Cylindrical lithium-ion rechargeable battery
The cylindrical lithium secondary battery addresses lithium plating issues through optimized design parameters, ensuring uniform electrolyte distribution and improved safety during rapid charging.
Patent Information
- Application Number
- JP2026529041
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-12-19
- Filing Date
- 2024-12-20
- Publication Date
- 2026-11-19
AI Technical Summary
Conventional cylindrical lithium-ion batteries face issues with lithium plating during rapid charging, leading to battery degradation and safety risks due to uneven electrolyte distribution and increased internal pressure.
A cylindrical lithium secondary battery design with specific parameters, including a P value less than 8.7, defined by the formula H*R/t_a*L_a*P_a*V_c, ensures adequate empty space and electrolyte distribution, preventing lithium plating and enhancing safety and lifespan.
The design suppresses electrolyte segregation and lithium plating, improving battery lifespan and safety during rapid charging by allowing uniform electrolyte contact and lithium ion movement.
Smart Images

Figure 2026539108000001_ABST
Abstract
Description
[Technical Field]
[0001] This application claims priority rights based on Korean Patent Application No. 10-2023-0190175, filed on 22 December 2023, and Korean Patent Application No. 10-2024-0191913, filed on 19 December 2024, and all content disclosed in the documents of said Korean Patent Applications is incorporated herein by reference.
[0002] The present invention relates to a cylindrical lithium secondary battery, and more particularly to a cylindrical lithium secondary battery with excellent rapid charging characteristics. [Background technology]
[0003] With technological advancements in electric vehicles, portable electronic devices, and other applications, the demand for lithium-ion batteries as an energy source is rapidly increasing.
[0004] Lithium-ion batteries can be classified into cylindrical, prismatic, and pouch-type batteries depending on the shape of the battery case. Among these, cylindrical batteries consist of a cylindrical battery case containing a jelly roll-type electrode assembly, which is manufactured by sequentially stacking sheet-shaped positive electrode, separator, and negative electrode, then winding it in one direction. The top of the battery case is then covered with a cap plate for sealing. The positive and negative electrodes are each provided with strip-shaped positive and negative electrode tabs, which are connected to electrode terminals to electrically connect to an external power source. For reference, the positive electrode terminal is the cap plate, and the negative electrode terminal is the battery case.
[0005] In particular, with the recent advancements in electric vehicle technology, the demand for high-capacity batteries has increased, and the development and use of large, cylindrical rechargeable batteries with larger volumes are being considered. Conventional small cylindrical batteries, such as those with the 1865 or 2170 form factors, have not been required to provide high rapid charging performance.
[0006] In contrast, large cylindrical secondary batteries are applied to electric vehicles, making rapid charging characteristics extremely important. However, when rapid charging is performed at high voltage and high C-rate, the electrolyte can rapidly decompose, generating large amounts of gases such as CO2 and CH4, which increase the internal pressure of the battery. This increased internal pressure pushes the electrolyte out, causing it to become unevenly distributed. Lithium ions moved by this unevenly distributed electrolyte concentrate in a specific negative electrode region, and lithium ions that were not inserted into the negative electrode are deposited on the surface of the negative electrode, resulting in a phenomenon called lithium plating (Li-plating). As a result, lithium plating can lead to battery degradation or ignition, negatively impacting the battery's lifespan and safety.
[0007] Therefore, there is a need to develop lithium secondary batteries with superior rapid charging performance by preventing lithium plating during rapid charging and improving battery life characteristics and safety. [Overview of the Initiative] [Problems that the invention aims to solve]
[0008] The present invention aims to solve the above-mentioned problems and to provide a cylindrical lithium secondary battery that prevents lithium plating during rapid charging and has excellent lifespan characteristics and stability. [Means for solving the problem]
[0009] [1] The present invention provides a cylindrical lithium secondary battery comprising an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; an electrolyte; and a battery case housing the electrode assembly and the electrolyte, wherein the electrolyte comprises a lithium salt and an organic solvent, and the P value defined by the following formula 1 is less than 8.7.
[0010] [Formula 1]
number
[0011] In the aforementioned Formula 1, H (unit: mm) means the height of the lithium secondary battery, R (unit: mm) means the diameter of the lithium secondary battery, t a (unit: μm) means the thickness of the negative electrode, L a (unit: g / 25cm 2 ) means the loading amount of the negative electrode, P a (unit: %) means the porosity of the negative electrode, V c (unit: cm 3 ) means the volume of the free space inside the lithium secondary battery.
[0012] [2] The present invention provides the cylindrical lithium secondary battery according to the aforementioned [1], wherein the P value represented by the aforementioned Formula 1 is 7.4 to 8.6.
[0013] [3] The present invention provides the cylindrical lithium secondary battery according to the aforementioned [1] or [2], wherein the aforementioned V c is 17.5cm 3 to 25cm 3 .
[0014] [4] The present invention provides the cylindrical lithium secondary battery according to any one of the aforementioned [1] to [3], wherein the ratio (V c ) of the volume of the free space inside the lithium secondary battery (V c / V) to the total volume (V) of the internal space of the battery case is 0.08 to 0.25.
[0015] [5] The present invention provides the cylindrical lithium secondary battery according to any one of the aforementioned [1] to [4], wherein the ratio of H to R (R / H) is 0.4 or more.
[0016] [6] The present invention provides the cylindrical lithium secondary battery according to any one of the aforementioned [1] to [5], wherein the aforementioned P a is 23.5% or more.
[0017] [7] The present invention provides the aforementioned La 0.25g / 25cm 2 ~0.45g / 25cm 2 The present invention provides a cylindrical lithium secondary battery as described in any one of the above [1] to [6].
[0018] [8] The present invention relates to the t a The present invention provides a cylindrical lithium secondary battery according to any one of [1] to [7] above, wherein the diameter is 180 μm to 200 μm.
[0019] [9] The present invention provides a cylindrical lithium secondary battery according to any one of [1] to [8] above, wherein the negative electrode comprises a negative electrode active material layer containing a negative electrode active material, and the negative electrode active material comprises a carbon-based active material.
[0020]
[10] The present invention provides a cylindrical lithium secondary battery according to any one of [1] to [9] above, wherein the negative electrode comprises a negative electrode active material layer containing a negative electrode active material, and the negative electrode active material is present in an amount of 90% to 99% by weight based on the total weight of the negative electrode active material layer.
[0021]
[11] The present invention provides a cylindrical lithium secondary battery according to any one of [1] to
[10] , wherein the concentration of the lithium salt is 1.0 M to 1.5 M.
[0022]
[12] The present invention provides a cylindrical lithium secondary battery according to any one of [1] to
[11] above, wherein the lithium salt comprises one or more selected from the group consisting of LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, and LiI.
[0023]
[13] The present invention provides a cylindrical lithium secondary battery according to any one of [1] to
[12] above, wherein the organic solvent comprises one or more selected from the group consisting of cyclic carbonate organic solvents, linear carbonate organic solvents, linear ester organic solvents, and cyclic ester organic solvents.
[0024]
[14] The present invention provides a cylindrical lithium secondary battery according to any one of [1] to
[13] , wherein the cylindrical lithium secondary battery is a 46110 cell, a 48110 cell, a 4880 cell, or a 4680 cell.
[0025]
[15] The present invention provides a cylindrical lithium secondary battery according to any one of [1] to
[14] , wherein the cylindrical lithium secondary battery includes blank portions on at least a portion of the positive electrode and the negative electrode where no active material layer is formed, and the blank portions on the positive electrode and the negative electrode are defined as electrode tabs.
[0026]
[16] The present invention provides a cylindrical lithium secondary battery as described in
[15] , wherein the blank positive electrode portion and the blank negative electrode portion are each formed at one end of the positive electrode and the negative electrode in the direction in which the electrode assembly is wound, a current collector plate is bonded to each of the blank positive electrode portion and the blank negative electrode portion, and the current collector plate is connected to an electrode terminal.
[0027]
[17] The present invention provides a cylindrical lithium secondary battery according to
[15] or
[16] , wherein the positive electrode blank portion and the negative electrode blank portion are processed into a plurality of independently bendable segment pieces, and at least a portion of the plurality of segment pieces are bent toward the winding center of the electrode assembly.
[0028]
[18] The present invention provides a cylindrical lithium secondary battery according to
[17] , wherein at least a portion of the bent segments overlap on the upper and lower ends of the electrode assembly, and a current collector plate is bonded to the overlapping segments.
[0029]
[19] The present invention provides a battery pack that includes a cylindrical lithium secondary battery as a unit cell, according to any one of [1] to
[18] above. [Effects of the Invention]
[0030] The cylindrical lithium secondary battery according to the present invention, by ensuring that the form factor, the volume of the empty space inside the battery, and the negative electrode meet specific conditions, can suppress the phenomenon of electrolyte segregation due to increased internal pressure even when gas is generated by the decomposition of the electrolyte during rapid charging, and prevent lithium ions moving during the charge and discharge process from concentrating in a specific negative electrode region. This reduces the lithium plating phenomenon and improves the battery's lifespan characteristics and safety during rapid charging. [Brief explanation of the drawing]
[0031] [Figure 1] This figure shows the stacked state of the electrode assembly according to the present invention before it is wound up. [Figure 2] This is a cross-sectional view showing the structure of an electrode in an electrode assembly according to one embodiment of the present invention. [Figure 3] This diagram illustrates the structure of an electrode assembly according to one embodiment of the present invention. [Figure 4] This is a cross-sectional view showing the structure of a cylindrical lithium secondary battery according to one embodiment of the present invention. [Figure 5] This is a cross-sectional view showing the structure of a cylindrical lithium secondary battery according to another embodiment of the present invention. [Figure 6] This is a diagram illustrating the battery pack according to the present invention. [Modes for carrying out the invention]
[0032] The present invention will be described in more detail below.
[0033] The terms and words used herein and in the claims should not be interpreted in a manner limited to their general or dictionary meanings, but rather in a manner consistent with the technical idea of the present invention, in accordance with the principle that inventors may appropriately define the concepts of terms in order to best describe their invention.
[0034] The terms used herein are for illustrative purposes only and are not intended to limit the invention. Unless the context clearly indicates otherwise, singular expressions include plural expressions.
[0035] In this specification, terms such as “includes,” “equip,” or “have” are intended to specify the presence of implemented features, figures, steps, components, or combinations thereof, and should be understood not to preemptively exclude the presence or possibility of adding one or more other features, figures, steps, components, or combinations thereof.
