Lithium-ion rechargeable battery
The lithium secondary battery with lithium iron phosphorus oxide and controlled electrolyte additives addresses the limitations of high-nickel materials by enhancing electrolyte impregnation and charge transfer, maintaining high-temperature stability and cycle capacity.
Patent Information
- Application Number
- JP2026530499
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2024-11-19
- Filing Date
- 2024-11-20
- Publication Date
- 2026-11-19
AI Technical Summary
High-nickel-content positive electrode active materials in lithium-ion batteries suffer from limited SOC range, structural instability, and reduced electrolyte impregnation due to high-loading electrodes, leading to decreased battery performance and capacity.
A lithium secondary battery design using lithium iron phosphorus oxide with controlled electrolyte additives, including lithium nitrate, cyclic lactone, and carbonate-based solvents, to enhance electrolyte impregnation and charge transfer, forming a stable film on the electrode surface.
Improves electrolyte impregnation and charge transfer, maintaining high-temperature stability and cycle capacity retention, ensuring excellent battery performance.
Smart Images

Figure 2026539116000001_ABST
Abstract
Description
[Technical Field]
[0001] This application claims priority rights under Korean Patent Application No. 10-2023-0189753 dated December 22, 2023, and Korean Patent Application No. 10-2024-0165719 dated November 19, 2024, and all content disclosed in the documents of said Korean Patent Applications is incorporated herein by reference.
[0002] The present invention relates to a lithium secondary battery, and more particularly to a lithium secondary battery with improved high-temperature cycle characteristics. [Background technology]
[0003] In recent years, the application areas of lithium-ion batteries have expanded beyond power supply for electronic devices such as electrical, electronic, telecommunications, and computers to include power storage and supply for large-area equipment such as automobiles and power storage devices. fart The market is expanding rapidly, and consequently, there is a growing demand for high-capacity, high-output, and highly stable secondary batteries.
[0004] In particular, for lithium-ion batteries to be used as a power source for electric vehicles, it is necessary to stably produce high output at high temperatures and high voltages. To this end, the use of negative electrode active materials such as lithium metal, carbon compounds, and silicon compounds, and positive electrode active materials with high nickel content and high energy density is being considered.
[0005] However, the aforementioned high-nickel-content positive electrode active material has the disadvantage of severely limiting the usable SOC range because its output drops sharply in the low SOC range (e.g., SOC 30% or less). Therefore, it has limitations in its application to fields where output characteristics are particularly important, such as electric vehicles. Furthermore, because the aforementioned high-nickel-content positive electrode active material has low stability, when driving lithium secondary batteries under high voltage or high temperature conditions, structural instability can cause structural deformation as charging and discharging progresses, or side reactions with the electrolyte can degrade the coating formed on the surface of the positive and / or negative electrode, or the structure of the electrode surface, potentially leading to the elution of transition metal ions from the positive electrode surface. In this way, the eluted transition metal ions electrodeposit onto the negative electrode, reducing the passivation ability of the SEI, resulting in the deterioration of the negative electrode.
[0006] recent years To address these problems, a method using lithium iron phosphate oxide with an olivine structure, which offers superior high-temperature safety, as a replacement for nickel-high-content cathode active material is attracting attention.
[0007] However, the aforementioned lithium iron phosphorus oxide has been conventionally from Because its theoretical capacity is lower compared to the nickel-high-content cathode active material that was previously used, it has the disadvantage of having a relatively lower energy density when designing electrodes under the same conditions.
[0008] Therefore, in order to solve these problems, in recent years, high-loading electrodes have been tested that increase the amount of electrode active material coated per unit area (loading amount) when using lithium iron phosphate.
[0009] However, such high-loading electrodes have a drawback: not only is the degree of active material coating high, but the design also increases the electrode density, resulting in a very high degree of electrode compression. This leads to insufficient porous structure inside the electrode, reducing electrolyte impregnation. When electrolyte impregnation decreases in this way, "charge transfer," which is the reaction between lithium ions and electrons, decreases, which manifests as an increase in battery resistance and affects the battery capacity characteristics. decline There is a risk that this may happen.
[0010] Therefore, there is a need to develop a new type of secondary battery that can improve electrolyte impregnation and charge transfer during the manufacturing of secondary batteries using high-loading electrodes. [Overview of the Initiative] [Problems that the invention aims to solve]
[0011] The present invention aims to solve the above-mentioned problems and provides a lithium secondary battery that, when applying a high-loading positive electrode, improves electrolyte impregnation by using an electrolyte in which the content range of a specific electrolyte additive is controlled according to the loading amount of the positive electrode, and also increases the charge transfer phenomenon by forming a stable film on the electrode surface, thereby suppressing the increase in resistance during high-temperature storage and ensuring an excellent cycle capacity retention rate. [Means for solving the problem]
[0012] [1] The present invention provides a lithium secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, wherein the positive electrode comprises lithium iron phosphorus oxide as a positive electrode active material, the electrolyte comprises a lithium salt, a first organic solvent, a second organic solvent, and an additive, the first organic solvent being a cyclic lactone compound, the second organic solvent being a carbonate-based organic solvent, and the additive being lithium nitrate (LiNO3), satisfying the following formula 1.
[0013] [Formula 1]
number
[0014] In the above formula 1, A is the total amount (g) of electrolyte injected into the lithium secondary battery. B is the content (by weight) of lithium nitrate (LiNO3) contained in the injected electrolyte. C is the loading amount of the positive electrode (g / cm³). 2 ) and D is the total surface area (cm²) of the positive electrode current collector. 2 )
[0015] [2] The present invention provides the lithium secondary battery described in [1] above, wherein the lithium iron phosphorus oxide comprises a compound represented by the following chemical formula 1.
[0016] [Chemical formula 1] Li 1+a Fe x M y (PO 4-b )X' b
[0017] In the above chemical formula 1, M is one selected from the group consisting of Al, Mg, Ni, Co, Mn, Ti, Ga, Cu, V, Nb, Zr, Ce, In, Zn, and Y, and X' is one or more elements selected from the group consisting of F, S, and N, where -0.5 ≤ a ≤ 0.5, 0 <x≦1、0≦y≦1、および0≦b≦0.3である。
[0018] [3] The present invention provides a lithium secondary battery according to [1] or [2], wherein the lithium iron phosphate is lithium iron phosphate (LiFePO4) or lithium manganese iron phosphate (LiFeMnPO4).
[0019] [4] The present invention provides a lithium secondary battery according to any one of [1] to [3] above, wherein the cyclic lactone compound comprises gammabutyrolactone.
[0020] [5] The present invention provides the lithium secondary battery according to any one of the above [1] to [4], wherein the carbonate-based organic solvent is a cyclic carbonate-based organic solvent.
[0021] [6] The present invention provides the lithium secondary battery according to any one of the above [1] to [5], wherein the first organic solvent and the second organic solvent are contained at a volume ratio of 50:50 to 99:1.
[0022] [7] The present invention provides the lithium secondary battery according to any one of the above [1] to [6], wherein in the above Formula 1, A is 3.0 g to 8.5 g.
[0023] [8] The present invention provides the lithium secondary battery according to any one of the above [1] to [7], wherein in the above Formula 1, C is 0.032 g / cm 2 ~0.064 g / cm 2 .
[0024] [9] The present invention provides the lithium secondary battery according to any one of the above [1] to [8], wherein in the above Formula 1, D is 310 cm 2 ~450 cm 2 .
[0025]
[10] The present invention provides the lithium secondary battery according to any one of the above [1] to [9], wherein the negative electrode comprises a carbon-based active material, a silicon-based active material, or a mixture of a carbon-based active material and a silicon-based active material.
