Composite materials

The composite material design addresses bonding and airtightness issues in dissimilar materials by forming an internal space through controlled molding, enabling stable heat exchange and durability in large-scale applications.

JP2026539050APending Publication Date: 2026-11-19LG CHEM LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026524655
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-10-24
Filing Date
2024-10-24
Publication Date
2026-11-19

AI Technical Summary

Technical Problem

Existing technologies face challenges in firmly bonding dissimilar materials like metal and plastic without deformation, particularly in creating an airtight internal space for effective heat exchange and maintaining airtightness in large-area composite materials used as heat sinks.

Method used

A composite material design where a metal plate and plastic plate are joined with an internal space formed by convex and concave portions, ensuring high bonding strength and airtightness through controlled temperature and pressure during molding, with surface treatments on the metal plate to enhance bonding and airtightness.

Benefits of technology

The composite material achieves stable and effective heat exchange with a cooling medium, maintaining airtightness and durability even in large-scale applications, ensuring high bonding strength and minimal leakage.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539050000001_ABST
    Figure 2026539050000001_ABST
Patent Text Reader

Abstract

This specification discloses composite materials and their applications. In one example, the composite material may be a composite material in which a metal plate and a plastic plate are joined together, and an internal space exists at the interface between the metal plate and the plastic plate. According to the disclosures herein, when the composite material is used as a heat dissipation material (e.g., a heat sink) in which a fluid such as a cooling medium moves through the internal space, the internal space can be designed to allow the fluid to perform stable and effective heat exchange with a heat-generating element. Furthermore, according to the disclosures herein, high airtightness can be ensured in the internal space so that the heat exchange performance can be maintained without loss over the long term. According to the disclosures herein, even when the composite material is manufactured in large area or on a large scale, it can exhibit the excellent heat exchange performance and durability due to its airtightness. This specification also discloses applications of composite materials.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This application claims priority under Korean Patent Application No. 10-2023-0143263 dated October 24, 2023, and all content disclosed in the said Korean Patent Application is incorporated herein as part of this specification.

[0002] This specification discloses composite materials and their applications. [Background technology]

[0003] The technology to firmly bond dissimilar materials (for example, metal and plastic) to each other without deformation of their appearance is useful in a variety of fields.

[0004] For example, heat dissipation materials such as heat sinks are usually made of metal. Metals are useful as heat dissipation materials because they have excellent thermal conductivity, but they are not good at reducing weight. Therefore, if the part of a heat dissipation material such as a heat sink that is mainly needed for heat transfer can be made of metal, and the other parts can be made of a material such as plastic, it is possible to create a material that satisfies both heat transfer properties and lightweight properties at the same time.

[0005] However, firmly and stably bonding dissimilar materials such as metal and plastic to each other is not an easy problem.

[0006] For example, one method is to use adhesive materials such as glues to bond dissimilar materials. However, there are not many adhesive materials that exhibit high adhesion to different materials simultaneously.

[0007] Another method that can be considered involves melting one or more dissimilar materials, such as metal and / or plastic, and then pressing them together to bond them. However, in this case, the heat applied for melting may cause deformation such as warping in the metal and / or plastic materials being joined. Therefore, it is difficult to perform the joining while stably forming a certain internal space (cavity) between the joining interfaces of the dissimilar materials, and it is even more difficult to suppress such deformation, especially in the process of manufacturing large-area materials.

[0008] Furthermore, when joining dissimilar materials as a composite material for heat sinks and the like, while forming the internal space, the internal space must be airtight.

[0009] In the case of materials used as heat sinks, a cooling medium such as cooling water or air is sometimes circulated within the internal space to cool the heat transferred from the outside. Since such cooling mediums are often fluids, they can leak out to the outside even if there are tiny gaps connecting the internal space to the outside. Therefore, in addition to joining dissimilar materials with high bonding strength, it is necessary to ensure airtightness by minimizing the presence of such tiny gaps at the joint. [Overview of the Initiative] [Problems that the invention aims to solve]

[0010] This specification discloses composite materials and their applications. In one example, the composite material may be a composite material in which a metal plate and a plastic plate are joined together, and an internal space exists at the interface between the metal plate and the plastic plate. One objective of this specification is to disclose a design for the internal space of the composite material so that when the composite material is used as a heat dissipation material (e.g., a heat sink) in which a fluid such as a cooling medium moves through the internal space, the fluid can perform stable and effective heat exchange with a heat-generating element or the like. Another objective of this specification is to disclose a composite material in which high airtightness is ensured in the internal space so that the heat exchange performance can be maintained without loss over the long term.

[0011] This specification also aims to disclose composite materials that can exhibit the aforementioned excellent heat exchange performance and durability due to airtightness, even when manufactured in large area or on a large scale.

[0012] This specification also aims to disclose applications of the composite material. [Means for solving the problem]

[0013] Of the physical properties mentioned herein, those affected by temperature are those measured at room temperature unless otherwise specified.

[0014] In this specification, the term "room temperature" refers to the natural temperature, without heating or deheating, and means any temperature within the range of approximately 10°C to 30°C, for example, approximately 23°C or approximately 25°C. Furthermore, unless otherwise specified, the unit of temperature in this specification is °C.

[0015] In this specification, if pressure affects the results of any physical properties mentioned, unless otherwise specified, those properties are those measured at atmospheric pressure. Atmospheric pressure is the natural pressure that is neither pressurized nor depressurized, and is generally considered to be in the range of approximately 700 mmHg to 800 mmHg.

[0016] In this specification, if humidity affects the results of any physical property, unless otherwise specified, such physical property is measured at standard humidity. Standard humidity means relative humidity of 40%, 50%, or 65%.

[0017] This specification discloses composite materials.

[0018] The term "composite material" can refer to a material that includes a plastic sheet and a metal sheet. Specifically, the composite material may include a metal sheet having a first surface and a second surface opposite it, and a plastic sheet also having a first surface and a second surface opposite it.

[0019] In the foregoing, the terms "first surface" and "second surface" refer to the main surface of the metal or plastic sheet and the surface opposite to that main surface, and do not define any hierarchical or hierarchical relationship. In the foregoing, the main surface means the surface of the metal or plastic sheet with the largest surface area.

[0020] The metal plate and the plastic plate may be joined together. For example, the first surface of the metal plate and the second surface of the plastic plate may be joined together. The metal plate and the plastic plate may be joined while physically touching each other. This can mean, for example, that the joining is performed without using other materials such as adhesives.

[0021] The composite material may include an internal space formed at the bonding interface between the plastic plate and the metal plate. Such an internal space can be formed, for example, by forming convex and concave portions on either one or both of the plastic plate and the metal plate, and then joining the plastic plate and the metal plate together.

[0022] For example, as illustrated in Figure 1, a recess is formed on the second surface (102) of the composite plastic plate (100), and the surface (1021) of the second surface (102) of the plastic plate (100) on which the recess is not formed is joined to the first surface (201) of the metal plate (200) as a joining surface, and an internal space (300) can be formed at the joining interface between the plastic plate (100) and the metal plate (200) by the recess.

[0023] Figure 1 illustrates a case where a recess is formed in a plastic plate (100), but such a recess can also be formed in a metal plate (200), or it may be formed in both the metal plate (200) and the plastic plate (100).

[0024] Such internal spaces can become flow channels, as will be discussed later.

[0025] There are no particular restrictions on the type of plastic sheet included in the composite material; an appropriate type can be selected and used depending on the purpose. In one example, the plastic sheet can be a plastic sheet containing a resin component and a filler component.

[0026] There are no particular restrictions on the type of resin component contained in the plastic sheet. For example, the resin component can be appropriately selected and used from among resin components known to be moldable by applying heat or other means.

[0027] For example, a thermoplastic polymer can be used as the resin component. The types of applicable thermoplastic polymers include various crystalline and amorphous polymers, and examples include, but are not limited to, polyolefin series polymers such as PP (polypropylene) or PE (polyethylene), polyalkylene oxide series polymers such as mPPO (Modified PPO (Polyethylene oxide)), polyamide series polymers such as PA (polyamide), acetal series polymers such as POM (polyoxymethylene), polyester series polymers such as PC (polycarbonate), PBT (polybutylene terephthalate), or PET (polyethylene terephthalate), acrylic series polymers such as PMMA (poly(methyl methacrylate)), and polystyrene series polymers such as PS (polystyrene) and ABS (Acrylonitrile butadiene styrene).

[0028] There are no particular restrictions on the ratio of the resin components within the plastic sheet, and the ratio can be adjusted to an appropriate level depending on the purpose.

[0029] The aforementioned plastic sheet may contain filler components as additional components. Such filler components may be included, for example, as reinforcing materials.

[0030] There are no particular restrictions on the examples of filler components. For example, organic fillers such as glass fillers, carbon fillers and / or silica fillers, or inorganic fillers or organic-inorganic fillers can be used as filler components.

[0031] The shape of the filler is determined according to the purpose and is not particularly limited. For example, the filler may be a particulate filler (spherical, angular, amorphous, or other particulate filler), a plate-shaped filler, or a fibrous filler.

