Lithium-ion battery
By using a non-aqueous electrolyte with specific additives in lithium iron phosphate electrodes, the challenges of electrolyte impregnation and capacity issues in high-loading lithium-ion batteries are addressed, resulting in enhanced performance and low-temperature capabilities.
Patent Information
- Application Number
- JP2026532619
- Authority / Receiving Office
- JP · JP
- Patent Type
- Applications
- Current Assignee / Owner
- Priority Date
- 2023-12-21
- Filing Date
- 2024-12-19
- Publication Date
- 2026-11-19
AI Technical Summary
Lithium iron phosphate-based positive electrodes in lithium-ion batteries face challenges with non-aqueous electrolyte impregnation at high loading amounts, leading to reduced capacity, increased resistance, and decreased lifespan performance, especially at low temperatures.
Incorporating a non-aqueous electrolyte with specific additives represented by chemical formulas 1 to 3, in a range of 0.1% to 3% by weight, to improve electrolyte impregnation in lithium iron phosphate positive electrodes with loading amounts between 450 mg/25 cm² to 740 mg/25 cm², enhancing capacity development and resistance characteristics.
The solution results in improved electrolyte impregnation, leading to superior capacity, lifespan performance, and low-temperature power characteristics of lithium-ion batteries.
Smart Images

Figure 2026539118000001 
Figure 2026539118000002 
Figure 2026539118000003
Abstract
Description
[Technical Field]
[0001] This invention relates to a lithium secondary battery. [Background technology]
[0002] With the development of the information society, individuals For With the development of IT devices and computer networks, the overall dependence of society on electrical energy has increased. Increasing Therefore, there is a need to develop technologies for efficiently storing and utilizing electrical energy.
[0003] Rechargeable batteries are the most suitable technology for a wide range of applications among the technologies currently under development, and among such rechargeable batteries, For There is growing interest in lithium-ion batteries, which not only can be miniaturized to a degree suitable for application in IT devices, but also have the highest energy density. [Overview of the Initiative] [Problems that the invention aims to solve]
[0004] This invention One embodiment The present invention provides a lithium secondary battery comprising a positive electrode containing lithium iron phosphate particles as a positive electrode active material and having a loading amount of a specific amount or more, wherein the impregnation of the non-aqueous electrolyte into the positive electrode is improved, and the lithium secondary battery has excellent low-temperature output performance. [Means for solving the problem]
[0005] [1] The present invention One embodiment The device comprises a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte. The positive electrode contains a positive electrode active material, which contains lithium iron phosphate oxide particles. The loading amount of the positive electrode is approximately 450 mg / 25 cm². 2 ~740mg / 25cm 2The present invention provides a lithium secondary battery in which the non-aqueous electrolyte comprises a lithium salt, an organic solvent, and an additive, the additive comprising at least one compound selected from the group consisting of compounds represented by the following chemical formulas 1 to 3, and the additive is present in the non-aqueous electrolyte in an amount of about 0.1% to 3% by weight.
[0006] [Chemical formula 1] [ka]
[0007] In the above chemical formula 1, R1 is hydrogen or an alkyl group having 1 to 3 carbon atoms, and n is an integer from 1 to 10.
[0008] [Chemical formula 2] [ka]
[0009] In the above chemical formula 2, m is an integer between 0 and 18.
[0010] [Chemical formula 3] [ka]
[0011] In the above chemical formula 3, R2 and R3 are each independently an alkylene group having 1 to 10 carbon atoms, and R4 is an alkyl group having 1 to 20 carbon atoms substituted with one or more fluorine atoms.
[0012] [2] The present invention One embodiment The present invention provides a lithium secondary battery according to [1], wherein in the chemical formula 1, n is an integer from 3 to 8.
[0013] [3] The present invention One embodiment The present invention provides a lithium secondary battery according to either [1] or [2], wherein R1 in the chemical formula 1 is hydrogen.
[0014] [4] The present invention One embodiment The present invention provides a lithium secondary battery according to any one of [1] to [3], wherein the compound represented by chemical formula 1 includes at least one selected from the group consisting of compounds represented by the following chemical formulas 1-1 to 1-3.
[0015] [Chemical formula 1-1] [ka]
[0016] [Chemical formula 1-2] [ka]
[0017] [Chemical formula 1-3] [ka]
[0018] [5] The present invention One embodiment The present invention provides a lithium secondary battery according to any one of the above [1] to [4], wherein in the above chemical formula 2, m is an integer from 2 to 8.
[0019] [6] The present invention One embodiment The present invention provides a lithium secondary battery according to any one of [1] to [5], wherein the compound represented by chemical formula 2 includes at least one selected from the group consisting of compounds represented by the following chemical formulas 2-1 to 2-4.
[0020] [Chemical formula 2-1] [ka]
[0021] [Chemical formula 2-2] [ka]
[0022] [Chemical formula 2-3] [ka]
[0023] [Chemical formula 2-4] [ka]
[0024] [7] The present invention One embodiment The present invention provides a lithium secondary battery according to any one of [1] to [6], wherein in the chemical formula 3, R2 and R3 are each independently an alkylene group having 1 to 5 carbon atoms, and R4 is an alkyl group having 3 to 20 carbon atoms substituted with one or more fluorines.
[0025] [8] The present invention One embodiment The present invention provides a lithium secondary battery according to any one of [1] to [7], wherein in the chemical formula 3, R4 is an alkyl group having 4 to 8 carbon atoms substituted with one or more fluorines.
[0026] [9] The present invention One embodiment The present invention provides a lithium secondary battery according to any one of [1] to [8] above, wherein the compound represented by chemical formula 3 includes the compound represented by chemical formula 3-1 below.
[0027] [Chemical formula 3-1] [ka]
[0028]
[10] The present invention One embodiment The loading amount of the positive electrode is approximately 500 mg / 25 cm 2 ~600mg / 25cm 2 The present invention provides a lithium secondary battery as described in any one of the above [1] to [9].
[0029]
[11] The present invention One embodimentprovides the lithium secondary battery according to any one of the above [1] to
[10] , wherein the non-aqueous electrolyte further contains vinylene carbonate.
[0030]
[12] The present invention One embodiment provides the lithium secondary battery according to any one of the above [1] to
[11] , wherein the organic solvent includes a cyclic carbonate-based solvent and a linear carbonate-based solvent.
[0031]
[13] The present invention One embodiment wherein the linear carbonate Solvent system contains dimethyl carbonate, provides the lithium secondary battery according to any one of the above [1] to
[12] .
[0032]
[14] The present invention One embodiment provides the lithium secondary battery according to any one of the above [1] to
[13] , wherein the lithium iron phosphate oxide particles include a compound represented by the following Chemical Formula A.
[0033] [Chemical Formula A] Li 1+a Fe 1-s M s (PO 4-b )X b
[0034] In the above Chemical Formula A, M is one or more elements selected from Co, Ni, Mn, Al, Mg, Ti, and V, X is F, S, or N, and 0≦s≦0.5; -0.5≦a≦+0.5; 0≦b≦0.1.
