Spiral-wound pipe insulation

The spirally winding method with a two-stage binder and controlled humidity ensures efficient production of high-quality fibrous pipe insulation, addressing the limitations of conventional processes by enhancing production speed and product characteristics.

JP2026539023APending Publication Date: 2026-11-19OWENS CORNING INTELLECTUAL CAPITAL LLC
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026523438
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-27
Filing Date
2024-10-18
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Conventional fibrous pipe insulation production processes are slow, limiting production capacity and unable to produce flexible and high-quality pipe insulation efficiently.

Method used

A method involving spirally winding individual sheets of fibrous insulation material around a mandrel, applying a two-stage binder to ensure material shape and tensile strength, and controlling humidity to maintain dimensional stability, allowing for high-speed production of integrated tubular pipe insulation.

Benefits of technology

The method enables production of fibrous pipe insulation at rates exceeding 30 feet per minute with improved flexibility, appearance, and performance compared to conventional methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539023000001_ABST
    Figure 2026539023000001_ABST
Patent Text Reader

Abstract

The pipe insulation is formed from multiple individual sheets of glass fiber moistened with a binder composition. The sheets are spirally wound around a mandrel so as to partially overlap. The wound sheets are further processed to join together to form a single elongated cylinder. The binder within the elongated cylinder is then cured to form the pipe insulation.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] (CROSS-REFERENCE TO RELATED APPLICATIONS) This application claims the priority and benefit of U.S. Provisional Application No. 63 / 593,557, filed on October 27, 2023, the entire content of which is incorporated herein by reference.

[0002] (FIELD OF THE INVENTION) The general concept of the present invention relates to fibrous pipe insulation, and more specifically, to spirally wound pipe insulation.

BACKGROUND ART

[0003] It is known to enclose pipes with fibrous insulation, for example to improve energy efficiency. A conventional process for forming fibrous pipe insulation is the continuous molded pipe (CMP) process. The CMP process is typically used to form smaller diameter pipe insulation, such as those having an inner diameter of 6 inches (15.24 cm) or less.

[0004] In the CMP process, raw materials ("batch"), which may include recycled glass cullet, are melted at high temperatures (e.g., above 2,000°F (1,093.33°C)) to produce molten glass. The molten glass is then used to form solid fibers, which are deposited on a conveyor to form a fiber "pack" having a desired thickness. The pack is cut into specific lengths and / or widths each forming a "belt" having a thickness. The width of the belt substantially corresponds to the circumference of the pipe insulation to be produced.

[0005] The belt is then fed into a mold and folded around a fixed hollow mandrel centered within the mold. The mold itself is a hollow tube that is at least partially perforated so that heated air can be forced into and drawn out of the mold.

[0006] The pelt is cured in a mold and on a mandrel to form a pipe insulation section as a tubular body. In particular, the size of the mandrel defines the inner diameter of the pipe. Similarly, the mold defines the outer diameter of the pipe, and the distance between the mold and the mandrel limits the wall thickness of the pipe.

[0007] Hardening can be achieved by using multiple heat sources, such as an induction heater (located at the beginning of the mold), to harden the outer surface of the tube, and by applying heated air to both the inside of the mold and the through-holes formed in the mandrel. As a result, the outside of the tube is rigid, while the inside has a softer core that can be compressed to form fittings and other complex pipe shapes.

[0008] The pipe insulation section is stretched through a mold using woven fiberglass scrim, and the fiberglass scrim separates from the pipe insulation as it exits the mold.

[0009] As the pipe insulation section exits the mold, a longitudinal seam is cut through the top of the pipe insulation section, and a partial longitudinal back cut is formed along the bottom of the pipe insulation. These cuts facilitate the later installation of the pipe insulation around the pipe. As the pipe insulation section exits the mold, it is cut transversely to the desired length of pipe insulation (e.g., up to 36 inches (91.44 cm)).

[0010] In some embodiments, the jacket is applied to the outer surface of the pipe insulation (e.g., by being bonded).

[0011] An exemplary pipe insulation 100 produced by CMP or other conventional mandrel-based processes is shown (in cross-section) in Figure 1. The pipe insulation 100 is formed from a fibrous insulation material 102 (e.g., glass fiber) as an elongated hollow cylinder having a wall thickness 104 and an internal cavity 106. The internal cavity 106 defines the inner diameter 108 of the pipe insulation 100. The inner diameter 108 of the pipe insulation 100 is selected to match the outer diameter of the pipe or pipe-like member to be insulated. An optional outer jacket 110 is wrapped around the insulation material 102 and, among other things, serves as a vapor barrier for the pipe insulation 100. The outer jacket 110 can also serve as an aesthetic cover for the insulation material 102. Slits 112 are formed through the insulation material 102 to facilitate the placement of the pipe insulation 100 around the pipe. To further facilitate the installation of the pipe insulation 100, a partial slit 114 can also be formed on the side of the insulation material 102 opposite to the slit 112. The partial slit 114 typically does not extend through the entire thickness 104 of the insulation material 102 (and does not break through the outer jacket 110). After the pipe insulation 100 is fitted around the pipe, a portion of the outer jacket 110 forms a cover 116 that extends over (and seals) the slit 112.

