Preparations for preparing optical layers containing metal oxides
A novel formulation using metal oxide precursors and solvents addresses gap filling issues in optical grating manufacturing, enabling efficient, crack-free, and cost-effective production of optical layers without CMP, suitable for augmented and mixed reality glasses.
Patent Information
- Application Number
- JP2026525622
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-10-30
- Filing Date
- 2024-10-28
- Publication Date
- 2026-11-19
AI Technical Summary
Existing manufacturing techniques for optical gratings, particularly in augmented and mixed reality glasses, face challenges such as incomplete gap filling during deposition processes, leading to voids and the need for costly chemical mechanical planarization (CMP), which increases production costs and time.
A novel formulation using metal oxide precursors, solvents, and optional acids is developed for preparing optical layers, enabling gap-free filling of trenches and cavities through spin coating or inkjet printing, eliminating the need for CMP.
The formulation allows for cost-effective, crack-free, and dense optical layer production, suitable for continuous inkjet printing, with improved gap filling and reduced viscosity, enhancing manufacturing efficiency and reducing costs.
Smart Images

Figure 2026539079000011 
Figure 2026539079000012 
Figure 2026539079000013
Abstract
Description
Field of Invention
[0001] The present invention relates to formulations for preparing an optical layer containing a metal oxide, a method for preparing the formulation, the use of the formulation, a method for preparing a composite, the composite, an optical device, and a display device. [Background technology]
[0002] State-of-the-art optical devices typically include optical gratings fabricated from composite materials, having a substrate as a support and a complex interlaced pattern on it, where the pattern consists of different layers or stacks of layers. Creating such complex interlaced patterns usually requires a structuring process, which becomes increasingly difficult as the size of the prepared structural dimensions decreases.
[0003] In addition to its wide range of potential uses in various application fields, such as spectrometers or optical storage systems (CDs, DVDs, etc.), diffraction gratings are a core component of so-called XR devices, usually in the form of glasses. In this context, R represents the term reality, and X represents different attributes, such as virtual, augmented, or mixed reality. Thus, diffraction gratings form a core part of the so-called optical engine in XR devices, particularly in augmented and mixed reality glasses. Virtual reality glasses, when constructed as head-mounted displays, often consist of conventional liquid crystal (LC) organic light-emitting diode (OLED) displays embedded directly in the device in front of the user's eyes, and therefore do not necessarily require diffraction gratings. In contrast, augmented and mixed reality glasses are designed to allow consumers to obtain a visual impression of their environment in the best possible way, as if they were not wearing glasses at all. However, they also enable the provision and delivery of digital information, and even the projection of it into the individual's field of vision. Further digital information is collected by recognizing and analyzing the environment that the individual is observing or fixating on. To transmit and project assisted digital information to an individual's eyes, augmented or mixed reality glasses include an information supply unit coupled to an optical waveguide system, through which optically encoded assisted information is transmitted directly to the lenses of the glasses. Here, the information passes through a diffraction grating, which couples the incident light to the lens and, by diffraction, splits it according to its angular information and spectral band. After the light is captured, the lens acts as a waveguide, enabling the transmission of the light to the individual's pupil. The position of light capture is independent of any preferred position and is therefore independent of the influence of technical necessity. The transverse direction of the light within the lens is determined by the diffraction grating that diffracts or splits the light. At specific locations on the lens, second and third diffraction gratings function to change the transverse direction of the light, thereby projecting the light into the user's pupil. The transverse direction of the light within the glass is achieved by total internal reflection (TIR), and therefore the light bounces several times between glass interfaces until it reaches another diffraction grating that changes the internal TIR direction of the light (see Figure 2).The second and third gratings can be aligned geometrically in different directions from the first capture grating, for example, by a specific angular distortion of the longitudinal axis, and thus the direction of propagation of totally reflected light can be altered. Needless to say, the lens itself or the material from which the lens is made must not be absorptive. Otherwise, the supporting information will not reach the user's pupil, or will only reach it with a greatly reduced light intensity. The process works regardless of the use of reflective or transmissive gratings. Typically, lenses have both types of gratings to properly guide light. It should also be mentioned that there are differences in the optical performance of reflective and transmissive gratings, but these are of no further concern in the context of this invention. The basic structures of the gratings are very similar, and these are more important at this point.
[0004] Nevertheless, different designs and structures exist for realizing waveguides, such as surface relief (SR) or volume phase holographic (VPH) gratings. Both types are very similar in appearance. In the simplest case, the grating is attached to the surface of the waveguide material, in this case the lens. The grating itself consists of an array of fine structures, many of which are trenches of a first material type Material 01 with refractive index RI 01, but are not limited to these. The geometric shape of the trenches can vary from rectangular to V-shaped trenches, U-shaped, and so on. The width, including structures of different widths, the geometric shape of the trenches, the pitch, and the depth, including different depths, are specifically designed to affect the diffraction pattern of the incident light being diffracted.
[0005] In the case of a VPH grating, a trench or structure of a first material type (Material 01) having a refractive index (RI 01) is filled with a second material type (Material 02) having a refractive index (RI 02), where RI 02 is progressively different from RI 01 (see Figures 1 and 3). For completeness, it should be noted that Material 01 or Material 02 may consist of a stack of structured layers stacked on top of each other, each containing different material compositions with different refractive indices, thereby forming Material 01 or Material 02 having effective or gradient refractive indices RI 01 or RI 02, respectively. Note that the (effective or gradient) refractive indices RI 01 and RI 02 depend on the refractive index of the waveguide or lens from which the glass is fabricated. When a glass lens with a high refractive index (n03 > 1.46) is used, the (effective or gradient) refractive indices of Material 01 and Material 02 are considered to be higher than the refractive index of the lens itself, thereby reaching and exceeding an RI value of 2.0. Surface relief (SR) grids may have a similar appearance and may contain a second type of material as a trench filler, although the trenches may also be simply air. High-performance grids, particularly VPH type grids, may be manufactured using standard lithography and deposition techniques known from microfabrication, e.g., the manufacture of integrated circuits.
[0006] Such standard techniques typically involve physical vapor deposition (PVD) or chemical vapor deposition (CVD) processes and often suffer from incomplete gap filling due to undesirable deposition and / or layer growth characteristics, including increased deposition and / or growth rates at corners and edges. Such incomplete gap filling creates voids within the structure filled by the PVD and CVD material. In addition to void formation, the substrate surface is covered by a PVD and / or CVD layer approximately the same thickness as the maximum depth of the deepest structure filled by the deposited gap-filling material (see Figures 4 and 5). However, in some applications, it may be necessary to expose the substrate surface for use in further processing. As a result, the unwanted overburden layer from PVD or CVD needs to be removed without damaging the original substrate surface underneath, for example, by chemical mechanical planarization (CMP). While CMP is very well established in integrated circuit manufacturing, it is a time-consuming and expensive process and can be seen as a potential economic drawback in the mass production of state-of-the-art optical devices, particularly diffraction gratings. Therefore, it is desirable to have a solution for the advanced and cost-effective manufacturing of optical gratings that does not require CMP for gap filling (see Figure 6).
[0007] Therefore, more cost-effective production technologies are needed that enable lower ownership costs. [Overview of the Initiative]
[0008] The inventors have newly discovered that one or more significant problems that require improvement still exist, as listed below: To provide a printable formulation for preparing optical layers / composites containing a material that provides a sufficiently high refractive index after curing; to provide a formulation for producing optical layers that enable the preparation of dense, crackless or crack-free optical layers and enable the filling of cavities, trenches or gaps after curing; To provide a formulation for preparing an optical layer containing a metal oxide precursor material of a high refractive index that is well dispersed in the formulation; a simpler and / or more cost-effective method for preparing an optical layer / composite using the formulation; to achieve a more stable formulation, zero or reduced viscosity change of the formulation, to provide a formulation suitable for wet printing, i.e., spin coating or ink jetting, and to enable continuous inkjet printing.
[0009] The present inventors aimed to solve one or more of the above problems.
[0010] And, surprisingly, the inventors have found that one or more of the above-mentioned technical problems can be solved by features as defined in the claims.
[0011] That is, a novel formulation for preparing an optical layer containing a metal oxide, preferably for preparing a composite, more preferably for preparing a layered composite, wherein at least; - A metal oxide precursor comprising Group 4 and / or Group 5 elements of the periodic table, preferably the metal oxide precursor being a metal alkoxide, metal halide, or metal carboxylate comprising Group 4 and / or Group 5 elements of the periodic table, and more preferably the metal oxide precursor being a metal alkoxide comprising Group 4 and / or Group 5 elements of the periodic table; - Optionally, an acid selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides, and carboxylic acids; and - a solvent, wherein the solvent is a secondary alcohol having one or two alkoxy groups or one or two alkyl groups, wherein one or more non-adjacent groups of the alkyl group are replaced by an oxygen atom, or a secondary linear or branched ≥C3 alcohol, preferably selected from one or more members of 2-propanol, 2-butanol, 2-pentanol and 3-pentanol, preferably a secondary linear or branched ≥C4 alcohol; preferably, the solvent is a solvent selected from propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, glycerol 1,3-dialkyl ether, or a combination of propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether and glycerol 1,3-dialkyl ether comprising, - the total amount of the metal oxide precursor in the formulation is in the range of 0.1 to 40 wt%, preferably 1 to 35 wt%, more preferably 2 to 30 wt%, even more preferably 3 to 28 wt%, based on the total amount of the formulation, a novel formulation is found.
