Polyimide film for flexible metal clad laminates and method for manufacturing the same
The polyimide film with a diamine coating layer and surface modifications addresses the bonding issues by enhancing adhesion, achieving superior adhesive strength and heat-resistant properties.
Patent Information
- Application Number
- JP2026524606
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-15
- Filing Date
- 2024-11-14
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional polyimide films face challenges in achieving sufficient adhesive strength with metal layers due to the uneven distribution and limited interaction of coupling agents within the film, leading to inadequate bonding between the polyimide film and metal layers, especially with the reduction in microcircuit pitch.
A polyimide film comprising a polyimide layer and a diamine coating layer formed on one or both sides, where the polyimide layer is derived from a polyamic acid solution, and a diamine compound is applied to enhance adhesion, with specific concentrations and surface modifications like corona treatment to activate -OH groups.
The polyimide film exhibits significantly improved adhesive strength to adhesive sheets and metal layers, with enhanced room temperature and heat-resistant adhesion, surpassing conventional films.
Smart Images

Figure 2026539047000001 
Figure 2026539047000002 
Figure 2026539047000003
Abstract
Description
Technical Field
[0001] The present invention relates to a polyimide film for flexible metal-clad laminates and a method for producing the same, and more specifically, relates to a polyimide film comprising a polyimide layer and a diamine coating layer formed on one or both sides of the polyimide layer, and a method for producing the same.
Background Art
[0002] Polyimide (PI) is a polymer material that has the highest heat resistance, chemical resistance, electrical insulation, and weather resistance among organic materials, based on an imide ring with a strong aromatic main chain and excellent chemical stability. Therefore, polyimide is widely used as an insulating material for microelectronic components that strongly require the aforementioned properties.
[0003] Examples of microelectronic components include highly integrated and flexible thin circuit boards that support the weight reduction of electronic products, and the polyimide is widely used as an insulating film for thin circuit boards.
[0004] The thin circuit board generally has a structure in which a circuit including a metal foil is formed on an insulating film. Such a thin circuit board is broadly referred to as a flexible metal-clad laminate, and when a thin copper plate is used as the metal foil, it is also referred to in the narrow sense as a flexible copper-clad laminate (FCCL).
[0005] Examples of methods for producing such a flexible metal-clad laminate include (i) a casting method in which polyamic acid, which is a precursor of polyimide, is cast or applied onto a metal foil and then imidized, (ii) a metallization method in which a metal layer is formed directly on a polyimide film by sputtering, and (iii) a lamination method in which a polyimide film and a metal foil are bonded by heat and pressure using an adhesive film.
[0006] Among these methods, the lamination method has the advantage of a wider range of applicable metal foil thicknesses than the casting method and lower equipment costs than the metallization method. Lamination equipment includes roll laminating machines that continuously laminate while supplying roll-shaped material, and double belt press machines. Of these, from the viewpoint of productivity, the hot roll lamination method using a hot roll laminating machine is more preferably used.
[0007] In recent years, the pitch between microcircuits and their respective line widths have been further reduced, resulting in a decrease in the bonding area between the polyimide film and the metal layer. Therefore, a stronger adhesive force is required between the polyimide film and the metal layer.
[0008] Conventionally, coupling agents that can chemically and / or physically bond the surface of a polyimide film to the surface of a metal layer have been used to improve the adhesion between the surface of a polyimide film and the surface of a metal layer. In this case, chemical bonding generally refers to an interaction in which a portion of the coupling agent forms hydrogen bonds with a portion of the polymer chains of the polyimide film, and another portion forms hydrogen bonds with oxygen or other elements present on the surface of the metal layer.
[0009] On the other hand, by depositing a metal layer such as copper through sputtering, the surface energy of the polyimide film could be increased, thereby improving the adhesive strength.
[0010] On the other hand, polyimide films can be produced from their precursor, a polyamic acid solution. Specifically, a polyimide film can be produced by an "imidization" process, in which a polyamic acid solution is coated onto a support in a thin film, and then the amic acid groups in the polyamic acid are converted to imide groups by ring-closing and dehydration reactions using heat and / or chemical catalysts.
[0011] Here, the coupling agent and metal powder may physically and / or chemically bond to a portion of the polyimide polymer chain during the imidation process. For this reason, the coupling agent and metal powder are used as a liquid mixture in a polyamic acid solution.
