Electrolyte for lithium-sulfur batteries and lithium-sulfur batteries containing the same

The electrolyte composition for lithium-sulfur batteries addresses polysulfide leaching by altering the reduction reaction pathway, improving discharge capacity and energy density through a stable film formation on the negative electrode.

JP2026539042APending Publication Date: 2026-11-19LG ENERGY SOLUTION LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026524110
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-01-26
Filing Date
2025-01-24
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Lithium-sulfur batteries face challenges in maintaining high energy density and battery life due to polysulfide leaching, which causes side reactions and reduces discharge capacity.

Method used

An electrolyte composition for lithium-sulfur batteries comprising a non-aqueous solvent, lithium salt, nitrate, and aryl derivatives that alter the reduction reaction pathway of lithium sulfide, using heterocyclic compounds and glycol ethers to form a stable film on the negative electrode, thereby controlling polysulfide leaching.

Benefits of technology

The electrolyte enhances discharge capacity and energy density while extending battery life by stabilizing the electrode interface and reducing side reactions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539042000001_ABST
    Figure 2026539042000001_ABST
Patent Text Reader

Abstract

The present invention relates to an electrolyte for lithium-sulfur batteries and a lithium-sulfur battery containing the same, wherein the electrolyte for lithium-sulfur batteries comprises a non-aqueous solvent, a lithium salt, a nitrate, and an aryl derivative, wherein the non-aqueous solvent comprises a heterocyclic compound containing one oxygen atom (O) or sulfur atom (S) in its ring structure, and a glycol ether, and the aryl derivative comprises a combination of a selenium-based aryl derivative and a tellurium-based aryl derivative.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to an electrolyte for lithium-sulfur batteries and a lithium-sulfur battery comprising the same.

[0002] This application claims priority based on Korean Patent Application No. 2024-0012696 filed on January 26, 2024, and all contents disclosed in the specification and drawings of the said application are incorporated herein by reference in their entirety.

Background Art

[0003] A lithium-sulfur battery refers to a battery system that uses a sulfur-based material having a sulfur-sulfur bond as a positive electrode active material, and uses lithium metal as a negative electrode active material. Sulfur, which is the main material of the positive electrode active material, has the advantages of abundant global resources, non-toxicity, and low atomic weight.

[0004] As the application fields of secondary batteries expand to Electric Vehicles (EVs), Energy Storage Systems (ESS) and the like, lithium-sulfur battery technology that can realize a theoretically high gravimetric energy storage density (about 2,600 Wh / kg) compared to lithium ion secondary batteries having a relatively low gravimetric energy storage density (about 250 Wh / kg) is attracting attention.

[0005] In a lithium-sulfur battery, during discharge, lithium, the negative electrode active material, releases electrons and oxidizes while ionizing into lithium cations, while the sulfur-based material, the positive electrode active material, is reduced while accepting electrons. Here, through the reduction reaction of the sulfur-based material, the sulfur-sulfur bond (SS bond) accepts two electrons and is converted into a sulfur anion. The lithium cations generated by the oxidation reaction of lithium move to the positive electrode via the electrolyte and combine with the sulfur anions generated by the reduction reaction of the sulfur-based compound to form a salt. Specifically, the sulfur before discharge has a cyclic S8 structure, which, through the reduction reaction, becomes lithium polysulfide (LiS x It is converted to ) and completely reduced to produce lithium sulfide (Li2S).

[0006] In this case, due to the low electrical conductivity of sulfur, it is difficult to ensure reactivity with electrons and lithium ions in the solid state of the sulfur-based compound, which is the positive electrode active material. For this reason, in order to improve the reactivity of sulfur in lithium-sulfur batteries, Li2S x Techniques have been developed to improve reactivity by generating intermediate polysulfides to induce liquid-phase reactions. In such techniques, ether-based solvents such as dioxolane and dimethoxyethane (DME), which have high solubility for lithium polysulfides, are used as the electrolyte solvent. As a result, the reactivity of sulfur and the battery life are affected depending on the electrolyte content.

[0007] Furthermore, polysulfide (PS) generated from the positive electrode during the discharge process of lithium-sulfur batteries dissolves into the electrolyte and undergoes a reaction. This polysulfide causes side reactions within the battery, leading to battery degradation. Reducing the amount of electrolyte is important to achieve high energy density cells, but reducing the amount of electrolyte increases the concentration of polysulfide, further accelerating side reactions and reducing battery life. Therefore, there is a need to develop technologies that can achieve high energy density while maintaining a certain amount of electrolyte. [Overview of the Initiative] [Problems that the invention aims to solve]

[0008] Therefore, the problem that the present invention aims to solve is to solve the above-mentioned problems and, according to one embodiment, to provide a lithium-sulfur battery with improved discharge capacity.

[0009] To this end, the aim is to provide an electrolyte for lithium-sulfur batteries that improves problems caused by polysulfide leaching, such as the decrease in resistance characteristics, by controlling the leaching characteristics of polysulfide (PS) by altering the reaction pathway of sulfur (S).

[0010] This aims to provide a lithium-sulfur battery with high energy density and long life characteristics by applying an appropriate amount of electrolyte. [Means for solving the problem]

[0011] To solve the above problems, According to one aspect of the present invention, an electrolyte for a lithium-sulfur battery is provided in the following embodiment.

[0012] The electrolyte for the lithium-sulfur battery according to the first embodiment is A non-aqueous solvent, a lithium salt, a nitrate, a first aryl derivative, and a second aryl derivative, wherein the non-aqueous solvent includes a heterocyclic compound containing one oxygen atom (O) or sulfur atom (S) in its ring structure; and a glycol ether, the first aryl derivative includes at least one compound represented by any one of the following Chemical Formula 1 to Chemical Formula 4, and the second aryl derivative includes at least one compound represented by any one of the following Chemical Formula 5 to Chemical Formula 8.

