Aqueous method for titaniumizing alkali metal-based chromium / silica catalysts

The use of alkali metals and peroxide compounds in an aqueous process for preparing chromium titanate catalysts on silica supports addresses emission and efficiency issues, enabling high melt index HDPE production with uniform titanium distribution and reduced VOCs.

JP2026538994APending Publication Date: 2026-11-19CHEVRON PHILLIPS CHEMICAL COMPANY LP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026523149
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-07-23
Filing Date
2024-10-22
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing chromium/silica catalysts for producing high-density polyethylene (HDPE) suffer from high volatile organic compound emissions and non-uniform titanium incorporation when titanium is added via an anhydrous route, while aqueous alternatives have low titanium efficiency.

Method used

An aqueous method for preparing chromium titanate catalysts using alkali metals and peroxide compounds to impregnate silica with titanium, resulting in a titanated silica support with uniform titanium distribution and reduced emissions.

Benefits of technology

The method achieves high melt index potential with less titanium, producing HDPE with lower molecular weight and minimal volatile organic compound emissions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026538994000001_ABST
    Figure 2026538994000001_ABST
Patent Text Reader

Abstract

Disclosed are methods for producing a titrated silica support, a titrated chromium / silica pre-catalyst, and an activated titrated chromium / silica catalyst, wherein hydrogen peroxide and an alkali metal precursor are used during catalyst preparation. The resulting titrated chromium / silica pre-catalyst often contains silica, 0.1 to 5% by weight of chromium, 0.1 to 10% by weight of titanium, and 4% by weight or less of carbon, and further contains an alkali metal or zinc, with an alkali metal:titanium or zinc:titanium molar ratio of 0.02:1 to 3:1, and / or an amount of alkali metal or zinc in the range of 0.01 to 2 mmol per gram of silica. Using the high melt index potential activated titrated chromium / silica catalyst, olefins can be polymerized to produce, for example, ethylene-based homopolymers and copolymers having an HLMI value of more than 30 g / 10 min.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] Reference to related applications This application was filed on 22 October 2024 as a PCT international patent application and claims the benefit of priority to U.S. Patent Application No. 18 / 780,704 filed on 23 July 2024 and U.S. Patent Application No. 18 / 492,911 filed on 24 October 2023, the disclosures thereof being incorporated in their entirety by reference herein. U.S. Patent Application No. 18 / 492,911 is a continuation-in-part application of the concurrently pending U.S. Patent Application No. 18 / 306,326 filed on 25 April 2023, which claims the benefit of U.S. Provisional Patent Application No. 63 / 334,741 filed on 26 April 2022.

[0002] This disclosure generally relates to chromium titanate catalysts, methods for preparing chromium titanate catalysts, methods for polymerizing olefins using chromium titanate catalysts, polymer resins produced using such chromium catalysts, and articles produced using these polymer resins. More specifically, this disclosure relates to aqueous methods for producing chromium titanate catalysts in which alkali metals are utilized during catalyst preparation. [Background technology]

[0003] HDPE can be produced using a chromium / silica catalyst. Adding titanium to chromium / silica can enhance the activity of the catalyst, but more importantly, it can increase the melt index potential of the catalyst, that is, the ability of the catalyst to produce a polymer with a higher melt index or a higher melt flow. In many cases, titanium addition is achieved via an anhydrous route, in which a titanium precursor is used to impregnate chromium / silica with a suitable organic solvent such as a hydrocarbon, alcohol, or ether. Unfortunately, the presence of organic matter may result in high emissions of volatile organic compounds (VOCs) during the preparation, activation, and processing of the titanated chromium catalyst. Aqueous alternatives can be utilized, but they often suffer from low titanium efficiency and non-uniform incorporation. In view of these drawbacks, it would be beneficial to provide an improved process for making titanated chromium catalysts. Accordingly, the present invention is generally directed to this objective. SUMMARY OF THE INVENTION

[0004] This summary is provided to introduce a selection of concepts in a simplified form that are further described below in the Detailed Description. This summary is not intended to identify required or essential features of the claimed subject matter. Nor is this summary intended to be used to limit the scope of the claimed subject matter.

[0005] In one aspect of the present invention, a titanated silica support is disclosed, and in this aspect, the titanated silica support can comprise silica, 0.1 to 10 wt% titanium, 0.5 to 12 wt% water, 2 wt% or less carbon, and bound alkali metal and / or zinc, wherein the molar ratio of alkali metal:titanium or zinc:titanium is 0.02:1 to 3:1, and / or the alkali metal or zinc is present in an amount ranging from 0.01 to 2 mmol per gram of silica.

[0006] In another aspect of the present invention, a titanated chromium / silica pre-catalyst is disclosed, in this aspect, the titanated chromium / silica pre-catalyst can comprise silica, 0.1 to 5 wt% chromium, 0.1 to 10 wt% titanium, 0.5 to 12 wt% water, 4 wt% or less carbon, and bound alkali metal and / or zinc, wherein the molar ratio of alkali metal:titanium or zinc:titanium is 0.02:1 to 3:1, and / or the alkali metal or zinc is present in an amount ranging from 0.01 to 2 mmol per gram of silica.

[0007] In yet another aspect, a titanated chromium / silica catalyst is disclosed, in this aspect, the titanated chromium / silica catalyst can comprise silica, 0.1 to 5 wt% chromium, 0.1 to 10 wt% titanium, and bound alkali metal and / or zinc, wherein the molar ratio of alkali metal:titanium or zinc:titanium is 0.02:1 to 3:1, and / or the alkali metal or zinc is present in an amount ranging from 0.01 to 2 mmol per gram of silica, and at least 60 wt% of the chromium is present in the +6 oxidation state. In still yet another aspect, the titanated chromium / silica catalyst can comprise silica, 0.1 to 5 wt% chromium, and 0.1 to 10 wt% titanium, wherein at least 60 wt% of the chromium is present in the +6 oxidation state, and the catalyst satisfies the formula Y(HLMI)=(-9.6153x 3 +21.088x 2 +25.835x+5.7983) (wherein x is the number of titanium atoms per square nanometer of silica surface area of the titanated chromium / silica catalyst), characterized by a polymer HLMI (g / 10 min) greater than that defined by the foregoing formula.

[0008] The present invention also envisions and encompasses olefin polymerization processes. Such processes may include contacting one of the (activated) chromium titanate / silica catalysts disclosed herein and an optional co-catalyst with an olefin monomer and an optional olefin co-monomer in a polymerization reactor system under polymerization conditions to produce an olefin polymer. Beneficially, the chromium titanate / silica catalysts have a high melt index potential, which allows for the production of olefin polymers with a lower melt index (lower molecular weight) despite having less titanium in the catalyst.

[0009] Processes for preparing titrated silica supports and subsequent chromium catalysts are also described herein. A process for preparing a titrated silica support may include: (i) contacting water, a peroxide compound, a titanium precursor, and silica (under conditions sufficient for titanium to adsorb onto the silica) to form a first mixture; (ii) isolating a solid fraction from the first mixture; and (iii) drying the solid fraction to form a titrated silica support. Several variations of this process are also provided herein. A titrated chromium / silica pre-catalyst can be prepared using the same general process, but by impregnating a silica support with a chromium precursor at an appropriate step in each process. Subsequently, an (activated) titrated chromium / silica catalyst can be prepared by activating the titrated chromium / silica pre-catalyst under suitable activation conditions.

[0010] Both the above summary and the following detailed description are illustrative and provide examples only. Therefore, the above summary and the following detailed description should not be considered limiting. Furthermore, additional features or variations may be provided beyond those described herein. For example, certain embodiments may encompass combinations and partial combinations of the various features described in the detailed description of the invention.

[0011] The following drawings form part of this specification and are included to further illustrate certain aspects of the invention. The invention can be better understood by referring to these drawings in conjunction with the detailed description. [Brief explanation of the drawing]

[0012] [Figure 1] The plots of the HLMI of the polymer versus the number of titanium atoms per square nanometer are shown for the control group of chromium titanate / silica catalysts and the chromium titanate / silica catalysts from Examples 28 to 41. [Figure 2] The plots of the HLMI of the polymer versus the molar ratio of sodium:titanium for the titerated chromium / silica catalysts of Examples 199-204 are shown. [Figure 3] The plots of residual sodium versus total wash water for Comparative Examples 205-206 and the embodiments of the present invention shown in Table 23 are presented.

[0013] The invention disclosed herein is susceptible to various modifications and alternative forms, but only a few specific embodiments are shown in the drawings as examples and described in detail below. The drawings and detailed description of specific embodiments do not in any way limit the scope or range of the concept of the invention or the appended claims. Rather, the drawings and detailed description illustrate the concept of the invention to those skilled in the art and provide them with the means to create and use the concept of the invention.

[0014] definition To more clearly define the terms used herein, the following definitions are provided. Unless otherwise indicated, the following definitions apply to this disclosure. If a term is used herein but is not specifically defined herein, the definition in the IUPAC Compendium of Chemical Terminology, 2nd Ed (1997) may apply, provided that the applicable definition does not conflict with any other disclosure or definition applicable herein, or that it does not obscure or make impossible any patent claim to which the definition applies. To the extent that any definition or use provided by any document incorporated herein by reference conflicts with any definition or use provided herein, the definition or use provided herein shall prevail.

[0015] In this specification, subject matter features are described in such a way that different combinations of features may be envisioned within a particular embodiment. For all embodiments and features disclosed herein, all combinations that do not adversely affect the compounds, compositions, processes, or methods described herein, whether or not a particular combination is explicitly stated, are intended. In addition, unless expressly stated otherwise, any embodiment or feature disclosed herein may be combined to illustrate inventive compounds, compositions, processes, or methods consistent with this disclosure.

[0016] Generally, element groups are indicated using the numbering system shown in the version of the periodic table published in Chemical and Engineering News, 63(5), 27, 1985. In some cases, element groups can be indicated using the common names assigned to the groups, for example, alkali metals for group 1 elements, alkaline earth metals for group 2 elements, transition metals for group 3-12 elements, and halogens or halides for group 17 elements.

[0017] For any particular compound or group disclosed herein, any name or structure (general or specific) shown is intended to include, unless otherwise specified, all conformational isomers, positional isomers, stereoisomers, and mixtures thereof that may result from a particular group of substituents. Unless otherwise specified, the name or structure (general or specific) also includes all enantiomers, diastereomers, and other optical isomers, as well as mixtures of stereoisomers, whether in enantiomer or racemic form (if any), as recognized by those skilled in the art. For example, a general reference to pentane includes n-pentane, 2-methylbutane, and 2,2-dimethylpropane, and a general reference to a butyl group includes n-butyl, sec-butyl, isobutyl, and t-butyl.

[0018] In this specification, the terms “contact” and “combine” are used, unless otherwise specified, to describe compositions, processes, and methods in which materials or components are contacted or combined together in any order, in any manner, and for any length of time. For example, materials may be blended, mixed, slurried, dissolved, reacted, treated, formulated, or contacted or combined in several other ways or by any preferred method or technique.

[0019] In this disclosure, compositions, processes, and methods are described using the term "including" various components or steps, but unless otherwise stated, compositions, processes, and methods may "essentially consist of" or "consist of" various components or steps.

[0020] Terms such as "a," "an," and "the" are intended to include multiple options, e.g., at least one, unless otherwise specified. For example, the disclosure "a reactor" or "a comonomer" means, unless otherwise specified, to include one or more reactors or comonomers, respectively.

[0021] The term “polymer” is used herein to generally include olefin homopolymers, copolymers, terpolymers, and their alloys and blends. The term “polymer” also includes impact copolymers, block copolymers, graft copolymers, random copolymers, and alternating copolymers. Copolymers can be derived from an olefin monomer and one olefin comonomer, while terpolymers can be derived from an olefin monomer and two olefin comonomers. Thus, “polymer” encompasses copolymers and terpolymers. Similarly, the term “polymerization” encompasses homopolymers, copolymers, and ternary copolymers. Thus, ethylene polymers include ethylene homopolymers, ethylene copolymers (e.g., ethylene / α-olefin copolymers), ethylene terpolymers, and their blends or mixtures. Thus, ethylene polymers encompass polymers often referred to in the art as LLDPE (linear low-density polyethylene) and HDPE (high-density polyethylene). As an example, ethylene copolymers can be derived from ethylene and comonomers such as 1-butene, 1-hexene, or 1-octene. When the monomer and comonomer are ethylene and 1-hexene, respectively, the resulting polymer can be classified as an ethylene / 1-hexene copolymer. The term “polymer” also includes all possible geometric configurations, if present and unless otherwise specified, including isotactic, syndiotactic, and random symmetry. The term “polymer” also means polymers of any molecular weight.

[0022] The terms “catalytic composition,” “catalytic mixture,” and “catalytic system” are independent of the actual products or compositions resulting from the contact or reaction of the initial components of the disclosed or requested catalytic composition / mixture / system, the properties of the active catalytic sites, or the results of the cocatalyst or chromium titanate catalyst after these components are combined. Therefore, the terms “catalytic composition,” “catalytic mixture,” and “catalytic system” encompass the initial starting components of the composition, as well as any products(s) that may result from the contact of these initial starting components, including both heterogeneous and homogeneous catalytic systems or compositions. The terms “catalytic composition,” “catalytic mixture,” and “catalytic system” may be used interchangeably throughout this disclosure.

[0023] In this invention, several types of ranges are disclosed. Where any type of range is disclosed or claimed, the intent is to individually disclose or claim each number that can be reasonably considered to be included in such range, including the endpoint values ​​of that range, as well as any partial ranges and combinations of partial ranges that are included within that range. As a typical example, the chromium content of a pre-catalyst or catalyst may be a specific range in various embodiments of this invention. The disclosure that a pre-catalyst or catalyst contains 0.1 to 5 wt% chromium is intended to enumerate that the chromium content may be any amount within the range, including, for example, any range or combination of ranges of 0.1 to 5 wt% chromium, such as 0.3 to 3 wt%, 0.4 to 2 wt%, 0.5 to 1.5 wt%, or 0.7 to 1.5 wt%. Similarly, all other ranges disclosed herein should be interpreted in the same manner as these examples.

[0024] In general, quantities, sizes, formulations, parameters, ranges, or other quantities or characteristics are "about" or "approximate," whether explicitly stated as such. Whether modified by the terms "about" or "approximate," the claims include equivalents of such quantities or characteristics.

[0025] While any method, device, or material similar to or equivalent to those described herein may be used in carrying out or testing the present invention, this specification describes typical methods, devices, and materials.

[0026] All publications and patents referenced herein, for example, constructs and methodologies described in those publications and patents, are incorporated herein by reference in their entirety for the purpose of describing and disclosing constructs and methodologies that may be used in connection with the present invention as described herein. [Modes for carrying out the invention]

[0027] This specification discloses processes for preparing titrated silica supports and titrated chromium / silica pre-catalysts and activated catalysts. Advantageously, the presence of peroxide compounds and / or alkali metals during the steps used to prepare these support and catalyst materials significantly and unexpectedly increases the melt index potential of the titrated chromium catalyst. While we do not wish to be bound by the following theory, it is believed that the disclosed methods result in more uniform titanium incorporation, more efficient titanium use, and reduced titanium required to achieve the desired HLMI of the resulting polymer due to titanium adsorption onto the silica support. Furthermore, it is believed that the titanium content is uniformly distributed across all particle sizes, rather than being widely distributed depending on the relative size of the catalyst particles—whether small or large.

[0028] Titanized silica support and titrated chromium catalyst Typical and non-limiting examples of titrated silica supports conforming to the present invention include silica, 0.1 to 10 wt% titanium, 0.5 to 12 wt% water, 2 wt% or less carbon, and a bound alkali metal and / or zinc, wherein the alkali metal:titanium or zinc:titanium molar ratio is 0.02:1 to 3:1, and / or the alkali metal or zinc is present in an amount in the range of 0.01 to 2 mmol per gram of silica. These titrated silica supports are associated with a titrated chromium / silica pre-catalyst, one example of which includes silica, 0.1 to 5 wt% chromium, 0.1 to 10 wt% titanium, 0.5 to 12 wt% water, 4 wt% or less carbon, and a bound alkali metal and / or zinc, wherein the alkali metal:titanium or zinc:titanium molar ratio is 0.02:1 to 3:1, and / or the alkali metal or zinc is present in an amount in the range of 0.01 to 2 mmol per gram of silica. In this specification, “pre-catalyst” means that the catalyst has not been activated or calcined, in which all or most of the low-oxidation chromium is converted to the +6 (hexavalent chromium) oxidation state. Referring here to this chromium titanate / silica pre-catalyst, at least 75% by weight of the chromium is often present in an oxidation state of 3 or less. In some embodiments, at least 80% by weight, or at least 90% by weight, or at least 95% by weight, or all or substantially all of the chromium in the pre-catalyst may be present in an oxidation state of 3 or less.

[0029] Beneficially, there may be virtually no VOCs (volatile organic compounds) emitted during the heat treatment (e.g., calcination or activation) step. For example, there may be virtually no VOCs emitted during the calcination or activation of the chromium titanate / silica pre-catalyst (or chromium titanate / silica support). Accordingly, according to certain embodiments of the present invention, the chromium titanate / silica pre-catalyst (or chromium titanate / silica support) may contain 3% by weight or less, 2% by weight or less, or 1% by weight or less of carbon, and in some examples, it may contain 0.5% by weight or less, 0.3% by weight or less, or 0.1% by weight or less of carbon. These weight percentages are based on the amount of carbon (by weight) relative to the total weight of the pre-catalyst or support, respectively, and can be determined by CHN analysis.

[0030] Chromium titanate / silica pre-catalysts and silica titanate supports are generally in the form of free-flowing powders or particles. Nevertheless, these chromium titanate / silica pre-catalysts and silica titanate support materials may contain water / moisture, and on a weight basis, they may independently contain 0.5–12 wt% water / moisture. More often, the amount of water / moisture ranges from 1–11 wt%, 2.5–10 wt%, 3–9 wt%, or 5–8 wt%. These weight percentages are based on the amount of water / moisture relative to the total weight of each pre-catalyst or support and can be determined using thermogravimetric analysis (TGA).

[0031] A typical and non-limiting example of a chromium titanate / silica catalyst consistent with the present invention may include silica, 0.1 to 5 wt% chromium, 0.1 to 10 wt% titanium, and a bonded alkali metal and / or zinc, where the molar ratio of alkali metal:titanium or zinc:titanium is 0.02:1 to 3:1, and / or the amount of alkali metal or zinc per gram of silica is in the range of 0.01 to 2 mmol, and at least 60 wt% of chromium is present in an oxidized state of +6. Another non-limiting example of a typical chromium titanate / silica catalyst of the present invention may include silica, 0.1 to 5 wt% chromium, and 0.1 to 10 wt% titanium, where at least 60 wt% of chromium is present in an oxidized state of +6, and the catalyst is given by the formula Y(HLMI)=(-9.6153x 3 +21.088x 2 The polymer is characterized by an HLMI (g / 10 min) greater than +25.835x+5.7983) (wherein x is the number of titanium atoms per square nanometer of silica surface area of ​​the titrated chromium / silica catalyst). In this specification, “catalyst” is distinguished from “pre-catalyst” and means that the catalyst has been activated or calcined (activated catalyst), so that all or most of the chromium in the low oxidation state has been converted to the +6 oxidation state (hexavalent chromium). Thus, a “catalyst” can be formed by activating or calcining a “pre-catalyst”.

[0032] With respect to this chromium titanate / silica catalyst, at least 60% by weight of chromium is present in the +6 oxidation state. In one embodiment, at least 70% by weight of chromium in the chromium titanate / silica catalyst may be present in the +6 oxidation state; in another embodiment, at least 75% by weight; in yet another embodiment, at least 80% by weight; in yet another embodiment, at least 85% by weight; in yet another embodiment, at least 90% by weight; and in yet another embodiment, at least 95% by weight. The amount of Cr(VI) can be measured by mixing 2 g of catalyst with a solution of 20 mL of 2 M H2SO4, and then adding 5 drops of ferroin Fe(+3) indicator. This usually turns the mixture blue-green, indicating the presence of Fe(III) ions. Next, the mixture is titrated to the ferroin endpoint (red) using a solution of ammonium ferrous sulfate that has been precautioned by reaction with a standardized 0.1 M sodium dichromate solution. The endpoint is reached when the mixture turns red, the titration volume is recorded, and the oxidizing capacity of the catalyst is calculated and expressed in weight % of Cr(VI).

[0033] After calcination / activation, the amount of water / moisture present on the chromium titanide / silica catalyst is generally very low, for example, less than 3% by weight of water / moisture based on the total weight of the catalyst. More often, the chromium titanide / silica catalyst has a water / moisture content of less than 2% by weight, less than 1.5% by weight, less than 1% by weight, or less than 0.5% by weight. The disclosed chromium titanide / silica catalyst may also contain a bound alkali metal and / or zinc in a molar ratio of alkali metal:titanium or zinc:titanium of 0.02:1 to 3:1, or it may also contain an alkali metal and / or zinc in an amount ranging from 0.01 to 2 mmol of alkali metal or zinc per gram of silica, or both.

[0034] In one embodiment, a chromium titanate / silica catalyst can be characterized as having a melt index potential (MIP), i.e., HLMI (g / 10 min) due to polymer production, where HLMI (g / 10 min) is given by the formula Y(HLMI) = (-9.6153x 3 +21.088x2 +25.835x+5.7983) (wherein x is the number of titanium atoms per square nanometer of silica surface area of the titanated chromium / silica catalyst). This is illustrated in Figure 1 and is further discussed in the examples below. In some aspects, the titanated chromium / silica catalyst is such that Y=1.1*(-9.6153x 3 +21.088x 2 +25.835x+5.7983); alternatively Y=1.15*(-9.6153x 3 +21.088x 2 +25.835x+5.7983); alternatively Y=1.2*(-9.6153x 3 +21.088x 2 +25.835x+5.7983); or alternatively Y=1.3*(-9.6153x 3 +21.088x 2 +25.835x+5.7983). For these formulas, in general, the pore volume of the catalyst is no more than 2.2, 2.0, 1.8, or 1.6 mL / g; the catalyst is activated / calcined in dry air at 650°C for 3 hours; the polymer is produced with an isobutane diluent at an ethylene pressure of 105°C and 550 psig (3792 kPa) with a productivity of about 3000 g polymer / g catalyst (e.g., at least 2500, 2800, 3000, or 3200 g polymer / g catalyst).

[0035] The amount of chromium in the titanated chromium / silica precatalysts and titanated chromium / silica catalysts disclosed herein is not particularly limited. However, in general, the chromium content in each of the precatalyst or catalyst may range from 0.1 to 5 wt%; alternatively from 0.3 to 3 wt%; alternatively from 0.4 to 2 wt%; alternatively from 0.5 to 1.5 wt%; or alternatively from 0.7 to 1.5 wt%. These weight percentages are based on the amount of chromium relative to the total weight of the respective precatalyst or catalyst.

[0036] Here, referring to the titrated silica support, the titrated chromium / silica pre-catalyst, and the titrated chromium / silica catalyst, the amount of titanium present is also not particularly limited. However, generally, the amount of titanium in the support, pre-catalyst, or catalyst, respectively, may range from 0.1 to 10 wt%; alternatively 0.5 to 7 wt%; alternatively 0.5 to 3 wt%; alternatively 0.8 to 2 wt%; alternatively 1 to 6 wt%; or alternatively 1.5 to 4 wt%. These weight percentages are based on the amount of titanium relative to the total weight of the support, pre-catalyst, or catalyst, respectively. As disclosed herein, due to the catalyst preparation process utilizing alkali metals (or zinc) and peroxides, a lower titanium load is required to achieve a specific HLMI value of the resulting polymer compared to conventional titrated chromium catalysts.