[0036] In this invention, "the loading amount of the negative electrode (L) a Unit: g / 25cm 2 )" is 25cm 2 This refers to the mass (g) of the negative electrode active material layer contained per unit area. After punching out the negative electrode to a size of 5cm x 5cm, the weight W1 of the punched-out area and the weight W2 of the negative electrode current collector are measured. If the negative electrode active material layer is formed on both sides of the negative electrode current collector, it can be obtained by substituting these values into the following formula A-1. If the negative electrode active material layer is formed on one side of the negative electrode current collector, it can be obtained by substituting these values into the following formula A-2.
[0037] [Formula A-1] Loading amount L of the negative electrode a (g / 25cm 2 ) = (W1 - W2) / 2 [Formula A-2] Loading amount L for the negative electrode a (g / 25cm 2 )=(W1-W2)
[0038] In this invention, "the volume of the empty space inside the lithium secondary battery (V c Unit: cm 3 ")" refers to the space within the battery case of a lithium secondary battery, excluding the space occupied by the electrolyte and electrode assembly. Specifically, it can be measured after an activation process has been performed following the manufacture of the lithium secondary battery, but is not limited to this.
[0039] The aforementioned activation refers to the process of charging and / or discharging a lithium secondary battery that has been manufactured but has not undergone charging or discharging to impart electrical properties, and stabilizing the battery by forming an SEI (Solid Electrolyte Interphase) film on the electrodes, thereby making the battery usable.
[0040] The aforementioned V C In connection with this, the activation is performed by charging the lithium secondary battery to a voltage of 4.0V or higher at 25°C and discharging it to a voltage of 2.5V or lower, one or more times, but is not limited to this.
[0041] The volume of the empty space inside the lithium secondary battery (V c Unit: cm 3 )" refers to the dead volume (V) inside the battery case of a lithium secondary battery. d , void volume (V) p , and the volume V of the electrolyte e After measuring, the result can be substituted into the following formula B for measurement.
[0042] [Equation B] Volume V of the empty space inside the lithium secondary battery c (cm 3 )=V d +V p -V e
[0043] Specifically, in formula B, the dead volume V inside the battery case dThis refers to the volume of a cylindrical lithium secondary battery excluding the volume occupied by the electrode assembly and the volume occupied by the battery case. The volume of the cylindrical lithium secondary battery is measured based on the external shape of the cylindrical lithium secondary battery, and specifically refers to the volume of the space occupied by the external shape of the cylindrical lithium secondary battery, and in this case the internal space of the cylindrical lithium secondary battery is not taken into consideration. In this case, the external shape of the lithium secondary battery is the same as the external shape of the battery case when the battery case is sealed.
[0044] The volume occupied by the electrode assembly refers to the total volume occupied by the negative electrode, positive electrode, and separator contained within the electrode assembly. In this case, the volume occupied by the electrode assembly can be measured based on the external shapes of the negative electrode, positive electrode, and separator, without considering the volume of the voids contained within the negative electrode, positive electrode, and separator.
[0045] The volume occupied by the battery case refers to the volume of space physically occupied by the battery case itself, excluding the internal space of the battery case and including only the structural parts of the battery case itself, and can be measured based on the external dimensions of the battery case.
[0046] The aforementioned void volume V p This involves measuring the combined volume of the voids in the negative and positive electrodes and the voids in the separator interposed between the positive and negative electrodes. Specifically, it can be measured by combining the volume of the voids in the negative and positive electrodes and the voids in the separator and SRS coating layer interposed between the positive and negative electrodes. In this case, the respective void volumes of the positive electrode, negative electrode, separator, and SRS coating layer are obtained by multiplying the respective volumes of the positive electrode, negative electrode, separator, and SRS coating layer by their respective porosities.
[0047] Volume V of the electrolyte e This refers to the combined volume of the electrolyte impregnated into the internal void of the electrode assembly and the volume of the electrolyte located outside the electrode assembly within the internal space of the battery case. Specifically, the V eThis can be calculated by dividing the weight of the electrolyte by the density of the electrolyte.
[0048] The weight of the electrolyte is (1) the weight of the activated lithium secondary battery with the electrode assembly, electrolyte, and battery case sealed (M L (1) The steps of measuring the weight (M) of the dried battery case; (2) Disassembling the lithium secondary battery and removing the electrolyte present in the battery case; (3) Immersing the battery case and electrode assembly in a solvent such as dimethyl carbonate to remove the electrolyte present on the surface of the battery case, the surface of the electrode assembly, and the internal voids, and then drying the battery case and electrode assembly; (4) Measuring the weight (M) of the dried battery case. C ), and the weight (M) of the dried electrode assembly. A After going through the step of measuring ), the measured M L M C M A This can be measured by substituting it into the following formula B-1.
[0049] [Formula B-1] Weight of electrolytes = M L -M C -M A
[0050] In this specification, the "negative electrode porosity" can be calculated using the following formula C.
[0051] [Formula C] Porosity (%) = {1 - (Density of negative electrode active material layer / True density of negative electrode active material layer)} × 100
[0052] In the above equation C, the true density of the negative electrode active material layer is a calculated density obtained from the density and mass ratio of each constituent material making up the negative electrode active material layer, under the assumption that it does not contain pores, and the density of the negative electrode active material layer is a measured density of the negative electrode active material layer obtained by taking a sample of a certain size of negative electrode active material layer and measuring it.
[0053] The inventors of this invention conducted extensive research to develop a lithium secondary battery that can suppress the lithium plating phenomenon during rapid charging and improve its lifespan and safety. As a result, they discovered that when the form factor, the volume of empty space inside the battery, and the negative electrode meet specific conditions, the uneven distribution of the electrolyte due to gas generated during rapid charging can be suppressed, minimizing the lithium plating phenomenon and thereby improving the lifespan and safety during rapid charging. This led to the completion of the present invention.
[0054] The cylindrical lithium secondary battery according to the present invention includes at least one of the configurations disclosed below, and may include any combination of technically possible configurations from the following configurations.
[0055] The present invention will be described in more detail below.
[0056] Cylindrical lithium-ion rechargeable battery The cylindrical lithium secondary battery according to the present invention comprises an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; an electrolyte; and a battery case in which the electrode assembly and the electrolyte are housed, wherein the electrolyte comprises a lithium salt and an organic solvent, and has a P value defined by the following formula 1 that is less than 8.7.
[0057] [Formula 1]
number
[0058] In the above formula 1, H (unit: mm) represents the height of the lithium secondary battery, R (unit: mm) represents the diameter of the lithium secondary battery, and t a (Unit: μm) represents the thickness of the negative electrode, L a (Unit: g / 25cm) 2 ) refers to the loading amount of the negative electrode, P a (Unit: %) represents the porosity of the negative electrode, V c (Unit: cm) 3) refers to the volume of empty space inside a lithium-ion battery.
[0059] The cylindrical lithium secondary battery according to the present invention has a P value defined by formula 1 that is less than 8.7, specifically less than 8.7, 8.6 or less, 8.5 or less, 8.4 or less, 8.3 or less, 8.2 or less, 8.1 or less, 8.0 or less, 7.9 or less, 7.8 or less, 7.7 or less, 7.6 or less, or 7.5 or less, and may be 5 or more, 5.2 or more, 5.4 or more, 5.6 or more, 5.8 or more, 6 or more, 6.2 or more, 6.4 or more, 6.6 or more, 6.8 or more, 7 or more, 7.1 or more, 7.2 or more, 7.3 or more, 7.4 or more, or 7.5 or more. For example, the P value defined by formula 1 may be less than 8.7, 5 to 8.6, 7.4 to 8.5, 7.4 to 8, or 7.4 to 7.7.
[0060] In recent years, with the development of electric vehicle technology, the rapid charging characteristics of lithium-ion batteries have become extremely important in order to meet the demands for increased driving range and faster charging speeds. During the rapid charging process of lithium-ion batteries, as high voltage and / or high-rate charging and discharging are repeated, lithium ions that were not inserted into the negative electrode active material are deposited and exist on the surface of the negative electrode in the form of Li2CO3, etc. This causes side reactions of the electrolyte to become more vigorous, and a large amount of gas such as CO2 and CH4 is generated inside the battery. The generated gas moves into the empty space inside the battery. At this time, if the empty space inside the battery is insufficient and the pressure from the generated gas cannot be relieved, an electrolyte segregation phenomenon occurs in which the electrolyte is squeezed out by the pressure of the gas. As a result, the electrolyte cannot make uniform contact with the positive and negative electrodes and is concentrated in specific areas, and lithium ions cannot move uniformly but concentrate in specific areas, leading to the lithium plating phenomenon in which lithium ions that were not contained in the negative electrode are deposited on the surface of the negative electrode. Lithium plating causes capacity loss in lithium-ion batteries, degrading them and reducing their lifespan. It also leads to additional electrolyte side reactions, further degrading the performance of lithium-ion batteries. Furthermore, lithium plating can damage the separator, causing internal short circuits and potentially leading to battery explosion or fire, thus impacting battery safety.
[0061] To solve the above problems, the cylindrical lithium secondary battery according to the present invention has its form factor, the volume of the internal space of the battery, and the characteristics of the negative electrode all adjusted to specific conditions.
[0062] Specifically, the cylindrical lithium secondary battery according to the present invention ensures sufficient volume of empty space inside the battery to accommodate the gas generated during rapid charging and relieve pressure by setting the P value defined by formula 1 to less than 8.7, and adjusts the characteristics of the negative electrode to allow lithium ions to move smoothly by sufficiently impregnating the negative electrode with electrolyte, and optimizes the characteristics of the negative electrode and the volume of empty space inside the battery according to the form factor and the shape of the battery case.
[0063] Therefore, if the P value defined by formula 1 is less than 8.7, the uneven distribution of the electrolyte and the lithium plating phenomenon caused by gas generated during rapid charging can be improved, thereby enhancing the lifespan characteristics and safety during rapid charging.
[0064] Furthermore, when the P value defined by formula 1 is between 7.4 and 8.6, the lifespan characteristics and safety during rapid charging are improved, and the initial resistance characteristics and capacity characteristics can be excellent. This can occur when the loading amount or thickness of the negative electrode is excessively reduced, or when the porosity of the negative electrode or the volume of empty space inside the battery is excessively increased, resulting in a decrease in the amount of lithium ions that can be accommodated in the negative electrode or a decrease in the amount of electrolyte to which lithium ions can move.
[0065] The volume V of the empty space inside the lithium secondary battery. c It is 17.5cm 3 ~25cm 3 , 18cm 3 ~23cm 3 18.5cm 3 ~21.5cm 3 , or 19.7cm 3 ~20.5cm 3 This may be the case. The volume V of the empty space inside the lithium secondary battery. c If the above conditions are met, the pressure caused by the gas generated during rapid charging can be reduced, suppressing the uneven distribution of the electrolyte, thereby improving lithium plating and lifespan characteristics during rapid charging.
