Highly branched polythioethers, curable high refractive index compositions and articles thereof, and methods for producing such compounds and articles.

Highly branched polythioethers with terminal functional groups react with polyfunctional compounds to create high refractive index layers in optical devices, addressing the need for improved thin-film encapsulation in displays by enhancing performance and durability.

JP2026539190APending Publication Date: 2026-11-203M INNOVATIVE PROPERTIES CO
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
JP2026526884
Authority / Receiving Office
JP · JP
Patent Type
Applications
Current Assignee / Owner
Priority Date
2023-11-08
Filing Date
2024-10-11
Publication Date
2026-11-20

AI Technical Summary

Technical Problem

Existing thin-film encapsulation technologies in optical displays, such as OLEDs and quantum dot displays, face challenges in achieving high refractive index layers that are inkjet printable and can be used to prepare curable organic compositions for enhancing the performance and lifespan of these devices.

Method used

The development of highly branched polythioethers with multiple terminal functional groups, such as carbon-carbon double bonds or thiol groups, which react with polyfunctional compounds via a thiol-ene reaction to form curable compositions with a high refractive index, suitable for use in optical devices.

Benefits of technology

The resulting curable compositions provide high refractive index layers that enhance the performance and lifespan of optical devices by forming smooth, precise, and durable organic layers in thin-film encapsulation, without the need for solvent-based deposition methods.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure 2026539190000001_ABST
    Figure 2026539190000001_ABST
Patent Text Reader

Abstract

The invention describes a highly branched polythioether having multiple terminal functional groups, wherein the terminal functional groups have terminal carbon-carbon double bonds or thiol groups, and the highly branched polythioether has a refractive index of at least 1.600 and a number-average molecular weight of at least 1000 g / mol and up to 5000 g / mol. In some embodiments, the highly branched polythioether reacts with a polyfunctional compound, the polyfunctional compound having complementary terminal functional groups that can react with the highly branched polythioether in a thiol-ene reaction. These curable compositions, when cured, have a high refractive index of at least 1.660 (measured at 450 nm) and can be used in optical devices.
Need to check novelty before this filing date? Find Prior Art

Description

[Technical Field]

[0001] This specification discloses highly branched polythioethers having multiple terminal thiol groups or carbon-carbon double bonds, and methods for producing the same. It is also disclosed that these highly branched polythioethers may be reacted with polyfunctional compounds in a thiol-ene reaction to achieve compositions with a high refractive index. For example, curable compositions and articles using such compositions in optical devices are disclosed. [Background technology]

[0002] In the display industry, a series of alternating organic and inorganic layers (known as thin-film encapsulation, or TFE) can be used on top of optical displays such as organic light-emitting devices (OLEDs) or quantum dot displays to protect the underlying display and improve its performance and lifespan.

[0003] In thin-film encapsulation, the function of the inorganic layer is to block the intrusion of air and moisture into the underlying optical device. The organic layer has two functions: 1) to planarize the substrate and present a smooth interface for the deposition of the inorganic layer; and 2) to decouple any defects (pinholes, microcracks) that may occur in the inorganic layer on both sides of the organic layer. The organic layer can be considered a buffer layer that is crucial for the success of the inorganic layer barrier function.

[0004] In some embodiments, it is desirable to identify novel compounds having a high refractive index that are inkjet printable, can be used to prepare curable organic compositions, and can be used to prepare high refractive index layers. [Overview of the project]

[0005] In one embodiment, a highly branched polythioether is described. The highly branched polythioether has multiple terminal carbon-carbon double bonds or thiol groups, and has a refractive index of at least 1.600, and a number-average molecular weight of at least 1000 g / mol and up to 5000 g / mol.

[0006] In one embodiment, a method for producing a highly branched polythioether is described. The method comprises combining at least one unsaturated compound having p independent vinyl or allyl groups and consisting of C, H, and optionally O and / or Si atoms, where each p is an independent integer of 2 or more, and at least one organic thiol having q thiol groups and consisting of C, H, S, and optionally O atoms, where each q is an independent integer of 2 or more.

[0007] In one embodiment, a curable composition is described, and the curable composition is (i) A highly branched polythioether having multiple terminal carbon-carbon double bonds or thiol groups, wherein the highly branched polythioether has a refractive index of at least 1.660 and a number-average molecular weight of at least 1000 g / mol and at most 5000 g / mol; (ii) at least one polyfunctional compound and It contains, and components (i) and (ii) react via a thiol-ene reaction; The curable composition is substantially solvent-free.

[0008] In another embodiment, an article is disclosed. The article comprises a substrate having a first main surface and a second main surface; A cured organic layer adjacent to at least a portion of the second main surface of the substrate, wherein the cured organic layer is (i) Highly branched polythioethers; and (ii) at least one polyfunctional compound An organic layer derived from; The inorganic barrier layer in contact with the hardened organic layer The cured organic layer contains [the specified material] and has a refractive index of at least 1.660 (measured at 450 nm).

[0009] In yet another embodiment, a method for preparing an article is described. The method is: To provide a substrate having a first main surface and a second main surface; To provide a curable composition, the curable composition, (i) A highly branched polythioether having multiple terminal carbon-carbon double bonds or thiol groups, wherein the highly branched polythioether has a refractive index of at least 1.600 and a number-average molecular weight of at least 1000 g / mol and at most 5000 g / mol; (ii) at least one polyfunctional compound and It includes, and components (i) and (ii) react via a thiol-ene reaction; The curable composition is placed on at least a portion of the second main surface of the substrate to form a curable layer; The method involves curing a curable layer to form a cured organic layer, wherein the cured organic layer has a refractive index of at least 1.660 as measured at 450 nm; Depositing an inorganic barrier layer on a hardened organic layer. Includes.

[0010] The above summary is not intended to describe each embodiment. Details of one or more embodiments of the present invention are also described below. Other features, purposes, and advantages will become apparent from this description and the claims. [Brief explanation of the drawing]

[0011] This application may be better understood by considering the following detailed description of various embodiments of the present disclosure in relation to the accompanying drawings.

[0012] [Figure 1] A cross-sectional view of one embodiment of the article of this disclosure is shown.

[0013] [Figure 2] A cross-sectional view of an embodiment of another article of the present disclosure is shown.

[0014] In the following description of the illustrated embodiments, reference is made to the accompanying drawings, which show by way of illustration various embodiments in which the present disclosure may be practiced. It is to be understood that embodiments may be utilized and structural changes may be made without departing from the scope of the present disclosure. The drawings are not necessarily to scale. Like numbers used in the drawings refer to like components. However, the use of a number to refer to a component in a given drawing is not intended to limit the component in another drawing labeled with the same number. DETAILED DESCRIPTION OF EMBODIMENTS

[0015] As used herein, the term "a", "an", and "the" are used interchangeably and mean one or more; and "and / or" is used to indicate that one or both of the stated cases may occur, for example A and / or B includes (A and B) and (A or B).

[0016] Also herein, the recitation of ranges by endpoints includes all numbers subsumed within that range (e.g., 1 to 10 includes 1.4, 1.9, 2.33, 5.75, 9.98, etc.).

