Asymmetrical layered glazing and method for manufacturing the same
Asymmetric laminated glazing with specific bending curvatures and a flattening coefficient greater than 250 enhances robustness and reduces weight by avoiding chemical strengthening, addressing production inefficiencies and environmental concerns.
Patent Information
- Application Number
- JP2026529109
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-11-15
- Filing Date
- 2024-11-13
- Publication Date
- 2026-11-19
AI Technical Summary
Existing asymmetric laminated glazing production methods are costly, time-consuming, and environmentally undesirable due to chemical strengthening, leading to low yields and increased weight and bulk, while lacking robustness due to thinner glass sheets.
Asymmetric laminated glazing with a thicker first glass sheet thermally strengthened and a thinner second glass sheet not chemically or thermally strengthened, featuring specific bending curvatures and a flattening coefficient greater than 250, allowing for a substantially planar geometry that enhances robustness without additional strengthening treatments.
The method produces a simpler, more environmentally friendly, and robust laminated glazing with reduced weight and bulk, eliminating the need for chemical strengthening and maintaining excellent impact resistance.
Smart Images

Figure 2026539109000001_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the general field of glazing production.
[0002] The present invention relates more particularly to asymmetric laminated glazing as well as methods for manufacturing such asymmetric laminated glazing. The invention is particularly advantageously applied, without being limited thereto, in the manufacture of laminated glazing for the automotive field (roofs, side window panes, windshields, rear windows).
Background Art
[0003] The technology for manufacturing glazing to be fitted to motor vehicles has evolved significantly in response to various design criteria.
[0004] Thus, automotive glazing, in particular side glazing, was initially designed in a monolithic manner using thermal tempering treatment. This approach made it possible to achieve excellent strength properties.
[0005] Subsequently, designs of laminated glazing in which the glass sheets used have the same thickness were proposed. Such laminated glazing makes it possible to achieve very high strength, while at the same time proposing the addition of various functionalities, such as, for example, an acoustic attenuation function. Furthermore, the combination of this lamination principle with thermal tempering or semi-tempering operations of the glass sheets further enhances the strength of the produced glazing, particularly against external impacts (especially in the case of break-ins and sometimes flying gravel) or internal impacts (laminated glazing makes it possible to keep occupants inside the vehicle in the event of an accident and vehicle rollover; thus preventing fatal injuries when occupants are partially ejected from the vehicle).
[0006] However, such laminated glazing is not without its drawbacks. In particular, these laminated glazings constitute an extremely heavy and bulky element. Therefore, design practice has continued to evolve towards the production of laminated glazing with reduced weight and external dimensions. Thus, more recently, it has been proposed to manufacture laminated glazing called "asymmetrical," that is, laminated glazing in which two combined glass sheets have different thicknesses. In practice, the glazing generally consists of very thin glass sheets, typically in the millimeter range, which are positioned facing the internal environment (e.g., the inside of the vehicle). Therefore, generally, the thicker glass sheet is positioned facing the external environment (e.g., the outside of the vehicle).
[0007] The fact that one glass sheet is much thinner than the other can lead to a decrease in rigidity and, consequently, a deterioration in impact resistance. To mitigate this drawback, manufacturers have consistently chosen to harden even the thinnest glass sheets, more specifically by using chemical strengthening.
[0008] This method has several drawbacks. In fact, chemical strengthening is a costly, time-consuming, and complex process because it requires maintaining glass sheets at high temperatures for several hours in different alkaline salt baths to obtain a good surface stress level. This results in extremely low yields due to significant breakage during handling, cleaning before and after chemical strengthening, and during the strengthening process itself. Moreover, it is an environmentally undesirable solution because the treated products are difficult to reuse.
