimen is heated at a controlled rate to a test temperature within the γ' precipitation temperature range and then pulled until fracture. CHRT elongation indicates the alloy's resistance to strain aging cracking / weldability. During the CHRT test, the sample undergoes γ' precipitation, simulating the effects of welding and subsequent cooling. Therefore, the CHRT test reliably predicts the behavior of the material in the as-welded state. The CHRT test was designed to be a relatively easy test to perform, but the results are in good agreement with reported strain aging cracking studies (see Rowe, e.g., Welding Journal Appendix, February 2006, pp. 27–34). Key variables found to affect the performance of the CHRT test include composition and grain size. In the modified CHRT test, the width of the gauge section is variable, and the test is performed in a dynamic thermomechanical simulator rather than a screw-driven tensile unit. While the results of the two different forms of testing are expected to be qualitatively similar, the absolute quantitative results differ.

[0055] Modified CHRT tests were performed on 41 experimental alloys using solution-treated and surface-ground samples. The tests were conducted at 1450°F (788°C), and the reported CHRT ductility values ​​were measured as elongation over 1.5 inches (38 mm). The results are shown in Table 12. Similar tests were performed on three commercially available alloys (282 alloy, Waspaloy alloy, and 233 alloy) under mill annealing conditions, and the results are also shown in Table 12. The CHRT elongation values ​​for 282 alloy and 233 alloy were 13.0% and 12.5%, respectively. These relatively high values ​​indicate that both alloys have excellent resistance to strain aging cracking. This is consistent with the field experience reported for these two alloys. However, the reputation of Waspaloy alloy is quite different. While moderately weldable, Waspaloy may be prone to strain aging cracking under certain conditions. CHRT tests were performed on Waspaloy under two conditions: mill annealing and mill annealing + surface grinding. The CHRT elongation values ​​under these two conditions were 6.8% and 6.0%, respectively. In order to ensure a certain degree of weldability in the alloy of the present invention, it is preferable that the CHRT elongation is greater than that of Waspaloy in the surface-ground state. That is, it is preferable that it exceeds 6.0%. More preferably, it is preferable that it has a CHRT ductility greater than that of Waspaloy in the as-mill annealed state, i.e., greater than 6.8%.

[0056] Figure 5 shows graphs of CHRT ductility for alloy 282, Waspaloy alloy, and 233 alloy, as well as experimental alloys 8, 9, 17, 22, 23, and 30 in Table 1. Three of the experimental alloys (22, 23, and 30) have higher CHRT ductility than mill-annealed Waspaloy alloy (6.8%). The CHRT ductility of experimental alloy 17 was close to 6.7%. The CHRT ductility of experimental alloys 8 and 9 is clearly below 6.8%. Of these two alloys, experimental alloy 9 has a CHRT ductility of 6.0%, which is comparable to the ductility of Waspaloy in a surface-ground state, while experimental alloy 8 has a ductility of less than 6.0%.

[0057] [Table 12]

[0058] It was found that CHRT elongation exceeding 6.0% could be achieved by further restricting the amount of γ'-forming elements. Specifically, it was found that Al should be restricted to 3.1-4.1 wt%, Ti to 0.4 wt% or less, Nb to 1.3 wt% or less, and Ta to 2.5 wt% or less. In addition, the R factor needs to be further restricted as follows (elemental composition is shown in wt%).

number

[0059] [Table 13]

[0060] Adding compositional constraints can further improve weldability and other properties. Specifically, we discovered alloy compositions in which the CHRT elongation is greater than that of Waspaloy alloy (surface-ground) and all three key properties (containment performance, thermal stability, and mechanical strength) are significantly improved simultaneously. These improved compositions are referred to herein as “more preferred” compositions and are summarized in Table 14 for the major alloying elements. More preferred compositions involve tightening the elemental ranges of several elements, such as adding the required minimum values ​​for tungsten and iron, both of which have been found to be beneficial in maximizing the alloy properties. In addition, the R and G factors need to be further restricted as follows (elemental composition is given in weight %).

number

[0061] [Table 14]