[0032] There are no particular restrictions on the thickness of the plastic sheet. The thickness of the plastic sheet can be adjusted to an appropriate level considering the desired strength, thermal conductivity, and other physical properties. For example, the lower limit of the thickness of the plastic sheet may be around 0.5 mm, 0.6 mm, 0.7 mm, 0.8 mm, 0.9 mm, 1.0 mm, 1.1 mm, 1.2 mm, 1.3 mm, 1.4 mm, 1.5 mm, 1.6 mm, 1.7 mm, 1.8 mm, 1.9 mm, or 2.0 mm, and the upper limit may be around 20.0 mm, 19.0 mm, 18.0 mm, 17.0 mm, 16.0 mm, 15.0 mm, 14.0 mm, 13.0 mm, 12.0 mm, 11.0 mm, 10.0 mm, 9.0 mm, 8.0 mm, 7.0 mm, 6.0 mm, 5.0 mm, 4.0 mm, 3.0 mm, or 2.0 mm. The thickness may be within a range where it is greater than or greater than any one of the lower limits mentioned above; or within a range where it is less than or less than any one of the upper limits mentioned above; or within a range where it is greater than or greater than any one of the lower limits mentioned above, and at the same time less than or less than any one of the upper limits mentioned above.

[0033] The shape of the plastic plate is not limited. For example, the plastic plate may be in the form of a plate. To form the internal space, the plastic plate may be a molded body having an uneven shape formed by including raised portions (convex portions) and recessed portions (recessed portions).

[0034] The method for forming the uneven shape for creating the recesses in the plastic sheet is not particularly limited. For example, the uneven shape can be formed by applying known plastic molding methods such as injection molding, vacuum forming, or press molding. In order to ensure the desired airtightness and bonding strength, it is necessary that no air bubbles or pores are formed inside the plastic sheet during the process of forming the uneven shape. Furthermore, in order to ensure the airtightness and bonding strength, it is necessary that the plastic sheet itself has high strength uniformly, and that the strength deviation between the convex and concave parts of the uneven shape is small. In order to produce such a plastic sheet, it is necessary that pressure be applied to both the upper and lower parts of the plastic sheet during the process of forming the uneven shape. For this reason, for example, the uneven shape can be formed by a molding method that combines vacuum forming and press molding.

[0035] For example, the uneven shape can be formed by heating the plastic sheet to a certain temperature and applying pressure to the upper and lower parts of the plastic sheet.

[0036] In such cases, the relationship between the heating temperature and the glass transition temperature of the plastic plate (or the resin component contained therein) can be adjusted. For example, when the heating temperature is T and the glass transition temperature is Tg, the upper limit of the absolute value of the temperature deviation calculated by formula 100 × (T - Tg) / Tg may be around 60%, 55%, 50%, 45%, 40%, or 35%, and the lower limit may be around 1%, 5%, 10%, 15%, 20%, 25%, or 30%. The absolute value of the temperature deviation may be within a range that is less than or equal to any one of the upper limits mentioned above; or it may be within a range that is greater than or equal to any one of the lower limits mentioned above, and at the same time less than or equal to any one of the upper limits mentioned above. By applying pressure to a plastic plate heated within such a range to form an uneven shape, it is possible to provide a plastic plate in which pores are minimized internally and uniform strength is ensured.

[0037] When applying pressure at the aforementioned temperature to form irregularities, the pressure can be applied simultaneously to the upper and lower parts of the plastic plate. In such a case, the magnitude of the pressure applied to the upper part of the plastic plate is P. U Let P be the magnitude of the pressure applied at the bottom. L When this is the case, the formula is 100 × (P U -P L ) / P L The upper limit of the absolute value of the pressure deviation calculated may be around 60%, 55%, 50%, 45%, 40%, 35%, 30%, 28%, 26%, 24%, 22%, or 21%, and the lower limit may be around 1%, 5%, 10%, 15%, or 20%. The absolute value of the pressure deviation may be within a range where it is less than or equal to any one of the upper limits mentioned above; or within a range where it is greater than or equal to any one of the lower limits mentioned above, and at the same time less than or equal to any one of the upper limits mentioned above. By applying pressure to the plastic plate within such a range to form an uneven shape, it is possible to provide a plastic plate in which pores are minimized internally and uniform strength is ensured.

[0038] The molding method described above is illustrated in Manufacturing Example 1 of this specification. However, the methods that can be applied to realize the uneven shape are not limited to the above method.

[0039] There are no particular restrictions on the type of metal sheet used in the composite material. The metal sheet can be selected according to the application of the composite material. For example, when the composite material is used as a heat dissipation material, a metal sheet with a certain level of thermal conductivity or higher can be used. Such a metal sheet may be an aluminum sheet, a stainless steel (SUS) sheet, a tungsten sheet, an iron sheet, a cast iron sheet, and / or a copper sheet.

[0040] There are no particular restrictions on the thickness of the metal plate. The thickness of the metal plate can be adjusted to an appropriate level depending on the purpose. For example, the lower limit of the thickness of the metal plate may be around 0.5mm, 0.6mm, 0.7mm, 0.8mm, 0.9mm, 1.0mm, 1.1mm, 1.2mm, 1.3mm, 1.4mm, 1.5mm, 1.6mm, 1.7mm, 1.8mm, 1.9mm, 2.0mm, 2.1mm, 2.2mm, 2.3mm, 2.4mm, 2.5mm, 2.6mm, 2.7mm, 2.8mm, 2.9mm, or 3.0mm, and the upper limit may be 20.0mm, 19.5mm, 19.0mm, or 18.5mm. The thickness may be approximately m, 18.0 mm, 17.5 mm, 17.0 mm, 16.5 mm, 16.0 mm, 15.5 mm, 15.0 mm, 14.5 mm, 14.0 mm, 13.5 mm, 13.0 mm, 12.5 mm, 12.0 mm, 11.5 mm, 11.0 mm, 10.5 mm, 10.0 mm, 9.5 mm, 9.0 mm, 8.5 mm, 8.0 mm, 7.5 mm, 7.0 mm, 6.5 mm, 6.0 mm, 5.5 mm, 5.0 mm, 4.5 mm, 4.0 mm, 3.5 mm, or 3.0 mm. The thickness may be within a range where it is greater than or greater than any one of the lower limits mentioned above; or within a range where it is less than or less than any one of the upper limits mentioned above; or within a range where it is greater than or greater than any one of the lower limits mentioned above, and at the same time less than or less than any one of the upper limits mentioned above.

[0041] If necessary, the metal plate may also have an uneven surface, including recesses, similar to those found in the plastic plate, in order to form the internal space. There are no particular restrictions on the method of forming such a shape on the metal plate; for example, it can be formed by appropriately bending or shaping the metal plate using a known metal forming method. However, in the process of forming such an uneven surface on the metal plate, it may become difficult to ensure airtightness at the bent parts, etc., so in some cases, the metal plate may not have an uneven surface.

[0042] The surface of the metal plate, at least the surface in contact with the plastic plate, may be surface-treated. Such surface treatment can more effectively ensure the desired bonding strength and airtightness. The surface treatment can form a per pattern on the metal plate. The term per pattern can refer to an area that includes a groove recessed downwards relative to the surface of the metal plate and a projection that protrudes upwards relative to the surface of the metal plate. Such a per pattern can be observed when viewing the cross-section of the metal plate in a direction perpendicular to the normal direction of the surface of the metal plate. The projection may also be called a burr. Therefore, the per pattern may be formed on the surface of the metal plate, for example, at least the surface in contact with the plastic plate.

[0043] Figure 2 is an illustrative diagram of the aforementioned par pattern.

[0044] The depth of the groove (groove depth in Figure 2), the width of the groove (groove width in Figure 2), and the height of the protrusion (burr height in Figure 2) in the aforementioned burr pattern can be selected considering the desired joint strength or airtightness, and are not particularly limited.

[0045] For example, the lower limit of the groove depth of the per pattern may be approximately 30 μm, 50 μm, 70 μm, 90 μm, 110 μm, 130 μm, 150 μm, or 155 μm, and the upper limit may be approximately 500 μm, 450 μm, 400 μm, 350 μm, 300 μm, 250 μm, 200 μm, 190 μm, 180 μm, 170 μm, 160 μm, 150 μm, 140 μm, 130 μm, 120 μm, 100 μm, or 95 μm. The depth may be within a range where it is greater than or greater than any one of the lower limits mentioned above; or within a range where it is less than or less than any one of the upper limits mentioned above; or within a range where it is greater than or greater than any one of the lower limits mentioned above, and at the same time less than or less than any one of the upper limits mentioned above. The aforementioned depth was measured relative to the surface of the metal plate.

[0046] For example, the lower limit of the groove width of the per pattern may be approximately 50 μm, 70 μm, 90 μm, 110 μm, 130 μm, 150 μm, 160 μm, or 170 μm, and the upper limit may be approximately 1,000 μm, 900 μm, 800 μm, 700 μm, 600 μm, 500 μm, 400 μm, 300 μm, 200 μm, 190 μm, 180 μm, 170 μm, 160 μm, 150 μm, 140 μm, 130 μm, or 125 μm. The width may be within a range where it is greater than or greater than any one of the lower limits mentioned above; or within a range where it is less than or less than any one of the upper limits mentioned above; or within a range where it is greater than or greater than any one of the lower limits mentioned above, and at the same time less than or less than any one of the upper limits mentioned above. The width is a value measured at the cross-section of the metal plate on which the par pattern is formed, and is the maximum value among the values ​​measured at the cross-section of the groove.

[0047] For example, the lower limit of the height of the protrusions (Burr) of the par pattern may be approximately 1 μm, 5 μm, 10 μm, 15 μm, 20 μm, 25 μm, 30 μm, 35 μm, 40 μm, 45 μm, or 55 μm, and the upper limit may be approximately 500 μm, 450 μm, 400 μm, 350 μm, 300 μm, 250 μm, 200 μm, 190 μm, 180 μm, 170 μm, 160 μm, 150 μm, 140 μm, 130 μm, 120 μm, 100 μm, 90 μm, 80 μm, 70 μm, 60 μm, 50 μm, 40 μm, 30 μm, or 20 μm. The height may be within a range where it is greater than or greater than any one of the aforementioned lower limits; or within a range where it is less than or less than any one of the aforementioned upper limits; or within a range where it is greater than or greater than any one of the aforementioned lower limits and simultaneously less than or less than any one of the aforementioned upper limits. The height is measured with respect to the surface of the metal plate.

