A method for producing carbon black using sustainable burner fuel, and products produced therefrom.

By integrating sustainable burner fuels into the carbon black production process, the method ensures high-quality carbon black production with sustainable materials, addressing the need for environmentally friendly and cost-effective carbon black manufacturing.

JP2026539160APending Publication Date: 2026-11-20CABOT CORP
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026526148
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-03
Filing Date
2024-10-31
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

The industry needs a method to utilize large quantities of sustainable materials as burner fuels in existing carbon black furnace processes while maintaining the quality and yield of carbon black production comparable to that produced from traditional fossil fuel-based materials.

Method used

A method is developed to produce carbon black by introducing at least one sustainable burner fuel into a carbon black reactor, igniting it to form a hot gas flow, combining it with carbon black production raw materials, and quenching the reaction to form carbon black, ensuring that the sustainable fuel constitutes a majority of the total fuel used.

Benefits of technology

This method allows for the production of carbon black with acceptable yield and quality, using a significant proportion of sustainable fuels without compromising the properties of the carbon black, offering environmental and economic benefits.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539160000001_ABST
    Figure 2026539160000001_ABST
Patent Text Reader

Abstract

Methods for producing carbon black using at least one type of sustainable burner fuel, for example, a burner fuel containing, but not limited to, tire pyrolysis oil, are described. The carbon black produced by these methods is further described. The benefits achieved by these methods are further described.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] The present invention relates to a method for producing carbon black from sustainable or alternative burner fuels. The present invention further relates to carbon black formed by using sustainable burner fuels in the present method.

[0002] Carbon black has been used to modify the mechanical, electrical, and optical properties of compositions. Carbon black and other fillers have been used as pigments, fillers, and / or reinforcing agents in the formulation and preparation of compositions used in rubber, plastic, paper, or textile applications. The properties of carbon black or other fillers are important factors in determining the various performance characteristics of these compositions. A key application of elastomer compositions is in tire manufacturing, where additional components are often added to impart specific properties to the final product or its components. Carbon black has been used to modify the functional properties, conductivity, rheology, surface properties, viscosity, appearance, and other properties of elastomer compositions and other types of compositions.

[0003] The most common conventional process for the industrial production of carbon black is the furnace process. In this process, a primary or main liquid carbon-containing raw material, such as decanted oil, is injected into a gas stream after or during combustion of a lean, high-temperature fuel. The post-combustion high-temperature stream is formed by oxidizing burner fuel, typically natural gas or coal gas, or a liquid fuel similar to or identical to the main raw material, in air, oxygen-enriched air, or oxygen. Some of the raw material is thermally decomposed to produce carbon black and by-products (mainly hydrogen and carbon monoxide), while the remainder is oxidized to produce CO2 and H2O. Conventional or traditional raw materials include decanted oil, slurry oil, coker oil, coal tar derivatives, or heavy liquid residues from the ethylene cracker process. These carbon black raw materials are typically heavy (specific gravity greater than 1.02), have an H:C atomic ratio of less than 1.23, are rich in aromatic compounds (Bureau of Mines Correlation Index, BMCI greater than 100), and are liquid at room temperature and pressure (e.g., 25°C, 1 atm). The amounts of hydrogen and carbon can be measured according to ASTM D5291 or an equivalent method. They are all generally derived from fossil fuels.

[0004] The furnace black process differs from the channel black process and the thermal black process, which use natural gas as a raw material.

[0005] Using one or more sustainable burner fuels in existing carbon black furnace processes can be economically beneficial and environmentally advantageous. These burner fuels do not necessarily have to be fossil fuel-based. Examples include vegetable oil, recycled tires (tire pyrolysis oil or TPO), plastics, oils derived from the pyrolysis of municipal waste or biomass, or natural gas produced from landfills or agricultural waste.

[0006] Therefore, there is a need in the industry to provide a solution that allows for the use of large quantities of sustainable materials in existing carbon black furnace processes and to produce carbon black comparable to that formed from traditional burner fuels and main raw materials (e.g., producing carbon black with acceptable yields, and / or high surface area and / or high structure). One way to do this is to use sustainable materials as burner fuels (where at least the majority of all burner fuels are sustainable burner fuels). Using these sustainable burner fuels in existing furnace processes would save significant capital and development resources compared to developing, designing, and building new methods for using them.

[0007] All patents and publications mentioned throughout this document are incorporated herein by reference in their entirety. [Overview of the project]

[0008] A key feature of the present invention is to provide a method for preparing or producing carbon black using burner fuel containing at least one sustainable burner fuel.

[0009] An additional feature of the present invention is to provide carbon black produced from a method utilizing burner fuels that include at least one sustainable burner fuel.

[0010] A further feature is the provision of a method for producing carbon black using conventional carbon black forming raw materials together with burner fuel containing at least one type of sustainable burner fuel.

[0011] An additional feature is to provide a method for producing carbon black using burner fuel containing at least one sustainable burner fuel (e.g., here, on a weight basis, the majority of the burner fuel is at least one sustainable burner fuel), wherein the resulting carbon black has an acceptable (e.g., good) yield for a given acceptable (e.g., high) surface area and / or acceptable structure (e.g., high structure).

[0012] To achieve these and other advantages, and in accordance with the objectives of the present invention, the present invention relates in part to a method for producing carbon black, as embodied and broadly described herein. The method comprises introducing burner fuel, which includes at least one sustainable burner fuel, into a carbon black reactor, and then igniting the burner fuel in the reactor to form a flow of hot gas from the burner fuel. The method then comprises introducing at least one carbon black production raw material into the carbon black reactor at one or more introduction points, and combining the at least one carbon black production raw material with the flow of hot gas to form carbon black in the reaction flow. The method further comprises quenching the reaction flow containing carbon black and recovering the carbon black.

[0013] Furthermore, the present invention relates in part to carbon black, wherein in a method for forming carbon black, at least a portion or at least a majority of the burner fuel used is sustainable burner fuel.

[0014] The present invention further relates to products and / or articles, such as elastomer composites, formed from one or more of the carbon blacks of the present invention, but is not limited thereto.

[0015] Please understand that both the general description above and the detailed description below are merely illustrative and descriptive, and further illustrate the scope of the claimed invention.

[0016] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate various features of the present invention and, together with the detailed description, serve to explain the principles of the present invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] [Figure 1A] It is a cross-sectional view of an example of a reactor suitable for preparing the carbon black of the present invention.

[0018] [Figure 1B] It is a cross-sectional view of another example of a reactor suitable for preparing the carbon black of the present invention.

[0019] [Figure 2] It is a cross-sectional view of a further example of a reactor suitable for preparing the carbon black of the present invention.

[0020] [Figure 3] It is a graph plotting OAC (%) and STSA (unit: m² / g) for two examples of the present invention and one comparative example using different burner fuels.

[0021] [Figure 4] It is a graph plotting the dimensionless yield and STSA (unit: m² / g) for two examples of the present invention and one comparative example using different burner fuels.

[0022] [Figure 5] It is a graph plotting COAN and STSA (unit: m² / g) for two examples of the present invention and one comparative example using different burner fuels.

[0023] [Figure 6] It is a graph plotting the specific tint strength and STSA (unit: m² / g) for two examples of the present invention and one comparative example using different burner fuels.

[0024] [Figure 7] This graph plots the iodine value and STSA (unit: m2 / g) for two examples and one comparative example of the present invention using different burner fuels. [Modes for carrying out the invention]

[0025] The present invention relates to a method for producing carbon black using burner fuels, including one or more sustainable burner fuels as defined and described herein. For the purposes of the present invention, the term “sustainable” burner fuel as used herein may be or include, for example, materials that may be called circular or recycled materials, or materials and / or fuels that may be called “sustainable” materials and / or fuels from biosources. Examples of burner fuels that can be used are described in detail below.

[0026] The present invention further relates to carbon black produced by one or more of these methods.

[0027] In the method of the present invention, preferably, at least the majority of all burner fuels used can be one or more sustainable burner fuels.

[0028] The method of the present invention not only allows for the use of large quantities of sustainable burner fuel as burner fuel, but also does not impair the quality of the carbon black produced. Therefore, the method of the present invention utilizes sustainable burner fuel, which is more desirable for environmental and / or other reasons, and further produces carbon black of at least equivalent quality to, though not superior to, carbon black produced using 100% traditional burner fuel in the furnace carbon black process.

