Polyethylene composition for improved shrink film for integrated packaging
A LDPE/HDPE polymer blend with controlled density and molecular weight ratios addresses the challenge of maintaining mechanical and optical properties in polyethylene films, enhancing stiffness and transparency for packaging applications.
Patent Information
- Application Number
- JP2026523383
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-24
- Filing Date
- 2024-10-17
- Publication Date
- 2026-11-19
AI Technical Summary
Existing polyethylene blends face a challenge in maintaining good mechanical properties such as stiffness while preserving optical properties, as increasing density to improve mechanical properties often degrades optical qualities.
A polymer blend comprising low-density polyethylene (LDPE) with a density of 0.910 to 0.925 g/cc and less than 10 wt% high-density polyethylene (HDPE) is used, balancing mechanical and optical properties by maintaining a specific density range and molecular weight ratios.
The blend achieves a surprising balance of stiffness and optical properties, with improved mechanical strength and retention of transparency, suitable for various packaging applications.
Smart Images

Figure 2026539013000001_ABST
Abstract
Description
Technical Field
[0001] (Cross-Reference to Related Applications) This application claims the benefit of European Patent Application Publication No. 23383090.0 filed on October 24, 2023, the content of which is fully incorporated herein by reference.
[0002] (Field of the Invention) The present application relates to polymer compositions, and in particular, to compositions comprising a low-density polyethylene (LDPE)-based polymer blended with a high-density polyethylene (HDPE)-based polymer.
Background Art
[0003] The use of polyolefin compositions in packaging applications is generally known. Specifically, high-density (>0.925 g / cc) low-density polyethylene (LDPE) is attractive in flexible packaging applications including collation shrink films, shrink hood films, heavy-duty shipping sack films, and industrial high-durability films, as it imparts good mechanical properties (e.g., stiffness) to the film while maintaining good optical properties.
[0004] However, it is difficult to maintain good optical properties in high-density polyethylene blends. Typically, increasing the density of polyethylene increases crystallinity, which adversely affects optical properties. Blends with HDPE increase density and improve mechanical properties such as stiffness, while often degrading optical properties.
[0005] Accordingly, there exists a need for an improved polyethylene composition that exhibits good mechanical properties and optical properties.
Summary of the Invention
[0006] Embodiments of the present disclosure meet this need by utilizing a slightly lower density (≤0.925 g / cc) LDPE-based resin and a minimal amount of HDPE (<10 wt%) to produce an LDPE / HDPE polymer composition that has a surprisingly good balance of mechanical and optical properties of the film. Without being limited by theory, maintaining the HDPE at less than 10 wt% allows the blend to possess stiffness and mechanical properties while retaining optical properties.
[0007] A first aspect includes a polymer blend comprising low density polyethylene (LDPE) and less than 10 wt% high density polyethylene (HDPE), where the LDPE has a density of 0.910 to 0.925 g / cc, a melt index (I2) of 0.2 to 0.8 dg / min, and an M of 4 to 10 w (cc) / M n (cc), the HDPE has a density of 0.940 to 0.970 g / cc, an I2 of 0.6 to 10 dg / min, and an M of 2 to 5 w (cc) / M n (cc), and the polymer blend has a density of 0.918 to 0.926 g / cc, an I2 of 0.2 to 0.8 dg / min, and an M of 4 to 9 w (cc) / M n (cc).
[0008] A second aspect includes the polymer blend of the first aspect, where the LDPE has a density of 0.920 to 0.925 g / cc, an I2 of less than 0.5 dg / min, and an M w (cc) / M n (cc) of 6 to 9.
[0009] A third aspect includes the polymer blend of the first or second aspect, wherein the LDPE has an M of 5 to 20 as measured according to triple-detector GPC (TD-GPC) z (abs) / M w (abs) and a gpcBR greater than 0.05, where "abs" refers to absolute molecular weight.
[0010] The fourth embodiment comprises a polymer blend from any one of the first to third embodiments, wherein the LDPE has a melt strength of 15 to 25 cN.
[0011] The fifth embodiment comprises a polymer blend from any one of the first to fourth embodiments, wherein the polymer blend comprises 2 to 10% by weight of HDPE or 3.5 to 5% by weight of HDPE.
[0012] The sixth aspect comprises a polymer blend of any one of the first to fifth aspects, wherein the polymer blend comprises 14 to 21 M z (abs) / M w (abs) and gpcBR greater than 0.05.
[0013] The seventh embodiment comprises any one of the polymer blends of the first to sixth embodiments, wherein the I2 of the polymer blend is less than 0.5 dg / min.
[0014] The eighth aspect comprises a polymer blend from any one of the first to seventh aspects, wherein the polymer blend has a melt strength of 15 to 25 cN.
[0015] The ninth embodiment includes a film comprising a polymer blend from any one of the first to eighth embodiments, wherein the film is a single-layer film or a multi-layer film.
[0016] A tenth aspect includes the film of the ninth aspect, wherein the film is a multilayer film containing a polymer blend in a core layer.
[0017] The eleventh embodiment comprises a composition containing an ethylene polymer, the ethylene polymer having a density of 0.918 to 0.926 g / cc, an I2 of 0.2 to 0.8 dg / min, and a Mw(cc) / Mn(cc) ratio of 4 to 9.
[0018] The twelfth embodiment comprises the composition of the eleventh embodiment, wherein the ethylene polymer is LDPE.
[0019] Additional features and benefits are described below in the “Modes for Carrying Out the Invention,” some of which will be readily apparent to those skilled in the art from the description therefrom, or will be recognized by carrying out the embodiments described herein, including the “Modes for Carrying Out the Invention” and the “Claims.”
[0020] It should be understood that both the general description above and the detailed description below are intended to illustrate various embodiments and to provide an overview or framework for understanding the nature and characteristics of the claimed subject matter. [Brief explanation of the drawing]
[0021] The embodiments shown in the drawings are for illustrative purposes only and are not intended to limit the subject matter defined by the claims. A detailed description of the following exemplary embodiments can be understood in conjunction with the following drawings, in which similar structures are shown with similar reference numerals. [Figure 1] This diagram schematically illustrates a system for processing ethylene polymers. [Modes for carrying out the invention]
[0022] As discussed above, the polymer blend compositions disclosed and described herein comprise low-density polyethylene (LDPE) and less than 10% by weight of high-density polyethylene (HDPE), wherein the LDPE has a density of 0.910 to 0.925 g / cc, a melt index (I2) of 0.2 to 0.8 dg / min, and a molecular weight of 4 to 10. w (cc) / M n HDPE has a density of 0.940-0.970 g / cc, an I2 of 0.6-10 dg / min, and 2-5 M w (cc) / M n The polymer blend has a density of 0.918-0.926 g / cc, an I2 of 0.2-0.8 dg / min, and 4-9 M w (cc) / M n (cc) is included.