[0012] The drawbacks of conventional molding processes, as well as other fibrous pipe insulation production processes, are that they often involve relatively slow production times, which significantly limits the amount of material that can be produced over a given period. For example, conventional molding processes may only be able to produce about 12 sections of 3-foot (0.9144-meter) pipe insulation per minute. Therefore, there is an unmet need for a faster and more efficient fibrous pipe insulation production process that can produce fibrous pipe insulation comparable to the slower conventional processes. Furthermore, since the spiral winding process "constructs" the pipe insulation from multiple separate layers, it can increase the flexibility of product offerings or product characteristics that cannot be achieved with conventional production processes. In addition, spiral winding pipe insulation may exhibit improved appearance and / or performance compared to conventional pipe insulation. [Overview of the Initiative]

[0013] The general concept of the present invention encompasses a method for forming pipe insulation by joining individual sheets of fibrous insulation material to form a substantially integrated tubular structure. In particular, the sheets are spirally wound around a mandrel or similar structure to form pipe insulation.

[0014] In one exemplary embodiment, a method for forming pipe insulation is disclosed. This method includes providing a plurality of sheets of insulation material, each containing a plurality of glass fibers and a binder; compressing each sheet of insulation material (for example, to have a thickness in the range of about 1.5 mm to about 6.5 mm); drying each sheet of insulation material (to remove most of the water from the sheet); orienting each sheet of insulation material toward a mandrel at an approach angle α, where α ≠ 90 degrees; and spirally winding each sheet so as to partially overlap each other to form an elongated hollow cylinder of insulation material having a wall thickness in the range of about 10 mm to about 55 mm. The binder of each insulation sheet is substantially uncured when the sheet is spirally wound onto the mandrel. In some embodiments, each sheet of insulation material has a width in the range of about 35 mm to about 80 mm. In some embodiments, each sheet of insulation material has a density of about 195 g / m². 2 ~about 410g / m 2 It has a fiber area weight (FAW) within the range of [specify range]. In some embodiments, each sheet of the thermal insulation material has a fiber basis weight variation within the range of approximately FAW ± 50%.

[0015] In some exemplary embodiments, each sheet of the thermal insulation material has a first scrim bonded to the upper surface of the sheet and a second scrim bonded to the bottom surface of the sheet, the first and second scrims being removed from the sheet after drying and before the sheet is spirally wound.

[0016] In some exemplary embodiments, the method further includes hydrating each sheet of thermal insulation material on a mandrel by applying about 1% to about 5% by weight of water to the sheet based on the weight of the sheet.

[0017] In some exemplary embodiments, the method further includes kneading sheets of thermal insulation material on a mandrel to redistribute a portion of the binder located in the overlapping portions of the sheets.

[0018] In some exemplary embodiments, the method further comprises baking at least a portion of each innermost sheet of insulation material on the mandrel (i.e., the sheet in contact with the mandrel) and a portion of each outermost sheet (i.e., the sheet farthest from the mandrel).

[0019] In some exemplary embodiments, baking comprises applying heat in a range of about 750°F (398.89°C) to about 900°F (482.22°C) to the innermost sheet and the outermost sheet for about 1 / 8 second to about 1 second.

[0020] In some exemplary embodiments, the method further comprises curing the binder of the elongated hollow cylinder on the mandrel.

[0021] In some exemplary embodiments, curing comprises applying heat in a range of about 475°F (246.11°C) to about 650°F (343.33°C) to the sheets for at least about 5 seconds.

[0022] In some exemplary embodiments, the method further comprises cutting the elongated hollow cylinder to a desired length as the elongated hollow cylinder exits the mandrel.

[0023] In some exemplary embodiments, the method further comprises cutting a longitudinal slit into the length of the elongated hollow cylinder.

[0024] In some exemplary embodiments, the method further comprises applying an outer jacket material to the length of the elongated hollow cylinder.

[0025] In some exemplary embodiments, spiral winding is effective to produce about 24 sections of 3-foot (0.9144 meter) pipe insulation per minute.

[0026] In some exemplary embodiments, the internal cavity of the elongated hollow cylinder has a diameter of less than 67 mm.

[0027] In some exemplary embodiments, the fibers in each sheet have an average fiber diameter ranging from about 6 μm to about 9 μm.

[0028] In some exemplary embodiments, each sheet has a binder of about 5% LOI to about 8% LOI.

[0029] In some exemplary embodiments, the pipe insulation has a density of about 56,000 g / m 3 to about 88,000 g / m 3 in the range.

[0030] In some exemplary embodiments, the uncured binder is substantially free of formaldehyde.

[0031] In some exemplary embodiments, the binder comprises polyacrylic acid and sorbitol.

[0032] In some exemplary embodiments, at least one belt is used to helically wind the sheet along the mandrel.

[0033] In some exemplary embodiments, 2 to 32 sheets are used to form the pipe insulation.

[0034] In some exemplary embodiments, the number of sheets is selected to define the thickness of the elongated hollow cylinder of insulating material.

[0035] In some exemplary embodiments, the mandrel is stationary.

[0036] In some exemplary embodiments, the mandrel is hollow and includes a plurality of apertures extending therethrough.

[0037] In some exemplary embodiments, pipe insulation is formed at a rate of more than 12 sections of 3-foot (0.9144 meter) pipe insulation per minute. In some exemplary embodiments, pipe insulation is formed at a rate of more than 18 sections of 3-foot (0.9144 meter) pipe insulation per minute. In some exemplary embodiments, pipe insulation is formed at a rate of more than 24 sections of 3-foot (0.9144 meter) pipe insulation per minute.

