Microwave-band electromagnetic wave absorbing material and method for manufacturing the same
A solid-phase reaction process creates W-type hexaferrite with controlled ion content, addressing the lack of suitable materials for 5G communication by enhancing electromagnetic wave absorption in the 26.5-40 GHz range, thus mitigating interference.
Patent Information
- Application Number
- JP2026523172
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-04-08
- Filing Date
- 2024-05-14
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional electromagnetic wave absorbing materials, such as Ni-Zn ferrite and Mn-Zn ferrite, are unsuitable for the high-frequency bands required by 5G communication due to low magnetic anisotropy, leading to electromagnetic interference (EMI) issues, and there is a shortage of suitable materials for the 28GHz band.
A method for producing an electromagnetic wave absorbing material containing W-type hexaferrite with a specific chemical composition (CaBaSrReCoFeO₂₇) and controlled ion content, using a solid-phase reaction process involving mixing precursors, heat treatments, and ball-milling to achieve high magnetic anisotropy and ferromagnetic resonance in the 26.5-40 GHz range.
The method produces a material with excellent absorption characteristics in the 5G Ka-band (26.5-40 GHz) by adjusting ferromagnetic resonance frequency, providing effective electromagnetic interference mitigation.
Smart Images

Figure 2026538997000001_ABST
Abstract
Description
[Technical Field]
[0001] This invention relates to an electromagnetic wave absorbing material and a method for producing the same, and more specifically, Fe 2+ This invention relates to a method for manufacturing an electromagnetic wave absorbing material for the Ka-band (26.5-40 GHz band), which is the 5G communication area, and contains W-type hexaferrite that does not contain ions or contains only a very small amount of ions. [Background technology]
[0002] With the advancement of information and communication technology, the development of next-generation technologies such as autonomous vehicles, the Internet of Things (IoT), smartphones, artificial intelligence (AI), and virtual reality is progressing rapidly.
[0003] Furthermore, the miniaturization of electronic devices and the increasing frequency of usable operating frequencies are leading to a rapid increase in the amount of data and communication volume being processed. Consequently, as communication between electronic devices becomes more complex and diverse, problems such as communication errors due to frequency interference are becoming apparent, increasing the need for electromagnetic shielding and absorption.
[0004] Hexaferrite possesses high magnetic anisotropy, making it a suitable material for electromagnetic wave absorption in the GHz frequency range. Therefore, for stable communication of electronic devices in the Ka-band (26.5-40 GHz band), which is the 5G communication band, electromagnetic interference must be eliminated. For this reason, the use of hexaferrite, which exhibits excellent absorption characteristics in frequency bands of several to tens of GHz, is gradually increasing in 5G communication technology.
[0005] However, in conventional systems, with the increase in electronic devices and communication traffic, electromagnetic interference (EMI) problems have emerged, which can cause signal interference from peripheral devices, potentially degrading performance or leading to malfunctions.
[0006] In particular, electronic devices closely related to daily life, such as unmanned aerial vehicles, autonomous vehicles, and bio-implantable sensors, can cause serious problems.
[0007] To mitigate such EMI problems, electromagnetic compatibility (EMC), an international standard, has been legalized as a mandatory regulation. Therefore, one method introduced from the product design stage to meet EMC standards is electromagnetic shielding and absorption technology, which blocks the ingress and egress of electromagnetic waves. This is used to minimize the emission of unwanted electromagnetic waves from the final product and maximize the equipment's resistance to unwanted electromagnetic waves.
[0008] However, as the operating frequency gradually shifts to higher frequency bands, conventional materials such as Ni-Zn ferrite, Mn-Zn ferrite, and Sendust are unsuitable as electromagnetic shielding and absorption materials in the several to tens of GHz band due to their low magnetic anisotropy in their crystal structure.
[0009] Currently, with the advent of fifth-generation mobile communication (5G), the need for electromagnetic wave absorbing materials in the 3.5GHz and 28GHz bands is increasing, and the demand for absorbing materials in the 28GHz band is particularly high, but there is a shortage of suitable materials. [Prior art documents] [Patent Documents]
[0010] [Patent Document 1] Korean Registered Patent No. 10-2621490 [Overview of the project] [Problems that the invention aims to solve]
[0011] The problem that this invention aims to solve is to provide a method for manufacturing an electromagnetic wave absorbing material. The electromagnetic wave absorbing material is Fe 2+It contains W-type hexaferrite that contains no ions or contains only a very small amount of ions. Further, the electromagnetic wave absorbing material is for the Ka band (26.5 to 40 GHz band) which is the 5G communication region.
[0012] The problem to be solved by the present invention is not limited to the problems mentioned above, and other problems not mentioned will be clearly understood by those of ordinary skill in the art to which the present invention pertains from the following description. [MEANS FOR SOLVING THE PROBLEM]
[0013] To achieve the above object, one embodiment of the present invention provides a method for producing an electromagnetic wave absorbing material.
[0014] A method for producing an electromagnetic wave absorbing material according to an embodiment of the present invention comprises:
[0015] a step of mixing powders containing at least one selected from the group consisting of a Ca precursor, a Ba precursor, a Sr precursor, a Re precursor, a Me precursor, a Co precursor, and a Fe precursor; a step of subjecting the mixed powder to a first heat treatment; a step of ball-milling the heat-treated powder; a step of subjecting the ball-milled powder to a second heat treatment;
[0016] and can produce an electromagnetic wave absorbing material containing W-type hexaferrite represented by the following Chemical Formula 1.
[0017] [Chemical Formula 1] Ca a Ba b Sr 1-a-b-c Re c Co 2+ x Me 2+ 2-x Fe 3+ 16 O 27
[0018] In the above chemical formula 1, Re is at least one selected from the group consisting of rare earth elements, and Me 2+ x is at least one selected from the group consisting of divalent transition metals, where a is a value between 0.0 and 1.0, b is a value between 0.0 and 1.0, c is a value between 0.0 and 1.0, and x is a value between 0.0 and 2.0.