[0017] Also herein, the recitation of "at least one" includes all numbers of one and greater (e.g., at least 2, at least 4, at least 6, at least 8, at least 10, at least 25, at least 50, at least 100, etc.).

[0018] The terms "room temperature" and "ambient temperature" are used interchangeably, have their ordinary meanings, and refer to a temperature of 20 to 25°C.

[0019] As used herein, the term “adjacent” refers to two layers that are adjacent to another layer. Adjacent layers may be in direct contact with each other, or there may be an intervening layer. There is no empty space between adjacent layers.

[0020] This disclosure describes highly branched polythioether compounds having multiple terminal functional groups. The terminal functional groups may be carbon-carbon double bonds (e.g., vinyl or allyl groups) or thiol groups.

[0021] The polythioether compounds of this disclosure are highly branched, which means that the polythioether compounds are polydisperse dendritic polymers.

[0022] In some embodiments, the highly branched polythioethers according to the Disclosure have a molecular weight of at least 1000, 1500, or even 2000 g / mol. In some embodiments, the highly branched polythioethers according to the Disclosure have a molecular weight of up to 5000, 4000, 3500, 3000, or even 2500 g / mol.

[0023] The highly branched polythioethers of this disclosure have at least two terminal functional groups, more preferably at least three, or even more preferably at least four terminal functional groups. Typically, the highly branched polythioethers of this disclosure have 10 or fewer, 15 or fewer, or even 20 or fewer terminal functional groups. Generally, the highly branched polythioethers have either multiple terminal carbon-carbon double bonds (either vinyl or allyl groups) or terminal thiol groups, but not both.

[0024] The highly branched polythioethers of this disclosure have a high refractive index. In one embodiment, the highly branched polythioether, as a liquid, has a refractive index of at least 1.600, 1.610, 1.620, 1.640, 1.650, 1.660, or even 1.680 when measured by a refractive index measurement method.

[0025] The highly branched polythioethers relating to this disclosure can be prepared by a so-called thiol-ene click reaction. The thiol-ene reaction is known in the art and is a reaction between a thiol group and an alkene to form a thioether. The reaction typically has high rate and high yield. In some embodiments, at least one unsaturated compound reacts with at least one organic thiol in a thiol-ene type reaction.

[0026] In some embodiments, at least one unsaturated compound independently has p vinyl groups or p allyl groups and consists of C, H, and optionally Si and / or O atoms. Each p is independently an integer of 2 or more (e.g., 3, 4, 5, 6, 7, or 8).

[0027] In some embodiments, the useful unsaturated compound has 4 to 20 carbon atoms (e.g., 4 to 20, 4 to 18, 4 to 16, or 4 to 12 carbon atoms), 0 to 10 silicon atoms (e.g., 0 to 10, 1 to 10, 0 to 6, 1 to 6, 2 to 10, 2 to 6, or 2 to 4 silicon atoms), and 0 to 9 oxygen atoms (e.g., 0 to 9, 0 to 6, 0 to 4, 0 to 2, or 0 to 1 oxygen atom). If O is present, O is preferably in an ether bond (i.e., COC). In some embodiments, the useful unsaturated compound consists of C and H atoms. In some embodiments, the useful unsaturated compound consists of C, H, and O atoms. In some embodiments, the useful unsaturated compound consists of C, H, and Si atoms. In some embodiments, the useful unsaturated compound consists of C, H, Si, and O atoms. In some embodiments, the useful unsaturated compound contains aromatic carbon atoms, but in other embodiments, the useful unsaturated compound does not contain aromatic carbon atoms.

[0028] In some embodiments, the useful unsaturated compound is an organosilane. An exemplary organosilane is given by formula Si(OSiR 2 2CH=CH2) b (R 2CH=CH2) c (R 1 ) d such as those represented by, has at least one silicon atom. each R 2 is independently a direct bond (i.e., a covalent bond) or a hydrocarbylene group having 1 to 12 carbon atoms, optionally having at least one ether bond. Examples include methylene, ethylene, propane-1,3-diyl, propane-1,2-diyl, butane-1,4-diyl, butane-1,3-diyl, pentane-1,5-diyl, pentane-1,4-diyl, hexane-1,6-diyl, octane-1,8-diyl, decane-1,10-diyl, dodecane-1,12-diyl, 1,4-phenylene, and 1,8-biphenylene. each R 1 is independently a hydrocarbyl group having 1 to 12 carbon atoms (e.g., methyl, ethyl, n-propyl, isopropyl, n-butyl, sec-butyl, n-pentyl, n-hexyl, phenyl, biphenylyl, and alkyl-substituted phenyl), optionally having at least one ether bond. In some embodiments, R 1 has an optionally substituted phenyl group (e.g., phenyl, biphenylyl, tolyl, xylyl, methoxyphenyl). b is an integer of 0 to 4 (i.e., 0, 1, 2, 3, or 4), c is an integer of 0 to 4 (i.e., 0, 1, 2, 3, or 4), d is an integer of 0 to 2 (i.e., 0, 1, or 2), with the proviso that b+c≧2 (in some embodiments, b+c≧3), and b+c+d=4.

[0029] Examples of organosilanes include 1,3-divinyl-1,3-diphenyl-1,3-dimethyldisiloxane; 1,1,3,3-tetraphenyl-1,3-divinyldisiloxane; 1,4-bis(vinyldimethylsilyl)benzene; 1,5-divinyl-3-phenylpentamethyltrisiloxane; 1,3-divinyl-1,1,3,3-tetramethyldisiloxane; 1,4-divinyl-1,1,4,4-tetramethyl-1,4-disilabutane; divinyldimethylsilane; 1,5-divinyl-3,3-diphenyl-1,1,5,5-tetramethyltrisiloxane; 1,3-divinyltetrakis(trimethylsiloxy)disiloxane; 1,5-divinylhexamethyltrisiloxane; bis(divinyl)-terminated polydimethylsiloxane; 1,3 Examples include divinyltetraethoxydisiloxane; 1,3-divinyl-1,3-dimethyl-1,3-dimethoxydisiloxane; trivinylmethoxysilane; 1,3,5-trivinyl-1,3,5-trimethylcyclotrisiloxane; 1,3,5-trivinyl-1,1,3,5,5-pentamethyltrisiloxane; 1,3,5,7-tetravinyl-1,3,5,7-tetramethylcyclotetrasiloxane; 1,1,3,3-tetravinyldimethyldisiloxane; tetravinylsilane; tetraallylsilane; 1,3,5,7,9-pentavyl-1,3,5,7,9-pentamethylcyclopentasiloxane; hexavyldisiloxane; and 1,3,5,7,9,11-hexavylhexamethylcyclohexasiloxane. The aforementioned vinyl compounds are available from commercial suppliers such as Gelest, Inc., Morrisville, Pennsylvania, and / or can be synthesized by known methods. Of these, tetravinylsilane; tetraallylsilane; 1,2,4-trivinylcyclohexane; and 1,1,3,3-tetraphenyl-1,3-divinyldisiloxane are preferred in some embodiments.