[0012] In another aspect, the present invention further comprises at least the following steps; (X1) a step of dissolving a metal oxide precursor in solvent 1 to form a metal oxide precursor solution, preferably wherein said solvent 1 is a dry or anhydrous solvent; (X2) optionally, a step of dissolving an acid in solvent 2 to form an acid solution, preferably wherein said solvent 2 is dry or anhydrous, and said acid is selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides and carboxylic acids; (X3) optionally, a step of adding said acid solution obtained in step (X2) to the metal oxide precursor solution obtained in step (X1); (X4) a step of mixing water and solvent 3 to form an aqueous solvent; and (X5) a step of adding said aqueous solvent to the alkoxide solution obtained in step (X1) or the metal oxide precursor solution obtained in step (X3); (X6) optionally, a step of dissolving an acid and water in solvent 4 to form an acid solution to form an aqueous acid solution, preferably said solvent 4 is a dry or anhydrous solvent, and said acid is selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides and carboxylic acids; (X7) optionally, the step of adding said aqueous acid solution (X6) to the metal oxide precursor solution (X1) , wherein said solvents 1 to 4 are, independently of each other, propylene glycol monoalkyl ether, which is preferably propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether and / or propylene glycol monopropyl ether; glycerol 1,3-dialkyl ether, 1,3-dimethoxy-2-propanol; secondary linear or branched ≥C3 alcohol, which is preferably 2-propanol, 2-butanol, 2-pentanol, 3-pentanol, more preferably a linear or branched secondary ≥C4 alcohol; selected from one or more members selected from the group consisting of, preferably, said solvent is selected from propylene glycol monoalkyl ether and glycerol 1,3-dialkyl ether, the present invention relates to a method for preparing the formulation of the present invention.
[0013] In another aspect, the present invention also relates to the use of the formulation of the present invention for preparing an optical layer comprising a metal oxide, preferably for preparing a composite, more preferably for preparing a layered composite.
[0014] In another aspect, the present invention further relates to a method for preparing a composite comprising a metal oxide, preferably, said metal oxide is selected from metal monoxide, metal dioxide and metal pentoxide, or combinations thereof; the following steps (a) and (b): (a) providing the formulation of the present invention to the surface of a substrate, preferably by a wet deposition process, more preferably by spin coating or area-selective printing, preferably by area-selective printing wherein said area-selective printing is inkjet, even more preferably by inkjet; and (b) A step of applying heat treatment to the preparation provided on the surface of the substrate to convert at least a portion of the metal oxide precursor in the preparation into a metal oxide. Regarding methods including
[0015] Preferably, the composite is a layered composite, and more preferably, the layered composite is an optical layer.
[0016] In another aspect, the present invention further relates to a composite, preferably a layered composite, which is obtained or can be obtained by the method of the present invention, and preferably the layered composite is an optical layer.
[0017] In another aspect, the present invention further relates to a composite, preferably a layered composite, derived from the formulation of the present invention, wherein the layered composite is an optical layer.
[0018] In another aspect, the present invention further relates to an optical device comprising the composite of the present invention and a substrate having a patterned or non-uniform surface. Preferably, gaps or trenches in the patterned or non-uniform surface of the substrate are at least partially filled with the composite.
[0019] Preferably, the substrate is a patterned substrate having topographic features on its surface. Preferably, the composite fills at least some of the gaps between the topographic features, and more preferably, the composite fills trenches in the patterned substrate.
[0020] In another aspect, the present invention further relates to a display device comprising: at least one functional medium configured to direct and modulate light, or to emit light; and a composite of the present invention. Technical effects of the invention
[0021] The present invention provides one or more of the following effects: To provide a printable formulation for preparing optical layers / composites containing a material that provides a sufficiently high refractive index after curing; to provide a formulation that enables the preparation of dense, crackless or crack-free optical layers and allows for defect-free filling of cavities, trenches, or gaps after curing; To provide a formulation for preparing an optical layer containing a metal oxide precursor material of a high refractive index that disperses well in the formulation; to provide a simpler and / or more cost-effective method for preparing an optical layer / composite using the formulation; to achieve a more stable formulation; to provide a formulation with zero or reduced viscosity change; to provide a formulation suitable for wet printing, i.e., spin coating or ink jetting; and to enable continuous inkjet printing.
[0022] Preferred embodiments of the present invention are described below and in dependent claims. [Brief explanation of the drawing]
[0023] [Figure 1] This is a schematic cross-sectional view of a VPH lattice having Material 01 and Material 02, where the refractive index IR01 of Material 01 is progressively different from the refractive index IR02 of Material 02. [Figure 2] This is a schematic cross-sectional view of a VPH grating that enables the diffraction (in the case of transmission) of light, including the propagation of diffracted light within a waveguide (e.g., a lens) due to total internal reflection. [Figure 3] This is a schematic cross-sectional view of a VPH lattice with trenches filled with a high refractive index material (Material 02), where the refractive index of Material 02 gradually differs from that of Material 01 on either side of the trenches. [Figure 4] This is a schematic diagram of a gap filling process via PVD or CVD and the removal of unwanted overburden. [Figure 5] This is a schematic diagram of a void-filling process via PVD or CVD that creates and leaves voids within interstitial spaces and sedimentary layers. [Figure 6]This is a schematic diagram of a gap-filling process using a formulation containing the metal complex or formulation of the present invention that has been converted to a metal oxide. [Figure 7a] The TEM image of the Zr-2 sample is shown. [Figure 7b] The TEM image of sample Zr-3 is shown. Detailed description of the invention
[0024] List of reference symbols 1. Material 02 having RI 02 2. Material 01 having RI 01 3. Substrate (e.g., glass) 4. Diffraction of incident light represented by a broad arrow. 5. Total Internal Reflection (TIR) 6. Waveguides 7. Structured layer stack with gaps (trenches) 8. Substrate (e.g., glass or silicon) 9. Material overburden (e.g., high refractive index materials or high etching resistance materials) 10. Materials that provide gap filling (e.g., high refractive index materials or high etching resistance materials) 11.Void 12. Formulations of high refractive index materials (e.g., metal oxide precursors) (e.g., inks) 13. High refractive index materials (e.g., metal oxides) that provide gap filling with an arbitrarily selected concave shape. 14. Overbaden layer (optional) 15. Energy
[0025] Definition of Terms In the context of the present invention, the terms “formulation medium” or the plural “formulation media” as used herein refer to one or more compounds that function as a solvent, suspension, carrier, and / or matrix for the metal oxide precursor compound and any other components contained in the formulation. The formulation medium is generally an inert compound that does not react with the metal oxide precursor compound and the other components. The formulation medium may be a liquid compound, a solid compound, or a mixture thereof. Typically, the formulation medium is an organic compound.
[0026] The term "surfactant" used here refers to an additive that reduces the surface tension of a given formulation.
[0027] The term "wetting and dispersing agent" used here refers to an additive that enhances the spreadability and filling properties of a given formulation. In this way, the tendency of molecules to adhere to one another is reduced.
[0028] The term "adhesion promoter" used here refers to an additive that enhances the adhesion of a given mixture.
[0029] The term "polymer matrix" as used herein refers to an additive that acts as a polymer matrix for one or more components of a given formulation.
[0030] As used herein, the term “optical device” refers to a device comprising one or more optical components for forming a light beam, including but not limited to gratings, lenses, prisms, mirrors, optical windows, filters, polarizing optics, UV and IR optics, waveguides, and optical coatings. In the context of the present invention, preferred optical devices are waveguides for augmented reality (AR) devices, virtual reality (VR) devices, and / or mixed reality (MR) devices, or preferred optical devices are augmented reality (AR) glasses, virtual reality (VR) glasses, and / or mixed reality (MR) glasses.
[0031] As used herein, the term "display device" refers to a type of optical device configured to output / present information in a visual or tactile form. Examples include liquid crystal displays (LCDs), light-emitting diode displays (LEDs), organic light-emitting displays (OLEDs), micro-LED displays, quantum dot displays (QLEDs), augmented reality (AR) displays, virtual reality (VR) displays, mixed reality (MR) displays, plasma display (PDP) displays, and electroluminescent (ELD) displays. Preferred optical devices in the context of this invention are AR displays, VR displays, or MR displays.
[0032] Detailed description of the invention The present invention relates to a formulation for preparing an optical layer containing a metal oxide, preferably for preparing a composite, more preferably for preparing a layered composite, and at least; - A metal oxide precursor comprising Group 4 and / or Group 5 elements of the periodic table, preferably the metal oxide precursor being a metal alkoxide, metal halide, or metal carboxylate comprising Group 4 and / or Group 5 elements of the periodic table, and more preferably the metal oxide precursor being a metal alkoxide comprising Group 4 and / or Group 5 elements of the periodic table; - Optionally, an acid selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides, and carboxylic acids; and - A solvent, wherein the solvent is a secondary alcohol having one or two alkoxy groups or one or two alkyl groups, wherein one or more non-adjacent groups of the alkyl group are replaced by oxygen atoms, or a secondary linear or branched ≥ C3 alcohol, preferably selected from one or more members of 2-propanol, 2-butanol, 2-pentanol, and 3-pentanol, preferably a secondary linear or branched ≥ C4 alcohol; preferably, the solvent comprises, essentially comprises, or consists of a solvent selected from propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, glycerol 1,3-dialkyl ether, or a combination of propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, and glycerol 1,3-dialkyl ether. - The present invention relates to a formulation in which the total amount of metal oxide precursors in the formulation is in the range of 0.1 to 40% by weight, preferably 1 to 35% by weight, more preferably 2 to 30% by weight, and even more preferably 3 to 28% by weight, based on the total amount of the formulation.
