Method for forming a memory device within a concave feature

Low-temperature atomic layer deposition methods prevent premature crystallization of transition metal oxide layers, enabling the formation of ferroelectric and antiferroelectric films with controlled crystallization for improved memory device performance in high aspect ratio structures.

JP2026539143APending Publication Date: 2026-11-20TOKYO ELECTRON LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026524488
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2024-08-27
Filing Date
2024-08-29
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Current semiconductor manufacturing processes face challenges in forming ferroelectric and antiferroelectric films within deep aspect ratio structures due to premature crystallization of hafnium-zirconium oxide layers during atomic layer deposition, which hinders the development of optimal ferroelectric properties in high aspect ratio features.

Method used

A method involving low-temperature atomic layer deposition processes is employed to form memory devices, maintaining the amorphous state of transition metal oxide layers until a controlled crystallization step, using specific substrate temperatures and gas mixtures to prevent premature crystallization and ensure uniform deposition within high aspect ratio features.

Benefits of technology

This approach enables the formation of ferroelectric and antiferroelectric films with stable and controllable properties, allowing for precise control over the crystalline phase and electrical properties of memory devices, ensuring consistent performance across the structure.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539143000001_ABST
    Figure 2026539143000001_ABST
Patent Text Reader

Abstract

A method for forming a memory device on a substrate includes depositing a first electrode layer in a concave feature of the substrate using a first atomic layer deposition process, and depositing an amorphous transition metal oxide layer on top of the first electrode layer using a second atomic layer deposition process at a first substrate temperature. The method further includes depositing a second electrode layer on top of the amorphous transition metal oxide layer using a third atomic layer deposition process at a second substrate temperature while maintaining the amorphous state of the amorphous transition metal oxide layer, wherein the second substrate temperature is lower than the recrystallization temperature of the amorphous transition metal oxide material of the amorphous transition metal oxide layer, and the first electrode layer, the amorphous transition metal oxide layer, and the second electrode layer are deposited to form a memory layer stack.
Need to check novelty before this filing date? Find Prior Art

Description

TECHNICAL FIELD

[0001] CROSS-REFERENCE TO RELATED APPLICATIONS This application claims the benefit of U.S. Provisional Patent Application No. 63 / 546,141 filed on October 27, 2023 and U.S. Non-Provisional Patent Application No. 18 / 816,978 filed on August 27, 2024, and these applications are incorporated herein by reference in their entirety.

[0002] The present invention relates to semiconductor processing and semiconductor devices, and more particularly to a method of forming a memory device within a recessed feature. BACKGROUND ART

[0003] In the semiconductor industry, the integration of non-volatile memory technology, sensor technology, transmitter technology, electronic filter technology, receiver technology and the like can be useful for various types of devices and applications. According to various aspects, electronic devices, such as non-volatile memories, can be integrated on a chip. The demand for film stacks including dielectric materials that are ferroelectric (FE) and antiferroelectric (AFE) includes good control over the crystalline phases in advanced 3D structures. SUMMARY OF THE INVENTION MEANS FOR SOLVING THE PROBLEMS

[0004] According to one embodiment of the present disclosure, a method for forming a memory device on a substrate includes the steps of: depositing a first electrode layer in a concave feature of the substrate using a first atomic layer deposition process; and depositing an amorphous transition metal oxide layer on the first electrode layer using a second atomic layer deposition process at a first substrate temperature. The method further includes the step of depositing a second electrode layer on the amorphous transition metal oxide layer using a third atomic layer deposition process at a second substrate temperature while maintaining the amorphous state of the amorphous transition metal oxide layer, wherein the second substrate temperature is lower than the recrystallization temperature of the amorphous transition metal oxide material of the amorphous transition metal oxide layer, and the first electrode layer, the amorphous transition metal oxide layer, and the second electrode layer form a memory layer stack.

[0005] According to another embodiment of the present disclosure, a method for forming a memory device on a substrate includes the steps of loading the substrate into a first atomic layer deposition (ALD) chamber of an ALD system, and performing a first ALD process, which includes flowing a first metal precursor gas to deposit a first electrode layer in a high aspect ratio opening of the substrate. The method further includes the steps of loading the substrate into a second ALD chamber of an ALD system, and performing a second ALD process, which includes flowing a gas mixture containing tetrakis(ethylmethylamino)hafnium (TEMAHf), tetrakis(ethylmethylamino)zirconium (TEMAZr), and an oxidizing agent to deposit an amorphous transition metal oxide layer on top of the first electrode layer. The method further includes the steps of loading a substrate into a third atomic layer deposition (ALD) chamber of an ALD system and maintaining the substrate at a temperature below the amorphous-crystal temperature of the amorphous transition metal oxide layer, and carrying out a third ALD process, wherein a second metal precursor gas is flowed through the substrate while maintaining the substrate at the above temperature to deposit a second electrode layer, the first electrode layer, the amorphous transition metal oxide layer, and the second electrode layer form a memory layer stack.

[0006] Furthermore, according to yet another embodiment of the present disclosure, a method for forming a memory device on a substrate includes the steps of: depositing a first electrode layer in a concave feature of the substrate using a first atomic layer deposition process; and depositing an amorphous transition metal oxide layer on the first electrode layer using a second atomic layer deposition process at a first substrate temperature. The method further includes the step of depositing a second electrode layer on the amorphous transition metal oxide layer using a third atomic layer deposition process at a second substrate temperature. The method further includes the step of annealing the substrate at a third substrate temperature to crystallize the amorphous transition metal oxide layer and form a crystalline transition metal oxide layer, wherein the crystalline transition metal oxide layer has a ferroelectric crystalline phase or an antiferroelectric crystalline phase.