[0066] The volume of the empty space inside the lithium secondary battery relative to the total volume (V) of the internal space inside the battery case. c ) ratio (V c The voltage (V) may be 0.08 to 0.25, preferably 0.1 to 0.22, more preferably 0.11 to 0.20, 0.13 to 0.18, or 0.15 to 0.17. When the proportion of the volume of empty space inside the lithium secondary battery satisfies the above range, the pressure due to gas generation can be relieved and the rapid charging characteristics can be improved.
[0067] The diameter R of the lithium secondary battery may be 40 mm or more, 42 mm or more, or 46 mm or more, and the height H of the lithium secondary battery may be 70 mm or more, 75 mm or more, or 80 mm or more. When the above ranges are met, excellent capacity characteristics can be achieved. The diameter of the lithium secondary battery refers to the diameter of the external shape of the lithium secondary battery and is the same as the external diameter of the battery case. The height of the lithium secondary battery refers to the height of the external shape of the lithium secondary battery and is the same as the external height of the battery case.
[0068] The ratio of the height H of the lithium secondary battery to its diameter R (R / H, form factor ratio) may be 0.4 or greater, 0.4 to 0.6, or 0.5 to 0.6. When the form factor ratio is within this range, high capacity characteristics can be achieved as a large cylindrical lithium secondary battery.
[0069] The loading amount L of the aforementioned negative electrode a It is 0.25g / 25cm 2 ~0.45g / 25cm 2 0.3g / 25cm 2 ~0.4g / 25cm 2 , 0.32g / 25cm 2 ~0.38g / 25cm 2 , or 0.33g / 25cm 2 ~0.37g / 25cm 2 This may be the case. If the load amount range of the negative electrode is met, the capacity characteristics and life characteristics can be improved.
[0070] The negative electrode void ratio P a This can be 23.5% or more, 23.5% to 27.0%, 24.0% to 26.5%, or 25.0% to 26.0%. When the above range of negative electrode porosity is met, energy density, capacity characteristics, and electrolyte impregnation can all be improved.
[0071] The thickness t of the negative electrode a The thickness may be 180 μm to 200 μm, 185 μm to 195 μm, or 189 μm to 192 μm. When the thickness range of the negative electrode is met, both capacitance characteristics and lifetime characteristics can be improved.
[0072] Next, we will describe in more detail each component of the cylindrical lithium secondary battery according to the present invention.
[0073] The cylindrical lithium secondary battery according to the present invention includes an electrode assembly comprising a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode; an electrolyte; and a battery case in which the electrode assembly and the electrolyte are housed.
[0074] (1) Electrode assembly The electrode assembly according to the present invention includes a positive electrode, a negative electrode, and a separator interposed between the positive electrode and the negative electrode.
[0075] Figure 1 shows the laminated structure of an electrode assembly according to one embodiment of the present invention before winding, Figure 2 shows the cross-sectional structure of an electrode plate (positive or negative electrode) according to one embodiment of the present invention, and Figure 3 shows the structure of an electrode assembly according to one embodiment of the present invention.
[0076] Referring to Figures 1 and 2, the electrode assembly A of the present invention can be manufactured by winding a laminate formed by stacking separator 12, positive electrode 10, separator 12, and negative electrode 11 in order at least once in one direction (X).
[0077] The following describes in more detail each component of the electrode assembly of the present invention.
[0078] 1) Positive electrode The positive electrode can be manufactured by applying a positive electrode slurry to one or both sides of a sheet-shaped positive electrode current collector, removing the solvent from the positive electrode slurry through a drying process, and then rolling it. Alternatively, a positive electrode including a plain area can be manufactured by not applying the positive electrode slurry to a part of the positive electrode current collector, for example, one end of the positive electrode current collector.
[0079] Furthermore, the positive electrode slurry can be manufactured by dispersing the positive electrode material according to the present invention in a solvent such as dimethyl sulfoxide (DMSO), isopropyl alcohol, N-methylpyrrolidone (NMP), acetone, or water.
[0080] The positive electrode produced thereby includes a positive electrode current collector and a positive electrode active material layer, the positive electrode active material layer may contain positive electrode active material.
[0081] Various positive electrode current collectors used in the art can be used as the positive electrode current collector. For example, the positive electrode current collector may be stainless steel, aluminum, nickel, titanium, calcined carbon, or aluminum or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc. The positive electrode current collector may typically have a thickness of 3 μm to 500 μm, and the adhesion strength of the positive electrode active material may be increased by forming fine irregularities on the surface of the positive electrode current collector. The positive electrode current collector can be used in various forms such as film, sheet, foil, mesh, porous material, foam, nonwoven fabric, etc.
[0082] The positive electrode active material layer is located on the positive electrode current collector, specifically on one or both sides of the positive electrode current collector. The positive electrode active material layer may be a single layer or a multilayer structure of two or more layers.
[0083] As the positive electrode active material, positive electrode active materials commonly used in the relevant technical field can be used, and the type thereof is not particularly limited. The positive electrode active material is a compound capable of reversible intercalation and deintercalation of lithium, and specifically, may include a lithium transition metal composite oxide containing lithium and at least one transition metal selected from the group consisting of nickel, cobalt, manganese, and aluminum, preferably a lithium transition metal composite oxide containing lithium and a transition metal including nickel, cobalt, and manganese.
[0084] More specifically, examples of the lithium transition metal composite oxide include lithium-manganese-based oxides (e.g., LiMnO2, LiMn2O4, etc.), lithium-cobalt-based oxides (e.g., LiCoO2, etc.), lithium-nickel-based oxides (e.g., LiNiO2, etc.), lithium-nickel-manganese-based oxides (e.g., LiNi 1-Y Mn Y O2 (where 0<Y<1), LiMn 2-Z Ni Z O4 (where 0<Z<2), etc.), lithium-nickel-cobalt-based oxides (e.g., LiNi 1-Y1 Co Y1 O2 (where 0<Y1<1), etc.), lithium-manganese-cobalt-based oxides (e.g., LiCo 1-Y2 Mn Y2 O2 (where 0<Y2<1), LiMn 2-Z1 Co Z1 O4 (where 0<Z1<2), etc.), lithium-nickel-manganese-cobalt-based oxides (e.g., Li(Ni p Co q Mn r1 )O2 (where 0<p<1, 0<q<1, 0<r1<1, p+q+r1=1) or Li(Ni p1 Co q1 Mn r2 )O4 (where 0<p1<2, 0<q1<2, 0<r2<2, p1+q1+r2=2), etc.), or lithium-nickel-cobalt-transition metal (M) oxides (e.g., Li(Ni p2 Co q2 Mn r3M s2 )O₂ (wherein M is selected from the group consisting of Al, Fe, V, Cr, Ti, Ta, Mg, and Mo, and p2, q2, r3, and s2 are each independent atomic fractions of the elements, satisfying 0<p2<1, 0<q2<1, 0<r3<1, 0<s2<1, and p2+q2+r3+s2=1) and the like) and the like, and any one or two or more of these compounds may be included. Above all, from the viewpoint of being able to enhance the capacity characteristics and stability of the battery, the lithium transition metal composite oxide is LiCoO₂, LiMnO₂, LiNiO₂, lithium nickel-manganese-cobalt oxide (for example, Li(Ni 0.6 Mn 0.2 Co 0.2 )O₂, Li(Ni 0.5 Mn 0.3 Co 0.2 )O₂, Li(Ni 0.7 Mn 0.15 Co 0.15 )O₂, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O₂ and the like), or lithium nickel cobalt aluminum oxide (for example, Li(Ni 0.8 Co 0.15 Al 0.05 )O₂ and the like). In consideration of the remarkableness of the improvement effect by controlling the type and content ratio of the constituent elements forming the lithium transition metal composite oxide, the lithium transition metal composite oxide may be Li(Ni 0.6 Mn 0.2 Co 0.2 )O₂, Li(Ni 0.5 Mn 0.3 Co 0.2 )O₂, Li(Ni 0.7 Mn 0.15 Co 0.15 )O₂, or Li(Ni 0.8 Mn 0.1 Co 0.1 )O₂ and the like, and any one or a mixture of two or more of these can be used.
[0085] On the other hand, the positive electrode active material layer may optionally further include at least one of a positive electrode conductive material and a positive electrode binder.
[0086] The positive electrode conductive material is used to impart conductivity to the electrode and can be used in the battery without particular limitations, as long as it does not cause chemical changes and has electronic conductivity. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. One of these can be used alone, or a mixture of two or more. The positive electrode conductive material is usually included in an amount of 1% to 30% by weight, preferably 1% to 20% by weight, and more preferably 1% to 10% by weight, based on the total weight of the positive electrode active material layer.
[0087] The positive electrode binder plays a role in improving the adhesion between positive electrode material particles and the adhesion between the positive electrode material and the positive electrode current collector. Specific examples include fluororesin binders containing polyvinylidene fluoride (PVDF) or polytetrafluoroethylene (PTFE); rubber binders containing styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose binders containing carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol binders containing polyvinyl alcohol; polyolefin binders containing polyethylene and polypropylene; polyimide binders; polyester binders; and silane binders. One of these can be used alone, or a mixture of two or more. The positive electrode binder may be present in an amount of 1% to 30% by weight, preferably 1% to 20% by weight, and more preferably 1% to 10% by weight, relative to the total weight of the positive electrode active material layer.
[0088] 2) Negative electrode The negative electrode can be manufactured by applying a negative electrode slurry to one or both sides of a sheet-shaped negative electrode current collector, removing the solvent from the negative electrode slurry through a drying process, and then rolling it. Alternatively, a negative electrode including a plain area can be manufactured by not applying the negative electrode slurry to a part of the negative electrode current collector, for example, one end of the negative electrode current collector.
[0089] The negative electrode slurry can be manufactured by dispersing the negative electrode active material in a solvent such as distilled water, ethanol, methanol, or isopropyl alcohol.
[0090] Alternatively, the negative electrode may be manufactured by casting the negative electrode slurry onto another support, peeling it off the support, and then laminating the resulting film onto the negative electrode current collector.
[0091] The negative electrode produced thereby includes a negative electrode current collector and a negative electrode active material layer, the negative electrode active material layer may contain a negative electrode active material.
[0092] The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. For example, copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel with surface treatment using carbon, nickel, titanium, silver, etc., and aluminum-cadmium alloy may be used. The negative electrode current collector may also typically have a thickness of 3 μm to 500 μm.
[0093] Furthermore, similar to the positive electrode current collector, the negative electrode current collector may have fine irregularities formed on its surface to strengthen the bonding force of the negative electrode active material. For example, it can be used in various forms such as film, sheet, foil, mesh, porous material, foam, and nonwoven fabric.