[0035]
[15] The present invention One embodiment provides the lithium secondary battery according to any one of the above [1] to
[14] , wherein the lithium iron phosphate oxide particles contain LiFePO4. Effects of the Invention
[0036] The present invention One embodimentThe lithium secondary battery relating to this invention is characterized by having a loading amount of a specific amount or more and comprising a positive electrode containing lithium iron phosphate oxide particles as a positive electrode active material, and a non-aqueous electrolyte containing at least one compound represented by the chemical formulas 1 to 3 in a specific content as an additive. One embodiment According to the lithium secondary battery, by using a non-aqueous electrolyte containing the above-mentioned additives in specific amounts, the electrolyte impregnation of the positive electrode with a high loading capacity can be improved, resulting in superior capacity development, lifespan performance, and resistance characteristics of the lithium secondary battery. [Modes for carrying out the invention]
[0037] First, prior to describing the present invention, the terms and words used in this specification and the claims should not be interpreted in a manner limited to their ordinary or dictionary meanings, but rather in a manner consistent with the technical idea of the present invention, in accordance with the principle that inventors may appropriately define the concepts of terms in order to best describe their invention.
[0038] On the other hand, the terms used herein are used solely to describe exemplary embodiments and are not intended to limit the invention. Singular expressions are used only when the context is clear. Multiple items have not been excluded. This includes multiple expressions, as far as is possible.
[0039] In this specification, terms such as “includes,” “equip,” or “have” are intended to specify the presence of implemented features, figures, steps, components, or combinations thereof, and should be understood not to preemptively exclude the presence or possibility of adding one or more other features, figures, steps, components, or combinations thereof.
[0040] In this specification, "%" means weight percent unless explicitly indicated otherwise.
[0041] Before describing the present invention, in the description of "carbon number a to b" in the specification, "a" and "b" refer to the number of carbon atoms contained in a specific functional group. That is, the functional group may contain "a" to "b" carbon atoms.
[0042] Furthermore, in this specification, unless otherwise defined, "substitution" means that at least one hydrogen atom bonded to a carbon atom is replaced by an element other than hydrogen, for example, by an alkyl group having 1 to 5 carbon atoms or by a fluorine element.
[0043] In this specification, the average particle size (D 50 The average particle size (D) can be defined as the particle size corresponding to 50% of the cumulative volume in the particle size distribution curve. 50 The particle size can be measured, for example, by laser diffraction. This laser diffraction method can generally measure particle sizes from the submicron region to several millimeters in size, and can yield highly reproducible and high-resolution results.
[0044] As used herein, “approximately,” “essentially,” and “substantially” are used to mean a range of values or degrees, or something close to them, taking into account inherent manufacturing and material tolerances.
[0045] Typically, lithium-ion batteries are manufactured by injecting or impregnating an electrode assembly, consisting of a positive electrode, a negative electrode, and a porous separator, with a non-aqueous electrolyte.
[0046] For the negative electrode active material of such lithium secondary batteries, carbon-based active materials and silicon-based active materials are being considered. On the other hand, for the positive electrode active material, lithium-containing cobalt oxide, layered crystal structure LiMnO2, spinel crystal structure LiMn2O4, and lithium-containing nickel oxide (LiNiO2) are being considered.
[0047] In recent years, lithium iron phosphate oxide (e.g., LiFePO4)-based active materials, which have excellent thermal stability and are relatively inexpensive, have been considered for use as cathode active materials.
[0048] However, since the lithium iron phosphate active material has a lower specific capacity compared to lithium cobalt oxide, lithium nickel oxide, etc., it is necessary to use the lithium iron phosphate active material with a high loading amount in order to increase the energy density of the positive electrode and lithium secondary battery containing it. However, high-load lithium iron phosphate positive electrodes have the problem that the non-aqueous electrolyte is not easily impregnated into the positive electrode, making it difficult to achieve capacity, increasing resistance, and reducing lifespan.
[0049] Taking these points into consideration, the present invention One embodiment This invention provides a lithium secondary battery comprising a positive electrode containing lithium iron phosphate particles as a positive electrode active material and having a loading amount of a specific amount or more, thereby improving the impregnation of the non-aqueous electrolyte into the positive electrode and providing a lithium secondary battery having excellent low-temperature output performance.
[0050] The present invention is described below. One embodiment I will explain this in detail.
[0051] Lithium-ion battery This invention One embodiment This relates to lithium-ion batteries.
[0052] In one embodiment, the present invention One embodiment The lithium secondary battery relating to this invention comprises a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte. The positive electrode comprises a positive electrode active material, which comprises lithium iron phosphate oxide particles. The loading amount of the positive electrode is approximately 450 mg / 25 cm². 2 ~740mg / 25cm 2 The non-aqueous electrolyte comprises a lithium salt, an organic solvent, and an additive, wherein the additive comprises at least one compound selected from the group consisting of compounds represented by the following chemical formulas 1 to 3, and the additive is present in the non-aqueous electrolyte in an amount of about 0.1% to 3% by weight.
[0053] [Chemical formula 1] [ka]
[0054] In the above chemical formula 1, R1 is hydrogen or an alkyl group having 1 to 3 carbon atoms, and n is an integer from 1 to 10.
[0055] [Chemical formula 2] [ka]
[0056] In the above chemical formula 2, m is an integer between 0 and 18.
[0057] [Chemical formula 3] [ka]
[0058] In the above chemical formula 3, R2 and R3 are each independently an alkylene group having 1 to 10 carbon atoms, and R4 is an alkyl group having 1 to 20 carbon atoms substituted with one or more fluorine atoms.
[0059] This invention One embodiment The lithium secondary battery relating to this invention is characterized by having a loading amount of a specific amount or more and comprising a positive electrode containing lithium iron phosphate oxide particles as a positive electrode active material, and a non-aqueous electrolyte containing at least one compound represented by the chemical formulas 1 to 3 in a specific content as an additive. One embodiment According to the lithium secondary battery, by using a non-aqueous electrolyte containing the above-mentioned additives in specific amounts, the electrolyte impregnation of the positive electrode with a high loading capacity can be improved, resulting in superior capacity development, lifespan performance, and resistance characteristics of the lithium secondary battery.
[0060] The lithium secondary battery includes a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte. For example, the lithium secondary battery includes a positive electrode, a negative electrode facing the positive electrode, a separator interposed between the positive electrode and the negative electrode, and a non-aqueous electrolyte.
[0061] In one embodiment, the lithium secondary battery can be manufactured by a method comprising the steps of: manufacturing an electrode assembly including a positive electrode, a negative electrode, and a separator; housing the electrode assembly in a battery case; manufacturing a non-aqueous electrolyte including a lithium salt, an organic solvent, and an additive; and injecting or impregnating the battery case with the non-aqueous electrolyte.
[0062] (1) Positive electrode The positive electrode includes a positive electrode active material. The positive electrode active material includes lithium iron phosphate oxide (e.g., LiFePO4) particles.
[0063] The lithium iron phosphorus particles may contain a compound represented by the following chemical formula A.
[0064] [Chemical formula A] Li 1+a Fe 1-s M s (PO 4-b )X b
[0065] In the above chemical formula A, M is one or more elements selected from Co, Ni, Mn, Al, Mg, Ti, and V, and X is F, S, or N, with 0 ≤ s ≤ 0.5; -0.5 ≤ a ≤ +0.5; 0 ≤ b ≤ 0.1.
[0066] The aforementioned chemical formula A can be represented, for example, as LiFePO4 (a=0, s=0, and b=0).
[0067] The lithium iron phosphate particles may be in the form of primary particles or secondary particles formed by the aggregation of two or more primary particles. In one embodiment, the lithium iron phosphate particles may be in the form of primary particles.
[0068] The lithium iron phosphate particles may consist of primary particles, secondary particles formed by aggregating two or more primary particles, or a mixture of primary particles and secondary particles formed by aggregating two or more primary particles.