[0007] To fully understand the present invention and its advantages, refer hereto to the following description, which should be read in conjunction with the accompanying drawings. [Brief explanation of the drawing]

[0008] [Figure 1A] This is a cross-sectional view of a structure illustrating various steps in a method for forming a memory device within a high aspect ratio feature according to one embodiment of the present disclosure. [Figure 1B] This is a cross-sectional view of a structure illustrating various steps in a method for forming a memory device within a high aspect ratio feature according to one embodiment of the present disclosure. [Figure 1C] This is a cross-sectional view of a structure illustrating various steps in a method for forming a memory device within a high aspect ratio feature according to one embodiment of the present disclosure. [Figure 1D] This is a cross-sectional view of a structure illustrating various steps in a method for forming a memory device within a high aspect ratio feature according to one embodiment of the present disclosure. [Figure 2] This is a cross-sectional view of a structure showing an annealing step according to one embodiment of the present disclosure. [Figure 3] This is a schematic diagram of an atomic layer deposition (ALD) system according to one embodiment of the present disclosure. [Figure 4]This figure shows a plot of X-ray diffraction (XRD) results of a hafnium zirconium oxide (HZO) film deposited using an ALD process at high temperature according to one embodiment of the present disclosure. [Figure 5] This figure shows a plot illustrating the XRD results of an HZO film deposited using a low-temperature ALD process according to one embodiment of the present disclosure. [Figure 6] This is a flowchart of a method for forming a memory device within a high aspect ratio feature according to one embodiment of the present disclosure. [Figure 7] This is a flowchart of a method for forming a memory device within a high aspect ratio feature according to one embodiment of the present disclosure. [Figure 8] This is a flowchart of a method for forming a memory device within a high aspect ratio feature according to one embodiment of the present disclosure. [Modes for carrying out the invention]

[0009] The formation of ferroelectric (FE) and antiferroelectric (AFE) films within deep aspect ratio structures presents challenges in semiconductor manufacturing. Current processes using atomic layer deposition (ALD) of titanium nitride (TiN) as a capping layer at 430°C result in undesirable premature crystallization of the hafnium-zirconium oxide (HZO) layer (or other amorphous transition metal oxide layer). This premature crystallization hinders the development of optimal ferroelectric properties in high aspect ratio features. Additionally, controlling the oxygen content of the TiN layer (or other electrode layer) is beneficial for maximizing ferroelectric properties.

[0010] This disclosure presents a method for forming a memory device within a high aspect ratio feature, enabling stable and controllable ferroelectric properties in the transition metal oxide layer of the memory device. The methods of the embodiments described throughout this disclosure employ a series of low-temperature ALD processes incorporated into the formation of a ferroelectric stack. The low temperatures used in the ALD process prevent premature crystallization of the amorphous transition metal oxide layer of the memory device (such as a memory capacitor). The low-temperature ALD process is useful for preventing premature crystallization of the amorphous transition metal oxide layer and maintaining it in an amorphous state until the intended annealing step. Furthermore, the second electrode layer may be designed to contain approximately 20% oxygen, which is beneficial for achieving maximum ferroelectric properties. This low-temperature all-ALD method enables the formation of ferroelectric and antiferroelectric films within a high aspect ratio structure.

[0011] The embodiments provided below describe various methods and systems for forming memory devices, in particular, methods and systems using low-temperature atomic layer deposition to form memory devices within high-aspect-ratio features. The embodiments are described below. Figures 1A–1D are used to illustrate various steps for forming memory devices within high-aspect-ratio features on an exemplary substrate. Figure 2 is used to illustrate an annealing step that may be performed after the methods described using Figures 1A–1D. Figure 3 shows an exemplary atomic layer deposition system that may be used to perform the steps described using Figures 1A–1D. Figure 4 illustrates an X-ray diffraction (XRD) plot showing early crystallization of a hafnium zirconium oxide (HZO) layer deposited using an ALD process at a substrate temperature of 430°C. Figure 5 illustrates an XRD plot showing an HZO layer that maintains an amorphous state using an ALD process at a substrate temperature of 330°C. Figures 6–8 are flowcharts used to illustrate three other exemplary embodiments of the methods for forming memory devices within high-aspect-ratio features of the present disclosure.

[0012] Figures 1A to 1D show cross-sectional views of structure 100 through various steps of the method for forming a memory device within high aspect ratio (HAR) features of the present disclosure. The various figures of structure 100 show only a portion of the substrate to highlight the method of the present disclosure. However, the method of the present disclosure can be applied over an entire substrate or wafer, such as over an entire substrate containing many HAR features. Furthermore, the method of the present disclosure can be initiated after receiving a substrate containing pre-formed HAR features (or openings), such as structure 100 shown in Figure 1A.

[0013] Figure 1A shows structure 100 after an etching process has formed a recessed feature 110 in the substrate portion 102 of structure 100. The recessed feature 110 can be formed by any suitable etching process known in the art for forming HAR features, and the recessed feature 110 may be a HAR feature (or opening). For example, the recessed feature 110 may be a trench or a hole. In various embodiments, the recessed feature 110 is part of a three-dimensional structure within the substrate portion 102.

[0014] Structure 100 includes a substrate portion 102 having a concave feature 110. The substrate portion 102 can be made of various materials suitable for semiconductor device manufacturing, such as silicon, silicon-on-insulator (SOI), germanium, III-V compound semiconductors, or other suitable substrates. In some embodiments, the substrate portion 102 may be a bulk semiconductor substrate, and in other embodiments, it may be a layer in a more complex material stack.

[0015] The recessed feature 110 is formed within the substrate portion 102 and serves as a foundation for the memory device. This recessed feature 110 can take various forms depending on the specific device architecture. In some embodiments, the recessed feature 110 may be a trench with vertical or inclined sidewalls. In other embodiments, the recessed feature 110 may be a cylindrical hole or a more complex three-dimensional structure.

[0016] In various embodiments, the recessed feature 110 has a high aspect ratio. The aspect ratio of the recessed feature 110 may vary depending on the specific device being fabricated. In some embodiments, the aspect ratio may be greater than 5:1, while for more aggressive designs, the aspect ratio may exceed 20:1 or even 50:1. In various embodiments, the recessed feature 110 may comprise a high aspect ratio between about 40:1 and 10:1.

[0017] The dimensions of the recessed feature 110 may vary significantly based on the intended application and the level of device scaling. In some embodiments, the critical dimension (CD) of the recessed feature 110 may be in the range of several nanometers to hundreds of nanometers. The depth of the recessed feature 110 may be in the range of tens of nanometers to several micrometers, depending on the desired capacitance and other device parameters.

[0018] In various embodiments, the sidewalls and bottom of the recessed feature 110 may be treated or modified prior to subsequent deposition steps. For example, they may be subjected to a cleaning process, a surface treatment to enhance adhesion, or the formation of additional layers not shown in Figure 1A.

[0019] With continued reference to Figure 1A, the structure 100 at this stage serves as a starting point for subsequent deposition steps that will form memory devices within the recessed features 110. An atomic layer deposition (ALD) process, such as the first ALD process described with reference to Figure 1B, may be used on the structure 100 of Figure 1A to deposit various layers of the memory device within the recessed feature 110 such that the various layers are uniform and conformal.