[0048] There are no particular limitations on the method for forming the pattern on the metal plate. For example, the pattern can be formed by scanning the surface of the metal plate with a laser of appropriate power or by physically scratching it.

[0049] The aforementioned internal space in the composite material can form a channel through which fluid can move at the bonding interface. The composite material can be used as a heat dissipation material while a cooling medium such as water or air moves through the channel.

[0050] Such a flow path can be designed so that the cooling medium effectively exchanges heat with the heat-generating element when the cooling medium is applied.

[0051] For example, the flow channel is formed by the joint surface of the plastic plate and the metal plate, and the joint surface can be formed to include an external joint surface located outside the flow channel and a plurality of internal joint surfaces located inside the flow channel.

[0052] In this specification, the term "internal joint surface" means a region where the plastic plate and the metal plate are joined, and the joint surface is formed such that, as the fluid moves through the channel, the fluid is divided by the joined region and then rejoins.

[0053] In this specification, the term "external bonding surface" refers to the region where the plastic plate and the metal plate are joined, and is not the internal bonding surface.

[0054] The joining surface will be explained with reference to Figure 3.

[0055] Figure 3 is a schematic view of the composite material disclosed in the present specification when observed from the front (for example, the direction perpendicular to the normal direction of the second surface of the plastic plate), wherein the internal joint surface (500) and the external joint surface (600) are indicated by hatching, and the portions not indicated by the hatching are the flow paths. In the embodiment as shown in Figure 3, after the fluid is injected into the injection port (In), it can move through the flow paths and be discharged again to the discharge port (Out).

[0056] Looking at the drawings, it can be seen that the fluid comes into contact with the internal joint surface (500) during the movement process, is divided by the internal joint surface (500), and then rejoins in the flow path, while the external joint surface does not perform such a function. In the drawings, the aforementioned fluid flow is exemplarily indicated by arrows in a part of the flow path.

[0057] Such a fluid can move through the flow path while in contact with the metal plate.

[0058] In one example, the flow path (internal space) can be formed such that the fluid injected into the bonding interface between the plastic plate and the metal plate moves over an area equal to or greater than a certain ratio of the total area of the metal plate (or the plastic plate) before being discharged. This means, for example, that the area of the flow path accounts for a certain ratio or more of the area of the metal plate. For example, the area of the metal plate (A M ) relative to the area of the flow path (A F ) (100×A F / A M ) may have a lower limit of about 60%, 62%, 64%, 66%, 68%, 70%, 72%, 74%, 76%, 78% or 80%, and an upper limit of about 99%, 97%, 95%, 93%, 91%, 89%, 87%, 85%, 83% or 81%. The ratio (100×A F / A MThe ratio is the same as the ratio of the area of ​​the metal plate (or plastic plate) over which the fluid injected into the joint interface between the plastic plate and the metal plate moves to the area of ​​the metal plate (or plastic plate). The ratio may be within the range of being greater than or greater than any one of the aforementioned lower limits; or it may be within the range of being greater than or greater than any one of the aforementioned lower limits, and simultaneously less than or less than any one of the aforementioned upper limits. The larger the ratio, the more effectively the fluid can exchange heat. However, the larger the ratio, the smaller the area of ​​the joint surface between the plastic plate and the metal plate, and in that case, it is not easy to ensure excellent joint strength and airtightness, etc. However, the composite material manufactured by the method disclosed herein has a ratio of 100 × A F / A M While maximizing this, it is possible to ensure high bonding strength between the plastic plate and the metal plate, as well as airtightness of the internal space (flow channel).

[0059] As illustrated in Figure 3, the internal joint surfaces (500) are formed within the flow path, and the density of these internal joint surfaces (500) can be controlled to enable effective heat exchange. The density of the internal joint surfaces is the ratio of the number of internal joint surfaces formed within the flow path to the total area of ​​the flow path. The lower limit of the density of the internal joint surfaces is 10 surfaces / m 2 , 15 pieces / m 2 , 20 pieces / m 2 , 25 pieces / m 2 , 30 pieces / m 2 , 35 pieces / m 2 , 40 pieces / m 2 , 45 pieces / m 2 , 50 pieces / m 2 , 51 pieces / m 2 , 52 pieces / m 2 , 53 pieces / m 2 Or 54 pieces / m 2 It can be as low as 500 pieces / m 2 , 450 pieces / m 2 , 400 pieces / m 2 , 350 pieces / m 2 , 300 pieces / m 2 , 250 pieces / m 2 , 200 pieces / m2 , 150 pieces / m 2 , 100 pieces / m 2 , 95 pieces / m 2 , 90 pieces / m 2 , 85 pieces / m 2 , 80 pieces / m 2 , 75 pieces / m 2 , 70 pieces / m 2 , 65 pieces / m 2 , 60 pieces / m 2 or 55 pieces / m 2 The density may be within a range that is greater than or greater than any one of the aforementioned lower limits; or it may be within a range that is greater than or greater than any one of the aforementioned lower limits, and at the same time less than or less than any one of the aforementioned upper limits. The internal joint surface formed with the density allows the fluid moving through the flow path to move while effectively scanning the entire area of ​​the flow path, thereby enabling stable and efficient heat exchange.

[0060] The aforementioned internal joint surface can be designed such that R1 in the following equation 1 is within a certain range. [Formula 1] R1 = A1 / A2 In Equation 1, A1 is the total area of ​​the flow path, and A2 is the sum of the areas of the multiple internal joint surfaces (total area), and the units of A1 and A2 are the same.

[0061] The lower limit of R1 in Equation 1 may be approximately 2, 4, 6, 8, 10, 12, 14, 16, 18, or 20, and its upper limit may be approximately 90, 85, 80, 75, 70, 65, 60, 55, 50, 45, 40, 35, 30, 25, 23, or 21. R1 may be within a range that is greater than or greater than any one of the lower limits mentioned above; or within a range that is less than or less than any one of the upper limits mentioned above; or within a range that is greater than or greater than any one of the lower limits mentioned above, and at the same time less than or less than any one of the upper limits mentioned above. An internal joint surface formed to satisfy the range of R1 allows the fluid moving through the flow path to move while effectively scanning the entire area of ​​the flow path, thereby enabling stable and efficient heat exchange.

[0062] The aforementioned internal joint surface can be designed such that R2 in Equation 2 below is within a certain range. [Formula 2] R2 = A1 / A3 In Equation 2, A1 is the total area of ​​the flow path, and A3 is the area of ​​a single internal joint surface. For example, if the areas of multiple internal joint surfaces are not constant, A3 may be the arithmetic mean of the areas of the multiple internal joint surfaces. The units of A1 and A3 are the same.

[0063] The lower limit of R2 in Equation 2 may be approximately 95, 100, 110, 120, 130, 140, 150, 160, or 165, and its upper limit may be approximately 500, 450, 400, 350, 300, 250, 200, 190, 180, or 175. R2 may be within a range that is greater than or greater than any one of the aforementioned lower limits; or within a range that is less than or less than any one of the aforementioned upper limits; or within a range that is greater than or greater than any one of the aforementioned lower limits and simultaneously less than or less than any one of the aforementioned upper limits. An internal joint surface formed to satisfy the range of R2 allows the fluid moving through the flow path to effectively scan the entire area of ​​the flow path, thereby enabling stable and efficient heat exchange.

[0064] The aforementioned internal joint surface can be designed such that R3 in the following equation 3 is within a certain range. [Formula 3] R3 = L 2 / A3 In Equation 3, L is the distance between multiple internal joint surfaces, and A3 is the area of ​​a single internal joint surface.

[0065] In the above, the units of L squared and A3 are the same.

[0066] In the above, the interval between multiple internal joint surfaces is the interval between the centers of adjacent internal joint surfaces (for example, L1 and L2 in Figure 3). For example, if the centers of any two internal joint surfaces are connected and no other internal joint surfaces lie on the imaginary line connecting the centers, then those two internal joint surfaces can be said to be adjacent to each other. In another example, if a fluid flows through a channel and is divided by one of the internal joint surfaces, then rejoins, and subsequently meets another internal joint surface, then those two internal joint surfaces can be said to be adjacent to each other. On the other hand, in the above, the center of an internal joint surface means the center of mass. Furthermore, if there are multiple intervals between internal joint surfaces and they are not constant, then in Equation 3, the smallest interval among the multiple intervals, the longest interval among the multiple intervals, or the arithmetic mean of the multiple intervals is applied.

[0067] The lower limit of R3 in Equation 3 may be approximately 1, 2, 3, 4, 5, 6, 7, 8, 9, or 10, and its upper limit may be approximately 50, 45, 40, 35, 30, 25, 20, 15, 14, 13, 12, or 11. R3 may be within a range that is greater than or greater than any one of the aforementioned lower limits; or within a range that is less than or less than any one of the aforementioned upper limits; or within a range that is greater than or greater than any one of the aforementioned lower limits and simultaneously less than or less than any one of the aforementioned upper limits. An internal joint surface formed to satisfy the range of R3 allows the fluid moving through the flow path to effectively scan the entire area of ​​the flow path, thereby enabling stable and efficient heat exchange.

[0068] The aforementioned internal joint surface can be designed such that R4 in the following equation 4 is within a certain range. [Formula 4] R4 = A1 / T 2 In Equation 4, T is the thickness of the flow path, and A1 is the total area of ​​the flow path.