[0069] If the lithium iron phosphorus particles are in the form of primary particles, the average particle size (D 50 The particle size may be approximately 0.2 μm to 3.0 μm, or 0.2 μm to 2.0 μm, or 0.3 μm to 1.5 μm. Furthermore, if the lithium iron phosphate particles are in the form of secondary particles formed by the aggregation of two or more primary particles, the primary particles have an average particle size (D 50 The particle size may be 0.2 μm to 3.0 μm, or 0.2 μm to 2.0 μm, or 0.3 μm to 1.5 μm, and the secondary particles have an average particle size (D 50 The size of the ) may be 7 μm to 25 μm, or 10 μm to 20 μm.
[0070] In one embodiment, the positive electrode active material may further include a carbon coating layer located on the surface of the lithium iron phosphate particles. The carbon coating layer may be introduced for purposes such as protecting the lithium iron phosphate particles and improving electrical conductivity.
[0071] The loading amount of the positive electrode is approximately 450 mg / 25 cm³. 2 ~740mg / 25cm 2 That is the case.
[0072] The aforementioned lithium iron phosphate particles have advantages over other cathode active materials such as lithium cobalt oxide and lithium nickel-cobalt-manganese oxide, including superior thermal stability and relatively low cost. However, due to their low specific capacity, the loading amount needs to be increased to achieve high energy density. Increasing the loading amount of the cathode (for example, approximately 450 mg / 25 cm³) 2 ~740mg / 25cm 2In this case, a high-energy-density battery (for example, a lithium secondary battery with a cell design capacity of at least 500 mAh and an initial discharge capacity of at least 500 mAh) can be realized, but because the non-aqueous electrolyte does not sufficiently impregnate the inside of the positive electrode, it becomes difficult for the lithium secondary battery to achieve its full capacity, resistance increases, and lifespan performance tends to decrease.
[0073] Taking these points into consideration, the present invention One embodiment The lithium secondary battery relating to this invention is characterized by using a non-aqueous electrolyte in which at least one compound selected from the compounds represented by chemical formulas 1 to 3 is used as an additive to the non-aqueous electrolyte, and the content of these compounds is adjusted to a specific range. Due to these characteristics, approximately 450 mg / 25 cm³ 2 ~740mg / 25cm 2 The electrolyte impregnation of the positive electrode with a loading amount can be improved, enabling the realization of a superior level of lithium secondary battery capacity, and improving lifespan performance and resistance characteristics. For example, the present invention One embodiment The lithium secondary battery described herein is advantageous in terms of improving low-temperature power characteristics.
[0074] In one embodiment, the loading amount of the positive electrode is approximately 450 mg / 25 cm³. 2 ~740mg / 25cm 2 450mg / 25cm 2 ~730mg / 25cm 2 450mg / 25cm 2 ~720mg / 25cm 2 450mg / 25cm 2 ~710mg / 25cm 2 , or 450 mg / 25 cm 2 ~700mg / 25cm 2 , or approximately 500 mg / 25 cm 2 ~680mg / 25cm 2 500mg / 25cm 2 ~650mg / 25cm 2 500mg / 25cm 2 ~625mg / 25cm 2 , or 500mg / 25cm 2~600mg / 25cm 2 That's fine.
[0075] The positive electrode may include a positive electrode current collector and a positive electrode active material layer disposed on at least one side of the positive electrode current collector. In this case, the positive electrode active material layer may include the aforementioned positive electrode active material.
[0076] The positive electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. For example, the positive electrode current collector can be made of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel with surface treatment using carbon, nickel, titanium, silver, etc., or aluminum-cadmium alloy.
[0077] The thickness of the positive electrode current collector is typically between 3 μm and 500 μm.
[0078] The positive electrode current collector may have its surface textured to enhance the bonding force of the positive electrode active material. For example, the positive electrode current collector can be used in various forms such as film, sheet, foil, mesh, porous material, foam, or nonwoven fabric.
[0079] The positive electrode active material layer is disposed on at least one side of the positive electrode current collector. In one embodiment, the positive electrode active material layer may be disposed on one or both sides of the positive electrode current collector.
[0080] The positive electrode active material may be included in the positive electrode active material layer in an amount of approximately 80% to 99% by weight, taking into consideration the sufficient capacity exertion of the positive electrode active material.
[0081] The positive electrode active material layer may further include a binder and / or a conductive material along with the positive electrode active material.
[0082] The binder is a component that assists in the bonding of the active material to the conductive material and to the current collector, and may include, for example, at least one selected from the group consisting of polyvinylidene fluoride, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, ethylene-propylene-dientelpolymer (EPDM), sulfonated EPDM, styrene-butadiene rubber, and fluororubber, or polyvinylidene fluoride.
[0083] The binder may be included in the positive electrode active material layer in an amount of about 1% to 20% by weight, or about 1.2% to 10% by weight, in order to ensure sufficient binding force between components such as the positive electrode active material.
[0084] The conductive material is used to assist and improve the conductivity of a secondary battery, and is not particularly limited as long as it does not cause chemical changes and is conductive. Specifically, the positive electrode conductive material may be graphite such as natural graphite or artificial graphite; carbon black, acetylene black, or Ketjenblack. (Registered trademark) The material may contain at least one selected from the group consisting of: carbon black such as channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; and polyphenylene derivatives. Preferably, it may contain carbon black in order to improve conductivity.
[0085] The conductive material may be included in the positive electrode active material layer in an amount of about 1% to 20% by weight, or about 1.2% to 10% by weight, in order to ensure sufficient electrical conductivity.
[0086] The thickness of the positive electrode active material layer may be approximately 100 μm to 300 μm, or 150 μm to 250 μm.
[0087] The positive electrode can be manufactured by coating a positive electrode slurry containing a positive electrode active material and selectively a binder, conductive material, and solvent for forming the positive electrode slurry onto the positive electrode current collector, followed by drying and rolling.
[0088] The solvent for forming the positive electrode slurry may include an organic solvent such as NMP (N-methyl-2-pyrrolidone). The solid content of the positive electrode slurry may be about 40% to 90% by weight, or in one embodiment, about 50% to 80% by weight.
[0089] (2) Negative electrode The negative electrode faces the positive electrode.
[0090] The aforementioned negative electrode contains a negative electrode active material.
[0091] The negative electrode may include a negative electrode current collector and a negative electrode active material layer disposed on at least one side of the negative electrode current collector. In this case, the negative electrode active material may be contained in the negative electrode active material layer.
[0092] The negative electrode current collector is not particularly limited as long as it does not cause chemical changes in the battery and has high conductivity. For example, the negative electrode current collector may be made of copper, stainless steel, aluminum, nickel, titanium, calcined carbon, copper or stainless steel with a surface treatment of carbon, nickel, titanium, silver, etc., or an aluminum-cadmium alloy.
[0093] The negative electrode current collector typically has a thickness of approximately 3 μm to 500 μm.
[0094] The negative electrode current collector may have its surface textured to enhance the bonding force of the negative electrode active material. For example, the negative electrode current collector can be used in various forms such as film, sheet, foil, mesh, porous material, foam, or nonwoven fabric.
[0095] The negative electrode active material layer is disposed on at least one side of the negative electrode current collector. In one embodiment, the negative electrode active material layer may be disposed on one or both sides of the negative electrode current collector.
[0096] The aforementioned negative electrode active material layer may contain a negative electrode active material.
[0097] The negative electrode active material is a material capable of reversibly intercalating / deintercalating lithium ions, and may include at least one selected from the group consisting of carbon-based active materials, metalloid-based active materials, and lithium metal. In one embodiment, it may include at least one selected from carbon-based active materials and metalloid-based active materials.