[0029] The present invention provides a method for producing carbon black, comprising introducing a burner fuel containing at least a portion of one or more sustainable burner fuels into a carbon black reactor. The method further comprises ignition to form a flow of hot gas or heated gas into the carbon black reactor (e.g., a furnace carbon black reactor). The method also comprises introducing at least one carbon black production raw material (or carbon black raw material) into the carbon black reactor via one or more introduction points. The method then comprises combining the carbon black production raw material with the flow of hot gas to form carbon black in the reaction flow. The method then comprises quenching the reaction flow containing carbon black and recovering the carbon black. In the method, preferably, the sustainable burner fuel constitutes the majority of the total burner fuel, and more preferably, at least 60% by weight of the total burner fuel.

[0030] Sustainable burner fuels may be fuels derived from sources considered sustainable, biological, and / or recycled. For example, sustainable burner fuels may be or may contain ethylene, which is a gas at room temperature and room pressure. Ethylene can be produced from bio-derived ethanol, for example, from maize fermentation or other plant material fermentation. Alternatively or additionally, sustainable burner fuels may be oils derived from biomass or hydrothermal liquefaction (HTL) of tires, plastics, or other waste.

[0031] For the purposes of the present invention, sustainable burner fuel can be a fuel that does not originate from fossil fuel-based gasoline production or coal cracking, nor from cracking for the production of olefins. Therefore, sustainable burner fuel is a fuel other than coal tar liquid, petroleum refined liquid, or ethylene cracker residue.

[0032] Other examples of sustainable burner fuels include, but are not limited to, tire pyrolysis oil, plastic pyrolysis oil, plant-derived oils, tree-derived oils, oils derived from the pyrolysis of municipal solid waste, oils derived from the pyrolysis or decomposition of biomass (e.g., animal, plant, tree, or vegetable) or other agricultural waste, oils derived from the processing of paper manufacturing by-products, and / or other oils primarily sourced from bio-based materials, or any combination thereof. These liquid raw materials have an H:C atomic ratio greater than 1.23, a specific gravity less than 1.02, or a BMCI value less than 100. Specific examples of liquid sustainable burner fuels are shown in Table 1 below. [Table 1]

[0033] Other examples of sustainable burner fuels include, but are not limited to, sustainable raw materials, bio-derived or bio-based raw materials, and / or other by-products of refining processes, or any combination thereof.

[0034] Other examples of sustainable burner fuels include, but are not limited to, oils derived from vegetables, fruits, nuts, or other plants (e.g., corn oil and / or corn distillate) or oils derived from trees.

[0035] Other examples of sustainable burner fuels include, but are not limited to, bio-derived ethanol (obtained from fermentation products of corn or other plants, vegetables, or fruits).

[0036] Other examples of sustainable burner fuels include, but are not limited to, plant or animal waxes and resins, such as lanolin or lac.

[0037] Other examples of sustainable burner fuels include, but are not limited to, oils derived from animal fats.

[0038] Other examples of sustainable burner fuels include, but are not limited to, algal oil.

[0039] Other examples of sustainable burner fuels include, but are not limited to, oils obtained from the pyrolysis of sewage sludge or agricultural waste.

[0040] Other examples of sustainable burner fuels include, but are not limited to, liquid by-products from the processing of bio-based materials.

[0041] Other examples of sustainable burner fuels include, but are not limited to, liquids produced by the hydrothermal liquefaction of bio-based materials, rubber, plastics, or other waste.

[0042] Other examples of sustainable burner fuels include, but are not limited to, crude tall oil, tall oil rosin, tall oil pitch, or tall oil fatty acids (e.g., derived from papermaking processes).

[0043] Other examples of sustainable burner fuels include, but are not limited to, oils made from sustainable raw materials, such as recycled materials.

[0044] Other examples of sustainable burner fuels include, but are not limited to, oil derived from the pyrolysis of low-quality, substandard, or end-of-life tires.

[0045] Other examples of sustainable burner fuels include, but are not limited to, oil derived from waste or recycled plastics.

[0046] Other examples of sustainable burner fuels include, but are not limited to, oil derived from the pyrolysis of municipal solid waste.

[0047] Other examples of sustainable burner fuels include, but are not limited to, biomass (biotils), such as those derived from animals or plants (e.g., vegetables) or trees, or from the pyrolysis of crushed biochar.

[0048] Other examples of sustainable burner fuels include, but are not limited to, recovered hydrogen and / or ammonia, or recycled hydrogen and / or ammonia, or environmentally friendly hydrogen and / or ammonia, or other sustainably produced hydrogen and / or ammonia.

[0049] In the present invention, the burner fuel may comprise, be comprised of, essentially comprise, or include at least one sustainable burner fuel. The weight percentage of sustainable burner fuel based on the total weight percentage of the burner fuel may be any value in the range of 5% to 100% by weight, for example, 10% to 100% by weight, or 20% to 100% by weight, or 30% to 100% by weight, or 40% to 100% by weight, or 50% to 100% by weight, or greater than 50% by weight. Preferably, although not required, in the present invention, at least a large portion (by weight) of the total burner fuel used in some of the methods of the present invention is one or more sustainable burner fuels. Preferably, this amount is at least 60% by weight, or at least 65% by weight, or at least 70% by weight, or at least 75% by weight, or at least 80% by weight, or at least 85% by weight, or at least 90% by weight, based on the total weight percentage of all burner fuels used, for example, 51% to 95% by weight, or 60% to 95% by weight, or 65% to 95% by weight, or 70% to 95% by weight, or 75% to 95% by weight, or 60% to 95% by weight, or 60% to 90% by weight, or 60% to 85% by weight, or 60% to 80% by weight, or 60% to 75% by weight.

[0050] Any portion of the burner fuel that is not sustainable may be any traditional burner fuel used in a carbon black production process using a carbon black reactor. For example, the traditional burner fuel portion, if present, may be a readily combustible gas, vapor, or liquid stream, such as natural gas, hydrogen, carbon monoxide, methane, acetylene, alcohol, or kerosene.

[0051] A mixture of two or more sustainable burner fuels can be used.

[0052] Two different burner fuels, (for example, a) two or more sustainable burner fuels, or b) at least one sustainable burner fuel and one non-sustainable burner fuel, for example, if conventional burner fuels are used, the different burner fuels may be introduced into the carbon black reactor as a mixture, or separately, or continuously through the same supply line, or in any combination thereof, and may be introduced at different locations at the discretion of the system.

[0053] With respect to the raw materials for carbon black production, these raw materials may be the carbon black raw materials traditionally used in the furnace carbon black process ("traditional" carbon black raw materials).

[0054] Carbon black raw materials are typically derived from decant or slurry oil, coal tar or coal tar distillate, or families of ethylene or phenol cracker residues. Their distinct characteristics in typical furnace carbon black production are further described below.

[0055] Carbon black raw materials may have one or more or all of the following properties: 1) Over 100 (for example, over 101, over 102, over 103, over 104, over 105, over 110, over 115, over 120, over 130, over 140, over 150, over 160, over 170, for example, 100.1~180, 100.5~180, 101~180, 102~180, 103~180, 104~180, 105~180) BMCI of 110-180, 115-180, 120-180, 130-180, 140-180, 150-180, 160-180, 100.1-175, 100.1-170, 100.1-165, 110-175, 115-175, 120-175, 125-170, 130-170), and / or 2) Specific gravity greater than 1.02 (for example, greater than 1.025, greater than 1.03, greater than 1.035, greater than 1.04, greater than 1.05, for example, 1.021-1.3, or 1.025-1.3, or 1.03-1.3, or 1.05-1.3, or 1.07-1.25), and / or 3) H:C atomic ratios less than 1.23 (e.g., less than 1.22, less than 1.21, less than 1.2, less than 1.15, less than 1.1, less than 1.05, less than 1, less than 0.9, less than 0.8, e.g., 1.225~0.7, 1.225~0.8, 1.225~0.9, 1.225~1, 1.225~1.1, 1.22~0.7, 1.21~0.7, 1.2~0.7), and / or 4) Liquid at room temperature and room pressure (e.g., 25°C and 1 atm).