[0020] FIG. 1B shows the structure 100 after performing a first ALD process to deposit a first material within the recessed feature 110 to form the first electrode layer 104. The first ALD process may be a conventional ALD process suitable for forming the first electrode layer within the recessed feature 110. For example, the first ALD process may include a first precursor gas exposure that adsorbs on the surface of the structure 100. The first ALD process may then use a first purge gas to purge excess first precursor gas and any byproducts, where the first purge gas is an inert gas. Thereafter, the first ALD process may expose the structure 100 to a first reactant gas to react with the adsorbed first precursor gas, forming a first monolayer of the desired material to form the first electrode layer 104. Subsequent steps include performing another purge step, then repeating the above-described steps until the desired thickness for the deposited layer is achieved. Conventional temperatures for the structure 100 may be used during the first ALD process.

[0021] The first electrode layer 104 is deposited using the first atomic layer deposition (ALD) process described above, which enables conformal coating along the sidewalls and bottom of the high aspect ratio recessed feature 110. This conformal coating is beneficial for ensuring uniform electrical characteristics across the entire device.

[0022] In various embodiments, the first electrode layer 104 may comprise a conductive material suitable for use as an electrode in a memory device. Materials that may be used for the first electrode layer 104 include titanium nitride, tantalum nitride, tungsten, ruthenium, or other transition metals, and compounds thereof. The selection of a specific material depends on factors such as conductivity, work function, and compatibility with subsequent processing steps.

[0023] The thickness of the first electrode layer 104 is precisely controlled by the first ALD process. Typical thicknesses may be in the range of 2 to 20 nanometers, but thicker or thinner layers may be employed depending on the specific device specifications. Furthermore, the number of cycles of the first ALD process passing through the first precursor gas, the first reactant gas, and the first purge gas determines the thickness of the first electrode layer 104. The ability to deposit conformal ultrathin layers with high uniformity within concave features 110 is an advantage of the ALD technique in this disclosure.

[0024] The first electrode layer 104 is deposited at a controlled temperature selected to optimize film properties while maintaining compatibility with the substrate and subsequent processing steps. This temperature is typically in the range of 200°C to 500°C, but in some embodiments, lower or higher temperatures may be used.

[0025] The first ALD process for depositing the first electrode layer 104 includes alternating pulses of a precursor gas and a reactant gas, with a purge step between each pulse. For example, in the case of titanium nitride, the process may be carried out alternately between a titanium-containing precursor and a nitrogen-containing reactant. The specific precursor, pulse time, and purge time can be optimized to achieve the desired film properties and deposition rate. Furthermore, the first ALD process ensures that the layer thickness remains constant from the top to the bottom of the concave feature 110, avoiding potential difficulties such as pinch-off or void formation that may occur with other deposition techniques.

[0026] In various embodiments, the first precursor gas of the first ALD process may include TiCl4 or tetrakis(dimethylamino)titanium (TDMAT). In similar embodiments, the first reactant gas may include NH3 (or the deuterated version ND3) or N2H4. The first purge gas may be a suitable inert gas such as argon (Ar) or nitrogen (N2).

[0027] By utilizing a first ALD process for the deposition of the first electrode layer 104, this method establishes a foundation for subsequent layers of the memory device, ensuring excellent coverage and precise thickness control within the difficult-to-process geometry of high-aspect-ratio concave features 110.

[0028] Figure 1C shows the structure 100 after depositing an appropriate material within the concave features 110 on the first electrode layer 104 to form an amorphous transition metal oxide layer 106.

[0029] The amorphous transition metal oxide layer 106 is deposited using a second ALD process at a first substrate temperature. The first substrate temperature is selected to be low enough to prevent crystallization of the transition metal oxide material. The first substrate temperature ensures that the amorphous transition metal oxide layer 106 remains in an amorphous state.

[0030] Various transition metal oxides can be used for the amorphous transition metal oxide layer 106, each offering distinct properties suitable for different memory applications. In various embodiments, the amorphous transition metal oxide layer 106 includes hafnium oxide (HfO2), zirconium oxide (ZrO2), hafnium-zirconium oxide (HfZrO2), titanium oxide (TiO2), tantalum oxide (Ta2O5), and niobium oxide (Nb2O5). The composition of the amorphous transition metal oxide layer 106 can be adjusted by controlling the ratios of various precursors during the second ALD process. For example, in the case of hafnium-zirconium oxide, the ratio of hafnium to zirconium can be precisely controlled to optimize the electrical properties of the resulting amorphous transition metal oxide layer 106. In other embodiments, the amorphous transition metal oxide layer 106 includes high-k oxides such as HfZrO, or HfZrO doped with La or Nb.

[0031] In various embodiments, the thickness of the amorphous transition metal oxide layer 106 may be in the range of 3 to 15 nanometers, but thicker or thinner layers may also be employed depending on the specific device specifications and the desired electrical characteristics of the manufactured memory device, such as capacitance.

[0032] The first substrate temperature for depositing the amorphous transition metal oxide layer 106 is determined to maintain the amorphous state. In various embodiments, the first substrate temperature can be between 300°C and 350°C, and the exact value depends on the specific material of the structure 100 and the desired properties. For example, in embodiments where the amorphous transition metal oxide layer is amorphous hafnium zirconium oxide, the first substrate temperature may be 330°C.

[0033] A second ALD process for amorphous transition metal oxide layer 106 involves alternating pulses of a metal precursor and an oxygen-containing reactant, with a purge step between each pulse. The difference between the second ALD process and the first ALD process lies in the precursor gas, reactant gas, and the temperature maintained during the corresponding ALD process. For example, the deposition of hafnium oxide can be carried out alternately between a hafnium-containing precursor (such as tetrakis(ethylmethylamino)hafnium) and an oxygen-containing reactant (such as water or ozone).

[0034] As an example, the second ALD process can carry out the same steps as described for the first ALD process, but using a second precursor gas, a second reactant gas, and a second purge gas. Furthermore, the second ALD process is carried out at a first substrate temperature below the amorphous-crystallization temperature (or recrystallization temperature) of the amorphous transition metal oxide material of the amorphous transition metal oxide layer 106.

[0035] In various embodiments, the second precursor gas of the second ALD process may include a metal-organic compound such as tetrakis(ethylmethylamino)hafnium (TEMAHf), tetrakis(ethylmethylamino)zirconium (TEMAZr), tris(dimethylamide)cyclopentadienylhafnium (Hy-ALD), or tris(dimethylamino)cyclopentadienylzirconium (ZY-ALD). In similar embodiments, the second reactant gas may include an oxidizing agent such as ozone, water, deuterated water (D2O), or oxygen. The second purge gas may be any suitable inert gas, similar to those described for the first purge gas above.

[0036] By maintaining the amorphous state of the amorphous transition metal oxide layer 106 at this stage, a memory device with improved ferroelectric or antiferroelectric properties can be formed through a subsequent controlled crystallization process. The amorphous structure allows for greater flexibility in the manipulation of the final crystalline phase, which directly affects the electrical properties of the memory device.