[0009] While the elements described above have been explained in relation to applications in autonomous vehicles, it is important to note that they are equally valid in other application areas, such as the housing sector, and even in fields like aviation, maritime, or rail transport. [Overview of the Initiative] [Problems that the invention aims to solve]
[0010] The object of the present invention is to improve, in whole or in part, the shortcomings of the prior art, particularly those mentioned above, by proposing a solution that enables the production of asymmetric laminated glazing having a slightly curved appearance and whose production is simpler and more environmentally friendly than the production of asymmetric glazing in the current technological standing. [Means for solving the problem]
[0011] For this purpose, according to a first aspect, the present invention relates to a laminated glazing comprising first and second glass sheets combined by an intermediate layer, wherein the first glass sheet is heat-strengthened and has a thickness greater than 1.8 mm, and the second glass sheet is not strengthened and has a thickness less than 1.6 mm, and the glazing has at least one first bending curvature (curve) that defines the bending depth between the arc of the surface and the chord supporting the arc, and is associated with a first bending ratio between the length of the chord and the bending depth, and the glazing is further molded to have a flattening coefficient greater than 250 which is at least equivalent to the first bending ratio.
[0012] In its general principle, the laminated glazing according to the present invention corresponds to asymmetric laminated glazing and is configured to avoid the drawbacks inherent in the implementation of chemical strengthening, based on the results obtained by the inventors after conducting simulations and tests.
[0013] More specifically, starting from the confirmed fact that laminated glazings are increasingly being manufactured to have a nearly planar geometry (which is particularly, but not exclusively, valuable in the automotive field), the inventors have sought to characterize acceptable curvatures for asymmetric laminated glazings, assuming that the asymmetric laminated glazing, once assembled, possesses excellent robustness (due to sufficient stress levels within the thickest glass sheet and the presence of an intermediate layer), while ensuring a low stress level within the thinnest glass sheet (i.e., the second glass sheet in this case), eliminating the need to strengthen all or part of the glass sheets included in its composition.
[0014] Therefore, the solution proposed by the present invention consists of an asymmetrical laminated glazing in which the thinnest glass sheet is not subjected to any strengthening treatment. In other words, the second glass sheet is not subjected to any thermal strengthening (semi-strengthening or strengthening) or any chemical strengthening, and is therefore formed directly from flat glass supplied at the exit of the float glass (so-called "float" glass in English literature) production line.
[0015] Furthermore, in order to compensate for the absence of a reinforcing treatment of the second glass sheet and to minimize the risk of breakage of this glass sheet, the glazing according to the present invention has a substantially planar geometry characterized by the values that the flattening coefficient can take.
[0016] This substantially planar geometry is realized within limits that allow for advantageously superior robustness while avoiding the need to perform a second strengthening treatment on the glass sheet.
[0017] In certain embodiments, the laminated glazing may further include one or more of the following features, which are addressed individually or in all technically possible combinations:
[0018] In certain embodiments, the glazing has a second curvature in a direction substantially orthogonal to the first curvature so as to be associated with a second bending ratio, and the flattening factor is equal to the sum of the first and second bending ratios.
[0019] In certain embodiments, the flattening factor is greater than 500.
[0020] In certain embodiments, the thickness of the second glass sheet is less than 1.2 mm, for example less than 1 mm.
[0021] In certain embodiments, the thickness of the first glass sheet is greater than 2.1 mm, or greater than 2.6 mm, or greater than 2.85 mm, or greater than 3.15 mm, or greater than 3.5 mm, or greater than 3.85 mm.
[0022] In certain embodiments, the intermediate layer comprises a polymer material including a polyvinyl butyral layer having a loss factor tan(δ) of greater than 0.8 and a shear modulus G' of less than 20 MPa at a temperature of 20°C and at frequencies from 500 Hz to 5000 Hz.
[0023] In certain embodiments, the intermediate layer comprises a transparent adhesive material of the "OCA" type, such as a latex adhesive.
[0024] In certain embodiments, the intermediate layer is made of ethylene vinyl acetate.
[0025] In a second aspect, the present invention relates to the use of the glazing according to the present invention as glazing for windows in residential buildings or land, air, marine or rail transportation means, preferably for motor vehicle windows, in particular as windshields, rear glazing, side glazing or roof glazing.
[0026] According to a third aspect, the present invention relates to a motor vehicle comprising the glazing according to the present invention.