[0013] [Chemical Formula 1] R 1 -Se-Li [Chemical Formula 2] R 2 -Se-Se-R 3 [Chemical Formula 3] R 4 -Se-S x -Li [Chemical Formula 4] R 5 -Se-S x -Se-R 6 [Chemical Formula 5] R 7 -Te-Li [Chemical Formula 6] R 8 -Te-Te-R 9 [Chemical Formula 7] R 10 -Te-S x -Li [Chemical Formula 8] R 11 -Te-S x -Te-R 12 In the above Chemical Formula 1 to Chemical Formula 8, R 1 to R 12 are each independently a C6 to C 20 aryl group, x is a number from 1 to 8.

[0014] According to the second embodiment, in the first embodiment, The first aryl derivative may include diphenyl diselenide (PDSe).

[0015] According to the third embodiment, in the first embodiment or the second embodiment, The second aryl derivative may include diphenyl ditelluride (DPDTe).

[0016] According to the fourth embodiment, in any one of the first to third embodiments, The weight ratio of the first aryl derivative to the second aryl derivative may be 3:2 to 2:3.

[0017] According to the fifth embodiment, in any one of the first to fourth embodiments, The weight ratio of the first aryl derivative to the second aryl derivative may be 1:1.

[0018] According to the sixth embodiment, in any one of the first to fifth embodiments, The combined weight of the first aryl derivative and the second aryl derivative may be equal to or less than the weight of the nitrate.

[0019] According to the seventh embodiment, in any one of the first to sixth embodiments, The sum of the weights of the first aryl derivative and the second aryl derivative may be 3% by weight or more based on the total weight of the electrolyte.

[0020] According to the eighth embodiment, in any one of the first to seventh embodiments, The volume ratio of the heterocyclic compound to the glycol ether may be 1:3 to 1:10.

[0021] According to another aspect of the present invention, a lithium-sulfur battery of the following embodiment is provided.

[0022] The lithium-sulfur battery according to the ninth embodiment is The lithium sulfur battery comprises: an electrolyte according to any one of the first to eighth embodiments; a positive electrode containing a positive electrode active material; and a negative electrode containing a negative electrode active material, wherein the positive electrode active material includes a sulfur element, a sulfur compound, or a mixture thereof.

[0023] According to the tenth embodiment, in the ninth embodiment, The specific capacity at 0.1C discharge may be 1400mAh / gs or more. [Effects of the Invention]

[0024] An electrolyte for a lithium-sulfur battery according to one embodiment of the present invention has the effect of changing the discharge mechanism of a lithium-sulfur battery by changing the reduction reaction pathway of lithium sulfide.

[0025] As a result, lithium-sulfur batteries using this technology exhibit increased discharge capacity due to the development of additional capacity, thereby achieving a high energy density. [Brief explanation of the drawing]

[0026] [Figure 1] This graph shows the results of evaluating the charge and discharge characteristics of lithium-sulfur batteries using Example 1 and Comparative Examples 1 to 3 in this specification. [Modes for carrying out the invention]

[0027] The present invention will be described in detail below. However, the present invention is not limited to the following, and each component may be modified in various ways or selectively mixed as needed. Therefore, it should be understood that the present invention includes all modifications, equivalents, and substitutions that fall within the spirit and technical scope of the invention.

[0028] In this specification, when a configuration is described as "including" a component, this does not mean that other components are excluded, but rather that other components may be included, unless otherwise specified.

[0029] In this specification, the term "(poly)sulfide (PS)" means "(poly)sulfide ion (S) x 2- , 1≦x≦8) and "Lithium (poly) sulfide (Li2S x or LiS x - This concept encompasses both "1 ≤ x ≤ 8" and "x ≤ 8".

[0030] In this specification, the term "lithium sulfide" refers to the substance Li2S.

[0031] An electrolyte for a lithium-sulfur battery according to one aspect of the present invention is The material comprises a non-aqueous solvent, a lithium salt, a nitrate, and a first aryl derivative and a second aryl derivative, wherein the non-aqueous solvent comprises a heterocyclic compound containing one oxygen atom (O) or sulfur atom (S) in its ring structure, and a glycol ether, the first aryl derivative comprises at least one compound represented by any of the following chemical formulas 1 to 4, and the second aryl derivative comprises at least one compound represented by any of the following chemical formulas 5 to 8.

[0032] [Chemical formula 1] R 1 -Se-Li [Chemical formula 2] R 2 -Se-Se-R 3 [Chemical formula 3] R 4 -Se-S x -Li [Chemical formula 4] R 5 -Se-S x -Se-R 6 [Chemical formula 5] R 7 -Te-Li [Chemical formula 6] R 8 -Te-Te-R 9 [Chemical formula 7] R 10 -Te-S x -Li [Chemical formula 8] R 11 -Te-S x -Te-R 12 In the above chemical formulas 1 to 8, R 1 ~R 12 These are C6~C, each independently. 20 It is an aryl group, x is a number between 1 and 8.

[0033] In one embodiment of the present invention, the non-aqueous solvent is included as a medium in the electrolyte for a lithium-sulfur battery. The lithium salt is included as an electrolyte salt in the electrolyte for a lithium-sulfur battery. The nitrate is included as an additive to form a stable film on the negative electrode made of a material such as lithium metal and to improve charge-discharge efficiency. The aryl derivative is included as an additive to alter the reduction reaction pathway of lithium sulfide and provide additional discharge capacity.