[0037] The conformal nature of the second ALD process ensures that the amorphous transition metal oxide layer 106 maintains a constant thickness throughout the high-aspect-ratio concave features 110, which enables uniform device performance throughout the structure 100.

[0038] Figure 1D shows the structure 100 after a second electrode layer 108 has been formed by depositing another suitable material within the recessed feature 110 and on top of the amorphous transition metal oxide layer 106 at a second substrate temperature. In various embodiments, the second electrode layer 108 may function as a capping layer for a memory device formed within the recessed feature 110.

[0039] The second electrode layer 108 is deposited using a third atomic layer deposition (ALD) process at a second substrate temperature. The second substrate temperature is carefully selected to be low enough to prevent crystallization of the underlying amorphous transition metal oxide layer 106. The third ALD process can also perform the same ALD steps as described for the first or second ALD process, but using a second substrate temperature, a third precursor gas, a third reactant gas, and a third purge gas suitable for the material of the second electrode layer 108.

[0040] The second electrode layer 108 may include a variety of conductive materials suitable for use as the upper electrode (or capping layer) in a memory device. Possible materials include titanium nitride (TiN), tantalum nitride (TaN), tungsten (W), ruthenium (Ru), platinum (Pt), iridium (Ir), and conductive metal oxides (e.g., indium tin oxide). The selection of the material for the second electrode layer 108 depends on factors such as the work function, compatibility with the underlying transition metal oxide, and subsequent processing specifications.

[0041] The thickness of the second electrode layer 108 is typically in the range of 2 to 20 nanometers, but this can vary depending on the specific device design and performance targets. Here again, the thickness of the second electrode layer 108 can be determined by the number of cycles of the third ALD process.

[0042] The temperature of the second substrate for depositing the second electrode layer 108 is low enough to prevent crystallization of the amorphous transition metal oxide layer 106. The temperature of the second substrate is generally maintained between 200°C and 350°C, depending on the specific electrode material and the crystallization temperature of the underlying amorphous transition metal oxide layer 106. This temperature is kept low enough to be below the amorphous-crystallization temperature (or recrystallization temperature) of the amorphous transition metal oxide layer 106.

[0043] The third ALD process for the second electrode layer 108 includes alternating pulses of a precursor gas, a reactant gas, and a third purge gas specific to the selected electrode material. For example, in the case of titanium nitride, the process may be carried out alternately between a titanium-containing precursor (such as tetrakis(dimethylamino)titanium) and a nitrogen-containing reactant (such as ammonia). Here again, the third ALD process may be similar to those described for the first and second ALD processes, but using a second substrate temperature, a third precursor gas, a third reactant gas, and a third purge gas. In some embodiments, the third ALD process may be the same as the first ALD process, both of which use a second substrate temperature to deposit the first electrode layer 104 and the second electrode layer 108 of the same material.

[0044] In various embodiments, the third precursor gas of the third ALD process may include TiCl4 or tetrakis(dimethylamino)titanium (TDMAT). In similar embodiments, the third reactant gas may include NH3 (or the deuterated version ND3) or N2H4. The third purge gas may be any suitable inert gas, such as argon (Ar) or nitrogen (N2), as described above for the first or second purge gas.

[0045] In some embodiments, the second electrode layer 108 may be designed to have a specific amount of oxygen. For example, when using titanium nitride, the process may be adjusted to incorporate about 18–22 atomic percent oxygen into the second electrode layer 108. This oxygen content plays a role in the subsequent crystallization of the amorphous transition metal oxide layer 106 and may affect the final electrical properties of the device (or structure 100).

[0046] The conformal nature of the third ALD process ensures that the second electrode layer 108 maintains a constant thickness and composition throughout the high-aspect-ratio concave features 110. This uniformity also enables consistent electrical performance throughout the structure 100.

[0047] By depositing the second electrode layer 108 at a carefully controlled low temperature (second substrate temperature), this method preserves the amorphous state of the underlying amorphous transition metal oxide layer 106, preparing it for a subsequent controlled crystallization step that defines the final electrical properties of the memory device. In various embodiments, the first substrate temperature may be higher than the second substrate temperature. In other embodiments, the first substrate temperature may be lower than the second substrate temperature. In yet another embodiment, the first substrate temperature may be the same as the second substrate temperature. The second substrate temperature is selected so as not to cause premature crystallization of the amorphous transition metal oxide layer 106 by the second electrode layer 108.

[0048] The resulting structure 100 comprises a memory layer stack formed within the concave feature 110. The memory layer stack comprises a first electrode layer 104, an amorphous transition metal oxide layer 106, and a second electrode layer 108. This memory layer stack forms the foundation for the memory device, and a controlled deposition temperature allows for precise control of the amorphous state of the amorphous transition metal oxide layer 106. The deposition process described using Figures 1A-1E also deposits layers on the upper surface (or field region) surrounding the concave feature 110. In various embodiments, after depositing various layers and the second electrode layer 108, a planarization process, such as a chemical mechanical planarization (CMP) process, can be performed to remove the material deposited on the upper surface. Furthermore, Figure 1E may show structure 100 after the second electrode layer 108 has been deposited and the planarization process has been performed. In various embodiments, an annealing process may be performed after the completion of the deposition of the second electrode layer 108, as described below with reference to Figure 2.

[0049] Figure 2 shows the structure 100 after the annealing process has been performed, converting the previously amorphous transition metal oxide layer 106 into a crystalline transition metal oxide layer 112.

[0050] The annealing process is carried out at a third substrate temperature higher than the second substrate temperature used to deposit the second electrode layer 108. This high temperature provides recrystallization energy, inducing crystallization in the amorphous transition metal oxide material.

[0051] The third substrate temperature is typically in the range of 350°C to 600°C, depending on the specific composition of the amorphous transition metal oxide and the desired crystalline phase. The duration of the annealing process can vary from a few seconds to several minutes, balancing the desire for complete crystallization with consideration of the thermal budget.

[0052] During the annealing process, the amorphous transition metal oxide layer 106 undergoes a phase transition and forms a crystalline structure. The resulting crystalline transition metal oxide layer 112 may exhibit different crystalline phases depending on the annealing conditions and the composition of the original amorphous layer. Furthermore, the oxygen content of the second electrode layer 108 can further assist in the formation of the desired crystalline phase of the crystalline transition metal oxide layer 112. For example, in the case of hafnium zirconium oxide, the crystalline phase may be ferroelectric or antiferroelectric, depending on the specific processing conditions and composition.

[0053] The crystallization process can significantly alter the electrical properties of the crystalline transition metal oxide layer 112. In the ferroelectric phase, the material exhibits spontaneous electric polarization that can be reversed by an applied electric field, forming the basis for non-volatile memory operation.