[0027] According to a fourth aspect, the present invention relates to a method for producing a glazing according to the present invention, the method comprising: - obtaining a first flat glass sheet and a second flat glass sheet; - a step of hot bending the first glass sheet in accordance with a flattening coefficient; - a step of thermally strengthening the first glass sheet; - a step of assembling the first glass sheet and the second glass sheet into a single laminated glazing, wherein an interlayer is arranged between the first glass sheet and the second glass sheet, and the assembling includes cold bending of the second glass sheet relative to the first glass sheet; - a step of extracting air contained in the assembled laminated glazing; The present invention relates to a method including the above steps.
[0028] The production method according to the present invention is particularly advantageous in that it makes it possible to obtain a robust asymmetric laminated glazing whose production is simpler and more environmentally friendly compared to asymmetric glazings of the current state of the art, due to the absence of a strengthening treatment for the thinnest glass sheet.
[0029] In certain embodiments, the production method may further comprise one or more of the following features, taken individually or in all technically possible combinations.
[0030] In certain embodiments, the air extraction step is performed by calendering the laminated glazing.
[0031] In certain embodiments, where the glazing comprises a PVB interlayer, in particular for example an acoustic PVB, the method further comprises, after the air extraction step, an autoclaving step of the assembled laminated glazing.
[0032] In certain embodiments, the assembly step includes maintaining the stack formed by the glass sheets and the intermediate layer in place after the cold bending of the second glass sheet.
[0033] Other features and advantages of the present invention will become apparent from the following description with reference to the accompanying drawings illustrating embodiments that are not limiting in any way. [Brief explanation of the drawing]
[0034] [Figure 1] This diagram schematically illustrates a specific embodiment of the asymmetric laminated glazing according to the present invention. [Figure 2] Figure 1 schematically shows the two bending curvatures of the asymmetric laminated glazing. [Figure 3] This table illustrates surface stress values measured at the level of the thinnest glass sheet belonging to the asymmetrical laminated glazing shown in Figure 1. [Figure 4] The main steps of the manufacturing method for asymmetric laminated glazing according to the present invention are shown in flowchart form. [Modes for carrying out the invention]
[0035] [Detailed description of the invention] Figure 1 schematically shows a specific embodiment of the laminated glazing 100 according to the present invention.
[0036] For the purposes of the following explanation, we will assume, in no particular way, that the laminated glazing 100 is intended for use in an automated vehicle, such as a passenger car. More specifically, this refers to the side glazing of a passenger car, but naturally, the possibility of using it for rear glazing, windshield glazing, and even roof glazing is not ruled out.
[0037] However, it is important to note that considering this type of glazing and the fields of application for its use constitutes only one variation of the implementation of the present invention. In general, there are no limitations on the possible uses of glazing 100. For example, it can be used in housing (room separation, wall glazing, etc.) and even in all types of transportation (land, air, sea, or rail).
[0038] As illustrated in Figure 1, the glazing 100 includes a first glass sheet 110 and a second glass sheet 120 combined by an intermediate layer 130.
[0039] A "glass sheet" refers to a plate formed from a transparent material. For example, the transparent material may be mineral glass such as soda-lime glass, aluminosilicate glass, or borosilicate glass. Alternatively, the transparent material may be organic glass, such as stretched polymethyl methacrylate (stretched PMMA), unstretched polymethyl methacrylate, polycarbonate (PC), polyethylene terephthalate (PET), or polyurethane (PU). It is appropriate to note that two glass sheets 110 and 120 can be manufactured from different transparent materials.
[0040] Furthermore, one or both of the glass sheets 110 and 120 can be colored glass sheets (colored glass is glass containing a desired inorganic pigment, such as iron oxide, cobalt oxide, or chromium oxide). Note here that the two glass sheets 110 and 120 may be of different colors.