[0030] Exemplary unsaturated compounds that do not contain Si atoms include trivinylcyclohexane and triallyl isocyanurate.

[0031] To produce highly branched polythioethers, an unsaturated compound is reacted with at least one organic thiol. In some embodiments, the organic thiol has q thiol groups and consists of C, H, S, and optionally O and / or N atoms. Each q is independently an integer of 2 or more (e.g., 3, 4, 5, 6, 7, or 8).

[0032] In some embodiments, a useful organic thiol has 4 to 20 carbon atoms (e.g., 4 to 20, 4 to 18, or 4 to 12 carbon atoms), 2 to 10 sulfur atoms (e.g., 2 to 10, 2 to 8, 2 to 6, or 2 to 4 silicon atoms), 0 to 9 oxygen atoms (e.g., 0 to 9, 0 to 6, 0 to 4, 0 to 2, or 0 to 1 oxygen atom), and 0 to 9 nitrogen atoms (e.g., 0 to 9, 0 to 6, 0 to 4, 0 to 2, or 0 to 1 nitrogen atom). In some embodiments, a useful organic thiol consists of C, H, and S atoms. In some embodiments, a useful organic thiol consists of C, H, S, and O and / or N atoms.

[0033] In some embodiments, the organic thiol is independently of formula HS-R 4 -Ar-R 4 - Represented by SH, where each R 4 A is independently a hydrocarbylene group having direct bonds or 1 to 12 carbon atoms (e.g., 1 to 12, 2 to 12, or 4 to 12 carbon atoms), and Ar is an arylene group having C, H, and optionally S and / or N atoms.

[0034] Examples of organic thiols include 1,3-benzenedithiol; 1,3-benzenedimethanethiol; and 2,3-bis-2-mercaptoethylthio-1-propanethol.

[0035] In some embodiments, the reaction between at least one unsaturated compound and at least one organothiol is initiated by at least one free radical initiator. Typically, the initiator is a photoinitiator, meaning that the initiator is activated by light, generally ultraviolet (UV) light, although other light sources can be used with the appropriate selection of an initiator, such as a visible light initiator or an infrared light initiator. Photoinitiators are known in the art. Examples of suitable free radical photoinitiators include OMNIRAD 4265, OMNIRAD 184, OMNIRAD 651, OMNIRAD 1173, OMNIRAD 819, OMNIRAD TPO, and OMNIRAD TPO-L, which are commercially available from IGM Resins, Charlotte, and NC. Particularly suitable photoinitiators are those that exhibit high absorbance above 365 nm wavelength. These include the acylphosphine oxide family of photoinitiators such as OMNIRAD TPO, OMNIRAD TPO-L, and OMNIRAD 819.

[0036] When an initiator is used, it is generally used in an amount of 0.01 to 10 parts by weight, more typically 0.1 to 2.0 parts by weight, per 100 parts by weight of the total reactive components (i.e., thiols and carbon-carbon double bonds) in the reaction composition.

[0037] In the reaction of an unsaturated compound with an organic thiol, one terminal carbon-carbon double bond reacts with one terminal thiol; therefore, a greater number of moles of one of the functional groups is required to produce a functionalized highly branched polythioether. In other words, p(C=C bond) + q(thiol group) is greater than 4 (e.g., greater than 5, 6, 7, 8, or even 9). Thus, if more p C=C bonds are used, this results in a highly branched polythioether with multiple terminal carbon-carbon double bonds. Similarly, if more q thiol groups are used, a highly branched polythioether with multiple terminal thiol groups is obtained.

[0038] The resulting reaction mixture is exposed to a light source necessary to initiate the reaction, such as UV light or visible light.

[0039] The resulting highly branched polythioethers can have a high refractive index, for example, greater than 1.600. The presence of phenyl groups and / or sulfur can increase the refractive index. Thus, in some embodiments, the highly branched polythioether has at least one phenyl group. Such a phenyl group can be incorporated by using a phenyl-containing reactant, such as a phenyl-containing organosilane. Advantageously, the presence of a phenyl group can also cause an increase in the glass transition temperature (Tg) of the molecule. In some embodiments, the highly branched polythioether has at least 20, 25, 30, or even 40% by weight of sulfur, the amount of sulfur can be experimentally determined by calculating the weight of the sulfur atom relative to the total weight of atoms in the highly branched polythioether.

[0040] curable composition

[0041] In this disclosure, it has been found that curable compositions comprising highly branched polythioethers and polyfunctional compounds disclosed herein may have a high refractive index and, in some embodiments, result in curable compositions having an elevated glass transition temperature (Tg) upon curing.

[0042] The curable compositions of this disclosure are substantially solvent-free and comprise at least one polyfunctional compound. In one embodiment, the polyfunctional compound can react with a highly branched polythioether in a thiol-ene type reaction as discussed above. In another embodiment, a highly branched polythioether having terminal carbon-carbon double bonds can react with a polyfunctional compound having terminal carbon-carbon double bonds, optionally, in the presence of a free radical initiator to form a cured article.

[0043] In the first embodiment, the polyfunctional compound of the present disclosure has a plurality of functional groups, the plurality of functional groups can react with a highly branched polythioether via a thiol-ene reaction. For example, when a highly branched polythioether having terminal carbon-carbon double bonds is used, the polyfunctional compound has a plurality of terminal thiol groups. Such a polyfunctional compound has at least two thiol (i.e., -SH) groups, but such a polyfunctional compound may have more than two thiol groups, for example, three, four, or even five thiol groups. These polyfunctional compounds can have a molecular weight of about 70 to 1000 g / mol in the case of small molecules, and a molecular weight of about 1000 to 5000 g / mol in the case of the highly branched polythioether disclosed herein.

[0044] To ensure a cured composition with a high refractive index, it is useful to select a polyfunctional compound with a high refractive index. Typically, aromatic groups can increase the refractive index of a compound. Generally, the refractive index of non-aromatic polyfunctional thiols does not exceed 1.620 when measured with a white light refractometer. However, polyfunctional compounds having multiple terminal thiol groups can be aromatic thiols or non-aromatic thiols.

[0045] Examples of non-aromatic polyfunctional compounds include 2,3-bis-2-mercaptoethylthio-1-propanthol, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane; 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane; 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane; and 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane. Other non-aromatic polyfunctional thiols include poly(ethylene glycol)dithiol; 1,2,3-trimercaptopropane; 2,3-bis-2-mercaptoethylthio-1-propanthol; 1,2-ethanedithiol; 2,2'-thiodiethanethiol; bi(mercaptoethyl)sulfide; 2,5-bis(mercaptomethyl)-1,4-dithiane; tetra(ethylene glycol)dithiol; 2,2'-(ethylenedioxy)diethanethiol; pentaerythritoltetrakis(3-mercaptopropionate); trimethylolpropanetris(3-mercaptopropionate); [ka] These are some examples.