[0026]
[11] The present invention provides the lithium secondary battery according to any one of the above [1] to
[10] , wherein the capacity of the lithium secondary battery is 1,000 mAh to 3,000 mAh. Effects of the Invention
[0027] The lithium secondary battery according to the present invention comprises an organic solvent containing a cyclic lactone compound as a main solvent, and lithium nitrate (LiNO3) whose content range is controlled according to the loading amount of the positive electrode as an additive andBy applying an electrolyte containing [the specified element], the impregnation of the electrolyte into the high-loading positive electrode can be improved, and by forming a low-resistance coating on the surface of the high-loading positive electrode, the charge transfer on the surface of the high-loading positive electrode can be improved. Therefore, the lithium secondary battery of the present invention in This relates to cycle characteristics and storage characteristics at high temperatures. of improvement Let It is possible. [Modes for carrying out the invention]
[0028] The terms and words used herein and in the claims are used solely to illustrate exemplary embodiments. General It should not be interpreted in a way that is limited to its literal or dictionary meaning, and the inventors is To explain my invention in the best possible way Use It is possible to appropriately define the concept of a word. 、 In accordance with this principle, it should be interpreted in a way that is consistent with the technical concept of the present invention.
[0029] In this specification, terms such as “includes,” “equip,” or “have” are intended to specify the presence of implemented features, figures, steps, components, or combinations thereof, and should be understood not to preemptively exclude the presence or possibility of adding one or more other features, figures, steps, components, or combinations thereof.
[0030] Furthermore, in this specification, when "a to b carbon atoms" is mentioned, "a" and "b" refer to the number of carbon atoms contained in a specific functional group. That is, the functional group may contain "a" to "b" carbon atoms. For example, "alkylene group with 1 to 5 carbon atoms" means an alkylene group containing 1 to 5 carbon atoms, i.e., -CH2-, -CH2CH2-, -CH2CH2CH2-, -CH2(CH3)CH-, -CH2CH2CH2CH2CH2-, and -CH(CH3)CH2CH2-, etc.
[0031] Furthermore, in this specification, the term "alkylene group" means a branched or unbranched aliphatic hydrocarbon group, or a functional group in which one hydrogen atom has been removed from each of the carbon atoms at both ends of the aliphatic hydrocarbon group. In one embodiment, the alkylene group may be substituted or unsubstituted. The alkylene group includes, but is not limited to, a methylene group, an ethylene group, a propylene group, an isopropylene group, a butylene group, an isobutylene group, a tert-butylene group, a pentylene group, a 3-pentylene group, and each of these may be selectively substituted in other embodiments.
[0032] Furthermore, in this specification, "substitution" means, unless otherwise defined, that at least one hydrogen atom bonded to a carbon atom is substituted with another element, such as fluorine.
[0033] Furthermore, in this specification, "loading amount" means the amount of active material per unit area of the positive electrode active material layer containing lithium iron phosphate formed on the current collector, and is expressed as "g / cm²". 2 This shall be written as "[positive electrode loading amount]". In this specification, "positive electrode loading amount" means the sum of the loading amounts on both sides of the positive electrode.
[0034] The present invention will be described in detail below.
[0035] The lithium secondary battery according to the present invention includes at least one of the configurations disclosed below, and may include any combination of technically possible configurations from the following configurations.
[0036] Lithium-ion rechargeable battery This invention relates to a lithium secondary battery.
[0037] Specifically, the present invention provides a lithium secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte.
[0038] The positive electrode may contain lithium iron phosphorus oxide as the positive electrode active material.
[0039] The electrolyte may include a lithium salt, a first organic solvent, a second organic solvent, and an additive.
[0040] The first organic solvent may contain a cyclic lactone compound.
[0041] The second organic solvent may include a carbonate-based organic solvent.
[0042] The aforementioned additive is lithium nitrate (LiNO3), which can satisfy the following formula 1.
[0043] [Formula 1]
number
[0044] In the above formula 1, A is the total amount (g) of electrolyte injected into the lithium secondary battery. B is the content (by weight) of lithium nitrate (LiNO3) contained in the injected electrolyte. C is the loading amount of the positive electrode (g / cm³). 2 ) and D is the total surface area (cm²) of the positive electrode current collector. 2 )
[0045] The following describes in detail each component of the lithium secondary battery of the present invention.
[0046] (1) Positive electrode The positive electrode of the present invention may contain lithium iron phosphorus oxide as the positive electrode active material, and the lithium iron phosphorus oxide may be represented by the following chemical formula 1.
[0047] [Chemical formula 1] Li 1+a Fe x M y (PO 4-b )X' b
[0048] In the above chemical formula 1, M is one selected from the group consisting of Al, Mg, Ni, Co, Mn, Ti, Ga, Cu, V, Nb, Zr, Ce, In, Zn, and Y. X' is one or more elements selected from the group consisting of F, S, and N. -0.5 ≤ a ≤ 0.5, 0 <x≦1、0≦y≦1、および0≦b≦0.3である。
[0049] The lithium iron phosphorus oxide represented by chemical formula 1 may include, as a representative example, lithium iron phosphorus oxide (LiFePO4, LFP) or lithium manganese iron phosphorus oxide (LiFeMnPO4, LFMP).
[0050] The lithium iron phosphate oxide represented by chemical formula 1 may use nanometer-sized primary particles for high lithium ion input and output, and these primary particles can also be granulated and used as secondary particles which are aggregates of these primary particles. For example, when primary particles are used as the lithium iron phosphate oxide, the particle size is 50 nm ~2000nm, more specifically 200 nm The particle size may be ~1100 nm. Furthermore, when these primary particles are granulated and used as secondary particles which are aggregates of these primary particles, the average particle size (D50) of the secondary particles may be 0.5 μm to 30 μm.
[0051] The lithium iron phosphate represented by chemical formula 1 has a strong covalent bond between phosphorus and oxygen within the tetrahedral structure of PO4, thus ensuring structural and thermal stability even with respect to volume changes due to charging and discharging. Furthermore, the lithium iron phosphate represented by chemical formula 1 may be coated with an amorphous layer of carbon or metal oxide on its surface. In this case, since the amorphous layer of carbon or metal oxide coated on the surface is not crystalline, intercalation and deintercalation of lithium ions occurs in the lithium iron phosphate core through the amorphous layer of the shell. The amorphous layer of carbon or metal oxide coated on the surface allows lithium ions to pass through while also exhibiting excellent electronic conductivity. living things Because it can also serve as a conduction path to the lithium iron phosphate core, it enables high-rate charging and discharging. Furthermore, when the surface of the lithium iron phosphate is coated with an amorphous layer of carbon or metal oxide, unwanted reactions between the core material and the electrolyte can be controlled, thus ensuring safety. of moreover improve It is possible.
[0052] On the other hand, in this invention, in order to design the electrode for high capacitance, the loading amount of the positive electrode is 0.032 g / cm³. 2 (Loading amount of single-sided reference positive electrode: 0.016 g / cm²) 2 The above is acceptable, specifically 0.032 g / cm³. 2 ~0.064 g / cm³ 2 It may be, and more preferably, 0.040 g / cm³. 2 ~0.060 g / cm³ 2 This may be the case. If the loading amount of the positive electrode active material satisfies the above range, a high-energy-density battery can be designed.
[0053] The positive electrode of the present invention may include a positive electrode current collector and a positive electrode composite layer disposed on at least one side of the positive electrode current collector. In this case, the positive electrode composite layer may contain the lithium iron phosphorus oxide described above as the positive electrode active material.
[0054] The thickness of the positive electrode current collector is typically 3 μm It can be ~500 μm.