[0012] However, as mentioned above, the coupling agent mixed in the polyamic acid solution is dispersed throughout the solution and can maintain its dispersed state until the imidization of the polyamic acid solution is complete. Therefore, in the manufactured polyimide film, the majority of the coupling agent is located inside the film where it is difficult to interact with the metal layer, and is present in relatively small amounts, or in some cases not at all, on the film surface and surrounding areas where it can interact with the metal layer.
[0013] Furthermore, in the case of conventional polyimide films containing coupling agents and metal powders, there may be a significant deficiency in the amount of coupling agent and / or metal powder that can interact with the surface of the metal layer. As a result, there is a problem in that it is difficult to achieve the desired level of adhesion strength with the metal layer.
[0014] Therefore, there is a need for polyimide films with improved adhesive strength by improving the interaction between the polyimide film and the surface of metal particles or metal layers. [Overview of the Initiative] [Problems that the invention aims to solve]
[0015] The object of the present invention is to provide a polyimide film comprising a polyimide layer and a diamine coating layer formed on one or both sides of the polyimide layer, and a method for producing the same. [Means for solving the problem]
[0016] To achieve the aforementioned technical objectives, according to one aspect of the present invention, a polyimide film is provided comprising a polyimide layer derived from a polyamic acid solution and a diamine coating layer containing a diamine compound formed on one or both sides of the polyimide layer, wherein the polyimide film has an adhesive strength to an adhesive sheet of 1,400 gf / cm or more.
[0017] According to another aspect of the present invention, a method for producing a polyimide film is provided, comprising the steps of: a step of producing a polyimide layer by applying a polyamic acid solution onto a substrate and heat-treating it; and a step of forming a diamine coating layer by applying a diamine compound solution, obtained by dissolving a diamine compound in an organic solvent, to one or both sides of the polyimide layer and heat-treating it, wherein the concentration of the diamine compound in the diamine compound solution is 0.01 to 10% by weight.
[0018] According to yet another aspect of the present invention, an electronic component comprising the polyimide film of the present invention is provided. [Effects of the Invention]
[0019] The polyimide film according to the present invention comprises a polyimide layer and a diamine coating layer formed on one or both sides of the polyimide layer, thereby exhibiting higher room temperature and heat-resistant adhesion to adhesive sheets and metal layers than conventional films. [Modes for carrying out the invention]
[0020] Embodiments and examples of the present invention will be described in detail below so that those skilled in the art can easily implement the invention. However, the present invention can be implemented in a variety of different forms and is not limited to the embodiments and examples described herein. Throughout this specification, where a part is described as "including" a particular component, unless otherwise specified, this does not exclude other components, but rather means that other components may be included.
[0021] The singular forms used in this specification shall include the plural forms as well unless the context clearly dictates otherwise.
[0022] A component, even if not explicitly stated, shall be construed to include the ordinary range of error.
[0023] In this specification, the expression "a to b" used to denote a specific numerical range means "≥a and ≤b".
[0024] A polyimide film according to one aspect of the present invention includes a polyimide layer derived from a polyamic acid solution, and a diamine coating layer containing a diamine compound formed on one or both sides of the polyimide layer, wherein the polyimide film has an adhesive strength to an adhesive sheet of 1,400 gf / cm or more.
[0025] The polyimide layer included in the polyimide film of the present invention can be produced by imidizing a polyamic acid solution containing a polyamic acid formed by the reaction of a dianhydride monomer and a diamine monomer, and may include the dianhydride monomer and the diamine monomer as polymerization units. The weight average molecular weight of the polyamic acid may be 100,000 to 500,000. For example, it may be 150,000 to 500,000, as another example 100,000 to 400,000, and as a further example 250,000 to 400,000, but is not limited thereto.