[0034] In the present invention, by including the aryl derivative in the electrolyte for a lithium-sulfur battery, the aryl derivative can extend the chain length of lithium sulfide (Li2S) present in the positive electrode or electrolyte, thereby altering the lithium sulfide reduction reaction pathway.

[0035] According to the present invention, by including a first aryl derivative which is at least one compound represented by any of the chemical formulas 1 to 4, and a second aryl derivative which is at least one compound represented by any of the chemical formulas 5 to 8, the discharge capacity of the lithium sulfur battery is improved and a synergistic effect is achieved in terms of realizing a high nominal voltage.

[0036] Specifically, when the aryl derivative contains a compound represented by chemical formula 1 or chemical formula 5, the electrolyte for lithium sulfur batteries containing this contains -Se-R with respect to lithium sulfide. 1 The form or -Te-R 7 It can have the effect of extending the chain in this form.

[0037] Furthermore, if the aryl derivative contains a compound represented by chemical formula 2 or chemical formula 6, the Se-Se bond or Te-Te bond is decomposed, and as a result, in the electrolyte for lithium sulfur batteries containing this, the -Se-R bond is formed relative to lithium sulfide. 2 , -Se-R 3 ,-Te-R 8 , or -Te-R 9 It can have the effect of extending the chain in this form.

[0038] Furthermore, if the aryl derivative contains a compound represented by chemical formula 3 or chemical formula 7, the electrolyte for lithium sulfur batteries containing this contains -S relative to lithium sulfide. x -Se-R 4 or -S x -Te-R 10 It can have the effect of extending the chain in this form.

[0039] Furthermore, if the aryl derivative contains a compound represented by chemical formula 4 or chemical formula 8, -S is added to lithium sulfide. x -Se-R 5 , -S x -Se-R 6 , -S x -Te-R 11 , or -S x-Te-R 12 It can have the effect of extending the chain in this form.

[0040] In one embodiment of the present invention, the electrolyte for the lithium-sulfur battery may contain diphenyl diselenide (PDSe) as the first aryl derivative.

[0041] In one embodiment of the present invention, the electrolyte for the lithium-sulfur battery may contain diphenyl ditelluride (DPDTe) as a second aryl derivative.

[0042] According to one embodiment of the present invention, the electrolyte for the lithium-sulfur battery exhibits a more advantageous effect in improving battery performance when the first aryl derivative and the second aryl derivative are used in combination, compared to when the first aryl derivative or the second aryl derivative is used alone.

[0043] In particular, in one embodiment of the present invention, the weight ratio of the first aryl derivative to the second aryl derivative can be 3:2 to 2:3, 2:1 to 1:2, 2:1 to 1:1, or 1:1 to 1:2, and specifically can be 1:1. This allows for an even greater synergistic effect when the first aryl derivative and the second aryl derivative are used in combination.

[0044] In the present invention, the electrolyte for the lithium-sulfur battery contains a nitrate. Specifically, the nitrate refers collectively to nitrate-based compounds or nitrite-based compounds that can be used as additives in the electrolyte for the lithium-sulfur battery. The nitrate-based compounds or nitrite-based compounds can, for example, form a stable film on the negative electrode made of a material such as lithium metal, thereby improving the charge-discharge efficiency, but the mechanism of the present invention is not limited to this.

[0045] In one embodiment of the present invention, the nitrate is not limited to, but may include, for example, inorganic nitrates or nitrite compounds such as lithium nitrate (LiNO3), potassium nitrate (KNO3), cesium nitrate (CsNO3), barium nitrate (Ba(NO3)2), ammonium nitrate (NH4NO3), lithium nitrite (LiNO2), potassium nitrite (KNO2), cesium nitrite (CsNO2), and ammonium nitrite (NH4NO2); methyl nitrate, dialkylimidazolium nitrate, guanidine nitrate, imidazolium nitrate, pyridinium nitrate, and ethyl nitrite. Organic nitric or nitrite compounds such as nitrite, propyl nitrite, butyl nitrite, pentyl nitrite, octyl nitrite; organic nitro compounds such as nitromethane, nitropropane, nitrobutane, nitrobenzene, dinitrobenzene, nitropyridine, dinitropyridine, nitrotoluene, and dinitrotoluene; or mixtures of two or more of these.

[0046] In one embodiment of the present invention, the cation of the nitrate may be selected from alkali metals, such as lithium, sodium, potassium, rubidium, and cesium, but is not limited to these.

[0047] In another embodiment of the present invention, the nitrate may include lithium nitrate (LiNO3).

[0048] In one embodiment of the present invention, the sum of the weights of the nitrate and the aryl derivative may be 4% by weight or more, based on the total weight of the electrolyte for the lithium-sulfur battery. Specifically, the sum of the weights of the nitrate and the aryl derivative may be 5% by weight or more and 10% by weight or less, 5% by weight or more and 9% by weight or less, or 5% by weight or more and 7% by weight or less, based on the total weight of the electrolyte for the lithium-sulfur battery. When the sum of the weights of the nitrate and the aryl derivative is within the above range, advantageous effects can be obtained in terms of increasing discharge capacity and improving life characteristics during the operation of the lithium-sulfur battery using it, but the present invention is not limited thereto.

[0049] In other embodiments of the present invention, the weight of the aryl derivative may be the same as or less than the weight of the nitrate. Specifically, the weight of the aryl derivative may be less than the weight of the nitrate. When the weight ratio of the nitrate to the aryl derivative is within the above range, advantageous effects can be obtained in terms of increasing discharge capacity and improving life characteristics during the operation of a lithium sulfur battery using this, but the present invention is not limited thereto.