[0055] The positive electrode current collector may have fine irregularities formed on its surface to strengthen the bonding force of the positive electrode active material. For example, the positive electrode current collector can be used in various forms such as film, sheet, foil, mesh, porous material, foam, or nonwoven fabric.
[0056] The positive electrode composite layer is disposed on at least one side of the positive electrode current collector. Specifically, the positive electrode composite layer may be disposed on one or both sides of the positive electrode current collector.
[0057] Furthermore, the lithium iron phosphorus oxide represented by chemical formula 1 may be included in the positive electrode composite layer in an amount of 80% to 99% by weight, taking into consideration factors such as sufficient capacity.
[0058] Furthermore, the porosity of the positive electrode composite layer measured by the BET method may be 20% to 40%, specifically 20% to 30%.
[0059] When the porosity of the positive electrode composite layer satisfies the above range, the density of the electrode is ensured, the interfacial resistance of the positive electrode is reduced, and the output characteristics of the battery are improved. It is possible .
[0060] On the other hand, the positive electrode composite layer may further contain a binder and / or a conductive material along with the positive electrode active material.
[0061] The binder plays a role in improving the adhesion between positive electrode active material particles and the adhesion between the positive electrode active material and the current collector. Examples of such binders include fluororesin-based binders such as polyvinylidene fluoride (PVDF); rubber-based binders including styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimidazole-based binders; polyester-based binders; and silane-based binders. One of these may be used alone or in mixtures of two or more.
[0062] The binder is present in the positive electrode composite layer at a concentration of 0.1 weight% ~15% by weight, preferably 0.1 weight% It may be included in an amount of ~10% by weight.
[0063] Next, the conductive material is used to impart conductivity to the electrodes and can be used in the battery without any particular limitations as long as it does not cause a chemical change and has electronic conductivity. Specific examples of the conductive material include carbon black such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystalline structure; conductive fibers such as carbon fibers or metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives.
[0064] The conductive material is contained in the positive electrode composite layer. weight% It may be added at a concentration of approximately 30% by weight.
[0065] The positive electrode is manufactured by coating the positive electrode current collector with a positive electrode slurry containing a positive electrode active material and selectively a binder, conductive material, and solvent for forming the positive electrode slurry, followed by drying and rolling. do Alternatively, a positive electrode can be manufactured by mixing a positive electrode active material with a binder, conductive material, etc., to produce a film, and then laminating it onto a positive electrode current collector.
[0066] The porosity of the cathode composite layer measured by the BET method after rolling may be 20% to 40%, and more specifically, 20% to 30%.
[0067] The solvent for forming the positive electrode slurry may include, for example, at least one selected from the group consisting of distilled water, N-methylpyrrolidone, ethanol, methanol, and isopropyl alcohol, preferably N-methylpyrrolidone, in order to facilitate the dispersion of the positive electrode active material, binder, and / or conductive material.
[0068] (2) Negative electrode Next, I will explain the negative electrode.
[0069] The negative electrode may include a negative electrode active material.
[0070] As the negative electrode active material, a carbon-based active material, a silicon-based active material, or a mixture of a carbon-based active material and a silicon-based active material may be used.
[0071] As the carbon-based active material, various carbon-based active materials used in the art, for example, graphite-based materials such as natural graphite, artificial graphite, and Kish graphite; pyrolytic carbon, mesophase pitch based carbon fiber, meso-carbon microbeads, mesophase pitches, and petroleum or High-temperature calcined carbon such as petroleum or coal tar pitch derived cokes, soft carbon, hard carbon and the like can be used. The shape of the carbon-based active material is not particularly limited, and materials in various shapes such as amorphous, plate-like, scaly, spherical, or fibrous can be used.
[0072] Specifically, as the carbon-based active material, either one of natural graphite or artificial graphite can be used, and both natural graphite and artificial graphite may be used in order to enhance the adhesive force with the current collector and suppress detachment of the active material.
[0073] In addition, the silicon-based active material is, for example, metal silicon (Si), silicon oxide (SiO x , where 0<x<2), silicon carbide (SiC), and Si-Y alloy (where Y is an alkali metal, alkaline earth kindThe element Y may include one or more elements selected from the group consisting of metals, group 13 elements, group 14 elements, transition metals, rare earth elements, and combinations thereof, but not Si. The element Y may include Mg, Ca, Sr, Ba, Ra, Sc, Y, Ti, Zr, Hf, Rf, V, Nb, Ta, Db ( Dubnium dubnium ) ), Cr, Mo, W, Sg, Tc, Re, Bh, Fe, Pb, Ru, Os, Hs, Rh, Ir, Pd, Pt, Cu, Ag, Au, Zn, Cd, B, Al, Ga, Sn, In, Ti, Ge, P, As, Sb, Bi, S, Se, Te, Po, and combinations thereof may be selected from the group.
[0074] The average particle size (D) of the silicon-based active material 50 The thickness of the ) may be 1 μm to 30 μm, preferably 2 μm to 15 μm, in order to ensure structural stability during charging and discharging and to reduce side reactions with the electrolyte.
[0075] Furthermore, the negative electrode of the present invention may contain at least one selected from the carbon-based active material and the silicon-based active material.
[0076] Specifically, the negative electrode of the present invention may contain the carbon-based active material and the silicon-based active material.
[0077] In this case, the weight ratio of the silicon-based active material to the carbon-based active material may be 1:99 to 30:70, specifically 3:97 to 15:85. When the mixing ratio of the silicon-based active material to the carbon-based active material satisfies the above range, the capacity characteristics are improved, the volume expansion of the silicon-based active material is suppressed, and excellent cycle performance can be ensured.
[0078] The negative electrode may include a negative electrode current collector and a negative electrode composite layer disposed on at least one side of the negative electrode current collector. In this case, the negative electrode active material may be included in the negative electrode composite layer.
[0079] The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. Specifically, the negative electrode current collector can be made of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, or the surface of copper or stainless steel. charcoal Materials such as aluminum, nickel, titanium, silver, or aluminum-cadmium alloys may be used, as they may have been surface-treated.
[0080] The aforementioned negative electrode current collector is typically 3 μm It has a thickness of approximately 500 μm.
[0081] The negative electrode current collector may have its surface textured to enhance the bonding force of the negative electrode active material. For example, the negative electrode current collector can be used in various forms such as film, sheet, foil, mesh, porous material, foam, or nonwoven fabric.
[0082] The negative electrode composite layer is disposed on at least one side of the negative electrode current collector. Specifically, the negative electrode composite layer may be disposed on one or both sides of the negative electrode current collector.
[0083] The negative electrode active material may be included in the negative electrode composite layer in an amount of 60% to 99% by weight, in order to minimize the effect of volume expansion / contraction on the battery and to achieve sufficient capacity in a secondary battery.
[0084] Furthermore, the porosity of the negative electrode composite layer measured by the BET method may be 20% to 40%, specifically 20% to 30%.
[0085] When the porosity of the negative electrode composite layer satisfies the above range, the interfacial resistance of the negative electrode becomes lower, and the output characteristics of the battery can be improved.
[0086] On the other hand, the negative electrode composite layer may further contain a conductive material and / or a binder together with the negative electrode active material.
[0087] The conductive material is a component for further improving the conductivity of the negative electrode active material and is not particularly limited as long as it does not cause a chemical change in the battery and is conductive. Examples include carbon black such as carbon black, acetylene black, Ketjen black, channel black, furnace black, lamp black, or thermal black; graphite powder such as natural graphite, artificial graphite, or graphite with a highly developed crystalline structure; conductive fibers such as carbon fibers or metal fibers; conductive powders such as carbon fluoride powder, aluminum powder, and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and conductive materials such as polyphenylene derivatives.