[0026] The polyamic acid solution used in the polyimide film of the present invention contains polyamic acid formed by the reaction of a dianhydride monomer and a diamine monomer, and the dianhydride monomer and the diamine monomer may be various monomers that have been conventionally used in the field of polyimide film production. For example, the dianhydride monomer may be an aromatic dianhydride monomer, and the diamine monomer may be an aromatic diamine monomer. The dianhydride monomers include pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 2,3,3',4'-biphenyltetracarboxylic acid dianhydride, oxydiphthalic acid dianhydride, diphenylsulfone-3,4,3',4'-tetracarboxylic acid dianhydride, bis(3,4-dicarboxyphenyl) sulfide dianhydride, 2,2-bis(3,4-dicarboxyphenyl)-1,1,1,3,3,3-hexafluoropropane dianhydride, 2,3,3',4'-benzophenonetetracarboxylic acid dianhydride, 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride, bis(3,4-dicarboxyphenyl)methane dianhydride, 2,2-bis(3,4-dicarboxyphenyl)propane dianhydride, and p-phenylenebis(trimellitic acid monoester anhydride). This includes, but is not limited to, p-biphenylenebis(trimellitic acid monoester anhydride), m-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, p-terphenyl-3,4,3',4'-tetracarboxylic acid dianhydride, 1,3-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)benzene dianhydride, 1,4-bis(3,4-dicarboxyphenoxy)biphenyl dianhydride, 2,2-bis[(3,4-dicarboxyphenoxy)phenyl]propane dianhydride, 2,3,6,7-naphthalenetetracarboxylic acid dianhydride, 1,4,5,8-naphthalenetetracarboxylic acid dianhydride, 4,4'-(2,2-hexafluoroisopropylidene)diphthalic acid dianhydride, or combinations thereof. Diamine monomers include diamine monomers containing one benzene ring (e.g., 1,4-diaminobenzene, 1,3-diaminobenzene, 2,4-diaminotoluene, 2,6-diaminotoluene, 3,Diamine monomers containing two benzene rings (e.g., 5-diaminobenzoic acid), such as 4,4'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, and other diaminodiphenyl ethers, 4,4'-diaminodiphenylmethane, 3,3'-dimethyl-4,4'-diaminobiphenyl, 2,2'-dimethyl-4,4'-diaminobiphenyl, 2,2'-bis(trifluoromethyl)-4,4'-diaminobiphenyl, 3,3'-dimethyl-4,4'-diaminodiphenylmethane, 3,3'-dicarboxy-4,4'-diaminodiphenylmethane Tan, 3,3',5,5'-tetramethyl-4,4'-diaminodiphenylmethane, bis(4-aminophenyl) sulfide, 4,4'-diaminobenzanilide, 3,3'-dimethylbenzidine, 2,2'-dimethylbenzidine, 3,3'-dimethoxybenzidine, 2,2'-dimethoxybenzidine, 3,3'-diaminodiphenyl ether, 3,4'-diaminodiphenyl ether, 4,4'-diaminodiphenyl ether, 3,3'-diaminodiphenyl sulfide, 3,4'-diaminodiphenyl sulfide, 4,4'-diaminodiphenyl Phenyl sulfide, 3,3'-diaminodiphenyl sulfone, 3,4'-diaminodiphenyl sulfone, 4,4'-diaminodiphenyl sulfone, 3,3'-diaminobenzophenone, 4,4'-diaminobenzophenone, 3,3'-diamino-4,4'-dichlorobenzophenone, 3,3'-diamino-4,4'-dimethoxybenzophenone, 3,3'-diaminodiphenylmethane, 3,4'-diaminodiphenylmethane, 4,4'-diaminodiphenylmethane, 2,2-bis(3-aminophenyl)propane, 2,2-bis(4-aminophenyl (e.g., propane, 2,2-bis(3-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 2,2-bis(4-aminophenyl)-1,1,1,3,3,3-hexafluoropropane, 3,3'-diaminodiphenyl sulfoxide, 3,4'-diaminodiphenyl sulfoxide, 4,4'-diaminodiphenyl sulfoxide, etc.), diamine monomers containing three benzene rings (e.g., 1,3-bis(3-aminophenyl)benzene, 1,3-bis(4-aminophenyl)benzene, 1,4-bis(3-aminophenyl)benzene, 1,4-bis(4-aminophenyl)benzene, 1,3-bis(4-aminophenoxy)benzene, 1,4-bis(3-aminophenoxy)benzene, 1,3-bis(3-aminophenoxy)-4-trifluoromethylbenzene, 3,3'-diamino-4-(4-phenyl)phenoxybenzophenone, 3,3'-diamino-4,4'-di(4-phenylphenoxy)benzophenone, 1,3-bis(3-aminophenyl sulfide)benzene, 1,3-bis(4-aminophenyl sulfide)benzene, 1,4-bis(4-aminophenyl sulfide)benzene, 1,3-bis(3-A (Minophenylsulfone)benzene, 1,3-bis(4-aminophenylsulfone)benzene, 1,4-bis(4-aminophenylsulfone)benzene, 1,3-bis[2-(4-aminophenyl)isopropyl]benzene, 1,4-bis[2-(3-aminophenyl)isopropyl]benzene, 1,4-bis[2-(4-aminophenyl)isopropyl]benzene, etc.), diamine