[0038] Other aspects and features of the general concept of the present invention will become more readily apparent to those skilled in the art by considering the following description of various exemplary embodiments in conjunction with the accompanying drawings. [Brief explanation of the drawing]

[0039] The general concept of the present invention, as well as its embodiments and advantages, will be described in more detail below, with reference to the drawings as examples. [Figure 1] This is a cross-sectional view of a conventional pipe insulation material. [Figure 2] This is a cross-sectional view showing the buckling of hardened glass fiber material wrapped around a stationary mandrel. [Figure 3] A system for forming a glass fiber pelt for use in forming pipe insulation, according to one exemplary embodiment. [Figure 4] This diagram illustrates various concepts of spiral winding. [Figure 5] One exemplary embodiment is a system for conditioning and cutting the glass fiber pelt shown in Figure 3. [Figure 6] This is a system for spirally winding the glass fiber sheet shown in Figure 5, according to one exemplary embodiment. [Figure 7] A flowchart shows a method for forming a spiral-wound pipe insulation material according to one exemplary embodiment. [Modes for carrying out the invention]

[0040] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by those skilled in the art in which the present invention pertains. Any methods and materials similar or equivalent to those described herein may be used in carrying out or testing the present invention, but preferred methods, devices, and materials are described herein. All references, publications, patents, patent applications, and commercially available materials referenced herein are incorporated herein by reference for all purposes, including describing and disclosing methodologies reported in publications that may be used in connection with the present invention. Nothing herein should be construed as admitting that the present invention has no prior rights to such disclosures for the sake of prior art.

[0041] The general concept of the present invention relates to pipe insulation formed by spirally winding many binder-impregnated sheets of fibrous insulation material around a mandrel so as to partially overlap, and then curing the binder to form a substantially integral tubular body (e.g., an elongated hollow cylinder). In some embodiments, the resulting spiral-wound pipe insulation has an inner diameter of 6 inches (15.24 cm) or less.

[0042] In particular, spirally winding fibrous pipe insulation at a desired production rate of more than 30 feet (9.14 meters) per minute, more preferably more than 60 feet (18.29 meters) per minute, presents numerous technical challenges, some of which are described herein.

[0043] In the spiral winding process, several layers (e.g., sheets) of the introduced fiberglass material are wound around a mandrel, with each sheet supplied at a specific angle of incidence relative to the mandrel (see Figure 6). In some embodiments, 2 to 32 sheets of fiberglass material are used to form the pipe insulation. In some embodiments, the number of sheets is selected to achieve the desired wall thickness of the pipe insulation. In some embodiments, the wall thickness of the pipe insulation ranges from about 10 mm to about 55 mm.

[0044] As a first step, each layer of fiberglass must have a material shape and tensile strength that is sufficient and relatively consistent for good helical winding. If the input material is not sufficiently homogeneous, stable, and strong (within and across the layer), the layer may be damaged during the winding process (e.g., tear) and / or may not behave as required to form pipe insulation (e.g., may not align on the mandrel). These requirements are particularly important at high winding speeds when the layer is under high tension.

[0045] One method for obtaining a glass fiber layer that meets these requirements is to apply a binder to the glass fibers and then activate (i.e., harden) the binder. Hardening the binder makes the glass fiber layer thin and rigid, while also fixing its shape (i.e., the glass fibers retain the shape they had when hardened).

[0046] Curing the fiberglass layer before spiral winding imparts the necessary tensile strength and structural / geometric integrity, but presents at least three significant challenges in fabricating spiral-wound pipe insulation. Firstly, spiral winding a rigid, flat material around a mandrel tends to create creases and wrinkles in the material as it bends around the mandrel (see Figure 2), which can negatively affect the appearance and performance of the product. Secondly, after spiral winding, the pipe insulation needs to be cut along its length to be placed on top of the pipe section. Cutting the cured material can cause the wound fiberglass to undesirably "open up" or try to flatten out in a different way, based on the flat panel shape it had when cured. Finally, the cured layer of fiberglass does not allow the fiberglass within each layer to relax and mix with adjacent layers at the layer-to-layer interface. Thus, the pipe insulation behaves substantially like a laminate rather than a single piece of pipe insulation. This is because the laminated structure tends to separate the insulation layers at the interface between layers to the desired depth, making it unsuitable for filleting (i.e., manually cutting) each section of pipe insulation to a specific depth.

[0047] In some embodiments, the aforementioned problems are mitigated by applying a two-stage binder to the glass fiber layer. The first stage of the binder may be sufficient to impart the required material shape and tensile strength to the glass fiber layer, while also allowing the glass fiber layer to be spirally wound without significant wrinkles or folds. Then, once the glass fiber layer is spirally wound onto the mandrel, the second stage of the binder can be activated to loosen the fibers, promote fiber mixing at the layer interface, and newly fix the shape of the insulation material, thus addressing the problems of fillet formation and shape resetting.

[0048] In some embodiments, a water-soluble binder and water are used. In the first stage, the glass fiber material is treated with a water-soluble binder. The layers are then dried (without curing) to remove the water. As the layers dry, they are also mechanically compressed to bring the glass fiber material to the target thickness. At this point, the glass fiber material can meet the requirements of geometric shape and tensile strength, without "fixing" the shape of the cured profile as in the binder curing process. The material can then be spirally wound around a mandrel to form the appropriate pipe insulation shape. Once the layers are wound around the mandrel, the second stage can begin. In the second stage, water can be reintroduced into the glass fiber material (e.g., by steam) to rehydrate the binder. As the binder becomes fluid, the bonds that held the fibers together are released, allowing the fibers to move relative to each other (i.e., some of the energy stored in the fibers is released). As a result, the glass fiber material expands and begins to swell. By placing a physical barrier around the outer diameter of the fiberglass body and / or by sintering the outer diameter of the body, rigidity can be provided to the outer diameter surface, preventing further bulk expansion in the radial direction. As a result, the fibers within the wound body can be linked together as the binder continues to harden (i.e., crosslink) within the fiberglass body. The hardened binder determines the final shape of the fiberglass body. Relaxation and mixing (e.g., entanglement) of the fibers before the binder hardens results in a more integrated body.