[0062] The alloy of the present invention is a nickel-based alloy, as is the case with most so-called superalloys, a type of alloy known for providing high strength, environmental resistance, and other properties under the harsh conditions common to gas turbine engines. The advantages of the main alloying elements in the alloy of the present invention are briefly described below, but should not be considered exhaustive. Chromium provides useful oxidation resistance, high-temperature corrosion resistance, and some degree of strengthening. It is present in relatively large amounts in many forged superalloys, and 16-20 wt% of chromium in the alloy of the present invention is fairly typical. The specification range for chromium in nickel-based superalloys can be quite large. For example, one specification for chromium in Waspaloy is in the range of 3 wt% (or ±1.5 wt%), while one specification for 282 alloy is in the range of 2 wt% (or ±1 wt%). Cobalt provides some strengthening and adjusts the γ' sorbus temperature. However, because cobalt is chemically similar, it can be substituted for nickel in relatively large amounts without significantly affecting its properties. In the alloy of the present invention, cobalt can be in the range of 8-13 wt% (or ±2.5 wt%), more preferably 9-11 wt% (or 10 ± 1 wt%). These ranges are equivalent to industry specifications. Similar to chromium, the specification range for cobalt in nickel-based superalloys can be quite large. For example, one specification for cobalt in Waspaloy is in the range of 3 wt% (or ±1.5 wt%), while one specification for 282 alloy is in the range of 2 wt% (or ±1 wt%). Iron may be intentionally added or present as a typical impurity in nickel-based alloys. We have found that intentionally adding at least 1.5 wt% iron provides a beneficial effect on workability. However, to meet all important property targets, the iron content must be kept below 5 wt%. More preferably, iron should be kept below 4 wt%. Aluminum, titanium, niobium, and tantalum contribute significant strength by forming γ' phases during heat treatment. Regarding the relative amounts of these four γ'-forming elements, it has been found that higher levels of aluminum are beneficial, and it is preferable to keep titanium below 0.4 wt%. Further benefits should be obtained at even lower titanium levels of 0.1 wt% or less.Aluminum must be present in an amount of at least 2.1% by weight, preferably at least 3.1% by weight. Molybdenum and tungsten are effective solid solution strengthening elements. At least 4% by weight of molybdenum is required. Tungsten is not essential in this invention, but since it has been shown to provide beneficial effects, a more preferable composition would have at least 1% by weight. A level of tungsten of at least 2% by weight is even better. However, to avoid thermal stability issues, tungsten must be kept below 8% by weight. More preferably, tungsten should be limited to below 6% by weight.

[0063] As mentioned above, providing the necessary balance of alloy properties requires careful control of the amounts of both γ'-forming elements and solid solution strengthening elements (using the compositional relationships I have discovered and described herein). Because these compositional relationships must be satisfied, certain alloys may satisfy all the individual elemental requirements but are still outside the scope of the invention. For example, alloys 7, 28, 29, and 32 are within the broad elemental range of the invention, but their G factors are too high (>2.40) and they do not meet one of the key property objectives, as listed in Table 9. Similarly, an alloy may satisfy the requirements of a compositional relationship but fall outside one or more individual elemental ranges. For example, alloys 3, 4, and 21 satisfy all the requirements of a compositional relationship, but alloys 3 and 4 have too much molybdenum, and alloy 21 has too much iron. In addition to the broad claims described herein, similar results may occur with respect to preferred or more preferred claims.

[0064] Figure 6 was created to graphically illustrate the limits of the R, G, and T factors and the compositional relationships given by Equations 1, 2, 4, 5, and 6. This figure shows many of the compositions of the experimental, commercial, and predicted alloys described above. All alloys of the present invention (broad claims) are contained within a larger parallelogram inscribed by four lines: G=1.8, G=2.4, R=0.7, and R=1. Preferred alloys of the present invention are located within a medium-sized parallelogram to the right of the line R=0.9. More preferred alloys are all located within the smallest parallelogram to the right of the line R=0.95, between the lines G=2.4 and G=1.9. Experimental and commercial alloys outside the largest parallelogram in Figure 6 are not alloys of the present invention and do not meet one or more important property objectives. For clarity, experimental and commercial alloys containing one or more individual elements that are within a given parallelogram but outside the scope of the relevant claims have been omitted from Figure 6. Regarding the selected predicted alloys shown in Figure 6, those inside the largest parallelogram are expected to satisfy the important property objectives of the present invention, while those outside (particularly predicted alloys XX and YY) are not expected to satisfy all major property objectives. The compositions of the predicted alloys are shown in Table 18.