monomers containing four benzene rings (e.g., 3,3'-bis(3-aminophenoxy)biphenyl, 3,3'-bis(4-aminophenoxy)biphenyl, 4,4'-bis(3-aminophenoxy)biphenyl, 4,4,4'-bis(4-aminophenoxy)biphenyl, bis[3-(3-aminophenoxy)phenyl] ether, bis[3-(4-aminophenoxy)phenyl] ether, bis[4-(3-aminophenoxy)phenyl] ether, bis[4-(4-aminophenoxy)phenyl] ether, bis[3-(3-aminophenoxy)phenyl] ketone, bis[3-(4-aminophenoxy)phenyl] ketone, bis[4-(3-aminophenoxy)phenyl] ketone, bis[4-(4-aminophenoxy)phenyl] ketone, bis[3-(3-aminophenoxy)phenyl] sulfide, bis[3-(4-aminophenoxy)phenyl] sulfide, bis[4-(3-aminophenoxy)phenyl] sulfide, bis[4-(4-aminophenoxy)phenyl] sulfide, bis[3-(3-aminophenoxy)phenyl] sulfone, bis[3-(4-aminophenoxy)phenyl] sulfone, bis[4-(3-aminophenoxy)phenyl] sulfone, bis[4-(4-aminophenoxy)phenyl] sulfone, bis[3-(3-aminophenoxy)phenyl] methane, bis[3-(4-aminophenoxy)phenyl] methane, bis[4-(3-aminophenoxy)phenyl] methane, bis[4-(4-aminophenoxy)phenyl] methane, 2,2-bis[3-(3-aminophenoxy)phenyl] propane, 2,2-bis[3-(4-aminophenoxy)phenyl] propane, 2,2-bis[4-(3-aminophenoxy)phenyl] propane, 2,2-bis[4-(4-aminophenoxy)phenyl] propane, 2,2-bis[3-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[3-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(3-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, 2,2-bis[4-(4-aminophenoxy)phenyl]-1,1,1,3,3,3-hexafluoropropane, and the like), or a combination thereof, but is not limited to these.
[0027] In particular, as the dianhydride monomer, one or more selected from the group consisting of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 2,3,3',4-biphenyltetracarboxylic acid dianhydride, oxydiphthalic acid anhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, and 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride can be used, and as the diamine monomer, one or more selected from the group consisting of 4,4'-oxydianiline, 3,4'-oxydianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-methylenedianiline, 3,3'-methylenedianiline, and 4,4'-diamino-2,2'-dimethylbiphenyl can be used.
[0028] The solvents contained in the polyamic acid solution of the present invention may be sulfoxide-based solvents such as dimethyl sulfoxide and diethyl sulfoxide; formamide-based solvents such as N,N-dimethylformamide and N,N-diethylformamide; acetamide-based solvents such as N,N-dimethylacetamide and N,N-diethylacetamide; pyrrolidone-based solvents such as N-methyl-2-pyrrolidone and N-vinyl-2-pyrrolidone; phenol-based solvents such as phenol, o-, m-, or p-cresol, xilenol, halogenated phenol, and catechol; aprotic polar solvents such as hexamethylphosphoramide and γ-butylol lactone; and quinoline, either alone or in combination of two or more, but are not limited to these.
[0029] The polyamic acid solution used in the production of the polyamide layer may contain an imidation catalyst and, without being particularly limited, may also contain other catalysts necessary for the production of polyimide films, such as dehydrating agents.
[0030] The aforementioned imidation catalyst promotes the cyclization reaction of polyamic acids, and examples include aliphatic tertiary amines, aromatic tertiary amines, and heterocyclic tertiary amines. Among these, heterocyclic tertiary amines can be used from the viewpoint of catalytic reactivity.
[0031] Examples of heterocyclic tertiary amines include quinoline, isoquinoline, β-picoline, and pyridine, which can be used individually or in combination of two or more.
[0032] Furthermore, one or both sides of the polyimide layer of the present invention may be surface-modified by corona treatment or plasma treatment. Such surface modification activates the -OH groups on the surface of the polyimide layer, thereby increasing the adhesive strength.
[0033] Corona treatment uses 150-400 W / m². 2 This can be carried out under conditions of / min, and if the surface activity of the film composition is sufficient, a higher treatment dose can be applied.