[0088] The conductive material is present in the negative electrode composite layer in an amount of 10% by weight or less, preferably 5% by weight or less. in It may be added.
[0089] The aforementioned binder is a component that assists in bonding between the conductive material, the active material, and the current collector, and typically includes fluororesin-based binders such as polyvinylidene fluoride (PVDF); rubber-based binders including styrene-butadiene rubber (SBR), acrylonitrile-butadiene rubber, and styrene-isoprene rubber; cellulose-based binders including carboxyl methyl cellulose (CMC), starch, hydroxypropyl cellulose, and regenerated cellulose; polyalcohol-based binders including polyvinyl alcohol; polyolefin-based binders including polyethylene and polypropylene; polyimidazole-based binders; polyester-based binders; and silane-based binders.
[0090] The binder is present in the negative electrode composite layer at a concentration of 0.1 weight% ~15% by weight, preferably 0.1 weight% It may be included in an amount of ~10% by weight.
[0091] The negative electrode is manufactured by coating the negative electrode current collector with a negative electrode slurry containing a negative electrode active material and selectively a binder, conductive material, and solvent for forming the negative electrode slurry, followed by drying and rolling. do Alternatively, a negative electrode can be manufactured by mixing a negative electrode active material with a binder, conductive material, etc., to produce a film, and then laminating it onto a negative electrode current collector.
[0092] The porosity of the negative electrode composite layer, measured by the BET method after rolling, may be 20% to 40%, and more specifically, 20% to 30%.
[0093] The solvent for forming the negative electrode slurry may include, for example, at least one selected from the group consisting of distilled water, N-methylpyrrolidone, ethanol, methanol, and isopropyl alcohol, preferably distilled water, in order to facilitate the dispersion of the negative electrode active material, binder, and / or conductive material.
[0094] (3) Separator The separator separates the negative electrode and the positive electrode and provides a passage for lithium ions to move. It can be used without particular limitations as long as it is one that is commonly used as a separator in lithium secondary batteries. In particular, it is preferable that it has low resistance to the movement of ions in the non-aqueous electrolyte and has excellent non-aqueous electrolyte moisture retention capacity.
[0095] Specifically, as separators, porous polymer films, such as porous polymer films made from polyolefin polymers like ethylene homopolymer, propylene homopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, or ethylene / methacrylate copolymer, or laminated structures of two or more layers thereof, can be used. Alternatively, ordinary porous nonwoven fabrics, such as nonwoven fabrics made from high-melting-point glass fibers or polyethylene terephthalate fibers, may be used. Furthermore, coated separators containing ceramic components or polymeric substances may be used to ensure heat resistance or mechanical strength, and may be used selectively as single-layer or multi-layer structures.
[0096] (4) Electrolyte Next, the electrolyte of the present invention may include a lithium salt, a first organic solvent, a second organic solvent, and an additive, and specific examples of each component are described below.
[0097] (4-1) Lithium salt First, the lithium salt as This can be used without restriction, including those commonly used in lithium secondary battery electrolytes, for example, Li as the cation. + It includes, as an anion, F - Cl - , Br - , I - , N(CN)2 - BF4 - ClO4 - B 10 Cl 10 - AlCl4 - AlO2 - PF6 - CF3SO3 - CH3CO2 - CF3CO2 - AsF6 - SbF6 - CH3SO3 - , (CF3CF2SO2)2N - , (CF3SO2)2N - , (FSO2)2N - BF2C2O4 - BC4O8 - PF4C2O4 - PF2C4O8 - (CF3)2PF4 - (CF3)3PF3 - (CF3)4PF2 - (CF3)5PF - (CF3)6P - , C4F9SO3 - CF3CF2SO3 - CF3CF2(CF3)2CO - (CF3SO2) 2CH - CF3(CF2)7SO3- , and SCN - One of the following can be selected from the group consisting of these.
[0098] Specifically, the lithium salts are LiCl, LiBr, LiI, LiBF4, LiClO4, and LiB 10 Cl 10 It may contain a single substance or a mixture of two or more substances selected from the group consisting of LiAlCl4, LiAlO2, LiPF6, LiCF3SO3, LiCH3CO2, LiCF3CO2, LiAsF6, LiSbF6, LiCH3SO3, LiN(SO2F)2(Lithium bis(fluorosulfonyl)imide, LiFSI), LiN(SO2CF2CF3)2(lithium bis(pentafluoroethanesulfonyl)imide, LiBETI), and LiN(SO2CF3)2(lithium bis(trifluoromethane sulfonyl)imide, LiTFSI), specifically LiBF4, LiPF6, LiN(SO2F)2(Lithium bis(fluorosulfonyl)imide, LiFSI), LiN(SO2CF2CF3)2(lithium bis(pentafluoroethanesulfonyl)imide, LiBETI), and LiN(SO2CF3)2(lithium It may contain any one selected from the group consisting of bis(trifluoromethane sulfonyl)imide (LiTFSI). In addition to these, lithium salts commonly used as electrolytes for lithium secondary batteries of It can be used without restriction.
[0099] The lithium salt may be changed as appropriate within the range of normal use, but in order to obtain the optimal effect of forming a corrosion-preventive film on the electrode surface, it may be included in the electrolyte at a concentration of 0.8 M to 3.0 M, specifically 1.0 M to 2.0 M, preferably 1.0 M to 1.8 M.
[0100] When the concentration of the lithium salt is within the above range, the viscosity of the electrolyte can be controlled to achieve optimal impregnation, thereby improving the mobility of lithium ions and improving the capacity characteristics and cycle characteristics of the lithium secondary battery.
[0101] (4-2) First Organic Solvent Next, we will explain the first organic solvent.
[0102] The first organic solvent may contain a cyclic lactone compound.
[0103] The cyclic lactone compound is a compound having high dielectric constant and ionic conductivity, and can improve the charge transfer reduction phenomenon that occurs when a high-loading electrode is driven.
[0104] The cyclic lactone compound may include gamma-butyrolactone.
[0105] The first organic solvent may be present in an amount of 39% to 80% by weight based on the total weight of the electrolyte, more specifically in an amount of 48% to 80% by weight, and more preferably in an amount of 52% to 70% by weight.
[0106] When the content of the first organic solvent of the present invention satisfies the above range, the lithium ion transfer characteristics can be improved and the effect of reducing battery resistance can be achieved.
[0107] (4-3) Second Organic Solvent Next, we will explain the second organic solvent.
[0108] The second organic solvent is decomposed by oxidation reactions during the charging and discharging process of the secondary battery. of Minimize do It may contain a carbonate organic solvent to achieve the desired properties in conjunction with additives.
[0109] Specifically, the carbonate organic solvent preferably includes one selected from the group consisting of a cyclic carbonate organic solvent having high ionic conductivity and high dielectric constant, and a linear carbonate organic solvent having low viscosity and low dielectric constant, and may specifically include a cyclic carbonate organic solvent.
[0110] The cyclic carbonate organic solvents include, specifically, any one or two or more organic solvents selected from the group consisting of ethylene carbonate (EC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, vinylene carbonate, and fluoroethylene carbonate (FEC), among which ethylene carbonate is particularly noteworthy for its ability to maintain the passivation capacity of a stable SEI film.
[0111] The linear carbonate-based organic solvents include one or more selected from the group consisting of dimethyl carbonate (dimethyl carbonate, DMC), diethyl carbonate (diethyl carbonate, DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate. Among these, dimethyl carbonate (dimethyl carbonate, DMC) is particularly noteworthy as it has a small molecular size and low viscosity.
[0112] Specifically, the second organic solvent may be ethylene carbonate, propylene carbonate, or a mixture thereof.