[0037] Alkali metals or zinc are components of the support or catalyst in very small amounts, but their influence on the catalyst's performance is significant. Each support, pre-catalyst, or catalyst contains a suitable amount of (bound) alkali metal or zinc, and in many cases the minimum molar ratio of alkali metal:titanium or zinc:titanium is 0.02:1, 0.05:1, 0.08:1, 0.1:1, 0.12:1, 0.15:1, or 0.2:1, and additionally or alternatively, the maximum molar ratio is 3:1, 2.5:1, 2.2:1, 2:1, or 1.8:1. In general, the molar ratio of alkali metal:titanium or zinc:titanium may range from any minimum molar ratio to any maximum molar ratio described herein. For example, typical and non-limiting examples of suitable molar ratio ranges include 0.02:1~3:1, 0.08:1~3:1, 0.1:1~3:1, 0.12:1~3:1, 0.2:1~3:1, 0.02:1~2.5:1, 0.05:1~2.5:1, 0.12:1~2.5:1, 0.15:1~2.5:1, 0.05:1~2.2:1, and 0.1:1~2.2:1. Examples of molar ratios include 0.2:1-2.2:1, 0.02:1-2:1, 0.05:1-2:1, 0.1:1-2:1, 0.12:1-2:1, 0.15:1-2:1, 0.2:1-2:1, 0.02:1-1.8:1, 0.08:1-1.8:1, 0.1:1-1.8:1, 0.12:1-1.8:1, 0.15:1-1.8:1, or 0.2:1-1.8:1. This molar ratio is determined by ICP analysis.

[0038] Additionally or alternatively, each of the carrier, pre-catalyst, or catalyst contains a suitable amount of (bound) alkali metal or zinc, often in a minimum of 0.01, 0.02, 0.04, 0.08, 0.1, 0.11, 0.13, 0.15, or 0.2 mmol / g per gram of silica, and additionally or alternatively in a maximum of 2, 1.5, 1.2, 1, 0.9, or 0.8 mmol / g. Generally, the amount of alkali metal or zinc may be in the range of any minimum to any maximum amount in mmol / g units as described herein. For example, typical and non-limiting examples of preferred ranges for alkali metal or zinc amounts (mmol / g) include 0.01~2, 0.02~2, 0.08~2, 0.1~2, 0.11~2, 0.13~2, 0.15~2, 0.01~1.5, 0.04~1.5, 0.11~1.5, 0.2~1.5, 0.01~1.2, 0.04~1.2, 0.1~1.2, 0.11~1.2, 0.15~1.2, and 0.01. Examples include mmol / g of ~1, 0.04~1, 0.08~1, 0.1~1, 0.11~1, 0.13~1, 0.15~1, 0.2~1, 0.02~0.9, 0.08~0.9, 0.11~0.9, 0.15~0.9, 0.2~0.9, 0.01~0.8, 0.02~0.8, 0.04~0.8, 0.1~0.8, 0.11~0.8, 0.13~0.8, 0.15~0.8, or 0.2~0.8 mmol / g. The alkali metal (or zinc) content is based on the mmol of alkali metal (or zinc) versus the total weight (in grams) of silica in the carrier, pre-catalyst, or catalyst, respectively. This is determined by ICP analysis.

[0039] In one embodiment, the carrier, pre-catalyst, or catalyst may contain an alkali metal, and in another embodiment, the carrier, pre-catalyst, or catalyst may contain zinc. The alkali metal present on the carrier, pre-catalyst, or catalyst may be cesium, lithium, sodium, or potassium, or any combination thereof (or may include these). Thus, the alkali metal may be lithium (or may include these); alternatively, it may be sodium; or alternatively, it may be potassium. Since sodium and other such metals are typically catalyst poisons, it is unexpected that the presence of alkali metals on the pre-catalyst and catalyst, particularly in the amounts described above, does not impair catalytic activity.

[0040] Nitrogen may also be present on the support, pre-catalyst, or catalyst, depending on the properties of the materials used during catalyst preparation and the chromium source / precursor, among other factors. However, the support, pre-catalyst, or catalyst may each contain 0.01–1.5 wt% of N, for example, 0.1–1.5 wt%, 0.3–1 wt%, 0.4–1.2 wt%, 0.4–1 wt%, or 0.5–0.7 wt%. These weight percentages are based on the total weight of the support, pre-catalyst, or catalyst and can be determined by CHN analysis.

[0041] In terms of weight, the majority of the support, pre-catalyst, or catalyst is silica, often at least 70% by weight, at least 80% by weight, at least 85% by weight, or at least 90% by weight. An exemplary and non-limiting range of silica amounts for the support, pre-catalyst, or catalyst includes 70–99.5% by weight, 80–98% by weight, 80–95% by weight, 85–98% by weight, 85–95% by weight, 90–99.5% by weight, or 90–98% by weight, and so on.

[0042] The pore volume of the titrated silica support, the titrated chromium / silica pre-catalyst, and the titrated chromium / silica catalyst is not particularly limited. For example, the pore volume (total pore volume due to nitrogen sorption) of the support, pre-catalyst, or catalyst, respectively, can be in the range of 0.5-3 mL / g, 0.8-2.5 mL / g, 1-2 mL / g, 1.3-1.8 mL / g, etc. (determined according to Halsey, GD, J. Chem. Phys. (1948), 16, pp. 931). Similarly, the surface area of ​​the titrated silica support, the titrated chromium / silica pre-catalyst, and the titrated chromium / silica catalyst is not limited to a specific range. However, generally, the BET surface area of ​​the support, pre-catalyst, or catalyst, respectively, is 100-700 m². 2 / g, 150~650m 2 / g, 200-600m 2 / g, or 250-550m 2 It can be in the range of / g, etc. (determined using the BET nitrogen adsorption method described in Brunauer et al., J. Am. Chem. Soc., 60, 309 (1938) as described in ASTMD1993-91).

[0043] The titrated silica support, titrated chromium / silica pre-catalyst, and titrated chromium / silica catalyst can have any suitable particle size, as will be understood by those skilled in the art. Exemplary and non-limiting ranges of the average particle size (d50) of the support, pre-catalyst, or catalyst, respectively, may include 15–350 μm, 25–300 μm, 40–120 μm, 50–200 μm, or 75–150 μm (determined using laser diffraction in accordance with ISO 13320).

[0044] Unexpectedly, unlike other aqueous catalyst preparation procedures, titanium is adsorbed onto silica in the disclosed support, pre-catalyst, and catalyst. The adsorbed titanium and the color changes observed during catalyst preparation are described in the following examples.

[0045] Furthermore, in the disclosed support, pre-catalyst, and catalyst, at least a portion of the zinc or alkali metal is (chemically) bonded to titanium. For example, although not bound by theory, it is thought that at least a portion of the sodium (or other alkali metal, or zinc) is bonded to titanium via oxygen atoms. Additionally or alternatively, at least a portion of the zinc and titanium exists as zinc titanate, and / or at least a portion of the alkali metal and titanium exists as alkali metal titanate, one example being sodium titanate. These features can be determined using suitable analytical techniques such as XPS and XRD.

[0046] Unexpectedly, sodium (or other alkali metals, or zinc) present on the titrated silica support, titrated chromium / silica pre-catalyst, and titrated chromium / silica catalyst is "bound" (or often referred to as "firmly bound") to the support / catalyst and is not readily removed by conventional washing of the support / catalyst. Herein, "bound" alkali metal or zinc refers to the amount of each alkali metal or zinc remaining after three equivalent washing / filtration cycles, on a dry basis, resulting in a total of 300 lbs of washing water per lb of support / catalyst. In the first cycle, each lb of support or catalyst required by the context is combined with 100 lbs of deionized water, mixed / slurred at 25°C for 30 minutes, and then filtered. This washing / filtration cycle is repeated two more times for the filtered solid support or catalyst. Sodium (or other alkali metals, or zinc) not "bound" to the support / catalyst is virtually completely removed after these three equivalent washing / filtration cycles, resulting in a total of 300 lbs of washing water per lb of support / catalyst.

[0047] Polymerization process Using the activated chromium titanate / silica catalyst of the present invention, olefins can be polymerized to form homopolymers, copolymers, terpolymers, and the like. One such process for polymerizing olefins may involve contacting any (activated) chromium titanate / silica catalyst disclosed herein (e.g., produced by any process disclosed herein) and an optional co-catalyst with an olefin monomer and an optional olefin comonomer in a polymerization reactor system under polymerization conditions to produce an olefin polymer.

[0048] Polymerization processes disclosed herein often utilize cocatalysts. In some embodiments, the cocatalyst may include metal hydrocarbyl compounds, examples of which include non-halide metal hydrocarbyl compounds, metal hydrocarbyl halide compounds, non-halide metal alkyl compounds, and metal alkyl halide compounds, where the metal is any suitable metal, often a Group 13 metal. Thus, in certain embodiments of the present invention, the metal may be boron or aluminum, and the cocatalyst may include boron hydrocarbyl or alkyl, or aluminum hydrocarbyl or alkyl, and combinations thereof.

[0049] In one embodiment, the cocatalyst may include an aluminoxane compound, an organoaluminum compound, or an organoboron compound, which includes combinations of two or more cocatalyst compounds. Representative and non-limiting examples of aluminoxanes include methylaluminoxane, modified methylaluminoxane, ethylaluminoxane, n-propylaluminoxane, isopropylaluminoxane, n-butylaluminoxane, t-butylaluminoxane, sec-butylaluminoxane, isobutylaluminoxane, 1-pentylaluminoxane, 2-pentylaluminoxane, 3-pentylaluminoxane, isopentylaluminoxane, neopentylaluminoxane, or any combination thereof. Representative and non-limiting examples of organoaluminum compounds include trimethylaluminum, triethylaluminum, tri-n-propylaluminum, tri-n-butylaluminum, triisobutylaluminum, tri-n-hexylaluminum, tri-n-octylaluminum, diisobutylaluminum hydride, diethylaluminum ethoxide, diethylaluminum chloride, or any combination thereof. Representative and non-limiting examples of organoborones include tri-n-butylborane, tripropylborane, triethylborane, or any combination thereof. Co-catalysts that can be used with the catalyst of the present invention are not limited to the above-mentioned co-catalysts. Other suitable co-catalysts (such as organomagnesium and organolithium) are well known to those skilled in the art and include, for example, those disclosed in U.S. Patents 3,242,099, 4,794,096, 4,808,561, 5,576,259, 5,807,938, 5,919,983, 7,294,599, 7,601,665, 7,884,163, 8,114,946, and 8,309,485.

[0050] The unsaturated monomers that can be used with the titrated chromium / silica catalyst and polymerization process of the present invention typically include olefin compounds having 2 to 30 carbon atoms per molecule and at least one olefinic double bond. The present invention encompasses homopolymerization processes using a single olefin such as ethylene or propylene, as well as copolymerization, ternary copolymerization, and other reactions using an olefin monomer with at least one different olefin compound. For example, the resulting ethylene copolymers, terpolymers, etc., may generally contain a majority amount of ethylene (>50 mole percent) and a small amount of comonomer (<50 mole percent), but this is not essential. Comonomers that can copolymerize with ethylene may often have 3 to 20 carbon atoms or 3 to 10 carbon atoms in their molecular chains.

[0051] In the present invention, acyclic olefins, cyclic olefins, polycyclic olefins, terminal (α) olefins, internal olefins, linear olefins, branched olefins, substituted olefins, unsubstituted olefins, functionalized olefins, and unfunctionalized olefins can be used. For example, typical unsaturated compounds that can be polymerized using the titranidized chromium / silica catalyst of the present invention include, but are not limited to, ethylene, propylene, 1-butene, 2-butene, 3-methyl-1-butene, isobutylene, 1-pentene, 2-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 2-hexene, 3-hexene, 3-ethyl-1-hexene, 1-heptene, 2-heptene, 3-heptene, four n-octenenes (e.g., 1-octene), four n-nonenes, five n-decenes, or mixtures of two or more of these compounds. Without limitation, cyclic and bicyclic olefins, including cyclopentene, cyclohexene, norbornylene, norbornadiene, etc., can also be polymerized as described herein. Styrene can also be used as a monomer in the present invention. In one embodiment, the olefin monomer is C2-C 20 Olefin; alternatively, C2-C 20Alpha-olefin; alternatively, C2-C 10 Olefin; alternatively, C2-C 10 It may contain alpha-olefins; alternatively, the olefin monomer may contain ethylene; or alternatively, the olefin monomer may contain propylene.

[0052] If a copolymer (or alternatively, a terpolymer) is desired, the olefin monomer and olefin comonomer are independently, for example, C2-C 20 It may contain alpha-olefins. In some embodiments, the olefin monomer is at least one comonomer (e.g., C2-C 20 Alpha-olefin, C3-C 20 It may include ethylene or propylene copolymerized with alpha-olefins (such as alpha-olefins). According to one aspect of the present invention, the olefin monomer used in the polymerization process may include ethylene. In this aspect, suitable olefin comonomers include, but are not limited to, propylene, 1-butene, 2-butene, 3-methyl-1-butene, isobutylene, 1-pentene, 2-pentene, 3-methyl-1-pentene, 4-methyl-1-pentene, 1-hexene, 2-hexene, 3-ethyl-1-hexene, 1-heptene, 2-heptene, 3-heptene, 1-octene, 1-decene, styrene, etc., or combinations thereof. According to another aspect of the present invention, the olefin monomer may include ethylene, and the comonomer may be C3-C 10 It may contain alpha-olefins; alternatively, the comonomer may contain 1-butene, 1-pentene, 1-hexene, 1-octene, 1-decene, styrene, or any combination thereof; alternatively, the comonomer may contain 1-butene, 1-hexene, 1-octene, or any combination thereof; alternatively, the comonomer may contain 1-butene; alternatively, the comonomer may contain 1-hexene; alternatively, the comonomer may contain 1-octene.

[0053] Generally, the amount of comonomer introduced into a polymerization reactor system to produce a copolymer may be 0.01 to 50 weight percent based on the total weight of the monomer and comonomer. According to another aspect of the present invention, the amount of comonomer introduced into a polymerization reactor system may be 0.01 to 40 weight percent of comonomer, or alternatively, 0.1 to 35 weight percent of comonomer, or 0.5 to 20 weight percent of comonomer, based on the total weight of the monomer and comonomer.

[0054] While not intended to be bound by this theory, it is believed that steric hindrance can hinder and / or delay the polymerization process when branched, substituted, or functionalized olefins are used as reactants. Therefore, branched and / or cyclic portions of an olefin that are somewhat distant from the carbon-carbon double bond are not expected to inhibit the reaction as much as the same olefin substituents located closer to the carbon-carbon double bond.

[0055] According to one aspect of the present invention, at least one monomer / reactant may be ethylene (or propylene), and therefore the polymerization reaction may be homopolymerization with ethylene (or propylene) alone, or copolymerization with different acyclic olefins, cyclic olefins, terminal olefins, internal olefins, linear olefins, branched olefins, substituted olefins, or unsubstituted olefins. Furthermore, the titranidized chromium / silica catalyst of the present invention can be used for the polymerization of diolefin compounds, including but not limited to 1,3-butadiene, isoprene, 1,4-pentadiene, and 1,5-hexadiene.

[0056] The titrated chromium / silica catalyst of the present invention is intended for any olefin polymerization method using various types of polymerization reactor systems and reactors. Polymerization reactor systems may include any polymerization reactor capable of polymerizing olefin monomers and comonomers (one or more comonomers) to produce homopolymers, copolymers, terpolymers, etc. Various types of reactors may be referred to as batch reactors, slurry reactors, gas-phase reactors, solution reactors, high-pressure reactors, tubular reactors, autoclave reactors, or combinations thereof. Polymerization conditions for various reactor types are well known to those skilled in the art. Gas-phase reactors may include fluidized bed reactors or multi-stage horizontal reactors. Slurry reactors may include vertical loops or horizontal loops. High-pressure reactors may include autoclaves or tubular reactors. These reactor types can generally be operated continuously. In continuous processes, intermittent or continuous polymer product discharge may be used. Polymerization reactor systems and processes may also include partial or complete direct recycling of unreacted monomers, unreacted comonomers, and / or diluents.

[0057] The polymerization reactor system of the present invention may include one type of reactor, or multiple reactors of the same or different types (e.g., a single reactor, a double reactor, or two or more reactors). For example, the polymerization reactor system may include a solution reactor, a gas-phase reactor, a slurry reactor, or a combination of two or more of these reactors. Polymer production in multiple reactors may include multiple steps in at least two separate polymerization reactors interconnected by a transfer device that allows the polymer obtained from a first polymerization reactor to be transferred to a second reactor. The polymerization conditions in one of the reactors may differ from the operating conditions of the other reactors. Alternatively, polymerization in multiple reactors may include manual transfer of the polymer from one reactor to the next for continuous polymerization. The multiple reactor system may include, but is not limited to, multiple loop reactors, multiple gas-phase reactors, a combination of loop reactors and gas-phase reactors, multiple high-pressure reactors, or a combination of high-pressure reactors and loop reactors and / or gas-phase reactors. Multiple reactors can be operated in series, in parallel, or both. Therefore, the present invention encompasses polymerization reactor systems comprising a single reactor, two reactors, and more than two reactors. In certain embodiments of the present invention, the polymerization reactor system may include slurry reactors, gas-phase reactors, solution reactors, and combinations of multiple reactors thereof.

[0058] In one embodiment, the polymerization reactor system may include, for example, at least one loop slurry reactor, including a vertical or horizontal loop. Monomers, diluents, catalysts, and optionally selected comonomers are continuously supplied to the loop reactor where polymerization takes place. Generally, the continuous process may include continuously introducing monomers / comonomers, catalysts, and diluents into the polymerization reactor and continuously removing the suspension containing polymer particles and diluents from the reactor. The reactor effluent can be flashed to remove the solid polymer from the liquid containing the diluents, monomers, and / or comonomers. This separation step may include, but is not limited to, a variety of techniques, including flashing which may include any combination of heating and reduced pressure, separation by cyclone action in either cyclone treatment or hydrocyclone treatment, or separation by centrifugation.

[0059] Typical slurry polymerization processes (also known as particle formation processes) are disclosed, for example, in U.S. Patents 3,248,179, 4,501,885, 5,565,175, 5,575,979, 6,239,235, 6,262,191, 6,833,415, and 8,822,608. Suitable diluents used in slurry polymerization include, but are not limited to, hydrocarbons that are liquid under the reaction conditions and the monomers being polymerized. Examples of suitable diluents include, but are not limited to, hydrocarbons such as propane, cyclohexane, isobutane, n-butane, n-pentane, isopentane, neopentane, and n-hexane. Some loop polymerization reactions can occur under bulk conditions without the use of diluents and can be used in the bulk polymerization of propylene to form polypropylene homopolymers.

[0060] In yet another embodiment, the polymerization reactor system may include at least one gas-phase reactor (e.g., a fluidized bed reactor). Such a reactor system can utilize a continuous recycle flow containing one or more monomers that are continuously circulated through a fluidized bed in the presence of a catalyst under polymerization conditions. The recycle flow can be recovered from the fluidized bed and recycled back into the reactor. Simultaneously, the polymer product can be recovered from the reactor and replaced with new or fresh monomers. Such a gas-phase reactor may include a multi-step gas-phase polymerization process of olefins, in which the olefin is polymerized in the gas phase in at least two independent gas-phase polymerization zones, while a catalyst-containing polymer formed in a first polymerization zone is supplied to a second polymerization zone. One type of gas-phase reactor is disclosed in U.S. Patents 5,352,749, 4,588,790, 5,436,304, 7,531,606, and 7,598,327.

[0061] In yet another embodiment, the polymerization reactor system may include a high-pressure polymerization reactor, which may include, for example, a tubular reactor or an autoclave reactor. The tubular reactor may have several zones to which fresh monomers, initiators, or chromium titanate / silica catalysts are added. The monomers may be entrained in an inert gas stream and introduced in one zone of the reactor. Initiators, chromium titanate / silica catalysts, and / or catalyst components may be entrained in a gas stream and introduced in another zone of the reactor. The gas streams may be internally mixed for polymerization. Heat and pressure may be appropriately used in such a high-pressure polymerization reactor to obtain optimal polymerization reaction conditions.

[0062] In yet another embodiment, the polymerization reactor system may include a solution polymerization reactor, where monomers / comonomers can be brought into contact with a catalyst by suitable stirring or other means. An inert organic diluent or a carrier containing excess monomer can be used. If desired, the monomers / comonomers can be brought into contact with the catalytic reaction product in the gas phase, in or out of the presence of a liquid substance. The polymerization zone can be maintained at a temperature (e.g., between 150°C and 180°C) and pressure that leads to the formation of a polymer solution in the reaction medium. Stirring can be used to obtain better temperature control and maintain a uniform polymerization mixture throughout the polymerization zone. Appropriate means are used to dissipate the heat generated by polymerization.

[0063] In some embodiments, the polymerization reactor system may include any combination of a feed system, a feed system for catalysts and / or catalyst components, and / or a polymer recovery system, including a continuous system. In other embodiments, a suitable reactor system may include systems for feed material purification, catalyst storage and preparation, extrusion, reactor cooling, polymer recovery, fractionation, recycling, storage, loading, laboratory analysis, and process control.

[0064] Polymerization conditions that can be monitored, adjusted, and / or controlled to obtain efficiency and desired polymer properties include, but are not limited to, reactor temperature, reactor pressure, catalyst flow rate to the reactor, monomer flow rate to the reactor (and monomer-monomer, if used), monomer concentration in the reactor, olefin polymer yield, recycling rate, hydrogen flow rate (if used), and reactor cooling state. The polymerization temperature can affect catalyst productivity, polymer molecular weight, and molecular weight distribution. A suitable polymerization temperature may be any temperature below the depolymerization temperature according to the Gibbs free energy equation. Typically, this includes 60°C to 280°C, e.g., 60°C to 185°C, 60°C to 120°C, or 130°C to 180°C, depending on the type of polymerization reactor, polymer grade, etc. In some reactor systems, the polymerization reactor temperature may generally be in the range of 70°C to 110°C, or 125°C to 175°C. Various polymerization conditions can be kept substantially constant, for example, for the production of a particular grade of olefin polymer.

[0065] The preferred pressure also varies depending on the reactor and polymerization type. For liquid-phase polymerization in loop reactors, the pressure can typically be less than 1000 psig (6.9 MPa). For gas-phase polymerization, the pressure can usually be in the range of 200 psig to 500 psig (1.4 MPa to 3.4 MPa). High-pressure polymerization in tubular or autoclave reactors can generally be carried out at 20,000 psig to 75,000 psig (138 MPa to 517 MPa). Polymerization reactors can also generally be operated in the supercritical region, which occurs at higher temperatures and pressures (e.g., above 92°C and 700 psig (4.83 MPa)). Operating above the critical point of the pressure / temperature diagram (supercritical phase) can offer advantages to the polymerization reaction process.

[0066] Aspects of the present invention also relate to olefin polymerization processes carried out in the absence of added hydrogen. The olefin polymerization process of the present invention comprises producing an olefin polymer by contacting a chromium titanate / silica catalyst and an optional co-catalyst with an olefin monomer and optionally an olefin co-monomer in a polymerization reactor system under polymerization conditions, wherein the polymerization process is carried out in the absence of added hydrogen (no hydrogen is added to the polymerization reactor system). As will be recognized by those skilled in the art, hydrogen can be generated in situ by certain catalyst systems in various olefin polymerization processes, and the amount generated can vary depending on the catalyst components used, the type of polymerization process used, the polymerization reaction conditions utilized, and so on.

[0067] In other embodiments, it may be desirable to carry out the polymerization process in the presence of a certain amount of added hydrogen. Therefore, the olefin polymerization process of the present invention comprises producing an olefin polymer by contacting a chromium titanate / silica catalyst and an optional co-catalyst with an olefin monomer and optionally an olefin co-monomer in a polymerization reactor system under polymerization conditions, wherein the polymerization process is carried out in the presence of added hydrogen (by adding hydrogen to the polymerization reactor system). For example, the ratio of hydrogen to olefin monomer in the polymerization process can often be controlled by the supply ratio of hydrogen entering the reactor to the olefin monomer. The amount of hydrogen added to the process (based on the amount of olefin monomer) can generally be controlled in molar percentages within the ranges of 0.05 to 20 mol%, 0.1 to 15 mol%, 0.25 to 10 mol%, or 0.5 to 10 mol%. In some embodiments of the present invention, the supply of hydrogen to olefin monomer or reactant ratio can be kept substantially constant during polymerization runs of a particular polymer grade. That is, the hydrogen:olefin monomer ratio can be selected at a specific ratio and maintained within + / - 25% during polymerization runs. Furthermore, the amount of comonomer (or multiple comonomers) added may be substantially constant throughout the polymerization run of a particular polymer grade, and is generally constant. However, in other embodiments, it is intended that monomers, comonomers (or multiple comonomers), and / or hydrogen can be periodically pulsed into the reactor in a manner similar to that used, for example, in U.S. Patent No. 5,739,220 and U.S. Patent Publication No. 2004 / 0059070.