[0041] The intermediate layer 130 is made of a polymer material such as PVB (polyvinyl butyral). More specifically, in this embodiment, this polymer material is of the "acoustic" type, i.e., a type that has the function of reducing sound passing through the glazing 100. To be called acoustic, such a polymer material includes at least one polymer material (generally PVB) layer having a loss factor tan(δ) greater than 0.8 and a shear modulus G' less than 20 MPa at a temperature of 20°C and a frequency of 500 Hz to 5000 Hz. These viscoelastic properties can be evaluated by those skilled in the art, for example, using a Metravib 01dB Metravib VA4000 type viscoanalyzer with plane shear measurements in accordance with ISO 6721 (Determination of Dynamic Mechanical Properties).
[0042] When such an acoustic polymer material layer is used, it may constitute the sole layer of the intermediate layer 130 or be juxtaposed with at least one other polymer material layer. The acoustically property-possessed intermediate layer 130 can be realized, in particular, by an assembly of at least three PVB layers, where one inner layer is more flexible than the other two surrounding it. Generally, acoustic polymer materials slightly reduce the stiffness of the laminated glazing compared to conventional polymer materials. Therefore, conventional polymer materials are suitable for laminated glazing where high stiffness is preferred. Conventional polymer materials generally have a shear modulus G' greater than 100 MPa and a loss factor tan(δ) less than 0.4 at a temperature of 20°C and frequencies of 500 Hz to 5000 Hz.
[0043] Furthermore, it is appropriate to point out that the mere consideration of the presence of PVB polymer material, particularly acoustic polymer material, as the intermediate layer 130 constitutes only one variant of the implementation of the present invention. Therefore, the possibility of contemplating other embodiments in which the intermediate layer 130 includes, in combination with or as an alternative to, PVB polymer material, a transparent adhesive material of the "OCA" (an acronym for "Optical Clear Adhesive") type, such as a latex adhesive, more specifically an acoustic latex adhesive (with an adhesive thickness of, for example, less than 100 μm, ideally 30 μm). As an alternative to these embodiments, other embodiments in which the intermediate layer 130 is realized with EVA (ethylene vinyl acetate) are also conceivable.
[0044] The glazing 100 specifically corresponds to asymmetric laminated glazing. As a result, the first and second glass sheets 110 and 120 have different thicknesses. In particular, in the embodiment described with reference to Figure 1, the first glass sheet 110 has a thickness of more than 1.8 mm, while the second glass sheet 120 has a thickness of less than 1.6 mm.
[0045] Considering the intended use of the glazing 100, the first glass sheet 110 (in particular, surface 1 of the glazing 100, in accordance with conventional practices in the field of glazing) is configured to face the external environment of the vehicle. The second glass sheet 120 (in particular, surface 4 of the glazing 100) is configured to face the internal environment of the vehicle (i.e., the passenger compartment).
[0046] It is appropriate to point out that the respective thickness values of the first and second glass sheets 110 and 120 considered in this embodiment do not limit the present invention. Therefore, it is possible to consider other embodiments in which the thickness of the second glass sheet 120 is less than 1.2 mm, for example less than 1 mm, and / or the thickness of the first glass sheet 110 is greater than 2.1 mm, or greater than 2.6 mm, or greater than 2.85 mm, or greater than 3.15 mm, or greater than 3.5 mm, or greater than 3.85 mm.
[0047] The first glass sheet 110, that is, the thicker of the two glass sheets of glazing 100, is thermally strengthened. In other words, the first glass sheet 110 is semi-strengthened or strengthened.
[0048] Thermal strengthening through reinforcement is generally performed immediately after bending the glass (by rapidly cooling the glass from the bending temperature by blowing air onto both sides of the glass) and before assembly of the laminated glazing 100.
[0049] The manufacturing of semi-tempered glass (also known as "thermosetting glass") is carried out using the same equipment as that used for heat-tempered glass. Although the heating conditions are the same, the cooling air blowing output is weaker.
[0050] As is well known, very thin glass sheets, such as the second glass sheet 120, can be subjected to cold bending during the manufacturing of laminated glazing. Cold bending is preferred for this type of glass sheet because hot bending generally affects the optical quality of the glass sheet.