[0098] The carbon-based active material may include at least one selected from the group consisting of graphite, hard carbon, soft carbon, carbon black, graphene, and fibrous carbon, and preferably includes graphite. The graphite may include at least one selected from the group consisting of artificial graphite and natural graphite.
[0099] The average particle size (D) of the carbon-based active material 50 The thickness of the ) may be approximately 10 μm to 30 μm, or approximately 15 μm to 25 μm, in order to ensure structural stability during charging and discharging and to reduce side reactions with the electrolyte.
[0100] For example, the metalloid active material may include: at least one metalloid selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, V, Ti, and Sn; an alloy of lithium with at least one metalloid selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, V, Ti, and Sn; an oxide of at least one metalloid selected from the group consisting of Cu, Ni, Na, K, Rb, Cs, Fr, Be, Mg, Ca, Sr, Si, Sb, Pb, In, Zn, Ba, Ra, Ge, Al, V, Ti, and Sn; lithium titanium oxide (LTO); lithium vanadium oxide; and the like.
[0101] In one embodiment, the metalloid active material may include a silicon-based active material.
[0102] The silicon-based active material is SiO x The compound may contain compounds represented by (0 ≤ x < 2). SiO2 does not react with lithium ions and therefore cannot store lithium. For this reason, x is within the above range, and in one embodiment, the silicon-based active material may be SiO2.
[0103] The average particle size (D) of the silicon-based active material 50 The thickness of the ) may be approximately 1 μm to 30 μm, or 2 μm to 15 μm, in order to ensure structural stability during charging and discharging and to reduce side reactions with the electrolyte.
[0104] The negative electrode active material may be present in the negative electrode active material layer in an amount of approximately 60% to 99% by weight, or approximately 75% to 95% by weight.
[0105] The negative electrode active material layer may further include a binder and / or a conductive material together with the negative electrode active material.
[0106] The binder is used to improve the performance of the battery by improving the adhesion between the negative electrode active material layer and the negative electrode current collector, and may contain, for example, at least one selected from the group consisting of polyvinylidene fluoride-hexafluoropropylene copolymer (PVDF-co-HFP), polyvinylidene fluoride (PVDF), polyacrylonitrile, polymethyl methacrylate, polyvinyl alcohol, carboxymethylcellulose (CMC), starch, hydroxypropylcellulose, regenerated cellulose, polyvinylpyrrolidone, polytetrafluoroethylene, polyethylene, polypropylene, polyacrylic acid, ethylene-propylene-diene monomer (EPDM), sulfonated EPDM, styrene-butadiene rubber (SBR), fluororubber, and substances in which the hydrogen of these substances is substituted with Li, Na, or Ca, or may contain various copolymers thereof.
[0107] The binder may be included in the negative electrode active material layer in an amount of about 0.5% to 10% by weight, or about 1% to 5% by weight.
[0108] The conductive material is not particularly limited as long as it does not cause a chemical change in the battery and is conductive, for example, graphite such as natural graphite or artificial graphite; carbon black, acetylene black, Ketjenblack. (Registered trademark) ), carbon black such as channel black, furnace black, lamp black, and thermal black; conductive fibers such as carbon fibers and metal fibers; conductive tubes such as carbon nanotubes; fluorocarbons; metal powders such as aluminum and nickel powder; conductive whiskers such as zinc oxide and potassium titanate; conductive metal oxides such as titanium oxide; conductive materials such as polyphenylene derivatives may be used.
[0109] The conductive material may be included in the negative electrode active material layer in an amount of about 0.5% to 10% by weight, or about 1% to 5% by weight.
[0110] The thickness of the negative electrode active material layer may be approximately 50 μm to 300 μm, or approximately 100 μm to 200 μm.
[0111] The loading amount of the negative electrode active material layer is approximately 200 mg / 25 cm 2 ~500mg / 25cm 2 , or approximately 250 mg / 25 cm 2 ~400mg / 25cm 2 That's fine.
[0112] The negative electrode can be manufactured by coating at least one surface of a negative electrode current collector with a negative electrode slurry containing a negative electrode active material, a binder, a conductive material, and / or a solvent for forming the negative electrode slurry, followed by drying and rolling.
[0113] The solvent for forming the negative electrode slurry may include, for example, at least one selected from the group consisting of distilled water, NMP (N-methyl-2-pyrrolidone), ethanol, methanol, and isopropyl alcohol, or distilled water, in order to facilitate the dispersion of the negative electrode active material, binder, and / or conductive material. The solid content of the negative electrode slurry may be about 30% to 80% by weight, or in one embodiment, about 40% to 70% by weight.
[0114] (3) Separator The separator can be interposed between the positive electrode and the negative electrode.
[0115] The separator may be a conventional porous polymer film used as a separator, such as a porous polymer film made from polyolefin polymers such as ethylene monopolymer, propylene monopolymer, ethylene / butene copolymer, ethylene / hexene copolymer, and ethylene / methacrylate copolymer, used alone or in a laminated form. Alternatively, a conventional porous nonwoven fabric, such as a nonwoven fabric made of high-melting-point glass fiber or polyethylene terephthalate fiber, may be used, but is not limited to these. Furthermore, a coated separator containing ceramic components or polymeric substances may be used to ensure heat resistance or mechanical strength, and may be selectively used as a single-layer or multi-layer structure.
[0116] (4) Non-aqueous electrolytes 1) Lithium salt First, let me explain lithium salts as follows:
[0117] In the non-aqueous electrolyte for lithium secondary batteries according to one embodiment of the present invention, the lithium salt can be any lithium salt that is not limited to those commonly used in electrolytes for lithium secondary batteries, for example, Li as the cation. + It includes, as an anion, F - Cl - , Br - , I - NO3 - , N(CN)2 - BF4 - ClO4 - AlO4 - AlCl4 - PF6 - SbF6 - AsF6 - B 10 Cl 10 - BF2C2O4 - BC4O8 - PF4C2O4 - PF2C4O8 - (CF3)2PF4 - (CF3)3PF3 -, (CF3)4PF2 - , (CF3)5PF - , (CF3)6P - , CF3SO3 - , C4F9SO3 - , CF3CF2SO3 - , (CF3SO2)2N - , (FSO2)2N - , CF3CF2(CF3)2CO - , (CF3SO2)2CH - , CH3SO3 - , CF3(CF2)7SO3 - , CF3CO2 - , CH3CO2 - , SCN - , and (CF3CF2SO2)2N - at least any one selected from the group consisting of is mentioned. For example, examples of the lithium salt include LiCl, LiBr, LiI, LiBF4, LiClO4, LiAlO4, LiAlCl4, LiPF6, LiSbF6, LiAsF6, LiB 10 Cl 10 , at least any one or more selected from the group consisting of LiBOB (LiB(C2O4)2), LiCF3SO3, LiTFSI (LiN(SO2CF3)2), LiFSI (LiN(SO2F)2), LiCH3SO3, LiCF3CO2, LiCH3CO2, and LiBETI (LiN(SO2CF2CF3)2) can be cited. In one embodiment, the lithium salt may include a single substance or a mixture of two or more selected from the group consisting of LiBF4, LiClO4, LiPF6, LiBOB (LiB(C2O4)2), LiCF3SO3, LiTFSI (LiN(SO2CF3)2), LiFSI (LiN(SO2F)2), and LiBETI (LiN(SO2CF2CF3)2), or may include LiPF6.
[0118] The lithium salt may be modified as appropriate within the range of normal use, but in order to obtain the effect of forming a corrosion-preventive film on the electrode surface, it may be included in the electrolyte at a concentration of approximately 0.8 M to 3.0 M, or approximately 1.0 M to 3.0 M. In this case, the unit "M" is molar concentration, and specifically may mean "mol / L".