[0019] Furthermore, according to one embodiment of the present invention, the method for manufacturing an electromagnetic wave absorbing material is characterized in that, in the chemical formula 1, x is a value of 0.0 or more and 0.3 or less.
[0020] Furthermore, according to one embodiment of the present invention, in the chemical formula 1, Me 2+ is Zn 2+ Fe 2+ Ni 2+ Mn 2+ , and Mg 2+ The method for producing an electromagnetic wave absorbing material is characterized by being at least one selected from the group consisting of the following.
[0021] Furthermore, according to one embodiment of the present invention, in the chemical formula 2, Me 2+ is Zn 2+ Fe 2+ Ni 2+ Mn 2+ , and Mg 2+ The method for producing an electromagnetic wave absorbing material is characterized by being at least one selected from the group consisting of the following.
[0022] Furthermore, according to one embodiment of the present invention, the first heat treatment step may be performed in a temperature range of 1200°C to 1400°C, which may be a method for manufacturing an electromagnetic wave absorbing material.
[0023] Furthermore, according to one embodiment of the present invention, the W-type hexaferrite represented by chemical formula 1 contains Fe in proportion to 2 moles of the total divalent transition metal contained in chemical formula 1. 2+ The method for producing an electromagnetic wave absorbing material is also characterized by having an ion content of 0.5 moles or less.
[0024] Furthermore, according to one embodiment of the present invention, the second heat treatment step may be a method for manufacturing an electromagnetic wave absorbing material, characterized in that it is performed in a temperature range of 1200°C to 1400°C.
[0025] Furthermore, according to one embodiment of the present invention, the second heat treatment step may be characterized by being performed by sintering in air, which is a method for manufacturing an electromagnetic wave absorbing material.
[0026] To achieve the aforementioned objectives, another embodiment of the present invention provides an electromagnetic wave absorbing material.
[0027] An electromagnetic wave absorbing material according to one embodiment of the present invention may be an electromagnetic wave absorbing material characterized by containing W-type hexaferrite represented by the following chemical formula 1.
[0028] [C1] Ca a Ba b Sr 1-a-b-c Re c Co 2+ x Me 2+ 2-x Fe 3+ 16 O 27
[0029] In the above chemical formula 1, Re is at least one selected from the group consisting of rare earth elements, and Me 2+ x is at least one selected from the group consisting of divalent transition metals, where a is a value between 0.0 and 1.0, b is a value between 0.0 and 1.0, c is a value between 0.0 and 1.0, and x is a value between 0.0 and 2.0.
[0030] Furthermore, according to one embodiment of the present invention, the W-type hexaferrite represented by chemical formula 1 contains Fe in proportion to 2 moles of the total divalent transition metal contained in chemical formula 1. 2+ The electromagnetic wave absorbing material may also be characterized by having an ion content of 0.5 moles or less.
[0031] Furthermore, according to one embodiment of the present invention, the electromagnetic wave absorbing material may be characterized by having a ferromagnetic resonance frequency in the range of 26.5 GHz to 40 GHz.
[0032] Furthermore, according to one embodiment of the present invention, the electromagnetic wave absorbing material may be characterized in that, in the chemical formula 1, x is a value of 0.0 or more and 0.3 or less.
[0033] Furthermore, according to one embodiment of the present invention, the electromagnetic wave absorbing material may be characterized by having a thickness range of 0.97 mm to 1.05 mm.
[0034] Furthermore, according to one embodiment of the present invention, in the chemical formula 1, the Me 2+ is, Zn 2+ Fe 2+ Ni 2+ Mn 2+ , and Mg 2+ The electromagnetic wave absorbing material may be characterized by being at least one selected from the group consisting of the following. [Effects of the Invention]
[0035] According to one embodiment of the present invention, Fe 2+ This invention provides a method for manufacturing an electromagnetic wave absorbing material for the Ka-band (26.5~40GHz), which is the 5G communication band, containing W-type hexaferrite that contains a very small amount of ions.
[0036] According to one embodiment of the present invention, Me in W-type hexaferrite 2+ Zn on the site 2+ Co 2+ Ni 2+ Mn 2+ Cu 2+ Mg 2+ By substituting ions such as those mentioned above, a method for manufacturing an electromagnetic wave absorber containing W-type hexaferrite having high complex dielectric constant and complex permeability in the high-frequency range can be provided.
[0037] According to one embodiment of the present invention, it is possible to provide a compositional design that adjusts the ferromagnetic resonance frequency to have excellent absorption capability in the Ka-band (26.5~40GHz), which is the 5G communication band.