[0023] LDPE In the embodiment, the density of the LDPE or blend is 0.910 to 0.925 g / cc, for example, 0.910 to 0.920 g / cc, 0.910 to 0.915 g / cc, 0.915 to 0.925 g / cc, 0.918 to 0.925 g / cc, 0.920 to 0.925 g / cc, or 0.922 to 0.925 g / cc.
[0024] In an embodiment, the melt index (I2) of the LDPE is 0.2 to 0.8 dg / min, for example, 0.2 to 0.7 dg / min, 0.2 to 0.5 dg / min, or 0.2 to 0.3 dg / min.
[0025] In this embodiment, M of LDPE w (cc) / M n (cc) is 4-10, for example, 6-10 or 6-9, and these are measured according to TD-GPC.
[0026] In the embodiment, when measured according to a triple-detector GPC (TD-GPC), the LDPE has a molecular weight of 5-20, for example, 7-18, 9-18, 9-15, 9-13. z (abs) / M w It has (abs).
[0027] In the embodiment, the LDPE has a melt strength of 15-25 cN, for example, 16-24 cN, 17-23 cN, 18-22 cN, or 19-21 cN.
[0028] In one embodiment, the LDPE has a gpcBR greater than 0.05. In another embodiment, the LDPE has a gpcBR of 0.5 to 2.0, for example, 0.75 to 2.0, 0.8 to 2.0, 1.0 to 1.9, 1.2 to 1.8, or 1.4 to 1.8.
[0029] In yet another embodiment, the density of the LDPE is 0.920 to 0.925 g / cc, the I2 of the LDPE is less than 0.5 dg / min, and the M of the LDPE is w (cc) / M n(cc) is 6-9. In the embodiment, LDPE is 5-20 M z (abs) / M w (abs) and gpcBR greater than 0.05.
[0030] HDPE In this embodiment, the density of the HDPE is 0.940 to 0.970 g / cc, for example, 0.940 to 0.960 g / cc, 0.940 to 0.955 g / cc, 0.940 to 0.950 g / cc, 0.940 to 0.945 g / cc, 0.945 to 0.965 g / cc, 0.945 to 0.960 g / cc, 0.945 to 0.955 g / cc, 0.945 to 0.950 g / cc, 0.950 to 0.965 g / cc, 0.950 to 0.960 g / cc, 0.950 to 0.955 g / cc, 0.955 to 0.965 g / cc, 0.955 to 0.960 g / cc, or 0.960 to 0.965 g / cc. While not strictly theoretical, maintaining a density in the range of 0.940–0.965 g / cc is beneficial for improving or maintaining the density and stiffness of the final blend while minimizing the impact on optical properties.
[0031] In an embodiment, the melt index (I2) of HDPE is 0.6 to 10 dg / min, for example, 0.6 to 8 dg / min, 0.6 to 6 dg / min, 0.6 to 2.5 dg / min, 0.6 to 1 dg / min, 1 to 10 dg / min, 1 to 8 dg / min, 1 to 6 dg / min, 1 to 2.5 dg / min, 2.5 to 10 dg / min, 2.5 to 8 dg / min, 2.5 to 6 dg / min, 6 to 10 dg / min, 6 to 8 dg / min, or 8 to 10 dg / min.
[0032] In this embodiment, M of HDPE w (cc) / M n (cc) is between 2 and 5, for example, 2.5 to 4.5, or 2.5 to 4.0.
[0033] In yet another embodiment, the density of HDPE is 0.940-0.970 g / cc, the I2 of HDPE is 0.6-10 dg / min, and the M of HDPE is w (cc) / M n(cc) is between 2 and 5.
[0034] In embodiments, HDPE may be produced by a gas-phase, solution-phase, or slurry polymerization process, or any combination thereof. Catalysts used to produce the polyethylene described herein include Ziegler-Natta catalysts, metallocene catalysts, constrained geometry catalysts, single-site catalysts, or chromium-based catalysts. In further embodiments, HDPE is produced in a solution phase.
[0035] LDPE / HDPE polymer blend In some embodiments, the polymer blend comprises 2 to 10% by weight of HDPE or 3.5 to 5% by weight of HDPE. In further embodiments, the polymer blend comprises 90% to 98% by weight of LDPE, or 90% to 96.5% by weight, 90% to 95% by weight, 95% to 98% by weight, 95% to 96.5% by weight, or 96.5% by weight of LDPE, based on the weight of the composition.
[0036] In some embodiments, the density of the polymer blend is 0.918–0.926 g / cc. In further embodiments, the density of the ethylene-based polymer is 0.918–0.926 g / cc, e.g., 0.920–0.926 g / cc, 0.922–0.926 g / cc, or 0.924–0.926 g / cc. While not theoretically bound, maintaining a density of 0.926 g / cc or less is beneficial because higher density blends result in undesirable optical property trade-offs.
[0037] In this embodiment, the polymer blend M w (cc) / M n (cc) is between 4 and 9, for example, 4 to 8, 4 to 6, 5.5 to 7.5, or 6 to 8, and these are measured according to TD-GPC.
[0038] In embodiments, the polymer blend is 6-22, for example, 9-21, or 12-21, or 14-21 M z (abs) / M wIt has (abs).
[0039] In embodiments, the polymer blend has gpcBR greater than 0.05, for example, 0.5 to 2.4, for example, 0.75 to 2.4, 0.8 to 2.4, 1.0 to 2.4, 1.2 to 2.4, or 1.4 to 2.4, 1.7 to 2.4, 1.7 to 2.2, or 1.7 to 2.0.
[0040] In yet another embodiment, the density of the polymer blend is 0.918 to 0.926 g / cc, the I2 of the polymer blend is 0.2 to 0.8 dg / min, and the M of the polymer blend is 0.918 to 0.926 g / cc. w (cc) / M n (cc) is 4 to 9. In the embodiment, the M of the polymer blend z (abs) / M w The (abs) ranges from 14 to 21, and the gpcBR of polymer blends is greater than 0.05.
[0041] In one embodiment, the melt index (I2) of the polymer blend is 0.2 to 0.8 dg / min. In a further embodiment, the I2 of the polymer blend is less than 0.5 dg / min, for example, 0.2 to 0.5 dg / min, or 0.3 to 0.5 dg / min.
[0042] In one embodiment, the polymer blend has a melt strength of 15 to 25 cN. In a further embodiment, the polymer blend may have a melt strength of 15 to 20 cN, 15 to 18 cN, 15 to 17 cN, 15 to 16 cN, 16 to 20 cN, 16 to 19 cN, 16 to 18 cN, 16 to 17 cN, 17 to 20 cN, 17 to 19 cN, 17 to 18 cN, 18 to 20 cN, 18 to 19 cN, or 19 to 20 cN.