[0049] In some embodiments, the two-step binder includes a thermoplastic step and a thermosetting step. In some embodiments, a blocked thermosetting binder material is used in which crosslinking of the fibers does not occur until a critical temperature is reached. The general concept of the present invention encompasses any other suitable techniques to meet the required shape and tensile strength requirements so that the glass fiber layer can be spirally wound, particularly at production rates of more than 30 feet (9.14 meters) per minute, more preferably more than 60 feet (18.29 meters) per minute. In other words, the technique should enable efficient handling of the glass fiber layer, conforming the glass fiber layer to the shape of the mandrel, bonding the glass fiber layers to each other, and curing the glass fiber layer to form an integral body of pipe insulation.

[0050] A system 300 or module for producing a glass fiber material suitable for use in forming spiral-wound pipe insulation, according to an exemplary embodiment, is shown in Figure 3.

[0051] In an exemplary system 300, a fiber forming station 302 or other fiber source provides glass fibers 304 to which a binder 306 is applied (e.g., by spraying).

[0052] The glass fibers 304 have an average diameter in the range of about 20 HT (5.1 μm) to about 36 HT (8.9 μm). In some embodiments, the glass fibers 304 have an average fiber diameter of about 33 HT (8.4 μm). The glass fibers 304 are formed or manipulated (e.g., shredded) to have a desired average length.

[0053] The binder 306 is typically an aqueous binder 306 composition. In some embodiments, the binder 306 is substantially free of added formaldehyde. In some embodiments, the binder 306 comprises polyacrylic acid and sorbitol.

[0054] In some embodiments, the binder 306 constitutes about 2% to about 12% of the LOI. In some embodiments, the binder 306 constitutes about 6.5% of the LOI.

[0055] In some embodiments, the binder 306 is a composition described or suggested in U.S. Publication No. 2022 / 0106419, the entire disclosure of which is incorporated herein by reference. These binders have properties (e.g., hygroscopic, water-soluble, low viscosity) that facilitate conditioning of the glass fiber pelt in the helical winding applications of the present invention.

[0056] In some embodiments, the lower scrim 320 is supplied onto the conveyor 308. The glass fibers 304, to which the binder 306 has been applied, are deposited onto the lower scrim 320 located on the conveyor 308. In this way, the glass fibers 304 impregnated with the binder 306 form a glass fiber pelt 310. In some embodiments, the conveyor 308 moves at a speed of approximately 5 feet (1.52 meters) per minute to approximately 25 feet (7.62 meters) per minute.

[0057] As the fiberglass pelt 310 passes through the conveyor 308, the trimmer 312 removes excess material from the edges of the fiberglass pelt 310. As a result, the fiberglass pelt 310 is appropriately sized to form many individual fiberglass sheets (see Figure 4). In some embodiments, after passing through the trimmer 312, an upper scrim 330 is applied to the fiberglass pelt 310. The fiberglass pelt 310, including the scrims 320 and 330, is then wound onto a roll 340. Assuming the necessary criteria are met, the roll 340 of fiberglass material (i.e., the fiberglass pelt 310) can be used to form fiberglass sheets, and the fiberglass sheets can also be used to form spiral-wound pipe insulation. For example, as described herein, the distribution of fibers 304 within the pelt 310 must match with minimal variation so that the sheets formed therefrom (see Figure 5) also match each other, which is important when the sheets are fed into a spiral winder (see Figure 6). Generally, the use of scrims 320 and 330 is optional.

[0058] It was found that in order to successfully wind the uncured fiberglass material onto the spiral tube, the input material must be dimensionally stable and possess sufficient tensile strength to prevent the belt from breaking when it is drawn onto the mandrel. Furthermore, the belt must exhibit sufficient shear strength to withstand and evenly distribute the driving force applied from the winder belt through the belt without losing its integrity.

[0059] Uncured or undried, uncompressed pelt has been found to exhibit variations in area weight, making it difficult to consistently guide the pelt onto a spiral winder mandrel. Because the compressive strength of uncured pelt is extremely low, it deforms (compresses) locally when pressed against a guide, making it impossible to use edge guides to control the pelt's path. Therefore, tension is a preferred means of controlling unstable pelt. However, tension through unstable pelt follows a path determined by the region of highest fiber density. This is because these regions generally exhibit higher tensile strength and less elongation under stress than lower density regions. When unstable pelt is subjected to tension, the tensile load path defined by the high-density region is stretched almost linearly. Then, randomly distributed low-density regions bordering the tension path form the edges of the unstable pelt as it is wound onto the mandrel. The resulting pelt edges are no longer linear, making consistent alignment with adjacent wound pelt edges virtually impossible without active pelt alignment. The density variations of unstable pelt also cause problems when wrapping too many additional layers to increase thickness or when overlapping adjacent wraps to increase structural integrity. Low-density areas are more compressed than high-density areas. Generally, when wrapping unstable pelt under tension, the pelt tends to follow a path influenced by the local total density with adjacent pelts. The pelt tends to move towards low total density areas and away from high total density areas. This makes the production of consistent pipe sections from unstable pelt impossible.

[0060] It has been found that drying glass pelt to a consistent compression thickness significantly improves its physical properties. For example, an uncured pelt may have a tensile strength of about 5 pounds compared to the same pelt compressed and dried to a tensile strength of over 25 pounds. This improvement is a result of additional solid bonds formed under compression. In some exemplary embodiments, the binder consists mainly of sorbitol and polyacrylic acid. When completely dry but not cured, the binder creates functional bonds between two or more adjacent fibers. This binder formulation is highly hygroscopic and can absorb enough water from the atmosphere to allow the binder to become fluid when the relative humidity exceeds 35%. Once the binder is sufficiently hydrated, its viscosity is low enough to allow fibers to move within the pack structure. The higher the tensile, compressive, and shear strengths, the more dimensionally stable the dried pelt is under the loads applied for winding. The pelt path can be controlled (e.g., using edge guides), and local density variations have minimal impact on pelt tracking during winding.