[0034] The polyimide film of the present invention may include a diamine coating layer containing a diamine compound formed on one or both sides of the polyimide layer.
[0035] The diamine compound contained in the diamine coating layer may be one or more selected from the group consisting of 4,4'-oxydianiline (ODA), 3,4'-oxydianiline (ODA), p-phenylenediamine, m-phenylenediamine, 4,4'-methylenedianiline, 3,3'-methylenedianiline, and 4,4'-diamino-2,2'-dimethylbiphenyl.
[0036] The polyimide film may have an adhesive strength with the adhesive sheet of 1,400 gf / cm or more, 1,420 gf / cm or more, 1,450 gf / cm or more, 1,500 gf / cm or more, 1,550 gf / cm or more, or 1,590 gf / cm or more, and may be 1,800 gf / cm or less, 1,750 gf / cm or less, 1,700 gf / cm or less, 1,650 gf / cm or less, or 1,600 gf / cm or less, for example, 1,400 to 1,800 gf / cm, 1,420 to 1,700 gf / cm, or 1,450 gf / cm to 1,600 gf / cm.
[0037] The adhesive sheet may include, but is not limited to, epoxy-based or fluorine-based compounds.
[0038] The contact angle of the polyimide film may be 110° or less, 100° or less, 98° or less, 85° or less, 75° or less, 35° or more, 45° or more, 50° or more, 55° or more, or 60° or more, for example, 45° to 98° or 50° to 75°.
[0039] Furthermore, the polyimide film of the present invention may have an improvement rate of 10% or more, 15% or more, 25% or more, or 30% or more in heat-resistant plating adhesion compared to a conventional polyimide film without a diamine coating layer, and may also have an improvement rate of 60% or less, 55% or less, or 50% or less.
[0040] According to another aspect of the present invention, a method for producing a polyimide film is provided, comprising the steps of: a step of producing a polyimide layer by applying a polyamic acid solution onto a substrate and heat-treating it; and a step of forming a diamine coating layer by applying a diamine compound solution, obtained by dissolving a diamine compound in an organic solvent, to one or both sides of the polyimide layer and heat-treating it, wherein the concentration of the diamine compound in the diamine compound solution is 0.01 to 10% by weight.
[0041] In the manufacturing process of the polyimide layer, a polyamic acid solution can be produced by polymerizing one or more dianhydride monomers and one or more diamine monomers in a solvent, and a dehydrating agent, an imidation catalyst, etc., can be mixed into the polyamic acid solution. The components contained in the polyamic acid solution are as described above.
[0042] The imidation process of the polyamic acid solution can be carried out using known imidation methods, such as thermal imidation, chemical imidation, or a combined imidation method that combines thermal imidation and chemical imidation.
[0043] In the manufacturing process of the polyimide layer, the polyamic acid solution of the present invention may be applied in a film-like manner to a substrate, and a gel film may be produced by heating and drying at a temperature of 30 to 200°C for 15 seconds to 30 minutes. After removing the substrate, the gel film may be heat-treated at a temperature of 250 to 600°C for 15 seconds to 30 minutes, but is not limited to this.
[0044] The manufacturing method of the present invention may further include a surface modification step after the manufacturing step of the polyimide layer, in which one or both sides of the polyimide layer are subjected to corona treatment or plasma treatment. Such surface modification can activate the -OH groups on the surface of the polyimide layer and increase the adhesive strength.
[0045] Corona treatment uses 150-400 W / m². 2 This can be carried out under conditions of / min, and if the surface activity of the film composition is insufficient, a higher treatment dose can be applied.
[0046] In the step of forming the diamine coating layer, a diamine compound solution, in which the diamine compound is dissolved in an organic solvent, can be applied to one or both sides of the surface-modified polyimide layer and then heat-treated.
[0047] The concentration of the diamine compound in the diamine compound solution may be 0.01% by weight or more, 0.02% by weight or more, 0.03% by weight or more, 0.05% by weight or more, or 0.08% by weight or more, and may also be 10% by weight or less, 8% by weight or less, 5% by weight or less, 3% by weight or less, 1% by weight or less, 0.8% by weight or less, 0.6% by weight or less, 0.5% by weight or less, 0.3% by weight or less, or 0.2% by weight or less, for example, 0.01 to 10% by weight, 0.02 to 5% by weight, 0.05 to 1% by weight, or 0.08 to 0.3% by weight. If the concentration of the diamine compound is lower than the above range, the adhesive strength with the adhesive sheet may decrease, and if the concentration of the diamine compound is higher than the above range, the coating properties (appearance of the coating film) may deteriorate.