[0065] In addition to the carbon required for these alloys, other trace elements may be added, including boron, manganese, silicon, zirconium, magnesium, calcium, hafnium, and one or more rare earth elements (including, but not limited to, yttrium, lanthanum, and cerium). The acceptable ranges for trace elements are described below and summarized in Table 15. These acceptable ranges apply whether the trace elements are intentionally added or present only as impurities.

[0066] Carbon is intentionally added to the alloys of the present invention to provide interstitial strengthening, carbide strengthening, and improved grain size control. Carbon is limited to a maximum of 0.15 wt% in the alloys of the present invention, a maximum of 0.1 wt% in preferred compositions, and a maximum of 0.08 wt% in more preferred compositions. Boron may be added in small but effective trace amounts up to 0.015 wt% to obtain certain advantages known in the art. In preferred and more preferred compositions, boron is limited to a maximum of 0.008 wt% to ensure good weldability. Boron is present in all experimental alloys and is considered to have primarily beneficial effects, although this is an optional addition. These alloys may contain small amounts of manganese up to about 1 wt%, and in some cases, trace amounts of magnesium, calcium, and rare earth elements (such as yttrium, cerium, and lanthanum) up to about 0.05 wt%, each, to allow for the removal of oxygen and sulfur during the melting process. Similarly, silicon may be added to the alloys to control oxygen and sulfur, but silicon has been found to adversely affect the LCF strength of these alloys. Therefore, silicon should be limited to 0.13 wt%, preferably 0.12 wt%, and even more preferably less than 0.1 wt%. Zirconium may be present in these alloys as an impurity or intentional addition (e.g., to improve creep life), but to maintain proper workability, it should be kept below 0.06 wt% in these alloys. To ensure sufficient resistance to hot cracking during welding, it is preferable to limit the zirconium content to 0.03 wt% or less, more preferably 0.02 wt% or less. Hafnium may be present in these alloys as an impurity or intentional addition, but it should be kept below 0.5 wt%.

[0067] [Table 15]

[0068] Table 16 provides an overview of tolerance to specific impurities. Additional impurities not listed may exist, but are acceptable if they do not degrade important properties below defined limits.

[0069] [Table 16]

[0070] For convenience, experimental and commercially available alloys are listed in Table 17, indicating which alloys satisfy a broad composition range, a preferred range, and a more preferred range.

[0071] [Table 17]

[0072] Based on the information presented herein, all predicted alloy compositions shown in Table 18 are also expected to possess the desired properties of the present invention (with the exception of alloys XX, YY, and ZZ, which are outside the broad claims of the present invention).

[0073] [Table 18]

[0074] It is beneficial to further consider three commercially available alloys: 282 alloy, Waspaloy alloy, and 233 alloy. Regarding the key properties of the turbine case identified here, all three alloys were found to possess acceptable containment performance and thermal stability. All three alloys also possessed sufficient weldability / strain-resistant age cracking (although Waspaloy had limitations). However, the mechanical strength of the three alloys at 1500°F (816°C) was unacceptable. Looking at the compositions of these three alloys reveals why this occurred. All three commercially available alloys have compositions other than those of the present invention. The 282 alloy composition does not meet the composition requirements of the present invention, mainly due to the γ'-forming elements. This alloy does not satisfy formula (1), and both aluminum and titanium are outside the broad range. Also, the levels of molybdenum, tungsten, and iron are outside the more preferable range. Similarly, the Waspaloy alloy composition does not satisfy formula (1), and again, both aluminum and titanium are outside the broad range. Furthermore, the levels of cobalt, tungsten, and iron are outside the more preferred range. Alloy 233 is close to the alloy of the present invention. However, the cobalt level is far above the broad range of the alloy of the present invention. Also, the level of titanium is outside the preferred range, while the levels of tungsten, iron, carbon, silicon, and zirconium are outside the more preferred range.

[0075] In addition to the three important properties mentioned above and the secondary properties of good weldability / strain-resistant age cracking, other desirable properties of the alloy of the present invention may include high room temperature tensile strength and ductility in the age-hardened state, good resistance to hot cracking during welding, good oxidation / high-temperature corrosion resistance, good hot forgeability, and good cold formability.