[0046] In some embodiments, the polyfunctional compound is an aromatic thiol. Aromatic thiols can have a high refractive index. Exemplary aromatic polyfunctional thiols include 1,3-benzenedithiol; toluenedithiol, 1,3-benzenedimethanethiol; 1,3,4-thiadiazole-2,5-dithiol, (1,2,4)thiadiazole-3,5-dithiol, 1,3,5-trimercaptobenzene, 2-thiazoline-2-thiol, 1,1',4',1”-terphenyl-4-thiol, 5-bromopyridine-2-thiol, biphenyl-4-thiol, 1,7-naphthalenedithiol, and 1,5-naphthalenedithiol.

[0047] When highly branched polythioethers having terminal thiol groups are used, the polyfunctional compound has multiple terminal carbon-carbon double bonds.

[0048] Examples of polyfunctional compounds having terminal carbon-carbon double bonds include tetravinylsilane, tetraallylsilane, and trivinylcyclohexane.

[0049] In some embodiments, a highly branched polythioether having multiple terminal carbon-carbon double bond groups reacts with a highly branched polythioether having multiple terminal thiols.

[0050] Highly branched polythioethers and the polyfunctional compounds described above react. Typically, the highly branched polythioethers and polyfunctional compounds are reacted in amounts sufficient to ensure that no reactive groups remain in the cured product. The terminal double bonds react with one thiol. Therefore, ideally, the molar ratio of terminal double bonds in the highly branched polymer to the thiol group in the polyfunctional thiol compound should be 1:1. In some embodiments, the molar ratio of terminal carbon-carbon double bonds in the highly branched polymer to the thiol (-SH) in the polyfunctional thiol compound is 0.8:1 to 1:0.8, or even 0.9:1 to 1:0.9.

[0051] In some embodiments, the polyfunctional compounds are liquid under ambient conditions, in other words, at room temperature and 1 atmosphere. In some embodiments, the polyfunctional thiols of the present disclosure have melting points / on-melting temperatures of 80, 70, 60, 50, 40, or even less than 30°C at ambient pressure (e.g., 760 mmHg).

[0052] In another embodiment, a first highly branched polythioether having a terminal carbon-carbon double bond may be reacted with another polyfunctional compound having a terminal carbon-carbon double bond in the presence of a free radical initiator. Examples of such polyfunctional compounds having a terminal carbon-carbon double bond include the tetravinylsilane, tetraallylsilane, and trivinylcyclohexane mentioned above, but a second highly branched polythioether having a terminal carbon-carbon double bond may also be mentioned. Such a second highly branched polythioether having a terminal carbon-carbon double bond may be the same as or different from the first highly branched polythioether having a terminal carbon-carbon double bond.

[0053] When preparing a curable composition, the composition is substantially solvent-free. As used herein, “substantially solvent-free” means a curable composition having 5, 4, 3, 2, 1, or even less than 0.5% by weight of a nonpolymerizable (e.g., organic) solvent. The concentration of the solvent can be determined by known methods such as gas chromatography (e.g., as described in ASTM D5403-93). It should be noted that whether a curable composition is substantially solvent-free or solvent-free, no solvent is intentionally added to the composition. The term “solvent” is used herein in accordance with commonly understood technical terms and includes volatile organic and non-organic materials that are liquid at room temperature.

[0054] In some embodiments, the curable composition comprises at least one free radical initiator previously described for the synthesis of highly branched polythioether compounds.

[0055] When an initiator is used, it is generally used in an amount of 0.01 to 10 parts by weight, more typically 0.1 to 2.0 parts by weight, per 100 parts by weight of the total reactive components (i.e., thiols and C=C bonds) in the curable composition.

[0056] In some embodiments, the curable composition may contain additional non-curable components, provided that such components do not interfere with the curing of the curable composition and do not adversely affect the properties of the curable composition. The curable composition may also contain polymerization inhibitors, UV absorbers, light stabilizers (e.g., hindered amine light stabilizers (HALS)), adhesion promoters, sensitizers, synergists, antioxidants, catalysts, dispersants, drying agents, surfactants, leveling agents, and the like, as needed or desired.

[0057] In some embodiments, the curable composition further comprises polymerization inhibitors and / or heat stabilizers. Generally, these polymerization inhibitors and / or heat stabilizers are added to the curable composition in an amount of 2% by weight or less. Exemplary inhibitors include BHT (2,6-di-t-butyl-p-cresol), MEHQ (4-methoxyphenol), and pyrogallol. Exemplary heat stabilizers include 4-methoxyphenol, pyrogallol, or 4-tert-butyl-1,2-dihydroxybenzene. Acidic compounds, including benzoic acid, benzenesulfonic acid, phenylphosphonic acid, and vinylphosphonic acid, can also be used as co-stabilizers. Typical concentrations of co-stabilizers in the curable composition range from 1 mM to 1 M. Useful antioxidants include, but are not limited to, amines such as N-N'di-β-naphthyl-1,4-phenylenediamine available as "AGERITE D"; 2,5-di-(t-amyl)hydroquinone available as "SANTOVAR A" from Monsanto Chemical Co.; tetrakis[methylene 3-(3',5'-di-tert-butyl-4'-hydroxyphenyl)propionate]methane available as "IRGANOX 1010" from Ciba-Geigy Corp.; and phenols such as 2-2'-methylenebis(4-methyl-6-tert-butylphenol) available as Antioxidant 2246; as well as dithiocarbamates such as zinc dithiodibutylcarbamate.

[0058] In some embodiments, the curable composition has a viscosity of 100 centipoise (cP) or less at temperatures from room temperature to about 60°C. In some embodiments, the curable composition has a viscosity of at least 1, 2, 3, 4, or even 5 cp; and a maximum of 100, 80, 60, 50, 40, 30, 25, 20, 15, or even 10 cP at room temperature. In some embodiments, the curable composition has a viscosity of at least 1, 2, 3, 4, or even 5 cp; and a maximum of 100, 80, 60, 50, 40, 30, 25, 20, 15, or even 10 cP at 35°C. In some embodiments, the curable composition has a viscosity of at least 1, 2, 3, 4, or even 5 cp; and a maximum of 30, 25, 20, 15, or even 10 cP when measured by a viscometer under ambient conditions at 60°C. For example, viscosity can be measured by taking 17 mL of the curable composition and filling it into a 25 mm diameter double-gap coaxial concentric cylindrical apparatus on a viscometer (BOHLIN VISCO 88, Malvern Instruments Ltd, Malvern, UK). Water heated to 25°C can be recirculated in a heat jacket on the double-gap cell of the viscometer to maintain a constant temperature during the test. For example, the system can be equilibrated for 30 minutes before each measurement. The shear rate can be increased from 100 to 1000 Hz in 100 Hz increments, and the measurement is repeated three times to determine the average viscosity.

[0059] Curable compositions can be deposited on surfaces using techniques known in the art, including conventional coating techniques such as bar coating, roll coating, curtain coating, rotogravure coating, spray coating, or dip coating. The curable compositions disclosed herein may be particularly useful as organic layers in thin-film encapsulation components. Often, printing techniques such as inkjet printing are used to deposit these organic layers.