[0043] In yet another embodiment, the polymer blend composition contains an ethylene polymer, the density of the ethylene polymer is 0.918 to 0.926 g / cc, the I2 of the ethylene polymer is 0.2 to 0.8 dg / min, and the M of the ethylene polymer is 0.2 to 0.8 dg / min. w (cc) / M n(cc) is 4 to 9. In further embodiments, the ethylene polymer is LDPE.
[0044] LDPE / HDPE polymer blend film Polymer blend compositions can be used in a wide variety of conventional thermoplastic manufacturing processes to produce useful articles including extrusion coatings; shrink films for aggregate packaging, shrink hood films, heavy transport sack films, heavy industrial films; and molded articles, such as blow-molded, injection-molded, or rotationally molded articles; foams; and wires and cables, fibers, woven or nonwoven fabrics.
[0045] The disclosure also provides articles comprising at least one component formed from the compositions of the disclosure. In embodiments, the articles are selected from coatings, films, foams, laminates, fibers, tapes, or combinations thereof.
[0046] In some embodiments, the article is a film containing a polymer blend, and the film containing the polymer blend is a single-layer film or a multilayer film. In further embodiments, the film is a multilayer film containing a polymer blend in a core layer.
[0047] In the embodiment, the multilayer film containing the polymer blend has an internal haze of less than 3.5%, a total haze of less than 6.0%, and a transparency of more than 65% when measured for a film with a thickness of 50 μm.
[0048] definition Unless otherwise stated, implied by the context, or customary in the art, all parts and percentages are based on weight, and all test methods are current as of the filing date of this disclosure.
[0049] As used herein, the term “composition” refers to a mixture of materials comprising the composition, as well as reaction products and decomposition products formed from the materials of the composition.
[0050] The terms “blend” or “polymer blend,” when used, mean a close physical mixture (i.e., unreacted) of two or more polymers. A blend may or may not be miscible (not phase-separated at the molecular level). A blend may or may not be phase-separated. A blend may or may not contain one or more domain configurations determined by transmission electron spectroscopy, light scattering, X-ray scattering, and other methods known in the art. A blend may be achieved by physically mixing two or more polymers at a macro level (e.g., molten blend resin or compound) or at a micro level (e.g., simultaneous molding in the same reactor).
[0051] The term "polymer" refers to a compound prepared by polymerizing monomers, whether of the same or different types. Therefore, the general term polymer encompasses the terms homopolymer (referring to a polymer prepared from a single type of monomer, assuming that trace amounts of impurities may be incorporated into the polymer structure) and the term "interpolymer," as defined below. Trace amounts of impurities may be incorporated into and / or within the polymer.
[0052] The term "interpolymer" refers to a polymer prepared by the polymerization of at least two different types of monomers. The general term interpolymer includes copolymers (which refer to polymers prepared from two different monomers) and polymers prepared from two or more different types of monomers.
[0053] The term "ethylene polymer" or "ethylene polymer" refers to a polymer that, based on the weight of the polymer, contains the majority amount of polymerized ethylene and may optionally contain at least one comonomer.
[0054] The terms “polyethylene,” “ethylene copolymer,” or “ethylene copolymer” refer to polymers containing more than 50% by weight of units derived from ethylene monomers. This includes polyethylene homopolymers or copolymers (meaning units derived from two or more comonomers). Common forms of polyethylene known in the art include low-density polyethylene (LDPE), linear low-density polyethylene (LLDPE), ultra-low-density polyethylene (ULDPE), very low-density polyethylene (VLDPE), single-site catalyst linear low-density polyethylene (m-LLDPE), medium-density polyethylene (MDPE), and high-density polyethylene (HDPE), which include both linear low-density resins and substantially linear low-density resins.
[0055] When used herein, the term "high-pressure free radical polymerization process" refers to free radical-initiated polymerization carried out at a high pressure of at least 1000 bar (100 MPa).
[0056] The terms “comprising,” “including,” and “having,” and their derivatives, are not intended to exclude the existence of any additional components, steps, or procedures, whether or not they are specifically disclosed. To avoid any doubt, all compositions claimed through the use of the term “comprising” may include any additional additives, adjuvants, or compounds, whether or not they are polymers, unless otherwise stated. In contrast, the term “consisting essentially of” excludes any other components, processes, or procedures from the scope of any subsequent description, except those not essential to the operability. The term “consisting of” excludes any components, processes, or procedures that are not specifically described or enumerated.
[0057] Test method Triple Detector Gel Permeation Chromatography (TD-GPC). The chromatography system consisted of a PolymerChar GPC-IR (Valencia, Spain) high-temperature GPC chromatograph equipped with an internal IR5 infrared detector (IR5), and a 4-capillary viscometer (DV) coupled to a Precision Detectors (now Agilent Technologies) Model 2040 2-angle laser light scattering (LS) detector. For all absolute light scattering measurements, a 15-degree angle was used. The autosampler's oven compartment was set to 160°C, and the column compartment to 150°C. The columns used were four Agilent "Mixed A" columns (30 cm, 20 micrometers, linear mixed-bed columns). The chromatography solvent used was 1,2,4-trichlorobenzene (TCB) containing 200 ppm butylated hydroxytoluene (BHT). The solvent source was spurged with nitrogen. The injection volume used was 200 microliters, and the flow rate was 1.0 milliliter / minute.
[0058] The GPC column set was calibrated using 21 polystyrene standards with narrow molecular weight distributions ranging from 580 to 8,400,000, placed in six "cocktail" mixtures with at least a 10-fold gap between individual molecular weights. The standards were purchased from Agilent Technologies. Polystyrene standards were prepared using 0.025 grams in 50 ml of solvent for molecular weights greater than 1,000,000, and 0.05 grams in 50 ml of solvent for molecular weights less than 1,000,000. The polystyrene standards were dissolved at 80°C with gentle stirring for 30 minutes, then cooled, and the room temperature solution was transferred to an autosampler dissolution oven at 160°C for 30 minutes and cooled. The peak molecular weights of the polystyrene standards were converted to polyethylene molecular weights using equation (1) (as described in Williams and Ward, J. Polym. Sci., Polym. Let., 6, 621 (1968)). M polyethylene =A × (M polystyrene ) B (Equation 1) In the formula, M is the molecular weight, A has a value of 0.3988, and B is equal to 1.0.
[0059] A quintic polynomial was used to fit each polyethylene equivalent calibration point.
[0060] The total plate count of the GPC column set was performed using decane introduced into the blank sample via a micropump controlled by the PolymerChar GPC-IR system. The plate count of the chromatography system must be greater than 18,000 for four Agilent "Mixed A" columns (30 cm, 20 micrometers, linear mixed bed columns).