[0048] As described above, the diamine compounds are as described, and the solvent for the diamine compound solution can be selected from acetone, dimethylformamide, or a mixture thereof.
[0049] The diamine coating layer formation process can be carried out at a temperature of 150-300°C, for example, 160-290°C, 170-250°C, or 180-220°C, for 1-10 minutes, for example, 1-8 minutes, 1-5 minutes, or 1-3 minutes.
[0050] In one embodiment, the diamine coating layer formation step can be carried out by coating the surface of the modified polyimide layer with a diamine compound solution using a bar coater, but the coating method is not limited thereto.
[0051] According to another aspect of the present invention, an electronic component comprising the polyimide film of the present invention is provided. In one embodiment, the polyimide film may be included as an insulating film.
[0052] The electronic component may be a semiconductor device or a flexible circuit board. The flexible circuit board may also include a polyimide film and layers formed on one or both sides of the polyimide film, such as an adhesive sheet, a metal layer, or a combination thereof.
[0053] The adhesive sheet may, but is not limited to, epoxy and / or fluorine-based compounds.
[0054] The aforementioned metal layer may be, but is not limited to, copper deposited by sputtering.
[0055] The present invention will be described in more detail through the following examples and comparative examples. However, the scope of the present invention is not limited thereto. [Examples]
[0056] 1. Manufacturing Example 1 (Manufacturing of Surface-Modified Polyimide Layer) 164.0 g of dimethylformamide and 41.0 g of quinoline were added to the reactor as solvents, and the temperature was adjusted to 20°C. 21.5 g of 4,4'-oxydianiline (ODA) was added as the diamine monomer, followed by 23.4 g of pyromellitic dianhydride (PMDA) as the dianhydride monomer to prepare a polyamic acid solution. Furthermore, polyamic acid solutions were prepared by adding 0.45 moles, 2.34 moles, and 2.83 moles of a catalyst component containing β-picoline (BP) as an imidizing agent, acetic anhydride (AA) as a dehydrating agent, and dimethylformamide (DMF) as a catalyst solvent to 1 mole of amic acid groups in the polyamic acid. The manufactured polyamic acid solution was cast to a thickness of 500 μm onto a SUS plate (100SA, manufactured by Sandvik) using a doctor blade, and dried in a temperature range of 100°C to 200°C to produce a self-standing gel film. Next, the gel film was peeled off with a SUS plate, fixed to a pin frame, and transferred to a high-temperature tenter. The film was heated in the high-temperature tenter from 200°C to 700°C, cooled to 25°C, and then separated from the pin frame to obtain a polyimide layer. On one side of the polyimide layer, 250 W / m 2 Surface modification was performed by activating the -OH groups on the surface through corona (air plasma) treatment under conditions of / min.
[0057] 2. Manufacturing Example 2 (Formation of Diamine Coating Layer) As shown in Table 1 below, a diamine compound solution was prepared by dissolving oxydianiline (ODA) as a diamine compound in acetone and DMF, which are organic solvents. This diamine compound solution was applied to one side of the surface-modified polyimide layer formed in Production Example 1, and the layer was heat-treated in a hot air oven at 200°C for 2 minutes to form a diamine coating layer. The results of the evaluation of the coating properties (appearance) are shown in Table 1.
[0058] [Table 1]
[0059] As can be seen from Table 1 above, when ethanol was used as the organic solvent, ODA did not dissolve. Furthermore, when acetone and DMF were used as the organic solvent, good coating properties were observed at an ODA concentration of 0.1% by weight, but it was confirmed that poor appearance occurred at an ODA concentration of 1% by weight.
[0060] 3. Example 1 (Comparison of adhesive strength of polyimide films) Surface-modified polyimide layer of manufacturing example 1 (Comparative Example 1-1), Polyimide films (Comparative Examples 1-2) were prepared by forming a diamine coating layer on a polyimide layer produced in the same manner as in Production Example 1, except for surface modification, using a 0.1% by weight acetone-ODA diamine compound solution. A polyimide film (Example 1) in which a diamine coating layer was formed on the surface-modified polyimide layer of Production Example 1 using a 0.1% by weight diamine compound solution of acetone-ODA, A polyimide film (Example 2) was prepared by forming a diamine coating layer on a polyimide layer prepared in the same manner as in Production Example 1, except for surface modification, using a 1% by weight acetone-ODA diamine compound solution, and For a polyimide film (Example 3) in which a diamine coating layer was formed on the surface-modified polyimide layer of Production Example 1 using a 1% by weight acetone-ODA diamine compound solution, the contact angle, adhesion to the adhesive sheet (BS), and peel surface were evaluated, and the results are shown in Table 2.