[0054] The controlled crystallization made possible by this method allows for precise design of the crystal structure, which directly affects the performance characteristics of the memory device, such as polarization, coercivity, and retention. Furthermore, the memory layer stack comprises, here, a first electrode layer 104, a crystalline transition metal oxide layer 112, and a second electrode layer 108. In various embodiments, the memory layer stack can be used to form a memory capacitor.

[0055] Additionally, the crystallization process can affect surrounding layers. For example, oxygen from the transition metal oxide layer can diffuse into adjacent electrode layers, particularly the second electrode layer 108. This oxygen diffusion can affect the electrical properties of the electrode and the overall device performance.

[0056] The high aspect ratio of the concave features 110 presents a challenge to uniform thermal distribution during the annealing process. However, the conformal nature of the pre-deposited layers helps ensure consistent crystallization throughout the structure 100, which is an advantage of the method of this disclosure over conventional methods for forming memory devices.

[0057] By carefully controlling the annealing conditions, this step completes the formation of active memory elements within a high aspect ratio structure, creating a functional device with desired crystalline properties for memory applications. In various embodiments, after performing the annealing process described with reference to Figure 2, the concave features 110 may be overfilled with material, and a planarization process may be performed to remove the excess material from the concave features 110. For example, a chemical polymerization (CMP) process may be performed after annealing to remove excess material from the concave features 110 and prevent CMP residue from accumulating within the concave features 110. Using Figure 3, an atomic layer deposition (ALD) system 300 capable of depositing various layers of a memory device formed within the concave features 110 of Figures 1A-1D is described.

[0058] Figure 3 shows a schematic diagram of the ALD system 300 capable of performing the methods described in Figures 1A to 1D for forming a memory device within a high aspect ratio structure.

[0059] The ALD system 300 includes a processing chamber 310 that houses a substrate holder 320. The substrate holder 320 may be designed to accommodate various substrate sizes and may include a heating element for temperature control. In some embodiments, the substrate holder 320 may also have a rotation function to improve deposition uniformity.

[0060] The upper assembly 330 is positioned above the substrate holder 320 and includes a gas inlet 332 for introducing precursor and reactant gases into the chamber. The upper assembly 330 may be designed to facilitate uniform gas distribution across the substrate surface.

[0061] A gas system 340 is connected to the processing chamber 310 and supplies various gases for the ALD process, whether it be a first, second, or third ALD process. The gas system 340 provides a first processing gas 342, a second processing gas 344, and a carrier gas 346. These gases can be precisely controlled and introduced into the chamber as defined by a specific ALD recipe. For example, the first processing gas 342 may be a first, second, or third precursor gas in various embodiments. The second processing gas 344 may be a first, second, or third reactant gas in various embodiments. The carrier gas 346 may be a first, second, or third purge gas in various embodiments. The gas system 340 may be designed to accommodate any of the first, second, or third ALD processes performed in the processing chamber 310.

[0062] In some embodiments, the ALD system 300 may comprise a plurality of processing chambers 310 having similar elements but used for different ALD processes of this disclosure. For example, the ALD system 300 may comprise three processing chambers 310, where, as described above, a first processing chamber may be used for a first ALD process, a second processing chamber for a second ALD process, and a third processing chamber for a third ALD process.

[0063] When depositing the amorphous transition metal oxide layer 106, the first treatment gas 342 may be a metal precursor such as tetrakis(ethylmethylamino)hafnium for hafnium oxide, and the second treatment gas 344 may be an oxygen source such as water or ozone.

[0064] The carrier gas 346 may be an inert gas such as argon or nitrogen, used to purge the chamber between precursor pulses and assist in precursor delivery.

[0065] The temperature control system 350 regulates the temperature within the processing chamber 310. This system may include heating elements, a cooling system, and temperature sensors to maintain precise temperature control throughout all stages of the deposition process. For example, the temperature control system 350 can be used to maintain a first substrate temperature or a second substrate temperature depending on the ALD process being carried out within the processing chamber 310.

[0066] The substrate power supply 360 is coupled to the substrate holder 320. This power supply may be used for the plasma-enhanced ALD process or for substrate biasing to affect film properties.

[0067] To maintain an appropriate pressure level, the vacuum pump 370 is connected to the processing chamber 310 via a valve 372. This configuration enables precise pressure control throughout the deposition process, typically maintaining the pressure within the range of 0.1 to 10 Torr.

[0068] The ALD system 300 is managed by a controller 380 that adjusts various components and process parameters. The controller 380 may be a microprocessor-based system capable of executing pre-programmed instructions.

[0069] The controller 380 is coupled to a memory 385 that stores a process recipe, parameters, and control program for executing a desired deposition sequence. The memory 385 may include various types of storage media such as RAM, ROM, or magnetic disks or optical disks.

[0070] The configuration of this ALD system 300 enables carefully controlled layer-by-layer deposition, which is desirable for forming memory device structures within high aspect ratio features. The ability to precisely control gas flow, temperature, and pressure is beneficial in maintaining the amorphous state of the transition metal oxide layer during initial deposition, and enables subsequent crystallization during the annealing process.

[0071] Figure 4 shows the first plot 400, which illustrates the X-ray diffraction (XRD) results for a hafnium zirconium oxide (HZO) film deposited using the ALD process at high temperature. This plot shows undesirable premature crystallization of the HZO film during the ALD process, which can be highlighted by peak 410, corresponding to the premature crystallization of the HZO layer.

[0072] The X-axis of the plot typically represents the diffraction angle (2θ) within the range of 20° to 45°. The Y-axis shows the intensity of the diffracted X-rays, measured in counts.

[0073] In the first plot 400, prominent peaks are observed at specific diffraction angles (e.g., peak 410), indicating the presence of a crystalline phase within the HZO film. These peaks correspond to various crystal planes of the HZO material. The presence of these peaks demonstrates that crystallization occurred during the deposition process rather than maintaining the desired amorphous state.

[0074] The premature crystallization observed in the first plot 400 is undesirable for the method described in Figures 1A-1D because it reduces control over the final crystal structure and can result in non-uniform electrical properties in the resulting memory device. Consequently, the use of a low-temperature ALD process can prevent premature crystallization of the transition metal oxide layer, as shown in the second plot 500 in Figure 5.

[0075] Figure 5 shows a second plot 500 showing the XRD results of an HZO film deposited using the low-temperature ALD process described herein (specifically at 330°C). This plot demonstrates the successful prevention of premature crystallization in the HZO film.