[0061] The sample was prepared semi-automatically using PolymerChar's "Instrument Control" software, with a target weight of 2 mg / mL. The solvent (containing 200 ppm BHT) was added to a vial with a pre-nitrogen-spurged septum cap via PolymerChar's high-temperature autosampler. The sample was dissolved at 160°C for 3 hours under "low-speed" shaking.
[0062] M n (cc), M w (cc) , , and M z The calculation of (cc) was based on GPC results using the internal IR5 detector (measurement channel) of the PolymerChar GPC-IR chromatograph, using PolymerChar GPCOne® software, the IR chromatogram with the baseline subtracted at each equally spaced data acquisition point (i), and the polyethylene-equivalent molecular weight obtained from the narrow standard calibration curve for acquisition point (i) of equation (1), following equations (2) to (4).
[0063]
number
[0064] To monitor deviations over time, a flow rate marker (decane) was introduced into each sample via a micropump controlled by a PolymerChar GPC-IR system. Using this flow rate marker (FM), the pump flow rate (nominal flow rate) for each sample was linearly corrected by RV matching the RV of each decane peak in the sample (RV(FM sample)) with the RV of the calibrated decane peak in the narrow standard material (RV(FM calibrated)). It was assumed that any temporal changes in the decane marker peak corresponded to a linear shift in the overall flow rate (effective flow rate). After calibrating the system based on the flow rate marker peaks, the effective flow rate (relative to the narrow standard calibration) was calculated using equation (5). The processing of the flow rate marker peaks was performed via PolymerChar GPCOne® software. An acceptable flow rate correction was defined as an effective flow rate within ±0.5% of the nominal flow rate.
[0065]
number
[0066] Regarding the determination of viscometer and light scattering detector offsets from the IR5 detector, a systematic method for determining multiple detector offsets was implemented in a manner consistent with that published by Balke, Mourey et al. (Mourey and Balke, Chromatography Polym. Chpt 12, (1992)) (Balke, Thitiratsakul, Lew, Cheung, Mourey, Chromatography Polym. Chpt 13, (1992)), using PolymerChar GPCOne™ software, with linear homopolymer polyethylene standard materials (3.5>M) having molecular weights in the range of 115,000 to 125,000 g / mol. w / M n>2.2) The results of the triple detector log(MW and IV) obtained from this are optimized to the results of the narrow standard column calibration obtained from the narrow standard calibration curve.
[0067] Absolute molecular weight data was obtained using PolymerChar's GPCOne® software in a format consistent with that published by Zimm (Zimm, BH, J. Chem. Phys., 16, 1099 (1948)) and Kratochvil (Kratochvil, P., Classical Light Scattering from Polymer Solutions, Elsevier, Oxford, NY (1987)). The total injection concentration used in determining the molecular weight was obtained from the mass detector area and mass detector constant derived from one of the following: a suitable linear polyethylene homopolymer or a polyethylene standard material with a known weight-average molecular weight. The molecular weight calculated (using GPCOne®) was obtained using the light scattering constant derived from one or more of the polyethylene standards described below, and the refractive index concentration coefficient, dn / dc, of -0.104. In general, the mass detector response (IR5) and light scattering constant (determined using GPCOne®) should be determined from linear standards with a molecular weight greater than approximately 50,000 g / mol. Calibration of the viscometer (determined using GPCOne®) can be achieved using the method described by the manufacturer, or alternatively, by using published values of a suitable linear standard such as Standard Reference Material (SRM) 1475a (available from the National Institute of Standards and Technology, NIST). The specific viscosity area (DV) and injected mass for the calibration standard are used to calculate the viscometer constant (obtained using GPCOne®) related to its intrinsic viscosity. The chromatographic concentration is assumed to be low enough to eliminate the consideration of the second viral coefficient effect (concentration effect on molecular weight).
[0068] Absolute weight average molecular weight (MW) (Abs) The following was obtained (using GPCOne®) from a light scattering (LS) area integrated chromatogram (factored by the light scattering constant), divided by the mass reconstructed from the mass constant and mass detector (IR5) area. The molecular weight and intrinsic viscosity response were linearly extrapolated (using GPCOne®) at the edge of the chromatogram where signal-to-noise is low. The other respective moments are M n (abs), M w (abs), and M z (abs) is calculated according to the following equations (6) to (8).
[0069]
number
[0070] gpcBR branching index obtained by triple detector GPC (TD-GPC). The gpcBR branching index was determined, as described above, by first calibrating the light scattering, viscosity, and infrared IR5 detectors. The baseline was then subtracted from the light scattering, viscometer, and IR5 (measurement channel) chromatograms. Next, an integration window was set to ensure integration of all low molecular weight retention volume ranges of the light scattering and viscometer chromatograms indicating the presence of detectable polymers from the infrared (IR5) chromatogram. Subsequently, the Mark-Houwink constants for polyethylene and polystyrene were established using linear polyethylene standards. After determining the constants, two linear criterion conventional calibrations for polyethylene molecular weight and polyethylene intrinsic viscosity as functions of elution volume were constructed using the two values, as shown in equations (9) and (10).
[0071]
number
[0072] The gpcBR branching index is a robust method for characterizing long-chain branching, as described in Yau, Wallace W., "Examples of Using 3D-GPC-TREF for Polyolefin Characterization," Macromol.Symp., 2007, 257, 29-45. This index prioritizes the entire polymer detector area, avoiding the conventional "per-slice" 3D-GPC calculations used in determining g' values and calculating branching frequencies. From TD-GPC data, the peak area method is used to determine the absolute weight-average molecular weight (M) of the sample bulk measured by a light scattering (LS) detector. w (abs)) can be obtained. This method avoids the "per slice" ratio of the light scattering detector signal to the concentration detector signal, as required in conventional g' determination.
[0073] In TD-GPC, the intrinsic viscosity of the sample was also obtained independently using equation (11). The area calculation in equation (11) provides higher accuracy because, as the overall sample area, it is less affected by the fluctuations caused by detector noise and TD-GPC settings to the baseline and integration limit. More importantly, the peak area calculation was unaffected by the detector volume offset. Similarly, the high-precision intrinsic viscosity ([h]) was obtained by the area method shown in equation (11).
[0074]
number
[0075] To determine the gpcBR branching index, the light scattering elution area of the sample polymer is used, and the molecular weight (M) of the sample is determined. w The (abs) was determined. The intrinsic viscosity ([h]) of the sample polymer was determined using the elution area of the viscosity detector.
[0076] First, the molecular weight and intrinsic viscosity of linear polyethylene standard samples such as SRM1475a or equivalents were determined using conventional calibration ("cc") as functions of elution volume, according to equations (3) and (12).
[0077]
number
[0078] The GPCBR branch index was determined using equation (13).