[0068] By controlling the concentration of reactants entering the polymerization reactor system, resins with specific physical and mechanical properties can be produced. The proposed end-use products formed from the polymer resin and the methods for ultimately forming those products can determine the desired polymer properties and attributes. Mechanical properties include tensile tests, bending tests, impact tests, creep tests, stress relaxation tests, and hardness tests. Physical properties include density measurements, molecular weight measurements, molecular weight distribution measurements, melting point temperature measurements, glass transition temperature measurements, temperature melt of crystallization measurements, density measurements, stereoregularity measurements, crack growth measurements, long-chain branching measurements, and rheological measurements. The present invention also covers and encompasses polymers produced by any of the polymerization processes disclosed herein. Manufactured articles can be formed from and / or contain polymers produced according to the present invention.

[0069] Polymers and Articles The olefin polymers incorporated herein may include any polymer produced from any olefin monomer and any select comonomer(s) described herein. For example, the olefin polymer may include ethylene homopolymers, ethylene copolymers (e.g., ethylene / α-olefin, ethylene / 1-butene, ethylene / 1-hexene, ethylene / 1-octene, etc.), propylene homopolymers, propylene copolymers, ethylene terpolymers, propylene terpolymers, etc., and any combination thereof. In one embodiment, the olefin polymer may include ethylene homopolymers; in another embodiment, the olefin polymer may include ethylene / 1-butene copolymers, ethylene / 1-hexene copolymers, and / or ethylene / 1-octene copolymers; and in yet another embodiment, the olefin polymer may include ethylene / 1-hexene copolymers.

[0070] If the polymer produced according to the present invention is, for example, an ethylene polymer, its properties are known in the polyolefin industry and can be characterized by various analytical techniques used. The manufactured articles can be formed from and / or contain the olefin polymers of the present invention (e.g., ethylene polymers), and typical properties of these polymers are shown below.

[0071] Ethylene polymers produced according to the present invention may have a melt index (MI) of 100 g / 10 min or less. Preferred ranges for MI may include, but are not limited to, 0.1 to 10, 0.2 to 5, or 0.25 to 2 g / 10 min. Additionally or alternatively, ethylene polymers may have high-load melt indices (HLMI) such as 1 to 1000, 5 to 500, 6 to 40, 8 to 60, 10 to 100, or 12 to 50 g / 10 min.

[0072] The density of ethylene-based polymers produced using titanated chromium / silica catalysts and the processes disclosed herein is often 0.91 g / cm³. 3 That concludes the explanation. In one aspect of the present invention, the density of the ethylene polymer is 0.92 to 0.965 g / cm³. 3 It may be in the range of 0.93 to 0.96 g / cm³. Furthermore, in another embodiment, the density may be 0.93 to 0.96 g / cm³. 3 For example, 0.935~0.955 g / cm³ 3 , or 0.94~0.95 g / cm³ 3 It could be within a range such as these.

[0073] In some embodiments, the ethylene polymers described herein may have an Mw / Mn ratio or polydispersity index of 5 or greater, 7 or greater, or 9 or greater. In many cases, Mw / Mn may be in the range of 15 to 30, so the non-limiting range of Mw / Mn includes 5 to 30, 7 to 25, 9 to 20, 10 to 25, or 10 to 15, etc. Additionally or alternatively, ethylene polymers may have an Mw in the range of 10 to 500 kg / mol, more often in the range of 30 to 300, 50 to 400, 50 to 250, 80 to 200, or 100 to 250 kg / mol. Additionally or alternatively, ethylene polymers may have an Mn in the range of 1 to 50 kg / mol, more often in the range of 3 to 30, 4 to 40, 5 to 25, or 8 to 20 kg / mol.

[0074] The Carreau-Yasuda "a" parameter (CY-a parameter) is particularly sensitive to slight changes in LCB. In some embodiments, the ethylene polymers described herein may have a CY-a parameter in the range of 0.05–0.5, 0.08–0.4, or 0.1–0.3, while in other embodiments, the ethylene polymers described herein may have a CY-a parameter in the range of 0.1–0.25, or 0.15–0.25.

[0075] Ethylene polymers, whether homopolymers or copolymers, can be formed into a variety of manufactured articles. Articles that may contain the polymers of the present invention include, but are not limited to, agricultural films, automotive parts, bottles, drums, textiles or fabrics, food packaging films or containers, food service articles, fuel tanks, geomembranes, household containers, liners, molded articles, medical devices or materials, pipes, sheets or tapes, and toys. These articles can be formed using a variety of processes. Non-limiting examples of these processes include injection molding, blow molding, rotational molding, film extrusion, sheet extrusion, shape extrusion, and thermoforming. Furthermore, additives and modifiers are often added to these polymers to provide beneficial polymer processing or end-use product attributes. Such processes and materials are described in Modern Plastics Encyclopedia, Mid-November 1995 Issue, Vol. 72, No. 12; and Film Extrusion Manual ― Process, Materials, Properties, TAPPI Press, 1992.

[0076] Process for manufacturing titanium silica support Aspects of the present invention relate to a process for preparing a titrated silica support. The first process may include (i) contacting water, a peroxide compound, a titanium precursor, and silica (under conditions sufficient for titanium to adsorb onto the silica) to form a first mixture; (ii) isolating a solid fraction from the first mixture; and (iii) drying the solid fraction to form a titrated silica support. The second process may include (a) contacting water, hydrogen peroxide, an alkali metal precursor and / or a zinc precursor, a titanium precursor, and silica (under conditions sufficient for titanium to adsorb onto the silica) to form a first mixture; (b) contacting the first mixture with a nitrogen-containing compound (e.g., NH4OH) to form a second mixture; (c) subjecting the second mixture to a reaction temperature in the range of 40 to 270°C; (d) isolating a solid fraction from the second mixture and washing the solid fraction; and (e) drying the solid fraction to form a titaniumated silica support. The third process may include (or may essentially consist of, or may consist of) (A) contacting water, hydrogen peroxide, an alkali metal precursor and / or a zinc precursor, a titanium precursor, and silica (under conditions sufficient for titanium to adsorb onto silica) to form a first mixture; (B) subjecting the first mixture to a reaction temperature in the range of 40 to 270°C; (C) isolating a solid fraction from the first mixture and washing this solid fraction; and (D) drying this solid fraction to form a titaniumated silica support. In the second and third processes, the alkali metal precursor (or zinc precursor) is any suitable source of alkali metal (or zinc), or any compound that produces alkali metal (or zinc) in water. The third process does not require nitrogen compounds and organic matter (hydrocarbons), so emissions are very low.

[0077] In general, the characteristics of these processes (e.g., the relative amounts of water, peroxide, alkali metal or zinc precursor, and titanium precursor; alkali metal precursor; titanium precursor; pH; silica properties; reaction temperature; isolation and washing techniques; and characteristics of the drying step) are described independently herein, and these characteristics can be combined in any combination to further describe the disclosed processes for producing titaniumated silica supports. Furthermore, additional process steps can be performed before, during, and / or after any step in any of the processes disclosed herein, and unless otherwise stated, these processes can be used in any combination without limitation to further describe them. Furthermore, any titaniumated silica supports produced according to the disclosed processes are within the scope of this disclosure and are incorporated herein.

[0078] The specific peroxide compounds used herein are not particularly limited and may be any peroxide compounds suitable for providing effective titaniumation of olefin polymerization catalysts and their pre-catalysts. In one embodiment, the peroxide compound includes organic peroxides, diacyl peroxides, peroxydicarbonates, monoperoxycarbonates, peroxyketals, peroxyesters, dialkyl peroxides, hydroperoxides, peracids, or any combination thereof. In another embodiment, the peroxide compound includes hydrogen peroxide, di-tert-butyl peroxide, benzoyl peroxide, dicumyl peroxide, cumene hydroperoxide, tert-butyl hydroperoxide, phthaloyl peroxide, or any combination thereof. In yet another embodiment, the peroxide compound includes (or is essentially made from or consists of) hydrogen peroxide.

[0079] In the first step of the first, second, and third processes, the materials can be brought into contact or combined in any order to form a first mixture. For example, in the first process, in one embodiment, water and silica can be combined first, followed by the addition of a peroxide compound (e.g., hydrogen peroxide), and then a titanium precursor; on the other hand, these four components can be combined substantially simultaneously. For example, in the second process, in one embodiment, for example, water, silica, and an alkali metal precursor and / or zinc precursor can be combined first, followed by the addition of hydrogen peroxide, and then a titanium precursor to form a first mixture, after which a nitrogen-containing compound can be added to form a second mixture. However, in another embodiment, the five components can be combined substantially simultaneously to form a first mixture. For example, in the third process, in one embodiment, for example, water, silica, and an alkali metal precursor and / or zinc precursor can be combined first, followed by the addition of hydrogen peroxide, and then a titanium precursor to form a first mixture; on the other hand, these five components can be combined substantially simultaneously. In these processes, the step of forming the first mixture can be carried out at any suitable temperature (e.g., room temperature) and for any suitable period of time, and the step of forming the second mixture in the second process can be carried out similarly.

[0080] The first step of each of these processes can alternatively be described as the formation of a first mixture. Thus, step (i) of the first process can be described as the formation of a first mixture comprising (or essentially consisting of, or derived from) water, peroxide, titanium precursor, and silica; while step (a) of the second process can be described as the formation of a first mixture comprising (or essentially consisting of, or derived from) water, hydrogen peroxide, alkali metal precursor and / or zinc precursor, titanium precursor, and silica; and step (A) of the third process can be described as the formation of a first mixture comprising (or essentially consisting of, or derived from) water, hydrogen peroxide, alkali metal precursor and / or zinc precursor, titanium precursor, and silica.

[0081] The relative amounts of components in the first step are not particularly limited, as long as no component or reaction product adversely affects the porosity of the silica support and the supported chromium catalyst in the subsequent processing steps discussed below. Generally, the molar ratio of peroxide compounds or hydrogen peroxide to titanium (e.g., H2O2:Ti) in the first step of the first, second, and third processes can be in the range of 0.5:1 to 100:1, for example, 2:1 to 50:1, 3:1 to 20:1, or 5:1 to 11:1. Additionally or alternatively, the molar ratio of alkali metals (or zinc) to titanium in the first step of the second and third processes can be in the range of 0.1:1 to 300:1, for example, 0.2:1 to 100:1, 0.5:1 to 20:1, 0.7:1 to 10:1, 1:1 to 5:1, or 1:1 to 3:1. It should be noted that excess zinc or alkali metals such as sodium may be used during the first step, but can then be washed away during subsequent steps in each process. Additionally or alternatively, in the first step of the first, second, and third processes, the weight ratio of titanium to water (Ti:H2O) may be in the range of 0.0001:1 to 0.02:1 in one embodiment, 0.001:1 to 0.02:1 in another embodiment, 0.005:1 to 0.02:1 in yet another embodiment, and 0.03:1 to 0.07:1 in yet another embodiment.

[0082] The specific titanium source or precursor used in the first step is not particularly limited. In accordance with certain aspects of the present invention, the titanium precursor may include Ti(III) compounds and / or Ti(IV) compounds. Representative and non-limiting examples of suitable titanium precursors include titanium carboxylates (e.g., titanium oxalate, titanium glycolate, titanium lactate, titanium citrate, titanium malate), titanium halides, titanium oxide, titanium hydroxide, titanium alkoxides (e.g., titanium isopropoxide, titanium n-propoxide), titanium sulfate, titanium nitrate, and titanium-oxy compounds (e.g., oxysulfate (TiOSO4), or oxynitrate (TiO(NO3)2), or oxychloride (TiOCl2), etc.). Mixtures, combinations, or two or more titanium compounds can be used as titanium precursors. In some embodiments contemplated herein, the titanium precursor may include TiOSO4, Ti(OH)4, Ti metal, Ti(OR)4, TiO(OH)2, TiO2, etc., and any mixture or combination thereof; on the other hand, in other embodiments, the titanium precursor may include TiOSO4; alternatively, Ti(OH)4; alternatively, Ti metal; alternatively, Ti(OR)4; alternatively, Ti acetylacetonate or a derivative thereof; alternatively, TiO(OH)2; or alternatively, TiO2.

[0083] When nitrogen-containing compounds are used (e.g., in the second step of the second process), exemplary and non-limiting examples include ammonia, ammonium hydroxide, alkyl-substituted ammonium hydroxide, ammonium salts, amines, alkanolamines, and, if desired, mixtures of two or more suitable nitrogen-containing substances may be used. The relative amount of the nitrogen-containing compound is not particularly limited, as long as the desired pH is reached. However, typical weight ratios of the nitrogen-containing compound (e.g., NH4OH or NH3) to titanium include 5:1 to 300:1, 10:1 to 200:1, 25:1 to 150:1, or 50:1 to 100:1.

[0084] In many cases, the pH of the first (or second) mixture in the first, second, and third processes is adjusted by the relative amounts of the titanium precursor and H2O2 (acid) to the nitrogen-containing compound and alkali metal precursor (base). Nevertheless, before subjecting the first (or second) mixture to the reaction temperature or before isolating the solid fraction, these processes may optionally further include a step of adjusting the pH of the first (or second) mixture to a range of 3–12. More often, the pH is adjusted to a range such as 3–10, 4–12, 4–10, 6–10, or 8–10.

[0085] In the first, second, and third processes, suitable silica is brought into contact to form the first mixture. In one embodiment, the silica is a pre-formed xerogel silica and may have any of the pore volume, surface area, and average particle size characteristics disclosed for the titrated silica support and the titrated chromium / silica pre-catalyst, for example, a pore volume of 0.5 to 3 mL / g and a BET surface area of ​​100 to 700 m². 2 The particle size is 15-350 μm, and the average (d50) particle size is 15-350 μm. The pre-formed silica used in the first step is not colloidal or sol, and typically contains 25% or less water / moisture by weight, more often 20% or less, 15% or less, or 10% or less water / moisture by weight, based on the total weight of the silica. The pre-formed silica is typically in powder or bead form.

[0086] In another embodiment, the silica contacted to form the first mixture is a silica hydrogel, colloid, or sol, and in such examples it may contain at least 50% by weight of water, and in some embodiments it may contain at least 60% by weight, at least 70% by weight, or at least 80% by weight of water.

[0087] In the first, second, and third processes, any reasonable amount of silica can be added to form the first mixture. In one embodiment, for example, the weight ratio of silica to water (silica:H2O) may be in the range of 0.001:1 to 1:1; in another embodiment, the weight ratio may be in the range of 0.01:1 to 0.5:1; in yet another embodiment, the weight ratio may be in the range of 0.05:1 to 0.4:1; and in yet another embodiment, the weight ratio may be in the range of 0.1:1 to 0.3:1.

[0088] Unlike other aqueous catalyst preparation procedures, as discussed herein, titanium is adsorbed onto silica in the first step of the first, second, and third processes. The adsorbed titanium is generally accompanied by a color change of the silica support—typically initially white, and changing to yellow upon adsorption of the Ti peroxo complex—and this color change is not washed away from the support in subsequent steps. The yellow color is thought to be due to the adsorption of the peroxy complex of titanium, and the color change observed during catalyst preparation is described in the following examples. Analysis of titanium on the silica and in solution before and after adsorption demonstrates that titanium is adsorbed onto the silica, usually quantitatively and reliably, as part of the catalyst preparation. If Ti is not adsorbed, for example, due to insufficient contact time, the MI potential of the final catalyst is usually low, indicating that Ti did not bind to the silica surface in the desired manner. If adsorption does not occur, the Ti can also be washed away in subsequent steps.

[0089] This step, which forms a first mixture in which titanium is adsorbed onto silica, can be carried out under any conditions suitable for titanium absorption by silica (e.g., accompanied by a color change in the silica). Any suitable temperature (e.g., room temperature) and time, and any suitable pH can be used in this step. Titanium adsorption can be determined by slurring a solid fraction (discussed further below) isolated from the first or second mixture in water, filtering the slurry, and passing a clear solution (filtrate) through the filter, often leaving a yellow solid on the filter. The color change can be measured using spectroscopic analysis of the silica solid before and after this step. The filtrate solution can then be acidified by adding 3 mL of concentrated H2SO4 to bring the pH to approximately 1, and 5 mL of 30% H2O2. This combination (acid and H2O2) will result in a deep orange color if titanium is present in the filtrate. If no color change is observed, titanium is adsorbed onto the silica. The color change of the filtrate, if any, can also be measured using spectroscopic analysis.

[0090] In the formation of the first mixture (and the second mixture) in the first, second, and third processes, an aqueous medium substantially free of hydrocarbon or alcohol solvents is generally used. For example, the first and second mixtures may contain 20% by weight or less of hydrocarbons and alcohols, for example, 10% by weight or less, 5% by weight or less, 2% by weight or less, or 1% by weight or less of hydrocarbons and alcohols.

[0091] Although not required, the second mixture in step (c) of the second process and the first mixture in step (B) of the third process are subjected to a reaction temperature in the range of 40–270°C. Other representative and non-limiting ranges for the reaction temperature include 60–260°C, 80–220°C, 40–100°C, 60–100°C, 70–100°C, or 80–100°C. These temperature ranges also include situations in which this step is carried out at a series of different temperatures, rather than a single fixed temperature within each temperature range, where at least one temperature is within each temperature range. If the preceding steps in the second and third processes are carried out at room temperature, each mixture is heated to the desired reaction temperature. In some embodiments, the reaction temperature can be controlled by heating to the boiling point of the solvent, for example, by refluxing. In other embodiments, each mixture can be heated in an autoclave or similar vessel to the reaction temperature under pressures such as 15–300 psig or 15–100 psig. Typically, this step can be easily carried out at atmospheric pressure at a reaction temperature of less than 100°C.

[0092] The duration for which each mixture is subjected to the reaction temperature is not particularly limited and can be carried out for any suitable period, which may depend greatly on the reaction temperature. In some embodiments, the duration may range from 10 minutes to 4 days or from 20 minutes to 2 days. In other embodiments, the duration may range from 1 minute to 1 hour, 30 minutes to 24 hours, or from 40 minutes to 2 hours.

[0093] In steps (ii), (d), and (C) of the first, second, and third processes, the solid fraction is isolated from either the first or second mixture, and optionally, the solid fraction is washed. Any suitable technique can be used for the first isolation of the solid fraction (e.g., removal of water), exemplary examples including filtration, sedimentation, decantation, compression, centrifugation, cyclone treatment, and hydrocyclone treatment. Two or more of these techniques can be used, and the isolation step can be carried out in batches or continuously and at any suitable temperature (e.g., 25°C to 100°C).

[0094] If washing is performed, the solid fraction is washed one or more times with any suitable washing solution. The washing solution may, but is not limited to, water, alcohol (e.g., ethanol), or mixtures thereof. For example, the solid fraction may be washed one or more times with water, and one or more times with alcohol, in any order or sequence. As with the isolation step, washing may be performed in batches or continuously and at any suitable temperature (e.g., 25°C to 100°C). Other organic solvents such as ketones or glycols may also be used for washing, either alone or in mixtures with water or other solvents. The washing step may include one or more steps in which the solid fraction is redispersed in a solution. The redispersion solution may contain filtrate, water, alcohol (e.g., ethanol), or mixtures thereof. This solution may also contain any suitable acid, such as a dilution acid such as nitric acid or acetic acid. While not wishing to be bound by theory, it is assumed that the washing step removes loosely bound titanium and alkali metal species (if present) from the surface. However, even after washing, some sodium is thought to remain "bound" or "firmly bound" to the support (or pre-catalyst) of the present invention and not be washed away. The presence of a relatively large amount of "bound" or "firmly bound" sodium is unexpected, as these high levels of sodium are normally catalyst poisons.

[0095] The drying of the solid fraction to form a titaniumated silica support can encompass a wide range of drying times, temperatures, and pressures, depending on the drying device or technique used. For example, drying times can range from 1 second to 1 day, 1 hour to 12 hours, 2 hours to 8 hours, or 0.1 to 5 seconds, and drying temperatures can range from 25°C to 200°C, 50°C to 150°C, 70°C to 120°C, or 90°C to 110°C. Drying pressure can be atmospheric pressure or near atmospheric pressure, but in many cases, the drying step can be carried out under vacuum conditions at any suitable near-atmospheric pressure, such as less than 100 torr (13.3 kPa), less than 50 (6.67 kPa) torr, or less than 10 torr (1.33 kPa).

[0096] The drying step can be performed using, but is not limited to, various types of drying techniques, such as spray drying, tray drying, flash drying, freeze drying, oven drying, or microwave drying. In one embodiment, the drying step includes spray drying, while in another embodiment, the drying step includes flash drying.

[0097] An exemplary process for preparing a titrated silica support may include the following steps: (1) combining water, silica, and a sodium precursor (e.g., a sodium salt); (2) adding hydrogen peroxide; (3) adding a titanium precursor (e.g., TiOSO4) to form a first mixture which may have a red color due to the formation of a Ti-peroxy complex under acidic conditions; (4) adding a nitrogen-containing compound (e.g., NH4OH) to form a second mixture whose color may change from red to pale yellow; (5) subjecting the second mixture to a reaction temperature of 90°C for 30 minutes to 1 hour until the color changes from pale yellow to colorless (indicating that titanium has been adsorbed onto the silica); (6) separating the solid fraction from the second mixture by filtering and washing the solid fraction to remove ammonium and excess sodium; and (7) spray-drying the solid fraction to form a titrated silica support. While we do not wish to be bound by theory, the use of peroxide compounds is considered beneficial for retaining titanium in solution, alkali metals further enhance the HLMI potential, nitrogen compounds adjust the pH, and the reaction temperature shortens the process duration without compromising the HLMI potential.

[0098] Process for manufacturing chromium titanide silica catalyst Aspects of the present invention also cover processes for preparing chromium titanate / silica pre-catalysts and chromium titanate / silica catalysts. One such process for preparing a chromium titanate / silica pre-catalyst may include performing one of the processes for preparing a titanium titanate support disclosed above (e.g., the first process, the second process, or the third process) and contacting a chromium precursor with the first or second mixture in any step prior to the step of isolating a solid fraction from the first or second mixture. Another process for preparing a chromium titanate / silica pre-catalyst may include performing one of the processes for preparing a titanium titanate support disclosed above and contacting a chromium precursor with the solid fraction after isolating a solid fraction from the first or second mixture (this contact may be performed before or after drying the solid fraction). For example, after drying to form a titanium titanate support (dried), the chromium precursor may be contacted with the titanium titanate support (e.g., wet or dry mixing) and optionally dried as needed. In yet another process, a chromium / silica pre-catalyst (pre-formed) is used instead of silica, and in this embodiment, the process for preparing the titrated chromium / silica pre-catalyst may include performing any of the processes for preparing the titrated silica support disclosed above (e.g., the first process, the second process, or the third process), but instead of contacting silica to form the first mixture, the chromium / silica pre-catalyst is contacted to form the first mixture. Thus, the first process for preparing the titrated silica support can be rephrased as the process for preparing the titrated chromium / silica pre-catalyst and would include the following steps: (i) contacting water, a peroxide compound, a titanium precursor, and a chromium / silica pre-catalyst (under conditions sufficient for titanium to adsorb onto the chromium / silica pre-catalyst) to form the first mixture; (ii) isolating a solid fraction from the first mixture; and (iii) drying the solid fraction to form the titrated chromium / silica pre-catalyst.Titanide chromium / silica precatalysts manufactured according to any of these processes are within the scope of this disclosure and are incorporated herein.