[0069] In the above, the units of T squared and A1 are the same.

[0070] The lower limit of R4 in Equation 4 may be approximately 5,000, 5,500, 6,000, 6,500, 7,000, 7,500, 8,000, 8,500, or 9,000, and its upper limit may be approximately 50,000, 45,000, 40,000, 35,000, 30,000, 25,000, 20,000, 15,000, 10,000, 9,500, or 9,200. R4 may be within the range of being greater than or exceeding any one of the lower limits mentioned above; or within the range of being less than or equal to any one of the upper limits mentioned above; or within the range of being greater than or exceeding any one of the lower limits mentioned above, and simultaneously being less than or equal to any one of the upper limits mentioned above. The internal joint surface, formed to satisfy the range of R4, can move at a suitable speed while effectively scanning the entire area of ​​the flow path, thereby enabling stable and efficient heat exchange.

[0071] The shape of the internal joint surface described above is not particularly limited, and various shapes can be formed as long as the fluid flowing through the channel is appropriately divided and then rejoined, as described above.

[0072] In the composite material, the total area of ​​the external and internal bonding surfaces (A A The total area of ​​the composite material relative to (A T ) ratio (A T / A A ) can be adjusted. For example, the ratio (A T / A AThe lower limit of ) may be around 1.5, 2, 2.5, 3, 3.5, 4, 4.5, or 5, and the upper limit may be around 50, 45, 40, 35, 30, 25, 20, 15, 10, 9.5, 9, 8.5, 8, 7.5, 7, 6.5, 6, or 5.5. The ratio may be within a range where it is greater than or greater than any one of the lower limits mentioned above; or within a range where it is less than or less than any one of the upper limits mentioned above; or within a range where it is greater than or greater than any one of the lower limits mentioned above, and at the same time less than or less than any one of the upper limits mentioned above.

[0073] A flow path designed to satisfy the above conditions can enable effective heat exchange while the fluid moving inside effectively scans the entire area of ​​the flow path at an appropriate speed. However, such a design may reduce the bonding efficiency between the plastic and metal plates, and may make it difficult to ensure stable airtightness in the internal space.

[0074] However, in composite materials manufactured by the method disclosed herein, the internal space can exhibit excellent airtightness.

[0075] For example, the composite material or internal space (flow channel) can exhibit a certain level of maximum allowable internal pressure. The maximum allowable internal pressure is the internal pressure achieved by injecting a fluid into the internal space of the composite material (the internal space in a sealed state), and means an internal pressure that can be maintained substantially constant in bar units for a certain period of time (approximately 60 seconds) from the time when the injection of the fluid used to achieve the internal pressure is interrupted. In this case, the injected fluid may be, for example, air. Furthermore, the maintenance of a substantially constant internal pressure may also mean exhibiting a 60-second pressure drop, as described later. A method for evaluating such a maximum allowable internal pressure is described in Test Example 2 of the Examples section of this specification. For example, the lower limit of the maximum allowable internal pressure may be at a level of approximately 1.5 bar, 2 bar, 2.1 bar, 2.2 bar, 2.3 bar, 2.4 bar, or 2.5 bar, and the upper limit may be at a level of approximately 5 bar, 4.5 bar, 4 bar, 3.5 bar, 3 bar, 2.9 bar, 2.8 bar, 2.7 bar, 2.6 bar, or 2.5 bar. The maximum allowable internal pressure may be within a range that is greater than or greater than any one of the lower limits mentioned above; or it may be within a range that is greater than or greater than any one of the lower limits mentioned above, and at the same time less than or less than any one of the upper limits mentioned above.

[0076] The internal space (flow channel) of the composite material may also have airtightness exhibiting a certain level of pressure drop rate. The pressure drop rate is the rate of pressure drop measured from the point when the fluid injection is interrupted after the fluid has been injected into the internal space (sealed internal space) of the composite material to achieve the maximum allowable internal pressure or a pressure greater than or equal to the maximum allowable internal pressure, and its unit is Pa / sec. A method for evaluating the pressure drop rate is described in Test Example 2 of the Examples section of this specification. The upper limit of the pressure drop rate may be approximately 20, 18, 16, 14, 12, 10, 8, or 6, and its lower limit may be approximately 1, 3, 5, or 7. The pressure drop rate may be within a range that is less than or equal to any one of the upper limits mentioned above; or within a range that is greater than or equal to any one of the lower limits mentioned above, and at the same time less than or equal to any one of the upper limits mentioned above.

[0077] The internal space of the composite material may also have airtightness exhibiting a certain level of 60-second pressure drop. The 60-second pressure drop refers to the value obtained by subtracting the pressure (P2) at 60 seconds after the injection of fluid (air) into the internal space to achieve the target pressure (P1) from the target pressure (P1 - P2). At this time, the target pressure may be the maximum allowable internal pressure or a pressure greater than or equal to the target pressure. A method for evaluating the 60-second pressure drop is described in Test Example 2 of the Examples section of this specification. The lower limit of the 60-second pressure drop is 10 × 10 -4 bar, 15 x 10 -4 bar, 20 x 10 -4 bar, 25 x 10 -4 bar, 30 x 10 -4 bar, 35 x 10 -4 bar or 40x10 -4 It can be as small as a bar, and the upper limit is 200 x 10 -4 bar, 180 x 10 -4 bar, 160 x 10 -4 bar, 140 x 10 -4 bar, 120 x 10 -4 Bar, 100 x 10-4 bar, 80 x 10 -4 bar, 60 x 10 -4 bar, 55 x 10 -4 Bar, 50 x 10 -4 bar, 45 x 10 -4 bar, 40 x 10 -4 bar or 35 x 10 -4 It may be in the range of bar. The 60-second pressure drop may be within the range of any one of the upper limits mentioned above or less than or equal to any one of the lower limits mentioned above, and simultaneously within the range of any one of the upper limits mentioned above or less than or equal to any one of the upper limits mentioned above.

[0078] The aforementioned internal space is subject to a pressure drop level L according to the following equation 5. P This may be within a specified range. [Formula 5] L P = 100 × P 60 / P MAX In equation 5, P MAX This is the maximum allowable internal pressure, and P 60 This is the pressure drop over 60 seconds.

[0079] P to verify equation 5 60 When measuring, the target pressure shall be the maximum allowable internal pressure. A specific method for verifying Equation 5 is described in Test Example 2 of the embodiments of this specification.

[0080] For example, the pressure reduction level L P The upper limit may be around 0.5%, 0.4%, 0.3%, 0.200%, 0.197%, 0.194%, 0.191%, 0.188%, 0.185%, 0.182%, 0.179%, 0.176%, 0.173%, 0.170%, 0.167%, 0.164%, 0.161%, 0.158%, 0.155%, 0.152%, 0.149%, 0.146%, 0.143%, or 0.140%, and the lower limit may be around 0%, 0.01%, 0.05%, 0.1%, or 0.15%. The pressure drop level L PThis range is such that it is less than or equal to any one of the upper limits mentioned above; or it may be such that it is greater than or equal to any one of the lower limits mentioned above, and at the same time less than or equal to any one of the upper limits mentioned above.

[0081] This specification also discloses a method for manufacturing the composite material. The method makes it possible to manufacture the composite material having the excellent airtightness.

[0082] In the above manufacturing method, the composite material can be manufactured by joining the plastic plate and the metal plate.

[0083] Such a manufacturing method may include the step of heating and pressurizing the laminate of the plastic plate and the metal plate. The heating and pressurizing may be performed simultaneously or sequentially. For example, one of the heating and pressurizing steps may be performed first, followed by the next step in order. Alternatively, the heating and pressurizing steps may be performed simultaneously. Alternatively, one of the pressurizing and heating steps may be performed first, and the other step may be performed while maintaining that step. The heating and / or pressurizing steps may be performed one or more times.

[0084] A specific explanation of the plastic and metal plates applied to the aforementioned process is as described above. Therefore, the aforementioned recesses may be formed in at least one or both of the plastic plate and the metal plate. In such a case, the joining can be performed such that the recesses form an internal space at the joining interface between the plastic plate and the metal plate.

[0085] The shape of the recess is determined according to the application of the composite material and is not particularly limited. For example, the recess can be formed so that the flow channel of the design described above can be formed.

[0086] The conditions of the heating and / or pressurizing process can be adjusted for the production of the composite material.

[0087] For example, the heating can be carried out in such a way that the following condition 1 is satisfied. [Condition 1] A × Tg ≤ T PP <Tg<T MP <Tm In condition 1, T PP T is the temperature of the plastic plate of the laminate measured during heating, Tg is the glass transition temperature of the plastic plate or the resin component contained in the plastic plate, and T MP Tm is the interface temperature between the metal plate and the plastic plate of the laminate measured during heating, and Tm may be the melting temperature of the metal plate.

[0088] In condition 1, A is any number, for example, it may be a number of approximately 0.35, 0.4, 0.45, 0.5, 0.55, or 0.6.

[0089] As specified in Condition 1, the temperature T of the plastic plate of the laminate measured during heating. PP It is controlled so that it is greater than or equal to A × Tg, but less than Tg.