[0061] Furthermore, the inability to maintain the dimensional stability of the uncured pelt impairs the compressive, tensile, and shear strengths of the pelt, as well as the quality of the helical winding. As dimensional stability decreases, the overall stability of the pelt decreases, which reduces winding performance. Figure 4 provides a simplified diagram of the helical winding process to help illustrate the importance of dimensional stability. The winding angle α in Figure 4 is determined by the width of the fiberglass pelt (i.e., w in Figure 4) and its thickness. Generally, the thinner the material, the easier it is from a geometric standpoint to wind it in a way that avoids gaps between helices along the thickness of the material. Inconsistent width along the length of the pelt is undesirable because it requires dynamic adjustment of the winding angle. Changes in thickness throughout operation require dynamic adjustment of the pelt width, which is not possible.

[0062] As described above, the formation of wrinkles on the inner surface of the wrapped pelt, which results from wrapping the material around the mandrel, also differs depending on the thickness of the pelt. The bonding strength of the binder is sufficient to prevent any significant in-plane stretching or compression of the pelt, and thus wrinkles are formed when the inner surface fibers buckle in response to compressive forces arising from the circumferential difference between the inner and outer surfaces of the wrapped pelt. The thinner the pelt, the smaller the circumferential difference between the inner and outer surfaces, and consequently, the fewer wrinkles there are. In general, the feed material for the helical winding process (e.g., sheet 514) should typically be "as thin as possible".

[0063] Therefore, there is an interrelationship between the physical properties of each fiberglass sheet and its dimensional stability. The width and thickness of the sheet must be consistent over the length of the sheet, and the thickness must be "as thin as possible" to facilitate good spiral winding from a geometric standpoint. The compressive strength (i.e., the "tightening" of the material against the winding mandrel by the spiral winder belt), tensile strength (i.e., the tension of the material from the belt when pulled by the spiral winder), and shear strength (i.e., the tearing induced by the angle at which the material is supplied to the winder) should be sufficient from a mechanical standpoint to avoid affecting the dimensional stability of the sheet through physical deformation of the sheet.

[0064] Furthermore, the effect of humidity on the dimensional stability of the input material was considered. In some embodiments, the binder composition used in the input material (e.g., the binder composition described in U.S. Publication No. 2022 / 0106419) is highly hygroscopic and can absorb a significant amount of water from the atmosphere when the relative humidity exceeds 35%. In these cases, the dried and compressed fiberglass sheet would benefit from several measures to prevent the absorption of moisture from the air, which could cause the sheet to re-loft. Humidity-controlled storage and manufacturing spaces can prevent rehydration of the surroundings.

[0065] In some embodiments, the binder composition is formulated to maintain the dimensional stability of the sheet under typical ambient humidity conditions. For example, the binder composition may contain a secondary thermoplastic binder component that has sufficient strength to hold the sheet in its desired state in the presence of high humidity, but exhibits a low Tg with a rapid decrease in viscosity above 120°F (48.89°C), thus completely releasing all fiber bonds, while becoming liquid below 135°F (57.22°C), thus forming around the fibers at temperatures below the binder's curing temperature, and then forming bonds upon cooling.

[0066] Considering the above, it has been found that drying and compressing the uncured glass fiber material to form a sheet of a specific width and thickness can stabilize the material dimensionally and impart sufficient compressive, tensile, and shear strength to the material, thereby supporting the formation of a tubular insulation body by spiral winding. In some cases, it is also important to control the behavior of the binder composition before spiral winding of the uncured glass fiber material.

[0067] A system 500 or module for producing a fiberglass sheet or layer suitable for use in forming spiral-wound pipe insulation, according to an exemplary embodiment, is shown in Figure 5. System 500 prepares and divides suitable fiberglass material, such as a roll 340 (i.e., fiberglass pelt 310) of fiberglass material produced by system 300.

[0068] In the exemplary system 500, a roll 340 of fiberglass material is unwound and fed into an oven 502 (as fiberglass pelt 310). Specifically, the pelt 310 is pulled through the oven 502 in the direction indicated by arrow 504. For example, the pelt 310 is pulled in direction 504 by a winder 510 that exerts tension on the upper scrim 330 and lower scrim 320 of the pelt 310. The oven 502 dries (but does not harden) the pelt 310, removing a significant, if not all, of the water present in the binder of the pelt 310.

[0069] Generally, drying should remove an amount of moisture that prevents the binder from softening or flowing, over a certain period of time (e.g., 72 hours) at a given temperature. In some embodiments, the amount of moisture removed is such that the dimensional stability of the glass fiber pelt 310 is ensured when the material is subsequently exposed to a relative humidity of 30% or less.

[0070] Furthermore, the pelt 310 is pulled (by the winder 510) through a fixture 506 located inside the oven 502 (for example, extending through it). The fixture 506 compresses the pelt 310 to the desired thickness and maintains the pelt 310 at this thickness, while the pelt is dried inside the oven 502. In some embodiments, the desired thickness is in the range of about 1.5 mm to about 6.5 mm.

[0071] It is important that the compression of the pelt 310 is started before the pelt 310 dries. Therefore, the pelt 310 can enter the fixture 506 before or at the entrance of the oven 502. In some embodiments, at least a portion of the fixture 506 inside the oven 502 is perforated to facilitate the drying of the material passing through the fixture 506.