[0038] The effects of the present invention are not limited to those mentioned above, but should be understood to include all effects that can be inferred from the configuration of the invention as described in the specification or claims. [Brief explanation of the drawing]
[0039] [Figure 1] This is a flowchart showing a method for manufacturing an electromagnetic wave absorbing material containing W-type hexaferrite according to one embodiment of the present invention. [Figure 2a] This graph shows the complex permeability and complex dielectric constant (powder volume fraction 30%) of an electromagnetic wave absorbing material according to one embodiment of the present invention, with respect to changes in Co2+ content. [Figure 2b] This graph shows the complex permeability and complex dielectric constant (powder volume fraction 30%) of an electromagnetic wave absorbing material according to one embodiment of the present invention, with respect to changes in Co2+ content. [Figure 3a] This graph shows the regression analysis results of ferromagnetic resonance frequencies as CO2+ content changes in an electromagnetic wave absorbing material according to one embodiment of the present invention. [Figure 3b] This graph shows the regression analysis results of ferromagnetic resonance frequencies as CO2+ content changes in an electromagnetic wave absorbing material according to one embodiment of the present invention. [Figure 4] This graph shows the absorption characteristics (minimum reflection loss) of a composite sheet as the Co2+ content changes in an electromagnetic wave absorbing material according to one embodiment of the present invention. [Figure 5] This graph shows the absorption characteristics of a composite sheet as the thickness of an electromagnetic wave absorbing material changes, according to one embodiment of the present invention. [Figure 6a] This graph shows the absorption characteristics of a composite sheet (contour plot of absorption characteristics with respect to thickness and frequency) of an electromagnetic wave absorbing material according to one embodiment of the present invention, depending on the change in Co2+ content. [Figure 6b] This graph shows the absorption characteristics of a composite sheet (contour plot of absorption characteristics with respect to thickness and frequency) of an electromagnetic wave absorbing material according to one embodiment of the present invention, depending on the change in Co2+ content. [Figure 6c] This graph shows the absorption characteristics of a composite sheet (contour plot of absorption characteristics with respect to thickness and frequency) of an electromagnetic wave absorbing material according to one embodiment of the present invention, depending on the change in Co2+ content. [Figure 6d] This graph shows the absorption characteristics of a composite sheet (contour plot of absorption characteristics with respect to thickness and frequency) of an electromagnetic wave absorbing material according to one embodiment of the present invention, depending on the change in Co2+ content. [Figure 6e] This graph shows the absorption characteristics of a composite sheet (contour plot of absorption characteristics with respect to thickness and frequency) of an electromagnetic wave absorbing material according to one embodiment of the present invention, depending on the change in Co2+ content. [Figure 6f] This graph shows the absorption characteristics of a composite sheet (contour plot of absorption characteristics with respect to thickness and frequency) of an electromagnetic wave absorbing material according to one embodiment of the present invention, depending on the change in Co2+ content. [Figure 6g] This graph shows the absorption characteristics of a composite sheet (contour plot of absorption characteristics with respect to thickness and frequency) of an electromagnetic wave absorbing material according to one embodiment of the present invention, depending on the change in Co2+ content. [Figure 7a] This graph shows the complex permeability (epoxy powder volume fraction 30%) as the content of (Fe2+, Mg2+, Mn2+, Ni2+)-Co2+ changes. [Figure 7b] This graph shows the complex permeability (epoxy powder volume fraction 30%) as the content of (Fe2+, Mg2+, Mn2+, Ni2+)-Co2+ changes. [Figure 7c] This graph shows the complex permeability (epoxy powder volume fraction 30%) as the content of (Fe2+, Mg2+, Mn2+, Ni2+)-Co2+ changes. [Figure 7d] This graph shows the complex permeability (epoxy powder volume fraction 30%) as the content of (Fe2+, Mg2+, Mn2+, Ni2+)-Co2+ changes. [Figure 8] This is a regression analysis graph of ferromagnetic resonance frequencies as the content of various divalent transition metals and Co2+ ions changes. [Modes for carrying out the invention]
[0040] The present invention will be described below with reference to the attached drawings. However, the present invention can be carried out in many different forms and should not be construed as being limited to the embodiments described herein. Rather, these embodiments are provided to ensure that this disclosure is thorough and complete and to fully convey the scope of the invention to those skilled in the art.
[0041] In the drawings, parts not relevant to the description have been omitted in order to clearly illustrate the present invention, and similar parts are denoted by similar reference numerals throughout the specification.
[0042] Throughout the specification, when a part is described as being "connected (linked, in contact with, joined)" to another part, this includes not only cases where they are "directly connected" but also cases where they are "indirectly connected" through other components in between.
[0043] Furthermore, when a layer, membrane, region, or plate is said to be "on top of" another part, this includes not only cases where it is "directly above" the other part, but also cases where the other part is interposed between them. In this specification, when a layer, membrane, region, or plate is said to be formed "on top of" another part, the direction of formation is not limited to upward, but also includes cases where it is formed laterally or downward. Conversely, when a layer, membrane, region, or plate is said to be "below" another part, this includes not only cases where it is "directly below" the other part, but also cases where the other part is interposed between them.
[0044] In this specification, "top surface" and "bottom surface" are used as relative concepts to facilitate understanding of the technical concept of the present invention. Therefore, "top surface" and "bottom surface" do not refer to any particular direction, position, or component, and are interchangeable with each other.
[0045] For example, "top surface" can be interpreted as "bottom surface," and "bottom surface" can be interpreted as "top surface." Therefore, "top surface" can be expressed as "first" and "bottom surface" as "second," or "bottom surface" as "first" and "top surface" as "second." However, "top surface" and "bottom surface" are not used interchangeably within a single embodiment.
[0046] Unless otherwise specified, all terms used herein (including technical and scientific terms) have the same meaning as those generally understood by a person of ordinary skill in the art to which this invention pertains. Furthermore, terms defined in commonly used dictionaries, etc., shall be interpreted as having the meaning consistent with their meaning in the context of the relevant art, and shall not be interpreted in an idealized or overly formal sense unless expressly defined herein.
[0047] Furthermore, when a part is said to "contain" a particular component, unless otherwise specified, it does not mean that other components are excluded, but rather that it may contain other components.
[0048] The terms used herein are for the purpose of describing specific embodiments and do not limit the invention. In this specification, the singular form includes the plural form unless the context makes it clear otherwise. Furthermore, the terms “contains” and / or “contains,” as used herein, identify the presence of the described features, integers, processes, operations, elements, and / or components, and do not exclude the presence or addition of one or more other features, integers, processes, operations, elements, components, and / or groups thereof.
[0049] Embodiments of the present invention will be described in detail below with reference to the attached drawings.
[0050] Figure 1 is a flowchart showing a method for manufacturing an electromagnetic wave absorbing material containing W-type hexaferrite according to one embodiment of the present invention.
[0051] Referring to Figure 1, a method for manufacturing an electromagnetic wave absorbing material according to one embodiment of the present invention will be described.