[0113] When using a mixture of the cyclic carbonate and the linear carbonate as the second organic solvent, in order to ensure low viscosity characteristics, the cyclic carbonate organic solvent and the linear carbonate organic solvent may be mixed in a volume ratio of approximately 1:99 to 50:50, or in a volume ratio of 20:80 to 40:60.
[0114] The electrolyte of the present invention may further contain a linear ester-based organic solvent as a third organic solvent, if necessary.
[0115] A typical example of the linear ester-based organic solvent is at least one organic solvent selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate, and specifically may include at least one of methyl acetate and ethyl acetate.
[0116] On the other hand, in the electrolyte of the present invention, the first organic solvent and the second organic solvent may be contained in a volume ratio of 50:50 to 99:1, and more specifically, in a volume ratio of 70:30 to 99:1.
[0117] When the mixing ratio of the first organic solvent and the second organic solvent satisfies the above range, the effect of high ion transfer characteristics can be achieved, and battery performance with low resistance characteristics can be ensured. Specifically, when the volume ratio of the first organic solvent is 50 or more, the effect of ion transfer characteristics can be ensured, and when it is 99 or less by volume, a stable film can be formed, improving battery life characteristics.
[0118] (4-4) Additives Furthermore, the electrolyte of the present invention may contain lithium nitrate (LiNO3) as an additive.
[0119] The lithium nitrate (LiNO3) included as an additive can form an inorganic film containing lithium-nitrogen and lithium-oxygen bonds on the surface of the negative electrode during the activation step. This inorganic film increases the surface energy and acts as an ion carrier that enables uniform transfer of lithium ions, thereby improving the electrode impregnation of the electrolyte and inducing a more effective charge transfer reaction.
[0120] Furthermore, the lithium nitrate (LiNO3) included as an additive can form coordination bonds with transition metals eluted from the positive electrode under high-temperature conditions, or with Lewis acids generated by the decomposition products of the lithium salt, thereby suppressing the electrodeposition of transition metal ions onto the negative electrode surface and preventing the loss of reversible lithium, thus improving the degradation of cycle characteristics.
[0121] The content (by weight) of the aforementioned additive, lithium nitrate (LiNO3), varies depending on the loading amount of the positive electrode, and preferably satisfies, for example, the following formula 1.
[0122] [Formula 1]
number
[0123] In the above formula 1, A is the total amount (g) of electrolyte injected into the lithium secondary battery. B is the content (by weight) of lithium nitrate (LiNO3) contained in the injected electrolyte. C is the loading amount of the positive electrode (g / cm³). 2 ) and D is the total surface area (cm²) of the positive electrode current collector. 2 )
[0124] Specifically, in Formula 1, A may be between 3.0g and 8.5g. When A is 3.0g or more, the impregnation of the electrolyte into the electrode assembly can be easily controlled, and when it is 8.5g or less, the amount of gas generated inside the cell during battery operation can be controlled, preventing an increase in electrolyte impregnation and battery thickness.
[0125] Furthermore, in order to design for higher capacitance of the electrodes, in the above formula 1, C is 0.032 g / cm³. 2 ~0.064 g / cm³ 2 That's fine.
[0126] Furthermore, in the above formula 1, D represents the total surface area of both surfaces of the positive electrode current collector coated with the positive electrode active material, and specifically, 310 cm², so that it can be applied to small batteries. 2 ~450cm 2 That's fine.
[0127] On the other hand, the aforementioned 0.02 is a constant, and is an integer value that expresses the percentage of the additive content in the electrolyte as a decimal, which is 0.01. C This value was determined by multiplying the positive electrode loading amount by the integer value 2 in order to convert it to a single-sided loading amount.
[0128] In the electrolyte of the present invention, when the content (weight %) of the additive lithium nitrate (LiNO3) satisfies Formula 1, the impregnation of the electrolyte into the electrode can be increased, and an inorganic film containing lithium-nitrogen and lithium-oxygen bonds can be uniformly formed on the surface of the negative electrode, thereby improving ion transfer characteristics and ensuring excellent battery performance. Specifically, when the value of Formula 1 is 0.0001 or higher, or 0.0005 or higher, preferably 0.001 or higher, a film that can act as an effective ion carrier without acting as a low-level antibody can be uniformly formed, suppressing an increase in battery resistance and preventing a decrease in battery performance, thus preventing a decrease in lifespan performance at low temperatures (below freezing). Furthermore, when the value of Formula 1 is 0.050 or lower, or 0.040 or lower, preferably 0.030 or lower, side reactions can be suppressed and the generation of unwanted activated gases can be prevented, thus preventing a decrease in high-temperature cycling and high-temperature storage characteristics.
[0129] (4-5) Other additives On the other hand, the lithium secondary battery of the present invention may further contain other additives in the electrolyte as needed to prevent the electrolyte from decomposing and causing the anode to collapse in a high-power environment, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and the effect of suppressing battery swelling at high temperatures. When other additives are further contained in the electrolyte of the present invention, the lithium nitrate (LiNO3) may be named the first additive, and the other additives may be named the second additive.
[0130] The aforementioned other additives may include, as representative examples, any one other additive selected from the group consisting of cyclic carbonate compounds, sulfate compounds, sultone compounds, phosphate compounds, borate compounds, nitrile compounds, benzene compounds, amine compounds, silane compounds, and lithium salt compounds.
[0131] Specifically, vinylene carbonate (VC) is an example of the aforementioned cyclic carbonate compound.
[0132] Examples of the sulfate compounds include ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyl trimethylene sulfate (MTMS).
[0133] The sultone compound mentioned above is any one compound selected from the group consisting of 1,3-propanesultone (PS), 1,4-butanesultone, ethensultone, 1,3-propensultone (PRS), 1,4-butensultone, and 1-methyl-1,3-propensultone.
[0134] Examples of the phosphate compound include one or more compounds selected from the group consisting of lithium difluoro(bisoxalato) phosphate, lithium difluorophosphate, tris(trimethylsilyl) phosphate, tris(2,2,2-trifluoroethyl) phosphate, and tris(trifluoroethyl) phosphate.
[0135] Examples of the borate-based compounds include tetraphenylborate and lithium oxalyldifluoroborate.
[0136] The nitrile compound mentioned above is any one compound selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonile, cyclohexanecarbonile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile.
[0137] Examples of the benzene-based compound include fluorobenzene, examples of the amine-based compound include triethanolamine or ethylenediamine, and examples of the silane-based compound include tetravinylsilane.
[0138] The lithium salt compound is a compound different from the lithium salt contained in the electrolyte, such as LiPO2F2, LiODFB, or LiBOB (lithium bisoxalate borate (LiB(C2O4)2)). ) Examples include one or more compounds selected from the group consisting of LiBF4 and LiDFOP.
[0139] The aforementioned other additives may be used in a mixture of two or more types, and may be included in an amount of less than 10% by weight, specifically 0.01% by weight or more and less than 8.0% by weight, based on the total weight of the electrolyte, preferably in an amount of 0.05% to 5.0% by weight.
[0140] Preferably, in the electrolyte of the present invention, the additive lithium nitrate (LiNO3) and other additives may be present in a weight ratio of 1:0.01 to 1:50, 1:0.1 to 1:10, and more preferably 1:0.1 to 1:6.