[0090] Temperature T under condition 1 PP This is adjusted according to the glass transition temperature Tg of the plastic sheet to which it is applied. For example, the temperature T PP The lower limit may be around 50°C, 52.5°C, 55°C, 57.5°C, 60°C, 62.5°C, 65°C, 67.5°C, 70°C, 72.5°C, 75°C, 77.5°C, 80°C, 82.5°C, 85°C, 87.5°C, or 90°C, and the upper limit may be around 200°C, 195°C, 190°C, 185°C, 180°C, 175°C, 170°C, 165°C, 160°C, 155°C, 150°C, 145°C, 140°C, 135°C, 130°C, 125°C, 120°C, 115°C, 110°C, 105°C, 100°C, 95°C, or 90°C. PPmay be within a range that is equal to or greater than, or exceeds, any one of the aforementioned lower limits; within a range that is less than, or equal to, any one of the aforementioned upper limits; or within a range that is equal to or greater than, or exceeds, any one of the aforementioned lower limits, and at the same time is less than, or equal to, any one of the aforementioned upper limits.

[0091] The glass transition temperature Tg of the plastic plate or the resin component contained therein is selected according to the type of the applied plastic plate, and there is no particular limitation thereon. In one example, the lower limit of the glass transition temperature Tg in the aforesaid condition 1 may be about 55°C, 60°C, 65°C, 70°C, 75°C, 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C, 140°C or 145°C, and the upper limit thereof may be about 400°C, 390°C, 380°C, 370°C, 360°C, 350°C, 340°C, 330°C, 320°C, 310°C, 300°C, 290°C, 280°C, 270°C, 260°C, 250°C, 240°C, 230°C, 220°C, 210°C, 200°C, 190°C, 180°C, 170°C, 160°C or 150°C. The glass transition temperature Tg may be within a range that is equal to or greater than, or exceeds, any one of the aforementioned lower limits; or within a range that is less than, or equal to, any one of the aforementioned upper limits; or within a range that is equal to or greater than, or exceeds, any one of the aforementioned lower limits, and at the same time is less than, or equal to, any one of the aforementioned upper limits.

[0092] In the heating step that satisfies condition 1, T relative to the aforesaid Tg PP the ratio Tg / T PP can be adjusted. For example, the aforesaid ratio Tg / T PP may have an upper limit of about 2.5, 2.4, 2.3, 2.2, 2.1, 2, 1.9, 1.8, 1.7 or 1.65, and a lower limit of about 1, 1.1, 1.2, 1.3, 1.4, 1.5 or 1.6. The aforesaid ratio Tg / T PPmay be within a range that is equal to or more than, or exceeds any one of the aforementioned lower limits; or is less than or equal to any one of the aforementioned upper limits, or is within a range that is equal to or more than, or exceeds any one of the aforementioned lower limits, and at the same time is less than or equal to any one of the aforementioned upper limits.

[0093] In Condition 1, the interface temperature T of the metal plate and the plastic plate measured during heating MP is determined by the glass transition temperature Tg and the melting temperature Tm. In one example, the temperature T MP may have a lower limit of approximately 100°C, 110°C, 120°C, 130°C, 140°C, 150°C, 160°C, 170°C or 180°C, and an upper limit of approximately 300°C, 290°C, 280°C, 270°C, 260°C, 250°C, 240°C, 230°C, 220°C, 210°C, 200°C, 190°C, 180°C, 170°C or 160°C. The interface temperature may be within a range that is equal to or more than, or exceeds any one of the aforementioned lower limits; or within a range that is less than or equal to any one of the aforementioned upper limits; or within a range that is equal to or more than, or exceeds any one of the aforementioned lower limits, and at the same time is less than or equal to any one of the aforementioned upper limits.

[0094] When Condition 1 is satisfied, the ratio of T MP to T g T MP / Tg can be further adjusted. For example, the lower limit of the ratio T MP / Tg may be approximately 0.5, 0.6, 0.7, 0.8, 0.9, 1.0 or 1.1, and the upper limit thereof may be approximately 3.0, 2.9, 2.8, 2.7, 2.6, 2.5, 2.4, 2.3, 2.2, 2.1, 2.0, 1.9, 1.8, 1.7, 1.6, 1.5, 1.4, 1.3 or 1.2. The ratio T MP / Tg may be within the range of being greater than or greater than any one of the lower limits mentioned above; or within the range of being less than or less than any one of the upper limits mentioned above; or within the range of being greater than or greater than any one of the lower limits mentioned above, and simultaneously less than or less than any one of the upper limits mentioned above.

[0095] The melting temperature of the metal plate is adjusted according to the type of metal and is determined by the intrinsic melting temperature Tm of the metal plate. In one example, the lower limit of the melting temperature of the metal plate may be around 185°C, 190°C, 195°C, 200°C, 205°C, 210°C, 215°C, 220°C, 225°C, 230°C, 235°C, 240°C, 245°C, 250°C, 255°C, 260°C, or 265°C, and the upper limit may be around 900°C, 850°C, 800°C, 750°C, 700°C, 650°C, 600°C, 550°C, 500°C, 450°C, or 400°C. The melting temperature Tm of the metal plate may be within the range of being greater than or exceeding any one of the lower limits mentioned above; or within the range of being less than or equal to any one of the upper limits mentioned above; or within the range of being greater than or exceeding any one of the lower limits mentioned above, and simultaneously less than or equal to any one of the upper limits mentioned above.

[0096] When condition 1 is met, T for Tm MP The ratio Tm / T MP The Tm / T can be adjusted. For example, the Tm / T MPThe lower limits are 1.50, 1.55, 1.60, 1.65, 1.70, 1.75, 1.80, 1.85, 1.90, 2.00, 2.05, 2.10, 2.15, 2.20, 2.25, 2.30, 2.35, 2.40, 2.45, 2.50, 2.55, 2.60, 2.65, 2.70, 2.75, 2.80, 2.85, 2.90, 2.95, 3.00, 3.05, 3.10, 3.15, 3.20, 3.25, 3.30, 3.35, 3.40, 3.45, The ratio may be around 3.50, 3.55, 3.60, or 3.65, and its upper limit may be around 20.0, 19.5, 19.0, 18.5, 18.0, 17.5, 17.0, 16.5, 16.0, 15.5, 15.0, 14.5, 14.0, 13.5, 13.0, 12.5, 12.0, 11.5, 11.0, 10.5, 10.0, 9.5, 9.0, 8.5, 8.0, 7.5, 7.0, 6.5, 6.0, 5.5, 5.0, 4.5, or 4.0. The ratio Tm / T MP This may be within the range of being greater than or exceeding any one of the aforementioned lower limits; or within the range of being less than or equal to any one of the aforementioned upper limits; or within the range of being greater than or exceeding any one of the aforementioned lower limits, and simultaneously less than or equal to any one of the aforementioned upper limits.

[0097] By maintaining the above conditions during the heating process, the desired composite material can be effectively manufactured. Although the reason is not clear, it is presumed that when the temperature is adjusted to satisfy condition 1, the molten state or fluidity of the plastic sheet and / or metal sheet is optimized, thereby obtaining a composite material with the desired airtightness and bonding strength without deformation of its appearance. Furthermore, the above effects can also be obtained when manufacturing the composite material over a large area.

[0098] There are no restrictions on the method used to satisfy the above conditions in the heating process. For example, a method of applying heat from the top and / or bottom of the laminate can be used. If condition 1 is satisfied, the heat may be applied from either the top or the bottom. However, to more effectively satisfy the above conditions, it is advantageous that the heat be applied from both the top and the bottom of the laminate.

[0099] The heat can be applied using a known heater, such as a ceramic heater or a coil heater. For example, if a plastic plate is positioned at the top and a metal plate at the bottom, the upper heater can be positioned to heat the plastic plate and the lower heater to heat the metal plate, and the upper and lower heaters can be operated simultaneously. Alternatively, if a metal plate is positioned at the top and a plastic plate at the bottom, the upper heater can be positioned to heat the metal plate and the lower heater to heat the plastic plate, and the upper and lower heaters can be operated simultaneously.

[0100] In the above manufacturing method, the pressurization may be performed separately after the heating, as described above, or it may be performed simultaneously with the heating.

[0101] There are no particular restrictions on the method of applying such pressure. For example, a method of applying pressure to the laminate using a suitable mold or other means can be used. In this case, by adjusting the shape of the mold or the like, pressure can be applied only to the parts of the laminate where the protrusions are not formed or to the parts where the plastic plate and the metal plate are in direct contact.

[0102] Such pressurization can be performed, for example, simultaneously at the top and bottom of the laminate, or at the top or bottom of the laminate only.