[0076] The axes in Figure 5 are identical to those in Figure 4, allowing for a direct comparison of the two results. In contrast to Figure 4, the plot in Figure 5 shows broad, low-intensity features without prominent peaks. This diffraction pattern is characteristic of amorphous materials and indicates that the HZO film remains in an amorphous state after low-temperature ALD processes (such as the second ALD process described above).

[0077] The absence of sharp diffraction peaks in Figure 5 confirms that the low-temperature deposition method successfully prevented premature crystallization of the HZO film. This amorphous state is useful for the subsequent controlled crystallization step described in Figure 2, enabling precise design of the final crystal structure and electrical properties of the memory device.

[0078] In both Figure 4 and Figure 5, the represented HZO film corresponds to the amorphous transition metal oxide layer 106 described in Figures 1A-1D. These XRD results highlight the effect of temperature control during the ALD process on maintaining the desired amorphous state of the transition metal oxide layer, which is an advantage of the disclosed method for forming memory devices within high aspect ratio structures of this disclosure. Other embodiments of methods for forming memory devices within high aspect ratio features are described using flowcharts shown in Figures 6-8.

[0079] Figures 6–8 illustrate exemplary methods for forming a memory device within a high-aspect-ratio feature according to embodiments of the present disclosure. The methods of Figures 6–8 can be combined with other methods and may be implemented using the ALD system 300 shown in Figure 3 and other systems and apparatus described herein, such as the methods described using Figures 1A–1D and 2. While presented in a logical order, the arrangement and numbering of the steps in Figures 6–8 are not intended to be limiting. The method steps in Figures 6–8 may be performed in any suitable order.

[0080] Referring to Figure 6, step 610 of method 600 for forming a memory device within a high aspect ratio feature involves depositing a first electrode layer within a concave feature of the substrate using a first atomic layer deposition process. The concave feature may be the concave feature 110 in Figure 1A, and the first ALD process may be the same as that described for Figure 1B. Step 620 of method 600 involves depositing an amorphous transition metal oxide layer on top of the first electrode layer using a second atomic layer deposition process at a first substrate temperature. Step 620 may be shown by structure 100 in Figure 1C, and the amorphous transition metal oxide layer may be the amorphous transition metal oxide layer 106 in Figure 1C. Additionally, the second atomic layer deposition process may be the same as the second ALD process described above.

[0081] Continuing to refer to Figure 6, step 630 of method 600 involves depositing a second electrode layer on the amorphous transition metal oxide layer using a third atomic layer deposition process while maintaining the amorphous transition metal oxide layer. The second substrate temperature is lower than the recrystallization temperature of the amorphous transition metal oxide material of the amorphous transition metal oxide layer. The first electrode layer, the amorphous transition metal oxide layer, and the second electrode layer form a memory layer stack. The second electrode layer may be similar to the second electrode layer 108 described in Figure 1D, and step 630 may be the step described using Figure 1D. Similarly, the second substrate temperature may be as described above, and the third atomic layer deposition process may be the third ALD process described using Figure 1D. In some embodiments, method 600 may carry out an annealing step after step 630, as described using Figure 2.

[0082] Referring here to Figure 7, step 710 of method 700 for forming a memory device with high aspect ratio features is to load a substrate into a first atomic layer deposition (ALD) chamber of an ALD system. The substrate may be structure 100 shown in Figure 1A, and the ALD system may be ALD system 300 described using Figure 3. Step 720 is to carry out a first ALD process, which includes flowing a first metal precursor gas to deposit a first electrode layer within the high aspect ratio openings of the substrate. In one embodiment, step 720 may be the step described using Figure 1B, and the first electrode layer may be first electrode layer 104. Furthermore, the first ALD process may be the first ALD process described using Figure 1B, and the first metal precursor gas may be first precursor gas. Additionally, the high aspect ratio openings may be concave features 110 in Figure 1B.

[0083] Step 730 of Method 700 involves loading the substrate into the second ALD chamber of the ALD system. Step 740 then carries out a second ALD process, which includes flowing a gas mixture to deposit an amorphous transition metal oxide layer on the first electrode layer. The second ALD process may be as described above with reference to Figure 1C, and the amorphous transition metal oxide layer may be amorphous transition metal oxide layer 106. The gas mixture may be either a second precursor gas or a second reactant gas. Method 700 then proceeds to step 750.

[0084] Step 750 of Method 700 involves loading the substrate into a third ALD chamber of the ALD system and maintaining the substrate at a temperature below the amorphous-crystal temperature of the amorphous transition metal oxide layer. Step 760 then carries out a third ALD process, which includes depositing a second electrode layer by flowing a second metal precursor gas through the substrate while maintaining the substrate at the above temperature. The first electrode layer, the amorphous transition metal oxide layer, and the second electrode layer form a memory layer stack. Again, the second ALD process may be as described using Figure 1C, and the third ALD process may be as described using Figure 1D. The ALD system 300 in Figure 3 may comprise three processing chambers that can be used as the first ALD chamber, the second ALD chamber, and the third ALD chamber as specified in steps 710, 730, and 750.

[0085] Referring here to Figure 8, Method 800 for forming a memory device within a high aspect ratio feature involves, in step 810, depositing a first electrode layer within a concave feature of the substrate using a first atomic layer deposition process. Step 810 may be as described using Figure 1B and may be carried out in the same manner as described for step 610 of Method 600. Furthermore, the concave feature in step 810 may be the concave feature 110 shown in Figure 1B.

[0086] In step 820, method 800 deposits an amorphous transition metal oxide layer on the first electrode layer using a second atomic layer deposition process at a first substrate temperature. Here again, step 820 may be as described using step 620 of method 600 in Figure 1C and Figure 6. Step 830 of method 800 deposits a second electrode layer on the amorphous transition metal oxide layer using a third atomic layer deposition process at a second substrate temperature. Step 830 may be shown for structure 100 in Figure 1D.

[0087] Continuing to refer to Figure 8, Method 800, in step 840, anneals the substrate at a third substrate temperature to crystallize the amorphous transition metal oxide layer and form a crystalline transition metal oxide layer. The crystalline transition metal oxide layer has a ferroelectric crystalline phase or an antiferroelectric crystalline phase. The difference between Method 600 in Figure 6 and Method 800 in Figure 8 is the annealing step 840 in Figure 8. The first ALD process, the second ALD process, and the third ALD process may be as described above using Figures 1A to 1D.