[0119] When the concentration of the lithium salt satisfies the above range, the viscosity of the non-aqueous electrolyte can be controlled to achieve optimal impregnation, thereby improving the mobility of lithium ions and improving the capacity characteristics and cycle characteristics of the lithium secondary battery.
[0120] 2) Organic solvents The aforementioned organic solvent can be used without limitation, as long as it is an organic solvent used in the non-aqueous electrolyte of lithium secondary batteries.
[0121] For example, the organic solvent may include at least one selected from the group consisting of cyclic carbonate solvents and linear carbonate solvents. In one embodiment, the organic solvent may include a cyclic carbonate solvent and a linear carbonate solvent. The organic solvent may consist of a cyclic carbonate solvent and a linear carbonate solvent.
[0122] The cyclic carbonate solvent may include at least one selected from the group consisting of ethylene carbonate (EC), fluoroethylene carbonate (FEC), propylene carbonate (PC), 1,2-butylene carbonate, 2,3-butylene carbonate, 1,2-pentylene carbonate, 2,3-pentylene carbonate, and vinylene carbonate (VC). In one embodiment, it may include ethylene carbonate as a highly viscous organic solvent with a high dielectric constant that readily dissociates lithium salts in the electrolyte.
[0123] For example, the above linearThe carbonate-based solvent may include at least one selected from the group consisting of dimethyl carbonate (DMC), diethyl carbonate (DEC), dipropyl carbonate, ethyl methyl carbonate (EMC), methyl propyl carbonate, and ethyl propyl carbonate, and may include dimethyl carbonate in particular due to its excellent electrolyte impregnation properties, and is an organic solvent having low viscosity and low dielectric constant.
[0124] If the linear carbonate solvent contains dimethyl carbonate, the linear carbonate solvent may further contain ethyl methyl carbonate along with the dimethyl carbonate. Solvent system If the material further contains ethyl methyl carbonate, the stability of the SEI (Solid Electrolyte Interphase) coating can be further improved.
[0125] The volume ratio of the cyclic carbonate solvent to the linear carbonate solvent may be about 10:90 to 50:50, or about 15:85 to 50:50, or in one embodiment, about 20:80 to 35:65. When the ratio is within the above range, high ion transfer characteristics and low viscosity of the electrolyte can be achieved.
[0126] In one embodiment, the organic solvent may contain about 10% to 50% by volume of ethylene carbonate, about 5% to 55% by volume of dimethyl carbonate, and about 20% to 70% by volume of ethyl methyl carbonate; or it may contain about 20% to 40% by volume of ethylene carbonate, about 7% to 45% by volume of dimethyl carbonate, and about 25% to 65% by volume of ethyl methyl carbonate; or in one embodiment, it may contain about 25% to 35% by volume of ethylene carbonate, about 7% to 15% by volume of dimethyl carbonate, and about 50% to 68% by volume of ethyl methyl carbonate. When the organic solvent is within the above range, electrolyte impregnation is improved and the stability of the negative electrode SEI coating is enhanced.
[0127] On the other hand, the organic solvent may be further used with any organic solvent commonly used with non-aqueous electrolytes, without limitation, as needed. For example, it may further contain at least one or more organic solvents from the following categories: ester solvents, ether solvents, glyme solvents, and nitrile solvents.
[0128] The ester solvent may include at least one selected from the group consisting of methyl acetate, ethyl acetate, propyl acetate, butyl acetate, methyl propionate, ethyl propionate, propyl propionate, and butyl propionate, γ-butyrolactone, γ-valerolactone, γ-caprolactone, σ-valerolactone, and ε-caprolactone.
[0129] The ether-based solvent can be any one selected from the group consisting of dimethyl ether, diethyl ether, dipropyl ether, methyl ethyl ether, methyl propyl ether, ethyl propyl ether, 1,3-dioxolane (DOL), and 2,2-bis(trifluoromethyl)-1,3-dioxolane (TFDOL), or a mixture of two or more of these, but is not limited to these.
[0130] The aforementioned glyme-based solvent is a solvent that has a higher dielectric constant and lower surface tension than linear carbonate-based solvents, and has low reactivity with metals, and may include, but is not limited to, at least one selected from the group consisting of dimethoxyethane (glyme, DME), diethoxyethane, diglyme, triglyme, and tetraglyme (TEGDME).
[0131] The nitrile solvent may be one or more selected from the group consisting of acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonile, cyclohexanecarbonile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile, but is not limited to these.
[0132] On the other hand, the remainder of the non-aqueous electrolyte, excluding the lithium salt and additives, may be an organic solvent unless otherwise specified.
[0133] (3) Additives This invention One embodiment The non-aqueous electrolyte contains additives.
[0134] The aforementioned additive includes at least one compound selected from the group consisting of compounds represented by the following chemical formulas 1 to 3.
[0135] [Chemical formula 1] [ka]
[0136] In the above chemical formula 1, R1 is hydrogen or an alkyl group having 1 to 3 carbon atoms, and n is an integer from 1 to 10.
[0137] [Chemical formula 2] [ka]
[0138] In the above chemical formula 2, m is an integer between 0 and 18.
[0139] [Chemical formula 3] [ka]
[0140] In the above chemical formula 3, R2 and R3 are each independently an alkylene group having 1 to 10 carbon atoms, and R4 is an alkyl group having 1 to 20 carbon atoms substituted with one or more fluorine atoms.
[0141] For example, at least one compound represented by chemical formulas 1 to 3 is the loading amount (450 to 740 mg / 25 cm³). 2 This significantly improves the electrolyte impregnation of the positive electrode, preventing lithium deposition problems at low temperatures, thereby improving the output characteristics of lithium secondary batteries, especially low-temperature output characteristics, and achieving excellent capacity development.
[0142] Furthermore, at least one of the compounds represented by chemical formulas 1 to 3 contains a vinyl group or a propagyl group-containing functional group in its structure, which allows it to be easily reduced and decomposed on the surface of the negative electrode containing a silicon-based active material, forming an SEI film with low resistance and high passivation capacity. Additionally, at least one of the compounds represented by chemical formulas 1 to 3 contains a fluorocarbon functional group with one or more fluorine elements substituted at the ends of its structure, which allows it to form a coating on the surface of the positive electrode with ensured oxidation resistance, suppressing the elution of transition metals from the positive electrode and preventing the electrodeposition and deposition of eluted transition metals on the negative electrode, thereby preventing internal short circuits.
[0143] In the above chemical formula 1, R1 is hydrogen or an alkyl group having 1 to 3 carbon atoms. teyo stomach.
[0144] In the above chemical formula 1, n may be an integer between 1 and 10, and in one embodiment, it may be an integer between 3 and 8. When n is 0, it acts like a non-solvent, making it difficult to effectively form an electrode film containing inorganic components such as LiF. When n is an integer greater than 10, there is a risk that miscibility with organic solvents will decrease.
[0145] The compound represented by chemical formula 1 may include, for example, at least one compound selected from the group consisting of compounds represented by the following chemical formulas 1-1 to 1-3, and in one embodiment, it may include the compound represented by the following chemical formula 1-1.
[0146] [Chemical formula 1-1] [ka]
[0147] [Chemical formula 1-2] [ka]
[0148] [Chemical formula 1-3] [ka]
[0149] In the above chemical formula 2, m may be an integer from 0 to 18, for example, an integer from 1 to 10, or in one embodiment, an integer from 2 to 8.