[0033] - Metal oxide precursors According to the present invention, the metal oxide precursor comprises elements of Group 4 and / or Group 5 of the periodic table, preferably a metal alkoxide, metal halide, or metal carboxylate containing elements of Group 4 and / or Group 5 of the periodic table, and more preferably a metal alkoxide containing elements of Group 4 and / or Group 5 of the periodic table.
[0034] Any known metal oxide precursor can be used as the metal oxide precursor.
[0035] - Metal alkoxides According to the present invention, a metal alkoxide containing Group 4 and / or Group 5 elements of the periodic table is used. As the metal alkoxide, a commercially available metal alkoxide containing Group 4 and / or Group 5 elements of the periodic table can be used.
[0036] Preferably, titanium tetra-n-butoxide, zirconium tetra-n-butoxide, or niobium pentaethoxide can be used.
[0037] In a preferred embodiment of the present invention, the metal oxide precursor (preferably a metal alkoxide) is represented by the following chemical formula (IV) or formula (V): M b1 O(R b1 R b2 R b3 R b4 )4-(IV) M b2 O(R b1 R b2 R b3 R b4 R b5 )5-(V) (In the formula, M b1 is a tetravalent metal of Group 4 elements of the periodic table, preferably Ti or Zr; M b2 is a pentavalent metal of Group 5 elements of the periodic table, preferably Nb or Ta; R b1 , R b2 , R b3 , R b4 and R b5 are each independently selected from: H, D, a linear alkyl group having 1 to 25 carbon atoms, preferably 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms; a branched or cyclic alkyl group having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; an aryl group having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; a linear alkyl-cycloalkyl group having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; a branched alkyl-cycloalkyl group having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; a linear alkyl-aryl group having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; a branched alkyl-aryl group having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; One or more non-adjacent CH2 groups and / or one or more adjacent CH2 groups of the above group may be replaced by oxygen atoms, and one or more H atoms may be replaced by D or NO2; Each of the groups contains one or more groups R a It may be replaced with; R a Each of the above groups is, identically or differently in its appearance, a linear alkyl or alkoxy group having H, D, 1 to 15 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms; a branched or cyclic alkyl or alkoxy group having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; a linear alkenyl or alkynyl group having 2 to 15 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 5 carbon atoms; a branched alkenyl or alkynyl group having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; an aromatic or heteroaromatic ring system having 5 to 15 aromatic ring atoms, preferably 5 to 10 aromatic ring atoms; in each of the above groups, one or more H atoms may be replaced by D, where two or more adjacent substituents R a These can be represented by (which may optionally form monocyclic or polycyclic aliphatic ring systems with each other).
[0038] According to the present invention, the total amount of metal oxide precursors in the formulation is in the range of 0.1 to 40% by weight based on the total amount of the formulation, preferably 1 to 35% by weight, more preferably 2 to 30% by weight, and even more preferably 3 to 28% by weight.
[0039] The total amount of metal oxide precursors based on the total amount of the formulation is considered to be very important for achieving improved gap filling or for fabricating thin layers that are placed directly on a patterned or non-uniform surface of a substrate / underlying layer. When a thin layer is fabricated directly on a patterned or non-uniform surface of a substrate, or on a patterned or non-uniform surface of an underlying layer, it is desirable that the bumps, trenches, and grooves of the patterned surface and / or non-uniform structure are filled with air, and that the thin layer is positioned to cover the air-filled patterned bumps, trenches, and grooves. It is considered that improved gap filling or good thin layers can be preferably fabricated by adjusting the total amount of metal oxide precursors in the formulation. That is, to improve gap filling (filling of gaps between trenches, bumps, and grooves) of patterned surfaces and non-uniform structures, it is desirable to reduce the amount of metal oxide precursors in order to achieve a lower condensation rate. A preferred low amount of metal oxide precursor for achieving improved gap filling is, for example, in the range of 0.1 to 15% by weight based on the total amount of the formulation, more preferably in the range of 1 to 10% by weight based on the total amount of the formulation, and even more preferably in the range of 2 to 8% by weight.
[0040] According to the present invention, the nominal relative weight content of metal oxides in the formulation of the present invention is theoretically in the range of 0.1 to 15% by weight, preferably 0.2 to 10% by weight, more preferably 0.5 to 5% by weight, and even more preferably 0.7 to 4% by weight, based on the total amount of the complex.
[0041] According to the present invention, the nominal relative weight content of the metal oxide in the preparation is calculated using the following formula: M(OR)x and MOx(w%) in the total amount of the preparation = the general formulas (MO2 and M2O5) of metal alkoxides and metal oxides, and their nominal relative weight content in the preparation (sol-gel mixture).
[0042] - Solvent According to the present invention, the preparation of the present invention comprises a solvent, the solvent being a secondary alcohol having one or two alkoxy groups or one or two alkyl groups, wherein one or more non-adjacent groups of the alkyl group are replaced by oxygen atoms.
[0043] The secondary alcohol solvent is thought to chemically interact with the metal oxide precursor in the formulation, allowing for control over the formation rate of the continuous metal oxide material during the deposition and final thermal curing processes of the formulation.
[0044] Preferably, the alkoxy group of the secondary alcohol is an alkoxy group having 1 to 10 carbon atoms, more preferably an alkoxy group having 1 to 5 carbon atoms, and even more preferably an alkoxy group having 1 to 3 carbon atoms.
[0045] Preferably, the alkyl group in which one or more non-adjacent groups of the alkyl group are replaced by oxygen atoms is an alkyl group having 1 to 10 carbon atoms, more preferably 2 to 5 carbon atoms, and even more preferably 2 or 3 carbon atoms, in which one or more non-adjacent carbon groups of the alkyl group are replaced by oxygen atoms.
[0046] More preferably, the solvent is a propylene glycol monoalkyl ether, which is preferably propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether and / or propylene glycol monopropyl ether; selected from one or more members of the group consisting of glycerol 1,3-dialkyl ether and 1,3-dimethoxy-2-propanol; more preferably, the solvent is selected from propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether and secondary linear or branched ≥C3 alcohols, preferably selected from 2-propanol, 2-butanol, 2-pentanol, and 3-pentanol, more preferably a linear or branched secondary ≥C4 alcohol; preferably, the solvent is selected from propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether and glycerol 1,3-dialkyl ether.
[0047] Printing structures, particularly inkjet printing, is considered a cost-effective manufacturing process. Spin coating is a simple method and is preferred for forming uniform thin layers. Therefore, solvent formulations suitable for spin coating / inkjet printing of structures, or for filling cavities and structures, are described here.
[0048] It is believed that the formation rate of continuous metal oxide materials during formulation deposition and final thermal curing can be controlled by selecting a solvent from among chemically closely related secondary alcohols for reactive sol-gel mixtures containing Group 4 and / or Group 5 elements of the periodic table formed from metal alkoxides.
[0049] After the printing, deposition, and filling of the structure, at least a portion of the material as a metal oxide precursor needs to be converted to the respective metal oxide by any known means (thermal, photochemical, etc.) that are known to those skilled in the art.
[0050] - Acid According to the present invention, the formulation may optionally contain an acid selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides, and carboxylic acids. The acid is thought to be able to function as a reaction mediator.
[0051] In a preferred embodiment of the present invention, the preparation comprises an acid selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides, and carboxylic acids.
[0052] These acids are considered suitable as reaction mediators according to the present invention.
[0053] In a more preferred embodiment of the present invention, the sulfonic acid is of the following chemical formula (I) R a1 SO3H - (I) (In the formula, R a1 This is selected from the group consisting of: linear alkyl groups having 1 to 25 carbon atoms, preferably 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms; branched or cyclic alkyl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; aryl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; linear alkyl-cycloalkyl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; branched alkyl-cycloalkyl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; linear alkyl-aryl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; and branched alkyl-aryl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms. One or more non-adjacent CH2 groups of the above groups may be replaced with an oxygen atom, C=O, C=S, C=Se, C=NH, SiH2, SO, SO2, OS, or CONH, and one or more H atoms may be replaced with D, F, Cl, Br, I, CN, or NO2; Each of the groups contains one or more groups R ax It may be replaced with; R ax In each occurrence, these are identical or different linear alkyl or alkoxy groups having H, D, 1 to 15 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms; branched or cyclic alkyl or alkoxy groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; linear alkenyl or alkynyl groups having 2 to 15 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 5 carbon atoms; branched alkenyl or alkynyl groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; aromatic or heteroaromatic ring systems having 5 to 15 aromatic ring atoms, preferably 5 to 10 aromatic ring atoms; in each of the above groups, one or more H atoms may be replaced with D, F, Cl, Br, or I, where two or more adjacent substituents R ax These can be represented by (which may optionally form monocyclic or polycyclic aliphatic ring systems with each other), The aforementioned amine hydrochloride is given by the following chemical formula (II) HCl·R a2 -(II) (In the formula, R a2 (is represented by a selection from the group consisting of N2H4, ammonia, hydroxylamine, imidazole and 1,4-diazabicyclo[2.2.2]octane); and / or The carboxylic acid is given by the following chemical formula (III) R a3 -COOH (In the formula, R a3This is selected from the group consisting of: linear alkyl groups having 1 to 25 carbon atoms, preferably 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms; branched or cyclic alkyl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; aryl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; linear alkyl-cycloalkyl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; branched alkyl-cycloalkyl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; linear alkyl-aryl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; and branched alkyl-aryl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms. One or more non-adjacent CH2 groups of the above groups may be replaced with an oxygen atom, C=O, C=S, C=Se, C=NH, SiH2, SO, SO2, OS, or CONH, and one or more H atoms may be replaced with D, F, Cl, Br, I, CN, or NO2; Each of the groups contains one or more groups R ax It may be replaced with; R ax In each occurrence, these are identical or different linear alkyl or alkoxy groups having H, D, 1 to 15 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms; branched or cyclic alkyl or alkoxy groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; linear alkenyl or alkynyl groups having 2 to 15 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 5 carbon atoms; branched alkenyl or alkynyl groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; aromatic or heteroaromatic ring systems having 5 to 15 aromatic ring atoms, preferably 5 to 10 aromatic ring atoms; in each of the above groups, one or more H atoms may be replaced with D, F, Cl, Br, or I, where two or more adjacent substituents R axThese can be represented by (which may optionally form monocyclic or polycyclic aliphatic ring systems with each other).