[0051] "Cold bending" traditionally refers to a deformation process that operates within the elastic range of glass. Conversely, hot bending refers to bending at the glass's deformation temperature, causing permanent deformation after returning to ambient temperature. Hot bending is typically performed at temperatures higher than the glass transition temperature and generally above 550°C.
[0052] Cold bending, while preferred, has limitations because glass cannot reach high curvature without significantly increasing the risk of breakage. To limit this risk, current technical conditions indicate that thin glass sheets used in the manufacture of asymmetric laminated glazing should consistently be strengthened by chemical strengthening.
[0053] The general principle of the present invention aims to avoid the inherent drawbacks of chemical strengthening, based on results obtained by the inventors after conducting simulations and tests. In particular, starting from the confirmed fact that laminated glazings are increasingly being manufactured to have substantially planar geometry (which is especially, but not exclusively, valuable in the automotive field), the inventors have sought to characterize an acceptable curvature for asymmetric laminated glazings, assuming that such chemical strengthening treatment is unnecessary while ensuring low stress levels within the thinnest glass sheets, and that the asymmetric laminated glazings have excellent robustness once assembled (due to sufficient stress levels within the thickest glass sheets and the presence of intermediate layers).
[0054] For these reasons, the second glass sheet 120, i.e., the thinner of the two glass sheets of glazing 100, is not tempered. In other words, the second glass sheet 120 is not subjected to any thermal strengthening (partial or tempering) or chemical strengthening, and is therefore formed directly from the flat glass supplied at the exit of the float glass (so-called "float" glass in English literature) production line.
[0055] Furthermore, to compensate for the absence of the strengthening treatment of the second glass sheet 120, the glazing 100 has two bending curvatures that satisfy the features described below in this embodiment.
[0056] As is well known, a glass sheet may be bent along one or more directions, and each of these directions is associated with a single bending curvature (i.e., radius of curvature). From each bending curvature, the bending depth between the surface arc (i.e., the arc tracing the surface of the glass sheet) and the chord supporting the arc can be defined. Thus, since these features are applied similarly to each glass sheet entering into the composition of the laminated glazing, it is possible to refer to the bending curvature of the laminated glazing as a whole.
[0057] Figure 2 schematically shows the two bending curvatures of the asymmetric laminated glazing 100 in Figure 1.
[0058] As illustrated in Figure 2, the glazing 100 has a first bending curvature (corresponding to the most pronounced bending in this example) which is tied to the bending depth of the longest arc ARC_F tracing the surface of the glazing 100. This bending depth of the first bending curvature is also called "deflection F" and more specifically corresponds to the section whose endpoints are the midpoint of the arc ARC_F and the midpoint of the chord C_F supporting the arc ARC_F.
[0059] In this embodiment, the glazing 100 also has a second curvature in a direction essentially perpendicular to the first curvature. This second bending curvature, also called a double bend (or "cross-bending" or "cross-curvature" in English literature), is generally less pronounced than the first bending curvature. Furthermore, this second bending curvature is associated with the bending depth of arc ARC_DB, which is essentially perpendicular to the longest arc ARC_F. The bending depth of this second bending curvature is also called the "double bend DB," and more specifically, corresponds to a section whose endpoints are the midpoint of arc ARC_DB and the midpoint of chord C_DB supporting arc ARC_DB.
[0060] As a result of these arrangements, the asymmetrical stacked glazing 100 can be associated with the following: - The first bending ratio R_F between the length of the chord C_F and the bending depth F (i.e., R_F = C_F / F); - A second bending ratio R_DB between the length of the chord C_DB and the bending depth DB (i.e., R_DB = C_DB / DB).
[0061] As described above, the asymmetric laminated glazing 100 has a substantially planar geometry within the limits that advantageously allow for excellent robustness while avoiding the need to perform strengthening treatment on the second glass sheet 120. Specifically, in this embodiment, the glazing 100 is molded such that the flattening coefficient COEF_FLAT, which is equal to the sum of the first bending ratio R_F and the second bending ratio R_DB, is greater than 250.
[0062] Figure 3 is a table illustrating the surface stress values measured in the second glass sheet 120.