[0150] When m satisfies the above range, the thermal properties of the compound itself can be improved, and the stability of the resulting film can be expected to be enhanced. In chemical formula 2, if m exceeds 18, an excess amount of fluorine is present, increasing the viscosity and nonpolarity of the material, and decreasing its solubility in the electrolyte. This can lead to a decrease in ionic conductivity and a deterioration of battery performance.
[0151] The compound represented by chemical formula 2 may include at least one compound selected from the group consisting of compounds represented by the following chemical formulas 2-1 to 2-4, and may also include at least one compound selected from the group consisting of compounds represented by chemical formulas 2-1 to 2-2.
[0152] [Chemical formula 2-1] [ka]
[0153] [Chemical formula 2-2] [ka]
[0154] [Chemical formula 2-3] [ka]
[0155] [Chemical formula 2-4] [ka]
[0156] In the above chemical formula 3, R2 and R3 are each independently an alkylene group having 1 to 5 carbon atoms, and R4 may be an alkyl group having 3 to 20 carbon atoms substituted with one or more fluorine atoms.
[0157] Furthermore, in the above chemical formula 3, R2 and R3 are each independently an alkylene group having 1 to 3 carbon atoms, and R4 may be an alkyl group having 3 to 15 carbon atoms substituted with one or more fluorine atoms.
[0158] Alternatively, in the above chemical formula 3, R4 may be an alkyl group having 4 to 8 carbon atoms substituted with one or more fluorine atoms.
[0159] Alternatively, in one embodiment, the compound represented by chemical formula 3 may include the compound represented by the following chemical formula 3-1.
[0160] [Chemical formula 3-1] [ka]
[0161] At least one compound represented by the chemical formulas 1 to 3 is included in the non-aqueous electrolyte in an amount of 0.1% to 3% by weight.
[0162] In one embodiment, at least one compound represented by chemical formulas 1 to 3 may be present in the non-aqueous electrolyte in an amount of about 0.1% to 2.5% by weight, or about 0.2% to 1% by weight.
[0163] On the other hand, the non-aqueous electrolyte may further contain additional additives. If the non-aqueous electrolyte further contains additional additives, at least one compound represented by the above-mentioned chemical formulas 1 to 3 may be referred to as the "first additive," and the additional additive may be referred to as the "second additive."
[0164] The additive may, if necessary, include other additional additives in addition to the compound represented by Chemical Formula 1, in order to prevent the non-aqueous electrolyte from decomposing in a high-power environment and causing the anode to collapse, or to further improve low-temperature high-rate discharge characteristics, high-temperature stability, overcharge prevention, and the effect of suppressing battery swelling at high temperatures.
[0165] Examples of such additional additives include at least one selected from the group consisting of cyclic carbonate compounds, halogen-substituted carbonate compounds, sultone compounds, sulfate compounds, phosphate or phosphite compounds, borate compounds, nitrile compounds, benzene compounds, amine compounds, silane compounds, and lithium salt compounds.
[0166] The cyclic carbonate compound may be, for example, vinylene carbonate (VC) or vinylethylene carbonate.
[0167] The halogen-substituted carbonate compound may be, for example, fluoroethylene carbonate (FEC).
[0168] The sultone compound may be, for example, at least one compound selected from the group consisting of 1,3-propanesultone (PS), 1,4-butanesultone, ethensultone, 1,3-propensultone (PRS), 1,4-butensultone, and 1-methyl-1,3-propensultone.
[0169] The sulfate compound may be, for example, ethylene sulfate (Esa), trimethylene sulfate (TMS), or methyl trimethylene sulfate (MTMS).
[0170] The phosphate or phosphite compound may be, for example, one or more compounds selected from the group consisting of lithium difluoro(bisoxalato) phosphate, lithium difluorophosphate, tris(trimethylsilyl) phosphate, tris(trimethylsilyl) phosphite, tris(2,2,2-trifluoroethyl) phosphate, and tris(trifluoroethyl) phosphite.
[0171] Examples of the borate compounds include tetraphenyl borate, lithium difluoro(oxalato) borate (LiDFOB, LiB(C2O4)F2), or lithium bisoxalate borate (LiB(C2O4)2, LiBOB).
[0172] The nitrile compound may be, for example, at least one compound selected from the group consisting of succinonitrile, adiponitrile, acetonitrile, propionitrile, butyronitrile, valeronitrile, caprylonitrile, heptanenitrile, cyclopentanecarbonile, cyclohexanecarbonile, 2-fluorobenzonitrile, 4-fluorobenzonitrile, difluorobenzonitrile, trifluorobenzonitrile, phenylacetonitrile, 2-fluorophenylacetonitrile, and 4-fluorophenylacetonitrile.
[0173] The benzene-based compound may be, for example, fluorobenzene, the amine-based compound may be triethanolamine or ethylenediamine, and the silane-based compound may be tetravinylsilane.
[0174] The lithium salt compound is a compound different from the lithium salt contained in the non-aqueous electrolyte, and examples include lithium difluorophosphate (LiPO2F2) or LiBF4.
[0175] When the non-aqueous electrolyte contains vinylene carbonate, a stronger SEI film can be formed on the surface of the negative electrode during the initial activation process of the secondary battery.
[0176] The aforementioned additional additive may consist of two or more compounds, and the total content of the compound represented by chemical formula 1 and the additional additive may be approximately 50% by weight or less, or approximately 0.05% to 20% by weight, or approximately 0.05% to 10% by weight, based on the total weight of the non-aqueous electrolyte. When the total content of the additive satisfies the above range, the low-temperature power characteristics of the battery can be improved, the high-temperature storage characteristics and high-temperature life characteristics can be improved more effectively, and the occurrence of side reactions in the battery due to additives remaining after the reaction can be prevented.
[0177] The invention described above One embodiment The lithium secondary batteries described herein can be usefully used in portable devices such as mobile phones, notebook computers, and digital cameras, as well as in the field of electric vehicles such as hybrid electric vehicles (HEVs).
[0178] Accordingly, according to another embodiment of the present invention, a battery module including the lithium secondary battery as a unit cell and a battery pack including the same are provided.
[0179] The aforementioned battery module or battery pack can be used as a power source for one or more medium-to-large devices, including power tools; electric vehicles (EVs), hybrid electric vehicles, and plug-in hybrid electric vehicles (PHEVs); and power storage systems.
[0180] The external shape of the lithium secondary battery of the present invention is not particularly limited, but may be cylindrical, rectangular, pouch-shaped, or coin-shaped, using a can.
[0181] This invention One embodiment The lithium secondary battery described herein can be used not only as a battery cell for powering small devices, but also as a unit battery in medium- and large-sized battery modules containing a large number of battery cells.
[0182] The present invention will be specifically described below with reference to examples.
[0183] In this regard, the embodiments of the present invention can be modified into various other forms, and the scope of the invention should not be construed as being limited to the embodiments detailed below. The embodiments of the present invention are provided to give a more complete explanation of the invention to a person of average skill in the art.
[0184] Examples and Comparative Examples 1. Cathode loading amount: 600 mg / 25 cm 2 Example A-1 (Manufacturing of non-aqueous electrolytes) An organic solvent was prepared by mixing ethylene carbonate (EC), ethyl methyl carbonate (EMC), and dimethyl carbonate (DMC) in a volume ratio of 30:60:10.
[0185] LiPF6 was dissolved in the aforementioned organic solvent to a molar concentration of 1.0 M as a lithium salt.