[0103] There are no particular restrictions on the magnitude of the pressure (P1) applied during the pressurization process. The pressure can be adjusted to an appropriate level depending on the purpose. For example, the lower limit of the pressure (P1) is 7000 gf / cm². 2、7050gf / cm 2 、7100gf / cm 2 、7150gf / cm 2 、7200gf / cm 2 、7250gf / cm 2 、7300gf / cm 2 、7350gf / cm 2 、7400gf / cm 2 、7450gf / cm 2 、7500gf / cm 2 、7550gf / cm 2 、7600gf / cm 2 、7650gf / cm 2 、7700gf / cm 2 、7750gf / cm 2 、7800gf / cm 2 、7850gf / cm 2 、7900gf / cm 2 、7950gf / cm 2 、8000gf / cm 2 、8050gf / cm 2 、8100gf / cm 2 、8150gf / cm 2 、8200gf / cm 2 、8250gf / cm 2 、8300gf / cm 2 、8350gf / cm 2 、8400gf / cm 2 、8450gf / cm 2 、8500gf / cm 2 、8550gf / cm 2 、8600gf / cm 2 、8650gf / cm 2 、 8700gf / cm 2 、8750gf / cm 2 、8800gf / cm 2 、8850gf / cm 2 、8900gf / cm 2 、8950gf / cm 2 、9000gf / cm 2 、9050gf / cm 2 、9100gf / cm 2 、9150gf / cm 2or 9200 gf / cm² 2 It may be as low as 11,000 gf / cm³, with an upper limit of 11,000 gf / cm³. 2 , 10950 gf / cm 2 , 10900 gf / cm² 2 , 10850 gf / cm² 2 , 10800 gf / cm² 2 , 10750 gf / cm 2 , 10700 gf / cm² 2 , 10650 gf / cm 2 , 10600 gf / cm² 2 , 10550 gf / cm 2 , 10500 gf / cm² 2 , 10450 gf / cm 2 , 10400 gf / cm² 2 , 10350 gf / cm 2 , 10300 gf / cm 2 , 10250 gf / cm 2 , 10200 gf / cm 2 , 10150 gf / cm 2 , 10100 gf / cm 2 , 10050 gf / cm 2 , 10000 gf / cm² 2 9950 gf / cm² 2 9900 gf / cm² 2 9850 gf / cm² 2 9800 gf / cm² 2 9750 gf / cm² 2 9700 gf / cm² 2 9650 gf / cm² 2 9600 gf / cm² 2 9550 gf / cm² 2 9500 gf / cm² 2 9450 gf / cm² 2 9400 gf / cm² 2 9350 gf / cm² 2 9300 gf / cm² 2 9250 gf / cm² 2 or 9200 gf / cm² 2The degree may be such that the pressure (P1) applied during pressurization is within a range that is greater than or greater than any one of the lower limits mentioned above; or within a range that is less than or less than any one of the upper limits mentioned above; or within a range that is greater than or greater than any one of the lower limits mentioned above, and at the same time less than or less than any one of the upper limits mentioned above.

[0104] The pressurization time can also be determined according to the purpose and is not significantly limited. For example, the lower limit of the pressurization time may be around 10, 20, 30, 40, 41, 42, 43, 44, 45, 46, 47, 48, 49, or 50 seconds, and the upper limit may be around 3600, 3400, 3200, 3000, 2800, 2600, 2400, 2200, 2000, 1800, 1600, 1400, 1200, 1000, 800, 600, 400, 200, 100, 85, 80, 75, 70, 65, 60, 55, or 50 seconds. The pressurization time may be within a range where it is greater than or greater than any one of the aforementioned lower limits; or within a range where it is less than or less than any one of the aforementioned upper limits; or within a range where it is greater than or greater than any one of the aforementioned lower limits and simultaneously less than or less than any one of the aforementioned upper limits. Furthermore, the pressurization time can also be appropriately adjusted by the pressure applied during pressurization.

[0105] As described above, the heating and pressurizing can be performed simultaneously or sequentially.

[0106] For example, the heating and pressurizing can be carried out in a manner that includes a first step of heating the laminate of the plastic plate and the metal plate, and a second step of pressurizing the laminate.

[0107] In the aforementioned case, the second stage can be carried out under conditions that satisfy condition 1. For example, heating in the first stage can be performed in a manner that satisfies condition 1, and the second stage can be started while maintaining this state.

[0108] The method for manufacturing the composite material disclosed herein may further include a step of cooling the laminate, following the heating and pressurizing step.

[0109] The conditions in the cooling process can be adjusted to produce the desired composite material. For example, the cooling process can also be carried out while applying a certain level of pressure to the laminate.

[0110] For example, the cooling step can be carried out under pressurized conditions such that ΔP in the following formula 6 falls within a predetermined range. For example, following the heating and pressurizing step (or the second stage), the cooling step can be carried out while the pressure applied to the laminate is adjusted so that ΔP in the following formula 6 falls within a predetermined range. In one example, the upper limit of ΔP is 400%, 398%, 396%, 394%, 392%, 390%, 388%, 386%, 384%, 382%, 380%, 378%, 376%, 374%, 372%, 370%, 368%, 366%, 364%, 362%, 360%, 358%, 356%, 354%, Approximately 352%, 350%, 348%, 346%, 344%, 342%, 340%, 338%, 336%, 334%, 332%, 330%, 328%, 326%, 324%, 322%, 320%, 318%, 316%, 314%, 312%, 310%, 308%, 306%, 304%, 302%, or around 300% It may be present, and its lower limit is 200%, 202%, 204%, 206%, 208%, 210%, 212%, 214%, 216%, 218%, 220%, 222%, 224%, 226%, 228%, 230%, 232%, 234%, 236%, 238%, 240%, 242%, 244%, 246%, 248%, 2 △P may be approximately 50%, 252%, 254%, 256%, 258%, 260%, 262%, 264%, 266%, 268%, 270%, 272%, 274%, 276%, 278%, 280%, 282%, 284%, 286%, 288%, 290%, 292%, 294%, 296%, 298%, or 300%. The aforementioned △P may be within the range of being greater than or exceeding any one of the aforementioned lower limits; or within the range of being less than or equal to any one of the aforementioned upper limits; or within the range of being greater than or exceeding any one of the aforementioned lower limits, and simultaneously less than or equal to any one of the aforementioned upper limits.

[0111] [Formula 6] △P = 100 × (P2 - P3) / P3 In Equation 6, P2 is the pressure applied to the laminate during the pressurization step before cooling (for example, the second stage), and P3 is the pressure applied to the laminate during the cooling step. P2 may be the same as, for example, the range of the pressure P1 applied during pressurization.

[0112] The cooling of the laminate may be carried out by natural cooling or forced cooling. In the case of natural cooling, the laminate is maintained under low temperature conditions (e.g., room temperature conditions), while forced cooling can be carried out by bringing the laminate into contact with a suitable cooling medium (e.g., cooling water).

[0113] The desired composite material can be manufactured through the above process. The method for manufacturing the composite material may further include any additional steps necessary in addition to the above process. For example, the method may further include a step of deattachment after the cooling step.

[0114] Composite materials manufactured using this method possess excellent bonding strength and airtightness. Furthermore, such composite materials can be obtained without any changes in appearance during the manufacturing process.

[0115] This specification also discloses an apparatus comprising the composite material.

[0116] For example, the apparatus may include the composite material and a cooling medium. The cooling medium may be present in the flow path of the composite material or prepared to be injected into the flow path.

[0117] Such devices may include, for example, cooling devices such as heat sinks or thermal interface materials (TIMs).

[0118] In the foregoing, the type of cooling medium is not particularly limited, and for example, cooling water such as water or gases such as air can be used.

[0119] The apparatus may also include a heating element and the composite material. The apparatus may also include the heating element and the cooling device. In such cases, the composite material and the heating element may be in thermal contact. In this specification, the term thermal contact means contact that can transfer heat from the heating element to the composite material, and does not necessarily mean that they are physically touching each other.

[0120] In the foregoing, the type of heat-generating element is not particularly limited. The heat-generating element may be any kind of component, element, or device that generates heat during operation or storage and requires control of such heat. Examples of such heat-generating elements include, but are not limited to, battery cells, battery modules, or battery packs.

[0121] For example, the apparatus may further include the cooling medium. The cooling medium may be present in the flow path of the composite material or prepared to be injected into the flow path. [Effects of the Invention]

[0122] This specification discloses composite materials and their applications. In one example, the composite material may be a composite material in which a metal plate and a plastic plate are joined together, and an internal space exists at the interface between the metal plate and the plastic plate. According to the disclosure herein, when the composite material is used as a heat dissipation material (e.g., a heat sink) in which a fluid such as a cooling medium moves through the internal space, the internal space can be designed so that the fluid can perform stable and effective heat exchange with a heat-generating element or the like. Furthermore, according to the disclosure herein, high airtightness can be ensured in the internal space so that the heat exchange performance can be maintained without loss over the long term.

[0123] According to the disclosure herein, the composite material can exhibit the excellent heat exchange performance and durability due to its airtightness even when manufactured in large area or on a large scale. This specification also discloses applications of the composite material. [Brief explanation of the drawing]

[0124] [Figure 1] This is a schematic diagram of a cross-section of the side of the composite material. [Figure 2] This figure shows the pattern formed on the surface of the metal plate. [Figure 3] This is a schematic front view of the aforementioned composite material. [Figure 4] This is a schematic diagram illustrating the joining process between a plastic sheet and a metal sheet. [Figure 5] This is a schematic diagram illustrating the manufacturing process of a plastic sheet with a recess. [Figure 6] This is a schematic diagram illustrating the manufacturing process of a plastic sheet with a recess. [Figure 7] This figure shows the evaluation results of the maximum allowable internal pressure in Example 1. [Figure 8] This figure shows the pressure drop in Example 1. [Figure 9] This figure shows the pressure drop in Example 2. [Modes for carrying out the invention]

[0125] The present application will be described in detail through the following embodiments, but the scope of this application is not limited by the embodiments described below. [Examples]

[0126] Manufacturing example 1. As shown in Figure 4, a plastic plate (100) with an uneven shape formed by recesses (1001) and protrusions (1002) was manufactured using the following method. First, a rectangular plastic plate was prepared with a width of approximately 610 mm, a length of approximately 308 mm, and a thickness of approximately 2 mm. In the above, the shape of the recess (1001) was adjusted so that a flow channel with the shape shown in Figure 3 was formed after joining with the metal plate. The total area of ​​the flow channel formed according to Figure 3 was approximately 146,180 mm². 2 The total area of ​​the external joint surface (600) is approximately 29,308 mm². 2The total area of ​​the internal joint surfaces (500) is approximately 7,050 mm². 2 The recess (1001) was formed to such an extent. Furthermore, there are a total of eight internal joint surfaces (500) within the flow path, and each internal joint surface (500) has the same area, with the area of ​​a single internal joint surface being approximately 881.26 mm². 2 The resulting shape was such that the spacing between adjacent internal joining surfaces was approximately 78.38 mm (L2 in Figure 3) or 114.45 mm (L1 in Figure 3). Furthermore, after forming the recess, the total area of ​​the plastic plate as seen from the front was approximately 182,538 mm². 2 It was to that extent. Furthermore, the recess (1001) was formed to a depth of approximately 4 mm.