[0094] The negative electrode active material layer is located on the negative electrode current collector, specifically on one or both sides of the negative electrode current collector. The negative electrode active material layer may be a single layer or a multilayer structure of two or more layers.
[0095] The thickness of the negative electrode active material layer may be 180 μm to 200 μm, preferably 180 μm to 190 μm, and more preferably 184 μm to 190 μm. When the above range is met, the capacitance characteristics and lifetime characteristics can be improved.
[0096] The anode active material may include a carbon-based active material. For example, the carbon-based active material may be one or more selected from the group consisting of amorphous, plate-like, flaky, spherical, or fibrous natural or artificial graphite, Kish graphite, pyrolytic carbon, mesophase pitch-based carbon fiber, meso-carbon microbeads, mesophase pitches, and petroleum or coal tar pitch-derived cokes.
[0097] Preferably, the negative electrode active material may include one or more selected from the group consisting of natural graphite and artificial graphite. When the negative electrode active material is included, the capacity characteristics and lifetime characteristics can be improved.
[0098] The negative electrode active material may be present in an amount of 90% to 99% by weight, preferably 93% to 99% by weight, and more preferably 96% to 99% by weight, based on the total weight of the negative electrode active material layer.
[0099] On the other hand, the negative electrode active material layer may selectively further contain a negative electrode conductive material and a negative electrode binder in addition to the negative electrode active material.
[0100] The negative electrode conductive material is used to impart conductivity to the electrode and is not particularly limited as long as it does not cause chemical changes and has electronic conductivity in the battery it is used in. Specific examples include graphite such as natural graphite or artificial graphite; carbon-based materials such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, thermal black, carbon fiber, and carbon nanotubes; metal powders or metal fibers such as copper, nickel, aluminum, and silver; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; or conductive polymers such as polyphenylene derivatives. One of these can be used alone, or a mixture of two or more. The negative electrode conductive material is usually included in an amount of 1% to 30% by weight, preferably 1% to 20% by weight, and more preferably 1% to 10% by weight, relative to the total weight of the negative electrode active material layer.
[0101] The negative electrode binder plays a role in improving the adhesion between negative electrode active material particles and the adhesion between the negative electrode active material and the negative electrode current collector. Specific examples include polyvinylidene fluoride (PVDF), vinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinyl alcohol, polyacrylonitrile, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-diene monomer rubber (EPDM rubber), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, or various copolymers thereof, and one of these can be used alone or a mixture of two or more. The negative electrode binder may be present in an amount of 1% to 30% by weight, preferably 1% to 20% by weight, and more preferably 1% to 10% by weight, based on the total weight of the negative electrode active material layer.
[0102] Since the thickness, porosity, and loading amount of the negative electrode are as described above, a detailed explanation will be omitted.
[0103] 3) Separator The separator is interposed between the positive electrode and the negative electrode, separating them and providing a passage for lithium ions to move. It is not particularly limited to any separator commonly used in lithium secondary batteries. Specifically, the separator can be a porous polymer film, for example, a porous polymer film made from polyolefin polymers such as ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, or a laminated structure of two or more layers thereof. Alternatively, a conventional porous nonwoven fabric, for example, a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used. Furthermore, a coated separator containing ceramic components or polymeric substances may be used to ensure heat resistance or mechanical strength.
[0104] On the other hand, the positive electrode 10 and the negative electrode 11 have a structure in which an active material layer 21 is formed on a sheet-like current collector 20, and a plain portion 22 in which the active material layer 21 is not formed may be included in a part of the current collector 20.
[0105] As described above, by using a positive electrode 10 and a negative electrode 11 that include a blank portion 22, it is possible to realize a battery in which at least a portion of the blank portions of the positive electrode 10 and the negative electrode 11 defines an electrode tab, without providing a separate electrode tab.
[0106] Specifically, the blank portion 22 is formed at one end of the current collector 20, extending along the winding direction (X). By attaching a current collector plate to the positive electrode blank portion and the negative electrode blank portion, and connecting the current collector plate to the electrode terminal, it can function as an electrode tab.
[0107] For example, a battery can be manufactured in which the blank positive electrode portion and the blank negative electrode portion function as electrode tabs by the following method. First, a separator, positive electrode, separator, and negative electrode are stacked in order so that the blank positive electrode portion and the blank negative electrode portion are positioned in opposite directions to each other, and then wound in one direction to manufacture a jelly roll type electrode assembly. After that, the blank positive and negative electrode portions are bent towards the winding center (C), and then current collector plates are welded to the blank positive electrode portion and the blank negative electrode portion, respectively, and the current collector plates are connected to the electrode terminals to manufacture the battery. The current collector plates have a larger cross-sectional area than strip-shaped electrode tabs, and since resistance is inversely proportional to the cross-sectional area of the current passage, the cell resistance can be significantly reduced when a secondary battery is formed with the above structure.
[0108] On the other hand, the blank positive electrode portion and the blank negative electrode portion are processed into a plurality of independently bendable segment pieces, and at least a portion of the plurality of segment pieces may be bent toward the winding center (C) of the electrode assembly.
[0109] The segment pieces may be formed by processing the positive and negative electrode current collectors using metal foil cutting processes such as laser cutting, ultrasonic cutting, or punching.
[0110] When the plain portions of the positive and negative electrodes are processed into the form of multiple segment pieces, the stress applied to the plain portions during bending can be reduced, preventing deformation and damage to the plain portions, and improving the welding characteristics with the current collector plate.
[0111] Normally, the current collector plate and the blank section are joined by welding. However, to improve welding characteristics, strong pressure must be applied to the welding area of the blank section, causing it to bend as flat as possible. However, this bending process can cause uneven distortion and deformation of the blank section, potentially leading to internal short circuits due to contact with electrodes of opposite polarity or causing microscopic cracks in the blank section. However, if the blank sections of the positive and negative electrodes are processed into multiple independently bendable segment pieces, the stress applied to the blank section during bending is reduced, minimizing deformation and damage to the blank section.
[0112] Furthermore, if the plain portion is processed into the form of segment pieces as described above, multiple segment pieces will overlap when bent. This increases the welding strength with the current collector plate and prevents the problem of the laser penetrating into the electrode assembly and ablating the separator or active material when using advanced technologies such as laser welding. Preferably, at least a portion of the bent multiple segment pieces may overlap on the upper and lower ends of the electrode assembly, and the current collector plate may be bonded to the overlapping multiple segment pieces.
[0113] On the other hand, the electrode assembly according to the present invention may be formed in a structure in which an insulating layer 24 is further formed on the positive electrode 10, as shown in Figure 3. Specifically, the insulating layer 24 may be formed in a direction parallel to the winding direction of the electrode assembly, covering a part of the positive electrode active material layer and a part of the plain area.
[0114] In a tabletless battery that uses the blank portion 22c of the positive electrode 10 and the blank portion 22a of the negative electrode 11 as electrode tabs, the electrode assembly is formed such that the positive electrode 10 protrudes above the separator 12 and the negative electrode 11 protrudes below the separator 12. The protruding positive electrode 10 and / or negative electrode 11 are then bent and connected to the current collector plate. However, when the positive electrode 10 or negative electrode 11 is bent as described above, the current collector of the positive electrode 10 or negative electrode 11 extends beyond the separator and comes into close proximity to the electrode of the opposite polarity. This can cause the positive and negative electrodes to come into electrical contact, potentially leading to an internal short circuit. However, as shown in Figure 3, when an insulating layer 24 is formed that covers the positive electrode active material layer and a portion of the blank portion, the insulating layer 24 can prevent the positive electrode 10 and negative electrode 11 from coming into electrical contact, thus preventing a short circuit from occurring inside the battery.
[0115] Preferably, the insulating layer 24 may be provided on at least one side of the current collector of the positive electrode 10, and preferably on both sides of the positive electrode 10.
[0116] Furthermore, the insulating layer 24 may be formed in the region of the positive electrode 10 in an area that may face the active material layer 21a of the negative electrode 11. For example, in the plain portion 22c of the positive electrode 10, the insulating layer 24 may extend to the end of the plain portion 22c on the surface that faces the negative electrode 11 after being folded. However, on the opposite surface of the surface that faces the negative electrode 11 after being folded, it is preferable that the insulating layer 24 be formed only in a part of the plain portion 22c, for example, up to the point before the folded portion of the plain portion 22c. This is because if the insulating layer 24 is formed over the entire area of the plain portion on the opposite surface of the surface that faces the negative electrode 11, electrical contact with the current collector plate becomes impossible, and it cannot function as an electrode tab.
[0117] On the other hand, the insulating layer 24 only needs to ensure insulating performance and be able to adhere to the positive electrode, and its material and components are not particularly limited. For example, the insulating layer may be an insulating coating layer or an insulating tape, and the insulating coating layer may contain an organic binder and inorganic particles. In this case, the organic binder may be, for example, styrene-butadiene rubber (SBR), and the inorganic particles may be alumina oxide, but are not limited to these.
[0118] (2) Battery case The battery case is for housing the electrode assembly and electrolyte, and may be a cylindrical battery case.
[0119] The form factor ratio of the cylindrical lithium secondary battery according to the present invention (defined as the ratio of the diameter (R) to the height (H) of the cylindrical battery, i.e., the ratio of the diameter (R) to the height (H)) is as described above, so a detailed explanation is omitted.
[0120] The cylindrical lithium secondary battery according to the present invention may be, for example, a 46110 cell (diameter 46 mm, height 110 mm, form factor ratio 0.418), a 4875 cell (diameter 48 mm, height 75 mm, form factor ratio 0.640), a 48110 cell (diameter 48 mm, height 110 mm, form factor ratio 0.436), a 4880 cell (diameter 48 mm, height 80 mm, form factor ratio 0.600), a 4680 cell (diameter 46 mm, height 80 mm, form factor ratio 0.575), or a 4695 cell (diameter 46 mm, height 95 mm, form factor ratio 0.484). In the numerical values indicating the form factor, the first two numbers represent the diameter (R) of the lithium secondary battery, and the next two or three numbers represent the height (H) of the lithium secondary battery.
[0121] (3) Electrolyte The electrolyte according to the present invention comprises a lithium salt and an organic solvent.