[0050] In yet another embodiment of the present invention, the sum of the total weights of the nitrate and the aryl derivative is 4% by weight or more, based on the total weight of the electrolyte for the lithium sulfur battery, the total weight of the aryl derivative is the same as or less than the weight of the nitrate, and the total molar ratio of the aryl derivative to the nitrate is 0.5:1 or less.

[0051] According to the present invention, the non-aqueous solvent includes a combination of a heterocyclic compound and a glycol ether.

[0052] The glycol ether is an acyclic ether containing two oxygen atoms and can be used without particular limitation as long as it is suitable for use as an electrolyte in a lithium-sulfur battery.

[0053] In one embodiment of the present invention, the glycol ether may be represented by the following chemical formula: R 13 -O-(CH2CH2O) x -R 14 (In the above chemical formula, R 13 and R 14 These are either identical or different from each other, and each is independently an unsubstituted or substituted alkyl group C1-C6, and C6-C 12 Unsubstituted or substituted aryl groups, or C7-C 13 (This is an unsubstituted or substituted arylalkyl group, where x is an integer between 0 and 4.)

[0054] The glycol ether may include, but is not limited to, dimethoxyethane, diethoxyethane, ethylene glycol ethyl methyl ether, diethylene glycol dimethyl ether, diethylene glycol diethyl ether, diethylene glycol methyl ethyl ether, triethylene glycol dimethyl ether, triethylene glycol diethyl ether, triethylene glycol methyl ethyl ether, tetraethylene glycol dimethyl ether, tetraethylene glycol diethyl ether, tetraethylene glycol methyl ethyl ether, polyethylene glycol dimethyl ether, polyethylene glycol diethyl ether, polyethylene glycol methyl ethyl ether, or two or more of these.

[0055] According to one embodiment of the present invention, the non-aqueous solvent may include dimethoxyethane as a glycol ether.

[0056] The heterocyclic compound is an ether containing one oxygen atom (O) or sulfur atom (S) in its ring structure and one -COC- or -CSC- structure in its ring structure, and can be used without particular limitation as long as it is suitable for use as an electrolyte in a lithium-sulfur battery.

[0057] In one embodiment of the present invention, the heterocyclic compound contains two or more double bonds and either an oxygen atom or a sulfur atom, thereby forming a solid electrolyte interface (SEI layer) on the surface of the negative electrode (lithium-based metal) through a ring-opening polymerization reaction of the heterocyclic compound during the initial discharge stage of the battery, thereby suppressing the formation of lithium dendrites. Furthermore, by reducing the decomposition of the electrolyte on the lithium-based metal surface and the associated side reactions, the lifespan characteristics of the lithium-sulfur battery can be improved. In addition, the delocalization of lone pair electrons of the heteroatom (oxygen atom or sulfur atom) gives it the property of being less soluble in salt, which can reduce the amount of polysulfide eluted into the electrolyte, but the present invention is not limited thereto.

[0058] In one embodiment of the present invention, the heterocyclic compound must contain two or more double bonds in order to form an SEI layer on the surface of the negative electrode (lithium-based metal), and must contain a heteroatom (oxygen atom or sulfur atom) in order to exhibit effects such as increasing affinity with other solvents in the electrolyte by making it polar.

[0059] In one embodiment of the present invention, the heterocyclic compound may be a heterocyclic compound having 4 to 15 members, more specifically 4 to 7 members, and more specifically 5 to 6 members. Furthermore, the heterocyclic compound may be a heterocyclic compound substituted or unsubstituted with one or more groups selected from the group consisting of C1-C4 alkyl groups, C3-C8 cyclic alkyl groups, C6-C10 aryl groups, halogen groups, nitro groups (-NO2), amino groups (-NH2), and sulfonyl groups (-SO2). In one embodiment of the present invention, when the heterocyclic compound is substituted as described above, radicals are stabilized, which can be advantageous in terms of suppressing side reactions between electrolytes; however, the present invention is not limited thereto.

[0060] The heterocyclic compound may include, but is not limited to, furan, 2-methylfuran, 3-methylfuran, 2-ethylfuran, 2-propylfuran, 2-butylfuran, 2,3-dimethylfuran, 2,4-dimethylfuran, 2,5-dimethylfuran, pyran, 2-methylpyran, 3-methylpyran, 4-methylpyran, benzofuran, 2-(2-nitrovinyl)furan, thiophene, 2-methylthiophene, 2-ethylthiophene, 2-propylthiophene, 2-butylthiophene, 2,3-dimethylthiophene, 2,4-dimethylthiophene, 2,5-dimethylthiophene, or two or more of these.

[0061] In one embodiment of the present invention, the non-aqueous solvent may include 2-methylfuran as a heterocyclic compound.

[0062] In one embodiment of the present invention, the glycol ether may be included in a volume percentage of, for example, 60% by weight or more, 65% by weight or more, 70% by weight or more, 75% by weight or more, 80% by weight or more, or 85% by weight or less, based on the total volume of the non-aqueous solvent. When the volume percentage of the glycol ether is within the above range, it can provide appropriate solubility to lithium salts, nitrates, aryl derivatives, and lithium polysulfide eluted from the positive electrode during battery operation, but the present invention is not limited thereto.

[0063] In one embodiment of the present invention, the heterocyclic compound may constitute, for example, a volume other than the glycol ether, based on the total volume of the non-aqueous solvent. For example, based on the total volume of the non-aqueous solvent, the heterocyclic compound may be included in a volume percentage of, for example, 15% by weight or more, 20% by weight or more, 40% by weight or less, 35% by weight or less, 30% by weight or less, or 25% by weight or less, but is not limited to these. When the volume percentage of the heterocyclic compound is within the above range, it can have the effect of imparting appropriate solubility to lithium salts, nitrates, aryl derivatives, and lithium polysulfide eluted from the positive electrode during battery operation, but the present invention is not limited thereto.