[0060] A wide variety of substrates are suitable for the articles of this disclosure. Suitable substrates include a wide variety of flexible and non-flexible substrates. For example, the substrate may be a relatively thick layer of glass, silicon nitride, silicon oxynitride, or a polymer material such as PMMA (polymethyl methacrylate) or PC (polycarbonate). Alternatively, the substrate may be a flexible polymer film such as a film of PET (polyethylene terephthalate), PEN (polyethylene naphthalate), PC (polycarbonate), polyimide, or PEEK (polyether ether ketone). In some embodiments, the substrate includes a heat-sensitive substrate. A wide variety of heat-sensitive substrates are suitable, such as OLED panels.

[0061] The curable composition may be exposed to thermal or light radiation to initiate the reaction of thiols with the carbon-carbon double bonds of the highly branched polymer, resulting in a cured composition. The curable composition may be exposed to ultraviolet (UV) A with a maximum value in the range of 280-425 nanometers. The UV light source can be of various types. Low-intensity light, such as blacklights, is generally 0.1 or 0.5 mW / cm². 2 (milliwatts per square centimeter) ~10mW / cm 2 It provides an intensity in the range of (for example, measured using a UVIMAP UM 365 LS radiometer manufactured by Electronic Instrumentation & Technology, Inc. in Sterling, VA, following procedures approved by the National Institute of Standards and Technology). High light intensity sources are generally 10, 15, or 20 mW / cm². 2 Even larger, 450 mW / cm² 2 It provides intensities in the range described above. In some embodiments, the high-intensity light source can reach up to 500, 600, 700, 800, 900, or 1000 mW / cm². 2The UV light for polymerization of monomer components can be provided by various light sources such as light-emitting diodes (LEDs), black lights, medium-pressure mercury lamps, or combinations thereof. Reagents can also be polymerized using high-intensity light sources available from Fusion UV Systems Inc. The UV exposure time for polymerization and curing may vary depending on the intensity of the light source used. For example, complete curing with a low-intensity light source can be achieved with exposure times ranging from about 30 to 300 seconds; on the other hand, complete curing with a high-intensity light source can be achieved with shorter exposure times ranging from about 5 to 20 seconds. Partial curing with a high-intensity light source can typically be achieved with exposure times ranging from about 2 seconds to about 5 or 10 seconds.

[0062] Generally, the cured layer has a refractive index of at least 1.660, 1.670, or even 1.680 when measured at 450 nm. High refractive index nanoparticles, such as polymer particles, metal particles, or metal oxide particles having a refractive index of at least 1.6, are typically used to increase the refractive index of the cured layer. However, advantageously, the cured compositions of this disclosure have a high refractive index without the use of nanoparticles.

[0063] Ideally, the cured composition is optically transparent. Unless otherwise specified, “optically transparent” means a layer, film, or article that has high light transmittance over at least a portion of the visible light spectrum (approximately 400 to 700 nm) and exhibits low haze. Typically, an optically transparent layer, film, or article has a visible light transmittance value of at least 85%, or even 90%, often at least 95%, and a haze value of 5% or less, often 2% or less, when measured using techniques such as ASTM D1003-21.

[0064] In some embodiments, the cured composition has a glass transition temperature of at least -20, -10, 0, or even 5°C. The terms “Tg” and “glass transition temperature” are used interchangeably. When measured, the Tg value at midpoint (or height at half maximum) is determined by differential scanning calorimetry (DSC) at a scanning rate of 10°C / min using a second heating.

[0065] Articles are also disclosed herein. A wide variety of articles can be prepared using the curable compositions described above. The articles may be relatively simple articles, such as a substrate on which a layer of the curable composition is disposed, as shown in Figure 1, where article 100 includes a substrate 120 having a cured organic layer 110 disposed on the substrate. The substrate 120 includes a wide variety of flexible and non-flexible substrates. For example, the substrate 120 may be a relatively thick layer of glass, silicon nitride, silicon oxynitride, or a polymer material such as PMMA or PC. Alternatively, the substrate 120 may be a flexible polymer film such as PET, PEN, PC, polyimide, or PEEK. The cured organic layer 110 is a cured layer derived from the curable compositions described herein. In some embodiments, the cured organic layer has a thickness of 1 to 50 micrometers, and in some embodiments, 5 to 30 micrometers.

[0066] In other embodiments, the article is more complex, such as a multilayer article comprising a substrate, an inorganic barrier layer, and a cured organic layer between them, where the cured layer functions as a decoupling layer. The substrate may optionally have an inorganic coating layer on its surface, thereby the cured organic layer may be in contact with the substrate surface or any inorganic coating layer.

[0067] In some embodiments, the article comprises a substrate having a first main surface and a second main surface, and a cured organic layer having a first main surface and a second main surface, wherein the first main surface of the cured organic layer is adjacent to at least a portion of the second main surface of the substrate.

[0068] Figure 2 shows a device comprising a multilayer article of the present disclosure. Figure 2 shows an article 200 comprising a substrate 230 and a device 240 disposed on the substrate 230. An inorganic barrier layer 250 is in contact with the device 240, and a cured organic layer 210 is in contact with the inorganic barrier layer 250. Figure 2 also includes an arbitrary inorganic layer 260 in contact with the cured organic layer 210. An arbitrary layer 270 is in contact with the arbitrary inorganic layer 260 and is also in contact with the substrate 280. Furthermore, any alternating pair of layers of cured organic layer (210) and inorganic layer (260) may exist between any layer 260 and any layer 270. For clarity, these arbitrary layers are not shown, but it is easy to imagine stacking of layers in the order of 250 / 210 / 260 / 210 / 260, or 250 / 210 / 260 / 210 / 260 / 210 / 260, etc.

[0069] The curable compositions disclosed herein may be cured and used as organic layers in thin-film encapsulation components. These organic layers should be deposited on a surface in a precise and consistent manner, which is typically done using printing techniques. In printing techniques, the curable composition, which forms a polymer upon curing, is printed onto the substrate surface to form a layer. A wide variety of printing techniques can be used, and inkjet printing is particularly preferred due to its superior precision. Since the curable compositions may be printable, they may also be referred to herein as inks. The curable compositions do not necessarily have to be used as inks; that is, they do not necessarily have to be cured after printing, and they can be delivered to the substrate surface in a wide variety of ways, but they can be printed. In particular, the printable compositions of this disclosure are typically inkjet printable, which means that the printable compositions of this disclosure have the appropriate viscosity and other attributes necessary for inkjet printing. The term "inkjet printable" is a description of the material rather than a description or limitation of a process, and means that the curable composition can be inkjet printable, not that the composition has necessarily been inkjet printed. This disclosure describes a curable composition that can be considered a printable “ink,” having several features that make it suitable for forming layers in multilayer optical devices. As stated above, the curable composition of this disclosure is substantially solvent-free, which is advantageous because drying a coating to remove a solvent can not only reduce the thickness of the layer but also adversely affect the smoothness of the surface and can cause defects in the coating. In many applications of optical devices, it is desirable that the coating be accurate, that is, that the coating does not lose thickness or smoothness when it dries. Therefore, the curable composition of this disclosure is preferably “100% solids,” which means that the curable composition of this disclosure does not contain a volatile solvent, all of the mass deposited on the surface remains there, and no volatile mass is lost from the coating.

[0070] The thickness of the cured composition is limited by the intended use. For thin-film encapsulation products, the cured organic layer typically has a thickness of 1 to 50 micrometers, and in some embodiments, 5 to 30 micrometers. Furthermore, in many embodiments, the cured organic layer has a surface roughness of 10 nanometers or less, and in some embodiments, 5 nanometers or less.

[0071] An example of an optical device that utilizes thin film layers is an OLED (organic light-emitting diode) device. In particular, organic light-emitting devices are susceptible to degradation due to the permeation of certain liquids and gases such as water vapor and oxygen. To reduce permeability to these liquids and gases, barrier coatings are applied to OLED devices. Typically, these barrier coatings are not used alone, but rather in the form of barrier laminates that can contain multiple dyads. A dyad is a two-layer structure containing a barrier layer (i.e., an inorganic layer) and a decoupling layer (i.e., an organic layer). The decoupling layer provides a planarized and / or smooth surface for the deposition of the inorganic barrier layer.

[0072] The inorganic barrier layer 250 in contact with the hardened organic layer 210 can be prepared from a variety of materials, including metals, metal oxides, metal nitrides, metal oxynitrides, metal carbides, metal oxybolds, and combinations thereof. A wide range of metals are suitable for use in metal oxides, metal nitrides, and metal oxynitrides, with particularly suitable metals including Al, Zr, Si, Zn, Sn, and Ti. One particularly suitable inorganic barrier layer material is silicon nitride.

[0073] The thickness of the inorganic barrier layer 250 is not particularly limited, and is generally between 20 nanometers and 1 micrometer (1000 nanometers). More typically, the thickness is between 20 nanometers and 100 nanometers.

[0074] Any inorganic barrier layer 260 may have the same thickness as the inorganic barrier layer 250 and may contain the same inorganic material, or it may contain a different inorganic material.

[0075] One embodiment of device 200 is a touch-sensing device. In this device, substrate 230 is a thin-film transistor, device 240 is an OLED device, an optional layer 270 is an optically transparent adhesive layer, and substrate 280 is a touch sensor.

[0076] In some embodiments, the curable composition is placed on the surface of a substrate and then cured to form a cured organic layer. In some embodiments, an inorganic barrier layer is placed on the exposed surface of the cured organic layer.

[0077] In some embodiments, the curable composition can be printed and then cured to form a layer. In some embodiments, the curable composition has a thickness of 5 to 30 micrometers and a surface roughness of 5 nanometers or less. In many embodiments, placing the curable composition on a second main surface of a substrate to form a curable layer involves printing, particularly inkjet printing. As described above, inkjet printing has various desirable features that make it particularly suitable for preparing a curable layer, including the ability to deposit precise patterns on complex substrates and form a uniform coating with a low surface roughness of less than 10 nanometers, and in some embodiments, 5 nanometers or less.

[0078] In some embodiments, the article further includes a device positioned on a second main surface of the substrate and adjacent to a cured organic layer.

[0079] In some embodiments, the substrate includes an inorganic coating layer present on a second main surface, and the first main surface of the thus cured organic layer is in contact with the inorganic coating layer.

[0080] The above configuration can also be used as a component of a more complex article. In some embodiments, the article further includes a device disposed on a second main surface of a substrate and adjacent to a first main surface of a cured organic layer. In some embodiments, an inorganic coating layer is disposed on the device and on the second main surface of the substrate, so that the first main surface of the cured organic layer is in contact with the inorganic coating layer. In some specific embodiments, the device includes an OLED (organic light-emitting diode). [Examples]

[0081] Unless otherwise stated, all parts, percentages, ratios, etc., in the examples and the remainder of this specification are by weight, and all reagents used in the examples are obtained or available from common chemical suppliers such as Millipore-Sigma Company, Saint Louis, Missouri, or Gelest, Morristown, Pennsylvania, or can be synthesized by conventional methods. [Table 1]

[0082] Preparation of highly branched polymer (HBP) examples HBP1 (allyl terminus) A mixture of 13BDT (0.36 g, 5.06 mmol thiol) and excess Si(allyl)4 (0.75 g, 15.6 mmol allyl) was subjected to UV irradiation (395 nm, 2 minutes, 319 mW / cm²). 2 The mixture was stirred in a glass vial with TPOL (0.02 g) at 100% intensity (at a distance of 1 cm from the vial for 2 minutes). The resulting colorless oil was precipitated in methanol, the methanol portion at the top was removed, and the product was washed three times with acetonitrile to remove excess monomers. The product was obtained as a colorless, viscous liquid.

[0083] HBP2 (thiol terminus) A mixture of Si(allyl)4 (0.24 g, 5.06 mmol allyl) and excess 13BDT (1.11 g, 15.6 mmol thiol) was stirred in a glass vial with TPOL (0.02 g) under UV irradiation (as described above). The resulting colorless oil was precipitated in heptane, the upper heptane portion was removed, and the product was washed three times with methanol to remove excess monomers. The product was obtained as a colorless, viscous liquid.

[0084] HBP3 (Vinyl End Cap) A mixture of 13BDT (0.36 g, 5.06 mmol thiol) and excess Si(vinyl)4 (0.54 g, 15.6 mmol vinyl) was stirred in a glass vial with TPOL (0.02 g) under UV irradiation (as described above), and isolated as a colorless viscous liquid as described for HBP1 above.

[0085] HBP4 (thiol terminus) A mixture of Si(vinyl)4 (0.17 g, 5.06 mmol vinyl) and excess 13BDT (1.11 g, 15.6 mmol thiol) was stirred in a glass vial with TPOL (0.02 g) under UV irradiation (as described above), and isolated as a colorless viscous liquid as described for HBP2 above.

[0086] HBP5 (Vinyl End Cap) A mixture of 13BDT (0.36 g, 5.06 mmol thiol) and excess TVCH (0.57 g, 10.5 mmol vinyl) was stirred in a glass vial with TPOL (0.02 g) under UV irradiation (as described above) and isolated as a colorless, very viscous liquid, as described for HBP1 above.

[0087] HBP6 (thiol terminus) A mixture of TVCH (0.17 g, 5.06 mmol vinyl) and an excess of 13BDT (0.75 g, 10.5 mmol thiol) was stirred in a glass vial with TPOL (0.02 g) under UV irradiation (as described above) and isolated as a colorless, very viscous liquid, as described for HBP2 above.

[0088] HBP7 (Vinyl End Cap) A mixture of 13BDMT (0.43 g, 5.06 mmol thiol) and excess Si(vinyl)4 (0.54 g, 15.6 mmol vinyl) was stirred in a glass vial with TPOL (0.02 g) under UV irradiation (as described above), and isolated as a colorless viscous liquid as described for HBP1 above.