[0122] The lithium salt can be any compound capable of providing lithium ions for use in lithium secondary batteries, and is not particularly limited. Specifically, the lithium salt may include one or more selected from the group consisting of LiPF6, LiClO4, LiAsF6, LiBF4, LiSbF6, LiAlO4, LiAlCl4, LiCF3SO3, LiC4F9SO3, LiN(C2F5SO3)2, LiN(C2F5SO2)2, LiN(CF3SO2)2, LiCl, LiI, or LiB(C2O4)2, preferably one or more selected from the group consisting of LiPF6. The concentration of the lithium salt may be 1.0M to 1.5M, preferably 1.0M to 1.4M, more preferably 1.0M to 1.3M, and more preferably 1.15M to 1.3M. When the concentration of the lithium salt falls within the above range, the electrolyte has appropriate conductivity and viscosity, exhibiting excellent electrolyte performance and allowing lithium ions to move effectively.
[0123] The organic solvent may include one or more selected from the group consisting of cyclic carbonate organic solvents, linear carbonate organic solvents, linear ester organic solvents, and cyclic ester organic solvents.
[0124] The cyclic carbonate-based organic solvent is a highly viscous organic solvent and may typically include at least one organic solvent selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate.
[0125] Furthermore, the linear carbonate-based organic solvent is an organic solvent having low viscosity and low dielectric constant, and as a typical example, at least one organic solvent selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate may be used, and specifically, ethyl methyl carbonate (EMC) may be included.
[0126] Specific examples of the linear ester-based organic solvent include at least one organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate.
[0127] The cyclic ester organic solvents include at least one organic solvent selected from the group consisting of γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0128] Preferably, the electrolyte according to the present invention may contain ethylene carbonate and dimethyl carbonate as organic solvents.
[0129] On the other hand, the electrolyte may also contain other additives in addition to the components of the electrolyte, for purposes such as improving the battery's lifespan, suppressing the decrease in battery capacity, and improving the battery's discharge capacity.
[0130] Such other additives may include, as representative examples, at least one other additive selected from the group consisting of cyclic carbonate compounds, halogen-substituted carbonate compounds, sultone compounds, sulfate compounds, borate compounds, nitrile compounds, benzene compounds, amine compounds, silane compounds, and lithium salt compounds different from the lithium salt contained in the electrolyte.
[0131] Specifically, the other additives include vinylene carbonate (VC), vinylethylene carbonate, fluoroethylene carbonate (FEC), 1,3-propanesultone (PS), 1,4-butanesultone, ethensultone, 1,3-propensultone (PRS), 1,4-butensultone, 1-methyl-1,3-propensultone, ethylene sulfate (Esa), trimethylene sulfate (TMS), and methyl trimethylene sulfate. Examples include one or more compounds selected from the group consisting of sulfate (MTMS), tetraphenyl borate, lithium oxalyl difluoroborate, succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonile, cyclohexanecarbonile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, 4-fluorophenylacetonitrile, fluorobenzene, triethanolamine, ethylenediamine, tetravinylsilane, LiN(SO2F)2 (Lithium bis(fluorosulfonyl)imide, LIFSI), LiN(SO2CF3)2 (lithium bis(trifluoromethane sulfonyl)imide, LiTFSI), LiPO2F2, LiODFB, LiBOB (lithium bisoxalate borate (LiB(C2O4)2)), and LiBF4.
[0132] The aforementioned other additives may be present in an amount of 0.01% to 20% by weight, preferably 0.05% to 5.0% by weight, based on the total weight of the electrolyte. If the content of the aforementioned other additives is less than 0.01% by weight, the effect of improving the low-temperature output of the battery, as well as the high-temperature storage characteristics and high-temperature life characteristics, will be minimal. If the content of the aforementioned other additives exceeds 20% by weight, excessive side reactions may occur in the electrolyte during charging and discharging of the battery. In particular, if an excessive amount of the SEI film-forming additive is added, it may not decompose sufficiently at high temperatures and may remain unreacted or precipitated in the electrolyte at room temperature. Therefore, there is a risk of side reactions occurring that reduce the life or resistance characteristics of the secondary battery.
[0133] Next, the structure of the lithium secondary battery according to the present invention will be described.
[0134] Figures 4 and 5 disclose embodiments of the lithium secondary battery according to the present invention. The lithium secondary battery according to the present invention will be described below with reference to Figures 4 and 5. However, Figures 4 and 5 merely show one embodiment of the present invention, and the structure of the battery of the present invention is not limited to the scope disclosed in Figures 4 and 5.
[0135] Figure 4 shows a cross-sectional view of a lithium secondary battery with a tablet structure according to one embodiment of the present invention.
[0136] Referring to Figure 4, the lithium secondary battery 140 according to the present invention may include an electrode assembly 141, a battery case 142 in which the electrode assembly 141 and an electrolyte (not shown) are housed, and a seal 143 that seals the open end of the battery case 142.
[0137] In this case, the electrode assembly may be a laminate of a positive electrode, a separator, and a negative electrode wound in one direction. Furthermore, each positive electrode and negative electrode of the electrode assembly may include a plain portion where no active material layer is formed, and the electrode assembly may be laminated and wound so that the plain portions of the positive electrode and negative electrode are located at the upper and lower ends of the electrode assembly, respectively. Since the electrode assembly has been described above, only the components other than the electrode assembly will be described below.
[0138] On the other hand, the battery case 142 is a can-shaped container with an open end formed at the top, and is made of a conductive metal material such as aluminum or steel. The battery case houses the electrode assembly 141 in its inner space through the open end at the top, and also houses the electrolyte (not shown) together with it.
[0139] On the other hand, it is preferable that the lithium secondary battery 140 of the present invention does not include a current interruption device (CID).
[0140] On the other hand, as shown in Figure 4, the battery case 142 is electrically connected to the blank portion 146b of the negative electrode and can function as a negative electrode terminal that transmits current applied from an external power source to the negative electrode by contacting an external power source.
[0141] If necessary, a beading portion 147 and a crimping portion 148 may be provided at the upper end of the battery case 142. The beading portion 147 may be formed by press-fitting around the outer circumferential surface of the battery case 142 to a distance D1. The beading portion 147 can prevent the electrode assembly 141 housed inside the battery case 142 from passing through the upper end opening of the battery case 142, and can also function as a support portion on which the seal 143 is placed.
[0142] The crimping portion 148 is formed on the upper part of the beading portion 147 and has an extended and bent shape that surrounds the outer circumferential surface and a part of the upper surface of the cap plate 143a which is placed on the beading portion 147.
[0143] Next, the sealing body 143 is for sealing the open end of the battery case 142 and includes a cap plate 143a and a first gasket 143b that provides airtightness and insulation between the cap plate 143a and the battery case 142, and may further include a connecting plate 143c electrically and mechanically coupled to the cap plate 143a as needed. The cap plate 143a can be crimped onto a beading portion 147 formed on the battery case 142 and secured by a crimping portion 148.
[0144] The cap plate 143a is a component made of a conductive metal material and covers the upper opening of the battery case 142. The cap plate 143a is electrically connected to the positive electrode of the electrode assembly 141 and electrically insulated from the battery case 142 via the first gasket 143b. Therefore, the cap plate 143a can function as the positive electrode terminal of the lithium secondary battery. The cap plate 143a has a projection 143d that protrudes upward from its center C, and the projection 143d can come into contact with an external power source, allowing current to be applied from the external power source.
[0145] A first gasket 143b may be interposed between the cap plate 143a and the crimping portion 148 to ensure airtightness of the battery case 142 and to provide electrical insulation between the battery case 142 and the cap plate 143a.
[0146] On the other hand, the lithium secondary battery 140 according to the present invention may further include current collector plates 144 and 145 as needed. The current collector plates are coupled to a blank positive electrode portion 146a and a blank negative electrode portion 146b and connected to electrode terminals (i.e., positive electrode terminal and negative electrode terminal).
[0147] Specifically, the cylindrical battery 140 according to the present invention may include a first current collector plate 144 coupled to the upper part of the electrode assembly 141, and a second current collector plate 145 coupled to the lower part of the electrode assembly 141.
[0148] The system may further include a first current collector plate 144 and / or a second current collector plate 145.
[0149] The first current collector plate 144 is coupled to the upper part of the electrode assembly 141. The first current collector plate 144 is made of a conductive metal material such as aluminum, copper, or nickel, and is electrically connected to the positive electrode blank portion 146a. A lead 149 can be connected to the first current collector plate 144. The lead 149 extends above the electrode assembly 141 and may be coupled to the connecting plate 143c or directly to the lower surface of the cap plate 143a. The lead 149 may be coupled to other components by welding. Preferably, the first current collector plate 144 may be formed integrally with the lead 149. In this case, the lead 149 may have a plate shape extending outward from the center of the first current collector plate 144.
[0150] On the other hand, the first current collector plate 144 is connected to the end of the positive electrode blank portion 146a, and this connection may be made by methods such as laser welding, resistance welding, ultrasonic welding, or soldering.
[0151] The second current collector plate 145 is coupled to the lower part of the electrode assembly 141. The second current collector plate 145 is made of a conductive metal material such as aluminum, copper, or nickel, and is electrically connected to the blank portion 146b of the negative electrode. One side of the second current collector plate 145 may be coupled to the blank portion 146b of the negative electrode, and the opposite side may be coupled to the inner bottom surface of the battery case 142. In this case, the coupling may be performed by methods such as laser welding, resistance welding, ultrasonic welding, or soldering.
[0152] On the other hand, the lithium secondary battery 140 according to the present invention may further include an insulator 146 as needed. The insulator 146 may be positioned to cover the upper surface of the first current collector plate 144. By covering the first current collector plate 144 with the insulator 146, it is possible to prevent the first current collector plate 144 from coming into direct contact with the inner surface of the battery case 142.
[0153] The insulator 146 is provided with a lead hole 151 through which a lead 149 extending upward from the first current collector plate 144 is drawn out. The lead 149 is drawn out upward through the lead hole 151 and coupled to the lower surface of the coupling plate 143c or the lower surface of the cap plate 143a.
[0154] The insulator 146 may be made of an insulating polymer resin, such as polyethylene, polypropylene, polyimide, or polybutylene terephthalate.
[0155] On the other hand, the lithium secondary battery 140 according to the present invention may further include a venting portion 152 formed on the lower surface of the battery case 142, if necessary. The venting portion 152 corresponds to an area on the lower surface of the battery case 142 that has a thinner thickness compared to the surrounding area. Because the venting portion 152 is thin, it is structurally weaker than the surrounding area. Therefore, if the internal pressure of the lithium secondary battery 140 increases above a certain level, the venting portion 152 will rupture, releasing the gas inside the battery case 152 to the outside, thus preventing the battery from exploding.
[0156] Figure 5 shows a cross-sectional view of a lithium secondary battery with a tablet structure according to another embodiment of the present invention.
[0157] Referring to Figure 5, the cylindrical lithium secondary battery 170 according to another embodiment of the present invention differs from the lithium secondary battery 140 shown in Figure 4 in the structure of the battery case and seal, while the configuration of the electrode assembly and electrolyte is substantially the same.