[0072] As the dried and compressed pelt 508 exits the oven 502, the upper scrim 330 and lower scrim 320 are removed from the pelt 508 (e.g., by a winder 510). In this way, the dried and compressed pelt 508 proceeds to the slitting station 512, where the pelt 508 is separated (e.g., cut) into a plurality of individual sheets 514 having a desired width. In some exemplary embodiments, the pelt 508 is slit to form a plurality of sheets, each having a width of about 12 inches (30.48 cm), each having the same desired width. In some embodiments, the desired width ranges from about 35 mm to about 80 mm.

[0073] The sheets 514 are collected onto one or more rolls 516 (for example, by a winder 520) for later use when forming spiral-wound pipe insulation.

[0074] As a measure of material consistency, each individual fiberglass sheet 514 produced by System 500 weighs approximately 195 g / m². 2 ~about 410g / m 2 It has a fiber area weight (FAW) within a certain range and a fiber basis weight variation within a range of approximately FAW ± 50%. Therefore, any variation in FAW along the length of the glass fiber sheet 514 (for example, when measured in increments of 1 foot (0.9144 meters)) should be within ± 50% of the FAW. The variation in fiber basis weight can be measured, for example, by X-ray gauge measurement.

[0075] Using appropriate input material (e.g., sheet 514), the spiral winding process can wind multiple layers of input material around a stationary mandrel to form and determine a desired shape corresponding to the pipe insulation body. In some embodiments, the pipe insulation body is an elongated hollow cylinder with a wall thickness ranging from about 10 mm to about 55 mm.

[0076] A system 600 or module for forming spiral-wound pipe insulation according to an exemplary embodiment is shown in Figure 6. The pipe insulation can be formed at a relatively high speed (e.g., more than 60 feet (18.29 meters) per minute) with minimal gaps, wrinkles, and bunching.

[0077] In the exemplary system 600, multiple layers (e.g., 2 to 32 layers) of input material 602 (e.g., sheet 514) are supplied to a stationary mandrel 604. Each layer of input material 602 has approximately the same thickness (e.g., about 1.5 mm to about 6.5 mm) and approximately the same width (e.g., about 35 mm to about 80 mm).

[0078] The supply direction indicated by arrow 606 forms the entry angle α of the input material 602 relative to the mandrel 604. The angle α is not equal to 90 degrees. The layers of input material 602 can overlap each other on the mandrel 604 to construct the desired wall thickness. In some embodiments, water 608 is applied (e.g., sprayed) to the glass fiber layer as it is supplied to the spiral winder to initiate rehydration of the layer. Similarly, in some embodiments, a binder / water mixture can be applied (e.g., sprayed) onto the glass fiber layer as it is supplied to the spiral winder to improve adhesion.

[0079] The primary winder 610 is formed from a belt driven by a pair of rotating shafts. The central section of the belt is wound around or twisted around the mandrel 604 so that it can contact the layer of input material 602 on the mandrel 604. Thus, the rotation of the belt drives the input material 602 downward along the length of the mandrel 604 in the production direction indicated by arrow 612.

[0080] As individual layers of input material 602 are placed on the mandrel 604 and advanced along their length by the primary winder 610, further processing of the input material 602 is required to form a single tubular body (i.e., pipe insulation).

[0081] In some embodiments of the system 600, as described above, water 608 can be applied (e.g., sprayed) to the layer of input material 602 before the layer is wrapped around the mandrel 604. The amount of water 608 applied to the layer is at least about 1% of the weight of the incoming glass fiber layer and no more than 5% of the weight of the layer.

[0082] In some embodiments of the system 600, instead of applying water 608 to the layer of input material 602, or in addition to it, a source of saturated steam 614 may be applied at a mass flow rate similar to that of water. For example, 0-50% of the steam 614 can be applied to the inside of the mandrel 604 and allowed to flow into the glass fibers through the holes 616 along the length and circumference of the mandrel 604. The remainder (50-100%) of the steam 614 can be applied to the outer surface of the glass fibers on the mandrel 604 via an annular nozzle arrangement located close to the mandrel 604. In this case, the total amount of water applied is still in the range of about 1-5% of the weight of the glass fibers.

[0083] In any case, rehydrating the previously compressed and dried fiberglass sheet 514 as the input material 602 restores the binder to a fluid state, allowing the fiberglass material to begin decompression (i.e., re-lofting), which can assist in further processing of the fiberglass material on the mandrel 604. For example, rehydrating the binder can promote the mobility of the binder and fibers, relieve internal fiber stress, smooth out wrinkles, form new bonds, and promote interlayer bonding. In some embodiments, as the thickness of the input material 602 expands, an external physical barrier (e.g., a rigid sleeve) can be used to control its final thickness.

[0084] In some embodiments of the system 600, the fiberglass layer (e.g., sheet 514) on the mandrel 604 is physically manipulated. For example, a kneading mechanism 618 can engage with the fiberglass layer on the mandrel 604. In some embodiments, the kneading mechanism 618 comprises a ring that surrounds the layer on the mandrel 604 and rotates at an absolute speed equivalent to the surface speed of the layer as it moves downward on the mandrel 604. The ring may have several (e.g., 2 to 4) rollers on it. The rollers are pressed into the glass while rotating circumferentially so that the movement of the glass proceeds in the mechanical direction 612. Massaging of individual fiberglass layers is performed to induce slippage between fibers within the layer, which causes displacement of the binder and redistribution of the binder at the layer interface. This process breaks down the individual layer arrangement over the thickness and length of the tubular body formed on the mandrel 604, facilitates the formation of new bonds, and also helps to smooth out wrinkles. Those skilled in the art will understand that other mechanical means can be used instead of the exemplary kneading mechanism 618 to achieve these results.

[0085] In some embodiments of the system 600, the glass fiber layers closest to and furthest from the mandrel 604 (e.g., sheet 514) are subjected to initial (i.e., pre-curing) heating by the curing mechanism 620. In some embodiments, the curing mechanism 620 is an induction-heated sleeve and an induction-heated steel mandrel (e.g., mandrel 604), with the sheet positioned between them. The heated sleeve is in contact with the outermost layer, and the heated mandrel is in contact with the innermost layer.

[0086] The baking mechanism 620 rapidly dries and hardens the binder in shallow zones located near the outer and inner surfaces of the wrapped fiberglass layer, stabilizing the formed tubular structure, adding tensile strength, and minimizing binder adhesion. Depending on the production speed (e.g., 60 feet (18.29 meters) per minute), the baking mechanism 620 can form the required outer "crust" by applying heat in the range of approximately 750°F (398.89°C) to approximately 900°F (482.22°C) for approximately 1 / 8 second to approximately 1 second. The baked layer 622 forms a more uniform structure as a result of the baking.

[0087] The baking layer 622 is then driven along a portion of the mandrel 604 as it passes through the oven 630. Heated air 632 is introduced into the oven 630 (e.g., by flow), surrounding the baking layer 622 on the mandrel 604, and then exits the oven 630 as cooler air 634. Thus, the forced hot air convection oven 630 removes excess moisture from the baking layer and cures (i.e., crosslinks) the binder within it. Typically, the baking layer 622 is cured as quickly as possible in the oven 630.

[0088] In some embodiments of the system 600, an optional secondary winder 640 is utilized. The secondary winder 640 is formed from a belt driven by a pair of rotating shafts. The central section of the belt is wrapped around or twisted around the mandrel 604 so that it can contact the layer of input material 602 on the mandrel 604. Thus, the rotation of the belt further drives the input material 602 downward along the length of the mandrel 604 in the production direction 612. If necessary, the secondary winder 640 provides tensile force to help move the fiberglass material wrapped along the mandrel 604. When using the secondary winder 640, its belt rotation speed should be synchronized with the belt rotation speed of the primary winder 610. Furthermore, tension control can be used to avoid excessive compression or crushing of the pipe insulation section.

[0089] In some embodiments, the spiral winding and other processing steps involved in determining the shape of the pipe insulation material occur on the same stationary mandrel 604, thereby avoiding problems that may arise when moving the unfinished fiberglass material from one location (e.g., the mandrel) to another.

[0090] In system 600, further processing of the spiral-wound pipe insulation (i.e., tubular bodies formed from individual layers) may include cutting sections from the tubular bodies having a desired length (e.g., up to 36 inches (91.44 cm)), cutting necessary slits into the tubular body sections so that they can be installed around the pipe, and adding outer jacket material to the tubular body sections.

[0091] A method 700 for forming a spiral-wound pipe insulation material according to an exemplary embodiment is shown in Figure 7.

[0092] In method 700, a suitable fiberglass pelt is formed in step 702. The fiberglass pelt is formed from fiberglass and an aqueous binder applied to the fiberglass. The binder-impregnated fiberglass is located between the upper and lower scrims. After being trimmed to the desired width, the fiberglass pelt located between the two scrims is wound onto a roll for subsequent processing.

[0093] As described above, to be suitable for spiral winding, the glass fiber pelt should have substantially consistent dimensions (e.g., width, thickness), fiber distribution, binder distribution, and physical properties (e.g., tensile strength, compressive strength, shear strength) along its length.

[0094] To further prepare the fiberglass pelt for spiral winding, the undried fiberglass pelt is compressed to a reduced thickness in step 704. In some embodiments, the reduced thickness is in the range of about 1.5 mm to about 6.5 mm.

[0095] To further prepare the fiberglass pelt for spiral winding, the compressed fiberglass pelt is dried in step 706 to remove most of the water from the pelt, particularly the binder in the pelt. In some embodiments, substantially all of the water is removed by drying.

[0096] To further prepare the fiberglass pelt for spiral winding, the compressed and dried fiberglass pelt is cut in step 708 to form multiple individual sheets or layers from a single pelt. The width of the sheets may vary based on the position or layer to which the sheets are applied during winding. Ideally, each sheet has a relatively consistent fiber distribution along its length (i.e., across its width and thickness).

[0097] In order to further prepare the fiberglass pelt for spiral winding, in step 710 the cut fiberglass pelt (i.e., sheet) may be subjected to one or more of the following: rehydration, kneading, and baking.

[0098] Hydrating the sheets may involve applying water (e.g., liquid water and / or steam) before the sheets are wound onto the mandrel and / or after the sheets are wound onto the mandrel. In some embodiments, about 1% to about 5% by weight of water is applied to each sheet of the fiberglass material, based on the weight of the sheets.

[0099] Mixing the sheets may include, for example, mechanically massaging the sheets on a mandrel to improve interlayer bonding by redistributing some of the binder located between the sheets (layers).

[0100] Baking the sheets may involve applying enough heat to rapidly (e.g., within 1 second) cure the outer and / or inner surfaces of the tubular body formed from overlapping sheets on a mandrel. The baked outer and / or inner surfaces stabilize the tubular body formed by the sheets.

[0101] Finally, in step 712, the sheet on the mandrel is cured. For example, the sheet on the mandrel may be moved through an oven where it encounters sufficient heat to cure (i.e., crosslink) the binder and "fix" the tubular shape of the fibrous material, forming the pipe insulation body. Since the glass fiber material is first spirally wound into its final shape and then cured, the material is fixed in its spiral shape and can be further processed without issue (for example, it can be cut longitudinally). Therefore, it is important to work with the uncured material from the moment the glass fiber material is formed until it is spirally wound.

[0102] In accordance with Method 700, further processing of the spiral-wound pipe insulation (i.e., a tubular body formed from individual layers) may include cutting sections from the tubular body having a desired length (e.g., up to 36 inches (91.44 cm)), cutting necessary slits into the tubular body sections so that they can be installed around the pipe, and adding outer jacket material to the tubular body sections.

[0103] The systems and methods of the present invention described and suggested herein represent a more efficient and customizable approach for forming fibrous pipe insulation.

[0104] In some embodiments, it may be conceivable that various inventive concepts be combined and utilized. Furthermore, any particular element cited as relating to a specifically disclosed embodiment shall be construed as being available for use in all disclosed embodiments, provided that incorporating that particular element does not conflict with the express conditions of the embodiment. The scope of the general inventive concepts presented herein is not intended to be limited to the specific exemplary embodiments shown and described herein. From the given disclosure, those skilled in the art will not only understand the general inventive concepts and their associated advantages, but will also find a variety of obvious changes and modifications thereto. For example, pipe insulation is described herein as being formed from glass fibers, but other types of fibrous insulation materials (e.g., mineral wool) may also be suitable. It is therefore required to include all such changes and modifications that fall within the spirit and scope of the general inventive concepts described and / or claimed herein, as well as any equivalents thereof.

Claims

1. A method for forming pipe insulation, To provide multiple thermal insulation material sheets, each containing multiple glass fibers and a binder, Each sheet of the insulation material is compressed to have a thickness ranging from approximately 1.5 mm to approximately 6.5 mm. To remove most of the water, dry each sheet of insulation material, This involves orienting each sheet of insulation material toward the mandrel at an approach angle α, where α ≠ 90 degrees. This includes winding each sheet spirally around the mandrel so that they partially overlap, forming an elongated hollow cylinder of the thermal insulation material having a wall thickness in the range of approximately 10 mm to approximately 55 mm. Each sheet of the insulation material has a width ranging from approximately 35 mm to 80 mm. Each sheet of insulation material weighs approximately 195 g / m². 2 ~Approx. 410g / m 2 It has a fiber area weight (FAW) within the range of, Each sheet of the insulation material has a fiber basis weight variation within a range of approximately FAW ± 50%, and A method wherein the binder of each thermal insulation sheet is substantially uncured when the sheet is spirally wound onto the mandrel.

2. Each sheet of the thermal insulation material has a first scrim joined to the upper surface of the sheet and a second scrim joined to the lower surface of the sheet. The method according to claim 1, wherein the first scrim and the second scrim are removed from the sheet after drying and before spiral winding of the sheet.

3. The method according to claim 1, further comprising hydrating each sheet of the insulating material on the mandrel by applying about 1% to about 5% by weight of water to the sheet based on the weight of the sheet.

4. The method according to claim 1, further comprising kneading the sheets of the insulating material on the mandrel in order to redistribute a portion of the binder located in the overlapping portions of the sheets.

5. The method according to claim 1, further comprising baking the innermost and outermost sheets of the thermal insulation material on the mandrel.

6. The method according to claim 5, wherein the baking includes applying heat in the range of approximately 750°F (398.89°C) to approximately 900°F (482.22°C) to the innermost sheet and the outermost sheet for approximately 1 / 8 second to approximately 1 second.

7. The method according to claim 1, further comprising curing the binder of the elongated hollow cylinder on the mandrel.

8. The method according to claim 7, wherein the curing includes applying heat in the range of about 475°F (246.11°C) to about 650°F (343.33°C) to the sheet for at least about 5 seconds.

9. The method according to claim 1, further comprising cutting the elongated hollow cylinder to a desired length when the elongated hollow cylinder exits the mandrel.

10. The method according to claim 9, further comprising cutting a longitudinal slit into the elongated hollow cylinder along the aforementioned length.

11. The method according to claim 10, further comprising applying an outer jacket material to the length of the elongated hollow cylinder.

12. The method according to claim 1, wherein the spiral winding is effective in producing approximately 24 three-foot (0.9144-meter) sections of the pipe insulation per minute.

13. The method according to claim 1, wherein the internal cavity of the elongated hollow cylinder has a diameter of less than 67 mm.

14. The method according to claim 1, wherein the fibers in each sheet have an average fiber diameter in the range of about 6 μm to about 9 μm.

15. The method according to claim 1, wherein each sheet has a binder with an LOI of about 5% to about 8%.

16. The aforementioned pipe insulation material weighs approximately 56,000 g / m 3 ~Approx. 88,000g / m 3 The method according to claim 1, having a density in the range of [value].

17. The method according to claim 1, wherein the uncured binder substantially does not contain formaldehyde.

18. The method according to claim 1, wherein the binder comprises polyacrylic acid and sorbitol.

19. The method according to claim 1, wherein at least one belt is used to spirally wind the sheet along the mandrel.

20. The method according to claim 1, wherein 2 to 32 sheets are used to form the pipe insulation material.

21. The method according to claim 1, wherein the number of sheets is selected to define the thickness of the elongated hollow cylinder of the thermal insulation material.

22. The method according to claim 1, wherein the mandrel is fixed.

23. The method according to claim 1, wherein the mandrel is hollow and includes a plurality of apertures extending through its interior.

24. The method according to claim 1, wherein the pipe insulation is formed at a rate of more than 12 three-foot (0.9144-meter) sections per minute.