[0054] In some preferred embodiments, the acid is of the following chemical formula (II) HCl·R a2 -(II) (In the formula, R a2 It is an amine hydrochloride represented by (selected from the group consisting of N2H4, ammonia, hydroxylamine, imidazole, and 1,4-diazabicyclo[2.2.2]octane).
[0055] In a preferred embodiment, the acid is a sulfonic acid represented by the following chemical formula (I). R a1 SO3H - (I) (In the formula, R a1 This is selected from the group consisting of: linear alkyl groups having 1 to 25 carbon atoms, preferably 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms; branched or cyclic alkyl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; aryl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; linear alkyl-cycloalkyl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; branched alkyl-cycloalkyl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; linear alkyl-aryl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; and branched alkyl-aryl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms. One or more non-adjacent CH2 groups of the above groups may be replaced with an oxygen atom, C=O, C=S, C=Se, C=NH, SiH2, SO, SO2, OS, or CONH, and one or more H atoms may be replaced with D, F, Cl, Br, I, CN, or NO2; Each of the groups contains one or more groups R ax It may be replaced with; R ax In each occurrence, these are identical or different linear alkyl or alkoxy groups having H, D, 1 to 15 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms; branched or cyclic alkyl or alkoxy groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; linear alkenyl or alkynyl groups having 2 to 15 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 5 carbon atoms; branched alkenyl or alkynyl groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; aromatic or heteroaromatic ring systems having 5 to 15 aromatic ring atoms, preferably 5 to 10 aromatic ring atoms; in each of the above groups, one or more H atoms may be replaced with D, F, Cl, Br, or I, where two or more adjacent substituents R ax These elements may optionally form monocyclic or polycyclic aliphatic ring systems with each other. In a preferred embodiment of the present invention, the stoichiometric molar ratio of the acid to the metal oxide precursor, preferably the metal alkoxide, is in the range of 0.01:100 to 120:100, and preferably the relative molar amount of the acid based on the total amount of the metal oxide precursor is in the range of 0.1 to 50, more preferably 1 to 10.
[0056] When the stoichiometric molar ratio of the acid to the metal oxide precursor falls within the above range, it is believed that film stability, gap-filling properties, and / or refractive index values are improved.
[0057] - water According to the present invention, the preparation contains water, and the stoichiometric amount of water is in the range of 100 to 400 mol% based on the total amount of metal oxide precursors, preferably in the range of 150 to 300 mol%, and more preferably in the range of 180 to 270 mol% based on the total amount of metal oxide precursors.
[0058] - Additives In some embodiments of the present invention, the formulation may optionally contain one or more additives selected from surfactants, wetting agents and dispersants, adhesion promoters, and polymer matrices. Alternatively, in some embodiments, the formulation of the present invention does not contain any additives.
[0059] In some embodiments of the present invention, the formulation may further contain one or more additional metal complexes that may act as further metal oxide precursors.
[0060] The total content of metal oxide precursors in the formulation is preferably in the range of 0.1% to 50% (w / w), more preferably 0.5% to 40% (w / w), and more preferably 1% to 30% (w / w), based on the total mass of the formulation.
[0061] In a preferred embodiment of the present invention, the formulation is an ink formulation suitable for inkjet printing. Typical requirements for the ink formulation are a surface tension in the range of 20 mN / m to 30 mN / m and a viscosity in the range of 5 mPa·s to 30 mPa·s.
[0062] - Method for preparing a compound In another aspect, the present invention also involves at least the following steps; (X1) A step of dissolving a metal oxide precursor in solvent 1 to form a metal oxide precursor solution, wherein the solvent 1 is preferably dry or anhydrous; (X2) Optionally, a step of dissolving an acid in solvent 2 to form an acid solution, preferably the solvent 2 being dry or anhydrous, and the acid being selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides, and carboxylic acids; (X3) Optionally, adding the acid solution obtained in step (X2) to the metal oxide precursor solution obtained in step (X1); (X4) A step of mixing water and solvent 3 to form an aqueous solvent; and (X5) A step of adding the aqueous solvent obtained in step (X4) to the alkoxide solution obtained in step (X1) or the metal oxide precursor solution obtained in step (X3); (X6) Optionally, a step of dissolving an acid and water in solvent 4 to form an acid solution and then forming an aqueous acid solution, preferably wherein the solvent 4 is dry or anhydrous, and the acid is selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides, and carboxylic acids; (X7) Optionally, adding the acid aqueous solution (X6) to the metal oxide precursor solution (X1). The present invention relates to a method for preparing formulations of the present invention, comprising, essentially, or consisting of, wherein the solvents 1 to 4 are independently of each other, propylene glycol monoalkyl ether, preferably propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether and / or propylene glycol monopropyl ether; glycerol 1,3-dialkyl ether, 1,3-dimethoxy-2-propanol, and more preferably the solvent is propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, glycerol 1,3-dialkyl ether; secondary linear or branched ≥C3 alcohol, preferably 2-propanol, 2-butanol, 2-pentanol, 3-pentanol, and more preferably linear or branched secondary ≥C4 alcohol, and more preferably the solvent is selected from propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, glycerol 1,3-dialkyl ether.
[0063] Preferably, the total amount of metal oxide precursor added in step (X1) is set in the range of 0.1 to 40% by weight based on the total amount of the resulting formulation, preferably in the range of 1 to 35% by weight, more preferably 2 to 30% by weight, and even more preferably 3 to 28% by weight.
[0064] Preferably, the metal oxide precursor is a metal alkoxide, metal halide, or metal carboxylate containing a Group 4 and / or Group 5 element of the periodic table, and more preferably, the metal oxide precursor is a metal alkoxide containing a Group 4 and / or Group 5 element of the periodic table.
[0065] - use In another aspect, the present invention also relates to the use of the formulations of the present invention for preparing optical layers containing metal oxides, preferably for preparing composites, and more preferably for preparing layered composites. The present invention may also relate to the use of the formulations of the present invention for preparing encapsulation layers for electronic devices.
[0066] - Method for preparing composites containing metal oxides In another aspect, the present invention also relates to a method for preparing a composite comprising a metal oxide, preferably the metal oxide being selected from a metal monooxide, a metal dioxide, or a metal pentaoxide, or a combination thereof; and at least the following steps (a) and (b): (a) A step of providing the formulation of the present invention to the surface of a substrate or the surface of an underlying layer disposed on the substrate, preferably by a wet deposition process, more preferably by spin coating or ink spraying, and even more preferably by ink spraying; and (b) A step of applying heat treatment to the surface of the substrate or the surface of an underlying layer placed on the substrate to convert at least a portion of the metal oxide precursor in the preparation into a metal oxide. Regarding methods including
[0067] Preferably, the composite is a layered composite, and more preferably, the layered composite is an optical layer or a sealing layer.
[0068] - Process (a) According to the present invention, the formulation may preferably be provided to the surface of a substrate or a sublayer by a wet deposition process. The wet deposition process is drop casting, coating, or printing. More preferred coating methods are spin coating, spray coating, slit coating, or slot die coating. More preferred printing methods are flexographic printing, gravure printing, inkjet printing, EHD printing, offset printing, or screen printing. Even more preferred printing methods are spray coating and inkjet printing, with inkjet printing being the most preferred.
[0069] Therefore, in a preferred embodiment, the formulation is applied to the surface of the substrate or the underlying layer in step (a) by spin coating or ink spraying. From a cost-effective viewpoint, ink spraying can be preferably used.
[0070] In a preferred embodiment of the present invention, the formulation provided in step (a) of the method is an ink formulation suitable for inkjet printing. Typical requirements for the ink formulation are a surface tension in the range of 20 mN / m to 30 mN / m and a viscosity in the range of 5 mPa·s to 30 mPa·s.
[0071] Depending on the specific problem to be solved, the formulation may need to be deposited as a homogeneous, dense thin layer covering the entire surface of the substrate or the entire surface of the underlying layer by a coating method, or the formulation may need to be deposited locally in a structured manner, thus requiring a printing method. In both coating and printing methods, the formulation must be formulated in an appropriate manner to suit the physicochemical requirements of the respective coating and printing methods, as well as to suit the specific requirements of the surface of the substrate to be coated or printed.
[0072] In a preferred embodiment of the method of the present invention, the surface of the substrate is pretreated by a surface cleaning process. Preferred surface cleaning processes include silicon wafer cleaning processes, e.g., W. Kern, The Evolution of Silicon Wafer Cleaning Technology, J. Electrochem. Soc., Vol. 137, 6, 1990, 1887-1892 and in New Process Technologies for Microelectronics, RCA Review 1970, 31, 2, 185-454. Such silicon wafer cleaning processes include wet cleaning processes containing a cleaning solvent (e.g., isopropanol (IPA)); wet etching processes containing hydrogen peroxide solutions (e.g., piranha solutions, SC1 and SC2), choline solutions, or HF solutions; dry etching processes containing chemical vapor etching, UV / ozone treatment, or glow discharge techniques (e.g., O2 plasma etching); and mechanical processes containing brush scrubbing, fluid jets, or ultrasonic techniques (ultrasonic treatment). The surface of the substrate may also be pretreated by a chlorination or atomic layer deposition (ALD) process. Surface pretreatment of the substrate plays a role in correcting the hydrophobicity / hydrophilicity of the surface. This can improve the adhesion and filling properties of the optical metal oxide layer on the substrate surface.
[0073] In a more preferred embodiment, a wet cleaning process comprising a cleaning solvent (e.g., isopropanol (IPA)) is combined with one or more wet etching processes comprising hydrogen peroxide solutions (e.g., piranha solutions, SC1 and SC2), choline solutions, or HF solutions; dry etching processes comprising chemical vapor etching, UV / ozone treatment, or glow discharge techniques (e.g., O2 plasma etching); and mechanical processes comprising brush scrubbing, fluid jets, or ultrasonic techniques (ultrasonic treatment).
[0074] In the most preferred embodiment, a wet cleaning process comprising a cleaning solvent (e.g., isopropanol (IPA)) is combined with a mechanical process comprising brush scrubbing, fluid jetting, or ultrasonic technology (ultrasonic treatment), and a wet etching process comprising a hydrogen peroxide solution (e.g., piranha solution, SC1 and SC2), a choline solution, or an HF solution.
[0075] Therefore, in a preferred embodiment, in step (a), the formulation is applied to the surface of the substrate or the surface of the underlying layer by spin coating or ink spraying.
[0076] In a preferred embodiment, the formulation is converted at least partially into a composite on the surface of the substrate or the surface of the underlying layer, the composite preferably comprising a metal oxide selected from metal monooxides, metal dioxides and / or metal pentaoxides; and a metal oxide precursor.
[0077] In a preferred embodiment, the substrate is a patterned substrate having topographic features on its surface. The patterned structure of the substrate may be an underlying layer (e.g., an underlying layer of a semiconductor device) placed on the substrate.
[0078] - Process (b) The formulation is thought to be converted at least partially to a metal oxide on the surface of the substrate or the underlying layer in step (b), and to form a composite upon exposure to heat treatment. The composite is preferably a layered composite. The solvent is usually removed in step (b).
[0079] A preferred heat treatment involves exposure to high temperatures of 50 to 600°C, preferably 80 to 500°C, and more preferably 100 to 300°C. For example, it is believed that improved gap filling can be achieved by applying higher temperatures in the range of 100 to 600°C, preferably 125 to 450°C, and more preferably 150 to 250°C.
[0080] To achieve improved gap filling, in step (a), a formulation is used that contains a smaller amount of metal oxide precursor based on the total amount of the formulation, for example, in the range of 0.1 to 15% by weight based on the total amount of the formulation, more preferably in the range of 1 to 10% by weight based on the total amount of the formulation, and even more preferably in the range of 2 to 8% by weight based on the total amount of the formulation. In step (b), to achieve improved gap filling, it is preferable to apply a higher temperature, for example, in the range of 100 to 600°C, preferably 125 to 450°C, and more preferably 150 to 250°C.
[0081] The heat treatment method in step (b) is not limited to a specific heat treatment method or duration. A person skilled in the art can determine a suitable heat treatment method depending on the type of substrate and formulation.
[0082] In some embodiments of the method for preparing an optical metal oxide layer according to the present invention, a pre-bake step to remove the solvent from the preparation may be applied before step (b) or after step (a). The preparation may also be partially converted into an optical metal oxide layer on the surface of the substrate by pre-bake (soft bake) at a temperature of 40-150°C, preferably 50-120°C, more preferably 60-100°C; then, bake (hard bake, sintering, or annealing) of step (b) is applied at a temperature of 100-600°C, preferably 125-450°C, more preferably 150-255°C.
[0083] Pre-baking (soft baking) serves to remove volatile, low-boiling-point components, such as volatile, low-boiling-point formulation media or additives, from drop-casting, coating, or printed films. Pre-baking is preferably performed for 1 to 60 minutes. After pre-baking, a substrate adhesive film layer of metal oxide precursor or metal oxide precursor mixture is obtained. The film may still contain residual formulation media or additives.
[0084] In an alternative preferred embodiment of the method for preparing an optical metal oxide layer according to the present invention, pre-baking is omitted, and as a result, in step (b), the formulation on the surface of the substrate or the underlying surface is directly converted into an optical metal oxide layer.
[0085] Baking (hard baking, sintering, or annealing) serves the purpose of converting a metal oxide precursor or metal oxide precursor mixture layer of the substrate into a metal oxide layer. Furthermore, the final properties of the metal oxide layer may be adjusted by the baking process. Baking is preferably carried out for a time in the range of 1 to 60 minutes, preferably 2 to 20 minutes, and more preferably 3 to 10 minutes.
[0086] The pre-bake and bake (step (b)) may be carried out in the ambient atmosphere or in an atmosphere with increased oxygen content to decompose unwanted organic components, which may lower the activation energy when the composite is formed, and is thought to improve the physicochemical properties of the resulting layered composite material.
[0087] In a preferred embodiment of the method of the present invention, the substrate or underlying layer is patterned and includes topographic features on its surface, and a layered composite, preferably an optical layer, covers the surface of the substrate and forms a coating layer that fills the topographic features. As a result, the topographic features are filled and planarized by the composition.
[0088] Preferred topographic features include, for example, gaps, grooves, trenches, and vias. The topographic features may be distributed uniformly or non-uniformly on the surface of the substrate. Preferably, they are arranged as an array or grid on the surface of the substrate. The topographic features preferably have different lengths, widths, diameters, and aspect ratios. The topographic features preferably have an aspect ratio of 1:20 to 20:1, more preferably 1:10 to 10:1. The aspect ratio is defined as the width of the structure versus its height (or depth). In terms of dimensions, the depth of the topographic features is preferably in the range of 10 nm to 10 μm, more preferably 50 nm to 5 μm, and most preferably 100 nm to 1 μm.
[0089] Furthermore, it is preferable that the topographic features are tilted at a specific angle, for example, 10 to 80°, preferably 20 to 60°, more preferably 30 to 50°, and most preferably about 40°. Such tilted topographic features are also referred to as slant-type or blazed topographic features.
[0090] Furthermore, it may be necessary to locally fill the topographic features with an optical metal oxide layer, either completely or to a specific level, but without covering adjacent surfaces of the substrate where topographic features to be filled are unavailable.
[0091] The substrate is preferably a substrate for an optical device. Preferred substrates are made from inorganic or organic-based materials, preferably inorganic-based materials. Preferred inorganic-based materials include materials selected from the list of ceramics, glass, fused silica, sapphire, silicon, silicon nitride, quartz, and transparent polymers or resins. The shape of the substrate is not particularly limited, but sheets or wafers are preferred.
[0092] In step (a) of the method, the formulation is applied to the surface of a substrate or the surface of a lower layer, the surface of which may be the surface of the base material of the substrate or the surface of a layer of a material different from the base material of the substrate, such layer being formed before the formulation is applied.
[0093] In this way, a sequence of different layers (a layer stack) can be formed on top of each other. Such a layer stack may also be structured, and such a structure typically has dimensions on the nanometer scale with respect to at least diameter, width, and / or aspect ratio.
[0094] Therefore, in a preferred embodiment, in step (b), the preparation is baked at a temperature of 100 to 600°C, preferably 125 to 450°C, more preferably 150 to 250°C, to be converted at least partially into a composite on the surface of the substrate, preferably a layered composite.
[0095] In a preferred embodiment of the present invention, the heat treatment in step (b) is performed for a time ranging from 1 to 60 minutes, preferably 2 to 20 minutes, and more preferably 3 to 10 minutes.
[0096] In some embodiments, the formulation is converted at least partially into a composite on the surface of the substrate during the heat treatment process of step (b), the composite preferably comprises a metal oxide selected from metal monooxides, metal dioxides and / or metal pentaoxides; as well as a metal alkoxide or metal halide, metal oxohalide or metal carboxylate.
[0097] - complex In another aspect, the present invention relates to a composite, preferably a layered composite, and preferably the layered composite is an optical layer obtained or obtainable by the method of the present invention.
[0098] In another aspect, the present invention relates to a composite, preferably a layered composite, and preferably the layered composite is an optical layer derived from the formulation of the present invention.
[0099] In a preferred embodiment of the present invention, the complex comprises at least a metal oxide derived from the metal oxide precursor of the formulation and a metal oxide precursor as the unconverted portion of the formulation used in step (a) of the method.
[0100] Details of the metal oxide precursors are shown in the section on metal oxide precursors above.
[0101] - Optical devices The present invention further relates to an optical device comprising the composite of the present invention, which is prepared using the formulations of the present invention described above.
[0102] The optical device is preferably a device comprising one or more optical components for forming a light beam, including but not limited to gratings, lenses, prisms, mirrors, optical windows, filters, polarizing optics, UV and IR optics, waveguides, and optical coatings. In the context of the present invention, a preferred optical device is a waveguide for augmented reality (AR) devices, virtual reality (VR) devices, and / or mixed reality (MR) devices, or a preferred optical device is augmented reality (AR) glasses, virtual reality (VR) glasses, and / or mixed reality (MR) glasses.
[0103] - Display devices Finally, the present invention relates to a display device comprising: at least one functional medium configured to modulate or emit light; and a composite or optical device of the present invention.
[0104] Examples of the display devices are selected from liquid crystal displays (LCDs), light-emitting diode displays (LEDs), organic light-emitting displays (OLEDs), micro-LED displays, quantum dot displays (QLEDs), augmented reality (AR) hardware, virtual reality (VR) hardware, mixed reality (MR) hardware, plasma (PDP) displays, and electroluminescent (ELD) displays. The AR, VR, and MR hardware are also called AR, VR, and MR displays. Preferably, the display device is AR hardware, VR hardware, or MR hardware.
[0105] The present invention will be further illustrated by the following examples, but this is not to be construed as limiting. Those skilled in the art will recognize that various modifications, additions, and changes can be made to the invention without departing from the spirit and scope of the invention as defined in the appended claims.
[0106] [example] - Analysis and measurement methods Ellipsometry is used to determine the layer thickness, refractive index (n), and absorption index (k) of the metal oxide layer. Measurements are performed using a JAWoolam M2000 ellipsometer and three different incident angles (65°, 70°, and 75°). The measurement data is analyzed using JAWoolam CompleteEase software, and B-spline fitting is applied to obtain the refractive index (n) and absorption index (k), assuming fully transparent or nearly fully transparent behavior at wavelengths above 600 nm (560 nm). Optical constants are averaged from 3-4 measurement samples, each offering different layer thicknesses after soft baking, hard baking, or a combination of soft baking and subsequent hard baking.
[0107] All synthetic chemicals listed are purchased from Sigma Aldrich and are used without further purification unless otherwise stated elsewhere.
[0108] Preparation of compound The precursor used Examples 1-5 include zirconium tetra-n-butoxide; Examples 6-11 include titanium tetra-n-butoxide; Examples 12-14 contain niobium pentaethoxide. Weigh the stock solution and organic co-solvent into glass bottles and stir the mixture for 30 minutes before use.
[0109] Example 1 Preparation of compound Zr-1 Preparation Zr-1: Zirconium tetra-n-butoxide with a nominal solid content of 17% by weight.
[0110] Zirconium tetra-n-butoxide is added to PGME (1-methoxy-2-propanol: dried on molecular sieves) in a two-necked Schlenk flask connected to an inert gas / vacuum line under an argon atmosphere. The solution is stirred at room temperature, and a solution of H2O and methanesulfonic acid (MSA) in the PGME is added dropwise at room temperature to obtain a clear solution, which is then stirred for a further 60 minutes. The amounts of solvent and starting material vary, but the mass concentration of the metal alkoxide starting material remains constant.
[0111] The weight percentages and molar percentages of each component used in the preparation of compound Zr-1 are shown in Table 1 of Zr-1.
[0112] Examples 2-5 Preparation of formulations Zr-2 to Zr-5a and b Preparations Zr-2 to Zr-5a and b are prepared in the same manner as described in Example 1, except that the materials listed in Table 1 (Zr-2 to Zr-5) are used in the quantities specified, instead of the materials used in Example 1.
[0113] Examples 6-11 Preparation of formulations Ti-1 to Ti-6 Preparations Ti-1 to Ti-6 are prepared in the same manner as described in Example 1, except that the materials listed in Table 1 (Ti-1 to Ti-6) are used in the quantities specified, instead of the materials used in Example 1.
[0114] Examples 12-14 Preparation of formulations Nb-1 to Nb-3 Preparations Nb-1 to Nb-3 are prepared in the same manner as described in Example 1, except that the materials listed in Table 1 (Nb-1 to Nb-3) are used in the quantities specified, instead of the materials used in Example 1.
[0115] [Table 1]
[0116] Example 15 Forming layers Sample Zr-1 is prepared by the following process. The Zr-1 preparation from Example 1 (WE1) is spin-coated onto an O2 plasma-pretreated Si3N4 / Si substrate having a 150 nm wide trench on its surface. The coating layer is then baked at 200°C for 5 minutes. The resulting Zr-1 sample is observed by TEM analysis.
[0117] Samples Zr-2, Zr-3, Zr-4, Zr-5a, and Zr-5b are prepared in the same manner as described in Example 15 above, except that different conditions are applied as shown in Table 1. Specifically, for sample Zr-3, two types of samples are prepared (sample Zr-3 (bake temperature 200°C / 5 min) and sample Zr-3 (bake temperature 300°C / 5 min)). For sample Zr-4, three types of samples are prepared (sample Zr-4 (bake temperature 100°C / 5 min), sample Zr-4 (bake temperature 200°C / 5 min), and sample Zr-4 (bake temperature 300°C / 5 min)).
[0118] In sol-gel derived ZrO2, the selectivity between upper layer formation and gap filling can be controlled by three different parameters. a) Curing temperature b) Solvent: PGME vs. DM2P c) Nominal ZrO2 solids content of the preparation
[0119] Generally, reactive building blocks contained in ZrO2 sol-gel formulations show a strong preference for overlayer deposition on O2 plasma-pretreated Si3N4 / Si substrates. This behavior is attributed to the high condensation rate of reactive Zr-oxoclusters formed from controlled hydrolysis of zirconium(IV)n-butoxide during formulation preparation. When stored in diluted form, the gelation of acid-stabilized sols containing nominal ZrO2 solids ≤ 8 w% is a slow process (several days to several weeks) under ambient conditions. Spin-coating deposition on O2 plasma-pretreated Si3N4 / Si substrates is thought to result in rapid evaporation of the solvent and condensation of reactive Zr-oxoclusters with Si-OH groups on the surface, thereby leading to high local concentrations and thus rapid condensation into a macroscopic network on the substrate surface.
[0120] Consistent with the mechanistic description of the rapid formation of macroscopic ZrO2 domains, the effect of curing temperature on the selectivity between gap filling and upper layer formation was observed only with ZrO2 sols with nominal solids content <3.7 w%. The viscoelasticity of the upper layer initially formed by spin coating of 1.3 w% ZrO2 sol appears sufficient to induce material flow into the gaps at curing T ≥ 200°C, but the upper layer persists at T = 100°C. However, increasing the solids content to ≥ ~3 w% ZrO2 yields an initial upper layer that is less susceptible to temperature-inducible flow from spin coating. This explanation is consistent with the finding that gap filling is not observed at gap widths < 100 nm.
[0121] Figures 7a and 7b show the temperature dependence of upper layer formation versus gap filling obtained from example Zr-2 and Zr-3, respectively, with a ZrO2 solid content of 1.3 w%. Specifically, Figure 7a shows the TEM image of sample Zr-2, and Figure 7b shows the TEM image of sample Zr-3.
[0122] The overall rate of condensation of reactive Zr-oxo species forming a macroscopic ZrO2 network can be controlled by the choice of solvent. Experimental data show that a decrease in condensation rate correlates with improved gap filling, and that this may be influenced by the solvent, which i) acts as a terminal ligand at metal sites on the surface of reactive Zr-oxo clusters and ii) is pH-responsive. Generally, secondary alcohols are preferred. More specifically, in the case of ZrO2, replacing 1,3-dimethoxy-2-propanol (DM2P) with 1-methoxy-2-propanol (PGME) allows for selective filling of gaps ≥100 nm at curing temperatures T=100~300°C. However, this positive solvent effect on gap filling is only applicable when the nominal ZrO2 solids content is <approximately 3 w%; otherwise, the formation of an upper layer prevails.
[0123] Table 2 shows the results of TEM analysis. Table 2 also shows the solvent dependence of upper layer formation versus gap filling obtained from examples Zr-2 and Zr-4, respectively.
[0124] [Table 2]
[0125] Table 3 shows the nominal ZrO2 solid content dependence of upper layer formation versus gap filling obtained from examples Zr-5 and Zr-4, respectively.
[0126] [Table 3]
[0127] Table 4 shows the relevant optical properties of ZrO2 films with a thickness of <100 nm.
[0128] [Table 4]
[0129] Example 16 Forming layers Example 16 provides O2 plasma pre-treated Si3N4 / Si substrates with trenches 50 nm wide, O2 plasma pre-treated Si3N4 / Si substrates with trenches 100 nm wide, and O2 plasma pre-treated Si3N4 / Si substrates with trenches 150 nm wide, for each respective case.
[0130] Next, the samples Ti-1 (trench width 50nm), Ti-1 (trench width 100nm), Ti-1 (trench width 150nm), Ti-2 (trench width 50nm), Ti-2 (trench width 100nm), Ti-2 (trench width 150nm), Ti-3 (trench width 50nm), Ti-3 (trench width 100nm), Ti-3 (trench width 150nm), Ti-4a (trench width 50nm), Ti-4a (trench width 100nm), Ti-4a (trench width 150nm), Ti-4b ( Ti-4b (trench width 50 nm), Ti-4b (trench width 100 nm), Ti-5 (trench width 50 nm), Ti-5 (trench width 100 nm), Ti-5 (trench width 150 nm), Ti-6 (trench width 50 nm), Ti-6 (trench width 100 nm), and Ti-6 (trench width 150 nm) are prepared in the same manner as described in Example 15 above, except that different conditions listed in Table 1 (Ti-1, 2, 3, 4a, 4b, 5, and 6) are applied.
[0131] In the case of sol-gel derived TiO2, the selectivity between upper layer formation and gap filling can be controlled primarily by two parameters. a) Solvent: PGME vs. DM2P b) Nominal TiO2 solids content of the preparation
[0132] Generally, reactive building blocks in TiO2 sol-gel formulations exhibit diverse reactivity, enabling TiO2 deposition in either a superlayer-forming or gap-filling form. These complementary deposition modes can be addressed by selecting a solvent that controls the condensation rate of reactive Ti-oxoclusters formed from the initial controlled hydrolysis of titanium(IV)n-butoxide. In addition to the solvent, the nominal TiO2 solids content is a second parameter influencing the gelation rate of acid-stabilized sols. 1-Methoxy-2-propanol (PGME) stabilizes reactive TiO2 sols with a nominal solids content of ≤8 w% under ambient conditions for several days to several weeks; however, substituting 1,3-dimethoxy-2-propanol reduces the sol's shelf life, requiring a reduction in the nominal solids content to ≤2.3 w%.
[0133] Table 5 shows the solvent dependence of upper layer formation versus gap filling obtained from examples Ti-5 and Ti-1, respectively.
[0134] [Table 5]
[0135] Spin coating deposition on O2 plasma-pretreated Si3N4 / Si substrates induced rapid evaporation of the solvent and condensation of reactive Ti-oxoclusters with surface Si-OH groups, likely resulting in high local concentrations favorable to easy condensation into macroscopic networks at the substrate surface. The effect of the solvent on the condensation rate, reflected in the storage life of the sol and the selectivity of TiO2 deposition as an overlayer or gap filler, is likely related to the acid-base properties of the Ti-oxo species. In contrast to PGME, when DM2P binds to the surface Ti(IV) sites of Ti-oxoclusters, the number of methoxy groups acting as potential but spatially more distant proton acceptors doubles. The net effect of the solvent is a reduced stabilizing effect on acidic components in the reactive TiO2 sol, which is further reflected in the lack of sol derived from DM2P for gap filling of 50 nm wide trenches.
[0136] Table 6 highlights the effect of nominal solid content on the selectivity of upper layer versus void filling for 8 and approximately 1 w% TiO2 sol formulations. Selective void filling was achieved from the 1 w% TiO2 sol at all void widths, whereas selective upper layer formation from the 8 w% sol was achieved only in the narrowest voids, while partial filling in addition to upper layer deposition was observed in trenches ≥ 100 nm wide.
[0137] Table 6 shows the nominal TiO2 solid content dependence of the upper layer formation versus gap filling obtained from examples Ti-3 and Ti-1, respectively.
[0138] [Table 6]
[0139] The inherently high refractive index of rutile and other forms of crystalline TiO2 is reflected in the optical properties of thin films deposited from reactive TiO2 sol formulations, and the relevant data, along with the processing conditions, are summarized in Table 7.
[0140] [Table 7]
[0141] Example 17 Forming layers Example 17 provides O2 plasma pre-treated Si3N4 / Si substrates with trenches 50 nm wide, O2 plasma pre-treated Si3N4 / Si substrates with trenches 100 nm wide, and O2 plasma pre-treated Si3N4 / Si substrates with trenches 150 nm wide for all cases.
[0142] Next, samples Nb-1 (trench width 50 nm), Nb-1 (trench width 100 nm), Nb-1 (trench width 150 nm), Nb-2 (trench width 50 nm), Nb-2 (trench width 100 nm), Nb-2 (trench width 150 nm), Nb-3 (trench width 50 nm), Nb-3 (trench width 100 nm), and Nb-3 (trench width 150 nm) are prepared in the same manner as described in Example 15 above, except that the different conditions described in Table 1 (Nb-1, 2, and 3) are applied to each case.
[0143] In the case of Nb2O5 derived from sol-gels, the selectivity between upper layer formation and gap filling can be controlled by two parameters. a) Solvent: PGME vs. DM2P b) Nominal Nb2O5 solids of the preparation
[0144] The chemical and depositional properties of sol preparations derived from Nb2O5 are nearly identical to those of TiO2, except that the solvent's influence on the sol's storage life and upper layer-to-gap packing selectivity is more pronounced, consistent with the similar ionic radii of 6-coordinate Ti(IV) and Nb(V). When the acid content is kept at 5 mol%, sols derived from DM2P tolerate only half of the nominal Nb2O5 solids (approximately 3 w%) that can be handled by PGME.
[0145] Table 8 shows the solvent dependence of upper layer formation versus gap filling obtained from examples Nb-3 and Nb-1, respectively.
[0146] [Table 8]
[0147] [Table 9]
[0148] Table 10 shows the relevant optical data for thin films derived from Nb2O5 sol.
[0149] [Table 10]
[0150] For Nb-4 in the table, a formulation containing 12.6% by weight of nominal solids of Nb2O5 (28.8% by weight of niobium pentaethoxide as a metal alkoxide) is prepared and used based on the total amount of the formulation.
Claims
1. A formulation for preparing an optical layer containing a metal oxide, preferably for preparing a composite, more preferably for preparing a layered composite, comprising at least: - A metal oxide precursor comprising Group 4 and / or Group 5 elements of the periodic table, preferably the metal oxide precursor being a metal alkoxide, metal halide, or metal carboxylate comprising Group 4 and / or Group 5 elements of the periodic table, and more preferably the metal oxide precursor being a metal alkoxide comprising Group 4 and / or Group 5 elements of the periodic table; - Optionally, an acid selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides, and carboxylic acids; and - A solvent, wherein the solvent is a secondary alcohol having no alkoxy groups, one or two alkoxy groups, or one or two alkyl groups, wherein one or more non-adjacent groups of the alkyl group are replaced by oxygen atoms, or is a secondary linear or branched ≥ C3 alcohol, preferably selected from one or more members of 2-propanol, 2-butanol, 2-pentanol, and 3-pentanol, preferably a secondary linear or branched ≥ C4 alcohol; preferably, the solvent is a solvent selected from propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, glycerol 1,3-dialkyl ether, or a combination of propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, and glycerol 1,3-dialkyl ether. Includes, - A formulation in which the total amount of the metal oxide precursor in the formulation is in the range of 0.1 to 40% by weight, preferably 1 to 35% by weight, more preferably 2 to 30% by weight, and even more preferably 3 to 28% by weight, based on the total amount of the formulation.
2. The metal oxide precursor is defined by the following chemical formula (IV) or formula (V): M b1 O 4 (R) b1 R b2 R b3 R b4 ) -(U) M b2 O 5 (R b1 R b2 R b3 R b4 R b5 ) -(V) (In the formula, M b1 is a tetravalent metal of Group 4 elements in the periodic table, preferably Ti or Zr; M b2 is a pentavalent metal of Group 5 elements in the periodic table, preferably Nb or Ta; R b1 , R b2 , R b3 , R b4 and R b5 Each is independently selected from H, D, a linear alkyl group having 1 to 25 carbon atoms, preferably 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms; a branched or cyclic alkyl group having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; an aryl group having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; a linear alkyl-cycloalkyl group having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; a branched alkyl-cycloalkyl group having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; a linear alkyl-aryl group having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; a branched alkyl-aryl group having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; One or more non-adjacent CH groups of the above-mentioned groups 2 CH4 group and / or one or more adjacent CH4 groups 2 The group may be replaced by an oxygen atom, and one or more H atoms may be D, CN, or NO 2 It can be replaced with; Each of the groups contains one or more groups R a It may be replaced with, R a In each occurrence, these are identical or different linear alkyl or alkoxy groups having H, D, 1 to 15 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms; branched or cyclic alkyl or alkoxy groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; linear alkenyl or alkynyl groups having 2 to 15 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 5 carbon atoms; branched alkenyl or alkynyl groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; aromatic or heteroaromatic ring systems having 5 to 15 aromatic ring atoms, preferably 5 to 10 aromatic ring atoms; in each of the above groups, one or more H atoms may be replaced by D, where two or more adjacent substituents R a (These elements may optionally form monocyclic or polycyclic aliphatic ring systems with each other.) The formulation according to claim 1, as represented by [the specified method].
3. The preparation according to claim 1 or 2, comprising an acid selected from one or more members of the group consisting of sulfonic acids, amine hydrochlorides, and carboxylic acids.
4. The aforementioned sulfonic acid has the following chemical formula (I) R a1 SO 3 H - (I) (In the formula, R a1 This is selected from the group consisting of: linear alkyl groups having 1 to 25 carbon atoms, preferably 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms; branched or cyclic alkyl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; aryl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; linear alkyl-cycloalkyl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; branched alkyl-cycloalkyl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; linear alkyl-aryl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; and branched alkyl-aryl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms. One or more non-adjacent CHs of the above-mentioned base 2 The groups are oxygen atom, C=O, C=S, C=Se, C=NH, SiH 2 , SO, SO 2 It may be replaced with OS or CONH, and one or more H atoms may be D, F, Cl, Br, I, CN, or NO 2 It can be replaced with; Each of the groups contains one or more groups R ax It may be replaced with; R ax In each occurrence, these are identical or different linear alkyl or alkoxy groups having H, D, 1 to 15 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms; branched or cyclic alkyl or alkoxy groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; linear alkenyl or alkynyl groups having 2 to 15 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 5 carbon atoms; branched alkenyl or alkynyl groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; aromatic or heteroaromatic ring systems having 5 to 15 aromatic ring atoms, preferably 5 to 10 aromatic ring atoms; in each of the above groups, one or more H atoms may be replaced with D, F, Cl, Br, or I, where two or more adjacent substituents R ax (These elements may optionally form monocyclic or polycyclic aliphatic ring systems with each other.) It is represented by the following chemical formula (II) ・| a2 (I) (In the formula, R a2 is, N 2 H 4 , represented by a selection from the group consisting of ammonia, hydroxylamine, imidazole and 1,4-diazabicyclo[2.2.2]octane; and / or The carboxylic acid is of the following chemical formula (III) R a3 -COOH (In the formula, R a3 This is selected from the group consisting of: linear alkyl groups having 1 to 25 carbon atoms, preferably 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms; branched or cyclic alkyl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; aryl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; linear alkyl-cycloalkyl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; branched alkyl-cycloalkyl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; linear alkyl-aryl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; and branched alkyl-aryl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms. One or more non-adjacent CHs of the above-mentioned base 2 The groups are oxygen atom, C=O, C=S, C=Se, C=NH, SiH 2 , SO, SO 2 It may be replaced with OS or CONH, and one or more H atoms may be D, F, Cl, Br, I, CN, or NO 2 It can be replaced with; Each of the groups contains one or more groups R ax It may be replaced with; R ax In each occurrence, these are identical or different linear alkyl or alkoxy groups having H, D, 1 to 15 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms; branched or cyclic alkyl or alkoxy groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; linear alkenyl or alkynyl groups having 2 to 15 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 5 carbon atoms; branched alkenyl or alkynyl groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; aromatic or heteroaromatic ring systems having 5 to 15 aromatic ring atoms, preferably 5 to 10 aromatic ring atoms; in each of the above groups, one or more H atoms may be replaced with D, F, Cl, Br, or I, where two or more adjacent substituents R ax (These elements may optionally form monocyclic or polycyclic aliphatic ring systems with each other.) A composition as described in any one of the preceding claims, represented by [the specified term].
5. The aforementioned acid is of the following chemical formula (II) ・| a2 (I) (In the formula, R a2 is, N 2 H 4 (Selected from the group consisting of ammonia, hydroxylamine, imidazole, and 1,4-diazabicyclo[2.2.2]octane) A preparation according to any one of the preceding claims, which is an amine hydrochloride represented by .
6. The acid in question has the following chemical formula (I): R a1 SO 3 H - (I) (In the formula, R a1 This is selected from the group consisting of: linear alkyl groups having 1 to 25 carbon atoms, preferably 1 to 15 carbon atoms, more preferably 1 to 10 carbon atoms; branched or cyclic alkyl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; aryl groups having 3 to 25 carbon atoms, preferably 3 to 15 carbon atoms, more preferably 3 to 10 carbon atoms; linear alkyl-cycloalkyl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; branched alkyl-cycloalkyl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms; linear alkyl-aryl groups having 4 to 25 carbon atoms, preferably 4 to 15 carbon atoms; and branched alkyl-aryl groups having 6 to 25 carbon atoms, preferably 6 to 15 carbon atoms. One or more non-adjacent CHs of the above-mentioned base 2 The groups are oxygen atom, C=O, C=S, C=Se, C=NH, SiH 2 , SO, SO 2 It may be replaced with OS or CONH, and one or more H atoms may be D, F, Cl, Br, I, CN, or NO 2 It can be replaced with; Each of the groups contains one or more groups R ax It may be replaced with; R ax In each occurrence, these are identical or different linear alkyl or alkoxy groups having H, D, 1 to 15 carbon atoms, preferably 1 to 10 carbon atoms, more preferably 1 to 5 carbon atoms; branched or cyclic alkyl or alkoxy groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; linear alkenyl or alkynyl groups having 2 to 15 carbon atoms, preferably 2 to 10 carbon atoms, more preferably 2 to 5 carbon atoms; branched alkenyl or alkynyl groups having 3 to 15 carbon atoms, preferably 3 to 10 carbon atoms, more preferably 3 to 5 carbon atoms; aromatic or heteroaromatic ring systems having 5 to 15 aromatic ring atoms, preferably 5 to 10 aromatic ring atoms; in each of the above groups, one or more H atoms may be replaced with D, F, Cl, Br, or I, where two or more adjacent substituents R ax (These elements may optionally form monocyclic or polycyclic aliphatic ring systems with each other.) The preparation according to any one of claims 1 to 4, wherein the sulfonic acid is represented by .
7. The formulation according to any one of the preceding claims, wherein the stoichiometric molar ratio of the acid to the metal oxide precursor is in the range of 0.01:100 to 120:100, and preferably the relative molar amount of the acid based on the total amount of the metal oxide precursor is in the range of 0.1 to 50, more preferably 1 to 10.
8. The preparation according to any one of the preceding claims, wherein the solvent is selected from propylene glycol monoalkyl ether, preferably propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether and / or propylene glycol monopropyl ether; glycerol 1,3-dialkyl ether, 1,3-dimethoxy-2-propanol, and more preferably the solvent is selected from propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, or a mixture thereof.
9. The preparation according to any one of the preceding claims, wherein the preparation contains water, and the stoichiometric amount of water is in the range of 100 to 400 mol% based on the total amount of the metal oxide precursor, preferably in the range of 150 to 300 mol%, and more preferably in the range of 180 to 270 mol%.
10. At least the following steps: (X1) A step of dissolving a metal oxide precursor in solvent 1 to form a metal oxide precursor solution, wherein solvent 1 is preferably a dry or anhydrous solvent; (X2) Optionally, a step of dissolving an acid in solvent 2 to form an acid solution, preferably the solvent 2 being a dry or anhydrous solvent, and the acid being selected from one or more members of the group consisting of sulfonic acids, hydrochloride salts, and carboxylic acids; (X3) Optionally, adding the acid solution obtained in step (X2) to the metal oxide precursor solution obtained in step (X1); (X4) A step of mixing water and solvent 3 to form an aqueous solvent; and (X5) A step of adding the aqueous solvent to the alkoxide solution obtained in step (X1) or the metal oxide precursor solution obtained in step (X3); (X6) Optionally, a step of forming an acid solution by dissolving an acid and water in solvent 4 to form an acid aqueous solution, preferably wherein solvent 4 is a dry or anhydrous solvent, and the acid is selected from one or more members of the group consisting of sulfonic acids, hydrochloride salts, and carboxylic acids; (X7) Optionally, adding the acid aqueous solution (X6) to the metal oxide precursor solution (X1). A method for preparing the formulation according to any one of the preceding claims, wherein the solvents 1 to 4 are independently selected from each other: propylene glycol monoalkyl ether, preferably propylene glycol monomethyl ether (PGME), propylene glycol monoethyl ether and / or propylene glycol monopropyl ether; glycerol 1,3-dialkyl ether, 1,3-dimethoxy-2-propanol; more preferably the solvent is selected from propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, glycerol 1,3-dialkyl ether; secondary linear or branched ≥ C3 alcohol, preferably 2-propanol, 2-butanol, 2-pentanol, 3-pentanol; more preferably selected from linear or branched secondary ≥ C4 alcohol; and preferably the solvent is selected from propylene glycol monoalkyl ether, glycerol 1,3-dialkyl ether, glycerol 1,3-dialkyl ether.
11. A method for preparing a composite comprising a metal oxide, wherein the metal oxide is selected from a metal monooxide, a metal dioxide, or a metal pentaoxide, or a combination thereof; the following steps (a) and (b): (a) a step of providing the formulation according to any one of claims 1 to 9 to the surface of a substrate or a lower layer, preferably by a wet deposition process, more preferably by spin coating or region-selective printing, preferably by region-selective printing in which the region-selective printing is ink spraying, and (b) A step of applying heat treatment to the preparation provided on the surface of the substrate or the surface of the underlying layer to convert at least a portion of the metal oxide precursor in the preparation into a metal oxide. A method comprising, preferably, the composite being a layered composite, and more preferably, the layered composite being an optical layer.
12. The method according to any one of claims 11, wherein the preparation is at least partially converted into a complex on the surface of the substrate, the complex comprising a metal oxide preferably selected from metal monooxides, metal dioxides and / or metal pentaoxides; and a metal alkoxide, metal halide, metal oxohalide or metal carboxylate.
13. A composite derived from a formulation according to any one of claims 1 to 9, preferably a layered composite, and preferably the layered composite being an optical layer.
14. An optical device comprising the composite according to claim 13 and a substrate having a patterned surface or a non-uniform surface.
15. A display device comprising: at least one functional medium configured to direct and modulate light, or configured to emit light; the composite according to claim 13, or the optical device according to claim 14.