[0127] First, a sheet of plastic material (a rectangular plastic sheet with a width of approximately 610 mm, a length of approximately 308 mm, and a thickness of approximately 2 mm) was manufactured. The sheet was manufactured to a thickness of approximately 2 mm by applying a material, which was a mixture of resin component (mPPO (Modified PPO (Polyethylene oxide))) and filler component (glass fiber) in a weight ratio of 8:2 (mPPO: filler component), to an extrusion process. The resin component, mPPO, has a glass transition temperature (T g The temperature was approximately 145°C, and the glass fiber had a cross-sectional diameter of approximately 12.5 μm and an aspect ratio of approximately 24.

[0128] The glass transition temperature was measured using a Differential Scanning Calorimeter (DSC 8000, Perkin Elmer (USA)). During measurement, the temperature range was from 40°C to 350°C, and the glass transition temperature was measured at a rate of 10°C / min using the Heating and Cooling modes while observing the change in heat flow. The samples used for measurement were weighed to have a diameter of approximately 2 mm or less and a weight of approximately 10 mg.

[0129] Using the aforementioned material, the molded body (plastic sheet (100)) shown in Figure 4 was manufactured in the following manner. As shown in Figure 5, the material (1000) was placed on a first mold (3000) which had incisions formed thereon corresponding to the uneven shape of the molded body. A second mold (4000) which had relief shapes formed thereon corresponding to the uneven shape was then placed on the material (1000).

[0130] Next, a ceramic heater was used to maintain the surface temperature of the fabric at approximately 195°C. The ceramic heater was located inside the heating equipment, and with the ceramic heater positioned above the fabric, the temperature was raised to the target temperature through the temperature control of a PLC (Programmable Logic Controller) system. Whether or not the surface temperature of the fabric was controlled to the target temperature was confirmed using a non-contact infrared thermometer.

[0131] Subsequently, while maintaining the temperature, suction (L) was performed at the bottom of the first mold (3000) as shown in Figure 5, and at the same time, the second mold (4000) was moved downwards to apply pressure to the fabric in the configuration shown in Figure 6.

[0132] The aforementioned suction (L) was performed with the equipment's gauge fully open. This type of suction resulted in a vacuum flow of approximately 1 atmosphere based on the rate, and the pressure applied to the fabric was approximately 690.2 gf / cm². 2 The applied load is approximately 1500 kg. Furthermore, the pressure applied by the second mold (4000) is approximately 548.7 gf / cm² to the molded body formed through the suction. 2 The process was carried out to apply a pressure level of approximately 1000 kg.

[0133] The state of the first mold (3000) and the second mold (4000) as shown in Figure 6 was maintained for about 10 seconds, and the temperature of the molded body (raw material) (1000) was reduced to about 40°C for a cooling process. After the cooling process, the first and second molds (3000, 4000) were separated, and the molded plastic sheet was recovered.

[0134] Example 1. A composite material was manufactured by bonding a plastic plate and a metal plate as in Manufacturing Example 1. The bonding was carried out so that the surface (1002) of the plastic plate (100) that does not have a recess (1001) was in contact with the metal plate (200), as shown in Figure 4.

[0135] The metal plate used was a rectangular aluminum plate with a width of approximately 610 mm, a length of approximately 308 mm, and a thickness of approximately 3 mm (melting temperature approximately 660.3°C). The melting temperature of the aluminum plate was measured under the same conditions and equipment as those used to measure the glass transition temperature of the mPPO.

[0136] Before adhesion, the surface of the metal plate (200) was first laser-treated to form a per pattern. This laser treatment was performed only on the portion of the metal plate (200) that would come into contact with the plastic plate (100).

[0137] The surface treatment was performed using a laser irradiation device (50W Fiber marking machine, K2 Laser) equipped with a fiber source. The laser irradiation device was used to irradiate the area requiring surface treatment. Laser irradiation was performed by cross-scanning (mesh configuration) the surface treatment surface at a scan speed of approximately 800 mm / sec to 900 mm / sec, with four scans performed on the same surface. The laser output was set to approximately 50W, and the repetition rate was set to approximately 70kHz, with laser energy applied accordingly.

[0138] The surface treatment described above formed a pattern (Per pattern) on the surface of the metal plate as shown in Figure 2. Figure 2 shows the shape observed when the cross-section of the surface-treated aluminum plate (the surface observed when the aluminum plate is cut along the direction normal to the surface) is viewed. In the pattern shown in Figure 2, the width (width of the Groove in Figure 2) was approximately 120 μm to 175 μm, the depth (depth of the Groove in Figure 2) was approximately 90 μm to 160 μm, and the height (height of the Burr in Figure 2) was approximately 15 μm to 55 μm.

[0139] Next, the plastic plate (100) and the metal plate (200) were stacked in the form shown in Figure 4 to produce a laminate, and the laminate was then heated and pressurized.

[0140] The heating and pressurizing described above were carried out using a device (BG-200 (Modified), SUNGSHIN hydraulic machine) capable of forming a sealed internal space, heating the internal space, adjusting the pressure in the internal space to pressurize the laminate while it was heated, and also capable of cooling. First, the laminate was placed in the sealed space of the device (BG-200 (Modified)). At this time, the plastic plate (100) of the laminate was positioned at the top, and the metal plate (200) was positioned below it.

[0141] The laminate was heated in the above state (heating step). The heating was performed by simultaneously operating the upper heater located on the plastic plate (100) side of the laminate and the lower heater located on the metal plate (200) side. As a result of the heating, the temperature (Tpp) of the plastic plate (100) became approximately 90°C, and the interface temperature (T) of the plastic plate (100) and the metal plate (200) MPThe material was heated until it reached approximately 180°C. In the above procedure, the temperature of the plastic plate was measured by cross-checking using a TC (Terminal couple) built into the device (BG-200 (Modified)) and a non-contact infrared thermometer, and the interface temperature between the plastic plate (100) and the metal plate (200) was confirmed by directly positioning a thermometer (mobile temperature loader (Terminal couple)) at the interface.

[0142] When the upper heater was operated at a temperature of 90°C and the lower heater at a temperature of 180°C, the temperature of the plastic plate and the interface temperature were confirmed approximately 1400 seconds after the start of operation.

[0143] When the temperature of the plastic sheet and the interface temperature reached the aforementioned temperature, the pressure in the sealed internal space of the equipment was adjusted to pressurize the laminate (pressurization step). Pressurization was performed by pressing the plastic sheet using a mold and applying a load. At this time, the pressurization was approximately 9,200 gf / cm². 2 The load was applied to the laminate at a pressure of approximately 20 tons. During the pressurization, only the joints of the laminate (the surface-treated parts of the plastic plate and metal part) were pressurized.

[0144] The aforementioned pressurization was carried out for approximately 50 seconds while maintaining the temperature of the plastic plate and the interface temperature achieved by heating before pressurization.

[0145] A cooling process was performed after the pressurization described above (cooling process).

[0146] The cooling process was carried out by circulating cooling water around the sealed space. The cooling was performed by applying a pressure of approximately 2300 gf / cm² to the laminate. 2 The procedure was carried out under conditions where the applied load was reduced to approximately 5 tons, and continued until the temperature of the laminate (temperature of the plastic plate and the interface temperature between the plastic plate and the metal plate) fell to approximately 60°C or below.

[0147] After the cooling process, the laminate was detached and the composite material was recovered.

[0148] Example 2. The composite material was manufactured in the same manner as in Example 1, except that the interface temperature (TMP) between the plastic plate (100) and the metal plate (200) was set to approximately 160°C during the heating process, and this interface temperature was maintained during the pressurizing process.

[0149] Example 3. The composite material was manufactured in the same manner as in Example 1, except that the upper heater was not operated during the heating process, only the lower heater was operated, the applied pressure and pressurization time in the pressurizing process were changed, and the applied pressure in the cooling process was changed.

[0150] The operation of the lower heater is controlled by the interface temperature (T) between the plastic plate (100) and the metal plate (200). MP The process was carried out until the temperature reached approximately 180°C. In this case, the temperature of the plastic plate (100) was maintained at approximately 50°C. This temperature was measured using the same method as in Example 1.

[0151] The pressurization process involves applying approximately 18,400 gf / cm³ to the laminate while maintaining the aforementioned interface temperature. 2 The load was applied at a pressure of approximately 40 tons for 90 seconds. The cooling process after the pressurization process was carried out in the same manner as in Example 1.

[0152] Example 4. During the pressurization process, the pressure increases to approximately 11,500 gf / cm². 2 The composite material was manufactured in the same manner as in Example 1, except that the load was applied to the laminate with a pressure of approximately 25 tons.

[0153] Test Example 1. Evaluation of joint strength and appearance deformation The bonding strength was evaluated using the following method. First, the same plastic plate (thickness: approximately 2 mm) and metal plate (thickness: approximately 3 mm) used in the example were prepared.

[0154] Next, the surface of the metal plate was laser-treated in the same manner as in Example 1. After that, the laser-treated surfaces of the plastic plate and the metal plate were laminated, and a test specimen was manufactured by heating, pressurizing, and cooling under the same conditions as in each example. In the above, the plastic plate (100) and the metal plate (200) were laminated with a slight offset from each other.

[0155] The bonding strength was evaluated for the specimens manufactured as described above. Since these specimens were manufactured using the same materials and under the same conditions as those used in each embodiment, the bonding strength of these specimens can be matched to that of each embodiment.