[0064] In other embodiments of the present invention, the ratio of the total volume of the glycol ether to the total volume of the heterocyclic compound may be 3:1 or greater. Specifically, the ratio of the total volume of the glycol ether to the total volume of the heterocyclic compound may be 3:1 to 5:1, 3:1 to 4:1, or 3.5:1 to 4:1. When the volume ratio of the heterocyclic compound to the glycol ether is within the above range, it may have an advantageous effect in terms of improving the operational stability of the battery, but the present invention is not limited thereto.

[0065] In one embodiment of the present invention, the non-aqueous solvent may further include an acyclic ether containing one oxygen atom, in addition to the heterocyclic compound and glycol ether described above. The further inclusion of an acyclic ether in the non-aqueous solvent may have advantageous effects in terms of improving overvoltage at a charge state (SOC) of 70% during battery operation, but the present invention is not limited thereto.

[0066] In one embodiment of the present invention, the acyclic ether containing one oxygen atom may be represented by the following chemical formula.

[0067] R 15 -OR 16 In the above chemical formula, R 15 and R 16 These are, independently, unsubstituted or substituted C1-C 20 It is an alkyl group.

[0068] In one embodiment of the present invention, the substituted C1 to C 20 The "substitution" in the alkyl group is, for example, a halogen atom, a hydroxyl group, a nitro group, a cyano group, an amino group, an amidino group, an acetamino group, a hydrazine, a hydrazone, a carboxyl group, a sulfonyl group, a sulfamoyl group, a sulfonic acid group, a phosphate group, a C1-C5 alkyl group, a C1-C5 alkoxy group, a C2-C5 alkenyl group, a C2-C5 alkynyl group, or a C4-C10 Cycloalkyl groups, C6~C 10 The aryl group, C6~C 10 heteroaryl group, C6~C 20 Aryl alkyl groups, C6~C 20 This may be due to heteroarylalkyl groups, or combinations thereof.

[0069] In another embodiment of the present invention, from the viewpoint of suppressing side reactions with polysulfide or lithium during battery operation, the R 15 and R 16 These are independent of each other, for example, the unsubstituted C1~C 20 It can be an alkyl group.

[0070] In yet another embodiment of the present invention, the R 15 and R 16These are, independently of each other, for example, methyl group, ethyl group, n-propyl group, n-butyl group, n-amyl group, n-hexyl group, n-heptyl group, n-octyl group, n-nonyl group, n-decyl group, n-undecyl group, n-dodecyl group, n-tridecyl group, n-tetradecyl group, n-pentadecyl group, n-hexadecyl group, n-heptadecyl group, n-octadecyl group, n-nonadecyl group, n-eicosanyl group, iso-propyl group, sec-butyl group, iso-butyl group, tert-butyl group, 1-methylbutyl group, 1-ethylpropyl group, 2-methylbutyl group, iso-amyl group, neopentyl group, 1,2-dimethylpropyl group, 1,1-dimethylpropyl group, tert-amyl group, 1,3-dimethylbutyl group, 3,3-dimethylbutyl group, 2-ethylbutyl group, 2-ethyl-2-methyl The group may be a propyl group, a linear or branched heptyl group, a 1-methylheptyl group, a 2-ethylhexyl group, a 1,5-dimethylhexyl group, a tert-octyl group, a branched nonyl group, a branched decyl group, a branched undecyl group, a branched dodecyl group, a branched tridecyl group, a branched tetradecyl group, a branched pentadecyl group, a branched hexadecyl group, a branched heptadecyl group, a branched octadecyl group, a linear or branched nonadecyl group, a linear or branched eicosanyl group, a cyclopropyl group, a cyclopropylmethyl group, a cyclobutyl group, a cyclobutylmethyl group, a cyclopentyl group, a cyclohexyl group, a cyclohexylmethyl group, a cycloheptyl group, a cyclooctyl group, a cyclohexylpropyl group, a cyclododecyl group, a norbornyl group, a bornyl group, a cyclopentylethyl group, or a bicyclooctyl group.

[0071] In other embodiments of the present invention, the present invention is not limited thereto, but for example, from the viewpoint of suppressing side reactions with polysulfide or lithium during battery operation, R 9 It may be preferable that the alkyl group is unsubstituted.

[0072] In one embodiment of the present invention, the acyclic ether may include, for example, bis(2,2,2-trifluoroethyl) ether, methyl propyl ether, ethyl propyl ether, dipropyl ether, methyl t-butyl ether, methyl hexyl ether, ethyl-t-butyl ether, ethyl hexyl ether, or two or more of these.

[0073] In one embodiment of the present invention, the aforementioned types of acyclic ethers can act as non-solvents for polysulfides eluting from the positive electrode, thereby exhibiting advantageous effects in suppressing the elution of polysulfides from the positive electrode.

[0074] In other embodiments of the present invention, the acyclic ether may be included, for example, in a content of 10% by volume or less based on the total volume of the non-aqueous solvent. Specifically, the content of the acyclic ether may be 1% by volume or more and 10% by volume or 5% by volume or more and 10% by volume or less based on the total volume of the non-aqueous solvent. When the content of the acyclic ether is within the above range, it may have an advantageous effect in terms of improving the operational stability of the battery, but the present invention is not limited thereto.

[0075] In another embodiment of the present invention, the acyclic ether is included in an amount of 10% by volume or less based on the total volume of the non-aqueous solvent, and the ratio of the total volume of the glycol ether to the total volume of the acyclic ether is not limited to this, but may be, for example, 6:1 or more, for example, 6:1 to 7.5:1, or 6.5:1 to 7:1.