[0088] Exemplary embodiments of the present invention are shown below. Other embodiments can also be understood from the entirety of this specification and the claims submitted herein. [Examples]

[0089] Example 1. A method for forming a memory device on a substrate includes depositing a first electrode layer in a concave feature of the substrate using a first atomic layer deposition process, and depositing an amorphous transition metal oxide layer on top of the first electrode layer using a second atomic layer deposition process at a first substrate temperature. The method further includes depositing a second electrode layer on top of the amorphous transition metal oxide layer using a third atomic layer deposition process at a second substrate temperature while maintaining the amorphous state of the amorphous transition metal oxide layer, wherein the second substrate temperature is lower than the recrystallization temperature of the amorphous transition metal oxide material of the amorphous transition metal oxide layer, and the first electrode layer, the amorphous transition metal oxide layer, and the second electrode layer are deposited to form a memory layer stack.

[0090] Example 2. The method according to Example 1, wherein the amorphous transition metal oxide layer comprises hafnium oxide, zirconium oxide, or hafnium-zirconium oxide.

[0091] Example 3. The method according to Example 1 or 2, wherein the first electrode layer contains a transition metal nitride and the second electrode layer contains a transition metal nitride.

[0092] Example 4. The method according to any one of Examples 1 to 3, wherein the first electrode layer and the second electrode layer contain titanium nitride.

[0093] Example 5. The method according to any one of Examples 1 to 4, wherein the temperature of the first substrate and the temperature of the second substrate are between 300°C and 350°C, and the temperature of the first substrate is higher than the temperature of the second substrate.

[0094] Example 6. The method according to any one of Examples 1 to 5, wherein the concave feature has a high aspect ratio of 40:1 to 10:1.

[0095] Example 7. The method according to any one of Examples 1 to 6, wherein the first atomic layer deposition process is a periodic process. One cycle of the periodic process comprises flowing a first precursor gas to adsorb it into a concave feature, flowing a first purge gas to purge the remaining first precursor gas and precursor reactants, flowing a first reactant gas to react within the concave feature to form a first monolayer, and flowing a first purge gas to purge the remaining first reactant gas and reactants.

[0096] Example 8. The method according to any one of Examples 1 to 7, wherein the second atomic layer deposition process is carried out at the first substrate temperature and is a periodic process. One cycle of the periodic process comprises flowing a second precursor gas to adsorb it into the concave features, flowing a second purge gas to purge the remaining second precursor gas and precursor reactants, flowing a second reactant gas to react within the concave features to form a second monolayer, and flowing a second purge gas to purge the remaining second reactant gas and reactants.

[0097] Example 9. The method according to any one of Examples 1 to 8, wherein the third atomic layer deposition process is carried out at the second substrate temperature and is a periodic process. One cycle of the periodic process comprises flowing a third precursor gas to adsorb it into the concave features, flowing a third purge gas to purge the remaining third precursor gas and precursor reactants, flowing a third reactant gas to react within the concave features to form a third monolayer, and flowing a third purge gas to purge the remaining third reactant gas and reactants.

[0098] Example 10. The method according to any one of Examples 1 to 9, further comprising annealing a memory layer stack at a third substrate temperature to crystallize an amorphous transition metal oxide layer and form a crystalline transition metal oxide layer, wherein the third substrate temperature is higher than the second substrate temperature.

[0099] Example 11. The method according to any one of Examples 1 to 10, wherein the first electrode layer, the crystalline transition metal oxide layer, and the second electrode layer form a memory capacitor.

[0100] Example 12. The method according to any one of Examples 1 to 11, wherein the crystalline transition metal oxide layer comprises a ferroelectric crystalline phase or an antiferroelectric crystalline phase.

[0101] Example 13. The method according to any one of Examples 1 to 12, wherein the oxygen content of the second electrode layer is 18 to 22 atomic percent.

[0102] Example 14. A method for forming a memory device on a substrate comprises loading the substrate into a first atomic layer deposition (ALD) chamber of an ALD system and performing a first ALD process, which includes flowing a first metal precursor gas to deposit a first electrode layer within a high aspect ratio opening of the substrate. The method further comprises loading the substrate into a second ALD chamber of an ALD system and performing a second ALD process, which includes flowing a gas mixture containing tetrakis(ethylmethylamino)hafnium (TEMAHf), tetrakis(ethylmethylamino)zirconium (TEMAZr), and an oxidizing agent to deposit an amorphous transition metal oxide layer on top of the first electrode layer. The method further includes carrying out a third ALD process, which comprises loading a substrate into a third atomic layer deposition (ALD) chamber of an ALD system, maintaining the substrate at a temperature below the amorphous-crystal temperature of the amorphous transition metal oxide layer, and depositing a second electrode layer by flowing a second metal precursor gas through the substrate while maintaining the temperature, wherein the first electrode layer, the amorphous transition metal oxide layer, and the second electrode layer form a memory layer stack.

[0103] Example 15. The method according to Example 14, wherein the gas mixture for the second ALD process is flowed by flowing TEMAHf and TEMAZr, followed by flowing an oxidizing agent.

[0104] Example 16. The method according to Example 14 or 15, further comprising annealing a memory layer stack at substrate temperature to crystallize an amorphous transition metal oxide layer and form a crystalline transition metal oxide layer, wherein the crystalline transition metal oxide layer has a ferroelectric crystalline phase or an antiferroelectric crystalline phase, the substrate temperature is higher than the amorphous-crystal temperature of the amorphous transition metal oxide layer, and the oxygen content of the second electrode layer after annealing is 18 to 22 atomic percent.

[0105] Example 17. A method for forming a memory device on a substrate comprises depositing a first electrode layer in a concave feature of the substrate using a first atomic layer deposition process, and depositing an amorphous transition metal oxide layer on the first electrode layer using a second atomic layer deposition process at a first substrate temperature. The method further comprises depositing a second electrode layer on the amorphous transition metal oxide layer using a third atomic layer deposition process at a second substrate temperature. The method further comprises annealing the substrate at a third substrate temperature to crystallize the amorphous transition metal oxide layer and form a crystalline transition metal oxide layer, wherein the crystalline transition metal oxide layer has a ferroelectric crystalline phase or an antiferroelectric crystalline phase.

[0106] Example 18. The method according to Example 17, wherein annealing is performed by diffusing oxygen from the amorphous transition metal oxide layer to the second electrode layer so that the oxygen content in the second electrode layer is 18 to 22 atomic percent.

[0107] Example 19. The method according to Example 17 or 18, wherein the temperature of the first substrate and the temperature of the second substrate are between 300°C and 350°C.

[0108] Example 20. The method according to any one of Examples 17 to 19, wherein the first electrode layer contains titanium nitride, the amorphous transition metal oxide layer contains hafnium zirconium oxide, the second electrode layer contains titanium nitride, and the crystalline transition metal oxide layer contains crystalline hafnium zirconium oxide.

[0109] Example 21. The method according to any one of Examples 17 to 20, wherein the first electrode layer is deposited at the temperature of the second substrate.