[0052] As an example of this embodiment, a method for producing an electromagnetic wave absorbing material containing W-type hexaferrite represented by the following chemical formula 1 includes the steps of: mixing powders; performing a first heat treatment on the mixed powders; ball milling the heat-treated powders; and performing a second heat treatment on the ball-milled powders. Here, the powders include at least one selected from the group consisting of Ca precursor, Ba precursor, Sr precursor, Re precursor, Me precursor, Co precursor, and Fe precursor.
[0053] [C1] Ca a Ba b Sr 1-a-b-c Re c Co 2+ x Me 2+ 2-x Fe 3+ 16 O 27
[0054] In the above chemical formula 1, Re is at least one selected from the group consisting of rare earth elements, and Me 2+ x is at least one selected from the group consisting of divalent transition metals, where a is a value between 0.0 and 1.0, b is a value between 0.0 and 1.0, c is a value between 0.0 and 1.0, and x is a value between 0.0 and 2.0.
[0055] In this context, hexaferrite is a magnetic material with a hexagonal crystal structure and high magnetic anisotropy, making it a material with high potential for application as an electromagnetic wave absorber in the high-frequency range of the GHz band.
[0056] Furthermore, hexaferrites exist in various types depending on their chemical composition, and among them, W-type hexaferrite has magnetic anisotropy in the c-axis direction, making it more likely to be used as an absorber in higher GHz bands compared to other hexaferrites.
[0057] As an example of this embodiment, in the chemical formula 1, Me 2+ is Zn 2+ Fe 2+ Ni 2+ Mn 2+ , and Mg 2+ The method for manufacturing an electromagnetic wave absorbing material may be at least one selected from the group consisting of the following.
[0058] In this embodiment, Me in W-type hexaferrite 2+ Zn on the site 2+ Fe 2+ Ni 2+ Mn 2+ Mg 2+ By substituting ions such as those mentioned above, a method for manufacturing an electromagnetic wave absorber containing W-type hexaferrite having high complex dielectric constant and complex permeability in the high-frequency range can be provided.
[0059] Furthermore, by providing a compositional design that adjusts the ferromagnetic resonance frequency to have excellent absorption capabilities in the Ka-band (26.5~40GHz), which is the 5G communication band, it is possible to clarify the correlation between absorption characteristics and ferromagnetic resonance frequency.
[0060] Ferromagnetic resonance is a phenomenon in which, when a magnetic material is exposed to microwave electromagnetic waves, its magnetic spins begin to precess, absorbing electromagnetic waves in a specific region. The ferromagnetic resonance frequency is the frequency at which this occurs.
[0061] The reason for adjusting the ferromagnetic resonance frequency, as mentioned above, is that it allows for the creation of electromagnetic wave absorbing materials with excellent absorption characteristics in the desired frequency band.
[0062] The composition of W-type hexaferrite is generally Sr(or Ba)Me2Fe 16 O 27 Here, Me is Mn 2+ Zn 2+ Mg 2+ Ni 2+Co 2+ Cu 2+ This represents divalent metal ions such as [examples of divalent metal ions].
[0063] Referring to Figure 1, we can see that the process for producing an electromagnetic wave absorbing material containing W-type hexaferrite represented by chemical formula 1 is as follows: a step of mixing a powder containing at least one selected from the group consisting of Ca precursor, Ba precursor, Sr precursor, Re precursor, Me precursor, Co precursor, and Fe precursor (S10); a step of performing a first heat treatment on the mixed powder (S20); a step of ball milling the heat-treated powder (S30); and a step of performing a second heat treatment on the ball-milled powder (S40).
[0064] In this embodiment, as an example, SrCO3 can be used as the Sr precursor, Fe2O3 as the Fe precursor, CoO as the Co precursor, and MeO as the Me precursor.
[0065] Referring to Figure 1, we can see the process for producing W-type hexaferrite substituted with divalent transition metal ions using precursor powders such as SrCO3, Fe2O3, CoO, MeO, and MeO.
[0066] The manufacturing method used in this case is a solid-phase reaction method.
[0067] When performing the first heat treatment step (S20), the sample may be in powder or pellet form.
[0068] In the step of ball milling the heat-treated powder (S30), a conventional pulverizer using beads can be used for ball milling.
[0069] Basically, in chemical formula 1, x may have a value between 0.0 and 2.0,
[0070] More preferably, the method for manufacturing an electromagnetic wave absorbing material is one in which x is a value of 0.0 or more and 0.3 or less.
[0071] Hereinafter, as can be confirmed in the experimental examples, Co 2+ As the content of increases, the ferromagnetic resonance frequency gradually shifts to the lower frequency band, and when the value of x is in the range of 0.0 to 0.3, a ferromagnetic resonance frequency value around 28 GHz can be confirmed.
[0072] Most preferably, in the method for producing an electromagnetic wave absorbing material, x may be a value of 0.25 or more and 0.3 or less.
[0073] When the range of x is 0.25 or more and 0.3 or less, the absorption characteristics for the target frequency of 28 GHz are the most excellent.
[0074] As an example of the present embodiment, Re (rare earth element) may be at least one selected from the group consisting of La, Ce, and Y.
[0075] As an example of the present embodiment, in the step of forming powder, when only the powders of the Ba precursor, Me precursor, Co precursor, and Fe precursor are mixed, an electromagnetic wave absorbing material containing W-type hexaferrite represented by the following Chemical Formula 2 can be produced instead of Chemical Formula 1.
[0076] [Chemical Formula 2] BaCo 2+ x Me 2+ 2-x Fe 3+ 16 O 27
[0077] In the Chemical Formula 2, Me 2+ is at least one selected from the group consisting of divalent transition metals, and x is a value of 0.0 or more and 2.0 or less.