[0141] When the electrolyte of the present invention contains the above-mentioned additive and other additives within the above-mentioned range, a stable coating can be formed simultaneously on the surfaces of the positive and negative electrodes. Specifically, when the other additives are included in a ratio of 50% by weight or less, a uniform coating can be formed on the surface of the negative electrode, preventing them from acting as low-level antibodies. Furthermore, by suppressing the elution of transition metals and preventing the electrodeposition of metallic substances on the negative electrode, an increase in coating thickness and resistance can be prevented. On the other hand, if the other additives are included in a slightly larger amount, the amount of other additives that are reductively decomposed on the surface of the negative electrode increases, which increases the thickness of the coating. As a result, the additives cannot function effectively and act as low-level antibodies, which may lead to a significant decrease in cell performance.
[0142] On the other hand, the external shape of the lithium secondary battery of the present invention is not particularly limited, but may be cylindrical, rectangular, pouch-shaped, or coin-shaped.
[0143] Furthermore, the lithium secondary battery of the present invention can be usefully used in portable devices such as mobile phones, notebook computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs).
[0144] Furthermore, the lithium secondary battery according to the present invention is applicable not only to battery cells used as power sources for small devices, but also to unit batteries in medium- and large-sized battery modules containing a large number of battery cells. Specifically, the lithium secondary battery of the present invention has a horizontal (33 mm (~39mm) x Height (80 mm It can be applied to battery cells for small devices with a volume of approximately 96mm x 3.0mm to 5.0mm in thickness, and a capacity of 1,000mAh to 3,000mAh.
[0145] The present invention will be described in detail below with reference to examples. However, the examples of the present invention can be modified into various other forms, and the scope of the present invention should not be construed as being limited to the examples detailed below. The examples of the present invention are provided to give a more complete explanation of the present invention to a person of average skill in the art.
[0146] [Examples] Example 1. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2Apply to the positive electrode (loading amount of positive electrode: 0.04) and dry, then roll press. 8g / cm 2 Positive electrode single-sided reference loading amount: 0.02 4g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0147] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0148] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0149] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive and negative electrodes produced by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 3.65 g of the lithium secondary battery electrolyte produced above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0150] Example 2. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0151] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 1, except that 4.98 g of the lithium secondary battery electrolyte manufactured as described above was injected (see Table 1 below).
[0152] Example 3. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0153] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 1, except that 6.64 g of the lithium secondary battery electrolyte manufactured as described above was injected (see Table 1 below).
[0154] Example 4. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.06) and dry, then roll press. 4g / cm 2 Positive electrode single-sided reference loading amount: 0.03 2g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0155] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 ofAfter dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0156] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 1, except that the positive electrode manufactured by the method described above was used and 4.65 g of the manufactured lithium secondary battery electrolyte was injected (see Table 1 below).
[0157] Example 5. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0158] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 4, except that 6.43 g of the lithium secondary battery electrolyte manufactured as described above was injected (see Table 1 below).
[0159] Example 6. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0160] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 4, except that 8.45 g of the lithium secondary battery electrolyte manufactured as described above was injected (see Table 1 below).
[0161] Example 7. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 312 cm²) of cathode current collector. 2 Apply to the positive electrode (loading amount of positive electrode: 0.04) and dry, then roll press. 8g / cm 2 Positive electrode single-sided reference loading amount: 0.02 4g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0162] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0163] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.5% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0164] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive and negative electrodes produced by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 3.10 g of the lithium secondary battery electrolyte produced above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0165] Example 8. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.5% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0166] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 7, except that 3.57 g of the lithium secondary battery electrolyte manufactured as described above was injected (see Table 1 below).
[0167] Example 9. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.5% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0168] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 7, except that 4.77 g of the lithium secondary battery electrolyte manufactured as described above was injected (see Table 1 below).
[0169] Example 10. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin Al film with a thickness of 15 μm, total surface area of the cathode current collector: 312 cm 2 Apply to the positive electrode (loading amount of positive electrode: 0.06) and dry, then roll press. 4g / cm 2Positive electrode single-sided reference loading amount: 0.03 2g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0170] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.5% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0171] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 7, except that the positive electrode manufactured by the method described above was used and 3.43 g of the manufactured lithium secondary battery electrolyte was injected (see Table 1 below).
[0172] Example 11. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.5% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0173] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 10, except that 4.55 g of the lithium secondary battery electrolyte manufactured as described above was injected (see Table 1 below).
[0174] Example 12. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.5% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0175] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 10, except that 6.07 g of the lithium secondary battery electrolyte manufactured as described above was injected (see Table 1 below).
[0176] Example 13. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.04) and dry, then roll press. 8g / cm 2 Positive electrode single-sided reference loading amount: 0.02 4g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0177] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0178] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.25% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0179] (Manufacturing of secondary batteries) After an electrode assembly was produced by a conventional method of sequentially laminating the positive electrode and negative electrode produced by the aforementioned method together with a polyethylene porous film, it was placed in a pouch-type secondary battery case, and 4.86 g of the lithium secondary battery electrolyte produced as described above was injected to fabricate a lithium secondary battery (see Table 1 below).
[0180] Example 14. (Production of Positive Electrode) A positive electrode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) were added at a weight ratio of 96:1:3 to N-methyl-2-pyrrolidone (NMP) as a solvent to prepare a positive electrode active material slurry (solid content: 67% by weight). The positive electrode active material slurry was applied to a 15 μm-thick positive electrode current collector (Al thin film, total surface area of the positive electrode current collector: 435 cm 2 ), dried, and subjected to roll pressing to produce a positive electrode (loading amount of the positive electrode: 0.06 4g / cm 2 , loading amount per one side of the positive electrode: 0.03 2g / cm 2 , porosity of the positive electrode composite material layer: 24%).
[0181] (Production of Negative Electrode) A negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material were added at a weight ratio of 96:3.5:0.5 to distilled water as a solvent to negative electrode prepare an active material slurry (solid content: 53% by weight). The negative electrode active material slurry was applied to an 8 μm-thick negative electrode current collector (Cu thin film), dried, and subjected to roll pressing to produce a negative electrode (porosity of the negative electrode composite material layer: 26%).
[0182] (Production of Electrolyte) To an organic solvent obtained by mixing gamma-butyrolactone and ethylene carbonate at a volume ratio of 70:30, LiPF6 of was dissolved to a concentration of 1.0 M, and then 0.25% by weight of lithium nitrate (LiNO3) was added to prepare the electrolyte for a lithium secondary battery of the present invention.
[0183] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive electrode and negative electrode manufactured by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 4.86 g of the lithium secondary battery electrolyte manufactured above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0184] Example 15. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.04) and dry, then roll press. 8g / cm 2 Positive electrode single-sided reference loading amount: 0.02 4g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0185] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0186] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 ofAfter dissolving to 1.0M, 3.0 wt% of lithium nitrate (LiNO₃) was added to prepare the electrolyte for a lithium secondary battery of the present invention.
[0187] (Production of Secondary Battery) The positive electrode and negative electrode prepared by the aforementioned method were sequentially laminated together with a polyethylene porous film by a conventional method to fabricate an electrode assembly, which was then placed in a pouch-type secondary battery case, and 4.65 g of the electrolyte for a lithium secondary battery prepared above was injected to fabricate a lithium secondary battery (see Table 1 below).
[0188] Example 16. (Production of Positive Electrode) A positive electrode active material (LiFePO₄), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) were added at a weight ratio of 96:1:3 to N-methyl-2-pyrrolidone (NMP) as a solvent to prepare a positive electrode active material slurry (solid content 67 wt%). The positive electrode active material slurry was applied onto a 15 μm-thick positive electrode current collector (Al thin film, total surface area of the positive electrode current collector: 435 cm 2 ), dried, and subjected to roll press to produce a positive electrode (loading amount of the positive electrode: 0.06 4g / cm 2 , loading amount based on one side of the positive electrode: 0.03 2g / cm 2 , porosity of the positive electrode composite material layer: 24%).