[0099] A chromium titanate / silica precatalyst can be formed using any suitable chromium source or chromium precursor. In accordance with certain aspects of the present invention, the titanium precursor may include chromium(II) compounds, chromium(III) compounds, or any combination thereof. Exemplary and non-limiting examples of chromium(II) compounds include chromium(II) acetate, chromium(II) chloride, chromium(II) bromide, chromium(II) iodide, chromium(II) sulfate, and combinations thereof. Similarly, exemplary and non-limiting examples of chromium(III) compounds include chromium(III) carboxylate, chromium(III) naphthenate, chromium(III) halides, chromium(III) sulfate, chromium(III) nitrate, chromium(III) dione, and combinations thereof. In some aspects, the chromium precursor may include chromium(III) acetate, chromium(III) acetylacetoneate, chromium(III) chloride, chromium(III) bromide, chromium(III) sulfate, chromium(III) nitrate, and combinations thereof.

[0100] In one embodiment, the chromium precursor may include chromium trioxide, chromium acetate, chromium hydroxyacetate, chromium nitrate, or any combination thereof; on the other hand, the chromium precursor may include chromium trioxide; alternatively, chromium acetate; alternatively, chromium hydroxyacetate; or alternatively, chromium nitrate.

[0101] While not essential, depending on which step of the process is the chromium incorporation step, it may be beneficial for the chromium precursor to be soluble in a suitable solvent such as an alcohol. Similarly, and again not essential, depending on which step of the process is the chromium incorporation step, it may be beneficial for the chromium precursor compound to be water-soluble.

[0102] The resulting chromium titanide / silica pre-catalyst can be converted into a chromium titanide / silica catalyst via a suitable activation step (often referred to as a calcination step). Therefore, typical processes for producing a chromium titanide / silica catalyst may include performing any of the processes disclosed above for preparing a chromium titanide / silica pre-catalyst, and activating the chromium titanide / silica pre-catalyst to form an activated chromium titanide / silica catalyst. Furthermore, any chromium titanide / silica pre-catalyst produced according to these processes is within the scope of this disclosure and is incorporated herein.

[0103] The activation step can generally be carried out at various temperatures and for a period of time, selected to convert all or most of the chromium to hexavalent chromium. Typical peak activation temperatures include the following representative ranges: 400°C–900°C, 500°C–850°C, 600°C–800°C, 600°C–700°C, etc. In these and other embodiments, these temperature ranges also include cases where the activation step is carried out at a series of different temperatures (e.g., initial temperature, peak temperature) rather than a single fixed temperature within each range. For example, the activation step may start at the initial temperature and then the temperature of the activation step may be increased to a peak temperature, for example, in the range of 500°C–850°C or 600°C–800°C.

[0104] The duration of the activation step is not limited to any specific period. Therefore, this activation step can be performed for a period ranging from, for example, about one minute to 12 to 24 hours or more. The appropriate activation time may depend, for example, on the initial / peak temperature, among other variables. However, generally, the activation step can be performed for a period ranging from 1 minute to 24 hours, 1 hour to 12 hours, 2 hours to 8 hours, or 2 hours to 6 hours.

[0105] Catalyst activation is typically carried out in an oxidizing atmosphere, which may include air, O2, N2O, NO2, or NO, and any mixture or combination thereof. In some embodiments, the activation atmosphere may include air (e.g., dry air), and in other embodiments, the atmosphere may include a mixture of air and nitrogen. If desired, the chromium titanate / silica catalyst may be reduced using CO or a suitable hydrocarbon. Activation can also be achieved by first exposing the catalyst to a non-oxidizing atmosphere and then to an oxidizing atmosphere, as described in U.S. Patent No. 11,149,098. Any suitable activation vessel can be used for the activation step and can be carried out in batch or continuously. For example, fluidized bed, tray, dropper, and fixed-bed vessels and related techniques can be used for the activation step. [Examples]

[0106] The present invention is further illustrated by the following embodiments, but these embodiments should not be construed as limiting the scope of the invention in any way. After reading this description, various other embodiments, modifications, and equivalents thereof can be suggested to those skilled in the art without departing from the spirit of the invention or the appended claims.

[0107] Titanium precursor. Approximately 35 g of tetraisopropoxytitanium solution was added to 200 mL of water and stirred for 30 minutes. Then, the water was removed using a rotary evaporator, and the resulting hydrated TiO2 was dissolved in an oxalic acid solution with a molar ratio of oxalic acid to titanium of 2:1. This solution is referred to herein as TiO2-OA. Other titanium precursors were tetraisopropoxytitanium and titanium(IV) oxysulfate solutions, which were used without further purification.

[0108] General procedure for aqueous titaniumization of silica support and preparation of pre-catalyst. An alkali metal salt was dissolved in water to form an alkaline solution of approximately 0.17 M. Hydrogen peroxide solution was then added to this alkaline solution and stirred for several minutes. Next, a titanium precursor was added in an alkali metal:titanium molar ratio ranging from 0.7:1 to 1.9:1 to form a homogeneous solution. Then, ammonium hydroxide solution was added to adjust the pH to a desired value in the range of 4 to 10. Finally, a pore volume of 1.6 mL / g and 500 m³ were prepared. 2 The required amount of pre-formed silica A (typically 5 g) having a BET specific surface area of ​​1 / g and a d50 average particle size of 80 μm was added, and the pH was readjusted with additional ammonium hydroxide solution as needed. The mixture was then heated to the desired temperature (typically 100°C under reflux conditions) for a predetermined time (typically 1 hour). The resulting mixture was filtered by suction through glass frit and washed with water and ethanol. The resulting titanated silica support was then dried at room temperature. Chromium(III) acetate hydroxide (CrOAc) dissolved in methanol was added to the dried titanated silica, and the mixture was dried at room temperature to deposit approximately 1 wt% chromium, forming a titanated chromium / silica pre-catalyst.

[0109] Catalyst activation. The above pre-catalyst was heated to 650°C at a rate of 4°C / min while flowing dry air at a rate of 0.57-0.75 L / min (1.2-1.6 scfh) in an activation tube with a diameter of 4.87 cm (1.88 inches) and held at 650°C for 3 hours to obtain the final titaniumated Cr(VI) / SiO2 catalyst.

[0110] Polymerization experiment. The polymerization test was carried out in a 2.65 L stainless steel reactor equipped with a marine-type agitator rotating at 500 rpm. The reactor was enclosed in a steel jacket, and the reaction temperature was controlled by circulating water throughout the jacket, being heated and cooled by a heat exchanger with high temperature (steam) and low temperature (plant water). First, a small amount of activated catalyst (0.05-0.10 g) was added to the reactor under dry nitrogen. Next, 1.2 L of isobutane liquid was added, and the reactor was heated to a set temperature of 105 °C. Then, ethylene was added to the reactor and maintained at 3.79 MPa (550 psig) throughout the entire experiment. The reaction was continued until a production capacity of approximately 3000 g of polyethylene per gram of catalyst was reached, measured by a flow controller that measured the flow of ethylene into the reactor. Once the target production capacity was achieved, the time was recorded, the ethylene flow was stopped, the reactor was cooled, the pressure was reduced, and the granular polymer powder was recovered. The dried powder was weighed, and the catalytic activity was quantified as the amount of polymer produced per gram of solid catalyst added per hour (g / g / hour).

[0111] The melt index (MI, g / 10 min) was determined according to ASTM D1238, using 2.16 kg of catalyst at 190°C. 10 (g / 10 min) was determined according to ASTM D1238 using 10 kg of catalyst at 190°C, and the high-load melt index (HLMI, I) was determined. 21 The density (g / cm³) was determined according to ASTM D1238 at 190°C using 21.6 kg of catalyst. The density was determined according to ASTM D1505 and ASTM D4703 on a compression molded sample cooled at 15°C per minute and conditioned at room temperature for 40 hours, in grams per cubic centimeter (g / cm³). 3 It can be determined in units of )

[0112] Molecular weight and molecular weight distribution can be obtained by operating a PL-GPC220 system (Polymer Labs, Agilent) equipped with an IR4 detector (Polymer Char, Slain) and three Styragel® HMW-6E GPC columns (Waters, MA) at 145°C. The mobile phase 1,2,4-trichlorobenzene (TCB) containing 0.5 g / L of 2,6-di-t-butyl-4-methylphenol (BHT) is set to a flow rate of 1 mL / min, and the polymer solution concentration ranges from 1.0 to 1.5 mg / mL depending on the molecular weight. Sample preparation is carried out at 150°C for a nominal 4 hours with occasional gentle stirring, after which the solution is transferred to a sample vial for injection. An injection volume of 200 μL is used. Molecular weight and molecular weight distribution are derived using the integral calibration method, with MAREX® BHB5003, an HDPE polyethylene resin from Chevron Phillips Chemical Company, as a broad standard. The integral tables for a wide range of standard materials are pre-determined in separate experiments using SEC-MALS. Mn is the number-average molecular weight, Mw is the weight-average molecular weight, Mz is the z-average molecular weight, Mv is the viscosity-average molecular weight, and Mp is the peak molecular weight (the position of the highest point on the molecular weight distribution curve).

[0113] Melt rheological characterization can be performed as follows: Using an Anton Paar MCR rheometer with parallel plate geometry, small strain (less than 10%) vibrational shear measurements are performed. All rheological tests are performed at 190°C. Then, the complex viscosity |η*| versus frequency (ω) data are curve-fitted using a modified 3-parameter Carreau-Yasuda (CY) empirical model, with zero shear viscosity -η0 and characteristic viscosity relaxation time -τ. η And the width parameter a (CY-a parameter) is determined. The simplified Carreau-Yasuda (CY) empirical model is as follows.

number

[0114] For details on the significance and interpretation of the CY model and derived parameters, please refer to: CA Hieber and HH Chiang, Rheol. Acta, 28, 321 (1989); CA Hieber and HH Chiang, Polym. Eng. Sci., 32, 931 (1992); and RB Bird, RC Armstrong and O. Hasseger, Dynamics of Polymeric Liquids, Volume 1, Fluid Mechanics, 2nd Edition, John Wiley & Sons (1987).

[0115] The metal content, including the amounts of alkali metals, titanium, and chromium present on the catalyst, was determined by ICP analysis using a PerkinElmer Optima 8300 instrument. The samples were ashed overnight in a Thermolyne furnace using sulfuric acid, followed by acid decomposition in a HotBlock with HCl and HNO3 (3:1v:v).

[0116] Examples 1-15 Table 1 summarizes comparative polymerization experiments using varying titanium loads and sources / precursors, but without the use of alkali metals during catalyst preparation. In Example 1, 0.21 g of CrOAc dissolved in 5 mL of methanol was added to 5 g of pre-formed silica A, dried at room temperature (RT), and activated in a fluidized bed at 650 °C in a stream of dry air for 3 hours.

[0117] In Example 2, 2.22 g of TiOSO4 was added to 20 mL of water containing 2.5 g of 35 wt% H2O2 solution and homogenized by stirring. Next, ammonium hydroxide was added to increase the pH of the solution to 10. Then, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0118] In Example 3, 0.60 g of Ti(OiPr)4 was added to 20 mL of water containing 2.5 g of 35 wt% H2O2 solution and homogenized by stirring. Next, ammonium hydroxide was added to increase the pH of the solution to 10. Then, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0119] In Examples 4-5, 0.25 g (for 5 wt% Ti) or 0.50 g (for 10 wt% Ti) of titanium metal powder was added to a mixture containing 20 g of 30 wt% H2O2 and 5 g of NH4OH solution, and the mixture was stirred to homogenize it (typically for 1.5-2 hours). Then, additional ammonium hydroxide was added to increase the pH of the solution to 10. Next, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Then, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0120] In Examples 6-11, the amount added varied from 1.7 mL (for 1% Ti) to 17 mL (for 10% Ti) depending on the concentration of the prepared TiO2-OA solution. The amount of 35% H2O2 added varied from 1.1 g to 10.3 g, and except for Example 6, the H2O2 / Ti molar ratio was approximately 10.1-10.8. Next, ammonium hydroxide was added to increase the pH of the solution to 10. Then, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0121] In Examples 12-15, a mixture containing 50 mL of H2O, 2.5 g of 35 wt% H2O2, and a complexing agent consisting of 0.50 g of glycolic acid (Example 12), 0.50 g of lactic acid (Example 13), 0.89 g of citric acid (Example 14), or 0.53 g of oxalic acid (Example 15) was prepared, to which 0.60 g of Ti(OiPr)4 was added. Ammonium hydroxide was then added to increase the pH of the solution to 10. Next, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0122] In Examples 2-15 of Table 1, the amount of Ti supported was varied within the range of 1-10% by weight by varying the amount of Ti source added. The pre-catalyst was prepared at pH 10 and heated at 100°C under reflux for 1 hour. The activated catalyst showed an increase in HLMI potential with increasing Ti support, but a high Ti support of 7-10% by weight was required for the HLMI value to exceed 30. [Table 1]

[0123] Examples 16-27 Table 2 summarizes catalyst preparation and polymerization experiments using TiO2-OA as the titanium source / precursor and Na2SiO3 during catalyst preparation, with varying amounts of titanium supported (the molar ratios of H2O2 / Ti and Na / Ti are listed in Table 2). In Examples 16-27, 0.55-2g of Na2SiO3 was added to a solution containing 10mL of water, 1-16.6g of 35 wt% H2O2, and 5g of ammonium hydroxide. After stirring for several minutes, TiO2-OA solution (the amount varied from 3.3g for 2 wt% Ti to 15.33g for 9 wt% Ti, depending on the concentration of the prepared solution) was added. Next, 5g of pre-formed silica A was added, the pH was adjusted to 10 as needed, and the mixture was heated under reflux at 100°C for 1 hour. The actual amounts of Na2SiO3, H2O2, and silica in grams are summarized in Table 2. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650 °C in a dry air stream for 3 hours. Polymerization experiments in Table 2 revealed that the HLMI potential increased 2 to 3 times compared to catalysts prepared without a sodium source (see Examples 6-11 in Table 1), indicating a beneficial and unexpected role of adding sodium during catalyst preparation. [Table 2]

[0124] Examples 28-41 Table 3 summarizes catalyst preparation and polymerization experiments using TiOSO4 solution as the titanium source / precursor, utilizing NaHCO3 or NaCl during catalyst preparation (other sodium precursors such as sodium carbonate can also be used), and varying the amount of titanium supported. In Examples 28-35, 0.05 g (Example 30), 0.14 g (Example 29), 0.29 g (Examples 28 and 32-35), 0.58 g (Example 31), or 0.29 g (Example 28) of NaHCO3 was dissolved in 20 mL of water. Then, 2.5 g of 35 wt% H2O2 (for Examples 28-32), 1.1 g of 35 wt% H2O2 (for Example 33), 4 g of 35 wt% H2O2 (for Example 34), or 5.8 g of 35 wt% H2O2 (for Example 35) was added. Next, TiOSO4 (approximately 1.1 g for 1 wt% Ti, 2.2 g for 2 wt% Ti, 4 g for 3.5 wt% Ti, and 5.8 g for 5 wt% Ti) was added. Then, ammonium hydroxide was added to increase the pH of the solution to 10. Next, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0125] In Examples 36-41, 0.05 g (Example 36), 0.10 g (Example 37), 0.20 g (Example 38), 0.35 g (Example 39), 0.50 g (Example 40), or 0.80 g (Example 41) of NaCl was dissolved in 20 mL of water. Then, 0.5 g (Example 36), 1.0 g (Example 37), 2.0 g (Example 38), 3.5 g (Example 39), 5.0 g (Example 40), or 8.0 g (Example 41) of 35 wt% H2O was added. Then, TiOSO4 (approximately 0.55 g for 0.5 wt% Ti, approximately 1.1 g for 1 wt% Ti, 2.2 g for 2 wt% Ti, 3.9 g for 3.5 wt% Ti, 5.8 g for 5 wt% Ti, and 9.3 g for 8 wt% Ti) was added. Next, ammonium hydroxide was added to increase the pH of the solution to 10. Then, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0126] The polymerization experiments in Table 3 surprisingly show that HLMI values ​​exceeding 30 were easily achieved with as little as 2% by weight of titanium under various catalyst preparation conditions. ICP composition analysis is also summarized in Table 3. This information is shown graphically in Figure 1, which plots the HLMI of the polymer against the number of titanium atoms per square nanometer for the control chromium titanate / silica catalyst and the chromium titanate / silica catalysts of Examples 28-41.

[0127] The control catalyst in Figure 1 is 480m 2Preparations were made from silica having a surface area of ​​1 / g, a pore volume of 1.67 mL / g, and an average particle size of 75 μm. Ten grams of this silica sample was placed in a muffle furnace at 200°C for 12 hours. These silica samples were then captured in airtight bottles while the silica was still hot. The silica samples were then slurryed with dry isopropyl alcohol, followed by the addition of titanium isopropoxide with constant stirring for 1 hour, and then a methanol solution of basic chromium acetate was added, resulting in 1 wt% chromium per catalyst. The slurry was dried under vacuum at 100°C for 2 hours. Titanium isopropoxide was added in amounts corresponding to a target range of 0.25 wt% to 8 wt% based on the weight of the silica. Silica surface area (m²) 2 / g) using nm 2 Convert these weight percentages to the number of Ti atoms / nm 2 By converting to this, the control line in Figure 1 was obtained (for example, 2 wt% titanium is 0.52 Ti / nm). 2 (That is.)

[0128] In Figure 1, the present invention set 1 consists of Examples 36-41, and the present invention set 2 consists of Examples 28-35. In these examples, the surface area is 500 m². 2 / g (2% by weight of titanium is 0.50Ti / nm) 2 (This is the case.) At equivalent titanium loads, the chromium titranide / silica catalysts of Examples 36-41 showed significantly higher HLMI values ​​compared to the control, with an unexpected increase of approximately 18-100% for the same titanium load. At lower titanium loads (e.g., 1-2 wt% titanium), Invention Set 2 also showed significantly higher HLMI values ​​compared to the control, with an unexpected increase of approximately 60-90%. Examples of Invention Set 2 with higher titanium loads were comparable to the control; this is due to the lower Na / Ti molar ratio, and it is thought that the HLMI values ​​would have been even higher with a higher ratio. [Table 3]

[0129] Examples 42-46 Table 4 summarizes catalyst preparation and polymerization experiments using Ti(OiPr)4 and complexing acids as titanium sources / precursors, and utilizing NaCl during catalyst preparation to maintain a constant titanium load. In Examples 42-46 (compared to Examples 3 and 12-15), 0.2 g of NaCl was dissolved in 50 mL of water. Next, 2.5 g of 35 wt% H2O2 and the complexing agents 0.50 g of glycolic acid (Example 44), 0.50 g of lactic acid (Example 43), 0.89 g of citric acid (Example 45), or 0.53 g of oxalic acid (Example 46) were added and dissolved. Then, 0.60 g of Ti(OiPr)4 was added, and the pH of the solution was increased to 10 by adding ammonium hydroxide. The molar ratios of H2O2 / Ti and alkali / Ti were 12.3:1 and 1.64:1, respectively. Next, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Then, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0130] Polymerization experiments in Examples 42-46 of Table 4 demonstrated that HLMI values ​​of 32-45 could be easily achieved with just 2% by weight of titanium, whereas in Comparative Examples 3 and 12-15, polymers with HLMI values ​​of only 11-15 were produced. [Table 4]

[0131] Examples 47-54 Table 5 summarizes catalyst preparation and polymerization experiments using various titanium loads when TiO2-OA was used as the titanium source / precursor and NaOH was utilized during catalyst preparation. In Examples 47-54, 20 mL of water containing 2.5 g of 35 wt% H2O2 and 3.3 g of TiO2-OA solution (2 wt% Ti in Examples 47-51 and 54) or 5.9 g of TiO2-OA solution (3.5 wt% Ti in Examples 52-53) was mixed with 1 N NaOH solution in the amounts shown in Table 5. Next, in Examples 47-53, ammonium hydroxide was added to increase the pH of the solution to 10. In Example 54, ammonium hydroxide was not added; the pH was increased to 10 using 1 N NaOH solution. Then, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried with RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0132] As shown in Table 5, the HLMI values ​​of polymers produced from the titrated chromium / silica catalyst increased with increasing Na content during catalyst preparation (see Examples 47-51). Although Example 54 did not exhibit polymerization activity, and we do not wish to be bound by theory, ammonium hydroxide is thought to play an important role in both increasing pH and assisting / improving titanium uptake (more effective titration). [Table 5]

[0133] Examples 55-57 Table 6 summarizes catalyst preparation and polymerization experiments using a constant titanium load and TiO2-OA titanium source / precursor, with different sodium sources used during catalyst preparation. In Examples 55-57, 20 mL of water containing 2.5 g of 35 wt% H2O2 and 3.3 g of TiO2 solution (in the case of 2 wt% Ti) was to be mixed with 0.29 g of NaHCO3 in Example 55, 0.26 g of NaOAc in Example 56, or 0.23 g of Na2C2O4 in Example 57, as shown in Table 6. Next, ammonium hydroxide was added to increase the pH of the solution to 10. Then, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried with RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0134] The polymerization experiments in Examples 55-57 in Table 6 demonstrate that an HLMI value of 30-40 was easily achieved with just 2% by weight of titanium, regardless of the alkali metal source / precursor. [Table 6]

[0135] Examples 58-68 Table 7 summarizes the catalyst preparation and polymerization experiments using potassium salts, and Table 8 summarizes the catalyst preparation and polymerization experiments using lithium salts. The pre-catalyst was prepared using ammonium hydroxide at a pH of 10, heated under reflux at 100°C for 1 hour, and the titanium source / precursor was TiO2-OA. For Examples 58-62, 2.5 g of 35 wt% H2O2 was added to 20 mL of water, and TiO2-OA solution (3.3 g for 2 wt% Ti in Examples 58 and 60-62, and 8.52 g for 5 wt% Ti in Example 59) was added. Next, 3.5 mL of 1N KOH solution (for Examples 58-59), or 1.9 mL of 1N KOH (for Example 60), or 2.8 mL of 1N KOH solution (for Example 61), or 0.24 g of K2CO3 (for Example 62) was added. Then, ammonium hydroxide was added to increase the pH of the solution to 10. Next, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Then, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a stream of dry air for 3 hours.

[0136] In Examples 63-68, the following amounts of 20 wt lithium polysilicate solution were added to 50 mL of water containing 2.5 g of 35 wt% H2O2 and 5 g of NH4OH: 0.71 g (Example 63), 1.64 g (Example 64), 2.50 g (Example 65), 3.30 g (Example 66), 4.20 g (Example 67), and 5.0 g (Example 68). Next, 3.3 g of TiO2-OA solution equivalent to 2 wt% Ti was added, and ammonium hydroxide was added as needed to increase the pH of the solution to 10. Then, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650°C in a dry air stream for 3 hours.

[0137] The polymerization experiments in Examples 58-68 in Tables 7-8 unexpectedly demonstrate that, using potassium and lithium during catalyst preparation, polymers with HLMI values ​​exceeding 30 were produced in a similar manner to sodium, with only 2 wt% titanium. Tables 7-8 also summarize the analysis results of the ICP composition of the activated titrated chromium / silica catalyst: chromium 0.78-0.92 wt%, titanium 0.9-3 wt%, potassium 0.4-0.8 wt%, and lithium 0.03-0.2 wt%. [Table 7] [Table 8]

[0138] Examples 69-78 Table 9 summarizes the effect of temperature on aqueous titration, using either NaOH or sodium silicate as the alkali metal source / precursor, with a Ti loading of either 2 wt% or 5 wt%. The catalyst mixture was heated at different temperatures from RT to reflux conditions (100°C). The H2O2 / Ti molar ratios were 32.7:1 and 12.3:1 for 5 wt% and 2 wt% Ti loadings, respectively. Similarly, the alkali / Ti molar ratios were 0.59:1 and 1.58:1 for 5 wt% and 2 wt% Ti loadings, respectively. The Ti source / precursor was TiO2-OA. The melt index potential of chromium titanate / silica catalysts prepared at low temperatures can be improved by reacting the catalyst mixture for a longer time before separating the liquid and solid and then drying.