[0056] As options, carbon black raw materials can have all four of these properties (BMCI, H:C atomic ratio, specific gravity, and liquid properties), three of the four properties, or two of the four properties.

[0057] Examples of carbon black raw materials are shown in Table 2 below, and include coal tar, liquid distilled from coal tar, decant or slurry oil obtained from catalytic cracking, and residue oil from ethylene cracking. As shown in Table 2, these raw materials have an H:C ratio of less than 1.23, a specific gravity greater than 1.02, and a BMCI value greater than 100.

[0058] [Table 2]

[0059] The carbon black raw material can be a liquid or a tar-like pitch-like amorphous solid at room temperature. For the purposes of this invention, the liquid is defined as being at room temperature (e.g., 25°F) and atmospheric pressure (e.g., 1 atm). "Rich in aromatic species" means that the raw material contains a large amount of aromatic compounds. For example, a large amount of aromatic compounds means that the total weight percentage of aromatic compounds present is at least 20% by weight, or the BMCI is at least 100, or both. The carbon black raw material can be heated to become a vapor or partially vapor, resulting in an aromatic species-rich vapor, or it can be used as an aromatic species-rich vapor.

[0060] As an alternative, sustainable burner fuel is consumed and burned substantially or completely as fuel, and no portion of sustainable burner fuel is used as raw material for pyrolysis to form carbon black.

[0061] As an option, based on the total weight of the raw materials used to produce carbon black, less than 5%, for example less than 1% by weight, of sustainable burner fuel can be used to form carbon black. Alternatively or additionally, the sustainable burner fuel is almost completely consumed (burned) as fuel, and less than 1% by weight of the total sustainable burner fuel used in the process undergoes pyrolysis to form carbon black.

[0062] The amount of sustainable burner fuel used can be sufficient to increase the yield of carbon black formed by 1% to 8% (e.g., 2% to 8%, 3% to 7%, or 2% to 6%) compared to burner fuel consisting of 100% natural gas.

[0063] The amount of sustainable burner fuel can be sufficient to increase the COAN (carbon black) produced by the burner fuel by 1% to 8% (e.g., 2% to 8%, 3% to 7%, or 2% to 6%) compared to burner fuel consisting of 100% natural gas.

[0064] As an alternative, a portion of the carbon black raw material may be a low-yield carbon black raw material, such as that described in International Publication No. 2023 / 055931, which is incorporated herein in whole by reference. The low-yield carbon black raw material may constitute at least 1% by weight, or at least 5% by weight, or at least 10% by weight, or at least 25% by weight, or at least 50% by weight, or at least 75% by weight, or about 1% to 90% by weight, based on the total amount of carbon black raw material used.

[0065] With respect to the method steps of the present invention, the method includes the step of introducing burner fuel, which includes at least one sustainable burner fuel as described herein, into a carbon black reactor. The burner fuel can be introduced into the reactor by one or more axial, radial, or tangential pipes and / or lances and / or injectors and / or other supply lines.

[0066] This method involves igniting a carbon black reactor (e.g., a furnace carbon black reactor) to form a flow of high-temperature gas from the burner fuel.

[0067] A "high-temperature gas flow" can be considered as a heated gas flow or a high-temperature combustion gas flow. A high-temperature gas flow can be generated by bringing a burner fuel into contact with a suitable oxidizer flow, such as, but not limited to, air, oxygen, or a mixture of air and oxygen. To facilitate the generation of high-temperature gas, the oxidizer flow may be preheated. Essentially, a heated gas flow is produced by igniting or burning the fuel and / or oxidizer. In a heated gas flow, temperatures such as about 1000°C to about 3500°C can be obtained.

[0068] The carbon black reactor is preferably a furnace carbon black reactor. In some embodiments, the carbon black reactor is a version of the furnace reactor called a stepwise carbon black reactor (e.g., a multi-step carbon black reactor or multi-step reactor). "Stepwise" means that the feed material is introduced or injected at two or more axial positions along the long axis of the furnace.

[0069] For the purposes of this method and other methods described herein, multi-stage carbon black reactors such as those described in U.S. Patents 4,383,973, 7,829,057, 5,190,739, 5,877,251, 6,153,684, or 6,403,695 (all incorporated herein by reference in their entirety) may be used.

[0070] Alternatively or additionally, sustainable burner fuels may be used to generate high-temperature combustion gases for methods such as those disclosed in U.S. Patent No. 1,0519298, whose entire contents are incorporated herein by reference, in which core particles are produced in situ, or core particles introduced into a reactor as pre-coated particles are coated with a layer of carbon.

[0071] A general process for forming carbon black using a carbon black reactor such as a multi-stage reactor, and achieving a suitable high-temperature gas to form carbon black, is incorporated herein by reference and further described in the above-mentioned reference patent, which can be applied to the present invention with the modifications described herein.

[0072] Figures 1A and 1B show cross-sectional views of usable carbon black reactors (50 in Figure 1A and 80 in Figure 1B). In Figure 1A, the flow of high-temperature gas or high-temperature combustion gas is generated within the combustion zone or combustion chamber 1 by bringing burner fuel, in the form of a liquid or gaseous fuel flow 9, into contact with an oxidizer flow 5, for example, air, oxygen, or a mixture of air and oxygen (also known in the art as "oxygen-enriched air"). The burner fuel can be in the form of a readily combustible gas, vapor, or liquid flow.

[0073] In this invention, the combustion process can consume the burner fuel completely or nearly completely. That is, the combustion or oxidation reaction of the burner fuel can reach a state very close to chemical equilibrium. Oxygen, fuel selection, burner design, jet speed, mixing conditions and / or pattern, fuel ratio to air, oxygen-enriched air or pure oxygen, temperature, and / or other factors can be adjusted or optimized.

[0074] The high-temperature gas flow or high-temperature combustion gas flow flows downstream from zones 1 and 2 to zones 3 and 4. Carbon black feedstock is introduced at one or more suitable locations relative to other reactor components and feedstocks. Zone 2 of the combustion chamber may be where one or more carbon black feedstocks are introduced. In Figure 1A, carbon black feedstock can be introduced into the reactor using injectors 10 and / or 6. Injector 10 can, for example, introduce or inject a first carbon black feedstock into the reactor. Alternatively, the first carbon black feedstock may also be introduced into the chamber using an axial pipe or lance (shown as pipe or lance 63 in Figure 1B). As a further alternative, carbon black feedstock may be injected or introduced simultaneously by multiple methods. Lances or any other injectors exposed to the reactor or combustion chamber may need to be cooled or protected from excessive heat in the combustion chamber by methods known in the art.

[0075] As an option, additional carbon black raw materials (which may be the same as or different from the carbon black raw materials) can be introduced into reactor zone 3 at injection point 7 by injector 6. Zones 3 and 4 are reaction zones, and zone 8 is a quenching zone. Q represents the length of zone 4 before quenching zone 8.

[0076] Carbon black raw materials can be injected into the combustion gas stream through one or more nozzles designed for optimal distribution of the raw materials into the combustion gas stream. Such nozzles may be single-fluid or dual-fluid. Dual-fluid nozzles may use, for example, steam, air, or nitrogen to atomize the raw materials. Single-fluid nozzles may be pressure-sprayed, or the raw materials may be injected directly into the gas stream. In the latter case, atomization is caused by the force of the gas stream.

[0077] The carbon black raw material may be injected by an axial injection lance, or a central pipe may be used, and / or one or more radial lances may be used, arranged around the reactor in a plane perpendicular to the flow direction. The reactor may include several planes with radial lances along the flow direction. Spray nozzles or injection nozzles may be placed on the heads of the lances, thereby mixing the raw material with the flow of heated gas.

[0078] Figure 1B shows a cross-section of another example of a carbon black reactor in a furnace process that can be used in the present invention. In this example, as in Figure 1A, the oxidizer stream 51 is combined with a burner or combustion fuel 52 in the combustion chamber 55.