[0186] Further, vinylene carbonate (VC) and the compound represented by Chemical Formula 1-1 were added to an organic solvent in which the lithium salt was dissolved to prepare a non-aqueous electrolyte. The vinylene carbonate was contained in the non-aqueous electrolyte at a content of 1 wt%. The compound represented by Chemical Formula 1-1 was contained in the non-aqueous electrolyte at a content of 0.2 wt%.
[0187] (Production of Secondary Battery) Lithium iron phosphate oxide (LiFePO4) particles with a carbon coating layer formed thereon as a positive electrode active material, carbon black as a conductive material, and polyvinylidene fluoride (PVDF) as a binder were added at a weight ratio of 94:3:3 to N-methyl-2-pyrrolidone (NMP) as a solvent to prepare a positive electrode slurry. The positive electrode slurry was applied onto a 15 μm thick positive electrode current collector (Al thin film) at 600 mg / 25 cm 2 loading amount, dried, and then roll-pressed to fabricate a positive electrode. The average particle diameter (D 50 ) of the positive electrode active material was 1.1 μm, and the lithium iron phosphate oxide (LiFePO4) particles with the carbon coating layer formed thereon were in the form of primary particles.
[0188] Artificial graphite as a negative electrode active material, SBR-CMC as a binder, and carbon black as a conductive material were added at a weight ratio of 97:2:1 to water as a solvent to prepare a negative electrode slurry. The negative electrode slurry was applied onto a 15 μm thick copper (Cu) thin film as a negative electrode current collector at 300 mg / 25 cm 2 loading amount, dried, and then roll-pressed to fabricate a negative electrode.
[0189] The positive electrode, the polyolefin-based porous separator, and the negative electrode were sequentially stacked to fabricate an electrode assembly.
[0190] After the assembled electrode assembly was accommodated in a battery case, the prepared non-aqueous electrolyte was injected thereto to fabricate a lithium secondary battery.
[0191] Example A-2 A lithium secondary battery was fabricated in the same manner as in Example A-1, except that the compound represented by Chemical Formula 1-1 was contained in the non-aqueous electrolyte at a content of 1 wt%.
[0192] Example A-3 A lithium secondary battery was fabricated in the same manner as in Example A-1, except that the compound represented by Chemical Formula 2-1 was contained in the non-aqueous electrolyte at a content of 0.2 wt% instead of the compound represented by Chemical Formula 1-1.
[0193] Example A-4 A lithium secondary battery was fabricated in the same manner as in Example A-3, except that the compound represented by Chemical Formula 2-1 was contained in the non-aqueous electrolyte at a content of 1 wt%.
[0194] Example A-5 A lithium secondary battery was fabricated in the same manner as in Example A-1, except that the compound represented by Chemical Formula 3-1 was contained in the non-aqueous electrolyte at a content of 0.2 wt% instead of the compound represented by Chemical Formula 1-1.
[0195] Example A-6 A lithium secondary battery was fabricated in the same manner as in Example A-5, except that the compound represented by Chemical Formula 3-1 was contained in the non-aqueous electrolyte at a content of 1 wt%.
[0196] Comparative Example A-1 A lithium secondary battery was fabricated in the same manner as in Example A-1, except that the compound represented by Chemical Formula 1-1 was not contained in the non-aqueous electrolyte.
[0197] Comparative Example A-2 A lithium secondary battery was fabricated in the same manner as in Example A-1, except that the compound represented by Chemical Formula 1-1 was contained in the non-aqueous electrolyte at a content of 0.05 wt%.
[0198] Comparative Example A-3 A lithium secondary battery was manufactured in the same manner as in Example A-1, except that the compound represented by chemical formula 1-1 was included in a non-aqueous electrolyte at a content of 5% by weight.
[0199] Comparative example A-4 A lithium secondary battery was manufactured in the same manner as in Example A-3, except that the compound represented by chemical formula 2-1 was included in the non-aqueous electrolyte at a content of 0.05% by weight.
[0200] Comparative example A-5 A lithium secondary battery was manufactured in the same manner as in Example A-3, except that the compound represented by chemical formula 2-1 was included in a non-aqueous electrolyte at a content of 5% by weight.
[0201] Comparative example A-6 A lithium secondary battery was manufactured in the same manner as in Example A-5, except that the compound represented by chemical formula 3-1 was included in the non-aqueous electrolyte at a content of 0.05% by weight.
[0202] Comparative example A-7 A lithium secondary battery was manufactured in the same manner as in Example A-5, except that the compound represented by chemical formula 3-1 was included in a non-aqueous electrolyte at a content of 5% by weight.
[0203] [Table 1]
[0204] 2. Cathode loading amount: 500 mg / 25 cm 2 Example B-1 The loading amount for the positive electrode is 600 mg / 25 cm. 2 Instead, 500mg / 25cm 2 A lithium secondary battery was manufactured in the same manner as in Example A-1, except that it was adjusted to the specified value.
[0205] Example B-2 A lithium secondary battery was produced in the same manner as in Example B-1, except that the compound represented by the above Chemical Formula 1-1 was contained in the non-aqueous electrolyte at a content of 1% by weight.
[0206] Comparative Example B-1 A lithium secondary battery was produced in the same manner as in Example B-1, except that the compound represented by the above Chemical Formula 1-1 was not contained in the non-aqueous electrolyte.
[0207] Comparative Example B-2 A lithium secondary battery was produced in the same manner as in Example B-1, except that the compound represented by the above Chemical Formula 1-1 was contained in the non-aqueous electrolyte at a content of 0.05% by weight.
[0208] Comparative Example B-3 A lithium secondary battery was produced in the same manner as in Example B-1, except that the compound represented by the above Chemical Formula 1-1 was contained in the non-aqueous electrolyte at a content of 5% by weight.
[0209] [Table 2]
[0210] 3. Positive electrode loading amount: 400 mg / 25 cm 2 Comparative Example C-1 The loading amount of the positive electrode was set to 600 mg / 25 cm 2 not but 400 mg / 25 cm 2 A lithium secondary battery was produced in the same manner as in Example A-2, except that the loading amount was adjusted to the above value.
[0211] Comparative Example C-2 A lithium secondary battery was produced in the same manner as in Comparative Example C-1, except that the compound represented by the above Chemical Formula 1-1 was not contained in the non-aqueous electrolyte.
[0212] [Table 3]
[0213] 4. Cathode loading amount: 750 mg / 25 cm 2 Comparative example D-1 The loading amount for the positive electrode is 600 mg / 25 cm. 2 Instead, 750mg / 25cm 2 A lithium secondary battery was manufactured in the same manner as in Example A-2, except that it was adjusted to the same value.
[0214] Comparative example D-2 A lithium secondary battery was manufactured in the same manner as in Comparative Example D-1, except that the compound represented by chemical formula 1-1 was not included in the non-aqueous electrolyte.
[0215] [Table 4]
[0216] Experimental example Experimental Example 1: Evaluation of Low-Temperature Discharge Capacity The low-temperature discharge capacity of the lithium secondary batteries manufactured as described above (Examples A-1 to A-6, Comparative Examples A-1 to A-7, Examples B-1 to B-2, Comparative Examples B-1 to B-3, Comparative Examples C-1 to C-2, and Comparative Examples D-1 to D-2) was evaluated.
[0217] The aforementioned lithium secondary battery was charged to 3.65V at -10°C under a current of 0.2C, and then discharged to 2.5V at 0.33C to perform initial charge and discharge. The initial discharge capacity (in mAh) at this time was measured.