[0156] The bonding strength was measured at room temperature (approximately 25°C) using a UTM (Universal Testing Machine, Zwick / roell Z030). After fixing the metal plate (200) of the test specimen and fixing the protruding portion of the plastic plate (100) to the equipment, the bonding strength was evaluated while peeling the plastic plate (100) from the metal plate (200). The peeling was performed at a peeling angle of approximately 180 degrees (parallel between the metal and plastic material parts) and a peeling speed of approximately 50 mm / min.

[0157] In addition to the above, the appearance of the composite material was evaluated. The appearance was evaluated directly on the composite material manufactured in the example. Specifically, the metal plate surface of the composite material was placed in contact with the floor, and it was observed from the side to measure whether there were any parts of the composite material that were separated from the floor due to warping, and if so, the distance of the separation. This was then evaluated according to the following criteria.

[0158] <Evaluation Criteria> ○: When the composite material does not lift off the floor, and the entire metal surface of the composite material is in contact with the floor. △: When there is a portion of the composite material metal plate surface that is not touching the floor. The evaluation results described above are shown in Table 1 below.

[0159] [Table 1]

[0160] Test Example 2. Evaluation of Airtightness The airtightness of the composite material was evaluated. Airtightness was assessed for Examples 1 and 2, where appropriate results were confirmed in terms of joint strength and appearance.

[0161] The evaluation of airtightness involves applying a constant pressure to the internal space formed by the joining of a protrusion (1002) of a plastic plate (100) and a metal plate (200) in a composite material, and observing the tendency for that pressure to be maintained or decreased. The better the tendency for the pressure in the internal space to be maintained in this evaluation, the stronger the joining of the plastic plate and the metal plate is reflected.

[0162] The composite material manufactured in the embodiment has an internal space formed by the joining of the plastic plate (100) and the metal plate (200), and this internal space is sealed by the joint between the plastic plate (100) and the metal plate (200). However, the internal space has two passages (inlet and outlet in Figure 3) that communicate with the outside, and one of the two passages is sealed by attaching a jig fitted with a rubber ring gasket. The other passage is also sealed by attaching a jig fitted with a rubber ring gasket, but this passage is made capable of being injected with air. The airtightness was evaluated according to the following procedure.

[0163] Step 1: Inject air until the pressure inside the composite material reaches the target pressure. Stage 2: Stabilize by injecting air for 20 seconds from the time air injection begins, so that the target pressure is maintained and stabilized. Stage 3: After Stage 2, stop air injection and check for pressure drop.

[0164] The airtightness was evaluated using the Pressure Decay Test Method, which identifies pressure changes due to leakage in the sealed internal space of the composite material, through the process described in steps 1 to 3 above.

[0165] Figure 7 shows the results of the evaluation performed on Example 1. Figure 7 shows the evaluation of airtightness while gradually increasing the target pressure to 0.5 bar, 1 bar, 1.5 bar, 2 bar, 2.5 bar, and 3.0 bar. Specifically, the evaluation was performed by first setting the target pressure to 0.5 bar and performing steps 1 to 3, and then setting the target pressure back to 1 bar and sequentially performing steps 1 to 3 again.

[0166] From the drawings, it can be confirmed that the internal pressure is stably maintained for approximately 80 seconds up to the target pressure of 2.5 bar. When the airtightness was evaluated with a target pressure of 3.0 bar, the plastic material rupture occurred when the internal pressure reached 2.8 bar, showing a rapid decrease in pressure, and the internal pressure could not be maintained. From these results, it can be confirmed that in Example 1, the maximum allowable internal pressure is at least 2.5 bar and less than 2.8 bar. In the evaluation of Example 2, it was also confirmed that the maximum allowable internal pressure is at least 2.5 bar and less than 2.8 bar.

[0167] If it was confirmed that the target pressure (bar) was maintained, the degree of pressure drop was checked and the level of pressure drop was confirmed in order to more specifically confirm whether or not there was a pressure decrease. To more clearly confirm whether or not there was a pressure decrease, the unit of pressure was converted to Pa and the level of pressure drop per unit time was checked in Pa / sec.

[0168] Figure 8 shows the results confirmed using the method described above. Since the results in Figure 8 represent the trend in step 3, 0 seconds on the x-axis in Figure 8 corresponds to 20 seconds on the x-axis in Figure 7. The y-axis in Figure 8 represents the pressure drop rate per unit time (unit: Pa / sec) at the corresponding point in time on the x-axis.

[0169] The airtightness was evaluated in the same manner for Example 2. Figure 9 shows the results of specifically confirming the reduction in internal pressure in Example 2, similar to Example 1.

[0170] The results of the airtightness evaluation are summarized in Table 2 below.

[0171] [Table 2]

[0172] In Table 2, the maximum allowable internal pressure is the maximum pressure at which the target pressure can be maintained for approximately 60 seconds from the point when air injection is interrupted, when the airtightness evaluation is performed while gradually increasing the target pressure from 0.5 bar to 0.5 bar in the order of 0.5 bar, 1 bar, 1.5 bar, 2 bar, 2.5 bar, and 3.0 bar. Here, maintaining the target pressure means that the pressure measured in bar units is maintained at a substantially constant level.

[0173] In Examples 1 and 2, as described above, when the target pressure was set to 2.5 bar, the pressure (bar) was maintained for approximately 60 seconds. However, when the target pressure was set to 3.0 bar, rupture occurred when it exceeded 2.8 bar, so the maximum allowable pressure was defined as 2.5 bar.

[0174] On the other hand, the pressure drop rate describes the rate and level of pressure decrease from the point when air injection is interrupted (approximately 20 seconds after air injection). This rate was measured by injecting air according to the maximum allowable internal pressure for each composite material, interrupting air injection approximately 20 seconds after injection, and evaluated by the pressure decrease until the pressure stopped decreasing.

[0175] In Table 2, the pressure drop over 60 seconds (P 60 ) is the maximum allowable internal pressure (P MAX ) and in the process of evaluating the descent speed, the difference in internal pressure (P) at 60 seconds after the air interruption (i.e., approximately 80 seconds after the start of air injection) (P MAX -P 60 ) and its unit is bar.

[0176] The pressure reduction level in Table 2 corresponds to the maximum allowable internal pressure P. MAX and the aforementioned 60-second pressure drop P 60100 x P 60 / P MAX This is the result of substituting the values ​​into the formula and performing the calculation.

[0177] On the other hand, Figure 7 shows the evaluation results of the maximum allowable internal pressure in Example 1, Figure 8 shows the pressure drop in Example 1, and Figure 9 shows the pressure drop in Example 2.

Claims

1. A composite material in which the first surface of a metal plate having a first surface and the second surface of a plastic plate having a second surface are joined together. A recess is formed on the second surface of the aforementioned plastic plate. The second surface of the plastic plate in which the recess is not formed is joined to the first surface of the metal plate as the joining surface. A space is formed at the bonding interface between the plastic plate and the metal plate by the recess. The space forms a channel through which fluid can move at the joint interface. The bonding surface is a composite material including an external bonding surface located outside the flow path and a plurality of internal bonding surfaces located inside the flow path.

2. The composite material according to claim 1, wherein the flow path is formed such that a fluid injected into the bonding interface is discharged after moving over an area of ​​60% or more of the total area of ​​the metal plate.

3. The composite material according to claim 1, wherein the internal bonding surface is formed such that, during the fluid's movement, the fluid is divided by the internal bonding surface and then rejoins.

4. The density of internal bonding surfaces relative to the total area of ​​the flow channel is 10 particles / m². 2 ~500 pieces / m 2 The composite material according to claim 3, which is within the range.

5. The composite material according to claim 3, wherein R1 in formula 1 below is in the range of 2 to 90, and R2 in formula 2 below is in the range of 95 to 500: [Formula 1] R1 = A1 / A2 [Formula 2] R2 = A1 / A3 In equations 1 and 2, A1 is the total area of ​​the flow path, A2 is the sum of the total areas of the internal joint surfaces, and A3 is the area of ​​a single internal joint surface.

6. The composite material according to claim 3, wherein R3 in the following formula 3 is in the range of 1 to 50: [Formula 3] R3 = L 2 / A3 In Equation 3, L is the distance between internal joint surfaces, and A3 is the area of ​​a single internal joint surface.

7. Total area of ​​external and internal joint surfaces (A A The total area of ​​the composite material relative to (A T ) ratio (A T / A A The composite material according to claim 1, wherein the coefficient of the coefficient of the material is in the range of 1.5 to 50.

8. The composite material according to claim 1, wherein the maximum allowable internal pressure of the flow path is in the range of 1.5 bar to 5 bar.

9. The composite material according to claim 1, wherein the pressure drop rate in the flow path is in the range of 1 to 20 Pa / sec.

10. The 60-second pressure drop of the flow path is 10×10 -4 to 200×10 -4 bar, the composite material according to claim 1.

11. L in equation 5 below P The composite material according to claim 1, wherein the content is 0.5% or less: [Formula 5] L P = 100×P 60 / P MAX In equation 5, P MAX This is the maximum allowable internal pressure, P 60 This is the pressure drop over 60 seconds.

12. The composite material according to any one of claims 1 to 11; and A cooling device comprising a cooling medium present in the flow channel of the composite material or prepared to be injected into the flow channel.

13. Heating element; and An apparatus comprising a composite material according to any one of claims 1 to 11, which is in thermal contact with the heating element.

14. The apparatus according to claim 13, wherein the heating element is a battery cell, a battery module, or a battery pack.

15. The apparatus according to claim 13, further comprising a cooling medium present in or prepared for injection into a composite material channel.