[0139] In Examples 69-73, 1 g of sodium silicate solution was added to 20 mL of water containing 16.6 g of 35 wt% H2O2 and 5 g of NH4OH. Then, 8.5 g of TiO2-OA solution equivalent to 5 wt% Ti was added, and ammonium hydroxide was added as needed to increase the pH of the solution to 10. Next, 5 g of pre-formed silica A was added, and the mixture was heated at the temperature shown in Table 9 for the period. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Then, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650 °C in a stream of dry air for 3 hours.

[0140] In Examples 74-78, 33 mL of 0.1 NNaOH solution was added to 17 mL of water containing 2.5 g of 35 wt% H2O2, followed by 3.3 g of TiO2-OA solution equivalent to 2 wt% Ti. Ammonium hydroxide was then added to increase the pH of the solution to 10. Next, 5 g of pre-formed silica A was added, and the mixture was heated at the temperatures shown in Table 9 for the specified period. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried at RT, and activated in a fluidized bed at 650 °C in a stream of dry air for 3 hours. [Table 9]

[0141] Examples 79-84 Table 10 summarizes the effect of pH on aqueous titration using NaOH as the alkali metal source / precursor and a Ti loading of 2 wt%. pH was varied in the range of 4–10 in the presence of sodium hydroxide and ammonium hydroxide. Notably, all chromium titanate / silica catalysts exhibited an HLMI potential encompassing the commercially relevant range of 25–40, with only slight titanium leaching observed at lower pH levels (e.g., pH range of 4–6). Leaching could be determined by ICP analysis of the filtrate or by the addition of hydrogen peroxide to the filtrate, which resulted in a color change. The H₂O₂ / Ti molar ratio was 12.3:1, and the alkali / Ti molar ratio was 1.58:1. The Ti source / precursor was TiO₂-OA.

[0142] In Examples 79-84, 33 mL of 0.1 N NaOH solution was added to 17 mL of water containing 2.5 g of 35 wt% H2O2, followed by the addition of 3.3 g of TiO2-OA solution equivalent to 2 wt% Ti. Ammonium hydroxide was then added to increase the pH of the solution to 4 (Example 84), 6 (Example 83), 7 (Example 82), 8 (Example 81), 9 (Example 80), and 10 (Example 79). Next, 5 g of pre-formed silica A was added, and the mixture was heated under reflux at 100°C for 3 days in Example 84, 21 hours in Example 83, 15 hours in Example 82, 2 hours in Examples 80-81, and 1 hour in Example 79. Therefore, 1-2 hours may be sufficient for pH ranges of 8-10, but longer times are required for lower pH values ​​in the range of 4-8. Unexpectedly, it should be noted that a neutral pH of 7 can be used upon request.

[0143] The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, and dried at room temperature. Next, 0.21 g of CrOAc dissolved in 5 mL of methanol was added, dried with RT, and activated in a fluidized bed at 650 °C in a stream of dry air for 3 hours. [Table 10]

[0144] Examples 85-86 Table 11 demonstrates that chromium can be added together with titanium, rather than being supported during the final stage of catalyst preparation, and this results in the same beneficial improvements in polymer HLMI. In Examples 85-86, 0.20 g of chromium(III) acetate hydroxide was dissolved in 20 mL of water, and then either 33 mL of 0.1 N NaOH solution (for Example 85) or 0.29 g of NaHCO3 (for Example 86) was added. Next, 2.5 g of 35 wt% H2O2 was added, followed by 3.3 g of Ti2-OA solution equivalent to 2 wt% Ti (for Example 85) or 2.2 g of TiOSO4 equivalent to 2 wt% Ti (for Example 86), and NH4OH was added to adjust the pH of the mixture to 10. After stirring for several minutes, 5 g of pre-formed silica A was added and the mixture was heated under reflux at 100°C for 1 hour. The catalyst was then filtered and washed with water and ethanol. The dried catalyst was activated in a fluidized bed in dry air at 650°C for 3 hours. [Table 11]

[0145] Examples 87-88 In Examples 87-88, 1 g of Na2SiO3 was added to a solution containing 10 mL of water, 16.6 g of 35 wt% H2O2, and 5 g of ammonium hydroxide. After stirring for several minutes, TiO2-OA solution was added, followed by 5 g of 0.5 wt% chromium / silica catalyst. The pH was adjusted to 10 as needed, and the mixture was heated under reflux at 100°C for 1 hour. The gram amounts of Na2SiO3, H2O2, and SiO2 are shown in Table 12. The solid was filtered at high temperature by suction filtration through glass frit, washed with water and ethanol, dried in RT, and then activated in a fluidized bed under a dry air stream at 650°C for 3 hours. Polymerization experiments using the catalyst of Example 87 revealed a lower HLMI potential (approximately 20 HLMI) compared to the chromium titanate / silica catalyst prepared using silica starting material (see Example 18 in Table 12) under similar conditions. While we do not wish to be bound by theory, the lower HLMI potential in Example 87 may be due to a variety of factors, including a smaller pore volume in the support and a lower chromium load (0.5 wt%). In titaniumization without sodium silicate using 0.5 wt% chromium / silica catalyst (Example 88), the HLMI potential was only 11.5, once again demonstrating the important role of alkali metals in effective titaniumization. [Table 12]

[0146] Examples 89-107 With the exception of zinc, Table 13 shows that during aqueous titration, divalent and trivalent metal ions do not offer the same advantages as alkali metals, which can form chromium / silica titration catalysts with an HLMI potential of approximately 30–50. Divalent metal cations including Mg (Example 89), Ba (Examples 90–92), Sr (Examples 93–97), and Zn (Examples 98–102, 107A–107B), as well as trivalent metal cations including B (Examples 103–105) and Al (Example 106), were tested. Hydroxides of Ba and Sr were sparingly soluble. MgSO4, Zn(NO3)2, H3BO3, and AlCl3 were used as sources for Mg, Zn, B, and Al, respectively (see Table 13). The Ti loading in these examples was 2% by weight, and the H2O2 / Ti molar ratio was 12.3:1. The resulting chromium titanate / silica catalysts were active but generally exhibited low HLMI potentials, mostly in the range of 10–15. An exception was the zinc examples 107A–107B (HLMI value approximately 30), where 0.5 g of ammonium sulfate was added in addition to increasing the pH to approximately 10 by adding ammonium hydroxide. [Table 13]

[0147] Examples 108-122 In Examples 108-122, the amount of sodium was varied. First, 25g of water, 1-4g of H2O2 (30-35%), and 1-4g of TiOSO4 solution were mixed in the H2O2 / Ti molar ratios listed in Table 14. Then, sodium hydroxide, or NaNO3, or a combination of both, was added as a sodium source to reach the listed Na / Ti ratios. Subsequently, an ammonium source (ammonium hydroxide, ammonium sulfate, or ammonium carbonate) was added. Depending on the ammonium and sodium sources, the pH of the final mixture ranged from 4 to 10.5. In Examples 114-116, NH4 was 1.92. +Maintaining a constant ratio of sodium / Ti, and without measuring pH, in Example 121, the ammonium source was ammonium carbonate. Next, 5 g of pre-formed silica A was added to the above solution and refluxed at 100°C for 1 hour. The slurry color changed from yellow to colorless or faintly yellow. The support was filtered, washed with water and ethanol, and 5 mL of chromium(III) acetate (1 mg Cr / mL) in methanol was added, and it was dried at room temperature. Activation was carried out at 650°C for 3 hours, and the polymerization results are shown in Table 14. Unexpectedly, high polymer HLMI values ​​were obtained even at very high levels of sodium (Na / Ti) (see also Table 5 above). [Table 14]

[0148] Examples 123-130 Examples 123-130 were carried out without the use of ammonium hydroxide and are summarized in Table 15. Sodium silicate was mixed with 40 g of water and 2-4 g of H2O2 (30-35%), then 2-4 g of TiOSO4 solution was added. Except for Example 126, potassium titanium oxalate was used as the titanium source, and the pH was adjusted to 6.7 with dilute HCl before silica addition. In Examples 123-127, the sodium source was a mixture of sodium silicate and NaOH, while in Examples 128-130, the sodium source was a mixture of NaOH and NaNO3. Next, 5 g of pre-formed silica A was added to the above solution and refluxed at 100°C for 1-3 hours. The yellow color of the slurry remained the same throughout the preparation. The support was filtered, washed several times with water, chromium(III) acetate in methanol was added, and it was dried at room temperature. In Example 127, the filtered support was redispersed in 500 mL of deionized water, and excess sodium was removed by adjusting the pH with an acid (nitric acid or acetic acid). Activation was carried out at 650°C for 3 hours, and the polymerization results are shown in Table 15. Unexpectedly, ammonium hydroxide was not required to achieve a very high polymer HLMI value. [Table 15]

[0149] Examples 131-143 Examples 131-143 were carried out using sodium hydroxide and various organic acids and bases (e.g., amines, tert-ammonium organic hydroxide, amino acids, glycols, hydroxy acids). The pH of the mixture was adjusted with either an organic acid, a base, or sodium hydroxide. Example 131 was prepared by mixing 50 g of H2O, 2.2 g of H2O2, and 3.5 g of TiOSO4, then adding NaOH to increase the pH to about 8.8. Next, 5 g of pre-formed silica A was added and refluxed at 100°C for 1 hour. The mixture was filtered at high temperature, washed with about 500 mL of water and about 20 mL of ethanol, and dried at room temperature. It was then dispersed in about 800 mL of water, and the pH of the solution (typically in the alkaline range of about 9) was adjusted to about 4 using dilute HNO3 or acetic acid, and stirred at room temperature for about 1 hour. It was then filtered again with about 2 L of water and about 20 mL of ethanol and dried at room temperature. Next, 5 mL of CrOAc / MeOH solution was added (initial wetting), followed by drying at room temperature and activation at 650°C for 3 hours. An organic acid or base was added in the organic / titanium molar ratio shown in Table 16. The organic compounds were tetraethylammonium hydroxide in Example 132, diethylamine in Example 133, ethanolamine in Example 134, triethanolamine in Example 135, ethylamine in Example 136, N-methyldiethanolamine in Example 137, acetamide in Example 138, glycolic acid in Example 139, glycine in Example 140, ethylene carbonate in Example 141, DMF in Example 142, and oxalic acid in Example 143. This procedure was then repeated by adjusting the pH with NaOH expressed in the form of Na / Ti molar ratio shown in Table 16. Beneficially, these examples demonstrate that various nitrogen sources can be used and very high polymer HLMI values ​​can be obtained.

[0150] Note that in Examples 131 and 141-143, the support was dispersed in a dilute nitric acid solution with a pH of approximately 3-4 and stirred for 30-60 minutes to further remove sodium from the filtered support or after the heating step. In Examples 138-139, the support was dispersed in acetic acid with a pH of approximately 3-4 and stirred for 30-60 minutes to further remove sodium from the filtered support or after the heating step. [Table 16]

[0151] Examples 144-157 Examples 144-157 were carried out using various inorganic ammonium salts such as NH4Cl, (NH4)2SO4, and (NH4)2CO3, as summarized in Table 17. First, 20 g of H2O was mixed with H2O2 and a different Ti source (titanium isopropoxide in Example 147, potassium titanyl oxalate in Example 148, ammonium titanyl oxalate in Example 149, and TiSO4 in other examples), and then NaOH and ammonium salts were added to adjust the pH to the values ​​listed in Table 17. Next, 5 g of pre-formed silica A was added and refluxed at 100°C for 1 hour. The support was filtered, washed several times with water, chromium(III) acetate in methanol was added, and it was dried at room temperature. In Examples 150-154, sodium was further removed from the filtered support or after the heating step by dispersing the support in a solution of dilute acid (nitric acid or acetic acid) at a pH of approximately 3-4 and stirring for 30-60 minutes. Activation was carried out at 650°C for 3 hours, and the polymerization results are listed in Table 17. Interestingly, in the absence of either the sodium salt (Example 157) or the ammonium salt (Example 151), the HLMI value of the catalyst was less than 6. By manipulating the concentrations of both the ammonium and sodium salts, catalysts with very high HLMI potential (HLMI values ​​of 30-50) were obtained. [Table 17]

[0152] Examples 158-195 The titaniumated supports of Examples 158-195 were prepared using a wide variety of reaction times, temperatures, concentrations, pH values, and components for aqueous titanium deposition on silica. Compared to previous examples, many of Examples 158-195 were carried out at lower pH without the use of nitrogen-containing compounds. Table 18 summarizes the results of Examples 158-195, as well as the ICP analysis (by weight %) of certain pre-catalysts and (activated) catalysts.

[0153] Example 158: 25.12 g of 15% TiOSO4 solution (containing sulfuric acid to maintain stability) was added to 50 mL of deionized water to achieve a target Ti loading of 5.0 wt%. Next, 11.0 g of Na2SO4 and 66 mL of 8.17% NaOH solution were added to obtain a total Na / Ti molar ratio of 13.16. Then, 20.0 g of silica (500 m) was added. 2 Adding sodium (1.6 mL / g, average size 100 μm), the slurry was heated to 75°C with a pH of approximately 3 and maintained at that temperature for 15 hours with stirring. To wash away the sodium, 4 L of water was added and the slurry was stirred for 1 hour. The solid was filtered off and approximately 20 mL of methanol solution of chromium(III) acetate containing 0.01 g of Cr per mL was added. The pre-catalyst was dried in a vacuum oven at 100°C for several hours and then passed through a 35-mesh screen. Finally, 10 g of this green powder was calcined in dry air at 650°C for 3 hours.

[0154] Example 159: The process of Example 158 was repeated, but without heating; only stirring was performed at 25°C for 3 days. 100 mL of water was used, and instead, 82 mL of 2.26 N NaOH stock solution was added (7.39 NaOH / Ti, 14.83 total Na / Ti, and approximately 4.5 pH). Here again, the target Ti load was 5.0% by weight.

[0155] Example 160: The same process as in Example 158 was used. 15.57 g of 15% TiiOSO4 solution was added to 100 mL of water (target Ti load of 3.47 wt%). In addition, 21.14 g of the same silica used in Example 158, 10.11 g of 30% H2O2 solution, and 11.14 g of Na2SO4 were added. This yielded a deep orange-red, almost black solution, indicating a peroxo-Ti complex. When 39 mL of 2.26 NaOH stock solution was added, the color faded to orange-yellow. Therefore, the total Na / Ti molar ratio in the slurry was 16.7. The slurry, with a pH of approximately 3.5, was then stirred at 25°C for 15 hours. At this point, the yellow color had been adsorbed onto the silica. When stirring was temporarily stopped, the silica settled to the bottom of the beaker. The silica was yellow, and the upper solution was clear and colorless, indicating that the peroxo-Ti complex had been adsorbed onto the silica from the aqueous solution. At this point, the pH was approximately 2.5. The slurry was then stirred and heated at 85°C for 2 hours. After that, it was diluted with an additional 4 L of water to wash away the sodium. After stirring for 30 minutes, the slurry was filtered, leaving a yellow solid on the filter and obtaining a clear solution that had passed through the filter. To this colorless solution, 3 mL of concentrated H2SO4 was added to acidify it to a pH of approximately 1, and 5 mL of 30% H2O2 was added. This combination (acid and H2O2) should give a deep orange color if titanium had passed through the filter. However, instead, no color change was observed. The solution remained colorless, indicating that all the Ti had indeed been adsorbed onto the silica. Finally, as shown in Example 158 above, the filtered cake was impregnated with Cr, dried, sieved, and calcined.

[0156] Example 161: The same procedure as in Example 158 was used again. 16.06 g of 15% TiOSO4 solution, 7.76 g of arginine alpha-ketogtalet (AKG), and 5 mL of 30% H2O2 were added to 199 mL of water. After dissolution, 9.21 g of Na2CO3 was added to raise the pH to approximately 9.5, and 20.2 g of the same silica used in Example 158 was added. The mixture was heated at 90°C for 7 hours with stirring. Then, it was stirred at room temperature for 3 days. First, during the heat treatment, the yellow color was adsorbed onto the silica, as described in Example 160. When stirring was temporarily stopped, the yellow silica settled at the bottom, leaving a clear, colorless solution at the top. However, after stirring at 90°C for 7 hours, the yellow color disappeared, indicating that the H2O2 decomposed in contact with AKG. Next, the support was filtered, and the liquid passing through the filter was tested for the presence of Ti using additional H2O2 and H2SO4 as described above. The solution showed no color change, indicating that no trace of Ti was found in the liquid, and therefore all the Ti remained adsorbed on the silica. The support was washed with 4 L of water acidified to approximately pH 4 using acetic acid, followed by another filtration. This was done to promote sodium removal. After the second filtration, the semi-dried support was impregnated with Cr, dried, sieved, and calcined, all as described in Example 158.

[0157] Example 162: 15.39 g of 15% TiiOSO4 solution and 5 mL of 30% H2O2 were added to 200 mL of water to prepare a dark orange solution. The orange solution turned yellow by adding 6.05 g of sodium bicarbonate to raise the pH from approximately 2 to approximately 4. Next, 20.8 g of the same silica used above was added together with 4 mL of ethylamine, and the slurry was heated at 92 °C for 4 hours. The pH after heating was approximately 6.5. The slurry was filtered, and the liquid was tested again for Ti as described above, but none were found. The solid support was washed twice with 1 L of acidified water, for example, with 2 mL of acetic acid, and filtered to remove sodium. The final support was impregnated with Cr, dried, sieved, and calcined in exactly the same manner as in Example 158 above.

[0158] Example 163: The same procedure as in Example 158 was used again. 1.1969 g of TiOSO4 powder was added to 96.06 mL of water along with 3.0 mL of 30% H2O2 and 2.01 g of Na2SO4 to prepare a dark orange solution. Then, 6.5 mL of 2.26 N NaOH stock solution was added to raise the pH to 3.6, obtaining a total molar Na / Ti ratio of 5.9. 20.02 g of silica, the same silica used in the above experiment, was added. After stirring at room temperature for 1 hour, stirring was temporarily stopped, and the yellow color settled with the silica. The yellow color was clearly adsorbed onto the silica, as evidenced by the colorless solution remaining on top of the settled yellow solid. The slurry was then heated to 80-85°C for 2 hours while stirring. The final pH was 6.0. When the slurry was filtered, a yellow solid remained on the filter, and a clear, colorless liquid passed through the filter. This liquid was acidified with H2SO4, and 2 mL of 30% H2O2 was added, but it still showed no color change, confirming that all the Ti had been quantitatively adsorbed onto the silica. Next, as described in Example 158, the solid was impregnated with Cr, dried, sieved, and calcined.

[0159] Example 164: The procedure described in Example 163 was repeated with the following changes: 105 mL of water, 1.52 g of Na2SO4, and 9.7 mL of NaOH solution were added, resulting in a total Na / Ti molar ratio of 8.9 and a pH of 7.7 (8.3 after heating). The slurry was heated at 80°C for 4 hours. Here again, the yellow color from the peroxo-Ti complex was completely adsorbed onto the silica, as indicated by precipitation and subsequently by testing the filtered colorless water with H2SO4 and H2O2.

[0160] Example 165: The procedure described in Example 163 was repeated, but with the following changes: no NaOH, 2.98 g of Na2SO4, pH 1.9, molar Na / Ti 5.6.

[0161] Example 166: 1.17 g of TiOSO4 powder, 3.03 g of Na2SO4, 3 mL of 35% H2O2, and 8.51 mL of 1.37N NH4OH solution were added to 96.6 mL of deionized water. This produced a yellow solution with a pH of 3.5. 20.1 g of silica (same grade as above) was added, and the mixture was stirred at 25°C for several minutes, causing the yellow color to be adsorbed onto the silica. After stirring the slurry at 25°C for 3 days, it was filtered, yielding a yellow solid on the filter and a clear, colorless liquid passing through. The liquid was tested for Ti using the usual method, but no Ti was detected, indicating that all of the Ti had been adsorbed onto the silica. The solid was washed with 2 L of water and stirred for 30 minutes to obtain a pH of 5. The solid was filtered again and then subjected to the following processes: Cr impregnation, drying, sieving, and calcination.

[0162] Example 167: 1.167 g of TiOSO4 powder, 3 mL of 35% H2O2, and 8 mL of 1.37N NH4OH solution were added to 98.8 mL of deionized water. This produced a yellow solution with a pH of 3.7. 20.0 g of silica (same grade as above) was added, and the mixture was stirred at 25°C for several minutes, causing the yellow color to be adsorbed onto the silica. After stirring the slurry at 98°C for 2 hours, it was filtered, yielding a yellow solid on the filter and a clear, colorless liquid passing through. The liquid was tested for Ti using the usual method, but no Ti was detected, indicating that all of the Ti had been adsorbed onto the silica. The solid was washed with 2 L of water and stirred for 1 hour. The solid was filtered again and then subjected to the following processes: Cr impregnation, drying, sieving, and calcination.

[0163] Example 168: 1.20 g of TiOSO4 powder, 3 mL of 35% H2O2, and 10 mL of Mg(OH)2 slurry (1.33 M) were added to 87.35 mL of deionized water. This produced a clear yellow solution with a pH of 4.1. 20.0 g of silica (same grade as above) was added, and the mixture was stirred at 25°C for 2 hours. The yellow color was adsorbed onto the silica. That is, when stirring was stopped, the yellow color settled with the silica, leaving a clear liquid on top. The slurry was stirred at 25°C for 15 hours and then filtered. A yellow solid was obtained on the filter, and a clear, colorless liquid passed through the filter. The liquid was tested for Ti using the usual method, but no Ti was detected, indicating that all of the Ti had been adsorbed onto the silica. The solid was washed with 2 L of water and stirred for 1 hour to obtain a pH of approximately 5. The solid was filtered again and then subjected to the same processes as above: Cr impregnation, drying, sieving, and calcination.

[0164] Example 169: 15.6 g of 15% TiiOSO4 solution, 3 mL of 35% H2O2, 13.83 g of Na2SO4, 20.25 g of MgSO4, and 50.0 mL of 2.26N NaOH were added to 108.5 mL of deionized water. This produced a clear yellow solution with a pH of 4.3. This yielded a Na / Ti molar ratio of 21.3 and a Mg / Ti molar ratio of 11.5. Next, 20.1 g of silica (the same grade as above) was added, and the slurry was heated at 92°C for 45 minutes. After sedimentation, the yellow color was adsorbed onto the silica, leaving a clear, colorless liquid with a pH above 6.2. When the slurry was filtered, a yellow solid formed on the filter, and a clear, colorless liquid passed through the filter. The liquid was tested for Ti using the usual method, but no Ti was detected, indicating that all of the Ti was adsorbed onto the silica. Next, 2 L of water with 5 mL of acetic acid added to achieve a pH of 3.7 was added, and the slurry was stirred for 30 minutes to remove the sodium. The solid was filtered off again, and then the following processes were carried out as described above: chromium impregnation, drying, sieving, and calcination.

[0165] Example 170: 15.43 g of 15% TiiOSO4 solution, 3 mL of 35% H2O2, 14.8 g of MgSO4, and 30.32 mL of 1.33 M Mg(OH)2 slurry were added to 92.3 mL of deionized water. This produced a clear yellow solution with a pH of 4.2 and a Mg / Ti molar ratio of 11.2. Next, 20.1 g of silica (same grade as above) was added, and the slurry was heated at 80°C for 5 hours. After sedimentation, the yellow color was adsorbed onto the silica, leaving a clear, colorless liquid with a pH above 5.8. When the slurry was filtered, a yellow solid formed on the filter, and a clear, colorless liquid passed through the filter. The liquid was tested for Ti using the usual method, but no Ti was detected, indicating that all of the Ti was adsorbed onto the silica. The solid was washed twice with 2 L of water, filtered, and 3 mL of acetic acid was added to achieve a pH of 3.8. In each washing stage, the slurry was stirred for 30 minutes to remove metal ions. The solid was then subjected to the finishing treatments described above: chromium impregnation, drying, sieving, and calcination.