[0076] In one embodiment of the present invention, if the content of the aforementioned solvent in the total volume of the non-aqueous solvent is within the above range, advantageous effects can be obtained in terms of suppressing the elution of polysulfide and improving the operational stability of the battery, but the present invention is not limited thereto.

[0077] The lithium salt may be used without limitation as long as it is a substance that can be ordinarily used in the electrolyte solution of a lithium-sulfur battery. Examples of the lithium salt include LiCl, LiBr, LiI, LiClO₄, LiBF₄, LiB 10 Cl 10 , LiPF₆, LiCF₃SO₃, LiCF₃CO₂, LiC₄BO₈, LiAsF₆, LiSbF₆, LiAlCl₄, CH₃SO₃Li, CF₃SO₃Li, (CF₃SO₂)₂NLi, (C₂F₅SO₂)₂NLi, (SO₂F)₂NLi, (CF₃SO₂)₃CLi, lithium chloroborane, lower aliphatic lithium carboxylate, lithium 4-phenylborate, lithium imide, or a mixture of two or more thereof, but the present invention is not limited thereto.

[0078] In one embodiment of the present invention, the lithium salt may not contain a lithium nitrate salt. The lithium nitrate salt may be included as an example of the nitrates described above.

[0079] In one embodiment of the present invention, the lithium salt may include an inorganic lithium salt. The inorganic lithium salt does not contain carbon (C) in its structure, and may be used without limitation as long as it is a substance that can be ordinarily used in the electrolyte solution of a lithium-sulfur battery. For example, the inorganic lithium salt may be LiCl, LiBr, LiI, LiClO₄, LiBF₄, LiB 10 Cl 10 , LiPF₆, LiAsF₆, LiSbF₆, LiAlCl₄, (SO₂F)₂NLi, lithium chloroborane, lithium imide, or a mixture of two or more thereof, and specifically may include (SO₂F)₂NLi (LiFSI), but the present invention is not limited thereto. When the lithium salt includes the inorganic lithium salt, it has a smaller structure than a conventional organic lithium salt and can be present at a higher density in the electrolyte solution, and thus can provide an advantageous effect in terms of ionic conductivity, and can further provide a more advantageous effect in terms of realizing a lithium-sulfur battery having a high electrolyte ratio (E / S), but the present invention is not limited thereto.

[0080] In one embodiment of the present invention, the lithium salt may include lithium bis(fluorosulfonyl)imide (LiFSI).

[0081] In one embodiment of the present invention, including lithium bis(fluorosulfonyl)imide (LiFSI) as the lithium salt may provide more advantageous effects in terms of performance such as the discharge capacity of the lithium-sulfur battery than including lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), but the effects of the present invention are not limited thereto.

[0082] According to one embodiment of the present invention, the lithium salt may further include an ordinary organic lithium salt in addition to an inorganic lithium salt. The organic lithium salts that may further include are lithium salts that contain carbon (C) in their structure, and such organic lithium salts can also be used without limitation as long as they are suitable for use in lithium-sulfur batteries. For example, the organic lithium salt may include, but is not limited to, LiCF3SO3, LiCF3CO2, LiC4BO8, CH3SO3Li, CF3SO3Li, (CF3SO2)2NLi, (C2F5SO2)2NLi, (CF3SO2)3Cli, lithium lower aliphatic carboxylate, lithium 4-phenylborate, or two or more of these.

[0083] In one embodiment of the present invention, the concentration of the lithium salt can be appropriately determined considering ionic conductivity, solubility, etc., and may be, for example, 0.1M to 4.0M, 0.3M to 3.0M, 0.5M to 2.0M, 0.5M to 1.5M, 0.5M to 1.0M, or 0.5M to 0.75M. When the concentration of the lithium salt is within the above range, it may have advantageous effects in terms of ionic conductivity and viscosity of the electrolyte, or it may have advantageous effects in terms of performance such as discharge capacity and / or nominal voltage of the lithium sulfur battery using it, but the present invention is not limited thereto.

[0084] In other embodiments of the present invention, the electrolyte for lithium-sulfur batteries may further contain other additives in addition to the composition described above, for the purpose of improving charge-discharge characteristics, flame retardancy, etc. Examples of such additives, as described in the present invention, include pyridine, triethyl phosphite, triethanolamine, ethylenediamine, n-glyme, hexaphosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ammonium salts, pyrrole, 2-methoxyethanol, aluminum trichloride, fluoroethylene carbonate (FEC), propene sultone (PRS), vinylene carbonate (VC), and the like.

[0085] The electrolyte for the lithium-sulfur battery according to one aspect of the present invention can be manufactured by conventional methods known to those skilled in the art, and is not particularly limited in the present invention.

[0086] A lithium-sulfur battery according to another aspect of the present invention includes the aforementioned electrolyte for lithium-sulfur batteries and comprises a positive electrode containing a positive electrode active material and a negative electrode containing a negative electrode active material. Specifically, the positive electrode active material includes a sulfur element, a sulfur compound, or a mixture thereof.

[0087] The positive electrode, positive electrode active material, negative electrode, and negative electrode active material can be used without particular limitation as long as they are suitable for use in a lithium-sulfur battery and do not hinder the objectives of the present invention.

[0088] For example, the positive electrode may include a positive electrode current collector and a positive electrode active material layer coated on one or both sides of the positive electrode current collector, and the negative electrode may include a negative electrode current collector and a negative electrode active material layer coated on one or both sides of the negative electrode current collector. In this case, the positive electrode current collector is not particularly limited as long as it supports the positive electrode active material and has high conductivity without inducing a chemical change in the battery, and the negative electrode current collector is not particularly limited as long as it supports the negative electrode active material and has high conductivity without inducing a chemical change in the battery.