[0078] As another example of the present embodiment, in the step of forming powder, when only the powders of the Sr precursor, Me precursor, Co precursor, and Fe precursor are mixed, an electromagnetic wave absorbing material containing W-type hexaferrite represented by the following Chemical Formula 3 can be produced instead of Chemical Formula 1.
[0079] [Chemical Formula 3] SrCo 2+ x Me 2+ 2-x Fe 3+ 16 O 27
[0080] In the aforementioned Chemical Formula 3, Me 2+ is at least one selected from the group consisting of divalent transition metals, and x is a value of 0.0 or more and 2.0 or less.
[0081] As an example of the present embodiment, in the aforementioned Chemical Formula 2, Me 2+ may be at least one selected from the group consisting of divalent transition metals, in the method for producing an electromagnetic wave absorbing material.
[0082] Different from Chemical Formula 2 and Chemical Formula 3, the W-type hexaferrite represented by Chemical Formula 1 includes a configuration in which not only the Sr element and Ba element are present, but all of Ba and Re (rare earth element) are present.
[0083] In Chemical Formula 1, when a, c, and b are 0, it is the same as Chemical Formula 3,
[0084] In Chemical Formula 1, when a and c are 0 and b is 1, it is the same as Chemical Formula 2.
[0085] More preferably, a may be a value of 0 or more and 0.5 or less.
[0086] More preferably, b may be a value of 0 or more and 1.0 or less.
[0087] More preferably, c may be a value of 0 or more and 0.5 or less.
[0088] As an example of this embodiment, the first heat treatment step may be performed in a temperature range of 1200°C to 1400°C in a method for manufacturing electromagnetic wave absorbing materials.
[0089] The first heat treatment step can be carried out by calcination.
[0090] Furthermore, the first heat treatment step can be performed in air and can be carried out for a period of 5 to 7 hours.
[0091] At this point, if the first heat treatment step is performed at a temperature of less than 1200°C, there is a problem in that the crystalline phases of W-type hexaferrite, M-type hexaferrite, and spinelferrite are formed in a mixed state.
[0092] As the heat treatment temperature increases, the M-type and spinel ferrite phases can be synthesized into the W-type hexaferrite phase at around 1300°C.
[0093] Conversely, if the second heat treatment process is carried out at a temperature exceeding 1400°C, magnetite and the liquid phase will exist, making phase synthesis difficult.
[0094] As an example of this embodiment, the W-type hexaferrite represented by chemical formula 1 contains Fe in proportion to 2 moles of the total divalent transition metal contained in chemical formula 1. 2+ The method for producing an electromagnetic wave absorbing material is also characterized by having an ion content of 0.5 moles or less.
[0095] In this case, the second heat treatment step can be carried out in a temperature range of 1200°C to 1400°C, and the second heat treatment step can be carried out by sintering in air.
[0096] At this point, if the second heat treatment step is performed at a temperature of less than 1200°C, there is a problem in that the crystalline phases of W-type hexaferrite, M-type hexaferrite, and spinelferrite are formed in a mixed state.
[0097] As the heat treatment temperature increases, the M-type and spinel ferrite phases can be synthesized into the W-type hexaferrite phase at around 1300°C.
[0098] Conversely, if the second heat treatment process is carried out at a temperature exceeding 1400°C, the magnetite and liquid phases will exist, making phase synthesis difficult.
[0099] Furthermore, the second heat treatment step can be carried out by sintering in an atmospheric environment.
[0100] Conventionally, the W type is generally a high-temperature stable phase, and in air, Fe 2+ Ions Fe 3+ Because it is easily oxidized by ions and undergoes phase decomposition, it was necessary to perform heat treatment at a low oxygen partial pressure.
[0101] However, in this embodiment, Fe is used for a total of 2 moles of divalent transition metals contained in chemical formula 1. 2+ Because the ion content is 0.5 moles or less, it has the advantage of being able to undergo heat treatment even in air.
[0102] For a total of 2 moles of divalent transition metals contained in chemical formula 1, Fe 2+ When the ion content is 0.5 moles or more, a stable W-type hexaferrite phase can be synthesized without phase decomposition, provided that a gas control or rapid cooling process is involved. Compared to processes that require adjustment of oxygen partial pressure, the second heat treatment step has the advantage of reducing process costs because it does not require additional gas control.
[0103] Another embodiment of the electromagnetic wave absorbing material of the present invention will be described.
[0104] Since the electromagnetic wave absorbing material is an invention of a different category having substantially the same technical characteristics as the method for manufacturing the electromagnetic wave absorbing material described above,
[0105] The method described in the above-mentioned explanation of how to manufacture electromagnetic wave absorbing materials can be applied directly.
[0106] As an example of this embodiment, an electromagnetic wave absorbing material may be characterized by containing W-type hexaferrite represented by the following chemical formula 1.
[0107] [C1] Ca a Ba b Sr 1-a-b-c Re c Co 2+ x Me 2+ 2-x Fe 3+ 16 O 27
[0108] In the above chemical formula 1, Re is at least one selected from the group consisting of rare earth elements, and Me 2+ x is at least one selected from the group consisting of divalent transition metals, where a is a value between 0.0 and 1.0, b is a value between 0.0 and 1.0, c is a value between 0.0 and 1.0, and x is a value between 0.0 and 2.0.
[0109] As an example of this embodiment, an electromagnetic wave absorbing material may be characterized by containing W-type hexaferrite represented by the following chemical formula 2.
[0110] [Case 2] BaCo 2+ x Me 2+ 2-x Fe 3+ 16 O 27
[0111] In the above chemical formula 2, Me 2+x is at least one selected from the group consisting of divalent transition metals, and x is a value between 0.0 and 2.0.
[0112] Another example of this embodiment is an electromagnetic wave absorbing material characterized by containing W-type hexaferrite represented by the following chemical formula 3.