[0189] (Production of Negative Electrode) A negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material were added at a weight ratio of 96:3.5:0.5 to distilled water as a solvent to negative electrode prepare an active material slurry (solid content 53 wt%). The negative electrode active material slurry was applied onto an 8 μm-thick negative electrode current collector (Cu thin film), dried, and subjected to roll press to produce a negative electrode (porosity of the negative electrode composite material layer: 26%).
[0190] (Production of Electrolyte) In an organic solvent obtained by mixing gamma-butyrolactone and ethylene carbonate at a volume ratio of 70:30, LiPF6 of was dissolved to a concentration of 1.0 M, then 3.0 wt% of lithium nitrate (LiNO3) was added to prepare the electrolyte for a lithium secondary battery of the present invention.
[0191] (Production of Secondary Battery) After an electrode assembly was produced by a conventional method of sequentially laminating the positive electrode and the negative electrode prepared by the aforementioned method together with a polyethylene porous film, the electrode assembly was placed in a pouch-type secondary battery case, and 4.65 g of the electrolyte for a lithium secondary battery prepared above was injected to fabricate a lithium secondary battery (see Table 1 below).
[0192] Example 17. (Production of Positive Electrode) A positive electrode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) were added at a weight ratio of 96:1:3 to N-methyl-2-pyrrolidone (NMP) as a solvent to prepare a positive electrode active material slurry (solid content: 67 wt%). The positive electrode active material slurry was applied onto a 15 μm-thick positive electrode current collector (Al thin film, total surface area of the positive electrode current collector: 435 cm 2 ), dried, and subjected to roll pressing to produce a positive electrode (loading amount of the positive electrode: 0.04 8g / cm 2 , loading amount based on one side of the positive electrode: 0.02 4g / cm 2 , porosity of the positive electrode composite material layer: 24%).
[0193] (Production of Negative Electrode) A negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material were added at a weight ratio of 96:3.5:0.5 to distilled water as a solvent to negative electrode prepare an active material slurry (solid content: 53 wt%). The negative electrode active material slurry was applied onto an 8 μm-thick negative electrode current collector (Cu thin film), dried, and subjected to roll pressing to produce a negative electrode (porosity of the negative electrode composite material layer: 26%).
[0194] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.5% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0195] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive electrode and negative electrode manufactured by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 8.29 g of the lithium secondary battery electrolyte manufactured above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0196] Example 18. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0197] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 17, except that 8.29 g of the lithium secondary battery electrolyte manufactured as described above was injected (see Table 1 below).
[0198] Example 19. (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 2.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0199] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 17 above, except that 8.29 g of the lithium secondary battery electrolyte prepared above was injected (see Table 1 below).
[0200] Example 20. (Preparation of Electrolyte) LiPF6 was dissolved in an organic solvent obtained by mixing gamma-butyrolactone and ethylene carbonate at a volume ratio of 70:30 of to a concentration of 1.0 M, and then 3.0 wt% of lithium nitrate (LiNO3) was added to prepare the electrolyte for a lithium secondary battery of the present invention.
[0201] (Manufacture of Secondary Battery) A lithium secondary battery was manufactured in the same manner as in Example 17 above, except that 8.29 g of the lithium secondary battery electrolyte prepared above was injected (see Table 1 below).
[0202] Example 21. (Production of Positive Electrode) A positive electrode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) were added at a weight ratio of 96:1:3 to N-methyl-2-pyrrolidone (NMP) as a solvent to prepare a positive electrode active material slurry (solid content: 67 wt%). The positive electrode active material slurry was applied onto a 15 μm-thick positive electrode current collector (Al thin film, total surface area of the positive electrode current collector: 280 cm 2 ), dried, and subjected to roll pressing to produce a positive electrode (loading amount of the positive electrode: 0.04 8g / cm 2 , reference loading amount per one side of the positive electrode: 0.02 4g / cm 2 , porosity of the positive electrode composite material layer: 24%).
[0203] (Production of Negative Electrode) A negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material were added at a weight ratio of 96:3.5:0.5 to distilled water as a solvent to negative electrodeAn active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0204] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0205] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive and negative electrodes produced by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 3.65 g of the lithium secondary battery electrolyte produced above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0206] Example 22. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 465 cm²) of cathode current collector. 2 Apply to the positive electrode (loading amount of positive electrode: 0.04) and dry, then roll press. 8g / cm 2 Positive electrode single-sided reference loading amount: 0.02 4g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0207] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 21, except that the positive electrode manufactured as described above was used (see Table 1 below).
[0208] Example 23. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.03) and dry, then roll press. 0g / cm 2 Positive electrode single-sided reference loading amount: 0.01 5g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0209] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 21, except that the positive electrode manufactured as described above was used (see Table 1 below).
[0210] Example 24. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 ) is applied and dried, and then roll-pressed to perform a positive electrode (positive electrode loading amount: 0.07 2g / cm 2 Positive electrode single-sided reference loading amount: 0.03 6g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0211] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 21, except that the positive electrode manufactured as described above was used (see Table 1 below).
[0212] Example 25. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.04) and dry, then roll press. 8g / cm 2 Positive electrode single-sided reference loading amount: 0.02 4g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0213] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0214] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 21, except that the positive electrode manufactured above was used and 2.98 g of the lithium secondary battery electrolyte manufactured above was injected (see Table 1 below).
[0215] Example 26. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.04) and dry, then roll press. 8g / cm 2 Positive electrode single-sided reference loading amount: 0.02 4g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0216] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 1.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0217] (Manufacturing of secondary batteries) A lithium secondary battery was manufactured in the same manner as in Example 21, except that the positive electrode manufactured above was used and 9.95 g of the lithium secondary battery electrolyte manufactured above was injected (see Table 1 below).
[0218] Comparative Example 1. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 312 cm²) of cathode current collector. 2 Apply to the positive electrode (loading amount of positive electrode: 0.03) and dry, then roll press. 2g / cm2 Positive electrode single-sided reference loading amount: 0.01 6g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0219] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0220] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 4.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0221] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive and negative electrodes produced by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 8.50 g of the lithium secondary battery electrolyte produced above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0222] Comparative Example 2. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 312 cm²) of cathode current collector. 2Apply to the positive electrode (loading amount of positive electrode: 0.06) and dry, then roll press. 4g / cm 2 Positive electrode single-sided reference loading amount: 0.03 2g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0223] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0224] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 11.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0225] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive and negative electrodes produced by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 4.77 g of the lithium secondary battery electrolyte produced above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0226] Comparative Example 3. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.04) and dry, then roll press. 8g / cm 2 Positive electrode single-sided reference loading amount: 0.02 4g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0227] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0228] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.025% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0229] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive and negative electrodes produced by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 3.48 g of the lithium secondary battery electrolyte produced above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0230] Comparative Example 4. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.04) and dry, then roll press. 8g / cm 2 Positive electrode single-sided reference loading amount: 0.02 4g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0231] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0232] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 6.5% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0233] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive electrode and negative electrode manufactured by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 8.29 g of the lithium secondary battery electrolyte manufactured above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0234] Comparative Example 5. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.06) and dry, then roll press. 4g / cm 2 Positive electrode single-sided reference loading amount: 0.03 2g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0235] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0236] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 of After dissolving to a concentration of 1.0 M, 0.02% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0237] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive electrode and negative electrode manufactured by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 3.00 g of the lithium secondary battery electrolyte manufactured above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0238] Comparative Example 6. (Manufacturing of positive electrodes) A cathode active material slurry (67% solids by weight) was prepared by adding a cathode active material (LiFePO4), a conductive material (carbon black), and a binder (polyvinylidene fluoride, PVDF) in a weight ratio of 96:1:3 to the solvent N-methyl-2-pyrrolidone (NMP). The cathode active material slurry was then used to prepare a cathode current collector (a thin aluminum film with a thickness of 15 μm; total surface area of the cathode current collector: 435 cm²). 2 Apply to the positive electrode (loading amount of positive electrode: 0.06) and dry, then roll press. 4g / cm 2 Positive electrode single-sided reference loading amount: 0.03 2g / cm 2 A positive electrode composite layer with a void ratio of 24% was manufactured.