[0089] HBP8 (thiol terminus) A mixture of Si(vinyl)4 (0.17 g, 5.06 mmol vinyl) and excess 1,3-benzenedimethanethiol (1.32 g, 15.6 mmol thiol) was stirred in a glass vial with TPOL (0.02 g) under UV irradiation (as described above), and isolated as a colorless viscous liquid as described for HBP2 above.

[0090] HBP9 (Vinyl End) A mixture of DMPT (0.44 g, 5.06 mmol thiol) and excess Si(vinyl)4 (1.06 g, 30.9 mmol vinyl) was stirred in a glass vial with TPOL (0.02 g) under UV irradiation (as described above), and isolated as a colorless viscous liquid as described for HBP1 above.

[0091] Gel permeation chromatography (GPC) Solutions of various highly branched polymers at a concentration of approximately 1.5 mg / mL were prepared in toluene. The samples were swirled on an orbital shaker for 12 hours. The sample solutions were filtered through a 0.45 μm PTFE syringe filter and then analyzed by GPC. A liquid chromatography apparatus (1260 LC, Agilent, Santa Clara, CA) was used with an Agilent "PLgel MIXED B+C" column at 40°C, toluene eluent at 1.0 mL / min, and an Agilent 1260 evaporative light scattering detector, along with a polystyrene, narrow molecular weight standard reference material available under trade name NIST SRM 705a.

[0092] Nuclear magnetic resonance (NMR) spectroscopy Various highly branched polymers were analyzed as solutions in deuterated chloroform. NMR spectroscopy was performed using a CPBBO gradient cryoprobe, a Bruker B-ACS 60 autosampler, and a Bruker AVANCE III 500 MHz NMR spectrometer with Bruker Topspin 3.04 software. Spectra were analyzed using Advanced Chemistry Development software (Toronto, Canada). Analysis of chemical shifts and integrals in the proton spectra confirmed the formation of target structures. For vinyl-terminated and allyl-terminated polymers, the end group content in mmol / g units was calculated by comparing the integral related to the end groups with the integral related to the internal polymer repeating units.

[0093] The number-average molecular weight (Mn) determined by GPC and the amount of terminal alkenes determined by NMR are reported in Table 2 for the selected highly branched polymers synthesized above. [Table 2]

[0094] Refractive index of a liquid The refractive index was measured using a refractometer (model number: 334610 Milton Roy, Houston, TX). The liquid sample was sealed between two prisms, and the refractive index was measured at 20°C on the 589 nm line of a sodium lamp. Results for various highly branched polymers are shown in Table 3.

[0095] Comparative Example 1 (C1) We used M1, a low-viscosity liquid and one of the highest refractive indices available as an acrylate. [Table 3]

[0096] hardening compound Examples 1 and 2 (E1-E2) A highly branched polythioether (0.5 g) was thoroughly mixed with TPO-L (0.015 g, 3 wt%). The colorless liquid formulation was cast onto a polyethylene terephthalate (PET) film using a Meyer rod (No. 10) and illuminated for 5 minutes at 319 mW / cm² at 395 nm, 1 cm from the surface of the sample, using an LED system (CF1000 UV, available from Clearstone, Palo Alto, CA). 2 It was UV-cured to 100% strength, resulting in a transparent hard coat on PET.

[0097] Differential Scanning Calorimetry (DSC) DSC samples were prepared for thermal analysis by weighing the material and filling it into aluminum DSC sample pans (TA Instruments, New Castle, DE). The specimens were analyzed using a DSC (TA Instruments Discovery Differential Scanning Calorimeter) with a heating-cooling-heating method in standard mode (-155°C to approximately 150°C, 10°C / min). After data acquisition, thermal transitions were analyzed using the TA Instruments Universal Analysis program. The glass transition temperature (Tg) was evaluated using the stepwise changes in the standard heat flow (HF) curve. The midpoint (height at half maximum) temperature of the second heating transition is reported.

[0098] Refractive index of solids The refractive index of the topcoat was determined by measuring samples E1 and E2 at 450 nm using a digital prism coupler (Model 2010, Metricon Inc., Pennington, NJ).

[0099] The Tg values ​​for both the colorless liquid formulation and the cured transparent hard coat are reported in Table 4 for the identified samples, and the refractive index of the cured transparent hard coat is also reported in Table 4. [Table 4]

[0100] As shown in Table 4 above, HBP1, allyl-terminated highly branched polythioether, and HBP7, vinyl-terminated highly branched polythioether all self-cured and showed an increase in Tg after curing.

[0101] Comparative Example 2 (C2) Acrylate formulation C2 was prepared from M1 and M2 in a weight ratio of 95:5, as described in Example 4 of U.S. Patent No. 11,584,863 (Schwartz et al.).

[0102] Examples 3 and 4 (E3-E4) The thiol-ene formulation was prepared from a mixture of thiol (SH)-terminated HBP and alkene-terminated analog HBP in a 1:1 functional group ratio. 3% by weight of TPO-L was added, and the formulation was thoroughly mixed. The liquid formulation was cast onto a polyethylene terephthalate (PET) film using a Meyer rod (number 10), and illuminated using an LED system (CF1000 UV, available from Clearstone, Palo Alto, CA) at 395 nm, 1 cm from the surface of the sample, for 2 minutes at 319 mW / cm². 2 It was UV-cured to 100% strength, resulting in a transparent hard coat on PET.

[0103] The refractive index of the hardened transparent hard coat was tested for various samples using the solid refractive index method described above, and the results are reported in Table 5. [Table 5]

[0104] Foreseeable modifications and changes to the present invention will be apparent to those skilled in the art without departing from the scope and spirit of the invention. The present invention should not be limited to the embodiments described herein for illustrative purposes. In the event of any inconsistency or conflict between the Specified herein and any disclosure in any document referred to or incorporated herein, the Specified herein shall prevail.

Claims

1. A highly branched polythioether having multiple terminal carbon-carbon double bonds or thiol groups, having a refractive index of at least 1,600, and a number-average molecular weight of at least 1,000 g / mol and up to 5,000 g / mol.

2. The highly branched polythioether according to claim 1, further comprising a phenyl group.

3. A highly branched polythioether according to claim 1 or 2, having at least 20% by weight of sulfur atoms.

4. The aforementioned highly branched polythioether At least one unsaturated compound having p independent vinyl or allyl groups, and consisting of C, H, and optionally Si and / or O atoms, where each p is an integer of 2 or more, Having q thiol groups, consisting of C, H, S, and optionally O and / or N atoms, where each q is an integer greater than or equal to 2, and p+q is greater than 4, at least one organic thiol and A highly branched polythioether according to any one of claims 1 to 3, which is a reaction product of the above.

5. The at least one unsaturated compound is independently of the formula: Si(OSiR 2 2 CH=CH 2 ) b (R 2 CH=CH 2 ) c (R 1 ) d [In the formula, each R 2 Each R is a hydrocarbylene group that is independently directly bonded or has 1 to 12 carbon atoms, 1 [where b is a hydrocarbyl group having 1 to 12 carbon atoms independently, b is an integer from 0 to 4, c is an integer from 0 to 4, and d is an integer from 0 to 2, where b + c ≥ 2 and b + c + d = 4] The highly branched polythioether according to claim 4, as represented by...