[0113] [C3] SrCo 2+ x Me 2+ 2-x Fe 3+ 16 O 27
[0114] In the above chemical formula 3, Me 2+ x is at least one selected from the group consisting of divalent transition metals, and x is a value between 0.0 and 2.0.
[0115] Unlike chemical formulas 2 and 3, W-type hexaferrite represented by chemical formula 1 has a composition that contains not only Sr and Ba elements, but also Ba and Re (rare earth elements).
[0116] In chemical formula 1, if a, c, and b are 0, it becomes the same as chemical formula 3.
[0117] In chemical formula 1, if a and c are 0 and b is 1, it becomes the same as chemical formula 2.
[0118] More preferably, a may be a value between 0 and 0.5.
[0119] More preferably, b may be a value between 0 and 1.0.
[0120] More preferably, c may be a value between 0 and 0.5.
[0121] As an example of this embodiment, the W-type hexaferrite represented by chemical formula 1 contains Fe in proportion to 2 moles of the total divalent transition metal contained in chemical formula 1. 2+ Ion content The electromagnetic wave absorbing material may be characterized by having a concentration of 0.5 moles or less.
[0122] As an example of this embodiment, the electromagnetic wave absorbing material may be characterized by having a ferromagnetic resonance frequency in the range of 26.5 GHz to 40 GHz.
[0123] As an example of this embodiment, the electromagnetic wave absorbing material may be one in which x in the chemical formula 1 is a value of 0.0 or more and 0.3 or less.
[0124] As an example of this embodiment, an electromagnetic wave absorbing material may be provided, characterized by having a thickness range of 0.97 mm to 1.05 mm.
[0125] As an example of this embodiment, in the chemical formula 1, Me 2+ is Zn 2+ Fe 2+ Ni 2+ Mn 2+ , and Mg 2+ It may be an electromagnetic wave absorbing material, which is at least one selected from the group consisting of the following.
[0126] As an example of this embodiment, Re (rare earth element) may be at least one selected from the group consisting of La, Ce, and Y.
[0127] The characteristics of the electromagnetic wave absorbing material according to this embodiment will be explained in detail through the following experimental examples.
[0128] Manufacturing Example 1. Electromagnetic wave absorbing material (SrCo) according to one embodiment of the present invention x Zn 2-x Fe 16 O 27 ).
[0129] This uses SrCO3, Fe2O3, CoO, ZnO, and ZnO precursor powders. This shows the manufacturing process for W-type hexaferrite substituted with divalent transition metal ions. The manufacturing method used is a solid-phase reaction method, and the sample may be in powder or pellet form during calcination.
[0130] For the ball mill, a conventional grinding machine using beads was used.
[0131] 1. Ball mill 1 mole of SrCO3, x moles of CoO, (2-x) moles of ZnO, and 8 moles of Fe2O3 precursor powder for 24 hours.
[0132] The total weight of these materials is 20g. Each material was prepared by adjusting the value of x, and the values applied to the x-value are listed below.
[0133] 2. Pre-bake in air at a temperature of 1250°C for 6 hours.
[0134] 3. After that, ball milling is performed again for 24 hours.
[0135] 4. Sinter again in air at a temperature of 1300°C for 2 hours.
[0136] Zirconia balls were used for grinding, and the weight of the zirconia balls was set at 240g, which is 12 times the weight of the precursor, based on a precursor weight of 20g.
[0137] Three types of balls with diameters of 1 mm, 0.5 mm, and 0.3 mm were used, with 80 g of each diameter ball being used.
[0138] The ball milling temperature and rpm were based on 150 rpm at room temperature.
[0139] Through this process, SrCo x Zn 2-x Fe 16 O 27 Hexaferrite powder is produced.
[0140] By adjusting the amount of precursor used, the values of x were adjusted to 0.0, 0.1, 0.2, 0.225, 0.250, 0.275, and 0.3, respectively.
[0141] Experimental Example 1. Co 2+ Characteristic analysis of electromagnetic wave absorbing materials based on their content and material thickness.
[0142] Figure 2 shows the Co in an electromagnetic wave absorbing material according to one embodiment of the present invention. 2+ This graph shows the complex permeability and complex permittivity (30% powder volume fraction) as the content changes.
[0143] Figure 3 shows the Co in an electromagnetic wave absorbing material according to one embodiment of the present invention. 2+ This graph shows the regression analysis results of ferromagnetic resonance frequencies as the content changes.
[0144] Figure 4 shows the Co in an electromagnetic wave absorbing material according to one embodiment of the present invention. 2+ This graph shows the absorption characteristics (minimum reflection loss) of the composite sheet as the content changes.
[0145] Figure 5 is a graph showing the absorption characteristics of a composite sheet with varying thickness in an electromagnetic wave absorbing material according to one embodiment of the present invention.
[0146] Figure 6 shows the Co in an electromagnetic wave absorbing material according to one embodiment of the present invention. 2+ This graph shows the absorption characteristics of the composite sheet as the content changes (contour plot of absorption characteristics with respect to thickness and frequency).
[0147] Examples of experiments will be explained with reference to Figures 2-6.
[0148] Figure 2 shows SrCo related to one embodiment of the present invention. x Zn 2-x Fe 16 O 27(0≦x≦0.3) To evaluate the absorption properties of hexaferrite compositions, composite sheets were prepared for each content level by mixing with epoxy solid resin.
[0149] Various types of resins can be used as needed, including epoxy, acrylic, silicone, urethane, and paraffin wax.
[0150] To evaluate the absorption of the fabricated composite sheet, the values of the material constants, complex permeability and complex permittivity, were obtained using a network analyzer.
[0151] The ferromagnetic resonance frequency is typically determined by the complex permeability (μ). r This can be confirmed by the region of the inflection point of the real part permeability (μ') and the maximum peak of the imaginary part permeability (μ'') at (=μ'-jμ'').