[0166] Example 171: The procedure described in Example 164 was repeated with the following changes: 100 mL of water, 1.237 g of TiOSO4 powder, 8.56 g of Na2SO4, and 9.7 mL of NaOH solution, thereby obtaining a total Na / Ti molar ratio of 9.8. The slurry was heated at 93°C for 2.5 hours. The yellow color from the peroxo-Ti complex was completely adsorbed onto the silica, as indicated by precipitation and subsequently by testing the filtered colorless water with H2SO4 and H2O2. When the slurry was filtered, a yellow solid remained on the filter, while a colorless, clear liquid passed through the filter. This liquid was acidified with 2 mL of concentrated H2SO4, and then 2 mL of H2O2 was added. No color was produced, indicating that all the Ti had been adsorbed onto the silica. The solid was washed with 2 L of water and then subjected to the finishing treatments shown above, i.e., Cr impregnation, drying, sieving, and calcination at 650°C.

[0167] Example 172: In this preparation, 2.417 g of TiOSO4 powder was dissolved in 229.3 mL of deionized water, 6 mL of 35% H2O2, 6.5 mL of 2.26 N NaOH stock solution, and 4.045 g of Na2SO4. This resulted in a Na / Ti molar ratio of 4.9. Next, 40.0 g of silica of the same grade used above was added, and the mixture was stirred for 4 hours. The yellow color was completely adsorbed on the silica; when stirring was temporarily stopped, the yellow silica rapidly settled, leaving a clear, colorless solution on top. This slurry was then divided in half. The first half was filtered without washing and then dried overnight in a vacuum oven at 100°C. The liquid that passed through the filter was acidified with H2SO4, and then 3 mL of H2O2 was added as a test for Ti. There was no change in color, indicating that all the Ti was adsorbed on the silica. Next, the dried silica was washed with 2 L of water containing 3 mL of acetic acid to a pH of approximately 3.5. After stirring at 25°C for 30 minutes, the silica was filtered again and subjected to the finishing treatment described in Example 158, i.e., impregnated with Cr, dried, sieved, and calcined at 650°C. The purpose of the additional drying step was to determine the effect of hydrothermal treatment in the presence of sodium.

[0168] Example 173: In this preparation, the remaining half of the slurry prepared in Example 172 was heated at 95°C for 2.5 hours. It was then filtered and washed with 2 L of water containing 3 mL of acetic acid. It was then finished in the manner of Example 158 (Cr, drying, sieving, calcination).

[0169] Example 174: To test the effect of very high sodium levels, in this preparation, 123.4 mL of water was weighed into a beaker, and 15.63 g of 15% TiOSO4, 3 mL of 35% H2O2, 30.66 g of Na2SO4, and 50 mL of 2.26 N NaOH solution were added to the beaker. This resulted in a Na / Ti molar ratio of 37.4. 20.0 g of the same silica used above was added. As NaOH was slowly added, the pH rose to 4.5 while the color of the solution changed from dark orange-red to pale yellow. It was then heated at 93°C for 1.5 hours to obtain a pH of 6.3. The support was washed with 1 L of water, then filtered, and finished in the same manner as in Example 158.

[0170] Example 175: To determine the effect of heat treatment, in this preparation, 129.9 mL of water was weighed into a beaker, and 17.31 g of 15% TiOSO4, 3 mL of 35% H2O2, 30.76 g of Na2SO4, and 54.5 mL of 2.26 N NaOH solution were added. This resulted in a Na / Ti molar ratio of 36.5. 20.9 g of the same silica used above was added. As NaOH was slowly added, the pH rose to 4.5 and the color of the solution changed from dark orange-red to pale yellow. It was then stirred at 25°C for 15 hours. After that, 2 L of water was added to obtain a pH of 5.5, and the support was stirred for 30 minutes to wash away the sodium ions. The support was then filtered and finished in the same manner as in Example 158.

[0171] Example 176: Once adsorbed onto silica, the H2O2 chelated to Ti can be reduced by the addition of a reducing agent to determine whether this promotes the deposition and adhesion of Ti to the silica surface. Therefore, in this experiment, 125 mL of water was poured into a beaker, followed by 16.59 g of 15% TiiOSO4 solution, 3 mL of 35% H2O2 solution, 29.76 g of Na2SO4, 20.0 g of silica (as above), and 53 mL of 2.26 N NaOH stock solution. The slurry was stirred for 30 minutes to adsorb the peroxo-Ti complex onto the silica. The final pH was 4.3. Next, 9.46 g of NaHSO3 was added. The pH dropped to 2.9, which should have returned it to a deep orange color, but instead it turned a very pale yellow, almost white. Next, heating was turned on, and the yellow color completely disappeared before the temperature rose to 66°C. Nevertheless, heating was continued to 90°C and held for 1 hour. Next, the carrier was washed with 2 L of water and finished in the same manner as in Example 158 (Cr, drying, sieving, calcination).

[0172] Example 177: In another experiment, 61.5 g of 15% TiOSO4 was added to 364.4 mL of water in a beaker along with 12 mL of 35% H2O2 and 92.95 g of Na2SO4. Then, 80.4 g of the same silica grade as above was added, followed by the slow addition of 194 mL of 2.26 N NaOH stock solution. The final mixture, pH 4.1, was stirred at 25°C for 15 hours. The next day, when the stirrer was temporarily turned off, it was observed that the yellow color had settled along with the silica, indicating that the peroxo-Ti complex had been adsorbed. The slurry was then divided into two parts. One part was then heated to 95°C for 3 hours to obtain pH 5.7. This part was then divided into two parts again. 9.0 g of (NH4)2SO4 was added to the first part, and the temperature was raised again to 95°C for 2 hours. The color remained yellow. This was done to determine whether NH4 ions were present during adsorption or could be added after adsorption to improve catalytic performance. This portion of the slurry was then finished in the usual manner. It was washed twice with 2 L of water and filtered. Each time, a clear, colorless solution passed through the filter, while the filter remained yellow. When tested, this clear solution was not found to contain Ti. Next, a solution of chromium acetate in 20 mL of methanol (0.01 g Cr / mL) was added to the filtered solid, the mixture was dried in a vacuum oven at 100°C for several hours, then pressed through a 35 mesh screen, and subsequently calcined in dry air at 650°C for 3 hours.

[0173] Example 178: In the second part from Example 177, 4.43 g of NaHSO3 was added to the slurry at 25°C. There was no color change within 30 minutes. Therefore, when the slurry was heated to 85°C, there it gradually changed color from yellow to white, indicating the reduction of the H2O2 ligand on Ti. It was heated for 2 hours, the slurry was filtered, and the clear liquid that passed through the filter was again found to be Ti-free in the standard test. The filtered solid was stirred in 2 L of water at pH 5.2 for 30 minutes. The solid was washed twice with 2 L of water and filtered. Next, a solution of chromium acetate in 20 mL of methanol (0.01 g Cr / mL) was added to the filtered solid, the mixture was dried in a vacuum oven at 100°C for several hours, then pressed through a 35 mesh screen, and subsequently baked in dry air at 650°C for 3 hours.

[0174] Example 179: The effect of the pH increase to 10.1, achieved by adding 11.47 g of Na2CO3 to the latter half of the procedure described in Example 177, was tested. This half was also divided into two equal parts. In the first part, the slurry was stirred at 25°C for 30 minutes, and then washed with 2 L of water containing 3 mL of acetic acid (pH 5.3). After stirring for 30 minutes, it was filtered, then washed again with 1 L of water, and filtered again. The solid on the filter was impregnated with 20 mL of a 0.01 g / mL methanolic chromium(III) acetate solution, dried overnight in a vacuum oven at 100°C, then pressed through a 35 mesh screen, and finally baked in dry air at 650°C for 3 hours.

[0175] Example 180: In the second part of Example 179, which is the second half of Example 177, the slurry was heated to 87°C for 2 hours. The yellow solid was then filtered, washed twice with 2 L of water, and filtered again. Next, a solution of chromium acetate in 20 mL of methanol (0.01 g Cr / mL) was added to the filtered solid, the mixture was dried in a vacuum oven at 100°C for several hours, then pressed through a 35 mesh screen, and subsequently baked in dry air at 650°C for 3 hours.

[0176] Example 181: This test was designed to adsorb Ti in the absence of sodium, followed by hydrothermal treatment in the presence of sodium. Therefore, 2.29 g of TiiOSO4 powder, 3 mL of 35% H2O2 solution, and 14.54 g of 1.37N NH4OH stock solution were dissolved in 111.11 g of deionized water. Upon addition of NH4OH, the dark orange-red starting color faded to a light orange, and the pH increased to 3.0. Next, 20.2 g of silica of the same grade used in Example 158 was added. The slurry was stirred at 25°C for 15 hours to allow adsorption. After this treatment, yellow was adsorbed onto the silica. When stirring was temporarily stopped, the yellow silica settled, leaving a clear, colorless solution on top. At this point, 30.2 g of Na2SO4 (28.0 Na / Ti molar ratio) was added, and the temperature was raised to 85°C for 4 hours. Next, the silica was filtered off, washed with 2 L of water for 30 minutes, filtered again, impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0177] Example 182: This test was designed to reverse the process of Example 181, that is, Ti was adsorbed in the presence of sodium, but hydrothermally treated in the absence of sodium. Therefore, 2.34 g of TiOSO4 powder, 3 mL of 35% H2O2 solution, 30.39 g of Na2SO4, and 12.6 mL of 2.26N NaOH stock solution were dissolved in 116.09 g of deionized water. As NaOH was slowly added, the deep orange-red color changed to pale yellow-orange and the pH rose to 4.2. 20.03 g of silica of the same grade used in Example 158 was added. The slurry was stirred at 25°C for 15 hours. After this treatment, the yellow color was adsorbed onto the silica. When stirring was temporarily stopped, the yellow silica settled, leaving a clear, colorless solution on top. At this point, the yellow silica was filtered, and the clear, colorless liquid that passed through the filter was tested for the presence of Ti. The solution was acidified by adding 3 mL of concentrated H2SO4, followed by the addition of 5 mL of 35% H2O2 solution, but there was no change to orange, indicating the absence of Ti in the solution. The yellow filtered silica was then washed twice more with 2 L of water and filtered again. The yellow silica was then slurryed in 200 mL of deionized water and heated at 90°C for 1.5 hours. After further filtration, it was impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0178] Example 183: This experiment was designed to test very high levels of sodium combined with a low hydrothermal temperature. Therefore, 15.64 g of 15% TiiOSO4 solution, 30.49 g of NaNO3, 29.69 g of Na2SO4, 3 mL of 35% H2O2 solution, and 50 mL of 2.26N NaOH stock solution were dissolved in 95.36 g of deionized water. This yielded a total Na / Ti molar ratio of 60.74. As NaOH was slowly added, the deep orange-red color changed to pale yellow-orange, and the pH rose to 4.0. 20.8 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 56°C for 15 hours. After this treatment, the yellow color was adsorbed onto the silica. When stirring was temporarily stopped, the yellow silica settled, leaving a clear, colorless solution at the top. At this point, the yellow silica was filtered, and the clear, colorless liquid passing through the filter was tested for the presence of Ti. The solution was acidified by adding 3 mL of concentrated H2SO4, followed by the addition of 5 mL of 35% H2O2 solution, but there was no change to orange, indicating the absence of Ti in the solution. The yellow filtered silica was then washed twice more with 2 L of water and filtered again. The yellow silica was then impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0179] Example 184: This experiment was designed to test very high levels of sodium combined with a moderate hydrothermal temperature. Therefore, 16.14 g of 15% TiiOSO4 solution, 62.09 g of NaNO3, 40.4 g of Na2SO4, 3 mL of 35% H2O2 solution, and 52 mL of 2.26N NaOH stock solution were dissolved in 96.68 g of deionized water. This yielded a total Na / Ti molar ratio of 93.64. As NaOH was slowly added, the deep orange-red color changed to pale yellow-orange, and the pH rose to 3.8. 20.4 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 70°C for 5.5 hours. After this treatment, the yellow color was adsorbed onto the silica. When stirring was temporarily stopped, the yellow silica settled, leaving a clear, colorless solution at the top. At this point, the yellow silica was filtered, and the clear, colorless liquid passing through the filter was tested for the presence of Ti. The solution was acidified by adding 3 mL of concentrated H2SO4, followed by the addition of 5 mL of 35% H2O2 solution, but there was no change to orange, indicating the absence of Ti in the solution. The yellow filtered silica was then washed twice more with 2 L of water and filtered again. The yellow silica was then impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0180] Example 185: This experiment was designed to determine the effect of potassium, a different alkali metal ion. Therefore, 15.41 g of 15% TiO2O4 solution, 50.9 g of KNO3, 3 mL of 35% H2O2 solution, and 101.5 mL of 1.31N KOH stock solution were dissolved in 98.9 g of deionized water. This yielded a total K / Ti molar ratio of 44.08. As KOH was slowly added, the deep orange-red color changed to pale yellow-orange, and the pH rose to 3.5. 20.1 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 90°C for 1.5 hours. After this treatment, the yellow color was adsorbed onto the silica. When stirring was temporarily stopped, the yellow silica settled, leaving a clear, colorless solution at the top. At this point, the yellow silica was filtered, and the clear, colorless liquid passing through the filter was tested for the presence of Ti. The solution was acidified by adding 3 mL of concentrated H2SO4, followed by the addition of 5 mL of 35% H2O2 solution, but there was no change to orange, indicating the absence of Ti in the solution. The yellow filtered silica was then washed twice more with 2 L of water and filtered again. The yellow silica was then impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0181] Example 186: This experiment was designed to determine the effect of Ti adsorption from a very dilute Ti solution. Therefore, 15.43 g of 15% TiiOSO4 solution, 3 mL of 35% H2O2 solution, 179.94 g of Na2SO4, and 35.1 mL of 2.80N NaOH stock solution were dissolved in 624.61 g of deionized water. This resulted in a total Na / Ti molar ratio of 177.6. Although this ratio is high, it yields the same Na molar concentration (6.5 M) as used in Example 185 and earlier experiments. As NaOH was slowly added, the deep orange-red color changed to pale yellow-orange, and the pH rose to 3.6. 20.5 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 83°C for 2 hours. After this treatment, the yellow color was indeed adsorbed onto the silica. When stirring was temporarily stopped, the yellow silica settled, leaving a clear, colorless solution at the top. At this point, the yellow silica was filtered, and the clear, colorless liquid that passed through the filter was tested for the presence of Ti. It was acidified by adding 3 mL of concentrated H2SO4, followed by 5 mL of 35% H2O2 solution, but there was no change to orange, indicating the absence of Ti in the solution. Next, the filtered yellow silica was washed twice more with 2 L of water and filtered again. The yellow silica was then impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0182] Example 187: This experiment was designed to test the effect of Ti deposition from high Ti concentration at low pH. Therefore, 15.43 g of 15% TiOSO4 solution, 24.0 g of NaNO3, and 3 mL of 35% H2O2 solution were dissolved in 50.1 g of deionized water. This resulted in a total Na / Ti molar ratio of 19.5 and a pH of less than 1. 20.0 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 88°C for 4 hours. No yellow color remained. The silica was then filtered, washed twice again with 2 L of water, and filtered. The silica was then impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0183] Example 188: This experiment was designed to test the effect of Ti deposition from high Ti concentrations. Therefore, 15.43 g of 15% TiO2O4 solution, 24.02 g of NaNO3, 3 mL of 35% H2O2 solution, and 39.1 mL of 2.80 N NaOH stock solution were dissolved in 15.0 mL of deionized water. This resulted in a total Na / Ti molar ratio of 27.0. As NaOH was slowly added, the deep orange-red color changed to pale yellow-orange, and the pH rose to 4.7. 20.1 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 88°C for 2 hours. After this treatment, the yellow color was indeed adsorbed onto the silica. When stirring was temporarily stopped, the yellow silica settled, leaving a clear, colorless solution at the top. At this point, the yellow silica was filtered, and the clear, colorless liquid passing through the filter was tested for the presence of Ti. The solution was acidified by adding 3 mL of concentrated H2SO4, followed by the addition of 5 mL of 35% H2O2 solution, but there was no change to orange, indicating the absence of Ti in the solution. The yellow filtered silica was then washed twice more with 2 L of water and filtered again. The yellow silica was then impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0184] Example 189: This experiment was designed to test the effect of high-level Ti deposition. Therefore, 67.0 g of 15% TiOSO4 solution and 3 mL of 35% H2O2 solution were dissolved in 63.24 g of deionized water to produce a dark red, almost black solution. Then, 18.38 g of Na2CO3 was slowly added, resulting in a pH of 3.3. This gave a total Na / Ti molar ratio of 5.5. As Na2CO3 was slowly added, the dark red-black color changed to pale yellow-orange, and the pH rose to 3.3. 20.1 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 85°C for 1.5 hours. The yellow filtered silica was then washed twice more with 2 L of water and filtered again. Next, yellow silica was impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35-mesh screen, and then baked in dry air at 650°C for 3 hours.

[0185] Example 190: This experiment was designed to test the effect of high-level Ti deposition from the base side. Therefore, 31.37 g of Na2CO3 and 3 mL of 35% H2O2 solution, followed by 44.61 g of 15% TiOSO4 solution were dissolved in 144.2 g of deionized water to produce a yellow solution with a pH of 8.3. This resulted in a total Na / Ti molar ratio of 14.1. 20.1 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 80°C for 3 hours. The yellow silica was filtered and washed twice more with 2 L of water and filtered again. However, in each wash, the pH of the washing water was measured at 9.5. It was found that it was difficult to remove sodium at this pH, so another wash was performed by adding 5 mL of acetic acid to 2 L of water to acidify it to pH 3.5. The slurry was stirred for 30 minutes and then filtered again. Next, yellow silica was impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35-mesh screen, and then baked in dry air at 650°C for 3 hours.

[0186] Example 191: This experiment was designed to test the effect of Ti deposition from the base side at a neutral pH. Therefore, 8.80 g of 15% TiiOSO4 solution, 4 mL of 35% H2O2 solution, and 68.4 mL of 1.00 N NaOH were dissolved in 99.6 g of deionized water. This produced a clear yellow solution. Next, 12.02 g of NaNO3 was added to raise the pH to 6.2 and induce precipitation. However, since precipitation did not necessarily stop Ti deposition on the silica, it is suggested that the Ti precipitate was still partially dissolved and therefore may be moving in the solution. This resulted in a total Na / Ti molar ratio of 25.4. Next, 20.1 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 90°C for 1.5 hours. The silica was filtered, washed twice more with 2 L of water, and filtered again. Next, silica was impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35-mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0187] Example 192: This experiment was designed to test the effect of restricting the H2O2 concentration to 1H2O2 / Ti on Ti deposition. Therefore, 15.5 g of 15% TiiOSO4 solution, 0.5 mL of 35% H2O2 solution (H2O2 / Ti = 1), and 37.0 mL of 2.80N NaOH stock solution were dissolved in 94.5 g of deionized water. This produced a clear yellow solution with a pH of 4.4. This yielded a total Na / Ti molar ratio of 7.1. Next, 20.4 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 90°C for 5 hours. The silica was then filtered, washed twice more with 2 L of water, and filtered again. Next, silica was impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35-mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0188] Example 193 This experiment was designed to determine whether Ti can deposit when sodium is absent from oxalate, i.e., when oxalate / Ti is 2. Therefore, 3.68 g of oxalic acid dihydrate and 3 mL of 35% H2O2 solution were dissolved in 100.0 g of deionized water. Next, 4.43 mL of titanium tetraisopropoxide was added, which immediately hydrolyzed to precipitate hydrated titania. However, with continued stirring at 25°C, the precipitate dissolved in about 10 minutes, forming a dark orange solution. Next, 5.5 g of NH4Cl was added, and over the next 20 minutes, 55.1 mL of 1.37 N NH4OH was added dropwise to the mixture, resulting in a pH of 8.1. Finally, 20.0 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 90°C for 1.5 hours. Yellow to orange colors were adsorbed onto the silica, but with continued heating, the color changed to white or colorless. The final pH was measured at 7.0. The silica was then filtered, washed twice again with 2 L of water, and filtered again. Next, the silica was impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0189] Example 194: This experiment was designed to determine whether Ti can deposit when sodium is absent from oxalate, i.e., when oxalate / Ti is 1. Therefore, 1.84 g of oxalic acid dihydrate and 3 mL of 35% H2O2 solution were dissolved in 100.0 g of deionized water. Next, 4.43 mL of titanium tetraisopropoxide was added, which immediately hydrolyzed to precipitate hydrated titania. However, with continued stirring at 25°C, the precipitate dissolved in about 10 minutes, forming a dark orange solution. Next, 5.9 g of NH4Cl was added, and over the next 20 minutes, 36.96 mL of 1.37N NH4OH was added dropwise to the mixture, resulting in a pH of 8.1. Finally, 20.0 g of silica of the same grade used in Example 158 was added, and the slurry was stirred at 90°C for 1.5 hours. Yellow to orange colors were adsorbed onto the silica, but with continued heating, the color changed to white or colorless. The final pH was measured at 7.0. The silica was then filtered, washed twice again with 2 L of water, and filtered again. Next, the silica was impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35 mesh screen, and then calcined in dry air at 650°C for 3 hours.

[0190] Example 195: This experiment was designed to investigate the use of lithium ions instead of the usual sodium ions. 2.52 g of oxalic acid dihydrate, 3 mL of 35% H2O2, and 4.4 mL of titanium tetraisopropoxide were added to 100 mL of deionized water. After about 10 minutes, the titanium dissolved in the solution, and a dark orange solution with pH < 1 was prepared. Next, 10.9 g of LiNO3 was added. Then, 9.49 g of ammonium carbonate was added to raise the pH to 8.7. As the pH increased, the color also faded to yellow. This slurry was heated to 92°C and heated at that temperature for 1.5 hours. The silica was filtered, then washed again with 2 L of water and filtered again. Next, silica was impregnated with 20 mL of chromium acetate / methanol solution (0.01 g Cr / mL), dried in a vacuum oven at 100°C for several hours, pressed through a 35-mesh screen, and then calcined in dry air at 650°C for 3 hours. [Table 18] JPEG2026538994000021.jpg199162JPEG2026538994000022.jpg190162JPEG2026538994000023.jpg208162

[0191] Examples 196-198 A chromium / silica pre-catalyst was used for aqueous titration. In Example 196, the chromium / silica pre-catalyst was activated at 650°C for 3 hours, and polyethylene with an HLMI of 21 was produced using this catalyst (see Table 19). 0.29 g of NaHCO3 dissolved in 20 mL of water was mixed with 35 wt% of 2.5 g (Example 197) or 4.5 g (Example 198) of H2O2 and 2.2 g (Example 197) or 4.5 g (Example 198) of TiiOSO4. Then, 5 grams of inert chromium / silica pre-catalyst was added, and the mixture was refluxed at 100°C for 1 hour. The solid was filtered at high temperature by suction filtration, washed with water and ethanol to remove loosely bound Ti species, and dried at room temperature. Activation was carried out in a fluidized bed in dry air at 650°C for 3 hours. The titrated chromium / silica catalysts of Examples 197-198 produced polyethylene with an HLMI value of over 40 g / 10 min. [Table 19]

[0192] Examples 199-204 In Examples 199-204, pre-catalysts were prepared by mixing 30 g of H2O, 0.21 g of chromium(III) acetate, and 5 g of pre-formed silica A. Then, approximately 1 g of H2O2 and 1.08 g of TiOSO4 solution and varying amounts of NaNO3 were added. Finally, NH4OH was added to adjust the pH to approximately 10, and the mixture was subsequently heated at 95°C for 1.5 hours. As the amount of sodium increased (summarized in Table 20 and shown graphically in Figure 2), the HLMI potential unexpectedly increased to over 35 g / 10 min with catalysts containing only 1 wt% titanium, as reflected in the Na:Ti molar ratio. [Table 20]

[0193] Examples 205-209 Table 21 shows that sodium can be easily washed away from the Cr / silica-titania hydrogel pre-catalyst, meaning that the sodium is soluble and not bound to the support / catalyst. Comparative Examples 205-206 in Table 21 are representative of the comparative examples in “The Effect of Alkali Metal Doping on the Performance of Cr / Silica Catalysts in Ethylene Polymerization,” Journal of Catalysis, 176, 344-351, 1998. After the initial formation of the hydrogel, a very large amount of sodium is present from the gelation of water glass (Na2SiO3), and in this form, sodium is detrimental to catalytic activity and must be washed away. Comparative Examples 205-206 are silica-titania hydrogels that have undergone a series of washing steps to remove sodium. The only difference is that Comparative Example 206 used a smaller filter, resulting in twice the filter depth compared to Comparative Example 205. As shown in Table 21, the amount of sodium found in the washing water and the amount of sodium found on the catalyst (based on the catalyst's weight %) decreases significantly with each washing step, and is almost completely gone by washing cycles 8-9. Commercial hydrogel catalysts typically have sodium levels (less than 0.02% by weight) as shown in washing cycles 10-12.