[0079]
number
[0080] All statistical values with the subscript "cc" represent the respective elution volume, the corresponding conventional calibration method described above, and the concentration (c i Determined using "M w The values for (abs) and [h] are measurements based on the mass detector, LALLS, and viscometer area. PEThe value of is adjusted iteratively until the linear reference sample has a gpcBR measurement of zero. For example, the final values of α and LogK for determining the gpcBR in this particular case are 0.725 and -3.391 for polyethylene and 0.722 and -3.993 for polystyrene, respectively. These polyethylene coefficients were then substituted into equation (13).
[0081] After determining the K and α values using the previously discussed procedure, the procedure is repeated using the branched sample. The branched sample is analyzed using the final Mark-Houwink constant obtained from the linear reference when the best "cc" calibration value is applied.
[0082] Melt strength Melt strength measurements were performed using Goettfert Rheotens 71.97 (Goettfert Inc.; Rock Hill, SC) coupled to a Goettfert Rheotester 2000 capillary rheometer. A molten sample (approximately 25-30 grams) was fed into the Goettfert Rheotester 2000 capillary rheometer, which had a length of 30 mm, a diameter of 2.0 mm, and a flat inlet angle (180 degrees) with an aspect ratio (length / diameter) of 15. After equilibrating the sample at 190°C for 10 minutes, the piston was operated at a constant piston speed of 0.265 mm / second. The standard test temperature was 190°C. The sample was then subjected to a set of accelerating nips located 100 mm below the die at a speed of 2.4 mm / second. 2 Uniaxial stretching was performed at the specified acceleration. Tensile force was recorded as a function of the nip roll winding speed. Melt strength was reported as the average plateau force (cN) before the strand fractured. The following conditions were used for melt strength measurement: plunger speed = 0.265 mm / sec, wheel acceleration = 2.4 mm / sec. 2 Capillary diameter = 2.0 mm, capillary length = 30 mm, and barrel diameter = 12 mm.
[0083] density Samples for density measurement were prepared according to ASTM D 4703-10. The samples were pressed at 374°F (190°C) for 5 minutes at 10,000 psi (68 MPa). The temperature was maintained at 374°F (190°C) for the above 5 minutes, and then the pressure was increased to 30,000 psi (207 MPa) over 3 minutes. This was followed by holding at 70°F (21°C) and 30,000 psi (207 MPa) for 1 minute. Measurements were performed within 1 hour of sample compression using ASTM D792-08, Method B.
[0084] Melt Index The melt index (MI or I2) was measured according to ASTM D 1238-10, conditions 190°C / 2.16 kg, Method B, and reported as grams of eluted per 10 minutes.
[0085] Dynamic mechanical spectroscopy (DMS) The resin was compressed into a circular plate measuring 3 mm thick x 1 inch in air at a pressure of 25,000 psi for 5 minutes at 177°C. The sample was then removed from the compressor, placed on a counter, and cooled.
[0086] Constant temperature-frequency sweeps were performed using TA Instruments' Advanced Rheometric Expansion System (ARES) equipped with 25 mm (diameter) parallel plates under nitrogen purging. The sample was placed on the plate and melted at 190°C for 5 minutes. The plate was then closed to a 2 mm gap, the sample was trimmed (excess sample extending beyond the circumference of the 25 mm diameter plate was removed), and the experiment was initiated. This method incorporated an additional 5-minute delay to allow for temperature equilibrium. Experiments were conducted at 190°C over a frequency range of 0.1 to 100 radians / second. The strain amplitude remained constant at 10%. The complex dielectric loss tangent, viscosity at 0.1 radians / second (V0.1), viscosity at 100 radians / second (V100), and viscosity ratio (V0.1 / V100) were calculated from these data.
[0087] Differential Scanning Calorimetry (DSC). In preparation for a differential scanning calorimetry (DSC) test, the pellet sample is first loaded into a 1-inch diameter, 0.13 mm thick chase and compressed into a film at 190°C for approximately 10 seconds under a pressure of 25,000 lbs. The resulting film is then cooled to room temperature. The film is then subjected to a punch press to produce discs that fit into an aluminum DSC test pan. The discs are then individually weighed (note: sample weight is approximately 5-6 mg), placed in an aluminum pan, sealed, and inserted into the DSC test chamber.
[0088] In accordance with ASTM standard D3418, the DSC test was performed using a heating-cooling-heating cycle. First, the sample was heated to 150°C at a rate of 10°C / min and held isothermally for 5 minutes to remove thermal and process history. Next, the sample was rapidly cooled to -40°C at a rate of 10°C / min and held isothermally again for 5 minutes. Finally, for the second heating cycle, the sample was heated to 150°C at a rate of 10°C / min. For data analysis, the melting temperature and enthalpy of melting were extracted from the second heating curve, while the enthalpy of crystallization was determined from the cooling curve. Enthalpy of melting (H f The enthalpy of fusion and crystallization were obtained by integrating the DSC thermogram from -20°C to the end of melting and crystallization, respectively. Assuming the heat of fusion of 100% crystalline polyethylene is 292 J / g, the degree of crystallinity by weight % was calculated using the following equation (14). DSC tests were performed using TA Instruments Discovery DSC, and data analysis was performed using TA Instruments Universal Analysis and the TRIOS software package. Crystallinity %=((H f ) / 292J / g)×100 (Equation 14)
[0089] n-hexane extractable substance As used herein, the term “hexane extractable” refers to the amount of n-hexane-soluble material extracted from the resulting polymer composition by n-hexane. The extraction process follows both the Food and Drug Administration (FDA) procedure (21 CFR 177.1520 (d)(3)(ii)) and ASTM D5227 for determining the solvent extractable portion of polyolefins. The polymer pellets are compressed or extruded into a film having a thickness of 3-4 mils, and then cut into 1 x 1 inch square pieces. The film pieces are weighed (2.5 ± 0.05 g), then placed in a basket, and extracted in an n-hexane container at 49.5 ± 0.5 °C for 2 hours in a heated water bath, as described in ASTM D5227. After 2 hours, the film is removed, rinsed with clean n-hexane, and dried in a vacuum oven (80 ± 5 °C) under total vacuum for 2 hours. The film is then placed in a desiccator and allowed to cool to room temperature for at least 1 hour. Next, the film is reweighed, and the mass loss due to extraction in n-hexane is calculated. The n-hexane extractable material is reported in weight percent.
[0090] 1 1H NMR. Nuclear magnetic resonance (related to unsaturation). 1 (H NMR). For NMR spectroscopy to determine polyethylene unsaturation, see, for example, Busico, V., et al., Macromolecules, 2005, 38, 6988.
[0091] 1 H NMR sample preparation. The sample was prepared by adding approximately 0.1 g of the sample to 3.25 g of 1,1,2,2-tetrachloroethane-d2 / perchloroethylene (TCE / PCE) in a 50 / 50 weight ratio, containing 0.001 M Cr(AcAc)3 and approximately 75 ppm butylated hydroxytoluene (BHT), in a Norell 1001-7 10 mm NMR tube. The sample was covered, sealed with Teflon tape, and then heated and vortexed at approximately 110°C to 115°C to dissolve and ensure homogeneity.