[0218] Experimental Example 2: Evaluation of Low-Temperature Power Characteristics The low-temperature power characteristics were evaluated for the lithium secondary batteries of the manufactured Examples A-1 to A-6, Comparative Examples A-1 to A-7, Examples B-1 to B-2, Comparative Examples B-1 to B-3, Comparative Examples C-1 to C-2, and Comparative Examples D-1 to D-2.
[0219] The aforementioned lithium secondary battery was charged to 100% SOC (state of charge) at 25°C and 0.33C. The DC-IR (direct current internal resistance) was calculated from the voltage drop observed when a discharge pulse was applied at -10°C and 1.5C. The discharge pulse duration was set to 0.1 seconds or 10 seconds.
[0220] Experimental result 1. Cathode loading amount: 600 mg / 25 cm 2 [Table 5]
[0221] Referring to Table 5 above, the positive electrode active material contains lithium iron phosphate particles, and the positive electrode loading amount is 450-740 mg / 25 cm². 2 The lithium secondary batteries of Examples A-1 to A-6, which include a positive electrode and a non-aqueous electrolyte containing at least one compound represented by Chemical Formulas 1 to 3 in an appropriate content, can be confirmed to exhibit superior capacity development and superior low-temperature output performance compared to Comparative Examples A-1 to A-7.
[0222] The lithium secondary batteries of Comparative Examples A-1 to A-7 not only exhibit lower capacity compared to Examples A-1 to A-6, but also have poor low-temperature power characteristics. For example, Comparative Examples A-2 to A-7 either contain excessively low or excessive amounts of additives, resulting in no improvement in power characteristics compared to Comparative Example A-1, which contains no additives, or even a tendency for the power characteristics to be higher.
[0223] Experimental result 2. Cathode loading amount: 500 mg / 25 cm 2 [Table 6]
[0224] Referring to Table 6 above, the positive electrode active material contains lithium iron phosphate particles, and the positive electrode loading amount is 450-740 mg / 25 cm². 2The lithium secondary batteries of Examples B-1 to B-2, which include a positive electrode and a non-aqueous electrolyte containing at least one compound represented by Chemical Formulas 1 to 3 in an appropriate content, can be confirmed to exhibit superior capacity development and superior low-temperature output performance compared to Comparative Examples B-1 to B-3.
[0225] Experimental result 3. Cathode loading amount: 400 mg / 25 cm 2 [Table 7]
[0226] Referring to Table 7 above, the positive electrode active material contains lithium iron phosphate particles, and the positive electrode loading amount is 450 mg / 25 cm². 2 It can be confirmed that positive electrodes with a value less than 3 show no effect in terms of volume or output, regardless of whether the compounds represented by chemical formulas 1 to 3 are used as non-aqueous electrolyte additives.
[0227] Experimental result 4. Cathode loading amount: 750 mg / 25 cm 2 [Table 8]
[0228] Referring to Table 8 above, the positive electrode active material contains lithium iron phosphate particles, and the positive electrode loading amount is 740 mg / 25 cm². 2 It can be confirmed that positive electrodes exceeding a certain value do not exhibit any effect in terms of volume or output, regardless of whether the compounds represented by chemical formulas 1 to 3 are used as non-aqueous electrolyte additives.
[0229] Although preferred embodiments of the present invention have been described above with reference to the present invention, those skilled in the art or those with ordinary knowledge in the art will understand that the present invention can be modified and altered in various ways without departing from the spirit and art domain set forth in the appended claims.
[0230] Therefore, the technical scope of the present invention is not limited to what is described in the detailed description of the specification, but is determined solely by the claims.
Claims
1. It includes a positive electrode, a negative electrode, a separator, and a non-aqueous electrolyte. The positive electrode includes a positive electrode active material. The positive electrode active material contains lithium iron phosphorus oxide particles, The loading amount for the aforementioned positive electrode is 450 mg / 25 cm². 2 ~740mg / 25cm 2 And, The non-aqueous electrolyte comprises a lithium salt, an organic solvent, and an additive. The aforementioned additive includes at least one compound selected from the group consisting of compounds represented by the following chemical formulas 1 to 3: A lithium secondary battery in which the additive is contained in the non-aqueous electrolyte in an amount of 0.1% to 3% by weight. [Chemical formula 1] 【Chemistry 1】 (In the above chemical formula 1, R 1 n is a hydrogen atom or an alkyl group having 1 to 3 carbon atoms, and n is an integer from 1 to 10. [Chemical formula 2] 【Chemistry 2】 In the above chemical formula 2, m is an integer between 0 and 18. [Chemical formula 3] 【Transformation 3】 In the above chemical formula 3, R 2 and R 3 Each of these is an alkylene group having 1 to 10 carbon atoms, and R 4 (This refers to an alkyl group having 1 to 20 carbon atoms substituted with one or more fluorine atoms.)
2. The lithium secondary battery according to claim 1, wherein n in the chemical formula 1 is an integer from 3 to 8.
3. In the above chemical formula 1, R 1 A lithium secondary battery according to claim 1, wherein the hydrogen is hydrogen.
4. The lithium secondary battery according to claim 1, wherein the compound represented by chemical formula 1 includes at least one selected from the group consisting of compounds represented by the following chemical formulas 1-1 to 1-3. [Chemical formula 1-1] 【Chemistry 4】 [Chemical formula 1-2] 【Transformation 5】 [Chemical formula 1-3] 【Transformation 6】
5. The lithium secondary battery according to claim 1, wherein m in the chemical formula 2 is an integer from 2 to 8.
6. The lithium secondary battery according to claim 1, wherein the compound represented by chemical formula 2 includes at least one selected from the group consisting of compounds represented by the following chemical formulas 2-1 to 2-4. [Chemical formula 2-1] 【Transformation 7】 [Chemical formula 2-2] 【Transformation 8】 [Chemical formula 2-3] 【Chemistry 9】 [Chemical formula 2-4] 【Chemistry 10】
7. In the above Chemical Formula 3, R 2 and R 3 are each independently an alkylene group having 1 to 5 carbon atoms, and R 4 is an alkyl group having 3 to 20 carbon atoms substituted with one or more fluorine atoms, the lithium secondary battery according to claim 1.
8. In the above chemical formula 3, R 4 The lithium secondary battery according to claim 1, wherein the alkyl group having 4 to 8 carbon atoms is substituted with one or more fluorine atoms.
9. The lithium secondary battery according to claim 1, wherein the compound represented by chemical formula 3 includes the compound represented by the following chemical formula 3-1. [Chemical formula 3-1] 【Chemistry 11】
10. The loading amount of the aforementioned positive electrode is 500 mg / 25 cm². 2 ~600mg / 25cm 2 The lithium secondary battery according to claim 1.
11. The lithium secondary battery according to claim 1, wherein the non-aqueous electrolyte further comprises vinylene carbonate.
12. The lithium secondary battery according to claim 1, wherein the organic solvent comprises a cyclic carbonate solvent and a linear carbonate solvent.
13. The lithium secondary battery according to claim 12, wherein the linear carbonate comprises dimethyl carbonate.
14. The lithium secondary battery according to claim 1, wherein the lithium iron phosphorus particles include a compound represented by the following chemical formula A. [Chemical formula A] Li 1+a Fe 1-s M s (PO 4-b )X b (In the above chemical formula A, M is one or more elements selected from Co, Ni, Mn, Al, Mg, Ti, and V, and X is F, S, or N, with 0 ≤ s ≤ 0.5; -0.5 ≤ a ≤ +0.5; 0 ≤ b ≤ 0.1.)
15. The lithium iron phosphate particles are LiFePO 4 A lithium secondary battery according to claim 1, comprising: