Positive electrode active material, positive electrode containing the same, and lithium secondary battery
A lithium composite transition metal oxide doped with Zr and Y, with controlled particle size and composition, addresses the structural and thermal instability of conventional secondary particle materials, enhancing battery capacity and resistance performance.
Patent Information
- Application Number
- JP2026525686
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-03
- Filing Date
- 2024-11-01
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional lithium secondary battery positive electrode active materials, particularly those in spherical secondary particle form, face issues such as structural and thermal instability, leading to gas generation, swelling, and increased fire risk, especially with high nickel content. Single-particle form materials are needed to address these issues while maintaining optimal battery performance.
A lithium composite transition metal oxide with a specific chemical composition and doping of Zr and Y, along with controlled primary particle size and proportion of small particles, is used to enhance the stability and performance of single-particle positive electrode active materials.
The solution reduces particle cracking during manufacturing, improves capacity, initial efficiency, and resistance performance of lithium secondary batteries, ensuring stable operation and high energy density.
Smart Images

Figure 2026539084000001_ABST
Abstract
Description
TECHNICAL FIELD
[0001] This application claims the benefit of priority based on Korean Patent Application No. 10-2023-0151123 filed on November 3, 2023, and all contents disclosed in the documents of the corresponding Korean patent application are incorporated as part of the present specification.
[0002] The present invention relates to a positive electrode active material, a positive electrode comprising the same, and a lithium secondary battery, and specifically, relates to a single-particle form positive electrode active material, a positive electrode comprising the same, and a lithium secondary battery.
BACKGROUND ART
[0003] Recently, with the technological development and increasing demand for mobile devices and electric vehicles, the demand for secondary batteries as an energy source has increased sharply. Among such secondary batteries, lithium secondary batteries that have high energy density and voltage, long cycle life, and low self-discharge rate have been commercialized and are widely used.
[0004] As positive electrode active materials for lithium secondary batteries, lithium transition metal oxides such as lithium cobalt oxides like LiCoO2, lithium nickel oxides like LiNiO2, lithium manganese oxides like LiMnO2 or LiMn2O4, and lithium iron phosphate oxides like LiFePO4 have been developed, and recently, Li[Ni a Co b Mn c O2, Li[Ni a Co b Al c O2, Li[Ni a Co b Mn c Al d O2, lithium composite transition metal oxides containing two or more transition metals have been developed and are widely used.
[0005] Lithium composite transition metal oxides containing two or more transition metals developed to date are typically manufactured in a spherical secondary particle form, where tens to hundreds of primary particles aggregate. However, recently, in order to solve the structural and thermal stability problems of secondary particle-form positive electrode active materials, the development of single-particle-form positive electrode active materials has been accelerating. Specifically, when secondary particle-form positive electrode active materials are applied to lithium secondary batteries, they generate a large amount of gas, causing the battery volume to expand. Furthermore, increasing the nickel content in the positive electrode active material for high capacity increases the risk of fire. Therefore, there is a growing demand for the development of single-particle-form positive electrode active materials with superior stability.
[0006] Single-particle cathode active materials are a contrasting concept to conventional cathode active materials, which are spherical secondary particle forms formed by the aggregation of tens to hundreds of primary particles manufactured by conventional methods. Single-particle cathode active materials consist of 10 or fewer primary particles, and because the size of the primary particles has a very large influence on the performance of the cathode active material, it is necessary to carefully control this size.
[0007] On the other hand, when manufacturing a lithium secondary battery using the aforementioned single-particle positive electrode active material, cracks and collapses of the positive electrode active material particles are likely to occur during the rolling process after coating it onto the positive electrode current collector. As a result, during the charging and discharging process of the lithium secondary battery, gas is generated by a side reaction between the positive electrode active material and the electrolyte, causing a swelling phenomenon and degrading the battery's performance.
[0008] Therefore, there is a need to develop single-particle cathode active materials that can achieve optimal battery performance. [Overview of the Initiative] [Problems that the invention aims to solve]
[0009] The present invention aims to solve the above-mentioned problems and to provide a single-particle positive electrode active material that can exhibit optimal battery performance.
[0010] Furthermore, the present invention aims to provide a lithium secondary battery with improved performance by including the above-mentioned positive electrode active material. [Means for solving the problem]
[0011] To solve the above problems, the present invention provides a positive electrode active material, a positive electrode, and a lithium secondary battery.
[0012] (1) The present invention comprises a lithium composite transition metal oxide in single-particle form having a composition represented by the following chemical formula 1, and consisting of 10 or fewer primary particles, wherein the primary particles are derived from SEM images. v,50 The present invention provides a positive electrode active material in which the particle size is 2.2 μm to 3.7 μm and the proportion of small particles according to the following formula 1 is 5% to 10%: [Chemical formula 1] Li 1+x Ni a1 Co b1 Mn c1 Zr d1 Y e1 M f1 O 2-y A y In the above chemical formula 1, M is one or more elements selected from W, Cu, Sr, Mn, Ti, Mg, Mo, B, Sn, Fe, Zn, Si, and Al. A is one or more elements selected from F, Cl, Br, I, and S. -0.1 ≤ x ≤ 0.1, 0 <a1<1、0<b1<1、0<c1<1、0<d1<0.01、0<e1<0.01、0≦f1<0.1、0≦y≦0.2、a1+b1+c1+d1+e1+f1=1であり、 [Formula 1] The ratio of small particles (%) = (sum of the areas of primary particles with a particle size of 1 μm or less derived from the SEM image / sum of the areas of all primary particles derived from the SEM image) × 100.
[0013] (2) In the present invention, in (1) above, the primary particle is derived from the SEM image D v,50 The present invention provides a positive electrode active material having a diameter of 2.5 μm to 2.8 μm.
[0014] (3) In the present invention, in (1) or (2) above, the positive electrode active material is measured by a PSA (particle size analyzer) 50 The present invention provides a positive electrode active material with a particle size of 3.5 μm to 4 μm.
[0015] (4) The present invention provides a positive electrode active material in which, in any one of (1) to (3) above, the lithium composite transition metal oxide is doped with 1000 ppm to 4000 ppm of Zr and 1000 ppm to 4000 ppm of Y.
[0016] (5) The present invention provides a positive electrode active material in any one of (1) to (4) above, wherein the positive electrode active material further comprises a coating layer formed on the lithium composite transition metal oxide, and the coating layer comprises Al, W, or a combination thereof.
[0017] (6) The present invention provides a positive electrode comprising a positive electrode active material according to any one of (1) to (5) above.
[0018] (7) The present invention provides a lithium secondary battery comprising a positive electrode according to (6) above, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte. [Effects of the Invention]
[0019] The positive electrode active material of the present invention comprises a lithium composite transition metal oxide doped with Zr and Y, and the ratio of small particles and the particle size of primary particles according to Formula 1 described herein satisfy a specific range, improving particle cracking and enabling improvements in the capacity, initial efficiency, resistance performance, etc., of lithium secondary batteries.
[0020] The positive electrode and lithium secondary battery according to the present invention can be excellent in terms of capacity, initial efficiency, resistance performance, and so on. [Brief explanation of the drawing]
[0021] [Figure 1] This is an SEM image of the positive electrode active material of Example 1. [Figure 2] This is an SEM image of the positive electrode active material of Example 3. [Modes for carrying out the invention]
[0022] The present invention will be described in more detail below to aid in understanding the present invention.
[0023] The terms and words used herein and in the claims should not be interpreted in a manner limited to their ordinary or dictionary meanings, but rather in a manner consistent with the technical idea of the present invention, in accordance with the principle that inventors may define the concepts of terms as appropriate to best describe their invention.
[0024] In this specification, terms such as “includes,” “equip,” or “have” specify the presence of implemented features, figures, steps, components, or combinations thereof, but should be understood not to preclude the existence or possibility of adding one or more other features, figures, steps, components, or combinations thereof.
[0025] In this specification, the term “on top of” means not only when one configuration is formed directly on top of another, but also when a third configuration is interposed between these configurations.
[0026] In this specification, "single particle form" is a concept contrasted with the spherical secondary particle form formed by the aggregation of tens to hundreds of primary particles manufactured by conventional methods, and refers to a form consisting of 10 or fewer primary particles. Specifically, in the present invention, the single particle form may be a single particle consisting of one primary particle, or it may be a secondary particle form formed by the aggregation of 2 to 10 primary particles.
[0027] "Primary particles" refer to the smallest particle units that can be recognized when observing the positive electrode active material through a scanning electron microscope, while "secondary particles" refer to secondary structures formed by the aggregation of multiple primary particles.
[0028] In this specification, the term "D of primary particles derived from SEM images" is used. v,50 This can be determined by calculating the area of each primary particle based on the number of pixels corresponding to each of the n primary particles (at least 50) present in an SEM image at a specific magnification (e.g., 5,000x, 8,000x), calculating the particle size and volume of each primary particle present in the SEM image using the radius value of a circle having the same area as the area of each primary particle, and then calculating the particle size at the point where the cumulative volume distribution by particle size reaches 50%.
[0029] In this specification, the term "sum of areas of primary particles with a particle size of 1 μm or less derived from an SEM image" can be calculated by determining the area of each primary particle based on the number of pixels corresponding to each of the n primary particles (at least 50) present in an SEM image at a specific magnification (e.g., 5,000x, 8,000x), determining the particle size of each primary particle present in the SEM image using the radius value of a circle having the same area as the area of each primary particle, and then adding up the areas of primary particles with a particle size of 1 μm or less.
[0030] In this specification, the term "sum of the areas of all primary particles derived from an SEM image" can be calculated by determining the area of each primary particle based on the number of pixels corresponding to each of the n primary particles (at least 50) present in an SEM image at a specific magnification (e.g., 5,000x, 8,000x), determining the particle size of each primary particle present in the SEM image using the radius value of a circle having the same area as the area of each primary particle, and then adding up the areas of all primary particles.
[0031] In this specification, "D measured by a PSA (particle size analyzer)" 50 " refers to the particle size at the 50% point of the volume cumulative distribution by particle size. 50This method involves dispersing the powder to be measured in a dispersion medium, then introducing it into a commercially available laser diffraction particle size analyzer (for example, the S3500 from Microtrac). As the particles pass through the laser beam, the difference in diffraction patterns due to particle size is measured to calculate the particle size distribution. The particle size at the point where the cumulative volume distribution by particle size in the analyzer reaches 50% is then calculated.
[0032] positive electrode active material The present invention comprises a lithium composite transition metal oxide in single-particle form having a composition represented by the following chemical formula 1, and consisting of 10 or fewer primary particles, wherein the primary particles are derived from SEM images. v,50 The present invention provides a positive electrode active material having a particle size of 2.2 μm to 3.7 μm and a proportion of small particles according to the following formula 1 of 5% to 10%. The lithium composite transition metal oxide may have a layered structure.
[0033] [Chemical formula 1] Li 1+x Ni a1 Co b1 Mn c1 Zr d1 Y e1 M f1 O 2-y A y
[0034] In the above chemical formula 1, M is one or more elements selected from W, Cu, Sr, Mn, Ti, Mg, Mo, B, Sn, Fe, Zn, Si, and Al. A is one or more elements selected from F, Cl, Br, I, and S. -0.1 ≤ x ≤ 0.1, 0 <a1<1、0<b1<1、0<c1<1、0<d1<0.01、0<e1<0.01、0≦f1<0.1、0≦y≦0.2、a1+b1+c1+d1+e1+f1=1であり、 [Formula 1] The ratio of small particles (%) = (Sum of the areas of primary particles with a particle size of 1 μm or less derived from the SEM image / Sum of the areas of all primary particles derived from the SEM image) × 100
[0035] The inventors have found that when the positive electrode active material comprises a lithium composite transition metal oxide in single-particle form doped with Zr and Y, and the particle size of the primary particles is within a specific range, and the proportion of small particles according to Formula 1 described herein is 5% to 10%, then during rolling for the manufacture of lithium secondary batteries, cracking of the positive electrode active material particles is reduced, and the capacity, initial efficiency, and resistance performance of the lithium secondary battery can be improved, thus completing the present invention.
[0036] According to the present invention, the lithium composite transition metal oxide is doped with Zr and Y. In this case, Zr is stably doped into the transition metal layer, and a stable structure can be maintained even if lithium is repeatedly inserted and removed as charging and discharging are repeated. In addition, Y acts as a flux material during firing, enabling the achievement of an optimal primary particle size even at relatively low temperatures, which is advantageous for resistance and rate-limiting characteristics.
[0037] On the other hand, if the lithium composite transition metal oxide is not doped with Zr, the structural retention rate is poor and the lifetime performance is unfavorable. If it is not doped with Y, the firing temperature must be further increased to achieve the optimal primary particle size, resulting in unfavorable resistance and rate-limiting characteristics.
[0038] According to the present invention, the lithium composite transition metal oxide is doped with 1,000 ppm to 4,000 ppm of Zr and 1,000 ppm to 4,000 ppm of Y in order to have optimal performance in terms of lifetime and resistance, even when having the desired primary particle size.
[0039] The Zr content may be 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, 1,300 ppm or more, or 1,400 ppm or more relative to the total weight of the lithium composite transition metal oxide, and may be 1,500 ppm or less, 1,600 ppm or less, 1,700 ppm or less, 1,800 ppm or less, 1,900 ppm or less, 2,000 ppm or less, 2,100 ppm or less, 2,200 ppm or less, 2, It may be 300 ppm or less, 2,400 ppm or less, 2,500 ppm or less, 2,600 ppm or less, 2,700 ppm or less, 2,800 ppm or less, 2,900 ppm or less, 3,000 ppm or less, 3,100 ppm or less, 3,200 ppm or less, 3,300 ppm or less, 3,400 ppm or less, 3,500 ppm or less, 3,600 ppm or less, 3,700 ppm or less, 3,800 ppm or less, 3,900 ppm or less, or 4,000 ppm or less.
[0040] Specifically, the content of Y is 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, 1,300 ppm or more, 1,400 ppm or more, 1,500 ppm or more, 1,600 ppm or more, 1,700 ppm or more, 1,800 ppm or more, 1,900 ppm or more, 2,000 ppm or more, 2,100 ppm or more, 2,200 ppm or more, 2,300 ppm or more, and 2,400 ppm or more relative to the total weight of the lithium composite transition metal oxide. The above may be 2,500 ppm or more, 2,600 ppm or more, 2,700 ppm or more, 2,800 ppm or more, or 2,900 ppm or more, and may also be 3,000 ppm or less, 3,100 ppm or less, 3,200 ppm or less, 3,300 ppm or less, 3,400 ppm or less, 3,500 ppm or less, 3,600 ppm or less, 3,700 ppm or less, 3,800 ppm or less, 3,900 ppm or less, or 4,000 ppm or less.
[0041] When the Zr content is within the aforementioned range, excellent structural retention during charging and discharging and high capacity can be achieved. When the Y content is within the aforementioned range, the optimal primary particle size can be achieved even at relatively low temperatures, which is advantageous for resistance and rate-limiting characteristics, and high capacity can be achieved.
[0042] According to the present invention, the positive electrode active material has a small particle ratio of 5% to 10% according to Formula 1. When the small particle ratio is 5% to 10%, it has optimal performance in terms of battery performance, particle cracking, and rolling density.
[0043] On the other hand, if the proportion of small particles in the positive electrode active material is less than 5%, there are problems with the efficiency and resistance performance of the battery, and if it exceeds 10%, there are problems with particle cracking and rolling density.
[0044] According to the present invention, the primary particle is derived from the SEM image D v,50 The particle size is 2.2 μm to 3.7 μm, preferably 2.5 μm to 2.8 μm. In this case, it has optimal performance in terms of battery performance, particle cracking, and rolling density. On the other hand, the primary particle D v,50 If the particle size is less than 2.2 μm, there is a problem with the rolling density and / or the battery's lifespan performance, and if it is greater than 3.7 μm, there is a problem with the battery's efficiency and / or resistance performance.
[0045] D of the primary particle v,50 This can be adjusted during the manufacturing of the positive electrode active material according to the type and content of doping elements, the amount of lithium raw material added, and the firing temperature.
[0046] According to the present invention, the positive electrode active material is measured by a PSA (particle size analyzer) and D 50 The diameter may be 3.5 μm to 4.0 μm. The D of the positive electrode active material 50 Specifically, it may be 3.50 μm or larger, 3.80 μm or smaller, 3.85 μm or smaller, 3.90 μm or smaller, 3.95 μm or smaller, or 4.0 μm or smaller. The D of the positive electrode active material measured by PSA (particle size analyzer) 50 If it falls within the aforementioned range, the lifespan and capacity characteristics of the battery including it will both be improved, and its electrochemical performance can be optimized. For reference, D 50 If the particle size is less than 3.5 μm, the battery life may be reduced, and if it is greater than 4.0 μm, the battery capacity may be reduced.
[0047] According to the present invention, 3 g of the positive electrode active material is placed in a mold with an inner diameter of 13 mm, pressurized at 9 tons for 1 minute, and the ratio of the number of particles with a particle size of less than 1 μm measured by a PSA (particle size analyzer) to the total number of particles (amount of fine powder generated) may be 2.5% or less, specifically 2.0% or less, 1.5% or less, 1.0% or less, or 0.6% or less. In this case, the specific surface area in contact with the particles and the electrolyte is reduced, so side reactions can be suppressed, and the capacity retention rate (life) due to charging and discharging and gas generation can be improved.
[0048] According to the present invention, the lithium composite transition metal oxide may contain 60 mol% or more of nickel relative to the total number of moles of metals other than lithium. That is, the lithium composite transition metal oxide may be a high-nickel (High Ni) lithium composite transition metal oxide. In this case, the energy density of the lithium secondary battery can be improved.
[0049] According to the present invention, in the chemical formula 1, x may be -0.1 or greater, -0.09 or greater, -0.08 or greater, -0.07 or greater, -0.06 or greater, -0.05 or greater, -0.04 or greater, -0.03 or greater, -0.02 or greater, -0.01 or greater, or 0 or greater, and may be 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.1 or less. When x satisfies the above range, high capacity characteristics and high energy density per unit volume can be achieved.
[0050] According to the present invention, in the chemical formula 1, a1 means the atomic fraction of nickel among the metal elements in the lithium composite transition metal oxide, and may be 0.6 or more, 0.61 or more, or 0.62 or more, and may be 0.7 or less, 0.71 or less, 0.72 or less, 0.73 or less, 0.74 or less, 0.75 or less, 0.76 or less, 0.77 or less, 0.78 or less, 0.79 or less, 0.8 or less, 0.81 or less, 0.82 or less, 0.83 or less, 0.84 or less, 0.85 or less, 0.86 or less, 0.87 or less, 0.88 or less, 0.89 or less, 0.91 or less, 0.92 or less, 0.93 or less, 0.94 or less, 0.95 or less, 0.96 or less, 0.97 or less, 0.98 or less, 0.99 or less, or less than 1. When a1 satisfies the aforementioned range, high capacitance characteristics can be achieved. In particular, when a1 is between 0.6 and 0.75, high energy density is observed during high-voltage driving, enabling high capacitance characteristics to be realized.
[0051] According to the present invention, in the chemical formula 1, b1 represents the atomic fraction of cobalt among the metal elements in the lithium composite transition metal oxide, and may be greater than 0, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, or 0.05 or more, and may be 0.10 or less, 0.11 or less, 0.12 or less, 0.13 or less, 0.14 or less, 0.15 or less, 0.16 or less, 0.17 or less, or 0.1 It may be 8 or less, 0.19 or less, 0.20 or less, 0.21 or less, 0.22 or less, 0.23 or less, 0.24 or less, 0.25 or less, 0.26 or less, 0.27 or less, 0.28 or less, 0.29 or less, 0.30 or less, 0.31 or less, 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, or less than 0.4. When b1 satisfies the above range, stability can be improved and rate characteristics can be enhanced during the charge-discharge process.
[0052] According to the present invention, in the chemical formula 1, c1 represents the atomic fraction of manganese among the metal elements in the lithium composite transition metal oxide, and can be greater than 0, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, 0.1 or more, 0.11 or more, 0.12 or more, 0.13 or more, 0.14 or more, 0.15 or more, 0.16 or more, or 0. It may be 17 or greater, 0.18 or greater, 0.19 or greater, 0.2 or greater, 0.21 or greater, 0.22 or greater, 0.23 or greater, 0.24 or greater, 0.25 or greater, 0.26 or greater, 0.27 or greater, 0.28 or greater, 0.29 or greater, or 0.30 or greater, and may be 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, or less than 0.4. When c1 satisfies the above range, high capacity characteristics can be achieved. In addition, high-temperature stability is increased and side reactions with the electrolyte can be relatively reduced.
[0053] According to the present invention, in the chemical formula 1, d1 means the atomic fraction of zirconium among the metal elements in the lithium composite transition metal oxide, and may be 0 or more, or 0.0005 or more, and may be 0.001 or less, 0.002 or less, 0.003 or less, 0.004 or less, 0.005 or less, 0.006 or less, 0.007 or less, 0.008 or less, 0.009 or less, or 0.01 or less. When d1 satisfies the above range, the stability of the positive electrode active material crystal structure is improved, and the resistance and lifespan of the battery can be improved by the increase in structural stability.
[0054] According to the present invention, in the chemical formula 1, e1 means the atomic fraction of yttrium among the metal elements in the lithium composite transition metal oxide, and may be 0 or more, 0.001 or more, 0.002 or less, 0.003 or less, 0.004 or less, 0.005 or less, 0.006 or less, 0.007 or less, 0.008 or less, 0.009 or less, or 0.01 or less. When e1 satisfies the above range, particle growthability can be improved, and capacity and lifetime can be improved.
[0055] According to the present invention, in the chemical formula 1, f1 means the atomic fraction of element M among the metal elements in the lithium composite transition metal oxide, and may be 0 or greater, and may be 0.01 or less, 0.02 or less, 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.10 or less. When f1 satisfies the above range, the stability of the positive electrode active material crystal structure is improved and the grain shape can be improved.
[0056] According to the present invention, the positive electrode active material further comprises a coating layer formed on the lithium composite transition metal oxide, and the coating layer may contain Al, W, or a combination thereof. In this case, the capacity and lifespan of the battery containing the positive electrode active material can be optimized.
[0057] According to the present invention, the Al content in the coating layer may be 1,000 ppm to 2,000 ppm relative to the total weight of the positive electrode active material. Specifically, the Al content may be 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, 1,300 ppm or more, or 1,400 ppm or more relative to the total weight of the positive electrode active material, and may also be 1,500 ppm or less, 1,600 ppm or less, 1,700 ppm or less, 1,800 ppm or less, 1,900 ppm or less, or 2,000 ppm or less. In this case, the electrical conductivity of the positive electrode active material is improved, the formation of by-products formed by side reactions with the electrolyte in the battery is suppressed, and the capacity characteristics, resistance characteristics, and life characteristics of the positive electrode active material can be improved.
[0058] According to the present invention, the W content in the coating layer may be 2,000 ppm to 4,000 ppm relative to the total weight of the positive electrode active material. Specifically, the W content may be 2,000 ppm or more, 2,100 ppm or more, 2,200 ppm or more, 2,300 ppm or more, 2,400 ppm or more, 2,500 ppm or more, 2,600 ppm or more, 2,700 ppm or more, 2,800 ppm or more, or 2,900 ppm or more relative to the total weight of the positive electrode active material, and may be 3,000 ppm or less, 3,100 ppm or less, 3,200 ppm or less, 3,300 ppm or less, 3,400 ppm or less, 3,500 ppm or less, 3,600 ppm or less, 3,700 ppm or less, 3,800 ppm or less, 3,900 ppm or less, or 4,000 ppm or less, relative to the total weight of the positive electrode active material. In this case, the electrical conductivity of the positive electrode active material is improved, the formation of by-products due to side reactions with the electrolyte in the battery is suppressed, and the capacitance characteristics, resistance characteristics, and life characteristics of the positive electrode active material can be improved.
[0059] Method for manufacturing positive electrode active material The positive electrode active material according to the present invention can be manufactured by the following method for manufacturing a positive electrode active material, but is not limited thereto.
[0060] The present invention provides a method for producing a positive electrode active material in single particle form, comprising the steps of (A) mixing a positive electrode active material precursor having a composition represented by the following chemical formula 2, a zirconium-containing raw material, a yttrium-containing raw material, and a lithium-containing raw material to produce a mixture, and (B) continuously firing the mixture in an atmospheric environment at 600°C to 850°C for primary firing, at 960°C to 970°C for secondary firing, and then at 500°C to 850°C for tertiary firing to produce a fired product.
[0061] [Chemical formula 2] Ni a2 Co b2 Mn c2 M 1 d2 (OH)2
[0062] In the aforementioned chemical formula 2, M 1is one or more selected from Zr, Y, W, Cu, Sr, Mn, Ti, Mg, Mo, B, Sn, Fe, Zn, Si, and Al. 0 <a2<1、0<b2<1、0<c2<1、0≦d2<0.1、a2+b2+c2+d2=1である。
[0063] The inventors of the present invention have discovered that when the mixture obtained by mixing the positive electrode active material precursor with a zirconium-containing raw material, a yttrium-containing raw material, and a lithium-containing raw material is subjected to primary calcination at 800°C to 900°C, secondary calcination at 940°C to 970°C, and tertiary calcination at 550°C to 650°C, a positive electrode active material with uniform particle size is produced, and there is less cracking of the positive electrode active material particles during rolling for the manufacture of lithium secondary batteries, thus completing the present invention.
[0064] (A) Step Step (A) is a step of mixing a positive electrode active material precursor having the composition represented by the chemical formula 2, a zirconium-containing raw material, a yttrium-containing raw material, and a lithium-containing raw material to produce a mixture.
[0065] According to the present invention, the positive electrode active material precursor may contain nickel (Ni) in an amount of 60 mol% or more relative to the total number of moles of transition metals contained in the positive electrode active material precursor. In this case, the energy density of the lithium secondary battery can be improved.
[0066] According to the present invention, in the chemical formula 2, a2 means the atomic fraction of nickel among the metal elements in the composite transition metal hydroxide, and may be 0.6 or more, 0.61 or more, or 0.62 or more, and may be 0.7 or less, 0.71 or less, 0.72 or less, 0.73 or less, 0.74 or less, 0.75 or less, 0.76 or less, 0.77 or less, 0.78 or less, 0.79 or less, 0.8 or less, 0.81 or less, 0.82 or less, 0.83 or less, 0.84 or less, 0.85 or less, 0.86 or less, 0.87 or less, 0.88 or less, 0.89 or less, 0.91 or less, 0.92 or less, 0.93 or less, 0.94 or less, 0.95 or less, 0.96 or less, 0.97 or less, 0.98 or less, 0.99 or less, or less than 1. When a2 satisfies the aforementioned range, the resulting battery containing the positive electrode active material can achieve high capacity characteristics. In particular, when a2 is between 0.6 and 0.75, the resulting battery containing the positive electrode active material exhibits high energy density and achieves high capacity characteristics when driven at high voltage.
[0067] According to the present invention, in the chemical formula 2, b2 represents the atomic fraction of cobalt among the metal elements in the composite transition metal hydroxide, and may be greater than 0, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, or 0.05 or more, and may be 0.10 or less, 0.11 or less, 0.12 or less, 0.13 or less, 0.14 or less, 0.15 or less, 0.16 or less, 0.17 or less, or 0.18. The following ranges may also be 0.19 or less, 0.20 or less, 0.21 or less, 0.22 or less, 0.23 or less, 0.24 or less, 0.25 or less, 0.26 or less, 0.27 or less, 0.28 or less, 0.29 or less, 0.30 or less, 0.31 or less, 0.32 or less, 0.33 or less, 0.34 or less, 0.35 or less, 0.36 or less, 0.37 or less, 0.38 or less, 0.39 or less, or less than 0.4. When b2 satisfies the above range, the stability during the charge-discharge process of the battery containing the resulting positive electrode active material can be improved and the rate characteristics can be enhanced.
[0068] According to the present invention, in the chemical formula 2, c2 represents the atomic fraction of manganese among the metal elements in the composite transition metal hydroxide, and can be greater than 0, 0.01 or more, 0.02 or more, 0.03 or more, 0.04 or more, 0.05 or more, 0.06 or more, 0.07 or more, 0.08 or more, 0.09 or more, 0.1 or more, 0.11 or more, 0.12 or more, 0.13 or more, 0.14 or more, 0.15 or more, 0.16 or more, or 0.17. The values may be 0.18 or higher, 0.19 or higher, 0.2 or higher, 0.21 or higher, 0.22 or higher, 0.23 or higher, 0.24 or higher, 0.25 or higher, 0.26 or higher, 0.27 or higher, 0.28 or higher, 0.29 or higher, or 0.30 or higher, and may also be 0.32 or lower, 0.33 or lower, 0.34 or lower, 0.35 or lower, 0.36 or lower, 0.37 or lower, 0.38 or lower, 0.39 or lower, or less than 0.4. When c2 satisfies the above range, high capacity characteristics can be achieved in the battery containing the resulting positive electrode active material. In addition, the high-temperature stability of the battery can be increased, and side reactions with the electrolyte can be relatively reduced.
[0069] According to the present invention, in the chemical formula 2, d2 is M among the metal elements in the composite transition metal hydroxide. 1 This refers to the atomic fraction of an element, and may be greater than or equal to 0, and may be 0.01 or less, 0.02 or less, 0.03 or less, 0.04 or less, 0.05 or less, 0.06 or less, 0.07 or less, 0.08 or less, 0.09 or less, or 0.10 or less. When d2 satisfies the above range, the crystalline structure stability of the resulting positive electrode active material is improved, and the grain shape can be improved.
[0070] According to the present invention, the lithium-containing raw material can be lithium-containing sulfates, nitrates, acetates, carbonates, oxalates, citrates, halides, hydroxides, or oxyhydroxides, and is not particularly limited as long as it is soluble in water. Specifically, the lithium-containing raw material may be Li2CO3, LiNO3, LiNO2, LiOH, LiOH·H2O, LiH, LiF, LiCl, LiBr, LiI, CH3COOLi, Li2O, Li2SO4, CH3COOLi, or Li3C6H5O7, and one or more of these can be used as a mixture.
[0071] According to the present invention, the positive electrode active material precursor and the lithium-containing raw material can be mixed such that the ratio (M:Li) of the total number of moles of transition metal (M) contained in the positive electrode active material precursor to the number of moles of lithium (Li) contained in the lithium-containing raw material is 1:1.03 to 1.07. In this case, the resulting positive electrode active material can have the desired primary particle size, and the battery life and resistance characteristics can be improved.
[0072] According to the present invention, the zirconium (Zr)-containing raw material is Zr(OH)4, ZrO2, Zr(NO3)4, ZrCl4, ZrS2, Zr(SO4)2, and C8H 12 It may be one or more selected from O8Zr, specifically one or more selected from ZrO2, Zr(OH)4 and Zr(NO3)4, and more specifically ZrO2.
[0073] According to the present invention, the zirconium-containing raw material can be added in an amount such that the zirconium content is 1,000 ppm to 4,000 ppm relative to the total weight of the positive electrode active material precursor. Specifically, the zirconium-containing raw material can contain zirconium in amounts of 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, 1,300 ppm or more, or 1,400 ppm or more, as well as 1,500 ppm or less, 1,600 ppm or less, 1,700 ppm or less, 1,800 ppm or less, 1,900 ppm or less, 2,000 ppm or less, 2,100 ppm or less, 2,200 ppm or less, 2,300 ppm or less, relative to the total weight of the composite transition metal hydroxide. It can be added in amounts such that the concentration is 0 ppm or less, 2,400 ppm or less, 2,500 ppm or less, 2,600 ppm or less, 2,700 ppm or less, 2,800 ppm or less, 2,900 ppm or less, 3,000 ppm or less, 3,100 ppm or less, 3,200 ppm or less, 3,300 ppm or less, 3,400 ppm or less, 3,500 ppm or less, 3,600 ppm or less, 3,700 ppm or less, 3,800 ppm or less, 3,900 ppm or less, or 4,000 ppm or less. In this case, Zr is stably doped into the transition metal layer, and a stable structure can be maintained even if lithium is repeatedly inserted and removed as charging and discharging are repeated.
[0074] According to the present invention, the yttrium (Y)-containing raw material may be one or more selected from YCl3, Y2O3, Y(NO3)3, Y(OH)3, YSZ, Y2(SO4)3, and Y2S3, and more specifically one or more selected from Y2O3, Y(OH)3, and YSZ, and more specifically Y2O3.
[0075] According to the present invention, the yttrium-containing raw material can be added in an amount such that the yttrium content is 1,000 ppm to 4,000 ppm relative to the total weight of the positive electrode active material precursor. Specifically, the yttrium-containing raw material can be added in an amount such that the yttrium content is 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, 1,300 ppm or more, 1,400 ppm or more, 1,500 ppm or more, 1,600 ppm or more, 1,700 ppm or more, 1,800 ppm or more, 1,900 ppm or more, 2,000 ppm or more, 2,100 ppm or more, 2,200 ppm or more, 2,300 ppm or more, and 2,400 ppm relative to the total weight of the composite transition metal hydroxide. Y can be added in amounts such that the concentration is m or more, 2,500 ppm or more, 2,600 ppm or more, 2,700 ppm or more, 2,800 ppm or more, or 2,900 ppm or more, or 3,000 ppm or less, 3,100 ppm or less, 3,200 ppm or less, 3,300 ppm or less, 3,400 ppm or less, 3,500 ppm or less, 3,600 ppm or less, 3,700 ppm or less, 3,800 ppm or less, 3,900 ppm or less, or 4,000 ppm or less. In this case, Y acts as a flux material during calcination, enabling the achievement of the optimal primary particle size even at relatively low temperatures, which is advantageous for resistance and rate-limiting characteristics.
[0076] (B) Step Step (B) is a step in which the mixture is first fired at 600°C to 850°C in an atmospheric atmosphere, then secondly fired at 960°C to 970°C, and finally tertiarily fired at 500°C to 850°C to produce a fired product.
[0077] According to the present invention, when the mixture is first calcined at 600°C to 850°C, the lithium-containing raw material melts and is sufficiently and uniformly distributed on the surface of the precursor, thereby allowing lithium and the precursor to react effectively and producing an active material having a uniform primary particle shape. Specifically, the first calcination temperature may be 600°C or higher, 650°C or higher, 700°C or higher, or 750°C or higher, or 800°C or lower, or 850°C or lower. When the first calcination temperature is within the above range, the lithium-containing raw material melts and can be sufficiently and uniformly distributed on the surface of the precursor. On the other hand, when the first calcination temperature is below 600°C, there is a problem that the lithium-containing raw material cannot melt sufficiently, and when it is above 850°C, the lithium-containing raw material intercalates into the interior of the precursor before it can melt and be sufficiently and uniformly distributed, and an active material having a relatively non-uniform shape can be produced.
[0078] According to the present invention, the primary calcination is carried out in an atmospheric environment for the uniform distribution of lithium-containing raw materials.
[0079] According to the present invention, the primary calcination may be carried out for 1 to 8 hours. In this case, the lithium-containing raw material can melt and be sufficiently and uniformly distributed on the surface of the precursor.
[0080] Immediately after the completion of the primary firing, the temperature is continuously raised to 960°C to 970°C for secondary firing. This causes lithium to intercalate within the precursor, forming a layered structure, which unites the primary particle interfaces and promotes primary particle growth. When the secondary firing temperature is within the aforementioned range, the optimal primary particle size can be achieved, resulting in optimal performance in terms of particle cracking, rolling density, battery capacity, resistance, and lifespan. On the other hand, if the secondary firing temperature is below 960°C, the primary particle size becomes smaller, leading to problems with particle cracking and rolling density. If the temperature exceeds 970°C, the primary particle size becomes larger, resulting in problems with efficiency and resistance performance.
[0081] The aforementioned secondary firing is carried out in an atmospheric environment, which is suitable for the proper growth of the primary particles.
[0082] According to the present invention, the secondary calcination may be carried out for 3 to 12 hours. In this case, lithium can be sufficiently intercalated into the precursor, and the primary particles can be grown appropriately.
[0083] Immediately after the completion of the secondary firing, the temperature is continuously raised to 500°C to 850°C, and a tertiary firing is performed at 500°C to 850°C. This mitigates defects in the active material crystal structure that occurred due to the high temperature of the secondary firing, resulting in a fired product with fewer structural defects. The tertiary firing temperature may be, specifically, 500°C or higher, 510°C or higher, 520°C or higher, 530°C or higher, 540°C or higher, 550°C or higher, 560°C or higher, 570°C or higher, 580°C or higher, 590°C or higher, or 600°C or higher, and may also be 650°C or lower, 660°C or lower, 670°C or lower, 680°C or lower, 690°C or lower, 700°C or lower, 710°C or lower, 720°C or lower, 730°C or lower, 740°C or lower, 750°C or lower, 760°C or lower, 770°C or lower, 780°C or lower, 790°C or lower, 800°C or lower, 810°C or lower, 820°C or lower, 830°C or lower, 840°C or lower, or 850°C or lower. Here, the fired product is a lithium composite transition metal oxide in single-particle form. When the tertiary firing temperature is within the above range, structural defects can be effectively mitigated. On the other hand, if the tertiary firing temperature is below 500°C or above 850°C, structural defects cannot be effectively mitigated.
[0084] The aforementioned tertiary firing is carried out in an atmospheric environment in order to minimize structural defects.
[0085] According to the present invention, the tertiary firing may be carried out for 1 to 8 hours. In this case, defects in the crystal structure can be minimized.
[0086] The method for producing a positive electrode active material according to the present invention may further include (C) a step of finely grinding the calcined product, in terms of producing an effective electrode and efficient reaction at the active material-electrolyte interface. The fine grinding is performed by measuring the D of the positive electrode active material with a PSA (particle size analyzer). 50 The process may be carried out so that the thickness is between 3.5 μm and 4.0 μm.
[0087] According to the present invention, the fine grinding may be performed by airflow grinding. In this case, not only is the grinding efficiency better than existing physical grinding methods, but heat is not generated, and surface deformation of the active material can be suppressed.
[0088] According to the present invention, the airflow grinding may be carried out under a pressure of 1 bar to 5 bar. In this case, the target particle size can be effectively achieved.
[0089] The method for producing a positive electrode active material according to the present invention may further include the step of (C') mixing the calcined product with one or more selected from aluminum raw materials and tungsten raw materials, then heat-treating the mixture to form a coating layer on the calcined product containing one or more selected from Al and W. In this case, a coating portion containing one or more selected from Al and W is formed on the calcined product (single-particle lithium composite transition metal oxide).
[0090] According to the present invention, the aluminum raw material may be one or more selected from Al2O3, Al(OH)3, AlCl3, AlF3, and Al2(SO4)3, more specifically one or more selected from Al2O3, Al(OH)3, and AlF3, and more specifically Al2O3.
[0091] According to the present invention, the aluminum raw material can be added in an amount such that the aluminum content is 1,000 ppm to 2,000 ppm relative to the total weight of the fired product. Specifically, the aluminum raw material can be added in an amount such that the aluminum content is 1,000 ppm or more, 1,100 ppm or more, 1,200 ppm or more, 1,300 ppm or more, or 1,400 ppm or more, or 1,500 ppm or less, 1,600 ppm or less, 1,700 ppm or less, 1,800 ppm or less, 1,900 ppm or less, or 2,000 ppm or less relative to the total weight of the fired product.
[0092] In this case, the capacity retention rate due to charging and discharging can be improved.
[0093] According to the present invention, the tungsten raw material may be one or more selected from WO3, WC, and H2WO4, and more specifically, it may be WO3.
[0094] According to the present invention, the tungsten raw material can be added in an amount such that the tungsten content is 2,000 ppm to 4,000 ppm relative to the total weight of the calcined product. Specifically, the tungsten raw material can be added in an amount such that the tungsten content is 2,000 ppm or more, 2,100 ppm or more, 2,200 ppm or more, 2,300 ppm or more, 2,400 ppm or more, 2,500 ppm or more, 2,600 ppm or more, 2,700 ppm or more, 2,800 ppm or more, or 2,900 ppm or more, or 3,000 ppm or less, 3,100 ppm or less, 3,200 ppm or less, 3,300 ppm or less, 3,400 ppm or less, 3,500 ppm or less, 3,600 ppm or less, 3,700 ppm or less, 3,800 ppm or less, 3,900 ppm or less, or 4,000 ppm or less, relative to the total weight of the calcined product. In this case, the output performance can be improved when the battery is running.
[0095] According to the present invention, the heat treatment can be performed at 400°C to 600°C. In this case, the lifespan performance of the positive electrode active material can be further improved.
[0096] According to the present invention, the heat treatment can be performed in an atmospheric environment on the surface for stabilization.
[0097] According to the present invention, the heat treatment may be performed for 3 to 12 hours. In this case, surface stabilization of the positive electrode active material suppresses side reactions between the positive electrode active material and the electrolyte as charging and discharging are repeated, thereby improving the battery's lifespan performance.
[0098] positive electrode The present invention provides a positive electrode containing the positive electrode active material.
[0099] The positive electrode may include a positive electrode current collector and a positive electrode active material layer formed on the positive electrode current collector, and the positive electrode active material layer may include the positive electrode active material.
[0100] The positive electrode current collector is not particularly limited as long as it contains a highly conductive metal, allows for easy adhesion of the positive electrode active material layer, and is unreactive within the battery voltage range. Examples of materials that can be used for the positive electrode current collector include stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with surface treatments such as carbon, nickel, titanium, or silver. Furthermore, the positive electrode current collector can typically have a thickness of 3 μm to 500 μm, and fine irregularities can be formed on its surface to enhance the adhesion of the positive electrode active material. It can be used in various forms, such as films, sheets, foils, meshes, porous materials, foams, and nonwoven fabrics.
[0101] The positive electrode active material layer may optionally contain a conductive material and a binder along with the positive electrode active material. Here, the positive electrode active material can be included in an amount of 80% to 99% by weight, more specifically 85% to 98.5% by weight, relative to the total weight of the positive electrode active material layer, and excellent capacity performance can be observed within this range.
[0102] The conductive material is used to impart conductivity to the electrodes and can be used without particular limitations in the battery it is configured in, as long as it does not cause chemical changes and has electronic conductivity. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, and carbon fiber; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive tubes such as carbon nanotubes; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. Of these, one or more can be used. The conductive material can be included in an amount of 0.1% to 15% by weight relative to the total weight of the positive electrode active material layer.
[0103] The binder plays a role in improving the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the current collector. Specific examples include polyvinylidene fluoride (PVDF), polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, polymethyl methacrylate, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, polyacrylic acid, and polymers in which the hydrogen atoms of these materials are substituted with Li, Na, or Ca, or various copolymers thereof. One of these materials alone or a mixture of two or more materials can be used. The binder can be present in an amount of 0.1% to 15% by weight relative to the total weight of the positive electrode active material layer.
[0104] The positive electrode can be manufactured by a conventional method for manufacturing a positive electrode, except that the positive electrode active material is used. Specifically, the positive electrode can be manufactured by coating a positive electrode active material layer-forming composition, which is prepared by dissolving or dispersing the positive electrode active material and, if necessary, selectively, a binder, a conductive material, and a dispersant in a solvent, onto a positive electrode current collector, followed by drying and rolling; or by casting the positive electrode active material layer-forming composition onto another support, peeling it off the support, and laminating the resulting film onto the positive electrode current collector.
[0105] The solvent can be any solvent commonly used in the art, such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), dimethylformamide (DMF), acetone, or water, and one or more of these can be used individually or in mixtures of two or more. The amount of solvent used should be sufficient to dissolve or disperse the positive electrode active material, conductive material, binder, and dispersant, taking into consideration the coating thickness of the slurry and the manufacturing yield, and to have a viscosity that allows for excellent thickness uniformity when applied for the manufacture of the positive electrode.
[0106] Lithium-ion battery The present invention provides a lithium secondary battery comprising a positive electrode, a negative electrode, a separator interposed between the positive electrode and the negative electrode, and an electrolyte.
[0107] The lithium secondary battery may further optionally include a battery container for housing the electrode assembly comprising the positive electrode, negative electrode, and separator, and a sealing member for sealing the battery container.
[0108] The negative electrode may include a negative electrode current collector and a negative electrode active material layer located on the negative electrode current collector.
[0109] The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel with surface treatment using carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloys can be used. The negative electrode current collector can usually have a thickness of 3 μm to 500 μm, and, similar to the positive electrode current collector, fine irregularities can be formed on the surface of the current collector to strengthen the bonding force of the negative electrode active material. For example, it can be used in various forms such as film, sheet, foil, mesh, porous material, foam, and nonwoven fabric.
[0110] The negative electrode active material layer may selectively include a binder and a conductive material along with the negative electrode active material.
[0111] As the negative electrode active material, compounds capable of reversible intercalation and deintercalation of lithium can be used. Specific examples include carbonaceous materials such as artificial graphite, natural graphite, graphitized carbon fiber, and amorphous carbon; metallic compounds capable of alloying with lithium, such as Si, Al, Sn, Pb, Zn, Bi, In, Mg, Ga, Cd, Si alloys, Sn alloys, or Al alloys; and SiO2. β Examples include metallic oxides that can be doped and dedoped with lithium, such as (0<β<2), SnO2, vanadium oxide, and lithium vanadium oxide; or composites containing the metallic compound and carbonaceous material, such as Si-C composites or Sn-C composites, and any one or more mixtures thereof can be used. A metallic lithium thin film can also be used as the negative electrode active material. Furthermore, both low-crystallinity carbon and high-crystallinity carbon can be used as the carbon material. Typical low-crystalline carbons include soft carbon and hard carbon, while typical high-crystalline carbons include amorphous, plate-like, flaky, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and high-temperature calcined carbons such as petroleum or coal tar pitch-derived cokes. The anode active material can be present in an amount of 80% to 99% by weight relative to the total weight of the anode active material layer.
[0112] The binder in the negative electrode active material layer is a component that helps to bond the conductive material, active material, and current collector, and is usually added in an amount of 0.1% to 10% by weight relative to the total weight of the negative electrode active material layer. Examples of such binders include polyvinylidene fluoride (PVDF), polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene polymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, nitrile-butadiene rubber, fluororubber, and various copolymers thereof.
[0113] The conductive material in the negative electrode active material layer is a component for further improving the conductivity of the negative electrode active material, and may be included in an amount of 10% by weight or less, preferably 5% by weight or less, relative to the total weight of the negative electrode active material layer. Such conductive material is not particularly limited as long as it does not cause a chemical change in the battery and is conductive, and for example, graphite such as natural graphite or artificial graphite; carbon black such as acetylene black, Ketjen black, channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; carbon fluoride; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives can be used.
[0114] The negative electrode can be manufactured by coating a negative electrode active material layer-forming composition, which is prepared by dissolving or dispersing a negative electrode active material and a binder and conductive material selectively in a solvent, onto a negative electrode current collector and then drying it, or by casting the negative electrode active material layer-forming composition onto another support, peeling it off the support, and then laminating the resulting film onto the negative electrode current collector.
[0115] The separator separates the negative and positive electrodes and provides a passage for lithium ions to move. It can be used without particular limitations as long as it is a separator commonly used in lithium secondary batteries. Particularly preferred is one that exhibits low resistance to ion movement in the electrolyte and has excellent electrolyte moisture absorption capacity. Specifically, porous polymer films, such as polyolefin polymers like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or laminated structures of two or more layers thereof, can be used. Alternatively, ordinary porous nonwoven fabrics, such as nonwoven fabrics made of high-melting-point glass fibers or polyethylene terephthalate fibers, can also be used. Furthermore, coated separators containing ceramic components or polymeric substances may be used to ensure heat resistance or mechanical strength, and can be selectively used in single-layer or multi-layer structures.
[0116] Examples of the electrolyte include, but are not limited to, organic liquid electrolytes, inorganic liquid electrolytes, solid polymer electrolytes, gel-type polymer electrolytes, solid inorganic electrolytes, and molten inorganic electrolytes that can be used in the manufacture of lithium secondary batteries. Specifically, the electrolyte may contain an organic solvent and a lithium salt.
[0117] The organic solvent can be used without particular limitations, as long as it can act as a medium through which ions involved in the electrochemical reaction of the battery can move. Specifically, the organic solvents include ester solvents such as methyl acetate, ethyl acetate, γ-butyrolactone, and ε-caprolactone; ether solvents such as dibutyl ether or tetrahydrofuran; ketone solvents such as cyclohexanone; aromatic hydrocarbon solvents such as benzene and fluorobenzene; dimethyl carbonate (DMC), diethyl carbonate (DEC), ethyl methyl carbonate (EMC), ethylene carbonate (EC), and propylene carbonate (propylene Carbonate solvents such as carbonate (PC); alcoholic solvents such as ethyl alcohol and isopropyl alcohol; nitriles such as R-CN (where R is a linear, branched, or cyclic hydrocarbon group having 2 to 20 carbon atoms, and can include a double-bonded aromatic ring or ether bond); amides such as dimethylformamide; dioxolanes such as 1,3-dioxolane; or sulfolanes can be used. Among these, carbonate solvents are preferred, and a mixture of a cyclic carbonate (e.g., ethylene carbonate or propylene carbonate) having high ionic conductivity and high dielectric constant that can improve the charge and discharge performance of the battery, and a low-viscosity linear carbonate compound (e.g., ethyl methyl carbonate, dimethyl carbonate, or diethyl carbonate) is more preferred.
[0118] The lithium salt can be used without particular limitations as long as it is a compound that can provide lithium ions for use in lithium secondary batteries. Specifically, the anion of the lithium salt is F - Cl - , Br - , I - NO3 - , N(CN)2 - BF4 - CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - CF3CF2(CF3)2CO - (CF3SO2) 2CH - (SF5)3C - (CF3SO2)3C - CF3(CF2)7SO3 - CF3CO2 - CH3CO2 - SCN - and (CF3CF2SO2)2N - The lithium salt can be selected from the group consisting of LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2, etc. The concentration of the lithium salt is preferably in the range of 0.1M to 2.0M. When the concentration of the lithium salt falls within this range, the electrolyte can exhibit excellent electrolyte performance due to having appropriate conductivity and viscosity, and lithium ions can move effectively.
[0119] In addition to the components of the electrolyte, the electrolyte may also contain one or more additives for purposes such as improving battery life, suppressing the decrease in battery capacity, and improving battery discharge capacity. These additives may include, for example, haloalkylene carbonate compounds such as difluoroethylene carbonate, pyridine, triethyl phosphite, triethyl alcoholamine, cyclic ethers, ethylenediamine, n-glyme, hexaphosphate triamide, nitrobenzene derivatives, sulfur, quinone imine dyes, N-substituted oxazolidinone, N,N-substituted imidazolidine, ethylene glycol dialkyl ether, ammonium salts, pyrrole, 2-methoxyethyl alcohol, or aluminum trichloride. Here, the additives may be present in an amount of 0.1% to 5% by weight relative to the total weight of the electrolyte.
[0120] The lithium secondary battery containing the positive electrode active material according to the present invention has excellent performance and is therefore useful in fields such as portable devices like mobile phones, notebook computers, and digital cameras, as well as electric vehicles such as hybrid electric vehicles (HEVs) and electric vehicles (EVs).
[0121] The external shape of the lithium secondary battery of the present invention is not particularly limited, but may be cylindrical, rectangular, pouch-type, or coin-type, using a can.
[0122] The lithium secondary battery according to the present invention can be used not only as a battery cell used as a power source for small devices, but also preferably as a unit battery in medium- and large-sized battery modules containing a large number of battery cells.
[0123] Therefore, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0124] The aforementioned battery module or battery pack can be used as a power source for one or more medium-to-large devices, including power tools; electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); or power storage systems. [Examples]
[0125] Hereinafter, embodiments of the present invention will be described in detail so that they can be easily implemented by a person with ordinary skill in the art to which the present invention pertains. However, the present invention can be realized in various different forms and is not limited to the embodiments described herein.
[0126] Examples and Comparative Examples Example 1 In an acoustic mixer, tens to hundreds of primary particles aggregate to form a composite transition metal hydroxide (composition: Ni) in the form of secondary particles. 0.62 Co 0.06 Mn 0.32 (OH)2, D 50 A mixture was prepared by adding 3.5 μm of nitrate, ZrO2 (in an amount such that Zr constitutes 1500 ppm relative to the total weight of the composite transition metal hydroxide), and Y2O3 (in an amount such that Y constitutes 3000 ppm relative to the total weight of the composite transition metal hydroxide), and mixing sequentially at 40 g (g: acceleration due to gravity) for 2 minutes, 80 g for 1 minute, and 50 g for 2 minutes. Subsequently, Li2CO3 was added to the acoustic mixer in such a ratio ((Ni+Co+Mn):Li) of the total number of moles of transition metals in the composite transition metal hydroxide (Ni+Co+Mn) to the number of moles of lithium in the Li2CO3 ((Ni+Co+Mn):Li) that was 1:1.05, and mixing sequentially at 40 g (g: acceleration due to gravity) for 2 minutes, 80 g for 1 minute, and 50 g for 2 minutes to produce a mixture.
[0127] The mixture was placed in a rectangular alumina crucible (150 mm x 150 mm), and then subjected to primary firing at 850°C for 4 hours under an air atmosphere. The temperature was then continuously increased to 965°C (heating rate: 1.3°C / min), followed by secondary firing at 965°C for 6 hours. The temperature was then continuously decreased to 600°C (cooling rate: 4°C / min), followed by tertiary firing at 600°C for 3 hours to produce the fired product.
[0128] The aforementioned fired product was finely ground using a jet mill (Isaacenc, 2-inch Air Jet Mill) at 4 bar for 10 minutes.
[0129] The finely ground calcined product was mixed with Al2O3 (added in an amount such that Al constitutes 1500 ppm of the total weight of the calcined product) and WO3 (added in an amount such that W constitutes 3000 ppm of the total weight of the calcined product), and then heat-treated at 500°C under an air atmosphere to produce a positive electrode active material containing a coating layer containing Al and W.