[0061] For the measurement of BS adhesion strength, copper foil adhesive sheet (BS)-polyimide samples were laminated onto both sides of a surface-modified or unmodified polyimide layer. After high-pressure pressing at 150°C, the samples were cut into 1.5 cm wide slices. The adhesive strength was analyzed using a UTM instrument. Analysis was performed on a 50 mm section at a speed of 20 mm / min under 90-degree peel conditions. -Adhesive sheet (BS): An epoxy resin adhesive sheet was used. - Contact angle: The contact angle with the film surface through which water was passed was measured. -Coating properties: Visual inspection was performed to confirm whether the coating was applied uniformly and evenly. - Detachment surface: The detachment surface of the sample after adhesive strength measurement was completed was analyzed using EDS in a SEM device, and the components of the detachment surface were identified through EDS analysis.
[0062] [Table 2]
[0063] Comparative Example 1-1, which does not contain a diamine coating layer, was found to have significantly lower BS adhesion and a much smaller contact angle compared to Comparative Examples 1-2 and Examples 1-3, which do contain a diamine coating layer. Comparative Examples 1-2 and Example 1, where the ODA concentration was 0.1% by weight, all showed good coating properties and adhesion to BS. However, in Example 1, where the surface of the polyimide layer was modified, a low contact angle and high adhesion to BS were observed. As a result, the peeled surface showed a state where the BS and copper foil were integrated, indicating high adhesion between the polyimide layer and BS. On the other hand, in Comparative Examples 1-2, where the surface of the polyimide layer was not modified, the contact angle was larger and the adhesion to BS was lower compared to Example 1. The peeled surface also appeared as a film-like BS, indicating that the adhesion between the polyimide layer and BS was relatively low. In Example 2, where the ODA concentration was 1% by weight, high adhesion to BS was confirmed, but the coating performance was found to be slightly inferior to that of Example 1. In Example 3, where surface modification was performed with an ODA concentration of 1% by weight, high BS adhesion strength was confirmed, but the coating properties were found to be slightly inferior to those of Example 1.
[0064] 4. Example 2 (Evaluation of heat-resistant plating adhesion) The polyimide film of Comparative Example 1-1, which underwent surface modification but was not coated with diamine, was used as Comparative Examples 2-1 to 2-4, and the polyimide film of Example 1, which underwent surface modification and diamine coating, was used as Examples 2-1 to 2-4 to evaluate its heat-resistant plating adhesion. The polyimide films of each comparative example and example were manufactured in the same manner as in Manufacturing Example 1, except that the diamine monomer and dianhydride monomer listed in Table 3 below were used (in the comparative examples, surface modification and diamine coating were not performed).
[0065] To prepare samples for evaluating heat-resistant plating adhesion, sputtering was performed on the surface of a polyimide film using a sputtering apparatus, with nickel and copper electrodes. The sputtered samples were then plated with copper to a thickness of 8 μm using an electroplating method with a copper plating solution. After attaching a DFR film to the polyimide, an exposure treatment was performed to form an exposed DFR film pattern with a width of 2 mm. The unexposed DFR film and copper layer were removed by etching and development. The exposed DFR film was dissolved in a basic aqueous solution and washed with water to prepare samples for evaluating plating adhesion. The heat-resistant plating adhesion was measured by the following method and is shown in Table 4. - Heat-resistant plating adhesion: After heating in a hot air oven at a high temperature (150°C) for 7 days, the adhesion between the copper layer and polyimide of the plated sample was measured. The adhesion was analyzed using a UTM instrument. The analysis was performed on a 50 mm section at a speed of 20 mm / min under 90-degree peel conditions. The improvement rate of heat-resistant plating adhesion was calculated as (Example PI - Comparative Example PI) / Comparative Example PI × 100.
[0066] [Table 3]
[0067] [Table 4]
[0068] The polyimide films of Examples 2-1 to 2-4, which have surface modification and a diamine coating layer, were found to have significantly better heat-resistant plating adhesion than the comparative examples.