[0079] The high-temperature combustion or partial combustion gas flow prepared in the chamber 55 flows in direction A toward the throat or constriction 64. The carbon black raw material is introduced into the furnace carbon black reactor 80. The carbon black raw material can be introduced using an optional central pipe 63, or using a lance or injector or a set of lances 56, or via a lance or injector positioned in or near the throat 64 as indicated by 57. The carbon black raw material can be introduced at one of these locations, or at two of these locations simultaneously at the same time, or at all three locations simultaneously. The method and division of the first raw material injection can be modified between these locations, if more than two locations are used, to alter the product characteristics and process economics. The injectors and the combustion chamber itself (or a part thereof) can be cooled as needed by methods known in the art.

[0080] In Figure 1B, the length between the optional central pipe injector 63 and the center of the tapered section 64 is shown as length 60. When this central pipe is used, this length is preferably 1 × 10 times the narrowest diameter of the first tapered section 64. When the central pipe is used simultaneously with an injector or lance array 57 for introducing carbon black raw material, the length 60 can be as described above or reduced to about 0. By adjusting this length, it is possible to balance the economics of the structure and process. The height or diameter 54 of the combustion chamber is shown, and this height is greater than the height or diameter 64, and the height or diameter 64 may be at least 20%, at least 30%, at least 40%, or at least 50% smaller than the height or diameter 54.

[0081] Following the introduction of the carbon black raw material, the high-temperature gas stream mixed with the raw material enters the first reaction chamber 58. The purpose of this chamber is to provide a residence time so that the pyrolysis reaction producing carbon black can complete its induction time and begin, and optionally to generate a seed particle population for later structure growth, as taught in U.S. Patent No. 7,829,057. The length of this chamber 66 can typically be 1 to 20 times the narrowest diameter of the first reduction section 64.

[0082] At the end of the first reaction chamber 58, additional carbon black raw material may be optionally introduced. This may be introduced using an injector or injector array 59 located in or near the second reduction section 65. Alternatively, it may be introduced using a lance located substantially upstream of the reduction section 65 but within the chamber 58.

[0083] After the introduction of any additional carbon black raw materials, the mixture flows into a second reaction chamber 61. It is then quenched using a cooling spray of liquid or vapor 62, as is known in the art. The length from the injection point 59 of the additional carbon black raw materials to the quenching position 62 is shown as 67 in Figure 1B. This length is set to provide a residence time that controls specific product properties, as is known in the art of furnace processes.

[0084] In an alternative configuration, carbon black raw materials are introduced at positions 63 and / or 56, and then any additional carbon black raw materials are introduced at positions 57 and / or 59, or simultaneously if both positions are used.

[0085] Generally, any of the carbon black feedstocks used in any of the methods of the present invention can be injected into the reactor in a single or multiple flow using an injector that penetrates the internal region of the high-temperature combustion gas flow. The injector can ensure a higher mixing ratio and shear between the high-temperature combustion gas and the carbon black feedstock(s). This ensures that the feedstock is thermally decomposed, preferably at a fast rate and / or in high yield, to form the carbon black of the present invention.

[0086] Figure 2 shows a specific example of a reactor that may be used to carry out the present invention and was used to produce the embodiments described below.

[0087] The carbon black raw material can be introduced at one or more locations in the reactor. This introduction can be carried out in the reactor throat 76 using one or more pipes or injectors 83. The reactor 90 has, for example, a combustion chamber 74 having a maximum diameter D chamber 75, as shown in Figure 2. The burner fuel can be introduced via one or more locations upstream of the initial introduction of the carbon black raw material. One or more pipes or injectors 71 may be locations where the burner fuel, or at least a portion thereof, is introduced into the combustion chamber 74. One or more pipes or injectors 72 may be locations where an oxidizer (e.g., air or oxygen) can be introduced into the combustion chamber 74.

[0088] In one embodiment of the present invention, the carbon black raw material is introduced at one location (e.g., 83) in the reactor, or at multiple locations in the reactor. Any further introduction of the carbon black raw material can be selected using one or more injectors (e.g., metal pipes located on the reactor wall) that introduce the raw material into the combustion chamber of the reactor, as shown, for example, in Figures 1A and 1B. The injectors may have an injector head or a spray head at their tip. The injectors on the tip may have, for example, one or more holes (two, three, four, or more) around the tip (multiple holes spaced roughly evenly apart).

[0089] As an option, the introduction of any carbon black raw material into the reactor and reaction flow can be such that the raw material is introduced perpendicular to the lateral flow of the reaction flow through the reactor, as shown, for example, in Figures 1A and 1B. Perpendicular can be ±15 degrees from true vertical injection of the raw material into the reaction flow.

[0090] As an option, the introduction of any carbon black raw material into the reactor can be carried out at a location with a diameter narrower than the diameter of the reactor to which the initial carbon black was introduced. This location can be considered a "throat" in some carbon black reactors. Figures 1A and 1B show an example of this throat or throat region in a reactor. This narrower diameter can be at least 10%, at least 20%, at least 30%, or 10% to 40% smaller than the diameter of the reactor to which the initial carbon black was introduced. In Figure 2, this is the D throat 76 relative to the D chamber 75.

[0091] After the raw materials (the initial carbon black raw material and any further optional carbon black raw materials) are combined in the reaction flow, the method of the present invention generally includes a step of quenching the reaction. In Figure 2, this is the quenching spray 81. The reaction zone after the throat 76, indicated as 80, has a reactor with a maximum diameter D. L quenching indicates the length from the point where the carbon black raw material is introduced to the point where quenching occurs. L quenching is the length from the last optional introduction of the carbon black raw material into the reactor to the quenching spray 81.

[0092] The reaction is stopped in the quenching zone of the reactor (see zone 8 in Figure 1A). As shown in Figure 1A, quenching 8 is located downstream of reaction zone 4 and involves spraying a quenching fluid, such as water, into the flow of newly formed carbon black particles. Generally, quenching helps to cool the carbon black particles, lower the temperature of the gas flow, and reduce the reaction rate. Q is the distance from the starting point of reaction zone 4 to quenching point 8, and varies depending on the location of the quenching. Optionally, quenching may be stepwise or performed at several points in the reactor. Pressure spraying, gas atomization spraying, or other quenching techniques are also available. With regard to completely quenching the reaction that forms carbon black, any conventional means for quenching the reaction downstream of the introduction of the carbon black production raw materials can be used, and these means are known to those skilled in the art. For example, a quenching fluid, which may be water or other suitable liquid, can be injected to stop the chemical reaction.

[0093] After rapid cooling, the cooled gas and carbon black pass downstream to any conventional cooling means and a separation means from which the product is recovered. Separation of carbon black from the gas stream can be easily achieved by conventional means such as a dust collector, cyclone separator, bag filter, or other means known to those skilled in the art. After separating the carbon black from the gas stream, the carbon black can optionally be subjected to a pelletizing step.

[0094] As an option, one or more of the burner fuel and / or carbon black raw materials or other components used in the method of the present invention may be preheated before being introduced into the reactor. For example, U.S. Patent No. 3,095,273 issued to Austin on June 25, 1963; U.S. Patent No. 3,288,696 issued to Orbach on November 29, 1966; U.S. Patent No. 3,984,528 issued to Cheng et al. on October 5, 1976; U.S. Patent No. 4,315,901 issued to Cheng et al. on February 16, 1982; U.S. Patent No. 4,765,964 issued to Gravley et al. on August 23, 1988; and December 1999. Suitable preheating temperatures and / or preheating techniques can be used in the present invention as described in U.S. Patent No. 5,997,837 issued to Lynum et al. on 7th of the month, U.S. Patent No. 7,097,822 issued to Godal et al. on 29 August 2006, U.S. Patent No. 8,871,173(B2) issued to Nester et al. on 28 October 2014, or Canadian Patent No. 682982 (all documents are incorporated herein by reference in their entirety).

[0095] Alternatively, this method may be carried out in the absence of at least one Group IA or Group IIA element (or its ion) of the periodic table, or at least one substance containing it.