[0076] Even if the tested samples were limited to forged sheet materials, alloys having compositions within the ranges of Tables 10, 13, and / or 14 should exhibit similarly improved properties in other forging forms (e.g., plates, bars, tubes, pipes, forgings, and wires) and in casting, spray molding, additive manufacturing (including powders for producing these), or powder metallurgy forms, i.e., powders, compacts, and sintered compacts. Therefore, the present invention encompasses all forms of alloy composition. It should be noted that the target values ​​of key properties defined herein are specific to the product form, processing parameters, and microstructure (e.g., grain size) used to obtain supporting data. These variables were kept as constant as possible between experimental alloys to facilitate fair comparisons. If these variables are changed (e.g., if the product form is a hot-rolled ring instead of a sheet, or if the material is annealed to produce a different grain size), the absolute values ​​of the key property values ​​may change. However, the relative improvements brought about by the alloys of the present invention are still expected to be effective.

[0077] The alloy of the present invention uniquely combines three key properties: high containment performance, good thermal stability, and excellent mechanical strength, which can be further controlled to provide superior resistance to strain aging cracking. These properties make the alloy of the present invention useful for gas turbine engine components, particularly for the turbine cases of these engines. Such components and engines containing them can operate at high temperatures without failure and should have a longer service life than currently available components and engines. It is recognized that this unique combination of properties may also be attractive for other high-temperature applications not described herein.

[0078] While specific preferred embodiments of the alloy have been disclosed, it should be clearly understood that the present invention is not limited thereto and can be embodied in various ways within the scope of the claims.

Claims

1. 16-20% by weight of chromium, 8-13% by weight of cobalt, 4-8.5% by weight of molybdenum, Tungsten of 8% by weight or less, Iron at a weight of 5% or less, 2.1 to 4.1% by weight of aluminum, 1. Titanium of 1.9% by weight or less, 7.1% by weight or less of tantalum, 3. Niobium at a weight of 3.7% or less, Carbon exceeding 0% by weight and 0.15% by weight or less, Boron at a concentration of 0.015% by weight or less, Silicon of 0.13% by weight or less, Manganese of 1% by weight or less, 0.06% by weight or less of zirconium, Magnesium at a concentration of 0.05% by weight or less, Calcium of 0.05% by weight or less, Yttrium of 0.05% by weight or less, Lanterns with a weight of 0.05% or less, 0.05% by weight or less of cerium, Hafnium at a concentration of 0.5% by weight or less It contains nickel and impurities, with the remainder being nickel and impurities. It has a composition consisting of, The following compositional relationships, where elemental amounts are defined in weight percent: T=Al+0.56Ti+0.29Nb+0.15Ta R=Al / T; 0.7≦R≦1 G=T-1.67R; 1.8<G<2.4 Z=Mo+0.52W; 7.5<Z<9.5 A nickel-chromium-cobalt alloy that further satisfies these requirements.

2. 1.0% by weight or less of titanium, 2.5% by weight or less of tantalum, 2. Niobium at a concentration of 2.7% by weight or less A nickel-chromium-cobalt alloy according to claim 1, comprising the above.

3. The aforementioned nickel-chromium-cobalt alloy is 3.1% to 4.1% by weight of aluminum, Titanium at 0.4% by weight or less, 2.5% by weight or less of tantalum, 1. Niobium at a weight of 3% or less Includes, The aforementioned nickel-chromium-cobalt alloy has the following compositional relationship, with elemental amounts defined in weight percent: T=Al+0.56Ti+0.29Nb+0.15Ta R=Al / T; 0.9≦R≦1 G=T-1.67R; 1.8<G<2.4 Z=Mo+0.52W; 7.5<Z<9.5 The nickel-chromium-cobalt alloy according to claim 1, further satisfying the above conditions.

4. Carbon exceeding 0% by weight and 0.1% or less, Boron at a concentration of 0.008% by weight or less, Silicon of 0.12% by weight or less, 0.03% by weight or less of zirconium and A nickel-chromium-cobalt alloy according to claim 1, comprising the above.