[0092] 1 1H NMR data acquisition parameters. Using a Bruker AVANCE 600MHz spectrometer equipped with a Bruker high-temperature CryoProbe, at a sample temperature of 120°C. 1 1H NMR was performed. Spectra were acquired with a ZG pulse, 1.8-second AQ, 64 or 128 scans, and a 14-second relaxation delay.
[0093] 1 1H NMR data analysis. Number of unsaturated groups per 1000 carbon atoms (1000C) 1 1H NMR calculation. The spectrum was referenced to the residual proton signal of TCE at 6.0 ppm. The integral value of the entire polymer from approximately -0.5 to 2.5 ppm was set to an arbitrary value, e.g., 2000. The corresponding integral values for unsaturated groups were obtained (cis- and trans-vinylenes at approximately 5.40-5.60 ppm, trisubstituted compounds at approximately 5.16-5.35 ppm, vinyl at approximately 5.0-5.15 ppm, and vinylidene at approximately 4.75-4.85 ppm). The -OH signal of BHT at approximately 4.9 ppm was not included in the integral area. Dividing the integral value of the entire polymer by 2 gives the total polymer carbon, 1000 in this example. The unsaturated group integral value, divided by the corresponding number of protons contributing to that integral value, represents the number of moles of each type of unsaturated group per 1000 moles of total polymer carbon. This is referred to as the number of unsaturated groups per 1000 carbon atoms ("100 / C").
[0094] 13 C nuclear magnetic resonance (branching) 13 (C NMR). 13Samples for 13C NMR were prepared in a 10mm NMR tube by adding approximately 3g of 1,1,2,2-tetrachloroethane (TCE) containing 25 wt% TCE-d2 and 0.025M Cr(AcAc)3 to approximately 0.25g of a polymer sample. The sample was then dissolved and homogenized by heating the tube and its contents to 120°C-140°C using a heating block and vortex mixer. Each dissolved sample was visually inspected to ensure homogeneity. The sample was thoroughly mixed immediately before analysis and kept from cooling until it was inserted into a heated NMR sample holder.
[0095] All data were acquired using a Bruker 600MHz spectrometer equipped with a 10mm high-temperature cryoprobe. At a sample temperature of 120°C, with a pulse repetition delay of 7.8 seconds, a flip angle of 90 degrees, and decoupling with reverse gate, the analysis was performed. 13 C data was acquired. All measurements were performed on a non-rotating sample in lock mode. The sample was thermally equilibrated before data acquisition. 13 The 30¹³C NMR chemical shift was internally referenced to a 30.0 ppm EEE triad. Table A lists the peak identifications used for branching measurements in LDPE. 6+ The value is C in LDPE. 6+ This is a direct measure of branching, and long branches are not distinguished from "chain ends". The peak at "32.2 ppm" represents the third carbon from the end of all chains or branches with 6 or more carbons, and is used for "C 6+ Determine the value.
[0096] [Table 1]
[0097] Total (overall) haze and internal haze Samples for measuring internal and overall haze were sampled and prepared according to ASTM D1003. Internal haze was obtained by matching the refractive index using mineral oil on both sides of the film. Hazegard Plus (BYK-Gardner USA, Columbia, MD) was used for the test.
[0098] Zebedee Transparency Zebedee clarity was measured according to ASTM D1746-15. A Zebedee CL-100 Clarity Meter was used (Model: CI-100 SN: 212615). The average of five samples was reported.
[0099] Secture modulus The tensile strength of the film was measured according to ASTM D-882. Using ASTM D-882, the tensile strength, 1% secant modulus, and 2% secant modulus were determined in the MD (machine direction) and CD (transverse direction). The Elmendorf tear strength in the MD and CD directions was determined using ASTM D-1922.
[0100] Contraction force, contraction, and shrinking force Shrinkage force and shrinkage were measured using a "Retratech" apparatus. In this method, a film strip 15 mm wide and 100 mm long was used as a test specimen and cut along either the machine direction (MD) or the cross-direction (CD). Two specimens were allowed to move freely, while six specimens were restrained to prevent movement in the test direction (MD or CD). Free shrinkage was measured using the two freely moving specimens, and shrinkage force was measured using the six restrained specimens. The test strips were subjected to a rapid increase in temperature when an oven preheated to a selected temperature (setpoint) was mechanically engaged to cover the specimens, which were initially at ambient temperature. The specimens physically shrank, and the amount of shrinkage was measured using a displacement sensor attached to one end of the specimen.
[0101] The specimens used to determine the shrinkage force of the test pieces were connected to load cells that provided force signals. These measurements could be obtained as a function of time as the temperature around the specimens changed during the test. The temperature profile experienced by the film specimens was a result of the selected test conditions and influenced the test data.
[0102] Typically, there were two methods for selecting the test conditions (oven temperature setpoint, residence time, and total time): (1) the method described in ISO 14616, and (2) the fixed-condition method. In method (1), the test conditions were selected to conform to the ISO 14616 requirements for MD specimens. In method (2), a fixed set of temperature setpoint and residence time was set for all samples, and the values for the samples were selected to achieve a clear peak in force in MD during the temperature rise phase and to finally relax to zero before the oven was released. If the oven was released before the force specimen relaxed to zero force (during the ISO 14616 method), the force increased as the film specimen cooled. The maximum contraction at the end of the total analysis time was referred to as "free contraction". [Examples]
[0103] Various embodiments of compositions for LDPE / HDPE blends containing less than 10% HDPE, and films containing LDPE / HDPE blends, will be further illustrated by the following examples. These examples should be understood to be illustrative in nature and not limiting the subject matter of this application.
[0104] Ethylene polymer process conditions Table 1 lists the ethylene polymers used to form the examples and comparative examples of the present invention. Figure 1 schematically shows the process for forming LDPE and HDPE.
[0105] [Table 2] ND=Not determined
[0106] The process for forming LDPE is described in general terms. Ethylene polymers LDPE1, 2, 4, 5, and 6 were each produced by a high-pressure free-radical polymerization process according to the generalized block diagram shown in Figure 1 and the specific details provided in Tables 2 and 3.
[0107] In particular, LDPE1 was produced in a tubular reactor containing four reaction zones. Ethylene was injected into the front of the first reaction zone, and a chain transfer agent (CTA) was injected into the first reaction zone. Additional ethylene and CTA were injected into the side of the second reaction zone. LDPE2, 4, and 6 were produced in tubular reactors containing three reaction zones. Ethylene was injected into the front of the first reaction zone, and CTA was injected into the first reaction zone. Additional ethylene and CTA were injected into the side of the second reaction zone. LDPE5 was produced in a reactor having a configuration including an autoclave with two reaction zones and a tubular reactor with two subsequent reaction zones. Ethylene and CTA were injected into the front of the first reaction zone in the autoclave section and into the side of the second reaction zone in the autoclave.