[0194] Table 22 summarizes Comparative Examples 207-209, again demonstrating that sodium or potassium present in hydrogel catalysts can be easily removed by washing. Comparative Example 207 (CE207) was a silica-titania cogelated hydrogel, Comparative Example 208 (CE208) was a silica-titania-chromia targelated hydrogel, and Comparative Example 209 (CE209) was a targelated hydrogel prepared using potassium silicate (K2SiO3) instead of sodium silicate (Na2SiO3) as the silica source. In CE209, it was potassium, not sodium, that was washed away. Since potassium has a higher atomic weight than sodium, the weight percentage value for CE209 was higher. As with Table 21, the cumulative amount of washing water in these three examples is shown, and almost all of the sodium / potassium was removed after washing with only 270-438 lb per lb of catalyst.

[0195] Table 23 summarizes some of Examples 173-191 of the present invention, prepared as described above for each example. In all examples, a pre-catalyst with Ti deposited on pre-formed silica was prepared using the technique described above for each example. The amount of sodium used in catalyst preparation (wt% Na based on the catalyst) is shown in Table 23, and then the catalyst was subjected to a series of washes, as also shown in Table 23 (note that potassium was used instead of sodium in Example 185). The relative amount of Na that should remain after each wash / filtration is shown for each wash / filtration, assuming that all Na is soluble and not bound to the support / catalyst, and that the sodium concentration in the bulk wash solution reaches equilibrium with the sodium concentration in the wash solution within the pores. The theoretical cumulative amount of sodium that would remain after all washing steps is then shown (theoretical wt% Na remaining if soluble). Immediately below that calculation is the actual amount of Na present via ICP analysis (see also Table 18), which is, in most cases, orders of magnitude larger. These surprising results indicate that the majority of the Na used in the catalyst and preparation process of the present invention is in a different form, bound to the carrier / catalyst, insoluble, and not easily removed by washing. In most cases, 300 lbs (dry basis) of washing water were used per lb of catalyst.

[0196] Figure 3 shows and compares the differences in sodium levels in Comparative Examples 205-206 and the examples of the present invention shown in Table 23. The amount of sodium remaining after each wash is plotted again against the total wash water. In the comparative examples, the amount of sodium decreases rapidly with increasing washes, indicating that the sodium is not bound and is easily removed. In contrast, the sodium on the catalyst of the present invention is not removed by washing, regardless of the total wash water used. Note that because the Y-axis is on a logarithmic scale, the separation between the comparative samples and the samples of the present invention is actually much greater than what the graph appears to show.

[0197] As stated above, “bound” alkali metal or zinc means, in this specification, the amount of alkali metal or zinc, respectively, remaining after three equivalent washing / filtration cycles, on a dry basis, resulting in a total of 300 lbs of washing water per lb of carrier / catalyst. In the first cycle, each lb of carrier or catalyst required by the context is combined with 100 lbs of deionized water, mixed / slurred at 25°C for 30 minutes, and then filtered. This washing / filtration cycle is repeated two more times for the filtered solid carrier or catalyst. Sodium (or other alkali metals, or zinc) not “bound” to the carrier / catalyst is virtually completely removed after these three equivalent washing / filtration cycles, resulting in a total of 300 lbs of washing water per lb of carrier / catalyst. This washing / filtration procedure is demonstrated by at least Examples 182–186, 188, and 190–191 in Table 23, which are described in detail above. In Example 182 above, for example, after the addition of silica, a yellow color was adsorbed onto the silica, and a clear, colorless solution appeared when stirring was stopped. The yellow solid was filtered at room temperature to remove the colorless solution and some unbound sodium. In the first wash / filter cycle, the yellow solid was mixed with 2 L of DI water at room temperature for 30 minutes, and this wash / filter cycle was repeated two more times.

[0198] As described in the aforementioned paper (Journal of Catalysis, 176, 344-351, 1998), even in the presence of trace amounts of sodium, the presence of sodium in conventional catalysts causes a significant decrease in surface area, pore volume, and catalytic activity. In contrast, another unexpected and beneficial advantage of the catalyst of the present invention is that the presence of sodium does not have this adverse effect—there is no loss of catalytic activity. Even more surprisingly, even when the sodium level exceeds 1% by weight, the catalyst of the present invention does not lose catalytic activity, whereas with conventional catalysts (e.g., those in the aforementioned paper) the same amount results in a catalyst with no catalytic activity at all.

[0199] Table 18 above summarizes the BET specific surface area and pore volume values ​​for some of the embodiments of the present invention shown in Table 23, after calcination at 650°C for 3 hours in dry air. Despite the presence of high levels of sodium, these activated (or calcined) catalysts have a surface area of ​​(230-465 m²). 2 The surface area (1.2–1.8 mL / g) and pore volume (1.2–1.8 mL / g) were unexpectedly maintained. This differs from conventional catalysts where high levels of sodium cause sintering, resulting in a significant decrease in surface area and pore volume (and therefore catalytic activity). [Table 21] [Table 22] [Table 23]

[0200] Examples 210-211 In Example 210, sodium sulfate (4.4 lb) was dissolved in DI water (202.2 lb), followed by the addition of a 50% H2O2 solution (9.6 lb). Then, solid TiOSO4 (5 lb) was added; the target Ti loading on the support / pre-catalyst was 2.5% by weight. After mixing and homogenization, 40 lb of silica (482 m) was added. 2A solution (1.95 mL / g, average size 60 μm) was added while mixing. Then, 28% ammonium hydroxide (11.9 lb) was added to increase the pH to 9.5, and the temperature of the mixture was raised to 80°C and maintained at that temperature for 2 hours. The solid was removed by microfiltration, and the solid was washed with water. The conductivity (microsiemens, in μs) of the wash water after contact with the titrated silica support was checked every 15 to 30 minutes, and samples with specific conductivity values ​​were collected (Example 210, Samples A to F), and the residual sodium and other elemental content was measured. The titrated silica support was spray-dried. To evaluate the polymerization performance, 1 wt% chromium was added to the titrated silica support according to the procedure of Example 1 above, and then calcined at 650°C for 3 hours. Table 24 summarizes the conductivity and polymerization results, and Table 25 shows the surface area (SA, m) of the pre-catalyst and activated catalyst. 2 This summarizes the pore volume (PV, mL / g), corresponding ICP analysis of the titrated silica support (for sulfur and sodium), and CHN analysis for nitrogen. Example 211 was a laboratory sample prepared by first mixing water, sodium sulfate, H2O2, and ammonium nitrate. Then, TiOSO4 and the same silica as in Example 210 were added, and the pH was adjusted to 8.4 with sodium carbonate. The mixture was heated to 80°C, maintained at that temperature for 2 hours, microfiltered, washed with 4 L of DI water as described in Example 158 above, and dried with acetone.

[0201] As shown in Tables 24-25, the conductivity (abbreviated as "Cond") of samples B-F ranged from 1200 to 200 microsiemens (μS), but when measured by ICP, 0.33-0.36 wt% of sodium remained bound to the support / catalyst. Note that the conductivity in the presence of free sodium generally exceeds 50,000 microsiemens. Activation at 650°C for 3 hours reduced both the surface area and pore volume in samples A-F. Sample A, with a conductivity of 4560 microsiemens and a bound sodium level of approximately 0.5 wt%, was subjected to high-temperature activation at 850°C for 3 hours, resulting in sintering and a surface area of ​​121 m². 2The pore volume decreased to 0.66 mL / g.

[0202] Unexpectedly, samples A through F contained significantly higher levels of sulfur than Example 211, which was prepared on a laboratory scale. While sulfur levels ranged from over 0.01% by weight to approximately 0.2% by weight at their highest, they did not appear to affect the melt flow characteristics. [Table 24] [Table 25]

[0203] The present invention has been described above with reference to numerous aspects and specific examples. In light of the above detailed description, many variations will be apparent to those skilled in the art. All such obvious variations are within the fully intended scope of the appended claims. Other aspects of the present invention may include, but are not limited to, the following (aspects are described as "including," but can alternatively be "essentially consisting of" or "consisting of"):

[0204] Embodiment 1. A titrated silica carrier comprising silica, 0.1 to 10% by weight of titanium, 0.5 to 12% by weight of water, 2% by weight or less of carbon, and a bonded alkali metal and / or zinc, wherein the molar ratio of alkali metal:titanium or zinc:titanium is 0.02:1 to 3:1, and / or the amount of alkali metal or zinc per gram of silica is in the range of 0.01 to 2 mmol.

[0205] Embodiment 2. A chromium titanate / silica pre-catalyst comprising silica, 0.1 to 5% by weight of chromium, 0.1 to 10% by weight of titanium, 0.5 to 12% by weight of water, 4% by weight or less of carbon, and a bonded alkali metal and / or zinc, wherein the molar ratio of alkali metal:titanium or zinc:titanium is 0.02:1 to 3:1, and / or the amount of alkali metal or zinc per gram of silica is in the range of 0.01 to 2 mmol.

[0206] Embodiment 3. A pre-catalyst as defined in Embodiment 2, wherein at least 75% by weight, at least 80% by weight, at least 90% by weight, or at least 95% by weight of chromium is present in an oxidation state of 3 or less.

[0207] Embodiment 4. A carrier or pre-catalyst as defined in any one of the prior embodiments, wherein the carrier or pre-catalyst contains any suitable amount of carbon, or any range of amounts disclosed herein, for example, in amounts of 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.5% by weight or less, 0.3% by weight or less, or 0.1% by weight or less, based on the total weight of the carrier or pre-catalyst, respectively.

[0208] Embodiment 5. A carrier or pre-catalyst as defined in any one of the prior embodiments, wherein the carrier or pre-catalyst contains any suitable amount of water / moisture, or any range of amounts disclosed herein, for example, 0.5 to 12% by weight, 1 to 11% by weight, 2.5 to 10% by weight, 3 to 9% by weight, or 5 to 8% by weight, based on the total weight of the carrier or pre-catalyst, respectively.

[0209] Embodiment 6. A chromium titanate / silica catalyst comprising silica, 0.1 to 5% by weight of chromium, 0.1 to 10% by weight of titanium, and a bonded alkali metal and / or zinc, wherein the molar ratio of alkali metal:titanium or zinc:titanium is 0.02:1 to 3:1, and / or the amount of alkali metal or zinc per gram of silica is in the range of 0.01 to 2 mmol, wherein at least 60% by weight of the chromium is present in an oxidized state of +6.

[0210] Embodiment 7. A chromium titanate / silica catalyst comprising silica, 0.1 to 5% by weight of chromium, and 0.1 to 10% by weight of titanium, wherein at least 60% by weight of the chromium exists in an oxidized state of +6, and the catalyst is given by the formula Y(HLMI) = (-9.6153x 3 +21.088x 2 The chromium titanate / silica catalyst characterized by a polymer HLMI (g / 10 min) greater than (+25.835x+5.7983) (wherein x is the number of titanium atoms per square nanometer of silica surface area of ​​the chromium titanate / silica catalyst).

[0211] Embodiment 8. The catalyst as defined in Embodiment 7, wherein the catalyst further comprises an alkali metal and / or zinc in a molar ratio of alkali metal:titanium or zinc:titanium of 0.02:1 to 3:1, and / or alkali metal and / or zinc in an amount of alkali metal or zinc in the range of 0.01 to 2 mmol per gram of silica.

[0212] Embodiment 9. A catalyst as defined in any one of Embodiments 6 to 8, wherein at least 70% by weight, at least 75% by weight, at least 80% by weight, at least 85% by weight, at least 90% by weight, or at least 95% by weight of the chromium is present in an oxidized state of +6.

[0213] Aspect 10. A catalyst defined in any one of aspects 6 to 9, wherein the formula Y(HLMI) = (-9.6153x 3 +21.088x 2 The polymer is characterized by an HLMI (g / 10 min) greater than +25.835x+5.7983), where x is the number of titanium atoms per square nanometer of silica surface area of ​​the titrated chromium / silica catalyst; alternatively, Y = 1.1*(-9.6153x 3 +21.088x 2 +25.835x+5.7983); Alternatively, Y=1.15*(-9.6153x 3 +21.088x 2(+25.835x+5.7983)); Alternatively, Y=1.2*(-9.6153x 3 +21.088x 2 +25.835x+5.7983); Alternatively, Y=1.3*(-9.6153x 3 +21.088x 2 The catalyst is (+25.835x+5.7983).

[0214] Embodiment 11. A catalyst as defined in any one of Embodiments 6 to 10, wherein the catalyst contains any suitable amount of water / moisture, or any range of amounts disclosed herein, for example, 3% by weight or less, 2% by weight or less, 1.5% by weight or less, 1% by weight or less, or 0.5% by weight or less, based on the total weight of the catalyst.

[0215] Embodiment 12. A carrier or pre-catalyst as defined in any one of Embodiments 2 to 11, wherein the pre-catalyst contains any suitable amount of chromium, or any range of amounts disclosed herein, for example, 0.3 to 3% by weight, 0.4 to 2% by weight, 0.5 to 1.5% by weight, or 0.7 to 1.5% by weight, based on the total weight of each catalyst.

[0216] Embodiment 13. A carrier, pre-catalyst, or catalyst as defined in any one of the prior embodiments, wherein the carrier, pre-catalyst, or catalyst contains any suitable amount of titanium, or any range of amounts disclosed herein, for example, in amounts of 0.5 to 7% by weight, 0.5 to 3% by weight, 0.8 to 2% by weight, 1 to 6% by weight, or 1.5 to 4% by weight, based on the total weight of the carrier, pre-catalyst, or catalyst, respectively.

[0217] Aspect 14. The support, pre-catalyst, or catalyst as defined in any one of the preceding aspects, which comprises any suitable amount of nitrogen, or any range of amounts disclosed herein, for example, in an amount of 0.01 to 1.5 wt%, 0.1 to 1.5 wt%, 0.3 to 1 wt%, 0.4 to 1.2 wt%, 0.4 to 1 wt%, or 0.5 to 0.7 wt%, based on the total weight of each of the support, the pre-catalyst, or the catalyst.

[0218] Aspect 15. The support, pre-catalyst, or catalyst as defined in any one of the preceding aspects, which comprises any suitable amount of the alkali metal or the zinc, or any range of amounts disclosed herein, for example, the minimum molar ratio of alkali metal:titanium or zinc:titanium is 0.02:1, 0.05:1, 0.08:1, 0.1:1, 0.12:1, 0.15:1, or 0.2:1, and the maximum molar ratio is 3:1, 2.5:1, 2.2:1, 2:1, or 1.8:1, and said molar ratio can range from any minimum molar ratio disclosed herein to any maximum molar ratio disclosed herein.

[0219] Aspect 16. The support, pre-catalyst, or catalyst as defined in any one of the preceding aspects, which comprises any suitable amount of the alkali metal or the zinc, or any range of amounts disclosed herein, for example, a minimum amount of the alkali metal or the zinc of 0.01, 0.02, 0.04, 0.08, 0.1, 0.11, 0.13, or 0.15 mmol per gram of silica, and a maximum amount of 2, 1.5, 1.2, 1, 0.9, or 0.8 mmol / g, and the amount in the unit of mmol / g can range from any minimum amount disclosed herein to any maximum amount disclosed herein.

[0220] Aspect 17. The support, pre-catalyst, or catalyst as defined in any one of the preceding aspects, which comprises the alkali metal.

[0221] Embodiment 18. A carrier, pre-catalyst, or catalyst as defined in any one of the prior embodiments, comprising zinc.

[0222] Embodiment 19. A carrier, pre-catalyst, or catalyst as defined in any one of the prior embodiments, wherein the alkali metal comprises lithium, sodium, potassium, or a combination thereof; alternatively, lithium; alternatively, sodium; or alternatively, potassium.

[0223] Embodiment 20. A carrier, pre-catalyst, or catalyst as defined in any one of the prior embodiments, comprising any suitable amount of sulfuric acid, or any range of amounts disclosed herein, for example, in amounts of 0.005 to 0.25% by weight, 0.01 to 0.2% by weight, 0.02 to 0.25% by weight, 0.02 to 0.2% by weight, 0.02 to 0.2% by weight, 0.02 to 0.15% by weight, 0.02 to 0.1% by weight, 0.03 to 0.25% by weight, 0.03 to 0.2% by weight, 0.03 to 0.15% by weight, or 0.03 to 0.1% by weight, based on the total weight of the carrier, pre-catalyst, or catalyst, respectively.

[0224] Embodiment 21. A carrier, pre-catalyst, or catalyst as defined in any one of the preceding embodiments, wherein the titanium is adsorbed on the silica and / or at least a portion of the zinc or alkali metal is (chemically) bonded to the titanium.

[0225] Embodiment 22. A carrier, pre-catalyst, or catalyst as defined in any one of the preceding embodiments, wherein at least a portion of the zinc and the titanium exists as zinc titanate, and / or at least a portion of the alkali metal and the titanium exists as alkali metal titanate, for example, sodium titanate.

[0226] Embodiment 23. A carrier, pre-catalyst, or catalyst as defined in any one of the prior embodiments, comprising any suitable amount of the silica, or any range of amounts disclosed herein, for example, 70-99.5% by weight, 80-98% by weight, 80-95% by weight, 85-98% by weight, 85-95% by weight, 90-99.5% by weight, or 90-98% by weight, based on the total weight of the carrier, pre-catalyst, or catalyst, respectively.

[0227] Embodiment 24. A carrier, pre-catalyst, or catalyst as defined in any one of the prior embodiments, wherein the carrier, pre-catalyst, or catalyst has a total pore volume in any preferred range or any range disclosed herein, for example, a total pore volume of 0.5 to 3 mL / g, 0.8 to 2.5 mL / g, 1 to 2 mL / g, or 1.3 to 1.8 mL / g.

[0228] Embodiment 25. A carrier, pre-catalyst, or catalyst as defined in any one of the prior embodiments, having a BET surface area of ​​any preferred range or any range disclosed herein, e.g., 100 to 700 m². 2 / g, 150~650m 2 / g, 200-600m 2 / g, or 250-550m 2 The carrier, the pre-catalyst, or the catalyst having a BET surface area of ​​1 / g.

[0229] Embodiment 26. A carrier, pre-catalyst, or catalyst as defined in any one of the prior embodiments, wherein the carrier, pre-catalyst, or catalyst has an average (d50) particle size in any preferred range or any range disclosed herein, for example, 15-350 μm, 25-300 μm, 50-200 μm, or 75-150 μm.

[0230] Embodiment 27. An olefin polymerization process comprising contacting a chromium titanate / silica catalyst and an optional co-catalyst, as defined in any one of Embodiments 6 to 26, with an olefin monomer and an optional olefin co-monomer in a polymerization reactor system under polymerization conditions to produce an olefin polymer.

[0231] Embodiment 28. An olefin polymerization process as defined in Embodiment 27, wherein a cocatalyst is used, the cocatalyst comprising any suitable cocatalyst or any cocatalyst disclosed herein, for example, an aluminoxane cocatalyst, an organoaluminum cocatalyst, an organoboron cocatalyst, or any combination thereof.

[0232] Embodiment 29. The olefin monomer is any olefin monomer disclosed herein, for example, any C2-C 20 An olefin polymerization process, comprising an olefin, as defined in embodiment 27 or 28.

[0233] Embodiment 30. The olefin monomer and the arbitrary olefin comonomer are independently C2-C 20 An olefin polymerization process comprising alpha-olefins, as defined in any one of embodiments 27 to 29.

[0234] Embodiment 31. An olefin polymerization process as defined in any one of Embodiments 27 to 30, wherein the olefin monomer comprises ethylene.

[0235] Embodiment 32. The chromium titanate / silica catalyst is made of ethylene and C3-C 10 An olefin polymerization process as defined in any one of embodiments 27 to 31, comprising contacting an olefin comonomer containing an alpha-olefin.

[0236] Embodiment 33. An olefin polymerization process as defined in any one of Embodiments 27 to 32, comprising contacting the chromium titanate / silica catalyst with an olefin comonomer comprising ethylene and 1-butene, 1-hexene, 1-octene, or a mixture thereof.

[0237] Aspect 34. The olefin polymerization process as defined in any one of aspects 27 to 33, wherein the polymerization reactor system comprises a batch reactor, a slurry reactor, a gas phase reactor, a solution reactor, a high pressure reactor, a tubular reactor, an autoclave reactor, or a combination thereof.

[0238] Aspect 35. The olefin polymerization process as defined in any one of aspects 27 to 33, wherein the polymerization reactor system comprises a slurry reactor, a gas phase reactor, a solution reactor, or a combination thereof.

[0239] Aspect 36. The olefin polymerization process as defined in any one of aspects 27 to 35, wherein the polymerization reactor system comprises a loop slurry reactor.

[0240] Aspect 37. The olefin polymerization process as defined in any one of aspects 27 to 36, wherein the polymerization reactor system comprises a single reactor.

[0241] Aspect 38. The olefin polymerization process as defined in any one of aspects 27 to 36, wherein the polymerization reactor system comprises two reactors.

[0242] Aspect 39. The olefin polymerization process as defined in any one of aspects 27 to 36, wherein the polymerization reactor system comprises two or more reactors.

[0243] Aspect 40. The olefin polymerization process as defined in any one of aspects 27 to 39, wherein the olefin monomer comprises any olefin polymer disclosed herein.

[0244] Aspect 41. The olefin polymerization process as defined in any one of aspects 27 to 40, wherein the olefin polymer comprises an ethylene homopolymer, an ethylene / 1-butene copolymer, an ethylene / 1-hexene copolymer, and / or an ethylene / 1-octene copolymer.

[0245] Embodiment 42. An olefin polymerization process as defined in any one of Embodiments 27 to 41, wherein the polymerization conditions include a polymerization reaction temperature in the range of 60°C to 120°C and a reaction pressure in the range of 200 to 1000 psig (1.4 to 6.9 MPa).

[0246] Embodiment 43. An olefin polymerization process as defined in any one of Embodiments 27 to 42, wherein the polymerization conditions are substantially constant for a particular polymer grade, for example.

[0247] Embodiment 44. An olefin polymerization process as defined in any one of Embodiments 27 to 43, wherein hydrogen is not added to the polymerization reactor system.

[0248] Embodiment 45. An olefin polymerization process as defined in any one of Embodiments 27 to 43, wherein hydrogen is added to the polymerization reactor system.

[0249] Embodiment 46. The olefin polymer has a density within any range disclosed herein, for example, 0.92-0.965, 0.93-0.96, 0.935-0.955, or 0.94-0.95 g / cm³. 3 An olefin polymerization process having a density as defined in any one of embodiments 27 to 45.

[0250] Embodiment 47. An olefin polymerization process defined in any one of Embodiments 27 to 46, wherein the olefin polymer has an MI in any range disclosed herein, for example, 0 to 100, 0.1 to 10, 0.2 to 5, or 0.25 to 2 g / 10 min MI.

[0251] Embodiment 48. An olefin polymerization process defined in any one of Embodiments 27 to 47, wherein the olefin polymer has an HLMI in any range disclosed herein, e.g., 1 to 1000, 5 to 500, 6 to 40, 8 to 60, 10 to 100, or 12 to 50 g / 10 min of HLMI.

[0252] Embodiment 49. An olefin polymerization process as defined in any one of Embodiments 27 to 48, wherein the olefin polymer has an Mw / Mn ratio within any range disclosed herein, for example, a Mw / Mn ratio of 5 to 30, 7 to 25, 9 to 20, 10 to 25, or 10 to 15.

[0253] Embodiment 50. An olefin polymerization process as defined in any one of Embodiments 27 to 49, wherein the olefin polymer has an Mw in any range disclosed herein, for example, 10 to 500, 30 to 300, 50 to 400, 50 to 250, 80 to 200, or 100 to 250 kg / mol.