6. The highly branched polythioether according to claim 4 or 5, wherein the at least one unsaturated compound is an organosilane selected from the group consisting of tetravinylsilane, tetraallylsilane, 1,2,4-trivinylcyclohexane, and combinations thereof.

7. R 1 and R 3 The highly branched polythioether according to any one of claims 4 to 6, having a phenyl group which may be substituted.

8. The at least one organic thiol has a divalent aromatic compound, and independently, the formula is: HS-R 4 -Ar-R 4 -SH [In the formula, each R 4 [Ar is an arylene group having a direct bond or 1 to 12 carbon atoms, and Ar is an arylene group having C, H, and optionally S or N atoms.] A highly branched polythioether according to any one of claims 4 to 7, as represented by [the specified method].

9. The highly branched polythioether according to claim 8, wherein the at least one organic thiol is selected from the group consisting of 1,3-benzenedithiol, 1,3-benzenedialkylthiol, or a combination thereof.

10. The highly branched polythioether according to any one of claims 4 to 7, wherein the at least one organic thiol comprises ,3-bis-2-mercaptoethylthio-1-propanthol, 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, and 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane. Other non-aromatic polyfunctional thiols include poly(ethylene glycol)dithiol, 1,2,3-trimercaptopropane, 2,3-bis-2-mercaptoethylthio-1-propanechol, 1,2-ethanedithiol, 2,2'-thiodiethanethiol, bi(mercaptoethyl)sulfide, 2,5-bis(mercaptomethyl)-1,4-dithiane, tetra(ethylene glycol)dithiol, 2,2'-(ethylenedioxy)diethanethiol, pentaerythritol tetrakis(3-mercaptopropionate), trimethylolpropanetris(3-mercaptopropionate), 【Chemistry 1】 Or a combination of these.

11. A method for producing highly branched polythioethers, wherein the method is At least one unsaturated compound having p independent vinyl or allyl groups, and consisting of C, H, and optionally Si and / or O atoms, where each p is an integer of 2 or more, At least one organic thiol having q thiol groups and consisting of C, H, S, and optionally O and / or N atoms, where each q is an integer of 2 or more independently. A method that includes combining [something].

12. A curable composition, (i) the highly branched polythioether according to any one of claims 1 to 11 and (ii) at least one polyfunctional compound and A curable composition comprising, wherein components (i) and (ii) react via a thiol-ene reaction, and the curable composition is substantially solvent-free.

13. The curable composition according to claim 12, wherein the terminal functional group of the highly branched polythioether has a carbon-carbon double bond, and the at least one polyfunctional compound has a plurality of terminal thiol groups.

14. The curable composition according to claim 13, wherein the at least one polyfunctional compound having a plurality of terminal thiol groups is an aromatic polythiol.

15. The curable composition according to claim 13, wherein the at least one polyfunctional compound having a plurality of terminal thiol groups is 4-mercaptomethyl-1,8-dimercapto-3,6-dithiaoctane, 5,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,8-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, 4,7-dimercaptomethyl-1,11-dimercapto-3,6,9-trithiaundecane, pentaerythritol tetrakis(3-mercaptopropionate), trimethylolpropanetris(3-mercaptopropionate), or a combination thereof.

16. The curable composition according to claim 12, wherein the terminal functional group of the highly branched polythioether has a thiol group, and the at least one polyfunctional compound has a plurality of terminal carbon-carbon double bonds.

17. The curable composition according to claim 16, wherein the at least one polyfunctional compound having a plurality of terminal carbon-carbon double bonds is a highly branched polythioether, tetravinylsilane, tetraallylsilane, trivinylcyclohexane, and a combination thereof.

18. The curable composition according to any one of claims 12 to 17, wherein the at least one polyfunctional compound is a highly branched polythiol ether according to any one of claims 1 to 11.

19. The curable composition according to any one of claims 12 to 18, wherein the ratio of thiol groups to terminal carbon-carbon double bonds is 1:0.8 to 0.8:

1.

20. The curable composition according to any one of claims 12 to 19, wherein the curable composition further comprises a free radical initiator.

21. A curable composition, (i) A highly branched polythioether according to any one of claims 1 to 11, having a plurality of terminal carbon-carbon double bonds, (ii) Free radical initiators, and (iii) Optionally, at least one polyfunctional compound having multiple terminal carbon-carbon double bonds. A curable composition comprising, wherein the curable composition is substantially solvent-free.

22. The curable composition according to claim 21, wherein the polyfunctional compound is a highly branched polythioether having a plurality of terminal carbon-carbon double bonds as described in any one of claims 1 to 11.

23. The curable composition according to claim 22, comprising at least two compositionally distinct, highly branched polythioethers having multiple terminal carbon-carbon double bonds.

24. A curable composition according to any one of claims 12 to 23, having a refractive index of 1.660 or higher (at 450 nm) after curing.

25. A curable composition according to any one of claims 12 to 24, further comprising an inhibitor.

26. A curable composition according to any one of claims 12 to 25, further comprising a heat stabilizer.

27. A curable composition according to any one of claims 12 to 26, further comprising an adhesion promoter.

28. A curable composition according to any one of claims 12 to 27, having a viscosity of 100 cps or less at temperatures from room temperature to 35°C.

29. Articles, A substrate having a first main surface and a second main surface, A cured organic layer adjacent to at least a portion of the second main surface of the substrate, wherein the cured organic layer is derived from the curable composition described in any one of claims 12 to 28. The inorganic barrier layer in contact with the aforementioned hardened organic layer An article comprising the above, wherein the cured organic layer has a refractive index of 1.660 or higher (measured at 450 nm).

30. The article according to claim 29, wherein the cured organic layer is optically transparent.

31. The article according to claim 29 or 30, wherein the cured organic layer has a glass transition temperature of at least 5°C.

32. The article according to any one of claims 29 to 31, wherein the cured organic layer has a thickness of 5 to 30 micrometers and a surface roughness of 5 nanometers or less.

33. The article according to any one of claims 29 to 32, further comprising a device disposed on a second main surface of the substrate and adjacent to the cured organic layer.

34. The article according to claim 33, wherein the device includes an OLED (organic light-emitting diode).

35. A method for preparing an article, To provide a substrate having a first main surface and a second main surface; To provide a curable composition according to any one of claims 12 to 28; The curable composition is placed on at least a portion of the second main surface of the substrate to form a curable layer; The curable layer is cured to form a cured organic layer, wherein the cured organic layer has a refractive index of at least 1.660 as measured at 450 nm; and Depositing an inorganic barrier layer on the aforementioned hardened organic layer. Methods that include...

36. The method according to claim 35, wherein the curable composition is placed on the second main surface of the substrate to form a curable layer, and this is further comprising inkjet printing to a thickness of 5 to 30 micrometers.

37. The method according to claim 35 or 36, further comprising providing a device and placing the device on the second main surface of the substrate before placing the curable composition on the second main surface of the substrate to form a curable layer.