[0069] As can be seen from the above, the polyimide film according to the present invention, by including a polyimide layer whose surface has been modified by corona treatment or plasma treatment, and a diamine coating layer formed on one or both sides of the polyimide layer, has been confirmed to exhibit higher room temperature and heat-resistant adhesion to adhesive sheets and metal layers than conventional films.
[0070] From the above description, those skilled in the art will understand that the present invention can be implemented in other specific forms without altering its technical idea or essential features. In this regard, it should be understood that the embodiments described above are illustrative in all respects and are not intended to be limiting. The scope of the present invention should be interpreted as including the meaning and scope of the claims described below, and all modifications or variations derived therefrom, rather than from the above detailed description.
Claims
1. A polyimide film comprising a polyimide layer derived from a polyamic acid solution and a diamine coating layer containing a diamine compound formed on one or both sides of the polyimide layer, The polyimide film is a polyimide film having an adhesive strength of 1,400 gf / cm or more to an adhesive sheet.
2. The polyimide film according to claim 1, wherein the diamine compound contained in the diamine coating layer is one or more selected from the group consisting of 4,4'-oxydianiline, 3,4'-oxydianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-methylenedianiline, 3,3'-methylenedianiline, and 4,4'-diamino-2,2'-dimethylbiphenyl.
3. The aforementioned polyimide layer has the following polymerization units: One or more dianhydride monomers selected from the group consisting of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 2,3,3',4-biphenyltetracarboxylic acid dianhydride, oxydiphthalic acid anhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, and 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride; and One or more diamine monomers selected from the group consisting of 4,4'-oxydianiline, 3,4'-oxydianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-methylenedianiline, 3,3'-methylenedianiline, and 4,4'-diamino-2,2'-dimethylbiphenyl; A polyimide film according to claim 1, comprising:
4. The polyimide film according to claim 1, wherein one or both sides of the polyimide layer are surface-modified by corona treatment or plasma treatment.
5. The polyimide film according to claim 1, wherein the improvement rate of heat-resistant plating adhesion is 10% to 60%.
6. The polyimide film according to claim 1, wherein the contact angle of the polyimide film is 35° or more.
7. A process for manufacturing a polyimide layer by applying a polyamic acid solution onto a substrate and heat-treating it; and A diamine coating layer formation step involves applying a diamine compound solution, obtained by dissolving a diamine compound in an organic solvent, to one or both sides of a polyimide layer and then heat-treating it; Includes, A method for producing a polyimide film, wherein the concentration of the diamine compound in the diamine compound solution is 0.01 to 10% by weight.
8. The aforementioned polyamic acid solution is One or more dianhydride monomers selected from the group consisting of pyromellitic dianhydride, 3,3',4,4'-biphenyltetracarboxylic acid dianhydride, 2,3,3',4-biphenyltetracarboxylic acid dianhydride, oxydiphthalic acid anhydride, bis(3,4-dicarboxyphenyl)sulfone dianhydride, and 3,3',4,4'-benzophenonetetracarboxylic acid dianhydride; and One or more diamine monomers selected from the group consisting of 4,4'-oxydianiline, 3,4'-oxydianiline, p-phenylenediamine, m-phenylenediamine, 4,4'-methylenedianiline, 3,3'-methylenedianiline, and 4,4'-diamino-2,2'-dimethylbiphenyl; A method for producing a polyimide film according to claim 7, including the following:
9. The method for manufacturing a polyimide film according to claim 7, further comprising a surface modification step of corona treatment or plasma treatment of one or both sides of the polyimide layer after the manufacturing step of the polyimide layer.
10. The aforementioned surface modification process uses a 150-400 W / m² 2 A method for producing a polyimide film according to claim 9, which is carried out under the conditions of / min.
11. The method for producing a polyimide film according to claim 7, wherein the solvent of the diamine compound solution is selected from acetone, dimethylformamide, or a mixture thereof.
12. The method for producing a polyimide film according to claim 7, wherein the step of forming the diamine coating layer is performed at a temperature of 150 to 300°C for 1 to 10 minutes.
13. An electronic component comprising a polyimide film according to any one of claims 1 to 6.
14. The electronic component according to claim 13, wherein the electronic component is a semiconductor device or a flexible circuit board.
15. The aforementioned flexible circuit board is The electronic component according to claim 14, comprising a polyimide film and a layer formed on one or both sides of the polyimide film, which includes an adhesive sheet, a metal layer, or a combination thereof.