[0158] Specifically, a cylindrical lithium secondary battery 170 according to another embodiment of the present invention includes a battery case 171 through which a rivet terminal 172 is installed. The rivet terminal 172 is installed on a partially closed closed surface (upper surface in the drawing) at one end of the battery case 171. The rivet terminal 172 is riveted into a through hole (first opening at the first end) of the battery case 171 with an insulating second gasket 173 interposed therebetween. The rivet terminal 172 is exposed to the outside in the direction opposite to the direction of gravity.
[0159] The rivet terminal 172 includes a terminal exposure portion 172a and a terminal insertion portion 172b. The terminal exposure portion 172a is exposed to the outside of the closed surface of the battery case 171. The terminal exposure portion 172a may be located approximately in the center of the partially closed surface of the battery case 171. The maximum diameter of the terminal exposure portion 172a may be larger than the maximum diameter of the through hole formed in the battery case 171. The terminal insertion portion 172b can be electrically connected to the positive terminal blank portion 146a by passing through approximately the center of the closed surface of the battery case 171. The terminal insertion portion 172b may be rivet-bonded to the inner surface of the battery case 171. That is, the end of the terminal insertion portion 172b may have a curved shape toward the inner surface of the battery case 171. The maximum diameter of the end of the terminal insertion portion 172b may be larger than the maximum diameter of the through hole in the battery case 171.
[0160] The lower end surface of the terminal insertion portion 172b may be welded to the first current collector plate 144, which is connected to the positive electrode blank portion 146a. An insulating cap 174 made of an insulating material may be interposed between the first current collector plate 144 and the inner surface of the battery case 171. The insulating cap 174 covers the upper part of the first current collector plate 144 and the upper edge portion of the electrode assembly 141. This prevents the blank portion on the outer circumference of the electrode assembly 141 from coming into contact with the inner surface of the battery case 171, which has a different polarity, and causing a short circuit. The terminal insertion portion 172b of the rivet terminal 172 may be welded to the first current collector plate 144, passing through the insulating cap 174.
[0161] The second gasket 173 is interposed between the battery case 171 and the rivet terminal 172, preventing the battery case 171 and the rivet terminal 172, which have opposite polarities, from making electrical contact. This allows the top surface of the battery case 171, which has a substantially flat shape, to function as the positive terminal of the cylindrical lithium secondary battery 170.
[0162] The second gasket 173 includes a gasket exposed portion 173a and a gasket inserted portion 173b. The gasket exposed portion 173a is interposed between the terminal exposed portion 172a of the rivet terminal 172 and the battery case 171. The gasket inserted portion 173b is interposed between the terminal inserted portion 172b of the rivet terminal 172 and the battery case 171. The gasket inserted portion 173b is deformed together with the terminal inserted portion 172b during reveting, and can be made to adhere tightly to the inner surface of the battery case 171. The second gasket 173 may be made of, for example, an insulating polymer resin.
[0163] The gasket exposed portion 173a of the second gasket 173 may have a shape that extends to cover the outer circumferential surface of the terminal exposed portion 172a of the rivet terminal 172. When the second gasket 173 covers the outer circumferential surface of the rivet terminal 172, it is possible to prevent short circuits from occurring during the process of connecting electrical connecting components such as busbars to the upper surface of the battery case 171 and / or the rivet terminal 172. Although not shown in the drawings, the gasket exposed portion 173a may have a shape that extends to cover not only the outer circumferential surface of the terminal exposed portion 172a but also a part of the upper surface.
[0164] When the second gasket 173 is made of a polymer resin, the second gasket 173 may be bonded to the battery case 171 and the rivet terminal 172 by heat fusion. In this case, the airtightness at the bonding interface between the second gasket 173 and the rivet terminal 172, and at the bonding interface between the second gasket 173 and the battery case 171 can be enhanced. On the other hand, when the gasket exposed portion 173a of the second gasket 173 extends to the upper surface of the terminal exposed portion 172a, the rivet terminal 172 may be integrally bonded to the second gasket 173 by insert injection.
[0165] On the upper surface of the battery case 171, the remaining area 175, excluding the area occupied by the rivet terminal 172 and the second gasket 173, corresponds to the negative terminal having the opposite polarity to the rivet terminal 172.
[0166] The second current collector plate 176 is coupled to the lower part of the electrode assembly 141. The second current collector plate 176 is made of a conductive metal material such as aluminum, steel, copper, or nickel, and is electrically connected to the blank portion 146b of the negative electrode.
[0167] Preferably, the second current collector plate 176 is electrically connected to the battery case 171. For this purpose, at least a portion of the edge of the second current collector plate 176 may be interposed and fixed between the inner surface of the battery case 171 and the first gasket 178b. For example, at least a portion of the edge of the second current collector plate 176 may be fixed to the beading portion 180 formed at the lower end of the battery case 171 by welding, while being supported by the lower end surface of the beading portion 180. In a modified example, at least a portion of the edge of the second current collector plate 176 may be directly welded to the inner wall surface of the battery case 171.
[0168] The second current collector plate 176 may have a plurality of radially formed bumps (not shown) on the surface facing the plain portion 146b. If bumps are formed, the second current collector plate 176 can be pressed to press the bumps into the plain portion 146b.
[0169] Preferably, the ends of the second current collector plate 176 and the plain portion 146b may be joined by welding, for example, laser welding.
[0170] The sealing body 178 that seals the lower open end of the battery case 171 includes a cap plate 178a and a first gasket 178b. The first gasket 178b electrically isolates the cap plate 178a from the battery case 171. The crimping portion 181 secures both the edge of the cap plate 178a and the first gasket 178b. The cap plate 178a is provided with a venting portion 179. The configuration of the venting portion 179 is substantially the same as that of the embodiment described above.
[0171] Preferably, the cap plate 178a is made of a conductive metal material. However, since the first gasket 178b is interposed between the cap plate 178a and the battery case 171, the cap plate 178a does not exhibit electrical polarity. The seal 178 seals the open end at the bottom of the battery case 171 and functions to release gas when the internal pressure of the battery cell 170 increases above a threshold.
[0172] Preferably, the rivet terminal 172 electrically connected to the blank positive electrode portion 146a is used as the positive electrode terminal. Also, on the upper surface of the battery case 171 electrically connected to the blank negative electrode portion 146b via the second current collector plate 176, the portion 175 excluding the rivet terminal 172 is used as the negative electrode terminal. In this way, when the two electrode terminals are located on the upper part of the lithium secondary battery, it is possible to arrange electrical connecting components such as busbars on only one side of the cylindrical lithium secondary battery 170. This leads to a simplification of the battery pack structure and an improvement in energy density. Furthermore, since the portion 175 used as the negative electrode terminal has a substantially flat shape, a sufficient bonding area can be secured when joining electrical connecting components such as busbars. As a result, the cylindrical lithium secondary battery 170 can reduce the resistance at the bonding site of the electrical connecting components to a desirable level.
[0173] When lithium secondary batteries are formed with a tabless structure as described above, current concentration is reduced compared to conventional batteries with electrode tabs. This effectively reduces heat generation inside the battery, thereby improving the thermal safety of the battery.
[0174] Battery pack The cylindrical lithium secondary battery of the present invention, as described above, may be included as a unit cell in the manufacture of a battery pack. Figure 6 schematically shows the configuration of a battery pack according to an embodiment of the present invention. Referring to Figure 6, the battery pack 3 according to an embodiment of the present invention includes an assembly of electrically connected lithium secondary batteries 1 and a pack housing 2 that houses them. The lithium secondary battery 1 is the lithium secondary battery according to the above embodiment. For convenience of illustration, the drawings omit the illustration of components such as busbars for the electrical connection of the lithium secondary battery 1, cooling units, and external terminals.
[0175] The battery pack 3 can be mounted in an automobile. The automobile may be, for example, an electric vehicle, a hybrid vehicle, or a plug-in hybrid vehicle. The automobile includes four-wheeled vehicles and two-wheeled vehicles.
[0176] The present invention will be described in more detail below with reference to specific examples.
[0177] Example 1 <Manufacturing of negative electrodes> A negative electrode slurry was prepared by adding a negative electrode active material, a conductive material, and a binder to distilled water in a weight ratio of 98:0.2:1.8. Graphite was used as the negative electrode active material, carbon nanotubes as the conductive material, and a cellulose-based binder.
[0178] The negative electrode slurry was applied to a copper current collector with a thickness of 8 μm and dried, and then roll-pressed to produce a negative electrode containing a negative electrode active material layer. At this time, the thickness of the negative electrode was 190 μm, and the loading amount was 0.35 g / 25 cm 2The porosity was 25.5%.
[0179] <Manufacturing of electrode assemblies> A cathode slurry was prepared by adding a cathode active material, a conductive material, and a binder to N-methylpyrrolidone in a weight ratio of 98:0.5:1.5. In this process, lithium nickel cobalt manganese oxide was used as the cathode active material, carbon nanotubes as the conductive material, and PVDF as the binder.
[0180] The positive electrode slurry was applied to an aluminum current collector and dried, after which a roll press was used to manufacture the positive electrode.
[0181] A jelly roll-type electrode assembly was manufactured by interposing a separator between the positive and negative electrodes produced as described above, stacking them in the order of separator / positive electrode / separator / negative electrode, and then winding them up.
[0182] <Electrolyte Manufacturing> An electrolyte was prepared by adding LiPF6 at a molar concentration of 1.25 M to an organic solvent mixture of ethylene carbonate (EC), dimethyl carbonate (DMC), and ethyl methyl carbonate (EMC) in a weight ratio of 2:7:1.
[0183] <Manufacturing of lithium-ion secondary batteries> The electrode assembly manufactured above has a total internal volume of 122.93 cm³. 3 After inserting it into a cylindrical battery case, 25.7 mL of the electrolyte prepared above was injected to produce 4680 cells (diameter: 46 mm, height: 80 mm). At this time, the dead volume (V) of the produced lithium secondary battery was measured. d ) is 16.7cm 3 , void volume (V p ) is 26cm 3 It was measured as follows.
[0184] Example 2 <Manufacturing of negative electrodes> The manufactured negative electrode has a thickness of 190 μm, and the loading amount is 0.35 g / 25 cm².2 The negative electrode was manufactured using the same method as in Example 1, except that the porosity was 25.5%.
[0185] <Manufacturing of electrode assemblies> The electrode assembly was manufactured in the same manner as in Example 1, except that the negative electrode manufactured as described above was used.
[0186] <Electrolyte Manufacturing> An electrolyte was produced by the same method as in Example 1.