[0110] While the present invention has been described with reference to exemplary embodiments, this specification is not intended to be constrained. Various modifications and combinations of the exemplary embodiments, as well as other embodiments of the invention, will become apparent to those skilled in the art through reference to this specification. Therefore, the appended claims are intended to encompass all such modifications or embodiments.

Claims

1. A method for forming a memory device on a substrate, A first electrode layer is deposited within a concave feature of the substrate using a first atomic layer deposition process, Depositing an amorphous transition metal oxide layer on the first electrode layer using a second atomic layer deposition process at a first substrate temperature, The method involves depositing a second electrode layer on the amorphous transition metal oxide layer using a third atomic layer deposition process at a second substrate temperature while maintaining the amorphous state of the amorphous transition metal oxide layer, wherein the second substrate temperature is lower than the recrystallization temperature of the amorphous transition metal oxide material of the amorphous transition metal oxide layer, and the first electrode layer, the amorphous transition metal oxide layer, and the second electrode layer are deposited to form a memory layer stack. A method that includes this.

2. The method according to claim 1, wherein the amorphous transition metal oxide layer comprises hafnium oxide, zirconium oxide, or hafnium-zirconium oxide.

3. The method according to claim 1, wherein the first electrode layer contains a transition metal nitride and the second electrode layer contains a transition metal nitride.

4. The method according to claim 1, wherein the first electrode layer and the second electrode layer contain titanium nitride.

5. The method according to claim 1, wherein the temperature of the first substrate and the temperature of the second substrate are between 300°C and 350°C, and the temperature of the first substrate is higher than the temperature of the second substrate.

6. The method according to claim 1, wherein the concave feature has a high aspect ratio of 40:1 to 10:

1.

7. The first atomic layer deposition process is a periodic process, and one cycle of the periodic process is The first precursor gas is flowed through and adsorbed into the concave feature, The process involves flowing a first purge gas to purge the remaining first precursor gas and precursor reactants. The process involves flowing a first reactant gas and allowing it to react within the concave feature to form a first monolayer, The process involves flowing the first purge gas to purge the remaining first reactant gas and reactants, The method according to claim 1, including the method described in claim 1.

8. The second atomic layer deposition process is carried out at the first substrate temperature, is a periodic process, and one cycle of the periodic process is A second precursor gas is introduced and adsorbed into the concave feature, The process involves flowing a second purge gas to purge the remaining second precursor gas and precursor reactants. A second reactant gas is introduced and reacted within the concave feature to form a second monolayer. The second purge gas is then purged to remove the remaining second reactant gas and reactants. The method according to claim 1, including the method described in claim 1.

9. The third atomic layer deposition process is carried out at the second substrate temperature, is a periodic process, and one cycle of the periodic process is A third precursor gas is flowed through the concave feature to cause it to be adsorbed, A third purge gas is introduced to purge the remaining third precursor gas and precursor reactants. A third reactant gas is introduced and reacted within the concave feature to form a third monolayer. The third purge gas is then flowed to purge the remaining third reactant gas and reactants. The method according to claim 1, including the method described in claim 1.

10. The memory layer stack is annealed at a third substrate temperature to crystallize the amorphous transition metal oxide layer and form a crystalline transition metal oxide layer, wherein the third substrate temperature is higher than the second substrate temperature. The method according to claim 1, further comprising:

11. The method according to claim 10, wherein the first electrode layer, the crystalline transition metal oxide layer, and the second electrode layer form a memory capacitor.

12. The method according to claim 10, wherein the crystalline transition metal oxide layer includes a ferroelectric crystalline phase or an antiferroelectric crystalline phase.

13. The method according to claim 10, wherein the oxygen content of the second electrode layer is 18 to 22 atomic percent.

14. A method for forming a memory device on a substrate, The substrate is loaded into the first atomic layer deposition (ALD) chamber of the ALD system, The first ALD process is carried out, which includes flowing a first metal precursor gas to deposit a first electrode layer within a high aspect ratio opening of the substrate. Loading the aforementioned substrate into the second ALD chamber of the ALD system, A second ALD process is carried out, which includes flowing a gas mixture containing tetrakis(ethylmethylamino)hafnium (TEMAHf), tetrakis(ethylmethylamino)zirconium (TEMAZr), and an oxidizing agent to deposit an amorphous transition metal oxide layer on the first electrode layer. The substrate is loaded into the third atomic layer deposition (ALD) chamber of the ALD system, and the substrate is maintained at a temperature below the amorphous-crystal temperature of the amorphous transition metal oxide layer. A third ALD process is carried out, which includes depositing a second electrode layer by flowing a second metal precursor gas through the substrate while maintaining the substrate at the temperature, wherein the first electrode layer, the amorphous transition metal oxide layer, and the second electrode layer form a memory layer stack. A method that includes this.

15. The method according to claim 14, wherein flowing the gas mixture for the second ALD process includes flowing the TEMAHf and TEMAZr, followed by flowing the oxidizer.

16. The memory layer stack is annealed at the substrate temperature to crystallize the amorphous transition metal oxide layer and form a crystalline transition metal oxide layer, wherein the crystalline transition metal oxide layer has a ferroelectric crystalline phase or an antiferroelectric crystalline phase, the substrate temperature is higher than the amorphous-crystal temperature of the amorphous transition metal oxide layer, and the oxygen content of the second electrode layer after annealing is 18 to 22 atomic percent. The method according to claim 14, further comprising:

17. A method for forming a memory device on a substrate, A first electrode layer is deposited within a concave feature of the substrate using a first atomic layer deposition process, Depositing an amorphous transition metal oxide layer on the first electrode layer using a second atomic layer deposition process at a first substrate temperature, A second electrode layer is deposited on the amorphous transition metal oxide layer using a third atomic layer deposition process at a second substrate temperature, The substrate is annealed at a third substrate temperature to crystallize the amorphous transition metal oxide layer and form a crystalline transition metal oxide layer, wherein the crystalline transition metal oxide layer has a ferroelectric crystalline phase or an antiferroelectric crystalline phase. A method that includes this.

18. The method according to claim 17, wherein the annealing diffuses oxygen from the amorphous transition metal oxide layer to the second electrode layer such that the oxygen content of the second electrode layer is 18 to 22 atomic percent.

19. The method according to claim 17, wherein the temperature of the first substrate and the temperature of the second substrate are between 300°C and 350°C.

20. The method according to claim 17, wherein the first electrode layer contains titanium nitride, the amorphous transition metal oxide layer contains hafnium zirconium oxide, the second electrode layer contains titanium nitride, and the crystalline transition metal oxide layer contains crystalline hafnium zirconium oxide.