[0063] In particular, to obtain the values shown in the table in Figure 3, we considered an asymmetrical laminated glazing 100 in which the thickness of the first glass sheet 110 was equal to 2.1 mm and the thickness of the second glass sheet 120 was equal to 1.1 mm. The intermediate layer 130 is a PVB layer with a thickness of equal to 0.76 mm.
[0064] In the table in Figure 3, the values of parameters C_F, F, R_F, C_DB, DB, and R_DB are expressed in millimeters. The first column, referenced with "%", corresponds to the ratio of the flattening of glazing 100 to the standard configuration of the same glazing 100 (where flattening means a reduction in bending depth F and DB). The standard configuration corresponds to a geometry that would typically be required with respect to curvature under the current technical conditions (i.e., when chemical treatment of the second glass sheet 120 is permitted), and is associated with F and DB values equal to 8.39 mm and 19.45 mm, respectively. This standard configuration is indicated in the 0% row in the table. Therefore, as an example, for the row corresponding to a 20% flattening ratio, F = 8.39 × (1 - 20%) = 6.71 mm.
[0065] Furthermore, in the table in Figure 3, the column labeled "CO_F4" contains the surface stress values measured on surface 4 of the glazing 100 (i.e., the surface of the second glass sheet 120 facing inward into the vehicle). These values are expressed in MPa units and are all negative, considering the selected measurement criterion and the fact that these are surface compressive stresses (positive stresses with the same value may be measured symmetrically on surface 3, and these positive stresses therefore correspond to tensile surface stresses).
[0066] Conventionally, these surface stresses correspond to mechanical residual stresses resulting from the assembly of the asymmetric laminated glazing 100. In particular, these residual stresses are a result of the thermal bending and thermal strengthening of the first glass sheet 110, as well as the cold bending of the second glass sheet 120. With respect to the second glass sheet 120, the surface stresses are essentially localized around the periphery, typically at the larger edges.
[0067] Within the scope of this application, surface stress is measured by instruments that operate on the principle of polarization, such as the Scalp-04 polarizer, which is commercially available from Glasstress Ltd. at Tallinn 10912, Estonia.
[0068] Furthermore, as can be seen in the table in Figure 3, the flattening coefficient COEFF_FLAT is greater than 250 for flattening ratios of 40%, 60%, and 80%. This corresponds, in particular, to a surface stress (in absolute value) of less than 20 MPa, which, as the inventors have considered, corresponds to a stress level that can very strongly limit the risk of breakage of the second glass sheet 120.
[0069] In other words, by proposing a geometry that is even flatter than the current technical geometry (COEFF_FLAT>250), it is possible to obtain an extremely robust asymmetric laminated glazing 100 that does not require strengthening treatment of the second glass sheet 120.
[0070] The inventors were further able to measure that the asymmetric laminated glazing 100 considered in the embodiment of Figure 3 has a surface stress level of over 40 MPa or over 80 MPa in the first glass sheet 110, depending on whether the first glass sheet 110 has undergone semi-strengthening or thermal strengthening. Such stress levels in the first glass sheet 110 support the conclusion that the glazing 100 thus obtained has excellent robustness.
[0071] Up to this point, we have described the asymmetric laminated glazing 100 assuming that the flattening coefficient COEFF_FLAT is at least greater than 250. However, in more specific embodiments, it is not at all ruled out to assume stricter constraints regarding flattening, such as a flattening coefficient COEFF_FLAT of at least greater than 500.
[0072] Furthermore, the asymmetric laminated glazing 100 has also been described assuming that the flattening coefficient COEFF_FLAT corresponds to the sum of the first bending ratio R_F and the second bending ratio R_DB. This method is merely a variation of the present invention and does not preclude the flattening coefficient COEFF_FLAT from being equal to only one of the two bending ratios R_F and R_DB.
[0073] The present invention also relates to a method for manufacturing the asymmetric laminated glazing 100 shown in Figure 1. The method is carried out using a molding apparatus that satisfies properties known to those skilled in the art. Thus, the molding apparatus typically includes a glass sheet heating apparatus (e.g., a furnace), a glass sheet hot bending apparatus, a glass sheet cold bending apparatus, and a glass sheet heat strengthening apparatus. The steps of the manufacturing method are illustrated in Figure 4 according to a particular embodiment.