[0187] <Manufacturing of lithium-ion secondary batteries> The electrode assembly manufactured as described above has an internal volume of 122.93 cm³. 3 After inserting it into a cylindrical battery case, 27.7 mL of the electrolyte prepared above was injected to produce 4680 cells (diameter: 46 mm, height: 80 mm). At this time, the dead volume (V) of the manufactured lithium secondary battery was measured. d ) is 16.7cm 3 , void volume (V p ) is 26cm 3 It was measured as follows.
[0188] Example 3 <Manufacturing of negative electrodes> The manufactured negative electrode had a thickness of 188 μm, and the loading amount was 0.35 g / 25 cm. 2 The negative electrode was manufactured using the same method as in Example 1, except that the porosity was 25.9%.
[0189] <Manufacturing of electrode assemblies> The electrode assembly was manufactured in the same manner as in Example 1, except that the negative electrode manufactured as described above was used.
[0190] <Electrolyte Manufacturing> An electrolyte was produced by the same method as in Example 1.
[0191] <Manufacturing of lithium-ion secondary batteries> The electrode assembly manufactured as described above has an internal volume of 122.93 cm³.3 After inserting it into a cylindrical battery case, 25.8 mL of the electrolyte prepared above was injected to produce a 4680 cell (diameter: 46 mm, height: 80 mm). At this time, the dead volume (V) of the manufactured lithium secondary battery was measured. d ) is 16.7cm 3 , void volume (V p ) is 26.2cm 3 It was measured as follows.
[0192] Example 4 <Manufacturing of negative electrodes> The manufactured negative electrode had a thickness of 184 μm, and the loading amount was 0.37 g / 25 cm². 2 The negative electrode was manufactured using the same method as in Example 1, except that the porosity was 24.7%.
[0193] <Manufacturing of electrode assemblies> The electrode assembly was manufactured in the same manner as in Example 1, except that the negative electrode manufactured as described above was used.
[0194] <Electrolyte Manufacturing> An electrolyte was produced by the same method as in Example 1.
[0195] <Manufacturing of lithium-ion secondary batteries> The electrode assembly manufactured as described above has an internal volume of 122.93 cm³. 3 After inserting it into a cylindrical battery case, 27.6 mL of the electrolyte prepared above was injected to produce a 4680 cell (diameter: 46 mm, height: 80 mm). At this time, the dead volume (V) of the produced 4680 cell was measured. d ) is 16.27cm 3 , void volume (V p ) is 26.07cm 3 It was measured as follows.
[0196] Example 5 <Manufacturing of negative electrodes> The manufactured negative electrode had a thickness of 184.1 μm, and the loading amount was 0.37 g / 25 cm². 2, and a porosity of 24.0%, a negative electrode was produced in the same manner as in Example 1 above.
[0197] <Production of Electrode Assembly> An electrode assembly was produced in the same manner as in Example 1 above, except that the negative electrode produced above was used.
[0198] <Production of Electrolyte> An electrolyte was produced in the same manner as in Example 1 above.
[0199] <Production of Lithium Secondary Battery> The electrode assembly produced above was placed in a cylindrical battery case having a total internal space volume of 122.93 cm 3 , and then 26.2 mL of the electrolyte produced above was injected, to fabricate a 4680 cell (diameter: 46 mm, height: 80 mm). At this time, the dead volume (V d ) of the fabricated 4680 cell was 16.27 cm 3 , and the void volume (V p ) was measured to be 25.17 cm 3 .
[0200] Comparative Example 1 <Production of Negative Electrode> A negative electrode was produced in the same manner as in Example 1 above, except that the produced negative electrode had a thickness of 190 μm, a loading amount of 0.35 g / 25 cm 2 , and a porosity of 25.5%.
[0201] <Production of Electrode Assembly> An electrode assembly was produced in the same manner as in Example 1 above, except that the negative electrode produced above was used.
[0202] <Production of Electrolyte> An electrolyte was produced in the same manner as in Example 1 above.
[0203] <Production of Lithium Secondary Battery> The electrode assembly produced above was placed in a cylindrical battery case having a total internal space volume of 122.93 cm 3After inserting into a cylindrical battery case, 29 mL of the electrolyte prepared above was injected to fabricate a 4680 cell (diameter: 46 mm, height: 80 mm. At this time, the dead volume (V of the fabricated 4680 cell d ) was 16.6 cm 3 , and the void volume (V p ) was measured to be 26.1 cm 3 .
[0204] Comparative Example 2 <Preparation of Negative Electrode> A negative electrode was fabricated in the same manner as in Example 1, except that the thickness of the fabricated negative electrode was 188 μm, and the loading amount was 0.36 g / 25 cm 2 , and the porosity was 25.0%.
[0205] <Fabrication of Electrode Assembly> An electrode assembly was fabricated in the same manner as in Example 1, except that the negative electrode prepared above was used.
[0206] <Preparation of Electrolyte> An electrolyte was prepared in the same manner as in Example 1.
[0207] <Fabrication of Lithium Secondary Battery> After inserting the electrode assembly fabricated above into a cylindrical battery case having a total internal space volume of 122.93 cm 3 , 29 mL of the electrolyte prepared above was injected to fabricate a 4680 cell (diameter: 46 mm, height: 80 mm). At this time, the dead volume (V of the fabricated 4680 cell d ) was 16.4 cm 3 , and the void volume (V p ) was measured to be 25.6 cm 3 .
[0208] Comparative Example 3 <Preparation of Negative Electrode> A negative electrode was fabricated in the same manner as in Example 1, except that the thickness of the fabricated negative electrode was 187 μm, and the loading amount was 0.36 g / 25 cm 2 , and the porosity was 25.3%.
[0209] <Manufacturing of electrode assemblies> The electrode assembly was manufactured in the same manner as in Example 1, except that the negative electrode manufactured as described above was used.
[0210] <Electrolyte Manufacturing> An electrolyte was produced by the same method as in Example 1.
[0211] <Manufacturing of lithium-ion secondary batteries> The electrode assembly manufactured as described above has an internal volume of 122.93 cm³. 3 After inserting it into a cylindrical battery case, 29 mL of the electrolyte prepared above was injected to produce a 4680 cell (diameter: 46 mm, height: 80 mm). At this time, the dead volume (V) of the produced 4680 cell was measured. d ) is 16.3cm 3 , void volume (V p ) is 26.1cm 3 It was measured as follows.
[0212] Comparative Example 4 <Manufacturing of negative electrodes> The manufactured negative electrode has a thickness of 190 μm, and the loading amount is 0.35 g / 25 cm². 2 The negative electrode was manufactured using the same method as in Example 1, except that the porosity was 25.0%.
[0213] <Manufacturing of electrode assemblies> The electrode assembly was manufactured in the same manner as in Example 1, except that the negative electrode manufactured as described above was used.
[0214] <Electrolyte Manufacturing> An electrolyte was produced by the same method as in Example 1.
[0215] <Manufacturing of lithium-ion secondary batteries> The electrode assembly manufactured as described above has an internal volume of 122.93 cm³. 3After inserting into a cylindrical battery case, 30.6 mL of the electrolyte prepared above was injected to fabricate a 4680 cell (diameter: 46 mm, height: 80 mm). At this time, the dead volume (V d ) of the fabricated 4680 cell was 16.5 cm 3 , and the void volume (V p ) was 25.6 cm 3 as measured.
[0216] Comparative Example 5 <Preparation of Negative Electrode> A negative electrode was fabricated in the same manner as in Example 1 above, except that the thickness of the fabricated negative electrode was 190 μm, the loading amount was 0.35 g / 25 cm 2 , and the porosity was 24.0%.
[0217] <Fabrication of Electrode Assembly> An electrode assembly was fabricated in the same manner as in Example 1 above, except that the negative electrode fabricated above was used.
[0218] <Preparation of Electrolyte> An electrolyte was prepared in the same manner as in Example 1 above.
[0219] <Fabrication of Lithium Secondary Battery> After inserting the electrode assembly fabricated above into a cylindrical battery case with a total internal space volume of 122.93 cm 3 , 30.6 mL of the electrolyte prepared above was injected to fabricate a 4680 cell (diameter: 46 mm, height: 80 mm). At this time, the dead volume (V d ) of the fabricated 4680 cell was 16 cm 3 , and the void volume (V p ) was 25.1 cm 3 as measured.
[0220] Comparative Example 6 <Preparation of Negative Electrode> The thickness of the fabricated negative electrode was 190 μm, and the loading amount was 0.0.33 g / 25 cm 2The negative electrode was manufactured using the same method as in Example 1, except that the porosity was 24.6%.
[0221] <Manufacturing of electrode assemblies> The electrode assembly was manufactured in the same manner as in Example 1, except that the negative electrode manufactured as described above was used.
[0222] <Electrolyte Manufacturing> An electrolyte was produced by the same method as in Example 1.
[0223] <Manufacturing of cylindrical lithium-ion secondary batteries> After inserting the electrode assembly manufactured above into a cylindrical battery case, the electrolyte manufactured above was injected to produce a 2170 cell (diameter: 21 mm, height: 70 mm).
[0224] Experimental Example 1: Measurement of P-value The characteristics of the cylindrical lithium secondary batteries manufactured in Examples 1 to 5 and Comparative Examples 1 to 6, and the P-values defined by the following formula 1, are shown in Table 1 below.
[0225] [Formula 1]
number
[0226] In the above formula 1, H (unit: mm) represents the height of the lithium secondary battery, R (unit: mm) represents the diameter of the lithium secondary battery, and t a (Unit: μm) represents the thickness of the negative electrode, L a (Unit: g / 25cm) 2 ) refers to the loading amount of the negative electrode, P a (Unit: %) represents the porosity of the negative electrode, V c (Unit: cm) 3 ) refers to the volume of empty space inside a lithium-ion battery.
[0227] In this case, the V cThe cylindrical lithium secondary batteries manufactured in Examples 1-5 and Comparative Examples 1-6 were activated by charging them to a voltage of 4.2V at 25°C and then discharging them, and the calculation was performed using the following formula B.
[0228] [Equation B] Volume V of the empty space inside the lithium secondary battery c (cm 3 )=V d +V p -V e
[0229] In the above formula B, V d This is the dead volume inside the battery case, V p V is the void volume. e V is the volume of the electrolyte. d , V p , V e These were measured using the following methods:
[0230] The dead volume V inside the aforementioned battery case d This is the volume of the cylindrical lithium secondary battery, excluding the volume occupied by the electrode assembly and the volume occupied by the battery case. The volume of the cylindrical lithium secondary battery was obtained by measuring the volume of the external shape of the cylindrical battery case when the cylindrical battery case used in Examples 1 to 5 and Comparative Examples 1 to 6 was sealed.