[0108] For LDPE1, 2, 4, 5, and 6, CTA was introduced to control the polymer molecular weight and achieve the target melt index (I2) value. Suitable CTAs may include alkanes, alkenes, ketones, or aldehyde functionalities, such as propylene, isobutane, n-butane, 1-butene, methyl ethyl ketone, acetone, and propionaldehyde. LDPE1 was prepared using propionaldehyde and propylene. LDPE2, 4, and 6 were prepared using propylene and methyl ethyl ketone. LDPE5 was prepared using propylene and propionaldehyde.
[0109] Next, the system for processing LDPE will be described. Referring to Figure 1, the process reaction system 100 shown in Figure 1 is a partially closed-loop, double-recycle, high-pressure LDPE production system. In the process reaction system 100, the fresh ethylene supply line 101 is mixed with a high-ethylene flow 161 (outlet flow of the booster compressor 160) and an optional chain transfer agent (CTA) flow 102 to form a mixed flow (i.e., a mixed flow of the fresh ethylene supply line 101, the high-ethylene flow 161, and the optional CTA flow 102). This mixed flow is introduced into the primary compressor 110, which is sequentially connected to the booster compressor 160 upstream and to the supercompressor 120 downstream. In the primary compressor 110, the mixed flow is compressed and exits the primary compressor 110 as a compressed flow 111.
[0110] The compressed flow 111 is mixed with the high-pressure recirculation flow 143 to form a mixed flow 112. The mixed flow 112 is optionally mixed with an optionally second CTA flow 113 to form a second mixed flow 114. The second mixed flow 114 is introduced into the hypercompressor 120, which is sequentially connected to both the primary compressor 110 and the high-pressure separator (HPS) 140, located upstream of the hypercompressor 120. In the hypercompressor 120, the mixed flow is compressed and exits the hypercompressor 120 as a compressed flow 121 and a second compressed flow 122. The compressed flow 121 and the second compressed flow 122 may be split before or after compression in the hypercompressor 120, and optionally cooled by an in-line cooler (not shown) before injection into the reactor 130.
[0111] Next, the process for forming LDPE in reactor 130 will be described. The process conditions in reactor 130 are summarized in Tables 2 and 3. For LDPE 1, 2, 4, 5, and 6, the compressed stream 121 containing ethylene and CTA was a pre-injection into reactor 130, which was sequentially connected to a hypercompressor 120 located upstream of reactor 130. In the examples, reactor 130 may be either a tubular reactor or an autoclave reactor connected in series to a tubular reactor. Peroxide injection is carried out at multiple locations within reactor 130 to initiate the reaction. Prior to the first peroxide injection, the compressed stream 121 is optionally heated to a desired temperature for reaction initiation. For LDPE 1, 2, 4, and 6, the pre-injection of ethylene and CTA, as well as the first peroxide injection, were injected into the tubular reactor section. For LDPE 5, the pre-injection of ethylene and CTA, as well as the first peroxide injection, were injected into the autoclave reactor section.
[0112] For LDPE1, 2, 4, 5, and 6, the second compressed flow 122 containing ethylene and CTA was the first side injection into reactor 130, entering the reactor sequentially after the first peroxide injection. The second peroxide injection was carried out simultaneously with the second compressed flow 122. For LDPE1, 2, 4, and 6, the first side injection of ethylene and CTA, as well as the second peroxide injection, were injected into the tubular reactor section. For LDPE5, the first side injection of ethylene and CTA, as well as the second peroxide injection, were injected into the autoclave reactor section.
[0113] For LDPE1, 2, 4, 5, and 6, a third peroxide injection was administered to the tubular reactor section.
[0114] For LDPE1 and 5, a fourth peroxide injection was administered to the tubular reactor section.
[0115] Next, the process for forming LDPE after reactor 130 will be described. The polymerization flow 131 passes through a pressure drop valve and an aftercooler (not shown) and is then introduced into an HPS 140 which is sequentially connected to a low-pressure separator (LPS) 150. In the HPS 140, the polymerization flow 131 is separated into an ethylene-enriched flow 141 and a polymer-enriched flow 144. A purge flow 142 is taken from the ethylene-enriched flow 141 to prevent the accumulation of low molecular weight molecules in the reaction system. The resulting high-pressure recirculated flow 143 is cooled and recirculated back to the hypercompressor 120.
[0116] The polymer-enriched stream 144 is introduced into the LPS 150, which is sequentially connected to the HPS 140 upstream and then to the booster compressor 160 downstream of the LPS. In the LPS, the polymer-enriched stream is separated into a second polymer-enriched stream 152 and a second ethylene-enriched stream 151. The second polymer-enriched stream 152 exits the process system 100, where it can be pelletized or otherwise finished for final use.
[0117] The second ethylene-enriched flow 151 is introduced into a booster compressor 160, which is sequentially connected to the LPS upstream of it, and then sequentially connected to the primary compressor 110 downstream of it. In the booster compressor 160, the second ethylene-enriched flow 151 is regulated, and the resulting regulated flow 161 is mixed with an optional CTA flow 102 and a fresh ethylene supply line 101.
[0118] [Table 3] TBPIV = tert-butylperoxypivalate, TBPA = tert-butylperoxyacetate, TBPO = tert-butylperoxy-2-ethylhexanoate, DTBP = di-tert-butylperoxide.
[0119] [Table 4]
[0120] Next, the process of forming HDPE will be described. HDPE1-3 were prepared according to the following procedure, namely, heterogeneous branched ethylene / α-olefin copolymers were prepared using the multi-component catalyst system described above, which is suitable for (co)polymerizing ethylene with one or more α-olefin comonomers, e.g., 1-octene or 1-hexene, in an adiabatic continuous stirred tank reactor CSTR under liquid-phase polymerization conditions. More specifically, in this embodiment, the reactor consisted of two adiabatic reactors linked in series and operated under liquid-phase polymerization conditions. All feed streams were introduced into the first reactor, which was a mechanically stirred adiabatic CSTR. The effluent from the first reactor was fed into the second reactor, which was identical to the first reactor, except that it was not mechanically stirred and the second reactor did not accept any feed other than the effluent from the first reactor.
[0121] The saturated hydrocarbon solvent, e.g., Shellsol 100-140, ethylene monomer, and 1-octene or 1-hexene comonomer reactor feed streams were purified using molecular sieves before being introduced into the reaction environment. The solvent, ethylene monomer, and 1-octene or 1-hexene comonomer were combined into a single feed stream and temperature-controlled before being introduced into the reaction environment. Hydrogen was also added to the combined single feed stream before being introduced into the reaction environment.