[0074] As illustrated in Figure 4, the manufacturing method begins with step H10, which involves obtaining a first glass sheet 110 and a second glass sheet 120 in a planar state. Typically, the first and second glass sheets 110 and 120 are cut from a strip of float glass. The first and second glass sheets 110 and 120 can have the same contour before bending. Furthermore, these glass sheets can be processed at their edges after cutting.
[0075] Generally, the term "obtain" can mean either having completed all or some of the intermediate steps (cutting, processing, etc.) in the production of a flat glass sheet, or simply possessing a glass sheet that has already undergone all of the aforementioned production operations.
[0076] Once the first glass sheet 110 is obtained in a planar state, this glass sheet is subjected to heat bending during step H20 of the manufacturing method. The heat bending is carried out according to the flattening coefficient COEFF_FLAT, that is, once bent, the first glass sheet 110 has a flattening coefficient of at least 250 and more than 500 as described above.
[0077] Therefore, the bending of the first glass sheet 110 determines the bending of the asymmetric laminated glazing 100 once completed. Suitable bending methods for the glass sheet are, for example, a "continuous movement between two roller beds" type (as described in International Publication No. 2005 / 047198 or International Publication No. 2004 / 033381) or a "press bending" type (as described in International Publication No. 02 / 06170 or International Publication No. 2017 / 178733).
[0078] The first glass sheet 110 is then heat-strengthened (strengthened or semi-strengthened) during step H30 of the manufacturing method.
[0079] In this case, the manufacturing method includes an assembly step H40 of the first and second glass sheets 110, 120 onto the laminated glazing 100, where an intermediate layer 130 is placed between the first and second glass sheets 110, 120. The assembly includes, in particular, a cold bending of the second glass sheet 120 relative to the first glass sheet 110.
[0080] In practice, the assembly of the asymmetric laminated glazing 100 using the first and second glass sheets 110, 120 and the intermediate layer 130 can be carried out according to any method known to those skilled in the art. In general principle, this assembly includes a pre-assembly in which the intermediate layer 130 is deposited onto one of the surfaces of the first glass sheet 110 or the second glass sheet 120. More specifically, if the intermediate layer 130 is made of PVB or EVA, it is typically deposited onto surface 2 of the first glass sheet 110. In contrast, if the intermediate layer 130 contains OCA material, in particular liquid OCA material, it is deposited onto surface 3 of the second glass sheet 120. A suitable apparatus is then pressed against surface 4 of the second glass sheet 120, for example at the central zone level of the second glass sheet 120, thus cold-deforming it and bonding it to the first glass sheet 110. It is appropriate to note that when OCA materials, particularly liquid OCA materials, are used, assembly step H40 may also include drying of the stack formed by the sheets 110, 120 and the intermediate layer 130.
[0081] In a more specific embodiment, assembly step H40 may also include a step of maintaining the stack formed by the first and second glass sheets 110, 120 and the intermediate layer 130 in place after the cold bending of the second glass sheet 120. Such position maintenance is advantageous in that it is possible to stabilize the stack and thus minimize the risk of alignment defects between the first glass sheet 110 and the second glass sheet 120. Such maintenance can be achieved by any method known to those skilled in the art, such as using clamps or by creating hot spots between the glass sheets 110, 120.
[0082] In the embodiment described with reference to Figure 4, the manufacturing method also includes a step H50 for extracting air contained within the assembled asymmetric laminated glazing 100. This air extraction or "degassing" step H50 is performed simultaneously with the drying of the assembled asymmetric laminated glazing 100, for example, when the intermediate layer 130 contains OCA material, particularly liquid OCA material.
[0083] The air extraction step H50 is carried out, for example, by calendering the assembled asymmetrical laminated glazing 100.