[0231] The aforementioned void volume V p The porosity was measured by multiplying the respective volumes of the positive electrode, negative electrode, and separator in Examples 1-5 and Comparative Examples 1-6 by their respective porosities.
[0232] Volume V of the electrolyte e The weight of the electrolyte remaining in the lithium secondary battery was calculated by dividing the weight of the electrolyte remaining in the lithium secondary battery by the density of the electrolyte. The weight of the electrolyte remaining in the lithium secondary battery was (1) the weight of the lithium secondary batteries produced in the above examples 1 to 5 and comparative examples 1 to 6 that underwent activation (M L(1) The steps of measuring the weight (M) of the dried battery case; (2) Disassembling the lithium secondary battery and removing the electrolyte present in the battery case; (3) Immersing the battery case and electrode assembly in dimethyl carbonate, which is a solvent, to remove the electrolyte present on the surface of the battery case, the surface of the electrode assembly, and in the internal voids, and then drying the battery case and electrode assembly; (4) Measuring the weight (M) of the dried battery case. C ), and the weight (M) of the dried electrode assembly. A After going through the step of measuring ), the measured M L M C M A This can be measured by substituting it into the following formula B-1.
[0233] [Formula B-1] Weight of electrolyte remaining in lithium secondary battery = M L -M C -M A
[0234] [Table 1]
[0235] Referring to Table 1 above, it can be confirmed that the lithium secondary batteries manufactured in Examples 1 to 5 have a P value of less than 8.7, while the lithium secondary batteries manufactured in Comparative Examples 1 to 6 have a P value of 8.7 or higher.
[0236] Experimental Example 2: Evaluation of the presence or absence of lithium plating during rapid charging Each lithium secondary battery manufactured in Examples 1-5 and Comparative Examples 1-6 was charged in CC / CV mode at 40°C with a constant current (CC) of 1.0C until it reached 4.2V (cut-off current 0.05C), and then discharged in CC mode with a constant current (CC) of 1.0C until it reached 2.5V. The charging and discharging process was considered one cycle, and after repeating the charge and discharge cycle 100 times, the lithium secondary batteries were disassembled, the electrode assemblies were separated, and it was visually checked whether lithium plating had occurred on the negative electrode surface. The results are shown in Table 2 below. -O: Lithium plating is occurring. -X: No lithium plating has occurred.
[0237] [Table 2]
[0238] Referring to Table 2 above, it can be confirmed that lithium plating did not occur in the lithium secondary batteries manufactured in Examples 1 to 5, but lithium plating did occur in the lithium secondary batteries manufactured in Comparative Examples 1 to 6. In particular, even the lithium secondary battery manufactured in Comparative Example 6, which has a smaller diameter and height compared to Examples 1 to 5 and Comparative Examples 1 to 5, has a P value of 11.0 or higher, indicating that lithium plating occurred.
[0239] Experimental Example 3: Lifetime characteristics during rapid charging Each lithium secondary battery manufactured in Examples 1-5 and Comparative Examples 1-6 was charged in CC / CV mode at 40°C with a constant current (CC) of 1.0C until it reached 4.2V (cut-off current 0.05C), and then discharged in CC mode with a constant current (CC) of 1.0C until it reached 2.5V. The charging and discharging process was considered one cycle, and after repeating the charge-discharge cycle 100 times, the capacity retention rate was measured. The results are shown in Table 3 below.
[0240] [Table 3]
[0241] Referring to Table 3 above, it can be confirmed that the lithium secondary batteries manufactured in Examples 1 to 5 have superior capacity retention at high temperatures compared to the lithium secondary batteries manufactured in Comparative Examples 1 to 6.
[0242] Experimental Example 4: Evaluation of Initial Battery Characteristics (1) Evaluation of initial discharge capacity The initial discharge capacity of the lithium secondary batteries manufactured in Examples 1-5 and Comparative Examples 1-6 was measured.
[0243] Specifically, each cell was charged to 4.2V at 40°C with a constant current of 0.33C, and then discharged to 2.5V with a power of 19.1W to evaluate its initial discharge capacity. The measurement results are shown in Table 4 below.
[0244] (2) Evaluation of initial resistance The initial resistance of the lithium secondary batteries manufactured in Examples 1-5 and Comparative Examples 1-6 was measured.
[0245] Specifically, each lithium secondary battery was charged to 100% State of Charge (SOC) at 40°C with a constant current of 0.25C, then discharged to 50% SOC with a constant current of 0.5C for 10 seconds. The initial resistance (DCIR) was then calculated from the voltage drop observed during this discharge. The measurement results are shown in Table 4 below.
[0246] [Table 4]
[0247] Referring to Table 4 above, it can be confirmed that the lithium secondary batteries manufactured in Examples 1, 2, 4, and 5 have improved initial resistance and discharge capacity compared to the lithium secondary battery manufactured in Example 3. From this, it can be seen that lithium secondary batteries with a P value of 7.4 to 8.6 are more preferable than lithium secondary batteries with a P value of less than 8.7 because they are superior in rapid charging characteristics, initial resistance, and capacity characteristics. [Explanation of symbols]
[0248] 1. Lithium-ion rechargeable battery 2-pack housing 3 Battery pack 10 positive electrode 11 Negative electrode 12 Separators 20 Current collector 21 Active material layer 21a Negative electrode active material layer 22 Plain section 22a Negative electrode blank area 22c Positive electrode blank area 24 Insulating layer C Winding center 140 Cylindrical Lithium Rechargeable Batteries 141 Electrode assembly 142 Battery Case 143 Sealed body 143a Cap plate 143b First Gasket 143c Connecting Plate 143d Protrusion 144 First current collection plate 145 Second current collection plate 146 Insulators 146a Positive electrode blank area 146b Negative electrode plain area 147 Beading section 148 Crimping section 149 Reed 151 lead holes 152 Venting section 170 Cylindrical Lithium Rechargeable Battery 171 Battery Case 172 Rivet terminals 172a Exposed terminal part 172b Terminal insertion section 173 Second Gasket 173a Exposed gasket portion 173b Gasket insertion section 174 Insulating cap 176 Second current collection plate 178 Sealed body 178a Cap plate 178b First Gasket 179 Venting section 180 Beading section 181 Crimping section
Claims
1. A cylindrical lithium secondary battery comprising an electrode assembly including a positive electrode, a negative electrode, and a separator interposed between the positive and negative electrodes, an electrolyte, and a battery case in which the electrode assembly and the electrolyte are housed, The electrolyte comprises a lithium salt and an organic solvent. A cylindrical lithium secondary battery having a p-value less than 8.7, as defined by the following formula 1. [Formula 1] [Math 1] (In formula 1 above, H (unit: mm) represents the height of the lithium secondary battery. R (unit: mm) refers to the diameter of the lithium secondary battery. t a (Unit: μm) represents the thickness of the negative electrode. L a (Unit: g / 25cm) 2 ) refers to the loading amount of the negative electrode, P a (Unit: %) represents the porosity of the negative electrode. V c (Unit: cm) 3 ) refers to the volume of empty space inside a lithium-ion battery.
2. The cylindrical lithium secondary battery according to claim 1, wherein the P value represented by the formula 1 is 7.4 to 8.
6.
3. The aforementioned V c is 17.5 cm 3 to 25 cm 3 , the cylindrical lithium secondary battery according to claim 1.
4. The volume of the empty space inside the lithium secondary battery relative to the total volume (V) of the internal space inside the battery case. c ) ratio (V c The cylindrical lithium secondary battery according to claim 1, wherein the voltage (V) is 0.08 to 0.
25.
5. The cylindrical lithium secondary battery according to claim 1, wherein the ratio of H to R (R / H) is 0.4 or more.
6. The aforementioned P a A cylindrical lithium secondary battery according to claim 1, wherein the content is 23.5% or more.
7. Said L a 0.25g / 25cm 2 ~0.45g / 25cm 2 The cylindrical lithium secondary battery according to claim 1.
8. Said t a The cylindrical lithium secondary battery according to claim 1, wherein the diameter is 180 μm to 200 μm.
9. The aforementioned negative electrode includes a negative electrode active material layer containing a negative electrode active material, The cylindrical lithium secondary battery according to claim 1, wherein the negative electrode active material includes a carbon-based active material.
10. The aforementioned negative electrode includes a negative electrode active material layer containing a negative electrode active material, The cylindrical lithium secondary battery according to claim 1, wherein the negative electrode active material is present in an amount of 90% to 99% by weight based on the total weight of the negative electrode active material layer.
11. The cylindrical lithium secondary battery according to claim 1, wherein the concentration of the lithium salt is 1.0 M to 1.5 M.
12. The lithium salt is LiPF 6 LiClO 4 LiAsF 6 LiBF 4 LiSbF 6 LiAlO 4 LiAlCl 4 LiCF 3 SO 3 LiC 4 F 9 SO 3 ,LiN(C 2 F 5 SO 3 ) 2 ,LiN(C 2 F 5 SO 2 ) 2 ,LiN(CF 3 SO 2 ) 2 A cylindrical lithium secondary battery according to claim 1, comprising one or more selected from the group consisting of LiCl and LiI.
13. The cylindrical lithium secondary battery according to claim 1, wherein the organic solvent comprises one or more selected from the group consisting of cyclic carbonate organic solvents, linear carbonate organic solvents, linear ester organic solvents, and cyclic ester organic solvents.
14. A cylindrical lithium secondary battery according to claim 1, comprising 46110 cells, 48110 cells, 4880 cells, or 4680 cells.
15. The cylindrical lithium secondary battery according to claim 1, wherein at least a portion of the positive electrode and the negative electrode includes a blank portion on which no active material layer is formed, and the blank portion of the positive electrode and the blank portion of the negative electrode are defined as electrode tabs.
16. The cylindrical lithium secondary battery according to claim 15, wherein the blank positive electrode portion and the blank negative electrode portion are each formed at one end of the positive electrode and the negative electrode, along the direction in which the electrode assembly is wound, a current collector plate is bonded to each of the blank positive electrode portion and the blank negative electrode portion, and the current collector plate is connected to an electrode terminal.
17. The plain positive electrode portion and the plain negative electrode portion are processed into a plurality of independently bendable segment pieces. The cylindrical lithium secondary battery according to claim 15, wherein at least a portion of the plurality of segment pieces is bent toward the winding center of the electrode assembly.
18. The cylindrical lithium secondary battery according to claim 17, wherein at least a portion of the bent plurality of segment pieces overlap on the upper and lower ends of the electrode assembly, and a current collector plate is bonded to the overlapping plurality of segment pieces.
19. A battery pack comprising a cylindrical lithium secondary battery as a unit cell according to any one of claims 1 to 18.