[0122] The catalyst system was supplied to the reaction environment separately from a single feed stream. The catalyst premix (i.e., a heterogeneous Ziegler-Natta type catalyst premix prepared according to U.S. Patent No. 4,612,300) was coupled inline to the reactor with a dilution stream of triethylaluminum (TEA). The TEA stream was controlled to achieve a specific molar ratio of Al to Ti with the catalyst premix. The catalyst-premix flow rate was controlled to control the degree of reaction in the reaction environment. Specific targets are included in Data Table 4.
[0123] The first reactor temperature and total ethylene conversion rate were controlled by adjusting the catalyst-premix flow and the total solvent flow introduced into the reaction environment. The melt index of the total polymer was controlled by adjusting the hydrogen supply to the reaction environment. The density of the total polymer was controlled by adjusting the comonomer supply to the reaction environment. The values of the control parameters are included in Data Table 4.
[0124] After leaving the reaction environment, the reaction was stopped by adding an active catalyst and reacting it with a fluid specially designed for that purpose, typically water. The polymer was separated from the solvent and any unreacted monomers, comonomers, and hydrogen, and the isolated polymer molten material was then pelletized and packaged. The separated stream containing the solvent, monomers, comonomers, and hydrogen was recycled after the removal of the purged stream.
[0125] [Table 5]
[0126] Polymer blending process conditions Polymer blends IE1-IE3 and CE3 were produced by compounding them in a twin-screw extruder. Table 5 lists the polymer blend compositions, and Table 6 lists the compounding conditions.
[0127] [Table 6]
[0128] [Table 7]
[0129] Polymer blend properties The polymer blend characteristics of the examples and comparative examples of the present invention are listed in Tables 7 to 10.
[0130] [Table 8]
[0131] [Table 9]
[0132] [Table 10] ND=Not determined
[0133] [Table 11] ND=Not determined.
[0134] film The three-layer film had an A / B / A structure, where A was a skin layer containing DOWLEX® 2045G, an LLDPE with a density of 0.920 g / cc and a melt index of 1, and B was a core layer containing the polymer blend composition of the present invention or a comparative polymer blend composition. The film was extruded using a 9-layer Collin Blown Film Line according to the processing parameters in Table 11.
[0135] [Table 12]
[0136] The mechanical and optical properties of the film examples and comparative film examples of the present invention are disclosed herein. As shown in Table 5, all examples of the present invention (IE1 to IE3) were LDPE / HDPE blends containing 5% by weight of HDPE, while comparative examples CE1 and CE2 contained 100% by weight of LDPE, and CE3 was an LDPE / HDPE blend containing 5% by weight of HDPE. The properties of the films containing the polymer blends are disclosed in Table 12. The performance of each polymer blend composition was compared in the form of a three-layer film. The mechanical and optical properties of the polymer blend films are listed in Table 12.
[0137] [Table 13]
[0138] Overall, the embodiments of the present invention demonstrated remarkable improvements in internal haze, total haze, and shrinkage %MD compared to the comparative examples (see Table 12). Due to the improved optical and mechanical properties, the embodiments of the present invention also exhibited comparable processability to the comparative examples described later.
[0139] Generally, there is a trade-off between the optical and mechanical properties of polyethylene. However, the inventive example exhibited desirable mechanical properties. In particular, the inventive example showed significantly greater shrinkage in the mechanical direction (MD) compared with the comparative example. The lateral (CD) shrinkage of the embodiment of the present invention remained equivalent to that of the comparative example. Therefore, these results suggest that the embodiment of the present invention had mechanical properties equivalent to or better than those of the 100 wt% LDPE embodiment and the comparative LDPE / HDPE blend embodiment.
[0140] As shown in Table 12, the embodiments of the present invention exhibited improved optical quality. In particular, the embodiments of the present invention showed a significant reduction in internal haze and overall haze compared to the comparative examples. The embodiments of the present invention also showed improved Zebedee clarity compared to CE2 and CE3.
[0141] In conclusion, the disclosed HDPE / LDPE blend composition improves mechanical properties without impairing optical properties.
[0142] It will be apparent to those skilled in the art that various modifications and changes can be made to the embodiments described herein without departing from the spirit and scope of the claimed subject matter. Accordingly, this specification is intended to cover such modifications and changes to the various embodiments described herein, provided that such modifications and changes fall within the scope of the appended claims and their equivalents.
Claims
1. A polymer blend comprising low-density polyethylene (LDPE) and less than 10% by weight of high-density polyethylene (HDPE), The LDPE has a density of 0.910 to 0.925 g / cc, a melt index (I2) of 0.2 to 0.8 dg / min, and a M content of 4 to 10. w (cc) / M n (cc) equipped, The HDPE has a density of 0.940 to 0.970 g / cc, an I2 of 0.6 to 10 dg / min, and 2 to 5 M w (cc) / M n (cc) equipped, The polymer blend has a density of 0.918 to 0.926 g / cc, an I2 of 0.2 to 0.8 dg / min, and 4 to 9 M w (cc) / M n A polymer blend containing (cc).
2. The density of the LDPE is 0.920 to 0.925 g / cc, the I2 of the LDPE is less than 0.5 d g / min, and the M of the LDPE is w (cc) / M n The polymer blend according to claim 1, wherein the (cc) is 6 to 9.
3. Said LDPE has, when measured according to TD-GPC, an M of 5 to 20 z (abs) / M w (abs) and a gpcBR greater than 0.05, the polymer blend according to claim 1 or 2.
4. The polymer blend according to any one of claims 1 to 3, wherein the LDPE has a melt strength of 15 to 25 cN.
5. The polymer blend according to any one of claims 1 to 4, wherein the polymer blend comprises 2 to 10% by weight of HDPE or 3.5 to 5% by weight of HDPE.
6. The polymer blend has 14 to 21 M z (abs) / M w A polymer blend according to any one of claims 1 to 5, having (abs) and gpcBR greater than 0.
05.
7. The polymer blend according to any one of claims 1 to 6, wherein the I2 of the polymer blend is less than 0.5 dg / min.
8. The polymer blend according to any one of claims 1 to 7, wherein the polymer blend has a melt strength of 15 to 20 cN.
9. A film comprising a polymer blend according to any one of claims 1 to 8, wherein the film is a single-layer film or a multi-layer film.
10. The film according to claim 9, wherein the film is a multilayer film containing the polymer blend in a core layer.
11. A composition comprising an ethylene polymer, wherein the ethylene polymer has a density of 0.918 to 0.926 g / cc, an I2 of 0.2 to 0.8 dg / min, and an M of 4 to 9. w (cc) / M n A composition comprising (cc).
12. The composition according to claim 11, wherein the ethylene-based polymer is LDPE.