[0152] Referring to Figure 2, Co 2+ As the content of increases, the ferromagnetic resonance frequency gradually shifts to a lower frequency band, Co 2+ When the content (x value) is in the range of 0.25 to 0.3, it can be confirmed that it has a ferromagnetic resonance frequency value around 28 GHz.
[0153] This can also be confirmed through Table 1 below.
[0154] [Table 1]
[0155] As mentioned above, Co 2+ As the + content increases, the ferromagnetic resonance frequency gradually shifts to a lower frequency band, Co 2+ When the content (x value) is in the range of 0.25 to 0.3, it can also be confirmed that it has a ferromagnetic resonance frequency value around 28 GHz.
[0156] In Figure 3, Co 2+The regression analysis results of ferromagnetic resonance frequencies due to changes in content can be examined.
[0157] Referring to Figure 3, similarly, Co 2+ As the content of increases, the ferromagnetic resonance frequency gradually shifts to a lower frequency band, Co 2+ When the content (x value) is in the range of 0.25 to 0.3, it can be confirmed that it has a ferromagnetic resonance frequency value around 28 GHz.
[0158] In Figure 4, Co 2+ To evaluate the absorption characteristics of the composite sheet as the content changes, impedance values were first obtained through Equation 1 below, according to transmission line theory.
[0159] Next, the impedance value was substituted into the following formula 2 to calculate the reflection loss (RL) value, which represents the absorption characteristics.
[0160]
number
[0161]
number
[0162] Referring to Figure 4, Co 2+ As the substitution content increases, the frequency at which maximum absorption capability is observed (lowest RL) shifts to a lower frequency band, which is consistent with the behavior of the ferromagnetic resonance frequency shift.
[0163] In the composition x=0.3 where the ferromagnetic resonance frequency appears at 26.9 GHz,
[0164] It demonstrated maximum absorption capability at a frequency of 27.7 GHz and excellent absorption capability of over 99.99% even at a frequency of 28 GHz.
[0165] Therefore, 2+ and Zn 2+By controlling the content, the 28GHz band Furthermore, it can be confirmed that excellent absorbers can be developed in other frequency bands besides Ka.
[0166] Figure 5 shows the absorption characteristics of the composite sheet in response to changes in the thickness of the absorbent material.
[0167] Referring to Figure 5, according to Equation 1, Z in The condition for / Z0 to be equal to 1. The absorbent material with a thickness of 1.01 mm showed the best absorption capacity, and it was confirmed that the absorption capacity decreased as the thickness changed.
[0168] In actual product development, there may be a variation of approximately 5% in thickness. Even if the difference is within a range of + / - 0.04 mm from the standard thickness of 1.01 mm, an absorption capacity of 99.0% or more will be maintained based on a 28 GHz frequency.
[0169] In Figure 6, Co 2+ The absorption characteristics of the composite sheet can be observed in response to changes in content (contour plots of absorption characteristics based on thickness and frequency).
[0170] Referring to Figure 6, Co 2+ As the content increases, the absorption peak gradually shifts to a lower frequency band. This is consistent with the shift in ferromagnetic resonance frequency observed earlier.
[0171] Table 2 below compares the absorption characteristics according to the reflection loss.
[0172] [Table 2]
[0173] Table 2 is a conversion table for reflection loss and absorptivity expressed in decibels.
[0174] In this case, if the reflection loss (RL) is 20 dB, it means that 99.0% of the electromagnetic waves incident on the absorber sample from the outside are absorbed inside the absorber, and only 1.0% are reflected to the outside.
[0175] Table 3 below shows Co 2+ This table summarizes the ferromagnetic resonance frequency, volume fraction, maximum absorption peak frequency and thickness, and frequency range above 99% absorption (-20dB) depending on the amount of substitution.
[0176] [Table 3]
[0177] To summarize the above, Co 2+ As the content of increases, the magnetic anisotropy of the C axis decreases, and the ferromagnetic resonance frequency gradually decreases.
[0178] Co 2+ It was confirmed that when the content is around 0.25 to 0.3, the ferromagnetic resonance frequency shifts to the target of around 28 GHz.
[0179] According to transmission line theory, the reflection loss value representing the absorption characteristics was calculated.
[0180] As a result, Co 2+ It was confirmed that when the content was 0.25 to 0.3 and the thickness was 0.97 mm to 1.05 mm, it exhibited an absorption characteristic of -65.5 dB at 27.7 GHz and an excellent absorption characteristic of -50.3 dB at 28.0 GHz.
[0181] Also, Co 2+ When the content is 0.3 and the volume fraction is 30%, it was confirmed that excellent absorption characteristics can be obtained between thicknesses of 0.97 mm and 1.05 mm, and the characteristics at this time were -20 dB or less, indicating an absorption rate of 99% or more.
[0182] This demonstrates that excellent absorption characteristics can be obtained by setting the ferromagnetic resonance frequency 1.0 to 1.5 GHz lower than the target frequency.
[0183] Furthermore, by changing the substitution ions and powder content, the ferromagnetic resonance frequency can be efficiently adjusted, confirming that it can be applied not only to the Ka-band (26.5~40GHz), which is the 5G communication band, but also to other application frequencies.
[0184] Experimental Example 2. Changes in ferromagnetic resonance frequency due to changes in transition metals.
[0185] SrCo 2+ x Me 2+ 2-x Fe 3+ 16 O 27 In Co 2+ Ions are fixed, Me 2+ Site Zn 2+ We observed changes in ferromagnetic resonance frequencies by substituting other applicable divalent transition metals for the ions.
[0186] Fe 2+ Mg 2+ Mn 2+ , and Ni 2+ By substituting each of these components and observing the change in ferromagnetic resonance frequency, it is possible to manufacture a magnetic composite sheet with excellent absorption characteristics at the target frequency.