[0239] (Manufacturing of negative electrodes) The negative electrode active material (100% artificial graphite), CMC-SBR as a binder, and carbon black as a conductive material are added to distilled water as a solvent in a weight ratio of 96:3.5:0.5. negative electrode An active material slurry (solid content 53% by weight) was prepared. The anode active material slurry was applied to an 8 μm thick anode current collector (Cu thin film) and dried, and a anode (porosity of the anode composite layer: 26%) was produced by roll pressing.
[0240] (Electrolyte manufacturing) Gamma-butyrolactone and ethylene carbonate are mixed in an organic solvent in a volume ratio of 70:30, and LiPF6 ofAfter dissolving to a concentration of 1.0 M, 12.0% by weight of lithium nitrate (LiNO3) was added to produce the electrolyte for lithium secondary batteries of the present invention.
[0241] (Manufacturing of secondary batteries) After manufacturing an electrode assembly by a conventional method in which the positive electrode and negative electrode manufactured by the method described above are sequentially laminated together with a polyethylene porous film, the assembly is placed in a pouch-type secondary battery case, and 6.43 g of the lithium secondary battery electrolyte manufactured above is injected to manufacture a lithium secondary battery (see Table 1 below).
[0242] [Table 1]
[0243] [Example of experiment] Experimental Example 1. Evaluation of High Temperature (45°C) Cycle Characteristics Each lithium secondary battery manufactured in the above examples and comparative examples was charged to a state of charge (SOC) of 64% at a high temperature (55°C) at a rate of 0.1C, followed by an aging process (48 hours) and a degassing process to perform an activation process.
[0244] After the activation process is complete, each lithium secondary battery is charged to 3.8V at room temperature (25°C) under constant current / constant voltage conditions at a 0.1C rate, and then under conditions at a 0.33C rate. Set Current conditions Up to 2.5V I discharged it and checked the initial capacity.
[0245] Next, each lithium secondary battery was charged to 3.8V at a high temperature (45°C) under constant current / constant voltage conditions at a 0.33C rate, and then discharged to 2.5V under constant current conditions at a 0.33C rate. This process was considered one cycle, and after 100 cycles, the discharge capacity was measured. The lithium secondary batteries were powered using a PNE-0506 charger / discharger (manufacturer: PNE solution).
[0246] 100th discharge relative to the obtained initial capacity capacityThe capacity retention rate (%) after high-temperature cycling was calculated using the ratio, and the results are shown in Table 2 below.
[0247] Experimental Example 2. Evaluation of Low Temperature (-10°C) Cycle Characteristics Each lithium secondary battery manufactured in the above examples and comparative examples was charged to a state of charge (SOC) of 64% at a high temperature (55°C) at a rate of 0.1C, followed by an aging process (48 hours) and a degassing process to perform an activation process.
[0248] After the activation process is complete, each lithium secondary battery is charged to 3.8V at room temperature (25°C) under constant current / constant voltage conditions at a 0.1C rate, and then under conditions at a 0.33C rate. Set Current conditions Up to 2.5V I discharged it and checked the initial capacity.
[0249] Next, each lithium secondary battery was charged to 3.8V at a low temperature (-10°C) under constant current / constant voltage conditions at a 0.2C rate, and then discharged to 2.0V under constant current conditions at a 0.33C rate. This constituted one cycle, and after 200 cycles, the discharge capacity was measured. The lithium secondary batteries were powered using a PNE-0506 charger / discharger (manufacturer: PNE solution).
[0250] The capacity retention rate (%) after low-temperature cycling was calculated using the obtained initial capacity and the discharge capacity after 200 cycles, and the results are shown in Table 2 below.
[0251] [Table 2]
[0252] Referring to Table 2 above, it can be confirmed that the lithium secondary batteries manufactured in Examples 1 to 26 of the present invention show improved capacity retention rates (%) after high-temperature cycling and low-temperature cycling compared to the lithium secondary batteries of Comparative Examples 1 to 6.
[0253] Although preferred embodiments of the present invention have been described above with reference to the present invention, those skilled in the art, or those with ordinary skill in the art, will understand that they can modify and change the present invention in various ways without departing from the spirit and technical scope of the invention as set forth in the appended claims. Therefore, the technical scope of the present invention is not limited to what is described in the detailed description of the specification, but is determined solely by the claims.
Claims
1. A lithium secondary battery comprising a positive electrode, a negative electrode, a separator, and an electrolyte, The positive electrode contains lithium iron phosphorus oxide as the positive electrode active material. The electrolyte comprises a lithium salt, a first organic solvent, a second organic solvent, and an additive. The first organic solvent is a cyclic lactone compound, The second organic solvent is a carbonate-based organic solvent, The aforementioned additive is lithium nitrate (LiNO 3 A lithium secondary battery that satisfies the following formula 1. [Formula 1] [Math 1] (In formula 1 above, A is the total amount (g) of electrolyte injected into the lithium secondary battery. B is lithium nitrate (LiNO) contained in the injected electrolyte. 3 This is the content (by weight %) of ) C is the loading amount of the positive electrode (g / cm³). 2 ) and D is the total surface area (cm²) of the positive electrode current collector. 2 )
2. The lithium secondary battery according to claim 1, wherein the lithium iron phosphorus oxide comprises a compound represented by the following chemical formula 1. [Chemical formula 1] Li 1+a Fe x M y (PO 4-b )X’ b (In the above chemical formula 1, M is one selected from the group consisting of Al, Mg, Ni, Co, Mn, Ti, Ga, Cu, V, Nb, Zr, Ce, In, Zn, and Y. X' is one or more elements selected from the group consisting of F, S, and N. (-0.5 ≤ a ≤ 0.5, 0 < x ≤ 1, 0 ≤ y ≤ 1, and 0 ≤ b ≤ 0.3.)
3. The lithium iron phosphorus oxide is lithium iron phosphorus oxide (LiFePO 4 ) or lithium manganese iron phosphate (LiFeMnPO 4 The lithium secondary battery according to claim 2, wherein the lithium secondary battery is as described in claim 2.
4. The lithium secondary battery according to claim 1, wherein the cyclic lactone compound comprises gammabutyrolactone.
5. The lithium secondary battery according to claim 1, wherein the carbonate-based organic solvent is a cyclic carbonate-based organic solvent.
6. The lithium secondary battery according to claim 1, wherein the first organic solvent and the second organic solvent are contained in a volume ratio of 50:50 to 99:
1.
7. The lithium secondary battery according to claim 1, wherein A in formula 1 is 3.0 g to 8.5 g.
8. In the above formula 1, C is 0.032 g / cm³. 2 ~0.064g / cm 2 The lithium secondary battery according to claim 1.
9. In the above equation 1, D is 310 cm. 2 ~450cm 2 The lithium secondary battery according to claim 1.
10. The lithium secondary battery according to claim 1, wherein the negative electrode comprises a carbon-based active material, a silicon-based active material, or a mixture of a carbon-based active material and a silicon-based active material.
11. The lithium secondary battery according to claim 1, wherein the capacity of the lithium secondary battery is 1,000 mAh to 3,000 mAh.