[0089] In one embodiment of the present invention, the positive electrode active material comprises a sulfur element, a sulfur compound, or a mixture thereof. Specifically, the positive electrode active material comprises inorganic sulfur (S8), Li2S n (n≧1), disulfide compounds, organosulfur compounds, carbon-sulfur polymers ((C2S x ) n x = 2.5 to 50, n ≥ 2), or may include two or more of these.

[0090] In one embodiment of the present invention, the negative electrode active material is lithium (Li + Any material that can be reversibly intercalated or deintercalated, or that can react with lithium ions to reversibly form a lithium-containing compound, can be used without particular limitation. For example, the negative electrode active material may include lithium metal, lithium alloy, or a mixture thereof. The lithium alloy may be, for example, an alloy of lithium (Li) with sodium (Na), potassium (K), rubidium (Rb), cesium (Cs), francium (Fr), beryllium (Be), magnesium (Mg), calcium (Ca), strontium (Sr), barium (Ba), radium (Ra), aluminum (Al), tin (Sn), or two or more of these metals.

[0091] Furthermore, the positive electrode active material layer and the negative electrode active material layer may each further contain conductive materials, binders, additives, etc., in addition to the active material. Since specific types of these can be those commonly used by those skilled in the art, a detailed explanation is omitted.

[0092] In one embodiment of the present invention, the external shape of the lithium-sulfur battery may be, for example, coin-shaped, cylindrical, pouch-shaped, or rectangular, and the external shape of the battery is not particularly limited. Furthermore, the lithium-sulfur battery may be used not only as a battery cell used as a power source for small devices, but also as a unit battery in a medium-to-large battery module containing multiple battery cells, and its usage is not particularly limited.

[0093] In one embodiment of the present invention, a lithium-sulfur battery using a positive electrode containing the carbon composite is not only superior in terms of initial capacity and cycle stability, but can also achieve excellent effects in terms of the energy density of the battery. However, the effects of the present invention are not limited to this.

[0094] In one embodiment of the present invention, the lithium-sulfur battery can increase energy density and improve side reactions caused by polysulfides in the electrolyte by ensuring a sufficient amount of electrolyte.

[0095] In one embodiment of the present invention, the lithium-sulfur battery may have an electrolyte / sulfur (E / S) ratio, which indicates the weight ratio of sulfur, the positive electrode active material, to the electrolyte, of, for example, 2 g / g or more. Specifically, the electrolyte / sulfur (E / S) ratio may be 2.3 g / g or more. For example, the electrolyte / sulfur (E / S) ratio may be 2 g / g to 3 g / g, 2.1 g / g to 2.7 g / g, or 2.3 g / g to 2.5 g / g. Conventionally, when the E / S ratio is reduced in order to increase the energy density, there is a problem that the polysulfide concentration in the electrolyte increases and side reactions are induced. In contrast, the present invention has the effect of increasing the energy density of the battery and stabilizing the E / S ratio, so the E / S ratio of the lithium-sulfur battery may have a value even larger than the above range, and it is obvious to those skilled in the art that there is no upper limit, and the present invention is not limited thereto.

[0096] In other embodiments of the present invention, the lithium-sulfur battery may have an energy density of 400 Wh / kg to 500 Wh / kg. Specifically, the lithium-sulfur battery may have an energy density of 430 Wh / kg or more, 450 Wh / kg or more, or 460 Wh / kg or more, but the present invention is not limited thereto.

[0097] In one embodiment of the present invention, the lithium-sulfur battery may exhibit a specific capacity of 1,400 mAh / gs or more. Specifically, when discharged at a rate of 0.1 C, the specific capacity may exhibit 1,400 mAh / gs or more.

[0098] The present invention will be described in more detail below based on examples, but these examples are for illustrative purposes only and the scope of the present invention is not limited to them.

[0099] First, we manufactured lithium-sulfur batteries in pouch cell form using the following method, and evaluated the performance of the manufactured batteries.

[0100] [Battery manufacturing] Example 1 Preparation of electrolyte for lithium-sulfur batteries An electrolyte was prepared by adding 0.5 M lithium bis(fluorosulfonyl)imide (LiFSI), 5.0 wt% lithium nitrate (LiNO3, molar mass 69 g / mol), 1.5 wt% diphenyl diselenide (PDSe, molar mass 312 g / mol), and 1.5 wt% diphenyl diterlide (DPDTe, molar mass 409 g / mol) to a mixture of dimethoxyethane (DME) and 2-methylfuran (2-MeF) (v / v=4:1) as a non-aqueous solvent, and stirring for 12 hours.

[0101] Electrode preparation A cathode slurry was prepared by mixing a sulfur-carbon composite (S:C=70:30 (weight ratio)) as the cathode active material and polyacrylic acid (PAA) as the binder in a weight ratio of 97:3 using distilled water as the solvent.

[0102] The prepared positive electrode slurry composition was applied to both sides of a 12 μm thick aluminum current collector, dried at 80°C, and then rolled using a roll press to produce the positive electrode. At this time, the loading amount of the positive electrode active material was 3.45 mAh / cm². 2 That was the case.

[0103] A 30 μm thick layer of lithium metal was prepared as the negative electrode.

[0104] Manufacturing of lithium-sulfur batteries The manufactured positive and negative electrodes were placed facing each other, and a polyethylene separator with a thickness of 16 μm and a porosity of 68% was placed between them for stacking. After stacking, a pouch cell was assembled, and 1 g of the electrolyte prepared above was injected and sealed so that the electrolyte / sulfur loading amount ratio was 2.15 g / g, thereby manufacturing a pouch-type lithium sulfur battery.