[0084] However, attempting to calender the assembled asymmetrical laminated glazing 100 constitutes only one variation of the implementation of the present invention. Generally, any air extraction method known to those skilled in the art can be attempted, such as vacuuming (for example, by sealing the assembled glazing 100 in a bag in which a vacuum is achieved).
[0085] It should be noted that if the asymmetrical laminated glazing 100 includes a PVB intermediate layer, particularly acoustic PVB, the manufacturing method may also include an autoclave step (not shown in Figure 4) of the assembled glazing 100 after the assembly step H40. [Explanation of symbols]
[0086] 100 glazing 110 First glass sheet 120 Second glass sheet 130 Middle Class
Claims
1. Laminated glazing (100) comprising first and second glass sheets assembled by an intermediate layer (130), wherein the first glass sheet (110) is heat-strengthened and has a thickness greater than 1.8 mm, and the second glass sheet (120) is not strengthened and has a thickness less than 1.6 mm, the glazing has at least one first bending curvature (curve) that defines a bending depth (F, DB) between a surface arc (ARC_F, ARC_DB) and a chord (C_F, C_DB) supporting the arc, and is associated with a first bending ratio (R_F, R_DB) between the length of the chord and the bending depth, the glazing is further molded such that the flattening coefficient (COEFF_FLAT) is greater than 250 and is at least equivalent to the first bending ratio, the laminated glazing (100).
2. The glazing (100) according to claim 1, wherein the glazing has a second curvature in a direction substantially perpendicular to the first curvature so as to be linked to a second bending ratio (R_F, R_DB), and the flattening coefficient (COEFF_FLAT) is equal to the sum of the first bending ratio and the second bending ratio.
3. The glazing (100) according to claim 1 or 2, wherein the flattening coefficient (COEFF_FLAT) is greater than 500.
4. The glazing (100) according to any one of claims 1 to 3, wherein the thickness of the second glass sheet (120) is less than 1.2 mm, for example, less than 1 mm.
5. The glazing (100) according to any one of claims 1 to 4, wherein the thickness of the first glass sheet (110) is greater than 2.1 mm, or greater than 2.6 mm, or greater than 2.85 mm, or greater than 3.15 mm, or greater than 3.5 mm, or greater than 3.85 mm.
6. The glazing (100) according to any one of claims 1 to 5, wherein the intermediate layer (130) comprises a polymer material including a polyvinyl butyral layer having a loss factor tan(δ) greater than 0.8 and a shear modulus G' of less than 20 MPa at a temperature of 20°C and a frequency of 500 Hz to 5000 Hz.
7. The glazing (100) according to any one of claims 1 to 6, wherein the intermediate layer (130) includes a transparent adhesive material of the "OCA" type, such as a latex adhesive.
8. The glazing (100) according to any one of claims 1 to 5, wherein the intermediate layer (130) is made of ethylene vinyl acetate.
9. Use of the glazing (100) according to any one of claims 1 to 8 as glazing for windows of a house or a means of transport by land, air, sea or rail, preferably an automatic vehicle, and more particularly as glazing for a windshield, rear glazing, side glazing or roof glazing.
10. An automatic vehicle comprising glazing (100) according to any one of claims 1 to 8.
11. In a method for manufacturing glazing (100) according to any one of claims 1 to 8, - Step (H10) to obtain a first glass sheet (110) in a flat state and a second glass sheet (120) in a flat state, - A first heat bending step (H20) of the glass sheet according to the flattening coefficient (CEOFF_FLAT), - The first step of heat strengthening the glass sheet (H30), - An assembly step (H40) of a first glass sheet and a second glass sheet into a single laminated glazing, wherein an intermediate layer (130) is placed between the first glass sheet and the second glass sheet, and the assembly includes cold bending of the second glass sheet relative to the first glass sheet. - Step (H50) of extracting air contained within the assembled laminated glazing, A method that includes this.
12. The method according to claim 11, wherein the air extraction step is carried out by calendering of laminated glazing.
13. The method according to claim 11 or 12, wherein the laminated glazing to be manufactured conforms to claim 6 or 7, and the method further comprises an autoclave step of the assembled laminated glazing after the air extraction step.