[0254] Embodiment 51. An olefin polymerization process defined in any one of Embodiments 27 to 50, wherein the olefin polymer has Mn in any range disclosed herein, i.e., Mn in the range of 1 to 50, 3 to 30, 4 to 40, 5 to 25, or 8 to 20 kg / mol.

[0255] Embodiment 52. An olefin polymerization process as defined in any one of Embodiments 27 to 51, wherein the olefin polymer has a CY-a parameter within any range disclosed herein, for example, 0.05 to 0.5, 0.08 to 0.4, 0.1 to 0.3, 0.1 to 0.25, or 0.15 to 0.25.

[0256] Embodiment 53. The olefin polymer produced by an olefin polymerization process defined in any one of Embodiments 27 to 52.

[0257] Embodiment 54. A manufactured article comprising the polymer defined in Embodiment 53.

[0258] Apparatus 55. Articles as defined in Apparatus 54, which are agricultural films, automobile parts, bottles, drums, textiles or fabrics, food packaging films or containers, food service supplies, fuel tanks, geomembranes, household containers, liners, molded articles, medical devices or materials, pipes, sheets or tapes, or toys.

[0259] Embodiment 56. A process for preparing a titrated silica support, comprising: (i) contacting water, a peroxide compound, a titanium precursor, and silica (under conditions sufficient to adsorb titanium onto the silica) to form a first mixture; (ii) isolating a solid fraction from the first mixture; and (iii) drying the solid fraction to form the titrated silica support.

[0260] Embodiment 57. A process for preparing a titrated silica support, comprising: (a) contacting water, hydrogen peroxide, an alkali metal precursor and / or a zinc precursor, a titanium precursor, and silica (under conditions sufficient for titanium to adsorb onto the silica) to form a first mixture; (b) contacting the first mixture with a nitrogen-containing compound to form a second mixture; (c) subjecting the second mixture to a reaction temperature in the range of 40 to 270°C; (d) isolating a solid fraction from the second mixture and washing the solid fraction; and (e) drying the solid fraction to form the titrated silica support.

[0261] Embodiment 58. A process for preparing a titrated silica support, comprising: (A) contacting water, hydrogen peroxide, an alkali metal precursor and / or a zinc precursor, a titanium precursor, and silica (under conditions sufficient for titanium to adsorb onto the silica) to form a first mixture; (B) subjecting the first mixture to a reaction temperature in the range of 40 to 270°C; (C) isolating a solid fraction from the first mixture and washing the solid fraction; and (D) drying the solid fraction to form the titrated silica support.

[0262] Embodiment 59. A process defined in any one of Embodiments 56 to 58, wherein the first mixture is formed by contacting the materials in any order or sequence.

[0263] Embodiment 60. A process defined in any one of Embodiments 56 to 59, wherein the molar ratio of the peroxide compound or the hydrogen peroxide to titanium is within any preferred range or any range disclosed herein, for example, 0.5:1 to 100:1, 2:1 to 50:1, 3:1 to 20:1, or 5:1 to 11:1.

[0264] Embodiment 61. A process defined in any one of Embodiments 56 to 60, wherein the molar ratio of the alkali metal or the zinc to titanium is within any preferred range or any range disclosed herein, for example, 0.1:1 to 300:1, for example 0.2:1 to 100:1, 0.5:1 to 20:1, 0.7:1 to 10:1, 1:1 to 5:1, or 1:1 to 3:1.

[0265] Embodiment 62. A process defined in any one of Embodiments 56 to 61, wherein the weight ratio of titanium to water (Ti:H2O) is any preferred range or any range disclosed herein, for example, 0.0001:1 to 0.02:1, 0.001:1 to 0.02:1, 0.005:1 to 0.02:1, or 0.03:1 to 0.07:1.

[0266] Embodiment 63. A process as defined in any one of Embodiments 56 to 62, wherein the titanium precursor comprises any suitable titanium compound or any titanium compound disclosed herein, for example, a Ti(III) compound, a Ti(IV) compound, or any combination thereof.

[0267] Embodiment 64. A process as defined in any one of Embodiments 56 to 62, wherein the titanium precursor includes titanium carboxylate (e.g., titanium oxalate, titanium glycolate, titanium lactate, titanium citrate, titanium malate), titanium halide, titanium oxide, titanium hydroxide, titanium alkoxide (e.g., titanium isopropoxide, titanium n-propoxide), titanium sulfate, titanium nitrate, or any combination thereof.

[0268] Embodiment 65. A process defined in any one of Embodiments 56 to 62, wherein the titanium precursor includes TiOSO4, Ti(OH)4, Ti metal, Ti(OR)4, TiO(OH)2, or any combination thereof.

[0269] Embodiment 66. A process defined in any one of Embodiments 56 to 65, further comprising the step of adjusting the pH of the first mixture to any preferred range or any range disclosed herein, for example, 3 to 12, 3 to 10, 4 to 12, 4 to 10, 6 to 10, or 8 to 10.

[0270] Embodiment 67. A process defined in any one of Embodiments 57 to 66, wherein the weight ratio of the nitrogen-containing compound to titanium is within any preferred range or any range disclosed herein, for example, 5:1 to 300:1, 10:1 to 200:1, 25:1 to 150:1, or 50:1 to 100:1.

[0271] Embodiment 68. A process defined in any one of Embodiments 56 to 67, wherein the (pre-formed) silica contains any suitable amount of water / moisture, or any range of amounts disclosed herein, for example, 25% by weight or less, 20% by weight or less, 15% by weight or less, or 10% by weight or less, based on the total weight of the silica.

[0272] Embodiment 69. A process defined in any one of Embodiments 56 to 68, wherein the (pre-formed) silica is characterized by the pore volume, surface area, and average particle size defined in any one of Embodiments 24 to 26.

[0273] Embodiment 70. A process defined in any one of Embodiments 56 to 67, wherein the silica contains any suitable amount of water, or any range of amounts disclosed herein, or a silica hydrogel, in an amount of at least 50% by weight, at least 60% by weight, at least 70% by weight, or at least 80% by weight.

[0274] Embodiment 71. A process defined in any one of Embodiments 56 to 70, wherein the weight ratio of silica to water (silica:H2O) is any preferred range or any range disclosed herein, for example, 0.001:1 to 1:1, 0.01:1 to 0.5:1, 0.05:1 to 0.4:1, or 0.1:1 to 0.3:1.

[0275] Embodiment 72. A process defined in any one of Embodiments 56 to 71, wherein the first mixture prior to step (ii) is subjected to the following reaction temperatures, or the reaction temperature is in any preferred range or any range disclosed herein, e.g., 40 to 270°C, 60 to 260°C, 80 to 220°C, 40 to 100°C, 60 to 100°C, 70 to 100°C, or 80 to 100°C (at any preferred pressure, e.g., from atmospheric pressure up to 100 or 300 psig).

[0276] Embodiment 73. A process defined in any one of Embodiments 56 to 72, wherein the first mixture or the second mixture is subjected to the reaction temperature for any preferred period or any range disclosed herein, for example, 1 minute to 1 hour, 10 minutes to 4 days, 20 minutes to 2 days, 30 minutes to 24 hours, or 40 minutes to 2 hours.

[0277] Embodiment 74. A process defined in any one of Embodiments 56 to 73, wherein the isolation of the solid fraction includes any preferred separation technique or any technique disclosed herein, such as filtration, sedimentation, decantation, compression, centrifugation, cyclone treatment, hydrocyclone treatment, or any combination thereof.

[0278] Embodiment 75. A process defined in any one of Embodiments 56 to 74, wherein washing the solid fraction comprises any suitable wash solution or any wash solution disclosed herein, e.g., water, an alcohol (e.g., ethanol), or a mixture thereof.

[0279] Embodiment 76. A process defined in any one of Embodiments 56 to 75, wherein drying is carried out at any preferred temperature or any range of temperatures disclosed herein, for example, 25°C to 200°C, 50°C to 150°C, 70°C to 120°C, or 90°C to 110°C.

[0280] Embodiment 77. A process defined in any one of Embodiments 56 to 76, wherein drying is carried out for any preferred period of time or any range disclosed herein, for example, 1 second to 1 day, 1 hour to 12 hours, 2 hours to 8 hours, or 0.1 to 5 seconds.

[0281] Embodiment 78. A drying process defined in any one of Embodiments 56 to 77, comprising spray drying, tray drying, flash drying, freeze drying, oven drying, microwave drying; alternatively, spray drying; or alternatively, flash drying.

[0282] Embodiment 79. A titaniumated silica support prepared by a process defined in any one of Embodiments 56 to 78.

[0283] Embodiment 80. A titanium silica support prepared by a process defined in any one of Embodiments 56 to 78, wherein the titanium silica support is defined in any one of Embodiments 1 to 26.

[0284] Embodiment 81. A process for preparing a titrated chromium / silica precatalyst, comprising: performing a process for preparing a titrated silica support as defined in any one of embodiments 56 to 78 below; and contacting a chromium precursor with the first mixture or the second mixture in any step prior to the step of isolating the solid fraction from the first mixture or the second mixture.

[0285] Embodiment 82. A process for preparing a chromium titanate / silica pre-catalyst, comprising: performing a process for preparing a silica titanate support as defined in any one of Embodiments 56 to 78; and, after isolating the solid fraction from the first mixture or the second mixture, contacting the solid fraction with a chromium precursor (before or after drying the solid fraction).

[0286] Embodiment 83. The process as defined in Embodiment 81 or 82, wherein the chromium precursor comprises any suitable chromium compound or any chromium compound disclosed herein, for example, a chromium(II) compound, a chromium(III) compound, or any combination thereof.

[0287] Embodiment 84. A process defined in any one of Embodiments 81 to 83, wherein the chromium precursor comprises chromium trioxide, chromium acetate, chromium hydroxyacetate, chromium nitrate, or any combination thereof.

[0288] Embodiment 85. A process defined in any one of Embodiments 81 to 84, wherein the chromium precursor is water-soluble.

[0289] Embodiment 86. A process for preparing a titrated chromium / silica pre-catalyst, comprising performing a process for preparing a titrated silica support as defined in any one of Embodiments 56 to 78, wherein instead of contacting silica to form the first mixture, the process comprises contacting a chromium / silica pre-catalyst to form the first mixture.

[0290] Embodiment 87. The chromium titanate / silica pre-catalyst manufactured by a process defined in any one of Embodiments 81 to 86.

[0291] Embodiment 88. The chromium titanide / silica precatalyst manufactured by a process defined in any one of Embodiments 81 to 86, wherein the chromium titanide / silica precatalyst is defined in any one of Embodiments 2 to 26.

[0292] Embodiment 89. A process for preparing a chromium titanide / silica catalyst, comprising: performing a process for preparing a chromium titanide / silica pre-catalyst as defined in any one of Embodiments 81 to 86 below; and activating the chromium titanide / silica pre-catalyst to form the (activated) chromium titanide / silica catalyst.

[0293] Embodiment 90. A process defined in Embodiment 89, wherein activation includes any preferred temperature and time conditions or any temperature and time conditions disclosed herein, for example, a temperature of 400°C to 900°C, 500°C to 850°C, 600°C to 800°C, or 600°C to 700°C, and a period of 1 minute to 24 hours, 1 hour to 12 hours, 2 hours to 8 hours, or 2 hours to 6 hours.

[0294] Embodiment 91. The chromium titanate / silica catalyst manufactured by the process defined in Embodiment 89 or 90.

[0295] Embodiment 92. The chromium titanate / silica catalyst manufactured by a process defined in Embodiment 89 or 90, as defined in any one of Embodiments 6 to 26.

Claims

1. A titanium silica support, the following: silica; 0.1 to 10% by weight of titanium; 0.5–12% by weight of water; 4% by weight or less of carbon; and Includes, The molar ratio of the bonded alkali metal to the titanium and / or the molar ratio of the bonded zinc to the titanium is 0.02:1 to 3:1; and / or The amount of the bonded alkali metal and / or the bonded zinc is in the range of 0.01 to 2 mmol per gram of silica, in the titrated silica carrier.

2. A chromium titanate / silica pre-catalyst, which includes the following: silica; 0.1 to 5% by weight of chromium; 0.1 to 10% by weight of titanium; 0.5–12% by weight of water; 4% by weight or less of carbon; and Includes, The molar ratio of the bonded alkali metal to the titanium and / or the molar ratio of the bonded zinc to the titanium is 0.02:1 to 3:1; and / or The amount of the bonded alkali metal and / or the bonded zinc is in the range of 0.01 to 2 mmol per gram of silica, in the titrated silica carrier.

3. The pre-catalyst according to claim 2, comprising 0.3 to 3% by weight, 0.4 to 2% by weight, 0.5 to 1.5% by weight, or 0.7 to 1.5% by weight of the chromium.

4. The pre-catalyst according to claim 2 or 3, wherein at least 75% by weight, at least 80% by weight, at least 90% by weight, or at least 95% by weight of the chromium is present in an oxidation state of 3 or less.

5. A carrier or pre-catalyst according to any one of claims 1 to 4, comprising 3% by weight or less, 2% by weight or less, 1% by weight or less, 0.5% by weight or less, 0.3% by weight or less, or 0.1% by weight or less of the carbon.

6. A carrier or pre-catalyst according to any one of claims 1 to 5, comprising 1 to 11% by weight, 2.5 to 10% by weight, 3 to 9% by weight, or 5 to 8% by weight of water.

7. A chromium titanate / silica catalyst, which includes the following: silica; 0.1 to 5% by weight of chromium, wherein at least 60% by weight of the chromium is present in an oxidized state of +6; 0.1 to 10% by weight of titanium; and Includes, The molar ratio of the bonded alkali metal to the titanium and / or the molar ratio of the bonded zinc to the titanium is 0.02:1 to 3:1; and / or The amount of the bonded alkali metal and / or the bonded zinc is in the range of 0.01 to 2 mmol per gram of silica, in the titrated silica carrier.

8. The catalyst according to claim 7, wherein the formula Y(HLMI) = (-9.6153x 3 +21.088x 2 The catalyst is characterized by a polymer HLMI (g / 10 min) greater than (+25.835x + 5.7983) (wherein x is the number of titanium atoms per square nanometer of silica surface area of ​​the titranidized chromium / silica catalyst).

9. The catalyst according to claim 7 or 8, wherein at least 70% by weight, at least 75% by weight, at least 80% by weight, at least 85% by weight, at least 90% by weight, or at least 95% by weight of the chromium is present in an oxidized state of +6.

10. The catalyst according to any one of claims 7 to 9, comprising 0.3 to 3% by weight, 0.4 to 2% by weight, 0.5 to 1.5% by weight, or 0.7 to 1.5% by weight of the chromium.

11. A catalyst according to any one of claims 7 to 10, comprising 3% by weight or less, 2% by weight or less, 1.5% by weight or less, 1% by weight or less, or 0.5% by weight or less of water.

12. A carrier, pre-catalyst, or catalyst according to any one of the prior claims, comprising 0.5 to 7% by weight, 0.5 to 3% by weight, 0.8 to 2% by weight, 1 to 6% by weight, or 1.5 to 4% by weight of titanium.

13. A carrier, pre-catalyst, or catalyst according to any one of the prior claims, further comprising 0.01 to 1.5% by weight, 0.1 to 1.5% by weight, 0.3 to 1% by weight, 0.4 to 1.2% by weight, 0.4 to 1% by weight, or 0.5 to 0.7% by weight of nitrogen.

14. A carrier, pre-catalyst, or catalyst according to any one of the prior claims, further comprising 0.005 to 0.25% by weight, 0.01 to 0.2% by weight, 0.02 to 0.25% by weight, 0.02 to 0.2% by weight, 0.02 to 0.15% by weight, 0.02 to 0.1% by weight, 0.03 to 0.25% by weight, 0.03 to 0.2% by weight, 0.03 to 0.15% by weight, or 0.03 to 0.1% by weight of sulfuric acid.

15. The molar ratio of the bonded alkali metal to the titanium or the molar ratio of the bonded zinc to the titanium is 0.08:1 to 3:1, 0.1:1 to 3:1, 0.12:1 to 3:1, 0.2:1 to 3:1, 0.02:1 to 2.5:1, 0.05:1 to 2.5:1, 0.12:1 to 2.5:1, 0.15:1 to 2.5:1, 0.05:1 to 2.2:1, 0.1:1 to 2.2:1, 0.2:1 to 2.2:1 A carrier, pre-catalyst, or catalyst according to any one of the prior claims, wherein the ratio is 0.02:1 to 2:1, 0.05:1 to 2:1, 0.1:1 to 2:1, 0.12:1 to 2:1, 0.15:1 to 2:1, 0.2:1 to 2:1, 0.02:1 to 1.8:1, 0.08:1 to 1.8:1, 0.1:1 to 1.8:1, 0.12:1 to 1.8:1, 0.15:1 to 1.8:1, or 0.2:1 to 1.8:

1.

16. The amount of the bonded alkali metal or the bonded zinc per gram of silica is 0.02-2, 0.08-2, 0.1-2, 0.11-2, 0.13-2, 0.15-2, 0.01-1.5, 0.04-1.5, 0.11-1.5, 0.2-1.5, 0.01-1.2, 0.04-1.2, 0.1-1.2, 0.11-1.2, 0.15-1.2, 0.01-1, 0.04-1, 0.08 A carrier, pre-catalyst, or catalyst according to any one of the prior claims, in the range of -1, 0.1-1, 0.11-1, 0.13-1, 0.15-1, 0.2-1, 0.02-0.9, 0.08-0.9, 0.11-0.9, 0.15-0.9, 0.2-0.9, 0.01-0.8, 0.02-0.8, 0.04-0.8, 0.1-0.8, 0.11-0.8, 0.13-0.8, 0.15-0.8, or 0.2-0.8 mmol / g.

17. A carrier, pre-catalyst, or catalyst according to any one of the prior claims, comprising the bonded alkali metal, wherein the bonded alkali metal comprises sodium.

18. The titanium is adsorbed on the silica; At least a portion of the sodium is bonded to the titanium; At least a portion of the sodium is present as sodium titanate; or Any combination thereof, the carrier, pre-catalyst, or catalyst according to claim 17.

19. A carrier, pre-catalyst, or catalyst according to any one of the prior claims, comprising 70-99.5% by weight, 80-98% by weight, 80-95% by weight, 85-98% by weight, 85-95% by weight, 90-99.5% by weight, or 90-98% by weight of the silica.

20. An olefin polymerization process comprising contacting a chromium titanate / silica catalyst and an optional co-catalyst described in any one of claims 7 to 19 with an olefin monomer and an optional olefin co-monomer in a polymerization reactor system under polymerization conditions to produce an olefin polymer.

21. A process for preparing a titaniumated silica support, the following: (i) Contacting water, a peroxide compound, a titanium precursor, and silica to form a first mixture; (ii) Isolating the solid fraction from the first mixture; (iii) The process comprising drying the solid fraction to form the titrated silica support.

22. Step (i) includes contacting the water, hydrogen peroxide, alkali metal precursor and / or zinc precursor, titanium precursor, and silica to form the first mixture; The first mixture is brought into contact with a nitrogen-containing compound to form a second mixture; The second mixture is subjected to a reaction temperature in the range of 40 to 270°C before isolating the solid fraction; and The process according to claim 21, wherein the solid fraction is washed before drying the solid fraction.

23. Step (i) includes contacting the water, hydrogen peroxide, alkali metal precursor and / or zinc precursor, titanium precursor, and silica to form the first mixture; The first mixture is subjected to a reaction temperature in the range of 40 to 270°C before isolating the solid fraction; and The process according to claim 21, wherein the solid fraction is washed before drying the solid fraction.

24. The process according to any one of claims 21 to 23, wherein the molar ratio of the peroxide compound or the hydrogen peroxide to the titanium precursor is 0.5:1 to 100:1, 2:1 to 50:1, 3:1 to 20:1, or 5:1 to 11:

1.

25. The process according to any one of claims 22 to 24, wherein the molar ratio of the alkali metal of the alkali metal precursor or the zinc of the zinc precursor to the titanium of the titanium precursor is 0.1:1 to 300:1, 0.2:1 to 100:1, 0.5:1 to 20:1, 0.7:1 to 10:1, 1:1 to 5:1, or 1:1 to 3:

1.

26. The weight ratio of titanium in the titanium precursor to water (Ti:H 2 The process according to any one of claims 21 to 25, wherein O) is 0.0001:1 to 0.02:1, 0.001:1 to 0.02:1, 0.005:1 to 0.02:1, or 0.03:1 to 0.07:

1.

27. The weight ratio of the silica to the water (silica:H 2 The process according to any one of claims 21 to 26, wherein O) is 0.001:1 to 1:1, 0.01:1 to 0.5:1, 0.05:1 to 0.4:1, or 0.1:1 to 0.3:

1.

28. The process according to any one of claims 22 to 27, wherein the weight ratio of the nitrogen-containing compound to the titanium precursor is 5:1 to 300:1, 10:1 to 200:1, 25:1 to 150:1, or 50:1 to 100:

1.

29. The process according to any one of claims 21 to 28, further comprising the step of adjusting the pH of the first mixture to within the range of 3 to 12, 3 to 10, 4 to 12, 4 to 10, 6 to 10, or 8 to 10.

30. The titanium precursor is titanium carboxylate, titanium halide, titanium oxide, titanium hydroxide, titanium alkoxide, titanium nitrate, titanium sulfate, or TiOSO 4 The process according to any one of claims 21 to 29, including, or any combination thereof.

31. The process according to any one of claims 21 to 30, wherein the silica is pre-formed silica.

32. The process according to any one of claims 21 to 30, wherein the silica is silica hydrogel.

33. The process according to any one of claims 21 to 32, wherein the first mixture prior to step (ii) is subjected to a reaction temperature in the range of 40 to 270°C, 60 to 260°C, 80 to 220°C, 40 to 100°C, 60 to 100°C, 70 to 100°C, or 80 to 100°C, or the reaction temperature is in the range of 40 to 270°C, 60 to 260°C, 80 to 220°C, 40 to 100°C, 60 to 100°C, 70 to 100°C, or 80 to 100°C.

34. The process according to any one of claims 21 to 33, wherein isolating the solid fraction comprises filtration, sedimentation, decantation, compression, centrifugation, cyclone treatment, hydrocyclone treatment, or any combination thereof.

35. The process according to any one of claims 22 to 34, wherein step (i) comprises the alkali metal precursor, the alkali metal precursor comprising sodium.

36. The titanium silica support prepared by the process described in any one of claims 21 to 35.

37. The titrated silica carrier prepared by a process according to any one of claims 21 to 35, wherein the carrier is according to any one of claims 1, 5 to 6, or 12 to 19.

38. A process for preparing a chromium titanate / silica pre-catalyst, the following: Performing a process for preparing a titaniumated silica support according to any one of claims 21 to 35; and The process comprising contacting a chromium precursor with the first mixture or the second mixture before isolating the solid fraction.

39. A process for preparing a chromium titanate / silica pre-catalyst, the following: Performing a process for preparing a titaniumated silica support according to any one of claims 21 to 35; and The process comprising, after isolating the solid fraction, contacting the solid fraction with a chromium precursor.

40. A process for preparing a chromium titanate / silica pre-catalyst, the following: The process comprises performing a process for preparing a titrated silica support according to any one of claims 21 to 35, wherein instead of contacting the silica to form the first mixture, a chromium / silica pre-catalyst is contacted to form the first mixture.

41. The chromium titanate / silica precatalyst prepared by the process described in any one of claims 38 to 40.

42. The chromium titanate / silica precatalyst prepared by the process described in any one of claims 38 to 40, wherein the precatalyst is the one described in any one of claims 2 to 6 or 12 to 19.

43. A process for preparing a chromium titanide / silica catalyst, the following: Performing a process for preparing a chromium titanate / silica pre-catalyst according to any one of claims 38 to 40; and The process comprising activating the chromium titanate / silica pre-catalyst to form the chromium titanate / silica catalyst.

44. The chromium titanate / silica catalyst manufactured by the process described in claim 43.

45. The chromium titanate / silica catalyst manufactured by the process described in claim 43, wherein the catalyst is the catalyst described in any one of claims 7 to 19.