[0096] As an option, any of the methods of the present invention may include a step of introducing at least one substance which is or contains at least one Group IA or Group IIA element (or an ion thereof) of the periodic table. Preferably, the substance contains at least one alkali metal or alkaline earth metal. Examples include lithium, sodium, potassium, rubidium, cesium, francium, calcium, barium, strontium, or radium, or combinations thereof. Any mixture of one or more of these components may be present in the substance. Such substance may be a solid, a solution, a dispersion, a gas, or any combination thereof. Two or more substances having the same or different Group IA or Group IIA metals may be used. If multiple substances are used, these substances may be added together, separately, sequentially, or at different reaction sites. For the purposes of the present invention, the substance may be the metal (or metal ion) itself, a compound containing one or more of these elements (including salts containing one or more of these elements), and so on. Preferably, the substance can introduce a metal or metal ion into the reaction in progress to form the carbon black product. For the purposes of the present invention, preferably, the substance is introduced before complete quenching as described above. For example, the substance can be added at any point before complete quenching, including before the introduction of one or both of the carbon black production raw materials, during the introduction of any of the carbon black production raw materials, after the introduction of any or all of the carbon black production raw materials, or after the introduction of all raw materials but before complete quenching. Two or more points of introduction of the substance can be used. The amount of the group IA or group IIA metal-containing substance can be any amount as long as the carbon black product can be formed. For example, the amount of substance can be added such that the final carbon black product contains 10 ppm or more, or 30 ppm or more, or 50 ppm or more, or 100 ppm or more, or 200 ppm or more of the group IA or group IIA element.Other amounts of group IA or group IIA elements present in the formed carbon black product include approximately 200 ppm to approximately 5000 ppm or more, and other ranges include approximately 300 ppm to approximately 1000 ppm, or approximately 500 ppm to approximately 1000 ppm. These levels may relate to metal ion concentrations. As mentioned above, these amounts of group IA or group IIA elements present in the formed carbon black product may relate to one element or two or more group IA or group IIA elements, and therefore may represent the total amount of group IA or group IIA elements present in the formed carbon black product. Substances can be added in any form, including any conventional means. In other words, substances can be added in the same way that carbon black production raw materials are introduced. Substances can be added as gases, liquids, or solids, or any combination thereof. Substances can be added at one or more locations, and can be added in a single or multiple flow. Substances can be mixed with raw materials, fuels, and / or oxidizers before or during their introduction.

[0097] With respect to carbon black formed by any of the methods of the present invention, the carbon black formed or manufactured may be any reinforced or unreinforced grade of carbon black. Examples of reinforced grades are N110, N121, N220, N231, N234, N299, N326, N330, N339, N347, N351, N358, and N375. Examples of semi-reinforced grades are N539, N550, N650, N660, N683, N762, N765, N774, N787, and / or N990.

[0098] Carbon black can also be furnace black.

[0099] In certain embodiments, the carbon black formed is less than or equal to 2% of the total weight of the carbon black, for example, less than 1.75%, less than 1.5%, less than 1.25%, less than 1%, less than 0.75%, or 0.5% to 2%, 0.6% to 2%, 0.7% to 2%, 0.8% to 2%, 0.9% to 2%, 1% to 2%, 1.1% to 2%, 1.2% to 2%, 1.3% to 2%, 1.4%. The carbon black may have a biogenic carbon content of %~2%, 1.5%~2%, 1.6%~2%, 0.5%~1.9%, 0.5%~1.8%, 0.5%~1.7%, 0.5%~1.6%, 0.5%~1.5%, 0.5%~1.4%, 0.5%~1.3%, 0.5%~1.2%, 0.5%~1.1%, 0.5%~1%, 0.5%~0.9%, 0.5%~0.8%, and 0.5%~0.7%, where % is by weight. The measurement of the biogenic carbon content can be carried out according to ASTM D6866. Optionally low biogenic content can be obtained when the carbon black forming material contains a small amount (e.g., less than 5% by weight) or no sustainably sourced bio-based material at all.

[0100] Carbon black can be characterized by its specific surface area, structure, aggregate size, shape, and distribution, as well as / or surface chemical and physical properties. The properties of carbon black are analytically determined by tests known in the art. For example, nitrogen adsorption surface area, and another measure of surface area, statistical thickness surface area (STSA), are determined by nitrogen adsorption according to ASTM test procedure D6556-10. Iodine value can be measured using ASTM procedure D-1510-13. The "structure" of carbon black represents the size and complexity of the carbon black aggregates formed by the fusion of primary carbon black particles. As used herein, the structure of carbon black can be measured as the oil absorption number (OAN) of unground carbon black, expressed as the number of milliliters of oil per 100 grams of carbon black, according to the procedure described in ASTM D-2414-13. The oil absorption number (COAN) of a compressed sample measures the portion of the carbon black structure that does not readily change under the application of mechanical stress. COAN is measured according to ATM D3493-13. Aggregate size distribution (ASD) is measured according to ISO 15825 using a disk centrifuge with a Brookhaven Instruments Model BI-DCP.

[0101] Carbon black materials with properties suitable for specific applications may be selected and defined by ASTM standards (see, for example, ASTM D 1765-03 Standard Classification System for Carbon Blacks Used in Rubber Products), Cabot Corporation specifications (see website www.cabot-corp.com), or other commercial grade specifications.

[0102] Carbon black is 5m 2 / g~250m 2 / g, 11m2 / g to 250m 2 / g, 20m² / g to 250m 2 / g or more, for example, at least 70m 2 / g, for example, 70m 2 / g to 250m 2 / g, or 80m² / g to 200m 2 / g, or 90m 2 / g to 200m 2 / g, or 100m 2 / g to 180m 2 / g, 110m 2 / g to 150m 2 / g, 120m 2 / g to 150m 2 / g, and any other STSA within such ranges. Alternatively, the carbon black can have an iodine number (I₂ No.) of about 5 mg I₂ / g to about 35 mg I₂ / g carbon black (according to ASTM D1510).

[0103] The carbon black particles disclosed herein can have a Brunauer / Emmett / Teller (BET) surface area of 5m, as measured by the BET technique following the procedure of ASTM D6556 2 / g to 300m 2 / g, for example, 50m 2 / g to 300m 2 / g, for example, 100m 2 / g to 300m 2 / g. The BET surface area can be about 100m 2 / g to about 200m 2 / g, or about 200m 2 / g to about 300m 2 / g.

[0104] The oil adsorption capacity (OAN) can be 40 mL / 100 g to 200 mL / 100 g, for example, 60 mL / 100 g to 200 mL / 100 g, for example, 80 mL / 100 g to 200 mL / 100 g, for example, 100 mL / 100 g to 200 mL / 100 g, or 120 mL / 100 g to 200 mL / 100 g, 140 mL / 100 g to 200 mL / 100 g, 160 mL / 100 g to 200 mL / 100 g, or for example, 40 mL / 100 g to 150 mL / 100 g.

[0105] COAN can be within the range of approximately 40 mL / 100g to approximately 150 mL / 100g, for example, approximately 55 mL / 100g to approximately 150 mL / 100g, for example, approximately 80 mL / 100g to approximately 150 mL / 100g, or approximately 80 mL / 100g to approximately 120 mL / 100g.

[0106] Carbon black can be a carbon product containing silicon-containing species and / or metal-containing species, which can be achieved by including a further step of introducing such species together with or in addition to any or both of the carbon black production raw materials. For the purposes of the present invention, carbon black can be a multiphase aggregate (also known as silicon-treated carbon black, e.g., ECOBLAK® material from Cabot Corporation) comprising at least one carbon phase and at least one metal-containing species phase or silicon-containing species phase.

[0107] As described above, the carbon black can be rubber black, in particular, a reinforced grade of carbon black or a semi-reinforced grade of carbon black.

[0108] As an option, the carbon black of the present invention may have functional or chemical groups (e.g., derived from ionic or nonionic small molecules or polymers) that are directly bonded (e.g., covalently) to the carbon surface. Examples of functional groups that can be directly bonded (e.g., covalently) to the surface of carbon black particles and methods for carrying out surface modification are described, for example, in U.S. Patent No. 5,554,739 issued to Belmont on September 10, 1996, and U.S. Patent No. 5,922,118 issued to Johnson et al. on July 13, 1999 (both incorporated herein by reference). As an example, surface-modified carbon black that can be used herein is obtained by treating carbon black with a diazonium salt formed by the reaction of either sulfanilic acid or para-aminobenzoic acid (PABA) with HCl and NaNO2. For example, surface modification by a sulfanilic or para-aminobenzoic acid process using a diazonium salt results in carbon black having an effective amount of hydrophilic moiety on the carbon coating.

[0109] Carbon black can be surface-modified in accordance with U.S. Patent No. 8,975,316 to Belmont et al., the contents of which are incorporated herein by reference in their entirety.

[0110] Other techniques that can be used to provide functional groups bonded to the surface of carbon black are described in U.S. Patent No. 7,300,964, issued to Niedermeier et al. on November 27, 2007.

[0111] Oxidized (modified) carbon black can be prepared in a manner similar to that used for carbon black, for example, as described in U.S. Patent No. 7,922,805 issued to Kowalski et al. on April 12, 2011, and U.S. Patent No. 6,471,763 issued to Karl on October 29, 2002 (these are incorporated herein by reference in their entirety). Oxidized carbon black is obtained by oxidizing with an oxidizing agent to introduce ionic groups and / or ionizable groups onto the surface. Such particles may have a higher degree of oxygen-containing groups on the surface. Examples of oxidizing agents include, but are not limited to, oxygen gas, ozone, peroxides such as hydrogen peroxide, persulfates including sodium persulfate and potassium persulfate, hypohalites such as sodium hypochlorite, oxidizing acids such as nitric acid, and transition metal-containing oxidizing agents such as permanganates, osmium tetroxide, chromium oxide, or cerium ammonium nitrate. Mixtures of oxidizing agents, in particular mixtures of gaseous oxidizing agents such as oxygen and ozone, can also be used. Other surface modification methods, such as chlorination and sulfonylation, can also be used to introduce ionic groups or ionizable groups.

[0112] This invention is partly based on the currently recognized need to develop a class of carbon black that can be produced using a lower overall combustion rate (OAC). Overall combustion rate is defined as the proportion of oxygen added to the entire reactor compared to the total amount of oxygen required to stoichiometrically react with all the fuel flow added to the entire reactor. By reducing the OAC and producing the same or essentially the same carbon black (based on parameters such as nitrogen surface area and / or COAN), it is possible to achieve a carbon black production process that is more yielding, more economically efficient, and / or more environmentally friendly.

[0113] Carbon black can be used in a variety of applications, such as as a reinforcing agent in rubber products, for example, in tire components.

[0114] Carbon black can be incorporated into rubber articles used, for example, in tire treads, particularly treads; sub-treads; wire skims; sidewalls; cushioning rubber for retreaded tires; and other tire applications, such as those used in tires for passenger cars, light vehicles, trucks and buses, off-road ("OTR") tires, and aircraft tires.

[0115] In other applications, the particles can be used in industrial rubber articles such as engine mounts, hydro mounts, bridge bearings and seismic isolation devices, tank trucks or treads, mining belts, hoses, gaskets, seals, blades, gap fillers, bumpers, and vibration damping components.

[0116] Carbon black may be added in place of or in addition to a primary reinforcing agent for tire components and / or other industrial rubber end applications. Carbon black may be combined with natural and / or synthetic rubber in a suitable dry or wet mixing process based on an internal batch mixer, continuous mixer, or roll mill.

[0117] Alternatively, carbon black may be mixed with rubber by a liquid masterbatch process. For example, a slurry containing the particles described herein may also be combined with an elastomer latex in a vat and then coagulated by adding a coagulant such as an acid using the technique described in U.S. Patent No. 6,841,606.

[0118] Carbon black can be introduced in accordance with U.S. Patent No. 6,048,923, issued to Mabry et al. on April 11, 2000, which is incorporated herein by reference in its entirety. For example, a method for preparing an elastomer masterbatch may include simultaneously supplying a granular packing fluid and an elastomer latex fluid to the mixing zone of a solidification reactor. The solidification zone extends from the mixing zone and preferably has a gradually increasing cross-sectional area downstream from the inlet end to the discharge end. The elastomer latex may be natural or synthetic, and the granular packing includes, is essentially, or consists of the materials described above. The granular packing is preferably supplied to the mixing zone as a continuous high-speed jet of injection fluid, and the latex fluid is supplied at a low speed. The velocity, flow rate, and particle concentration of the particulate filler fluid are sufficient to cause high-shear mixing of the latex fluid and turbulent mixing of the mixture flow in at least the upstream portion of the solidification zone, thereby substantially completely solidifying the elastomer latex with the particulate filler before the discharge end. Substantially complete solidification can be achieved without the need for an acid or salt solidifying agent. Additional elastomers may be added to the material coming out of the discharge end of the solidification reactor, as disclosed in U.S. Patent No. 6,075,084, which is incorporated herein by reference in its entirety. The solidified material may then be fed to a dewatering extruder, as disclosed in U.S. Patent No. 6,929,783, which is incorporated herein by reference in its entirety. Other examples of preferred masterbatch processes are disclosed in U.S. Patent No. 6,929,783 by Chung et al., U.S. Patent Application Publication No. 2012 / 0264875(A1) by Berriot et al., U.S. Patent Application Publication No. 2003 / 0088006(A1) by Yanagisawa et al., and European Patent No. 1834985(B1) issued to Yamada et al.

[0119] Carbon black can be evaluated in appropriate rubber formulations using natural or synthetic rubber. The appropriate amount of carbon black to use can be determined by conventional experiments and calculations, taking into account factors such as the typical filling amount of standard ASTM furnace black in comparable manufacturing processes, parameters specific to the technology and / or equipment used, the presence or absence of other additives, and the desired properties of the final product.

[0120] The performance of carbon black as a reinforcing agent for rubber compounds can be evaluated, for example, by comparing the performance of a rubber composition utilizing the particles with the performance of a comparative rubber composition that is identical in all respects except for the use of a carbon black grade suitable for a given application. Alternatively, the values ​​obtained for compositions prepared according to the present invention can be compared with values ​​known in the art that are relevant to desired parameters in a given application.

[0121] Appropriate tests include the green rubber test, the curing test, and the cured rubber test. Among the appropriate green rubber tests, ASTM D4483 provides a test method for the ML1+4 Mooney viscosity test at 100°C. The scorch time is measured according to ASTM D4818.

[0122] The hardening curve is obtained according to ASTM D5289 at 0.5°, 100 cpm, and 150C (NR) to 160C (SBR) using a rubber processing tester (RPA2000).

[0123] The performance characteristics of the cured sample can be determined by a series of appropriate tests. Tensile strength, elongation at fracture, and stress at various strains (e.g., 100% and 300%) are all obtained by ASTM D412 Method A. Dynamic mechanical properties, including storage modulus, loss modulus, and tanδ, are obtained by strain sweep tests at 10 Hz, 60°C, and various strain amplitudes from 0.1% to 63%. Shore A hardness is measured according to ASTM D2240. Tear strength of die B cured rubber samples is measured according to ASTM D624.

[0124] The undispersed area is calculated by analyzing images obtained by reflection-mode optical microscopy of the cross-sectional area of ​​a cured rubber compound, according to various reported methods. Dispersion can also be expressed by the Z value (measured after reticularization according to the method described in the paper titled "New Reference value for the description of Filler Dispersion with the Dispergrader 1000NT" by S. Otto and Al in Kautschuk Gummi Kunststoffe, 58Jahrgang, NR7-8 / 2005). Standard ISO 11345 specifies a visual method for rapid comparative evaluation of the macrodispersion of carbon black and carbon black / silica in rubber.

[0125] Abrasion resistance is quantified as an index based on the friction loss of hardened rubber by Cabot Abrader (Lambourn type). Attractive abrasion resistance results can indicate favorable wear characteristics. Good hysteresis results can be associated with lower rolling resistance (and correspondingly higher fuel economy) for automotive tire applications, reduced heat buildup, tire durability, tread life and casing life, and fuel economy features for automobiles.

[0126] The iodine value (I2 No.) is determined according to ASTM test procedure D1510. The STSA (Statistical Thickness Surface Area) is determined based on ASTM test procedure D-5816 (measured by nitrogen adsorption). The OAN is determined based on ASTM D2414 or D1765 (e.g., D1765-20). The COAN is determined based on ASTM D3493 (e.g., D3493-20).

[0127] Unless otherwise specified, all material percentages expressed herein as percentages are weight percentages.

[0128] The present invention will be further illustrated by the following embodiments, which are intended to be essentially illustrative.

[0129] Examples

[0130] For the purposes of the present invention and the examples presented herein, the following explanations of some terms are provided.

[0131] Total Combustion Rate (OAC) Ratio: The total combustion rate is defined as the percentage of oxygen added to the entire reactor compared to the total amount of oxygen required to react stoichiometrically with the entire fuel flow (burner fuel and carbon black production raw materials) added to the entire reactor. Under stoichiometric conditions, the OAC is 100%. If the mixture is fuel-rich, the OAC is less than 100%, and if the fuel is lean, the OAC is greater than 100%. Carbon black production is preferably carried out when the OAC is substantially fuel-rich, typically less than 60, and more often less than 40.

[0132] The primary combustion rate (PC), also known as the burner combustion rate, is the same as the OAC, except that it considers only the fuel and oxygen flow introduced into the burner (74 in Figure 2). This does not include the fuel or oxygen flow introduced downstream of the burner (e.g., 84 in Figure 2). The primary combustion rate (PC) is typically lean and typically ranges from 110% to 600%.

[0133] Yield: The yield is the mass of solid carbon obtained per unit of the total mass of raw materials injected into the carbon black reactor, excluding the burner fuel used in the combustion chamber shown in Figure 2, and is expressed in units of [kg C / kg raw materials]. The yield is equal to the total mass percentage of solid carbon produced in the reactor divided by the total mass percentage of raw materials, and is calculated based on measured values ​​of the reactor input rate and composition, as well as the tail gas composition. The yield may include sulfur, ash, and other components of carbon black in addition to carbon, but in these examples, the yield includes only the carbon content of the carbon black.

[0134] Toluene extractable components (SP20), I2, STSA, OAN, and COAN

[0135] OAN and COAN are analyzed on the dry pellets according to the ASTM standards specified above. I2 valent and STSA are analyzed on the dry pellets according to the ASTM methods specified above.

[0136] Reactor configuration and operation

[0137] Example 1

[0138] In Example 1, decant oil was used as the carbon black raw material (Table 6), and heavy TPO (Table 4) alone (100% by weight TPO) or approximately 50% by weight heavy TPO with approximately 50% by weight natural gas (Table 5) was used as the burner fuel. For comparison, 100% by weight natural gas (Table 5) was used as the burner fuel.

[0139] Each of these three burner fuel combinations was tested under various total combustion rate (OAC) flow conditions as shown in Table 7. Under all tested conditions, the process air flow rate was 1600 Nm³. 3 The flow rate was / h, and the process air inlet temperature was 500C. The burner combustion rate was 150% in all cases. The decanted oil carbon black raw material inlet temperature was 190C under all conditions. Table 7 shows the natural gas flow rate, heavy TPO flow rate, OAC, carbon black raw material flow rate, potassium additive flow rate, quenching water flow rate, and quenching length distance L. 急冷 The flow parameters, including those mentioned above, are shown as they vary for each condition.

[0140] As shown in Figure 2, the carbon black furnace method is used to combine burner fuel and high-temperature process air in a combustion chamber to provide a high-temperature post-combustion gas flow. The combustion chamber is lined with refractory material, and its inner diameter is shown in Table 3.

[0141] Natural gas and TPO burner fuel, along with high-temperature process air, were introduced into the burners (71 and 72) under the flow conditions shown in Table 7. Liquid heavy TPO was sprayed, and both TPO and natural gas were mixed and burned through a conventional combustion apparatus.

[0142] Next, the post-combustion gas from the chamber flowed into the contraction section, thereby entering the narrower throat (76 in Figure 2). In the throat, in all cases of the examples, the carbon black raw material was injected radially through the injector 83 toward the center of the reactor, positioned perpendicular to the direction of the post-combustion gas flow, as shown in Figure 2.

[0143] The throat was mounted in a reactor chamber lined with refractory material. The reactor chamber provided residence time for the feedstock to complete the thermal decomposition into carbon black particles. Quenching was performed using a water spray at a distance L quench 79 downstream of the injection surface shown in Figure 2, as is typical for the carbon black furnace method (see Table 7 for details). Downstream of quenching, a filter was used to separate the carbon black particles from the tail gas stream. The carbon black in the filter was sampled for I2 absorption and toluene extractable components (SP20). The carbon black was then pelletized and dried for STSA, OAN, and COAN measurements.

[0144] The filtered tail gas was sampled, its composition was measured under each condition, and the yield was determined. [Table 3]

[0145] The heavy TPO used as burner fuel was distilled by the supplier to obtain a high flash point for easier storage. The TPO used (Polimix 330) has the following properties / characteristics: [Table 4]

[0146] In the examples, when supplied to the combustion chamber shown in Figure 2, the natural gas had the measured average composition shown in Table 5. The components were measured by gas chromatography.

[0147] [Table 5]

[0148] The liquid decanted oils used in these examples were as shown in Table 6 below (the D-xxxx method has been established by ASTM International). [Table 6] [Table 7]

[0149] result

[0150] The results are shown in Figures 3 to 7 (Figures 5 to 7 show data only for 40 ppm potassium addition). Carbon black formed from experiments where the burner fuel was 100 wt% heavy TPO (HTPO, square; dotted line), or approximately 50 wt% HTPO and approximately 50 wt% natural gas (NG, triangle, dashed line), or 100 wt% NG (diamond; solid line) was collected and analyzed. The primary combustion rate was 150% in all cases. Figure 3 shows that when the burner fuel was 100% HTPO or 50 / 50 HTPO / NG, the required OAC was lower compared to NG alone in order to achieve a specific surface area (STSA). In other words, the present invention provides carbon black that has a specific surface area but is produced using a lower OAC. Generally, the lower the OAC, the higher the yield.

[0151] Figure 4 shows that, as expected from the lower OAC, the carbon black yield for a given STSA was actually higher when the burner fuel was 100% HTPO or 50% / 50% HTPO / NG compared to NG alone.

[0152] Figure 5 shows that when the burner fuel was 100% HTPO or 50% / 50% HTPO / NG, the COAN for a given STSA was higher compared to NG alone. For carbon black, in many cases, the higher the structure (OAN and / or COAN), the higher the value.

[0153] Figure 6 shows that when the burner fuel was 100% HTPO or 50% / 50% HTPO / NG, the specific coloring power in a given STSA was essentially the same as when NG was used alone.

[0154] Figure 7 shows that when the burner fuel was 100% HTPO or 50% / 50% HTPO / NG, the iodine value in a given STSA was essentially the same as when NG was used alone.

[0155] Example 2

[0156] In Example 2, decant oil was used as a carbon black raw material (Table 6), and liquid bio-oil (a product of rapid pyrolysis of biomass) was used as burner fuel in approximately 75% by weight along with 25% by weight natural gas. For comparison, 100% by weight natural gas (Table 5) was used as burner fuel.

[0157] Each of these burner fuel combinations is 1800 Nm 3 Tests are conducted across various total combustion rate (OAC) flow conditions as shown in Table 9, using a process air flow rate of / h and a process air inlet temperature of 500°C. The decanted oil (listed in Table 6) carbon black feedstock inlet temperature is maintained at 175°C for all conditions. Table 9 shows the natural gas flow rate, bio-oil flow rate, OAC, carbon black feedstock flow rate, potassium additive flow rate, quenching water flow rate, and quenching length distance L. 急冷 The flow parameters, including those mentioned above, are shown as they vary for each condition.

[0158] As shown in Figure 2, the carbon black furnace method is used to mix burner fuel and high-temperature process air in the combustion chamber to provide a high-temperature combustion gas flow. The combustion chamber is lined with refractory material, and its inner diameter is as follows: D チャンバ =20.3cm, D スロート =11.43cm, D 反応器 = 45.7cm.

[0159] Natural gas and bio-oil burner fuels, along with high-temperature process air, are introduced into the burners (71 and 72) under the flow conditions shown in Table 9. Bio-oil is sprayed, and both the bio-oil and natural gas are mixed and burned through a combustion device typical of conventional technology.

[0160] Next, the post-combustion gas from the chamber flows into the contraction section, thereby entering the narrower throat (76 in Figure 2). In the throat, in all cases of the embodiment, the carbon black raw material is injected radially through the injector 83 toward the center of the reactor, positioned perpendicular to the direction of the post-combustion gas flow, as shown in Figure 2.

[0161] The throat is fitted into a reactor chamber lined with refractory material. The reactor chamber provides residence time for the raw materials to complete the thermal decomposition into carbon black particles. Quenching is performed using a water spray at a distance L quench 79 downstream of the injection surface shown in Figure 2, as is typical for the carbon black furnace process (see Table 8 for details). Downstream of quenching, a filter is used to separate the carbon black particles from the tail gas stream.

[0162] Typical bio-oils have less sulfur, more ash, and more water than the TPO used in Example 1. However, they may have less asphaltene, or even no asphaltene at all. Typical bio-oils typically have more water than the TPO used in Example 1, and as a result, they may be denser in terms of mass, but their energy density may be lower. [Table 8]

[0163] Any water in bio-oil results in a slightly lower yield than the natural gas control, but the use of bio-oil is expected to enable comparable growth in surface area (STSA) as a function of total combustion rate (OAC) compared to 100% natural gas. Furthermore, by using bio-oil as burner fuel, along with decanted oil as a carbon black formation raw material, the bio-oil-derived carbon in the final carbon black product is expected to be less than 2% by weight.

[0164] The present invention includes the following aspects / embodiments / features in any order and / or any combination. 1. The present invention relates to a method for producing carbon black, Introducing burner fuel containing at least one type of sustainable burner fuel into the carbon black reactor, In the reactor, ignition is performed to form a flow of high-temperature gas from the burner fuel, Introducing at least one type of carbon black production raw material into the carbon black reactor at one or more points of introduction, Combining at least one carbon black production raw material with a high-temperature gas flow to form carbon black in a reaction flow, Rapid cooling of the reaction flow containing carbon black, To recover the carbon black, Includes methods. 2. The method according to any embodiment / feature / appearance described above or below, wherein at least one sustainable burner fuel is one or more of the following: tire pyrolysis oil, plastic pyrolysis oil, plant-derived oil, oil derived from the pyrolysis of municipal solid waste, oil derived from the pyrolysis or decomposition of biomass (e.g., animal, plant, tree, fruit, or vegetable) or other agricultural waste, oil derived from the processing of paper manufacturing by-products, and / or other oils primarily sourced from bio-derived materials, or any combination thereof. 3. The method according to any of the above or below embodiments / features / appearances, wherein the burner fuel comprises at least 50% by weight of the at least one type of sustainable burner fuel, based on the total weight of the burner fuel. 4. The method according to any of the above or below embodiments / features / appearances, wherein at least one sustainable burner fuel is tire pyrolysis oil (TPO). 5. The method according to any of the above or below embodiments / features / appearances, wherein the burner fuel contains at least 50% by weight of the TPO based on the total weight of the burner fuel. 6. The method of any of the above or below embodiments / features / appearances, wherein the burner fuel comprises at least 70% by weight of the at least one type of sustainable burner fuel, based on the total weight of the burner fuel. 7. The method according to any of the above or below embodiments / features / appearances, wherein the carbon black has a bio-derived carbon content of 2% by weight or less. 8. The method of any of the above or below embodiments / features / appearances, which ignites and forms a burner that consumes substantially or completely sustainable burner fuel. 9. The method of any above or below embodiment / feature / appearance, wherein less than 5% by weight or less than 1% by weight of sustainable burner fuel, based on the total weight of the carbon black production raw materials, is available for forming the carbon black. 10. The method according to any of the above or below embodiments / features / appearances, wherein sustainable burner fuel is present in an amount sufficient to increase the yield of carbon black formed by 1% to 8% compared to burner fuel consisting of 100% natural gas. 11. The method according to any of the above or below embodiments / features / appearances, wherein sustainable burner fuel is present in an amount sufficient to increase the COAN of the carbon black formed by 1% to 8% compared to burner fuel consisting of 100% natural gas. 12. Methods of any of the above or below embodiments / features / appearances, wherein TPO includes heavy TPO. 13. The method according to any of the above or below embodiments / features / appearances, wherein TPO consists of heavy TPO. 14. The method according to any of the above or below embodiments / features / appearances, wherein the recovered carbon black is N110, N121, N220, N231, N234, N299, N326, N330, N339, N347, N351, N358, N375, N539, N550, N650, N660, N683, N762, N765, N774, N787, or N990 grade carbon black. 15. Carbon black formed or manufactured by the method described in any of the above or below embodiments / features / appearances.

[0165] The present invention may include any combination of the various features or embodiments described above and / or below in any sentence and / or paragraph of this specification. Any combination of the features disclosed herein is deemed to be part of the invention and is not intended to limit the range of combinatable features.

[0166] The applicants hereby specifically incorporate into this disclosure the entire contents of all cited references. Furthermore, where a quantity, concentration, or other value or parameter is given as a range, a preferred range, or a list of preferred upper and lower limits, this should be understood as specifically disclosing all ranges formed from any pair of any upper or preferred value and any lower or preferred value of any range, regardless of whether the range is disclosed separately. Where a range of numerical values ​​is described herein, unless otherwise specified, the range is intended to include its endpoints, as well as all integers and fractions within that range. The range of the present invention is not intended to be limited to any specific values ​​enumerated when defining a range.

[0167] Other embodiments of the present invention will be apparent to those skilled in the art from the discussion herein and the practice of the present invention disclosed herein. This specification and the examples, together with the true scope and spirit of the present invention as set forth by the following claims and equivalents, are intended to be illustrative only.

Claims

1. A method for producing carbon black, Introducing burner fuel containing at least one type of sustainable burner fuel into the carbon black reactor, In the reactor, ignition is performed to form a flow of high-temperature gas from the burner fuel, Introducing at least one type of carbon black production raw material into the carbon black reactor at one or more points of introduction, The process involves combining the aforementioned at least one carbon black production raw material with the flow of the high-temperature gas to form carbon black in a reaction flow, The reaction flow containing the carbon black is rapidly cooled, To recover the aforementioned carbon black, Methods that include...

2. The method according to claim 1, wherein the at least one sustainable burner fuel is one or more of the following: tire pyrolysis oil, plastic pyrolysis oil, plant-derived oil, oil derived from the pyrolysis of municipal solid waste, oil derived from the pyrolysis or decomposition of biomass or other agricultural waste, oil derived from the processing of paper manufacturing by-products, and / or other oils mainly sourced from bio-derived materials, or any combination thereof.

3. The method according to claim 1 or 2, wherein the burner fuel comprises at least 50% by weight of the at least one sustainable burner fuel based on the total weight of the burner fuel.

4. The method according to any one of claims 1 to 3, wherein the at least one sustainable burner fuel is tire pyrolysis oil (TPO).

5. The method according to any one of claims 1 to 4, wherein the burner fuel contains at least 50% by weight of the TPO based on the total weight of the burner fuel.

6. The method according to any one of claims 1 to 5, wherein the burner fuel comprises at least 70% by weight of the at least one sustainable burner fuel based on the total weight of the burner fuel.

7. The method according to any one of claims 1 to 6, wherein the carbon black has a bio-derived carbon content of 2% by weight or less.

8. The method according to any one of claims 1 to 7, wherein ignition and formation consume substantially or completely the sustainable burner fuel.

9. The method according to any one of claims 1 to 8, wherein, based on the total weight of the carbon black production raw materials, less than 5% by weight or less than 1% by weight of sustainable burner fuel is available to form the carbon black.

10. The method according to any one of claims 1 to 9, wherein the sustainable burner fuel is present in an amount sufficient to increase the yield of carbon black formed by 1% to 8% compared to a burner fuel consisting of 100% natural gas.

11. The method according to any one of claims 1 to 10, wherein the sustainable burner fuel is present in an amount sufficient to increase the COAN of the carbon black formed by 1% to 8% compared to a burner fuel consisting of 100% natural gas.

12. The method according to any one of claims 1 to 11, wherein the TPO includes heavy TPO.

13. The method according to any one of claims 1 to 12, wherein the TPO is heavy TPO.

14. The method according to any one of claims 1 to 13, wherein the recovered carbon black is carbon black of grade N110, N121, N220, N231, N234, N299, N326, N330, N339, N347, N351, N358, N375, N539, N550, N650, N660, N683, N762, N765, N774, N787, or N990.