[0187] Figure 7 shows (Fe 2+ Mg 2+ , Mn 2+ , Ni 2+ )-Co 2+ This graph shows the complex permeability (epoxy powder volume fraction 30%) as the content changes.
[0188] Figure 8 shows various divalent transition metals and Co 2+ This is a regression analysis graph of ferromagnetic resonance frequency in response to changes in ion content.
[0189] Table 4 below summarizes the changes in ferromagnetic resonance frequency caused by variations in transition metals.
[0190]
Table 4
[0191] Experimental Example 2 will be described with reference to Figure 7, Table 4, and Figure 8.
[0192] Referring to Figure 7 and Table 4, SrCo 2+ x Me 2+ 2-x Fe 3+ 16 O 27 where Co 2+ ions are fixed, and the Me 2+ site is substituted with divalent transition metals that are applicable in addition to Zn 2+ ions, namely Fe 2+ , Mg 2+ , Mn 2+ , and Ni 2+ , it can be confirmed that the ferromagnetic resonance frequency gradually shifts within the Ka band region in accordance with the change in composition.
[0193] This suggests that a specific ferromagnetic resonance frequency can be controlled with various compositional formulas, and the material can be applied as a filler for absorbers in applications operating at the corresponding frequency.
[0194] Referring to Figure 8, Co 2+ -Me 2+ (Fe 2+ , Zn 2+ , Mg 2+ , Mn 2+ , Ni 2+ ) It is possible to confirm the results of regression analysis of ferromagnetic resonance frequency values measured in accordance with the substituted composition.
[0195] Through Figure 8, it is possible to confirm the content range of Co 2+ for obtaining a desired ferromagnetic resonance frequency value for each material.
[0196] The foregoing description of the present invention is provided for illustrative purposes, and a person of ordinary skill in the art to which the present invention pertains will appreciate that the present invention can be easily modified into other specific embodiments without altering the technical spirit or essential features thereof. Accordingly, the above-described embodiments are illustrative in all respects and not restrictive. For example, each component described as a single unit may be implemented in a distributed manner, and similarly, components described as distributed may also be implemented in a combined form.
[0197] The scope of the present invention is indicated by the appended claims hereinafter, and all changes or modified embodiments derived from the meaning and scope of the claims as well as their equivalents are intended to be included within the scope of the present invention.
Claims
1. A step of mixing a powder containing at least one selected from the group consisting of Ca precursor, Ba precursor, Sr precursor, Re precursor, Me precursor, Co precursor, and Fe precursor, The steps include: performing a first heat treatment on the mixed powder; The process involves ball milling the heat-treated powder, The process involves performing a second heat treatment on the ball-milled powder. Includes, Chemical formula 1 below: [Chemical formula 1] Approx a Ba b Sr 1-a-b-c Re c Co 2+ x Along with 2+ 2-x Feb 3+ 16 O 27 (In the formula, Re is at least one element selected from the group consisting of rare earth elements, Me 2+ is at least one selected from the group consisting of divalent transition metals, a is a value between 0.0 and 1.
0. b is a value between 0.0 and 1.
0. c is a value between 0.0 and 1.
0. x is a value between 0.0 and 2.
0. Includes W-type hexaferrite represented by A method for manufacturing an electromagnetic wave absorbing material characterized by the following:
2. In the above chemical formula 1, x is a value between 0.0 and 0.
3. A method for producing an electromagnetic wave absorbing material according to claim 1.
3. In the above chemical formula 1, the Me 2+ is, Zn 2+ Fe 2+ Ni 2+ Mn 2+ , and Mg 2+ It is at least one selected from the group consisting of A method for producing an electromagnetic wave absorbing material according to claim 1.
4. The first heat treatment step is performed in a temperature range of 1200°C to 1400°C. A method for producing an electromagnetic wave absorbing material according to claim 1.
5. The W-type hexaferrite represented by the chemical formula 1 contains Fe in proportion to 2 moles of the total divalent transition metal contained in the chemical formula 1. 2+ The ion content is 0.5 moles or less. A method for producing an electromagnetic wave absorbing material according to claim 1.
6. The second heat treatment step is carried out in a temperature range of 1200°C to 1400°C. A method for producing an electromagnetic wave absorbing material according to claim 1.
7. The second heat treatment step described above is performed by sintering in air. A method for producing an electromagnetic wave absorbing material according to claim 1.
8. Chemical formula 2 below: [Chemical 2] Approx a Ba b Sr 1-a-b-c Re c Co 2+ x Along with 2+ 2-x Feb 3+ 16 O 27 (In the formula, Re is at least one element selected from the group consisting of rare earth elements, Me 2+ is at least one selected from the group consisting of divalent transition metals, a is a value between 0.0 and 1.
0. b is a value between 0.0 and 1.
0. c is a value between 0.0 and 1.
0. x is a value between 0.0 and 2.
0. Includes W-type hexaferrite represented by An electromagnetic wave absorbing material characterized by the following features.
9. The W-type hexaferrite represented by the chemical formula 2 contains Fe in proportion to 2 moles of the total divalent transition metal contained in the chemical formula 1. 2+ The ion content is 0.5 moles or less. The electromagnetic wave absorbing material according to claim 8.
10. It has a ferromagnetic resonance frequency in the frequency band between 26.5 GHz and 40 GHz. The electromagnetic wave absorbing material according to claim 8.
11. In the chemical formula 2 above, x is a value between 0.0 and 0.
3. The electromagnetic wave absorbing material according to claim 8.
12. In the above chemical formula 2, the Me 2+ is, Zn 2+ Fe 2+ Ni 2+ Mn 2+ , and Mg 2+ It is at least one selected from the group consisting of The electromagnetic wave absorbing material according to claim 8.
Citation Information
Patent Citations
Electromagnetic wave absorber having electromagnetic wave absorption properties in high frequency band and method for preparing the same