[0130] Example 2 In an acoustic mixer, tens to hundreds of primary particles aggregate to form a composite transition metal hydroxide (composition: Ni) in the form of secondary particles. 0.62 Co 0.06 Mn 0.32 (OH)2, D 50 A mixture was prepared by adding 3.5 μm of nitrate, ZrO2 (in an amount such that Zr constitutes 1500 ppm relative to the total weight of the composite transition metal hydroxide), and Y2O3 (in an amount such that Y constitutes 3000 ppm relative to the total weight of the composite transition metal hydroxide), and mixing sequentially at 40 g (g: acceleration due to gravity) for 2 minutes, 80 g for 1 minute, and 50 g for 2 minutes. Subsequently, Li2CO3 was added to the acoustic mixer in such a ratio ((Ni+Co+Mn):Li) of the total number of moles of transition metals in the composite transition metal hydroxide (Ni+Co+Mn) to the number of moles of lithium in the Li2CO3 ((Ni+Co+Mn):Li) that was 1:1.04, and mixing sequentially at 40 g (g: acceleration due to gravity) for 2 minutes, 80 g for 1 minute, and 50 g for 2 minutes to produce the mixture.
[0131] The mixture was placed in a rectangular alumina crucible (150 mm x 150 mm), and then subjected to primary firing at 850°C for 4 hours under an air atmosphere. The temperature was then continuously increased to 965°C (heating rate: 1.3°C / min), followed by secondary firing at 965°C for 6 hours. The temperature was then continuously decreased to 600°C (cooling rate: 4°C / min), followed by tertiary firing at 600°C for 3 hours to produce the fired product.
[0132] The aforementioned fired product was finely ground using a jet mill (Isaacenc, 2-inch Air Jet Mill) at 4 bar for 10 minutes.
[0133] The finely ground calcined product was mixed with Al2O3 (added in an amount such that Al constitutes 1500 ppm of the total weight of the calcined product) and WO3 (added in an amount such that W constitutes 3000 ppm of the total weight of the calcined product), and then heat-treated at 500°C under an air atmosphere to produce a positive electrode active material containing a coating layer containing Al and W.
[0134] Example 3 In an acoustic mixer, tens to hundreds of primary particles aggregate to form a composite transition metal hydroxide (composition: Ni) in the form of secondary particles. 0.62 Co 0.06 Mn 0.32 (OH)2, D 50 A mixture was prepared by adding 3.5 μm of nitrate, ZrO2 (added in an amount such that Zr constitutes 1500 ppm relative to the total weight of the composite transition metal hydroxide), and Y2O3 (added in an amount such that Y constitutes 3000 ppm relative to the total weight of the composite transition metal hydroxide), and mixing sequentially at 40 g (g: acceleration due to gravity) for 2 minutes, 80 g for 1 minute, and 50 g for 2 minutes. After that, Li2CO3 was added to the acoustic mixer in such a ratio that the total number of moles of transition metals (Ni+Co+Mn) contained in the composite transition metal hydroxide to the number of moles of lithium (Li) contained in the Li2CO3 ((Ni+Co+Mn):Li) was 1:1.06, and mixing sequentially at 40 g (g: acceleration due to gravity) for 2 minutes, 80 g for 1 minute, and 50 g for 2 minutes to produce a mixture.
[0135] The mixture was placed in a rectangular alumina crucible (150 mm x 150 mm), and then subjected to primary firing at 850°C for 4 hours under an air atmosphere. The temperature was then continuously increased to 965°C (heating rate: 1.3°C / min), followed by secondary firing at 965°C for 6 hours. The temperature was then continuously decreased to 600°C (cooling rate: 4°C / min), followed by tertiary firing at 600°C for 3 hours to produce the fired product.
[0136] The aforementioned fired product was finely ground using a jet mill (Isaacenc, 2-inch Air Jet Mill) at 4 bar for 10 minutes.
[0137] The finely ground calcined product was mixed with Al2O3 (added in an amount such that Al constitutes 1500 ppm of the total weight of the calcined product) and WO3 (added in an amount such that W constitutes 3000 ppm of the total weight of the calcined product), and then heat-treated at 500°C under an air atmosphere to produce a positive electrode active material containing a coating layer containing Al and W.
[0138] Comparative Example 1 In an acoustic mixer, tens to hundreds of primary particles aggregate to form a composite transition metal hydroxide (composition: Ni) in the form of secondary particles. 0.62 Co 0.06 Mn 0.32 (OH)2, D 50 A mixture was prepared by adding 3.5 μm of nitrate, ZrO2 (in an amount such that Zr constitutes 1500 ppm relative to the total weight of the composite transition metal hydroxide), and Y2O3 (in an amount such that Y constitutes 3000 ppm relative to the total weight of the composite transition metal hydroxide), and mixing sequentially at 40 g (g: acceleration due to gravity) for 2 minutes, 80 g for 1 minute, and 50 g for 2 minutes. Subsequently, Li2CO3 was added to the acoustic mixer in such a ratio ((Ni+Co+Mn):Li) of the total number of moles of transition metals in the composite transition metal hydroxide (Ni+Co+Mn) to the number of moles of lithium in the Li2CO3 ((Ni+Co+Mn):Li) that was 1:1.05, and mixing sequentially at 40 g (g: acceleration due to gravity) for 2 minutes, 80 g for 1 minute, and 50 g for 2 minutes to produce a mixture.
[0139] After the mixture was charged into a square alumina crucible (150 mm × 150 mm), primary calcination was performed at 850°C for 4 hours in an air atmosphere, followed by continuous heating to 955°C (heating rate: 1.3°C / min), secondary calcination at 955°C for 6 hours, continuous cooling to 600°C (cooling rate: 4°C / min), and tertiary calcination at 600°C for 3 hours to produce a calcined product.
[0140] The calcined product was finely pulverized for 10 minutes under 4 bar using a jet mill (manufactured by isaacenc, 2 inch Air Jet Mill).
[0141] The finely pulverized calcined product was mixed with Al₂O₃ (added in an amount such that Al accounts for 1500 ppm relative to the total weight of the calcined product) and WO₃ (added in an amount such that W accounts for 3000 ppm relative to the total weight of the calcined product), and then heat-treated at 500°C in an air atmosphere to produce a positive electrode active material comprising a coating layer containing Al and W.
[0142] Comparative Example 2 A composite transition metal hydroxide in the form of secondary particles formed by aggregation of several tens to several hundreds of primary particles (composition: Ni 0.62 Co 0.06 Mn 0.32 (OH)₂, D 50 : 3.5 μm), ZrO₂ (added in an amount such that Zr accounts for 1500 ppm relative to the total weight of the composite transition metal hydroxide) and Y₂O₃ (added in an amount such that Y accounts for 3000 ppm relative to the total weight of the composite transition metal hydroxide) were sequentially mixed at 40 g (g: gravitational acceleration) for 2 minutes, at 80 g for 1 minute, and at 50 g for 2 minutes. Thereafter, Li₂CO₃ was charged into the acoustic mixer such that the ratio ((Ni+Co+Mn):Li) of the total number of moles of transition metals (Ni+Co+Mn) contained in the composite transition metal hydroxide to the number of moles of lithium (Li) contained in Li₂CO₃ was 1:1.05, and the mixture was sequentially mixed at 40 g (g: gravitational acceleration) for 2 minutes, at 80 g for 1 minute, and at 50 g for 2 minutes to prepare a mixture.
[0143] The mixture was placed in a rectangular alumina crucible (150 mm x 150 mm), and then subjected to primary firing at 850°C for 4 hours under an air atmosphere. The temperature was then continuously increased to 975°C (heating rate: 1.3°C / min), followed by secondary firing at 975°C for 6 hours. The temperature was then continuously decreased to 600°C (cooling rate: 4°C / min), followed by tertiary firing at 600°C for 3 hours to produce the fired product.
[0144] The aforementioned fired product was finely ground using a jet mill (Isaacenc, 2-inch Air Jet Mill) at 4 bar for 10 minutes.
[0145] The finely ground calcined product was mixed with Al2O3 (added in an amount such that Al constitutes 1500 ppm of the total weight of the calcined product) and WO3 (added in an amount such that W constitutes 3000 ppm of the total weight of the calcined product), and then heat-treated at 500°C under an air atmosphere to produce a positive electrode active material containing a coating layer containing Al and W.
[0146] Experimental example Experimental Example 1: Analysis of the shape of the positive electrode active material SEM (Inspect F, manufactured by FEI) was used to obtain SEM images of the cathode active materials produced in Examples 1 and 3. The SEM image of the cathode active material of Example 1 is shown in Figure 1, and the SEM image of the cathode active material of Example 3 is shown in Figure 2.
[0147] Referring to Figures 1 and 2, it can be confirmed that the positive electrode active materials of Examples 1 and 3 are in single-particle form.