[0105] Example 2 A lithium sulfur battery was manufactured using the same method as in Example 1, except that the amount of diphenyl diselenide (PDSe) was changed to 0.5% by weight and the amount of diphenyl diterlide (DPDTe) was changed to 2.5% by weight.

[0106] Comparative Example 1 A lithium-sulfur battery was manufactured using the same method as in Example 1, except that diphenyl diselenide (PDSe) and diphenyl diterlide (DPDTe) were not added.

[0107] Comparative Example 2 A lithium-sulfur battery was manufactured using the same method as in Example 1, except that diphenyl diterlide (DPDTe) was not added, and 3% by weight of diphenyl diselenide (PDSe) was added.

[0108] Comparative Example 3 A lithium-sulfur battery was manufactured using the same method as in Example 1, except that diphenyl diselenide (PDSe) was not added, and 3% by weight of diphenyl diterlide (DPDTe) was added.

[0109] Comparative Example 4 A lithium sulfur battery was manufactured using the same method as in Example 1, except that the non-aqueous solvent was changed to a mixture of dioxolane (DOL) and dimethoxyethane (DME) (v / v=1:1).

[0110] Comparative Example 5 A lithium-sulfur battery was manufactured in the same manner as in Example 1, except that the non-aqueous solvent was changed to a mixture of dioxolane (DOL) and dimethoxyethane (DME) (v / v=1:1), and the lithium salt was changed to 1.0 M lithium bis(trifluoromethanesulfonyl)imide (LiTFSI).

[0111] [Battery performance evaluation and results] The battery performance was evaluated using the following method, and the results are shown in Table 1 below.

[0112] The manufactured batteries were subjected to three cycles of 0.1C charging / 0.1C discharging (with a maximum voltage of 2.5V and a minimum voltage of 1.8V) under a temperature of 30°C. The initial discharge capacity was measured to evaluate the specific capacity, and the nominal voltage was also measured.

[0113] [Table 1]

[0114] As is clear from the results in Table 1, it was confirmed that high discharge capacity and nominal voltage can be simultaneously achieved by using a first aryl derivative and a second aryl derivative in combination as aryl derivatives in the electrolyte for lithium-sulfur batteries. In particular, it was confirmed that the discharge capacity increased compared to when only the first aryl derivative was used alone, and that the problem of the decrease in nominal voltage that occurred when only the second aryl derivative was used alone was resolved.

[0115] Furthermore, regarding the ratio of the first aryl derivative to the second aryl derivative, it was confirmed that when the second aryl derivative was used in a ratio greater than 1:1, the discharge capacity could increase, but the nominal voltage dropped to below 2.145V. In addition, it was confirmed that when the non-aqueous solvent did not contain a heterocyclic compound, the discharge capacity decreased significantly.

Claims

1. It comprises a non-aqueous solvent, a lithium salt, a nitrate, a first aryl derivative, and a second aryl derivative. The non-aqueous solvent comprises a heterocyclic compound containing one oxygen atom (O) or sulfur atom (S) in its ring structure, and a glycol ether. The first aryl derivative comprises at least one compound represented by any of the following chemical formulas 1 to 4: The second aryl derivative is an electrolyte for a lithium-sulfur battery comprising at least one compound represented by any of the following chemical formulas 5 to 8: [Chemical formula 1] R 1 -S%-L) [Chemical formula 2] R 2 -Se� 3 [Chemical formula 3] R 4 -S%-S x -L+ [Chemical formula 4] R 5 -S%-S x -S%-R 6 [Chemical formula 5] R 7 -T%-L [Chemical formula 6] R 8 -Te� 9 [Chemical formula 7] R 10 -T%-S x -L+ [Chemical formula 8] R 11 -T%-S x -T%-R 12 In the aforementioned chemical formulas 1 to 8, R 1 ~R 12 Each of them is independent of C 6 ~C 20 It is an aryl group, x is a number between 1 and 8.

2. The electrolyte for a lithium-sulfur battery according to claim 1, wherein the first aryl derivative comprises diphenyl diselenide (PDSe).

3. The electrolyte for a lithium sulfur battery according to claim 1, wherein the second aryl derivative comprises diphenyl diterlide (DPDTe).

4. The electrolyte for a lithium sulfur battery according to claim 1, wherein the weight ratio of the first aryl derivative to the second aryl derivative is 3:2 to 2:

3.

5. The electrolyte for a lithium sulfur battery according to claim 1, wherein the weight ratio of the first aryl derivative to the second aryl derivative is 1:

1.

6. The electrolyte for a lithium-sulfur battery according to claim 1, wherein the sum of the weights of the first aryl derivative and the second aryl derivative is equal to or less than the weight of the nitrate.

7. The electrolyte for a lithium sulfur battery according to claim 1, wherein the sum of the weights of the first aryl derivative and the second aryl derivative is 3% by weight or more based on the total weight of the electrolyte.

8. The electrolyte for a lithium sulfur battery according to claim 1, wherein the volume ratio of the heterocyclic compound to the glycol ether is 1:3 to 1:

10.

9. An electrolyte for a lithium sulfur battery according to any one of claims 1 to 8, A positive electrode containing a positive electrode active material, A negative electrode containing a negative electrode active material, Includes, The positive electrode active material comprises a sulfur element, a sulfur compound, or a mixture thereof, in a lithium-sulfur battery.

10. The lithium sulfur battery according to claim 9, wherein the specific capacity at 0.1C discharge is 1400 mAh / gs or more.