5. The nickel-chromium-cobalt alloy according to claim 1, comprising 8.5 to 11.5% by weight of cobalt.

6. The nickel-chromium-cobalt alloy according to claim 1, wherein the iron content is 1.5% by weight or more.

7. The nickel-chromium-cobalt alloy according to claim 1, wherein the titanium content is less than 0.1% by weight.

8. The aforementioned nickel-chromium-cobalt alloy is 16-20% by weight of chromium, 9-11% by weight of cobalt, 4.5 to 8% by weight of molybdenum, 1-6% by weight of tungsten, 1.5 to 4% by weight of iron, 3.1 to 4.1% by weight of aluminum, Titanium at 0.4% by weight or less, Tantalum of 1% by weight or less, Niobium at a weight of 1% or less, Carbon exceeding 0% by weight and 0.08% or less, Boron at a concentration of 0.008% by weight or less Includes, The aforementioned nickel-chromium-cobalt alloy has the following compositional relationship, with elemental amounts defined in weight percent: T=Al+0.56Ti+0.29Nb+0.15Ta R=Al / T; 0.95≦R≦1 G=T-1.67R; 1.9<G<2.4 Z=Mo+0.52W; 7.5<Z<9.5 The nickel-chromium-cobalt alloy according to claim 1, further satisfying the above conditions.

9. Silicon less than 0.1, Zirconium with a value of less than 0.02 and The nickel-chromium-cobalt alloy according to claim 8, further comprising the above.

10. The nickel-chromium-cobalt alloy according to claim 8, wherein the tungsten content exceeds 2% by weight.

11. The nickel-chromium-cobalt alloy according to claim 8, wherein the titanium content is less than 0.1% by weight.

12. The aforementioned impurities are Copper at a concentration of 0.5% by weight or less, 0.5% by weight or less of vanadium, Sulfur at a concentration of 0.015% by weight or less, Phosphorus at 0.03% by weight or less A nickel-chromium-cobalt alloy according to claim 1, comprising the above.

13. The aforementioned nickel-chromium-cobalt alloy is 16.80–19.46% by weight of chromium, 9.28–10.31% by weight of cobalt, 5.50 to 8.41% by weight of molybdenum, 5. Tungsten of 5.18% by weight or less, 0.89 to 4.49% by weight of iron, 3.0 to 3.90% by weight of aluminum, Titanium at 0.5% by weight or less, 2.01% by weight or less of tantalum, 2.2% by weight or less of niobium, 0.048 to 0.081 carbon atoms, Boron in concentrations of 0.003 to 0.006 and A nickel-chromium-cobalt alloy according to claim 1, comprising the above.

14. The nickel-chromium-cobalt alloy according to claim 1, further comprising at least one element selected from the group consisting of magnesium, calcium, yttrium, cerium, and lanthanum, wherein each of the elements is present in an amount of 0.05% by weight or less of the nickel-chromium-cobalt alloy.

15. The aforementioned nickel-chromium-cobalt alloy is 16-20% by weight of chromium, 8.5 to 11.5% by weight of cobalt, 4-8.5% by weight of molybdenum, Tungsten of 8% by weight or less, Iron at a weight of 5% or less, 3.1 to 4.1% by weight of aluminum, Titanium at 0.4% by weight or less, 2.5% by weight or less of tantalum, 1. Niobium at a weight of 1.3% or less, Carbon exceeding 0% by weight and 0.15% by weight or less, The remainder is nickel and impurities. Includes, The aforementioned nickel-chromium-cobalt alloy has the following compositional relationship, with elemental amounts defined in weight percent: T=Al+0.56Ti+0.29Nb+0.15Ta R=Al / T; 0.9≦R≦1 G=T-1.67R; 1.8<G<2.4 Z=Mo+0.52W; 7.5<Z<9.5 The nickel-chromium-cobalt alloy according to claim 1, further satisfying the above conditions.

16. The nickel-chromium-cobalt alloy according to claim 1, wherein the nickel-chromium-cobalt alloy is in a form selected from the group consisting of forging, casting, thermal spraying, and powder metallurgy.

17. The nickel-chromium-cobalt alloy according to claim 1, wherein the nickel-chromium-cobalt alloy is a forging form selected from the group consisting of sheets, plates, bars, wires, tubes, pipes, and forgings.

18. The nickel-chromium-cobalt alloy according to claim 1, wherein the nickel-chromium-cobalt alloy is formed as a component for a gas turbine engine case.

Citation Information

Patent Citations

  • Nickel-chromium-molybdenum-cobalt alloy

    GB1029609A

  • GB2712498

  • Ni-based alloy having excellent hot workability

    JP1989129942A

  • Screw material for resin molding

    JP1994172900A

  • US10,577,680