[0148] Experimental Example 2: ICP Analysis 0.1 g each of the calcined products (hereinafter referred to as lithium complex transition metal oxide) produced in the examples and comparative examples were taken, and 1 ml of hydrochloric acid was added and heated to dissolve the lithium complex transition metal oxide. Then, to accelerate the reaction, a small amount of hydrogen peroxide was added to completely dissolve the lithium complex transition metal oxide and prepare a solution. Next, the solution was diluted with deionized water to a total volume of 10 ml to prepare the analytical sample. Using an ICP instrument (ICP-OES; Agilent 5110, manufactured by Agilent Technologies), the weight ratio of the constituent elements present in the analytical sample was measured, and the composition of the lithium complex transition metal oxide, the Zr content (ppm) and Y content (ppm) present in the lithium complex transition metal oxide are shown in Table 1 below.
[0149] [Table 1]
[0150] Referring to Table 1, it was confirmed that the lithium composite transition metal oxides produced in Examples 1 to 3 have the composition represented by Chemical Formula 1 as described herein and contain the doping elements Zr and Y.
[0151] Experimental Example 3: Analysis of the particle size of the positive electrode active material (1) Using a SEM (FEI, Inspect F), SEM images of the cathode active materials produced in the examples and comparative examples were acquired. An image processing program (LG Chem, DX program) was then used to separate the boundaries of primary particles present in the SEM images and obtain images showing them in random colors.
[0152] Using an image in which the boundaries of the primary particles are separated and shown in random colors, the area of each primary particle is calculated based on the number of pixels corresponding to each of the n primary particles (an average of 50,000 or more primary particles), and the radius (r) of a circle having the same area as each of the primary particles is calculated. i Using ), the particle size (D) of each primary particle present in the SEM image i =2r i), the area of primary particles having a particle size of 1 μm or less among the primary particles is summed to obtain the sum of the areas of the primary particles having a particle size of 1 μm or less, the areas of all primary particles are summed to obtain the sum of the areas of all primary particles, then the ratio of small particles is determined by Equation 1 described in the present specification, and the results are shown in Table 2 below.
[0153] Furthermore, using an image in which the boundaries of the primary particles are divided and displayed in random colors, the area of each of the n primary particles (on average 50,000 or more primary particles) is calculated from the number of pixels corresponding to each primary particle, and the radius (r of a circle having the same area as the area of each of the primary particles i ) is used to determine the particle size (D of each primary particle present on the SEM image i =2r i ) and the volume (V i =4 / 3×πr i 3 ), the particle size at the point corresponding to 50% of the volume cumulative distribution by particle size is calculated to determine the D of the primary particles v,50 value, and the results are shown in Table 2 below.
[0154] Experimental Example 4: Analysis of Particle Size of Positive Electrode Active Material (2) After taking 0.01 g of each positive electrode active material (powder) produced in Examples and Comparative Examples, each was placed in a vial containing 30 mL of ultrapure water and 500 μL of a dispersant, the positive electrode active material was dispersed for 1 minute with a sonicator, and then analyzed using a PSA (manufactured by Microtrac, S3500), and D 50 was confirmed, and the results are shown in Table 2 below.
[0155] Here, D 50 means the particle size at the 50% point of the volume cumulative distribution by particle size.
[0156] Experimental Example 5: Evaluation of Fine Powder Generation Amount Three g of each positive electrode active material (powder) produced in the examples and comparative examples were taken, placed in a mold with an inner diameter of 13 mm, and pressurized at 9 tons for 1 minute. The number of particles with a particle size of less than 1 μm was then checked using a PSA (Microtrac S3500). The ratio of the number of particles with a particle size of less than 1 μm to the total number of particles (hereinafter referred to as the amount of fine powder generated) was calculated and is shown in Table 2 below.
[0157] Experimental Example 6: Measurement of Rolling Density 5g each of the positive electrode active material (powder) produced in the examples and comparative examples was taken, placed in a mold with an inner diameter of 20mm, and pressurized with 2 tons for 1 minute. The height of the mold after pressurization was then measured. The volume of the 5g positive electrode active material after pressure was calculated from this height, and the weight of the active material per unit volume after pressurization, i.e., the rolling density, was determined and is shown in Table 2 below.
[0158] [Table 2]
[0159] Referring to Table 2 above, the positive electrode active materials of Examples 1 to 3 satisfy the range of 5% to 10% for the proportion of small particles, and the primary particle D v,50 While the size of the particles satisfies 2.2 μm to 3.7 μm, the positive electrode active material of Comparative Example 1 had a high proportion of small particles, exceeding 10%, and the primary particle D v,50 It can be confirmed that the size is less than 2.2 μm. In addition, the positive electrode active material of Comparative Example 2 has a low proportion of small particles, less than 5%, and the primary particles are D v,50 It can be confirmed that the size is greater than 3.7 μm.
[0160] Generally, a lower amount of fine powder generation is advantageous because it reduces the specific surface area in contact between the particles and the electrolyte, thereby suppressing side reactions and improving capacity retention and gas generation during charging and discharging. On the other hand, a higher rolling density is advantageous because it allows for coating a larger amount of active material per unit volume during electrode fabrication. However, since the amount of fine powder generation and rolling density are mutually exclusive, the optimal conditions should be found by considering them in combination with other performance characteristics.
[0161] Experiment Example 7: Evaluation of Battery Performance The positive electrode active materials prepared in the examples and comparative examples were mixed with FX35 conductive material and polyvinylidene fluoride (PVDF) binder in an N-methylpyrrolidone (NMP) solvent in a ratio of 95:3:2 to produce a positive electrode slurry. The positive electrode slurry was applied to one surface of an aluminum current collector, dried at 130°C for 10 minutes or more, and then rolled to produce a positive electrode.
[0162] A lithium metal electrode was used as the negative electrode, and an electrode assembly was manufactured by interposing a porous polyethylene separator between the positive and negative electrodes. After positioning the electrode assembly inside a battery case, an electrolyte was injected into the case to manufacture a half-cell. The electrolyte was prepared by dissolving 1.0 M LiPF6 in an organic solvent mixture of ethylene carbonate (EC), ethyl methyl carbonate (EMC), and diethyl carbonate (DEC) in a volume ratio of 3:4:3.
[0163] For each half-cell manufactured in this manner, the initial charge capacity and initial discharge capacity were measured while charging at 25°C in CC-CV mode at 0.1C until the voltage reached 4.5V, and then discharging at a constant current of 0.1C to 2.5V. The initial charge / discharge capacity, initial efficiency, and DC internal resistance (DCIR) were calculated and are shown in Table 3 below. For reference, the initial efficiency value is the percentage of the initial discharge capacity relative to the initial charge capacity, and the DCIR value is calculated by dividing the difference between the voltage at 60 seconds of discharge at a constant current of 0.1C and the initial voltage by the applied current.
[0164] [Table 3]
[0165] Referring to Tables 2 and 3, the positive electrode active materials of Examples 1 to 3 have a small particle ratio in the range of 5% to 10%, and the primary particle D v,50When the particle size is 2.2 μm to 3.7 μm, it can be confirmed that batteries containing this particle exhibit superior battery capacity, initial efficiency, and resistance performance compared to batteries containing the positive electrode active materials of Comparative Examples 1 and 2.
Claims
1. It contains a lithium composite transition metal oxide in single-particle form consisting of 10 or fewer primary particles, having a composition represented by the following chemical formula 1. The primary particle was derived from the SEM image. v,50 The size is 2.2 μm to 3.7 μm. The positive electrode active material has a small particle ratio of 5% to 10% according to the following formula 1: [Chemical formula 1] Li 1+x Ni a1 Co b1 Mn c1 Zr d1 Y e1 M f1 O 2-y A y In the aforementioned chemical formula 1, M is one or more elements selected from W, Cu, Sr, Mn, Ti, Mg, Mo, B, Sn, Fe, Zn, Si, and Al. A is one or more elements selected from F, Cl, Br, I, and S. -0.1 ≤ x ≤ 0.1, 0 < a1 < 1, 0 < b1 < 1, 0 < c1 < 1, 0 < d1 < 0.01, 0 < e1 < 0.01, 0 ≤ f1 < 0.1, 0 ≤ y ≤ 0.2, a1 + b1 + c1 + d1 + e1 + f1 = 1, [Formula 1] The ratio of small particles (%) = (sum of the areas of primary particles with a particle size of 1 μm or less derived from the SEM image / sum of the areas of all primary particles derived from the SEM image) × 100.
2. The primary particle was derived from the SEM image. v,50 The positive electrode active material according to claim 1, wherein the particle size is 2.5 μm to 2.8 μm.
3. The positive electrode active material was measured using a PSA (particle size analyzer) 50 The positive electrode active material according to claim 1, wherein the particle size is 3.5 μm to 4 μm.
4. The positive electrode active material according to claim 1, wherein the lithium composite transition metal oxide is doped with 1,000 ppm to 4,000 ppm of Zr and 1,000 ppm to 4,000 ppm of Y.
5. The positive electrode active material further includes a coating layer formed on the lithium composite transition metal oxide, The positive electrode active material according to claim 1, wherein the coating layer comprises Al, W, or a combination thereof.
6. A positive electrode comprising the positive electrode active material described in any one of claims 1 to 5.
7. The positive electrode described in claim 6, The negative electrode and, A separator interposed between the positive electrode and the negative electrode, A lithium secondary battery containing an electrolyte.